Polypropylene Film

A polypropylene film with controlled thermal shrinkage and high mechanical strength is achieved through specific raw materials and processing, addressing peeling and curling issues during high-temperature processes.

JP7581876B2Active Publication Date: 2024-11-13TORAY INDUSTRIES INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020539114
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-28
Filing Date
2020-03-25
Publication Date
2024-11-13
Estimated Expiration
2040-03-25

AI Technical Summary

Technical Problem

Existing polypropylene films face challenges in maintaining low thermal shrinkage force while ensuring high mechanical strength, particularly at elevated temperatures, leading to issues such as peeling, curling, and wrinkles during high-temperature processes.

Method used

A polypropylene film with a heat shrinkage force of 400 mN or less at 140°C and a Young's modulus of 1.8 GPa or more in both main orientation axis and perpendicular directions, achieved through specific raw material composition and controlled film forming conditions, including the use of crystalline polypropylene with low cold xylene solubility and high melting point, and precise stretching and relaxation processes.

Benefits of technology

The film exhibits excellent mechanical strength at both room and high temperatures, preventing peeling and curling, and maintaining flatness during high-temperature applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581876000001
    Figure 0007581876000001
Patent Text Reader

Abstract

A polypropylene film according to the present invention has a thermal shrinkage force at 140°C of 400 mN or less in both a main orientation axis direction and a direction perpendicular thereto, and a Young's modulus of 1.8 GPa or more in both the main orientation axis direction and the direction perpendicular thereto. Provided is a polypropylene film having excellent thermal resistance and quality.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polypropylene film which is excellent in shrinkage characteristics at high temperatures and mechanical strength at high temperatures, and which is excellent in heat resistance, productivity, and quality. [Background technology]

[0002] Polypropylene films are excellent in transparency, mechanical properties, electrical properties, etc., and are therefore used in a variety of applications, including packaging, release, tape, cable wrapping, and electrical applications such as capacitors. In particular, because of their excellent surface release properties and mechanical properties, they are suitably used as release films and process films for a variety of components, such as plastic products, building materials, and optical components.

[0003] The properties required for a release film are set appropriately depending on the application, but one way it is used is when it is passed through a high-temperature process such as a heated roll or oven at 140 to 150°C after being attached to an adherend. In such cases, PET film, which has excellent heat resistance, has often been used up until now, but PET film has poor releasability and may not be able to satisfy the required properties, so there are cases where a film that has both excellent heat resistance and releasability is required.

[0004] If the shrinkage force at high temperatures is large, when the film is laminated to the adherend and passes through a heating process, it may peel off from the adherend or curl due to shrinkage. In particular, polypropylene has a low melting point of about 160°C, and it is very difficult to suppress the shrinkage force at about 140 to 150°C.

[0005] As a means for improving heat resistance, for example, Patent Document 1 describes an example in which the shrinkage force at 120°C is reduced by increasing the heat treatment temperature and relaxing the orientation. Patent Documents 3 and 4 describe examples in which the heat shrinkage rate is reduced by increasing the heat treatment temperature in the relaxation treatment and relaxing the orientation. Patent Document 2 describes an example in which the heat shrinkage rate is reduced by decreasing the molecular weight of the polypropylene raw material. Patent Document 5 describes an example in which the shrinkage force at 140°C is reduced by extremely increasing the relaxation rate after transverse stretching.

[0006] In general, a method of reducing the orientation of a polypropylene film is used to reduce the shrinkage force, but if the polypropylene film has low mechanical strength at high temperatures, problems may occur. For example, when an adhesive is applied to a polypropylene film and the adhesive layer is dried in a high-temperature oven, problems with quality such as wrinkles may occur. In addition, Patent Document 5 describes an example in which the shrinkage force at 140°C is reduced by making the relaxation rate after transverse stretching very large.

[0007] For these reasons, it is necessary to reduce the shrinkage force at high temperatures while maintaining the mechanical strength at high temperatures, but in general, when trying to increase the mechanical strength at high temperatures, it is necessary to increase the orientation of the polypropylene film, and when the orientation relaxes, a shrinkage force occurs, which may result in an increase in the shrinkage force. In other words, there is a trade-off between the shrinkage force and the mechanical strength, and it has been difficult to achieve both at the same time. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2003-041017 A [Patent Document 2] JP 2014-051657 A [Patent Document 3] JP 2017-125184 A [Patent Document 4] International Publication No. 2016 / 006578 [Patent Document 5] International Publication No. 2014 / 148547 Summary of the Invention [Problem to be solved by the invention]

[0009] However, the methods described in the above-mentioned Patent Documents 1 and 3 have problems such as low mechanical strength, and wrinkles occur when the polypropylene film and the adhesive film are transported at high temperatures. In addition, the methods described in Patent Documents 2 and 4 have problems such as high thermal shrinkage at high temperatures, peeling from the adherend, and curling. In addition, the method described in Patent Document 5 has problems such as low rigidity of the film at high temperatures, and the film stretches in the flow direction when the adhesive film is transported at high temperatures, resulting in large width shrinkage.

[0010] An object of the present invention is to solve the above-mentioned problems by providing a polypropylene film which has excellent mechanical strength at room temperature and at high temperatures despite its low heat shrinkage force and can be suitably used as a release film in a high-temperature environment. [Means for solving the problem]

[0011] In order to solve the above-mentioned problems and achieve the object, the polypropylene film of the present invention is characterized in that the heat shrinkage force at 140°C in both the main orientation axis direction and the direction perpendicular thereto is 400 mN or less, and the Young's modulus in both the main orientation axis direction and the direction perpendicular thereto is 1.8 GPa or more. Effect of the Invention

[0012] INDUSTRIAL APPLICABILITY The polypropylene film of the present invention has a low heat shrinkage force, yet has excellent mechanical strength at room temperature and at high temperatures, and can be suitably used as a release film in a high-temperature environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The polypropylene film of the present invention has a heat shrinkage force at 140° C. of 400 mN or less in both the main orientation axis direction and the direction perpendicular thereto, and a Young's modulus of 1.8 GPa or more in both the main orientation axis direction and the direction perpendicular thereto.

[0014] The heat shrinkage force at 140°C in the main orientation axis direction and the direction perpendicular thereto is more preferably 350mN or less, even more preferably 100mN or less, even more preferably 95mN or less, and most preferably 30mN or less. If the heat shrinkage force at 140°C in at least one of the main orientation axis direction and the direction perpendicular thereto exceeds 400mN, the film may be peeled off from the adherend or curled due to shrinkage when it is laminated to the adherend and passes through a heating process. The lower limit of the heat shrinkage force at 140°C in the main orientation axis direction and the direction perpendicular thereto is not particularly limited, but is substantially about -100mN. Here, the heat shrinkage force refers to the heat shrinkage force at a width of 4mm, and the measurement can be performed by the method shown in the examples.

[0015] In the present invention, the main orientation axis direction refers to the direction that shows the highest Young's modulus when the Young's modulus is measured in each direction that forms an angle of 15°, 30°, 45°, 60°, 75°, 90°, 105°, 120°, 135°, 150°, and 165° with respect to the longitudinal direction in the film plane, where the longitudinal direction is 0°. Here, in the polypropylene film of the present invention, the "longitudinal direction" refers to the direction corresponding to the flow direction in the film production process (hereinafter, sometimes referred to as "MD"), and the "width direction" refers to the direction perpendicular to the flow direction in the film production process (hereinafter, sometimes referred to as "TD"). When the film sample is in the form of a reel, roll, or the like, the film winding direction can be said to be the longitudinal direction. On the other hand, in the case of a film in which it is unclear from the appearance which direction corresponds to the flow direction in the film manufacturing process, for example, lines are drawn at 15° intervals based on an arbitrary straight line on the film plane, slit-shaped film pieces are sampled parallel to each line, and Young's modulus is obtained using a tensile tester, and the direction that gives the maximum Young's modulus is regarded as the main orientation axis direction. As will be described in detail later, if the width of the sample is less than 150 mm and Young's modulus cannot be obtained using a tensile tester, the crystal orientation of the α crystal (110) plane of the polypropylene film is measured using wide-angle X-rays as follows, and the film longitudinal and width directions are determined based on the following criteria. That is, X-rays are incident perpendicularly to the film surface, and the crystal peak at 2θ = approximately 14° (α crystal (110) plane) is scanned in the circumferential direction, and the direction with the highest diffraction intensity in the obtained diffraction intensity distribution is regarded as the main orientation axis direction.

