Heat shrinkable polyester film

A heat-shrinkable polyester film with controlled composition and manufacturing parameters addresses elongation loss and shrinkage stress issues, ensuring stable processing and adhesion even after long-term storage.

JP7582192B2Active Publication Date: 2024-11-13TOYOBO CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021536941
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-26
Filing Date
2020-07-17
Publication Date
2024-11-13
Estimated Expiration
2040-07-17

AI Technical Summary

Technical Problem

Conventional heat-shrinkable polyester films experience a decrease in tensile elongation over time, leading to breakage during processing, and have issues with shrinkage stress that can cause adhesive peeling or container deformation, especially when used on thin containers.

Method used

A heat-shrinkable polyester film with specific composition and manufacturing parameters, including a high diethylene glycol content, controlled plane orientation, and uniaxial stretching in the width direction, maintaining high heat-shrinkability and low shrinkage stress while preventing elongation loss over time.

Benefits of technology

The film maintains high heat-shrinkability and low shrinkage stress, preventing adhesive peeling and container deformation, ensuring stable processing even after long-term storage, with improved solvent adhesion and reduced breakage risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582192000001
    Figure 0007582192000001
  • Figure 0007582192000002
    Figure 0007582192000002
  • Figure 0007582192000003
    Figure 0007582192000003
Patent Text Reader

Abstract

[Problem] To provide a heat-shrinkable polyester-based film which has a high heat-shrinkability in the main shrinkage direction and a low shrinkage stress, and in which a decrease in tensile elongation at break with time is unlikely to occur. [Solution] A heat-shrinkable polyester-based film satisfies the following requirements (1)-(5). (1) The shrinkage rate (warm water shrinkage rate) when the film is immersed in hot water at 98°C for 10 sec is 40% or more in the main shrinkage direction of the film; (2) the plane orientation coefficient of the film is 0.035-0.070 (inclusive); (3) ethylene terephthalate is the main component, and the amount of diethylene glycol (DEG) component is 6-25 mol% (inclusive) out of 100 mol% of polyhydric alcohol components in the total polyester resin constituting the film; (4) the maximum shrinkage stress in the main shrinkage direction of the film measured in hot air at 90°C is 2-17 MPa (inclusive); and (5) the tensile elongation at break in the direction perpendicular to the main shrinkage direction after the film is allowed to stand for 28 days in an atmosphere of 40°C and 85% relative humidity is 20% or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a heat-shrinkable polyester film, and more particularly to a polyester heat-shrinkable film which is unlikely to break during processing steps such as printing and bag making because the tensile elongation of the film does not decrease even after long-term storage after film formation, and which does not decrease in shrinkage rate over time and is suitable for use as labels for beverage bottles, outer packaging for convenience store lunches, etc. [Background technology]

[0002] In recent years, stretched films (so-called heat-shrinkable films) made of polyvinyl chloride resins, polystyrene resins, polyester resins, etc., have been widely used for label packaging, cap seals, and integrated packaging that serve to protect glass bottles, PET bottles, etc. and display products. Among such heat-shrinkable films, polyvinyl chloride films have problems such as low heat resistance, generating hydrogen chloride gas when incinerated, and causing dioxins. In addition, polystyrene films have poor solvent resistance, require the use of ink with a special composition when printing, and must be incinerated at high temperatures, resulting in the problem of generating a large amount of black smoke accompanied by an unpleasant odor when incinerated. Therefore, polyester-based heat-shrinkable films, which are highly heat-resistant, easy to incinerate, and excellent in solvent resistance, have been widely used as shrink labels, and their usage tends to increase with the increase in the distribution volume of PET containers.

[0003] Normal heat-shrinkable polyester films that shrink significantly in the width direction are widely used. The film is stretched by a tenter stretching method or the like to produce a wide master roll, which is then slit to any width and wound into a roll of any length to produce a film roll product. The film is then subjected to a printing process in roll form to give it a design or to display products. After printing, the film is slit again to the required width and wound into a roll, and then goes through a center sealing process using solvent bonding to make a tube-shaped bag, which is then wound into a roll (to become a label roll).

[0004] The labels are made into tubular bags and wound up, then cut to the required length as they are unwound from the roll to become ring-shaped labels. The ring-shaped labels are attached to the packaged items by hand or other methods, and passed through a steam tunnel or hot air tunnel to shrink them and become labels.

[0005] Heat-shrinkable polyester films are required to be further improved in terms of their shrinkage properties. If the shrinkage stress during shrinkage is too high, the adhesive part of the tube may peel off due to shrinkage, resulting in not only a significant deterioration in appearance but also a loss of the function of protecting the packaged items. In recent years, in order to reduce waste, thin containers are used for lunch boxes and side dishes sold at convenience stores and supermarkets. However, if a shrink label is used on a thin container, problems such as deformation of the container may occur if the shrinkage stress is high. It is important that the shrinkage stress is not too high, and not too low in order to closely protect the packaged items.

[0006] Several methods for improving the shrinkage stress of labels have been reported in the past. Patent Document 1 describes a method for improving the shrinkage stress of labels that contains a diethylene glycol-derived structural unit as a polyhydric alcohol component. , and reduces shrinkage stress. However, the film uniaxially stretched in the width direction described in Patent Document 1 has a problem that the tensile elongation in the longitudinal direction of the film significantly decreases when stored for a long period after film formation. In addition, it is known that the inclusion of a diethylene glycol-derived structural unit facilitates hydrolysis of polyester, and the decrease in molecular weight due to hydrolysis also causes a decrease in tensile elongation.

[0007] The above-mentioned films are not immediately subjected to post-processing such as printing after being produced and wound into a roll, but are usually stored and transported at room temperature, but in some cases may be subjected to a long period of time, such as six months or more, before being subjected to the printing process. If the tensile elongation of the shrink film decreases during this long-term storage, it will be prone to breakage when tension is applied in the longitudinal direction in the post-processing, causing process troubles, and if the elongation decrease is significant, processing will become impossible, which is a problem.

[0008] As a method for improving the decrease in tensile elongation caused by long-term storage (aging), there is a method of biaxial stretching in which the film is stretched not only in the width direction but also in the longitudinal direction, but this is undesirable because it inevitably requires a long and large facility. In addition, it is possible to maintain the elongation by increasing the intrinsic viscosity of the polyester constituting the film, but the range that can be improved by the intrinsic viscosity is small, and in order to increase the intrinsic viscosity, the polymerization time is lengthened to increase the polymerization degree of the polyester, which is costly, and in addition, the filtration pressure increases greatly during melt extrusion, making high-precision filtration difficult, which is undesirable. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. WO2018 / 147249 Summary of the Invention [Problem to be solved by the invention]

[0010] An object of the present invention is to provide a heat-shrinkable polyester film which has a high heat shrinkage rate in the main shrinkage direction, low shrinkage stress, and is less susceptible to deterioration in tensile elongation at break over time. [Means for solving the problem]

[0011] The present inventors have conducted extensive research to solve the above problems and have completed the present invention.

