Polyester Film
Patent Information
- Application Number
- JP2020141514
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-30
- Filing Date
- 2020-08-25
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-08-25
AI Technical Summary
【0008】 本発明によれば、ポリエステルフィルムを粘着テープや離型用フィルムの基材として用いた後、その使用後においてポリエステルフィルム以外の層の除去性に優れたポリエステルフィルムを提供することができる。
Smart Images

Figure 0007581703000001 
Figure 0007581703000002 
Figure 0007581703000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyester film that is excellent in removing layers provided thereon. [Background technology]
[0002] Films are used in various industrial fields. In recent years, the evolution of IoT (Internet of Things) has led to a rapid increase in electronic devices such as CPUs installed in computers and smartphones, and the number of multilayer ceramic capacitors (MLCCs), which are important for driving electronic devices, has also increased explosively. The general manufacturing method for MLCCs is to laminate ceramic green sheets and electrodes on a release film, which has a release layer on a base film, and dry and harden the laminate, peel the laminate from the release film, stack multiple layers, and sinter. In this process, the release film is discarded as unnecessary material during the process.
[0003] In other words, the recent explosive increase in the number of MLCCs has resulted in an increase in the amount of release films discarded as unnecessary material, which is becoming an issue and putting a strain on the environment. From the perspective of releasability, the components of the release layer contained in the release film used in the MLCC manufacturing process generally have a different composition from the components that make up the film. Therefore, if a release film with a release layer is remelted as is, the components of the release layer will exist as foreign matter and it cannot be reused.
[0004] Patent Document 1 discloses a technique in which wax is kneaded into a film and used as a release film without providing a release layer. Patent Document 2 discloses a method in which a release film having a release layer is washed with a metal brush and the film is reused after the release layer is removed. Patent Document 3 discloses a method in which a water-soluble resin layer is provided between the release layer and the polyester film, and the release layer is removed by washing with water, and then the film is reused. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2013 / 15260 [Patent Document 2] JP 2012-171276 A [Patent Document 3] Patent No. 4284936 Summary of the Invention [Problem to be solved by the invention]
[0006] However, when wax is used as a release agent, the coating property of the slurry and the peelability of the green sheet dried from the slurry are not sufficient, and since the wax is a different substance from the components constituting the film, there is a problem that it becomes a foreign body when remelted and reused. In addition, when the release film is washed with a metal brush, there are problems that it cannot be washed uniformly and the removal property of the release layer is not sufficient. In addition, the method of providing a water-soluble resin layer between the release layer and the polyester film also has a problem that the removal property is not sufficient. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention has the following configuration. [I] A polyester film used in applications in which two or more layers are provided on at least one side of the polyester film and then the two or more layers are removed, the polyester film having an average Young's modulus of 3.5 GPa to 6.0 GPa in the direction parallel to the film surface where the Young's modulus is the highest and in the direction perpendicular to the parallel direction. [II] The polyester film according to [I], wherein the surface of the polyester film on which the resin layer is to be formed has an elastic modulus of 2.0 GPa to 4.5 GPa. [III] The polyester film according to [I] or [II], which contains at least two elements selected from the group consisting of alkali metal elements, alkaline earth metal elements, transition metal elements, and elements of groups 13 to 15. [IV] The polyester film according to any one of [I] to [III], which is used for applications in which an intermediate layer and a release layer are provided on at least one side of a polyester film, a releaseable layer is then provided on the release layer of the polyester film having the release layer, the releaseable layer is then released from the polyester film having the releaseable layer and the release layer, and the residue of the releaseable layer, the release layer and the intermediate layer are then removed from the polyester film having the release layer and intermediate layer from which the releaseable layer has been released. [V] The polyester film according to any one of [I] to [IV], which is used for the purpose of providing an intermediate layer and a release layer on at least one side of a polyester film, then providing a release layer on the release layer of the polyester film having the release layer, then releasing the release layer from the polyester film having the release layer and the release layer, then removing the residue of the release layer, the release layer, and the intermediate layer from the polyester film having the release layer and intermediate layer from which the release layer has been released, and then melting the polyester film from which the release layer, the release layer, and the intermediate layer have been removed, and then forming it into a film. [VI] A recycled polyester film obtained by providing two or more layers on at least one side of the polyester film described in any one of [I] to [V] and then removing said two or more layers, wherein the weight of the recycled polyester film is 95 to 101 parts by weight, based on 100 parts by weight of the polyester film described in any one of claims 1 to 5. Effect of the Invention
[0008] According to the present invention, it is possible to provide a polyester film which, after being used as a substrate for an adhesive tape or a release film, has excellent removability of layers other than the polyester film after use. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will be described in detail below with reference to specific examples.
[0010] The present invention relates to a polyester film used in applications in which two or more layers are provided on at least one side of the polyester film and then the two or more layers are removed. The polyester in the present invention is composed of a dicarboxylic acid component and a diol component. In this specification, the component refers to the smallest unit that can be obtained by hydrolyzing a polyester. Examples of the dicarboxylic acid component constituting such a polyester include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid, or ester derivatives thereof.
[0011] Examples of diol components constituting such polyesters include aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,2-butanediol, and 1,3-butanediol, alicyclic diols such as cyclohexanedimethanol and spiroglycol, and diols in which multiple units of the above-mentioned diols are linked together. Among these, from the viewpoints of mechanical properties and transparency, polyesters in which polyethylene terephthalate (PET), polyethylene-2,6-naphthalenedicarboxylate (PEN), and PET dicarboxylic acid components are copolymerized with isophthalic acid or naphthalenedicarboxylic acid, and PET diol components are copolymerized with cyclohexanedimethanol, spiroglycol, or diethylene glycol are copolymerized with a portion of the PET diol components are preferably used.
[0012] The polyester film of the present invention is used for the purpose of providing two or more layers on at least one side of the polyester film, and then removing the two or more layers. By providing a layer (hereinafter sometimes referred to as layer A) in contact with at least one side of the polyester film of the present invention and a layer (hereinafter sometimes referred to as layer B) disposed at the position furthest from the polyester film, and imparting functions such as release properties, adhesion, and light-shielding properties to layer B, it is possible to obtain a functional laminated film having functions such as a release film, an adhesive tape, light-shielding properties, and concealing properties. In addition, by configuring layer A to contain the substances shown below and washing it by the method described below, it is possible to remove layer A and layer B from the functional laminated film after use, and only the polyester film from which layer A and layer B have been removed can be taken out. Another layer may be laminated between layer A and layer B, or layer A and layer B may be laminated on both sides of the polyester film.
[0013] It is important that Layer A contains a water-soluble substance or a substance that absorbs a specific wavelength (e.g., infrared light or near-infrared light) and generates heat and vaporizes. When Layer A contains a water-soluble substance, by washing the laminated film including Layer A with water, Layer A dissolves in the water, causing peeling at the interface between the polyester film and Layer A, and only the polyester film can be taken out. When Layer A contains a substance that absorbs infrared light or near-infrared light, Layer A can be heated and vaporized by, for example, irradiating it with laser light of the relevant wavelength, and can be peeled off from the polyester film.
[0014] Examples of water-soluble substances include water-soluble metals such as Al, Cu, and Ti, and substances mainly composed of water-soluble polyester resins (chemical formula (1)), polyester urethane resins (chemical formula (2)), polyvinyl alcohol resins (chemical formula (3)), polyvinylpyrrolidone resins (chemical formula (4)), and starch (chemical formula (5)). The water-soluble substance referred to here refers to a substance whose weight change amount decreases by 15% by weight or more when immersed in water at 50°C for 10 minutes. Specifically, 5.0 g of particles with a particle size of 0.1 μm to 10 mm are immersed in 1 liter of water at 50°C for 10 minutes, and the powder remaining is separated by filtration, dried at 80°C for 30 minutes, and then the weight is measured to calculate the weight change amount. In addition, from the viewpoint of water solubility and the ease of handling water in which a water-soluble substance is dissolved, biodegradable polyvinyl alcohol resins and polyvinylpyrrolidone resins are preferred.
