Electrode structure and all-solid-state secondary battery including same

The electrode structure in all-solid-state secondary batteries, featuring a solid electrolyte layer with minimal margin and a high-modulus insulating layer, addresses flexibility and processability issues, enhancing stability and preventing short circuits while maintaining capacity.

JP7581279B2Active Publication Date: 2024-11-12SAMSUNG SDI CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022076171
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-06
Filing Date
2022-05-02
Publication Date
2024-11-12
Estimated Expiration
2042-05-02

AI Technical Summary

Technical Problem

All-solid-state secondary batteries face challenges with lower flexibility and processability, leading to difficulties in securing a width margin between electrode plates and electrolyte membranes, which can result in short circuits, capacity reduction, and decreased life characteristics due to burrs or cracks on the outermost edges.

Method used

An electrode structure with a solid electrolyte layer having minimal or no margin at both ends, surrounded by an insulating layer with a storage modulus of more than 4.0 GPa on both sides, composed of polymers or polymer-inorganic material composites, to prevent deformation and short circuits during battery manufacturing.

Benefits of technology

The proposed electrode structure effectively prevents short circuits and maintains life characteristics by minimizing initial capacity reduction, ensuring the battery's stability and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581279000003
    Figure 0007581279000003
  • Figure 0007581279000004
    Figure 0007581279000004
  • Figure 0007581279000005
    Figure 0007581279000005
Patent Text Reader

Abstract

To provide an electrode structure and an all-solid secondary battery including the same.SOLUTION: Provided are an electrode structure and an all-solid secondary battery including the same. The electrode structure includes a cathode layer, an anode layer, and a solid electrolyte layer between the cathode layer and the anode layer. The cathode layer includes a cathode current collector, and a cathode active material layer on at least one surface of the cathode current collector. The anode layer includes an anode current collector, and an anode active material layer on at least one surface of the anode current collector. The solid electrolyte layer has no margin or a margin of 2% or less of a width of the solid electrolyte layer, at two ends in a width direction, and includes an insulating layer having a storage elastic modulus (E') greater than 4.0 GPa at both sides integrally surrounding the cathode layer, the anode layer and the solid electrolyte layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrode structure and an all-solid-state secondary battery including the electrode structure. [Background technology]

[0002] Recently, due to industrial demand, there has been active development of batteries with high energy density and safety. For example, lithium ion batteries are being used not only in the fields of information-related equipment and communication equipment, but also in the field of automobiles. In the field of automobiles, safety is particularly important because life is at stake.

[0003] Currently available lithium-ion batteries use electrolytes containing flammable organic solvents, which may lead to overheating and fire if a short circuit occurs. In response to this, all-solid-state secondary batteries that use solid electrolytes instead of electrolytes have been proposed.

[0004] Since all-solid-state secondary batteries do not use flammable organic solvents, the possibility of fire or explosion can be significantly reduced even if a short circuit occurs, and therefore such all-solid-state secondary batteries can be significantly safer than lithium-ion batteries that use electrolytes. Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide an electrode structure having a new structure.

[0006] Another problem to be solved by the present invention is to provide an all-solid-state secondary battery including the electrode structure. [Means for solving the problem]

[0007] According to one aspect, An electrode structure including a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, the positive electrode layer includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, the negative electrode layer includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, the solid electrolyte layer has no margin at both ends in a width direction, or has margins of 2% or less of the width of the solid electrolyte layer; An electrode structure is provided, which includes insulating layers having a storage elastic modulus (E') of greater than 4.0 GPa on both sides integrally surrounding the positive electrode layer, the negative electrode layer and the solid electrolyte layer.

[0008] The insulating layer may have a loss tangent (tan δ) of less than 0.5.

[0009] The insulating layer is 1x10 6 It may have a resistivity of ohm / cm or more.

[0010] The insulating layer is at least one layer.

[0011] The insulating layer may also include a polymer or a composite of a polymer and an inorganic material.

[0012] The polymer may include a fluorine-based polymer, a cellulose-based polymer, an epoxy-based resin, or a combination thereof.

[0013] In the composite of the polymer and the inorganic material, the volume ratio of the polymer is 50% by volume or more based on 100% by volume of the entire composition for forming a composite.

[0014] The inorganic material may also include a metal oxide, a metal hydroxide, or a combination thereof.

[0015] The positive electrode active material layer has a mixture density of 3.0 g / cc or more.

[0016] The positive electrode active material layer also contains a sulfide-based solid electrolyte.

[0017] The negative electrode active material layer may include at least one selected from the group consisting of a carbon-based negative electrode active material, a metal negative electrode active material, and a semi-metal negative electrode active material.

[0018] The carbon-based negative electrode active material may include at least one selected from the group consisting of amorphous carbon and crystalline carbon.

[0019] The metal negative electrode active material or semi-metal negative electrode active material may include at least one selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn).

[0020] The solid electrolyte layer also includes a sulfide-based solid electrolyte represented by the following chemical formula 1:

[0021] [Chemical formula 1] Li + 12-n-x A n+ X 2- 6-x Y - x

[0022] In the formula 1, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb or Ta; X is S, Se or Te, and Y is Cl, Br, I, F, CN, OCN, SCN, or N3, where 1≦x≦5, 0≦n≦2.

[0023] The solid electrolyte layer has a peel strength with respect to the positive electrode layer or the negative electrode layer of 0.2 gf / mm or more.

[0024] The electrode structure may also be in a jelly roll or stack form.

[0025] The electrode structure may be such that no cracks are generated in the electrode structure when the electrode structure is compressed in a thickness direction by 20 to 30% of its thickness.

[0026] According to another aspect, An all-solid-state secondary battery is provided that includes the electrode structure described above. Effect of the Invention

[0027] According to one embodiment, the electrode structure includes a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer. The solid electrolyte layer has no margin at both ends in a width direction or has a margin of 2% or less of the width of the solid electrolyte layer. The electrode structure includes insulating layers having a storage elastic modulus (E') of more than 4.0 GPa on both sides integrally surrounding the positive electrode layer, the negative electrode layer, and the solid electrolyte layer.

[0028] The electrode structure can provide an all-solid-state secondary battery having improved life characteristics while suppressing short circuits through the insulating layer and minimizing initial capacity reduction, even when the solid electrolyte layer has very little or no width margin. [Brief description of the drawings]

[0029] [Figure 1] 1 is a schematic cross-sectional view of an electrode structure according to an embodiment; [Figure 2A] 1 is a schematic cross-sectional view showing a stacked electrode structure according to an embodiment; [Figure 2B] 2B is a schematic cross-sectional view showing the inside of the electrode structure of FIG. 2A (dotted line portion). [Diagram 3] 1 is a schematic diagram of an all-solid-state secondary battery according to an embodiment; [Figure 4] 1 is a graph showing the life characteristics of all-solid-state secondary batteries produced in Examples 1 to 3 and Comparative Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Hereinafter, an electrode structure according to an embodiment of the present invention and an all-solid-state secondary battery including the same will be described in detail with reference to the accompanying drawings. The following is provided as an example, and the present invention is not limited thereby, and the present invention is only defined by the scope of the claims described below.

[0031] As used herein, the terms "at least one," "one or more," or "one or more" preceding an element may supplement the entire list of elements and not each of the individual elements listed above. As used herein, the term "combination" is inclusive of mixtures, alloys, reaction products, and the like, unless specifically stated to the contrary.

[0032] In this specification, unless specifically stated to the contrary, the term "comprise" does not mean excluding other components, but means that other components may be further included.

