Active material, electrode, secondary battery, battery pack and vehicle

A composite active material with lithium composite oxide and cobalt-containing oxide particles coated with a solid electrolyte stabilizes cobalt-containing oxides at high potentials, addressing the challenge of hydrogen gas generation and enhancing cycle life and voltage stability in non-aqueous electrolyte batteries.

JP7581084B2Active Publication Date: 2024-11-12KK TOSHIBA
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021032659
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-02
Publication Date
2024-11-12
Estimated Expiration
2041-03-02

AI Technical Summary

Technical Problem

Non-aqueous electrolyte batteries face challenges in achieving high operating voltages while maintaining excellent cycle life characteristics due to the instability of cobalt-containing oxides at potentials above 4.4V, leading to hydrogen gas generation and structural instability.

Method used

A composite active material comprising first active material particles with a lithium composite oxide at 4.4V or higher and second active material particles with cobalt-containing oxide particles coated with a solid electrolyte layer, such as Li1+xAlxTi2-x(PO4)3, to stabilize the cobalt-containing oxide and oxidize hydrogen gas to protons, thereby maintaining high operating voltage and improving cycle life.

Benefits of technology

The composite active material effectively stabilizes cobalt-containing oxides, reducing hydrogen gas generation and enhancing cycle life characteristics while maintaining high operating voltage, thus improving the performance of secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581084000002
    Figure 0007581084000002
  • Figure 0007581084000003
    Figure 0007581084000003
  • Figure 0007581084000004
    Figure 0007581084000004
Patent Text Reader

Abstract

To provide an active material capable of realizing excellent cycle life characteristics while maintaining a high operating voltage.SOLUTION: An active material according to an embodiment includes a first active material particle containing a lithium composite oxide exhibiting an action potential of 4.4 V or higher relative to metallic lithium, and a second active material particle different from the first active material particle. The second active material particle includes a cobalt-containing oxide particle and a covering layer covering at least a part of the surface of the cobalt-containing oxide particle. The coating layer contains a solid electrolyte.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THE DISCLOSURE Embodiments of the present invention relate to an active material, an electrode, a secondary battery, a battery pack, and a vehicle. [Background technology]

[0002] Non-aqueous electrolyte batteries, such as lithium-ion batteries, in which lithium ions carry electric charge, are being widely used in a wide range of applications, from small applications such as portable electronic devices to large applications such as electric vehicles and power supply and demand adjustment, taking advantage of the advantages of being able to obtain high energy density and high output. To date, non-aqueous electrolyte batteries have used lithium transition metal composite oxides, such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), and lithium manganese oxide (LiMn2O4), as the positive electrode active material. In addition, batteries using carbon materials as the negative electrode active material have been commercially available.

[0003] Non-aqueous electrolyte batteries using lithium titanium composite oxide, which has a high lithium absorption / release potential of about 1.55 V versus metallic lithium, instead of carbon materials as the negative electrode active material, have also been put to practical use. Lithium titanium composite oxide has excellent cycle characteristics because there is little volume change during charging and discharging. In addition, negative electrodes containing lithium titanium composite oxide do not precipitate lithium metal during lithium absorption / release, so secondary batteries equipped with this negative electrode can be charged at a large current.

[0004] As for the positive electrode active material, lithium manganese oxide (LiMn2O4) is abundant, inexpensive, has a low environmental impact, and is highly safe in an overcharged state. For this reason, lithium manganese oxide is being considered as an alternative to lithium cobalt oxide (LiCoO2). However, the average operating potential of lithium manganese oxide is about 4.1 V based on metallic lithium. This makes it difficult to achieve a high battery voltage. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-134997 A [Patent Document 2] JP 2007-273260 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention aims to provide an active material capable of realizing excellent cycle life characteristics while maintaining a high operating voltage, an electrode containing this active material, a secondary battery including this electrode, a battery pack including this secondary battery, and a vehicle including this battery pack. [Means for solving the problem]

[0007] According to an embodiment, an active material is provided, which includes first active material particles including a lithium composite oxide exhibiting an operating potential of 4.4 V or more versus metallic lithium, and second active material particles different from the first active material particles. The lithium composite oxide contains a lithium phosphate compound. The lithium phosphate compound is represented by the following general formula (II). Li w M2 y Co 1-y PO 4 ···(II) In the general formula (II), M2 is at least one selected from the group consisting of Ni and Cu. w satisfies 0 < w ≦ 1, and y satisfies 0 ≦ y ≦ 1. The second active material particles include cobalt-containing oxide particles and a coating layer that covers at least a part of the surface of the cobalt-containing oxide particles. Each of the first active material particles and the second active material particles is selected from primary particles, secondary particles formed by agglomeration of the primary particles, and a mixture of primary particles and secondary particles. The coating layer includes a solid electrolyte. The solid electrolyte has a NASICON-type skeleton and is represented by the general formula Li 1+x Al x Ti 2-x It is an inorganic compound represented by the formula (PO4)3, where 0≦x≦0.5.

[0008] According to another embodiment, an electrode is provided that includes an active material according to the embodiment.

[0009] According to another embodiment, a secondary battery is provided, the secondary battery including a positive electrode which is an electrode according to the embodiment, a negative electrode, and an electrolyte.

[0010] According to another embodiment, a battery pack is provided, the battery pack including a secondary battery according to the embodiment.

[0011] According to another embodiment, a vehicle is provided, the vehicle including a battery pack according to an embodiment. [Brief description of the drawings]

[0012]

Figure 1

Figure 2

Figure 3

Figure 4

Figure 5

Figure 6

Figure 7

Figure 8

Figure 9

[0013] Hereinafter, the embodiments will be described with reference to the drawings as appropriate. Note that the same reference numerals are used to designate common components throughout the embodiments, and duplicated descriptions will be omitted. Also, each figure is a schematic diagram for explaining the embodiments and for facilitating understanding thereof, and the shapes, dimensions, ratios, etc. may differ from those of the actual device, but these can be appropriately modified in design by taking into consideration the following explanation and known techniques.

[0014] It is known that spinel-type lithium manganese oxide, which has been used as an active material, acts as a strong oxidizing agent and reacts with an electrolyte or an electrolyte salt to generate hydrogen gas. In addition, cobalt-containing oxides such as lithium cobalt oxide act as a buffer against the oxidizing action of spinel-type lithium manganese oxide. In other words, when spinel-type lithium manganese oxide and cobalt-containing oxide are mixed and used, the cobalt-containing oxide oxidizes the hydrogen gas generated by spinel-type lithium manganese oxide to protons.

[0015] The present inventors have developed a cobalt-containing oxide at 4.4 V (vs. Li / Li + ), it was found that the hydrogen gas could not be oxidized to protons sufficiently. + ) At operating potentials above this level, the crystal structure of the cobalt-containing oxide becomes unstable, so the above-mentioned effects are not obtained and, conversely, the amount of gas generated increases.

[0016] (First embodiment) According to a first embodiment, an active material is provided. The active material includes first active material particles including a lithium composite oxide exhibiting an operating potential of 4.4 V or more versus metallic lithium, and second active material particles different from the first active material particles. The second active material particles include cobalt-containing oxide particles and a coating layer that coats at least a portion of the surface of the cobalt-containing oxide particles. The coating layer includes a solid electrolyte.

[0017] The active material according to the embodiment includes first active material particles containing a lithium composite oxide exhibiting an operating potential of 4.4 V or more versus metallic lithium, and cobalt-containing oxide particles (second active material particles) at least partially coated with a coating layer containing a solid electrolyte. When the cobalt-containing oxide particles are coated with a coating layer, the active material has an operating potential of 4.4 V (vs. Li / Li + ) or higher, the crystal structure of the cobalt-containing oxide can be stably maintained. The reason for this is not clear in detail, but Cobalt-containing oxide The particle surface is covered with a coating layer, Cobalt-containing oxide This is believed to be because contact between the particles and the electrolyte is suppressed, reducing metal elution.

[0018] The second active material particles, which contain a stable cobalt-containing oxide, can oxidize the hydrogen gas generated by the first active material particles to protons. In other words, even when charging and discharging are repeated, it is possible to prevent hydrogen gas from filling the secondary battery. Therefore, the active material according to the embodiment can achieve excellent cycle life characteristics. In addition, the operating potential of the first active material particles is 4.4 V (vs. Li / Li + ) or more, a secondary battery exhibiting a high operating voltage can be realized.

[0019] Hereinafter, the active material according to the embodiment will be described in detail.

[0020] The active material according to the embodiment may be a positive electrode active material used in a positive electrode, or a negative electrode active material used in a negative electrode. Whether the active material according to the embodiment is a positive electrode active material or a negative electrode active material depends on the operating potential of the active material contained in the counter electrode.

[0021] The first active material particles are particles containing a lithium composite oxide that exhibits an operating potential of 4.4 V or more versus metallic lithium. The number of the first active material particles may be one or more. Each of the first active material particles has an operating potential of 4.4 V (vs. Li / Li +)It may consist only of the lithium composite oxide showing the above operating potential. That is, the first active material particles may consist only of the lithium composite oxide. In this case, since the operating potential of the entire first active material particles is high, a high battery capacity can be achieved.

[0022] As an example of the lithium composite oxide showing an operating potential of 4.4 V or more based on metallic lithium, for example, an oxide represented by the following general formula (A) can be mentioned.

[0023] Li u M1 x Mn 2-x O4···(A) In the general formula (A), M1 is at least one selected from the group consisting of Mn, Ni, Fe, Co, Cr, Mg, Zn, Al and Cu, u satisfies 0 < u ≦ 1, and x satisfies 0 < x ≦ 1.

[0024] As a specific example of the lithium composite oxide represented by the general formula (A), for example, LiNi 0.5 Mn 1.5 O4 and LiCu 0.5 Mn 1.5 O4 can be mentioned.

[0025] The first active material particles may contain only one kind of lithium composite oxide showing an operating potential of 4.4 V or more based on metallic lithium, or may contain a plurality of kinds of the lithium composite oxide.

[0026] The lithium composite oxide showing an operating potential of 4.4 V or more based on metallic lithium contains, for example, at least one selected from the group consisting of lithium nickel manganese oxide and lithium phosphate compound. Among the above lithium composite oxides, since the electron conductivity is high and the structure is stable even when the voltage is increased to around 5 V, the first active material particles preferably contain lithium nickel manganese oxide. Lithium nickel manganese oxide has, for example, a crystal structure of a spinel structure.

[0027] Lithium nickel manganese oxide is represented by, for example, the following general formula (I). In this case, as described above, since the structure is stable even when the voltage is increased, excellent cycle life characteristics are easily obtained while maintaining a high operating voltage. Li u Ni x Mn 2-x O4···(I) In general formula (I), u satisfies 0 < u ≦ 1, and x satisfies 0 < x ≦ 1.

[0028] As a specific example of the lithium nickel manganese oxide represented by general formula (I), for example, LiNi 0.5 Mn 1.5 O4 can be mentioned.

[0029] The lithium phosphate compound is represented by, for example, the following general formula (II).

[0030] Li w M2 y Co 1-y PO4···(II) In general formula (II), M2 is at least one selected from the group consisting of Ni and Cu, w satisfies 0 < w ≦ 1, and y satisfies 0 ≦ y ≦ 1. The lithium phosphate compound has, for example, a crystal structure of an olivine structure.

