Press-through package packaging, lid material for press-through package, and heat seal agent for press-through package
The use of a halogen-free α-olefin-(meth)acrylic acid ester copolymer-based heat sealing agent addresses the limitations of existing agents, offering versatile and environmentally friendly heat-sealability for diverse container materials.
Patent Information
- Application Number
- JP2022085920
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-02-10
- Filing Date
- 2022-05-26
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2042-05-26
AI Technical Summary
Existing heat sealing agents are not suitable for a wide range of materials, contain halogens, and often use aromatic solvents, posing safety and environmental concerns.
A heat sealing agent composed of an α-olefin-(meth)acrylic acid ester copolymer is used, which is free from halogens and aromatic solvents, and is applied to a base material forming a heat-sealing layer compatible with various containers made from materials like polyester resin, polyolefin resin, fluorine resin, polyvinyl chloride, and polyvinylidene chloride.
The solution provides excellent heat-sealability for various containers with low environmental impact, ensuring safety and reducing the risk of container damage during sealing.
Smart Images

Figure 0007582254000001 
Figure 0007582254000002 
Figure 0007582254000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a press-through package (PTP) that can be used for medical purposes, food, daily necessities, etc., a lid material for the press-through package, and a heat sealant for the press-through package. [Background technology]
[0002] A PTP package having a base and a lid is known as one of the packaging forms for medicines, foods, etc. A PTP package is a package in which a lid is attached to a container for accommodating contents by heat and pressure (heat sealing), and various heat sealing agents are used.
[0003] The lid material of the PTP package is composed of a metal foil such as aluminum foil (also called aluminum foil), a plastic film, a deposition film, a base material such as paper or nonwoven fabric, a heat seal layer, and a coating layer. For example, aluminum foil and plastic film are the mainstream for packaging medicines.
[0004] On the other hand, various materials are selected for PTP packaging containers depending on the application of the packaging material, and for example, polyvinyl chloride is the mainstream for pharmaceutical packaging. In recent years, with the movement towards dechlorination due to the problem of dioxin generation when polyvinyl chloride is burned, the use of non-oriented polypropylene (CPP) and amorphous polyethylene terephthalate (A-PET) is also increasing.
[0005] As described above, various materials are used for PTP packages, and the heat sealant suitable for each packaging material and application is selected. In particular, when packaging medicines, it is necessary to prevent the contents from deteriorating for a long period of time, so selecting the most suitable heat sealant is important.
[0006] For example, Patent Document 1 shows that a heat seal coating used in food packaging bags or blister packaging of medicines, which contains a polyester having a specific glass transition temperature and softening point, an anti-tack additive, and an organic solvent, is suitable for PET film and BOPP film. Patent Document 2 shows that a heat seal agent containing a polyester resin, a chlorinated polypropylene resin, and an organic solvent has excellent heat sealability between aluminum foil and a polypropylene sheet. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Special Publication No. 2017-512724 [Patent Document 2] Japanese Patent Publication No. 55-92778 Summary of the Invention [Problem to be solved by the invention]
[0008] Although various heat-sealing agents are provided according to the purpose, it is preferable that one type of heat-sealing agent can be applied to various substrates from the viewpoint of workability. In particular, in recent years, container materials have been reconsidered from the viewpoint of environmental load and diversification of container materials has progressed, so there is a great demand for heat-sealing agents that have excellent heat-sealing properties for all materials.
[0009] In addition, many conventional heat sealants contain halogens, such as the heat sealant described in Patent Document 2, and halogen-free materials are required from the viewpoint of safety. Furthermore, from the viewpoint of environmental safety, it is preferable that the material does not use aromatic solvents such as toluene and xylene or ketone solvents.
[0010] The present invention has been made to solve at least part of these problems, and has an object to provide a press-through package packaging body, a lid material for press-through packages, and a heat sealant for press-through packages that have excellent heat sealing properties for various containers. [Means for solving the problem]
[0011] The present invention relates to a press-through package comprising a base material, a lid material having a heat seal layer provided on the base material, and a container covered with the heat seal layer, the heat seal layer being a coating layer of a heat seal agent containing an α-olefin-(meth)acrylic acid ester copolymer, and the container being formed from a resin containing at least one member of the group consisting of polyester-based resins, polyolefin-based resins, fluorine-based resins, polyvinyl chloride, and polyvinylidene chloride.
[0012] The present invention also relates to a lid material for press-through packaging, which has a substrate and a heat seal layer provided on the substrate, the heat seal layer being a coating layer of a heat seal agent containing an α-olefin-(meth)acrylic acid ester copolymer, and the container is formed from a resin containing at least one member of the group consisting of polyester-based resins, polyolefin-based resins, fluorine-based resins, polyvinyl chloride, and polyvinylidene chloride.