[0012] 1. A heat-shrinkable polyester film satisfying the following requirements (1) to (5): (1) When the film is immersed in 98°C hot water for 10 seconds, the shrinkage rate (hot water shrinkage rate) is 40% or more in the main shrinkage direction of the film. (2) The film's plane orientation coefficient is 0.035 or more and 0.070 or less. (3) The main component is ethylene terephthalate, and the amount of diethylene glycol (DEG) is 6 mol% to 25 mol% of the polyhydric alcohol component (100 mol%) in the total polyester resin that constitutes the film. (4) The maximum shrinkage stress in the main shrinkage direction of the film measured in hot air at 90°C is 2 MPa to 17 MPa. (5) After the film is left in an atmosphere of 40°C and 85% relative humidity for 28 days, the tensile elongation at break in the direction perpendicular to the main shrinkage direction is 20% or more. 2. The heat-shrinkable polyester film according to 1, characterized in that the tensile elongation at break in the direction perpendicular to the main shrinkage direction is 100% or more after the film is aged for 28 days in an atmosphere having an atmospheric temperature of 40°C and a relative humidity of 85%. 3. A heat-shrinkable polyester film according to 1 or 2, characterized in that when the film is aged for 28 days in an atmosphere having an atmospheric temperature of 30°C and a relative humidity of 85%, and then immersed in 70°C hot water for 10 seconds, the difference between the shrinkage rate in the main shrinkage direction and the shrinkage rate before aging is less than 5%. 4. The heat-shrinkable polyester film according to any one of 1. to 3., wherein the heat-shrinkable polyester film has a solvent adhesion strength of 4 N / 15 mm width or more and 15 N / 15 mm width or less. 5. A heat-shrinkable polyester film according to any one of 1. to 4., characterized in that the natural shrinkage rate in the main shrinkage direction after the film is aged for 28 days in an atmosphere having an atmospheric temperature of 40°C and a relative humidity of 85% is less than 1.0%. 6. The heat-shrinkable polyester film according to any one of 1. to 5., wherein the intrinsic viscosity of the film is 0.60 dl / g or more and 0.75 dl / g or less. 7. The heat-shrinkable polyester film according to any one of 1. to 6., wherein the main shrinkage direction is a transverse direction. 8. The heat-shrinkable polyester film according to any one of 1. to 7., which is a uniaxially stretched film. 9. A label obtained from the heat-shrinkable polyester film described in any one of 1. to 8. 10. A package formed by covering at least a portion of the outer periphery of an object to be packaged with the label described in 9. above and then heat-shrinking it. Effect of the Invention

[0013] The heat-shrinkable polyester film of the present invention not only has a high heat shrinkage rate, but also has a low shrinkage stress, so that when it shrinks, the adhesive portion of the label does not peel off, and even if a thin container is used for the packaged item, the container does not deform. Furthermore, since the tensile elongation of the film does not decrease even after aging, it is possible to reduce problems in post-processing after film formation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The heat-shrinkable polyester film of the present invention will be described in detail below. The manufacturing method of the heat-shrinkable polyester film will be described in detail later, but the heat-shrinkable film is usually obtained by conveying and stretching using rolls or the like. At this time, the conveying direction of the film is called the longitudinal direction (or vertical direction), and the direction perpendicular to the longitudinal direction is called the width direction (or horizontal direction) of the film. Therefore, the width direction of the heat-shrinkable polyester film shown below is the direction perpendicular to the unwinding direction of the roll, and the longitudinal direction of the film is the direction parallel to the unwinding direction of the roll. In the present invention, it is preferable that the main shrinkage direction of the film is the width direction.

[0015] In order to obtain high heat shrinkability in heat shrinkable polyester films, it is widely practiced to copolymerize other polyvalent carboxylic acid components and other polyhydric alcohol components with homopolymers of ethylene terephthalate (PET). As polyhydric alcohol components to be used as copolymerized components, for example, neopentyl glycol and 1,4-cyclohexanediethanol are considered and widely used, but it is known that in the case of films copolymerized with these components, the heat shrinkability at low temperatures below 70°C decreases significantly over time in a temperature atmosphere of room temperature to about 40°C. On the other hand, the present inventors have found that in the case of films copolymerized with PET and diethylene glycol, such a decrease in the heat shrinkage rate at low temperatures over time is suppressed, and high heat shrinkability can be expressed and solvent adhesion is also excellent. In addition, when obtaining a raw material resin copolymerized with diethylene glycol, since diethylene glycol is liquid at room temperature, the melting process essential for powder raw materials such as neopentyl glycol is not required. Furthermore, compared to neopentyl glycol, it has the advantage of having a higher polymerization activity and less foaming during polymerization, which leads to a decrease in productivity.

[0016] The heat-shrinkable polyester film of the present invention is mainly composed of ethylene terephthalate. Here, the main component means that 50 mol% or more of all polymer components constituting the film is ethylene terephthalate. It is more preferable that the film contains 70 mol% or more of ethylene terephthalate. By using ethylene terephthalate as the main component, it is possible to obtain excellent mechanical strength and transparency.

[0017] As a polymerization method for polyethylene terephthalate (hereinafter, sometimes simply referred to as PET), any production method can be used, such as a direct polymerization method in which terephthalic acid is directly reacted with ethylene glycol, and, if necessary, other dicarboxylic acid components and diol components, and an ester exchange method in which a dimethyl ester of terephthalic acid (containing, if necessary, a methyl ester of another dicarboxylic acid) is subjected to an ester exchange reaction with ethylene glycol (containing, if necessary, another diol component).

[0018] Examples of dicarboxylic acid components other than terephthalic acid that constitute the polyester used in the film of the present invention include aromatic dicarboxylic acids such as isophthalic acid, naphthalenedicarboxylic acid, orthophthalic acid, aliphatic dicarboxylic acids such as adipic acid, azelaic acid, sebacic acid, decanedicarboxylic acid, and alicyclic dicarboxylic acids. The content of these dicarboxylic acid components other than terephthalic acid is preferably 0 mol % or more and 15 mol % or less, more preferably 0 mol % or more and 10 mol % or less, and particularly preferably 0 mol % or more and 4 mol % or less, based on 100 mol % of the polyvalent carboxylic acid component.

[0019] When an aliphatic dicarboxylic acid (such as adipic acid, sebacic acid, decadicarboxylic acid, etc.) is contained, the content is preferably 0 mol % or more and less than 3 mol %. Heat-shrinkable polyester films obtained using polyesters containing 3 mol % or more of these aliphatic dicarboxylic acids have insufficient film stiffness when installed at high speed.

[0020] It is also preferable not to contain trivalent or higher polyvalent carboxylic acids (e.g., trimellitic acid, pyromellitic acid, and anhydrides thereof, etc.), since it becomes difficult to achieve the required shrinkage in heat-shrinkable polyester films obtained by using polyesters containing these polyvalent carboxylic acids.

[0021] It is necessary that diethylene glycol accounts for 6 mol % or more and 25 mol % or less of 100 mol % of the polyhydric alcohol component constituting the polyester used in the film of the present invention.