[0033] In this specification, terms such as "first", "second", etc. do not denote an order, quantity, or importance, but are used to distinguish one element from another. In this specification, both the singular and the plural should be construed as including the plural, unless otherwise indicated or clearly contradicted by context. "Or" means "and / or" unless otherwise indicated.

[0034] Throughout this specification, the words "an embodiment," "an embodiment," and the like mean that a particular element described in connection with an embodiment is included in at least one embodiment described herein and may or may not be present in other embodiments, and it should be understood that the described elements may be combined in any suitable manner in the various embodiments.

[0035] Unless otherwise defined, technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application pertains. All cited patents, patent applications, and other references are incorporated herein by reference in their entirety. However, if a term from this specification contradicts or conflicts with a term from the incorporated reference, the term from this specification shall take precedence over the conflicting term in the incorporated reference. Although specific examples and embodiments have been described, alternatives, modifications, variations, improvements, and substantial equivalents that are not currently foreseeable or may not be foreseeable may occur to the applicant or those skilled in the art. Accordingly, the appended claims and amended subject matter are intended to include all such alternatives, modifications, variations, improvements, and substantial equivalents.

[0036] Although the all-solid-state secondary battery is advantageous in terms of stability, since the electrolyte is solid, it is less flexible and easier to process than a lithium-ion battery. For this reason, it is difficult to secure a width margin between the electrode plate and the electrolyte membrane in an electrode structure composed of a positive electrode plate, a negative electrode plate, and an electrolyte membrane. In addition, burrs or cracks may occur on the outermost edge surface between the electrode plate and the electrolyte membrane. In such a case, a short circuit occurs inside the all-solid-state secondary battery, and the capacity and life characteristics are reduced. The inventor of the present invention solves the problem of the capacity and life characteristics being reduced through the design of a new layer on the side of the electrode structure.

[0037] Hereinafter, the electrode structure and the all-solid-state secondary battery according to the example embodiments will be described in more detail.

[0038] [Electrode structure] According to an embodiment, the electrode structure includes a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer. The positive electrode layer includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector. The negative electrode layer includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector. The solid electrolyte layer may have no margin at both ends in a width direction or may have a margin of 2% or less of the width of the solid electrolyte layer. The electrode structure may include insulating layers having a storage elastic modulus (E') of more than 4.0 GPa on both sides integrally surrounding the positive electrode layer, the negative electrode layer, and the solid electrolyte layer.

[0039] The electrode structure includes insulating layers on both sides integrally surrounding the positive electrode layer, the negative electrode layer, and the solid electrolyte layer. The insulating layers have a storage elastic modulus (E') of more than 4.0 GPa. In general, when the storage elastic modulus (E') of the solid electrolyte layer is 1.3 to 4.0, the storage elastic modulus (E') of the insulating layer is high. Therefore, the electrode structure is not deformed by pressure during battery manufacturing, and as a result, short circuits are prevented. This is because short circuits can be prevented even when there is no margin at both ends in the width direction of the solid electrolyte layer, or when the margin is very small, less than 2% of the width of the solid electrolyte layer.

[0040] Fig. 1 is a schematic cross-sectional view of an electrode structure according to an embodiment. Fig. 2A is a schematic cross-sectional view of a stacked electrode structure according to an embodiment. Fig. 2B is a schematic cross-sectional view of the inside of the electrode structure of Fig. 2A (dotted line portion).

[0041] 1, in an electrode structure 10, a positive electrode layer 1, a solid electrolyte layer 2, and a negative electrode layer 3 are arranged in this order, and insulating layers 4 are arranged on both side surfaces that integrally surround the positive electrode layer 1, the solid electrolyte layer 2, and the negative electrode layer 3. The solid electrolyte layer 2 has a marginal width W at both ends in the width direction. For example, the marginal width W is 0.5 mm or less.

[0042] 2A and 2B, the electrode structure 30 has a bi-cell structure in a stack form. In the electrode structure 30, the positive electrode layers 26, 26', each having a positive electrode active material layer 22, 22', are disposed on the upper and lower surfaces of the positive electrode collector 21, the solid electrolyte layer 23, 23' is disposed on one surface of the positive electrode layer 26, 26', and the negative electrode layer 27, 27', each including the negative electrode active material layer 25, 25' and the negative electrode collector 24, 24', is disposed on one surface of the solid electrolyte layer 23, 23'. The positive electrode layer 26, 26', the solid electrolyte layer 23, 23', and the negative electrode layer 27, 27' are each disposed on both sides thereof with insulating layers 28, 28'.

[0043] Although the electrode structure 30 is illustrated in a stack configuration, it may also be in a jellyroll configuration.

[0044] When the electrode structure 30 is compressed in the thickness direction by 20 to 30% of its thickness, no cracks are generated in the electrode structure 30.

[0045] [Insulation layer] The insulating layer 28, 28' may have a storage modulus of elasticity (E') of more than 4.0 GPa. The electrode structure 10, 30 including the insulating layer 28, 28' having such a storage modulus of elasticity (E') is not deformed by pressure during battery manufacture in a jelly roll or stack form, and short circuits are prevented.

[0046] The insulating layer 28, 28' may have a loss tangent (tan δ) of less than 0.5. The loss tangent (tan δ) is the ratio of the storage non-elastic modulus (E'') to the storage elastic modulus (E'), i.e., E'' / E'. The loss tangent (tan δ) is related to the restoring force. The restoring force is a force that restores an original state after being deformed by pressure during battery manufacturing, and reduces the probability of short circuit during battery charging and discharging. In general, when the loss tangent (tan δ) of the solid electrolyte layer is 0.05 to 0.15, the loss tangent (tan δ) of the insulating layer 28, 28' is low. Therefore, the electrode structure 10, 30 exerts a restoring force during battery manufacturing, and does not deform by pressure, thereby preventing short circuit.

[0047] The storage elastic modulus (E') and storage inelastic modulus (E'') of the insulating layer 28, 28' can be obtained by using dynamic mechanical analysis (DMA). For example, the storage elastic modulus (E') and storage inelastic modulus (E'') can be derived by applying an external force in the form of a sine wave with a frequency of 1 Hz to a sample of 10 mm x 5 mm and measuring the displacement and phase of the sample deformed by the force.

[0048] The insulating layers 28, 28' are 1x10 6 The insulating layers 28, 28' may have a resistivity of 100 ohm / cm or more. The insulating layers 28, 28' are electrically insulating and may suppress short circuits within the electrode structures 10, 30.

[0049] The insulating layer 28, 28' may be at least one layer. For example, the insulating layer 28, 28' may be two layers or three or more layers. The number of layers of the insulating layer 28, 28' may be adjusted within a range that satisfies the storage elastic modulus (E'), the storage inelastic modulus (E'') and the loss tangent (tan δ).

[0050] The insulating layers 28, 28' may also include a polymer or a composite of a polymer and an inorganic material, such as a fluorine-based polymer, a cellulose-based polymer, an epoxy-based resin, or a combination thereof.

[0051] Examples of the fluorine-based polymer include a homopolymer of vinylidene fluoride monomer, or a copolymer of vinylidene fluoride monomer and one or more fluorine-containing monomers selected from tetrafluoroethylene, hexafluoropropylene, chlorotrifluoroethylene, fluorovinyl, and perfluoroalkyl vinyl ether. Specifically, the vinylidene fluoride-based monomer may be a vinylidene fluoride homopolymer, a vinylidene fluoride-hexafluoropropylene copolymer, or a vinylidene fluoride-chlorotrifluoroethylene copolymer.