[0013] The present invention also relates to a heat seal agent for press-through packaging, which is applied onto a substrate to form a heat seal layer for bonding the substrate and a container, the heat seal agent containing an α-olefin-(meth)acrylic acid ester copolymer, and the container being formed from a resin containing at least one member of the group consisting of polyester-based resins, polyolefin-based resins, fluorine-based resins, polyvinyl chloride, and polyvinylidene chloride. Effect of the Invention
[0014] According to the present invention, it is possible to provide a press-through package, a lid material for a press-through package, and a heat sealant for a press-through package that have excellent heat sealability for various containers and have a low environmental impact. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The press-through package of the present invention has a base material, a lid material having a heat seal layer provided on the base material, and a container covered by the heat seal layer. Each configuration of the package of the present invention will be described below. Note that the present invention is not limited to the following embodiments.
[0016] <Heat seal layer> The heat seal layer of the present invention is provided by applying a heat seal agent containing an α-olefin-(meth)acrylic acid ester copolymer to a substrate. In the present invention, the term "(meth)acrylic acid ester" refers collectively to acrylic acid ester and methacrylic acid ester.
[0017] The α-olefin-(meth)acrylic acid ester copolymer is a copolymer in which an α-olefin and a (meth)acrylic acid ester are copolymerized.
[0018] The α-olefin may be any known α-olefin without any particular limitation, and examples thereof include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 4-methyl-1-pentene, butadiene, etc., and one or more of these may be used. Among these, α-olefins mainly composed of ethylene or propylene are preferred.
[0019] As the (meth)acrylic acid ester, known (meth)acrylic acid esters can be used without any particular limitation, and for example, alkyl esters, hydroxyalkyl esters, alkoxyalkyl esters, etc. of acrylic acid or methacrylic acid can be used. Specific examples include acrylic acid esters such as methyl acrylate, ethyl acrylate, isopropyl acrylate, n-propyl acrylate, n-butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, isooctyl acrylate, n-octyl acrylate, 2-hydroxyethyl acrylate, and 2-methoxyethyl acrylate, and methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, n-lauryl methacrylate, 2-hydroxyethyl methacrylate, and 2-ethoxyethyl methacrylate. These can be used alone or in combination of two or more. Among them, it is preferable to use one or more of methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate as the (meth)acrylic acid ester, and it is preferable to use methyl (meth)acrylate as the main component in combination with n-butyl (meth)acrylate and isobutyl (meth)acrylate. For example, it is preferable that methyl (meth)acrylate is 60 mass% or more, and more preferably 70 mass% or more, of the total amount of the (meth)acrylic acid ester.
[0020] In addition, the α-olefin-(meth)acrylic acid ester copolymer may further comprise other monomers copolymerized therein, but the content of structural units derived from other monomers is preferably 30 mass % or less, more preferably 10 mass % or less, even more preferably 3 mass % or less, and even more preferably 1 mass % or less of the entire copolymer.
[0021] The proportion of ethylene in the α-olefin-(meth)acrylic acid ester copolymer is not particularly limited, but the proportion of ethylene in the copolymer is preferably 50% by mass or more, more preferably 60% by mass or more. On the other hand, the proportion of the (meth)acrylic acid ester copolymer in the copolymer is preferably 20% by mass or more, more preferably 30% by mass or more.
[0022] The weight average molecular weight of the α-olefin-(meth)acrylic acid ester copolymer is not particularly limited, but is preferably 200,000 or more from the viewpoint of blocking resistance, while the weight average molecular weight is preferably 1,000,000 or less, more preferably 500,000 or less from the viewpoint of adhesion and low-temperature heat sealability.
[0023] In addition, the glass transition temperature of the α-olefin-(meth)acrylic acid ester copolymer is preferably 20° C. or lower, more preferably 10° C. or lower, and even more preferably 0° C. or lower, since the heat sealability at low temperatures is good. On the other hand, the lower limit of the glass transition temperature is preferably −70° C. or higher, more preferably −60° C. or higher, and even more preferably −50° C. or higher.
[0024] The α-olefin-(meth)acrylic acid ester copolymer used in the present invention may be a known one, and a commercially available product may be used.
[0025] The heat-sealing agent of the present invention contains the above-mentioned α-olefin-(meth)acrylic acid ester copolymer and an organic solvent. In the heat-sealing agent, the α-olefin-(meth)acrylic acid ester copolymer is preferably adjusted to have a solid content concentration of 20 to 70% by weight.
