Fiber Reinforced Resin
The fiber-reinforced resin composition addresses delamination issues by using a thermoplastic resin with specific Hansen solubility parameters and a thermosetting resin, enhancing impact resistance and thermal cycle durability through improved adhesion and compatibility, resulting in a composite material with balanced environmental resistance.
Patent Information
- Application Number
- JP2020163104
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-29
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-09-29
AI Technical Summary
Existing fiber-reinforced resins (FRP) face issues with delamination during impact and thermal cycling due to insufficient adhesion between thermoplastic and thermosetting resins, leading to suboptimal mechanical and environmental resistance.
A fiber-reinforced resin composition comprising a thermoplastic resin material with specific Hansen solubility parameters and a thermosetting resin, where the thermoplastic resin is present between layers of a reinforcing fiber aggregate, ensuring a radius of interaction (Ra) that allows for improved adhesion and compatibility, with the thermoplastic resin having a notched Izod impact strength of 30 J/m or more and a Vicat softening temperature between 70 to 200°C.
The composition achieves enhanced mechanical properties such as impact resistance and thermal cycle durability, with improved adhesion and solvent resistance, resulting in a composite material with balanced environmental resistance.
Smart Images

Figure 0007581739000002 
Figure 0007581739000003 
Figure 0007581739000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a fiber-reinforced resin having excellent mechanical properties such as impact resistance and environmental resistance such as thermal cycle durability. [Background technology]
[0002] Fiber-reinforced plastics (FRP), in which reinforcing fibers are impregnated with a matrix resin, have been used primarily in aviation, space, and sports applications because they meet the required characteristics of excellent mechanical properties and lightweight weight. Autoclave molding is known as a typical manufacturing method for these materials. In this molding method, prepregs, in which reinforcing fiber bundles are pre-impregnated with a matrix resin, are stacked in a molding die and heated and pressurized in an autoclave to form the FRP. The use of prepregs has the advantage of producing highly reliable FRP, but has the problem of high manufacturing costs.
[0003] On the other hand, molding methods with excellent productivity for FRP include injection molding such as resin transfer molding (RTM). The RTM molding method is a molding method in which a reinforcing fiber substrate consisting of dry reinforcing fiber bundles that have not been pre-impregnated with matrix resin is layered in a molding die, and a liquid, low-viscosity matrix resin is injected into the substrate, which is then impregnated and solidified to form the FRP.
[0004] The injection molding method is excellent in terms of FRP productivity, but because it requires the matrix resin to have a low viscosity, the mechanical properties may not be fully demonstrated compared to FRP molded from the high-viscosity matrix resin used in prepregs.
[0005] As a solution to the above, an intermediate material has been proposed in which a unidirectional layer of carbon fiber having a specified basis weight is combined with a thermoplastic fiber web (nonwoven fabric) having a specified thickness, as disclosed in Patent Document 1, for example. However, although it is disclosed that certain mechanical properties can be exhibited when these thermoplastic fiber webs are used, some thermoplastic fiber webs may not have sufficient adhesion to the matrix resin, and therefore peeling may occur at the interface during deformation upon impact or expansion and contraction due to thermal cycles, preventing the mechanical properties and environmental resistance of the FRP from being fully exhibited.
[0006] Patent Document 2 discloses a technique for improving the adhesiveness between a thermoplastic polymer and a thermosetting polymer and improving their mechanical properties by controlling the solubility parameters of the polymers. However, depending on the selection of the thermoplastic polymer, the thermoplastic polymer and the thermosetting polymer may become completely compatible with each other, resulting in insufficient properties such as heat resistance and toughness, and preventing the mechanical properties and environmental resistance of the FRP from being fully exhibited. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Special Publication No. 2012-506499 [Patent Document 2] Special Publication No. 2009-511297 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention is intended to solve the problems of the conventional techniques, and relates to a fiber-reinforced resin that is excellent in mechanical properties such as impact resistance and in environmental resistance such as thermal cycle durability. [Means for solving the problem]
[0009] In order to solve the above problems, the present invention adopts the following means. (1)It has a porous shape made of fibers. The material contains at least a thermoplastic resin material, a thermosetting resin material, and a reinforcing fiber aggregate. The thermoplastic resin material is present between the layers of the reinforcing fiber assembly, and the spaces between the layers of the reinforcing fiber assembly are impregnated with a thermosetting resin. A fiber reinforced resin comprising: The thermoplastic resin material is present in an amount of 1 to 50% by weight based on the thermosetting resin, The dispersion term (dD 1 ) and the polarity term (dP 1 ) and the hydrogen bond term (dH 1 ) is the coordinate [dD 1 ,dP 1 ,dH 1 ] is the radius of the interaction sphere centered on (r 1 ), After hardening The dispersion term (dD 2 ) and the polarity term (dP 2 ) and the hydrogen bond term (dH 2 ) is the coordinate [dD 2 ,dP 2 ,dH 2 ] is the radius of the interaction sphere centered on (r 2 ), Ra = (4(dD 1 -dD 2 ) 2 +(dP 1 -dP 2 ) 2 +(dH 1 -dH 2 ) 2 ) 1 / 2 Then, Ra ≦ (r 1 +r 2 ) is satisfied , the Ra is 5.4 (MPa) 1 / 2 Above 8.8(MPa) 1 / 2 is as follows: And The thermoplastic resin material is a fiber-reinforced resin having a notched Izod impact strength of 30 J / m or more. ( 2 ) The thermoplastic resin material has a Vicat softening temperature in the range of 70 to 200 ° C. ( 1 ) The fiber reinforced resin described in the above. ( 3(1) The thermoplastic resin material is at least one selected from the group consisting of polyamide resin, polyester resin, polyphenylene sulfide resin, polyetherimide resin, polyethersulfone resin, polyvinyl formal resin, polyetheretherketone resin, polycarbonate resin, polysulfone resin, polyphenylene ether resin, polyimide resin, polyamideimide resin, and phenoxy resin, or a mixture thereof. Or (2) The fiber reinforced resin according to claim 1. ( 4 ) the thermoplastic resin material is an amorphous polyamide, 3 ) The fiber reinforced resin described in. ( 5 ) the thermoplastic resin material is a semi-aromatic polyamide containing an isophthalic acid component, 3 )or( 4 ) The fiber reinforced resin described in. ( 6 ) the reinforcing fiber assembly is an assembly of at least two layers selected from [1]: reinforcing fiber yarns, [2]: a reinforcing fiber yarn group formed by arranging reinforcing fiber yarns in parallel, and [3]: a reinforcing fiber fabric composed of [1] or [2], characterized in that the thermoplastic resin material is present between the layers of the reinforcing fiber assembly. 5 ) The fiber reinforced resin according to any one of the preceding claims. ( 7 ) the reinforcing fiber yarn group is a sheet-like material in which a plurality of reinforcing fiber yarns are aligned in parallel, ( 6 ) The fiber reinforced resin described in. ( 8 ) the reinforcing fiber yarn group is in the form of a sheet arranged in parallel by an automated fiber placement device, 6 )or( 7 ) The fiber reinforced resin described in. ( 9) the reinforcing fiber assembly is a unidirectional woven fabric composed of a group of reinforcing fiber threads formed by arranging reinforcing fiber threads in parallel in one direction, and a group of auxiliary fiber threads extending in a direction intersecting the reinforcing fiber threads and having a fineness of 1 / 5 or less of the fineness of the reinforcing fiber threads, (1) to ( 8 ) The fiber reinforced resin according to any one of the preceding claims. ( 10 The reinforcing fiber aggregate is arranged in one direction. Strong It is a bidirectional fabric composed of a group of synthetic fiber yarns and a group of reinforcing fiber yarns arranged in one direction in a different direction. 8 ) The fiber reinforced resin according to any one of the preceding claims. ( 11 ) the reinforcing fiber fabric is a stitched fabric in which at least two layers of the reinforcing fiber yarn group aligned in one direction and a reinforcing fiber yarn group aligned in a different direction are cross-laminated, and are sewn together by an auxiliary fiber yarn group having a fineness 1 / 5 or less of that of the reinforcing fiber yarn, 6 ) The fiber reinforced resin described in. ( 12 ) The volume content of reinforcing fibers is in the range of 53 to 65%, and the room temperature compressive strength after impact application described in SACMA-SRM-2R-94 is 240 MPa or more. 11 ) The fiber reinforced resin according to any one of the preceding claims. Effect of the Invention
[0010] According to the present invention, as described in detail below, it is possible to obtain a composite material that is excellent in mechanical properties such as impact resistance and in environmental resistance such as thermal cycle durability. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a schematic diagram illustrating the relationship between the Hansen solubility parameters of a thermoplastic resin material and a thermosetting resin material according to the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view illustrating one embodiment of a reinforcing fiber substrate in the present invention. [Diagram 3] FIG. 1 is a schematic side view showing one embodiment of a manufacturing apparatus for a reinforcing fiber substrate in the present invention. [Figure 4] FIG. 1 is a schematic perspective view showing one embodiment of a reinforcing fiber yarn group in the present invention. [Diagram 5] FIG. 1 is a schematic perspective view showing one embodiment of a unidirectional woven fabric as a reinforcing fiber assembly in the present invention. [Figure 6] FIG. 1 is a schematic perspective view showing one embodiment of a bidirectional woven fabric as a reinforcing fiber assembly in the present invention. [Figure 7] FIG. 1 is a schematic perspective view showing one embodiment of a stitched fabric as a reinforcing fiber assembly in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The fiber reinforced resin of the present invention will be specifically described below.
