Positive electrode plate for lithium ion secondary battery and lithium ion secondary battery
By integrating lithium carbonate and a controlled amount of fibrous conductive material into the positive electrode, the battery's durability and output are enhanced by preventing NiO formation and maintaining effective conductivity.
Patent Information
- Application Number
- JP2022101947
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-06-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-06-24
AI Technical Summary
Lithium ion secondary batteries face deterioration in high-temperature environments due to the formation of NiO, which reduces the amount of lithium ions available for the main reaction, leading to decreased battery capacity and life characteristics.
Incorporating a specific amount of lithium carbonate (0.31-1.29 wt%) and a fibrous conductive material (0.5-2.0 wt%) such as carbon nanotubes or nanofibers, with a coverage ratio of 11.0% or less, into the positive electrode active material to suppress NiO formation and maintain an effective conductive network.
The solution enhances battery durability and output characteristics by preventing NiO formation, ensuring a sufficient lithium ion supply and maintaining efficient conductivity, thereby improving the battery's life and performance.
Smart Images

Figure 0007581285000001 
Figure 0007581285000002 
Figure 0007581285000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode plate for a lithium ion secondary battery and a lithium ion secondary battery, and more particularly to an electrode plate for a lithium ion secondary battery and a lithium ion secondary battery having improved life characteristics. [Background technology]
[0002] Lithium ion secondary batteries have a large capacity and a high voltage, and are therefore used for in-vehicle applications such as electric vehicles and hybrid vehicles. They are also used as stationary batteries in homes and factories. Such lithium ion secondary batteries are required to have even higher output.
[0003] Therefore, an invention has been disclosed in which fibrous conductive materials such as carbon nanotubes (CNTs) and carbon nanofibers (CNFs) can form a conductive network between particles of positive electrode active material even in small amounts, thereby increasing the proportion of positive electrode active material in the positive electrode mixture layer.
[0004] For example, Patent Document 1 discloses a lithium ion secondary battery in which fine carbon fibers are attached in a mesh pattern to the particle surfaces of the positive and negative active materials, and all or part of the fibers are modified with hydrophilic groups. In Patent Document 2, a surfactant made of a fibrous carbon material such as carbon nanotubes is fixed to the surface of the conductive material to prevent secondary aggregation of the conductive material and capture the binder, thereby preventing the conductive material from agglomerating with the positive and negative electrode materials. Some positive electrode mixture layers as disclosed in Patent Document 1 and Patent Document 2 contain fibrous conductive materials such as carbon nanotubes. By adopting such a configuration, the fibrous conductive material forms a conductive path. This ensures excellent battery performance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2009-272041 A [Patent Document 2] JP 2015-519699 A Summary of the Invention [Problem to be solved by the invention]
[0006] As described above, the carbon nanotubes and the like increase the battery capacity, and the formed conductive paths increase the reaction area, reducing reaction resistance and improving input and output.
[0007] However, because the contact surface area between the positive electrode active material and the non-aqueous electrolyte increases, NiO2, which acts as a counter when the electrolyte decomposes during energization or storage in a high-temperature environment, can be reduced and decomposed to produce NiO. The production of NiO causes the battery to deteriorate and reduces the life characteristics, which is a problem.
[0008] The problem to be solved by the positive electrode plate for a lithium ion secondary battery and the lithium ion secondary battery of the present invention is to improve the life characteristics of the lithium ion secondary battery. [Means for solving the problem]
[0009] In order to solve the above problems, the positive electrode plate for a lithium ion secondary battery of the present invention is characterized in that, in a positive electrode composite layer of the positive electrode plate of a lithium ion secondary battery, a positive electrode active material in which the amount of lithium carbonate relative to the positive electrode active material is 0.31 [wt%] or more and 1.29 [wt%] or less, is combined with a fibrous conductive material, the composition ratio of the fibrous conductive material to the positive electrode active material is 0.5 [wt%] or more and 2.0 [wt%] or less, and the coverage rate of the fibrous conductive material with respect to the positive electrode active material is 11.0 [%] or less.
[0010] The positive electrode active material has the chemical formula LiNi x Co y M zIt is represented by O2. When M represents one or more metals selected from the group consisting of Fe, Cu, Ti, Mg, Al, W, B, Mo, Nb, Zn, Sn, Zr, Ga, and V, the composition ratio of Li / M is preferably 1.15 or more and 1.21 or less.
[0011] Further, when M represents one or more metals selected from the group consisting of Fe, Cu, Ti, Mg, Al, W, B, Mo, Nb, Zn, Sn, Zr, Ga, and V, the positive electrode active material has the chemical formula LiNi x Co y M z It is represented by O2, x = 1 - y - z, and it is also preferable that 0 < x ≤ 0.5, 0.2 ≤ y ≤ 0.5, y + z ≥ 0.5, and y / x ≥ 0.98.
[0012] Further, in this case, it is preferable that x ≤ 0.37. The fibrous conductive material may be made of carbon nanotubes or carbon nanofibers. In this case, the length of the fibrous conductive material is preferably 100 [nm] to 1000 [nm].
[0013] The lithium ion secondary battery of the present invention is characterized by using the positive electrode plate for a lithium ion secondary battery described above.
Effects of the Invention
[0014] The problem to be solved by the positive electrode plate for the lithium ion secondary battery 1 and the lithium ion secondary battery of the present embodiment is to improve the life characteristics of the lithium ion secondary battery.