[0026] The dilution solvent that can be used is not particularly limited, but examples thereof include various organic solvents such as aromatic hydrocarbons such as toluene, xylene, Solvesso #100, Solvesso #150, etc.; aliphatic hydrocarbons such as hexane, heptane, octane, decane, etc.; and esters such as methyl acetate, ethyl acetate, isopropyl acetate, butyl acetate, amyl acetate, ethyl formate, butyl propionate, etc. Examples of water-miscible organic solvents include alcohols such as methanol, ethanol, propanol, and butanol, ketones such as acetone, methyl ethyl ketone, and cyclohexanone, and glycol ethers such as ethylene glycol (mono, di) methyl ether, ethylene glycol (mono, di) ethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, monobutyl ether, diethylene glycol (mono, di) methyl ether, diethylene glycol (mono, di) ethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol monobutyl ether, triethylene glycol (mono, di) methyl ether, propylene glycol (mono, di) methyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, and dipropylene glycol (mono, di) methyl ether. Among these, it is preferable to use alcohols, ketones such as methyl ethyl ketone, and mixtures thereof. In recent years, from the viewpoint of the working environment, it is more preferable not to use aromatic solvents such as toluene and xylene, or ketone solvents.
[0027] The heat sealant of the present invention may contain additives in addition to the α-olefin-(meth)acrylic acid ester copolymer and the organic solvent. Examples of additives include wax, filler, viscosity modifier, preservative, antibacterial agent, rust inhibitor, antioxidant, crosslinking agent, curing agent, curing catalyst, light stabilizer, ultraviolet absorber, photocatalytic compound, dye, inorganic pigment, organic pigment, extender pigment, plasticizer, antistatic agent, etc. Among them, it is preferable to contain a filler such as silica and an antiblocking agent such as wax in order to prevent blocking.
[0028] On the other hand, the heat-sealing agent of the present invention is preferably substantially free of any other resin than the α-olefin-(meth)acrylic acid ester copolymer, and the resin component contained in the heat-sealing agent is preferably the α-olefin-(meth)acrylic acid ester copolymer. That is, the heat-sealing agent of the present invention is preferably a simple composition consisting of the α-olefin-(meth)acrylic acid ester copolymer.
[0029] The term "substantially free" means that no resin other than the α-olefin-(meth)acrylic acid ester copolymer is intentionally contained.
[0030] <Base material> The base material used as the lid material of the press-through package is not particularly limited, and known films, papers, metal foils, etc. that are usually used for packaging materials are preferably used. In the case of packaging medicines, it is preferable to use metal foils such as aluminum foil or films.
[0031] The metal foil may be, for example, an aluminum foil.
[0032] Examples of films include those made from PET (polyethylene terephthalate), A-PET (amorphous polyethylene terephthalate), PBT (polybutylene terephthalate), BOPP (biaxially oriented polypropylene), PE (polyethylene), PVC (polyvinyl chloride), PS (polystyrene), Ny (nylon), EVOH (ethylene-vinyl alcohol copolymer), etc. These films may have a metal deposition layer such as aluminum, or a metal oxide deposition layer such as silica, alumina, or a binary deposition of these. When the base film of the lid material and the container are made of the same material, recyclability can be improved by making them mono-material.
[0033] Examples of the paper include those made by a known papermaking machine using natural fibers for papermaking such as wood pulp. The papermaking conditions are not particularly specified. Examples of the natural fibers for papermaking include wood pulp such as softwood pulp and hardwood pulp, non-wood pulp such as Manila hemp pulp, sisal hemp pulp, and flax pulp, and pulps obtained by chemically modifying these pulps. Types of pulp that can be used include chemical pulp made by sulfate cooking, acidic / neutral / alkaline sulfite cooking, soda cooking, etc., ground pulp, chemi-ground pulp, thermomechanical pulp, etc.
[0034] More specifically, examples of such paper include uncoated papers such as various types of printing paper, gravure paper, kraft paper, Kent paper, copy paper, wood grain paper, and newspaper; lightly coated papers; coated papers such as art paper, one-sided art paper, coated paper, one-sided coated paper, and light-weight coated paper; high-quality paper; double-glazed kraft papers for heavy use, general use, and special use; unbleached wrapping papers such as veined kraft paper and one-sided glossy kraft paper; pure white roll paper; bleached kraft papers such as double-glazed bleached kraft paper and one-sided glossy bleached kraft paper; other bleached wrapping papers; resin-impregnated papers such as paraffin paper, cardboard and paperboard, vapor-deposited papers in which metals such as aluminum are vapor-deposited onto these papers, and laminated papers in which these papers are laminated with metal foil such as aluminum foil.
[0035] A printing layer may be provided on these substrates. The printing layer is formed by a general printing method that has been used for printing on polymer films using various printing inks such as gravure ink, flexographic ink, offset ink, stencil ink, and inkjet ink. The printing layer may be provided on the surface of the substrate on the heat seal layer side, or on the other surface.
[0036] In addition, the substrate preferably has an overcoat layer on the surface opposite to the surface on which the heat seal layer is provided, i.e., the outer surface on the side not adhered to the container. The overcoat layer is provided by applying an overcoating agent to the substrate. When the package is heat-sealed, heat of nearly 300°C is applied, which tends to cause problems such as bleeding of the printed layer and, for example, cracking of the metal layer when a metal foil is used as the substrate. However, by providing a coating agent, functionality such as heat resistance and abrasion resistance can be improved.