[0016] The Young's modulus in the main orientation axis direction and the direction perpendicular thereto is more preferably 2.0 GPa or more, and more preferably 2.3 GPa or more. If the Young's modulus in at least one of the main orientation axis direction and the direction perpendicular thereto is less than 1.8 GPa, wrinkles may occur when the adhesive layer is applied to a polypropylene film and dried in a high-temperature oven. The upper limit of the Young's modulus in the main orientation axis direction and the direction perpendicular thereto is not particularly limited, but is substantially about 10 GPa.

[0017] In order to set the heat shrinkage force at 140°C in the main orientation axis direction and the direction perpendicular thereto, and the Young's modulus within the above ranges, it is effective to set the raw material composition of the film within the range described later, set the film formation conditions within the range described later, and in particular to use a raw material that is highly crystalline, has a low cold xylene soluble content, and has a high melting point, set the preheat roll temperature during longitudinal stretching within the range described later, homogenize the crystalline state before stretching, and then perform high-orientation stretching.

[0018] The polypropylene film of the present invention preferably has a temperature of 116°C or higher in both the main orientation axis direction and the direction perpendicular thereto when the heat shrinkage force is 20 mN or more, more preferably 124°C or higher, even more preferably 132°C or higher, and most preferably 142°C or higher. If the temperature at which the heat shrinkage force is 20 mN or more is lower than 116°C in at least one of the main orientation axis direction and the direction perpendicular thereto, the film may be peeled off from the adherend or curled due to shrinkage when it is laminated to the adherend and passed through a heating step. The upper limit of the temperature at which the heat shrinkage force is 20 mN or more is not particularly limited, but is practically about 160°C. In order to set the temperature at which the heat shrinkage force is 20 mN or more within the above range, it is effective to set the raw material composition of the film within the range described below, set the film-forming conditions within the range described below, and in particular to use raw materials that are highly crystalline, have a low cold xylene soluble content, and have a high melting point, set the preheat roll temperature during longitudinal stretching within the range described below, make the crystalline state before stretching uniform, and moderately promote relaxation of the film in the heat treatment process after transverse stretching.

[0019] The polypropylene film of the present invention preferably has a maximum point stress at 120°C in both the main orientation axis direction and the direction perpendicular thereto of 80 MPa or more, more preferably 100 MPa°C or more, and even more preferably 120 MPa or more. If the maximum point stress at 120°C is less than 80 MPa in at least one of the main orientation axis direction and the direction perpendicular thereto, wrinkles may occur when the polypropylene film is coated with adhesive and the adhesive layer is dried in a high-temperature oven. The upper limit of the maximum point stress is not particularly limited, but is substantially about 300 MPa. In order to set the maximum point stress in the above range, it is preferable to set the raw material composition of the film to the range described later, and the film-forming conditions to the range described later, and in particular to use a raw material that is highly crystalline, has a low cold xylene soluble portion, and has a high melting point, and to set the preheat roll temperature during longitudinal stretching to the range described later, and to uniformize the crystalline state before stretching, and then perform high-orientation stretching. It is also preferable to set the heat treatment temperature and relaxation rate after transverse stretching to the range described later, and not relax the orientation of the film more than necessary.

[0020] The polypropylene film of the present invention has a maximum projection roughness St of at least one side of 2000 nm or more, more preferably 4000 nm or more, and even more preferably 6000 nm or more. If St on both sides of the film is less than 2000 nm, the releasability when peeled from the adherend may be insufficient, and the adherend may be deformed or broken. The upper limit of St is not particularly limited, but is substantially about 30000 nm. In order to set St within the above range, it is effective to set the raw material composition of the film within the range described below, set the film-forming conditions within the range described below, and in particular to increase the casting temperature to form β crystals in the unstretched film during the casting process.

[0021] The polypropylene film of the present invention has a thickness unevenness in the main orientation axis direction of preferably less than 6.0%, more preferably less than 4.0%, and even more preferably less than 2.0%. If the thickness unevenness in the main orientation axis direction is 6.0% or more, it becomes difficult to bond the film neatly to the adherend, and the film may peel off from the adherend or air may be mixed in. The lower limit of the thickness unevenness in the main orientation axis direction is not particularly limited, but is substantially about 0.1%. In order to make the thickness unevenness in the main orientation axis direction fall within the above range, it is effective to set the raw material composition of the film to the range described later, set the film-forming conditions to the range described later, and in particular, adjust the preheating and stretching temperatures during transverse stretching to the range described later, and increase the transverse stretching ratio.

[0022] The polypropylene film of the present invention has a heat shrinkage force at 140 ° C. in a direction perpendicular to the main orientation axis direction of 95 mN or less, more preferably 60 mN or less, even more preferably 30 mN or less, and most preferably 10 mN or less. If the heat shrinkage force at 140 ° C. in a direction perpendicular to the main orientation axis direction exceeds 95 mN, the film may be peeled off from the adherend or curled due to shrinkage when it is laminated to the adherend and passed through a heating process. The lower limit of the heat shrinkage force at 140 ° C. in a direction perpendicular to the main orientation axis direction is not particularly limited, but is substantially about −100 mN. In order to set the heat shrinkage force at 140 ° C. in a direction perpendicular to the main orientation axis direction to the above range, it is effective to set the raw material composition of the film to a range described later, set the film-forming conditions to a range described later, and in particular, set the preheat roll temperature during longitudinal stretching to a range described later, and uniformize the crystalline state before stretching, and then perform high-orientation stretching. It is even more effective to set the preheating temperature and stretching temperature during transverse stretching in the ranges described below, to increase the preheating temperature, to uniformly preheat the polypropylene film, and to stretch the film at high stress at a temperature lower than the preheating temperature.

[0023] The polypropylene film of the present invention preferably has a Young's modulus (GPa) at 120°C in a direction perpendicular to the main orientation axis direction multiplied by the thickness (μm) of the film of 1.5 (GPa·μm) or more, more preferably 3.0 (GPa·μm) or more, even more preferably 4.0 (GPa·μm) or more, and most preferably 5.5 or more. The Young's modulus at 120°C in a direction perpendicular to the main orientation axis direction multiplied by the thickness of the film is highly correlated with the rigidity of the film in a high-temperature environment, and if the value is less than 1.5, the film may stretch in the flow direction during transport when it is laminated to an adherend and passes through a heating process, resulting in a large shrinkage of the film width. The upper limit of the Young's modulus at 120°C in a direction perpendicular to the main orientation axis direction multiplied by the thickness of the film is not particularly limited, but is substantially about 30. In order to bring the Young's modulus at 120°C in the direction perpendicular to the main orientation axis direction into the above-mentioned range, multiplied by the thickness of the film, it is effective to set the raw material composition of the film within the range described below, set the film-forming conditions within the range described below, and in particular, set the preheating roll temperature during longitudinal stretching within the range described below, homogenize the crystalline state before stretching, and then perform high-orientation stretching, adjust the preheating and stretching temperatures during transverse stretching within the ranges described below, preheat uniformly at a high temperature, and perform high-orientation stretching at a low temperature, and not set the relaxation rate too large and not relax the orientation too much.

[0024] The polypropylene film of the present invention has a laminated structure of two or more layers, and at least one layer is preferably a layer containing 50% by mass or more and 100% by mass or less of polypropylene having a cold xylene soluble portion (CXS) of 3.5% or less in 100% by mass of the entire layer, more preferably 70% by mass or more and 100% by mass or less, even more preferably 90% by mass or more and 100% by mass or less, and most preferably 95% by mass or more and 100% by mass or less. Here, CXS refers to a polyolefin component dissolved in xylene when a sample is completely dissolved in xylene and then precipitated at room temperature, and is considered to correspond to a component that is difficult to crystallize due to low stereoregularity, low molecular weight, etc. If such a component is contained in a large amount in the resin, the thermal dimensional stability of the film may be poor. Therefore, the CXS of the polypropylene contained in the polypropylene film of the present invention is more preferably 2.0% or less, and even more preferably 1.5% or less. When the polypropylene film has a laminated structure of two or more layers and the content of polypropylene having a CXS of 3.5% or less in at least one layer is less than 50% by mass, the mechanical strength of the polypropylene film at high temperatures is insufficient. As a result, for example, when the polypropylene film is coated with adhesive and the adhesive layer is dried in a high-temperature oven, wrinkles may occur. In addition, when the polypropylene film has a laminated structure of two or more layers and contains 50% to 100% by mass of polypropylene having a CXS of more than 3.5% in at least one layer, the heat shrinkage force becomes large, and when the film is laminated with an adherend and passes through a heating process, the film may peel off from the adherend due to shrinkage or curl. The lower limit of the CXS of at least one layer is not particularly limited, but is substantially about 0.1%. In order to set the CXS within the above range, it is effective to set the raw material composition of the film to the range described below, and in particular to use a polypropylene raw material with a low CXS.

