Encapsulating material sheet for self-luminous display and self-luminous display using same
The encapsulant sheet with a Vicat softening point of 60°C to 90°C and optimized MFR addresses blocking and non-uniformity issues, improving productivity and optical properties in self-luminous displays like micro LED televisions.
Patent Information
- Application Number
- JP2023172618
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-10-04
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2038-03-30
AI Technical Summary
Existing encapsulant sheets for self-luminous displays, such as micro LED televisions, face issues with blocking, reduced productivity, and non-uniform film thickness due to low Vicat softening points and high material costs, especially when dealing with minute irregularities on the display surface.
The encapsulant sheet is formulated with a Vicat softening point between 60°C and 90°C and a melt flow rate (MFR) of 0.1 to 12.0 g/10 min, optimized for self-luminous displays, ensuring excellent moldability and uniform film thickness by using olefin resin as the base resin and avoiding crosslinking treatment.
This formulation enhances productivity, durability, and optical properties of self-luminous displays by preventing blocking, maintaining uniform film thickness, and reducing material costs.
Smart Images

Figure 0007582422000002 
Figure 0007582422000003 
Figure 0007582422000004
Abstract
Description
[Technical field]
[0001] The present invention relates to an encapsulant sheet for a self-luminous display device, and a self-luminous display device using the same. [Background technology]
[0002] 2. Description of the Related Art Self-luminous displays, such as micro LED televisions, are being developed as next-generation display devices to replace various liquid crystal display devices (Patent Document 1).
[0003] In this self-luminous display, an encapsulant sheet for protecting the light-emitting element is laminated on the light-emitting surface of the LED module, which is constructed by mounting light-emitting elements such as LED elements on a wiring board (Patent Document 2).
[0004] Here, the encapsulant sheet for electronic devices disclosed in Patent Document 2 is expected to be widely applied to various electronic devices including solar cells, and its Vicat softening point is required to be in a low temperature range of 60°C or less, particularly preferably 30 to 50°C or less. As described in the same document, this is intended to "demonstrate high adhesiveness by thermocompression bonding in a short time." Furthermore, in the past, it was thought that a Vicat softening point in the above low temperature range was preferable in order to ensure sufficient embedding (molding ability) of the encapsulant sheet into the unevenness of the surface of electronic devices with various surface shapes.
[0005] However, in the process of developing the above-mentioned micro LED TV, when the surface of the electronic device to be covered with the encapsulant sheet has only minute irregularities, such as the light-emitting surface of the above-mentioned LED module constituting the micro LED TV, and when the uniformity of the encapsulant film thickness after the heat press processing is required to be at a much higher level than in the case of a solar cell module, etc., in order to maintain image quality, doubts began to arise that an encapsulant sheet having a Vicat softening point in the above-mentioned low temperature range may not necessarily be optimal.
[0006] When the unevenness of the target surface to be covered with the encapsulant sheet is minute, there is no need to limit the Biquad softening point to the above-mentioned low temperature range (60°C or lower) from the viewpoint of molding properties, and in terms of productivity, the decrease in total productivity and quality stability due to the occurrence of blocking of the encapsulant sheet is more likely to become apparent than the above-mentioned advantage described in Patent Document 2 (that thermocompression bonding can be completed in a short time).
[0007] Furthermore, when the Vicat softening point of the encapsulant sheet is in the above-mentioned low temperature range, a crosslinking agent needs to be added to ensure sufficient heat resistance of the encapsulant sheet, which results in problems such as increased material costs for the encapsulant sheet and reduced productivity due to limitations on the film formation temperature.
[0008] In this situation, there has been a demand for the development of an encapsulant sheet that is suitable for various self-luminous display applications, such as micro LED televisions, which are increasingly expected to be the next generation of display devices. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2018-14481 A [Patent Document 2] JP 2014-148584 A Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been made in consideration of the above circumstances, and has an object to provide an encapsulant sheet that is particularly suitable for use in self-luminous display devices such as micro LED televisions. [Means for solving the problem]
[0011] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by specifying the Vicat softening point of an encapsulant sheet for electronic devices to a high temperature range different from the conventional range, and by maintaining the MFR within a specific low MFR range, it is possible to obtain an encapsulant sheet that is particularly suitable for use in self-luminous display devices such as micro LED televisions. Specifically, the present invention provides the following.
[0012] (1) An encapsulant sheet for a self-luminous display device, which is a resin sheet having an olefin-based resin as a base resin, has a Vicat softening point of greater than 60°C and less than 90°C, and has an MFR of 0.1 g / 10 min or more and less than 12.0 g / 10 min at 190°C.
