Composite structure, precursor of multilayer ceramic electronic component, method for manufacturing precursor of multilayer ceramic electronic component, and method for manufacturing multilayer ceramic electronic component

JP7582344B2Active Publication Date: 2024-11-13MURATA MFG CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022579371
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-02
Filing Date
2021-12-13
Publication Date
2024-11-13
Estimated Expiration
2041-12-13

AI Technical Summary

Benefits of technology

【0010】 本発明によれば、脂肪族ポリカーボネートと無機粒子とを含む構造体を含む複合構造体であって、脂肪族ポリカーボネートと無機粒子とを含む構造体と接触する他の構造体とが両者の界面において外力により剥離しにくい複合構造体と、前述の複合構造体を含む積層セラミック電子部品前駆体と、前述の積層セラミック電子部品前駆体の製造方法と、前述の積層セラミック電子部品前駆体の製造方法を含む、積層セラミック電子部品の製造方法とを提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582344000001
    Figure 0007582344000001
Patent Text Reader

Abstract

The present invention provides: a composite structure including structures that contain an aliphatic polycarbonate and inorganic particles, wherein a structure that includes an aliphatic polycarbonate and inorganic particles, and another structure that makes contact with said structure, are not readily detached from each other by external force at the interface therebetween; a layered ceramic electronic component precursor that includes the composite structure; a method for manufacturing the layered ceramic electronic component precursor; and a method for manufacturing a layered ceramic electronic component that includes the method for manufacturing the layered ceramic electronic component precursor. Provided is a composite structure including structures that contain an aliphatic polycarbonate and inorganic particles, wherein a composite is obtained from a first structure that contains an aliphatic polycarbonate and first inorganic particles, and a second structure that contains a branched polymer and second inorganic particles. In the polymer used as the branched polymer, the molecular chains have a main chain comprising a cellulose-based polymer, and a branch chain comprising the aliphatic polycarbonate or an aliphatic polyester.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite structure including a structure containing an aliphatic polycarbonate and inorganic particles, a multilayer ceramic electronic component precursor including the above-mentioned composite structure, a method for producing the above-mentioned multilayer ceramic electronic component precursor, and a method for producing a multilayer ceramic electronic component including the above-mentioned method for producing the multilayer ceramic electronic component precursor. [Background technology]

[0002] Conventionally, structures in which inorganic particles are dispersed in an aliphatic polycarbonate have been used for various purposes. Such structures are composited with structures containing a resin other than an aliphatic polycarbonate and inorganic particles for various purposes, and used as composite structures.

[0003] For example, Patent Document 1 proposes using an aliphatic polycarbonate, which has excellent thermal decomposition properties, as a binder for dispersing ceramic particles in a composition for molding a sintered ceramic. Patent Document 2 also proposes the use of ethyl cellulose as a component for dispersing conductive powder such as metal particles in a conductive paste for forming an internal electrode layer formed on a dielectric layer, which is a sintered ceramic in a multilayer ceramic capacitor. Ethyl cellulose imparts good printing characteristics and excellent dispersibility stability of the conductive powder to the conductive paste described in Patent Document 2. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2011-020916 A [Patent Document 2] JP 2018-168238 A Summary of the Invention [Problem to be solved by the invention]

[0005] For example, when a sheet-like layer made of a sintered ceramic molding composition as described in Patent Document 1 and a sheet-like layer made of a conductive paste as described in Patent Document 2 are laminated and combined, a laminate that provides a multilayer ceramic electronic component by firing is obtained. Such a laminate is often cut by a method such as press cutting according to the size of the multilayer ceramic electronic component to be manufactured, and then fired in a small divided state.

[0006] However, the aliphatic polyester contained in the composition for molding a sintered ceramic does not necessarily have good adhesion to other types of resins. Therefore, when a laminate in which a sheet-like layer made of the composition for molding a sintered ceramic as described in Patent Document 1 and a sheet-like layer made of a conductive paste as described in Patent Document 2 are laminated is cut by applying an external force by a method such as a push-cutting method, there is a problem that the layers are likely to peel off due to insufficient adhesion between the layers.

[0007] The present invention has been made in view of the above-mentioned problems, and has an object to provide a composite structure including a structure containing an aliphatic polycarbonate and inorganic particles, wherein the composite structure is unlikely to peel off due to an external force at the interface between the structure containing an aliphatic polycarbonate and inorganic particles and another structure in contact with the structure containing the aliphatic polycarbonate and the inorganic particles; a laminated ceramic electronic component precursor including the above-mentioned composite structure; a method for manufacturing the above-mentioned laminated ceramic electronic component precursor; and a method for manufacturing a laminated ceramic electronic component including the above-mentioned method for manufacturing the laminated ceramic electronic component precursor. [Means for solving the problem]

[0008] The present inventors have found that the above problems can be solved by combining a first structure containing an aliphatic polycarbonate and a first inorganic particle with a second structure containing a branched polymer and a second inorganic particle in a composite structure containing an aliphatic polycarbonate and a first inorganic particle, and using a polymer whose molecular chain has a main chain made of a cellulose-based polymer and a branch chain made of an aliphatic polycarbonate or an aliphatic polyester as the branched polymer, and have completed the present invention. More specifically, the present invention provides the following (1) to (6).

[0009] (1) A composite structure including a first structure and a second structure, The first structure and the second structure are in contact with each other, the first structure comprises an aliphatic polycarbonate and first inorganic particles; the second structure includes a branched polymer and a second inorganic particle; the molecular chain of the branched polymer has a main chain made of a cellulose-based polymer and a branch chain made of an aliphatic polycarbonate or an aliphatic polyester; The branched chain may be linear or branched. A branch may be attached to two or more backbones to cross-link two or more backbones, a composite structure. (2) A sheet-like first structure and a sheet-like second structure are repeatedly and alternately laminated, the first structure contains metal particles and ceramic particles as the first inorganic particles; The second structure contains ceramic particles as the second inorganic particles, and may contain metal particles; In the first structure, the volume of the metal particles is larger than the volume of the ceramic particles, 3. The composite structure according to claim 1, wherein in the second structure, the volume of the ceramic particles is greater than the volume of the metal particles. (3) A sheet-like first structure and a sheet-like second structure are repeatedly and alternately laminated, The first structure contains ceramic particles as the first inorganic particles, and may contain metal particles; the second structure contains metal particles and ceramic particles as the second inorganic particles, In the first structure, the volume of the ceramic particles is larger than the volume of the metal particles; 2. The composite structure according to claim 1, wherein in the second structure, the volume of the metal particles is greater than the volume of the ceramic particles. (4) A precursor of a multilayer ceramic electronic component, comprising the composite structure according to (2) or (3). (5) A method for producing a precursor of a multilayer ceramic electronic component, comprising cutting the composite structure according to (2) or (3) in a direction perpendicular or approximately perpendicular to a plane direction of the composite structure. (6) Producing a precursor of a multilayer ceramic electronic component by the method according to (5); and firing the multilayer ceramic electronic component precursor. Effect of the Invention

[0010] According to the present invention, it is possible to provide a composite structure including a structure containing an aliphatic polycarbonate and inorganic particles, wherein the composite structure includes an aliphatic polycarbonate and inorganic particles and another structure in contact with the structure is not easily peeled off due to an external force at the interface between the two structures, a precursor for a multilayer ceramic electronic component including the above-mentioned composite structure, a method for manufacturing the precursor for a multilayer ceramic electronic component, and a method for manufacturing a multilayer ceramic electronic component including the method for manufacturing the precursor for a multilayer ceramic electronic component. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] ≪Composite structure≫ The composite structure includes a first structure and a second structure, the first structure and the second structure being in contact with each other. The first structure includes an aliphatic polycarbonate and first inorganic particles. The second structure includes a branched polymer and second inorganic particles. The molecular chain of the branched polymer has a main chain made of a cellulose-based polymer and a branch chain made of an aliphatic polycarbonate or an aliphatic polyester. The branch chain may be linear or branched. The branch chain may be bonded to two or more of the main chains to crosslink the two or more main chains.

