Laminated Sheet
The laminated sheet with a thermoplastic resin and inorganic material layer addresses ink adhesion problems by ensuring high water resistance and printability through a balanced inorganic material content, enhancing mechanical strength and non-flammability.
Patent Information
- Application Number
- JP2020027225
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-02-20
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-02-20
AI Technical Summary
Conventional printing sheets with a resin layer on the surface suffer from dampening water mixing with oil-based ink, leading to unclear printing due to emulsification, despite having high water resistance and good adhesion.
A laminated sheet comprising a raw fabric layer with a thermoplastic resin and inorganic material, and a surface layer with a pigment and binder, where the inorganic material content is 15% to 90% by mass, ensuring high water resistance and printability.
The laminated sheet maintains high water resistance and achieves excellent printability by preventing ink adhesion issues while maintaining mechanical strength and non-flammability.
Smart Images

Figure 0007581628000002 
Figure 0007581628000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminated sheet. [Background technology]
[0002] Pulp paper and thermoplastic resin sheets that are microporous and have good air permeability, which have been hitherto capable of producing clear printing and allowing for mass printing, have been noted to have poor water resistance. In response to this, a printing sheet has been proposed in which a resin layer is provided on the surface of the sheet, thereby providing the sheet with high water resistance and good adhesion to ink (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-168685 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, printing sheets with a resin layer on the surface cannot absorb the dampening water that is used to moisten non-printed areas to prevent the printing ink from adhering to those areas, and therefore have the problem that the dampening water remaining on the surface mixes with the oil-based ink and emulsifies, resulting in unclear printing.
[0005] The present invention has been made in consideration of the above circumstances, and has an object to provide a laminate sheet that maintains high water resistance and also has excellent printability. [Means for solving the problem]
[0006] In order to solve the above problems, a laminated sheet according to one embodiment of the present invention comprises an original fabric layer containing a thermoplastic resin and an inorganic material, a surface layer formed on a first side of the original fabric layer, and a back layer formed on a second side of the original fabric layer opposite the first side, wherein the content of the inorganic material is in the range of 15 mass% or more and 90 mass% or less with respect to the mass of the original fabric layer. Effect of the Invention
[0007] According to one aspect of the present invention, it is possible to provide a laminate sheet that has excellent printability while maintaining high water resistance. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic configuration example of a laminate sheet according to a first embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, a laminated sheet according to one embodiment of the present invention will be described with reference to the drawings. Here, the drawings are schematic, and the relationship between thickness and planar dimensions, the ratio of thickness of each layer, etc. are different from the actual ones. In addition, the embodiment shown below is an example of a configuration for embodying the technical idea of the present invention, and the technical idea of the present invention is not limited to the material, shape, structure, etc. of the components described below. The technical idea of the present invention can be variously modified within the technical scope defined by the claims described in the claims.
[0010] First Embodiment [Laminated sheet composition] A basic configuration of the laminate sheet according to the first embodiment of the present disclosure will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view for explaining one configuration example of the laminate sheet according to the first embodiment of the present disclosure. As shown in FIG. 1, a laminate sheet 15 according to one embodiment of the present invention includes a back surface layer 5, an original fabric layer 1, and a surface layer 2 from the back surface side to the front surface side. Each layer constituting the laminated sheet 15 will now be described.
[0011] (Original layer) The raw fabric layer 1 is a layer (sheet) that becomes the base material of the laminated sheet 15, and is a layer that contains a thermoplastic resin and an inorganic material. The thermoplastic resin of this embodiment preferably contains at least one of polypropylene, polyethylene, and polyester, and more preferably contains polypropylene. By using at least one of polypropylene, polyethylene, and polyester as the thermoplastic resin, the dispersibility of the inorganic material is improved. Furthermore, by using polypropylene as the thermoplastic resin, the dispersibility of the inorganic material is further improved.