[0013] The invention (1) is an encapsulant sheet for encapsulating electronic devices, in which the Vicat softening point of the base resin is specified to be in a higher temperature range than conventional products, and the MFR of the same resin is maintained in a low MFR range similar to or lower than conventional products. This makes it possible to obtain an encapsulant sheet that is particularly suitable for use in self-luminous displays in terms of blocking resistance during the manufacturing process of the encapsulant sheet, molding properties during heat press processing, uniformity of film thickness after heat press processing, and suppression of resin overflow due to excessive flow.
[0014] (2) The encapsulating material sheet according to (1), having a MFR at 190° C. of less than 5.0 g / 10 min.
[0015] The invention (2) is an invention in which the Vicat softening point temperature of the encapsulant sheet of (1) is kept within the above-mentioned high temperature range while the MFR is further reduced, thereby further suppressing the excessive flow of the encapsulant sheet of (1) during heat press processing, and maintaining a higher level of uniformity in film thickness after heat press processing.
[0016] (3) The encapsulating material sheet according to (2), having a MFR at 190° C. of less than 0.5 g / 10 min.
[0017] The invention (3) relates to the encapsulant sheet (2), in which the Vicat softening point temperature is maintained in the above-mentioned high temperature range while the MFR is suppressed to an extremely low range. Such an encapsulant sheet can be obtained by a so-called weak crosslinking treatment. This further suppresses the excessive flow of the encapsulant sheet (1) during the heat press processing, and the uniformity of the film thickness after the heat press processing can be maintained at an extremely high level.
[0018] (4) A self-luminous display comprising: a light-emitting module for a self-luminous display comprising a plurality of light-emitting elements mounted on a wiring board; a sealant sheet covering the light-emitting elements and laminated on the mounting surface side of the wiring board on which the light-emitting elements are mounted; and a display surface panel laminated on the surface of the sealant sheet, the sealant sheet being an sealant sheet as described in any one of (1) to (3).
[0019] According to the invention (4), it is possible to obtain a self-luminous display device having excellent productivity, durability, and optical properties by taking advantage of the advantageous effects of the blocking resistance, molding properties, and film thickness uniformity that can be exhibited by any one of the encapsulant sheets (1) to (3).
[0020] (5) The self-luminous display according to (4), wherein the light-emitting element is an LED element.
[0021] The fifth aspect of the present invention is the application of the present invention to various self-luminous LED display devices, such as micro LED televisions, which are expected to be the mainstream of next-generation monitors. This makes it possible to obtain self-luminous LED display devices that are excellent in productivity, durability, and optical properties.
[0022] (6) The self-luminous display body described in (5), wherein the LED element has an LED light-emitting chip and a resin cover covering the LED light-emitting chip, the width and depth of the LED element are both 300 μm or less, the height is 200 μm or less, and the arrangement interval of each of the LED elements is 0.03 mm or more and 12.0 mm or less.
[0023] The invention of (6) applies the self-luminous display of (5) to a high-definition dot matrix display device in which LED elements are densely mounted using a chip-on-board method in which a large number of LED chips are directly mounted on a substrate, making it possible to obtain a high-definition LED display device with excellent productivity, durability, and optical properties.
[0024] (7) The self-luminous display according to (6), wherein the width and depth of the LED elements are both 50 μm or less, the height is 10 μm or less, and the spacing between the LED elements is 0.05 mm or more and 5 mm or less.
[0025] The invention (7) applies the self-luminous display element (5) to the "micro LED TV," which has been under development in recent years and is expected to be the next-generation image display device. This makes it possible to obtain an ultra-high definition LED display device with excellent productivity, durability, and optical properties.
[0026] (8) A self-luminous display body described in any one of (4) to (7), in which a plurality of the light-emitting modules have a light-emitting surface joined together on the same plane, and the sealing material sheet is laminated on the light-emitting surface.
[0027] The invention of (7) is to increase the screen size of various self-luminous displays, including micro LED TVs, by bonding multiple LED modules for self-luminous displays, which are constructed using the encapsulant sheet of (1) or (2). The encapsulant sheet of (1) or (2) has excellent surface smoothness after bonding by thermal lamination, so that the screen size of the self-luminous display can be flexibly increased without causing a decrease in screen quality due to the bonding of the modules. Effect of the Invention
[0028] According to the present invention, it is possible to provide an encapsulant sheet that is particularly suitable for use in various self-luminous display devices such as micro LED televisions. [Brief description of the drawings]
[0029] [Figure 1] 1 is a plan view and a partially enlarged plan view of an image display surface of a self-luminous display device obtained by laminating the encapsulant sheet of the present invention on a light-emitting module (LED module) for the self-luminous display device. [Diagram 2] 2 is a cross-sectional view showing a cross section of a portion AA in FIG. 1. [Diagram 3] FIG. 2 is a perspective view of an LED element constituting an LED module for the self-luminous display of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] <Self-luminous display> First, the term "self-luminous display" in this specification refers to a display device such as the micro LED television exemplified above, which is a display device for displaying visual information such as characters, images, videos, etc. This display device is a display device in which a large number of minute light-emitting elements are mounted in a matrix on a wiring board, and each light-emitting element is selectively made to emit light by a light-emitting control means connected thereto, thereby enabling the above visual information to be directly displayed on a display screen by blinking each light-emitting element.
