Negative electrode active material and lithium ion battery

A composite negative electrode active material with graphite-coated amorphous carbon and dispersed LiBOB particles addresses the expansion issue in spherical graphite, improving lithium ion battery cycle characteristics and conductivity.

JP7582269B2Active Publication Date: 2024-11-13TOYOTA JIDOSHA KK
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022113135
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-07-14
Publication Date
2024-11-13
Estimated Expiration
2042-07-14

AI Technical Summary

Technical Problem

Spherical graphite used in lithium ion batteries expands during charging, leading to increased internal pores and side reactions with the electrolyte, which reduces battery life and cycle characteristics.

Method used

A composite negative electrode active material is formed by aggregating graphite particles coated with amorphous carbon and dispersing lithium bisoxalatoborate (LiBOB) particles within, which forms a protective film during charging, suppressing the generation of new surfaces due to expansion and contraction.

Benefits of technology

The composite material improves cycle characteristics by preventing the formation of new surfaces and maintaining electronic conductivity, thereby enhancing the battery's lifespan and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582269000002
    Figure 0007582269000002
  • Figure 0007582269000003
    Figure 0007582269000003
  • Figure 0007582269000004
    Figure 0007582269000004
Patent Text Reader

Abstract

To provide a negative electrode active material improved in cycle characteristics.SOLUTION: A negative electrode active material for a lithium ion battery comprises first particles and second particles. The first particles include graphite and an amorphous carbon film that coats the graphite. The second particles contain a lithium bis-oxalate borate, and composite particles are formed as a result of agglomeration of the first particles. The second particles are at least partially dispersed inside the composite particles. In the negative electrode active material, the content of the lithium bis-oxalate borate is 3.0 mass% or less.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a negative electrode active material and a lithium ion battery. [Background technology]

[0002] Patent Document 1 (JP 2020-043069 A) discloses a negative electrode active material for a secondary battery that includes natural graphite containing secondary particles formed by assembling a plurality of primary particles, amorphous carbon present on the surfaces of the primary particles, and a coating layer containing amorphous carbon surrounding the secondary particles, and a lithium ion battery that includes a negative electrode that includes the negative electrode active material. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-043069 A Summary of the Invention [Problem to be solved by the invention]

[0004] Carbon-based materials such as graphite are widely used as negative electrode active materials in lithium ion batteries (hereinafter may be abbreviated as "batteries"). By reducing the size of the graphite particles (making them spherical), it is possible for the graphite to become a negative electrode active material with a large specific capacity. However, since the internal structure of spherical graphite is not dense, it may expand during charging. The expansion increases the internal pores of the graphite, which increases side reactions with the electrolyte, and this may result in a reduction in the battery life.

[0005] Therefore, in order to reduce the internal pores of graphite, the surface of graphite (primary particles) is coated with amorphous carbon in Patent Document 1. However, even when graphite is coated with amorphous carbon, new surfaces, that is, uncoated areas due to cracks or the like are generated due to expansion and contraction accompanying charging and discharging, so there is room for improvement in improving life (cycle) characteristics.

[0006] Therefore, an object of the present disclosure is to provide a negative electrode active material with improved cycle characteristics. [Means for solving the problem]

[0007] The technical configuration and effects of the present disclosure will be described below. However, the mechanism of action in this specification includes assumptions. The mechanism of action does not limit the technical scope of the present disclosure.

[0008] [1] A negative electrode active material for a lithium ion battery, comprising: comprising a first particle and a second particle, the first particles include graphite and an amorphous carbon film coating the graphite, the second particles include lithium bis(oxalato)borate; the first particles are aggregated to form composite particles, At least a portion of the second particles is dispersed within the composite particles, The negative electrode active material has a lithium bis(oxalato)borate content of 3.0% by mass or less.

[0009] When the negative electrode active material contains lithium bis(oxalato)borate (LiBOB), a coating derived from LiBOB is formed on the surface of the negative electrode during the initial charging process. The coating has excellent oxidation resistance and reduction resistance. By using such a negative electrode active material, it is believed that the generation of new surfaces due to expansion and contraction is suppressed even when repeated charging and discharging are performed, and the cycle characteristics are improved.