[0012] The inorganic material of this embodiment is a powder containing at least one of calcium carbonate and calcium carbonate salt. The powder containing at least one of calcium carbonate and calcium carbonate salt is preferably one containing at least one of calcium carbonate and calcium carbonate salt in a range of 50% by mass to 100% by mass with respect to the mass of the entire powder. In other words, the purity of the powder containing at least one of calcium carbonate and calcium carbonate salt is preferably in a range of 50% by mass to 100% by mass of calcium carbonate, etc. If the powder contains at least one of calcium carbonate and calcium carbonate salt with a content of calcium carbonate, etc. of 50% by mass or more, it can impart sufficient incombustibility or sufficient flame retardancy to the raw fabric layer 1 and can impart sufficient mechanical strength.
[0013] In addition to the powder containing at least one of the calcium carbonate and calcium carbonate salts, examples of the inorganic material include at least one of silica (particularly hollow silica), alumina, antimony trioxide, antimony soda, zirconium compounds such as zirconium silicate and zirconium oxide, magnesium hydroxide, aluminum hydroxide, basic magnesium carbonate, borax, zinc borate, complexes of molybdenum trioxide or antimony dimolybdate and aluminum hydroxide, complexes of antimony trioxide and silica, complexes of antimony trioxide and zinc oxide, silicic acid of zirconium, complexes of zirconium compounds and antimony trioxide, and salts thereof. In addition, the inorganic material may be, for example, limestone powder, sintered powder of eggshells, sintered powder of shells such as oysters and scallops, etc. Among the above-mentioned inorganic materials, calcium carbonate and calcium carbonate salts in particular are easy to control the particle size and compatibility with thermoplastic resins by the manufacturing method, and are inexpensive in terms of material cost. This is also preferable from the viewpoint of reducing the cost of the laminated sheet.
[0014] In addition, the inorganic material may be a powder material having crystallinity, so-called crystalline powder, or a powder material having no crystallinity, so-called amorphous type powder material. If the inorganic material is a powder material having crystallinity, the powder itself is homogeneous and isotropic, so that the mechanical strength of the powder itself tends to be improved, and the scratch resistance and durability of the laminated sheet tend to be improved. In addition, if the inorganic material is an amorphous type powder material, it is possible to appropriately adjust the electrical conductivity and thermal conductivity of the powder itself, or the light transmittance and light absorbance, so that it is possible to impart a design with a wide variety of textures, gloss, etc.
[0015] In addition, the inorganic material of this embodiment is preferably in a powder form (powder form), and its average particle size is preferably in the range of 1 μm or more and 3 μm or less, and the maximum particle size is preferably 50 μm or less. If the average particle size and maximum particle size of the inorganic material are within the above numerical range, the dispersibility of the inorganic material in the thermoplastic resin can be improved while maintaining the flatness of the surface of the raw fabric layer 1. If the average particle size of the inorganic material is less than 1 μm, the cohesive force between the inorganic materials increases, and the dispersibility in the thermoplastic resin described later may decrease. If the average particle size of the inorganic material exceeds 3 μm, the flatness of the surface of the raw fabric layer 1 may decrease, and the thickness of the surface layer 2 or the back layer 5 of the second embodiment described later may become uneven, or unevenness or chipping may occur. If the maximum particle size of the inorganic material exceeds 50 μm, the flatness of the surface of the raw fabric layer 1 may decrease, and the thickness of the surface layer 2 or the back layer 5 described later may become uneven, or unevenness or chipping may occur. In this embodiment, the "average particle size" means the mode diameter.
[0016] The content of the inorganic material in this embodiment may be in the range of 15% by mass to 90% by mass, more preferably in the range of 20% by mass to 80% by mass, and even more preferably in the range of 60% by mass to 80% by mass. If the content of the inorganic material is less than 15% by mass, the proportion of thermoplastic resin is relatively high, and it is difficult to obtain non-combustibility or flame retardancy. In addition, when the surface of the original layer 1 is scratched using a Hoffman scratch tester, visible scratches may be formed, that is, sufficient surface hardness may not be obtained. On the other hand, if the content of the inorganic material exceeds 90% by mass, the proportion of thermoplastic resin is relatively low. For this reason, when the surface of the original layer 1 is coated with an anchor layer or printed, so-called "powdering" may occur on the surface of the original layer 1. Here, "powdering" refers to the inorganic material contained in the original layer 1 protruding to the surface of the original layer 1.