[0025] The polypropylene film of the present invention is not particularly limited to a single layer or a laminated structure as long as it contains polypropylene, but as described above, the polypropylene film of the present invention is a laminated structure of two or more layers, and at least one layer is preferably a layer containing 50% by mass to 100% by mass of polypropylene having a CXS of 3.5% or less. The layer containing 50% by mass to 100% by mass of polypropylene having a CXS of 3.5% or less is preferably the thickest layer among the layers of the laminated structure. In particular, it is preferable that the inner layer of a three-layer structure is a layer containing 50% by mass to 100% by mass of polypropylene having a CXS of 3.5% or less.

[0026] The polypropylene film of the present invention has a laminated structure of two or more layers, and at least one layer has a crystallization peak temperature (Tc) of 110°C or more, more preferably 112°C or more, and even more preferably 114°C or more, when the temperature is increased from 25°C to 250°C at 20°C / min by a differential scanning calorimeter DSC and then decreased from 250°C to 25°C at 20°C / min. Tc is correlated with the ease of crystallization, and the higher the Tc, the easier it is to crystallize. When the polypropylene film is solidified on a cooling drum after melt extrusion, it crystallizes and forms spherulites. The higher the Tc, the more dense spherulites are generated in the unstretched sheet, and the surface shape of the film after biaxial stretching also has finer protrusions. From the viewpoint of obtaining a surface with fine protrusions that does not transfer dents to the adherend and has good releasability, the higher the Tc, the more preferable it is. There is no particular limit to the upper limit of Tc, but the upper limit is substantially about 125°C. In order to set Tc within the above range, it is effective to set the raw material composition of the film within the range described below, and in particular to use branched polypropylene or a high molecular weight polypropylene raw material. In determining the value of Tc, it is necessary to separate the polypropylene film into layers and evaluate each layer, but if it is difficult to separate the layers, the film as a whole is evaluated and the value is regarded as the representative value.

[0027] The thickness of the polypropylene film of the present invention is not particularly limited and is appropriately adjusted depending on the application, but is preferably 0.5 μm to 100 μm from the viewpoint of handling. In order to make the most of such characteristics, the thickness is more preferably 1 μm to 40 μm, even more preferably 1 μm to 30 μm, and most preferably 6 μm to 30 μm. The thickness can be adjusted by the screw rotation speed of the extruder, the width of the unstretched sheet, the film-forming speed, the stretching ratio, etc., within a range that does not deteriorate other physical properties.

[0028] Next, raw materials for the polypropylene film of the present invention will be described, but the raw materials are not necessarily limited thereto.

[0029] The polypropylene film of the present invention is not particularly limited to a single layer or a laminated structure as long as it contains polypropylene, but as described above, the polypropylene film of the present invention is preferably a laminated structure of two or more layers, and at least one layer is a layer containing 50% by mass to 100% by mass of polypropylene with a CXS of 3.5% or less. In order to obtain a polypropylene film having such a layer (a layer containing 50% by mass to 100% by mass of polypropylene with a CXS of 3.5% or less), it is preferable to use a raw material with a CXS of 3.5% or less (hereinafter, polypropylene with a CXS of 3.5% or less as a raw material is referred to as polypropylene raw material A). The CXS of polypropylene raw material A is more preferably 2.0% or less, and even more preferably 1.5% or less. The content of polypropylene raw material A is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and most preferably 95% by mass or more, when the layer containing polypropylene raw material A is 100% by mass. To obtain a polypropylene raw material that satisfies this CXS, a method of increasing the catalytic activity when obtaining the resin and a method of washing the obtained resin with a solvent or the olefin monomer itself can be used.

[0030] Moreover, from the viewpoints of strength and heat resistance, the polypropylene raw material A is preferably a homopolypropylene.

[0031] The polypropylene raw material A preferably has a melting point of 155° C. or higher, more preferably 160° C. or higher, and even more preferably 165° C. or higher. If the melting point is less than 155° C., the polypropylene raw material A has poor heat resistance, and may shrink and peel off from the adherend or curl when it is laminated to the adherend and passes through a heating process.

[0032] The polypropylene raw material A preferably has a mesopentad fraction of 0.94 or more, more preferably 0.97 or more. The mesopentad fraction is an index of the stereoregularity of the crystalline phase of polypropylene measured by nuclear magnetic resonance (NMR), and the higher the value, the higher the crystallinity, the higher the melting point, and the higher the dimensional stability at high temperatures, which is preferable. There is no particular upper limit for the mesopentad fraction. In order to obtain a resin with such high stereoregularity, a method of washing the resin powder obtained with a solvent such as n-heptane, a method of appropriately selecting a catalyst and / or cocatalyst, and a method of appropriately selecting a composition are preferably used.

[0033] Moreover, as the polypropylene raw material A, the melt flow rate (MFR) is more preferably in the range of 1 to 10 g / 10 min (230°C, 21.18 N load), more preferably 1 to 8 g / 10 min (230°C, 21.18 N load), and particularly preferably in the range of 4 to 8 g / 10 min (230°C, 21.18 N load) from the viewpoint of film formability and film strength. In order to adjust the melt flow rate (MFR) to the above value, a method of controlling the average molecular weight or molecular weight distribution is adopted.

[0034] The polypropylene raw material A may contain copolymerization components with other unsaturated hydrocarbons, or may be blended with polymers, within the scope of the present invention. Examples of monomer components constituting such copolymerization components or blends include ethylene, propylene (in the case of copolymerized blends), 1-butene, 1-pentene, 3-methylpentene-1, 3-methylbutene-1, 1-hexene, 4-methylpentene-1, 5-ethylhexene-1, 1-octene, 1-decene, 1-dodecene, vinylcyclohexene, styrene, allylbenzene, cyclopentene, norbornene, and 5-methyl-2-norbornene. From the viewpoint of dimensional stability, it is preferable that the copolymerization amount or blend amount is less than 1 mol% in terms of copolymerization amount and less than 10 mass% in terms of blend amount.

[0035] The content of the ethylene component contained in the polypropylene raw material A is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less. The higher the content of the ethylene component, the lower the crystallinity and the easier it is to improve transparency, but if the content of the ethylene component exceeds 10% by mass, the strength and heat resistance may decrease, resulting in a worsening of the heat shrinkage rate. In addition, the resin may be easily deteriorated during the extrusion process, and fish eyes may be easily generated in the film. The polyolefin raw material used for the polypropylene film of the present invention may contain various additives, such as a crystal nucleating agent, an antioxidant, a heat stabilizer, a slipping agent, an antistatic agent, an antiblocking agent, a filler, a viscosity modifier, and a color inhibitor, within the scope of not impairing the object of the present invention.

[0036] Among these, the selection of the type and amount of antioxidant is important from the viewpoint of antioxidant bleed-out. That is, such antioxidants are sterically hindered phenol-based, and at least one of them is preferably a high molecular weight type with a molecular weight of 500 or more. Specific examples include various ones, but for example, it is preferable to use 2,6-di-t-butyl-p-cresol (BHT: molecular weight 220.4) in combination with 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene (e.g., BASF's "Irganox" (registered trademark) 1330: molecular weight 775.2) or tetrakis[methylene-3(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane (e.g., BASF's "Irganox" (registered trademark) 1010: molecular weight 1177.7), etc. The total content of these antioxidants is preferably in the range of 0.03 to 1.0 mass% based on the total amount of polyolefin raw material. If the amount of antioxidant is too small, the polymer may deteriorate during the extrusion process, causing the film to become discolored and the long-term heat resistance may be poor. If the amount of antioxidant is too large, the transparency may decrease due to the bleed-out of the antioxidant. The content is more preferably 0.05 to 0.9 mass %, and particularly preferably 0.1 to 0.8 mass %.

