All solid state battery
By using an interface layer with small solid electrolyte particles in the separator layer, the battery resistance is suppressed, maintaining contact and capacity despite high volume change rates in active materials, addressing the trade-off between confining pressure and energy density in all-solid-state batteries.
Patent Information
- Application Number
- JP2022071638
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-04-25
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2042-04-25
AI Technical Summary
In all-solid-state batteries, maintaining contact between the active material and the solid electrolyte is crucial for reducing battery resistance, but increasing confining pressure to achieve this leads to a larger restraining member, decreasing energy density, while low confining pressure results in peeling and increased resistance due to volume changes during charging and discharging, especially with active materials like Si and S.
Incorporating an interface layer with small-sized solid electrolyte particles in the separator layer to maintain contact with electrodes containing active materials with high volume change rates, such as Si and S, thereby suppressing peeling and maintaining contact area even at low confining pressures.
This approach effectively suppresses the increase in battery resistance and maintains contact between the electrode and separator layer, enhancing the battery's performance and capacity even when using active materials with high volume change rates.
Smart Images

Figure 0007582245000002 
Figure 0007582245000003 
Figure 0007582245000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to all-solid-state batteries. [Background technology]
[0002] JP 2018-106984 A (Patent Document 1) discloses an all-solid-state lithium ion battery including a laminate of a positive electrode, a negative electrode, and a solid electrolyte layer (separator layer), and a restraining member that applies a restraining pressure to the laminate, in which the negative electrode has a solid electrolyte and a plurality of Si simplex particles as a negative electrode active material, the average particle size of the plurality of Si simplex particles is within a specific range, and the restraining pressure applied to the laminate by the restraining member is 0.1 MPa or more and 45 MPa or less. It is also disclosed that in this battery, since the restraining pressure by the restraining member is low, the restraining member can be made smaller, and the energy density of the entire battery can be increased. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-106984 A Summary of the Invention [Problem to be solved by the invention]
[0004] In all-solid-state batteries such as all-solid-state lithium ion batteries, a restraining pressure may be applied to a laminate of a positive electrode, a negative electrode, and a separator layer, which maintains contact between the active material and the solid electrolyte and can improve battery performance by reducing battery resistance.
[0005] However, if the restraining pressure is increased to maintain contact between the active material and the solid electrolyte in an all-solid-state battery, the restraining member becomes large, and the energy density of the entire battery decreases. On the other hand, if the restraining pressure is low, a large-scale restraining member is not required, and the energy density of the entire battery can be increased. Therefore, it is desirable to reduce the restraining pressure as much as possible and to make the restraining member small.
[0006] However, when the confinement pressure is relatively low (for example, when the confinement pressure is 1 MPa or less), when the active material shrinks due to charging and discharging, peeling easily occurs between the separator layer (solid electrolyte layer) and the active material of the electrode (positive or negative electrode). Therefore, repeated charging and discharging may reduce the contact area between the separator layer and the electrode, gradually increasing the battery resistance. It is considered that the battery resistance is likely to increase due to charging and discharging, especially when the volume change rate of the active material due to charging and discharging is large.
[0007] An object of the present disclosure is to provide an all-solid-state battery capable of suppressing an increase in battery resistance even when a confining pressure is relatively low. [Means for solving the problem]
[0008] [1] An all-solid-state battery comprising a positive electrode, a negative electrode, and a separator layer, the positive electrode or the negative electrode contains an active material whose volume change rate due to charging and discharging is 10% or more, the separator layer includes solid electrolyte particles and has an interface layer in contact with the positive electrode or the negative electrode including the active material, The D50 of the solid electrolyte particles contained in the interface layer (D50 SE ) is 1 / 7 or less of the ten-point average roughness (Rzjis) of the positive electrode or the negative electrode containing the active material (i.e., "Rzjis / D50 SE ≧7"), all-solid-state batteries.
[0009] According to the all-solid-state battery described in [1] above, an increase in battery resistance can be suppressed even when the confining pressure is relatively low.
[0010] In the electrode [1] above, "Rzjis / D50 SE An interface layer containing solid electrolyte particles having a relatively small particle size that satisfies ".gtoreq.7" is present at the interface between the separator layer and an electrode (at least one of the positive and negative electrodes) containing an active material with a volume change rate of 10% or more due to charging and discharging. Therefore, the small particle size solid electrolyte particles contained in the interface layer of the separator layer penetrate into the gaps at the interface of the electrode (active material layer), thereby increasing the contact area at the interface between the electrode and the separator layer and improving the adhesion. As a result, even when the restraining pressure is relatively low, peeling between the electrode and the separator layer due to charging and discharging is suppressed, so that contact (interface path) between the electrode and the separator layer is maintained, and it is considered that an increase in resistance in the all-solid-state battery is suppressed.