[0015] [ka]
[0016] R is any hydrocarbon group, and n is any natural number.
[0017] [ka]
[0018] In chemical formula (2), R1 is an organic chain containing a polyester bond, R2 is any hydrocarbon group, and n is any natural number.
[0019] [ka]
[0020] n and m are any natural numbers.
[0021] [ka]
[0022] n is any natural number.
[0023] [ka]
[0024] n is any natural number. Examples of substances that absorb infrared light or near-infrared light and vaporize by heat include metals such as Al, Cu, Au, Ag, and Ti, inorganic substances such as carbon black, and dyes such as sublimable phthalocyanine dyes. When Layer A contains a substance that absorbs infrared light or near-infrared light, a substance that is easily vaporized by the thermal energy generated by the substance absorbing infrared light or near-infrared light may be added to Layer A. As an easily vaporized substance, for example, nitrocellulose is preferably used.
[0025] The polyester film of the present invention needs to have an average value of the Young's modulus in the direction parallel to the film surface where the Young's modulus is the highest and the Young's modulus in the direction perpendicular to the direction, of 3.5 GPa to 6.0 GPa. If the average value of the Young's modulus is less than 3.5 GPa, when peeling off the layer A and the layer B from the polyester film, the polyester film is soft, and when the film is washed under tension, the film wrinkles under tension, and the flatness and extensibility of the film cannot be guaranteed in the film width direction, and the contact efficiency with water decreases, or the irradiation efficiency of light decreases, resulting in a decrease in cleaning efficiency and poor peelability. In particular, tension is concentrated in the center of the film width direction during film transport, and the flatness and extensibility at the center of the film width direction are poor, so that the peeling of the layer A and the layer B at the center of the film width direction tends to be insufficient.
[0026] Also, when it exceeds 6.0 GPa, when peeling off the layer A and layer B from the polyester film, the film is hard, and when washing the film while applying tension to the film, the film surface cannot be sufficiently stretched in the film width direction, and the contact efficiency with water decreases, and the light irradiation efficiency decreases, resulting in poor peelability. In particular, since tension is concentrated in the center of the film width direction during film transport, sufficient tension is not applied to the film width direction end, so that the stretchability and flatness are poor, and the peeling of the layer A and layer B at the film width direction end tends to be insufficient. More preferably, it is 3.8 to 6.0 GPa, and even more preferably, it is 4.0 to 5.5 GPa.
[0027] The polyester film of the present invention preferably has an elastic modulus of 2.0 GPa to 4.5 GPa on the film surface on the side where the layer A is provided. If the elastic modulus is less than 2.0 GPa, the film surface is soft, so that when the layer A and the layer B are peeled off from the polyester film, the polyester film may be damaged by the energy of vaporization of the layer A, or the surface may be easily deformed by water pressure, resulting in poor washability. If the elastic modulus is more than 4.5 GPa, the film surface is hard, so that when the layer A and the layer B are peeled off from the polyester film, the film is difficult to deform, and when the layer A is peeled off from the polyester film by washing with water, the contact area between the polyester film and the layer A is difficult to change, resulting in poor washability. More preferably, the elastic modulus is 2.2 to 4.5 GPa, and even more preferably, 3.0 to 4.5 GPa.
[0028] In order to set the Young's modulus of the polyester film of the present invention within the above-mentioned range, the production method for producing the film, particularly the stretching ratio, is important. A method for setting the Young's modulus of the polyester film within the above-mentioned range will be described below, but the present invention is not limited to the polyester film obtained by this method.
[0029] The polyester film of the present invention can be produced by a method (melt casting method) in which a dried raw material is heated and melted in an extruder as required, and extruded from a die onto a cooled casting drum to be processed into a sheet. The sheet is then cooled and solidified by static electricity on a drum cooled to a surface temperature of 20°C to 60°C to produce an unstretched sheet. The temperature of the casting drum is more preferably 20°C to 40°C, and even more preferably 20°C to 30°C.
[0030] Next, the unstretched sheet is biaxially stretched at a temperature T1n (°C) that satisfies the following formula (i), by 3.6 times or more in the longitudinal direction (MD) of the film, by 3.9 times or more in the transverse direction (TD) of the film, and by an area stretching ratio of 14.0 times to 20.0 times. (i)Tg(℃)≦T1n(℃)≦Tg+40(℃) Tg: Glass transition temperature of polyester film (℃) A method using the speed difference of the roll feeling is preferably used as a method of stretching the film in the longitudinal direction. In this case, it is also a preferred embodiment to stretch the film in a plurality of sections while fixing the film with nip rolls so that the film does not slip. By stretching in a plurality of sections, stress is efficiently and uniformly applied to the film, and orientation is easily imparted to the film, so that the Young's modulus can be set in a more preferred range.
[0031] Next, the biaxially stretched film is heat-set for 1 to 30 seconds at a temperature (Th0 (°C)) that satisfies the following formula (ii), and then uniformly and slowly cooled to room temperature to obtain a polyester film. (ii)Tmf-35(℃)≦Th0(℃)≦Tmf(℃) Tmf: Melting point of the film (℃) By obtaining a biaxially stretched film under the condition (ii), it is possible to impart an appropriate orientation to the film and adjust the Young's modulus to fall within a preferred range.
[0032] In order to make the surface elastic modulus of the polyester film of the present invention fall within the above range, in addition to the above-mentioned manufacturing method, it is also a preferred embodiment to add particles to the film.As the particles to be added, particles with high hardness are preferable, and diamond particles, zirconia particles, and aluminum oxide particles are preferably used.In particular, from the viewpoint of hardness and dispersibility in polyester, δ-crystal type alumina oxide particles are preferable.
[0033] Next, a method for providing Layer A and Layer B on the polyester film of the present invention will be described below.
[0034] When layer A is a metal, a general vacuum deposition method can be suitably used. When layer A is a metal, the thickness is preferably 50 nm or more. If it is less than 50 nm, the function of layer A may be insufficient and the peelability may be poor. There is no particular upper limit, but in consideration of productivity and handling, it is preferably 1000 nm or less.
[0035] When layer A contains a water-soluble resin, a method of dissolving the resin forming layer A in water and coating it on the polyester film of the present invention is preferably used. As a coating method, general coating methods such as gravure coating, Mayer bar coating, air knife coating, doctor knife coating, etc. can be used. When layer A is a water-soluble resin, the thickness is preferably 50 nm or more and 1000 nm or less. If it is less than 50 nm, the function of layer A may be insufficient and the peelability may be poor. If it exceeds 1000 nm, blocking may occur and the handleability may be reduced. When layer A is formed of a water-soluble resin, polyvinyl alcohol-based resins, starch, and polyvinylpyrrolidone-based resins that contain many hydroxyl groups in the molecule to improve water solubility are preferably used as the water-soluble resin from the viewpoint of biodegradability and removability, but polyvinyl alcohol-based resins are particularly preferably used from the viewpoint of removability.
[0036] When a polyvinyl alcohol resin is used as Layer A, the average degree of polymerization (the sum of n and m in chemical formula (3)) is 300 to 1000, more preferably 300 to 800, and even more preferably 400 to 600. When the average degree of polymerization exceeds 1000, the molecular chain of polyvinyl alcohol becomes long, and as a result, packing for crystallization is likely to occur even within the molecular chain, and the crystallinity may become high, and therefore the removability may be poor. When the average degree of polymerization is less than 200, when Layer A is provided on a polyester film by coating, the coatability may become poor, and lamination may not be possible, or the coatability may become poor, causing uneven distribution on the film and increasing the crystallinity, and the removability may be poor.