[0010] On the other hand, if the content of LiBOB in the negative electrode active material is large, the formation of a coating film becomes excessive, and the electronic conductivity between the negative electrode active materials may decrease. Therefore, it is considered necessary to set the content of LiBOB within a predetermined range.

[0011] [2] The negative electrode active material according to [1], wherein the first particles have an average particle size of 1.0 μm or more and 30 μm or less.

[0012] [3] A lithium ion battery comprising: a negative electrode containing the negative electrode active material according to [1] or [2]; a positive electrode; a separator; and an electrolyte solution, the electrolyte solution containing lithium bis(oxalato)borate.

[0013] [4] A negative electrode active material for a lithium ion battery, comprising: comprising a first particle and a second particle, the first particles include graphite and an amorphous carbon film coating the graphite, the second particles include lithium bis(oxalato)borate; the first particles are aggregated to form composite particles, At least a portion of the second particles is dispersed within the composite particles, The content of lithium bis(oxalato)borate in the negative electrode active material is 0.2% by mass or more and 2.0% by mass or less, The average particle size of the first particles is not less than 5.0 μm and not more than 20 μm. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a conceptual diagram showing a first particle in the present embodiment. [Diagram 2] FIG. 2 is a conceptual diagram showing a composite particle in this embodiment. [Diagram 3] FIG. 3 is a conceptual diagram showing the negative electrode active material in this embodiment. [Figure 4] FIG. 4 is a schematic diagram showing an example of the lithium ion battery of this embodiment. [Diagram 5] FIG. 5 is a schematic diagram showing an example of the electrode body of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an embodiment of the present disclosure (hereinafter may be abbreviated as "the present embodiment") and an example of the present disclosure (hereinafter may be abbreviated as "the present embodiment") will be described. However, the present embodiment and the example do not limit the technical scope of the present disclosure.

[0016] <Negative electrode active material> The negative electrode active material of this embodiment is for a lithium ion battery. The lithium ion battery will be described in detail later. The negative electrode active material includes first particles and second particles.

[0017] 《1st particle》 1 is a conceptual diagram showing a first particle in this embodiment. The first particle 11 includes graphite 13 and an amorphous carbon film 14 that covers the graphite 13. The first particle 11 may be substantially composed of the graphite 13 and the amorphous carbon film 14. The graphite 13 may be artificial graphite or natural graphite.

[0018] The graphite 13 is coated with an amorphous carbon film 14. By coating the graphite 13 with the amorphous carbon film 14, it is expected that cycle characteristics, storage characteristics, and the like are improved. The amorphous carbon film 14 may coat a portion of the graphite 13. The amorphous carbon film 14 may coat substantially the entire graphite 13. In other words, the amorphous carbon film 14 coats at least a portion of the surface of the graphite 13.

[0019] The amorphous carbon film 14 may have a thickness of, for example, 0.01 to 0.2 μm. If the thickness of the amorphous carbon film 14 is less than 0.01 μm, the effect of covering the graphite 13 with the amorphous carbon film 14 may not be obtained. If the thickness of the amorphous carbon film 14 exceeds 0.2 μm, the resistance may become high.

[0020] The thickness of the amorphous carbon film 14 can be measured, for example, by the following procedure. A sample is prepared by embedding the first particles in a resin material. The sample is thinned by FIB (Focused Ion Beam) processing. The sample is observed by STEM (Scanning Transmission Electron Microscope). The arithmetic average of the values ​​measured for a plurality of the first particles may be regarded as the thickness of the amorphous carbon film 14.

[0021] The amorphous carbon film 14 includes amorphous carbon. For example, the amorphous carbon film 14 may be substantially made of amorphous carbon. The amorphous carbon may include, for example, carbide of pitch. The content of amorphous carbon relative to the graphite 13 may be, for example, 1.0 to 10 mass %. If the content of amorphous carbon relative to the graphite 13 is less than 1.0 mass %, the amorphous carbon film 14 may not be formed. If the content of amorphous carbon relative to the graphite 13 exceeds 10 mass %, the electronic conductivity between the negative electrode active materials decreases, and thus the resistance may increase.