[0017] In addition, the total content of the thermoplastic resin and the inorganic material is preferably in the range of 90% by mass or more and 100% by mass or less with respect to the mass of the original layer 1. If the total content of the thermoplastic resin and the inorganic material is within the above numerical range, sufficient non-combustibility or sufficient flame retardancy can be obtained, while improving printability and lamination suitability, and cracks occurring at the folded portion of the sheet can be reduced. If the total content of the thermoplastic resin and the inorganic material is less than 90% by mass with respect to the mass of the original layer 1, sufficient non-combustibility or sufficient flame retardancy may not be obtained. In addition, printability and lamination suitability may decrease, and cracks may occur at the folded portion of the sheet.
[0018] In addition, when the total content of the thermoplastic resin and the inorganic material is 100% by mass relative to the mass of the raw layer 1, it is preferable that the content of the thermoplastic resin is in the range of 10% by mass to 85% by mass, and the content of the inorganic material is in the range of 15% by mass to 90% by mass. It is more preferable that the content of the thermoplastic resin is in the range of 20% by mass to 80% by mass, and the content of the inorganic material is in the range of 20% by mass to 80% by mass. It is even more preferable that the content of the thermoplastic resin is in the range of 20% by mass to 40% by mass, and the content of the inorganic material is in the range of 60% by mass to 80% by mass. If the total content of the thermoplastic resin and the inorganic material is within the above numerical range, it is possible to reliably obtain sufficient non-flammability or sufficient flame retardancy, reliably improve printability and lamination suitability, and reliably reduce cracks occurring at the folded part of the sheet.
[0019] In addition, the thickness of the raw fabric layer 1 is preferably in the range of 50 μm to 250 μm, more preferably in the range of 70 μm to 200 μm. If the thickness of the raw fabric layer 1 is within the above numerical range, the lamination suitability can be improved and cracks occurring at the folded part of the sheet can be reduced. If the thickness of the raw fabric layer 1 is less than 50 μm, the lamination suitability tends to decrease. If the thickness of the raw fabric layer 1 is more than 250 μm, cracks may occur at the folded part of the sheet. Moreover, the raw fabric layer 1 is preferably a uniaxially or biaxially oriented raw fabric layer. If the raw fabric layer 1 is a uniaxially or biaxially oriented raw fabric layer, the versatility of the laminated sheet 15 can be increased.
[0020] (Surface layer) The surface layer 2 is a layer formed so as to cover the entire surface (first surface) of the base layer 1, and is a layer containing a pigment and a binder. As the pigment of the present embodiment, any of organic pigments and inorganic pigments can be used or used in combination. The pigment of the present embodiment may be appropriately selected from, for example, kaolinite, aluminum hydroxide, calcium carbonate, titanium dioxide, barium sulfate, zinc oxide, silica, polystyrene particles, polymethyl methacrylate particles, etc., either alone or modified. The average particle size of the pigment is preferably from 0.01 μm to 5 μm. The pigment of the present invention is preferably used by mixing a first pigment having an average particle size of 1 μm or more and 7 μm or less with a second pigment having an average particle size of 0.02 μm or more and less than 1 μm. In this case, the content of the first pigment is preferably 50% by mass or more and 85% by mass or less with respect to the mass of the entire pigment.
[0021] The binder of the present embodiment is preferably an aqueous binder that can be applied in an aqueous manner, which may be appropriately selected from aqueous dispersion resins such as styrene-butadiene latex and acrylic latexes such as copolymers of acrylic acid esters and methacrylic acid esters, water-soluble adhesives such as casein, starch, polymeracrylic acid and its salts, polyvinyl alcohol, and carboxymethylcellulose, either alone or in modified form.