[0037] In addition, when a polyvinyl alcohol resin is used as layer A, the degree of saponification is preferably 30 mol% to 88 mol%, more preferably 60 mol% to 80 mol%. Polyvinyl alcohol has hydroxyl groups and acetate groups as side chains, and the higher the degree of saponification, the greater the amount of hydroxyl groups, which are small in bulk as functional groups. Therefore, when the degree of saponification is high, crystallization due to molecular chain packing tends to occur easily. When the degree of saponification exceeds 88 mol%, the degree of crystallization tends to increase, and the elution into water may decrease. When the degree of saponification is less than 30 mol%, the amount of acetate groups is large, and the water solubility may decrease, or the resistance to organic solvents may decrease.
[0038] In addition, it is also a preferred embodiment to use a copolymerized polyvinyl alcohol in which a functional group other than a hydroxyl group or an acetate group is copolymerized at the X position in the following chemical formula (6) as the side chain of the polyvinyl alcohol resin used as Layer A. In particular, a hydrophilic and bulky functional group, such as a 1,2-ethanediol group (chemical formula (7)) or a sodium sulfonate group (chemical formula (8)) can be introduced. The copolymerization amount is 3 mol% to 20 mol%, more preferably 5 mol% to 10 mol%, based on the entire polyvinyl alcohol resin. If the copolymerization amount exceeds 20 mol%, the coatability may be poor when Layer A is provided on a polyester film by coating, making lamination difficult.
[0039] [ka]
[0040] X is a functional group other than a hydroxyl group or an acetate group, and m, n, and l are any natural numbers.
[0041] [ka]
[0042] [ka]
[0043] When layer A contains a substance that absorbs infrared light or near infrared light, it is preferable to provide layer A by coating such as gravure coating, Mayer bar coating, air knife coating, doctor knife coating, spin coating, etc., from the viewpoint of containing a high concentration of the substance that absorbs infrared light or near infrared light. Examples of substances that absorb infrared light or near infrared light include inorganic substances such as carbon black, iron oxide, and indium tin oxide, cyanine compounds, phthalocyanine compounds, dithiol metal complexes, naphthoquinone compounds, diimmonium compounds, azo compounds, etc., and among them, compounds having a phthalocyanine skeleton that has sublimation properties are preferably used. In addition, it is also a preferred embodiment to use a substance that absorbs infrared light or near infrared light in combination with a substance that is easily vaporized by the heat energy generated by the substance absorbing infrared light or near infrared light, such as nitrocellulose. When Layer A contains a substance that absorbs infrared light or near-infrared light, Layer A is preferably composed of one or more resins selected from the group consisting of polyester, polycarbonate, epoxy resin, alkyd resin, acrylic resin, urea resin, and urethane resin, from the viewpoints of film-forming properties, chemical resistance, and dispersibility of the substance that absorbs infrared light or near-infrared light.
[0044] Next, a method for providing layer B will be described. Layer B is important for using the polyester film provided with layer A as a functional laminate film. As a component constituting layer B, when releasability is imparted to the laminate film consisting of the polyester film of the present invention and layer A, an alkyd resin-based release agent, a polyolefin-based release agent, a long-chain alkyl group-containing resin-based release agent, a fluorine-based release agent, a silicone-based release agent, a mixed or copolymerized organic and silicone resin-based release agent, etc. can be contained in layer B and used. When adhesiveness is imparted to the laminate film consisting of the polyester film of the present invention and layer A, a general acrylic adhesive, a silicone adhesive, or a rubber adhesive can be contained in layer B and used. In particular, a film provided with releasability can be suitably used as a release film for processing. When a film comprising layer A and layer B provided to the polyester film of the present invention is used as a release film for processing, it is particularly preferred because the polyester film (hereinafter sometimes referred to as a recycled polyester film) taken out by removing layer A and layer B from the release film for processing after use can be reused. The material to be released from the release film using the polyester film of the present invention is not particularly limited, but may be a ceramic green sheet.
[0045] When the polyester film of the present invention provided with layer A is used as a release film for processing, and only the polyester film of the present invention is taken out from the release film for processing after use and reused, it is preferable to melt the recycled polyester film and then form it into a film. This is a preferred embodiment because it can be used again as the film of the present invention by melting and forming it into a film.
[0046] When layer B provided on one side of the polyester film of the present invention contains a silicone release agent, particularly a release agent containing a dimethylsiloxane bond, the component containing the dimethylsiloxane bond is likely to become a foreign matter when mixed with the polyester film and remelted, which may accelerate the deterioration of the polyester or make extrusion molding difficult after melting. Therefore, the recovered polyester film of the present invention preferably has a residual amount of dimethylsiloxane of less than 0.5% by weight, more preferably less than 0.2% by weight, and even more preferably less than 0.05% by weight, based on the total weight of the recovered polyester film.
[0047] The weight of the recycled polyester film obtained by providing two or more layers on at least one side of the polyester film of the present invention and then removing the two or more layers is preferably 95 to 101 parts by weight, based on 100 parts by weight of the polyester film before providing two or more layers. If it is less than 95 parts by weight, it means that the recycled polyester film is damaged, and may deteriorate when remelted. If it exceeds 101 parts by weight, peeling of layer A and layer B is insufficient, and may deteriorate when remelted. More preferably, it is 99 to 101 parts by weight.
[0048] The polyester film of the present invention preferably contains at least two or more elements selected from the group consisting of alkali metal elements, alkaline earth metal elements, transition metal elements, and elements of groups 13 to 15. The polyester film of the present invention contains such elements, and thus the polyester film after removing layers A and B is remelted and the recycled polyester film is formed into a film. Although it is not clear what mechanism causes such an effect, the inventors presume that the above metal elements generally act as polymerization catalysts in polyesters, and therefore when the polyester film after removing layers A and B is remelted, the molecular chains cut by heat are promoted to polycondense again, resulting in good extrudability. The amount of metal contained is 100 ppm or more and 1000 ppm or less, more preferably 100 ppm or more and 500 ppm or less, in total. If the amount is less than 100 ppm, the action as a polymerization catalyst may be insufficient. If the amount exceeds 1000 ppm, the polyester may deteriorate during melting, possibly due to the promotion of reverse reaction. As the metal element, a Group 13 metal element or a transition metal element, which has a large valence and a high catalytic ability, is preferably used.
[0049] Next, a method for removing layer A and layer B will be described. When layer A is water-soluble, washing with water is a preferred embodiment. For example, it is preferable to subject a laminate film containing the polyester film of the present invention to a process of unwinding the laminate film, a process of supplying hot water to the surface of the unwound laminate film to peel off the surface laminated portion from the laminate film, and a process of winding up the polyester film after peeling. The temperature of the hot water is preferably 50°C or higher and 120°C or lower. If the temperature is less than 50°C, sufficient cleaning properties may not be obtained. If the temperature exceeds 120°C, the glass transition temperature of the polyester film may be exceeded, and the film may not be transported. The time that water contacts the surface of the laminate film is 5 seconds or more, preferably 10 seconds or more, and more preferably 30 seconds or more and 600 seconds or less. The process of supplying hot water to the surface of the unwound laminate film is preferably performed in a water tank, and the entire laminate film is preferably covered. By covering the entire laminate film with hot water, water pressure is generated in the direction of film flow, and when layer A is dissolved, layer B also easily moves from the film surface, improving cleaning properties. The speed at which the film is conveyed is 5 m / min or more, preferably 10 m / min or more, more preferably 20 m / min or more and 100 m / min or less. When conveying the laminated film provided with layers A and B in the process of removing layers A and B, it is also important to apply tension to the laminated film. By applying tension, the surface of the laminated film can be stretched and the washability can be improved. The tension is 5 N / m or more and 100 N / m or less, more preferably 20 N / m or more and 80 N / m or less, more preferably 30 N / m or more and 50 N / m or less. If it is less than 5 N / m, the surface of the laminated film may not be stretched and the washability may be poor. If it exceeds 100 N / m, the film may wrinkle, the surface may have poor stretchability, and the washability may be poor. By setting the Young's modulus of the polyester film in the above-mentioned range, it is possible to convey the film while removing layers A and B while applying a certain tension.
