Molded body

A polyimide-based fixing roller with polyether ether ketone and fluororesin layers addresses wear resistance and friction issues, enhancing durability and sliding performance.

JP7581583B2Active Publication Date: 2024-11-13SUMITOMO ELECTRIC FINE POLYMER INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021561340
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-27
Filing Date
2020-11-18
Publication Date
2024-11-13
Estimated Expiration
2040-11-18

AI Technical Summary

Technical Problem

Existing fixing rollers in image forming apparatuses face issues with wear resistance and high friction coefficient due to the use of polyimide materials, leading to increased torque and potential debris formation.

Method used

A molded article comprising a cylindrical base material layer of polyimide with a sliding layer of polyether ether ketone and an outermost layer of fluororesin, enhancing wear resistance and sliding properties while maintaining moldability.

Benefits of technology

The layered structure improves wear resistance, reduces friction coefficient, and maintains durability, providing excellent sliding properties and torque control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581583000002
    Figure 0007581583000002
  • Figure 0007581583000003
    Figure 0007581583000003
  • Figure 0007581583000001
    Figure 0007581583000001
Patent Text Reader

Abstract

A molded article according to one aspect of the present disclosure is provided with: a cylindrical base layer having a polyimide as a main component; a sliding layer which is laminated on an inner circumferential surface side of the base layer and has a polyether ether ketone as a main component; and an outermost layer which is laminated on an outer circumferential surface side of the base layer and has a fluororesin as a main component.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a molded body. This application claims priority based on Japanese Application No. 2019-214474 filed on November 27, 2019, and incorporates all of the contents of said Japanese application by reference. [Background technology]

[0002] In image forming devices such as copiers and laser beam printers, a thermal fixing method is generally adopted in the final stage of printing and copying. This thermal fixing method is a method in which an image is formed by passing a transfer target, such as a printing paper to which a toner image has been transferred, between a fixing roller, the inner circumferential surface of which is provided with a heat source, and a pressure roller, thereby heating and melting the unfixed toner, and fixing the toner to the transfer target.

[0003] The fixing roller has a structure in which a tubular core is formed from polyimide from the viewpoint of moldability. This polyimide tubular body is easily worn and generates wear debris due to sliding contact with a nip plate provided on the inner peripheral surface side. Furthermore, the wear debris of polyimide may aggregate together and form large lumps, accelerating wear. In addition, when a polyimide tubular body is used, the torque may increase due to the high initial friction coefficient. In response to these problems, a film tubular body for a fixing device using polyimide with added lubricant has been disclosed (see JP 2001-56615 A). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-56615 A Summary of the Invention

[0005] A molded article according to one embodiment of the present disclosure includes a cylindrical base layer containing polyimide as a main component, a sliding layer laminated on an inner circumferential surface side of the base layer and containing polyether ether ketone as a main component, and an outermost layer laminated on an outer circumferential surface side of the base layer and containing a fluororesin as a main component. [Brief description of the drawings]

[0006] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a molded body according to the first embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing a molded body according to the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] [Problem that this disclosure aims to solve] In recent years, in the field of office automation (OA), there has been a demand for faster printing and further improved durability. As described in the above publication, in the fixing roller made of a tubular body using polyimide to which a lubricant has been added, there is room for improvement in terms of improving the wear resistance of the inner circumferential surface and reducing the friction coefficient.

[0008] The present disclosure has been made based on these circumstances, and aims to provide a molded body that has high wear resistance and excellent sliding characteristics, even when a base layer containing polyimide as a main component is used.

[0009] [Effects of this disclosure] The molded article according to one embodiment of the present disclosure has high abrasion resistance and excellent sliding characteristics, even when a base layer containing polyimide as a main component is used.

[0010] [Description of the embodiments of the present disclosure] First, the embodiments of the present disclosure will be listed and described.

[0011] A molded article according to one embodiment of the present disclosure includes a cylindrical base layer containing polyimide as a main component, a sliding layer laminated on an inner circumferential surface side of the base layer and containing polyether ether ketone as a main component, and an outermost layer laminated on an outer circumferential surface side of the base layer and containing a fluororesin as a main component.