[0012] The first structure contains an aliphatic polycarbonate, and the second structure contains a branched polymer having a main chain made of an aliphatic polycarbonate or an aliphatic polyester, so that the first structure and the second structure are well adhered to each other. This is because the aliphatic polycarbonate and the branched polymer show high affinity based on the similarity of their chemical structures. Therefore, when an external force is applied to the composite structure, peeling is unlikely to occur at the interface where the first structure and the second structure come into contact with each other.

[0013] The shape, structure, and size of the first structure and the second structure constituting the composite structure are not particularly limited, so long as the first structure and the second structure can be composited in a contact state. The shapes of the first structural body and the second structural body can be a sheet, a prismatic shape, a cylindrical shape, etc. Prismatic shapes include rectangular parallelepiped shapes, cube shapes, triangular shapes, pentagonal prism shapes, etc. The first structure and the second structure may have a three-dimensional shape that allows them to be fitted together so that their contact surfaces are in close contact with each other.

[0014] When the composite structure is composed of a sheet-like first structure and a sheet-like second structure, it is preferable that the composite structure is a laminate in which the first structure and the second structure are laminated. As described above, the first structure and the second structure are well adhered to each other, and therefore, in this laminate, even if an external force is applied to the laminate, delamination is unlikely to occur.

[0015] Preferable examples of the composite structure that is a laminate include: A sheet-like first structure and a sheet-like second structure are repeatedly and alternately laminated, the first structure contains metal particles and ceramic particles as the first inorganic particles; The second structure contains ceramic particles as the second inorganic particles, and may contain metal particles; In the first structure, the volume of the metal particles is larger than the volume of the ceramic particles, The second structure includes a composite structure in which the volume of the ceramic particles is greater than the volume of the metal particles.

[0016] Other preferred examples of the composite structure that is a laminate include: A sheet-like first structure and a sheet-like second structure are repeatedly and alternately laminated, The first structure contains ceramic particles as the first inorganic particles, and may contain metal particles; the second structure contains metal particles and ceramic particles as the second inorganic particles, In the first structure, the volume of the ceramic particles is larger than the volume of the metal particles; The second structure includes a composite structure in which the volume of the metal particles is greater than the volume of the ceramic particles.

[0017] In the above composite structure which is a laminate, the ceramic particles as inorganic particles and the metal particles contained in the first structure and the second structure will be described later as components of the first structure and the second structure.

[0018] The composite structure described above can be suitably used for manufacturing multilayer ceramic electronic components. Examples of the multilayer ceramic electronic components include multilayer ceramic capacitors, inductors, piezoelectric elements, thermistors, etc. In multilayer ceramic electronic components such as multilayer ceramic capacitors, typically, dielectric layers and internal electrode layers are repeatedly and alternately laminated.

[0019] For example, when the multilayer ceramic electronic component is a multilayer ceramic capacitor, the thickness of the laminated dielectric layers is preferably 1.0 μm or less, more preferably 0.4 μm or less. The thickness of the laminated dielectric layers is preferably 0.15 μm or more. The thickness of the laminated dielectric layers is preferably 0.15 μm or more and 1.0 μm or less, more preferably 0.15 μm or more and 0.4 μm or less. In a composite structure as a laminate that is suitably used for producing a multilayer ceramic electronic component, the total number of dielectric layers is preferably 15 or more and 700 or less.

[0020] In the above composite structure, the sheet-like second structure containing ceramic particles and optionally containing metal particles as the second inorganic particles, or the sheet-like first structure containing ceramic particles and optionally containing metal particles as the first inorganic particles, is rich in ceramic particles, which are dielectric, and provides a dielectric layer when fired.

[0021] The second structure providing the dielectric layer and the first structure may contain additives, as described below. The content of the ceramic particles in the second structure that provides the dielectric layer is preferably 45 vol% or more and 70 vol% or less, and more preferably 55 vol% or more and 65 vol% or less, based on the total volume of the branched polymer contained in the second structure, the volume of the second inorganic particles, and the volume of the additive. The content of the ceramic particles in the first structure that provides the dielectric layer is preferably 45 volume % or more and 70 volume % or less, and more preferably 55 volume % or more and 65 volume % or less, based on the total volume of the aliphatic polycarbonate contained in the first structure, the volume of the first inorganic particles, and the volume of the additive. The volume may be calculated from the area of ​​each particle by observing the cross section of the center of the structure.

[0022] The sheet-like second structure or the sheet-like first structure that provides the dielectric layer is a so-called green sheet. The sheet-like second structure or the sheet-like first structure is typically formed by a known method such as a die coater sheet method or a doctor blade method using a paste for forming the second structure described later or a paste for forming the first structure described later. The film made of the molded paste is preferably dried. The thickness of the sheet-like second structure or the sheet-like first structure, which is a so-called green sheet, after molding and drying is preferably 4 μm or less, more preferably 3 μm or less.

[0023] When the multilayer ceramic electronic component is a multilayer ceramic capacitor, the thickness of the laminated internal electrode layers is preferably 0.20 μm or more and 1.0 μm or less, and more preferably 0.20 μm or more and 0.80 μm or less. In a composite structure as a laminate that is suitably used for manufacturing a multilayer ceramic electronic component, the total number of internal electrode layers is preferably 15 or more and 700 or less.

[0024] In the above composite structure, the sheet-like first structure containing metal particles and ceramic particles as the first inorganic particles, or the sheet-like second structure containing metal particles and ceramic particles as the second inorganic particles, is rich in metal particles and provides an internal electrode layer when fired. From the viewpoints of dispersibility and dispersion stability of metal particles, the structure providing the internal electrode layer is preferably the second structure containing a branched polymer described below.

[0025] The first structure providing the internal electrode layers and the second structure may contain additives, as described below. The content of the metal particles in the first structure that provides the internal electrode layer is preferably 50 volume % or more and 75 volume % or less, and more preferably 60 volume % or more and 70 volume % or less, based on the total volume of the aliphatic polycarbonate contained in the first structure, the volume of the first inorganic particles, and the volume of the additive. The content of the metal particles in the second structure that provides the internal electrode layer is preferably 50 vol% or more and 75 vol% or less, and more preferably 60 vol% or more and 70 vol% or less, based on the total volume of the branched polymer, the second inorganic particles, and the additive contained in the second structure. The volume may be calculated from the area of ​​each particle by observing the cross section of the center of the structure.

[0026] The content of the ceramic particles in the first structure that provides the internal electrode layer is preferably 3 volume % or more and 15 volume % or less, and more preferably 5 volume % or more and 10.5 volume % or less, based on the total volume of the aliphatic polycarbonate contained in the first structure, the volume of the first inorganic particles, and the volume of the additive. The content of the ceramic particles in the second structure that provides the internal electrode layers is preferably 3 vol% or more and 15 vol% or less, and more preferably 5 vol% or more and 10.5 vol% or less, based on the total volume of the branched polymer, the second inorganic particles, and the additive contained in the second structure.

[0027] The sheet-like first structure or the sheet-like second structure that provides the internal electrode layer is typically formed on the second structure or the first structure as a green sheet that provides the dielectric layer by a printing method such as gravure printing or screen printing using a paste for forming the second structure described later or a paste for forming the first structure described later. The thickness of the sheet-like first structure or the sheet-like second structure that provides the internal electrode layer after printing and drying is preferably, for example, 1.5 μm or less.

[0028] The shape of the internal electrode layer is not particularly limited. The shape of the internal electrode layer is preferably rectangular when the internal electrode layer is observed from a direction perpendicular to the surface direction of the internal electrode layer, and may be a coil shape or the like. The shape of the sheet-like first structure or the sheet-like second structure that provides the internal electrode layer is adopted to correspond to the shape of the internal electrode layer to be formed.