[0022] The amount of the binder in the aqueous dispersion resin, such as styrene-butadiene latex, relative to the mass of the pigment, may be 20 parts by mass or more, more preferably 25 parts by mass or more, and even more preferably 30 parts by mass or more. When the amount of the binder in the aqueous dispersion resin is 30 parts by mass or more, the adhesion between the surface layer 2 and the raw fabric layer 1 becomes strong, the printing strength of the present invention is increased, the water absorbency can be easily adjusted to a preferred range, and water resistance is significantly improved.
[0023] Furthermore, if the content of the aqueous dispersion resin exceeds 20 parts by mass relative to the mass of the pigment, migration occurs when the applied ink for forming the front layer and back layer is dried, and a resin film is formed on the sheet surface, causing deterioration of printability. However, the occurrence of such migration is suppressed in the raw sheet layer 1 of the present invention.
[0024] The surface layer 2 of the present invention can be prepared by preparing an ink for forming the surface layer and the back layer containing a pigment and a binder, and then providing the ink for forming the surface layer and the back layer on the original film layer 1 using a normal coating coater and drying device. In addition to the pigment and binder of the present invention, additives such as a pigment dispersant, a viscosity modifier, and a foam inhibitor that are normally used in coating solutions can be appropriately used in the ink for forming the surface layer and the back layer.
[0025] The concentration of the ink for forming the front layer and the back layer is generally 20% by mass or more and 75% by mass or less in terms of solid content, and can be appropriately adjusted and selected depending on the desired thickness, viscosity, type of coater, etc. of the front layer 2. The surface layer 2 has a coating amount of 0.5 g / m2 after drying. 2 More than 30g / m 2 Less than 1 g / m 2 More than 20g / m 2 Hereinafter, the coating film thickness after drying is preferably 1 μm or more and 20 μm or less. Before forming the surface layer 2 of the present invention, it is preferable to subject the base layer 1 to a treatment such as corona discharge, or alternatively, a subbing layer made of an aqueous binder such as latex having a thickness of 0.1 μm to 0.5 μm may be provided.
[0026] The water absorbency of the surface having the surface layer 2 of the present invention, as defined by the Klemm method of JIS P8140, is preferably within the range of 40 mm to 150 mm, more preferably within the range of 80 mm to 120 mm. The water absorbency is achieved when the surface having the surface layer 2 has pores with an average diameter of 0.1 μm to 3.0 μm, and the total area of the pores per unit area is 1.0% to 10.0% of the unit area.
[0027] In the present invention, the pore size was measured by devising a technique for measuring the size of submicron pores using gold deposition in combination with scanning electron microscope observation, and the average diameter and the total area of the pores were calculated. As the electron microscope, a Keyence ultra-deep multi-angle microscope DVHX-5000 and its attached image processing software were used. The average diameter and total area of the pores can be adjusted mainly by the type and amount of the pigment used in the surface layer 2 , but can also be adjusted by the drying conditions and the type of resin in the base layer 1 .
[0028] (Back layer) The back surface layer 5 is a layer formed so as to cover the entire back surface (second surface) of the original fabric layer 1, and is a layer containing a pigment and a binder. The pigment for the back layer 5 is not particularly limited, but may be, for example, the same material as that for the front layer 2. The average particle diameter of the pigment is preferably 0.01 μm or more and 5 μm or less. The pigment in the back layer 5 is preferably a mixture of a first pigment having an average particle size of 1 μm or more and 7 μm or less and a second pigment having an average particle size of 0.02 μm or more and less than 1 μm. In this case, the content of the first pigment is preferably 50 mass % or more and 85 mass % or less with respect to the mass of the entire pigment.
[0029] The binder in this embodiment is preferably an aqueous binder that can be applied with an aqueous solution. The aqueous binder is not particularly limited, but for example, the same material as that of the surface layer 2 can be used.