Brief Description of the Drawings
[0015] [Figure 1] It is a perspective view showing an outline of the configuration of the lithium ion secondary battery of the present embodiment. [Diagram 2] It is a schematic diagram showing the configuration of the wound electrode body of the present embodiment. [Diagram 3] It is a schematic diagram showing a positive electrode with less lithium carbonate. [Figure 4] It is a schematic diagram showing the deterioration state of a positive electrode with a small amount of lithium carbonate. [Diagram 5] It is a schematic diagram showing a positive electrode in which a sufficient amount of lithium carbonate is present. [Figure 6] It is a schematic diagram of a state in which deterioration is suppressed in a positive electrode in which a sufficient amount of lithium carbonate is present. [Figure 7] It is a table of experimental examples showing the relationship between the total carbon amount TC [wt%] and the durability characteristics [%]. [Figure 8] It is a graph showing the relationship between the total carbon amount TC [wt%] and the durability characteristics [%]. [Figure 9] It is a table of experimental examples showing the relationship between the CNT coating rate [%] and the output characteristics [%]. [Figure 10] It is a graph showing the relationship between the CNT coating rate [%] and the output characteristics [%].
Embodiments for Carrying Out the Invention
[0016] An electrode plate for a lithium-ion secondary battery and a lithium-ion secondary battery according to the present invention will be described with reference to FIGS. 1 to 10 according to an embodiment. (Overview of this Embodiment) <Fibrous conductive material 32b> As described in the prior art, since carbon nanotubes or the like are used as the fibrous conductive material 32b, the battery capacity can be increased, and due to the formed conductive path, the reaction resistance can be reduced by an increase in the reaction area, and the input / output can be improved.
[0017] <Generation of NiO> However, in a high-temperature environment during energization or storage, NiO may be generated during electrolyte decomposition. When NiO is generated, there is a problem that the deterioration of the battery progresses.
[0018] The present inventors have conducted extensive analysis of the cause. As a result, as shown in Fig. 4, the contact area between the positive electrode active material 32a and the nonaqueous electrolyte 13 increases, so that the electrolyte is decomposed due to a temperature rise during current application or storage, and the positive electrode active material 32a is easily reduced and decomposed as a counter. At this time, NiO that does not contribute to the main reaction is generated by the reaction of NiO2 → NiO + 0.5O2.
[0019] When NiO is produced, a structure caused by NiO is formed in the positive electrode active material 32a having a so-called layered rock salt structure. Therefore, the lithium ions (L + However, they found that this hinders the intercalation of ZnO, reducing the amount of electrons available for the main reaction.
[0020] Therefore, the present inventors focused on lithium carbonate 32c (Li2CO3), which was originally recognized by those skilled in the art as an impurity that should be excluded during the production of a positive electrode active material. As shown in Figure 6, the presence of a certain amount of lithium carbonate 32c acts as a so-called counter, and the reaction ROCO2R'+Li2CO3→ROLi+R'OLi+2CO2 (R and R' are substituents) occurs, and it has been found that this can suppress the production of NiO.
[0021] <About lithium carbonate> Lithium carbonate has been conventionally recognized by those skilled in the art as an impurity in positive electrode active materials that reduces battery capacity, and as a component that should be removed at high temperatures during the firing step of the positive electrode active material.
[0022] Meanwhile, in light of this awareness, the prior art also discloses an invention for a non-aqueous secondary battery in which the positive electrode active material contains lithium carbonate. For example, JP 2002-313340 A discloses the following invention. In the case where the positive electrode active material contains lithium carbonate, if the battery is overcharged, the lithium carbonate contained in the positive electrode active material is electrochemically decomposed to generate carbon dioxide gas. This reliably activates the current interrupt mechanism, thereby interrupting the charging current and preventing a rapid temperature rise in the battery. This ensures the safety of the battery. However, in this invention, lithium carbonate generates carbon dioxide gas, and there was no recognition that it inhibits the production of NiO.
[0023] In addition, JP 2018-172255 A discloses the following invention. In order to achieve high output, a positive electrode active material is used in which the Li / Me ratio is 1.00 to 1.20 and the amount of sulfate + lithium carbonate residue is 0.3 [wt%] or less. When the residue is all Li carbonate, the amount is Li2CO3≦0.3 [wt%].
[0024] The positive electrode active material has the chemical formula LiNi( 1-y-z-w )Co y Mn z M w It is represented as O2. Also, the condition is 0 <y≦0.5、0<z≦0.8、0≦w≦0.1、y+z+w<1.0である。
[0025] However, in this invention, there is a concern that the active surface in contact with the electrolyte increases due to an increase in the ratio of the positive electrode active material, and the active material itself may be subject to a reduction reaction and may be easily deteriorated during storage or current flow. Therefore, the amount of lithium carbonate is rather limited, and is an extremely small amount compared to the content of lithium carbonate in this embodiment, and there was no recognition that lithium carbonate suppresses the generation of NiO.
[0026] <First condition of this embodiment> In the positive electrode active material 32a in the positive electrode mixture layer 32 of the positive electrode plate 3 of the lithium ion secondary battery 1 of this embodiment, the amount of lithium carbonate 32c relative to the positive electrode active material 32a is set to 0.31 [wt %] or more and 1.29 [wt %] or less.
[0027] By allowing a certain amount of lithium carbonate 32c to exist, it becomes a counter (ROCO2R'+Li2CO3→ROLi+R'OLi+2CO2, etc.) in place of the positive electrode active material 32a when the electrolyte decomposes.