[0050] When the layer A contains a substance that absorbs infrared light or near infrared light, it is a preferred embodiment to irradiate with laser light or lamp light having an oscillation wavelength in infrared light or near infrared light. For example, it is preferred to subject a laminated film containing the polyester film of the present invention to a process of unwinding the laminated film, a process of irradiating the surface of the unwound laminated film with light to peel off the surface laminated part from the laminated film, and a process of winding up the polyester film after peeling. When using a laser light having an oscillation wavelength in infrared light or near infrared light, it may be a pulse wave or a continuous wave, but from the viewpoint of continuously and uniformly irradiating the film, it is preferable to use a continuous wave. In addition, the emission intensity of the laser light is preferably 5 W or more and 50 W or less from the viewpoint of the efficiency of the reactivity of the layer containing the infrared absorber. The irradiation time is not particularly limited, but it is preferable to irradiate for 0.1 seconds or more, and more preferably irradiate for 0.5 seconds or more and 100 seconds or less. The speed at which the film is transported is 5 m / min or more, preferably 10 m / min or more, more preferably 20 m / min or more and 100 m / min or less. When conveying the laminated film provided with layers A and B in the process of removing layers A and B, it is also important to apply tension to the laminated film. By applying tension, the surface of the laminated film can be stretched and the washability can be improved. The tension is 5 N / m to 100 N / m, more preferably 20 N / m to 80 N / m, more preferably 30 N / m to 50 N / m. If it is less than 5 N / m, the surface of the laminated film may not be stretched and the washability may be poor. If it exceeds 100 N / m, the film may wrinkle, the surface may not be stretched, and the washability may be poor. By setting the Young's modulus of the polyester film within the above-mentioned range, it is possible to convey the film while removing layers A and B while applying a certain tension.
[0051] As described above, the polyester film of the present invention has Layer A and Layer B on at least one side of the polyester film, and after using it as a release film for processing or as other functional layer films, Layer A and Layer B are washed away to easily leave only the polyester film of the present invention. In particular, the recovered polyester film obtained by a process including a step (step 1) of providing a layer (layer A) that contacts the polyester film and a release layer on at least one side of the polyester film, a step (step 2) of providing a release layer on the release layer of the polyester film having the release layer after step 1, a step (step 3) of releasing the release layer from the polyester film having the release layer and the release layer after step 2, and a step (step 4) of removing the residue of the release layer, the release layer, and layer A from the polyester film having the release layer and layer A from which the release layer has been released after step 3, has layer A and the release layer removed, so that the film can be reused as it is, or the film can be remelted and then chipped, and used as a recycled raw material for film production, and reused as a release film for the process.
[0052] [Characteristics evaluation method] A. Young's modulus of polyester film (GPa) Using an automatic film strength and elongation measuring device "Tensilon AMF / RTA-100" manufactured by Orientec Co., Ltd., a film cut to a width of 10 mm and a length of 150 mm was set in the device with a chuck distance of 50 mm, and a tensile test was performed under conditions of a tensile speed of 300 mm / min, a temperature of 23°C, and a relative humidity of 65%, and the tensile Young's modulus was calculated from the tangent to the rising part of the obtained load-elongation curve. The measurement was performed five times for each sample, and the evaluation was based on the average value.
[0053] The direction parallel to the film plane in which Young's modulus is highest is determined by setting one of the directions to 0° and measuring while changing the direction in 10° increments from -90° to 90° within the film plane. Next, the Young's modulus is determined in a direction perpendicular to the direction in question (direction a) within the same plane, and the average value between the direction in which Young's modulus is highest and the direction perpendicular to the direction in question is taken as Young's modulus.
[0054] B. Surface modulus of polyester film (GPa) The sample is left in an atmosphere at room temperature of 23°C and humidity of 65% for 24 hours, and then measurements are carried out in that atmosphere under the following conditions. Equipment: Bruker scanning probe microscope (SPM) NanoScopeV DimensionIcon Probe: Si cantilever (spring constant approx. 40N / m) Scanning modes: Tapping mode, Force volume (contact mode) Scanning range: 5μm square (scanning lines: 512) The surface elastic modulus obtained at each point is all averaged to obtain the surface elastic modulus.
[0055] C. Thickness of each layer (μm) When the polyester film was a laminated film, the thickness of each layer was measured by the following method: A cross section of the film was cut out with a microtome in a direction parallel to the width direction of the film, and the cross section was observed with a scanning electron microscope at a magnification of 5000 times to measure the thickness of each laminated layer.
[0056] D. Intrinsic viscosity (IV) The polyester film of the present invention is dissolved in 100 ml of orthochlorophenol (solution concentration C = 1.2 g / dl), and the viscosity of the solution at 25°C is measured using an Ostwald viscometer. The viscosity of the solvent is also measured in the same manner. Using the solution viscosity and solvent viscosity thus obtained, [η] (dl / g) is calculated according to the following formula (a), and the obtained value is taken as the intrinsic viscosity (IV). (a) ηsp / C=[η]+K[η] 2 C (Here, ηsp = (solution viscosity (dl / g) / solvent viscosity (dl / g)) - 1, and K is the Huggins constant (assumed to be 0.343).)
[0057] E. Metal element content Alkali metal elements are quantified by atomic absorption spectrometry (Uchida Seisakusho: polarized Zeeman atomic absorption spectrometer 180-80. Frame: acetylene-air), and other metal elements are quantified using a Rigaku Denki Corporation fluorescent X-ray analyzer (model number: 3270).
[0058] F. Residue Evaluation Method The polyester film after removing Layer A and Layer B is evaluated by the following methods (F-1), (F-2), and (F-3). (F-1) Absorbance measurement by infrared spectroscopy Using the following equipment and conditions, measure the absorbance of the polyester film after removing layers A and B. If there is little absorbance at the wavelengths characteristic of layers A and B, this indicates that layers A and B have been removed. Using a Frontier FTIR manufactured by PerkinElmer Co., Ltd. and a UATR IR unit, the medium crystal is diamond / ZnSe, and the spectral intensity is measured by the attenuated total reflection method (ATR method). The resolution of the spectrometer is 1 cm -1 The spectrum is measured with 16 integrations. The absorbance (arb.unit) at the angular wavelength is calculated and judged as follows: A: absorbance less than 0.04 B: absorbance is 0.04 or more and less than 0.08 C: absorbance is 0.08 or more (F-2) Si element content measurement (atomic%) by photoelectron spectroscopy Using the following equipment and conditions, the elemental concentrations (atomic%) of the polyester film after removing layers A and B are determined. If the concentrations of elements characteristic of layers A and B are low, this indicates that layers A and B have been removed. Equipment: K-Alpha+ (manufactured by Thermo Scientific) Excitation X-ray: Monochromatic Al Kα 1,2 Rays (1486.6 eV) X-ray diameter: 400 μm Photoelectron escape angle: 90° (detector angle relative to sample surface) A: Element concentration is less than 0.5 atomic% B: Element concentration is 0.5 atomic % or more and 1.0 atomic % or less C;Si element content is 1.0 atomic% or more (F-3) Weight of recycled polyester film The polyester film before providing layers A and B is cut into a 10 cm square, dried at 100°C for 30 minutes, and then left for 24 hours in an atmosphere at room temperature of 23°C and humidity of 65%, after which the weight is measured and designated as W1. After providing layers A and B and removing layers A and B, the polyester film is cut into a 10 cm square, dried at 100°C for 30 minutes, and then left for 24 hours in an atmosphere at room temperature of 23°C and humidity of 65%, after which the weight is measured and designated as W2. The parts by weight of W2 when W1 is 100 parts by weight is calculated and determined as follows:
[0059] A: 99.5 parts by weight or more and 100.5 parts by weight or less B: 99.0 parts by weight or more but less than 99.5 parts by weight, more than 100.5 parts by weight but not more than 101.0 parts by weight C: less than 99.0 parts by weight or more than 101.0 parts by weight.