[0037] In addition, the polypropylene film of the present invention preferably has at least one layer containing a branched polypropylene. The content of the branched polypropylene in the layer containing the branched polypropylene resin is preferably 0.05 to 10% by mass when the entire layer is taken as 100% by mass. From the viewpoint of increasing the crystallization peak temperature (Tc) of the polypropylene film, controlling the size of the spherulites generated in the cooling process of the melt-extruded resin sheet to be small, and forming dense and fine surface irregularities in which the steep height difference of the film surface irregularities after biaxial stretching is reduced, the lower limit of the content of the branched polypropylene resin is more preferably 0.5% by mass or more, and further preferably 1% by mass or more. On the other hand, the upper limit of the content of the branched polypropylene resin is more preferably 8% by mass or less, and further preferably 5% by mass or less.

[0038] In addition, a crystal nucleating agent can be added to the polypropylene raw material used for the polypropylene film of the present invention, within the scope of the object of the present invention. Examples of crystal nucleating agents include α crystal nucleating agents (dibenzylidene sorbitols, sodium benzoate, etc.), β crystal nucleating agents (potassium 1,2-hydroxystearate, magnesium benzoate, amide-based compounds such as N,N'-dicyclohexyl-2,6-naphthalenedicarboxamide, quinacridone-based compounds, etc.). However, since excessive addition of the above-mentioned other types of nucleating agents may cause a decrease in stretchability or a decrease in transparency and strength due to void formation, etc., the amount added is usually 0.5 mass% or less, preferably 0.1 mass% or less, and more preferably 0.05 mass% or less.

[0039] The polypropylene film of the present invention is preferably biaxially stretched using the above-mentioned raw material. As the biaxial stretching method, any of the inflation simultaneous biaxial stretching method, the stenter simultaneous biaxial stretching method, and the stenter sequential biaxial stretching method can be used. Among them, the stenter sequential biaxial stretching method is preferably used in terms of film formation stability, thickness uniformity, and control of high rigidity and dimensional stability of the film.

[0040] Next, one embodiment of the method for producing a polypropylene film of the present invention will be described as an example, but the present invention is not necessarily limited thereto.

[0041] First, 80 parts by mass of polypropylene raw material A and 20 parts by mass of branched chain polypropylene raw material are dry blended and fed to a single screw extruder for B layer (base layer (II)), and polypropylene raw material A is fed to a single screw extruder for A layer (surface layer (I)), and melt extrusion is performed at 200 to 280 ° C, more preferably 220 to 280 ° C, and even more preferably 240 to 270 ° C. Then, after removing foreign matter and modified polymers with a filter installed in the middle of the polymer tube, the mixture is laminated with a multi-manifold type A layer / B layer / A layer composite T die and discharged onto a casting drum to obtain a laminated unstretched sheet having a layer structure of A layer / B layer / A layer. At this time, the lamination thickness ratio is preferably in the range of 1 / 8 / 1 to 1 / 60 / 1. By setting it to the above range, at least one layer having a CXS of 3.5% or less and at least one layer having a Tc of 112 ° C or more are formed, and a film excellent in heat resistance and mechanical strength at high temperatures can be obtained.

[0042] The surface temperature of the casting drum is preferably 40 to 120°C, more preferably 60 to 120°C, and even more preferably 80 to 110°C. A two-layer laminate structure of layer A / layer B may also be used. The method of adhesion to the casting drum may be any of electrostatic application method, adhesion method using the surface tension of water, air knife method, press roll method, underwater casting method, etc., but the air knife method is preferred because it has good flatness and can control the surface roughness. The air temperature of the air knife is preferably 40 to 100°C, and the blowing air speed is preferably 130 to 150 m / s. In order to prevent vibration of the film, it is preferable to appropriately adjust the position of the air knife so that air flows downstream of the film production.

[0043] The obtained unstretched sheet is introduced into the longitudinal stretching process. In the longitudinal stretching process, the unstretched sheet is first preheated by contacting it with a plurality of metal rolls kept at 10°C to 160°C, preferably 140°C to 158°C, more preferably 145°C to 155°C, and then stretched 4 to 8 times in the longitudinal direction between rolls with a difference in peripheral speed, and then cooled to room temperature. The stretching temperature is 100°C to 150°C, preferably 100°C to 140°C, more preferably 110°C to 130°C. By heating to a high temperature in the preheating process of longitudinal stretching, the β crystals in the unstretched film are transformed into α crystals, and the crystalline state in the polypropylene film can be made uniform. In addition, by setting the stretching temperature lower than the preheating temperature, the polypropylene film can be stretched with high stress. In this way, by uniformizing the crystalline state in the polypropylene film and stretching it with high stress in the longitudinal stretching process, a polypropylene film having excellent mechanical strength at high temperatures and low heat shrinkage force can be obtained. The stretching ratio is preferably from 3 to 6 times, and more preferably from 4 to 5.5 times.

[0044] Next, the longitudinally uniaxially stretched film is introduced into a tenter, the ends of the film are held by clips, and the film is preheated, and then transversely stretched 7 to 13 times in the width direction. At this time, the preheating temperature is increased to a high temperature, the polypropylene film is uniformly preheated, and the polypropylene film is stretched under high stress at a temperature lower than the preheating temperature, thereby obtaining a polypropylene film having excellent mechanical strength at high temperatures and low heat shrinkage force. For this reason, the preheating temperature is 165 to 180°C, more preferably 170 to 180°C, and even more preferably 173 to 180°C. The transverse stretching temperature is 155 to 170°C, more preferably 155 to 165°C, and even more preferably 155 to 160°C.

[0045] In the subsequent heat treatment and relaxation treatment steps, the film is heat-fixed at a temperature of 140°C or higher and lower than 170°C, more preferably 140°C or higher and lower than 160°C, while being tension-held in the width direction with clips, and is guided to the outside of the tenter through a cooling step at 80 to 100°C while being tension-held in the width direction with clips, and the clips at the film end are released, and the film edge is slit in the winder step, and the film product roll is wound up. If the heat treatment is performed at a high temperature of 170°C or higher, the orientation of the polypropylene film may be relaxed, leading to a decrease in mechanical strength. In particular, the decrease in mechanical strength is significant in the high temperature range. Also, if the relaxation treatment is performed at a relaxation rate of 20% or higher, the orientation of the polypropylene film may be relaxed, leading to a decrease in mechanical strength. In particular, the decrease in mechanical strength is significant in the high temperature range.

[0046] The polypropylene film obtained in the above manner can be used for various applications such as packaging films, surface protection films, processing films, sanitary products, agricultural products, construction products, and medical products. Since the polypropylene film has excellent surface smoothness, it can be preferably used as a surface protection film, processing film, or release film, and more preferably used as a release film.

[0047] Next, an example of using the polypropylene film of the present invention as a coating substrate (substrate film) for an adhesive film will be described. The polypropylene film of the present invention can be made into an adhesive film having an adhesive layer on at least one side thereof.

[0048] The adhesive used in the adhesive layer in the adhesive film of the present invention is not particularly limited, and rubber-based, vinyl polymerization-based, condensation polymerization-based, thermosetting resin-based, silicone-based, etc. can be used. Among these, examples of rubber-based adhesives include butadiene-styrene copolymer-based, butadiene-acrylonitrile copolymer-based, and isobutylene-isoprene copolymer-based. Examples of vinyl polymerization-based adhesives include acrylic-based, styrene-based, vinyl acetate-ethylene copolymer-based, and vinyl chloride-vinyl acetate copolymer-based. Examples of condensation polymerization-based adhesives include polyester-based. Examples of thermosetting resin-based adhesives include epoxy resin-based and urethane resin-based.

[0049] Among these, acrylic adhesives are preferably used in consideration of excellent transparency, weather resistance, heat resistance, moist heat resistance, adhesion to substrates, etc. Specific examples of such acrylic adhesives include "SK DYNE" (registered trademark) 1310, 1435, SK DYNE 1811L, SK DYNE 1888, SK DYNE 2094, SK DYNE 2096, SK DYNE 2137, SK DYNE 3096, SK DYNE 1852, etc., manufactured by Soken Chemical & Engineering Co., Ltd.