[0037] Although known coating agents can be used, those containing a polyvinyl butyral resin are preferred. Coating agents containing a polyvinyl butyral resin are excellent in adhesion, heat resistance, and abrasion resistance, and also have a high function of protecting the metal foil or metal layer.
[0038] The weight-average molecular weight of the polyvinyl butyral resin used in the coating agent is preferably 5000 to 150000, more preferably 6000 to 100000, and further preferably 7000 to 50000. By setting the weight-average molecular weight of the polyvinyl butyral resin within the above range, it is possible to obtain a coating agent having an excellent balance between the fluidity and dispersibility of the coating composition, and the strength of the coating film.
[0039] The glass transition temperature (hereinafter sometimes referred to as Tg) of the polyvinyl butyral resin is preferably in the range of 50° C. to 120° C., more preferably in the range of 55° C. to 115° C., and more preferably in the range of 60 to 90° C. In the present invention, the glass transition temperature is obtained by measurement with a differential scanning calorimeter.
[0040] The hydroxyl value of the polyvinyl butyral resin is preferably in the range of 10 to 50 mol / %, more preferably 30 to 40 mol / %. By setting the hydroxyl value of the polyvinyl butyral resin in the above range, the resin has excellent curability when reacted with a crosslinking agent, and can provide a coating film having both strength and appropriate flexibility.
[0041] The polyvinyl butyral resin content (solid content of polyvinyl butyral resin) is preferably 10 to 50 mass % relative to 100 mass % of the coating agent, more preferably 15 to 40 mass %, and most preferably 20 to 30 mass %.
[0042] The polyvinyl butyral resin contained in the coating agent may be used alone or in combination of two or more kinds.
[0043] The coating agent preferably contains a polyisocyanate compound together with the polyvinyl butyral resin. By containing polyvinyl butyral and a polyisocyanate compound, a crosslinked resin can be formed by the curing reaction between them. Therefore, the adhesion, abrasion resistance, and heat resistance can be improved.
[0044] The polyisocyanate is not particularly limited as long as it is an isocyanate compound having a plurality of isocyanate groups that can react with polyvinyl butyral. For example, polyisocyanates such as tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, 1,6-hexamethylene diisocyanate, isophorone diisocyanate, 4,4'-methylenebis(cyclohexylisocyanate), lysine diisocyanate, trimethylhexamethylene diisocyanate, 1,3-(isocyanatomethyl)cyclohexane, 1,5-naphthalene diisocyanate, and triphenylmethane triisocyanate; and derivatives (modified products) of polyisocyanates such as adducts of these polyisocyanates, biurets of these polyisocyanates, or isocyanurates of these polyisocyanates.
[0045] The polyisocyanate compound acts as a curing agent and can be appropriately selected for use, and may be aromatic or aliphatic. Examples of polyisocyanate compounds preferably used in the present invention include polyisocyanates such as hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), xylylene diisocyanate (XDI), tolylene diisocyanate (TDI), and diphenylmethane diisocyanate (MDI).
[0046] Among these, xylylene diisocyanate (XDI) and tolylene diisocyanate (TDI) are preferred.
[0047] [Isocyanate group content (equivalent)] The isocyanate group content (equivalent) of the polyisocyanate relative to the hydroxyl value of the polyvinyl butyral resin is preferably in the range of 0.1 to 5.0, more preferably in the range of 0.2 to 4.0, and even more preferably in the range of 0.3 to 3.0. By setting it in this range, it is possible to achieve both adhesion to the metal foil or metal layer and abrasion resistance. The isocyanate group content (equivalent) of the polyisocyanate relative to the hydroxyl value of the polyvinyl butyral resin was calculated by the following method. Hydroxyl value of polyvinyl butyral resin: A (mgKOH / g) Mass of polyvinyl butyral resin: B (g) Polyisocyanate NCO%:C(%) Mass of polyisocyanate: D(g) NCO / OH ratio=C×D×561 / (A×B×42) D(g)=((A×B) / C)×(42 / 561)×NCO / OH(equivalent ratio) The coating agent may contain a general-purpose resin in addition to the polyvinyl butyral resin and polyisocyanate. For example, epoxy resin, cellulose resin, polyamide resin, vinyl chloride-vinyl acetate copolymer resin, vinyl chloride-acrylic copolymer resin, rosin resin, ethylene-vinyl acetate copolymer resin, vinyl acetate resin, acrylic resin, styrene resin, dammar resin, styrene-maleic acid copolymer resin, polyester resin, alkyd resin, terpene resin, phenol-modified terpene resin, ketone resin, cyclized rubber, chlorinated rubber, polyacetal resin, petroleum resin, and modified resins thereof. These resins may be used alone or in combination of two or more. In the case of pharmaceutical or food applications, it is preferable not to use epoxy resin or chlorine-based resin from the viewpoint of safety and hygiene.