[0031] As specific examples of the lithium phosphate compound represented by general formula (II), for example, LiNiPO4 and LiCoPO4 can be mentioned.

[0032] The second active material particles include at least one cobalt-containing oxide particle and a coating layer that coats at least a part of the surface of the cobalt-containing oxide particle. In an embodiment, the cobalt-containing oxide particle included in the second active material particle is a different active material from the first active material particle. The number of the second active material particles can be one or more. A part of the cobalt-containing oxide particles included in the second active material particles may have a coating layer, or all of the cobalt-containing oxide particles included in the second active material particles may have a coating layer.

[0033] The cobalt-containing oxide particles are, for example, Li x Ni a Co b Mn c M3 d O2 (where 0 < x ≤ 1.0, 0.3 ≤ a ≤ 1.0, 0 ≤ b ≤ 0.4, 0 ≤ c ≤ 0.4, 0 ≤ d ≤ 0.4, and M3 is at least one selected from the group consisting of Mg, Fe, Ni, Co, W, Ta, and Mo), LiM x Co 1-x PO4, Li2M x Co 1-x PO4F, LiM x Co 1-x O2, LiM x Co 1-x BO3, and LiM x Co 1-x SiO4 (in these general formulas, x satisfies 0 ≤ x ≦ < 0.8, and M is at least one selected from the group consisting of Mn, Ni, Fe, Mg, Zn, and Al), and contains at least one selected from the group consisting of these.

[0034] Among these, Li x Ni a Co b Mn c M3 d O2 (also referred to as NCM), and LiM x Co 1-x PO4 (also referred to as LCP) are preferable because they have high structural stability and a high effect of oxidizing hydrogen gas to protons. All of the cobalt-containing oxide particles contained in the second active material particles may be NCM, or may be LCP. Alternatively, the cobalt-containing oxide particles contained in the second active material particles may be a mixture of NCM and LCP.

[0035] The cobalt-containing oxide particles may also include at least one selected from the group consisting of cobalt oxide, iron cobalt oxide, cobalt (II) carbonate, cobalt (II) phosphate, cobalt (III) acetylacetonate, cobalt (II) thiocyanate, lithium cobalt phosphate, cobalt hydroxide, nickel cobalt oxide, cobalt nitrate, cobalt acetate, aluminum cobalt oxide, and lithium nickel manganese cobalt oxide.

[0036] The mass ratio of the coating layer to the mass of the second active material particles is in the range of 0.1% by mass to 10% by mass, preferably in the range of 1.0% by mass to 5.0% by mass, and more preferably in the range of 2.0% by mass to 5.0% by mass. If the ratio is too small, the effect of suppressing side reactions by the coating layer may not be sufficiently obtained. If the ratio is too large, the mass or volume of the coating layer in the active material-containing layer constituting the electrode is too large, which is undesirable because it reduces the energy density per weight or volume of the battery. The mass ratio of the coating layer to the mass of the second active material particles can be analyzed by inductively coupled plasma (ICP) spectroscopy, which will be described later.

[0037] The coating layer includes a solid electrolyte. The coating layer may be made of a solid electrolyte. The lithium ion conductivity of the solid electrolyte is 1×10 at 25° C. -10 It is preferable that the lithium ion conductivity of the solid electrolyte at 25° C. is 1×10 -10 By having a lithium ion conductivity of 1×10 S / cm or more, the lithium ion concentration near the surface of the solid electrolyte is likely to be high, which can improve the rate performance and life characteristics. The lithium ion conductivity of the solid electrolyte at 25°C is 1×10 -6 The upper limit of the lithium ion conductivity of the solid electrolyte is, for example, 2×10 -2 S / cm.

[0038] Examples of the solid electrolyte include sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and polymer solid electrolytes. Specific examples of the solid electrolyte include sulfide-based Li2SeP2S5-based glass ceramics and lithium lanthanum titanium composite oxides (e.g., Li 0.5 La 0.5 TiO3), inorganic compounds with LISICON structure (e.g., Li 3.6 S 0.6 P 0.4 O4), an inorganic compound with a NASICON structure, and amorphous LIPON (Li 2.9 PO 3.3 N 0.46 ), lithium calcium zirconium oxide (Li 1.2 Zr 1.9 Ca 0.1 (PO4)3) and at least one selected from the group consisting of inorganic compounds having a garnet structure. The coating layer may contain one type of solid electrolyte or may contain two or more types of solid electrolytes.

[0039] The inorganic compound having a NASICON skeleton is preferably an inorganic compound represented by the general formula LiM2(PO4)3 (wherein M is at least one selected from Ti, Ge, Sr, Zr, Sn, and Al). 1+x Al x Ge 2-x (PO4)3, Li 1+x Al x Zr 2-x (PO4)3, Li 1+x Al x Ti 2-x (PO4)3(LATP) is preferred because it has high ionic conductivity and high electrochemical stability against water. In the above, x preferably satisfies 0≦x≦0.5.

[0040] Examples of inorganic compounds having a garnet structure include Li 5+x A y La 3-y M2O 12(A is at least one selected from the group consisting of Ca, Sr and Ba, and M is at least one selected from the group consisting of Nb and Ta), Li3M 2-x ZrO 12 (M is at least one selected from the group consisting of Ta and Nb), Li 7-3x Al x La3Zr3O 12 , and Li7La3Zr2O 12 In the above, x is, for example, 0≦x<0.8, and preferably 0≦x≦0.5. y is, for example, 0≦y<2. The oxide having a garnet structure may be composed of one of these compounds, or may contain a mixture of two or more of these compounds. Among these, Li 6.25 Al 0.25 La3Zr3O 12 and Li7La3Zr2O 12 Since it has high ionic conductivity and is electrochemically stable, it has excellent discharge performance and cycle life performance.

[0041] It is not preferable for the solid electrolyte to contain elemental sulfur, since the sulfur component dissolves in the organic electrolyte described below.It is preferable for the solid electrolyte to not contain elemental sulfur.

[0042] A preferred solid electrolyte is LATP (Li 1+x Al x Ti 2-x (PO4)3), amorphous LIPON, garnet-type lithium lanthanum zirconium oxides (e.g., Li7La3Zr2O 12 :LLZ) and other oxides.

[0043] The lithium ion conductivity of the inorganic compound represented by LiM2(PO4)3 having a NASICON structure at 25°C is, for example, 1×10 -3 S / cm~1×10 -5 S / cm range. 2.9 PO 3.3 N 0.46 ) at 25°C has a lithium ion conductivity of 3×10-6 S / cm. Garnet-type LLZ (Li7La3Zr2O 12 ) at 25°C has a lithium ion conductivity of 3×10 -4 S / cm.

[0044] Among these, the solid electrolyte is preferably LATP having a NASICON-type skeleton. LATP has high lithium ion conductivity and is not decomposed by water, so it can exist stably even in air.

[0045] In addition, it is preferable that the above-mentioned first active material particles are not coated on the surface with the coating layer. That is, it is preferable that the first active material particles are made of only a lithium composite oxide exhibiting an operating potential of 4.4 V or more based on metallic lithium. Of the first active material particles and the second active material particles, it is preferable that only the second active material particles have a coating layer. When the surface of the first active material particles is not covered with a coating layer, it is possible to prevent an excessive increase in resistance and a decrease in battery capacity.

[0046] The ratio (MP1 / MP2) of the mass of the first active material particles (MP1) to the mass of the second active material particles (MP2) is, for example, in the range of 2 to 20, preferably in the range of 3 to 10, and more preferably in the range of 5 to 10. When the mass ratio is within this range, there is an effect of reducing gas generation while maintaining the high operating voltage and input / output characteristics attributable to the first active material particles.

[0047] The active material according to the embodiment may contain another active material different from the first active material particles and the second active material particles. The proportion of the other active material in the entire active material may be 20% by mass or less, 10% by mass or less, or 0% by mass.

[0048] Other active materials include, for example, oxides and polymers. Examples of oxides include lithium-absorbed manganese dioxide (MnO2), iron oxide, copper oxide, nickel oxide, and lithium manganese composite oxides (e.g., Li x Mn2O4 or Li xMnO2), lithium nickel composite oxide (e.g., Li x NiO2), lithium phosphate having an olivine structure (e.g., Li x FePO4, Li x Fe 1-y Mn y PO4), iron sulfate (Fe2(SO4)3), and vanadium oxide (e.g., V2O5). It is preferable that the above x satisfies 0 < x ≤ 1 and y satisfies 0 ≤ y ≤ 1.

[0049] As the polymer, for example, a conductive polymer material such as polyaniline and polypyrrole, or a disulfide-based polymer material can be used. Sulfur (S) and carbon fluoride can also be used as the active material.

[0050] The median diameter (D50, hereinafter referred to as "MD1") of the first active material particles is, for example, in the range of 0.1 μm to 100 μm, preferably in the range of 1 μm to 10 μm. If the median diameter of the first active material particles is excessively small, there tend to be many side reactions and an increase in gas, which is not preferable. Also, if the median diameter of the first active material particles is excessively large, the specific surface area is small, so the contact interface with the electrolyte decreases, and the input / output characteristics tend to deteriorate, which is not preferable.

[0051] The first active material particles can be primary particles, secondary particles in which the primary particles are aggregated, and mixtures thereof.

[0052] The median diameter (D50, hereinafter referred to as "MD2") of the second active material particles is, for example, in the range of 0.01 μm to 100 μm, preferably in the range of 0.05 μm to 10 μm. When the median diameter of the second active material particles is within the preferable range, it is possible to ensure an appropriate surface area for treating the gas generated from the first active material particles while suppressing side reactions. Incidentally, cobalt-containing oxide particles are LCP (LiM x Co 1-xIn the case of particles with low conductivity such as PO4, the median diameter of the second active material particles is preferably in the range of 0.05 μm to 5 μm. By making the median diameter of the second active material particles relatively small, the electrode density can be increased, so that an electron conduction path in the active material-containing layer can be formed well.

[0053] The second active material particles can be primary particles, secondary particles in which the primary particles are aggregated, and mixtures thereof.

[0054] The value of the ratio (MD1 / MD2) of the median diameter MD1 of the first active material particles to the median diameter MD2 of the second active material particles is, for example, 1.0 or more. When the ratio (MD1 / MD2) is 1.0 or more, the second active material particles are likely to be dispersed between the first active material particles, which is advantageous for oxidizing the hydrogen gas generated from the first active material particles to protons. The ratio (MD1 / MD2) may be in the range of 1.0 or more and 5.0 or less, or may be in the range of 2.0 or more and 5.0 or less. When the ratio (MD1 / MD2) is within this range, the dispersibility of the first and second active material particles in the active material-containing layer tends to be good. That is, in the active material-containing layer, both are distributed without being biased. Therefore, the second active material particles can easily oxidize the hydrogen gas generated from the first active material particles. As a result, excellent cycle life characteristics can be achieved. In addition, since the second active material particles are likely to be dispersed between the first active material particles, the electrode density can be increased and a high capacity can be realized.