[0022] Examples of polyhydric alcohol components other than ethylene glycol and diethylene glycol constituting the polyester used in the present invention include aliphatic diols such as 1-3 propanediol, 1-4 butanediol, neopentyl glycol, and hexanediol, alicyclic diols such as 1,4-cyclohexanedimethanol, and aromatic diols such as bisphenol A. The content of these polyhydric alcohol components other than ethylene glycol and diethylene glycol is preferably 0 mol % or more and 15 mol % or less, more preferably 0 mol % or more and 10 mol % or less, and particularly preferably 0 mol % or more and 4 mol % or less, based on 100 mol % of the polyhydric alcohol components.

[0023] It is preferable not to contain diols having 8 or more carbon atoms (e.g., octanediol, etc.) or polyhydric alcohols having three or more valences (e.g., trimethylolpropane, trimeritolethane, glycerin, diglycerin, etc.). Heat-shrinkable polyester films obtained using polyesters containing these diols or polyhydric alcohols are difficult to achieve the required high shrinkage.

[0024] Various additives, such as waxes, antioxidants, antistatic agents, crystal nucleating agents, viscosity reducers, heat stabilizers, coloring pigments, coloring inhibitors, and ultraviolet absorbers, may be added to the resin forming the heat-shrinkable polyester film of the present invention, as necessary.

[0025] It is preferable to add fine particles as a lubricant to improve the workability (slipperiness) of the film to the resin forming the heat-shrinkable polyester film of the present invention. Any fine particles can be selected, and examples of inorganic fine particles include silica, alumina, titanium dioxide, calcium carbonate, kaolin, barium sulfate, etc., and organic fine particles include acrylic resin particles, melamine resin particles, silicone resin particles, crosslinked polystyrene particles, etc. The average particle size of the fine particles can be appropriately selected as needed within the range of 0.05 to 3.0 μm (measured with a Coulter counter). The lower limit of the fine particle content in the film is preferably 0.01% by weight, more preferably 0.015% by weight, and even more preferably 0.02% by weight. If it is less than 0.01% by weight, the slipperiness may decrease. The upper limit is preferably 1% by weight, more preferably 0.2% by weight, and even more preferably 0.1% by weight. If it exceeds 1% by weight, the transparency may decrease, which is not preferable.

[0026] The method of blending the above particles into the resin forming the heat-shrinkable polyester film can be, for example, addition at any stage of the production of the polyester resin, but it is preferable to add the particles as a slurry dispersed in ethylene glycol or the like at the stage of esterification or after the completion of the transesterification reaction and before the start of the polycondensation reaction, and proceed with the polycondensation reaction. It is also preferable to blend a slurry of the particles dispersed in ethylene glycol or water or the like with the polyester resin raw material using a vented kneading extruder, or to blend the dried particles with the polyester resin raw material using a kneading extruder.

[0027] In order to prevent problems during processing even after long-term storage, it is preferable that the tensile elongation of the heat-shrinkable polyester film is small over time. In general, the molecular orientation contributes greatly to the elongation of the film against tension. When the molecular chains of a polymer are stretched by stretching (the molecules are oriented), the rigidity increases, and furthermore, the molecules are entangled with each other to form a strong network, which makes the film stronger against tension and improves its elongation. However, it is known that the elongation against tension decreases over a long period of time after film formation (aging) because the molecular orientation is relaxed. It is also known that the molecular weight decreases due to hydrolysis of polyester over time, and the elongation against tension decreases. It has been found that it is possible to prevent the decrease in elongation over time by sufficiently increasing the molecular orientation (planar orientation) in the film plane direction after film formation against this deterioration over time. It is considered that when the planar orientation is high, the rigidity and entanglement of the molecular chains are strong, which is difficult to relax over time, and even if hydrolysis occurs, the decrease in elongation is unlikely to occur. A method for evaluating the decrease in elongation over time will be described later. A method for increasing the planar orientation will also be described later.

[0028] In addition, it is preferable that the heat shrinkable polyester film of the present invention has a heat shrinkage rate in the main shrinkage direction of the film (i.e., hot water heat shrinkage rate at 98°C) of 40% or more when treated in 98°C hot water for 10 seconds under no load, calculated from the lengths before and after shrinkage using the following formula 1. Heat shrinkage rate = {(length before shrinkage - length after shrinkage) / length before shrinkage} × 100 (%) Formula 1

[0029] If the hot water shrinkage rate in the main shrinkage direction at 98°C is less than 40%, when the film is used for beverage labels or lunch box packaging, the shrinkage amount is small, which is undesirable because it causes wrinkles and sagging in the label after heat shrinkage. It is more preferable that the hot water shrinkage rate at 98°C is 42% or more, and particularly preferably 45% or more.

[0030] The hot water shrinkage rate in the main shrinkage direction at 70°C is not particularly limited, but is preferably 10% to 40%. If it is less than 10%, it is not preferable when used as a beverage label or a film for lunch box packaging, because the shrinkage amount is small and label wrinkles and sagging occur after heat shrinkage. Also, if it is 40% or more, it is not preferable because rapid shrinkage occurs inside a shrink tunnel using steam, resulting in wrinkles and distortion. More preferably, it is 15% to 35%, and particularly preferably 20% to 30%.

[0031] The plane orientation coefficient of the film is preferably 0.035 or more and 0.070 or less. The plane orientation coefficient is calculated by the following formula 2. Plane orientation coefficient ΔP=(Nx+Ny) / 2-Nz Equation 2 Nx: Refractive index in the longitudinal direction of the film Ny: Refractive index in the film width direction Nz: Refractive index in the film thickness direction

[0032] If the plane orientation coefficient is less than 0.035, the initial breakage due to aging, which will be described later, will deteriorate, and the tensile elongation will decrease if the film is stored for a long period of time after film formation, which is undesirable. If the plane orientation coefficient is more than 0.070, the crystallinity will be too high, and the solvent adhesive strength will decrease when the film is made into a tube-shaped bag for a beverage label, which is undesirable. The plane orientation coefficient is more preferably 0.040 to 0.065, and even more preferably 0.045 to 0.060.

[0033] Of the 100 mol % polyhydric alcohol components constituting the polyester used in the film of the present invention, diethylene glycol is preferably 6 mol % or more and 25 mol % or less. If the diethylene glycol content is less than 6 mol %, the shrinkage rate at 70°C for 10 seconds over time, as described below, is significantly reduced, which is not preferred. If the diethylene glycol content exceeds 25 mol %, the planar orientation coefficient is reduced, and elongation is likely to decrease over time, which is not preferred. The content ratio of diethylene glycol is more preferably 8 mol % or more and 24 mol % or less, even more preferably 10 mol % or more and 23 mol % or less, and particularly preferably 12 mol % or more and 21 mol % or less.

[0034] The heat-shrinkable polyester film of the present invention preferably has a maximum shrinkage stress in the main shrinkage direction of 2 MPa to 17 MPa as measured under hot air at 90° C. The shrinkage stress is measured by the method described in the examples. If the maximum shrinkage stress at 90°C in the main shrinkage direction exceeds 17 MPa, the label attachment portion may lift or peel off, or a thin-walled container may be crushed due to the shrinkage stress during shrinkage, which is not preferred. The maximum shrinkage stress at 90°C is more preferably 15 MPa or less, and even more preferably 13 MPa or less. If the maximum shrinkage stress at 90°C is less than 2 MPa, the label may become loose and not adhere to the container when used as a label for the container, which is not preferred. The maximum shrinkage stress at 90°C is more preferably 3 MPa or more, and even more preferably 4 MPa or more.