[0050] In addition, it is preferable to use a curing agent together with the acrylic adhesive. Specific examples of the curing agent include, for example, in the case of isocyanate, toluene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, diphenylmethane-4-4'-diisocyanate, diphenylmethane-2-4'-diisocyanate, 3-methyldiphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4-4'-diisocyanate, dicyclohexylmethane-2-4'-diisocyanate, and lysine isocyanate. The mixing ratio of the curing agent is 0.1 to 10 parts by mass, preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the adhesive. If the amount is less than 0.1 parts by mass, the adhesive layer may not be cured sufficiently in the drying oven, resulting in peeling. If the amount is more than 10 parts by mass, the excess curing agent may migrate to the substrate or gasify at high temperatures, causing contamination.

[0051] In addition, depending on the material of the adherend (glass or functional film), an antioxidant, an ultraviolet absorber, a silane coupling agent, a metal deactivator, etc. may be appropriately added to the acrylic pressure-sensitive adhesive.

[0052] The adhesive film using the polypropylene film of the present invention preferably has a thickness d of the adhesive layer of 2.0 μm or less. More preferably, it is 1.5 μm or less, and even more preferably, it is 1.0 μm or less. If the thickness d of the adhesive layer exceeds 2.0 μm, the slipperiness between the back surface of the base film and the surface of the adhesive layer may deteriorate, making winding difficult. In addition, the drying of the adhesive layer in the drying oven may be insufficient, causing backing. Backing refers to a phenomenon in which a part of the adhesive layer is transferred to the back surface of the base film when the adhesive film is unwound during use after the adhesive film of the present invention is wound into a roll shape without a release film by drying and curing in a drying oven after coating one side of the base film with a solution of the adhesive layer. The method of setting the thickness of the adhesive layer in the above range can be performed by using a known technique, and can be controlled by adjusting the solid content concentration of the solution of the adhesive layer or the coating thickness in various coating methods. If the thickness of the adhesive layer is too thin, stable coating may be difficult, or the adhesive strength may be too low to adhere to the adherend, so the lower limit is about 0.1 μm.

[0053] The adhesive film using the polypropylene film of the present invention preferably has a 180° peel strength of 200 mN / 25 mm or less after being attached to an acrylic plate. The peel strength is more preferably 100 mN / 25 mm or less, and even more preferably 80 mN / 25 mm or less. If the peel strength exceeds 200 mN / 25 mm, the slipperiness between the back surface of the base film and the surface of the adhesive layer may deteriorate, making winding difficult or causing backing. In order to set the peel strength within the above range, it is effective to set the composition and thickness of the adhesive layer to the range described below, and to set the raw material composition of the film and the film-forming conditions to the range described below, and to control the surface roughness of the base film. If the peel strength is less than 10 mN / 25 mm, the adhesive film may peel off during transportation after being attached to the adherend, so the lower limit is about 10 mN / 25 mm.

[0054] Next, a method for producing the adhesive layer will be described, but the method is not necessarily limited thereto.

[0055] First, a coating agent for the adhesive layer is prepared. The coating agent can be used by dissolving the above-mentioned adhesive and additives such as a curing agent in a solvent. The solvent can be appropriately adjusted depending on the drying temperature in the coater and the viscosity of the coating agent, and specific examples include at least one solvent selected from methanol, ethanol, isopropyl alcohol, n-butanol, tert-butanol, ethylene glycol monomethyl ether, 1-methoxy-2-propanol, propylene glycol monomethyl ether, cyclohexanone, toluene, ethyl acetate, butyl acetate, isopropyl acetone, methyl ethyl ketone, methyl isobutyl ketone, diacetyl acetone, and acetyl acetone.

[0056] The solid content concentration in the coating agent is appropriately selected depending on the viscosity of the coating agent and the thickness of the adhesive layer, but is preferably 5 to 20% by mass.

[0057] Next, the above-mentioned base film is conveyed by a coater, and the coating agent for the adhesive layer is applied. Here, the surface to be coated with the adhesive layer may be either side of the base film, but it is preferable to improve the wettability with the coating agent by pretreatment such as corona treatment on the coated surface. On the other hand, it is preferable not to perform pretreatment such as corona treatment on the back surface of the base film in order to improve releasability. The coating method (coating method) is not particularly limited, and existing coating methods such as metabar method, doctor blade method, gravure method, die method, knife method, reverse method, and dip method can be adopted. However, as described above, the adhesive layer has a thickness of 2.0 μm or less, which is a thin film, and the gravure method and reverse method are preferable from the viewpoint of stably obtaining a thin coating layer.

[0058] After the adhesive layer coating agent is applied to the substrate film, the substrate is introduced into a drying oven to remove the solvent in the coating agent to obtain an adhesive film. The drying temperature is appropriately set depending on the heat resistance of the substrate film and the boiling point of the solvent, and is preferably 60 to 170°C. If the temperature is less than 60°C, the adhesive layer may not be cured sufficiently, resulting in backing off. If the temperature exceeds 170°C, the substrate film may deform and the flatness may deteriorate. The drying time is preferably 15 to 60 seconds. If the temperature is less than 15 seconds, the adhesive layer may not be cured sufficiently, resulting in backing off. If the temperature exceeds 60 seconds, the productivity decreases, which is not preferable.

[0059] The dried adhesive film is wound up by a winder without laminating a release film or the like on its adhesive surface to obtain an adhesive film roll. By making the adhesive film of the present invention have the above-mentioned configuration, the adhesive layer is sufficiently cured and the slipperiness between the back surface of the base film and the surface of the adhesive layer is also good, so that even if the film is wound up without a release film, there are no problems such as backing up or wrinkles during winding, and a high-quality adhesive film roll can be obtained.

[0060] The adhesive film of the present invention obtained as described above can be used for various purposes such as packaging films, surface protection films, processing films, sanitary products, agricultural products, building products, and medical products, but since it has particularly excellent surface smoothness, it can be preferably used as a surface protection film or processing film.

[0061] Furthermore, since the polypropylene film of the present invention has excellent heat resistance and quality, it can be preferably used as a release film for optical members, semiconductor manufacturing processes, and the like, which require extremely high quality. EXAMPLES

[0062] The present invention will be described in detail below with reference to examples. The properties were measured and evaluated by the following methods.

[0063] (1) Film thickness The thickness was measured using a micro thickness meter (manufactured by Anritsu Corp.) The film was sampled in a 10 cm square area, and measurements were taken at five random points to calculate the average value.

[0064] (2) Heat shrinkage force, temperature at which the heat shrinkage force becomes 20 mN or more Using a TMA (Model TMA / SS6100 manufactured by SII Nano Technology Co., Ltd.), the thermal shrinkage force curve was measured in the measurement directions (main orientation axis direction and the direction perpendicular thereto) under the following conditions.

[0065] (a) Sample: Width 4 mm x Length 20 mm (b) Temperature program: Heating rate 10°C / min from 30°C <Heat shrinkage force> The heat shrinkage force (mN) at 140° C. was read from the heat shrinkage force curve. The measurement was carried out three times and the average was calculated.

[0066] <Heat shrinkage start temperature> In the above heat shrinkage force curve, the temperature was read when the heat shrinkage force reached 20 mN during the temperature rise process. The measurement was carried out three times and the average was calculated.

[0067] (3) Young’s modulus Young's modulus was measured at 23°C and 65% RH using a film strength and elongation measuring device (AMF / RTA-100) manufactured by Orientec Co., Ltd. Samples were cut to a size of 25 cm in the measurement direction (main orientation axis direction and direction perpendicular thereto) and 1 cm in the direction perpendicular to the measurement direction, and stretched to an original length of 100 mm at a tensile speed of 300 mm / min, and Young's modulus was measured according to the method specified in JIS-Z1702 (1994).

[0068] (4) Young's modulus at 120℃ The Young's modulus at 120°C was measured using a film strength and elongation measuring device (AMF / RTA-100) manufactured by Orientec Co., Ltd. The film was placed in an oven heated to 120°C with the chuck, heated for 1 minute, and then subjected to a tensile test at a tensile speed of 300 mm / min. The sample was cut to a size of 25 cm in the measurement direction (direction perpendicular to the main orientation axis) and 1 cm in the direction perpendicular to the measurement direction, and stretched to an original length of 100 mm at a tensile speed of 300 mm / min, according to the method specified in JIS-Z1702 (1994).