[0011] [2] The all-solid-state battery according to [1], wherein the negative electrode contains, as the active material, a negative electrode active material containing Si.
[0012] A negative electrode active material containing Si (Si simple substance, Si alloy, etc.) may be used as the negative electrode active material. When the negative electrode active material contains Si, which has a higher capacity than carbon-based materials, the capacity and capacity density of the all-solid-state battery can be increased. However, since the negative electrode active material containing Si has a relatively large volume change rate due to charging and discharging, when the negative electrode active material contains Si, peeling is likely to occur at the interface between the negative electrode (negative electrode active material layer) and the separator layer. For this reason, when the negative electrode active material contains Si, it is generally necessary to increase the restraining pressure of the battery. However, in the all-solid-state battery of this embodiment, for the same reason as in [1] above, even when the restraining pressure is relatively low, the contact area between the negative electrode and the separator layer is easily maintained. Therefore, it is considered that an increase in resistance in the all-solid-state battery can be suppressed even when the negative electrode active material contains Si.
[0013] [3] The all-solid-state battery according to [1] or [2], wherein the positive electrode contains a positive electrode active material containing S as the active material.
[0014] A positive electrode active material containing S may be used as the positive electrode active material. However, since the positive electrode active material containing S has a relatively large volume change rate due to charging and discharging, when the positive electrode active material contains S, peeling is likely to occur at the interface between the positive electrode (positive electrode active material layer) and the separator layer. For this reason, when the positive electrode active material contains S, it is generally necessary to increase the restraining pressure of the battery. However, in the all-solid-state battery of this embodiment, for the same reason as in [1] above, even when the restraining pressure is relatively low, it is easy to maintain the contact area between the positive electrode and the separator layer. Therefore, even when the positive electrode active material contains S, it is considered that an increase in resistance in the all-solid-state battery can be suppressed. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a conceptual diagram illustrating an example of an all-solid-state battery according to an embodiment of the present invention. [Diagram 2] 1 is a graph showing the relationship between battery resistance and Rzjis / ΦSE in Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment of the present disclosure (hereinafter may be abbreviated as "the present embodiment") and an example of the present disclosure (hereinafter may be abbreviated as "the present embodiment") will be described. However, the present embodiment and the example do not limit the technical scope of the present disclosure.
[0017] In this specification, elements expressed in the singular form include the plural form unless otherwise specified. For example, a "particle" can mean not only "one particle" but also "an aggregate of particles (powder, powder, particle group)."
[0018] When a compound is expressed by a stoichiometric composition formula (e.g., "LiCoO2", etc.), the stoichiometric composition formula is merely a representative example of the compound. The compound may have a non-stoichiometric composition. For example, when lithium cobalt oxide is expressed as "LiCoO2", unless otherwise specified, the lithium cobalt oxide is not limited to the composition ratio of "Li / Co / O=1 / 1 / 2" and may contain Li, Co, and O in any composition ratio. Furthermore, doping, substitution, etc. with trace elements may be allowed.
[0019] <All-solid-state battery> Fig. 1 is a conceptual diagram showing an example of an all-solid-state battery in this embodiment. The all-solid-state battery 100 shown in Fig. 1 includes an electricity storage element 5. The electricity storage element 5 includes a positive electrode 1, a negative electrode 2, and a separator layer 3. The positive electrode 1 includes a positive electrode current collector 11 and a positive electrode active material layer 12. The negative electrode 2 includes a negative electrode current collector 21 and a negative electrode active material layer 22.
[0020] The positive electrode 1 (positive electrode active material layer 12) or the negative electrode 2 (negative electrode active material layer 22) contains an active material having a volume change rate due to charge and discharge of 10% or more (or 50% or more). In this embodiment, it is sufficient that either the positive electrode 1 (positive electrode active material layer 12) or the negative electrode 2 (negative electrode active material layer 22) contains an active material having a volume change rate due to charge and discharge of 10% or more, and further, both the positive electrode 1 (positive electrode active material layer 12) or the negative electrode 2 (negative electrode active material layer 22) may contain an active material having a volume change rate due to charge and discharge of 10% or more.
[0021] The separator layer 3 includes solid electrolyte particles, and has an interface layer in contact with the positive electrode 1 or the negative electrode 2 including the above-mentioned active material (an active material having a volume change rate of 10% or more upon charging and discharging).