[0029] A multiplicity of two-layer laminates having layers providing internal electrode layers as the second structure or the first structure are laminated and pressed onto the green sheets of the first structure or the second structure thus formed, to obtain a laminate that can be suitably used as a precursor of a multilayer ceramic electronic component. Pressing may be performed by a method such as isostatic pressing.

[0030] A multilayer ceramic electronic component can be manufactured by firing the above-mentioned composite structure, which is a laminate, itself, and then adding a configuration corresponding to the type of multilayer ceramic electronic component to the fired laminate, or by firing a laminate in which a configuration corresponding to the type of multilayer ceramic electronic component has been added to the above-mentioned composite structure, which is a laminate. In other words, a multilayer ceramic electronic component precursor including the above-mentioned composite structure, which is a laminate, can be suitably used for producing a multilayer ceramic electronic component.

[0031] The multilayer ceramic electronic component is preferably manufactured by the following method. First, a laminate is formed by stacking sheet-like structures that provide dielectric layers and sheet-like structures that provide internal electrode layers. Next, the obtained laminate is cut perpendicularly or approximately perpendicularly to the surface direction of the laminate by a method such as press cutting to form a laminate block of a desired size. Thereafter, the obtained laminate block is subjected to well-known processing including firing, to manufacture a multilayer ceramic electronic component. Such a laminate block, or a laminate block that has been subjected to well-known processing, also corresponds to a precursor of a multilayer ceramic electronic component.

[0032] When cutting a composite structure that is a laminate, delamination is likely to occur due to shear force applied to the cut surface, etc. However, a laminate structure in which a first structure containing an aliphatic polycarbonate and a second structure containing a branched polymer having a specific structure are laminated together is unlikely to undergo delamination near the cut surface even when cut by a method such as push cutting.

[0033] The first structure and the second structure will be described below.

[0034] <First structure> As described above, the first structure includes an aliphatic polycarbonate and the first inorganic particles. The first structure may include other components than the aliphatic polycarbonate and the first inorganic particles as long as the desired effect is not impaired. Components that the first structure may contain and a method for forming the first structure will be described below.

[0035] [Aliphatic polycarbonate] The aliphatic polycarbonate is not particularly limited as long as it can form the first structure. Conventionally known aliphatic polycarbonates can be used as a component of the first structure. Examples of the aliphatic polycarbonate include those represented by the following formula (1): -(-O-CO-O-CR 1 R 2 -CR 3 R 4 -)-···(1) Examples of the resin include a resin composed of a structural unit represented by the following formula:

[0036] In formula (1), R 1 , R 2 , R 3 , and R 4 R is independently a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent. 1 , R 2 , R 3 , and R 4 At least two of the above may be bonded to form an aliphatic ring having 3 to 10 ring atoms.

[0037] R 1 , R 2 , R 3 , and R 4 The structure of the alkyl group, which may have a substituent, as R may be linear or branched. 1 , R 2 , R 3 , and R 4The number of carbon atoms in the alkyl group which may have a substituent as the substituent is preferably 1 or more and 4 or less, and more preferably 1 or 2. The number of carbon atoms in the substituent is not included in the number of carbon atoms in the alkyl group.

[0038] R 1 , R 2 , R 3 , and R 4 Specific examples of the alkyl group as the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, and an n-decyl group.

[0039] R 1 , R 2 , R 3 , and R 4 When the alkyl group has a substituent, the number of the substituents bonded to the alkyl group is not particularly limited as long as the desired effect is not impaired. The number of the substituents bonded to the alkyl group is preferably 1 or 2.

[0040] R 1 , R 2 , R 3 , and R 4 Specific examples of the substituent that the alkyl group which may have a substituent as the substituent include a hydroxyl group, an alkoxy group, an ester group, a silyl group, a sulfanyl group, a cyano group, a nitro group, a sulfo group, a formyl group, a carboxy group, and a halogen atom.

[0041] The number of carbon atoms of the alkoxy group as a substituent is not particularly limited, but is, for example, preferably from 1 to 4, more preferably 1 or 2. Specific preferred examples of the alkoxy group as a substituent include a methoxy group, an ethoxy group, an n-propyloxy group, an isopropyloxy group, an n-butyloxy group, an isobutyloxy group, a sec-butyloxy group, and a tert-butyloxy group.

[0042] Preferable specific examples of the halogen atom as the substituent include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.

[0043] R 1 , R 2 , R 3 , and R 4 may contain one or more groups. For example, R 1 , R 2 , R 3 , and R 4 may be the same group. 1 , R 2 , and R 3 are the same group, and R 4 But R 1 , R 2 , and R 3 R 1 , R 3 , and R 4 are the same group, and R 2 But R 1 , R 3 , and R 4 R 1 , R 2 , R 3 , and R 4 may be four different groups.

[0044] R 1 , R 2 , R 3 , and R 4 At least two of the above may be bonded to form an aliphatic ring having 3 to 10 ring-constituting atoms. The aliphatic ring may be a saturated aliphatic ring or an unsaturated aliphatic ring. The aliphatic ring may have a substituent. The number of the substituents that the aliphatic ring may have is not particularly limited as long as the desired effect is not impaired. When the aliphatic ring has a substituent, the number of the substituents is preferably 1 or 2.

[0045] Specific examples of the aliphatic ring include a cyclopentane ring, a cyclopentene ring, a cyclohexane ring, a cyclohexene ring, and a cycloheptane ring.

[0046] The aliphatic ring may have a substituent such as an alkyl group, an alkoxy group, an acyloxy group, an alkoxycarbonyl group, a silyl group, a sulfanyl group, a cyano group, a nitro group, a sulfo group, a formyl group, or a halogen atom. Specific examples of the alkyl group as a substituent include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group. Specific examples of the alkoxy group as a substituent include a methoxy group, an ethoxy group, an n-propyloxy group, an isopropyloxy group, an n-butyloxy group, an isobutyloxy group, a sec-butyloxy group, and a tert-butyloxy group. Specific examples of the acyloxy group as a substituent include an acetoxy group, a propionyloxy group, a butanoyloxy group, an isobutanoyloxy group, and a pivaloyloxy group. Specific examples of the alkoxycarbonyl group as a substituent include a methoxycarbonyl group, an ethoxycarbonyl group, and a tert-butoxycarbonyl group. Specific examples of the halogen atom as a substituent include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.

[0047] In addition to the aliphatic polycarbonate consisting of the structural unit represented by the above formula (1), polytrimethylene carbonate, polytetramethylene carbonate, polyhexamethylene carbonate, poly-2,2-dimethyltrimethylene carbonate, poly-1,4-cyclohexanedimethylene carbonate, and the like can be suitably used as the aliphatic polycarbonate.

[0048] Among the aliphatic polycarbonates described above, polyethylene carbonate, polypropylene carbonate, polytriethylene carbonate, and polytetramethylene carbonate are preferred, polypropylene carbonate and polytetramethylene carbonate are more preferred, and polypropylene carbonate is even more preferred.

[0049] The composite structure may be fired. When the preferred aliphatic polycarbonates are used, the residue after pyrolysis by firing is small, and the first structure having a desired shape can be easily formed. In addition, these aliphatic polycarbonates have excellent affinity with the first inorganic particles.

[0050] The aliphatic polycarbonates may be used alone or in combination of two or more.

[0051] The end groups of the aliphatic polycarbonate may be modified to the extent that the desired effects are not impaired. Examples of the modification of the end groups include modification with an acid anhydride, a cyclic acid anhydride, an acid halide, an isocyanate compound, and the like.