[0069] (5) Maximum point stress at 120℃ The maximum point stress at 120°C was measured using a film strength and elongation measuring device (AMF / RTA-100) manufactured by Orientec Co., Ltd. The film was placed in an oven heated to 120°C with a chuck, heated for 1 minute, and then subjected to a tensile test at a tensile speed of 300 mm / min. The load value at the time of sample breakage was read, and the value was divided by the cross-sectional area of ​​the sample before the test (film thickness x width (10 mm)) to calculate the stress of the breaking strength. Measurements were performed five times for each sample, and the average value was used for evaluation. The film thickness used to calculate the breaking strength was the value measured in (1) above.

[0070] (6) Maximum asperity roughness (St) The measurements were performed using a VertScan2.0 R5300GL-Lite-AC manufactured by Ryoka Systems Co., Ltd., and the attached analysis software was used to perform surface correction of the captured image using a polynomial 4th order approximation to determine the surface shape. The maximum projection roughness (St) refers to the difference between the maximum height value (Peak) and the minimum height value (Valley) within the measurement area. The measurement conditions are as follows. Measurements were performed on both sides of the film, n=3 (number of measurements=3), and the average value of each side was calculated and used as the St for each side. The larger of the St values ​​for both sides of the film is listed in the table. Manufacturer: Ryoka Systems Co., Ltd. Device name:VertScan2.0 R5300GL-Lite-AC Measurement conditions: CCD camera SONY HR-57 1 / 2 inch Objective lens: 5x Intermediate lens: 0.5x Wavelength filter: 530nm white Measurement mode: Wave Measurement software: VS-Measure Version 5.5.1 Analysis software: VS-Viewer Version 5.5.1 Measurement area: 1.252mm x 0.939mm.

[0071] (7) Uneven thickness A polypropylene film was prepared, cut into 10 mm widths, and measured at 20 points at 50 mm intervals along the main orientation axis. The average of the 20 data points was calculated, and the difference (absolute value) between the maximum and minimum values ​​was calculated. The absolute value of the difference between the minimum and maximum values ​​was divided by the average value to determine the thickness unevenness along the main orientation axis of the film. The measurements were performed in an atmosphere of 23°C and 65% RH using a contact-type electronic micrometer (K-312A model) manufactured by Anritsu Corporation.

[0072] (8) Crystallization peak temperature (Tc) Using a differential scanning calorimeter (EXSTAR DSC6220 manufactured by Seiko Instruments Inc.), the temperature of each layer of 3 mg of polypropylene film was raised from 25°C to 250°C at a rate of 20°C / min in a nitrogen atmosphere and held for 5 minutes. The temperature was then lowered from 250°C to 25°C at a rate of 20°C / min. The peak temperature of the heat generation curve obtained during this temperature drop was taken as the crystallization temperature (Tc) of the polypropylene film. When multiple peak temperatures were observed, the highest temperature in the range from 80°C to 130°C was taken as the crystallization temperature (Tc) of the polypropylene film.

[0073] (9) Evaluation of curl after heating Polypropylene film and 40 μm-thick "ZEONORFILM" (registered trademark) manufactured by Zeon Corporation were sampled into a square measuring 100 mm wide and 100 mm long, and the sample was overlapped so that side A of the polypropylene film was in contact with the "ZEONORFILM", sandwiched between two acrylic plates (100 mm wide, 100 mm long) and a load of 2 kg was applied. The sample was left to stand for 1 hour in an atmosphere at 23°C, and then heated in an oven at 120°C for 1 hour, and a bonded sample was removed. The sample was placed on the floor with the ZEONORFILM side down, and the height of the curled bonded sample was measured with a ruler and evaluated according to the following criteria.

[0074] S: The height of the curled laminated sample is less than 5 mm. A: The height of the curled laminated sample is 5 mm or more and less than 10 mm. B: The height of the curled laminated sample is 10 mm or more and less than 15 mm. C: The height of the curled laminated sample is 15 mm or more.

[0075] (10) Planarity of adhesive film having adhesive layer An adhesive film with a 500mm wide adhesive layer wound around a core was unwound by 1m, and free tension (the film was allowed to hang vertically under its own weight) and tensions of 1kg / m and 3kg / m were applied uniformly and without unevenness across the entire width of the film, and the film was visually inspected for any areas of poor flatness such as wrinkles or dents.

[0076] S: Free tension with no poor flatness. A: Poor flatness can be seen with free tension, but disappears with a tension of 1kg / m width. B: Areas of poor flatness are observed with a tension of 1 kg / m width, but disappear with a tension of 3 kg / m width. C: The areas with poor flatness do not disappear even with a tension of 3 kg / m width.

[0077] (9) Width shrinkage of adhesive film having adhesive layer After applying the adhesive coating to a 500 mm wide polypropylene film, the film was introduced into a drying oven at 100°C and transported for 30 seconds at a tension of 200 N to remove the solvent in the coating, obtaining an adhesive film. The width of the polypropylene film and the width of the adhesive film were measured with a tape measure, and the width shrinkage rate was calculated based on the following formula.

[0078] Width shrinkage rate (%) = (500 - adhesive film width) / 500 x 100 Based on the calculated width shrinkage rate, the evaluation was made according to the following criteria.

[0079] S: Width shrinkage rate is less than 0.5%. A: The width shrinkage rate is 0.5% or more and less than 1.0%. B: The width shrinkage rate is 1.0% or more and less than 2.0%. C: The width shrinkage rate is 2.0% or more.

[0080] Example 1 As the raw materials for the surface layer (I), 98.5 parts by mass of homopolypropylene raw material A (MFR: 7.5 g / 10 min, melting point: 163 ° C, CXS: 1.0%) manufactured by Sumitomo Chemical Co., Ltd. and Ziegler-Natta catalyst-based branched chain polypropylene raw material B (Profax PF-814) was dry-blended with 1.5 parts by mass and fed to a single-screw extruder for the surface layer (I), and 98.5 parts by mass of homopolypropylene raw material C (MFR: 4.0 g / 10 min, melting point: 166 ° C, CXS: 1.7%) manufactured by Prime Polymer Co., Ltd. as the raw material for the inner layer (II) and 1.5 parts by mass of the branched polypropylene B were dry-blended and fed to a single-screw extruder for the inner layer (II), melt-extruded at 260 ° C, and after removing foreign matter with a sintered filter with a cut of 20 μm, laminated at a thickness ratio of 1 / 10 / 1 with a feed block type A / B / A composite T die, discharged onto a casting drum with a controlled surface temperature of 102 ° C, and adhered to the casting drum with an air knife to obtain an unstretched sheet. Subsequently, the sheet was preheated to 155 ° C using a ceramic roll, and stretched 4.0 times in the longitudinal direction of the film between rolls at 148 ° C with a peripheral speed difference. The film was then introduced into a tenter-type stretching machine with the ends held by clips, preheated at 180°C for 5 seconds, stretched 9.6 times at 170°C, heat-treated at 167°C while giving 14% relaxation in the width direction, and then cooled to 100°C before being introduced to the outside of the tenter, the clips at the film ends were released, and the film was wound around a core to obtain a polypropylene film with a thickness of 25 μm. The physical properties and evaluation results of the obtained film are shown in Table 1.

[0081] Example 2 90 parts by mass of homopolypropylene raw material D (MFR: 3.0 g / 10 min, melting point: 164°C, CXS: 3.3%) manufactured by Prime Polymer Co., Ltd. and 10 parts by mass of 4-methyl-1-pentene polymer "MX004" (melting point: 230°C) manufactured by Mitsui Chemicals, Inc. were fed from a metering hopper to a twin-screw extruder so as to be mixed in this ratio, melt-kneaded at 260°C, extruded from a die in the form of strands, cooled and solidified in a water tank at 25°C, and cut into chips to obtain polypropylene raw material (1). As the raw material for the surface layer (I), 98 parts by mass of the homopolypropylene raw material C and 2 parts by mass of the polypropylene raw material (1) were dry-blended and fed to a single-screw extruder for the surface layer (I). As the raw material for the inner layer (II), 98.5 parts by mass of the homopolypropylene raw material C and 1.5 parts by mass of the branched chain polypropylene raw material B were dry-blended and fed to a single-screw extruder for the inner layer (II). Melt extrusion was performed at 260 ° C., and after removing foreign matter with a sintered filter with a 20 μm cut, the mixture was laminated at a thickness ratio of 1 / 12 / 1 with a feed block type A / B / A composite T die, discharged onto a casting drum with a surface temperature controlled at 93 ° C., and adhered to the casting drum with an air knife to obtain an unstretched sheet. Subsequently, the sheet was preheated to 153 ° C. using a ceramic roll, and stretched 4.9 times in the longitudinal direction of the film between rolls at 128 ° C. with a peripheral speed difference. The film was then introduced into a tenter-type stretching machine with the ends held by clips, preheated at 179°C for 5 seconds, stretched 9.5 times at 173°C, heat-treated at 148°C while giving 11% relaxation in the width direction, and then cooled to 100°C before being introduced to the outside of the tenter, the clips at the film ends were released, and the film was wound around a core to obtain a polypropylene film with a thickness of 25 μm. The physical properties and evaluation results of the obtained film are shown in Table 1.