[0028] Here, examples of the nonaqueous electrolyte 13 in this embodiment include ethylene carbonate (EC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), etc. Examples of the side chains -R and -R' include -CH3, -C2H5, -C3H6O, -C2H3, and -SO2CH3.
[0029] By setting the amount of lithium carbonate 32c to be 0.05 [wt%] or more and 0.21 [wt%] in terms of carbon (hereinafter referred to as "total carbon amount TC"), the amount of lithium carbonate relative to the positive electrode active material 32a can be set to be 0.31 [wt%] or more and 1.29 [wt%] or less.
[0030] Here, the amount of lithium carbonate required can be calculated from the total carbon amount TC by the following formula. Amount of lithium carbonate = Total amount of carbon TC × (molecular weight of lithium carbonate / atomic weight of carbon) = Total carbon amount TC × (73.893 / 12.011) ≒Total carbon amount TC x 6.152 <Conductive materials> As described above, the fibrous conductive material 32b such as carbon nanotubes (CNTs) and carbon nanofibers (CNFs) can form an efficient conductive network even with a small mass. This increases the battery capacity, and the formed conductive path reduces the reaction resistance by increasing the reaction area, thereby improving input and output.
[0031] For this purpose, in this embodiment, the length of the fibrous conductive material 32b is set to be 100 nm or more and 1000 nm or less. However, no matter how much the conductivity is increased, the main reaction of the positive electrode plate 3 of the lithium ion secondary battery 1 basically occurs mainly on the surface of the positive electrode active material 32a. Therefore, the presence of excess fibrous conductive material 32b overcoats the surface of the positive electrode active material 32a, and ends up restricting the main reaction of the positive electrode active material 32a.
[0032] Here, the ratio of the area of the surface of the positive electrode active material 32a covered by the carbon nanotubes (CNTs) of the fibrous conductive material 32b is defined as the CNT coverage θ [%] (or the “coverage θ [%]”). The coverage θ [%] in this embodiment is theoretically derived.
[0033] <Second condition of this embodiment> Therefore, in this embodiment, the amount of fibrous conductive material 32b is set to a composition ratio of 0.5 wt% to 2.0 wt% relative to positive electrode active material 32a in order to ensure that the amount of fibrous conductive material 32b is necessary and sufficient.
[0034] <Third condition of this embodiment> Specifically, the coverage θ [%] of the fibrous conductive material 32b with respect to the positive electrode active material 32a is set to be 11.0 [%] or less. If the coverage θ [%] exceeds 11.0 [%], the excess fibrous conductive material 32b will over-cover the surface of the positive electrode active material 32a, and will instead limit the main reaction of the positive electrode active material 32a.
[0035] <Condition 1 for the positive electrode active material 32a> An example of the positive electrode active material 32a in this embodiment is represented by the chemical formula LiNi x Co y M z O2, where "M" represents one or more metals selected from the group consisting of Fe, Cu, Ti, Mg, Al, W, B, Mo, Nb, Zn, Sn, Zr, Ga, and V. The Li / M composition ratio is set to 1.15 or more and 1.21 or less.
[0036] The reason for setting the Li / M composition ratio to 1.15 or more is to ensure a sufficient amount of lithium ions. Setting it to 1.21 or less is to enhance the battery stability. <Condition 2 for the positive electrode active material 32a> Also, in this embodiment, for the chemical formula LiNi x Co y M z in O2 (a) x = 1 - y - z, that is, the total of Ni, Co, and M is 100 [mol%].
[0037] (b) 0 < x ≤ 0.5, that is, Ni is 50 [mol%] or less. (c) 0.2 ≤ y ≤ 0.5, that is, Co is 20 - 50 [mol%]. (d) y + z ≥ 0.5, that is, as can be seen from (a) and (b) above, the total of Co and M is 50 [mol%] or more.
[0038] (e) y / x ≥ 0.98, that is, Co is contained more than 98 [mol%] of Ni. In particular, preferably, (b’) x satisfies x ≤ 0.37. The reason for this is that when the composition ratio of Ni is high, due to cation mixing, Ni enters the positions where Li should originally be arranged in the positive electrode active material 32a, causing Ni-derived deterioration where the amount of Li decreases.
[0039] Also, when a large amount of NiO is generated, a structure caused by NiO is formed in the so-called layered rock salt structure positive electrode active material 32a. For this reason, it hinders the intercalation of lithium ions (L + ) used in the main reaction, causing Ni-derived deterioration where the amount of electrons used in the main reaction decreases.
[0040] In addition, when the ratio of x (Ni) is low and the ratio of y (Co) is high, the total carbon content TC is generally 0.04 or less. The reason is that the reaction rate with Li is low for Ni and high for Co, making it easier to incorporate Li into the crystal. For this reason, Co is set to be 20 to 50 mol%.
[0041] (Configuration of this embodiment) The overall configuration of the lithium ion secondary battery 1 having the above-mentioned characteristics will now be briefly described. <Configuration of lithium-ion secondary battery 1> 1 is a perspective view showing the outline of the configuration of a lithium ion secondary battery 1 according to the present embodiment. Next, the configuration of the lithium ion secondary battery 1 according to the present embodiment will be described.
[0042] As shown in FIG. 1, the lithium ion secondary battery 1 is configured as a cell battery. The lithium ion secondary battery 1 includes a rectangular parallelepiped battery case 11 having an opening on the upper side. An electrode body 12 is housed inside the battery case 11. A nonaqueous electrolyte 13 is filled into the battery case 11 through a filling hole. The battery case 11 is made of a metal such as an aluminum alloy, and forms a sealed battery container. The lithium ion secondary battery 1 also includes a positive electrode external terminal 14 and a negative electrode external terminal 15 used for charging and discharging power. The shapes of the positive electrode external terminal 14 and the negative electrode external terminal 15 are not limited to those shown in FIG. 1.