[0060] G.Recovery melt film forming After removing layers A and B, the polyester film is pulverized and dried at 180°C for 2 hours, then fed into an extruder and melt-extruded at 280°C, after which it is formed into a sheet on a cast drum cooled to 25°C, and the intrinsic viscosity of the sheet obtained is measured by the method in D above. The difference (ΔIV) between the intrinsic viscosity IV(R) and the intrinsic viscosity IV(I) of the polyester film is calculated by the following formula (b), and judged as follows: (b) ΔIV = IV(R) - IV(I) A: The difference in intrinsic viscosity is 0.05 or less B: The difference in intrinsic viscosity is greater than 0.0 and less than 0.1. C: The difference in intrinsic viscosity is more than 0.1.
[0061] H. Melting point of polyester film Tm (℃) The samples are measured according to the method based on JIS K 7122 (1999) using a differential scanning calorimeter "Robot DSC-RDC220" manufactured by Seiko Instruments Inc. and Disk Session "SSC / 5200" for data analysis, as described below. Weigh out 5 mg of sample into a sample pan and heat the sample from 25°C to 300°C at a heating rate of 10°C / min (1st RUN). Obtain a differential scanning calorimetry chart (vertical axis represents heat energy, horizontal axis represents temperature) for the 1st RUN. Determine the peak temperature of the endothermic peak in the differential scanning calorimetry chart for the 1st Run and define it as Tm (°C).
[0062] I. Amount of dimethylsiloxane (wt%) Weigh out 20 g of the sample and dissolve it in orthochlorophenol. The insoluble matter is separated by centrifugation and dried for 2 hours at 150°C. A certain amount of the resulting insoluble matter is weighed out and pressure decomposed with sulfuric acid and nitric acid, after which the ash is dissolved with sodium carbonate and boric acid, and then dissolved with dilute nitric acid to a constant volume. The silicon element concentration is measured using ICP emission spectrometry (ICP emission spectrometer PS3520VDDII, manufactured by Hitachi High-Tech Science Corporation), converted to dimethylsiloxane, and expressed as a percentage of the sample amount, and judged as follows:
[0063] A: Less than 0.05% by weight B: 0.05% by weight or more and less than 0.2% by weight C: 0.2% by weight or more and less than 0.5% by weight D: 0.5% by weight or more. EXAMPLES
[0064] The present invention will be described below with reference to examples, but the present invention is not necessarily limited to these.
[0065] [Production of PET-1] Terephthalic acid and ethylene glycol were polymerized in the usual manner using antimony trioxide and magnesium acetate tetrahydrate as catalysts to obtain melt-polymerized PET. The resulting melt-polymerized PET had a glass transition temperature of 81°C, a melting point of 255°C, an intrinsic viscosity of 0.65, and a terminal carboxyl group content of 20eq. / t.
[0066] [Production of PET-2] A melt-polymerized PET was obtained in the same manner as PET-1, except that 0.1 μm δ-crystalline alumina particles were added to the polymerization of PET-1 so that the content was 0.1%. The glass transition temperature of the obtained melt-polymerized PET was 81°C, the melting point was 255°C, the intrinsic viscosity was 0.65, and the amount of terminal carboxyl groups was 20 eq. / t.
[0067] [Production of PET-3] Terephthalic acid and ethylene glycol were polymerized in the usual manner using antimony trioxide, magnesium acetate tetrahydrate, and aluminum acetate as catalysts to obtain melt-polymerized PET. The glass transition temperature of the resulting melt-polymerized PET was 81°C, the melting point was 255°C, the intrinsic viscosity was 0.65, and the amount of terminal carboxyl groups was 22eq. / t.
[0068] [Production of PET-4] Terephthalic acid and ethylene glycol were polymerized in the usual manner using antimony trioxide, magnesium acetate tetrahydrate, and tetrabutyl titanate as catalysts to obtain melt-polymerized PET. The glass transition temperature of the resulting melt-polymerized PET was 81°C, the melting point was 255°C, the intrinsic viscosity was 0.65, and the amount of terminal carboxyl groups was 18eq. / t.
[0069] [Production of PET-5] A melt-polymerized PET was obtained in the same manner as PET-1, except that the amount of cyclohexylene dimethanol copolymerized during polymerization of PET-1 was 20 mol% relative to the diol component. The glass transition temperature of the obtained melt-polymerized PET was 77°C, the melting point was 250°C, the intrinsic viscosity was 0.65, and the amount of terminal carboxyl groups was 23 eq. / t.
[0070] [Production of PET-6] Terephthalic acid and ethylene glycol were polymerized in the usual manner using antimony trioxide as a catalyst to obtain melt-polymerized PET. The resulting melt-polymerized PET had a glass transition temperature of 81°C, a melting point of 255°C, an intrinsic viscosity of 0.65, and a terminal carboxyl group content of 20eq. / t.
[0071] [Production of PEN] Dimethyl 2,6-naphthalenedicarboxylate and ethylene glycol were subjected to an ester exchange reaction using manganese acetate as a catalyst. After the ester exchange reaction was completed, PEN was obtained by a conventional method using antimony trioxide as a catalyst. The glass transition temperature of the obtained PEN was 124°C, the melting point was 265°C, the intrinsic viscosity was 0.62, and the terminal carboxyl group concentration was 25eq. / t.
[0072] [Preparation of Coating A] 100 parts by weight of an addition reaction type silicone resin release agent (manufactured by Dow Corning Toray Silicones Co., Ltd., product name LTC750A) and 2 parts by weight of a platinum catalyst (manufactured by Dow Corning Toray Silicones Co., Ltd., product name SRX212) were mixed in toluene as a solvent to give a solids content of 5% by weight, to obtain Coating A.
[0073] [Preparation of Coating Agent B] Polyvinyl alcohol "Poval 5-74" (average polymerization degree 500, degree of saponification 74 mol%) manufactured by Kuraray Co., Ltd. was dissolved in water to a concentration of 4% by weight, to obtain Coating Agent B.
[0074] [Preparation of Coating Agent C] 97.98 parts of n-butyl acrylate, 2 parts of acrylic acid, and 0.02 parts of 4-hydroxybutyl acrylate were polymerized in an ethyl acetate solution at 80°C for 8 hours using 0.2 parts of azobisisobutyronitrile as a polymerization initiator to obtain an acrylic polymer with a weight average molecular weight of 900,000. 100 parts of the acrylic polymer were added with 5 parts of polymerized rosin ester (trade name "D-135" manufactured by Arakawa Chemical Industries, Ltd.), 20 parts of disproportionated rosin ester (trade name "KE-100" manufactured by Arakawa Chemical Industries, Ltd.), 25 parts of styrene resin (trade name "FTR6100" manufactured by Arakawa Chemical Industries, Ltd.), and 1 part of terpene phenol resin (trade name "YP90LL" manufactured by Mitsui Chemical Industries, Ltd.), and ethyl acetate was added to prepare an adhesive solution with a solid content of 40%. Further, 0.8 parts of an isocyanate-based crosslinking agent (product name "NC40" manufactured by DIC Corporation) was added and mixed with stirring until homogeneous, thereby obtaining coating agent C, which is an adhesive.