[0035] The polyester used in the film of the present invention preferably has a tensile elongation at break in the longitudinal direction of the film of 20% or more after the film is aged for 28 days in an atmosphere of 40°C and 85% relative humidity. If the elongation at break after aging falls below 20%, it is undesirable because the film is likely to break due to tension in the process when it is aged after long-term storage. The elongation at break before and after aging is more preferably in the range of 100% or more, even more preferably 200% or more, and particularly preferably 300% or more. The higher the elongation at break, the better, but in the case of the product of the present invention, the upper limit is 700%.

[0036] The heat-shrinkable polyester film of the present invention is preferably aged for 28 days under an atmosphere of 40°C and 85% relative humidity, and then immersed in 70°C warm water for 10 seconds, with the difference between the shrinkage rate in the main shrinkage direction and the shrinkage rate before aging being 0% or more and 5% or less. If the shrinkage rate difference exceeds 5%, the shrinkage rate at low temperatures decreases when the formed film is stored for a long period of time, which is undesirable because wrinkles and shrinkage spots tend to occur when the film is shrunk as a label or the like. More preferably, the shrinkage rate difference is 4% or less, and particularly preferably 3% or less. The lower limit of the shrinkage rate difference is the more preferable, but since it is unlikely that the shrinkage rate will increase after aging, 0% is considered to be the lower limit.

[0037] The heat-shrinkable polyester film of the present invention preferably has a solvent adhesion strength of 4 (N / 15 mm) or more. If the solvent adhesion strength is less than 4 (N / 15 mm), the solvent-bonded portion is likely to peel off due to the shrinkage force when the label is heat-shrunk, which is not preferable. The solvent adhesion strength is more preferably 5 (N / 15 mm) or more, and particularly preferably 7 (N / 15 mm) or more. The higher the solvent adhesion strength, the better, but the upper limit of the solvent adhesion strength is thought to be about 15 (N / 15 mm). If the solvent adhesion strength is too high, when two films are solvent-bonded to form a label, the films are likely to be unnecessarily bonded together, which may reduce the productivity of the label, so a solvent adhesion strength of 10 (N / 15 mm) or less may be acceptable in practice.

[0038] The heat-shrinkable polyester film of the present invention preferably has a natural shrinkage rate of 1.0% or less in the main shrinkage direction after aging for 28 days in an atmosphere at a temperature of 40° C. and a humidity of 85% RH. The method for evaluating the natural shrinkage rate is shown in the Examples. If the natural shrinkage rate exceeds 1.0%, the film roll is likely to wrinkle when the product is stored in a roll shape, which is undesirable. The smaller the natural shrinkage rate, the more preferable it is. The natural shrinkage rate is preferably 0.9% or less, and more preferably 0.8% or less. More preferred.

[0039] The intrinsic viscosity (IV) of the heat-shrinkable polyester film of the present invention is preferably 0.60 dl / g or more and 0.75 dl / g or more. If the intrinsic viscosity (IV) of the film is 0.60 dl / g or more, the tensile elongation does not decrease even if the film is stored for a long time, and the occurrence of troubles such as breakage during processing and defects can be reduced. In addition, in order to increase the intrinsic viscosity, the polymerization time is extended to increase the polymerization degree of the polyester, which is costly, and the filtration pressure increases greatly during melt extrusion, making high-precision filtration difficult, so the upper limit is preferably 0.75 dl / g.

[0040] The thickness of the heat-shrinkable polyester film of the present invention is not particularly limited, but is preferably 8 to 100 μm, more preferably 10 to 60 μm, for use as a heat-shrinkable film for label applications or lunch box packaging. If the film is less than 8 μm thick, the stiffness of the film is significantly reduced, and the roll is prone to wrinkles, which is undesirable. On the other hand, even if the film is thick, there is no problem as a film roll, but it is preferable to make the film thinner from the viewpoint of cost. The film thickness is more preferably 10 to 58 μm, and particularly preferably 12 to 56 μm.

[0041] The heat-shrinkable polyester film of the present invention can be obtained by melt-extruding the above-mentioned polyester raw material with an extruder to form an unstretched film, and then stretching the unstretched film in the width direction. The polyester can be obtained by polycondensing the above-mentioned suitable dicarboxylic acid component and diol component by a known method. In addition, chip-shaped polyester is usually used as the raw material for the film.

[0042] When melt extruding the raw resin, it is preferable to dry the polyester raw material using a dryer such as a hopper dryer or a paddle dryer, or a vacuum dryer. After drying the polyester raw material in this way, it is melted at a temperature of 230 to 270°C and extruded into a film using an extruder. For extrusion, any existing method such as a T-die method or a tubular method can be used.

[0043] The extruded sheet-like molten resin can then be quenched to obtain an unstretched film. As a method for quenching the molten resin, a method in which the molten resin is cast from a die onto a rotating drum and rapidly cooled and solidified to obtain a substantially unoriented resin sheet can be suitably adopted.

[0044] The unstretched film thus obtained can be stretched in the width direction under predetermined conditions to obtain the heat-shrinkable polyester film of the present invention. Preferred stretching methods for obtaining the heat-shrinkable polyester film of the present invention are described below.

[0045] A typical heat-shrinkable polyester film is produced by stretching an unstretched film in the direction in which it is desired to shrink. In the present invention, the film is uniaxially stretched in the width direction, which is the main shrinkage direction. The production method using uniaxial stretching in the width direction has the advantage that it can be produced with simple equipment since no equipment for stretching in the longitudinal direction is used.

[0046] For widthwise stretching, the unstretched film is introduced into a tenter device capable of heating the film by holding both ends of the film with clips, and the film is preheated to a temperature of Tg+10°C or higher and 25°C or lower with hot air. The film is then stretched by increasing the distance between the clips while transporting it in the longitudinal direction. The stretch ratio is preferably 4.5 times or more and 6 times or less. If the stretch ratio is less than 4.5, it is difficult to obtain the required plane orientation coefficient, which is not preferable. If the stretch ratio is more than 6 times, the risk of breakage during film formation increases and the equipment becomes long and large, which is not preferable. More preferably, it is 4.7 times or more and 5.8 times or less.

[0047] The stretching strain rate is preferably different between the first and second halves of the stretching, and the ratio of the stretching strain rates in the first and second halves of the stretching (stretching strain rate ratio) is expressed by the following formula, and the stretching strain rate ratio is preferably 2.5 to 5.0. The stretching strain rate is expressed as a nominal strain per unit time (second) (% / s). Stretching strain rate ratio = (Stretching strain rate in the second half of stretching) ÷ (Stretching strain rate in the first half of stretching) Equation 3

[0048] Here, the first half of the stretching refers to the stretching up to the square root of the final stretching ratio, and the second half of the stretching refers to the stretching thereafter. For example, when the final stretching ratio is 5.0 times, the first half of the stretching refers to the stretching up to a ratio of 2.2 times, and the remaining stretching of 2.3 times thereafter is the second half of the stretching. When the stretching strain rate ratio is less than 2.5, the necessary plane orientation coefficient is not obtained, which is not preferable. When the stretching strain rate ratio is more than 5.0, breakage during stretching is likely to occur, and the shrinkage stress of the film is high, which is not preferable. More preferably, it is 2.7 to 4.8, and even more preferably, it is 2.9 to 4.6.