[0043] <Electrode body 12> 2 is a schematic diagram showing the configuration of a wound electrode assembly 12. The electrode assembly 12 is formed by winding a large number of negative electrode plates 2 and positive electrode plates 3, with separators 4 arranged between them, flatly. The negative electrode plates 2 have a negative electrode composite layer 22 formed on a negative electrode current collector 21 that serves as a base material. A negative electrode connection part 23 is provided at one end in a width direction W (winding axis direction) perpendicular to the winding direction (winding direction L), where the negative electrode composite layer 22 is not formed and the negative electrode current collector 21 is exposed.
[0044] <Layer structure of electrode body 12> 3 is a schematic partial cross-sectional view showing the laminated configuration of the electrode body 12 of the lithium-ion secondary battery 1. As shown in FIG. 2, the electrode body 12 of the lithium-ion secondary battery 1 basically comprises a negative electrode plate 2, a positive electrode plate 3, and a separator 4.
[0045] The negative electrode plate 2 includes a negative electrode mixture layer 22 on both sides of a negative electrode current collector 21 serving as a negative electrode base material. One end of the negative electrode current collector 21 serves as a negative electrode connection portion 23 where the metal is exposed. The positive electrode plate 3 includes a positive electrode mixture layer 32 on both sides of a positive electrode current collector 31 serving as a positive electrode base material. The other end of the positive electrode current collector 31 serves as a positive electrode connection portion 33 where the metal is exposed.
[0046] The negative electrode plate 2 and the positive electrode plate 3 are stacked with a separator 4 interposed therebetween to form a laminate. This laminate is wound in the longitudinal direction around a winding axis, and formed into a flat wound electrode body 12.
[0047] <Nonaqueous electrolyte 13> As shown in FIG. 1, the nonaqueous electrolyte 13 is filled in a battery container formed by a battery case 11. The nonaqueous electrolyte 13 of the lithium ion secondary battery 1 is a composition in which a lithium salt is dissolved in an organic solvent. Examples of the lithium salt that can be used include LiClO4, LiPF6, LiAsF6, LiBF4, and LiSO3CF3. Examples of the organic solvent include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, and trifluoropropylene carbonate (F.PC), chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and dipropyl carbonate (DPC), ether compounds such as tetrahydrofuran (TFH), 2-methyltetrahydrofuran (2-MeTHF), and dimethoxyethane, sulfur compounds such as ethyl methyl sulfone and butane sultone, and phosphorus compounds such as triethyl phosphate and trioctyl phosphate. The nonaqueous electrolyte solution may be one of these or a mixture of a plurality of types. The composition of the nonaqueous electrolyte solution 13 is not limited to these.
[0048] <Components of electrode body 12> Next, the negative electrode plate 2, the positive electrode plate 3, and the separator 4, which are the components that make up the electrode assembly 12, will be described.
[0049] In this embodiment, the "average diameter" refers to the median diameter (D 50 Average particle size (50% volume average particle size) refers to the average particle size in the range of approximately 1 μm or more, which can be determined by the laser diffraction / light scattering method. In addition, average particle size in the range of approximately 1 μm or less can be determined by the dynamic light scattering (DLS) method. The average particle size based on the DLS method can be measured in accordance with JIS Z 8828:2013.
[0050] <Negative electrode plate 2> The negative electrode plate 2 is constituted by forming a negative electrode mixture layer 22 on both sides of a negative electrode current collector 21, which is a negative electrode base material. In this embodiment, the negative electrode current collector 21 is made of Cu foil. The negative electrode current collector 21 serves as a base for the aggregate of the negative electrode mixture layer 22, and also functions as a current collecting member that collects electricity from the negative electrode mixture layer 22. In this embodiment, the negative electrode active material is a material capable of absorbing and releasing lithium ions, and a powdered carbon material made of graphite or the like is used.
[0051] The negative electrode plate 2 is produced, for example, by kneading a negative electrode active material, a solvent, and a binding agent (binder), applying the kneaded negative electrode mixture paste to the negative electrode current collector 21, and drying it. <Positive electrode plate 3> The positive electrode plate 3 is composed of a positive electrode current collector 31 and a positive electrode mixture layer 32 applied thereto.
[0052] <Positive electrode current collector 31> A positive electrode mixture layer 32 is formed on both sides of a positive electrode current collector 31, which is a positive electrode base material, to form a positive electrode plate 3. In this embodiment, the positive electrode current collector 31 is made of an Al foil. The positive electrode current collector 31 serves as a base for the aggregate of the positive electrode mixture layer 32, and also functions as a current collecting member that collects electricity from the positive electrode mixture layer 32.
[0053] First, the positive electrode base material constituting the positive electrode current collector 31 is exemplified as an Al foil, but may be made of a conductive material made of a metal having good conductivity. As the conductive material, for example, a material containing aluminum or a material containing an aluminum alloy may be used. The configuration of the positive electrode current collector 31 is not limited to this.
[0054] <Positive electrode mixture layer 32> Positive electrode mixture layer 32 is formed by applying a positive electrode mixture paste to positive electrode current collector 31 and drying it. Positive electrode mixture layer 32 contains, in addition to positive electrode active material 32a, fibrous conductive material 32b, binder 32d, and additives such as a dispersant.