[0052] Alternatively, the fluorine-based polymer may be a copolymer of a monomer containing a polar functional group and a vinylidene fluoride monomer, or may further include a copolymer of a monomer containing a polar functional group, a vinylidene fluoride monomer, and the above-mentioned other fluorine-based monomer. For example, the vinylidene fluoride polymer containing a polar functional group may be a copolymer of a monomer containing a polar functional group and vinylidene fluoride, a copolymer of a monomer containing a polar functional group and vinylidene fluoride and hexafluoropropylene, or a copolymer of a monomer containing a polar functional group and vinylidene fluoride and chlorotrifluoroethylene. The polar functional group may be one or more selected from a carboxylic acid group, a sulfonic acid group, a phosphoric acid group, a hydroxyl group, and salts thereof, but is not necessarily limited thereto, and may be any group that can be used as a polar functional group in the art. The introduction of the polar functional group into the fluorine-based polymer may be achieved by polymerizing a monomer containing a carboxylic acid group, a sulfonic acid group, a phosphoric acid group, a hydroxyl group, and salts thereof. Examples of monomers having a carboxylic acid group include monocarboxylic acids and their derivatives, dicarboxylic acids and their derivatives, etc. Examples of monocarboxylic acids include acrylic acid, methacrylic acid, crotonic acid, etc. Examples of the monocarboxylic acid derivatives include 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, α-chloro-β-E-methoxyacrylic acid, β-diaminoacrylic acid, etc. Examples of the dicarboxylic acid include maleic acid, fumaric acid, itaconic acid, etc. Examples of the dicarboxylic acid derivatives include maleic acid such as methylmaleic acid, dimethylmaleic acid, phenylmaleic acid, chloromaleic acid, dichloromaleic acid, and fluoromaleic acid; and methylallyl maleate; maleates such as diphenyl maleate, nonyl maleate, decyl maleate, dodecyl maleate, octadecyl maleate, and fluoroalkyl maleate; and the like. Also, acid anhydrides that generate a carboxylic acid group by hydrolysis can be used. Examples of the acid anhydride of a dicarboxylic acid include maleic anhydride, acrylic anhydride, methylmaleic anhydride, and dimethylmaleic anhydride.In addition, it may have monoesters and diesters of α,β-ethylenically unsaturated polycarboxylic acids such as monoethyl maleate, diethyl maleate, monobutyl maleate, dibutyl maleate, monoethyl fumarate, diethyl fumarate, monobutyl fumarate, dibutyl fumarate, monocyclohexyl fumarate, dicyclohexyl fumarate, monoethyl itaconate, diethyl itaconate, monobutyl itaconate, and dibutyl itaconate. Examples of monomers having a sulfonic acid group include vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allyl sulfonic acid, styrene sulfonic acid, (meth)acrylic acid-2-ethyl sulfonate, 2-acrylamido-2-methylpropane sulfonic acid, and 3-allyloxy-2-hydroxypropane sulfonic acid. Examples of monomers having a phosphoric acid group include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, ethyl-(meth)acryloyloxyethyl phosphate, etc. Examples of monomers having a hydroxyl group include ethylenically unsaturated alcohols such as (meth)allyl alcohol, 3-buten-1-ol, and 5-hexen-1-ol; alkanol esters of ethylenically unsaturated carboxylic acids such as 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, di-2-hydroxyethyl maleate, di-4-hydroxybutyl maleate, and di-2-hydroxypropyl itaconate; and monomers having the general formula CH2=CR1-COO-(C. n H 2n O) m-H (m is an integer of 2 to 9, n is an integer of 2 to 4, and R1 is hydrogen or a methyl group) and (meth)acrylic acid esters; mono(meth)acrylic acid esters of dihydroxy esters of dicarboxylic acids such as 2-hydroxyethyl-2'-(meth)acryloyloxyphthalate and 2-hydroxyethyl-2'-(meth)acryloyloxysuccinate; vinyl ethers such as 2-hydroxyethyl vinyl ether and 2-hydroxypropyl vinyl ether; (meth)allyl-2-hydroxyethyl ether, (meth)allyl-2-hydroxypropyl ether, (meth)allyl-3-hydroxypropyl ether, (meth)allyl-2-hydroxybutyl ether, (meth)allyl-3-hydroxybutyl ether, (meth)allyl-4-hydroxybutyl ether, (meth)allyl-6-hydroxyhexyl ether, mono(meth)allyl ethers of alkylene glycols such as diethylene glycol mono(meth)allyl ether and dipropylene glycol mono(meth)allyl ether; mono(meth)allyl ethers of halogen- and hydroxy-substituted (poly)alkylene glycols such as glycerin mono(meth)allyl ether, (meth)allyl-2-chloro-3-hydroxypropyl ether and (meth)allyl-2-hydroxy-3-chloropropyl ether; mono(meth)allyl ethers of polyhydric phenols such as eugenol and isoeugenol and halogen-substituted products thereof; (meth)allyl thioethers of alkylene glycols such as (meth)allyl-2-hydroxyethyl thioether and (meth)allyl-2-hydroxypropyl thioether; etc. The fluorine-based polymers can improve the adhesive strength and flexibility of the electrode plate, and provide a battery having improved energy density and life characteristics.

[0053] Examples of the cellulose-based polymer include at least one selected from cellulose, methyl cellulose, ethyl cellulose, butyl cellulose, hydroxypropyl cellulose, cellulose acetate, cellulose acetate propionate, and cellulose acetate butyrate. The form of the cellulose-based polymer is not limited, and may be, for example, a nanofiber form. The cellulose-based polymer has excellent mechanical strength and optical transparency. Therefore, a battery including the cellulose-based polymer as the insulating layer 28, 28' may have excellent life characteristics and stability.

[0054] The epoxy resin may be at least one selected from cresol novolac epoxy resin, bisphenol A type epoxy resin, bisphenol A type novolac epoxy resin, phenol novolac epoxy resin, tetrafunctional epoxy resin, biphenyl type epoxy resin, triphenol methane type epoxy resin, alkyl modified triphenol methane epoxy resin, naphthalene type epoxy resin, dicyclopentadiene type epoxy resin, dicyclopentadiene modified phenol type epoxy resin, urethane modified epoxy resin, and combinations thereof, but is not limited thereto. The epoxy resin has excellent mechanical properties and electrical insulation properties.

[0055] In the composite of the polymer and the inorganic material, the volume ratio of the polymer is 50% or more by volume based on 100% by volume of the entire composition for forming a composite. Within the range of the volume ratio of the polymer, the physical properties such as the storage modulus of elasticity (E') and the storage inelastic modulus (E'') of the insulating layer 28, 28' can be enhanced. In addition, by increasing the weight ratio of the inorganic material in the composite of the polymer and the inorganic material, the strength and the storage modulus of elasticity (E') of the composite of the polymer and the inorganic material can be increased, and the storage inelastic modulus (E'') can also be increased. Therefore, in the composite of the polymer and the inorganic material, the weight ratio of the polymer to the inorganic material is 1:1 to 1:5. Within the range of the weight ratio of the polymer to the inorganic material, the physical properties such as the storage modulus of elasticity (E') and the storage inelastic modulus (E'') of the insulating layer 28, 28' can be enhanced.

[0056] The inorganic material may include metal oxides, metal hydroxides, or combinations thereof. Examples of the inorganic material include, but are not limited to, Al2O3, Al(OH)3, etc., and all inorganic materials that can be used in the field of all-solid-state secondary batteries can be used.

