Thermoplastic resin film, laminate and component

The laminated thermoplastic resin film with optimized resin and particle composition addresses the challenges of thickness and weight, offering superior vibration damping and thermal energy conversion across a wide temperature range without plasticizer contamination.

JP7581716B2Active Publication Date: 2024-11-13TORAY INDUSTRIES INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020152693
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-26
Filing Date
2020-09-11
Publication Date
2024-11-13
Estimated Expiration
2040-09-11

AI Technical Summary

Technical Problem

Existing vibration damping materials face challenges in achieving sufficient damping performance without increasing thickness and weight, and they often suffer from reduced performance at low temperatures or contamination issues due to plasticizer bleed-out.

Method used

A laminated thermoplastic resin film with a structure of five or more layers, containing at least one layer with 1% by weight particles, and optimized resin composition to enhance damping properties, including specific resin types and particle types with controlled glass transition temperatures and aspect ratios, to improve vibration damping across a wide temperature range.

Benefits of technology

The film provides excellent vibration damping properties with efficient energy conversion to thermal energy through shear friction, maintaining performance across varying temperatures and preventing plasticizer contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581716000001
    Figure 0007581716000001
Patent Text Reader

Abstract

To provide a thermoplastic resin film excellent in damping property.SOLUTION: A thermoplastic resin film has a laminate structure obtained by laminating five or more layers. Particles are contained in at least one layer, a content of the particles is 1 wt.% or more with respect to the whole film, the film is stuck onto SPCC steel plate with a width of 10 mm, a length of 220 mm and a thickness of 0.8 mm, and an average value of a loss coefficient determined by a half-value width method from a third-order or more antiresonance peak of a frequency response function obtained on the condition of 23°C and 2-12,800 Hz by a center vibration method is 0.006 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic resin film, a laminate, and a member that contain particles and have a laminate structure. [Background technology]

[0002] With the recent advancement and complexity of social life and the development of science and technology in automobiles, electrical and electronic equipment, railway vehicles, architecture, aircraft, etc., there are increasing demands for vibration and noise issues such as micro-vibration countermeasures for advanced communication equipment and electronic equipment, practical application of electric vehicles and AI-driven unmanned vehicles, the demand for flame-retardant, highly damping materials in high-performance ships, and applications to space-related equipment, and the performance required for vibration damping equipment and damping materials used there is becoming more complex. Meanwhile, in earthquake-prone Japan, urgent and effective vibration damping measures are also required for earthquake resistance measures. Vibration damping materials are required to demonstrate vibration control properties in environments suited to their respective applications, such as temperature and vibration frequency.

[0003] Materials with high vibration-damping properties include those in which particles or plasticizers are added to rubber, asphalt, urethane foam, elastomers, etc. (Patent Documents 1 and 2). Materials with high sound-absorbing properties include those in which plasticizers are added to polyvinyl acetal (Patent Document 3). Materials with vibration-damping properties that do not use plasticizers include those in which plate-shaped or needle-shaped particles are contained within a film (Patent Document 4). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-181155 A [Patent Document 2] JP 2018-012785 A [Patent Document 3] International Publication No. 2010-095749 [Patent Document 4] International Publication No. 2018-079161 Summary of the Invention [Problem to be solved by the invention]

[0005] The technologies described in Patent Documents 1 and 2 require thicker and heavier vibration-damping materials to ensure sufficient vibration-damping performance, which poses a challenge for application to electric and electronic devices that are becoming increasingly smaller and automobiles that are becoming increasingly lighter.

[0006] Furthermore, the technology described in Patent Document 3 makes it possible to obtain a transparent and relatively thin sound-absorbing film, but the addition of a large amount of plasticizer essentially makes it impossible to avoid deterioration and contamination due to bleed-out.

[0007] The technology described in Patent Document 4 does not have sufficient vibration damping properties (tan δ, an index of vibration damping properties, is at most about 0.12). In addition, there is a problem that the vibration damping properties are significantly reduced over a wide temperature range, particularly in the range below 0 degrees. [Means for solving the problem]

[0008] The present invention aims to solve the above problems by providing a thermoplastic resin film having a laminated structure of 5 or more layers, containing particles in at least one layer, with the particle content being 1% by weight or more relative to the entire film, and having an average loss factor of 0.006 or more determined by a half-width method from third-order or higher anti-resonance peaks of a frequency response function obtained by a central excitation method at 23°C and 2 Hz to 12,800 Hz. Effect of the Invention

[0009] According to the present invention, a thermoplastic resin film having excellent vibration damping properties can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the embodiments of the present invention will be described in detail. However, the present invention should not be construed as being limited to the embodiments including the following examples, and various modifications are naturally possible within the scope of the invention that can achieve the object of the invention and does not deviate from the gist of the invention.

[0011] The present invention relates to a thermoplastic resin film. The thermoplastic resin in the present invention is a resin that exhibits plasticity when heated, and representative examples of such resins include polymers such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polyethylene α,β-dicarboxylate, and p-hexahydroxylylene terephthalate, polymers made of 1,4-cyclohexanedimethanol, poly-p-ethyleneoxybenzoate, polyarylate, polycarbonate, and copolymers thereof, polyesters having ester bonds in the main chain, further polyamides having amide bonds in the main chain, such as nylon 6, nylon 66, nylon 610, nylon 12, and nylon 11, polyethylene, polypropylene, and the like. These include polyolefins, which are primarily composed of hydrocarbons, such as propylene, ethylene-vinyl acetate copolymer, polymethylpentene, polybutene, polyisobutylene, and polystyrene; polyethers, such as polyethersulfone (PES), polyphenylene oxide (PPO), polyether ether ketone (PEEK), polyethylene oxide, polypropylene oxide, and polyoxymethylene; halogenated polymers, such as polyvinyl chloride, polyvinylidene chloride, polyvinylidene fluoride, and polychlorotrifluoroethylene; polyphenylene sulfide (PPS), polysulfone, and their copolymers and modified products, and polyimide (PI).

[0012] In the present invention, from the viewpoint of film formability and durability, thermoplastic resins including polyester, polyolefin, polyphenylene sulfide and polyimide are preferred, and among these, polyester is more preferred.

[0013] The polyester in the present invention is obtained by polycondensation of a dicarboxylic acid component and a diol component. In this specification, the term "component" refers to the minimum unit obtainable by hydrolysis of a polyester.