[0052] As long as the desired effect is not impaired, the aliphatic polycarbonate may partially contain other structural units than the polycarbonate structural units, such as polyether structural units, polyester structural units, polyamide structural units, and polyacrylate structural units. The content of other structural units in the aliphatic polycarbonate is preferably 10 mol % or less, more preferably 5 mol % or less, even more preferably 3 mol % or less, and particularly preferably 1 mol % or less, based on the number of moles of all structural units of the aliphatic polycarbonate.

[0053] [First inorganic particles] The first structure includes first inorganic particles. As the first inorganic particles, any inorganic particles that have been conventionally added to various resin compositions can be used without any particular limitation. Typically, the first inorganic particles are preferably ceramic particles and / or metal particles.

[0054] As described above, a suitable example of the composite structure is a laminate useful as a precursor of a multilayer ceramic electronic component. When the first structure is a green sheet that provides a dielectric layer in the multilayer ceramic electronic component, or when the first structure is a conductive sheet made of a conductive paste that provides an internal electrode layer in the multilayer ceramic electronic component, the ceramic particles are useful as a component of the first structure. The ceramic particles preferably contain at least one material selected from the group consisting of Ba, Ti, Sr, Ca, and Zr. Preferable specific examples of the ceramic particles include barium titanate particles, calcium titanate particles, strontium titanate particles, and lead zirconate titanate particles. As the ceramic particles, one type may be used alone, or two or more types may be used in combination.

[0055] When the first structure is a conductive sheet made of a conductive paste that provides an internal electrode layer in a multilayer ceramic electronic component, metal particles as the first inorganic particles are useful as a constituent component of the first structure. The metal constituting the metal particles is preferably at least one selected from the group consisting of Ni, Cu, Ag, Pt, and Au. The metal particles may contain two or more kinds of metal particles. The metal particles may be particles of an alloy containing two or more kinds of metals.

[0056] The content of the first inorganic particles in the first structure is not particularly limited. The content of the first inorganic particles in the first structure is appropriately determined in consideration of the use of the composite structure and the composition of the second structure. The content of the first inorganic particles is typically preferably 5% by volume or more and 95% by volume or less, more preferably 10% by volume or more and 90% by volume or less, based on the volume of the first structure.

[0057] [Plasticizer] The first structure may contain a plasticizer in addition to the aliphatic polycarbonate and the first inorganic particles in order to improve the processability of the composite structure. Specific examples of suitable plasticizers include phthalic acid-based plasticizers such as dimethyl phthalate, diethyl phthalate, n-dibutyl phthalate, dibutyl benzyl phthalate, and alkyl butyl benzyl phthalate; glycol-based plasticizers such as diethylene glycol dibenzoate, dipropylene glycol dibenzoate, and polyethylene glycol; phosphoric acid-based plasticizers such as tricresyl phosphate, tributoxyethyl phosphate, 2-ethylhexyl diphenyl phosphate, and isodecyl diphenyl phosphate; citric acid-based plasticizers such as triethyl O-acetyl citrate and tributyl O-acetyl citrate; adipic acid-based plasticizers such as dibutyl adipate and dihexyl adipate; carbonate-based plasticizers such as ethylene carbonate and propylene carbonate; and epoxy-based plasticizers such as epoxidized soybean oil and epoxidized linseed oil.

[0058] [Other additives] The first structure may contain other additives besides the aliphatic polycarbonate, the first inorganic particles, and the plasticizer, depending on the application of the composite structure. The other additives include, for example, at least one selected from the group consisting of a dispersant and an antistatic agent. The amount of other additives to be used is not particularly limited as long as the desired effect is not impaired. The amount of other additives to be used is appropriately determined taking into consideration the amount that can be normally used depending on the type of additive.

[0059] [Method of forming the first structure] The method for forming the first structure is not particularly limited. When the ratio of the aliphatic polycarbonate in the first structure is sufficiently high, a melt molding method such as injection molding or extrusion molding can be applied as a method for forming the first structure. In addition, aliphatic polycarbonate is soluble in various solvents. Therefore, after preparing a paste for forming the first structure by adding aliphatic polycarbonate, an organic solvent, the first inorganic particles, and other additives as necessary, the obtained paste is molded into a desired shape by a coating method such as a die coater sheet method or a doctor blade method, or a casting method, and then the molded paste is dried to obtain the first structure. Depending on the particle size of the first inorganic particles and the viscosity of the paste for forming the first structures, gravure printing or screen printing can be used as a method for forming the paste into a sheet. Furthermore, the aliphatic polycarbonate, the first inorganic particles, and, if necessary, other additives can be uniformly mixed in a solid state, and then the resulting mixture can be filled into a mold and compressed while being heated if necessary to form the first structure.

[0060] When the first structure is formed using a paste, suitable examples of the organic solvent added to the paste include alkanols such as isopropanol; water-soluble hydrocarbon solvents such as toluene, xylene, and isophorone; terpineol-based solvents such as terpineol and dihydroterpineol; ester-based solvents such as ethyl acetate, n-propyl acetate, n-butyl acetate, terpineol acetate, and dihydroterpineol acetate; ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, methyl carbitol, ethyl carbitol, and butyl carbitol. Examples of suitable organic solvents include glycol ether-based solvents such as propylene glycol monomethyl ether, ethylene glycol dimethyl ether, and diethylene glycol dimethyl ether; glycol ester-based solvents such as ethylene glycol monomethyl ether acetate and propylene glycol monomethyl ether acetate; carbonate-based solvents such as dimethyl carbonate and propylene carbonate; ketone-based solvents such as acetone, methyl ethyl ketone, and cyclohexanone; and nitrogen-containing polar organic solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone.

[0061] The amount of the organic solvent used when preparing the paste using the organic solvent is not particularly limited. The amount of the organic solvent used is appropriately adjusted so that the viscosity of the paste is suitable for the printing method or coating method carried out using the paste.

[0062] <Second structure> The second structure includes a branched polymer and a second inorganic particle. The second structure may include other components than the branched polymer and the second inorganic particle as long as the desired effect is not impaired. Components that the second structure may contain will be described below.

[0063] [Branched polymer] The molecular chain of the branched polymer has a main chain and branch chains. The main chain is made of a cellulose-based polymer. The branch chains are made of an aliphatic polycarbonate or an aliphatic polyester. The branch chains may be linear or branched. The branch chains may be attached to two or more main chains to cross-link two or more main chains. The second structure containing the branched polymer adheres well to the first structure containing the aliphatic polycarbonate, and the branched polymer disperses the second inorganic particles well.

[0064] In the branched polymer, the graft ratio, which is the ratio of the mass of the branched chain to the mass of the main chain, is not particularly limited as long as the desired effect is not impaired. In order to obtain a particularly good affinity between the branched polymer and the aliphatic polycarbonate contained in the first structure, the graft ratio is preferably 10% by mass or more and 400% by mass or less, more preferably 50% by mass or more and 250% by mass or less. The graft ratio can be determined by nuclear magnetic resonance spectroscopy (NMR analysis).

[0065] The mass average molecular weight of the branched polymer is not particularly limited. The mass average molecular weight of the branched polymer is, for example, preferably 50,000 to 1,000,000, more preferably 100,000 to 600,000. When the mass average molecular weight of the branched polymer is within this range, the branched polymer has good mechanical properties such as strength, elongation, and toughness, and good moldability.

[0066] The methods for producing the main chain, branch chain, and branched polymers are described below.