[0055] <Composition of Positive Electrode Active Material 32a> The primary particles of the positive electrode active material 32a contain a lithium transition metal oxide having a layered crystal structure, without being limited to those exemplified in the above embodiment. The lithium transition metal oxide contains one or more predetermined transition metal elements in addition to Li. The transition metal element contained in the lithium transition metal oxide is preferably at least one of Ni, Co, and Mn. A suitable example of the lithium transition metal oxide is a lithium transition metal oxide containing all of Ni, Co, and Mn.
[0056] The positive electrode active material 32a may contain one or more additional elements in addition to a transition metal element (i.e., at least one of Ni, Co, and Mn). The additional elements may include any of elements belonging to Group 1 (alkali metals such as sodium), Group 2 (alkaline earth metals such as magnesium and calcium), Group 4 (transition metals such as titanium and zirconium), Group 6 (transition metals such as chromium and tungsten), Group 8 (transition metals such as iron), Group 13 (metalloid element boron or metals such as aluminum), and Group 17 (halogens such as fluorine) of the periodic table.
[0057] <Fibrous conductive material 32b> The fibrous conductive material 32b is a material for forming a conductive path in the positive electrode mixture layer 32. By mixing an appropriate amount of a conductor into the positive electrode mixture layer 32, the conductivity inside the positive electrode can be increased, and the charge / discharge efficiency and output characteristics of the battery can be improved. As the conductor of this embodiment, for example, a fibrous conductive material 32b made of a carbon material such as carbon nanotube (CNT) or carbon nanofiber (CNF) can be used. In addition, it is desirable to use a string-like material with an aspect ratio of length to diameter of 30 or more. The length is preferably 100 [nm] or more and 1000 [nm]. If it is less than 100 [nm], a sufficient conductive network cannot be formed. If it exceeds 1000 [nm], it becomes difficult to disperse.
[0058] <Binding material 32d> For example, polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyacrylic acid, polyacrylate, or the like can be used for the binder 32d.
[0059] (Action of this embodiment) Next, the operation of the lithium ion secondary battery 1 of this embodiment configured as described above will be described with reference to FIGS.
[0060] 3 is a schematic diagram showing a positive electrode with a small amount of lithium carbonate 32c. Specifically, the total carbon amount TC, which is an index of lithium carbonate 32c, is set to 0.05 [wt%], and the coverage θ [%] of the fibrous conductive material 32b with respect to the positive electrode active material 32a is set to 11.0 [%] or less.
[0061] FIG. 4 is a schematic diagram showing the deterioration state of the positive electrode with a small amount of lithium carbonate 32c. When the nonaqueous electrolyte 13 of the lithium ion secondary battery 1 reaches a high temperature where electrolysis occurs due to charging / discharging, micro-short circuiting, or environmental temperature, ROCO2R' decomposes to become ROLi+R'OLi+2CO2. However, at high temperatures, the reaction NiO2→NiO+0.5O2 occurs to produce NiO. This NiO causes deterioration as described above. That is, the amount of Li in the positive electrode active material 32a decreases, and the battery capacity decreases. In addition, NiO increases the internal resistance (C-D).
[0062] FIG. 5 is a schematic diagram showing a positive electrode in which a sufficient amount of lithium carbonate 32c is present. Compared with FIG. 3, in FIG. 5, lithium carbonate 32c is shown as a number of white circles. The total carbon amount TC, which is an index of lithium carbonate 32c, is set to be as large as 0.05 [wt%]≦TC≦0.21 [wt%]. In addition, the coverage θ [%] of the fibrous conductive material 32b with respect to the positive electrode active material 32a is set to be 11.0 [%] or less, as in FIG. 3.
[0063] FIG. 6 is a schematic diagram of a state in which deterioration is suppressed in a positive electrode in which a sufficient amount of lithium carbonate 32c is present. As in FIG. 4, when the nonaqueous electrolyte 13 of the lithium ion secondary battery 1 becomes high enough to cause electrolysis due to charging / discharging, micro-short circuiting, or environmental temperature, ROCO2R' decomposes. At this time, the lithium carbonate 32c (Li2CO3) acts as a counter, causing the reaction Li2CO3→2Li+0.5O2+CO2, suppressing the reaction NiO2→NiO+0.5O2. That is, Li2CO3 contributes to the reductive decomposition reaction instead of the active material NiO2. In this way, by setting the total carbon amount TC, which is an index of the lithium carbonate 32c, to a predetermined amount, the capacity is improved by the fibrous conductive material 32b made of CNT, and the input / output is improved. At the same time, it is possible to suppress the deterioration of the positive electrode active material 32a, NiO2, to NiO during the oxidative decomposition of the nonaqueous electrolyte 13.
[0064] (Experimental Example of the Present Embodiment) <Experiment 1: TC [wt%] and durability [%]> 7 is a table of an experimental example showing the relationship between the total carbon amount TC [wt%] and durability characteristics [%]. Here, since carbon (C) in the "total carbon amount TC" is mainly derived from lithium carbonate 32c (Li2CO3), in this embodiment, the amount of lithium carbonate 32c is controlled using the amount converted to carbon as an index. In the first condition, by setting the total carbon amount TC to 0.05 [wt%] or more and 0.21 [wt%], the amount of lithium carbonate 32c relative to the positive electrode active material 32a can be set to 0.31 [wt%] or more and 1.29 [wt%] or less.