[0014] Examples of dicarboxylic acid components constituting such polyesters include aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, sebacic acid, dodecanedioic acid, dimer acid, eicosanedioic acid, pimelic acid, azelaic acid, methylmalonic acid, and ethylmalonic acid; alicyclic dicarboxylic acids such as adamantanedicarboxylic acid, norbornenedicarboxylic acid, isosorbide, cyclohexanedicarboxylic acid, and decalindicarboxylic acid; and aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 5-sodiumsulfoisophthalic acid, phenylendanedicarboxylic acid, anthracenedicarboxylic acid, phenanthrenedicarboxylic acid, and 9,9'-bis(4-carboxyphenyl)fluorene acid, or ester derivatives thereof.

[0015] Examples of diol components constituting such polyesters include aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,2-butanediol, and 1,3-butanediol; alicyclic diols such as cyclohexanedimethanol, spiroglycol, and isosorbide; diols such as bisphenol A, 1,3-benzenedimethanol, 1,4-benzenedimethanol, 9,9'-bis(4-hydroxyphenyl)fluorene, and aromatic diols; and diols in which a plurality of the above-mentioned diols are linked together.

[0016] The polyester used in the present invention may be copolymerized with monofunctional compounds such as lauryl alcohol and phenyl isocyanate, or may be copolymerized with trifunctional compounds such as trimellitic acid, pyromellitic acid, glycerol, pentaerythritol, and 2,4-dioxybenzoic acid, within the range where the polymer is substantially linear without excessive branching or crosslinking. In addition to the acid component and the diol component, aromatic hydroxycarboxylic acids such as p-hydroxybenzoic acid, m-hydroxybenzoic acid, and 2,6-hydroxynaphthoic acid, as well as p-aminophenol and p-aminobenzoic acid, can be copolymerized. As the polyester, polyethylene terephthalate and polyethylene naphthalate are preferably used. The polyester may also be a copolymer or modified product of these. From the viewpoint of improving vibration damping, it is also preferable to use a mixture of two or more resins.

[0017] In particular, it is preferable to combine a resin having a glass transition temperature in the range from the lowest temperature to the center temperature in the temperature range in which vibration damping properties are desired to be exhibited with a resin having a glass transition temperature in the range from the center temperature to the highest temperature. From the above viewpoint, polyester resins copolymerized with at least one of a diol having an alkyl group having 3 or more carbon atoms and / or an alkylene group having 3 or more carbon atoms and a dicarboxylic acid having an alkyl group having 3 or more carbon atoms and / or an alkylene group having 3 or more carbon atoms, and thermoplastic resins copolymerized with a diol or dicarboxylic acid having a bicyclic structure sharing one or more carbon or nitrogen atoms, such as 1,4:3,6-dianhydro-D-glucitol, 1,4:3,6-dianhydro-D-mannitol, or 1,4:3,6-dianhydro-L-iditol, are particularly preferable.

[0018] The thermoplastic resin film of the present invention is required to have an average loss factor of 0.006 or more calculated by the half-width method from the third or higher mode of the anti-resonance peak at 23°C and 2 to 21800 Hz measured by the central vibration method. The loss factor is an index of the viscoelasticity of the film, and the higher the loss factor, the higher the viscosity of the film, and the more efficiently the vibration energy can be converted into heat energy. If the loss factor is less than 0.006, the vibration damping may be insufficient. The loss factor is preferably 0.007 or more, more preferably 0.008 or more, and particularly preferably 0.009 or more. On the other hand, the upper limit of the loss factor is not particularly limited, but is 1 or less from the viewpoint of feasibility. The method of setting the loss factor within the range is not particularly limited, but includes a method of using a resin with low viscosity in the room temperature range, a method of adding a low-molecular plasticizer, a method of adding particles, and the like. Among them, the method of using a resin with low viscosity in the room temperature range and the method of adding particles are preferable because there is no concern about contamination due to bleeding out of the plasticizer. In addition, a method using shear friction at the interface by laminating five or more layers of low-viscosity resin or resin containing flat particles is particularly preferable because it can efficiently absorb vibration energy. In this case, it is preferable to use a resin with a low temperature (Tmax) at which the crystal melting enthalpy is maximized, as described below, because this can further increase energy absorption at the interface.

[0019] In the thermoplastic resin film of the present invention, the Tmax of the resin as the main component is preferably 210°C or less. This is because, as described below, when shear friction occurs at the resin-particle interface and the resin-resin interface, stress is applied locally to the resin within each interface, generating heat energy. In this case, when the Tmax of the resin as the main component is 210°C or less, a local decrease in viscosity occurs, enabling efficient absorption of vibration energy. The Tmax of the resin as the main component is 210°C or less here means that the peak top temperature of the peak with the largest ΔH (crystal melting enthalpy) calculated from the peak area of ​​the melting peak in the differential scanning calorimetry (DSC) chart of the 1st RUN obtained by heating from 25°C to 300°C at a heating rate of 20°C / min by differential scanning calorimetry (DSC) is 210°C or less. The measurement method of DSC will be described later. The Tmax of the resin as the main component is preferably 200°C or less, more preferably 190°C or less. On the other hand, if Tmax is 100°C or less, it may lead to deformation during processing or reduced durability.

[0020] In addition, from the viewpoint of vibration damping, the thermoplastic resin film of the present invention has one endothermic peak observed in the range of 50°C to 300°C in the differential scanning calorimetry chart of the 1st RUN obtained by heating from 25°C to 300°C at a heating rate of 20°C / min by differential scanning calorimetry (DSC), or has two or more endothermic peaks, and the peak top temperature of the peak with the second largest ΔH is less than 210°C. By making the Tmax of the resin contained in the second largest amount after the main component less than 210°C, vibration damping can be improved. The peak top temperature of the peak with the second largest ΔH is more preferably less than 200°C, and particularly preferably less than 190°C. On the other hand, if Tmax is less than 100°C, deformation during processing or deterioration of durability may occur.

[0021] In addition, the thermoplastic resin film of the present invention preferably contains two or more resins with different glass transition temperatures from the viewpoint of improving vibration damping in a wide temperature range. Since the viscosity of the thermoplastic resin decreases near the glass transition temperature, vibration damping is improved by absorbing vibration energy. When the thermoplastic resin constituting the film has only one glass transition temperature, the vibration damping is excellent near that temperature, but may be poor in other temperature ranges (temperature dependency of vibration damping becomes large). In this case, if the thermoplastic resin constituting the film contains two or more resins with different glass transition temperatures, there are multiple temperature ranges where vibration damping is high, and the viscosity decreases between each glass transition temperature because the resin (molecule) that has already decreased in viscosity is dragged by the other resin (molecule), so that the temperature dependency of vibration damping is suppressed while maintaining high vibration damping. In particular, from the viewpoint of improving vibration damping in the actual use temperature range, it is preferable that the glass transition temperatures of two or more components contained in the thermoplastic resin film are all in the range of -40°C to 60°C. It is more preferable that the glass transition temperatures of all the resin components contained in the thermoplastic resin film are in the range of −40° C. to 60° C. On the other hand, from the viewpoints of film formability and durability, it is also a preferable embodiment that the glass transition temperature of some of the components in the thermoplastic resin film is 50° C. or higher.