[0022] In one example of the all-solid-state battery according to the present embodiment shown in FIG. 1, the negative electrode 2 (negative electrode active material layer) contains an active material having a volume change rate of 10% or more due to charge and discharge, and the separator layer 3 is composed of a main layer 31 and an interface layer 32 in contact with the negative electrode 2.
[0023] 1, the separator layer 3 may have an interface layer in contact with the positive electrode 1. The separator layer 3 may have both an interface layer in contact with the positive electrode 1 and an interface layer in contact with the negative electrode 2.
[0024] The D50 of the solid electrolyte particles contained in the interface layer 32 of the separator layer 3 (D50 SE ) is 1 / 7 or less of the ten-point average roughness of the positive or negative electrode containing the active material. SE ≧7".
[0025] The ten-point average roughness of the positive electrode or negative electrode can be measured by observing a cross section (a cross section parallel to the lamination direction of the positive electrode 1 or negative electrode 2, and the separator layer 3) of the interface between the positive electrode 1 (positive electrode active material layer 12) or the negative electrode 2 (negative electrode active material layer 22) and the separator layer 3 with an SEM, reading the roughness of the positive electrode or negative electrode interface (the interface between the positive electrode or negative electrode and the separator layer) from the SEM image, and measuring the ten-point average roughness (Rzjis) standardized in JIS B 0601:2001.
[0026] The all-solid-state battery 100 may include, for example, an exterior body (not shown) that houses the electricity storage element 5. The exterior body may be, for example, a pouch made of a metal foil laminate film.
[0027] 《Positive electrode》 The positive electrode 1 includes a positive electrode current collector 11 and a positive electrode active material layer 12. The positive electrode 1 is in a layered form.
[0028] The positive electrode current collector 11 may be, for example, an Al foil. The positive electrode current collector 11 may have a thickness of, for example, 5 to 50 μm. For example, the positive electrode active material layer 12 may be formed by applying a positive electrode mixture to the surface of the positive electrode current collector 11.
[0029] The positive electrode active material layer 12 is in close contact with the separator layer 3. The positive electrode active material layer 12 may have a thickness of, for example, 10 to 200 μm.
[0030] The positive electrode active material layer 12 may contain positive electrode active material particles and solid electrolyte particles.
[0031] Examples of the components of the positive electrode active material particles include LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li(NiCoMn)O2, Li(NiCoAl)O2, LiFePO4, Li2S, and P2S. 5、 For example, the "(NiCoMn)" in "Li(NiCoMn)O2" indicates that the sum of the composition ratios in the parentheses is 1. As long as the sum is 1, the amount of each component is arbitrary. Li(NiCoMn)O2 is, for example, Li(Ni 1 / 3 Co 1 / 3 Mn 1 / 3 )O2, Li(Ni 0.5 Co 0.2 Mn 0.3 )O2, Li(Ni 0.8 Co 0.1 Mn 0.1 ) O2, etc.
[0032] The positive electrode active material particles may contain an active material (positive electrode active material) whose volume change rate due to charging and discharging of the all-solid-state battery is 10% or more. The positive electrode active material particles may contain an active material (positive electrode active material) whose volume change rate due to charging and discharging of the all-solid-state battery is 30% or more or 50% or more.
[0033] When a positive electrode active material having a relatively large volume change rate due to charging and discharging is used, peeling is likely to occur at the interface between the positive electrode (positive electrode active material layer) and the separator layer. Therefore, when the positive electrode active material particles contain an active material having a volume change rate of 10% or more due to charging and discharging of the all-solid-state battery, in order to suppress such peeling, it is preferable that the separator layer 3 has an interface layer in contact with the positive electrode 1 (positive electrode active material layer 12).
[0034] The volume change rate of the active material of an all-solid-state battery due to charging and discharging is the rate of change in the volume of the active material when it is most expanded relative to the volume of the active material when it is most contracted, for an active material that expands and contracts due to charging and discharging. That is, the volume change rate of the active material of an all-solid-state battery due to charging and discharging is expressed by the following formula. "Volume change rate of active material" (%) = [("Volume of active material when it expands the most" - "Volume of active material when it contracts the most") / "Volume of active material when it contracts the most"] x 100
[0035] The volume change rate of the above active materials can be measured by a known method, and the volume change rate due to charging and discharging is known for each of the common active materials. The volume change rate (expansion rate) of the active materials due to charging and discharging can be measured, for example, by calculating the lattice volume before and after charging using in-situ XRD. The volume change rate (expansion rate) of each active material measured by such a method is as follows. Si (single unit): 300% Carbon-based negative electrode active material (graphite): 10% Li2S: 50~100%
[0036] The active material (positive electrode active material) having a volume change rate of 10% or more (or 50% or more) due to charging and discharging of the all-solid-state battery is not particularly limited, but may be, for example, a positive electrode active material containing S (elemental sulfur). Examples of the positive electrode active material containing S include Li2S, P2S 5、 Examples include SiS2.