[0065] Example 1: The total carbon content TC is 0.08 [wt%], which satisfies the first condition. Ni is 35.3 [mol%], Co is 35.0 [mol%], Mn is 29.7 [mol%], and the active material D 50 was set to 4.2 [wt%]. The amount of CNT in the electrode plate was 0.8 [wt%], which satisfied the second condition. The CNT coverage rate θ was 9.4 [%], which satisfied the third condition. The durability characteristics at this time were set to 100 [%]. The "durability characteristics" are determined by the amount of charge and discharge [Wh] until the battery capacity reaches the set threshold value.
[0066] Example 2: The total carbon content TC is 0.14 [wt%], which satisfies the first condition. Ni is 35.2 [mol%], Co is 35.0 [mol%], Mn is 29.8 [mol%], and the active material D 50 was set to 3.9 [wt%]. The amount of CNT in the electrode plate was 0.8 [wt%], which satisfied the second condition. The CNT coverage rate θ was 8.8 [%], which satisfied the third condition. The durability characteristic at this time was 95.8 [%].
[0067] Example 3: The total carbon content TC is 0.21 [wt%], which satisfies the first condition. Ni is 35.2 [mol%], Co is 35.0 [mol%], Mn is 29.8 [mol%], and the active material D 50was set to 3.9 [wt%]. The amount of CNT in the electrode plate was 0.8 [wt%], which satisfied the second condition. The CNT coverage rate θ was 8.8 [%], which satisfied the third condition. The durability characteristic at this time was 91.4 [%].
[0068] Comparative Example 1: The total carbon content TC is 0.04 [wt%], which does not satisfy the first condition. Ni is 35.1 [mol%], Co is 35.0 [mol%], Mn is 29.9 [mol%], and active material D 50 was set to 3.9 [wt%]. The amount of CNT in the electrode plate was 0.8 [wt%], which satisfied the second condition. The CNT coverage rate θ was 8.8 [%], which satisfied the third condition. The durability characteristic at this time was 84.5 [%].
[0069] Reference Example 1: The total carbon content TC is 0.03 [wt%], which does not satisfy the first condition. Ni is 37.8 [mol%], Co is 32.3 [mol%], Mn is 29.8 [mol%], and active material D 50 was set to 5 wt%. The amount of CNT in the electrode plate was 1 wt%, which satisfied the second condition. The CNT coverage θ was 13.4%, which did not satisfy the third condition. The durability characteristic at this time was 70.2%.
[0070] <Summary of Experiment 1> Fig. 8 is a graph plotting the relationship between the total carbon amount TC [wt%] and the durability [%] shown in Fig. 7. Plot point P1 is a plot of the total carbon amount TC [wt%] and the durability [%] of Reference Example 1. Similarly, plot point P2 corresponds to Comparative Example 1, plot point P3 corresponds to Example 1, plot point P4 corresponds to Example 2, and plot point P5 corresponds to Example 3. Graph L1 is a graph obtained based on these plot points, including plot points other than the exemplified plot points P1 to P5.
[0071] In this embodiment, the plot point P1 of Reference Example 1 does not satisfy the first condition, and the durability characteristic [%] is low at 70.2 [%]. The plot point P2 of Comparative Example 1 also does not satisfy the first condition, and the durability characteristic [%] is 84.5 [%], which is smaller than the value set in this embodiment. The plot point P3 of Example 1 satisfies the first condition, and the durability characteristic [%] is almost the peak value, 100 [%]. The plot point P4 of Example 2 satisfies the first condition, and the durability characteristic [%] is 95.4 [%], which is close to Example 1. The plot point P5 of Example 3 also satisfies the first condition, and the durability characteristic [%] is 91.4 [%], which is a value that is almost satisfactory as a product.
[0072] From these experimental results, graph L1 was derived by multiple regression analysis. From this graph L1, the total carbon content TC [wt%] that can be expected to achieve approximately 90% durability [%] is 0.05% or more and 0.21% or less, and this was set as the first condition.
[0073] <Experiment 2: CNT coverage θ [%] and output characteristics [%]> Fig. 9 is a table of an experimental example showing the relationship between the CNT coverage θ [%] and the output characteristics [%]. In the third condition, the coverage θ [%] of the fibrous conductive material 32b with respect to the positive electrode active material 32a is set to 11.0 [%] or less. In experiment 2, the output characteristics [%] were measured for this coverage θ [%]. The output characteristics are determined by the battery capacity [Wh].
[0074] Example 4: The total carbon content TC is 0.08 [wt%], which satisfies the first condition. Ni is 35.0 [mol%], Co is 35.0 [mol%], Mn is 30.0 [mol%], and active material D 50 was set to 3.6 [wt%]. The amount of CNT in the electrode plate was 0.8 [wt%], which satisfied the second condition. The CNT coverage θ [%] was 8.2 [%], which satisfied the third condition. The output characteristics at this time were set to 100 [%].
[0075] Example 5: The total carbon content TC is 0.08 [wt%], which satisfies the first condition. Ni is 35.3 [mol%], Co is 35.0 [mol%], Mn is 29.7 [mol%], and the active material D 50 was set to 4.2 [wt%]. The amount of CNT in the electrode plate was 0.8 [wt%], which satisfied the second condition. The CNT coverage rate θ [%] was 9.4 [%], which satisfied the third condition. The output characteristics at this time were 98.8 [%].