[0022] The thermoplastic resin film of the present invention has a laminated structure of 5 or more layers, at least one of which contains particles, and the particle content must be 1% by weight or more relative to the entire film of the present invention. By containing particles at 1% by weight or more, when the thermoplastic resin film containing particles vibrates, shear friction occurs at the interface between the particles and the resin, and vibration energy is converted into thermal energy, thereby improving vibration damping properties. The particle content is preferably 1% by weight or more and 60% by weight or less. By making the particle content 60% by weight or less, it is possible to suppress the occurrence of breakage and obtain good film formability when producing a thermoplastic resin film by the production method described below. More preferably, it is 10% by weight or more and 50% by weight or less, and even more preferably, it is 15% by weight or more and 40% by weight or less. The particles referred to here include, for example, metals such as gold, silver, copper, platinum, palladium, rhenium, vanadium, osmium, cobalt, iron, zinc, ruthenium, praseodymium, chromium, nickel, aluminum, tin, zinc, titanium, tantalum, zirconium, antimony, indium, yttrium, and lanthanum, metal oxides such as zinc oxide, titanium oxide, cesium oxide, antimony oxide, tin oxide, indium-tin oxide, yttrium oxide, lanthanum oxide, zirconium oxide, aluminum oxide, magnesium oxide, and silicon oxide, metal fluorides such as lithium fluoride, magnesium fluoride, aluminum fluoride, and cryolite, metal phosphates such as calcium phosphate, carbonates such as calcium carbonate, sulfates such as barium sulfate, nitrides such as boron nitride and carbon nitride, silicates such as talc, mica, and kaolin, and carbon-based compounds such as carbon, fullerene, carbon fiber, carbon nanotubes, graphene, and graphite. Two or more of these particles may be used.

[0023] Moreover, the particles contained in the thermoplastic resin film of the present invention are preferably non-spherical particles (particularly needle-shaped or plate-shaped particles) with an aspect ratio (major axis / minor axis) of 2 or more. When the non-spherical particles have an aspect ratio (major axis / minor axis) of 2 or more, the particles are aligned in the orientation direction when the thermoplastic resin film of the present invention is oriented in a uniaxial or biaxial direction, so that the vibration damping property due to shear friction between the particles and the resin can be further improved. The aspect ratio (major axis / minor axis) is more preferably 5 or more, and even more preferably 10 or more. There is no particular upper limit, but it is preferably 10,000 or less.

[0024] In addition, the particles contained in the thermoplastic resin film of the present invention preferably have a layered structure. The layered structure here refers to a structure in which flat primary particles exist as secondary particles in which the minor axis is approximately parallel to the primary particles. Here, the "flat primary particles" refers to particles in which, when the particle is surrounded by a rectangular parallelepiped so as to have the smallest volume, the longest side is the major axis and the shortest side is the minor axis, the length of the minor axis is half or less of the major axis, and the length of the side perpendicular to the major axis and the minor axis is 1.5 times or more of the minor axis but less than the length of the major axis. The elements constituting the primary particles are strongly bonded to each other, for example, by covalent bonds or metal bonds. The stacking of the primary particles constituting the secondary particles attracts each other with a weaker force than that of the elements constituting the primary particles, for example, by van der Waals forces or hydrogen bonds. When the particles have such a layered structure, it is possible to convert vibration energy into heat energy by shear friction between the layers of the particles themselves, thereby improving vibration damping properties.

[0025] Whether or not a particle has a layered structure can be determined by powder X-ray diffraction. Specifically, when the interplanar spacing d(001) of a particle is measured by powder X-ray diffraction, if the Debye rings are anisotropic and the interplanar spacing d(001) peak is in the range of 0.5 nm to 50 nm, the particle can be determined to be layered.

[0026] The thermoplastic resin film of the present invention must be laminated with 5 or more layers. Preferably, 9 or more layers, more preferably 17 or more layers, and even more preferably 51 or more layers. By laminating, vibration damping can be improved by shear friction between the layers. There is no particular upper limit, but from the viewpoint of productivity, it is preferable that the number of layers is 5000 or less. The thickness of each layer is preferably greater than the thickness of the particles. The thickness of a particle refers to the short diameter of the particle when the particles are not aggregated (when they exist as primary particles), and refers to the shortest side when the aggregate is surrounded by a rectangular parallelepiped so as to minimize the volume when multiple particles are aggregated to form a layered structure.

[0027] If each layer is thinner than the thickness of the particles, the particles may disturb the interface between the layers, resulting in a decrease in vibration damping. The thickness of each layer is preferably 20 times or less than the thickness of the particles. If the thickness of each layer is more than 20 times the thickness of the particles, the arrangement of the particles may be disturbed, resulting in a decrease in vibration damping due to shear friction. From the above viewpoint, the thickness of each layer is preferably 10 times or less than the thickness of the particles, more preferably 2 times or less than the thickness of the particles. The thickness of the particles can be measured by X-ray diffraction.

[0028] The thermoplastic resin film of the present invention is preferably oriented by stretching at least in one direction from the viewpoint of durability and vibration damping of the film. By stretching the film, the particles contained therein are aligned in the stretching direction, and vibration damping due to shear friction is further improved. A biaxially oriented film oriented in two axial directions is more preferable. It is further preferable to stretch the film in both directions by 1.5 times or more, and particularly preferable to stretch the film in both directions by 2.0 times or more.

[0029] In the case where the thermoplastic resin film of the present invention is oriented in at least one axial direction, when the film is cut in a direction parallel to the strongest orientation direction and perpendicular to the film thickness direction, and the shape of the particles in the film cross section is observed, it is preferable that t1 / t2 is 0.01 to 0.95, where t1 is the length of the particle in the film thickness direction and t2 is the length parallel to the film's strongest orientation direction. t1 / t2 is an index that indicates the extent to which non-spherical particles are aligned in the film orientation direction in the direction in which the film is most strongly oriented. When t1 / t2 is 1, it indicates that the particles contained in the film are spherical particles or that the particles contained in the film are not aligned at all in the direction in which the film is most strongly oriented. When the value of t1 / t2 is small, it indicates that particles with a high aspect ratio (major axis / minor axis) are aligned in the direction in which the film is most strongly oriented. When the value of t1 / t2 is large (exceeding 1), it indicates that particles with a high aspect ratio (major axis / minor axis) are aligned in the film thickness direction. When t1 / t2 is 0.95 or less, it indicates that the area of ​​contact between the particles and the resin is large, and the shear friction at the interface between the particles and the resin is large, improving the vibration damping. Even if t1 / t2 is greater than 1, the contact area between the particles and the resin is large, but the particles may break through the interface between the layers. When t1 / t2 is 0.01 or less, the particles are easily cracked, and the vibration damping may be reduced. From the above viewpoint, t1 / t2 is preferably 0.01 or more and 0.90 or less, more preferably 0.01 or more and 0.80 or less, and particularly preferably 0.01 or more and 0.49 or less.