[0049] In addition, the total stretching strain rate from the start to the end of stretching is preferably 10% / sec or more and 30% / sec or less. If it is less than 10% / sec, the molecular orientation becomes small and the initial breakage over time becomes worse, which is not preferable. If it exceeds 30% / sec, the shrinkage stress of the film becomes too high, which is not preferable. More preferably, it is 13% or more and 27% or less, and even more preferably, it is 16% or more and 24% or less.

[0050] As described above, the stretching strain rate ratio of 2.5 to 5.0 means that the stretching rate is faster in the latter half of the stretching than in the first half, and the strain rate is accelerated. As a result of the inventor's research, it was found that by increasing the strain rate in the latter half of the stretching, the molecular orientation of the film is increased, the plane orientation coefficient is increased, and the elongation is less likely to decrease over time. It is known that the stress value increases significantly in the latter half of the stretching in the stress-strain curve of the unstretched film in the heat tensile test, and it is considered that the molecular orientation progresses significantly in the latter half of the stretching. It is considered that by increasing the stretching rate in the latter half of the stretching, the stretching stress becomes higher and the molecular orientation becomes higher. Conventionally, in tenter stretching, stretching is performed at an almost constant speed from the start to the end of stretching (i.e., the stretching strain rate ratio is approximately 1), and at this time, although it is effective in increasing the molecular orientation, the energy given to the film by stretching becomes large, and the shrinkage stress of the film after stretching becomes too high, which is not preferable. In the present invention, it is important to reduce the shrinkage stress in the main shrinkage direction of the film while suppressing a decrease in elongation in the direction perpendicular to the main shrinkage direction of the film over time, by setting the stretching strain rate low in the first half of the stretching and high in the second half.

[0051] Specifically, the stretching strain rate is adjusted by adjusting the film transport speed in the tenter and the tenter pattern, and the stretching strain rate ratio is adjusted by the tenter pattern. It is preferable not to perform longitudinal stretching since it requires large-scale equipment. In addition, although not particularly limited, heat treatment may be performed after widthwise stretching to adjust the shrinkage rate. The heat treatment temperature is preferably 70°C or higher and 110°C or lower. Heat treatment at less than 70°C is not preferable because the widthwise shrinkage rate at 70°C exceeds 40%. Furthermore, if the heat treatment temperature exceeds 110°C, it is not preferable because the widthwise shrinkage rate at 98°C falls below 40%. A more preferable range is 75°C or higher and 105°C or lower, and even more preferably 80°C or higher and 100°C or lower.

[0052] The film temperature during width direction stretching is preferably Tg+5°C or more, Tg+40°C. If the film temperature is less than Tg+5°C, the stretching force becomes too high, which is undesirable as it increases the shrinkage stress of the film. If the film temperature exceeds Tg+40°C, the stretching force is too low, which is undesirable as it does not provide molecular orientation and reduces the planar orientation, which makes it easy for elongation to decrease over time. Although not particularly limited, the film temperature may be the same in the first and second half of stretching, but it is preferable that the temperature in the second half of stretching is lower than that in the first half, as this increases the planar orientation.

[0053] The packaging body of the present invention is formed by covering at least a part of the outer periphery of the packaging object with a label obtained from the heat-shrinkable polyester film of the present invention and heat-shrinking it. Examples of the packaging object include PET bottles for beverages, various bottles, cans, plastic containers for sweets and lunch boxes, and paper boxes. In addition, when the label obtained from the heat-shrinkable polyester film is heat-shrunk to cover such packaging objects, the label is usually heat-shrunk by about 5 to 70% to be adhered to the packaging body. In addition, the label to be covered on the packaging object may or may not be printed.

[0054] The method for producing the label is to apply an organic solvent to one side of a rectangular film, slightly inward from the edge, and then immediately roll the film and overlap and glue the edges together to form a label, or to apply an organic solvent to one side of a rolled film, slightly inward from the edge, and then immediately roll the film and overlap and glue the edges together to form a tube, which is then cut into a label. As the organic solvent for adhesion, cyclic ethers such as 1,3-dioxolane or tetrahydrofuran are preferred. Other examples that can be used include aromatic hydrocarbons such as benzene, toluene, xylene, and trimethylbenzene, halogenated hydrocarbons such as methylene chloride and chloroform, and phenols such as phenol, or mixtures of these. EXAMPLES

[0055] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the embodiments of the examples, and can be modified as appropriate without departing from the spirit of the present invention.

[0056] The film was evaluated as follows.

[0057] [Tg (glass transition temperature)] Using a differential scanning calorimeter (DSC220, manufactured by Seiko Electric Industries Co., Ltd.), 5 mg of the unstretched film was placed in a sample pan, the pan was covered, and the temperature was increased from -40°C to 120°C at a heating rate of 10°C / min in a nitrogen gas atmosphere. Tg (°C) was determined based on JIS-K7121-1987.

[0058] [Intrinsic viscosity (IV)] 0.2 g of polyester was dissolved in 50 ml of a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (60 / 40 (weight ratio)), and the viscosity was measured using an Ostwald viscometer at 30° C. The unit is dl / g.

[0059] [Heat shrinkage rate (hot water heat shrinkage rate)] The film was cut into a 10 cm x 10 cm square and immersed in warm water of a specified temperature ±0.5°C for 10 seconds without load to allow it to shrink, then immersed in water at 25°C ±0.5°C for 10 seconds and pulled out of the water to measure the longitudinal and transverse dimensions of the film, and the thermal shrinkage rate was calculated according to the following formula (1). The direction with the largest thermal shrinkage rate was determined as the main shrinkage direction. Heat shrinkage rate = {(length before shrinkage - length after shrinkage) / length before shrinkage} x 100 (%) Formula 1

[0060] [Maximum shrinkage stress] A strip-shaped film sample having a length of 150 mm in the main shrinkage direction and a width of 20 mm was cut out from the heat-shrinkable film, and the shrinkage stress was measured using a Tesilon universal testing machine PTM-250 (registered trademark of Orientec Co., Ltd.) with a heating furnace manufactured by Toyo Baldwin Co., Ltd. (currently Orientec Co., Ltd.). The heating furnace of the strength and elongation measuring machine was heated to 90°C in advance, and the distance between the chucks for holding the film sample was 100 mm. When attaching the sample to the chuck of the strength and elongation measuring machine, the air blowing of the heating furnace was stopped once, the door of the heating furnace was opened, and 25 mm each of both ends of the sample with a length of 150 mm was clamped between the chucks, the distance between the chucks was set to 100 mm, and the sample was fixed without loosening so that the distance between the chucks and the length direction of the sample coincided and the sample was horizontal. After attaching the sample to the chuck, the door of the heating furnace was quickly closed, and the air blowing was resumed. The point at which the door of the heating furnace was closed and air flow was resumed was regarded as the starting point for measuring the shrinkage stress, and the maximum value of the measured shrinkage stress from the starting point for measuring the shrinkage stress up to 30 seconds after the start of the measurement was regarded as the maximum value of the shrinkage stress (maximum shrinkage stress (MPa)).