[0030] The amount of the binder in the aqueous dispersion resin, such as styrene-butadiene latex, is 20 parts by mass or more, more preferably 25 parts by mass or more, and even more preferably 30 parts by mass or more, relative to the mass of the pigment. When the amount of the binder in the aqueous dispersion resin is 30 parts by mass or more, the adhesion between the back layer 5 and the raw fabric layer 1 becomes strong, the printing strength of the present invention is increased, the water absorbency can be easily adjusted to a preferred range, and the water resistance is significantly improved.
[0031] Furthermore, if the content of the aqueous dispersion resin exceeds 20 parts by mass relative to the mass of the pigment, migration occurs when the applied ink for forming the front layer and back layer is dried, and a resin film is formed on the sheet surface, causing deterioration of printability. However, the occurrence of such migration is suppressed in the raw sheet layer 1 of the present invention.
[0032] The back layer 5 of the present invention can be formed by preparing an ink for forming the front layer and the back layer containing a pigment and a binder, and then providing the ink for forming the front layer and the back layer on the original film layer 1 using a normal coating coater and drying device. In addition to the pigment and binder of the present invention, the ink for forming the front layer and the back layer can appropriately contain additives such as a pigment dispersant, a viscosity modifier, and a foam inhibitor that are normally used in coating solutions.
[0033] The concentration of the ink for forming the front layer and the back layer is generally 20% by mass or more and 75% by mass or less in terms of solid content, and can be appropriately adjusted and selected depending on the desired thickness, viscosity, type of coater, etc. of the back layer 5. The coating amount of this back layer 5 after drying is 0.5 g / m 2 More than 30g / m 2 Less than 1 g / m 2 More than 20g / m 2 Hereinafter, the coating film thickness after drying is preferably 1 μm or more and 20 μm or less. Before forming the back layer 5 of the present invention, it is preferable to subject the base layer 1 to a treatment such as corona discharge, or alternatively, a subbing layer made of an aqueous binder such as latex having a thickness of 0.1 μm to 0.5 μm may be provided.
[0034] The water absorbency of the surface having the back surface layer 5 of the present invention, as defined by the Klemm method of JIS P8140, is preferably within the range of 40 mm to 150 mm, more preferably within the range of 80 mm to 120 mm. The water absorbency is achieved when the surface having the back surface layer 5 has pores with an average diameter of 0.1 μm to 3.0 μm, and the total area of the pores per unit area is 1.0% to 10.0% of the unit area.
[0035] In the present invention, the pore size was measured by devising a technique for measuring the size of submicron pores using gold deposition in combination with scanning electron microscope observation, and the average diameter and the total area of the pores were calculated. As the electron microscope, a Keyence ultra-deep multi-angle microscope DVHX-5000 and its attached image processing software were used. The average diameter and total area of the pores can be adjusted mainly by the type and amount of the pigment used in the surface layer 2 , but can also be adjusted by the drying conditions and the type of resin in the base layer 1 .
[0036] Here, in the technical standards for non-combustible materials stipulated in the Enforcement Order of the Building Standards Act, the following requirements must be met in a heat generation test using a cone calorimeter tester conforming to ISO5660-1 (Article 108-2, Items 1 and 2 of the Enforcement Order of the Building Standards Act). In order for the laminated sheet 15 of this embodiment to be certified as a non-combustible material, it must meet the following requirements: 2 When heated by radiant heat for 20 minutes, all of the following requirements 1 to 3 must be met. 1. Total calorific value is 8MJ / m 2 below 2. The maximum heat generation rate is 200kW / m for 10 seconds or more. 2 Not to exceed 3. No cracks or holes that penetrate to the back surface and are harmful to fire resistance
[0037] Furthermore, the laminated sheet 15 of this embodiment having the aforementioned base fabric layer 1 realizes a non-combustible material that satisfies both of the requirements set forth in Article 108-2, Paragraphs 1 and 2 of the Enforcement Order in a heat generation test using a cone calorimeter tester conforming to ISO 5660-1.