[0022] The first particle 11 has an average particle size (D50) of, for example, 1.0 to 30 μm. If the D50 of the first particle 11 is less than 1.0 μm, the distribution of the second particle in the composite particle described below may be non-uniform. If the D50 of the first particle 11 exceeds 30 μm, the first particle 11 expands with charging, and the internal pores in the composite particle become larger, so that the cycle characteristics may deteriorate. The first particle 11 preferably has a D50 of 5.0 to 20 μm. Here, D50 indicates the particle size at which the cumulative frequency from the small particle size side reaches 50% in the volume-based particle size distribution. D50 can be measured by a laser diffraction method.

[0023] (composite particles) 2 is a conceptual diagram showing a composite particle in this embodiment. Composite particles 15 are formed by aggregation of first particles 11. The formation of composite particles 15 is carried out, for example, by granulation.

[0024] 《Second particle》 FIG. 3 is a conceptual diagram showing the negative electrode active material in this embodiment. The second particles 12 contain LiBOB. Since the negative electrode active material 10 contains LiBOB, a coating derived from LiBOB is formed on the surface of the negative electrode in the initial charging process. As a result, even when repeated charging and discharging are performed, the generation of new surfaces due to expansion and contraction is suppressed, and improvement in cycle characteristics is expected. The second particles 12 may be substantially made of LiBOB. The second particles 12 may have a D50 of, for example, 0.5 to 3.0 μm. When the second particles 12 have a D50 of 0.5 to 3.0 μm, the second particles 12 are easily dispersed inside the composite particles 15, as described later.

[0025] The second particles 12 are supported by the first particles 11. At least a portion of the second particles 12 is dispersed inside the composite particles 15. It is believed that the dispersion of at least a portion of the second particles 12 inside the composite particles 15 promotes the formation of a coating derived from LiBOB.

[0026] The fact that the second particles 12 are dispersed inside the composite particles 15 can be confirmed, for example, by the following procedure. A sample is prepared by embedding the negative electrode active material 10 in a resin material. The sample is processed with a cross-section polisher (CP) by argon (Ar) etching. After the CP processing, the sample is observed with an ultra-low voltage scanning electron microscope (ULV-SEM).

[0027] The content of LiBOB in the negative electrode active material 10 is 3.0% by mass or less. If the content of LiBOB in the negative electrode active material 10 exceeds 3.0% by mass, the formation of a coating film becomes excessive, and the electronic conductivity between the negative electrode active materials 10 may be reduced. The content of LiBOB in the negative electrode active material 10 is preferably 2.0% by mass or less. If the content of LiBOB in the negative electrode active material 10 is small, the effect of containing LiBOB may not be exhibited. Therefore, the content of LiBOB in the negative electrode active material 10 may be, for example, 0.1% by mass or more, or 0.2% by mass or more.

[0028] <Lithium-ion battery> 4 is a schematic diagram showing an example of a lithium ion battery of this embodiment. The battery 100 includes a case 90. The case 90 has any shape. The case 90 may be, for example, rectangular or cylindrical. The case 90 may be, for example, made of metal, or may be a pouch made of an aluminum (Al) laminate film. A positive electrode terminal 91 and a negative electrode terminal 92 may be provided on the case 90.

[0029] The case 90 houses the electrode assembly 50 and an electrolyte. The electrolyte is impregnated in the electrode assembly 50. The electrode assembly 50 is connected to a positive electrode terminal 91 and a negative electrode terminal 92.

[0030] FIG. 5 is a schematic diagram showing an example of an electrode body of this embodiment. The electrode body 50 includes a positive electrode 20, a separator 40, and a negative electrode 30. The electrode body 50 has an arbitrary structure. For example, the electrode body 50 may be a wound type. The positive electrode 20, the separator 40, and the negative electrode 120 may all be strip-shaped sheets. The electrode body 50 may be formed, for example, by laminating the positive electrode 20, the separator 40 (first sheet), the negative electrode 30, and the separator 40 (second sheet) in this order. After winding, the electrode body 50 may be formed into a flat shape.