[0012] The molded article is laminated on the inner peripheral side of a base layer mainly composed of polyimide and has a sliding layer mainly composed of polyether ether ketone, so that the friction coefficient of the molded article is reduced while maintaining the characteristics of the polyimide base material having good moldability, and the molded article has an excellent effect of suppressing torque increase. Furthermore, since the molded article has an outermost layer mainly composed of a fluororesin, the molded article can improve releasability. Therefore, the molded article according to one embodiment of the present disclosure can have high wear resistance, excellent sliding characteristics, and improved durability while using polyimide having good processability for the base layer.

[0013] The average thickness of the sliding layer is preferably 5 μm or more and 100 μm or less. When the average thickness of the sliding layer is in the above range, the wear resistance of the molded article can be further improved. Here, the "average thickness" refers to the average value of thicknesses measured at any ten points.

[0014] The molded article preferably further comprises an elastic layer mainly made of rubber, laminated on the outer peripheral surface side of the base layer and on the inner peripheral surface side of the outermost layer. The outermost layer is mainly made of fluororesin, and therefore tends to have relatively low elasticity. However, in the molded article, the elastic layer mainly made of rubber is laminated on the outer peripheral surface side of the base layer and on the inner peripheral surface side of the outermost layer mainly made of fluororesin, thereby improving the elasticity of the outermost layer.

[0015] Here, the term "main component" refers to the component that is contained in the largest amount, for example, a component that is contained in an amount of 50 volume % or more.

[0016] In the molded article, the content of the polyimide in the base layer is preferably 70% by volume or more and 100% by volume or less, which improves the flexibility and heat resistance of the molded article.

[0017] In the molded article, the content of the polyimide in the base layer is preferably 99.5% by volume or more and 100% by volume or less, which further improves the flexibility and heat resistance of the molded article.

[0018] In the molded article, the content of the polyether ether ketone in the sliding layer is preferably 51% by volume or more and 100% by volume or less, which improves the wear resistance of the sliding layer.

[0019] In the molded article, the content of the polyether ether ketone in the sliding layer is preferably 70% by volume or more and 100% by volume or less, which further improves the wear resistance of the sliding layer.

[0020] In the molded article, the content of the fluororesin in the outermost layer is preferably 50% by volume or more, which improves the abrasion resistance of the outermost layer.

[0021] In the molded article, the rubber content in the elastic layer is preferably 70% by mass or more and 100% by mass or less. By laminating such an elastic layer on the inner peripheral side of the outermost layer, the elasticity of the outermost layer is improved.

[0022] In the molded article, the rubber content in the elastic layer is preferably 99% by mass or more and 100% by mass or less. By laminating such an elastic layer on the inner peripheral side of the outermost layer, the elasticity of the outermost layer is further improved.

[0023] In the molded article, the average thickness of the sliding layer is preferably 10 μm or more and 50 μm or less. This embodiment improves the film-forming properties of the sliding layer.

[0024] In the molded article, the inner circumferential surface of the sliding layer preferably has an arithmetic mean roughness Ra of 1.4 μm or more and 3.3 μm or less. According to this embodiment, the lubricity of the inner circumferential surface of the sliding layer is improved.

[0025] In the molded article, the inner circumferential surface of the sliding layer preferably has a ten-point average roughness Rz of 6.8 μm or more and 11.7 μm or less. According to this embodiment, the lubricity of the inner circumferential surface of the sliding layer is improved.

[0026] In the molded article, the base layer preferably contains a filler, and the filler is at least one selected from the group consisting of titanic acid compounds, titanium oxide, carbon nanotubes, natural graphite, carbon fibers, glass fibers, and wollastonite. According to this embodiment, the wear resistance of the molded article can be further improved.

[0027] In the molded article, the elastic layer preferably contains vulcanized rubber. According to this embodiment, the elasticity of the elastic layer can be further improved, and as a result, the elasticity of the molded article is further improved.

[0028] In the molded article, the sliding layer constitutes the inner peripheral surface of the molded article. According to this embodiment, the inner peripheral surface includes a sliding layer mainly composed of polyether ether ketone, and therefore the sliding characteristics are excellent. Also, in the molded article, the outermost layer constitutes the outer peripheral surface of the molded article. According to this embodiment, the outermost layer mainly composed of fluororesin is provided on the outer peripheral surface, and therefore the mold releasability is excellent.