[0037] The positive electrode active material particles may be secondary particles (aggregates of primary particles). The secondary particles of the positive electrode active material particles may have a D50 of, for example, 1 to 50 μm, may have a D50 of 1 to 20 μm, or may have a D50 of 5 to 15 μm. The primary particles of the positive electrode active material particles may have a maximum Feret diameter of, for example, 0.1 to 3 μm.
[0038] In this specification, "D50" refers to the particle size at which the cumulative frequency from the smaller particle size side reaches 50% in the volume-based particle size distribution. D50 can be measured by a laser diffraction method.
[0039] The surface of the positive electrode active material particles may be covered with, for example, a coating film for suppressing reaction with the solid electrolyte particles and the like.
[0040] The components of the solid electrolyte particles used in the positive electrode active material layer 12 may be the same as or different from the components of the solid electrolyte particles used in the separator layer 3 described below.
[0041] The positive electrode active material layer 12 may further include, for example, a conductive material. The conductive material can form an electronic conduction path in the positive electrode active material layer. The conductive material can include any component. The conductive material may include, for example, at least one selected from the group consisting of carbon black, vapor grown carbon fiber (VGCF), carbon nanotubes (CNT), and graphene flakes. The blending amount of the conductive material may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the positive electrode active material particles.
[0042] The positive electrode active material layer 12 may further include, for example, a binder. The binder may include any component. The binder may include, for example, at least one selected from the group consisting of polyvinylidene fluoride (PVdF), vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), styrene butadiene rubber (SBR), and polytetrafluoroethylene (PTFE). The amount of the binder may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the positive electrode active material particles.
[0043] The positive electrode active material particles may be subjected to a heat treatment (baking). The heat treatment temperature may be, for example, 150 to 300° C. The heat treatment time may be, for example, 1 to 10 hours. For example, the heat treatment may be performed in air, or in an inert atmosphere.
[0044] 《Negative electrode》 The negative electrode 2 may include a negative electrode current collector 21 and a negative electrode active material layer 22. The negative electrode 2 is layered.
[0045] The negative electrode current collector 21 may include, for example, a Cu foil, a Ni foil, etc. The negative electrode current collector may have a thickness of, for example, 5 to 50 μm. For example, a negative electrode active material layer may be formed by applying a negative electrode mixture onto the surface of the negative electrode current collector.
[0046] The negative electrode active material layer 22 is in close contact with the separator layer 3. The negative electrode active material layer 22 may have a thickness of, for example, 10 to 200 μm.
[0047] The negative electrode active material layer 22 may contain negative electrode active material particles and solid electrolyte particles.
[0048] Examples of the components of the negative electrode active material particles include carbon materials such as graphite, Si, SiO x (0 < x < 2), Li4Ti5O 12 and the like.
[0049] The negative electrode active material particles may contain an active material (negative electrode active material) having a volume change rate of 10% or more due to charge and discharge of the all-solid-state battery. Note that the negative electrode active material particles may contain an active material (negative electrode active material) having a volume change rate of 100% or more or 200% or more due to charge and discharge of the all-solid-state battery.
[0050] When a negative electrode active material having a relatively large volume change rate due to charge and discharge is used, peeling at the interface between the negative electrode (negative electrode active material layer) and the separator layer is likely to occur. Therefore, when the negative electrode active material particles contain an active material having a volume change rate of 10% or more due to charge and discharge of the all-solid-state battery, in order to suppress such peeling, it is preferable that the separator layer 3 has an interface layer that contacts the negative electrode 2 (negative electrode active material layer 22).
[0051] The active material (negative electrode active material) having a volume change rate of 10% or more due to charge and discharge of the all-solid-state battery is not particularly limited, and examples thereof include a negative electrode active material containing Si (silicon element). Examples of the negative electrode active material containing Si include Si (single substance) or Si alloy. Examples of the Si alloy include SiO x (0 < x < 2). Note that since the negative electrode active material containing Si has a higher capacity than the carbon-based negative electrode active material, the capacity of the all-solid-state battery can be improved by the negative electrode active material particles containing Si. However, carbon materials such as graphite can also be included in the active material (negative electrode active material) having a volume change rate of 10% or more due to charge and discharge of the all-solid-state battery.
[0052] The negative electrode active material particles may be secondary particles (aggregates of primary particles). The negative electrode active material particles (secondary particles) may have a D50 of, for example, 1 to 50 μm, may have a D50 of 1 to 20 μm, or may have a D50 of 5 to 15 μm. The primary particles may have a maximum Feret diameter of, for example, 0.1 to 3 μm.