[0076] Example 6: The total carbon content TC was 0.04 [wt%], which slightly did not satisfy the first condition. Ni was 35.1 [mol%], Co was 35.0 [mol%], Mn was 29.9 [mol%], and the active material D 50 was set to 3.9[wt%]. The amount of CNT in the electrode plate was 1[wt%], which satisfied the second condition. The CNT coverage θ[%] was 11.1[%], which just did not satisfy the third condition. The output characteristics at this time were 94.6[%].
[0077] Comparative Example 2: The total carbon content TC is 0.07 wt%, which satisfies the first condition. Ni is 35.1 mol%, Co is 32.0 mol%, Mn is 33.0 mol%, and the active material D 50 was set to 4.5 [wt%]. The amount of CNT in the electrode plate was 1 [wt%], which satisfied the second condition. The CNT coverage θ was 12.4 [%], which did not satisfy the third condition. The output characteristics at this time were 74.1 [%].
[0078] Reference Example 2: The total carbon content TC is 0.03 [wt%], which does not satisfy the first condition. Ni is 37.8 [mol%], Co is 32.3 [mol%], Mn is 29.8 [mol%], and the active material D 50 was set to 5 [wt%]. The amount of CNT in the electrode plate was 1 [wt%], which satisfied the second condition. The CNT coverage θ [%] was 13.4 [%], which did not satisfy the third condition. The output characteristics at this time were 55.4 [%].
[0079] <Summary of Experiment 2> Fig. 10 is a graph plotting the relationship between the CNT coverage θ [%] and the output characteristics [%] shown in Fig. 9. Plot point P6 is a plot of the CNT coverage θ [%] and the output characteristics [%] of Example 4. Similarly, plot point P7 corresponds to Example 5, plot point P8 corresponds to Example 6, plot point P9 corresponds to Comparative Example 2, and plot point P10 corresponds to Reference Example 2. Graph L2 is a graph obtained by multiple regression analysis based on these plot points, including plot points other than the illustrated plot points P6 to P10.
[0080] As can be seen from graph L2, Example 4, in which the CNT coverage θ [%] is 8.2 [%], is used as the standard for the output characteristics [%]. In this case, when the CNT coverage θ [%] is 11.0 [%], the output characteristics [%] is approximately 95 [%], and this range is acceptable as the standard set for the product in this embodiment. Therefore, in this embodiment, the third condition is set so that the coverage θ [%] of the fibrous conductive material 32b with respect to the positive electrode active material 32a is 11.0 [%] or less.
[0081] A preferable coverage θ [%] of the fibrous conductive material 32b on the positive electrode active material 32a can be theoretically derived, for example, from the following (Equation 1). Here, "a [%]" is the composition ratio of the fibrous conductive material 32b to the positive electrode active material 32a, and is preferably 0.5 [wt%] or more and 2.0 [wt%] or less. "b [%]" is the coverage θ [%] of the fibrous conductive material 32b. "c [μm]" is the D of the positive electrode active material 32a. 50 The average diameter [μm] of the particles is preferably 2.5 μm or more and 5.5 μm or more.
[0082] b=-8.583+(a×11.63)+(c×2.07)≦11.0…(Formula 1) (Effects of this embodiment) (1) According to the positive electrode plate 3 for the lithium ion secondary battery 1 of this embodiment, there is an effect that the durability characteristics of the lithium ion secondary battery 1 can be improved.
[0083] (2) The amount of lithium carbonate 32c in the positive electrode active material 32a is 0.31 wt% or more and 1.29 wt% or less. The positive electrode active material 32a is combined with the fibrous conductive material 32b. This has the effect of suppressing the generation of NiO by the lithium carbonate 32c. In addition, the fibrous conductive material 32b has the effect of constructing an effective conductive network even with a small amount.
[0084] (3) The composition ratio of fibrous conductive material 32b to positive electrode active material 32a is set to 0.5 wt % or more, which has the effect of ensuring a sufficient amount of fibrous conductive material 32b for constructing a conductive network.
[0085] (4) The fibrous conductive material 32b is made of carbon nanotubes (CNTs) or carbon nanofibers (CNFs) and has a length of 100 nm to 1000 nm. This has the effect of enabling the fibrous conductive material 32b to construct an effective conductive network.
[0086] (5) The composition ratio of fibrous conductive material 32b to positive electrode active material 32a is set to 2.0 wt% or less, and the coverage θ of the fibrous conductive material to positive electrode active material 32a is set to 11.0% or less. This has the effect that fibrous conductive material 32b itself does not interfere with the main reaction of positive electrode active material 32a.
[0087] (6) The positive electrode active material 32a has the chemical formula LiNi x Co y M z O2. Here, M represents one or more metals selected from the group consisting of Fe, Cu, Ti, Mg, Al, W, B, Mo, Nb, Zn, Sn, Zr, Ga, and V. At this time, the Li / M composition ratio is set to 1.15 or more and 1.21 or less. This ensures a sufficient amount of lithium and stabilizes the performance of the battery.
[0088] (7) The positive electrode active material 32a has the chemical formula LiNi x Co y M zIn O2, x = 1 - y - z, and 0 < x ≤ 0.5, and 0.2 ≤ y ≤ 0.5, and y + z ≥ 0.5, and y / x ≥ 0.98. Particularly preferably, x ≤ 0.37. Therefore, by suppressing the amount of Ni and ensuring the amount of Co, the capacity of lithium ions in the positive electrode can be increased, and the deterioration derived from Ni such as cation mixing and the formation of a rock salt structure can be effectively suppressed.