[0031] 《Negative electrode》 The negative electrode 30 may include a negative electrode current collector and a negative electrode active material layer. The negative electrode current collector may include, for example, copper (Cu) foil, etc. The negative electrode active material layer may further include, for example, a conductive material, a binder, etc.

[0032] The conductive material may include, for example, carbon nanotubes (CNTs), etc. The binder may include, for example, polyvinylidene fluoride (PVdF), etc. The blending amounts of the conductive material and the binder may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the negative electrode active material.

[0033] 《Positive electrode》 The positive electrode 20 may include a positive electrode current collector and a positive electrode active material layer. The positive electrode current collector may include, for example, aluminum (Al) foil or the like. The positive electrode active material layer includes a positive electrode active material. The positive electrode active material layer may further include, for example, a conductive material, a binder, or the like.

[0034] The positive electrode active material may be, for example, particulate. The positive electrode active material may have, for example, a D50 of 1 to 30 μm. The positive electrode active material may include, for example, at least one selected from the group consisting of LiCoO2, LiNiO2, LiMnO2, Li(NiCoMn)O2, and Li(NiCoAl)O2. For example, "(NiCoMn)" in "Li(NiCoMn)O2" indicates that the sum of the composition ratios in parentheses is 1. As long as the sum is 1, the amount of each component is arbitrary.

[0035] The conductive material may include, for example, acetylene black (AB), etc. The binder may include, for example, PVdF, etc. The blending amount of the conductive material and the binder may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the positive electrode active material.

[0036] <Separator> The separator 40 is porous. The separator 40 is permeable to an electrolyte. The separator 40 separates the positive electrode 20 and the negative electrode 30. The separator 40 is electrically insulating. The separator 40 may contain, for example, a polyolefin resin such as polyethylene (PE) or polypropylene (PP). The separator 40 may have, for example, a single-layer structure or a multi-layer structure. The separator 40 may be substantially composed of a PE layer, or may be formed by laminating a PP layer, a PE layer, and a PP layer in this order. For example, a heat-resistant layer may be formed on the surface of the separator 40. The heat-resistant layer may contain, for example, a heat-resistant material such as boehmite or alumina.

[0037] 《Electrolyte》 The electrolyte includes a solvent, a Li salt, and LiBOB. The electrolyte may further include an optional additive. The solvent is aprotic. The solvent may include an optional component. The solvent may include at least one selected from the group consisting of, for example, ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC).

[0038] The Li salt is a supporting electrolyte. The Li salt is dissolved in a solvent. The Li salt may include at least one selected from the group consisting of LiPF6 and LiBF4. The Li salt may have a molar concentration of, for example, 0.5 to 2.0 mol / L (hereinafter, mol / L may also be simply referred to as "M").

[0039] LiBOB is dissolved in a solvent. LiBOB preferably has a molar concentration of 0.01 to 0.1 M. When the molar concentration of LiBOB is 0.01 to 0.1 M, it is believed that the formation of a coating derived from LiBOB is further promoted, improving cycle characteristics.

[0040] <Method of manufacturing negative electrode active material> The method for producing the negative electrode active material of this embodiment includes "(A) Formation of first particles" and "(B) Formation of the negative electrode active material".

[0041] (A) Formation of the first particle The graphite is coated with an amorphous carbon film to form a first particle. The graphite is prepared. The graphite may be artificial graphite or natural graphite.

[0042] For example, pitch is prepared. Graphite and pitch are mixed. The mixture is heat-treated (calcined). The calcination temperature may be, for example, 800°C to 1000°C. The calcination time may be, for example, 30 minutes or more and 2 hours or less. The calcination causes a decomposition reaction of the pitch to proceed. As a result, the graphite is coated with an amorphous carbon film, and first particles are formed.

[0043] (B) Formation of negative electrode active material The negative electrode active material is formed by agglomeration (granulation) of the first particles and mixing of the second particles. The aggregation of the first particles and mixing of the second particles are preferably carried out simultaneously. By carrying out the aggregation and mixing of the second particles simultaneously, the second particles are easily dispersed inside the composite particles.