[0055] <X-ray Diffraction (XRD) and Rietveld analysis> The mass ratio between the first active material particles and the second active material particles can be measured by performing XRD and Rietveld analysis. First, after completely discharging the battery, it is disassembled in an inert atmosphere, and the electrode containing the active material according to the embodiment is cut out. This electrode is, for example, the positive electrode. The cut-out electrode is first impregnated for 10 minutes in a mixed solvent with a volume ratio of 1:1 of propylene carbonate, which is a cyclic solvent, and diethyl ether, which is a chain solvent, to dissolve the lithium salt remaining in the active material-containing layer. Further, it is impregnated in the diethyl ether solvent for 10 minutes to remove the solvent from the electrode active material layer. The washed electrode is punched out to, for example, 14 mmφ and placed in a measurement holder. It is preferable to perform X-ray diffraction measurement while maintaining an inert atmosphere. For the measurement, an XRD measurement device such as a BRUKER desktop X-ray diffractometer D2 PHASER, or a device having an equivalent function is used. The measurement conditions are as follows. That is, a Cu-Kα ray source is used as the X-ray source, the diffraction angle 2θ is from 10 degrees to 80 degrees, the step width is 0.02 degrees, and the integration time is 2.0 seconds. The mass ratio between the first active material particles and the second active material particles is identified by performing Rietveld analysis on the obtained diffraction peaks.

[0056] Rietveld analysis can be performed, for example, by TOPAS (BRUKER) as follows. First, assume the crystal structure of the active material contained in the electrode, define the background function, and perform fitting. Since the sample is completely discharged, the initial value of the occupancy of the Li site is set to 1, but fitting is performed without fixing the occupancy. For a compound system that forms a solid solution having the same crystal structure but different composition ratios of transition metals, a plurality of corresponding transition metals are given for the same site, and fitting is performed with the occupancy as a parameter. Fitting is considered complete when the S value (Goodness-of-fit) converges to 1.3 or less. The mass ratio between the first active material particles and the second active material particles is obtained from the composition ratio of the active material given from the analysis results.

[0057] <ICP (Inductively Coupled Plasma) Optical Emission Spectrometry> The proportion of the coating layer in the second active material particles can be measured from the mass ratio of the first active material particles and the second active material particles obtained by the above-mentioned XRD and Rietveld analysis and the results of the ICP analysis described below.

[0058] The abundance ratio (molar ratio) of each element contained in the active material to be analyzed depends on the sensitivity of the analysis device used. Therefore, the measured molar ratio may deviate from the actual molar ratio by the error of the measurement device. However, even if the value deviates from the error range of the analysis device, the performance of the active material according to the embodiment can be fully exhibited.

[0059] When analyzing the active material incorporated in a battery, prepare the active material powder using the procedure explained in the section on laser diffraction scattering method below. By dissolving this powder in acid, a liquid sample containing the active material can be created. The acid that can be used in this case includes hydrochloric acid, nitric acid, sulfuric acid, and hydrofluoric acid. By subjecting this liquid sample to ICP analysis, the elemental composition of the active material can be determined.

[0060] <Particle size distribution measurement using laser diffraction scattering method> The median diameter (MD1) of the first active material particles and the median diameter (MD2) of the second active material particles can be measured, for example, by the following method.

[0061] When the active material according to the embodiment is incorporated into a secondary battery, the measurement is carried out according to the following procedure.

[0062] First, the electrode is removed from the secondary battery. At this time, the electrode is brought into a state close to a state in which lithium ions are completely removed from the active material in the electrode. For example, when the active material is contained in the negative electrode, the battery is brought into a fully discharged state. For example, the battery is discharged at a current of 0.1 C in a 25°C environment until the rated end voltage or the battery voltage reaches 1.0 V, and the current value during discharge is 1 / 100 or less of the rated capacity, thereby bringing the battery into a discharged state.

[0063] Next, the battery is disassembled in a dry atmosphere such as a glove box filled with argon to remove the electrodes. The removed electrodes are washed with an appropriate solvent and dried under reduced pressure. For example, ethyl methyl carbonate is used as the solvent. After washing and drying, it is confirmed that there is no white precipitate such as lithium salt on the surface of the electrodes. In this way, an electrode sample is obtained.

[0064] From the obtained electrode sample, a portion containing an active material such as an active material-containing layer is peeled off. For example, the portion containing the active material can be peeled off by irradiating ultrasonic waves. As a specific example, the electrode is placed in ethyl methyl carbonate in a glass beaker and vibrated in an ultrasonic cleaner, whereby the active material-containing layer containing the active material can be peeled off from the current collector. Next, the peeled off portion is heated in air for a short time (for example, for about 1 hour at 500°C) to burn off unnecessary components such as binder components and carbon, thereby obtaining an active material powder. Thereafter, the obtained active material powder is separated into first and second active material particles by centrifugation. Note that, when the active material powder itself to be measured is available, it is separated into first and second active material particles by centrifugation.

[0065] The first and second active material particles thus obtained are subjected to particle size distribution measurement according to the following procedure, thereby measuring the median diameter of each particle. The active material particles are dispersed in pure water and ultrasonically treated to obtain a dispersion liquid as a sample for particle size distribution measurement. The particle size distribution of the constituent particles of this dispersion liquid is measured using a laser diffraction distribution measuring device. As a measuring device, for example, Microtrack MT3100II manufactured by Microtrack Bell Co., Ltd. can be used. The ultrasonic treatment for obtaining the dispersion solvent is performed by a sample supply system associated with the laser diffraction distribution measuring device. The ultrasonic treatment is performed for 180 seconds at an output of 40 kHz and 30 W.

[0066] <Scanning Electron Microscopy-Energy Dispersive X-ray Spectroscopy (SEM-EDX)> In addition, by carrying out SEM-EDX (Scanning Electron Microscope - Energy Dispersive X-ray Spectroscopy) on the first active material particles and the second active material particles separated by the above-mentioned procedure, it can be confirmed that a coating layer is formed only on the second active material particles. First, the powder to be analyzed is attached to the SEM sample stage. At this time, the powder may be treated with conductive tape or the like so that it does not peel off from the sample stage. The powder attached to the SEM sample stage is observed with an SEM to obtain an SEM image. During SEM measurement, the observation is performed at a magnification of 10,000 times. It is preferable to maintain an inert atmosphere when introducing the powder into the sample chamber.

[0067] Furthermore, an element mapping image corresponding to the SEM image is obtained by EDX. By observing the element mapping images of the first active material particles and the second active material particles, it is possible to confirm that a coating layer is formed only on the second active material particles. If EDX observation is not possible due to sensitivity issues, X-ray fluorescence analysis (XRF) can be performed instead to detect and map the elements contained in the coating layer.

[0068] Next, a method for producing the second active material particles, that is, a method for forming a coating layer on the surface of the cobalt-containing oxide particles will be described.

[0069] The method for forming the coating layer is not particularly limited, and for example, a sol-gel method or a thermal solid solution method can be adopted. From the viewpoint of forming the coating layer uniformly on the particle surface, the sol-gel method, which can obtain a solution containing a solid electrolyte, is preferred.

[0070] A solution obtained by a sol-gel method or the like is applied (coated) onto the surface of the cobalt-containing oxide particles, and then dried to form a coating layer. Specifically, the solution can be applied onto the particle surface by a spray-drying method, a spraying method using a tumbling fluidizer, an impregnation method, a vacuum impregnation method using an evaporator, or the like. The coating layer may also be formed by a sputtering method.

[0071] If the concentration of the sol-gel liquid is too high, the particle size distribution tends to be broad, and if it is too low, it takes a long time for the water to evaporate during firing, so the solid concentration of the sol-gel liquid is preferably within the range of 1% to 60%. By increasing the solid concentration in the sol-gel liquid, the mass of the coating layer provided on the second active material particles tends to increase.

[0072] In this way, the second active material particles are obtained. The active material according to the embodiment can be produced by mixing the obtained second active material particles with the first active material particles having a desired composition in any ratio.

[0073] According to a first embodiment, an active material is provided. The active material includes first active material particles including a lithium composite oxide exhibiting an operating potential of 4.4 V or more versus metallic lithium, and second active material particles different from the first active material particles. The second active material particles include cobalt-containing oxide particles and a coating layer that coats at least a portion of the surface of the cobalt-containing oxide particles. The coating layer includes a solid electrolyte. This active material can achieve excellent cycle life characteristics while maintaining a high operating voltage.

[0074] Second embodiment According to a second embodiment, an electrode is provided. The electrode according to the second embodiment includes the active material according to the first embodiment. The electrode according to the embodiment may be a negative electrode or a positive electrode. The electrode according to the embodiment is, for example, an electrode for a battery, an electrode for a secondary battery, or an electrode for a lithium secondary battery. The electrode may be a positive electrode including the active material according to the first embodiment as a positive electrode active material.

[0075] The electrode according to the second embodiment may include a current collector and an active material-containing layer including the active material according to the first embodiment. The active material-containing layer may be formed on one or both sides of the current collector. The active material-containing layer may include an active material, and optionally a conductive agent and a binder.

[0076] The active material-containing layer may contain a single active material according to the first embodiment, or may contain two or more types of active materials according to the first embodiment. The active material-containing layer may contain a mixture of one or more types of active materials according to the first embodiment and one or more types of other active materials.

[0077] The conductive agent is blended to improve current collection performance and reduce contact resistance between the active material and the current collector. Examples of the conductive agent include carbonaceous materials such as acetylene black, carbon black, graphite, carbon nanofibers, and carbon nanotubes. One of these may be used as the conductive agent, or two or more may be used in combination as the conductive agent. The conductive agent may also be omitted.

[0078] The binder is blended to fill the gaps between the dispersed active materials and to bind the active materials and the current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene butadiene rubber, acrylic resin or its copolymer, polyacrylic acid, and polyacrylonitrile. One of these may be used as the binder, or two or more may be used in combination as the binder.

[0079] The total amount of the active material in the active material-containing layer, the conductive agent, and the binder are preferably mixed in proportions of 80% by mass or more and 95% by mass or less, 3% by mass or more and 18% by mass or less, and 2% by mass or more and 17% by mass or less, respectively. The conductive agent can exhibit the above-mentioned effects by being mixed in an amount of 3% by mass or more. The conductive agent can be reduced in an amount of 18% by mass or less to reduce the decomposition of the electrolyte on the conductive agent surface during high-temperature storage. The binder can be reduced in an amount of 2% by mass or more to obtain sufficient electrode strength. The binder, which is an insulating material, can be mixed in an amount of 17% by mass or less to reduce internal resistance.

[0080] The current collector is preferably an aluminum foil or an aluminum alloy foil containing one or more elements selected from Mg, Ti, Zn, Ni, Cr, Mn, Fe, Cu, and Si. The thickness of the aluminum foil or aluminum alloy foil is preferably 5 μm or more and 20 μm or less, more preferably 15 μm or less. The purity of the aluminum foil is preferably 99% by mass or more. The content of transition metals such as iron, copper, nickel, and chromium contained in the aluminum foil or aluminum alloy foil is preferably 1% by mass or less.

[0081] The current collector may also include a portion on the surface of which no active material-containing layer is formed, and this portion can function as a current collecting tab.

[0082] The electrode can be produced, for example, by the following method. First, the active material according to the embodiment, the conductive agent, and the binder are suspended in a solvent to prepare a slurry. This slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate of an active material-containing layer and a current collector. After that, the laminate is pressed. In this manner, the electrode is produced.

[0083] Alternatively, the electrode may be prepared by the following method: first, the active material, the conductive agent, and the binder are mixed to obtain a mixture, then the mixture is formed into pellets, and then the pellets are placed on a current collector to obtain an electrode.

[0084] The electrode according to the second embodiment includes the active material according to the first embodiment, and therefore the electrode can achieve excellent cycle life characteristics while maintaining a high operating voltage.