[0067] (Main Chain) The branched polymer has a main chain made of a cellulose-based polymer. The type of the cellulose-based polymer is not particularly limited as long as the main chain of the cellulose-based polymer has a functional group to which a branch chain can be bonded. Specific examples of suitable cellulose-based polymers include cellulose; alkyl celluloses such as methyl cellulose, ethyl cellulose, n-propyl cellulose, isopropyl cellulose, n-butyl cellulose, tert-butyl cellulose, and n-hexyl cellulose; hydroxyalkyl celluloses such as hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, and hydroxybutyl cellulose; cellulose esters such as cellulose acetate, cellulose diacetate, cellulose triacetate, cellulose acetate propionate, and cellulose acetate butyrate; carboxyalkyl celluloses such as carboxymethyl cellulose, carboxyethyl cellulose, and carboxypropyl cellulose; and cellulose derivatives such as nitrocellulose, aldehyde cellulose, dialdehyde cellulose, and sulfonated cellulose. The branched polymer may contain two or more types of branched polymer molecules having different types of cellulosic polymers as the backbone.

[0068] The cellulose-based polymer is preferably at least one selected from the group consisting of alkyl cellulose, hydroxyalkyl cellulose, and cellulose ester, in that it is easy to produce a branched polymer and to obtain a branched polymer having excellent compatibility with the aliphatic polycarbonate contained in the first structure. Among the above-mentioned preferred cellulose-based polymers, at least one selected from the group consisting of methyl cellulose, ethyl cellulose, cellulose acetate butyrate, cellulose acetate propionate, and cellulose acetate is preferred. The mass average molecular weight of the cellulose-based polymer is not particularly limited. The mass average molecular weight of the cellulose-based polymer is, for example, preferably 5,000 or more, more preferably 10,000 or more, and particularly preferably 100,000 or more. The mass average molecular weight of the cellulose-based polymer is preferably 1,000,000 or less, more preferably 750,000 or less, and even more preferably 500,000 or less. More specifically, the molecular weight of the cellulose-based polymer is preferably 5,000 or more and 1,000,000 or less, more preferably 10,000 or more and 750,000 or less, and even more preferably 10,000 or more and 750,000 or less.

[0069] The degree of substitution of the cellulose-based polymer is not particularly limited as long as the desired effect is not impaired. The degree of substitution of the cellulose-based polymer is preferably 2 or more and 3 or less, and typically 2.5. The degree of substitution of a cellulose-based polymer is the total number of hydroxyl groups substituted by groups other than those on branch chains, out of all hydroxyl groups in the constituent units of the cellulose-based polymer.

[0070] (branch chain) The branched polymer has a branch chain attached to a main chain made of a cellulose-based polymer. The branch chain is made of an aliphatic polycarbonate or an aliphatic polyester. The branch chain may be linear or branched. Typically, a branch chain is attached to only one backbone, however, a branch chain may be attached to more than one backbone to cross-link two or more backbones.

[0071] As long as the branch chain can be formed in a state of being bonded to the main chain or can be bonded to the main chain, the aliphatic polycarbonate or aliphatic polyester constituting the branch chain is not particularly limited. Typical examples of aliphatic polycarbonates or aliphatic polyesters constituting branched chains will be shown in the following description of the method for producing a branched polymer.

[0072] (Method of Producing Branched Polymer) The method for producing the branched polymer is not particularly limited. Typically, a graft polymerization method is used. The graft polymerization method can be appropriately selected from various known methods depending on the type of branch chain.

[0073] As the graft polymerization method, for example, a ring-opening polymerization method can be adopted, in which a cyclic carbonate compound or a cyclic ester compound such as lactone is subjected to ring-opening polymerization in the presence of a cellulose-based polymer, whereby an aliphatic polycarbonate or an aliphatic polyester is formed as a graft chain on the molecular chain of the cellulose-based polymer.

[0074] For example, propylene carbonate as a cyclic compound gives a branch chain made of polypropylene carbonate. Butylene carbonate as a cyclic compound gives a branch chain made of polybutylene carbonate. Cyclohexene carbonate as a cyclic compound gives a branch chain made of polycyclohexene carbonate. Trimethylene carbonate as a cyclic compound gives a branch chain made of polytrimethylene carbonate. 2,2-dimethyltrimethylene carbonate as a cyclic compound gives a branch chain made of poly(2,2-dimethyltrimethylene carbonate).

[0075] ε-caprolactone as a cyclic compound gives a branch chain of polycaprolactone, an aliphatic polyester. L-lactide as a cyclic compound gives a branch chain of polylactic acid in the L-form, an aliphatic polyester. D-lactide as a cyclic compound gives a branch chain of polylactic acid in the D-form, an aliphatic polyester. Meso-lactide as a cyclic compound gives a branch chain of polylactic acid in the syndiotactic form, an aliphatic polyester. β-propiolactone as a cyclic compound gives a branch chain of poly(3-hydroxypropionic acid), an aliphatic polyester, in the D-form. β-butyrolactone as a cyclic compound gives a branch chain of poly(3-hydroxybutyric acid), an aliphatic polyester, in the γ-butyrolactone as a cyclic compound gives a branch chain of poly(4-hydroxybutyric acid), an aliphatic polyester. δ-valerolactone as a cyclic compound gives a branch chain of poly(3-hydroxyvaleric acid), an aliphatic polyester. p-Dioxanone as a cyclic compound gives the aliphatic polyester poly(p-dioxanone) as a branched chain.

[0076] Typically, the ring-opening polymerization is carried out in the presence of a catalyst. Specific examples of catalysts that can be used in the ring-opening polymerization include alkali metals such as sodium and potassium; metal-containing catalysts such as sodium hydroxide, potassium hydroxide, triethylaluminum, aluminum triisopropoxide, n-butyllithium, titanium tetraisopropoxide, titanium tetrachloride, zirconium tetraisopropoxide, tin tetrachloride, sodium stannate, tin octanoate, and dibutyltin dilaurate diethylzinc; pyridine, 4-N,N-dimethylaminopyridine, 1,5, Basic organic compounds such as 7-triazabicyclo[4.4.0]dec-5-ene (TBD) and 1,8-diazabicyclo[5.4.0]undec-7-ene (DBT); acid catalysts such as hydrochloric acid, acetic acid, methanesulfonic acid, trifluoromethanesulfonic acid, p-toluenesulfonic acid, diphenylphosphoric acid, and phenol; and N-heterocyclic carbenes such as 1,3-bis(2-propyl)-4,5-dimethylimidazol-2-ylidene and 1,3-diisopropylimidazol-2-ylidene. The catalyst may be used alone or in combination of two or more kinds.

[0077] When ring-opening polymerization is carried out using a cyclic carbonate, it is also preferable to use a cocatalyst together with the catalyst.Specific examples of the cocatalyst include N-cyclohexyl-N'-phenylthiourea, N,N'-bis[3,5-bis(trifluoromethyl)phenyl]thiourea, N-[3,5-bis(trifluoromethyl)phenyl]-N'-cyclohexylthiourea, and (-)-sparteine.

[0078] The amount of catalyst that can be used in ring-opening polymerization is appropriately determined by considering the amount of catalyst used in conventionally known ring-opening polymerization reactions.Typically, the amount of catalyst used is preferably 0.001 mol or more, more preferably 0.005 mol or more, per 1 mol of cyclic compound.The amount of catalyst used is preferably 0.2 mol or less, more preferably 0.1 mol or less, per 1 mol of cyclic compound. More specifically, the amount of the catalyst used is preferably 0.001 mol or more and 0.2 mol or less, and more preferably 0.005 mol or more and 0.1 mol or less, per 1 mol of the cyclic compound. The amount of the cocatalyst used is similar to that of the catalyst used.

[0079] The ring-opening polymerization is preferably carried out in the presence of a solvent. The type of the solvent is not particularly limited as long as it does not inhibit the ring-opening polymerization reaction. Specific examples of suitable solvents include aliphatic hydrocarbon solvents such as pentane, hexane, octane, decane, and cyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, and xylene; halogenated hydrocarbon solvents such as methylene chloride, chloroform, 1,1-dichloroethane, 1,2-dichloroethane, chlorobenzene, and bromobenzene; ether solvents such as ethylene glycol dimethyl ether (monoglyme), diethylene glycol dimethyl ether (diglyme), triethylene glycol dimethyl ether (triglyme), tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, and anisole; ester solvents such as ethyl acetate, n-propyl acetate, and isopropyl acetate; and amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone.