[0013] The fiber reinforced resin of the present invention comprises at least a thermoplastic resin material, a thermosetting resin material, and a reinforcing fiber aggregate, and the dispersion term (dD 1 ) and the polarity term (dP 1 ) and the hydrogen bond term (dH 1 ) is the coordinate [dD 1 ,dP 1 ,dH 1 ] is the radius of the interaction sphere centered on (r 1 ), the dispersion term of the Hansen solubility parameter of the thermosetting resin (dD 2 ) and the polarity term (dP 2 ) and the hydrogen bond term (dH 2 ) is the coordinate [dD 2 ,dP 2 ,dH 2 ] is the radius of the interaction sphere centered on (r 2 ), the following equation is obtained: (4(dD 1 -dD 2 ) 2 +(dP 1 -dP 2 ) 2 +(dH 1 -dH 2 ) 2 ) 1 / 2 ≦ (r 1 +r2 ) and the notched Izod impact strength of the thermoplastic resin is 30 J / m or more.
[0014] Hildebrand solubility parameter (hereinafter sometimes simply referred to as SP value) has been widely used as an index to express the affinity of two materials, and it is empirically known that the smaller the difference in the SP value of two materials, the better the solubility and adhesion. The SP value is derived from regular solution theory and is calculated from the latent heat of vaporization and density, but there have been problems with this, such as the occurrence of phenomena that cannot be explained by the SP value alone, such as solvents with similar SP values showing completely different dissolution behaviors, and a mixed solvent of butanol and nitroethane in a 1:1 ratio being able to dissolve epoxy resin, even though the SP values of these two solvents are almost the same and neither dissolves epoxy resin.
[0015] To address these issues, the Hansen Solubility Parameter (hereinafter sometimes referred to as HSP value) is a parameter that divides the Hildebrand Solubility Parameter into three components: dispersion term (dD), polar term (dP), and hydrogen bond term (dH), and is expressed as a point in three-dimensional space, making it an affinity evaluation index that includes the direction of the vector. In other words, even if the magnitude of the HSP value vectors of two materials is the same, if the directions of the HSP value vectors are significantly different, the affinity is estimated to be low.
[0016] For example, the HSP value can be obtained from the handbook (see Hansen Solubility Parameters A User's Handbook Second Edition, CRC Press (2007)). It is also possible to obtain the HSP value by performing a solubility test (a test to determine solubility / insolubility) on a sample using multiple test solvents with known HSP values. When the results of a solubility test are plotted in three-dimensional space, good solvents are concentrated in similar positions, so the largest sphere can be considered in which the good solvents are on the inside and the poor solvents are on the outside, and the center of this sphere can be determined as the HSP value of the sample. This sphere is called the interaction sphere, and the radius of this sphere is called the interaction radius (r).
[0017] FIG. 1 is a schematic diagram illustrating the relationship between the Hansen solubility parameters of a thermoplastic resin material and a thermosetting resin material according to the present invention.
[0018] The dispersion term (dD 1 ) and the polarity term (dP 1 ) and the hydrogen bond term (dH 1 ) is the coordinate [dD 1 ,dP 1 ,dH 1 ] is the radius of the interaction sphere centered on (r 1 ), the dispersion term of the Hansen solubility parameter of the thermosetting resin (dD 2 ) and the polarity term (dP 2 ) and the hydrogen bond term (dH 2 ) is the coordinate [dD 2 ,dP 2 ,dH 2 ] is the radius of the interaction sphere centered on (r 2 ), the distance between the two coordinates (Ra) is Ra = (4(dD 1 -dD 2 ) 2 +(dP 1 -dP 2 ) 2 +(dH 1 -dH 2 ) 2 ) 1 / 2 It can be estimated that the smaller the Ra, the greater the affinity between the two substances.
[0019] where r 1 and r 2Since Ra indicates the soluble range in the solvent when a solubility test is performed, it is considered that the two substances can have an IPN or semi-IPN structure in the overlapping range. Here, IPN is an abbreviation for Interpenetrating Polymer Network, and refers to an interpenetrating network structure between crosslinked polymers. On the other hand, semi-IPN refers to an interpenetrating network structure between a crosslinked polymer and a linear polymer. Therefore, when Ra of the thermoplastic resin material and the thermosetting resin material is (r 1 +r 2 ) or less, the affinity between the thermoplastic resin material and the thermosetting resin material, i.e., wettability, is improved. In addition, the formation of an IPN or semi-IPN structure during the molding process improves solvent resistance and adhesion, making it possible to efficiently express many properties, such as mechanical properties such as impact resistance (compressive strength after compression: CAI), heat cycle durability, and solvent resistance.
[0020] Therefore, Ra ≦ (r 1 +r 2 ) is important. Furthermore, Ra≦r 1 or r 2 It is even more preferable that:
[0021] Here, the radius of the interaction sphere (r) is also an index of chemical resistance to various solvents. For thermoplastic materials, the radius of the interaction sphere (r 1 If a material with a large radius of interaction sphere (r 1 ) is 10(MPa) 1 / 2 and the radius of the interaction sphere of the thermosetting resin material (r 2 ) or less, that is, r 1 ≦r 2 It is more preferable that:
[0022] Furthermore, if the thermoplastic resin material and the thermosetting resin material are completely compatible with each other, properties such as heat resistance and impact resistance may deteriorate. 1 / 2 It is preferable that Ra≧4.5(MPa) 1 / 2 It is more preferable that the notched Izod impact strength of the thermoplastic resin material is 30 J / m or more. Here, in the present invention, the notched Izod impact strength refers to a value measured according to ASTM D256 (2018). If the notched Izod impact strength is less than 30 J / m, the impact resistance of the FRP decreases, which is not preferable.