[0029] [Details of the embodiment of the present disclosure] Hereinafter, a molded body according to an embodiment of the present disclosure will be described in detail with reference to the drawings.

[0030] [First embodiment] <Molded body> The molded body according to the first embodiment includes a cylindrical base layer, a sliding layer laminated on the inner peripheral surface side of the base layer, and an outermost layer laminated on the outer peripheral surface side of the base layer and mainly composed of fluororesin. FIG. 1 is a schematic cross-sectional view showing the molded body 1 according to the first embodiment. The molded body 1 includes a cylindrical base layer 2, a sliding layer 3 laminated on the inner peripheral surface of the base layer 2, and an outermost layer 4 laminated on the outer peripheral surface of the base layer 2 and mainly composed of fluororesin. The sliding layer 3 constitutes the inner peripheral surface A of the molded body 1, and the outermost layer 4 constitutes the outer peripheral surface B of the molded body 1. The molded body 1 has a cylindrical shape, and can be suitably used for various rotating bodies (rollers), such as a fixing roller in a fixing unit of an image forming device such as a copier, a printer, or a facsimile, a developing roller in a developing unit, a charging roller, a transfer roller, a roller for supporting an endless belt in other parts, a paper discharge roller, a dust removal roller, a conveying roller, etc.

[0031] The lower limit of the average thickness of the molded body 1 is not particularly limited, but is preferably, for example, 30 μm, and the upper limit of the average thickness is preferably, for example, 150 μm.

[0032] [Base material layer] The base layer 2 has a cylindrical shape and can be suitably used for various rotating bodies (rollers) of image forming devices.

[0033] The base layer 2 is mainly composed of polyimide. The polyimide is relatively light and has excellent heat resistance and flexibility. The base layer 2 is mainly composed of polyimide, which improves moldability. Polyimide is a resin having an imide bond in the molecule. Polyimide can be obtained, for example, by polycondensing tetracarboxylic acid or its anhydride as an acid component and a diamine compound as an amine component in a reaction solvent, and dehydrating and ring-closing the obtained polyimide precursor by heating or the like.

[0034] Examples of the tetracarboxylic acid or anhydride thereof include pyromellitic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, benzene-1,2,3,4-tetracarboxylic dianhydride, naphthalene-2,3,6,7-tetracarboxylic dianhydride, 3,3',4,4'-diphenyltetracarboxylic dianhydride, 2,2'',3,3''-p-terphenyltetracarboxylic dianhydride, 2,2-bis(2,3-dicarboxyphenyl)-propane dianhydride, bis(2,3-dicarboxyphenyl)ether dianhydride, bis(2,3-dicarboxyphenyl)ether dianhydride, and bis(2,3-dicarboxyphenyl)ether dianhydride. Examples of the tetracarboxylic acid dianhydride include aromatic tetracarboxylic acid dianhydrides such as bis(2,3-dicarboxyphenyl)methane dianhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic acid dianhydride, bis(2,3-dicarboxyphenyl)sulfone dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, perylene-3,4,9,10-tetracarboxylic acid dianhydride, and phenanthrene-1,2,7,8-tetracarboxylic acid dianhydride, alicyclic acid anhydrides such as cyclopentane-1,2,3,4-tetracarboxylic acid dianhydride, and heterocyclic derivatives such as pyrazine-2,3,5,6-tetracarboxylic acid dianhydride. The above tetracarboxylic acids or anhydrides thereof can be used alone or in combination of two or more.

[0035] Examples of the diamine compound include aromatic diamines such as 2,2-di(p-aminophenyl)-6,6'-bisbenzoxazole, p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenylpropane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminodiphenylsulfone, 4,4'-diaminodiphenylether, benzidine, 4,4'-diamino-p-terphenyl, p-bis(2-methyl-4-aminopentyl)benzene, 1,5-diaminonaphthalene, 2,4-diaminotoluene, m-xylene-2,5-diamine, and m-xylylenediamine, and aliphatic diamines such as piperazine, methylenediamine, ethylenediamine, and tetramethylenediamine. The diamine compounds can be used alone or in combination of two or more.