[0057] [Positive electrode layer] The positive electrode layers 26, 26' include a positive electrode current collector 21 and positive electrode active material layers 22, 22' disposed on at least one surface of the positive electrode current collector 21.

[0058] The positive electrode active material layer 22, 22' includes, for example, a positive electrode active material and a solid electrolyte. The solid electrolyte included in the positive electrode layer 26, 26' may be the same as or different from the solid electrolyte included in the solid electrolyte layer 23, 23'. For example, the solid electrolyte may include a sulfide-based solid electrolyte. For details regarding the solid electrolyte, please refer to the solid electrolyte layer 23, 23'.

[0059] The positive electrode active material is a positive electrode active material that can reversibly absorb and desorb lithium ions. The positive electrode active material may be, for example, lithium transition metal oxides such as lithium cobalt oxide (LCO), lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese oxide (NCM), lithium manganate, and lithium iron phosphate; nickel sulfide; copper sulfide; lithium sulfide; iron oxide; or vanadium oxide, but is not necessarily limited thereto. Any positive electrode active material that is used as a positive electrode active material in the technical field is possible. The positive electrode active material may be a single material or a mixture of two or more materials.

[0060] Lithium transition metal oxides are, for example, Li a A 1-b B' b D'2 (wherein, in the above formula, 0.90≦a≦1 and 0≦b≦0.5); Li a E 1-b B' b O 2-c D' c (wherein, 0.90≦a≦1, 0≦b≦0.5, and 0≦c≦0.05); LiE 2-b B' b O 4-c D' c (wherein, 0≦b≦0.5 and 0≦c≦0.05); Li a Ni 1-b-c Co b B' c D' α (wherein, in the formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Co b B' c O 2-α F' α (wherein, in the formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Co b B' c O 2-α F'2 (wherein, in the above formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B' c D' α (wherein, in the formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Mn b B' c O 2-α F' α (wherein, in the formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B' c O 2-αF'2 (wherein, in the above formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni b E c G d O2 (wherein the formula is 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, and 0.001≦d≦0.1); Li a Ni b Co c Mn d G e O2 (wherein, in the above formula, 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, 0.001≦e≦0.1); Li a NiG b O2 (wherein, in the above formula, 0.90≦a≦1, 0.001≦b≦0.1); Li a CoG b O2 (wherein, in the above formula, 0.90≦a≦1, 0.001≦b≦0.1); Li a MnG b O2 (wherein, in the above formula, 0.90≦a≦1, 0.001≦b≦0.1); Li a Mn2G b O4 (wherein the above formula is 0.90≦a≦1, 0.001≦b≦0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiI'O2; LiNiVO4; Li (3-f) J2(PO4)3(0≦f≦2);Li (3-f)A compound represented by any one of the chemical formulas Fe2(PO4)3(0≦f≦2);LiFePO4. In such a compound, A is Ni, Co, Mn, or a combination thereof, B' is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof, D' is O, F, S, P, or a combination thereof, E is Co, Mn, or a combination thereof, F' is F, S, P, or a combination thereof, G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof, Q is Ti, Mo, Mn, or a combination thereof, I' is Cr, V, Fe, Sc, Y, or a combination thereof, and J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. A compound having a coating layer added to the surface of such a compound can also be used, and a mixture of the above-mentioned compound and a compound having a coating layer added can also be used. The coating layer added to the surface of such a compound includes, for example, a coating element compound such as an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, an oxycarbonate of a coating element, or a hydroxycarbonate of a coating element. The compound forming such a coating layer is amorphous or crystalline. The coating element contained in the coating layer is Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method of forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method is, for example, a spray coating method, a dipping method, etc. The specific coating method is a content that can be fully understood by those skilled in the art, so a detailed description is omitted.

[0061] The positive electrode active material includes, for example, in the above-described lithium transition metal oxide, a lithium salt of a transition metal oxide having a layered rock salt type structure. The "layered rock salt type structure" is, for example, a structure in which oxygen atom layers and metal atom layers are regularly arranged alternately in the <111> direction of a cubic rock salt type structure, whereby each atomic layer forms a two-dimensional plane. The "cubic rock salt type structure" indicates a sodium chloride type (NaCl type) structure which is a kind of crystal structure. Specifically, it indicates a structure in which face-centered cubic lattices (FCC) formed by cations and anions, respectively, are arranged so as to be shifted from each other by about 1 / 2 of the ridge of the unit lattice. Such a lithium transition metal oxide having a layered rock salt type structure is, for example, LiNi x Co y Al z O2 (NCA) or LiNi x Co y Mn z O2 (NCM) (0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1), which is a ternary lithium transition metal oxide. When the positive electrode active material includes a ternary lithium transition metal oxide having a layered rock salt type structure, the energy density and thermal stability of the all-solid-state secondary battery are further improved.

[0062] As described above, the positive electrode active material is also covered with a coating layer. The coating layer may be any one as long as it is known as a coating layer for the positive electrode active material of an all-solid-state secondary battery. The coating layer is, for example, Li2O-ZrO2 (LZO) or the like.

[0063] When the positive electrode active material is, for example, LiNi x Co y Al z O2 (NCA) or LiNi x Co y Mn zAs a ternary lithium transition metal oxide such as O2(NCM) (0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1), when nickel (Ni) is included, the capacity density of the all-solid-state secondary battery can be increased, and metal elution from the positive electrode active material can be reduced in the charged state. As a result, the cycle characteristics of the all-solid-state secondary battery in the charged state are improved.

[0064] The shape of the positive electrode active material is, for example, a particle shape such as a true spherical shape or an elliptical spherical shape. The particle size of the positive electrode active material is not particularly limited and is within the range applicable to the positive electrode active material of a conventional all-solid-state secondary battery. The content of the positive electrode active material in the positive electrode layers 26, 26' is also not particularly limited and is within the range applicable to the positive electrode layer of a conventional all-solid-state secondary battery.

[0065] The solid electrolyte contained in the positive electrode active material layers 22, 22' also has a smaller D50 average particle size than the solid electrolyte contained in the solid electrolyte layers 23, 23'. For example, the D50 average particle size of the solid electrolyte contained in the positive electrode active material layers 22, 22' is 90% or less, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, or 20% or less of the D50 average particle size of the solid electrolyte contained in the solid electrolyte layers 23, 23'.

[0066] The D50 average particle size is, for example, the median particle diameter (D50). The median particle diameter (D50) is, for example, in the particle size distribution measured by the laser diffraction method, calculated from the side of the particles having a small particle size, and is the size of the particles corresponding to 50% cumulative volume.

[0067] The positive electrode active material layers 22, 22' also contain a binder. The binder is, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., but is not limited thereto, and any binder that can be used in the technical field is possible.

[0068] The positive electrode active material layers 22, 22' also contain a conductive material, such as, but not limited to, graphite, carbon black (CB), acetylene black (AB), Ketjen black (KB), carbon fiber, metal powder, etc., and any material that is used as a conductive material in the relevant technical field is possible.

[0069] The positive electrode active material layers 22, 22' further contain additives such as a filler, a coating agent, a dispersant, and an ion-conducting assistant in addition to the above-mentioned positive electrode active material, solid electrolyte, binder, and conductive material.

[0070] The filler, coating agent, dispersant, ion-conducting assistant, and the like contained in the positive electrode active material layers 22, 22' may be any known material generally used for electrodes of all-solid-state secondary batteries.

[0071] The positive electrode active material layers 22, 22' also have a mixture density of 3.0 g / cc or more.