[0044] The second particles containing LiBOB are prepared. Any mixing device, granulator, etc. may be used. For example, the first particles and the second particles are put into a granulator. The rotation speed of the granulator may be, for example, 1000 rpm or more and 10000 rpm or less. The granulation time may be, for example, 30 minutes or more and 2 hours or less. This forms a negative electrode active material. EXAMPLES

[0045] The present embodiment will be described below using examples, but the present embodiment is not limited to these.

[0046] Example 1 (Negative electrode active material) Natural graphite was prepared as the graphite, and coal tar pitch was prepared as the pitch. The graphite and coal tar pitch were mixed so that the mass of the coal tar pitch was 5.0 mass% relative to the graphite. The mixture was fired at 1000°C for 1 hour to produce first particles in which an amorphous carbon film was formed on the graphite. The D50 of the first particles was 15 μm.

[0047] LiBOB particles (D50: 2 μm) were prepared as the second particles. An "MP Mixer" manufactured by Nippon Coke & Engineering Co., Ltd. was prepared as a granulator. The first particles and LiBOB particles were fed into the granulator. The LiBOB particles were fed so that their content in the negative electrode active material was 0.2 mass %. The mixture was granulated at 5000 rpm for 1 hour to produce the negative electrode active material. It was confirmed by the above-mentioned method that the LiBOB particles were dispersed inside the negative electrode active material.

[0048] (Negative electrode) A Cu foil (thickness: 10 μm) was prepared as the negative electrode current collector, PVdF as the binder, and N-methyl-2-pyrrolidone (NMP) as the dispersion medium. The negative electrode active material, the binder, and the dispersion medium were mixed to prepare a negative electrode slurry. The mixing ratio (mass ratio) of the negative electrode active material to the binder was 92:8. The negative electrode slurry was applied to the surface of the negative electrode current collector and dried to form a negative electrode active material layer. The negative electrode active material layer was compressed to produce a negative electrode.

[0049] (positive electrode) The positive electrode current collector was made of Al foil (thickness: 15 μm), and the positive electrode active material was Li(Ni 1 / 3 Co 1 / 3 Mn 1 / 3 )O2 was prepared, AB was prepared as a conductive material, PVdF was prepared as a binder, and NMP was prepared as a dispersion medium. The positive electrode active material, the conductive material, the binder, and the dispersion medium were mixed to prepare a positive electrode slurry. The mixture ratio (mass ratio) of the positive electrode active material, the conductive material, and the binder was 92:5:3. The positive electrode slurry was applied to the surface of a positive electrode current collector and dried to form a positive electrode active material layer. The positive electrode active material layer was compressed to manufacture a positive electrode.

[0050] (Separator) A separator (porous membrane) with a thickness of 24 μm was prepared. This separator has a three-layer structure. The three-layer structure is composed of a PP porous layer, a PE porous layer, and a PP porous layer laminated in this order. Alumina (thickness: 4 μm) is applied to one side of the separator as a heat-resistant material.

[0051] (electrolyte) A mixed solvent was prepared by mixing EC, DMC, and EMC. The mixing ratio (volume ratio) of EC, DMC, and EMC was 3:3:4. An electrolyte was prepared by dissolving LiPF6 and LiBOB in the solvent. LiPF6 and LiBOB were dissolved so that their concentrations in the electrolyte were 1.0M and 0.05M, respectively.

[0052] (Lithium-ion battery) The electrode body was formed by stacking the positive electrode, separator, and negative electrode in this order. The separator was stacked so that the alumina-coated surface of the separator faced the positive electrode. A pouch made of laminated film was prepared as a case. The electrode body was stored in the case. An electrolyte was injected into the case. After the electrolyte was injected, the case was sealed. After an interval of 3 hours or more, the initial charge was performed, and then aging was performed for 20 hours in an environment at 60°C, thereby producing the battery of Example 1. Note that "aging" refers to storing the battery for a predetermined period of time in a temperature environment above room temperature.

[0053] Examples 2 to 4 Except for the fact that the content of LiBOB particles in the negative electrode active material was adjusted to 0.8 mass%, 1.5 mass%, and 3.0 mass%, respectively, the negative electrode active materials were produced in the same manner as in Example 1. Then, the batteries of Examples 2 to 4 were produced in the same manner as in Example 1.