[0048] To improve wear resistance, anti-wear agents, slip agents, etc. may be added. Fatty acid amides, silicones, polyethylene, polypropylene, PTFE, etc. may be used alone or in combination of two or more.
[0049] In order to improve the curability, a catalyst may be added, such as an organic tin compound, a tertiary amine compound, an organic titanium compound, or an organic zirconium compound.
[0050] If necessary, it is preferable to use an organic compound-based blocking inhibitor such as fatty acid amide, fatty acid ester, or higher fatty acid other than the above. These organic compound-based blocking inhibitors prevent blocking by bleeding out onto the heat seal layer surface. Therefore, a particle-based blocking inhibitor and an organic compound-based blocking inhibitor may be used in combination. If a large amount of an organic compound-based blocking inhibitor is added, it inhibits adhesion and is likely to cause poor adhesion, so it is preferable to add only a small amount.
[0051] When actually applying the coating agent to a substrate, it is preferable to dissolve the agent in various organic solvents to a solid content of 20% by mass in order to improve the application performance.
[0052] The dilution solvent that can be used is not particularly limited, but examples thereof include various organic solvents such as aromatic hydrocarbons such as toluene, xylene, Solvesso #100, Solvesso #150, etc.; aliphatic hydrocarbons such as hexane, heptane, octane, decane, etc.; and esters such as methyl acetate, ethyl acetate, isopropyl acetate, butyl acetate, amyl acetate, ethyl formate, butyl propionate, etc. Examples of water-miscible organic solvents include alcohols such as methanol, ethanol, propanol, and butanol, ketones such as acetone, methyl ethyl ketone, and cyclohexanone, and glycol ethers such as ethylene glycol (mono, di) methyl ether, ethylene glycol (mono, di) ethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, monobutyl ether, diethylene glycol (mono, di) methyl ether, diethylene glycol (mono, di) ethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol monobutyl ether, triethylene glycol (mono, di) methyl ether, propylene glycol (mono, di) methyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, and dipropylene glycol (mono, di) methyl ether. Among these, it is preferable to use alcohols, ketones such as methyl ethyl ketone, and mixtures thereof. In recent years, from the viewpoint of the working environment, it is more preferable not to use aromatic solvents such as toluene and xylene, or ketone solvents.
[0053] The coating method for the substrate can be, for example, a bar coater, a gravure coat method, a roll coat method, a knife coat method, a kiss coat method, etc. In order to maximize the effect of the present invention, the coating amount for the metal foil or metal layer is 0.5 to 5 g / m 2 The drying conditions are preferably within a range of 120 to 200° C. for 5 to 100 seconds.
[0054] [Lid material] The lid material of the present invention is obtained by applying a heat sealant to a substrate and drying it. A heat seal layer (a dried coating of the heat sealant of the present invention) may be provided directly on the substrate, or one or more primer layers may be provided on the substrate. When a primer layer is provided, the primer used to form the primer layer is not particularly limited, and a known primer may be used.
[0055] The heat sealing agent can be applied by a known method, such as a roll coater, gravure coater, flexo coater, air doctor coater, blade coater, air knife coater, squeeze coater, impregnation coater, transfer roll coater, kiss coater, curtain coater, cast coater, spray coater, die coater, offset printing machine, screen printing machine, etc. After application, a drying step may be performed in an oven, etc.
[0056] The drying method may be a known method such as hot air, electric heat, infrared rays, electron beams, etc. The heating temperature is preferably 50 to 250° C., and the heating time is preferably 0.1 to 30 seconds.
[0057] The amount of heat sealant applied is adjusted appropriately depending on the desired seal strength and the substrate. For example, 1.0 g / m 2 ~5.0g / m 2 It is.
[0058] [container] The container of the press-through package has a pocket-shaped recess for accommodating the contents, and a flange provided at the end of the container is bonded to the lid material via a heat seal layer, so that the contents can be accommodated in a sealed state. A heat seal layer may be provided on the flange of the container.
[0059] The container is a transparent thermoplastic resin sheet formed from at least one resin selected from the group consisting of polyester resin, polyolefin resin, fluorine resin, polyvinyl chloride, and polyvinylidene chloride. A laminated sheet formed by laminating two or more of these thermoplastic resin sheets may also be used.
[0060] Also, a sheet laminated or coated with a resin containing at least one of the group consisting of polyester resin, polyolefin resin, fluorine resin, polyvinyl chloride, and polyvinylidene chloride may be used as a known PTP container or thermoplastic resin sheet. It is sufficient that the layer in direct contact with the heat seal layer is formed of a resin containing at least one of the group consisting of polyester resin, polyolefin resin, fluorine resin, polyvinyl chloride, and polyvinylidene chloride.
[0061] Examples of polyester resins include polyethylene terephthalate, polyethylene naphthalate, polyethylene isophthalate, and polybutylene terephthalate.