[0036] The lower limit of the polyimide content in the base layer 2 is preferably 50 vol. %, more preferably 70 vol. %, further preferably 80 vol. %, further preferably 90 vol. %, and particularly preferably 99.5 vol. %. The content may be 100% by volume. That is, the base layer 2 may be a polyimide layer made of only polyimide and containing no binder, etc. If the content is less than the lower limit, the flexibility and heat resistance of the molded body 1 may be insufficient.

[0037] The base layer 2 may contain a filler. When the base layer 2 contains a filler, the electrical conductivity of the molded article can be improved.

[0038] As the filler, known ones can be used, and examples thereof include titanate compounds such as potassium titanate and aluminum titanate, titanium oxide, carbon nanotubes, natural graphite, carbon fibers, glass fibers, wollastonite, etc. A plurality of types of the filler can be used.

[0039] The shape of the filler is preferably needle-like or scale-like from the viewpoint of further improving the wear resistance of the molded article. Here, "needle-like" means a shape having an aspect ratio (ratio of the diameter to the length of the filler) of 1.5 or more, preferably 2 or more. The cross-sectional shape perpendicular to the length direction of the filler is not limited to a circle. When the cross section of the filler is not a circle, the aspect ratio is calculated by taking the maximum length of the cross section as the diameter. In addition, "scale-like" also includes a thin flake shape and a plate shape.

[0040] The average thickness of the base layer 2 is not particularly limited as long as sufficient strength can be maintained, and is preferably, for example, 5 μm or more and 300 μm or less.

[0041] [Sliding layer] The sliding layer 3 is laminated on the inner circumferential surface of the base layer 2. The sliding layer 3 is mainly composed of polyether ether ketone. Since the sliding layer 3 is mainly composed of polyether ether ketone, the molded body 1 has high wear resistance and excellent sliding characteristics.

[0042] The lower limit of the average thickness of the sliding layer 3 is preferably 5 μm, more preferably 10 μm. On the other hand, the upper limit of the average thickness is preferably 100 μm, more preferably 50 μm, and even more preferably 30 μm. If the average thickness is less than 5 μm, the film-forming properties of the sliding layer 3 may be reduced. Conversely, if the average thickness exceeds 100 μm, the thermal conductivity of the molded body 1 may be reduced. The "average thickness" is determined by measuring the thickness of the sliding layer in a cross section perpendicular to the longitudinal direction of the sliding layer 3 at any 10 points using an optical microscope, and averaging the measurements.

[0043] The lower limit of the polyether ether ketone content in the sliding layer 3 is preferably 50 volume %, more preferably 51 volume %, and even more preferably 70 volume %. The polyether ether ketone content in the sliding layer 3 may be 100 volume %. If the polyether ether ketone content in the sliding layer 3 is less than the above lower limit, the wear resistance of the sliding layer 3 decreases, and the wear resistance of the molded body 1 may become insufficient.

[0044] In addition to polyether ether ketone, the sliding layer 3 preferably further contains polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkoxyethylene copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-ethylene copolymer (ETFE) or a combination thereof, and more preferably further contains polytetrafluoroethylene. When the sliding layer 3 contains polyether ether ketone as the main component and further contains the above-mentioned resin components, the wear resistance and heat resistance can be further improved.

[0045] (outermost layer) The outermost layer 4 is mainly composed of a fluororesin. Since the outermost layer 4 is mainly composed of a fluororesin, it has excellent abrasion resistance. The content of the fluororesin in the outermost layer 4 is preferably 50% by volume or more. The outermost layer 4 may contain other optional components within a range that does not impair the effects of the present disclosure.

[0046] Examples of the fluororesin include polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkoxyethylene copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), polyvinylidene fluoride (PVDF), tetrafluoroethylene-ethylene copolymer (ETFE), polychlorotrifluoroethylene (PCTFE), chlorotrifluoroethylene-ethylene copolymer (ECTFE), polyvinyl fluoride (PVF), fluoroolefin-vinyl ether copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer, etc. Among these, the fluororesin is preferably PTFE, PFA, and FEP, more preferably PFA and PTFE, and even more preferably PTFE from the viewpoint of abrasion resistance, chemical resistance, and heat resistance. The fluororesin may be used alone or in combination of two or more.