[0030] In addition, when the thermoplastic resin film of the present invention is biaxially oriented, when the film is cut in a direction perpendicular to the strongest orientation direction and perpendicular to the film thickness direction, and the shape of the particles in the film cross section is observed, the length of the particle in the film thickness direction is t3, and the length in the direction perpendicular to the strongest orientation direction is the minor axis t4 of the particle, and it is preferable that t3 / t4 is 0.01 or more and 1.00 or less. t3 / t4 is an index that indicates the extent to which non-spherical particles are aligned in the film orientation direction perpendicular to the direction in which the film is most strongly oriented. When t3 / t4 is 1, it indicates that the particles contained in the film are spherical particles or that the particles contained in the film are not aligned at all in the direction perpendicular to the direction in which the film is most strongly oriented. When the value of t1 / t2 is small, it indicates that particles with a high aspect ratio (major axis / minor axis) contained in the film are aligned in the direction perpendicular to the direction in which the film is most strongly oriented. When the value of t1 / t2 is large (exceeding 1), it indicates that particles with a high aspect ratio (major axis / minor axis) are present in the film and arranged in the film thickness direction. When t3 / t4 is 1.00 or less, it indicates that the area of ​​the particles that contact the resin is large, and the shear friction at the interface between the particles and the resin increases, improving vibration damping. When t3 / t4 is 0.01 or less, the particles are easily cracked, and vibration damping may decrease. It is preferably 0.01 or more and 0.95 or less, more preferably 0.01 or more and 0.80 or less, and even more preferably 0.01 or more and 0.79 or less.

[0031] The method for setting t1 / t2 and t3 / t4 in the above-mentioned ranges is not particularly limited, but an example is a method in which particles having a high aspect ratio (major axis / minor axis) are used as the particles to be contained in the film, and the film stretching conditions are controlled to align the particles in the film orientation direction.

[0032] The density of the particles contained in the thermoplastic resin film of the present invention is 1.0 g / cm 3 More than 5.0g / cm 3 It is preferable that the density of the particles is 1.0 g / cm or less. 3If the particle density is less than 5.0 g / cm, the inertial force of the particles is small, and it may not be possible to obtain sufficient frictional energy due to shear friction with the resin that constitutes the film. 3 If the density exceeds 1.1 g / cm, the vibration of the particles will be small, and it may not be possible to obtain sufficient frictional energy due to shear friction with the resin that constitutes the film. In addition, problems such as damage to the razor blade used to cut the film during processing may occur. A density of 1.1 g / cm is more preferable. 3 More than 4.0g / cm 3 Is less than or equal to In addition, when the thermoplastic resin film of the present invention is measured for tensile dynamic viscoelasticity at 10 Hz, the ratio (E" / E') of the loss modulus E" to the storage modulus E' preferably has two or more maximum values ​​in the range of -40 to 60°C. Both the loss modulus E" and the storage modulus E' are indicators of the viscoelasticity of the film material, and the larger the ratio (E" / E'), the higher the viscosity. High viscosity makes it easier to absorb external vibrations and convert them into thermal energy, resulting in high vibration damping properties. However, when the ratio (E" / E') of the loss modulus E" to the storage modulus E' has one maximum value in the range of -40 to 60°C, the temperature dependency of E" / E' becomes large, and the temperature range of use as a vibration damping material may become narrow. Therefore, it is preferable that E" / E' has two or more maximum values ​​in the range of -40 to 60°C. It is preferable that E" / E' has at least one maximum value in the range of -40 to 5°C and at least one maximum value in the range of 5°C to 60°C, since this provides good vibration damping properties over a wide temperature range. More preferably, the temperature difference between the two maximum values ​​is 10°C or more, and particularly preferably, the temperature difference between the two maximum values ​​is less than 80°C. There are no particular limitations on the method for setting the temperatures of the respective maximum values ​​within the above ranges, but examples of the method include using a resin whose glass transition temperature is within the above range, or using a plasticizer.

[0033] When the thermoplastic resin film of the present invention has a tensile dynamic viscoelasticity measured at 10 Hz, the ratio of loss modulus E" to storage modulus E' (E" / E') preferably has a minimum value of 0.15 or more in the range of 15 to 40°C. If the minimum value of E" / E' in the range of 15 to 40°C is 0.15 or more, stable vibration damping properties can be obtained in the room temperature range. It is more preferably 0.16 or more, and even more preferably 0.19 or more. There is no particular upper limit, but it is preferably 1.0 or less. There is no particular limit to the method for setting E" / E' in this range, but a method using a resin with low viscosity in this temperature range can be preferably used.

[0034] Furthermore, when the thermoplastic resin film of the present invention has a tensile dynamic viscoelasticity measured at 10 Hz, the ratio of loss modulus E" to storage modulus E' (E" / E') preferably has a minimum value of 0.10 or more in the range of -25 to 15°C. If the minimum value of E" / E' in the range of -25 to 15°C is 0.10 or more, the film can have stable vibration damping properties in the low temperature range. The minimum value is more preferably 0.11 or more, and even more preferably 0.14 or more. There is no particular upper limit, but it is preferably 0.50 or less.

[0035] The method for setting E" / E' in the above range is not particularly limited, but examples of the method include using a resin having a glass transition temperature in the above range or close to the above range, adjusting the compatibility of each component when a resin mixture is used, and using a plasticizer.

[0036] When the thermoplastic resin film of the present invention is measured for tensile dynamic viscoelasticity at 10 Hz, the ratio of the loss modulus E" to the storage modulus E' (E" / E') divided by the thickness (mm) of the film is preferably 0.3 ( / mm) or more in the range of 15 to 40°C. The vibration-damping material may be used to suppress vibration in small electric and electronic devices, and it is preferable to set Tmin to 0.3 or more because it is possible to achieve both thinning and vibration-damping properties. There is no particular limitation on the method for setting Tmin within the range, but it can be adjusted by stretching the film about 1.1 to 3.0 times. In addition, when a resin with high crystallinity is used, the loss modulus is reduced due to oriented crystallization caused by stretching, and E" / E' is reduced, which may significantly reduce Tmin, so it is preferable to use a resin containing an amorphous component.