[0062] Examples of polyolefin resins include polyethylene resins, polypropylene resins, ethylene-vinyl alcohol copolymer resins, resins made of cyclic olefins, etc. Containers using polyolefin resins are preferred because they have excellent heat sealability with the heat sealing agent of the present invention, and among these, resins containing polypropylene are preferred.
[0063] Examples of fluorine-based resins include polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-hexafluoropropylene-perfluoroalkyl vinyl ether (EPA), tetrafluoroethylene-ethylene copolymer (ETFE), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), and chlorotrifluoroethylene-ethylene copolymer (ECTFE).
[0064] Among these, polyethylene terephthalate, polypropylene, polyethylene, polyvinyl chloride, polyvinylidene chloride, and polychlorotrifluoroethylene (PCTFE) are preferred. Polychlorotrifluoroethylene (PCTFE) has excellent water vapor barrier properties and oxygen barrier properties, making it possible to reduce the thickness and weight of the container, thereby providing a more sustainable package. Materials containing fluorine, such as PCTFE, generally have poor heat sealability, but by using the heat seal agent of the present invention, a container having excellent heat sealability can be realized even when a fluorine-based material is used. These sheets can be molded into a desired shape by vacuum heating, pressure forming, or the like to obtain containers for press-through packages.
[0065] [Press-through package] The press-through package of the present invention is used by bonding the above-mentioned lid material and container with a heat seal layer. That is, the press-through package can be produced by a method in which a content such as a medicine is placed in a recess of the container, and the lid material is placed on the container with the heat seal layer facing the container and thermally bonded.
[0066] The press-through package of the present invention can be used as a packaging material for medicines, tablets, foods such as candy and chocolate, etc. It can also be used as a packaging material for blister packs of toothbrushes, dry batteries, toys, etc. EXAMPLES
[0067] The present invention will be described more specifically with reference to examples. In the following, all "parts" and "%" are based on mass.
[0068] In the present invention, the number average molecular weight and weight average molecular weight (converted into polystyrene) were measured by GPC using an HLC8220 system manufactured by Tosoh Corporation under the following conditions. Separation column: Four TSKgel GMHHR-N columns manufactured by Tosoh Corporation were used. Column temperature: 40 ° C. Mobile phase: Tetrahydrofuran (Wako Pure Chemical Industries, Ltd.). Flow rate: 1.0 ml / min. Sample concentration Concentration: 1.0% by weight. Sample injection volume: 100 microliters. Detector: differential refractometer.
[0069] The glass transition temperature (Tg) was measured in a differential atmosphere using a cooling device in the temperature range of -8 The analysis was carried out by DMA at 0 to 450°C with a temperature increase rate of 10°C / min.
[0070] [Preparation of heat sealant] (Heat sealant 1) A commercially available ethylene-methacrylic acid copolymer resin (solid content 45%) was dissolved in a mixed solvent of methyl ethyl ketone and ethyl acetate to a solid content of 25%, to prepare a heat sealing agent 1. The mass ratio of methyl ethyl ketone and ethyl acetate in the mixed solvent was methyl ethyl ketone / ethyl acetate = 50 / 50.
[0071] (Heat sealant 2) Vinyl chloride-vinyl acetate copolymer resin (weight average molecular weight 50,000, vinyl chloride ratio 85%, glass transition point (Tg) 75°C, K value measured by ISO1628-2 45) was dissolved in a mixed solvent of methyl ethyl ketone and ethyl acetate to a solid content of 25% to prepare heat sealing agent 2. The mass ratio of methyl ethyl ketone and ethyl acetate in the mixed solvent was methyl ethyl ketone / ethyl acetate = 50 / 50.
[0072] (Heat sealant 3) Heat sealing agent 3 was prepared by dissolving vinyl chloride-vinyl acetate copolymer resin (weight average molecular weight 50,000, vinyl chloride ratio 85%, glass transition point (Tg) 75°C, K value 45 measured by ISO1628-2) and polyester resin (number average molecular weight 30,000, glass transition point (Tg) -20°C) in a mixed solvent of methyl ethyl ketone and ethyl acetate to a solid content of 16%. The ratio of the vinyl chloride-acetate copolymer resin to the polyester resin was 1:1 by mass. The ratio of methyl ethyl ketone and ethyl acetate in the mixed solvent was methyl ethyl ketone / ethyl acetate = 60 / 40 by mass.
[0073] [Preparation of lid material] Example 1 Heat seal agent 1 was applied to hard aluminum foil (manufactured by Toyo Aluminum Co., Ltd.) using a bar coater (application amount 4 g / m 2 After coating, the mixture was dried at 180° C. for 10 seconds to form a heat seal layer, thereby preparing a cover material 1.
[0074] (Comparative Examples 1 and 2) Using the heat seal agents 2 and 3, the same hard aluminum foil as in Example 1 was coated with a bar coater (coating amount 4 g / m 2 After coating, the mixture was dried at 180° C. for 10 seconds to form a heat seal layer, thereby preparing cover materials 2 and 3.