[0053] The surface of the negative electrode active material particles may be covered with, for example, a coating film for suppressing reaction with the solid electrolyte particles and the like.
[0054] The components of the solid electrolyte particles used in the negative electrode active material layer 22 may be the same as or different from the components of the solid electrolyte particles used in the separator layer 3 described below.
[0055] The negative electrode active material layer 22 may further include, for example, a conductive material and a binder. As the conductive material and the binder, for example, the same conductive material and binder as those in the positive electrode active material layer can be used.
[0056] <Separator layer> The separator layer 3 is interposed between the positive electrode 1 and the negative electrode 2 . The separator layer 3 contains solid electrolyte particles. The solid electrolyte (component of the solid electrolyte particles) between the separator layer 3 and the positive electrode composite material may be the same or different. The solid electrolyte between the separator layer 3 and the negative electrode composite material may be the same or different.
[0057] The separator layer 3 may further contain a binder. The blending amount of the binder may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the solid electrolyte particles.
[0058] The separator layer 3 has an interface layer 32 that contacts an electrode (positive electrode or negative electrode) containing an active material whose volume change rate due to charging and discharging is 10% or more. In the all-solid-state battery shown in FIG. 1, the interface layer 32 is provided only on the side in contact with the negative electrode 2 (negative electrode active material layer 22), but the present invention is not limited to this. The interface layer may be provided only on the side in contact with the positive electrode 1 (positive electrode active material layer 12), or the interface layer may be provided on both the side in contact with the positive electrode 1 and the side in contact with the negative electrode 2.
[0059] The separator layer 3 may be composed of a main layer 31 and an interface layer 32, for example, as shown in FIG. 1. In this case, each of the main layer 31 and the interface layer 32 contains solid electrolyte particles. Each of the main layer 31 and the interface layer 32 may further contain a binder. The amount of the binder in the main layer 31 may be, for example, 0.1 to 10 parts by mass per 100 parts by mass of the solid electrolyte particles. The amount of the binder in the interface layer 32 may be, for example, 1 to 10 parts by mass per 100 parts by mass of the solid electrolyte particles.
[0060] The composition of the solid electrolyte particles in the interface layer 32 may be the same as or different from the composition of the solid electrolyte particles in the main layer 31, but it is preferable that they are the same composition.
[0061] The components of the solid electrolyte particles are not particularly limited, and may be any of a sulfide solid electrolyte, an oxide solid electrolyte, a boron hydrogen solid electrolyte, and the like.
[0062] The sulfide solid electrolyte may include S and P. The sulfide solid electrolyte may further include Li. The sulfide solid electrolyte may further include, for example, O, Si, etc. The sulfide solid electrolyte may further include, for example, a halogen, such as iodine (I) or bromine (Br).
[0063] Examples of sulfide solid electrolytes include LiI-LiBr-Li3PS4, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2O-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-P2S5, Li3PS4, LiCl-LiBr-Li3PS 4、 LiCl-LiBr-Li2S-P2S5, LiCl-LiBr-Li2S-SiS2, etc. can be used.
[0064] For example, "LiI-LiBr-Li3PS4" refers to a sulfide solid electrolyte produced by mixing LiI, LiBr, and Li3PS4 in any molar ratio. For example, the sulfide solid electrolyte may be produced by a mechanochemical method. "Li2S-P2S5" includes Li3PS4. Li3PS4 can be produced, for example, by mixing Li2S and P2S5 in a molar ratio of Li2S / P2S5=75 / 25.
[0065] The solid electrolyte may be any of an argyrodite type, a perovskite type, a glass ceramic type, and the like.
[0066] The average particle diameter (D50) of the solid electrolyte particles in the interface layer 32 may be the same as or different from the average particle diameter (D50) of the solid electrolyte particles in the main layer 31. For example, the average particle diameter (D50) of the solid electrolyte particles in the interface layer 32 may be smaller than the average particle diameter (D50) of the solid electrolyte particles in the main layer 31.
[0067] When the components of the solid electrolyte particles in interface layer 32 and the components of the solid electrolyte particles in main layer 31 are the same, the average particle size of the solid electrolyte particles in interface layer 32 and the average particle size of the solid electrolyte particles in main layer 31 are the same, and other components such as the binder are also the same, it is understood that interface layer 32 and main layer 31 cannot be distinguished, but separator layer 3 is composed of only the interface layer. In this embodiment, separator layer 3 also includes such a mode.