[0038] [Manufacturing method of laminated sheet] An example of a method for producing the laminated sheet 15 will be briefly described. First, an ink for forming a surface layer and a back layer is applied to the front surface, which is one surface of the raw fabric layer 1, to form the surface layer 2. Next, the back surface layer 5 is formed by applying ink for forming a front surface layer and a back surface layer to the other surface, ie, the back surface, of the original layer 1 . The back surface layer 5 may be formed simultaneously with the front surface layer 2. In this manner, the laminate sheet 15 according to the present embodiment is manufactured.
[0039] <Advantages of the First Embodiment> The laminate sheet 15 according to this embodiment has the following effects. (1) In the laminate sheet 15 of the present embodiment, the base layer 1 contains a thermoplastic resin and an inorganic material, and the front layer 2 and the back layer 5 contain a pigment and a binder. This configuration makes it possible to achieve higher water resistance.
[0040] (2) In the laminate sheet 15 of the present embodiment, the surface having the front layer and the back layer has a water absorbency of 40 mm or more and 150 mm or less according to the JIS P8141 Klemm method. This configuration makes it possible to achieve higher printing performance. EXAMPLES
[0041] [Example 1] First, a raw fabric layer composed of an inorganic material and a thermoplastic resin was formed. Titanium oxide having an average particle size of 10 μm and a maximum particle size of 50 μm was used as the inorganic material, and the content of titanium oxide was set to 90% by mass relative to the mass of the raw fabric layer. Polyethylene terephthalate was used as the thermoplastic resin. The total content of the inorganic material and the thermoplastic resin was adjusted to 88% by mass relative to the mass of the raw fabric layer. Raw materials obtained by adding additives such as lubricant and antistatic agent to the inorganic material and thermoplastic resin were extruded using a co-rotating twin-screw extruder, and then stretched 1.5 times by roll stretching to form the raw fabric layer of the present invention. The thickness of the raw fabric layer was set to 48 μm. The calcium carbonate powder used was one containing 90% by mass of calcium carbonate.
[0042] Next, inks for forming the surface layer 2 and back layer 5 were prepared. 70 parts by mass of kaolin clay and 30 parts by mass of precipitated calcium carbonate were used as pigments to prepare a uniform slurry of inorganic materials. Furthermore, styrene-butadiene latex was used as an aqueous binder with a content of 20% by mass, and this was added to the above-mentioned slurry and stirred with a mixer to prepare a uniform ink for forming the surface layer and back layer.
[0043] Next, the ink for forming the front and back layers was applied to the original layer. The prepared ink for forming the front and back layers was applied while applying corona discharge, and then dried to form the front and back layers. In this manner, the laminate sheet 15 of Example 1 was produced. The surface of the laminate sheet 15 having the front layer and the back layer had a water absorbency of 40 mm according to the JIS P8141 Klemm method.
[0044] [Example 2] The content of titanium oxide as the inorganic material of the raw sheet layer was 15 mass% relative to the mass of the raw sheet layer. In addition, the average particle diameter of titanium oxide as the inorganic material of the raw sheet layer was 1 μm and the maximum particle diameter was 50 μm. Except for this, the laminated sheet 15 of Example 2 was produced using the same materials and procedures as Example 1.
[0045] [Example 3] The inorganic material of the raw sheet layer was titanium oxide having an average particle size of 3 μm and a maximum particle size of 50 μm. Except for this, laminate sheet 15 of Example 3 was produced using the same materials and procedures as Example 1.
[0046] [Example 4] A laminated sheet 15 of Example 4 was produced using the same materials and procedures as in Example 1 except that antimony oxide was used as the inorganic material of the original sheet layer and the content of antimony oxide was 15 mass % relative to the mass of the original sheet layer.
[0047] [Example 5] A laminated sheet 15 of Example 5 was produced using the same materials and procedures as in Example 1 except that calcium carbonate was used as the inorganic material of the original sheet layer, and the content of calcium carbonate was 15 mass % relative to the mass of the original sheet layer.
[0048] [Example 6] A laminate sheet 15 of Example 6 was produced using the same materials and procedures as in Example 1, except that zinc borate was used as the inorganic material of the original layer, and the content of zinc borate was 15 mass % relative to the mass of the original layer.