[0047] The fluororesin may contain structural units derived from other copolymerizable monomers within the scope of the present disclosure. For example, PTFE may contain structural units such as perfluoro(alkyl vinyl ether), hexafluoropropylene, (perfluoroalkyl)ethylene, and chlorotrifluoroethylene. The upper limit of the content of the structural units derived from the other copolymerizable monomers is, for example, 3 mol% relative to the total structural units constituting the fluororesin.

[0048] The lower limit of the average thickness of the outermost layer 4 is preferably 5 μm, more preferably 20 μm. On the other hand, the upper limit of the average thickness is preferably 50 μm, more preferably 40 μm. If the average thickness is less than 5 μm, the durability of the molded body 1 may decrease. Conversely, if the average thickness exceeds 50 μm, the elasticity of the molded body 1 may decrease.

[0049] [Method of manufacturing molded body] The manufacturing method of the molded article preferably includes, for example, a step of laminating a sliding layer mainly composed of polyether ether ketone on the inner peripheral surface side of a cylindrical base layer mainly composed of polyimide, and a step of laminating an outermost layer mainly composed of a fluororesin on the outer peripheral surface side of the base layer. By including the above steps, the manufacturing method of the molded article can manufacture a molded article having high wear resistance and excellent sliding characteristics.

[0050] (Step of stacking the sliding layer) In this step, a sliding layer is laminated on the inner peripheral surface side of a cylindrical substrate layer mainly composed of polyimide. First, a resin composition for a sliding layer mainly composed of polyether ether ketone is prepared. Next, the sliding layer is formed by carrying out coating, extrusion molding, injection molding, or the like using the resin composition for a sliding layer, followed by baking. The coating means is not particularly limited, and various methods such as a spray coater, an electrostatic coating device, a flow coater, and a dip coater can be used. The baking temperature can be, for example, 100°C or more and 500°C or less.

[0051] (Step of laminating the outermost layer) In this step, an outermost layer mainly composed of a fluororesin is laminated on the outer peripheral surface side of the substrate layer after the sliding layer lamination step. Examples of the method for laminating the outermost layer include coating of a resin composition for the outermost layer mainly composed of a fluororesin, or covering with a PFA heat shrink tube. When coating the outer peripheral surface of the substrate layer with the resin composition for the outermost layer, a paint in which the resin composition for the outermost layer is dispersed or dissolved in a solvent is applied to the outer peripheral surface of the substrate layer. As the solvent, a mixture of water and an emulsifier, water and alcohol, water and acetone, water, alcohol and acetone, etc., which can efficiently disperse the fluororesin, can be used. Next, the substrate layer coated with the paint is placed in a heating furnace and heated to evaporate the solvent in the paint and bake the fluororesin. The baking temperature of the fluororesin can be, for example, 300°C or more and 400°C or less. Thereafter, the outer peripheral surface of the substrate layer is cooled to form the outermost layer on the outer peripheral surface of the substrate layer.

[0052] The molded article according to the first embodiment has high wear resistance and excellent sliding characteristics.

[0053] [Second embodiment] <Molded body> The molded article according to the second embodiment further includes an elastic layer containing rubber as a main component, laminated on the outer circumferential surface side of the base material layer and on the inner circumferential surface side of the outermost layer.

[0054] Fig. 2 is a schematic cross-sectional view showing a molded body 10 according to the second embodiment. The molded body 10 in Fig. 2 includes a cylindrical base layer 2, a sliding layer 3 laminated on the inner peripheral surface of the base layer 2, an elastic layer 5 laminated on the outer peripheral surface of the base layer 2, and an outermost layer 4 laminated on the outer peripheral surface of the elastic layer 5. The base layer 2, the sliding layer 3, and the outermost layer 4 are the same as those in the first embodiment, and therefore the same reference numbers are used and the description thereof is omitted.