[0061] [Change in shrinkage rate over time] After leaving the film in an atmosphere of 40°C x 85% RH for 28 days (672 hours) (aging), the above hot water shrinkage was measured in 70°C hot water to determine the 70°C hot water shrinkage in the longitudinal direction. The difference from the 70°C hot water shrinkage in the longitudinal direction before aging was determined and this was recorded as the "difference in shrinkage before and after aging."

[0062] [Solvent adhesion strength] 1,3-dioxolane was applied to a heat-shrinkable film in an amount of 5±0.3 g / m2 with a width of 5±1 mm, and two sheets were laminated together to form a seal. Then, a piece was cut to a width of 15 mm in the direction perpendicular to the sealing direction, and placed in a Baldwin Corporation universal tensile tester STM-50 with a chuck distance of 20 mm, and tensile peeled at a tensile speed of 200 mm / min to measure the peel resistance. The strength at that time was taken as the solvent adhesion strength.

[0063] [Natural shrinkage rate] The film was cut into a size of 200 mm × 30 mm (main shrinkage direction × perpendicular direction), and a 150 mm long marked line was drawn in the main shrinkage direction. After leaving the film for 28 days (aging) in an atmosphere of 40°C and 85% RH, the length of the marked line was measured and the natural shrinkage rate was calculated by the following formula. Natural shrinkage rate = (length of the gauge line before aging (150 mm) - length of the gauge line after aging) ÷ (length of the gauge line before aging (150 mm) × 100 (%) Formula 4

[0064] [Face orientation coefficient] The refractive index in the longitudinal, transverse and thickness directions of the film was measured using an Abbe Refractometer Model 4T manufactured by Atago Co., Ltd., after leaving each sample film in an atmosphere of 23°C and 65% RH for more than 2 hours. The plane orientation coefficient was calculated from the measurement results using the following formula 2. Plane orientation coefficient ΔP=(Nx+Ny) / 2-Nz Equation 2 Nx: Refractive index in the longitudinal direction of the film Ny: Refractive index in the film width direction Nz: Refractive index in the film thickness direction

[0065] [Tensile elongation at break] According to JIS-K-7127, a rectangular sample with a length of 50 mm in the direction perpendicular to the main shrinkage direction (film longitudinal direction) × length of 20 mm in the main shrinkage direction (film width direction) was prepared as a test piece, and a universal tensile tester (Shimadzu Corporation, Autograph (registered trademark)) was used to hold both ends of the test piece (longitudinal ends) and perform a tensile test at a tensile speed of 200 mm / min, and the elongation at break was taken as the breaking elongation. The tensile test was performed after film formation and after leaving it for 28 days (aging) in an atmosphere at a temperature of 40°C and 85% RH.

[0066] [Shrinkage finish (before and after aging)] A three-color print was applied to the heat-shrinkable film in advance using green, gold, and white inks from Toyo Ink Mfg. Co., Ltd. Then, both ends of the printed film were glued with dioxolane to prepare a cylindrical label (a label with the main shrinkage direction of the heat-shrinkable film as the circumferential direction), which was then cut. The diameter of the label in the shrinkage direction was 70 mm. Then, using a steam tunnel (model: SH-1500-L) manufactured by Fuji Astec Inc., the label was attached to a 500 ml PET bottle (body diameter 62 mm, minimum diameter of neck 25 mm) by heat shrinking it at a zone temperature of 90°C for 4 seconds. When attaching the label, the neck was adjusted so that the 30 mm diameter part was at one end of the label. The finish after shrinkage was evaluated visually, with the following criteria:

[0067] Label shrinkage distortion To evaluate the finish after shrinkage, the distortion of the top of the attached label in the 360-degree direction was measured using a gauge to determine the maximum distortion value. Evaluation was made according to the following criteria. ○: Maximum distortion less than 2.0 mm ×: Maximum distortion 2.0mm or more

[0068] [Label shrinkage is insufficient] The above-mentioned label shrinkage state was evaluated according to the following criteria. ○: The label is shrunk without any slack between the attached label and the container. ×: There is slack between the label and the container due to insufficient shrinkage.

[0069] [Wrinkles on label] Under the same conditions as those for the shrinkage distortion of the label described above, the occurrence of wrinkles was evaluated according to the following criteria. ○: The number of wrinkles larger than 2 mm is 2 or less. ×: 3 or more wrinkles measuring 2 mm or more.

[0070] [Peeling of adhesive joints] The above-mentioned label shrinkage state was evaluated according to the following criteria. ○: No peeling between the labels. ×: Peeling occurred at the adhesive joints between labels.

[0071] <Preparation of polyester raw materials> [Synthesis Example 1] In a stainless steel autoclave equipped with a stirrer, a thermometer and a partial reflux condenser, 100 mol% of dimethyl terephthalate (DMT) as a dicarboxylic acid component and 100 mol% of ethylene glycol (EG) as a polyhydric alcohol component were charged so that the molar ratio of ethylene glycol was 2.2 times that of dimethyl terephthalate, 0.05 mol% (relative to the acid component) of zinc acetate as an ester exchange catalyst and 0.225 mol% (relative to the acid component) of antimony trioxide as a polycondensation catalyst were added, and an ester exchange reaction was carried out while distilling off the produced methanol outside the system. Thereafter, a polycondensation reaction was carried out under reduced pressure conditions of 280°C and 26.7 Pa to obtain polyester 1 with an intrinsic viscosity of 0.75 dl / g. The composition is shown in Table 1.

[0072] [Synthesis Examples 2 to 5] Polyesters 2 to 4 shown in Table 1 were obtained by the same method as in Synthesis Example 1. When producing polyester 2, SiO2 (Silysia 266 manufactured by Fuji Silysia Corporation; average particle size 1.5 μm) was added as a lubricant at a ratio of 7200 ppm to the polyester. In the table, NPG stands for neopentyl glycol, and CHDM stands for 1,4-cyclohexanedimethanol. The intrinsic viscosities of the polyesters were 2:0.75 dl / g, 3:0.75 dl / g, 4:0.75 dl / g, and 5:0.75 dl / g, respectively. Each polyester was appropriately cut into chips. The composition of each polyester is shown in Table 1.