[0037] In addition, in the thermoplastic resin film of the present invention, the thickness of the film is preferably 50 μm or more and 2000 μm or less. If it is 50 μm or less, the strength and durability of the film may become a problem. If it is 2000 μm or more, the film may become too thick and its applications may be limited. More preferably, it is 100 μm or more and 1500 μm or less, and even more preferably, it is 200 μm or more and 1000 μm or less.

[0038] Depending on the application and processing method of vibration-damping and sound-absorbing materials, tear resistance may be required. In particular, when used as an interlayer for laminated glass, it is required that even if glass breaks during a disaster, fragments are not likely to scatter, that is, the film has high tear resistance and does not propagate the tear, so that the bonded fragments do not scatter. More specifically, it is preferable that the tear propagation resistance in the longitudinal direction and width direction is 5000g / mm or more. From the above viewpoint, the thermoplastic resin film of the present invention is preferably laminated in 9 to 501 layers. It is more preferable that the thermoplastic resin film is laminated in 9 to 51 layers. By laminating 9 or more layers, tearing is suppressed between the layers, so that tear resistance may be improved. On the other hand, by making the number of layers 501 or less, the thickness of each layer is ensured, and the decrease in tear resistance can be reduced.

[0039] The thermoplastic resin film of the present invention is mainly intended to attenuate vibration energy by shear friction between particles and resin, and is suitable for use in vibration damping and sound absorption applications, but it can also be used for vibration prevention, sound insulation, and shock absorption applications that take into account the vibration energy reflection effect. In addition, by providing an adhesive layer on at least one side, it can be used as an easy-to-use adhesive vibration damping material.

[0040] The thermoplastic resin film of the present invention can be suitably used for automobile parts, building parts, home appliance parts, and furniture parts by making use of its characteristics. In particular, since the thermoplastic resin is used, molding is easy, and therefore the film can be suitably used for automobile parts such as floors, doors, outer panel dashes, floor tunnels, exhaust system panels, wheel houses, roofs, luggage, room partitions, and interior materials. The film can be used not only for automobiles, but also for motorcycles, ships, railways, and aircraft parts. As building materials, the film can be used for exterior and interior walls, rooftops, underground continuous walls, and floor materials, as well as mechanical parking lots, roads, bicycle parking lots, areas around railway tracks, areas around highways, leisure facilities, concert halls, factories, and construction sites and event venues where rapid installation and removal are desired. As home appliances, the film can be suitably used for audio products such as televisions and amplifiers, products that are vibration sources such as electric fans and air conditioners that are built in, precision products that are sensitive to vibration such as personal computers, and products that users directly touch such as chairs and beds. EXAMPLES

[0041] The present invention will be described below with reference to examples, but the present invention is not necessarily limited to these. The characteristics were evaluated using the following methods. [Characteristics evaluation method] A. Loss factor Using an electric vibrator (Brüel & Kjær), the resonance and anti-resonance curves were measured using the central excitation method (JIS G 0602 (1993) compliant) (see items 1 to 4 below), and the loss factor was calculated using the half-width method (see items 5 to 6 below). The measurement and calculation procedures are as follows: (1) A vibration-damping material sample measuring 10 mm wide x 220 mm long is attached with adhesive to a SPCC steel plate (thickness 0.8 mm x width 10 mm x length 220 mm) specified in JIS G 3141 (2017). (2) The center of the sample is attached to an electric vibrator via an impedance head. (3) Leave the sample to stand for 30 minutes under conditions of 23°C and 65% RH. (4) A sinusoidal vibration of 2 to 12,800 Hz is applied to the sample by an electric vibrator, the load and acceleration are measured, and the resonance and anti-resonance curves of the mechanical impedance are obtained. (5) Calculate the peak frequency f at the anti-resonance frequency of the third or higher mode, and the frequencies f1 and f2 at the position 3 dB lower. (6) Calculate the loss factor e from the following formula.

[0042] e=f / (|f1-f2|).

[0043] B. Loss modulus E”, storage modulus E’ The film was cut into a strip of 10 mm width and measured using a dynamic viscoelasticity measuring device "DMS6100" manufactured by Seiko Instruments Inc. in accordance with JIS-K 7244 (1999 edition). The loss modulus E" and storage modulus E' were measured in the range of -40°C to 80°C under the following measurement conditions: tension mode, driving frequency 10Hz, chuck distance 20mm, heating rate 2°C / min, sampling interval 1sec.

[0044] C. Endothermic peak top temperature, ΔH temperature, glass transition temperature Using differential scanning calorimetry (DSC), the endothermic peak top temperatures were read in the range of 50-300°C on the DSC curve obtained by heating from 25°C to 300°C at a rate of 20°C / min. Peak reading and division were performed using the attached analysis software. The crystalline melting enthalpy in the range of 50-300°C was measured and calculated according to JIS-K-7122 (2012). The glass transition temperature was measured and calculated according to JIS-K-7121 (2012). Equipment: Seiko Instruments Inc. "EXSTAR DSC6200" Data analysis software: “MuseStandard Analysis Software, version 6.1U” Sample mass: 5mg D. Film thickness The thickness of the film was measured using a dial gauge thickness gauge with a flat tip and a diameter of 4 mm (manufactured by Mitutoyo Corp.) The measurement was carried out 10 times at different locations, and the average value was taken as the film thickness (μm).

[0045] E. t1, t2, t3, t4 A cross section of the film was cut out using a microtome. A cross section parallel to the strongest orientation direction and perpendicular to the film thickness direction, and a cross section perpendicular to the strongest orientation direction and perpendicular to the film thickness direction were cut out. After platinum-palladium was vapor-deposited on the cross section, a cross section photograph was taken at 3000 to 5000 times magnification using a Hitachi field emission scanning electron microscope (FE-SEM) S-800. The image was photographed so that at least 20 particles were captured in the image, and if 20 or more particles were not captured in the image, two or more images were photographed and joined to form one image. From the obtained image, the t1, t2, t3, and t4 of all particles in the image were read using software (image processing software ImageJ (National Institutes of Health, Wayne Rasband)). The measurement was performed on five images at different locations, and the average value was taken as the measured value.

[0046] F. Particle Density The film was dissolved in a solvent capable of dissolving the resin of the substrate, and the extracted and separated particles were dried at 200°C for 8 hours, after which the true density was measured by the pycnometer method according to JIS R 1620 (1995).

[0047] G. Processability The bending resistance was measured by the 45° cantilever method in accordance with JIS-L-1096 (2010). If the bending resistance is too high, the material will not conform well to unevenness or curved surfaces during processing as a vibration-damping material. A: Less than 20mm B: 20mm or more and less than 40mm C: 50mm or more When the traveled length of the test piece is A or B, the workability is good, with A being the best.