[0068] The D50 of the solid electrolyte particles used to form interface layer 32 is preferably 0.01 to 1.0 μm, more preferably 0.02 to 0.5 μm, and even more preferably 0.05 to 0.2 μm. The particle size (individual particle size) of each of all the solid electrolyte particles used to form interface layer 32 is preferably 0.5 μm or less, and more preferably 0.3 μm or less.
[0069] The solid electrolyte particles used to form interface layer 32 may be, for example, fine particles obtained by atomizing a larger solid electrolyte, such as by mechanical grinding.
[0070] The ratio of D50 of the solid electrolyte particles used to form interface layer 32 to D50 of the solid electrolyte particles used to form main layer 31 is preferably 0.5 or less, more preferably 0.01 to 0.3, and more preferably 0.02 to 0.2.
[0071] The content of solid electrolyte particles in the interface layer 32 may be, for example, 70 to 100 mass %, 80 to 99.9 mass %, or 90 to 99.8 mass %. The content of solid electrolyte particles in main layer 31 may be, for example, 70 to 100 mass %, 80 to 99.5 mass %, or 90 to 99.0 mass %.
[0072] The thickness of the interface layer may be 0.5 to 100 μm, or may be 1 to 50 μm. The thickness of the interface layer can be measured by X-ray fluorescence analysis (XRF). EXAMPLES
[0073] <Example 1> (Preparation of positive electrode) The following materials were prepared: Positive electrode active material: D50 is 10 μm, specific surface area is 1 m 2 / g LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2 powder (the surface of the positive electrode active material is LiNbO3で It is covered.) Solid electrolyte (sulfide solid electrolyte): D50 is 1μm, specific surface area is 9m 2 / g of "15LiBr-10LiI-75(0.75Li2S-0.25P2S5)" glass ceramic powder Conductive material: CNF (carbon nanofiber, specific surface area: 14 m 2 / g) Binder: SBR (styrene-butadiene rubber) binder Dispersion medium: butyl acetate Positive electrode current collector: Al foil (thickness: 15 μm)
[0074] The positive electrode active material, solid electrolyte, conductive material, binder, and dispersion medium were mixed to prepare a composition for forming a positive electrode active material layer (positive electrode slurry). For 100 parts by mass of the positive electrode active material, the amount of the solid electrolyte was 50 parts by mass, the amount of the conductive material was 10 parts by mass, and the amount of the binder was 0.7 parts by mass. The amount of the binder was 100 parts by mass per 1 m of the positive electrode active material layer. 2 The solid content of the positive electrode slurry was 60 mass %.
[0075] The positive electrode slurry was thoroughly stirred by ultrasonic dispersion treatment for 1 minute using an ultrasonic dispersion device. The positive electrode slurry was then applied to the positive electrode current collector by blade coating using a commercially available applicator until the coating weight (solid content) was 15 mg / cm. 2 The coating was then dried at 100° C. for 60 minutes to form a positive electrode active material layer on the positive electrode current collector. In this manner, a positive electrode was obtained.
[0076] (Preparation of negative electrode) The following materials were prepared: Negative electrode active material: D50 is 2.9 μm, specific surface area is 4 m 2 / g Si powder Solid electrolyte: The same sulfide solid electrolyte powder as the positive electrode Conductive material: CNF (specific surface area: 14m 2 / g) Binder: SBR binder Dispersion medium: butyl acetate Negative electrode current collector: Surface roughened copper foil (thickness: 20μm)
[0077] The negative electrode active material, solid electrolyte, conductive material, binder, and dispersion medium were mixed to prepare a composition for forming a negative electrode active material layer (negative electrode slurry). For 100 parts by mass of the negative electrode active material, the amount of the solid electrolyte was 10 parts by mass, the amount of the conductive material was 10 parts by mass, and the amount of the binder was 1.4 parts by mass. The amount of the binder was 1.0 parts by mass per 1 m of the negative electrode active material layer. 2 The solid content of the negative electrode slurry was 40 mass %.
[0078] The negative electrode slurry was thoroughly stirred by ultrasonic dispersion treatment for 1 minute using an ultrasonic dispersion device. The negative electrode slurry was then applied to the negative electrode current collector by blade coating using a commercially available applicator until the coating weight (solid content) was 3 mg / cm. 2 The coating was then dried at 100° C. for 60 minutes to form a negative electrode active material layer on the negative electrode current collector. In this manner, a negative electrode was obtained.
[0079] [Preparation of separator layer for measuring negative electrode roughness] First, the average particle size (D50) is 1.1 μm and the specific surface area is 5 m 2 A first solid electrolyte layer (main layer) was fabricated using a powder of “15LiBr-10LiI-75(0.75Li2S-0.25P2S5)” glass ceramics (first sulfide solid electrolyte) with a molecular weight of 1000–15000 / g.