[0073] [Table 1]

[0074] [Example 1] The above-mentioned polyester 1, polyester 2, and polyester 3 were mixed in a mass ratio of 80:5:15 and fed into an extruder. The mixed resin was then melted at 280°C, extruded from a T-die, and rapidly cooled by being wound around a rotating metal roll cooled to a surface temperature of 30°C to obtain an unstretched film having a thickness of 144 μm. The Tg of the unstretched film was 72°C. The unstretched film was introduced into a tenter, and while both ends of the film were held by clips, the film was preheated until the film temperature reached 82°C (Tg+10°C), and then stretched 4.8 times in the transverse direction at a film temperature of 82°C (Tg+10°C). At this time, the stretching strain rate in the first half of the stretching (up to a stretch ratio of 2.2 times) was 12.5% / sec, and the stretching strain rate in the second half of the stretching was 37.3% / sec. The overall stretching strain rate was 23% / sec, and the stretching speed ratio was 3.0. After stretching, the film was heated at 85°C in the tenter while the film width was kept constant. Both edges of the stretched film were cut and removed to continuously produce a uniaxially stretched film of about 30 μm over a predetermined length, thereby obtaining a film roll made of a heat-shrinkable polyester film. The properties of the obtained film were evaluated by the above-mentioned method. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0075] [Example 2] The conditions of Example 1 were changed such that the transverse stretching ratio was 5.3 times, the film temperature during preheating and stretching was 83° C., and the resin extrusion amount was adjusted so that the film thickness after stretching was about 30 μm. The stretching strain rate in the first half of the stretching (up to a stretch ratio of 2.3 times) was 14.3% / sec, and the stretching strain rate in the second half of the stretching was 40.4% / sec. The overall stretching strain rate was 26% / sec, and the stretching speed ratio was 2.8. Other than the above, the same as in Example 1. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0076] [Example 3] The conditions of Example 1 were changed to 5.8 times the transverse stretching ratio, and the film temperature during preheating and stretching was changed to 87° C., and the resin extrusion amount was adjusted so that the film thickness after stretching was about 30 μm. The stretching strain rate in the first half of the stretching (up to a stretch ratio of 2.4 times) was 16.0% / sec, and the stretching strain rate in the second half of the stretching was 43.9% / sec. The overall stretching strain rate was 29% / sec, and the stretching speed ratio was 2.7. Other than the above, the same as in Example 1. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0077] [Example 4] The same procedure as in Example 1 was followed except that the above polyester 1, polyester 2, and polyester 3 were mixed in a mass ratio of 70:5:25 and fed into an extruder, and the film temperature during preheating and stretching was 76° C. At this time, the Tg of the unstretched film was 68° C. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0078] [Example 5] The conditions of Example 4 were changed such that the transverse stretching ratio was 5.3 times, the film temperature during preheating and stretching was 77° C., and the resin extrusion amount was adjusted so that the film thickness after stretching was about 30 μm. The stretching strain rate in the first half of the stretching (up to a stretch ratio of 2.3 times) was 14.3% / sec, and the stretching strain rate in the second half of the stretching was 40.4% / sec. The overall stretching strain rate was 26% / sec, and the stretching speed ratio was 2.8. Other than the above, the same as in Example 4. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0079] [Example 6] The conditions of Example 4 were changed such that the transverse stretching ratio was 5.8 times, the film temperature during preheating and stretching was 81° C., and the resin extrusion amount was adjusted so that the film thickness after stretching was about 30 μm. The stretching strain rate in the first half of the stretching (up to a stretch ratio of 2.4 times) was 16.0% / sec, and the stretching strain rate in the second half of the stretching was 43.9% / sec. The overall stretching strain rate was 29% / sec, and the stretching speed ratio was 2.7. Other than the above, the same as in Example 4. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0080] [Example 7] The same procedure was followed as in Example 2, except that the above polyester 1, polyester 2, and polyester 3 were mixed in a mass ratio of 58:5:37 and fed into an extruder, and the film temperature during preheating and stretching was 75° C. At this time, the Tg of the unstretched film was 62° C. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0081] [Example 8] The conditions of Example 7 were changed such that the transverse stretching ratio was 5.8 times, the film temperature during preheating and stretching was 77° C., and the resin extrusion amount was adjusted so that the film thickness after stretching was about 30 μm. The stretching strain rate in the first half of the stretching (up to a stretch ratio of 2.4 times) was 16.0% / sec, and the stretching strain rate in the second half of the stretching was 43.9% / sec. The overall stretching strain rate was 29% / sec, and the stretching speed ratio was 2.7. Other than the above, the same as in Example 7. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0082] [Example 9] The conditions of Example 7 were changed such that the transverse stretching ratio was 4.8 times, the film temperature during preheating and stretching was 77° C., and the resin extrusion amount was adjusted so that the film thickness after stretching was about 30 μm. The stretching strain rate in the first half of the stretching (up to a stretch ratio of 2.2 times) was 12.0% / sec, and the stretching strain rate in the second half of the stretching was 39.5% / sec. The overall stretching strain rate was 23% / sec, and the stretching speed ratio was 3.3. Other than the above, the same as in Example 7. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0083] [Example 10] The stretching strain rate in the first half of the stretching (up to a stretch ratio of 2.2 times) was 11.5% / sec, and the stretching strain rate in the second half of the stretching was 42.3% / sec. The overall stretching strain rate was 23% / sec, and the stretching speed ratio was 3.7, but other than that, the same as in Example 9. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0084] [Comparative Example 1] The same procedure as in Example 1 was followed except that the above polyester 1, polyester 2, and polyester 3 were mixed in a mass ratio of 87:5:8 and fed into an extruder, and the film temperature during preheating and stretching was 84° C. At this time, the Tg of the unstretched film was 73° C. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0085] [Comparative Example 2] The same procedure as in Example 3 was followed except that the above polyester 1, polyester 2, and polyester 3 were mixed in a mass ratio of 87:5:8 and fed into an extruder, and the film temperature during preheating and stretching was 84° C. At this time, the Tg of the unstretched film was 73° C. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0086] [Comparative Example 3] The same procedure as in Example 3 was followed except that the above polyester 1, polyester 2, and polyester 3 were mixed in a mass ratio of 45:5:50 and fed into an extruder, and the film temperature during preheating and stretching was 72° C. At this time, the Tg of the unstretched film was 60° C. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0087] [Comparative Example 4] The stretching strain rate in the first half of the stretching (up to a stretch ratio of 2.3 times) was 30.0% / sec, the stretching strain rate in the second half of the stretching was 24.6% / sec, the overall stretching strain rate was 29% / sec, and the stretching speed ratio was 0.8, all of which were the same as in Example 7. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0088] [Comparative Example 5] The same procedure as in Example 1 was followed except that the above polyester 1, polyester 2, and polyester 4 were mixed in a mass ratio of 45:5:50 and fed into an extruder, and the film temperature during preheating and stretching was 76° C. At this time, the Tg of the unstretched film was 75° C. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0089] . [Comparative Example 6] The same procedure as in Example 1 was followed except that the above polyester 1, polyester 2, and polyester 5 were mixed in a mass ratio of 45:5:60 and fed into an extruder, and the film temperature during preheating and stretching was 76° C. At this time, the Tg of the unstretched film was 73° C. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0090] [Comparative Example 7] The above polyester 1, polyester 2, polyester 3, and polyester 4 were mixed in a weight ratio of 4:5:25:66 and fed into an extruder, and an unstretched sheet having a thickness of 153 μm was obtained in the same manner as in Example 1. The Tg of the unstretched film was 68 ° C. The unstretched film was introduced into a tenter, and while both ends of the film were held by clips, the film was preheated until the film temperature reached 73 ° C (Tg + 5 ° C), and then stretched 5.1 times in the transverse direction at a film temperature of 73 ° C (Tg + 5 ° C). At this time, the stretching strain rate in the first half of the stretching (up to a stretch ratio of 2.2 times) was 23.0% / sec, and the stretching strain rate in the second half of the stretching was 23.0% / sec. The overall stretching strain rate was 23% / sec, and the stretching speed ratio was 1.0. After stretching, the film was heated at a film temperature of 74 ° C. while relaxing the film by 5% in the transverse direction inside the tenter. After the tenter process, both edges of the film were cut and removed to produce a uniaxially stretched film of about 30 μm continuously over a predetermined length, thereby obtaining a film roll made of a heat-shrinkable polyester film. The production conditions are shown in Table 2, and the evaluation results are shown in Table 3.