[0023] The thermoplastic resin material preferably has a Vicat softening temperature in the range of 70 to 200°C. Here, in the present invention, the Vicat softening temperature (VST) refers to a value measured by the A-50 method according to JIS K7206 (2016). If the VST is less than 70°C, the mechanical properties of the FRP at high temperatures will decrease, which is not preferable. If the VST exceeds 200°C, the adhesion between the thermoplastic resin material and the thermosetting resin material will decrease, and the mechanical properties of the FRP (especially CAI and ILSS) may decrease. Therefore, it is more preferable that the thermoplastic resin material has a Vicat softening temperature in the range of 100 to 180°C.
[0024] The thermoplastic resin material used in the present invention is preferably 1 to 50% by weight of the thermosetting resin material. It is preferably 2 to 30% by weight, and more preferably 3 to 20% by weight. If the thermoplastic resin material is less than 1% by weight, the effect of improving the mechanical properties (particularly CAI) is reduced, which is not preferable. If the thermoplastic resin material is more than 50% by weight, the Vf of the FRP may be too low, and the heat resistance, chemical resistance, and compressive strength of the FRP may decrease, which is also not preferable.
[0025] The thermoplastic resin material of the present invention is preferably at least one selected from polyamide resin, polyester resin, polyphenylene sulfide resin, polyetherimide resin, polyethersulfone resin, polyvinyl formal resin, polyetheretherketone resin, polycarbonate resin, polysulfone resin, polyphenylene ether resin, polyimide resin, polyamideimide resin, and phenoxy resin, or a mixture thereof. These thermoplastic resin materials are not only excellent in impact resistance, but also have excellent affinity with thermosetting resin materials, so that composite materials can be obtained that are excellent in mechanical properties such as impact resistance and environmental resistance such as thermal cycle durability.
[0026] In addition, the thermoplastic resin material is preferably an amorphous polyamide from the viewpoints of heat resistance, impact resistance, and ease of processing. In the present invention, the term "amorphous" refers to a material having a crystalline melting enthalpy ΔHm value of less than 5 J / g, measured at a heating rate of 10° C. / min according to JIS K7121 (1987) using a differential scanning calorimeter (DSC).
[0027] Further, the thermoplastic resin material is preferably a semi-aromatic polyamide containing an isophthalic acid component. Examples of semi-aromatic polyamides containing an isophthalic acid component include polyamide 2I, polyamide 4I, polyamide 6I, polyamide 9I, polyamide 10I, polyamide 12I, polyamide 6-6 / 6-I resin, polyamide 6-10 / 6-I resin, polyamide 12 / 6-I resin, polyamide 6-6 / 6-T / 6-I resin, and polyamide MACMI. Among them, polyamide 9I, polyamide 10I, polyamide 12I, polyamide 6-6 / 6-I resin, polyamide 6-10 / 6-I resin, polyamide 12 / 6-I resin, polyamide 6-6 / 6-T / 6-I resin, and polyamide MACMI, which have long methylene chains, are preferred from the viewpoint of water absorption and flexibility. Such thermoplastic resin materials can form highly tough layers between the FRP layers by adhering closely to the thermosetting resin materials during FRP molding, thereby improving the mechanical properties (especially CAI and ILSS) and thermal cycle durability.
[0028] The thermoplastic resin material of the present invention is preferably in the form of particles or fibers. In the case of particles, it can be kneaded into a thermosetting resin or sprinkled on the surface of a reinforcing fiber assembly, thereby dramatically increasing the impact resistance of the reinforced fiber composite material. In the case of fibers, it can be used in the same way, and by using it as an auxiliary thread for fixing reinforcing fibers together, it is possible to improve durability against peeling and cracking due to heat cycles compared to conventional auxiliary threads. When used as a stitch thread, either monofilament or multifilament can be selected. If the fineness is too thin, thread breakage occurs, and if it is too thick, the fiber volume content (Vf) of the molded product may be reduced, so it is preferable that the fineness is in the range of 30 to 300 dtex.
[0029] In addition, the form of the thermoplastic resin material is preferably a porous form made of fibers. In the present invention, the porous form refers to a form in which holes are open in the thickness direction on a plane, and examples thereof include nonwoven fabric, mat, net, mesh, woven fabric, knitted fabric, and short fiber group. Among them, nonwoven fabric, mat, and mesh are preferable because they are inexpensive and have matrix resin and air flow paths formed in the plane direction. When the thermoplastic resin material is a nonwoven fabric, the form of the fibers constituting the nonwoven fabric includes long fibers and short fibers, and is produced by methods such as melt blowing, spunbonding, airlaid, carding, and papermaking, but is not particularly limited. In addition, a binder component for binding fibers together may be contained as a secondary component. The fiber diameter of the fibers constituting the nonwoven fabric is preferably 1 μm or more and less than 100 μm, more preferably 5 μm or more and less than 80 μm, and even more preferably 10 μm or more and less than 60 μm. If the fiber diameter is less than 1 μm, the surface area of the resin material will be large, which is undesirable as it may hinder the flow of the resin in the resin impregnation step described below, and if the fiber diameter is 100 μm or more, the thickness between the reinforcing fiber base layers will be large when made into FRP, which is undesirable as it reduces Vf.
[0030] Next, it is preferable that the reinforcing fiber aggregate is an aggregate of at least two layers selected from the following: [1]: reinforcing fiber yarns, [2]: a reinforcing fiber yarn group formed by arranging reinforcing fiber yarns in parallel, and [3]: a reinforcing fiber fabric composed of [1] or [2], and that the thermoplastic resin material is present between the layers of the reinforcing fiber aggregate.
[0031] A specific example of the form of the reinforcing fiber aggregate used in the present invention will be described with reference to the drawings. Fig. 2 is a schematic cross-sectional view illustrating one embodiment of a reinforcing fiber substrate 11 related to the reinforcing fiber resin in the present invention. The reinforcing fiber substrate 11 shown in Fig. 2 is formed by arranging a thermoplastic resin material 13 on one side of a reinforcing fiber aggregate 12 and then bonding and integrating the two.
[0032] The reinforcing fiber substrate 11 preferably has a thermoplastic resin material 13 on at least one surface of a reinforcing fiber assembly 12 selected from reinforcing fiber yarns, reinforcing fiber yarn groups, or a reinforcing fiber fabric composed of reinforcing fiber yarns or reinforcing fiber yarn groups. By having such a thermoplastic resin material 13 on at least one surface, it is possible to improve the shape stability of the reinforcing fiber substrate 11, such as the width and fiber orientation, and to improve the handleability during transportation of the sheet-like reinforcing fiber substrate 11 composed of reinforcing fiber yarn groups.
[0033] In addition, when obtaining a laminate (preform) by stacking the reinforcing fiber base material 11 or the reinforcing fiber assemblies 12 described below, it is possible to impart adhesion between the reinforcing fiber assemblies 12, it is possible to impart appropriate rigidity to the preform, it is possible to impart a shape stabilizing effect such as preventing misalignment of the reinforcing fibers in the preform, and the handleability of the preform can be improved.