[0080] The amount of the solvent used is not particularly limited as long as the ring-opening polymerization reaction proceeds well, and is preferably, for example, 100 parts by mass or more and 1000 parts by mass or less based on 100 parts by mass of the cyclic compound.

[0081] Typically, the cellulose-based resin, the cyclic compound, and the catalyst, and optionally a co-catalyst and / or a solvent, etc. are charged into a reaction vessel, and then the mixture in the reaction vessel is stirred to carry out the ring-opening polymerization.

[0082] The preferred reaction temperature for ring-opening polymerization varies depending on the cyclic compound, the type of catalyst, the amount of catalyst used, etc. Typically, the reaction temperature for ring-opening polymerization is preferably -80°C or higher, more preferably -40°C or higher, and even more preferably 0°C or higher. From the viewpoint of achieving both good yield and suppression of side reactions, the reaction temperature for ring-opening polymerization is preferably 250°C or lower, more preferably 200°C or lower, and even more preferably 150°C or lower. More specifically, the reaction temperature is preferably from -80°C to 250°C, more preferably from -40°C to 200°C, and even more preferably from 0°C to 150°C.

[0083] The reaction time of the ring-opening polymerization varies depending on the type of cyclic compound, the type of catalyst, the amount of catalyst used, etc. Typically, the reaction time of the ring-opening polymerization is preferably 1 hour or more and 40 hours or less.

[0084] The amount of the cyclic compound used in the ring-opening polymerization is appropriately determined taking into consideration the above-mentioned graft ratio.

[0085] Another preferred example of the method for producing a branched polymer is a method of copolymerizing a cyclic ether with carbon dioxide in the presence of a cellulose-based resin. This copolymerization reaction produces branched chains made of aliphatic polycarbonate. The cellulose-based resin is as described above.

[0086] As the cyclic ether, a cyclic ether corresponding to the aliphatic polycarbonate as a branched chain is appropriately selected. Preferred examples of cyclic ethers include ethylene oxide, propylene oxide, trimethylene oxide (oxetane), 3,3-dimethyltrimethylene oxide (3,3-dimethyloxetane), 1,2-butylene oxide, 2,3-butylene oxide, isobutylene oxide, 1-pentene oxide, 2-pentene oxide, 1-hexene oxide, 1-octene oxide, 1-dodecene oxide, cyclopentene oxide, cyclohexene oxide, vinylcyclohexane oxide, 3-phenylpropylene oxide, 3,3,3-trifluoropropylene oxide, 2-phenoxypropylene oxide, 3-naphthoxypropylene oxide, butadiene monoxide, 3-vinyloxypropylene oxide, and 3-trimethylsilyloxypropylene oxide.

[0087] Among the above cyclic ethers, ethylene oxide, propylene oxide, trimethylene oxide, and 1,2-butylene oxide are preferred, and ethylene oxide, propylene oxide, and trimethylene oxide are more preferred, because they have excellent polymerization reactivity and affinity with the aliphatic polycarbonate contained in the first structure of the branched polymer.

[0088] Examples of aliphatic polycarbonates produced by copolymerization of cyclic ethers with carbon dioxide are as follows: Ethylene oxide gives polyethylene carbonate; Propylene oxide gives polypropylene carbonate; Trimethylene oxide gives polytrimethylene carbonate.

[0089] The copolymerization of the cyclic ether and carbon dioxide is carried out in the presence of a metal catalyst. Preferred examples of the metal catalyst include zinc-based catalysts, aluminum-based catalysts, chromium-based catalysts, and cobalt-based catalysts. Among these, zinc-based catalysts and cobalt-based catalysts are preferred because of their high polymerization activity.

[0090] Specific examples of suitable zinc-based catalysts include diethylzinc-water catalyst, diethylzinc-pyrogallol catalyst, bis((2,6-diphenyl)phenoxy)zinc, N-(2,6-diisopropylphenyl)-3,5-di-tert-butylsalicylaldiminatozinc, 2-((2,6-diisopropylphenyl)amido)-4-((2,6-diisopropylphenyl)imino)-2-pentenoic acid acetate, zinc adipate, and zinc glutarate.

[0091] Specific examples of suitable cobalt-based catalysts include cobalt acetate-acetic acid-based catalysts, N,N'-bis(3,5-di-tert-butylsalicylidene)-1,2-cyclohexanediaminocobalt acetate, N,N'-bis-(3,5-di-tert-butylsalicylidene)-1,2-cyclohexanediaminocobalt pentafluorobenzoate, N,N'-bis-(3,5-di-tert-butylsalicylidene)-1,2-cyclohexanediaminocobalt chloride, N,N'-bis-(3,5-di-tert-butylsalicylidene)-1,2-cyclohexanediaminocobalt nitrate, N,N'-bis-(3,5-di-tert-butylsalicylidene)-1,2-cyclohexanediaminocobalt 2,4-dinitrophenoxide, tetraphenylporphyrin cobalt chloride, tetraphenylporphyrin cobalt acetate, N,N'-bis[2-(ethoxycarbonyl)-3-oxobutylidene]-1,2-cyclohexanediaminatocobalt chloride, and N,N'-bis[2-(ethoxycarbonyl)-3-oxobutylidene]-1,2-cyclohexanediaminatocobalt pentafluorobenzoate.

[0092] The cobalt-based catalyst is preferably used together with a promoter, specific examples of which include pyridine, 4-N,N-dimethylaminopyridine, N-methylimidazole, tetrabutylammonium chloride, tetrabutylammonium acetate, triphenylphosphine, bis(triphenylphosphoranylidene)ammonium chloride, and bis(triphenylphosphoranylidene)ammonium acetate.

[0093] The amount of catalyst that can be used for copolymerization of cyclic ether and carbon dioxide is appropriately determined in consideration of the amount of catalyst that is conventionally known for such copolymerization reaction.Typically, the amount of catalyst is preferably 0.001 mol or more, more preferably 0.005 mol or more, per 1 mol of cyclic ether.The amount of catalyst is preferably 0.2 mol or less, more preferably 0.1 mol or less, per 1 mol of cyclic ether. More specifically, the amount of the catalyst used is preferably 0.001 mol or more and 0.2 mol or less, and more preferably 0.005 mol or more and 0.1 mol or less, per 1 mol of the cyclic ether. The amount of the cocatalyst used is similar to that of the catalyst used.

[0094] The copolymerization of the cyclic ether with carbon dioxide is preferably carried out in the presence of a solvent. The type of the solvent is not particularly limited as long as it does not inhibit the copolymerization reaction. Specific examples of suitable solvents include aliphatic hydrocarbon solvents such as pentane, hexane, octane, decane, and cyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, and xylene; halogenated hydrocarbon solvents such as methylene chloride, chloroform, 1,1-dichloroethane, 1,2-dichloroethane, chlorobenzene, and bromobenzene; ether solvents such as ethylene glycol dimethyl ether (monoglyme), diethylene glycol dimethyl ether (diglyme), triethylene glycol dimethyl ether (triglyme), tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, and anisole; ester solvents such as ethyl acetate, n-propyl acetate, and isopropyl acetate; and amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone.

[0095] The amount of the solvent used is not particularly limited as long as the copolymerization reaction proceeds well, and is preferably, for example, 100 parts by mass or more and 1,000 parts by mass or less per 100 parts by mass of the cyclic ether.

[0096] Typically, the cellulose-based resin, the cyclic ether, and the catalyst, and optionally a cocatalyst and / or a solvent, etc. are charged into a reaction vessel, carbon dioxide is injected into the reaction vessel, and the mixture in the reaction vessel is stirred to carry out the copolymerization.