[0075] The produced lid materials 1 to 3 were evaluated as follows.
[0076] [Evaluation Criteria 1: Adhesion to substrate] The prepared lid material is placed on a flat table with the heat seal layer facing up, 24 mm wide cellophane tape from Nichiban is attached to the surface with the heat seal layer, and the cellophane tape is rubbed over the top of the cellophane tape with a cloth or the like so that the cellophane tape is completely adhered to the coating film. While pressing a frame about 2 mm larger than the attached cellophane tape firmly against the coating film on the outside of the cellophane tape, the cellophane tape attached to the coating film is forcefully peeled upwards, and the degree of adhesion of the coating film to the aluminum foil is visually judged.
[0077] (Evaluation Criteria) 5: No peeling of the coating film was observed in the area where the cellophane tape was attached. 4: Less than 10% of the coating film on the cellophane tape was peeled off. 3: 10% or more but less than 30% of the coating film in the cellophane tape adhesive area peeled off 2: 30% or more but less than 50% of the coating film at the cellophane tape attachment area peeled off. 1: Simple: More than 50% of the coating film at the cellophane tape attachment point peeled off.
[0078] [Evaluation Criteria 2: Blocking] The coated side of the heat sealant of the prepared lid material and the uncoated glossy hard aluminum side are overlapped for 24 hours in an atmosphere of 40°C under a pressure of 0.5 MPa (5.0 kgf / cm2), and then the state of blocking when peeled off is evaluated by the feel when peeled off by hand. Each test was performed three times and evaluated.
[0079] ○: No blocking at all. △: Some blocking. ×: Strong blocking.
[0080] The results are shown in Table 1.
[0081] [Table 1]
[0082] Next, test pieces were prepared using the lid materials 1 to 3 as follows.
[0083] (Examples 2 to 5 and 8) The covering material 1 was laminated with the various sheets shown in the table via a heat seal layer. Using a heat seal tester equipped with a heat seal section for embossing, each was heat sealed at 100°C, 140°C, and 180°C (all at 0.3 MPa for 1 second) to prepare test pieces.
[0084] Example 6 Polyvinyl butyral resin (weight average molecular weight 15,000, hydroxyl value approximately 35 mol / %, glass transition point 70°C) was dissolved in a mixed solvent of methyl ethyl ketone and isopropyl alcohol in a mass ratio of 45:55 to a solid content of 25% to prepare a polyvinyl butyral solution.
[0085] Next, 12 parts of Takenate D-110NB (xylylene diisocyanate (XDI)) as a polyisocyanate were mixed and stirred with 100 parts of the polyvinyl butyral solution so that the NCO group content (equivalent) of the isocyanate was 0.5 to 2.5 relative to the hydroxyl value of the polyvinyl butyral resin, to prepare an overcoating agent.
[0086] The prepared overcoating agent was applied to the hard aluminum foil on the opposite side of the heat seal layer of the lid material 1 so that the coating amount after baking was 2 g / m 2 The mixture was then dried at 180° C. for 10 seconds to obtain a lid material 4. A test piece of Example 6 was produced in the same manner as in Examples 2-5 using the lid member 4.
[0087] Example 7 A commercially available industrial nitrocellulose (solid content 70%), a commercially available acrylic resin (solid content 50%), a commercially available melamine resin (solid content 98%), a mixed solvent, and an acid catalyst as an additive were mixed in a mass ratio of 15:11:4:69:1 to prepare an overcoating agent with a solid content of 20%. The mixed solvent used was a mixture of methyl ethyl ketone, ethyl acetate, and isopropyl alcohol in a mass ratio of 50:30:20.
[0088] The prepared overcoating agent was applied to the hard aluminum foil on the opposite side of the heat seal layer of the lid material 1 so that the coating amount after baking was 2 g / m 2 The mixture was then dried at 180° C. for 10 seconds to obtain a lid material 5. A test piece of Example 7 was produced in the same manner as in Examples 2-6 using the lid member 5.
[0089] (Comparative Examples 2 to 9) Test pieces were prepared in the same manner as in Examples 1 to 4 by using each of Lid material 2 and Lid material 3 and overlapping it with the various films shown in the table via a heat seal layer. The test pieces thus prepared were subjected to the following evaluations.