[0034] In particular, the thermoplastic resin material 13 can secure a space between the layers of the reinforcing fiber aggregate 12 for the matrix resin to flow and diffuse (the matrix resin can impart plastic deformation ability between the layers of the reinforcing fiber aggregate 12), and can suppress damage between the layers of the reinforcing fiber aggregate 12 when it receives an impact, for example, by acting as a stopper for cracks that occur between the layers of the reinforcing fiber aggregate 12, thereby achieving particularly excellent mechanical properties (particularly compressive strength after impact: CAI). It also exhibits environmental resistance, such as mitigating stress during thermal cycle loading. In addition, the thermoplastic resin material 13 acts as a spacer to secure a flow path for the matrix resin between the layers of the reinforcing fiber aggregate 12, which not only makes it easier to impregnate the matrix resin when subjected to injection molding, but also increases the impregnation speed, resulting in superior productivity of FRP.
[0035] The thermoplastic resin material 13 is required to be bonded to the reinforcing fiber assembly 12 and to be present on at least one surface of the reinforcing fiber assembly 12, and may be present inside the reinforcing fiber assembly 12 (permeating the reinforcing fiber threads). For the reasons mentioned above, it is preferable that 50% by weight or more, more preferably 70% by weight or more of the thermoplastic resin material 13 is unevenly distributed on the surface of the reinforcing fiber assembly 12. In addition, the thermoplastic resin material 13 may contain a binder component for the purpose of bonding the thermoplastic resin material 13 to the reinforcing fiber bundle assembly 12, and for example, a thermoplastic resin or a thermosetting resin having a lower softening point (melting point or glass transition temperature Tg) than the thermoplastic resin material 13 can be used.
[0036] The thermoplastic resin material 13 is preferably in the form of a nonwoven fabric, a mat, a net, a mesh, a woven fabric, a knitted fabric, a short fiber group, etc. Such a form not only ensures flow paths for the matrix resin and air in the thickness direction of the reinforcing fiber substrate 11, but also provides connection in the planar direction, thereby improving the width stability when reinforcing fiber threads are used, the handleability during transport of the sheet-like reinforcing fiber substrate 11 made of reinforcing fiber thread groups, and the shape stability of the substrate when reinforcing fiber thread groups or cloth are used.
[0037] The reinforcing fiber yarn in the present invention is a multifilament yarn, such as a glass fiber yarn, an organic (aramid, PBO, PVA, PE, etc.) fiber yarn, a carbon fiber (PAN-based, pitch-based, etc.) yarn, etc. Carbon fiber is excellent in specific strength and specific modulus and hardly absorbs water, so it is preferably used as a reinforcing fiber for aircraft structural materials and automobiles.
[0038] The reinforcing fiber yarn used in the present invention preferably has 3,000 to 50,000 filaments, and from the viewpoint of handling, particularly preferably has 12,000 to 24,000 filaments. The form of the reinforcing fiber yarn is not particularly limited, but it is preferably a non-twisted yarn having excellent stability in yarn width and thickness, and more preferably a spread yarn having excellent fiber orientation.
[0039] Here, the reinforcing fiber substrate in the present invention is preferably made of a reinforcing fiber aggregate selected from any one of [1]: reinforcing fiber yarns, [2]: reinforcing fiber yarn groups formed by arranging reinforcing fiber yarns in parallel, or [3]: reinforcing fiber fabric composed of reinforcing fiber yarns or reinforcing fiber yarn groups.
[0040] First, the reinforcing fiber base material 21 made of reinforcing fiber yarns is created using, for example, the apparatus illustrated in FIG. 3. Specifically, the reinforcing fiber yarns 22 drawn from the bobbin 20 are opened by the opening unit 201, adjusted to a desired width by the width regulating roller 202, then overlapped with a resin material 23 (preferably a porous resin material) slit to a desired width in advance, and created by heating with the heater 203 and crimping with the press roller 204. The opening unit 201 is composed of, for example, a vibrating roller and has a mechanism for applying vibration in the vertical or horizontal direction perpendicular to the traveling direction of the reinforcing fiber yarns 22. Further, the opening unit 201 may be provided with a heater (not shown) for softening the sizing agent attached to the surface of the reinforcing fiber yarns 22. At this time, assuming the yarn width of the reinforcing fiber yarns 22 drawn from the bobbin 20 is w0, the width of the reinforcing fiber yarns 22 after opening is widened to w1 (w0 < w1), and then adjusted to a width w2 (w1 > w2) by the width regulating roller 202. It is preferable to adjust w2 according to the basis weight required for the reinforcing fiber base material 21. Further, in order to improve the width accuracy of the reinforcing fiber base material 21, the press roller 204 preferably has a grooved structure.
[0041] The reinforcing fiber base material 21 created by such an apparatus has good stability in width and basis weight, and also excellent fiber orientation, and thus can contribute to the improvement of the mechanical properties (particularly compressive strength) of the FRP. Further, it is preferable to dispose the resin material 23 on both sides of the reinforcing fiber yarn group because the morphological stability of the reinforcing fiber base material 21 is further improved.
[0042] Next, [2]: The reinforcing fiber substrate 21 made of a group of reinforcing fiber threads is prepared by, for example, hanging a plurality of bobbins 20 on an apparatus illustrated in FIG. 3 and drawing and aligning a plurality of reinforcing fiber threads 22 in parallel, in the same manner as in the preparation method of a reinforcing fiber substrate made of reinforcing fiber threads 22. Here, "drawing in parallel" means that adjacent reinforcing fiber threads 22 are drawn and aligned so that they do not substantially cross or intersect with each other, and preferably, when two adjacent reinforcing fiber threads are approximated to a straight line within a length of 100 mm, the angle formed by the approximated straight line is 5° or less, more preferably 2° or less. Here, "approximating the reinforcing fiber threads 22 to a straight line" means that a straight line is formed by connecting the starting point and the end point of 100 mm. In addition, adjacent reinforcing fiber threads 22 may be spaced apart at a certain interval according to the desired basis weight of the reinforcing fiber substrate 21, or may overlap each other. When they are spaced apart at a constant interval, the interval is preferably 200% or less of the width of the reinforcing fiber yarn 22, and when they overlap, they may overlap by 100% of the width of the reinforcing fiber yarn 22. The group of reinforcing fiber yarns thus drawn out while being parallel to each other is preferably passed through a spreading unit to uniformly distribute the basis weight in the width direction. In addition, the reinforcing fiber substrate 21 made from such a group of reinforcing fiber yarns can be slit, if necessary, to control the width to any desired value.
[0043] [3] Reinforced fiber fabrics composed of reinforcing fiber yarns or groups of reinforcing fiber yarns will be described later.
[0044] Furthermore, for the reinforcing fiber substrate 21 using the reinforcing fiber yarns 22 and the reinforcing fiber yarn groups, an automated fiber placement (AFP) or automated tape layup (ATL) device is preferably used. Such devices are used for the purpose of reducing the waste rate of the reinforcing fiber substrate 21 and automating the lamination process, but since strict requirements are placed on the width and fiber orientation after placement, the shape stability of the reinforcing fiber substrate 21 becomes important. Here, the porous resin material 23 used in the present invention has a porous shape, and therefore has excellent width stability and shape stability due to the connection in the planar direction, and can be preferably used for AFP or ATL.