[0072] The positive electrode current collector 21 may be, for example, a plate or foil made of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector 21 may be omitted. The thickness of the positive electrode current collector 21 is, for example, 1 μm to 100 μm, 1 μm to 50 μm, 5 μm to 25 μm, or 10 μm to 20 μm.

[0073] [Solid electrolyte layer] 1 and 2B, the solid electrolyte layer 2, 23, 23' includes a solid electrolyte layer disposed between a positive electrode layer 1, 26, 26' and a negative electrode layer 3, 27, 27'.

[0074] The solid electrolyte is, for example, a sulfide-based solid electrolyte. The sulfide-based solid electrolyte is, for example, Li2S-P2S5, Li2S-P2S5-LiX (X is a halogen element), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (m and n are positive numbers, and Z is one of Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (p and q are positive numbers, and M is one of P, Si, Ge, B, Al, and GaIn), Li 7-x P.S. 6-x Cl x (0≦x≦2), Li 7-x P.S. 6-x Br x (0≦x≦2), and Li 7-x P.S. 6-x I x (0≦x≦2) is one or more. The sulfide-based solid electrolyte is prepared by processing starting materials such as Li2S and P2S5 by melt quenching or mechanical milling. After such processing, heat treatment can be performed. The solid electrolyte is amorphous, crystalline, or a mixture of them. The solid electrolyte is also, for example, the above-mentioned sulfide-based solid electrolyte material, and includes at least sulfur (S), phosphorus (P), and lithium (Li) as constituent elements. For example, the solid electrolyte is also a material including Li2S-P2S5. When using a sulfide-based solid electrolyte material including Li2S-P2S5 to form the solid electrolyte, the mixed molar ratio of Li2S and P2S5 is, for example, in the range of Li2S:P2S5=50:50 to 90:10.

[0075] The sulfide-based solid electrolyte also includes, for example, an argyrodite-type solid electrolyte represented by the following chemical formula 1:

[0076] [Chemical formula 1] Li + 12-n-x A n+ X 2- 6-x Y - x

[0077] In the above formula 1, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb, or Ta, X is S, Se, or Te, and Y is Cl, Br, I, F, CN, OCN, SCN, or N3, where 1≦x≦5 and 0≦n≦2. The sulfide-based solid electrolyte is, for example, Li 7-x P.S. 6-x Cl x (0≦x≦2), Li 7-x P.S. 6-x Br x (0≦x≦2) and Li 7-x P.S. 6-x I x (0≦x≦2). The sulfide-based solid electrolyte is also an argyrodite-type compound containing one or more selected from Li6PS5Cl, Li6PS5Br, and Li6PS5I, for example.

[0078] The density of the argyrodite-type solid electrolyte is 1.5 to 2.0 g / cc. When the argyrodite-type solid electrolyte has a density of 1.5 g / cc or more, the internal resistance of the all-solid-state secondary battery is reduced, and the penetration of the solid electrolyte layer by Li can be effectively suppressed.

[0079] The solid electrolyte layer 2, 23, 23' may also contain, for example, a binder. The binder contained in the solid electrolyte layer 2, 23, 23' may be, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., but is not limited thereto, and any binder used as a binder in the relevant technical field is possible. The binder in the solid electrolyte layer 2, 23, 23' may be the same as or different from the binder contained in the positive electrode active material layer 22, 22' and the negative electrode active material layer 25, 25'. The binder may be omitted.

[0080] The binder content of the solid electrolyte layer 2, 23, 23' is 0 to 10 wt%, 0 to 5 wt%, 0 to 3 wt%, 0 to 1 wt%, 0 to 0.5 wt%, or 0 to 0.1 wt% based on the total weight of the solid electrolyte layer 2, 23, 23'.

[0081] The solid electrolyte layers 2, 23, 23' have a peel strength to the positive electrode layers 26, 26' or the negative electrode layers 27, 27' of 0.2 gf / mm or more.

[0082] [Negative electrode layer] The negative electrode layers 27, 27' include negative electrode current collectors 24, 24' and negative electrode active material layers 25, 25' disposed on at least one surface of the negative electrode current collectors 24, 24'.

[0083] The negative electrode active material layers 25, 25' contain, for example, a negative electrode active material and a binder.

[0084] The negative electrode active material contained in the negative electrode active material layer 25, 25' has, for example, a particle form. The average particle diameter of the negative electrode active material having the particle form is, for example, 4 μm or less, 3 μm or less, 2 μm or less, 1 μm or less, or 900 nm or less. The average particle diameter of the negative electrode active material having the particle form is, for example, 10 nm to 4 μm or less, 10 nm to 3 μm or less, 10 nm to 2 μm or less, 10 nm to 1 μm or less, or 10 nm to 900 nm or less. When the negative electrode active material has an average particle diameter in such a range, reversible absorbing and / or desorbing of lithium during charging and discharging is further facilitated. The average particle diameter of the negative electrode active material is, for example, a median diameter (D50) measured using a laser type particle size distribution meter.

[0085] The negative electrode active material contained in the negative electrode active material layers 25, 25' includes, for example, at least one selected from a carbon-based negative electrode active material, a metal negative electrode active material, and a semi-metal negative electrode active material.

[0086] The carbon-based negative electrode active material may include at least one selected from amorphous carbon and crystalline carbon. The carbon-based negative electrode active material may be, for example, amorphous carbon. The amorphous carbon may be, for example, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, etc., but is not necessarily limited thereto, and may be any material that is classified as amorphous carbon in the art. The amorphous carbon is carbon that has no crystallinity or has very low crystallinity, and is distinguished from crystalline carbon or graphite-based carbon.

[0087] The metal negative electrode active material or metalloid negative electrode active material includes, but is not limited to, at least one selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn), and may be any metal negative electrode active material or metalloid negative electrode active material that forms an alloy or compound with lithium in the art. For example, nickel (Ni) is not a metal negative electrode active material because it does not form an alloy with lithium.

[0088] The negative electrode active material layer 25, 25' may include one type of negative electrode active material or a mixture of a plurality of different negative electrode active materials. For example, the negative electrode active material layer 25, 25' may include only amorphous carbon or may include one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). Alternatively, the negative electrode active material layer 25, 25' may include a mixture of amorphous carbon and one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The mixing ratio of the mixture of the amorphous carbon and gold, etc., is, for example, 10:1 to 1:2, 5:1 to 1:1, or 4:1 to 2:1 by weight, but is not necessarily limited to such ranges and is selected according to the required characteristics of the all-solid-state secondary battery. When the negative electrode active material has such a composition, the life characteristics of the all-solid-state secondary battery are further improved.

[0089] The negative active material included in the negative active material layer 25, 25' includes a mixture of first particles made of amorphous carbon and second particles made of a metal or a metalloid. The metal or metalloid includes, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). Alternatively, the metalloid is a semiconductor. The content of the second particles is 8 to 60 wt%, 10 to 50 wt%, 15 to 40 wt%, or 20 to 30 wt%, based on the total weight of the mixture. When the second particles have a content in such a range, for example, the life characteristics of the all-solid-state secondary battery are further improved.

[0090] The binder contained in the negative electrode active material layer 25, 25' is, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited thereto, and any binder used as a binder in the relevant technical field is possible. The binder may be composed of a single binder or a plurality of different binders.