[0080] Specifically, the first sulfide solid electrolyte, an SBR binder, and a dispersion medium (butyl acetate) were mixed to prepare a composition for forming a first solid electrolyte layer (first solid electrolyte slurry). The amount of the SBR binder was 0.5 parts by mass per 100 parts by mass of the first sulfide solid electrolyte. The amount of the binder was 0.5 parts by mass per 1 m of the separator layer. 2 The solid content of the first solid electrolyte slurry was 50 mass %. Using the obtained first solid electrolyte slurry, a first solid electrolyte layer (main layer) was formed on a surface-roughened copper foil (substrate) in the same manner as in the preparation of the positive and negative electrodes described above. The basis weight (solid content) of the first solid electrolyte slurry was 3.0 mg / cm. 2 The thickness of the first solid electrolyte layer (main layer) was 15 μm.
[0081] Next, a ferroelectric material having an average particle diameter (D50) of 0.1 μm and a specific surface area of 30 m is applied onto the first solid electrolyte layer. 2 A second solid electrolyte layer (interface layer) was fabricated using a powder of “15LiBr-10LiI-75(0.75Li2S-0.25P2S5)” glass ceramics (second sulfide solid electrolyte) with a molecular weight of 1000–15000 / g.
[0082] Specifically, the second sulfide solid electrolyte, an SBR binder, and a dispersion medium (butyl acetate) were mixed to prepare a composition for forming a second solid electrolyte layer (second solid electrolyte slurry). The amount of the SBR binder was 3 parts by mass per 100 parts by mass of the second sulfide solid electrolyte. The amount of the binder was 10 parts by mass per 1 m of the separator layer. 2 The solid content of the first solid electrolyte slurry was 50 mass %.
[0083] Using the obtained second solid electrolyte slurry, a second solid electrolyte layer (interface layer) was formed on the first solid electrolyte layer formed on the copper foil in the same manner as in the preparation of the above-mentioned first solid electrolyte layer. The basis weight (solid content) of the second solid electrolyte slurry was 1.0 mg / cm. 2 and the thickness of the second solid electrolyte layer (interface layer) was 5 μm.
[0084] [Measurement of ten-point average roughness of negative electrode] The negative electrode prepared as described above and the separator layer for measuring roughness were stacked together and subjected to a pressure of 6 ton / cm 2The negative electrode and separator layer were then pressed for 1 minute at 100° C. The resulting assembly was cut together with the negative electrode current collector (current collector foil) to a size of 5 mm x 5 mm, and the cut cross section (cross section parallel to the lamination direction of the negative electrode and separator layer) was observed with an SEM. The roughness of the interface between the negative electrode (negative electrode active material layer) and the separator layer was read from the SEM image, and the ten-point average roughness (Rzjis) standardized in JIS B 0601:2001 was measured. The measurement results are shown in Table 1.
[0085] (Preparation of separator layer for battery production) A separator layer for producing a battery was prepared in the same manner as the separator layer for measuring roughness, except that the substrate was changed to aluminum foil.
[0086] (Battery Construction) The separator layer for battery production cut into a square shape of 5.2 cm x 5.2 cm with the aluminum foil and the negative electrode cut into the same shape were stacked together and roll-pressed with a pressure of 1 ton / cm. Next, the aluminum foil attached to the separator layer laminated on the negative electrode was peeled off, and the positive electrode cut into a square shape of 5.0 cm x 5.0 cm with the aluminum foil was stacked on the separator layer laminated on the negative electrode and roll-pressed with a pressure of 3 ton / cm. The laminated electrode body thus obtained was sealed with an exterior body made of an aluminum laminate film to which a positive electrode terminal and a negative electrode terminal were previously attached. In this way, the all-solid-state battery (all-solid-state lithium-ion secondary battery) of Example 1 was produced. As shown in FIG. 1, the positive electrode 1 is laminated on the surface of the separator layer 3 facing the main layer 31 (first solid electrolyte layer) so that the positive electrode active material layer 12 is in contact with the surface, and the negative electrode 2 is laminated on the surface of the separator layer 3 facing the interface layer 32 (second solid electrolyte layer) so that the negative electrode active material layer 22 is in contact with the surface.
[0087] <Example 2> In Example 2, in the preparation of the negative electrode, a negative electrode active material having a D50 of 0.5 μm and a specific surface area of 50 m 2 / g of Si powder was used. In the preparation of the second solid electrolyte layer (interface layer), D50 was 0.1 μm and the specific surface area was 30 m 2 / g of sulfide solid electrolyte was used. Except for the above, the all-solid-state battery of Example 2 was produced using the same materials and processes as those of Example 1.