[0045] Another embodiment of the reinforcing fiber thread group in the present invention is a sheet-like one arranged in parallel by AFP or ATL. FIG. 4 shows one embodiment of the reinforcing fiber thread group used in the present invention, in which reinforcing fiber threads 32 are supplied by an AFP head 300 and arranged in parallel. A porous resin material (not shown) is arranged so as to overlap the reinforcing fiber thread group 31, and heat-bonded by a far-infrared heater or the like to obtain a reinforcing fiber substrate. The sheet-like reinforcing fiber thread group 31 arranged in parallel by AFP or ATL has no constraint in a direction intersecting with the fiber direction, so there is a problem that the shape of the reinforcing fiber thread group 31 collapses during transport. In response to this problem, by arranging and bonding a porous resin material, a binding force is generated in a direction intersecting with the fiber direction, and the transport problem can be solved. In addition, the interval between the reinforcing fiber threads 32 when the reinforcing fiber threads 32 are arranged in parallel by AFP or ATL is preferably 0.5 to 2 mm. If the interval is less than 0.5 mm, the resin impregnation during RTM molding may be insufficient.If the interval exceeds 2 mm, when multiple reinforcing fiber substrates are laminated, the reinforcing fibers in the upper layer may fall between the reinforcing fiber threads 32 in the lower layer, causing undulation in the thickness direction and reducing the mechanical properties (especially the compressive strength).
[0046] Next, [3] examples of reinforced fiber fabrics composed of reinforcing fiber yarns or groups of reinforcing fiber yarns include woven fabrics (unidirectional, bidirectional, multiaxial), knitted fabrics, braided fabrics, sheets aligned in one direction (unidirectional sheets), and multiaxial sheets in which two or more layers of unidirectional sheets are superimposed. Such reinforced fiber assemblies may be integrated with a plurality of pieces by various bonding means such as stitch yarns, knotted yarns, sackcloth, and resins such as binders. In particular, when used as a structural (particularly primary structural) member of transportation equipment (particularly aircraft), a unidirectional sheet, unidirectional fabric, or multiaxial sheet (particularly one bonded by stitching) is preferable.
[0047] FIG. 5 is a schematic perspective view showing one embodiment of a unidirectional fabric 41 as a reinforcing fiber fabric used in the present invention. Reinforcing fiber threads 42 and warp auxiliary threads 43 are arranged in the length direction of the unidirectional fabric 41, i.e., in the warp direction, and weft auxiliary threads 44 thinner than the reinforcing fiber threads 42 are arranged in the weft direction, and the warp auxiliary threads 43 and the weft auxiliary threads 44 intersect with each other to form a unidirectional fabric having a weave structure as shown in FIG. 5. The auxiliary threads 43 are preferably low-shrinkage threads, and examples of such threads include glass fiber threads, aramid fiber threads, and carbon fiber threads. The fineness (weight per unit length) of the auxiliary threads is preferably 1 / 5 or less of the reinforcing fiber threads. If the fineness exceeds 1 / 5, the auxiliary threads become thick, so that the reinforcing fiber threads are crimped by the auxiliary threads, resulting in a slight decrease in the strength of the reinforcing fibers when the FRP is made. On the other hand, from the viewpoints of the shape stability and manufacturing stability of the reinforcing fiber assembly, the fineness of the auxiliary threads is preferably 0.05% or more of the reinforcing fiber threads. A fineness within the above range is preferable because it minimizes the decrease in strength and also because the gaps between the reinforcing fiber threads 42 formed by the warp auxiliary threads during molding become resin flow paths, facilitating the impregnation of the matrix resin.
[0048] 6 is a schematic perspective view showing one embodiment of a bidirectional fabric 51 as a reinforcing fiber fabric used in the present invention. Reinforcing fiber yarns 52 are arranged in the length direction of the bidirectional fabric 51, i.e., in the warp direction, reinforcing fiber yarns 53 are arranged in the weft direction, and the warp yarns 52 and weft yarns 53 cross each other to form a bidirectional fabric having the weave shown in FIG.
[0049] FIG. 7 is a schematic perspective view showing one embodiment of a stitched fabric 61 as a reinforced fiber fabric used in the present invention. From the bottom surface of the stitched fabric 61, first, a large number of reinforcing fiber threads are arranged in parallel in a diagonal direction with respect to the length direction A to form a +α° layer 62, then a large number of reinforcing fiber threads are arranged in parallel in the width direction of the reinforced fabric to form a 90° layer 63, then a large number of reinforcing fiber threads are arranged in parallel in a diagonal direction to form a -α° layer 64, and then a large number of reinforcing fiber threads are arranged in parallel in the length direction of the reinforced fabric to form a 0° layer 65. In a state in which four layers with mutually different arrangement directions are laminated, these four layers are sewn together by a stitch thread 66. Examples of the stitch structure formed by the stitch thread 66 in the stitching integration include single chain stitching and 1 / 1 tricot knitting. The material of the stitch thread can be selected from polyester resin, polyamide resin, polyethylene resin, vinyl alcohol resin, polyphenylene sulfide resin, polyaramid resin, compositions thereof, and the like. Among them, polyester resin and polyamide resin are preferable. From the viewpoint of the shaping property of the fabric, processed yarns of spandex (polyurethane elastic fiber), polyamide resin or polyester resin are preferable. The fineness of the stitch yarn is preferably 1 / 5 or less of the reinforcing fiber yarn in order to suppress crimp of the reinforcing fiber yarn. In addition, from the viewpoint of the shape stability and manufacturing stability of the reinforcing fiber assembly, it is preferable that the fineness is 10 dtex or more, more preferably 30 dtex or more. Furthermore, from the viewpoint of the shaping property in the preforming process described later, it is preferable that the stitch yarn has elasticity. In addition, in FIG. 7, the assembly of reinforcing fibers shown in an elliptical cross section is one yarn, and the stitch yarn 66 appears to be arranged between the reinforcing fiber yarns, but the stitch yarn 66 is randomly inserted into the reinforcing fiber yarns, and the assembly of reinforcing fibers shown in an elliptical shape is formed by the constraint of the stitch yarn 66.
[0050] Here, the reinforcing fiber configuration of the multiaxial stitch fabric 61 shown in FIG. 7 has been described as a four-layer configuration of +α° layer / 90° layer / -α° layer / 0° layer, but is not limited thereto. For example, it may be two layers consisting of 0° layer / 90° layer, +α° layer / -α° layer, 0° layer / +α° layer, etc., three layers consisting of +α° layer / 0° layer / -α° layer, +α° layer / -α° layer / 0° layer, etc., or it may be a configuration including four directions of 0°, +α°, -α°, and 90°, such as 0° layer / +α° layer / 0° layer / -α° layer / 90° layer / -α° layer / 0° layer / +α° layer / 0° layer, which includes many 0° layers. It may also be a configuration including any of 0°, +α°, -α°, and 90°. Note that the bias angle α° is preferably 45° from the viewpoint of effectively performing shear reinforcement by the reinforcing fiber by stacking the stitch fabric in the length direction of the FRP.