[0085] Third embodiment According to a third embodiment, a secondary battery is provided that includes a negative electrode, a positive electrode, and an electrolyte. The secondary battery includes the electrode according to the second embodiment as a positive electrode.

[0086] The secondary battery according to the embodiment may further include a separator disposed between the positive electrode and the negative electrode. The negative electrode, the positive electrode, and the separator may constitute an electrode group. The electrolyte may be held in the electrode group.

[0087] The secondary battery may further include an exterior member that contains the electrode group and the electrolyte.

[0088] Furthermore, the secondary battery may further include a negative electrode terminal electrically connected to the negative electrode and a positive electrode terminal electrically connected to the positive electrode.

[0089] The secondary battery may be, for example, a lithium ion secondary battery. Also, the secondary battery may be a non-aqueous electrolyte secondary battery that contains a non-aqueous electrolyte.

[0090] The positive electrode, the negative electrode, the electrolyte, the separator, the exterior member, the negative electrode terminal, and the positive electrode terminal will be described in detail below.

[0091] (1) Positive electrode The positive electrode may be the electrode described in the second embodiment. The positive electrode may include a positive electrode current collector and a positive electrode active material-containing layer. The positive electrode current collector and the positive electrode active material-containing layer may be the current collector and the active material-containing layer that may be included in the electrode according to the second embodiment, respectively. The positive electrode active material-containing layer includes the active material according to the first embodiment as a positive electrode active material.

[0092] Among the details of the positive electrode, parts that overlap with those explained in the first and second embodiments will be omitted.

[0093] The electrode density of the positive electrode (excluding the current collector) is 2.0 g / cm 3 More than 4.0g / cm 3 A positive electrode having a positive electrode active material-containing layer with a density within this range is excellent in energy density and electrolyte retention. The electrode density of the positive electrode is preferably 2.5 g / cm or less. 3 More than 3.5g / cm 3 It is more preferable that:

[0094] The positive electrode can be produced, for example, by the same method as that for the electrode according to the second embodiment.

[0095] (2) Negative electrode The negative electrode may include a negative electrode current collector and a negative electrode active material-containing layer. The negative electrode active material-containing layer may be formed on one or both sides of the negative electrode current collector. The negative electrode active material-containing layer may include a negative electrode active material, and optionally a conductive agent and a binder.

[0096] The negative electrode active material contains at least one titanium-containing oxide selected from the group consisting of titanium oxide, lithium titanium composite oxide, niobium titanium composite oxide, and sodium niobium titanium composite oxide. Specific examples of the titanium-containing oxide include lithium titanate having a ramsdellite structure (e.g., Li 2+y Ti3O7, 0≦y≦3), lithium titanates with spinel structure (e.g., Li 4+x Ti5O 12 , 0≦x≦3), monoclinic titanium dioxide (TiO2), anatase titanium dioxide, rutile titanium dioxide, hollandite titanium composite oxide, monoclinic niobium titanium composite oxide, and orthorhombic titanium-containing composite oxide. Among them, from the viewpoint of achieving both high capacity and high rate performance, it is preferable that the negative electrode active material contains at least one selected from the group consisting of lithium titanium composite oxide and niobium titanium composite oxide. The lithium titanium composite oxide may have a spinel type crystal structure. The niobium titanium composite oxide may have a monoclinic type crystal structure.

[0097] As an example of the monoclinic niobium titanium composite oxide, Li x Ti 1-y M1 y Nb 2-z M2 z O 7+δHere, M1 is at least one selected from the group consisting of Zr, Si, and Sn. M2 is at least one selected from the group consisting of V, Ta, and Bi. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3. Specific examples of monoclinic niobium titanium composite oxides include Li x Examples include Nb2TiO7 (0≦x≦5).

[0098] Another example of monoclinic niobium titanium composite oxide is Ti 1-y M3 y+z Nb 2-z O 7-δ Here, M3 is at least one selected from Mg, Fe, Ni, Co, W, Ta, and Mo. The subscripts in the composition formula are 0≦y<1, 0≦z≦2, and -0.3≦δ≦0.3.

[0099] As an example of the orthorhombic titanium-containing composite oxide, Li 2+a M(I) 2-b Ti 6-c M(II) d O 14+σ Here, M(I) is at least one selected from the group consisting of Sr, Ba, Ca, Mg, Na, Cs, Rb, and K. M(II) is at least one selected from the group consisting of Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni, and Al. The subscripts in the composition formula are 0≦a≦6, 0≦b<2, 0≦c<6, 0≦d<6, and -0.5≦σ≦0.5. Specific examples of orthorhombic titanium-containing composite oxides include Li 2+a Na2Ti6O 14 (0≦a≦6).

[0100] The conductive agent is blended to improve the current collecting performance and to reduce the contact resistance between the active material and the current collector. Examples of the conductive agent include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, and carbonaceous materials such as graphite. One of these may be used as the conductive agent, or two or more may be used in combination as the conductive agent. Alternatively, instead of using a conductive agent, a carbon coating or an electronically conductive inorganic material coating may be applied to the surface of the active material particles.

[0101] The binder is blended to fill the gaps between the dispersed active materials and to bind the active materials and the negative electrode current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene butadiene rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.

[0102] The mixing ratio of the negative electrode active material, the conductive agent, and the binder in the negative electrode active material-containing layer can be appropriately changed depending on the application of the negative electrode. For example, it is preferable to mix the negative electrode active material, the conductive agent, and the binder in a ratio of 70% by mass or more and 96% by mass or less, 2% by mass or more and 28% by mass or less, and 2% by mass or more and 28% by mass or less, respectively. By making the amount of the conductive agent 2% by mass or more, the current collection performance of the negative electrode active material-containing layer can be improved. In addition, by making the amount of the binder 2% by mass or more, the binding property between the negative electrode active material-containing layer and the current collector becomes sufficient, and excellent cycle performance can be expected. On the other hand, it is preferable to make the conductive agent and the binder 28% by mass or less, respectively, in order to increase the capacity.

[0103] The negative electrode current collector is provided with a potential at which lithium (Li) is inserted and extracted from the active material, for example, 1.0 V (vs. Li / Li +) is used. For example, the current collector is preferably made of copper, nickel, stainless steel, aluminum, or an aluminum alloy containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si. The thickness of the current collector is preferably 5 μm or more and 20 μm or less. A current collector having such a thickness can balance the strength and weight of the electrode.

[0104] The negative electrode current collector may also include a portion on the surface of which the negative electrode active material-containing layer is not formed, and this portion can function as a negative electrode current collecting tab.

[0105] The density of the negative electrode active material-containing layer (excluding the current collector) is 1.8 g / cm 3 More than 2.8g / cm 3 A negative electrode having a density of the negative electrode active material-containing layer within this range is excellent in energy density and electrolyte retention. The density of the negative electrode active material-containing layer is preferably 2.1 g / cm or less. 3 More than 2.6g / cm 3 It is more preferable that:

[0106] The negative electrode can be produced, for example, by the same method as that for the electrode according to the second embodiment, except that a negative electrode active material is used.

[0107] (3) Electrolyte The electrolyte may be, for example, a liquid nonaqueous electrolyte or a gel nonaqueous electrolyte. The liquid nonaqueous electrolyte is prepared by dissolving an electrolyte salt as a solute in an organic solvent. The concentration of the electrolyte salt is preferably 0.5 mol / L or more and 2.5 mol / L or less.

[0108] Examples of the electrolyte salt include lithium salts such as lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), and lithium bistrifluoromethylsulfonylimide (LiN(CF3SO2)2), and mixtures thereof. The electrolyte salt is preferably one that is difficult to oxidize even at high potentials, and LiPF6 is most preferred.

[0109] Examples of organic solvents include cyclic carbonates such as propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC); chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (MEC); cyclic ethers such as tetrahydrofuran (THF), 2-methyl tetrahydrofuran (2MeTHF), and dioxolane (DOX); chain ethers such as dimethoxyethane (DME) and diethoxyethane (DEE); γ-butyrolactone (GBL), acetonitrile (AN), and sulfolane (SL). These organic solvents can be used alone or as a mixed solvent.

[0110] The gelled non-aqueous electrolyte is prepared by compounding a liquid non-aqueous electrolyte with a polymeric material. As the polymeric material, for example, at least one selected from the group consisting of polyvinylidene fluoride, polyacrylonitrile, polyethylene oxide, acrylic polymer, polyamide, and polyvinyl alcohol can be used. By using a gelled electrolyte as the electrolyte, it is possible to suppress the elution of metal from the positive electrode and the generation of gas such as hydrogen. As a result, excellent cycle life characteristics can be obtained.

[0111] Alternatively, as the nonaqueous electrolyte, in addition to liquid nonaqueous electrolytes and gel nonaqueous electrolytes, room temperature molten salts containing lithium ions (ionic melts), polymer solid electrolytes, inorganic solid electrolytes, and the like may be used.

[0112] Room temperature molten salts (ionic melts) refer to organic salts consisting of a combination of organic cations and anions that can exist as a liquid at room temperature (15°C or higher and 25°C or lower). Room temperature molten salts include room temperature molten salts that exist as a liquid by themselves, room temperature molten salts that become liquid when mixed with an electrolyte salt, room temperature molten salts that become liquid when dissolved in an organic solvent, and mixtures of these. In general, the melting point of room temperature molten salts used in secondary batteries is 25°C or lower. In addition, organic cations generally have a quaternary ammonium skeleton.

[0113] The polymer solid electrolyte is prepared by dissolving an electrolyte salt in a polymer material and solidifying it.

[0114] The inorganic solid electrolyte is a solid material that has Li-ion conductivity.

[0115] The electrolyte may be an aqueous electrolyte that contains water.

[0116] The aqueous electrolyte includes an aqueous solvent and an electrolyte salt. The aqueous electrolyte is, for example, liquid. The liquid aqueous electrolyte is an aqueous solution prepared by dissolving an electrolyte salt as a solute in an aqueous solvent. The aqueous solvent is, for example, a solvent containing water in an amount of 50% by volume or more. The aqueous solvent may be pure water.

[0117] The aqueous electrolyte may be a gel aqueous electrolyte obtained by combining an aqueous electrolyte solution with the above-mentioned polymer material. Regardless of whether the electrolyte is an aqueous electrolyte or a non-aqueous electrolyte, when the electrolyte is a gel electrolyte, the above-mentioned effect, i.e., the effect of improving cycle life characteristics, can be obtained.

[0118] The aqueous electrolyte preferably contains 1 mol or more of the aqueous solvent per mol of the solute salt, and more preferably contains 3.5 mol or more of the aqueous solvent per mol of the solute salt.

[0119] The presence of water in aqueous electrolytes can be confirmed by GC-MS (Gas Chromatography - Mass Spectrometry) measurements. The salt concentration and water content in aqueous electrolytes can be calculated, for example, by ICP (Inductively Coupled Plasma) emission spectrometry. The molar concentration (mol / L) can be calculated by weighing a specified amount of aqueous electrolyte and calculating the salt concentration. The number of moles of solute and solvent can also be calculated by measuring the specific gravity of the aqueous electrolyte.

[0120] The aqueous electrolyte is prepared, for example, by dissolving an electrolyte salt in an aqueous solvent at a concentration of 1 to 12 mol / L.

[0121] In order to suppress electrolysis of the aqueous electrolyte, LiOH or Li2SO4 can be added to adjust the pH, preferably 3-13, more preferably 4-12.