[0097] The amounts of the cyclic ether and carbon dioxide used in the copolymerization are appropriately determined taking into consideration the above-mentioned graft ratio. In carrying out the copolymerization, the pressure of carbon dioxide in the reaction vessel is preferably 0.1 MPa or more, more preferably 0.2 MPa or more, and even more preferably 0.5 MPa or more, as a gauge pressure at the reaction temperature, from the viewpoint of good reaction progress. In terms of eliminating the need to use an expensive pressure-resistant vessel with high pressure resistance and of operational safety, the pressure of carbon dioxide in the reaction vessel is preferably 20 MPa or less, more preferably 10 MPa or less, and may be 5 MPa or less. More specifically, the pressure of carbon dioxide in the reaction solution is preferably 0.1 MPa or more and 20 MPa or less, more preferably 0.2 MPa or more and 10 MPa or less, and even more preferably 0.5 MPa or more and 5 MPa or less, in terms of gauge pressure. The copolymerization reaction may be carried out under supercritical conditions of carbon dioxide.

[0098] The preferred reaction temperature for copolymerization varies depending on the type of cyclic ether, the type of catalyst, the amount of catalyst used, etc. Typically, the reaction temperature for copolymerization is preferably 0° C. or higher, more preferably 20° C. or higher, and even more preferably 30° C. or higher. From the viewpoint of achieving both good yield and suppression of side reactions, the reaction temperature for copolymerization is preferably 100° C. or lower, more preferably 80° C. or lower, and even more preferably 60° C. or lower. From the above viewpoints, the reaction temperature of the copolymerization is preferably 0°C or higher and 100°C or lower, more preferably 20°C or higher and 80°C or lower, and even more preferably 30°C or higher and 60°C or lower.

[0099] The reaction time of the copolymerization varies depending on the type of cyclic ether, the type of catalyst, the amount of catalyst used, etc. Typically, the reaction time of the ring-opening polymerization is preferably 1 hour or more and 40 hours or less.

[0100] The amount of the cyclic compound used in the ring-opening polymerization is appropriately determined taking into consideration the above-mentioned graft ratio.

[0101] When the branch chains are made of an aliphatic polyester obtained by polycondensation of an aliphatic dicarboxylic acid and a glycol, such as polyethylene succinate, polyethylene adipate, polybutylene succinate, or polybutylene adipate, a branched polymer can also be produced by copolycondensing an aliphatic dicarboxylic acid and a glycol according to the structure of the aliphatic polyester in the presence of a cellulose-based resin according to a conventional method.

[0102] [Second inorganic particles] The second inorganic particles can be the same as the first inorganic particles without any particular limitation. The second inorganic particles can be the same type of inorganic particles as the first inorganic particles, or a different type of inorganic particles. The type of the second inorganic particles is usually selected taking into consideration the use of the composite structure and the type of the first inorganic particles. The second structure may contain two or more types of inorganic particles as the second inorganic particles.

[0103] [Other additives] The second structure may contain other additives other than the branched polymer and the second inorganic particles, depending on the application of the composite structure. Examples of the other additives include at least one selected from the group consisting of a dispersant, a plasticizer, and an antistatic agent. The amount of other additives to be used is not particularly limited as long as the desired effect is not impaired. The amount of other additives to be used is appropriately determined taking into consideration the amount that can be normally used depending on the type of additive.

[0104] [Method of forming second structure] The method for forming the second structure is not particularly limited. The second structure can be formed by the same method as the first structure. When the ratio of the branched polymer in the second structure is sufficiently high, the melt molding method such as injection molding or extrusion molding can be applied as the method for forming the second structure. In addition, the second structure is soluble in various solvents. Therefore, after preparing a paste for forming the second structure by adding a branched polymer, an organic solvent, the second inorganic particles, and other additives as necessary, the obtained paste is molded into a desired shape by a coating method such as a die coater sheet method or a doctor blade method, or a casting method, and then the molded paste is dried to obtain the second structure. Depending on the particle size of the second inorganic particles and the viscosity of the paste for forming the second structure, gravure printing or screen printing can be used as a method for forming the paste into a sheet. Furthermore, the branched polymer, the second inorganic particles, and, if necessary, other additives can be uniformly mixed in a solid state, and then the resulting mixture can be filled into a mold and compressed while being heated if necessary, to form the second structure.

[0105] When a paste is used to form the second structure, suitable examples of the organic solvent to be added to the paste are the same as the suitable examples of the organic solvent that can be used when preparing the paste described for the first structure.

[0106] The amount of the organic solvent used when preparing the paste using the organic solvent is not particularly limited. The amount of the organic solvent used is appropriately adjusted so that the viscosity of the paste is suitable for the printing method or coating method carried out using the paste.

[0107] The method for combining the first structure and the second structure described above is not particularly limited. For example, when the first structure and the second structure can be formed by injection molding, the first structure and the second structure can be simultaneously formed by a multi-color molding method such as a so-called two-color molding method, and the two structures can be combined. When the first structure and the second structure can be formed by extrusion molding, the first structure and the second structure can be simultaneously formed by co-extrusion molding to combine the two. Furthermore, the first structure and the second structure, which are formed separately, may be combined by a method such as thermocompression bonding. EXAMPLES

[0108] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0109] Example 1 (Preparation of dielectric paste) 7.2 parts by mass of polypropylene carbonate, which is an aliphatic polycarbonate, was dissolved in 26 parts by mass of n-butyl acetate and 26 parts by mass of dimethyl carbonate. The polypropylene carbonate has a carboxylic acid modified site in the repeating structure. The ratio of the carboxylic acid modified site is 0.8 mol% in the entire structure. 40 parts by mass of barium titanate particles (BET equivalent diameter 0.2 μm) as ceramic particles, 0.7 parts by mass of polyethylene glycol as a plasticizer, and 0.1 parts by mass of an antistatic agent were added to the obtained solution. Next, the obtained suspension was dispersed in a ball mill for a predetermined time to obtain a dielectric paste.

[0110] (Preparation of Green Sheet) The obtained dielectric paste was used to form a sheet using a doctor blade method so that the thickness after firing would be 1.4 μm. The formed sheet was dried to obtain a green sheet. The obtained green sheet corresponds to the first structure.

[0111] (Preparation of conductive paste) A resin having a main chain made of ethyl cellulose and a branch chain made of polypropylene carbonate was used as the branched polymer. The branched polymer was prepared by ring-opening polymerization of propylene carbonate in the presence of ethyl cellulose. The graft ratio of the branched polymer was 50% by mass.

[0112] (Coating conductive paste) The obtained conductive paste was applied onto the above-mentioned green sheet by screen printing. The coating film was then dried and fired to form a coating film that would provide an internal electrode layer. The coating film had a thickness of 0.4 μm. The formed coating film corresponds to the second structure.

[0113] (Laminated) 218 green sheets having a coating film that will provide an internal electrode layer when fired were stacked, and green sheets having no coating film were stacked on top and bottom layers and the whole was pressed together to obtain a laminate containing a total of 220 green sheets.

[0114] (Disconnect) The obtained laminate was divided by cutting in a direction perpendicular to the surface direction of the laminate with a dicing saw. The size of the divided laminate was adjusted so that the size of the surface perpendicular to the thickness direction was 1.0 mm × 0.5 mm when the divided laminate was fired.

[0115] (Firing) More than 100 divided laminates were heat-treated in an N2 gas flow at a maximum temperature of 270°C, and then further heat-treated in an N2-H2O-H2 gas flow at a maximum temperature of 800°C. After that, the laminate was heated in an N2-H2O-H2 gas flow at an oxygen partial pressure of 1.8×10 -9 ~8.7×10 -10 The firing was performed under the conditions of a pressure of 1.5 MPa, a heating rate of 100°C / min, and a maximum temperature of 1260°C. Note that, during firing, after the maximum temperature of 1260°C was reached, the temperature was maintained for 10 minutes and then immediately cooled to near room temperature. The thickness of the dielectric layer formed by firing the green sheet was 1.4 μm.