[0051] The preferred weight per layer of the reinforcing fiber substrate in the present invention is 50 to 800 g / m 2 More preferably, the thickness is within the range of 100 to 500 g / m 2 , and more preferably 120 to 300 g / m 2 Within the range of 50g / m 2 If the weight per layer is less than 800 g / m, the number of layers required to obtain a desired FRP thickness increases, which is undesirable as it makes the molding process less efficient. Also, if the weight per layer is small, gaps are formed between the reinforcing fiber threads in the layer, which makes the reinforcing fiber volume content Vf uneven in parts, and when molded, the FRP becomes thick where the reinforcing fiber volume content Vf is high and thin where the reinforcing fiber volume content Vf is low, resulting in an FRP with an uneven surface. In such cases, it is preferable to thinly spread the reinforcing fiber threads with a vibrating roller or air jet spray just before weaving or before integration processing with stitch threads, or / and after processing into a reinforced fabric, so that the volume ratio of the reinforcing fibers becomes uniform over the entire surface of the reinforced fabric and an FRP with a smooth surface can be obtained. Also, if the weight per layer is less than 800 g / m, gaps are formed between the reinforcing fiber threads in the layer, which makes the reinforcing fiber volume content Vf uneven in parts, which makes the FRP thicker where the reinforcing fiber volume content Vf is high and thin where the reinforcing fiber volume content Vf is low. 2 If it exceeds this value, the impregnation of the matrix resin becomes poor, which is not preferable.
[0052] Next, the reinforcing fiber laminate of the present invention will be described. Prior to FRP molding, the reinforcing fiber substrate of the present invention is laminated in multiple sheets until it reaches a desired thickness to form a reinforcing fiber laminate. In the present invention, it is preferable that the reinforcing fiber laminate is integrated by heat fusion or stitching in order to impart handling properties and dimensional stability to the reinforcing fiber laminate.
[0053] Furthermore, the reinforcing fiber laminate of the present invention can be made into a shape-fixed preform by imparting a three-dimensional shape to the carbon fiber laminate base material using a shaping mold, a jig, etc., in accordance with the shape of the desired carbon fiber reinforced resin molding. In particular, when the molding mold has a three-dimensional shape, this can easily prevent fiber disorder and wrinkles from occurring during mold clamping or resin injection / impregnation.
[0054] Next, the FRP of the present invention will be described. The FRP of the present invention is obtained by impregnating the above-mentioned reinforced fiber laminate with a matrix resin. Such a matrix resin is solidified (cured or polymerized) as necessary. Preferable examples of such a matrix resin include thermosetting resins and thermoplastic resins for RIM (Reaction Injection Molding), among which at least one resin selected from epoxy resins, phenolic resins, vinyl ester resins, unsaturated polyester resins, cyanate ester resins, bismaleimide resins, and benzoxazine resins, which are suitable for injection molding, are preferred.
[0055] In addition, since the FRP of the present invention has excellent mechanical properties and is lightweight, its use is preferably as a primary structural member, secondary structural member, exterior member or interior member in any of transportation machines such as aircraft, automobiles or ships.
[0056] Next, a method for molding FRP using the reinforcing fiber substrate of the present invention will be described.
[0057] Of the reinforcing fiber substrates in the present invention, the reinforcing fiber substrates made of reinforcing fiber threads or groups of reinforcing fiber threads are aligned and arranged in a desired shape by an AFP or ATL device.
[0058] Such an arrangement step may be performed in a two-dimensional planar shape or in a three-dimensional shape. In the case of a two-dimensional planar shape, a sheet-like reinforcing fiber substrate that is easy to transport layer by layer can be created by arranging and adhering a porous resin material after arranging the reinforcing fiber substrate for each layer, and it is possible to transport the reinforcing fiber substrate in a sheet-like shape in a separately prepared shaping mold without losing the shape in which it is aligned and arranged. At this time, it is preferable that the porous resin material to be arranged has at least a partial cut, since the shaping property in the preforming step described later is improved. In addition, as a transport means, a transport means using a method such as static electricity, suction, or needle piercing can be used.
[0059] In addition, the sheet-like reinforcing fiber substrates prepared for each layer may be laminated and integrated by heat fusion or stitching to make a reinforcing fiber laminate in order to further improve the handling. In this case, by making the arrangement direction of the reinforcing fiber substrates of the second layer and subsequent layers different from the arrangement direction of the (n-1)th layer, a multi-layer reinforcing fiber laminate that can be handled in the same way as a fabric can be made. The integration process of such reinforcing fiber substrates may be performed on the entire surface where the reinforcing fiber substrates are overlapped, or may be performed partially. When the reinforcing fiber substrates are integrated on the entire surface, the shape stability of the reinforcing fiber substrate is excellent. On the other hand, when the reinforcing fiber substrates are partially integrated, they are easily deformed when shaped into a molded product shape in the preforming process described later (i.e., good shapeability). Therefore, it is preferable to use these methods arbitrarily depending on the complexity of the molded product shape.
[0060] Here, the reinforcing fiber substrate in the present invention may also include a substrate in which a porous resin material is arranged and bonded to a group of reinforcing fiber threads (without a resin material attached thereto) that are aligned and arranged in a desired shape by an AFP or ATL device. This makes it possible to impart properties such as impact resistance to carbon fiber threads that do not have such properties.
[0061] Furthermore, after placing the first layer of reinforcing fiber substrate, the second and subsequent layers may be repeatedly placed on the same plane. In such a placing process, a heater is provided in the head of the AFP or ATL device, and the second and subsequent layers of reinforcing fiber substrate are placed while melting the resin material on the surface of the reinforcing fiber substrate, thereby integrating the placing process of the reinforcing fiber substrate and the integration process. In this case, by setting the arrangement direction of the nth reinforcing fiber substrate from the second layer onwards to a direction different from the arrangement direction of the (n-1)th layer, a multi-layer reinforcing fiber laminate that can be treated in the same way as a fabric can be obtained.
[0062] Among the reinforcing fiber substrates in the present invention, the reinforcing fiber substrate made of a reinforcing fiber aggregate and the reinforcing fiber laminate containing a resin material between layers of reinforcing fiber thread groups are used by being cut into a desired shape in accordance with the shape of a molded article.
[0063] The reinforcing fiber substrate or reinforcing fiber laminate thus prepared is laminated one layer at a time or multiple layers at a desired angle configuration, and then a preforming process is carried out to prepare a preform. In the preforming process, it is preferable to heat the resin material within a range of Vicat softening temperature -30°C to Vicat softening temperature +30°C. If the heating temperature is low, the resin material may not be softened sufficiently and the shape of the preform may not be fixed. Also, if the heating temperature is high, the resin material may penetrate the reinforcing fiber substrate, resulting in poor impregnation of the matrix resin.
[0064] The molding of the FRP of the present invention is performed by so-called resin injection molding, and RTM (Resin Transfer Molding) molding and VaRTM (Vacuum assisted Resin Transfer Molding) molding are preferably applied. The porous resin material arranged on at least one side of the reinforcing fiber substrate in the present invention functions as a flow path (air path) when discharging air inside the reinforcing fiber substrate and as a resin diffusion medium. Therefore, it is possible to improve the internal quality of the molded product and to speed up the resin injection process. In addition, since the porous resin material arranged on at least one side of the reinforcing fiber substrate in the present invention has a connection in the planar direction, it is possible to prevent deformation of the reinforcing fiber substrate when resin is injected at high pressure.
[0065] The thermosetting resin material according to the present invention has a Kic value, which is an index of resin toughness after curing, of 0.8 MPa m 1 / 2 It is preferable to use a resin with a Kic value of 1.0 MPa m. By using such a resin with high toughness, it is possible to suppress the occurrence of cracks caused by thermal cycle loads and the propagation of existing cracks. To further enhance the effect of suppressing the occurrence and propagation of cracks, the Kic value should be 1.0 MPa m. 1 / 2 The Kic value in the present invention is measured in accordance with ASTM-D5045.