[0088] <Example 3> In Example 3, a Si powder having a D50 of 10.0 μm was used as the negative electrode active material in the preparation of the negative electrode, and a sulfide solid electrolyte having a D50 of 1.1 μm was used in the preparation of the second solid electrolyte layer (interface layer). Except for the above, the all-solid-state battery of Example 2 was produced using the same materials and processes as those of Example 1.
[0089] <Comparative Example 1> In Comparative Example 1, in the preparation of the separator layer, the second solid electrolyte layer was not formed, and the first solid electrolyte layer was formed with a basis weight of 4.0 mg / cm 2 It was formed so as to have a thickness of 20 μm. Except for the above, the all-solid-state battery of Comparative Example 1 was produced using the same materials and processes as in Example 1.
[0090] <Comparative Example 2> In Comparative Example 2, a Si powder having a D50 of 10.0 μm was used as the negative electrode active material in the preparation of the negative electrode, and a sulfide solid electrolyte having a D50 of 2.2 μm was used in the preparation of the first solid electrolyte layer (interface layer). Except for the above, the all-solid-state battery of Comparative Example 2 was produced using the same materials and processes as those of Comparative Example 1.
[0091] <Battery resistance measurement> For each of the batteries (all-solid-state batteries) of the above examples and comparative examples, the battery resistance was measured by the following method.
[0092] Each battery was restrained at 0.1 MPa and subjected to constant current-constant voltage (CC-CV) charging and CC-CV discharging at a current value of 1 mA, upper limit voltage of 4.5 V, and lower limit voltage of 3.0 V. Next, CC-CV charging was performed at a current value of 1 mA and upper limit voltage of 3.3 V (SOC: 30%), and after a 10-minute pause, CC discharging was performed for 10 seconds at a current value of 100 mA and lower limit voltage of 0.0 V, and the voltage drop (ΔV) and current during discharge (I) were measured. From the measurement results, the battery resistance R (= ΔV / I) was calculated according to Ohm's law. Note that SOC stands for State of Charge. The measurement results of the battery resistance are shown in Table 1. The battery resistance and Rzjis / Φ SE A graph showing the relationship is shown in FIG.
[0093] [Table 1]
[0094] From the results shown in Table 1 and Figure 2, Rzjis / D50 SE is 7 or more (D50 SE In Examples 1 to 3, Rzjis / D50 is 1 / 7 or less. SE is less than 7 (D50 SE It can be seen that the battery resistance (battery resistance at SOC 30%) when the initial confining pressure was 0.1 MPa is significantly lower than that of Comparative Examples 1 and 2 in which / Rzjis is more than 1 / 7.
[0095] The present embodiment and the present embodiment are illustrative in all respects. The present embodiment and the present embodiment are not restrictive. The technical scope of the present disclosure includes all modifications within the meaning and scope equivalent to the description of the claims. For example, it is also intended from the beginning that any configuration may be extracted from the present embodiment and the present embodiment, and that they may be arbitrarily combined. [Explanation of symbols]
[0096] 1 positive electrode, 11 positive electrode current collector, 12 positive electrode active material layer, 2 negative electrode, 21 negative electrode current collector, 22 negative electrode active material layer, 3 separator layer, 31 main layer, 32 interface layer, 5 power storage element, 100 all-solid-state battery.
Claims
1. An all-solid-state battery comprising a positive electrode, a negative electrode, and a separator layer, the positive electrode or the negative electrode contains an active material whose volume change rate due to charging and discharging is 10% or more, the separator layer includes solid electrolyte particles and has an interface layer in contact with the positive electrode or the negative electrode including the active material, The solid-state battery, wherein D50 of the solid electrolyte particles contained in the interface layer is 1 / 7 or less of the ten-point average roughness of the positive electrode or the negative electrode containing the active material.
2. The all-solid-state battery according to claim 1 , wherein the negative electrode contains, as the active material, a negative electrode active material containing Si.
3. The all-solid-state battery according to claim 1 , wherein the positive electrode contains a positive electrode active material containing S as the active material.
Citation Information
Patent Citations
Negative electrode for lithium secondary battery, and the lithium secondary battery containing same
JP2004146348A
Negative electrode for secondary battery, copper foil for electrode, secondary battery, and process for producing the negative electrode for secondary battery
JP2010282958A
All-solid-state lithium ion secondary battery
JP2014035818A
All-solid type secondary battery, method for manufacturing electrode sheet for batteries, and method for manufacturing all-solid type secondary battery
JP2015195183A
Lithium solid type secondary battery and method for manufacturing the same
JP2016035867A