[0055] (Elastic layer) The elastic layer 5 is laminated on the outer peripheral surface of the base layer 2. The elastic layer 5 is mainly composed of rubber. Therefore, the elastic layer 5 has sufficient elasticity. The elasticity of the outermost layer 4 mainly composed of fluororesin tends to be relatively low, but in the molded body 10, the elastic layer mainly composed of rubber is laminated on the inner peripheral surface of the outermost layer mainly composed of fluororesin, thereby improving the elasticity of the outermost layer 4. Furthermore, by laminating the elastic layer 5 on the inner peripheral surface of the outermost layer 4, the interlayer adhesive strength between the elastic layer 5 and the outermost layer 4 can be further improved. Moreover, the rubber is preferably vulcanized. By vulcanizing the rubber, the elasticity of the elastic layer 5 can be further improved, and as a result, the elasticity of the molded body 10 is further improved.

[0056] The rubber is not particularly limited, but examples of the rubber that can be used include natural rubber, synthetic natural rubber, butadiene rubber, styrene butadiene rubber, butyl rubber, nitrile rubber, ethylene propylene rubber, chloroprene rubber, acrylic rubber, chlorosulfonated polyethylene rubber, urethane rubber, silicone rubber, fluororubber, ethylene vinyl acetate rubber, epichlorohydrin rubber, polysulfurized rubber, etc. The rubbers can be used alone or in combination of two or more.

[0057] The lower limit of the rubber content in the elastic layer 5 is preferably 70% by mass, more preferably 90% by mass, and even more preferably 99% by mass. The rubber content in the elastic layer 5 may be 100% by mass. If the rubber content in the elastic layer 5 is less than the above lower limit, the elasticity of the elastic layer 5 decreases, and the elasticity of the molded body 1 may become insufficient.

[0058] The elastic layer 5 may contain additives as components other than rubber. Examples of the additives include plasticizers, stabilizers, lubricants, antioxidants, UV absorbers, flame retardants, colorants, and fillers. In this way, the elastic layer 5 contains the additives, so that the elastic layer 5 can be given desired properties. The upper limit of the content of the additives in the elastic layer 5 is not particularly limited, but is preferably, for example, 30% by mass.

[0059] The average thickness of the elastic layer 5 is not particularly limited and can be appropriately changed depending on the application, but can be, for example, 0.1 mm or more and 50 mm or less.

[0060] <Method for manufacturing the molded article according to the second embodiment> The method for producing the molded body of the second embodiment may further include a step of laminating an elastic layer on the outer peripheral surface of the base layer after the sliding layer lamination step of the method for producing the molded body of the first embodiment. In the step of laminating the elastic layer, a resin composition for the sliding layer, mainly composed of rubber, is first prepared. Next, the resin composition for the sliding layer is applied to the outer peripheral surface of the base layer after the sliding layer lamination step by coating, extrusion molding, injection molding, or the like, and then solidified to form an elastic layer. The rubber of the elastic layer may be vulcanized at any time during the production of the molded body.

[0061] The molded article according to the second embodiment has high abrasion resistance, excellent sliding properties, and can improve the elasticity of the outermost layer. The molded article according to the second embodiment has a cylindrical shape like the molded article according to the first embodiment, and can be suitably used for various rotating bodies (rollers) such as fixing rollers in fixing units of image forming devices such as copiers, printers, and facsimiles, heating rollers, developing rollers in developing units, charging rollers, transfer rollers, rollers for supporting endless belts in other parts, paper discharge rollers, dust removal rollers, and conveying rollers.

[0062] [Other embodiments] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present disclosure is not limited to the configurations of the above-described embodiments, but is indicated by the scope of the claims, and is intended to include all modifications within the meaning and scope equivalent to the scope of the claims.

[0063] The molded article may have another layer between the sliding layer and the base layer, between the outermost layer and the base layer, between the outermost layer and the elastic layer, etc. Examples of the other layer include a primer layer.

[0064] The inner peripheral surface of the outermost layer may be subjected to a surface treatment to improve adhesion, such as roughening by plasma treatment, liquid ammonia treatment, corona treatment, tetra-etch treatment, or laser etching treatment.