[0066] Here, when the Vicat softening temperature of the thermoplastic resin material (1) is T1 (°C), it is preferable that the relationship between the injection temperature Ti (°C) at which the thermosetting resin material (2) is injected into the reinforcing fiber aggregate (3) and the hardening temperature Tr (°C) of the thermosetting resin is Tr (°C) ≧ Tt (°C) > Ti (°C).
[0067] If the softening temperature of such a thermoplastic resin material (1) is low and it softens or melts below the temperature at which the matrix resin is injected into the carbon fiber substrate, it may melt and spread between or on the surface of the carbon fibers before the matrix resin is impregnated, filling the gaps and hindering the impregnation of the carbon fiber substrate with the matrix resin. On the other hand, by starting to soften before the matrix resin starts to harden, the interface with the matrix resin is firmly bonded, impact resistance can be efficiently expressed, and peeling between materials, which is the cause of cracks that progress due to thermal cycle load, is less likely to occur.
[0068] The FRP of the present invention preferably has a reinforcing fiber volume fraction (Vf) in the range of 53 to 65%, and a room temperature compressive strength after impact application described in SACMA-SRM-2R-94 of 240 MPa or more. Note that Vf (unit: vol%) refers to the volume ratio of the reinforcing fibers in the fiber reinforced resin, and is specifically defined by the following formula, and the symbols used here are as shown below. Vf = (W x 100) / (ρ x T) W: Reinforced fiber base material 1cm 2 Weight of reinforcement fiber per unit (g / cm 2 ) ρ: Density of reinforcing fiber (g / cm 3 ) T: Thickness of fiber-reinforced resin (cm)
[0069] When the Vf of the fiber reinforced resin is in the range of 53 to 65%, the excellent mechanical properties of the fiber reinforced resin can be fully expressed. When the Vf is less than 53%, the weight reduction effect is poor, and when it exceeds 65%, molding by the above-mentioned injection molding becomes difficult, and the mechanical properties (especially impact resistance) may be deteriorated. That is, in this Vf range, when the room temperature compressive strength after impact application described in SACMA-SRM-2R-94 is 240 MPa or more, it can be a material that satisfies both the weight reduction effect and the mechanical properties. Fiber reinforced resins that satisfy such requirements are used in a wide variety of applications due to their excellent mechanical properties and weight reduction effect. They are used in primary structural members, secondary structural members, exterior members, interior members, or parts thereof in transportation equipment such as aircraft, automobiles, or ships, and their effects are fully expressed.
[0070] SACMA is an abbreviation for Suppliers of Advanced Composite Materials Association, and SACMA-SRM-2R-94 is the standard for the test method established by the association. The room temperature compressive strength after impact was measured at an impact energy of 270 inch pounds under dry conditions in accordance with SACMA-SRM-2R-94. EXAMPLES
[0071] The present invention will be further described below with reference to examples. The raw materials and molding methods used in the examples and comparative examples are as follows. However, the present invention is not limited to these examples and comparative examples.
[0072] <Hansen Solubility Parameter> The sample to be measured was immersed in 36 types of solvents with known HSP values, and the HSP value was calculated using HSP calculation software based on the results of judging the dissolution or swelling state of the sample. 1) Sample shape: Thermoplastic resin material: 2 mm diameter pellet or fiber Thermosetting resin material: Small pieces of hardened resin (cubes with each side measuring approximately 2 mm) 2) Test solvents: 36 solvents with different HSP values 3) Treatment conditions: Immersion at room temperature for 2 weeks 4) Judgment criteria: The condition of the sample was visually observed and judged according to the following criteria. ×: Not apparent dissolved, and no change in the appearance of the sample. △△: The sample is whitened (not swollen). △: The sample was whitened and clearly swollen. ○: The shape of the sample is distorted. ◎: The entire sample is dissolved. 5) Calculation software: HSPiP (Hansen Solubility Parameter in Practice) ver.5.0
[0073] <Izod impact test> An Izod impact test specimen with a length of 60 mm, width of 12.5 mm, and thickness of 3.2 mm was molded using a Sumitomo Heavy Industries SE75DUZ injection molding machine. A notch was made in this test specimen with a notch cutter, and the cut-notched Izod impact strength was measured according to ASTM D256 (2018) at a temperature of 23 °C and a relative humidity of 50%.
[0074] <Thermal cycle durability test> The fiber-reinforced resin samples were cut to 50 mm x 80 mm, and then subjected to the following pretreatment, followed by a thermal cycle test.
[0075] Pretreatment conditions: Immersed in 70°C hot water for 2 weeks.
[0076] Thermal cycle conditions: A cycle of low temperature -55°C and high temperature 70°C was repeated 2000 times. Each cycle was held at both low and high temperatures for 5 minutes.
[0077] After the thermal cycle test was completed, a cross section of the sample was cut out and observed under a microscope at a magnification of 200 times, and the occurrence of peeling and cracks was judged as follows. ×: Peeling and cracks are observed. △: Peeling is observed. ◯: No peeling or cracks observed.
[0078] <Reinforced fiber yarn> The carbon fiber yarn used was a PAN-based carbon fiber with 24,000 filaments, tensile strength of 6.0 GPa, and tensile modulus of elasticity of 294 GPa.
[0079] <Thermoplastic resin materials> Four types of thermoplastic resin materials were prepared as follows:
[0080] Example 1: Polyamide 6I / 12 was prepared by copolymerizing polyamide 6I and polyamide 12.
[0081] Example 2: "Grilamid (registered trademark)" TR90 (manufactured by M-Chemie Japan Co., Ltd.) was used.
[0082] Comparative Example 1: Hexamethylenediamine and isophthalic acid were polymerized in an equimolar ratio to prepare polyamide 6I.
[0083] Comparative Example 2: Copolymer polyamide "Amilan (registered trademark)" CM6041F1 (manufactured by Toray Industries, Inc.) was used.
[0084] The radius of the interaction sphere of the Hansen solubility parameter (r 1 ), Ra, Izod impact strength, and VST with the thermosetting resin material are as shown in Table 1.
[0085] <Porous resin material> The above thermoplastic resin material was made into nonwoven fabric by a melt blowing machine. The basis weight was 10 g / m 2 It was.
[0086] <Reinforced fiber base material> Using the device shown in Figure 3, a tape-shaped reinforcing fiber substrate with a width of 1 / 4 inch was produced. The weight of the reinforcing fiber substrate was 162 g / m 2 It was.
[0087] <Reinforced fiber laminate> The reinforcing fiber substrate is formed into a sheet using an AFP device and laminated in a pseudo-isotropic manner [45 / 0 / -45 / 90].3S (24 layers: here, "3S" refers to a configuration in which one set (4 layers x 2 = 8 layers) is made up of one set stacked in the orientation angle order shown in [ ] and one stacked in a symmetrical arrangement, and three sets of these are stacked (8 layers x 3 = 24 layers). The same applies below.) After stacking on a flat preform mold in this configuration, it was sealed with a bag film and sealant, and heated in a vacuum state in an oven at 100°C for 1 hour. The preform mold was then removed from the oven, cooled to room temperature, and the pressure was released to obtain a reinforcing fiber laminate.
[0088] <Thermosetting resin material> 80 parts by weight of tetraglycidyldiaminodiphenylmethane type epoxy ("Araldite (registered trademark)" MY-721, manufactured by Huntsman Japan Co., Ltd.), 20 parts by weight of bisphenol F type epoxy resin ("Epiclon (registered trademark)" 830, manufactured by DIC Corporation), and 70 parts by weight of 4,4'-methylenebis(2-isopropyl-6-methylaniline) ("Lonzacure (registered trademark)" M-MIPA, manufactured by Lonza Corporation) were weighed out and uniformly dissolved by stirring at 100°C for 1 hour. The interaction sphere radius (r 2 ) is 7.5 (MPa) 1 / 2 It was.