[0075] [Preparation of Coating D] 60 parts of 878B manufactured by Taihei Chemical Products Co., Ltd. as a color chip containing carbon black and nitrocellulose, 20 parts of Epicoat 828 manufactured by Mitsubishi Chemical Corporation as an epoxy resin, 19 parts of melamine resin (U-Ban 2061 manufactured by Mitsui Chemicals Inc.) as a hardener, and 1 part of catalyst (Light Ester PM manufactured by Kyoei Chemical Co., Ltd.) were dissolved in a solvent (90 parts of methyl isobutyl ketone, 10 parts of dimethylformamide) to a solids concentration of 10%, to obtain Coating D.
[0076] [Preparation of Coating Agent E] Polyvinyl alcohol "OKS-8089" manufactured by Mitsubishi Chemical Corporation (saponification degree 88 mol%, average polymerization degree 450, copolymerization amount of 1,2-ethanediol 6 mol%) was dissolved in water to make a concentration of 4.0% by weight, to obtain Coating Agent E.
[0077] [Preparation of Coating Agent F] Polyvinyl alcohol "ASP-05" manufactured by Nippon Vinyl Acetate & Poval Co., Ltd. (saponification degree 88 mol%, average polymerization degree 500, copolymerized with 3 mol% sodium sulfonate) was dissolved in water to a concentration of 4.0% by weight to obtain Coating Agent G.
[0078] [Preparation of Coating Agent G] Polyvinyl alcohol "JP-15" (average polymerization degree 1700, degree of saponification 88 mol%) manufactured by Nippon Vinyl Acetate & Poval Co., Ltd. was dissolved in water to a concentration of 4.0% by weight to obtain Coating Agent G.
[0079] [Preparation of dielectric paste] 100 parts by weight of barium titanate (manufactured by Fuji Titanium Kogyo Co., Ltd., product name HPBT-1), 10 parts by weight of polyvinyl butyral (manufactured by Sekisui Chemical Co., Ltd., product name BL-1), 5 parts by weight of dibutyl phthalate, and 60 parts by weight of toluene-ethanol (weight ratio 30:30) were added to glass beads with a number average particle size of 2 mm, mixed and dispersed in a jet mill for 20 hours, and then filtered to prepare a paste-like dielectric paste.
[0080] Example 1 PET-1 was vacuum dried at 160°C for 2 hours, then put into an extruder, melted at 280°C, and extruded through a die onto a casting drum with a surface temperature of 25°C to produce an unstretched sheet. The sheet was then preheated with a heated roll group, stretched 3.8 times in the longitudinal direction (MD direction) at a temperature of 90°C, and then cooled with a roll group at a temperature of 25°C to obtain a uniaxially stretched film. The obtained uniaxially stretched film was stretched 4.0 times in the width direction (TD direction) perpendicular to the longitudinal direction in a heating zone at a temperature of 100°C in a tenter while holding both ends of the film with clips. Further, the film was heat-set for 10 seconds at a temperature of 230°C in a heat treatment zone in the tenter. Next, the film was uniformly cooled slowly in the cooling zone, and then wound up to obtain a polyester film with a thickness of 30 μm. The properties of the obtained polyester film were as shown in the table.
[0081] On one side of the obtained polyester film, aluminum was vapor-deposited as layer A to a thickness of 0.1 μm under a reduced pressure atmosphere of 10 Pa or less. Furthermore, coating material A was applied as layer B to the layer A side by a gravure coating method so that the coating thickness after drying would be 1.0 μm, and a release film roll for process use was obtained. A dielectric paste was applied as a release object to the obtained release film for process use by a die coating method so that the thickness after drying would be 1.0 μm. Thereafter, the dielectric was released from the obtained laminate, and the release object was peeled off to obtain a release film roll for process use. The film roll was introduced into a water washing device equipped with an unwinding and winding device, and washed in 100° C. water for 2 minutes under a tension of 30 N / m, and the polyester film from which layers A and B had been removed was collected.
[0082] After removing layers A and B, the surface of the recovered polyester film was subjected to XPS measurement of the concentration (atomic%) of Al element, the main component of layer A, as the residue of layer A, and the concentration (atomic%) of Si element, the main component of layer B, as the residue of layer B. Since the residue of both layers A and B was small and the weight change of the polyester film was also small, the film had excellent removability of layers A and B. In addition, the film from which layers A and B were removed was cut into a size of 2 cm square, vacuum dried at 160 ° C for 2 hours, and then put into an extruder, melted at 280 ° C, and extruded through a die onto a casting drum with a surface temperature of 25 ° C to produce an unstretched sheet. The intrinsic viscosity of the produced unstretched sheet was within a range that would not be problematic as a melt-cast film.
[0083] Example 2 A laminated film was obtained in the same manner as in Example 1, with an aluminum layer provided as Layer A on one side of the polyester film, and the layer A was coated with Coating Agent C as Layer B by gravure coating so that the coating thickness after drying would be 1.0 μm, to obtain an adhesive film. The obtained adhesive film was washed with water in the same manner as in Example 1, and the polyester film from which Layer A and Layer B had been removed was collected.
[0084] After removing layers A and B, the surface of the recovered polyester film was subjected to XPS to measure the concentration (atomic%) of Al element, which is the main component of layer A, as the residue of layer A, and IR to measure the absorbance at 1040 cm-1, which is the absorption band of acrylic acid, which is the main component of layer B, as the residue of layer B. Since the residue of both layers A and B was small and the weight change of the polyester film was also small, the film had excellent removability of layers A and B. In addition, the film from which layers A and B were removed was cut into a size of 2 cm square, vacuum dried at 160 ° C for 2 hours, and then put into an extruder, melted at 280 ° C, and extruded through a die onto a casting drum with a surface temperature of 25 ° C to produce an unstretched sheet. The intrinsic viscosity of the produced unstretched sheet was within a range that would not be problematic as a melt-cast film.
[0085] Example 3 Coating agent B was used as layer A on one side of the polyester film obtained in the same manner as in Example 1, and the coating thickness after coating was 0.1 μm by gravure coating to obtain a laminated polyester film. Furthermore, coating agent A was applied as layer B on the layer A side by gravure coating to a coating thickness after drying of 1.0 μm to obtain a release film roll for processing. Dielectric paste was applied as a release object to the obtained release film for processing by die coating to a thickness after drying of 1.0 μm. Thereafter, the dielectric was released from the obtained laminate, and the release object was peeled off to obtain a release film roll for processing. The film roll was introduced into a water washing device equipped with an unwinding and winding device, and washed while immersing in 100° C. water for 2 minutes under a tension of 30 N / m, and the polyester film from which layers A and B were removed was collected.
[0086] After removing layers A and B, the surface of the recovered polyester film was measured for the absorbance at 3400 cm-1, which is the absorption band of the hydroxyl group of polyvinyl alcohol, the main component of layer A, by IR as the residue of layer A, and the concentration (atomic%) of the Si element, the main component of layer B, was measured for the residue of layer B by XPS. Since the residue of both layers A and B was small and the weight change of the polyester film was also small, the film had excellent removability of layers A and B. In addition, the film from which layers A and B were removed was cut into a size of 2 cm square, vacuum dried at 160 ° C for 2 hours, and then put into an extruder, melted at 280 ° C, and extruded through a die onto a casting drum with a surface temperature of 25 ° C to produce an unstretched sheet. The intrinsic viscosity of the produced unstretched sheet was in a range that was acceptable for a melt-cast film.