[0091] [Table 2]

[0092] [Table 3]

[0093] As a result of the evaluation, the films of Examples 1 to 10 had sufficient shrinkability and low shrinkage stress, and therefore the shrinkage finish was good. In addition, because the film plane orientation was high, the initial breakage occurrence rate after aging was good at 0%, and because the 70°C shrinkage rate hardly decreased even after aging, the shrinkage finish after aging was also good.

[0094] The film of Comparative Example 1 had a low diethylene glycol ratio, and therefore had low amorphousness, could not obtain a sufficient shrinkage rate, and had a large change in shrinkage rate at 70° C. over time. The shrinkage finish was poor, with shrinkage distortion and insufficient shrinkage both before and after aging.

[0095] The film of Comparative Example 2 had a low diethylene glycol ratio, so it had low amorphousness, could not obtain a sufficient shrinkage rate, had high shrinkage stress, and had a large change in shrinkage rate over time.The plane orientation coefficient was high, so the solvent adhesive strength was low, and the shrinkage finish was poor, with shrinkage distortion and insufficient shrinkage both before and after aging, and peeling of the sealed portion also occurred.

[0096] The films of Comparative Examples 3 and 4 had sufficient shrinkage and low shrinkage stress, but because the degree of planar orientation was small, the longitudinal elongation after aging was low and the films were prone to problems during post-processing.

[0097] The film of Comparative Example 5 has high amorphousness due to the neopentyl glycol component, sufficient shrinkage, high degree of planar orientation, and low shrinkage stress, but the diethylene glycol ratio is low, so the 70°C shrinkage rate changes greatly over time and the natural shrinkage rate is large. The shrinkage finish was good before aging, but after aging, shrinkage distortion and wrinkles occurred due to the decrease in the 70°C shrinkage rate, making it poor.

[0098] The film of Comparative Example 6 is highly amorphous due to the cyclohexanedimethanol component, has sufficient shrinkage, has high planar orientation, and has low shrinkage stress, but has a large change in 70°C shrinkage over time and a large natural shrinkage due to the low diethylene glycol ratio. The shrinkage finish was good before aging, but after aging, shrinkage distortion and wrinkles occurred due to the decrease in 70°C shrinkage, making it poor.

[0099] The film of Comparative Example 7 had sufficient shrinkage and low shrinkage stress, but because the degree of planar orientation was small, the film had low longitudinal elongation after aging and was prone to problems during post-processing. [Industrial Applicability]

[0100] The heat-shrinkable polyester film of the present invention has sufficient shrinkability as described above, and has a low shrinkage stress, so that the shrinkage finish is good, and the shrinkage finish after aging is also good because the shrinkage rate change over time is small. Furthermore, because the degree of planar orientation is high, the initial break rate over time is low, and even after long-term storage, the film is unlikely to cause breakage problems during post-processing such as printing. As described above, the film has excellent shrinkage finish and processability immediately after production and after long-term storage, and can be suitably used for labels for beverage bottles, banding packaging for lunch boxes, and the like.

Claims

1. A heat-shrinkable polyester film, which satisfies the following requirements (1) to (5) and is characterized in that the main shrinkage direction is the width direction: (1) The shrinkage rate (hot water shrinkage rate) when the film is immersed in 98°C hot water for 10 seconds is 40% or more in the main shrinkage direction of the film. (2) The plane orientation coefficient of the film is 0.035 or more and 0.070 or less. (3) The main component is ethylene terephthalate, the amount of diethylene glycol (DEG) component is 6 mol% to 25 mol% of 100 mol% of polyhydric alcohol components in the total polyester resin constituting the film, and the content of polyhydric alcohol components other than ethylene glycol and diethylene glycol is 0 mol% to 15 mol% of 100 mol% of polyhydric alcohol components. (4) The maximum shrinkage stress in the main shrinkage direction of the film measured in hot air at 90°C is 2 MPa or more and 17 MPa or less. (5) After the film is left in an atmosphere having an atmospheric temperature of 40° C. and a relative humidity of 85% for 28 days, the tensile elongation at break in the direction perpendicular to the main shrinkage direction is 20% or more.

2. 2. The heat-shrinkable polyester film according to claim 1, wherein the tensile elongation at break in a direction perpendicular to the main shrinkage direction is 100% or more after the film is aged for 28 days in an atmosphere having an atmospheric temperature of 40° C. and a relative humidity of 85%.

3. 3. The heat-shrinkable polyester film according to claim 1, wherein the difference between the shrinkage rate in the main shrinkage direction when the film is immersed in hot water at 70°C for 10 seconds after aging for 28 days in an atmosphere having an atmospheric temperature of 30°C and a relative humidity of 85% and the shrinkage rate before aging is less than 5%.

4. 4. The heat-shrinkable polyester film according to claim 1, wherein the solvent adhesion strength is 4 N / 15 mm width or more and 15 N / 15 mm width or less.

5. 5. The heat-shrinkable polyester film according to any one of claims 1 to 4, characterized in that the natural shrinkage rate in the main shrinkage direction after the film is aged for 28 days in an atmosphere having an atmospheric temperature of 40°C and a relative humidity of 85% is less than 1.0%.

6. 6. The heat-shrinkable polyester film according to claim 1, wherein the intrinsic viscosity of the film is 0.60 dl / g or more and 0.75 dl / g or less.

7. The heat-shrinkable polyester film according to any one of claims 1 to 6, which is a uniaxially stretched film.

8. A label obtained from the heat-shrinkable polyester film according to any one of claims 1 to 7.

9. A package formed by covering at least a part of the outer periphery of an object to be packaged with the label according to claim 8 and then heat-shrinking the label.

Citation Information

Patent Citations

  • Polyester film

    JP1998279707A

  • Heat-shrinkabile polyester film

    JP2004142126A

  • Film for heat-shrinkable packaging

    JP2004345298A

  • Thermally shrinkable polyester-based film and label and method for producing the same

    JP2007056156A

  • Raw copolyester material for amorphous film, heat-shrinkable polyester-based film, heat-shrinkable label, and package

    WO2018147249A1