[0122] (4) Separator The separator is formed, for example, from a porous film containing polyethylene (PE), polypropylene (PP), cellulose, or polyvinylidene fluoride (PVdF), or a synthetic resin nonwoven fabric. From the viewpoint of safety, it is preferable to use a porous film formed from polyethylene or polypropylene. This is because these porous films melt at a certain temperature and are capable of cutting off electric current.

[0123] A solid electrolyte layer containing solid electrolyte particles can also be used as the separator. The solid electrolyte layer may contain one type of solid electrolyte particles or may contain multiple types of solid electrolyte particles. The solid electrolyte layer may be a solid electrolyte composite membrane containing solid electrolyte particles. The solid electrolyte composite membrane is, for example, a membrane formed from solid electrolyte particles using a polymer material. The solid electrolyte layer may contain at least one selected from the group consisting of a plasticizer and an electrolyte salt. When the solid electrolyte layer contains an electrolyte salt, for example, the alkali metal ion conductivity of the solid electrolyte layer can be further increased.

[0124] Examples of the polymeric material include polyethers, polyesters, polyamines, polyethylenes, silicones, and polysulfides.

[0125] As the solid electrolyte, for example, the one shown in the first embodiment can be used.

[0126] (5) Exterior materials As the exterior member, for example, a container made of a laminate film or a metal container can be used.

[0127] The thickness of the laminate film is, for example, 0.5 mm or less, preferably 0.2 mm or less.

[0128] The laminate film is a multi-layer film including a plurality of resin layers and a metal layer interposed between the resin layers. The resin layers include polymeric materials such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET). The metal layer is preferably made of aluminum foil or aluminum alloy foil for weight reduction. The laminate film can be molded into the shape of the exterior member by sealing it by heat fusion.

[0129] The thickness of the wall of the metal container is, for example, 1 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less.

[0130] The metal container is made of, for example, aluminum or an aluminum alloy. The aluminum alloy preferably contains elements such as magnesium, zinc, and silicon. When the aluminum alloy contains transition metals such as iron, copper, nickel, and chromium, the content of the transition metals is preferably 100 ppm by mass or less.

[0131] The shape of the exterior member is not particularly limited. The shape of the exterior member may be, for example, flat (thin), rectangular, cylindrical, coin, or button. The exterior member can be appropriately selected depending on the battery dimensions and the application of the battery.

[0132] (6) Negative terminal The negative electrode terminal can be made of a material that is electrochemically stable at the Li absorption / release potential of the negative electrode active material and has electrical conductivity. Specifically, the material of the negative electrode terminal can be copper, nickel, stainless steel, aluminum, or an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The material of the negative electrode terminal is preferably aluminum or an aluminum alloy. The negative electrode terminal is preferably made of the same material as the negative electrode current collector in order to reduce the contact resistance with the negative electrode current collector.

[0133] (7) Positive terminal The positive electrode terminal has a potential range of 3V to 5V with respect to the redox potential of lithium (vs. Li / Li + ) and can be formed from a material that is electrically stable and conductive. Examples of the material for the positive electrode terminal include aluminum and an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The positive electrode terminal is preferably formed from the same material as the positive electrode current collector in order to reduce the contact resistance with the positive electrode current collector.

[0134] Next, the secondary battery according to the third embodiment will be described more specifically with reference to the drawings.

[0135] Fig. 1 is a cross-sectional view showing an example of a secondary battery according to a third embodiment of the present invention, and Fig. 2 is an enlarged cross-sectional view of a portion A of the secondary battery shown in Fig. 1.

[0136] The secondary battery 100 shown in Figures 1 and 2 includes a bag-shaped exterior member 2 shown in Figures 1 and 2, an electrode group 1 shown in Figure 2, and an electrolyte (not shown). The electrode group 1 and the electrolyte are stored in the bag-shaped exterior member 2. The electrolyte (not shown) is held in the electrode group 1.

[0137] The bag-shaped exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.

[0138] As shown in Fig. 1, the electrode group 1 is a flat wound-type electrode group. As shown in Fig. 2, the flat wound-type electrode group 1 includes a negative electrode 3, a separator 4, and a positive electrode 5. The separator 4 is interposed between the negative electrode 3 and the positive electrode 5.

[0139] The negative electrode 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b. In the negative electrode 3, in a portion located at the outermost shell of the wound-type electrode group 1, the negative electrode active material-containing layer 3b is formed only on the inner surface side of the negative electrode current collector 3a as shown in Fig. 2. In the other portions of the negative electrode 3, the negative electrode active material-containing layer 3b is formed on both sides of the negative electrode current collector 3a.

[0140] The positive electrode 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b formed on both sides of the positive electrode current collector 5a.

[0141] As shown in FIG. 1, the negative electrode terminal 6 and the positive electrode terminal 7 are located near the outer peripheral end of the wound electrode group 1. The negative electrode terminal 6 is connected to a portion located at the outermost shell of the negative electrode current collector 3a. The positive electrode terminal 7 is connected to a portion located at the outermost shell of the positive electrode current collector 5a. The negative electrode terminal 6 and the positive electrode terminal 7 extend to the outside from an opening of the bag-shaped exterior member 2. A thermoplastic resin layer is provided on the inner surface of the bag-shaped exterior member 2, and the opening is closed by heat sealing.

[0142] The secondary battery according to the third embodiment is not limited to the secondary battery having the configuration shown in FIGS. 1 and 2, but may be a battery having the configuration shown in FIGS.

[0143] Fig. 3 is a partially cutaway perspective view showing typically another example of the secondary battery according to embodiment 3. Fig. 4 is an enlarged cross-sectional view of part B of the secondary battery shown in Fig. 3.

[0144] The secondary battery 100 shown in Figures 3 and 4 includes an electrode group 1 shown in Figures 3 and 4, an exterior member 2 shown in Figure 3, and an electrolyte (not shown). The electrode group 1 and the electrolyte are housed in the exterior member 2. The electrolyte is held in the electrode group 1.

[0145] The exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.

[0146] The electrode group 1 is a laminated type electrode group, as shown in Fig. 4. The laminated type electrode group 1 has a structure in which negative electrodes 3 and positive electrodes 5 are alternately laminated with separators 4 interposed therebetween.

[0147] The electrode group 1 includes a plurality of negative electrodes 3. Each of the plurality of negative electrodes 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b supported on both sides of the negative electrode current collector 3a. The electrode group 1 also includes a plurality of positive electrodes 5. Each of the plurality of positive electrodes 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b supported on both sides of the positive electrode current collector 5a.

[0148] The negative electrode current collector 3a of each negative electrode 3 includes a portion 3c on one side of which the negative electrode active material-containing layer 3b is not supported on any surface. This portion 3c serves as a negative electrode current collector tab. As shown in FIG. 4, the portion 3c serving as the negative electrode current collector tab does not overlap with the positive electrode 5. In addition, the multiple negative electrode current collector tabs (portions 3c) are electrically connected to a strip-shaped negative electrode terminal 6. The tip of the strip-shaped negative electrode terminal 6 is pulled out to the outside of the exterior member 2.

[0149] Although not shown, the positive electrode current collector 5a of each positive electrode 5 includes a portion on one side where the positive electrode active material-containing layer 5b is not supported on any surface. This portion serves as a positive electrode current collector tab. The positive electrode current collector tab does not overlap with the negative electrode 3, similar to the negative electrode current collector tab (portion 3c). The positive electrode current collector tab is located on the opposite side of the electrode group 1 to the negative electrode current collector tab (portion 3c). The positive electrode current collector tab is electrically connected to a strip-shaped positive electrode terminal 7. The tip of the strip-shaped positive electrode terminal 7 is located on the opposite side to the negative electrode terminal 6, and is drawn out to the outside of the exterior member 2.

[0150] The secondary battery according to the third embodiment includes the electrode according to the second embodiment as a positive electrode, and therefore the secondary battery can achieve excellent cycle life characteristics while maintaining a high operating voltage.

[0151] (Fourth embodiment) According to a fourth embodiment, there is provided a battery pack. The battery pack according to the fourth embodiment includes a plurality of secondary batteries according to the third embodiment.

[0152] In the battery pack according to the fourth embodiment, the individual cells may be electrically connected in series or in parallel, or may be connected in a combination of series and parallel.

[0153] Next, an example of a battery pack according to a fourth embodiment will be described with reference to the drawings.

[0154] Fig. 5 is a perspective view showing an example of a battery pack according to the fourth embodiment. The battery pack 200 shown in Fig. 5 includes five cells 100a to 100e, four bus bars 21, a positive electrode lead 22, and a negative electrode lead 23. Each of the five cells 100a to 100e is a secondary battery according to the third embodiment.

[0155] The bus bar 21 connects, for example, the negative electrode terminal 6 of one cell 100a and the positive electrode terminal 7 of the adjacent cell 100b. In this way, the five cells 100 are connected in series by the four bus bars 21. That is, the battery pack 200 in FIG. 5 is a five-series battery pack. Although no example is shown, in a battery pack including a plurality of cells electrically connected in parallel, for example, the plurality of negative electrode terminals are connected to each other by a bus bar and the plurality of positive electrode terminals are connected to each other by a bus bar, so that the plurality of cells are electrically connected to each other.

[0156] The positive terminal 7 of at least one of the five cells 100a-100e is electrically connected to a positive lead 22 for external connection. Also, the negative terminal 6 of at least one of the five cells 100a-100e is electrically connected to a negative lead 23 for external connection.

[0157] The battery pack according to the fourth embodiment includes the secondary battery according to the third embodiment, and therefore this battery pack can achieve excellent cycle life characteristics while maintaining a high operating voltage.

[0158] Fifth embodiment According to a fifth embodiment, there is provided a battery pack. The battery pack includes the battery assembly according to the fourth embodiment. The battery pack may include a single secondary battery according to the third embodiment, instead of the battery assembly according to the fourth embodiment.

[0159] The battery pack according to the fifth embodiment may further include a protection circuit. The protection circuit has a function of controlling charging and discharging of the secondary battery. Alternatively, a circuit included in a device (e.g., electronic device, automobile, etc.) that uses the battery pack as a power source may be used as the protection circuit for the battery pack.

[0160] The battery pack according to the fifth embodiment may further include an external terminal for current flow. The external terminal for current flow is for outputting current from the secondary battery to the outside and / or for inputting current from the outside to the secondary battery. In other words, when the battery pack is used as a power source, current is supplied to the outside through the external terminal for current flow. When the battery pack is charged, a charging current (including regenerative energy from the power of an automobile or the like) is supplied to the battery pack through the external terminal for current flow.

[0161] Next, an example of a battery pack according to a fifth embodiment will be described with reference to the drawings.

[0162] Fig. 6 is an exploded perspective view showing an example of a battery pack according to the fifth embodiment, Fig. 7 is a block diagram showing an example of an electric circuit of the battery pack shown in Fig. 6.

[0163] The battery pack 300 shown in Figs. 6 and 7 includes a container 31, a lid 32, a protective sheet 33, a battery pack 200, a printed wiring board 34, wiring 35, and an insulating plate (not shown).

[0164] 6 is a bottomed, square container having a rectangular bottom. The container 31 is configured to be able to accommodate a protective sheet 33, a battery pack 200, a printed wiring board 34, and wiring 35. The lid 32 has a rectangular shape. The lid 32 covers the container 31 to accommodate the battery pack 200 and the like. Although not shown, the container 31 and the lid 32 are provided with openings or connection terminals for connection to an external device or the like.