[0087] (Examples 4 to 7) Except for changing the constituent components and film-forming conditions as shown in the table, a polyester film from which Layer A and Layer B were removed was obtained in the same manner as in Example 3. In Example 7, 50 parts by weight each of PET-1 and PET-2 were used.
[0088] In Example 4, the longitudinal stretching process was divided into three sections in stretching the polyester film, and the Young's modulus of the polyester film was set in a more preferable range, so that the film had excellent removability of Layer A and Layer B.
[0089] In Example 5, the Young's modulus of the polyester film was slightly low, and some residues of Layers A and B were observed, but the polyester film from which Layers A and B had been removed was able to withstand melt film formation.
[0090] In Examples 6 and 7, the elastic modulus of the film surface could be adjusted to a preferred range by adding alumina particles to the polyester film, and the films were excellent in the removability of Layer A and Layer B.
[0091] Example 8 Coating agent D was used as layer A on one side of the polyester film prepared in the same manner as in Example 1, and the coating thickness after coating was 0.1 μm by gravure coating to obtain a laminated polyester film. Furthermore, coating agent A was applied as layer B on the layer A side by gravure coating to a coating thickness after drying of 1.0 μm to obtain a release film roll for processing. Dielectric paste was applied as a release object to the obtained release film for processing by die coating to a thickness after drying of 1.0 μm. Thereafter, the dielectric was released from the obtained laminate, and the release object was peeled off to obtain a release film roll for processing. The film roll was introduced into a device with an unwinding and winding device, and while stretching the film under a tension of 30 N / m, laser light was irradiated at an intensity of 10 W and a frequency of 300 kHz using a semiconductor laser PLM-20M (wavelength 1064 nm) manufactured by Physical Photon Co., Ltd., to recover the polyester film from which layers A and B were removed.
[0092] After removing layers A and B, the surface of the recovered polyester film was measured for the absorbance at 850 cm-1, which is the absorption band of nitrocellulose, the main component of layer A, by IR as the residue of layer A, and the concentration (atomic%) of the Si element, the main component of layer B, was measured for the residue of layer B by XPS. Since the residue of both layers A and B was small and the weight change of the polyester film was also small, the film had excellent removability of layers A and B. In addition, the film from which layers A and B were removed was cut into a size of 2 cm square, vacuum dried at 160 ° C for 2 hours, and then put into an extruder, melted at 280 ° C, and extruded through a die onto a casting drum with a surface temperature of 25 ° C to produce an unstretched sheet. The intrinsic viscosity of the produced unstretched sheet was within a range that would not be problematic as a melt-cast film.
[0093] (Examples 9 and 10) Layer A and Layer B were formed in the same manner as in Example 8, except that the film-forming conditions for the polyester film were changed as shown in the table. After using the film as a release film for processing, Layer A and Layer B were removed to obtain a polyester film.
[0094] In Example 9, the Young's modulus of the polyester film was slightly low, and some residues of Layers A and B were observed, but the polyester film from which Layers A and B had been removed was able to withstand melt casting.
[0095] In Example 10, the longitudinal stretching process was divided into three sections in stretching the polyester film, and the Young's modulus of the polyester film was adjusted to a more preferable range, so that the film had excellent removability of Layer A and Layer B.
[0096] (Examples 11 to 13) Except for changing the constituent components as shown in the table, Layer A and Layer B were provided in the same manner as in Example 3 in Examples 11 and 12, and in the same manner as in Example 8 in Example 13. After using the film as a release film for processing, Layer A and Layer B were removed to recover the polyester film.
[0097] In Example 11, aluminum acting as a catalyst in the molten polyester was added, and therefore the intrinsic viscosity of the unstretched sheet melt-formed from the recovered polyester film was high. In Examples 12 and 13, titanium acting as a catalyst in the molten polyester was added, and therefore the intrinsic viscosity of the unstretched sheet melt-formed from the recovered polyester film was high, as in Example 11.
[0098] (Examples 14, 15, and 17) A polyester film from which layers A and B had been removed was obtained in the same manner as in Example 3, except that the coating agent used as layer A was changed to coating agent E in Example 14, coating agent F in Example 15, and coating agent G in Example 17.
[0099] In Examples 14 and 15, bulky functional groups were introduced into the side chains of the polyvinyl alcohol resin, resulting in films with excellent removability of Layer A and Layer B. In particular, Example 15, in which the average degree of polymerization and the degree of saponification were within preferred ranges and further an ionic functional group was introduced, showed excellent removability of Layer A and Layer B.
[0100] In Example 17, since the average degree of polymerization of the polyvinyl alcohol resin was large, the removability of Layers A and B was somewhat inferior, but was within a range that could withstand practical use.
[0101] (Example 16) Coating agent F was used as layer A on one side of the polyester film obtained in the same manner as in Example 1, and the coating thickness after coating was 0.1 μm by gravure coating to obtain a laminated polyester film. Furthermore, coating agent A was applied as layer B on the layer A side by gravure coating to a coating thickness after drying of 1.0 μm to obtain a release film roll for processing. An adhesive layer made of coating agent C was applied to the obtained release film for processing as a release object by die coating to a thickness after drying of 1.0 μm. Thereafter, the obtained laminate was attached to a polarizing plate made of triacetyl cellulose and polyvinyl alcohol, and the adhesive layer made of coating agent C was released and the release object was peeled off to obtain a release film roll for processing. The film roll was introduced into a water washing device equipped with an unwinding and winding device, and washed while immersing in 100° C. water for 2 minutes under a tension of 30 N / m, and the polyester film from which layers A and B had been removed was collected.
[0102] After removing layers A and B, the surface of the recovered polyester film was measured for the absorbance at 3400 cm-1, which is the absorption band of the hydroxyl group of polyvinyl alcohol, the main component of layer A, by IR as the residue of layer A, and the concentration (atomic%) of the Si element, the main component of layer B, was measured for the residue of layer B by XPS. Since the residue of both layers A and B was small and the weight change of the polyester film was also small, the film had excellent removability of layers A and B. In addition, the film from which layers A and B were removed was cut into a size of 2 cm square, vacuum dried at 160 ° C for 2 hours, and then put into an extruder, melted at 280 ° C, and extruded through a die onto a casting drum with a surface temperature of 25 ° C to produce an unstretched sheet. The intrinsic viscosity of the produced unstretched sheet showed excellent properties as a melt-cast film.
[0103] (Example 18) A polyester film was obtained by removing Layer A and Layer B in the same manner as in Example 3, except that PET-6 was used as the constituent component of the polyester film. The film had excellent removability of Layer A and Layer B, and was slightly inferior in recovery melt film-forming property, but was durable for practical use. Comparative Example 1 Layer A and Layer B were provided in the same manner as in Example 3, except that PET-1 was formed into a polyester film under the stretching conditions shown in the table, and the polyester film was used as a release film for processing. After that, Layer A and Layer B were removed, and the polyester film was recovered. The polyester film had a low Young's modulus, and the flatness of the central part of the film deteriorated due to tension during film transport, resulting in poor extensibility, resulting in a recycled polyester film in which the removability of Layers A and B was insufficient. Furthermore, the obtained recycled polyester film was melt-formed into an unstretched sheet in the same manner as in Example 3. The removal of Layers A and B was insufficient, and the polyester deteriorated during melting, resulting in a low intrinsic viscosity of the unstretched sheet, which was not suitable for practical use.