[0091] The negative electrode active material layer 25, 25' contains a binder, so that the negative electrode active material layer 25, 25' is stabilized on the negative electrode current collector 24, 24'. In addition, cracks in the negative electrode active material layer 25, 25' are suppressed despite volume changes and / or relative position changes of the negative electrode active material layer 25, 25' during charge and discharge processes. For example, if the negative electrode active material layer 25, 25' does not contain a binder, the negative electrode active material layer 25, 25' is easily separated from the negative electrode current collector 24, 24'. When the negative electrode active material layer 25, 25' is detached from the negative electrode current collector 24, 24', the negative electrode current collector 24, 24' comes into contact with the solid electrolyte layer 23, 23' at the portion where the negative electrode current collector 24, 24' is exposed, which increases the possibility of a short circuit occurring. The negative electrode active material layer 25, 25' is produced, for example, by applying a slurry in which materials constituting the negative electrode active material layer 25, 25' are dispersed onto the negative electrode current collector 24, 24' and drying the slurry. By including a binder in the negative electrode active material layer 25, 25', it is possible to stably disperse the negative electrode active material in the slurry. For example, when the slurry is applied onto the negative electrode current collector 24, 24' by a screen printing method, clogging of the screen (for example, clogging due to agglomerates of the negative electrode active material) can be suppressed.

[0092] The negative electrode active material layers 25, 25' can further contain additives used in conventional all-solid-state secondary batteries, such as a filler, a coating agent, a dispersant, and an ion-conducting assistant.

[0093] The thickness of the negative electrode active material layer 25, 25' is, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less of the thickness of the positive electrode active material layer 22, 22'. The thickness of the negative electrode active material layer 25, 25' is, for example, 1 μm to 20 μm, 2 μm to 10 μm, or 3 μm to 7 μm. If the thickness of the negative electrode active material layer 25, 25' is excessively thin, lithium dendrites formed between the negative electrode active material layer 25, 25' and the negative electrode current collector 24, 24' collapse the negative electrode active material layer 25, 25', making it difficult to improve the life characteristics of the all-solid-state secondary battery. If the thickness of the negative electrode active material layers 25, 25' is excessively large, the energy density of the all-solid-state secondary battery decreases, and the internal resistance of the all-solid-state secondary battery due to the negative electrode active material layers 25, 25' increases, making it difficult to improve the life characteristics of the all-solid-state secondary battery.

[0094] If the thickness of the negative electrode active material layer 25, 25' is reduced, the charge capacity of the negative electrode active material layer 25, 25' is reduced, for example. The charge capacity of the negative electrode active material layer 25, 25' is, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, 5% or less, or 2% or less compared to the charge capacity of the positive electrode active material layer 22, 22'. The charge capacity of the negative electrode active material layer 25, 25' is, for example, 0.1% to 50%, 0.1% to 40%, 0.1% to 30%, 0.1% to 20%, 0.1% to 10%, 0.1% to 5%, or 0.1% to 2% compared to the charge capacity of the positive electrode active material layer 22, 22'. If the charge capacity of the negative electrode active material layer 25, 25' is excessively small, the thickness of the negative electrode active material layer 25, 25' becomes very thin, and thus lithium dendrites formed between the negative electrode active material layer 25, 25' and the negative electrode current collector 24, 24' during repeated charge and discharge processes collapse the negative electrode active material layer 25, 25', making it difficult to improve the life characteristics of the all-solid-state secondary battery. If the charge capacity of the negative electrode active material layer 25, 25' is excessively increased, the energy density of the all-solid-state secondary battery decreases and the internal resistance of the all-solid-state secondary battery due to the negative electrode active material layer 25, 25' increases, making it difficult to improve the life characteristics of the all-solid-state secondary battery.

[0095] The charge capacity of the positive electrode active material layer 22, 22' is obtained by multiplying the charge capacity density (mAh / g) of the positive electrode active material by the mass of the positive electrode active material in the positive electrode active material layer 22, 22'. When various types of positive electrode active materials are used, the charge capacity density x mass value is calculated for each positive electrode active material, and the sum of these values ​​is the charge capacity of the positive electrode active material layer 22, 22'. The charge capacity of the negative electrode active material layer 25, 25' is also calculated by the same method. That is, the charge capacity of the negative electrode active material layer 25, 25' is obtained by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the negative electrode active material layer 25, 25'. When various types of negative electrode active materials are used, the charge capacity density x mass value is calculated for each negative electrode active material, and the sum of these values ​​is the capacity of the negative electrode active material layer 25, 25'. Here, the charge capacity density of the positive electrode active material and the negative electrode active material is a capacity estimated using an all-solid-state half-cell using lithium metal as a counter electrode. The charge capacity of the positive electrode active material layer 22, 22' and the negative electrode active material layer 25, 25' is directly measured by measuring the charge capacity using the all-solid-state half-cell. The charge capacity density is obtained by dividing the measured charge capacity by the mass of each active material. Alternatively, the charge capacity of the positive electrode active material layer 22, 22' and the negative electrode active material layer 25, 25' may be an initial charge capacity measured during the first cycle charge.

[0096] The negative electrode current collector 24, 24' is made of a material that does not react with lithium, i.e., does not form any alloy or compound. The material constituting the negative electrode current collector 24, 24' is, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), etc., but is not necessarily limited thereto, and any material that is used as an electrode current collector in the relevant technical field is possible. The negative electrode current collector 24, 24' is made of one of the above-mentioned metals, or an alloy or coating material of two or more metals. The negative electrode current collector 24, 24' is, for example, in the form of a plate or foil.

[0097] [All-solid-state secondary battery] The all-solid-state secondary battery includes the electrode structures 10, 30 described above.

[0098] FIG. 3 is a schematic diagram of an all-solid-state secondary battery according to an embodiment.

[0099] 3, the all-solid-state secondary battery is in a stack form. In the all-solid-state secondary battery 40, the positive electrode layers 36, 36', in which the positive electrode active material layers 32, 32' are disposed on the upper and lower surfaces of the positive electrode collector 31, the solid electrolyte layers 33, 33' are disposed on one surface of the positive electrode layers 36, 36', and the negative electrode layers 37, 37', which are constituted by the negative electrode active material layers 34, 34' and the negative electrode collectors 35, 35', are disposed on one surface of the solid electrolyte layers 33, 33'. The insulating layers 38, 38' are disposed on both sides of the positive electrode layers 36, 36', the solid electrolyte layers 33, 33', and the negative electrode layers 37, 37', respectively. The support members 39, 39' are disposed on one surface of the negative electrode collectors 35, 35'. The all-solid-state secondary battery 40 is manufactured by pressing the upper and lower support members 39, 39' with a warm isostatic press (WIP) and forming terminals for the positive and negative electrodes, respectively.

[0100] In the all-solid-state secondary battery 40, insulating layers 38, 38' are disposed on both sides of the positive electrode layers 36, 36', the solid electrolyte layers 33, 33', and the negative electrode layers 37, 37', thereby making it possible to prevent short circuits, minimize initial capacity reduction, and improve life characteristics.

[0101] The present invention will be described in more detail with reference to the following examples and comparative examples, however, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention. EXAMPLES

[0102] Example 1: Polyvinylidene fluoride (PVdF) + Al 2 O 3 All-solid-state secondary battery with insulating layer (Negative electrode layer manufacturing) A 10 μm thick SUS foil was prepared as the negative electrode current collector, and carbon black (CB) with a primary average particle size (D50) of about 35 nm and silver (Ag) particles with an average diameter (D50) of about 60 nm were prepared as the negative electrode active material.