[0049] [Example 7] The content of titanium oxide as the inorganic material of the raw sheet layer was 15 mass% relative to the mass of the raw sheet layer. In addition, polypropylene was used as the thermoplastic resin of the raw sheet layer. A laminated sheet 15 of Example 7 was produced using the same materials and procedures as Example 1 except for the above.
[0050] [Example 8] The content of titanium oxide as the inorganic material of the raw sheet layer was 15 mass% relative to the mass of the raw sheet layer. Polyethylene was used as the thermoplastic resin of the raw sheet layer. Except for the above, the laminated sheet 15 of Example 8 was produced using the same materials and procedures as in Example 1.
[0051] [Example 9] The content of titanium oxide as the inorganic material of the raw fabric layer was 15 mass% relative to the mass of the raw fabric layer. In addition, polyester was used as the thermoplastic resin of the raw fabric layer. A laminated sheet 15 of Example 9 was produced using the same materials and procedures as in Example 1.
[0052] [Example 10] The content of titanium oxide as the inorganic material of the raw fabric layer was 15 mass% relative to the mass of the raw fabric layer. The total content of the inorganic material and the thermoplastic resin was 90 mass% relative to the mass of the raw fabric layer. Except for this, the laminated sheet 15 of Example 10 was produced using the same materials and procedures as in Example 1.
[0053] [Example 11] A laminate sheet 15 of Example 11 was produced using the same materials and procedures as in Example 1, except that the total content of the inorganic material and the thermoplastic resin was 100 mass % relative to the mass of the original layer.
[0054] [Example 12] The content of titanium oxide as the inorganic material of the raw sheet layer was 15 mass % relative to the mass of the raw sheet layer. The thickness of the raw sheet layer was 50 μm. A laminated sheet 15 of Example 12 was produced using the same materials and procedures as in Example 1.
[0055] [Example 13] The thickness of the original layer was set to 250 μm. Except for that, the laminated sheet 15 of Example 13 was produced using the same materials and procedures as in Example 1.
[0056] [Example 14] The content of titanium oxide as the inorganic material of the raw sheet layer was set to 15% by mass relative to the mass of the raw sheet layer. In addition, the laminated sheet was made to meet the requirements for non-flammability certification at a high level in the heat generation test conforming to ISO5660-1. Except for this, the laminated sheet 15 of Example 14 was produced using the same materials and procedures as in Example 1.
[0057] [Example 15] Calcium carbonate with an average particle size of 4 μm and a maximum particle size of 50 μm was used as the inorganic material of the raw fabric layer, and the content of calcium carbonate was set to 60 mass% relative to the mass of the raw fabric layer. Polypropylene was used as the thermoplastic resin of the raw fabric layer. The total content of the inorganic material and the thermoplastic resin was adjusted to 98 mass% relative to the mass of the raw fabric layer. The thickness of the raw fabric layer was set to 150 μm. The laminated sheet also met the requirements for non-flammability certification at a high level in a heat generation test conforming to ISO5660-1. In this manner, a laminate sheet 15 of Example 15 was produced.
[0058] [Comparative Example 1] A laminated sheet 15 of Comparative Example 1 was produced using the same materials and procedures as in Example 1, except that the content of calcium carbonate as the inorganic material in the raw sheet layer was 14 mass % relative to the mass of the raw sheet layer.
[0059] (evaluation) With respect to the laminate sheets 15 of Examples 1 to 15 and Comparative Example 1 obtained by the above method, evaluations of water resistance and printability were carried out.
[0060] [Water resistance evaluation] Each sheet was immersed in water at 25° C. and left for 3 days, after which the condition was visually observed. ⊚: No peeling has occurred, and the film does not peel off even when scratched with a fingernail. ◯: No peeling occurred. △: The edge is curled up. ×: More than half peeled off
[0061] [Printability evaluation] The printed surface was observed with the naked eye and judged for unevenness in printing, printing density, smoothness of the printed surface, etc., with good prints being rated as ◎, completely poor prints being rated x, and the rest being rated as ◯ and △.