[0082] Example 3 As the raw material for the surface layer (I), 98 parts by mass of the homopolypropylene raw material A and 2 parts by mass of the polypropylene raw material (1) were dry-blended and fed to a single-screw extruder for the surface layer (I), and as the raw material for the inner layer (II), 70 parts by mass of the homopolypropylene raw material C and 30 parts by mass of the homopolypropylene raw material A were dry-blended and fed to a single-screw extruder for the inner layer (II), melt-extruded at 250 ° C, and after removing foreign matter with a sintered filter with a 20 μm cut, laminated at a thickness ratio of 1 / 8 / 1 with a feed block type A / B / A composite T die, discharged onto a casting drum with a surface temperature controlled at 58 ° C, and adhered to the casting drum with an air knife to obtain an unstretched sheet. Subsequently, the sheet was preheated to 144 ° C using a ceramic roll, and stretched 4.4 times in the longitudinal direction of the film between rolls at 138 ° C with a peripheral speed difference. The film was then introduced into a tenter-type stretching machine with the ends held by clips, preheated at 176°C for 5 seconds, stretched 8.8 times at 167°C, heat-treated at 163°C while giving 9% relaxation in the width direction, and then cooled to 100°C before being introduced to the outside of the tenter, the clips at the film ends were released, and the film was wound around a core to obtain a polypropylene film with a thickness of 25 μm. The physical properties and evaluation results of the obtained film are shown in Table 1.

[0083] Example 4 As the raw material for the surface layer (I), 95.7 parts by mass of the homopolypropylene raw material D, 2.3 parts by mass of the branched chain polypropylene raw material B, and 2 parts by mass of the polypropylene raw material (1) were dry-blended and fed to a single-screw extruder for the surface layer (I). As the raw material for the inner layer (II), 97.7 parts by mass of the homopolypropylene raw material D and 2.3 parts by mass of the branched chain polypropylene raw material B were dry-blended and fed to a single-screw extruder for the inner layer (II). Melt extrusion was performed at 250°C, foreign matter was removed with a sintered filter with a cutoff of 20 μm, and the mixture was laminated in a thickness ratio of 1 / 10 / 1 with a feed block type A / B / A composite T die, discharged onto a casting drum with a surface temperature controlled at 110°C, and adhered to the casting drum with an air knife to obtain an unstretched sheet. The sheet was then preheated to 159°C using a ceramic roll, and stretched 4.1 times in the longitudinal direction of the film between rolls at 125°C with a difference in peripheral speed. The film was then introduced into a tenter-type stretching machine with its ends held by clips, preheated at 180°C for 5 seconds, stretched 10.2 times at 175°C, and heat-treated at 140°C while giving 14% relaxation in the transverse direction, and then guided to the outside of the tenter through a cooling process at 100°C, the clips at the film ends were released, and the film was wound around a core to obtain a polypropylene film with a thickness of 25 μm. The physical properties and evaluation results of the obtained film are shown in Table 1.

[0084] Example 5 As the raw material for the surface layer (I), 98.5 parts by mass of the homopolypropylene raw material C and 1.5 parts by mass of the branched polypropylene raw material B were dry blended and fed to a single-screw extruder for the surface layer (I), and as the raw material for the inner layer (II), 100 parts by mass of the homopolypropylene raw material C was fed to a single-screw extruder for the inner layer (II), melt extrusion was performed at 250 ° C, foreign matter was removed with a sintered filter with a cut of 20 μm, and then laminated at a thickness ratio of 1 / 10 / 1 with a feed block type A / B / A composite T die, discharged onto a casting drum with a surface temperature controlled at 65 ° C, and adhered to the casting drum with an air knife to obtain an unstretched sheet. Subsequently, the sheet was preheated to 152 ° C using a ceramic roll, and stretched 4.6 times in the longitudinal direction of the film between rolls at 132 ° C with a peripheral speed difference. The film was then introduced into a tenter-type stretching machine with the ends held by clips, preheated at 177°C for 5 seconds, stretched 6.8 times at 169°C, heat-treated at 170°C while giving 16% relaxation in the width direction, and then cooled to 100°C before being introduced to the outside of the tenter, the clips at the film ends were released, and the film was wound around a core to obtain a polypropylene film with a thickness of 25 μm. The physical properties and evaluation results of the obtained film are shown in Table 1.

[0085] Example 6 As the raw material for the surface layer (I), 95 parts by mass of the homopolypropylene raw material D and 5 parts by mass of a metallocene catalyst-based branched chain polypropylene raw material (WAYMAX MFX3 manufactured by Japan Polypropylene Corporation) were dry blended and fed to a single-screw extruder for the surface layer (I). As the raw material for the inner layer (II), 100 parts by mass of the homopolypropylene raw material D were fed to a single-screw extruder for the inner layer (II), melt extrusion was performed at 250 ° C., foreign matter was removed with a sintered filter with a cut of 20 μm, and the mixture was laminated at a thickness ratio of 1 / 10 / 1 with a feed block type A / B / A composite T die, discharged onto a casting drum with a surface temperature controlled at 55 ° C., and adhered to the casting drum with an air knife to obtain an unstretched sheet. Subsequently, the sheet was preheated to 146 ° C. using a ceramic roll, and stretched 4.4 times in the longitudinal direction of the film between rolls at 133 ° C. with a peripheral speed difference. The film was then introduced into a tenter-type stretching machine with the ends held by clips, preheated at 176°C for 5 seconds, stretched 7.8 times at 166°C, heat-treated at 153°C while giving 11% relaxation in the width direction, and then cooled to 100°C before being introduced to the outside of the tenter, the clips at the film ends were released, and the film was wound around a core to obtain a polypropylene film with a thickness of 7 μm. The physical properties and evaluation results of the obtained film are shown in Table 1.

[0086] Comparative Example 1 A polypropylene-based resin (MFR: 2.0 g / 10 min) with a copolymerization composition of 98.4 parts by mass of propylene component and 1.6 parts by mass of ethylene component was fed to a single screw extruder, extruded into a sheet from a T-die at 280°C, cooled and solidified on a cooling roll at 60°C, then stretched 4.4 times longitudinally using a heating roll stretcher set at 141°C, then stretched 9.2 times transversely using a tenter stretcher set at 162°C, and heat-treated at 170°C after transverse stretching to obtain a 30 μm polypropylene-based film. The physical properties and evaluation results of the obtained film are shown in Table 1.

[0087] Comparative Example 2 Novatec SA4L (MFR=5.0 / 10min) manufactured by Japan Polypropylene Corporation was fed into a single-screw extruder, extruded from a T-die at 250°C into a sheet, cooled and solidified with a cooling roll at 30°C, then stretched 4.5 times longitudinally at 135°C, clamped at both ends and introduced into a hot air oven, preheated at 169°C, stretched 8.2 times transversely at 160°C, and then heat-treated at 168°C while relaxing at a relaxation rate of 6.7%, to obtain a 4μm polypropylene film. The physical properties and evaluation results of the obtained film are shown in Table 1.

[0088] Comparative Example 3 75 parts by mass of the homopolypropylene raw material D and 25 parts by mass of calcium carbonate particles (manufactured by Sankyo Flour Milling Co., Ltd., 2480K, particle size: 6 μm) were dry-blended and fed to a single-screw melt extruder for the inner layer (II), and the homopolypropylene raw material D was fed to a single-screw melt extruder for the surface layer (I), melt extruded at 240 ° C, and after removing foreign matter with a sintered filter with a cut of 80 μm, laminated at a thickness ratio of 1 / 50 / 1 with a feed block type B / A / B composite T die, and discharged into a cast drum with a controlled surface temperature of 30 ° C to obtain a cast sheet. Next, the film was preheated to 140 ° C using multiple ceramic rolls and stretched 4.6 times in the longitudinal direction of the film. Next, the end was held by a clip and introduced into a tenter type stretching machine, preheated at 165 ° C for 3 seconds, and then stretched 8.0 times at 160 ° C. In the subsequent heat treatment step, the film was heat-treated at 160°C while being relaxed by 10% in the width direction, and then cooled at 130°C before being led to the outside of the tenter, where the clips on the film ends were released and the film was wound around a core to obtain a polypropylene film with a thickness of 25 μm. The physical properties and evaluation results of the obtained film are shown in Table 1.