[0089] <Fiber reinforced resin> A resin diffusion medium (aluminum wire mesh) was laminated on the obtained reinforced fiber laminate, and a cavity was formed by sealing a flat molding die and a bag material using a sealant, and the cavity was placed in an oven at 100°C. After the temperature of the reinforced fiber laminate reached 100°C, the sealed cavity was depressurized to a vacuum, and the matrix resin was injected only with the pressure difference from atmospheric pressure while maintaining the temperature at 100°C. After the resin was impregnated, the temperature was raised to 180°C while continuing the depressurization, and the plate was left for 2 hours to harden and demold, obtaining an FRP plate. The Vf, CAI value, and heat cycle durability of the obtained FRP plate were as shown in Table 1.
[0090] [Table 1]
[0091] From the above comparison between the Examples and Comparative Examples, it can be seen that the thermoplastic resin material, thermosetting resin material, and reinforced fiber resin comprising the reinforced fiber aggregate of the present invention can achieve a high level of balance between mechanical properties such as impact resistance and environmental resistance such as thermal cycle durability. [Industrial Applicability]
[0092] Because the FRP of the present invention has excellent mechanical properties and is lightweight, its applications are not limited to primary structural components, secondary structural components, exterior components, or interior components in transportation equipment such as aircraft, automobiles, and ships, but it is also suitable for general industrial use components such as wind turbine blades, robot arms, and medical equipment such as X-ray tabletops. [Explanation of symbols]
[0093] 11: Reinforced fiber base material 12: Reinforced fiber assembly 13: Thermoplastic resin materials 20: Bobbin 21: Reinforced fiber base material 22: Reinforced fiber yarn 23: Thermoplastic resin materials 201: Spreading unit 202: Width control roller 203: Heater 204: Press roll 31: Reinforced fiber yarn group 32: Reinforced fiber yarn 300:AFP Head 41: Unidirectional fabric 42: Reinforced fiber yarn (warp thread) 43: Auxiliary thread (warp thread) 44: Auxiliary thread (weft thread) 51: Bidirectional fabric 52: Reinforced fiber yarn (warp) 53: Reinforced fiber yarn (weft) 61: Stitched fabric 62: +α° reinforced fiber layer forming reinforced fabric 63: 90° reinforcing fiber layer forming a reinforcing fabric 64: -α° reinforced fiber layer forming reinforced fabric 65: 0° reinforcing fiber layer forming reinforcing fabric 66: Stitching thread
Claims
1. A fiber-reinforced resin comprising at least a thermoplastic resin material having a porous shape made of fibers, a thermosetting resin material, and a reinforcing fiber assembly, the thermoplastic resin material being present between layers of the reinforcing fiber assembly, and the thermosetting resin being impregnated between the layers of the reinforcing fiber assembly, the thermoplastic resin material being present in a range of 1 to 50% by weight with respect to the thermosetting resin, and the dispersion term (dD 1 ) and polar term (dP 1 ) and the hydrogen bond term (dH 1 ) is the coordinate [dD 1 , dP 1 , dH 1 ] is the radius of the interaction sphere centered on (r 1 ), the dispersion term of the Hansen solubility parameter of the thermosetting resin after curing (dD 2 ) and polar term (dP 2 ) and the hydrogen bond term (dH 2 ) is the coordinate [dD 2 , dP 2 , dH 2 ] is the radius of the interaction sphere centered on (r 2 ), Ra=(4(dD 1 -dd 2 ) 2 + (dP 1 -dP 2 ) 2 + (dH 1 -dH 2 ) 2 ) 1/2 Then, Ra≦(r 1 +r 2 ) is satisfied, and the Ra is 5.4 (MPa) 1 / 2 or more and 8.8 (MPa) 1 / 2 or less, And the thermoplastic resin material has a notched Izod impact strength of 30 J / m or more.
2. The fiber reinforced resin according to claim 1, characterized in that the Vicat softening temperature of the thermoplastic resin material is in the range of 70 to 200 ° C.
3. The fiber-reinforced resin according to claim 1 or 2, characterized in that the thermoplastic resin material is at least one selected from the group consisting of polyamide resin, polyester resin, polyphenylene sulfide resin, polyetherimide resin, polyethersulfone resin, polyvinyl formal resin, polyetheretherketone resin, polycarbonate resin, polysulfone resin, polyphenylene ether resin, polyimide resin, polyamideimide resin and phenoxy resin, or a mixture thereof.
4. The fiber reinforced resin according to claim 3, wherein the thermoplastic resin material is an amorphous polyamide.
5. The fiber-reinforced resin according to claim 3 or 4, characterized in that the thermoplastic resin material is a semi-aromatic polyamide containing an isophthalic acid component.
6. The fiber-reinforced resin according to any one of claims 1 to 5, characterized in that the reinforcing fiber assembly is an assembly of at least two layers selected from [1]: reinforcing fiber yarns, [2]: a reinforcing fiber yarn group formed by arranging reinforcing fiber yarns in parallel, and [3]: a reinforcing fiber fabric composed of [1] or [2], and the thermoplastic resin material is present between the layers of the reinforcing fiber assembly.
7. The fiber reinforced resin according to claim 6, wherein the reinforcing fiber yarn group is in the form of a sheet in which a plurality of reinforcing fiber yarns are aligned in parallel.
8. The fiber-reinforced resin according to claim 6 or 7, wherein the group of reinforcing fiber threads is in the form of a sheet that is aligned in parallel by an automated fiber placement device.
9. The reinforcing fiber aggregate is a unidirectional fabric composed of a reinforcing fiber yarn group formed by arranging reinforcing fiber yarns in parallel in one direction and an auxiliary fiber yarn group extending in a direction intersecting the reinforcing fiber yarn and having a fineness of 1 / 5 or less of the fineness of the reinforcing fiber yarn. The fiber-reinforced resin according to any one of claims 1 to 8.
10. The reinforcing fiber aggregate is a bidirectional fabric composed of a group of reinforcing fiber yarns arranged in one direction and a group of reinforcing fiber yarns arranged in a different direction. Fiber reinforced resin according to any one of claims 1 to 8.
11. The fiber-reinforced resin according to claim 6, wherein the reinforcing fiber fabric is a stitched fabric in which at least two layers of the reinforcing fiber yarn group arranged in one direction and a reinforcing fiber yarn group arranged in a different direction are cross-laminated and sewn together by an auxiliary fiber yarn group having a fineness of 1 / 5 or less of the reinforcing fiber yarn.
12. The fiber reinforced resin according to any one of claims 1 to 11, wherein the reinforcing fiber volume content is in the range of 53 to 65%, and the room temperature compressive strength after impact application described in SACMA-SRM-2R-94 is 240 MPa or more.
Citation Information
Patent Citations
Method for bonding dry reinforcing fibers
JP2009511297A
Novel reinforcing material suitable for the fabrication of composite parts
JP2012506499A
Binder composition, reinforcing fiber base material, preform, fiber-reinforced composite material and method for producing the same
JP2013181112A
Reinforced-fiber base material, reinforced-fiber laminate, and fiber-reinforced resin
JP2020023182A
Fiber-reinforced resin
JP2020023691A