[0048] H.Durability Using an MIT folding endurance tester (No. 702 manufactured by Mize Co., Ltd.), samples cut into a length of 110 mm (test direction) and a width of 15 mm were subjected to bending tests in the longitudinal and transverse directions in accordance with JIS-P8115 (2001) at a load of 1000 g, a bending angle of 135° left and right (R: +135°, L: -135°), a bending speed of 175 times / min, and a chuck tip R: 0.38 mm. The number of times the film was bent when it broke was taken as the MIT bending breakage number. The test was performed three times, and the average value was used. A: More than 200,000 times B: 100,000 to 200,000 times C: Less than 100,000 times When the number of bending cycles is A or B, the workability is good, with A being the most excellent. When the number of bending cycles is C, the material can be used sufficiently as long as it is not bent too much.

[0049] I. Tear propagation resistance A light-load Elmendorf tear tester manufactured by Toyo Seiki Seisakusho Co., Ltd. was used. A sample film was sampled in a rectangle of 63.5 mm length and 50.8 mm width, and a 12.7 mm cut was made vertically at a right angle at the center of both grips along the horizontal direction, and the tear force (g) for the remaining 50.8 mm was obtained. This force was divided by the thickness of the film to obtain the tear propagation resistance (g / mm). The measurement was performed in both the longitudinal and transverse directions of the film. A: 10,000g / mm or more in both the vertical and horizontal directions B: Less than 10,000g / mm and 5,000g / mm or more in both the vertical and horizontal directions C: Less than 5000g / mm in both the vertical and horizontal directions When the tear propagation resistance is A or B, the tear resistance is good, with A being the best. When the tear propagation resistance is C, it can also be used for applications that do not require tear resistance.

[0050] J. Determination of layer structure of particles The matrix resin was dissolved in an appropriate solvent to extract the particles. The interplanar spacing d(001) of the obtained particles was measured by powder X-ray diffraction. If the Debye rings were anisotropic and the interplanar spacing d(001) peak was observed in the range of 0.5 nm to 50 nm, the particle was determined to be layered.

[0051] K. Viscosity of resin Each resin was dried under appropriate conditions and molded into a sheet with a thickness of 50 μm at 110 to 280°C. Each sheet was cut into a strip with a width of 10 mm and measured using a dynamic viscoelasticity measuring device "DMS6100" manufactured by Seiko Instruments Inc. in accordance with JIS-K 7244 (1999 edition). The loss modulus E" and storage modulus E' at 25°C were measured under the following measurement conditions: tension mode, driving frequency of 10 Hz, chuck distance of 20 mm, heating rate of 2°C / min, and sampling interval of 1 sec. The larger the E" / E', the higher the viscosity at room temperature.

[0052] [Ingredients used in film production] Resin A: PET / dimer acid copolymer (glass transition temperature (Tg): 20°C, melting point (Tm): 188°C. The dimer acid used was a dicarboxylic acid compound with 36 carbon atoms obtained by dimerizing oleic acid.) Resin B: 1,4:3,6-dianhydro-D-sorbitol copolymerized PET (Tg: -30°C, Tm: 115°C) Resin C: Polyethylene terephthalate (IV: 0.65, Tg: 85°C, Tm: 260°C) Resin D: Ethylene propylene copolymer (Tm: 210℃) Resin E: Polyamide polyether copolymer (Tg: 30°C, Tm: 174°C) Resin F: Isophthalic acid copolymerized PET (Tg: 75°C, Tm: 220°C) Resin G: Isophthalic acid copolymer PBT (Tg: 70°C, Tm: 195°C) Resin H: Polyester (Tg: 70, Tm: 220) consisting of 60 mol% terephthalic acid, 40 mol% sebacic acid, and 100 mol% ethylene glycol as diol component. Resin I: Polybutylene adipate terephthalate (Tg: -35°C, Tm: 110°C) Resin J: Sebacic acid adipic acid copolymer PET (Tg: 50°C, Tm: 180) Resin K: Polyethylene propylene terephthalate (Tg: 60°C. Tm: 200) Note that the viscosity at room temperature increases in the order of J < A < I < E < B < G < K < H < F < D < C. Particle A: Flat layered mica particles (density: 2.5 g / cm 3 , aspect ratio: 30 - 50, central thickness: 0.1 μm, average particle diameter: 4 μm) Particle B: Spherical silica particles (density: 1.9 g / cm 3 , aspect ratio: 1, average particle diameter: 0.1 μm) Particle C: Needle-shaped titanium particles (density: 4.2 g / cm 3 , aspect ratio: 10 - 20, average particle diameter: 0.2 μm, average length: 2.9 μm) Particle D: Plate-shaped zinc oxide particles (density: 5.6 g / cm 3 , aspect ratio: 4, average thickness: 0.08 μm, average particle diameter: 0.3 μm).

[0053] (Example 1) Resin A (50 parts by mass), resin B (50 parts by mass), and particles A (20 parts by mass) were kneaded and molded in a twin-screw extruder to obtain pellets A. Next, resin A (100 parts by mass) and particles A (20 parts by mass) were kneaded and molded in a twin-screw extruder to obtain pellets B. Pellet A and pellet B were melted at 260 ° C. in an extruder, respectively, and were alternately merged in a 51-layer feed block (26 layers of A layer, 25 layers of B layer) while being measured so that the discharge ratio (lamination ratio) was pellet A / pellet B = 1 / 1 with a gear pump and the film thickness after biaxial stretching was 500 μm. Next, the mixture was fed to a T-die and formed into a sheet, and then quenched and solidified on a casting drum maintained at a surface temperature of 25 ° C. while applying an electrostatic voltage of 8 kV with a wire, to obtain an unstretched multilayer laminate film. Sequential biaxial stretching was performed on this unstretched film. First, the film was transported on a "Teflon" (registered trademark) roll at 70°C, and then stretched 2 times in the longitudinal direction at 75°C while being heated by an infrared heater with an output of 500W to obtain a uniaxially stretched film. This uniaxially stretched film was stretched 2 times in the width direction at 80°C in a tenter, and then heat-set at 120°C, during which it was relaxed by 1.7% in the width direction. After that, it was cooled in the transport process, and after the edges were cut, it was wound up to obtain a film. The evaluation results of the obtained film are shown in Table 1. A film with excellent vibration damping properties over a wide temperature range from room temperature to low temperatures, as well as excellent processability and durability was obtained.

[0054] Example 2 A film was obtained in the same manner as in Example 1, except that Resin C was used instead of Resin A. The evaluation results of the obtained film are shown in Table 1. The obtained film had good vibration damping properties over a wide temperature range from room temperature to low temperatures, and was excellent in processability and durability.