[0104] Comparative Example 2 The PEN was vacuum dried at 160°C for 2 hours, and then fed into an extruder, melted at 300°C, and extruded through a die onto a casting drum with a surface temperature of 25°C to produce an unstretched sheet. This was then stretched under the conditions shown in the table to produce a polyester film. Layers A and B were provided in the same manner as in Example 3, except that this was used as a release film for processing, and the polyester film was then recovered by removing Layers A and B. The polyester film had a high Young's modulus, and the flatness of the film edge was deteriorated due to tension during film transport, resulting in poor extensibility, resulting in a recovered polyester film in which the removal of Layers A and B was insufficient. Furthermore, the recovered polyester film obtained was subjected to melt film formation in the same manner as in Example 3 to produce an unstretched sheet. The removal of Layers A and B was insufficient, and the polyester deteriorated during melting, resulting in a low intrinsic viscosity of the unstretched sheet, which was not suitable for practical use.
[0105] Comparative Example 3 A polyester film obtained in the same manner as in Example 1 was provided with layer B on one side of the polyester film without providing layer A, to obtain a release film for process use. As in Example 1, a dielectric paste was applied as a release object by die coating so that the thickness after drying would be 1.0 μm. Thereafter, the dielectric was released from the obtained laminate, and the release object was peeled off to obtain a release film roll for process use. The film roll was introduced into a water washing device equipped with an unwinding and winding device, washed in 100° C. water for 2 minutes under a tension of 30 N / m, and the polyester film was collected.
[0106] The surface of the recovered polyester film was treated as the residue of layer B, and the concentration (atomic %) of the Si element, which is the main component of layer B, was measured by XPS. There was a large amount of residue of layer B, and the weight change of the polyester film was also large, indicating that the removability of layers A and B was poor. In addition, the recovered polyester film was cut into pieces 2 cm square, vacuum dried at 160°C for 2 hours, and then put into an extruder, melted at 280°C, and passed through a die, but a large amount of foreign matter was generated and it was not possible to produce an unstretched sheet.
[0107] Comparative Example 4 A pressure-sensitive adhesive film was obtained by providing layer B on one side of a polyester film obtained in the same manner as in Example 2 without providing layer A. As in Example 2, the polyester film was introduced into a water washing device equipped with an unwinding and winding device, washed in 100°C water for 2 minutes under a tension of 30 N / m, and the polyester film was recovered.
[0108] The surface of the recovered polyester film was measured for the residue of layer B, which is the main component of layer B, by IR. There was a large amount of residue of layer B, and the weight change of the polyester film was also large, indicating that the removability of layers A and B was poor. In addition, the recovered polyester film was cut into a size of 2 cm square, vacuum dried at 160°C for 2 hours, and then put into an extruder, melted at 280°C, and passed through a die, but a large amount of foreign matter was generated and it was not possible to produce an unstretched sheet.
[0109] Comparative Example 5 The release film roll for the process from which the release object obtained in Comparative Example 3 was peeled off was unwound at a speed of 15 m / min using a film unwinding device, a winding device, and a cleaning brush provided between them, while being unwound at a speed of 15 m / min to peel off the release layer. The cleaning brush provided between them was made of a stainless steel wire with a wire diameter of 0.1 mm and a bristle length of 15 mm, finished to an outer diameter of 180 mm. A hard chrome-plated free roll was used as a backup roll when the brush contacted the film. The concentration (atomic%) of the Si element, which is the main component of layer B, was measured by XPS as the residue of layer B. There was a lot of residue of layer B, and the weight change of the polyester film was also large, and it was found that the removability of layers A and B was poor. In addition, the recovered polyester film was cut into a size of 2 cm square, vacuum dried at 160 ° C for 2 hours, and then fed into an extruder, melted at 280 ° C, and passed through a die, whereupon a large amount of foreign matter was generated and an unstretched sheet could not be produced.
[0110] [Table 1]
[0111] [Table 2]
[0112] [Table 3]
[0113] [Table 4]
[0114] [Table 5]
[0115] [Table 6]
[0116] [Table 7]
[0117] [Table 8]
[0118] [Table 9]
[0119] [Table 10]
[0120] [Table 11]
[0121] [Table 12] [Industrial Applicability]
[0122] The polyester film of the present invention is excellent in the removability of Layer A and Layer B after providing Layer A and Layer B. Therefore, Layer B can be given functionality such as releasability and used as a functional film. In particular, when releasability is given, it can be suitably used as a release film for the manufacturing process of multilayer ceramic capacitors (MLCCs) using a dielectric paste as the release material. In addition, since the polyester film can be easily recovered from the release film after use in the MLCC manufacturing process, the polyester film can be easily reused as a raw material for melt film formation.
Claims
1. The polyester film is used for applications in which two or more layers are provided on at least one side of the polyester film, and then the two or more layers are removed, the polyester film having an average Young's modulus of 3.5 GPa to 6.0 GPa in a direction parallel to the film surface in which the Young's modulus is the highest and in a direction perpendicular to the parallel direction, and a layer (layer A) that contains a water-soluble substance and is in contact with the polyester film on at least one side of the polyester film.
2. 2. The laminate film according to claim 1, wherein the surface of the polyester film on which the layer is to be formed has an elastic modulus of 2.0 GPa to 4.5 GPa.
3. A laminated film as described in claim 1 or 2, wherein the polyester film contains at least two or more elements selected from the group consisting of alkali metal elements, alkaline earth metal elements, transition metal elements, and elements of groups 13 to 15.
4. A laminate film as described in any of claims 1 to 3, for use in providing a release layer on layer A of a laminate film, then providing a release layer on the release layer of the laminate film having said release layer, then releasing the release layer from the laminate film having said release layer and the release layer, and then removing residues of the release layer, the release layer and layer A from the laminate film having the release layer and layer A from which the release layer has been released.
5. A laminated film as claimed in any one of claims 1 to 4, for use in the application of providing a release layer on layer A of a laminated film, providing a release layer on the release layer of the laminated film having said release layer, releasing the release layer from the laminated film having said release layer and the release layer, removing residues of the release layer, the release layer and layer A from the laminated film having the release layer and layer A from which the release layer has been released, and then melting the polyester film from which the release layer, release layer and layer A have been removed, and then forming it into a film.
6. A laminated film described in any one of claims 1 to 5, wherein layer A contains a polyvinyl alcohol-based resin.
7. The laminated film according to claim 6, wherein the polyvinyl alcohol resin has a degree of saponification of 30 to 88 mol%.
8. A recycled polyester film obtained by providing one or more layers on layer A of the laminate film according to any one of claims 1 to 5, and then removing layer A and the one or more layers, wherein the weight of the recycled polyester film is 95 to 101 parts by weight, when the weight of the polyester film of the laminate film according to any one of claims 1 to 5 is taken as 100 parts by weight.
9. A method for producing recycled polyester film, comprising the steps of: A step (step 1) of providing a release layer on layer A of the laminate film according to any one of claims 1 to 5; After the step 1, a step (step 2) of providing a release layer on the release layer of the laminated film having the release layer; After the step 2, a step (step 3) of releasing the release layer from the laminate film having the release layer and the release layer; A step (step 4) of removing the residue of the release layer, the release layer and the layer A from the laminate film having the release layer and the layer A from which the release layer has been released after the step 3; A method for producing recycled polyester film.
Citation Information
Patent Citations
Method for recovering mold release film
JP2002265665A
Method for manufacturing ceramic green sheet
JP2004050681A
Manufacturing method for mold-release polyester film
JP2010090219A
Apparatus and method for forming thermoplastic resin film
JP2012171276A
Release film
JP2014152240A