[0103] 4 g of mixed powder obtained by mixing carbon black (CB) and silver (Ag) particles at a weight ratio of 3:1 was placed in a container, and 4 g of N-methylpyrrolidone (NMP) solution containing 7 wt% of polyvinylidene fluoride (PVdF) binder (#9300 (Kureha)) was added thereto to prepare a mixed solution. Next, the mixed solution was stirred while adding NMP little by little to the mixed solution to prepare a slurry. The prepared slurry was applied to a SUS sheet using a doctor blade and dried in air at 60°C for 20 minutes. The laminate obtained by this was vacuum dried at 100°C for 12 hours to prepare a negative electrode layer. The thickness of the negative electrode active material layer of the Ag-C nanocomposite contained in the negative electrode layer was about 7 μm. The Ag volume ratio in the Ag-C nanocomposite was about 8 volume%, and the Ag content used in the battery production was about 12 mg / Ah.

[0104] (Positive electrode layer manufacturing) The positive electrode active material was LiNi coated with Li2O-ZrO2 (LZO). 0.8 Co 0.15 Mn 0.05O2 (NCM) was prepared. The LZO-coated positive active material was prepared by the method disclosed in Korean Patent Publication No. 10-2016-0064942. Argyrodite-type crystal Li6PS5Cl (D50=0.5μm, crystalline) was prepared as a solid electrolyte. Polytetrafluoroethylene (PTFE) binder (Teflon (registered trademark) binder (DuPont)) was prepared as a binder. Carbon nanofiber (CNF) was prepared as a conductive material. The material was mixed with xylene solvent in a weight ratio of positive active material: solid electrolyte: conductive material: binder = 85:15:3:1.5, and the mixture was formed into a sheet shape and dried in vacuum at 40 ° C for 8 hours to prepare a positive electrode sheet. The positive electrode sheet was pressed onto one side of a positive electrode current collector made of 18 μm thick carbon-coated aluminum foil to prepare a positive electrode layer. The thickness of the positive electrode layer was about 105 μm. The loading level of the positive electrode layer was about 6.8 mAh / cm2.

[0105] (Manufacturing of solid electrolyte layer) A mixture was prepared by adding 1 part by weight of an acrylic binder to 99 parts by weight of the solid electrolyte, Li6PS5Cl, which is an argyrodite-type crystal (D50=3.0 μm, crystalline). Xylene (FUJIFILM Wako Pure Chemical Corporation) and isobutyl isobutyrate (Aldrich) were added to the prepared mixture in a weight ratio of 50:50, and the mixture was stirred for 6 minutes at 2,000 rpm using a planetary centrifugal mixer (AR-100) to prepare a slurry. The prepared slurry was applied to a 75 μm-thick polyethylene terephthalate film using a doctor blade, and dried on a hot plate at a temperature of 50° C. for several minutes to obtain a laminate. The obtained laminate was vacuum-dried at 40° C. for 8 hours. A solid electrolyte layer was produced by the above process. The thickness of the solid electrolyte layer was about 40 μm, and was pressurized in the battery to make it about 30 μm.

[0106] (Slurry manufacturing for forming insulating layer) PVdF powder (#9300 (Kureha)) and Al2O3 powder (50 nm, Sigma Aldrich) were mixed in a weight ratio of 1:3, and 40 g of the mixed powder was placed in a container, to which acetone solvent was added to prepare a mixed solution. Next, the mixed solution was stirred while gradually adding acetone solvent to the mixed solution to produce a slurry for forming an insulating layer.

[0107] (Manufacturing all-solid-state secondary batteries) 3, a laminate was manufactured by disposing a solid electrolyte layer 33 on a negative electrode layer 37 such that the negative electrode active material layer 34 was in contact with the solid electrolyte layer 33, and disposing a positive electrode layer 36 on the solid electrolyte layer 33. The width margin of the solid electrolyte layer 33 was about 2%.

[0108] The produced insulating layer-forming slurry was integrally applied to both sides of a laminate composed of the negative electrode layer 37, the positive electrode layer 36, and the solid electrolyte layer 33 using a doctor blade, and then dried in air to produce an electrode structure provided with an insulating layer 38. The storage elastic modulus (E') of the insulating layer 38 was 6.471 GPa, and the loss tangent (tan δ) was 0.045.

[0109] The electrode structure with the insulating layers 38 on both sides was placed in a laminate bag and vacuum-sealed. Next, the vacuum-sealed electrode structure was pressurized with a hydrostatic press (WIP) at a pressure of 500 MPa. After that, the electrode structure was removed from the laminate bag, and the positive electrode Al terminal, the negative electrode, and the Ni terminal were welded using an ultrasonic welding machine, respectively. Next, the electrode structure with the protruding Al terminal and Ni terminal was placed in a laminate bag and further vacuum-sealed to manufacture an all-solid-state secondary battery 40.

[0110] Example 2: Cellulose + Glass Fiber + Al(OH) 3 All-solid-state secondary battery with insulating layer In the preparation of the slurry for forming the insulating layer, 30 g of a mixed powder obtained by adding nanocellulose (art clay, manufactured by Pinocchio Co., Ltd.), glass fiber (diameter = 2.7 μm, manufactured by Whatman Co., Ltd.), and Al(OH)3 powder (5 μm, manufactured by Sigma Aldrich Co., Ltd.) in a weight ratio of 1:1:1 was placed in a container, and purified water was added thereto and pulverized to prepare a slurry for forming the insulating layer. The slurry for forming the insulating layer was then dried at 100°C for 12 hours to form a sheet-shaped insulating layer, and the insulating layer was perforated in a "R" shape so as to have the same inner diameter as the solid electrolyte layer 33 of the laminate composed of the negative electrode layer 37, the positive electrode layer 36, and the solid electrolyte layer 33, and was arranged to surround the four sides of the laminate without any additional adhesion. An all-solid-state secondary battery 40 was prepared in the same manner as in Example 1. The storage elastic modulus (E') of the insulating layer 38 was 19.87 GPa, and the loss tangent (tan δ) was 0.024.

[0111] Example 3: All-solid-state secondary battery with an insulating layer of a three-layer structure of cellulose + epoxy resin + cellulose Instead of preparing a slurry for forming an insulating layer, 2 g of an epoxy adhesive (EP935, manufactured by Okong) was applied between two sheets of 60 μm thick cellulose paper to prepare a three-layer insulating layer structure in which cellulose, epoxy resin, and cellulose were arranged in this order, and the epoxy adhesive was used to fix the insulating layer structure to both sides of a laminate composed of the negative electrode layer 37, the positive electrode layer 36, and the solid electrolyte layer 33. An all-solid-state secondary battery 40 was manufactured in the same manner as in Example 1. The storage elastic modulus (E') of the insulating layer 38 was 39.63 GPa, and the loss tangent (tan δ) was 0.034.

[0112] Comparative Example 1: Polypropylene (PP) + ZrO 2 All-solid-state secondary battery with insulating layer Instead of preparing a slurry for forming an insulating layer, a polypropylene zirconia film (MKP1848C capacitor material (semi-finished product), manufactured by Vishay) having a thickness of about 230 μm was prepared, and a hole was formed in a square shape so as to have an inner diameter of the same size as the solid electrolyte layer 33 of the laminate composed of the negative electrode layer 37, the positive electrode layer 36, and the solid electrolyte layer 33, and the film was arranged to surround all four sides of the laminate without any additional adhesion. An all-solid-state secondary battery 40 was manufactured in the same manner as in Example 1. The storage elastic modulus (E') of the insulating layer 38 was 1.491 GPa, and the loss tangent (tan δ) was 0.098.