[0065] Furthermore, the wear resistance of the outermost layer 4 may be improved by irradiating the outermost layer 4 with ionizing radiation to crosslink the fluororesin. EXAMPLES

[0066] The present disclosure will be described more specifically below with reference to examples, but the present disclosure is not limited to the following examples.

[0067] <Films No.1 to No.9> Using the resin composition for base layer and the resin composition for sliding layer for forming the base layer and sliding layer of the molded article, films No. 1 to No. 3 having a base layer and two-layer films No. 4 to No. 9 having a base layer and a sliding layer were produced by the following procedure. The compositions (volume %) of the resin composition for base layer and the resin composition for sliding layer constituting the above films No. 1 to No. 9 and the average thickness of the sliding layer are shown in Table 1. In addition, "-" in Table 1 indicates that the corresponding component was not used.

[0068] (Resin composition for base layer) The resin composition for the base layer contains fillers other than the main components, such as needle-shaped titanium oxide, flake graphite, and carbon nanotubes.

[0069] (Resin composition for sliding layer) Polyether ether ketone was used as the material of the resin composition for the sliding layer.

[0070] (Film Creation) The resin composition for the base layer, which has the composition shown in Table 1, was coated in the form of a film. Then, the film was baked to 420°C to produce films No. 1 to No. 3. The resin composition for the base layer, which has the composition shown in Table 1, was coated in the form of a film to form a coating layer, and the surface of the coating layer was coated with a resin composition for the sliding layer, which is made of polyether ether ketone, to form a laminate. Then, the film was baked to 400°C to produce films No. 4 to No. 9. The average thickness of the base layer was 70 μm. The average thickness of the sliding layer is shown in Table 1.

[0071] [evaluation] Next, the abrasion resistance, friction resistance and surface roughness of Films No. 1 to No. 9 were evaluated.

[0072] (Evaluation of rotational friction wear using pin-on-disk type friction wear test) The pin-on-disk type friction and wear test means a test in which the tip of a metal pin, which is an indenter, is pressed perpendicularly against the sliding surface of the test subject while rotating the sliding surface, causing the test subject to revolve and slide. The pin-on-disk type friction and wear test was performed using an "EFM-3-EN" friction and wear tester manufactured by A&D Co., Ltd. Specifically, a pin-on-disk type friction and wear test was performed on the surfaces of films No. 1 to No. 9, in which two stainless steel pins with a diameter of 17.4 mm arranged on one circumference centered on the rotation axis were slid with a pressure load of 0.14 MPa and a rotation speed of 210 rpm for 2000 seconds under heating at 180°C, and the wear depth [μm] of the worn area was measured. The tip of the pin was made flat. The difference between the average thickness measured at eight points before the wear test and the average thickness measured at eight points after the wear test was calculated and used as the wear depth. Additionally, the maximum friction coefficient at the beginning (hereinafter referred to as the initial maximum friction coefficient) and the friction coefficient at the point when the friction coefficient became stable (defined as the stable friction coefficient) were measured, and the initial friction increase amount [%] shown below was calculated. Initial friction increase [%] = (initial maximum friction coefficient - stable friction coefficient) x 100 / stable friction coefficient

[0073] (Friction test) (1) Static friction coefficient Measurements were performed at room temperature using "AUTOGRAPH" manufactured by Shimadzu Corporation in accordance with ASTM-D (1894). (2) Coefficient of kinetic friction Measurements were taken in reciprocating mode in an environment of 200°C using a RHESCA Corporation "FPR-2100" with a load of 500 g and an indenter made of a stainless steel pin with a diameter of 3 / 16 inch. (3) Increase in static friction The static friction increase amount [%] shown below was calculated from the obtained values ​​of the static friction coefficient and the kinetic friction coefficient. Static friction increase [%] = (static friction coefficient - kinetic friction coefficient) x 100 / kinetic friction coefficient

[0074] (Surface roughness) The arithmetic mean roughness (Ra) and ten-point mean roughness (Rz) were measured in accordance with JIS-B-0601 (1994) using a surface roughness measuring instrument "Surfcom 408A" manufactured by Tokyo Seimitsu Co., Ltd. Ra and Rz were measured at three points and the average was calculated.