[0165] The battery pack 200 includes a plurality of cells 100, a positive electrode lead 22, a negative electrode lead 23, and an adhesive tape 24.

[0166] At least one of the plurality of unit cells 100 is a secondary battery according to the third embodiment. Each of the plurality of unit cells 100 is electrically connected in series as shown in FIG. 7. The plurality of unit cells 100 may be electrically connected in parallel, or may be connected in a combination of series and parallel connections. When the plurality of unit cells 100 are connected in parallel, the battery capacity is increased compared to when they are connected in series.

[0167] The adhesive tape 24 fastens the plurality of unit cells 100. The plurality of unit cells 100 may be fixed using heat shrink tape instead of the adhesive tape 24. In this case, the protective sheets 33 are disposed on both side surfaces of the battery pack 200, the heat shrink tape is wrapped around the battery pack 200, and the heat shrink tape is then thermally shrunk to bind the plurality of unit cells 100 together.

[0168] One end of the positive electrode lead 22 is connected to the battery pack 200. One end of the positive electrode lead 22 is electrically connected to the positive electrode of one or more cells 100. One end of the negative electrode lead 23 is connected to the battery pack 200. One end of the negative electrode lead 23 is electrically connected to the negative electrode of one or more cells 100.

[0169] The printed wiring board 34 is disposed along one of the short side surfaces of the inner surface of the container 31. The printed wiring board 34 includes a positive connector 342, a negative connector 343, a thermistor 345, a protection circuit 346, wiring 342a and 343a, an external terminal 350 for supplying electricity, a positive wiring (positive wiring) 348a, and a negative wiring (negative wiring) 348b. One main surface of the printed wiring board 34 faces one side of the battery pack 200. An insulating plate (not shown) is interposed between the printed wiring board 34 and the battery pack 200.

[0170] The other end 22a of the positive electrode lead 22 is electrically connected to the positive electrode connector 342. The other end 23a of the negative electrode lead 23 is electrically connected to the negative electrode connector 343.

[0171] The thermistor 345 is fixed to one main surface of the printed wiring board 34. The thermistor 345 detects the temperature of each of the cells 100, and transmits a detection signal to the protection circuit 346.

[0172] The external terminal 350 for current supply is fixed to the other main surface of the printed wiring board 34. The external terminal 350 for current supply is electrically connected to a device present outside the battery pack 300. The external terminal 350 for current supply includes a positive terminal 352 and a negative terminal 353.

[0173] The protection circuit 346 is fixed to the other main surface of the printed wiring board 34. The protection circuit 346 is connected to the positive terminal 352 via a positive wiring 348a. The protection circuit 346 is connected to the negative terminal 353 via a negative wiring 348b. The protection circuit 346 is also electrically connected to the positive electrode connector 342 via a wiring 342a. The protection circuit 346 is electrically connected to the negative electrode connector 343 via a wiring 343a. Furthermore, the protection circuit 346 is electrically connected to each of the plurality of single cells 100 via the wiring 35.

[0174] The protective sheet 33 is disposed on both inner surfaces in the long side direction of the container 31 and on the inner surface in the short side direction that faces the printed wiring board 34 via the battery pack 200. The protective sheet 33 is made of, for example, resin or rubber.

[0175] The protection circuit 346 controls charging and discharging of the multiple cells 100. In addition, the protection circuit 346 cuts off electrical connection between the protection circuit 346 and external terminals 350 (positive terminal 352, negative terminal 353) for supplying electricity to an external device, based on a detection signal transmitted from the thermistor 345, or a detection signal transmitted from each of the cells 100 or the battery pack 200.

[0176] An example of the detection signal transmitted from the thermistor 345 is a signal that detects that the temperature of the cell 100 is equal to or higher than a predetermined temperature. An example of the detection signal transmitted from each cell 100 or the battery pack 200 is a signal that detects overcharging, overdischarging, and overcurrent of the cell 100. When detecting overcharging or the like for each cell 100, the battery voltage may be detected, or the positive electrode potential or the negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 100.

[0177] The protection circuit 346 may be a circuit included in a device (such as an electronic device or an automobile) that uses the battery pack 300 as a power source.

[0178] As described above, the battery pack 300 includes the external terminal 350 for current supply. Therefore, the battery pack 300 can output a current from the assembled battery 200 to an external device and input a current from the external device to the assembled battery 200 via the external terminal 350 for current supply. In other words, when the battery pack 300 is used as a power source, the current from the assembled battery 200 is supplied to the external device through the external terminal 350 for current supply. When the battery pack 300 is charged, a charging current from the external device is supplied to the battery pack 300 through the external terminal 350 for current supply. When the battery pack 300 is used as an in-vehicle battery, regenerative energy of the vehicle's power can be used as the charging current from the external device.

[0179] The battery pack 300 may include a plurality of assembled batteries 200. In this case, the plurality of assembled batteries 200 may be connected in series, in parallel, or in a combination of series and parallel connections. The printed wiring board 34 and the wiring 35 may be omitted. In this case, the positive electrode lead 22 and the negative electrode lead 23 may be used as a positive terminal and a negative terminal, respectively, of the external terminals for current supply.

[0180] Such a battery pack is used in applications that require excellent cycle performance, for example, when a large current is drawn. Specifically, the battery pack is used, for example, as a power source for electronic devices, a stationary battery, or an on-board battery for various vehicles. An example of the electronic device is a digital camera. The battery pack is particularly suitable for use as an on-board battery.

[0181] The battery pack according to the fifth embodiment includes the secondary battery according to the third embodiment or the battery pack according to the fourth embodiment. Therefore, this battery pack can achieve excellent cycle life characteristics while maintaining a high operating voltage.

[0182] Sixth embodiment According to a sixth embodiment, a vehicle is provided. The vehicle is equipped with the battery pack according to the fifth embodiment.

[0183] In the vehicle according to the sixth embodiment, the battery pack, for example, recovers regenerative energy of the vehicle's motive power. The vehicle may include a mechanism for converting the kinetic energy of the vehicle into regenerative energy.

[0184] Examples of the vehicle according to the sixth embodiment include a two-wheeled to four-wheeled hybrid electric vehicle, a two-wheeled to four-wheeled electric vehicle, an electric-assisted bicycle, and a railroad car.

[0185] The mounting position of the battery pack in the vehicle is not particularly limited. For example, when the battery pack is mounted in an automobile, the battery pack can be mounted in the engine compartment, the rear of the vehicle body, or under the seat of the vehicle.

[0186] The vehicle may be equipped with a plurality of battery packs. In this case, the batteries included in each battery pack may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. For example, when each battery pack includes a battery pack, the battery packs may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. Alternatively, when each battery pack includes a single battery, the batteries may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections.

[0187] Next, an example of a vehicle according to a sixth embodiment will be described with reference to the drawings.

[0188] FIG. 8 is a partial see-through view that illustrates an example of a vehicle according to the embodiment.

[0189] A vehicle 400 shown in Fig. 8 includes a vehicle body 40 and a battery pack 300 according to the embodiment. In the example shown in Fig. 8, the vehicle 400 is a four-wheeled automobile.

[0190] The vehicle 400 may be equipped with a plurality of battery packs 300. In this case, the batteries (e.g., single cells or assembled batteries) included in the battery pack 300 may be connected in series, in parallel, or in a combination of series and parallel connections.

[0191] 8 illustrates an example in which the battery pack 300 is mounted in an engine room located in the front of the vehicle body 40. As described above, the battery pack 300 may be mounted, for example, in the rear of the vehicle body 40 or under a seat. This battery pack 300 can be used as a power source for the vehicle 400. In addition, this battery pack 300 can recover regenerative energy for the motive power of the vehicle 400.

[0192] Next, an embodiment of a vehicle according to the sixth embodiment will be described with reference to FIG.

[0193] Fig. 9 is a diagram illustrating an example of a control system for an electrical system in a vehicle according to embodiment 6. A vehicle 400 illustrated in Fig. 9 is an electric vehicle.

[0194] The vehicle 400 shown in FIG. 9 comprises a vehicle body 40, a vehicle power supply 41, a vehicle ECU (ECU: Electric Control Unit) 42 which is a higher-level control device of the vehicle power supply 41, an external terminal (terminal for connecting to an external power supply) 43, an inverter 44, and a drive motor 45.

[0195] The vehicle 400 has a vehicle power supply 41 mounted, for example, in an engine compartment, the rear of the vehicle body, or under a seat. Note that in the vehicle 400 shown in Fig. 9, the mounting location of the vehicle power supply 41 is shown diagrammatically.

[0196] The vehicle power supply 41 includes a plurality of (eg, three) battery packs 300a, 300b, and 300c, a battery management unit (BMU) 411, and a communication bus 412.

[0197] The battery pack 300a includes an assembled battery 200a and an assembled battery monitoring device 301a (e.g., VTM: Voltage Temperature Monitoring). The battery pack 300b includes an assembled battery 200b and an assembled battery monitoring device 301b. The battery pack 300c includes an assembled battery 200c and an assembled battery monitoring device 301c. The battery packs 300a-300c are battery packs similar to the above-mentioned battery pack 300, and the assembled batteries 200a-200c are assembled batteries similar to the above-mentioned battery pack 200. The assembled batteries 200a-200c are electrically connected in series. The battery packs 300a, 300b, and 300c can be removed independently and replaced with another battery pack 300.

[0198] Each of the assembled batteries 200a-200c includes a plurality of unit cells connected in series. At least one of the plurality of unit cells is the secondary battery according to the second embodiment. The assembled batteries 200a-200c are charged and discharged via a positive terminal 413 and a negative terminal 414, respectively.

[0199] The battery management device 411 communicates with the assembled battery monitoring devices 301a-301c and collects information on the voltage, temperature, and the like of each of the cells 100 included in the assembled batteries 200a-200c included in the vehicle power supply 41. In this way, the battery management device 411 collects information on the maintenance of the vehicle power supply 41.

[0200] The battery management unit 411 and the assembled battery monitoring units 301a-301c are connected via a communication bus 412. In the communication bus 412, one set of communication lines is shared by a plurality of nodes (the battery management unit 411 and one or more assembled battery monitoring units 301a-301c). The communication bus 412 is a communication bus configured based on, for example, the CAN (Control Area Network) standard.

[0201] The battery pack monitoring devices 301a-301c measure the voltage and temperature of each of the cells constituting the battery packs 200a-200c based on commands received through communication from the battery management device 411. However, the temperature can be measured at only a few points per battery pack, and it is not necessary to measure the temperatures of all the cells.

[0202] The vehicle power supply 41 may also have an electromagnetic contactor (for example, a switch device 415 shown in FIG. 9) that switches between the presence and absence of an electrical connection between the positive terminal 413 and the negative terminal 414. The switch device 415 includes a pre-charge switch (not shown) that is turned on when the assembled batteries 200a-200c are charged, and a main switch (not shown) that is turned on when the output from the assembled batteries 200a-200c is supplied to a load. Each of the pre-charge switch and the main switch includes a relay circuit (not shown) that is switched on or off by a signal supplied to a coil disposed near the switch element. The electromagnetic contactor such as the switch device 415 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 that controls the operation of the entire vehicle 400.