[0062] (Evaluation Results) Table 1 below shows the configuration of the laminate sheet of each of the Examples and Comparative Examples, and the evaluation results of the water resistance and printability of each of the Examples and Comparative Examples.
[0063] [Table 1]
[0064] As shown in Table 1, the evaluation results of Examples 1 to 15 and Comparative Example 1 show that when the content of inorganic material is within the range of 15 mass% or more and 90 mass% or less relative to the mass of the original fabric layer 1, as in Examples 1 to 15, the water resistance is higher than when the content of inorganic material is 15 mass% or less, as in Comparative Example 1. The laminate sheet of the present invention is not limited to the above-mentioned embodiments and examples, and various modifications are possible within the scope of the invention without impairing its characteristics. [Explanation of symbols]
[0065] 1…Original layer 2…Surface layer 5…Back layer 15...Laminated sheet
Claims
1. A raw material layer containing a thermoplastic resin and an inorganic material; A surface layer is formed on a first surface of the raw fabric layer, and a back surface layer is formed on a second surface of the raw fabric layer, the second surface being the surface opposite to the first surface, The content of the inorganic material is in the range of 15% by mass or more and 90% by mass or less with respect to the mass of the raw fabric layer, the front surface layer and the back surface layer are formed using a front surface layer forming ink or a back surface layer forming ink containing a pigment and a binder, The raw fabric layer is a single layer, A laminate sheet, characterized in that the thermoplastic resin contains only one of polypropylene, polyethylene, and polyester.
2. 2. The laminate sheet according to claim 1, wherein the inorganic material contains at least one of antimony trioxide, antimony soda, zirconium silicate, zirconium oxide, magnesium hydroxide, aluminum hydroxide, basic magnesium carbonate, borax, zinc borate, a complex of molybdenum trioxide or antimony dimolybdate with aluminum hydroxide, a complex of antimony trioxide with silica, a complex of antimony trioxide with zinc oxide, silicic acid of zirconium, a complex of a zirconium compound with antimony trioxide, and salts thereof.
3. 3. The laminate sheet according to claim 1, wherein the thermoplastic resin contains only polyester.
4. 3. The laminate sheet according to claim 1, wherein the thermoplastic resin contains only polyethylene terephthalate.
5. 5. The laminate sheet according to claim 1, wherein the thickness of the base layer is within a range of 50 μm or more and 250 μm or less.
6. 6. The laminate sheet according to claim 1, wherein the thickness of the base layer is within a range of 150 μm or more and 250 μm or less.
7. A raw material layer containing a thermoplastic resin and an inorganic material; A surface layer is formed on a first surface of the raw fabric layer, and a back surface layer is formed on a second surface of the raw fabric layer, the second surface being the surface opposite to the first surface, The content of the inorganic material is in the range of 15% by mass or more and 90% by mass or less with respect to the mass of the raw fabric layer, the front surface layer and the back surface layer are formed using a front surface layer forming ink or a back surface layer forming ink containing a pigment and a binder, The raw fabric layer is a single layer, The inorganic material is a laminated sheet containing at least one of antimony trioxide, antimony soda, zirconium silicate, zirconium oxide, magnesium hydroxide, aluminum hydroxide, basic magnesium carbonate, borax, zinc borate, a complex of molybdenum trioxide or antimony dimolybdate with aluminum hydroxide, a complex of antimony trioxide and silica, a complex of antimony trioxide and zinc oxide, silicic acid of zirconium, and a complex of a zirconium compound with antimony trioxide, and salts thereof.
Citation Information
Patent Citations
Synthetic paper
JP2000355076A
Printing sheet
JP2016168685A
Porous film capable of attaining oxidation treatment of carbon monoxide, and use thereof
WO2011096048A1
Thermosetting resin composition, dry film, cured product and printed wiring board
WO2016117237A1
Stretched multilayer resin film
WO2019188841A1