[0116] In the above steps, the laminate was evaluated for delamination during cut and for occurrence of structural defects after firing according to the following methods. The evaluation results are shown in Table 1.

[0117] <Evaluation of delamination during press cutting> The cut surface of each of the 100 laminates after being cut by the dicing saw was observed under an optical microscope to check for the presence or absence of delamination between the green sheet and the coating film formed using the conductive paste. The number of laminates in which delamination was observed is shown in Table 1 as the delamination occurrence rate (%).

[0118] <Evaluation of structural defects after firing> The 100 fired and divided laminates were observed under an optical microscope to check for the presence or absence of structural defects such as cracks and delamination that are thought to be caused by gas generation due to resin decomposition. The number of laminates in which structural defects were found is shown in Table 1 as the structural defect occurrence rate.

[0119] Example 2 The branched polymer used was a resin having a main chain made of ethyl cellulose and a branch chain made of polycaprolactone, an aliphatic polyester. The branched polymer was prepared by ring-opening polymerization of caprolactone in the presence of ethyl cellulose. The graft ratio of the branched polymer was 100% by mass. Except for using the branched polymer, the same operations as in Example 1 were carried out, and the evaluation of delamination during press cutting and the occurrence of structural defects after baking were carried out. The evaluation results are shown in Table 1.

[0120] Comparative Example 1 Except for changing the resin used in preparing the dielectric paste to polyvinyl butyral and the resin used in preparing the conductive paste to ethyl cellulose, the same operations as in Example 1 were carried out, and an evaluation of delamination during press cutting and the occurrence of structural defects after firing were performed. The evaluation results are shown in Table 1.

[0121] Comparative Example 1 Except for changing the resin used in preparing the conductive paste to ethyl cellulose, the same procedure as in Example 1 was carried out, and an evaluation of delamination during press cutting and the occurrence of structural defects after firing were carried out. The results of these evaluations are shown in Table 1.

[0122] [Table 1]

[0123] According to Table 1, it can be seen that a laminate in which a green sheet corresponding to a first structure containing an aliphatic polycarbonate and inorganic particles such as ceramic particles is combined with a coating film corresponding to a second structure containing a branched polymer having a main chain made of a cellulose-based polymer and a branch chain made of an aliphatic polycarbonate or an aliphatic polyester, and inorganic particles such as metal particles, is not easily peeled off by external forces such as a shear force during cutting or the pressure of gas generated during firing.

Claims

1. A composite structure including a first structure and a second structure, The first structure and the second structure are in contact with each other, the first structure includes an aliphatic polycarbonate and first inorganic particles; the second structure includes a branched polymer and a second inorganic particle; the molecular chain of the branched polymer has a main chain made of a cellulose-based polymer and a branch chain made of an aliphatic polycarbonate or an aliphatic polyester; The branched chain may be linear or branched, The branch chains may be bonded to two or more of the main chains to crosslink two or more of the main chains, The first structure and the second structure are both sheet-shaped, The first structure and the second structure are stacked, The first structure and the second structure are repeatedly and alternately stacked, the first structure contains metal particles and ceramic particles as the first inorganic particles, The second structure may include ceramic particles and metal particles as the second inorganic particles, In the first structure, a volume occupied by the metal particles is larger than a volume occupied by the ceramic particles, A composite structure, wherein in the second structure, a volume occupied by the ceramic particles is greater than a volume occupied by the metal particles.

2. A composite structure including a first structure and a second structure, The first structure and the second structure are in contact with each other, the first structure includes an aliphatic polycarbonate and first inorganic particles; the second structure includes a branched polymer and a second inorganic particle; the molecular chain of the branched polymer has a main chain made of a cellulose-based polymer and a branch chain made of an aliphatic polycarbonate or an aliphatic polyester; The branched chain may be linear or branched, The branch chains may be bonded to two or more of the main chains to crosslink two or more of the main chains, The first structure and the second structure are both sheet-shaped, The first structure and the second structure are stacked, The first structure and the second structure are repeatedly and alternately stacked, The first structure may include ceramic particles and metal particles as the first inorganic particles, the second structure contains metal particles and ceramic particles as the second inorganic particles, In the first structure, a volume occupied by the ceramic particles is larger than a volume occupied by the metal particles, A composite structure, wherein in the second structure, a volume occupied by the metal particles is larger than a volume occupied by the ceramic particles.

3. 3. The composite structure according to claim 1, wherein the metal constituting the metal particles is at least one selected from the group consisting of Ni, Cu, Ag, Pt, and Au.

4. The composite structure according to any one of claims 1 to 3, wherein the material constituting the ceramic particles includes at least one selected from the group consisting of Ba, Ti, Sr, Ca, and Zr.

5. The composite structure according to any one of claims 1 to 4, wherein the cellulose-based polymer comprises at least one selected from the group consisting of methyl cellulose, ethyl cellulose, cellulose acetate butyrate, cellulose acetate propionate, and cellulose acetate.

6. the molecular chain of the branched polymer has the branch chain made of the aliphatic polyester, The composite structure according to any one of claims 1 to 5, wherein the aliphatic polyester is at least one selected from the group consisting of polycaprolactone, polylactic acid, poly(3-hydroxybutyric acid), and polybutylene succinate.

7. The first structure and the second structure each independently contain at least one additive selected from the group consisting of a dispersant, a plasticizer, and an antistatic agent. The composite structure according to any one of claims 1 to 6.

8. The second structure contains or does not contain at least one additive selected from the group consisting of a dispersant, a plasticizer, and an antistatic agent; 2. The composite structure according to claim 1, wherein a content of the ceramic particles in the second structure is 45 vol% or more and 70 vol% or less with respect to a total volume of the branched polymer, the second inorganic particles, and the additive contained in the second structure.

9. The first structure contains or does not contain at least one additive selected from the group consisting of a dispersant, a plasticizer, and an antistatic agent; 2. The composite structure according to claim 1, wherein the content of the metal particles in the first structure is 50 volume % or more and 75 volume % or less with respect to the total volume of the aliphatic polycarbonate contained in the first structure, the volume of the first inorganic particles, and the volume of the additive.

10. The first structure contains or does not contain at least one additive selected from the group consisting of a dispersant, a plasticizer, and an antistatic agent; The composite structure according to claim 2, wherein the content of the ceramic particles in the first structure is 45 vol% or more and 70 vol% or less with respect to the total volume of the aliphatic polycarbonate contained in the first structure, the volume of the first inorganic particles, and the volume of the additive.

11. The second structure contains or does not contain at least one additive selected from the group consisting of a dispersant, a plasticizer, and an antistatic agent; 3. The composite structure according to claim 2, wherein a content of the metal particles in the second structure is 50 vol % or more and 75 vol % or less with respect to a total volume of the branched polymer, the second inorganic particles, and the additive contained in the second structure.

12. A precursor of a multilayer ceramic electronic component, comprising the composite structure according to any one of claims 1 to 11.

13. 12. A method for producing a precursor of a multilayer ceramic electronic component, comprising cutting the composite structure according to claim 1 in a direction perpendicular or approximately perpendicular to a plane direction of the composite structure.

14. Producing the multilayer ceramic electronic component precursor by the method according to claim 13; and firing the precursor of the multilayer ceramic electronic component.

Citation Information

Patent Citations

  • Film molded by using and molding high-molecular weight aliphatic polyester

    JP1993179016A

  • Biodegradable magnetic ink composition

    JP1998025439A

  • Magnetic recording medium

    JP2001209923A

  • Composition for molding sintered ceramic, method for producing sintered ceramic, and ceramic

    JP2011020916A

  • Conductive paste

    JP2018168238A