[0090] [Evaluation Criteria 3: Heat Sealability] For each test piece heat-sealed at 120°C, 160°C, and 200°C, the adhesive strength was measured at a peel speed of 100 mm / min, a peel direction of 180°, and a peel width of 15 mm using a small tabletop tester EZ test manufactured by Shimadzu Corporation. The evaluation criteria were 5-point scale as follows:
[0091] 5:9(N / 15mm) or more 4:6 (N / 15mm) or more and less than 9 (N / 15mm) 3:3 (N / 15mm) or more and less than 6 (N / 15mm) Less than 2:3 (N / 15mm) 1: No adhesion at all
[0092] [Evaluation Criteria 3: Moisture and Heat Resistance] Each test piece heat-sealed at 200°C was left in a thermostatic chamber under a 40°C / 75% humidity environment, and the heat sealability after 3 months was measured using a small tabletop tester EZ test made by Shimadzu Corporation at a peel speed of 100mm / min, a peel direction of 180°, and a peel width of 15mm. The evaluation criteria were as follows: 5: Retains 90% or more of the initial adhesive strength 4: 70% to less than 90% of the initial adhesive strength is maintained 3: Maintains 50% to 70% of the initial adhesive strength 2: Retains 30% to 50% of initial adhesive strength 1: Less than 30% of the initial adhesive strength is retained The results are shown in Tables 2 to 4.
[0093] [Table 2]
[0094] [Table 3]
[0095] [Table 4]
[0096] "PET" in the table means polyethylene terephthalate sheet (film thickness 250μm) "CPP" is a non-oriented polypropylene sheet (film thickness 250μm) "PVC" is a hard polyvinyl chloride sheet (film thickness 250 μm), "PVDC" is a sheet (film thickness 225μm) made by coating a rigid polyvinyl chloride sheet with polyvinylidene fluoride (PVDC). "PCTFE" is a composite sheet of polychlorotrifluoroethylene (film thickness 350μm) (heat seal surface is PCTFE side) Represents. In addition, "-" in the table means that no evaluation was performed.
[0097] From the table, it is clear that the package of the present invention has excellent heat sealability for various containers. In addition, since it can exhibit excellent heat sealability even at a relatively low temperature of 100°C, it is possible to reduce the damage that the package and contents suffer when exposed to high temperatures during heat sealing.
[0098] Furthermore, it was confirmed that the composition provided with an overcoat layer also had excellent properties, as shown in Examples 6 and 7. In particular, the overcoat layer of Example 6 showed no discoloration or blistering at all on the coating surface even after heat sealing, and was found to have excellent heat resistance.
Claims
1. Substrate and A heat seal layer is provided on the substrate, the heat seal layer is a coating layer of a heat seal agent containing an α-olefin-(meth)acrylic acid ester copolymer; the heat seal layer has a heat sealability with respect to any container formed of a resin containing at least one member of the group consisting of a polyester resin, a polyolefin resin, a fluorine resin, polyvinyl chloride, and polyvinylidene chloride; The lid material for press-through packages is used as a press-through package package in which the lid material for press-through packages and the container are bonded via the heat seal layer.
2. The lid material for press-through packages according to claim 1, wherein the substrate is a metal foil or a sheet having a metal layer.
3. The press-through package lid material according to claim 2, wherein the metal foil is an aluminum foil.
4. 3. The cover material for press-through packages according to claim 1, wherein the heat seal layer is substantially free of any resin other than the α-olefin-(meth)acrylic acid ester copolymer.
5. 3. The lid material for press-through packaging according to claim 1, further comprising an overcoat layer on the surface of the substrate opposite to the surface on which the heat seal layer is provided.
6. 6. The lid material for press-through packages according to claim 5, wherein the overcoat layer is a coating layer of an overcoating agent, and the overcoating agent contains a polyvinyl butyral resin and a polyisocyanate compound.
7. The α-olefin-(meth)acrylic acid ester copolymer is an ethylene-(meth)acrylic acid ester copolymer, and the proportion of ethylene in the copolymer is 50 mass% or more; The content of structural units derived from other monomers in the α-olefin-(meth)acrylic acid ester copolymer is 30% by mass or less of the total copolymer, The weight average molecular weight of the α-olefin-(meth)acrylic acid ester copolymer is 200,000 or more and 1,000,000 or less, The press-through package lid material according to claim 1, wherein the α-olefin-(meth)acrylic acid ester copolymer has a glass transition temperature of −70° C. or higher and 20° C. or lower.
8. A press-through package packaging body using the press-through package lid material described in claim 1.
9. A heat sealant for press-through packaging that is applied onto a substrate to form a heat seal layer for bonding the substrate and a container, The heat sealing agent contains an α-olefin-(meth)acrylic acid ester copolymer, the container is formed of a resin including at least one of the group consisting of a polyester-based resin, a polyolefin-based resin, a fluorine-based resin, polyvinyl chloride, and polyvinylidene chloride; A heat-sealing agent for press-through packaging, characterized in that the heat-sealing layer has heat-sealing properties with respect to any of the containers.
Citation Information
Patent Citations
Heattsealing agent
JP1980092778A
Laminate and covering material and bag used thereof
JP1996112880A
Cover material for press-through pack package, and package
JP2013216331A
Heat seal sheet and press through packaging body
JP2016204047A
Solvent-based low-temperature heat seal coating
JP2017512724A