[0075] Table 1 shows the results of the friction and abrasion test, the friction test and the surface roughness evaluation for the two-layer films No. 1 to No. 9.

[0076] [Table 1]

[0077] As shown in Table 1, films No. 4 to No. 9 having a sliding layer made of polyetheretherketone have small wear amount and initial friction increase in the pin-on-disk type wear test, and it is found that the sliding layer is not easily deformed during sliding. On the other hand, films No. 1 to No. 3, which do not have a sliding layer made of polyetheretherketone and are made only of a base layer mainly composed of polyimide, have large wear amount, as well as large initial and static friction increase, and are considered to require large torque. In addition, films No. 4 to No. 9 having a sliding layer made of polyetheretherketone have a much larger surface roughness than films No. 1 to No. 3 made only of a base layer. From this, it is presumed that films No. 4 to No. 9 having a sliding layer made of polyetheretherketone have improved sliding properties because the contact area with the wear indenter is small due to the very large surface roughness.

[0078] The above results demonstrate that the molded article has high wear resistance and excellent sliding properties. [Explanation of symbols]

[0079] 1, 10 Molded body 2 Base material layer 3. Sliding layer 4 Outermost layer 5 Elastic layer A: Inner surface of molded body B. Outer surface of molded body

Claims

1. A cylindrical base layer mainly composed of polyimide; a sliding layer laminated on the inner circumferential surface side of the base material layer and containing polyether ether ketone as a main component; an outermost layer made of a fluororesin as a main component and laminated on the outer peripheral surface side of the base material layer; Equipped with The sliding layer constitutes an inner peripheral surface of the molded body, The content of the polyimide in the base layer is 70% by volume or more and 100% by volume or less, The content of the polyether ether ketone in the sliding layer is 51 vol% or more and 100 vol% or less, The molded article, wherein the outermost layer has a fluororesin content of 50 volume % or more.

2. The molded article according to claim 1, wherein the average thickness of the sliding layer is from 5 μm to 100 μm.

3. The elastic layer is laminated on an outer peripheral surface side of the base layer and an inner peripheral surface side of the outermost layer, and the elastic layer is mainly composed of rubber.

3. The molded article according to claim 1, wherein the elastic layer has a rubber content of 70% by mass or more and 100% by mass or less.

4. 4. The molded article according to claim 1, wherein the content of the polyimide in the base layer is 99.5% by volume or more and 100% by volume or less.

5. 5. The molded article according to claim 1, wherein the content of the polyether ether ketone in the sliding layer is 70% by volume or more and 100% by volume or less.

6. The molded article according to claim 3 , wherein the elastic layer has a rubber content of 99% by mass or more and 100% by mass or less.

7. The molded article according to any one of claims 1 to 6, wherein the sliding layer has an average thickness of 10 µm or more and 50 µm or less.

8. 8. The molded article according to claim 1, wherein the inner circumferential surface of the sliding layer has an arithmetic mean roughness Ra of 1.4 μm or more and 3.3 μm or less.

9. 9. The molded article according to claim 1, wherein the inner circumferential surface of the sliding layer has a ten-point average roughness Rz of 6.8 μm or more and 11.7 μm or less.

10. The base layer contains a filler, 10. The molded article according to claim 1, wherein the filler is at least one selected from the group consisting of titanic acid compounds, titanium oxide, carbon nanotubes, natural graphite, carbon fibers, glass fibers, and wollastonite.

11. The molded article according to claim 3 or claim 6, wherein the elastic layer comprises vulcanized rubber.

12. The molded article according to claim 1 , wherein the outermost layer constitutes an outer peripheral surface of the molded article.

Citation Information

Patent Citations

  • Fixing device and film tube for fixing device

    JP2001056615A

  • Manufacturing method of addition curable liquid conductive silicone rubber composition, roll for business machine and belt for business machine

    JP2017132832A

  • Pressure roller

    JP2017207642A

  • Rotor for electrophotography, fixation device, electrophotographic image formation device and manufacturing method of rotor

    JP2018146835A

  • Fixing member and method for manufacturing fixing member

    JP2019028184A