[0055] Example 3 A film was obtained in the same manner as in Example 1, except that Resin C was used instead of Resin B. The evaluation results of the obtained film are shown in Table 1. The obtained film had excellent vibration damping properties at room temperature, good vibration damping properties over a wide temperature range from room temperature to low temperatures, and excellent processability and durability.

[0056] Example 4 A film was obtained in the same manner as in Example 1, except that the stretching ratios in both the longitudinal and transverse directions were 1.5 times. The evaluation results of the obtained film are shown in Table 1. The obtained film had excellent vibration damping properties over a wide temperature range from room temperature to low temperatures, and was excellent in processability and durability.

[0057] Example 5 A film was obtained in the same manner as in Example 1, except that particle B was used instead of particle A. The evaluation results of the obtained film are shown in Table 1. The obtained film had good vibration damping properties over a wide temperature range from room temperature to low temperatures, and was excellent in processability and durability.

[0058] Example 6 A film was obtained in the same manner as in Example 1, except that particle C was used instead of particle A. The evaluation results of the obtained film are shown in Table 1. The obtained film had good vibration damping properties over a wide temperature range from room temperature to low temperatures, and was excellent in processability and durability.

[0059] Example 7 A film was obtained in the same manner as in Example 1, except that particle D was used instead of particle A. The evaluation results of the obtained film are shown in Table 1. The obtained film had good vibration damping properties over a wide temperature range from room temperature to low temperatures, and was excellent in processability and durability.

[0060] Example 8 A film was obtained in the same manner as in Example 1, except that Resin D was used instead of Resin A. The evaluation results of the obtained film are shown in Table 1. The obtained film had excellent vibration damping properties over a wide low temperature range, good vibration damping properties in the room temperature range, and excellent processability and durability.

[0061] Example 9 A film was obtained in the same manner as in Example 1, except that Resin E was used instead of Resin B. The evaluation results of the obtained film are shown in Table 1. The obtained film had excellent vibration damping properties over a wide room temperature range, good vibration damping properties in a low temperature range, and excellent processability and durability.

[0062] Example 10 An unstretched film was obtained by casting and cooling and solidifying in the same manner as in Example 1. The evaluation results of the obtained film are shown in Table 1. The obtained film had excellent vibration damping properties over a wide temperature range from room temperature to low temperatures, good processability, and excellent durability.

[0063] Example 11 A film was obtained in the same manner as in Example 1, except that the extrusion rate was adjusted so that the film thickness after stretching would be 100 μm. The evaluation results of the obtained film are shown in Table 1. The obtained film had good vibration damping properties over a wide temperature range from room temperature to low temperatures, excellent processability, and good durability.

[0064] Example 12 A film was obtained in the same manner as in Example 1, except that the extrusion rate was adjusted so that the film thickness after stretching would be 50 μm. The evaluation results of the obtained film are shown in Table 1. The obtained film had good vibration damping properties over a wide temperature range from room temperature to low temperatures, excellent processability, and durability at a practical level.

[0065] (Example 13) A film was obtained in the same manner as in Example 1, except that a 9-layer feed block (5 A layers and 4 B layers) was used instead of the 51-layer feed block. The evaluation results of the obtained film are shown in Table 1. A film was obtained that had excellent vibration damping properties over a wide temperature range from room temperature to low temperatures, as well as excellent processability and durability.

[0066] Example 14 A film was obtained in the same manner as in Example 1, except that a 201-layer feedblock (101 layers of A and 100 layers of B) was used instead of the 51-layer feedblock. The evaluation results of the obtained film are shown in Table 1. A film was obtained that had excellent vibration damping properties over a wide temperature range from room temperature to low temperatures, as well as excellent processability and durability.

[0067] Example 15 A film was obtained in the same manner as in Example 1, except that Resin F was used instead of Resin A. The evaluation results of the obtained film are shown in Table 1. The obtained film had good vibration damping properties over a wide temperature range from room temperature to low temperatures, and was excellent in processability and durability.

[0068] (Example 16) A film was obtained in the same manner as in Example 1, except that Resin G was used instead of Resin A. The evaluation results of the obtained film are shown in Table 1. The obtained film had good vibration damping properties over a wide temperature range from room temperature to low temperatures, and was excellent in processability and durability.

[0069] (Example 17) A film was obtained in the same manner as in Example 1, except that a 17-layer feed block (9 A layers and 8 B layers) was used instead of the 51-layer feed block. The evaluation results of the obtained film are shown in Table 1. A film was obtained that had excellent vibration damping properties over a wide temperature range from room temperature to low temperatures, as well as excellent processability and durability.

[0070] (Example 18) A film was obtained in the same manner as in Example 1, except that a 501-layer feedblock (251 A layers and 250 B layers) was used instead of the 51-layer feedblock. The evaluation results of the obtained film are shown in Table 1. A film was obtained that had excellent vibration damping properties over a wide temperature range from room temperature to low temperatures, as well as excellent processability and durability.

[0071] (Example 19) A film was obtained in the same manner as in Example 1, except that Resin I was used instead of Resin B. The evaluation results of the obtained film are shown in Table 1. The obtained film had good vibration damping properties over a wide temperature range from room temperature to low temperatures, and was excellent in processability and durability.

[0072] (Example 20) A film was obtained in the same manner as in Example 1, except that Resin J was used instead of Resin A. The evaluation results of the obtained film are shown in Table 1. The obtained film had good vibration damping properties over a wide temperature range from room temperature to low temperatures, and was excellent in processability and durability.

[0073] Example 21 A film was obtained in the same manner as in Example 1, except that Resin G was used instead of Resin B. The evaluation results of the obtained film are shown in Table 1. The obtained film had good vibration damping properties over a wide temperature range from room temperature to low temperatures, and was excellent in processability and durability.

[0074] Example 22 A film was obtained in the same manner as in Example 1, except that Resin K was used instead of Resin B. The evaluation results of the obtained film are shown in Table 1. The obtained film had good vibration damping properties over a wide temperature range from room temperature to low temperatures, and was excellent in processability and durability.

[0075] Comparative Example 1 A film was obtained in the same manner as in Example 1, except that no particle A was added. The evaluation results of the obtained film are shown in Table 1. The film had poor vibration damping properties over a wide temperature range from room temperature to low temperatures.

[0076] Comparative Example 2 Only pellet A was melted at 260°C in an extruder, and was fed to a T-die without using a lamination feed block while being weighed so that the film thickness after biaxial stretching would be 500 μm, and molded into a sheet. Thereafter, a film was obtained in the same manner as in Example 1. The evaluation results of the obtained film are shown in Table 1. The film had poor vibration damping properties over a wide temperature range from room temperature to low temperatures.