[0203] The inverter 44 converts the input DC voltage into a three-phase alternating current (AC) high voltage for driving the motor. The three-phase output terminals of the inverter 44 are connected to the three-phase input terminals of the drive motor 45. The inverter 44 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 for controlling the operation of the entire vehicle. By controlling the inverter 44, the output voltage from the inverter 44 is adjusted.

[0204] The drive motor 45 rotates by electric power supplied from the inverter 44. A driving force generated by the rotation of the drive motor 45 is transmitted to the axles and drive wheels W via, for example, a differential gear unit.

[0205] Although not shown, the vehicle 400 is also equipped with a regenerative braking mechanism (regenerator). The regenerative braking mechanism rotates the drive motor 45 when the vehicle 400 is braked, and converts kinetic energy into regenerative energy as electrical energy. The regenerative energy recovered by the regenerative braking mechanism is input to the inverter 44 and converted into a direct current. The converted direct current is input to the vehicle power source 41.

[0206] One terminal of a connection line L1 is connected to the negative terminal 414 of the vehicle power supply 41. The other terminal of the connection line L1 is connected to a negative input terminal 417 of the inverter 44. A current detection unit (current detection circuit) 416 in the battery management device 411 is provided between the negative terminal 414 and the negative input terminal 417 on the connection line L1.

[0207] One terminal of a connection line L2 is connected to the positive electrode terminal 413 of the vehicle power supply 41. The other terminal of the connection line L2 is connected to a positive electrode input terminal 418 of the inverter 44. A switch device 415 is provided in the connection line L2 between the positive electrode terminal 413 and the positive electrode input terminal 418.

[0208] The external terminal 43 is connected to the battery management unit 411. The external terminal 43 can be connected to, for example, an external power source.

[0209] In response to operational inputs from the driver or the like, the vehicle ECU 42 coordinates with other management devices and control devices including the battery management device 411 to control the vehicle power supply 41, the switch device 415, the inverter 44, etc. Through the coordinated control of the vehicle ECU 42, etc., the output of power from the vehicle power supply 41 and the charging of the vehicle power supply 41 are controlled, and the entire vehicle 400 is managed. Data relating to the maintenance of the vehicle power supply 41, such as the remaining capacity of the vehicle power supply 41, is transferred between the battery management device 411 and the vehicle ECU 42 via a communication line.

[0210] The vehicle according to the sixth embodiment includes the battery pack according to the fifth embodiment. Therefore, according to the present embodiment, it is possible to provide a vehicle equipped with a battery pack that can maintain a high operating voltage and exhibit excellent cycle life characteristics.

[0211] [Example] Examples will be described below, but the embodiments are not limited to the examples described below.

[0212] Example 1 A secondary battery was fabricated in the following manner.

[0213] <Preparation of coating layer of second active material particles> LATP was prepared by the sol-gel method described below. 16.09 g of citric acid was dissolved in water, 5.95 g of titanium isopropoxide was added, and the mixture was refluxed for 4 hours. After further addition of water, 4.55 g of citric acid, 1.25 g of lithium nitrate, and 4.55 g of ammonium dihydrogen phosphate, which had been dissolved in water in advance, were added and stirred at room temperature for 5 minutes. Further, 2.00 g of citric acid and 1.93 g of aluminum nitrate nonahydrate, which had been dissolved in water, were added and stirred at room temperature for 30 minutes. 9.95 g of diethylene glycol was added to the solution after the reaction was completed, and the pH was adjusted to 7 with ammonium water. The obtained dispersion liquid is called LATP liquid. The composition formula of LATP is Li 1.4 Al 0.4 Ti 1.6 (PO4)3.

[0214] Next, NCM523 particles (LiNi 0.5 Co 0.2 Mn 0.3O2:NCM523) was coated with LATP. The NCM523 particles were added to the LATP solution so that the mass ratio of LATP to the mass of the second active material particles obtained after the coating layer was 3 mass%, and the mixture was subjected to ultrasonic treatment for 15 minutes. The obtained dispersion was then transferred to an evaporating dish. The evaporating dish was kept at 150°C for 3 hours in a small atmosphere furnace with oxygen and argon gas flowing at 1.0 L / min (nor), and then baked at 500°C for 8 hours to obtain second active material particles having LATP coated on the surface of the NCM523 particles. The median diameter of the obtained second active material particles was 5 μm.

[0215] <Preparation of positive electrode> The first active material particles were spinel-type lithium nickel manganese oxide (LiNi 0.5 Mn 1.5 A slurry was prepared by adding and mixing 90 parts by weight of O4:LNMO powder, 10 parts by weight of the second active material particles prepared previously as the second active material particles, 5 parts by weight of acetylene black as the conductive agent, and 2 parts by weight of polyvinylidene fluoride (PVdF) as the binder to N-methylpyrrolidone (NMP). The slurry was applied to both sides of a current collector made of aluminum foil with a thickness of 12 μm, and then dried and pressed in a thermostatic chamber at 120 ° C to obtain a positive electrode.

[0216] <Preparation of negative electrode> A slurry was prepared by mixing 100 parts by weight of niobium titanium composite oxide (Nb2TiO7) powder as the negative electrode active material, 4 parts by weight of acetylene black as the conductive agent, 2 parts by weight of carboxymethyl cellulose (CMC) as the binder, 2 parts by weight of styrene butadiene copolymer (SBR) as the binder, and pure water. This slurry was applied to both sides of a current collector made of aluminum foil with a thickness of 12 μm, and then dried and pressed in a thermostatic chamber at 120 °C to obtain a negative electrode.

[0217] <Preparation of electrode groups> A laminate was obtained by stacking the positive electrode, separator, negative electrode, and separator in this order. The laminate was then spirally wound. This was hot-pressed at 80°C to produce a flat electrode group. The resulting electrode group was housed in a pack made of a 0.1 mm-thick laminate film having a three-layer structure of nylon layer / aluminum layer / polyethylene layer, and dried in a vacuum at 120°C for 16 hours.

[0218] <Preparation of non-aqueous electrolyte and fabrication of secondary battery> A non-aqueous electrolyte was obtained by dissolving 1 mol / L of LiPF6 as an electrolyte in a mixed solvent of propylene carbonate (PC) and diethyl carbonate (DEC) (volume ratio 1:2). The electrolyte was prepared in an argon box.

[0219] A non-aqueous electrolyte was injected into the laminate film pack containing the electrode group, and the pack was then completely sealed by heat sealing to obtain a secondary battery.

[0220] Example 2 A secondary battery was fabricated in the same manner as in Example 1, except that LiFeMnO4 powder having a median diameter of 2 μm was used as the first active material particles instead of LNMO.

[0221] Example 3 A secondary battery was produced in the same manner as in Example 1, except that the mass ratio of the first active material particles to the second active material particles was changed to 80:20.

[0222] Example 4 A secondary battery was produced in the same manner as in Example 1, except that LiCoPO4 (LCP) powder was used instead of NCM523 powder as the cobalt-containing oxide particles contained in the second active material particles. The median diameter of the second active material particles containing LCP was 1 μm.

[0223] Example 5 A secondary battery was produced in the same manner as in Example 1, except that when producing the second active material particles, the proportion of the mass of the coating layer in the mass of the second active material particles was changed to 1 mass %.

[0224] Example 6 A secondary battery was produced in the same manner as in Example 4, except that when producing the second active material particles, the proportion of the mass of the coating layer in the mass of the second active material particles was changed to 5 mass %.

[0225] Example 7 A secondary battery was produced in the same manner as in Example 4, except that when producing the second active material particles, the proportion of the mass of the coating layer in the mass of the second active material particles was changed to 0.1 mass %.

[0226] Example 8 A secondary battery was produced in the same manner as in Example 4, except that a coating layer made of LiTi2(PO4)3 was formed instead of the coating layer made of LATP when the second active material particles were produced.

[0227] Example 9 A secondary battery was produced in the same manner as in Example 1, except that a gel electrolyte prepared as follows was used instead of the electrolytic solution.

[0228] The positive electrode active material-containing layer, the negative electrode active material-containing layer, and the separator were impregnated with a mixture of propylene carbonate (PC) and diethyl carbonate (volume ratio 1:2) in which LiPF6 was dissolved at a concentration of 1M, and a solution of a polymer (2% by weight) of methyl methacrylate-oxetanyl methacrylate copolymer. The cell was then sealed to prevent moisture from entering, and the mixture was gelled by heating at 60°C for 25 hours.

[0229] Comparative Example 1 A secondary battery was produced in the same manner as in Example 1, except that only the first active material particles were used as the positive electrode active material.

[0230] Comparative Example 2 A secondary battery was produced in the same manner as in Example 1, except that NCM523 particles not having a coating layer were used as the second active material particles.

[0231] Comparative Example 3 A secondary battery was produced in the same manner as in Example 1, except that LCP particles not having a coating layer were used as the second active material particles.

[0232] Comparative Example 4 A secondary battery was produced in the same manner as in Example 1, except that only the second active material particles were used as the positive electrode active material.

[0233] Comparative Example 5 The first active material particles are made of lithium manganese composite oxide (Li x A secondary battery was fabricated in the same manner as in Example 1, except that Mn2O4:LMO was used. The operating potential of LMO is 3.6 V versus metallic lithium. In other words, the operating potential of LMO is less than 4.4 V versus metallic lithium.

[0234] <Cycle life characteristic evaluation> The secondary batteries prepared in each example were subjected to testing in an environment of 45° C. In charging and discharging, the batteries were first charged to 3.7 V at 100 mA, and then discharged to 2.3 V at 20 mA to check the capacity of the batteries, and then charged and discharged at 100 mA for 100 cycles.

[0235] The above results are summarized in Table 1 below. In Table 1, the "Mass ratio" column shows the ratio (MP1 / MP2) of the mass of the first active material particles (MP1) to the mass of the second active material particles (MP2) in the active material-containing layer, and the ratio of these masses is shown in parentheses. The "Ratio (MD1 / MD2)" and "Gas generation amount" columns show the amount of gas generated after 100 cycles in the cycle life characteristic evaluation. The "Capacity retention rate" column shows the capacity retention rate after 100 cycles in the cycle life characteristic evaluation.

[0236] [Table 1]

[0237] Table 1 reveals the following:

[0238] As shown in Examples 1 to 9, even when a lithium composite oxide exhibiting an operating potential of 4.4 V or more versus metallic lithium was used, the amount of gas generation was reduced and the capacity retention rate was improved by using cobalt-containing oxide particles having a coating layer as the second active material particles in combination.

[0239] Comparative Example 1, which did not contain second active material particles, Comparative Examples 2 and 3, which contained a cobalt-containing oxide without a coating layer, and Comparative Examples 4 and 5, which did not contain a lithium composite oxide showing an operating potential of 4.4 V or more versus metallic lithium, all tended to have lower capacity retention rates and larger amounts of gas generated than the Examples.

[0240] Comparing Examples 1 and 3, it can be seen that a relatively small content of the second active material particles is preferable. This is believed to be due to the following reasons. First, in the operating potential range of the first active material particles (4.4 V or more), the second active material particles are not very involved in the charging and discharging of the battery. In addition, when the mass ratio of the second active material particles in the active material is increased, the mass ratio of the first active material particles decreases relatively. Therefore, in this case, the ratio of the first active material particles involved in charging and discharging (battery capacity) decreases. As a result, the active material balance between the positive and negative electrodes changes, and the load on the first active material particles, which is relatively reduced during charging and discharging, increases, and it is believed that the deterioration of the first active material particles is promoted.