[0089] (8) In the lithium ion secondary battery 1 of this embodiment, by using such a positive electrode plate 3 for the lithium ion secondary battery 1, there is an effect that battery performance with high durability characteristics and excellent output characteristics can be obtained.
[0090] (Alternative example) This embodiment is an example of the implementation of the present invention, and the present invention is not limited to the description of the embodiment and can be implemented as follows.
[0091] 〇In the lithium carbonate 32c of this embodiment, what is derived from the raw material of the positive electrode active material 32a is exemplified, but what is added to the positive electrode active material 32a afterwards may also be used. ○The numerical values and the like given in this embodiment are examples, and can be optimized by those skilled in the art without departing from the scope of the claims.
[0092] ○The drawings are schematically represented for the understanding of the specification, and do not show the actual size and shape of the fibrous conductive material 32b and the particles of the positive electrode active material 32a. ○In this embodiment, a battery pack combined with an in-vehicle cell battery is exemplified, but the present invention is not limited to its application and the like.
[0093] ○Also, the shape and size of the battery are not limited. ○The electrode body 12 is exemplified as a wound type having a cross-sectional race track shape, but a cylindrical one may be used. Furthermore, a laminated electrode body in which planar electrode plates are laminated may also be used.
[0094] Needless to say, those skilled in the art can add, delete, or modify the configuration of the present invention without departing from the scope of the claims. [Explanation of symbols]
[0095] W…Width direction (winding axis direction) θ[%]…(CNT) coverage rate P1~P10…plot points L1, L2… graph TC [wt%]…total carbon content 1...Lithium-ion secondary battery 11…Battery case 12...Electrode body 13...Nonaqueous electrolyte 14…Positive external terminal 15...Negative external terminal 2...Negative electrode plate 21...Negative electrode current collector 22...Negative electrode composite material layer 23...Negative electrode connection part 3…Positive electrode plate 31...Positive electrode current collector 32...Positive electrode mixture layer 32a...Cathode active material 32b…Fiber conductive material 32c…Lithium carbonate (Li2CO3) 32d…Binding material 33…Positive electrode connection 4…Separator
Claims
1. In the positive electrode mixture layer of the positive electrode plate of the lithium ion secondary battery, The positive electrode active material is represented by the chemical formula LiNixCoyMzO2, When M represents one or more metals selected from the group consisting of Fe, Cu, Ti, Mg, Al, W, B, Mo, Nb, Zn, Sn, Zr, Ga and V, The Li / M composition ratio is 1.15 or more and 1.21 or less, The amount of lithium carbonate relative to the positive electrode active material is 0.31 [wt %] or more and 1.29 [wt %] or less, and the positive electrode active material is combined with a fibrous conductive material, The composition ratio of the fibrous conductive material to the positive electrode active material is 0.5 wt % or more and 2.0 wt % or less, In addition, when the coverage rate of the fibrous conductive material is b [%], the composition ratio of the fibrous conductive material to the positive electrode active material is a [%], and the average diameter [μm] of D 50 of the positive electrode active material is c [μm], the coverage rate [%] is b=-8.583+(a×11.63)+(c×2.07)≦11.0…(Formula 1) When calculated by A positive electrode plate for a lithium ion secondary battery, wherein the coverage of the positive electrode active material with the fibrous conductive material is 11.0% or less.
2. In the positive electrode mixture layer of the positive electrode plate of the lithium ion secondary battery, The positive electrode active material is represented by the chemical formula LiNi x Co y M z O2, When M represents one or more metals selected from the group consisting of Fe, Cu, Ti, Mg, Al, W, B, Mo, Nb, Zn, Sn, Zr, Ga, and V, x=1−y−z, And 0<x≦0.5, And 0.2≦y≦0.5, And y + z ≧ 0.5, And y / x≧0.98; The amount of lithium carbonate relative to the positive electrode active material is 0.31 [wt %] or more and 1.29 [wt %] or less, and the positive electrode active material is combined with a fibrous conductive material, The composition ratio of the fibrous conductive material to the positive electrode active material is 0.5 wt % or more and 2.0 wt % or less, In addition, when the coverage rate of the fibrous conductive material is b [%], the composition ratio of the fibrous conductive material to the positive electrode active material is a [%], and the average diameter [μm] of D 50 of the positive electrode active material is c [μm], the coverage rate [%] is b=-8.583+(a×11.63)+(c×2.07)≦11.0…(Formula 1) When calculated by A positive electrode plate for a lithium ion secondary battery, wherein the coverage of the positive electrode active material with the fibrous conductive material is 11.0% or less.
3. 3. The positive electrode plate for a lithium ion secondary battery according to claim 2, wherein x is equal to or less than 0.
37.
4. 2. The positive electrode plate for a lithium ion secondary battery according to claim 1, wherein the fibrous conductive material is made of carbon nanotubes or carbon nanofibers.
5. 5. The positive electrode plate for a lithium ion secondary battery according to claim 4, wherein the length of the fibrous conductive material is 100 nm to 1000 nm.
6. A lithium ion secondary battery, characterized in that it uses a positive electrode plate for a lithium ion secondary battery described in any one of claims 1 to 5.
Citation Information
Patent Citations
Positive electrode activator and positive electrode using the same, lithium ion battery and lithium polymer battery using positive electrode
JP2004220909A
Lithium-ion secondary battery
JP2009272041A
Lithium-ion secondary battery and method for producing the same
JP2015519699A
Nonaqueous electrolyte secondary battery
JP2017212111A
Positive electrode active material for lithium secondary batteries, positive electrode for lithium secondary batteries, and lithium secondary battery