[0113] Comparative Example 2: All-solid-state secondary battery with PMMA insulating layer Instead of preparing a slurry for forming an insulating layer, a transparent polymethyl methacrylate (PMMA) film (manufactured by Sumitomo Chemical Co., Ltd.) having a thickness of 350 μm was prepared, and a hole was formed in a square shape so as to have an inner diameter of the same size as the solid electrolyte layer 33 of the laminate composed of the negative electrode layer 37, the positive electrode layer 36, and the solid electrolyte layer 33, and the film was arranged to surround all four sides of the laminate without any additional adhesive. An all-solid-state secondary battery 40 was manufactured in the same manner as in Example 1. The storage elastic modulus (E') of the insulating layer 38 was 2.520 GPa, and the loss tangent (tan δ) was 0.157.

[0114] Comparative Example 3: All-solid-state secondary battery with PTFE insulating layer Instead of preparing a slurry for forming an insulating layer, a 300 μm thick polytetrafluoroethylene (PTFE) film (Hypersheet, Goretech) was prepared, and perforated in a square shape to have the same inner diameter as the solid electrolyte layer 33 of the laminate composed of the negative electrode layer 37, the positive electrode layer 36, and the solid electrolyte layer 33, and was arranged to surround all four sides of the laminate without any additional adhesive. An all-solid-state secondary battery 40 was manufactured in the same manner as in Example 1. The storage elastic modulus (E') of the insulating layer 38 was 0.200 GPa, and the loss tangent (tan δ) was 0.198.

[0115] The materials constituting the insulating layers of the all-solid-state secondary batteries 40 manufactured in Examples 1 to 3 and Comparative Examples 1 to 3, and the storage elastic modulus (E'), storage inelastic modulus (E''), and loss tangent (tan δ(E'' / E')) of these materials are summarized and shown in Table 1 below. The storage elastic modulus (E') and storage inelastic modulus (E'') of the insulating layer materials were derived by dynamic mechanical analysis (DMS) using a sine wave form with a frequency of 1 Hz on a sample of 10 mm x 5 mm.

[0116] [Table 1]

[0117] Evaluation example 1: Charge / discharge test The charge / discharge characteristics of the all-solid-state secondary batteries produced in Examples 1 to 3 and Comparative Examples 1 to 3 were evaluated by the following charge / discharge test. The charge / discharge test was carried out by placing the all-solid-state secondary batteries in a thermostatic chamber at 45°C.

[0118] In the first cycle, the battery was charged at a constant current of 0.1 C until the battery voltage reached 4.25 V, after which it was changed to constant voltage charging and charged until the charging current reached 0.05 C. Next, the battery was discharged at a constant current of 0.1 C until the battery voltage reached 2.5 V.

[0119] Thereafter, the first cycle was repeated, and charging and discharging were repeated up to 50 cycles, and the capacity retention rate was calculated by the following Equation 1. The results of the initial capacity and the capacity retention rate are shown in the following Table 2 and FIG. 4. The initial capacity is the discharge capacity in the first cycle.

[0120] [Formula 1] Capacity retention rate (%) = [50th cycle discharge capacity / 1st cycle discharge capacity] x 100

[0121] [Table 2]

[0122] As can be seen from Table 1 and FIG. 4, the all-solid-state secondary batteries manufactured in Examples 1 to 3 had the same or improved initial capacity as the all-solid-state secondary batteries manufactured in Comparative Examples 1 to 3, and also had improved capacity retention rates.

[0123] From the above, it can be seen that the all-solid-state secondary batteries manufactured in Examples 1 to 3 include insulating layers having a storage elastic modulus of 6.471 GPa or more and a loss tangent of less than 0.045 on both sides of the electrode structure, and have a restoring force during charging and discharging while preventing the occurrence of initial short circuits, and are excellent in initial capacity and capacity retention rate. [Explanation of symbols]

[0124] 1,26,26',36,36' Positive electrode layer 2,23,23',33,33' solid electrolyte layer, 3,27,27',37,37' Negative electrode layer 4,28,28',38,38' Insulation layer 10,30 Electrode structure 21,31 Positive electrode current collector 22,22',32,32' Positive electrode active material layer 24,24',35,35' Negative electrode current collector 25,25',34,34' Negative electrode active material layer 39,39' Support member 40 All-solid-state secondary battery W: Extra width

Claims

1. An electrode structure including a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, the positive electrode layer includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, the negative electrode layer includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, the solid electrolyte layer has a margin of 2% or less of the width of the solid electrolyte layer at both ends in a width direction, The positive electrode layer, the negative electrode layer, and the solid electrolyte layer are integrally surrounded by insulating layers having a storage elastic modulus (E') of more than 4.0 GPa on both sides thereof, the insulating layer comprises a polymer or a composite of a polymer and an inorganic material; the polymer is a fluorine-based polymer, a cellulose-based polymer, or a combination thereof; The storage modulus (E') was derived by dynamic mechanical analysis (DMA) using a sinusoidal waveform at 1 Hz frequency on a sample of 10 mm x 5 mm size, electrode structure.

2. 2. The electrode structure of claim 1, wherein the insulating layer has a loss tangent (tan δ) of less than 0.

5.

3. The insulating layer is 1×10 6 2. The electrode structure of claim 1, having a resistivity of at least ohm / cm.

4. The electrode structure of claim 1 , wherein the insulating layer is at least one layer.

5. 2. The electrode structure according to claim 1, wherein in the composite of the polymer and the inorganic material, the volume ratio of the polymer is 50% by volume or more based on 100% by volume of the entire composite-forming composition.

6. The electrode structure of claim 1 , wherein the inorganic material comprises a metal oxide, a metal hydroxide, or a combination thereof.

7. 2. The electrode structure according to claim 1, wherein the positive electrode active material layer has a mixture density of 3.0 g / cc or more.

8. The electrode structure according to claim 1 , wherein the positive electrode active material layer comprises a sulfide-based solid electrolyte.

9. The electrode structure according to claim 1 , wherein the negative electrode active material layer comprises at least one selected from the group consisting of a carbon-based negative electrode active material, a metal negative electrode active material, and a semi-metal negative electrode active material.

10. The electrode structure according to claim 9 , wherein the carbon-based negative electrode active material comprises at least one selected from the group consisting of amorphous carbon and crystalline carbon.

11. 10. The electrode structure according to claim 9, wherein the metal negative electrode active material or the semi-metal negative electrode active material comprises one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn).

12. 2. The electrode structure according to claim 1, wherein the solid electrolyte layer comprises a sulfide-based solid electrolyte represented by the following chemical formula 1: [Chemical formula 1] Li + 12-n-x A n+ X 2- 6-x Y - x In the formula 1, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb or Ta; X is S, Se or Te, and Y is Cl, Br, I, F, CN, OCN, SCN or N 3 where 1≦x≦5 and 0≦n≦2.

13. 2. The electrode structure according to claim 1, wherein the solid electrolyte layer has an adhesive strength with the positive electrode layer or the negative electrode layer of 0.2 gf / mm or more.

14. The electrode structure of claim 1 , wherein the electrode structure is in a jelly roll or stack configuration.

15. 2. The electrode structure according to claim 1, wherein no cracks are generated in the electrode structure when the electrode structure is compressed in a thickness direction by 20 to 30% of its thickness.

16. An all-solid-state secondary battery comprising the electrode structure according to claim 1 .

Citation Information

Patent Citations

  • Whole solid battery and its manufacture

    JP2000106154A

  • Device and method for removing static electricity

    JP2005123150A

  • Solid-state secondary battery and manufacturing method of all-solid secondary battery

    JP2018206469A

  • All-solid battery

    JP2019153535A

  • Horizontal composite power-feeding structure

    JP2020024922A