[0241] Examples 4 and 6-8, which used LCP with a median diameter of the second active material particles of 1 μm, tended to show superior cycle life characteristics compared to Examples 1-3 and 5, which used NCM523 with a median diameter of the second active material particles of 5 μm. This is thought to be because in the former case, the second active material particles were easily dispersed between the first active material particles, and therefore the effect of the second active material particles to oxidize hydrogen gas to protons was easily obtained.

[0242] Compared with Example 5 in which the mass ratio of the coating layer provided on the second active material particles is 1 mass%, Example 1 in which the mass ratio is 3 mass% tends to generate less gas and have a higher capacity retention rate. Also, compared with Example 7 in which the mass ratio of the coating layer provided on the second active material particles is 0.1 mass%, Example 4 in which the mass ratio is 3 mass% tends to generate less gas and have a higher capacity retention rate. From this, it can be seen that the mass ratio of the coating layer to the mass of the second active material particles is preferably more than 1 mass%. However, as can be seen from the comparison between Example 7 and Comparative Examples 1 to 5, even if the mass ratio is 0.1 mass%, the amount of gas generated can be reduced and the capacity retention rate tends to be excellent.

[0243] As shown in Examples 2 and 8, even when the active material used as the first active material particles or the solid electrolyte composition contained in the coating layer was changed, excellent cycle life characteristics could be achieved.

[0244] According to at least one of the above-described embodiments and examples, an active material is provided. The active material includes first active material particles including a lithium composite oxide exhibiting an operating potential of 4.4 V or more versus metallic lithium, and second active material particles different from the first active material particles. The second active material particles include cobalt-containing oxide particles and a coating layer that coats at least a portion of the surface of the cobalt-containing oxide particles. The coating layer includes a solid electrolyte. This active material can achieve excellent cycle life characteristics while maintaining a high operating voltage.

[0245] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are also included in the scope of the invention and its equivalents described in the claims. The invention described in the claims of the present application at the time of filing is appended below. [1] A first active material particle containing a lithium composite oxide showing an operating potential of 4.4 V or more based on metallic lithium, and a second active material particle different from the first active material particle, wherein the second active material particle includes a cobalt-containing oxide particle and a coating layer covering at least a part of the surface of the cobalt-containing oxide particle, and the coating layer is an active material containing a solid electrolyte. [2] The active material according to [1], wherein the lithium composite oxide is represented by the following general formula (A). Li u M1 x Mn 2-x O 4 ···(A) In the general formula (A), M1 is at least one selected from the group consisting of Mn, Ni, Fe, Co, Cr, Mg, Zn, Al, and Cu, u satisfies 0 < u ≦ 1, and x satisfies 0 < x ≦ 1. [3] The active material according to [1] or [2], wherein the lithium composite oxide includes at least one selected from the group consisting of lithium nickel manganese oxide and a lithium phosphate compound. [4] The lithium composite oxide includes the lithium nickel manganese oxide, and the lithium nickel manganese oxide is the active material according to [3] represented by the following general formula (I). Li u Ni x Mn 2-x O 4 ···(I) In the general formula (I), u satisfies 0 < u ≦ 1, and x satisfies 0 < x ≦ 1. [5] The lithium composite oxide includes the lithium phosphate compound, and the lithium phosphate compound is the active material according to [3] represented by the following general formula (II). Li w M2 y Co 1-y PO 4 ···(II) In the general formula (II), M2 is at least one selected from the group consisting of Ni and Cu, w satisfies 0 < w ≦ 1, and y satisfies 0 ≦ y ≦ 1. [6] The cobalt-containing oxide particles are Li x Ni a Co b Mn c M3 d O 2 (Here, 0 < x ≤ 1.0, 0.3 ≤ a ≤ 1.0, 0 ≤ b ≤ 0.4, 0 ≤ c ≤ 0.4, 0 ≤ d ≤ 0.4, and M3 is at least one selected from the group consisting of Mg, Fe, Ni, Co, W, Ta, and Mo), LiM x Co 1-x PO 4 , Li 2 M x Co 1-x PO 4 F, LiM x Co 1-x O 2 , LiM x Co 1-xBO 3 , and LiM x Co 1-x SiO 4 (In these general formulas, x satisfies 0 ≤ x ≤ 0.8, and M is at least one selected from the group consisting of Mn, Ni, Fe, Mg, Zn, and Al), and the active material according to any one of [1] to [5] containing at least one selected from the group consisting of [7] The active material according to any one of [1] to [6], wherein only the second active material particles among the first active material particles and the second active material particles have the coating layer. [8] The active material according to any one of [1] to [7], wherein the value of the ratio (MP1 / MP2) of the mass MP1 of the first active material particles to the mass MP2 of the second active material particles is in the range of 2 to 20. [9] The active material according to any one of [1] to [8], wherein the ratio of the mass of the coating layer to the mass of the second active material particles is in the range of 0.1% by mass to 10% by mass.

[10] The active material according to any one of [1] to [9], wherein the solid electrolyte is at least one selected from the group consisting of a sulfide solid electrolyte, an oxide solid electrolyte, a nitride solid electrolyte, and a polymer solid electrolyte.

[11] An electrode containing the active material according to any one of [1] to

[10] .

[12] A secondary battery including a negative electrode, and an electrolyte, and the positive electrode is the electrode according to

[11] .

[13] The negative electrode contains a negative electrode active material, and the negative electrode active material contains at least one selected from the group consisting of a lithium titanium composite oxide and a niobium titanium composite oxide. The secondary battery according to

[12] .

[14] The secondary battery according to

[13] , wherein the electrolyte is a gel electrolyte containing a polymer material.

[15] A battery pack including the secondary battery according to

[13] or

[14] .

[16] The battery pack according to

[15] , further including an external terminal for energization and a protection circuit.

[17] The battery pack according to

[15] or

[16] , including a plurality of the secondary batteries, and the secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel.

[18] A vehicle equipped with the battery pack according to any one of

[15] to

[17] .

[19] A vehicle as described in

[18] , including a mechanism for converting kinetic energy of the vehicle into regenerative energy. [Explanation of symbols]

[0246] Reference Signs List 1...electrode group, 2...exterior member, 3...electrode (negative electrode), 3a...current collector (negative electrode current collector), 3b...active material-containing layer (negative electrode active material-containing layer), 3c...negative electrode current collector tab, 4...separator, 5...positive electrode, 5a...positive electrode current collector, 5b...positive electrode active material-containing layer, 6...negative electrode terminal, 7...positive electrode terminal, 21...bus bar, 22...positive electrode side lead, 22a...other end, 23...negative electrode side lead, 23a ...other end, 24...adhesive tape, 31...container, 32...lid, 33...protective sheet, 34...printed wiring board, 35...wiring, 40...vehicle body, 41...vehicle power source, 42...electrical control device, 43...external terminal, 44...inverter, 45...driving motor, 100...secondary battery, 200...battery pack, 200a...battery pack, 200b...battery pack, 200c...battery pack, 300 ...battery pack, 300a...battery pack, 300b...battery pack, 300c...battery pack, 301a...battery pack monitoring device, 301b...battery pack monitoring device, 301c...battery pack monitoring device, 342...positive connector, 343...negative connector, 345...thermistor, 346...protection circuit, 342a...wiring, 343a...wiring, 350...external terminal for energization, 352...positive terminal, 353...negative terminal, 348a...positive wiring, 348b...negative wiring, 400...vehicle, 411...battery management device, 412...communication bus, 413...positive terminal, 414...negative terminal, 415...switch device, 416...current detection unit, 417...negative input terminal, 418...positive input terminal, L1...connection line, L2...connection line, W...drive wheel.

Claims

1. The battery includes first active material particles including a lithium composite oxide exhibiting an operating potential of 4.4 V or more versus metallic lithium, and second active material particles different from the first active material particles, The lithium composite oxide includes a lithium phosphate compound, The lithium phosphate compound is represented by the following general formula (II): Li w M2 y Co 1-y PO 4 ... (II) In the general formula (II), M2 is at least one selected from the group consisting of Ni and Cu, w satisfies 0<w≦1, and y satisfies 0≦y≦1; the second active material particles include cobalt-containing oxide particles and a coating layer that coats at least a portion of a surface of the cobalt-containing oxide particles, each of the first active material particles and the second active material particles is selected from a primary particle, a secondary particle formed by aggregation of the primary particles, and a mixture of the primary particle and the secondary particle; the coating layer includes a solid electrolyte; The solid electrolyte has a NASICON-type skeleton and has the general formula Li 1+x A x Ti 2-x (P.O. 4 ) 3 and 0≦x≦0.5 is satisfied.

2. The cobalt-containing oxide particles include Li x Ni a Co b Mn c M3 d O 2 (wherein 0<x≦1.0, 0.3≦a≦1.0, 0≦b≦0.4, 0≦c≦0.4, 0≦d≦0.4, and M3 is at least one selected from the group consisting of Mg, Fe, Ni, Co, W, Ta, and Mo), LiM x Co 1-x P.O. 4 , Li 2 M x Co 1-x P.O. 4 F, LiM x Co 1-x O 2 , LiM x Co 1-x B.O. 3 , and LiM x Co 1-x SiO 4 (In these general formulas, x satisfies 0≦x≦0.8, and M is at least one selected from the group consisting of Mn, Ni, Fe, Mg, Zn, and Al).

3. The active material according to claim 1 , wherein, of the first active material particles and the second active material particles, only the second active material particles have the coating layer.

4. The active material according to any one of claims 1 to 3, wherein a ratio (MP1 / MP2) of a mass MP1 of the first active material particles to a mass MP2 of the second active material particles is in a range of 2 to 20.

5. 5. The active material according to claim 1, wherein a ratio of the mass of the coating layer to the mass of the second active material particles is within a range of 0.1% by mass to 10% by mass.

6. An electrode comprising the active material according to any one of claims 1 to 5.

7. A positive electrode and A negative electrode; and an electrolyte, The positive electrode of the secondary battery is the electrode according to claim 6.

8. The negative electrode includes a negative electrode active material, 8. The secondary battery according to claim 7, wherein the negative electrode active material comprises at least one selected from the group consisting of lithium titanium composite oxide and niobium titanium composite oxide.

9. 9. The secondary battery according to claim 8, wherein the electrolyte is a gel electrolyte containing a polymer material.

10. A battery pack comprising the secondary battery according to claim 8 or 9.

11. An external terminal for supplying electricity; The battery pack of claim 10, further comprising a protection circuit.

12. 12. The battery pack according to claim 10, comprising a plurality of the secondary batteries, the secondary batteries being electrically connected in series, in parallel, or in a combination of series and parallel.

13. A vehicle equipped with the battery pack according to any one of claims 10 to 12.

14. 14. The vehicle of claim 13, further comprising a mechanism for converting kinetic energy of the vehicle into regenerative energy.

Citation Information

Patent Citations

  • Positive electrode active material for lithium secondary battery

    JP2003217572A

  • Positive electrode active material and nonaqueous electrolyte secondary battery

    JP2005228706A

  • Manufacturing method of nonaqueous electrolyte secondary battery

    JP2007273260A

  • Positive electrode active material for lithium secondary battery, method of manufacturing positive electrode active material for lithium secondary battery, positive electrode for lithium secondary battery, and lithium secondary battery

    JP2012099482A

  • Positive electrode material for lithium secondary battery, and lithium secondary battery

    JP2015060767A