[0077] Comparative Example 3 A film was obtained in the same manner as in Comparative Example 2, except that Resin A was used instead of Resin B. The evaluation results of the obtained film are shown in Table 1. The film had poor vibration damping properties over a wide temperature range from room temperature to low temperatures.

[0078] Comparative Example 4 A film was obtained in the same manner as in Comparative Example 2, except that Resin C was used instead of Resin B. The evaluation results of the obtained film are shown in Table 1. The film had poor vibration damping properties over a wide temperature range from room temperature to low temperatures.

[0079] Comparative Example 5 A film was obtained in the same manner as in Comparative Example 4, except that the stretching ratio in the width direction was 1.05 times. The evaluation results of the obtained film are shown in Table 1. The film had poor vibration damping properties over a wide temperature range from room temperature to low temperatures.

[0080] Comparative Example 6 A film was obtained in the same manner as in Example 1, except that pellets of resin C were used instead of pellets A and resin H was used instead of pellets B. The evaluation results of the obtained film are shown in Table 1. The film had poor vibration damping properties over a wide temperature range from room temperature to low temperatures.

[0081] Comparative Example 7 A film was obtained in the same manner as in Example 1, except that Resin A was used instead of Resin B. The evaluation results of the obtained film are shown in Table 1. The film had poor vibration damping properties over a wide temperature range from room temperature to low temperatures.

[0082] [Table 1]

[0083] The film of Comparative Example 7 was obtained using a 51-layer feedblock, but the number of layers was set to 1 because the resin compositions fed from each extruder were the same.

Claims

1. A thermoplastic resin film having a laminated structure of five or more layers, at least one of which contains particles, the particle content being 1% by weight or more relative to the entire film, and which is attached to an SPCC steel plate having a width of 10 mm, a length of 220 mm and a thickness of 0.8 mm, and which has an average loss factor of 0.006 or more obtained by a half-width method from third-order or higher anti-resonance peaks of a frequency response function obtained by a central excitation method under conditions of 2 Hz to 12,800 Hz at 23°C.

2. 2. The thermoplastic resin film according to claim 1, wherein in a differential scanning calorimetry (DSC) curve obtained by heating from 25° C. to 300° C. at a rate of 20° C. / min, among endothermic peaks observed in the range of 50° C. to 300° C., the peak top temperature of a peak having the largest ΔH (crystalline melting enthalpy) is 210° C. or lower.

3. 3. The thermoplastic resin film according to claim 2, wherein the DSC curve has one endothermic peak observed in the range of 50° C. to 300° C., or when the DSC curve has two or more endothermic peaks, the peak top temperature of the peak having the second largest ΔH (crystalline melting enthalpy) is less than 210° C.

4. The thermoplastic resin film according to any one of claims 1 to 3, wherein the film is oriented in at least one axial direction, and when the film is cut in a direction parallel to the strongest orientation direction and perpendicular to the film thickness direction and the shape of particles in the film cross section is observed, t1 is the length of the particle in the film thickness direction and t2 is the length of the particle in the direction parallel to the strongest orientation direction of the film, and t1 / t2 is 0.01 or more and 0.95 or less.

5. 5. The thermoplastic resin film according to claim 4, wherein the film is oriented in two directions, and when the film is cut in a direction perpendicular to the direction of strongest orientation and perpendicular to the film thickness direction, and the particle shapes of the film cross section are observed, the length of the particle in the film thickness direction is t3 and the length of the particle in the direction perpendicular to the direction of strongest orientation of the film is t4, and the ratio t3 / t4 is 0.01 or more and 1.00 or less.

6. The density of the particles is 1.0 g / cm 3 5.0g / cm or more 3 The thermoplastic resin film according to any one of claims 1 to 5, wherein:

7. The thermoplastic resin film according to claim 1 , wherein the particles have a layered structure.

8. The thermoplastic resin film according to any one of claims 1 to 7, wherein, when the tensile dynamic viscoelasticity is measured at 10 Hz, the ratio (E" / E') of the loss modulus E" to the storage modulus E' has two or more maximum values ​​in the range of -40 to 60°C.

9. The thermoplastic resin film according to any one of claims 1 to 8, wherein, when tensile dynamic viscoelasticity is measured at 10 Hz, the ratio (E" / E') of loss modulus E" to storage modulus E' has a minimum value of 0.15 or more in the range of 15 to 40°C.

10. The thermoplastic resin film according to any one of claims 1 to 9, wherein, when tensile dynamic viscoelasticity is measured at 10 Hz, the minimum value of the ratio (E" / E') of the loss modulus E" to the storage modulus E' in the range of -25 to 15°C is 0.10 or more.

11. The thermoplastic resin film according to claim 1 , which is mainly composed of polyester.

12. The thermoplastic resin film according to any one of claims 1 to 11, wherein, when the tensile dynamic viscoelasticity is measured at 10 Hz, the minimum value of the ratio (E" / E') of the loss modulus E" to the storage modulus E' divided by the thickness (mm) of the film in the range of 15 to 40°C is 0.3 ( / mm) or more.

13. The thermoplastic resin film according to claim 1 , wherein the thickness of the film is 50 μm or more and 2000 μm or less.

14. The thermoplastic resin film according to any one of claims 1 to 13, comprising a resin copolymerized with one or more of the components shown in the following (1) to (4): (1) A diol having an alkyl group and / or an alkylene group having 3 or more carbon atoms. (2) Dicarboxylic acids having an alkyl group and / or an alkylene group having 3 or more carbon atoms. (3) Diols having a bicyclic structure in which one or more carbon or nitrogen atoms are shared. (4) Dicarboxylic acids having a bicyclic structure in which one or more carbon or nitrogen atoms are shared.

15. 15. The thermoplastic resin film according to claim 1, having a tear propagation resistance in the longitudinal and transverse directions of 5000 g / mm or more.

16. The thermoplastic resin film according to claim 1 , which is used for any one of a vibration damping material, a vibration isolation material, a sound absorbing material, a sound insulating material, and a shock absorbing material.

17. A laminate comprising the thermoplastic resin film according to claim 1 and an adhesive layer laminated thereon.

18. An automobile member comprising the thermoplastic resin film according to any one of claims 1 to 16 or the laminate according to claim 17.

19. A building member comprising the thermoplastic resin film according to any one of claims 1 to 16 or the laminate according to claim 17.

Citation Information

Patent Citations

  • Laminate

    JP2011011529A

  • Vibration damping sheet

    JP2013181155A

  • Polyester film and laminated sheet prepared therewith

    JP2017043768A

  • Laminated film

    JP2017100289A

  • Composition, method for producing heat-resistant vibration-isolation material and heat-resistant vibration-isolation material

    JP2018012785A