[0054] Comparative Example 1 Except for not using LiBOB particles, a negative electrode active material was prepared in the same manner as in Example 1. Then, a battery of Comparative Example 1 was prepared in the same manner as in Example 1.

[0055] Comparative Example 2 Except for the fact that the content of LiBOB particles in the negative electrode active material was adjusted to 3.5 mass %, a negative electrode active material was produced in the same manner as in Example 1. Then, a battery of Comparative Example 2 was produced in the same manner as in Example 1.

[0056] Comparative Example 3 A negative electrode active material was prepared in the same manner as in Example 1, except that LiBOB particles were not used. A battery of Comparative Example 3 was prepared in the same manner as in Example 1, except that LiBOB was dissolved in the electrolyte.

[0057] <Evaluation> Each battery was charged and discharged at 60°C, with an SOC (state of charge) of 0 to 100%, and at a rate of 2C, and the capacity was measured after 1 charge / discharge cycle and after 300 cycles. The capacity after 300 cycles was divided by the capacity after 1 cycle to measure the capacity retention rate (cycle characteristics). The results are shown in Table 1. Note that "C" is the unit of current rate. "1C" indicates the current rate at which the SOC reaches 100% from 0% by charging for 1 hour.

[0058] [Table 1]

[0059] <Result> Examples 1 to 4, which contained LiBOB particles, showed improved cycle characteristics compared to Comparative Example 1, which did not contain LiBOB particles.

[0060] On the other hand, in Comparative Example 2, in which the content of LiBOB particles was high, the cycle characteristics were deteriorated compared to Examples 1 to 4. It is considered that when the content of LiBOB particles was high, the coating was excessively formed, which deteriorated the cycle characteristics.

[0061] The present embodiment and the present embodiment are illustrative in all respects. The present embodiment and the present embodiment are not restrictive. The technical scope of the present disclosure includes all modifications within the meaning and scope equivalent to the description of the claims. For example, it is also intended from the beginning that any configuration may be extracted from the present embodiment and the present embodiment, and that they may be arbitrarily combined. [Explanation of symbols]

[0062] 10 negative electrode active material, 11 first particle, 12 second particle, 13 graphite, 14 amorphous carbon film, 15 composite particle, 20 positive electrode, 30 negative electrode, 40 separator, 50 electrode body, 90 case, 91 positive electrode terminal, 92 negative electrode terminal, 100 all-solid-state battery.

Claims

1. A negative electrode active material for a lithium ion battery, comprising: comprising a first particle and a second particle, the first particles include graphite and an amorphous carbon film coating the graphite, the second particles include lithium bis(oxalato)borate; the first particles are aggregated to form composite particles, At least a portion of the second particles is dispersed inside the composite particles, The negative electrode active material has a lithium bis(oxalato)borate content of 3.0% by mass or less.

2. The negative electrode active material according to claim 1 , wherein the first particles have an average particle size of 1.0 μm or more and 30 μm or less.

3. A battery comprising: a negative electrode containing the negative electrode active material according to claim 1 or 2; a positive electrode; a separator; and an electrolyte solution; The lithium ion battery, wherein the electrolyte contains lithium bis(oxalato)borate.

4. A negative electrode active material for a lithium ion battery, comprising: comprising a first particle and a second particle, the first particles include graphite and an amorphous carbon film coating the graphite, the second particles include lithium bis(oxalato)borate; the first particles are aggregated to form composite particles, At least a portion of the second particles is dispersed inside the composite particles, The content of lithium bis(oxalato)borate in the negative electrode active material is 0.2% by mass or more and 2.0% by mass or less, The first particles have an average particle size of 5.0 μm or more and 20 μm or less.

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery manufacturing method therefor

    JP2014056667A

  • Nonaqueous electrolyte secondary battery and manufacturing method of the nonaqueous electrolyte secondary battery

    JP2019149348A

  • Negative electrode active material for lithium secondary battery, manufacturing method thereof, negative electrode including the same, and lithium secondary battery including the same

    JP2020043069A

  • Method for manufacturing a lithium secondary battery having a protected high-capacity anode active material

    JP2020507904A

  • Method for manufacturing electrode, method for manufacturing nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery

    JP2022100539A