[0089] Comparative Example 4 The homopolypropylene raw material A was mixed in a ratio of 99.7 parts by mass, 0.3 parts by mass of N,N'-dicyclohexyl-2,6-naphthalenedicarboxamide (NU-100, manufactured by New Japan Chemical Co., Ltd.) as a β-crystal nucleating agent, and 0.1 parts by mass each of IRGANOX (registered trademark) 1010 and IRGAFOS (registered trademark) 168, manufactured by Ciba Specialty Chemicals, were fed from a metering hopper to a twin-screw extruder, melt-kneaded at 300°C, extruded from a die in the form of strands, cooled and solidified in a water tank at 25°C, and cut into chips to obtain polypropylene raw material (2).

[0090] The homopolypropylene raw material D was fed to a single-screw melt extruder for the inner layer (II), and the polypropylene raw material (2) was fed to a single-screw melt extruder for the surface layer (I). The melt extrusion was carried out at 240°C, and after removing foreign matter with a 60μm cut sintered filter, the mixture was laminated at a thickness ratio of 8 / 1 with a feedblock type A / B composite T die, and discharged into a cast drum with a controlled surface temperature of 90°C to obtain a cast sheet. Then, the film was preheated to 125°C using multiple ceramic rolls and stretched 4.6 times in the longitudinal direction of the film. Next, the film was introduced into a tenter-type stretching machine with the ends held by clips, preheated at 165°C for 3 seconds, and stretched 8.0 times at 160°C. In the subsequent heat treatment step, the film was heat-treated at 160°C while being relaxed by 10% in the width direction, and then cooled at 130°C before being led to the outside of the tenter, the clips at the film ends were released, and the film was wound around a core to obtain a polypropylene film with a thickness of 15 μm. The physical properties and evaluation results of the obtained film are shown in Table 1.

[0091] Comparative Example 5 As the raw material for the surface layer (I), 98.5 parts by mass of the homopolypropylene raw material A and 1.5 parts by mass of the branched polypropylene raw material B were dry-blended and fed to a single-screw extruder for the surface layer (I), and as the raw material for the inner layer (II), 98.5 parts by mass of the homopolypropylene raw material C and 1.5 parts by mass of the branched polypropylene raw material B were dry-blended and fed to a single-screw extruder for the inner layer (II), melt-extruded at 250 ° C, and after removing foreign matter with a sintered filter with a 20 μm cut, laminated at a thickness ratio of 1 / 10 / 1 with a feed block type A / B / A composite T die, discharged onto a casting drum with a surface temperature controlled at 35 ° C, and adhered to the casting drum with an air knife to obtain an unstretched sheet. Subsequently, the sheet was preheated to 153 ° C using a ceramic roll, and stretched 3.7 times in the longitudinal direction of the film between rolls at 148 ° C with a peripheral speed difference. The film was then introduced into a tenter-type stretching machine with the ends held by clips, preheated at 180°C for 5 seconds, stretched 7.2 times at 178°C, heat-treated at 170°C while giving 16% relaxation in the width direction, and then cooled to 100°C before being introduced to the outside of the tenter, the clips at the film ends were released, and the film was wound around a core to obtain a polypropylene film with a thickness of 25 μm. The physical properties and evaluation results of the obtained film are shown in Table 1.

[0092] Comparative Example 6 100 parts by mass of polypropylene resin manufactured by Prime Polymer Co., Ltd., which has a mesopentad fraction of 98.5% as a linear polypropylene and a melt mass flow rate (MFR) of 2.6 g / 10 min, was blended with 0.5 parts by mass of branched polypropylene resin manufactured by Basell (high melt tension polypropylene Profax PF-814 mesopentad fraction of 91.0%), and fed to an extruder at a temperature of 250 ° C., melt extruded into a sheet from a T-type slit die at a resin temperature of 250 ° C., and the molten sheet was cooled and solidified on a casting drum with a diameter of 1 m maintained at 90 ° C., at an air knife temperature of 90 ° C. and an air speed of 140 m / s. Next, the sheet was gradually preheated to 140 ° C., and then passed between rolls with a peripheral speed difference maintained at a temperature of 145 ° C., and stretched 4.8 times in the longitudinal direction. At that time, a radiation heater (output 3.5 kW) was used in the stretching section to supplement the heat and stretch. The film was then introduced into a tenter, stretched 10 times in the width direction at a stretching temperature of 160°C, and then relaxed in the width direction in three stages at a total relaxation rate of 23% (first stage: 12.0%, second stage: 9.0%, third stage: 3.9%). Heat treatment was performed at a heat setting temperature of 150°C and a cooling temperature of 140°C, and then quenched at room temperature for 5 seconds to obtain a biaxially oriented polypropylene film with a film thickness of 3.0 μm. The physical properties and evaluation results of the obtained film are shown in Table 1.

[0093] [Table 1]

[0094] In the table, "direction perpendicular to the main alignment axis" means a direction perpendicular to the main alignment axis direction. [Industrial Applicability]

[0095] As described above, the polypropylene film of the present invention can be used for various applications such as packaging films, release films, processing films, sanitary products, agricultural products, construction products, medical products, etc. In particular, since it has excellent heat resistance, mechanical strength, releasability, and quality, it can be preferably used as a release film or processing film that is subjected to high-temperature processing after being attached to an adherend.

Claims

1. A polypropylene film having a three-layer laminate structure, a surface layer of homopolypropylene with 0.05 to 10% by mass of branched polypropylene added, and a base layer of 100% homopolypropylene or homopolypropylene with 0.05 to 10% by mass of branched polypropylene added, wherein the heat shrinkage forces at 140°C in both the main orientation axis direction and the direction perpendicular thereto are 400 mN or less, the Young's moduli in both the main orientation axis direction and the direction perpendicular thereto are 1.8 GPa or more, the temperatures at which the heat shrinkage forces become 20 mN or more in both the main orientation axis direction and the direction perpendicular thereto are 116°C or more, and at least one side has a maximum protrusion roughness St of 4000 nm or more.

2. The polypropylene film according to claim 1, wherein the maximum point stress at 120°C in both the main orientation axis direction and the direction perpendicular thereto is 80 MPa or more.

3. The polypropylene film according to claim 1 or 2, wherein the thickness variation in the main orientation axis direction is less than 6.0%.

4. The polypropylene film according to any one of claims 1 to 3, having a heat shrinkage force of 95 mN or less at 140°C in a direction perpendicular to the main orientation axis direction.

5. The polypropylene film according to any one of claims 1 to 4, wherein the Young's modulus (GPa) at 120 ° C. in a direction perpendicular to the main orientation axis direction is multiplied by the thickness (μm) of the film to be 1.5 (GPa μm) or more.

6. The polypropylene film according to any one of claims 1 to 5, wherein the thickness of the film is 6 µm or more.

7. The polypropylene film according to any one of claims 1 to 6, which has a laminated structure of two or more layers, at least one of which contains 50% by mass or more and 100% by mass or less of polypropylene having a cold xylene solubles (CXS) content of 3.5% or less.

8. The polypropylene film according to any one of claims 1 to 7, which has a laminated structure of two or more layers, and at least one layer has a crystallization peak temperature (Tc) of 110°C or higher when heated from 25°C to 250°C at 20°C / min in a differential scanning calorimeter DSC and then cooled from 250°C to 25°C at 20°C / min.

9. An adhesive film having an adhesive layer on at least one side of the polypropylene film according to any one of claims 1 to 8.

10. A release film using the polypropylene film according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Polypropylene thermoforming sheet laminating film

    JP2003041017A

  • Polypropylene film

    JP2014051657A

  • Biaxially oriented polypropylene film, metal film laminated film, and film capacitor

    JP2016187959A

  • Polypropylene film and mold release film

    JP2017125184A

  • Polypropylene film roll

    JP2018028075A