[0031] The encapsulant sheet for a self-luminous display body of the present invention (hereinafter, also simply referred to as "encapsulant sheet") can be particularly preferably used in an LED display device that uses an LED element as a light-emitting element, among other "self-luminous display bodies". In this case, the LED element is more preferably a "microsized LED element". In this specification, the "microsized LED element" specifically refers to an LED element having a width (W) and depth (D) of 300 μm or less and a height (H) of 200 μm or less, with respect to the overall size of the light-emitting element including the LED light-emitting chip and the resin cover covering it (see FIG. 3).
[0032] Moreover, it is more preferable that the size of the "micro-sized LED element" is 50 μm or less in width and depth, and 10 μm or less in height. This size range is the standard size of LED elements mounted in micro LED televisions, which have been developed in recent years and are expected to become the mainstream of next-generation televisions. Hereinafter, in this specification, a self-luminous display device in which micro-sized LED elements, both of which are 50 μm or less in width and depth and 10 μm or less in height, are arranged in a matrix shape with a pitch of several μm to several tens of μm, with a number of several thousand by several thousand or more, is referred to as a "micro LED display device."
[0033] In the following, the present invention will be described in detail, taking up an embodiment in which the "self-luminous display body" is a "micro LED display device" as a particularly preferred specific example among various embodiments of the present invention. However, the technical scope of the present invention is not limited to application only to "micro LED display devices". It is a technology that can be applied to "self-luminous display bodies" in general as defined above.
[0034] [Micro LED display device] Fig. 1 is a front view of a micro LED display device 100, which is an embodiment of a self-luminous display body of the present invention, and a partially enlarged view (100A) thereof. Fig. 2 is a cross-sectional view showing a cross section of the AA portion of Fig. 1, and is a drawing for explaining the layer structure of the micro LED display device 100 shown in Fig. 1. This micro LED display device 100 is a self-luminous display device equipped with an LED module 30, which is a light-emitting module for a self-luminous display body, in which a large number of minute-sized LED elements 10 are mounted on a wiring board 20 as light-emitting elements, and the light emission of each LED element 10 is individually controlled by a light-emitting control means (not shown) such as an IC chip board that is separately bonded.
[0035] In the micro LED display device 100, a sealant sheet 1 for a self-luminous display is laminated on the mounting surface of the LED element 10 of the LED module 30 in a manner to cover the LED element 10. A display surface panel 2 such as various optical films and transparent protective glass is further laminated on the outer surface side of the sealant sheet 1 (the display surface side in the micro LED display device 100).
[0036] Moreover, a plurality of LED modules 30 for self-luminous display bodies can be joined in a matrix on the same plane, and the joined LED modules can be laminated with the sealing material sheet 1 in the same manner as above to form a large LED module for self-luminous display bodies and a large micro LED display device. In this case, the excellent uniformity of the film thickness after the heat press processing of the sealing material sheet 1 maintains the uniformity of the display surface at the joints between the individual joined LED modules, and also contributes to improving the image quality of such a large micro LED display device.
[0037] (Method of manufacturing micro LED display device) The micro LED display device 100 can be manufactured by laminating an LED module 30 for a self-luminous display body, which is formed by mounting an LED element 10 on a wiring board 20, an encapsulant sheet 1, a display surface panel 2, and other optical members arranged as necessary, into a laminate, and integrating the laminate by heat pressing. It is preferable that some of the laminate members are bonded in advance with an adhesive before the above heat pressing as necessary. The encapsulant sheet 1 of the present invention is characterized in that it exhibits sufficient molding properties during the heat pressing process for integration into the final product, and is also extremely excellent in the uniformity of the film thickness after the heat pressing process.
[0038] (LED module for self-luminous displays) An LED module 30, which is a light-emitting module for a self-luminous display according to the present invention, is constructed by mounting an LED element 10 on a wiring board 20 having a wiring portion 22 formed on a support substrate 21, as shown in FIG.
[0039] 2, the wiring board 20 is a circuit board in which wiring parts 22 made of, for example, a metal such as copper or other conductive material are formed on the surface of a support substrate 21 in a form capable of conducting with the LED elements 10. The support substrate 21 may be a hard glass epoxy substrate conventionally known as a substrate for electronic circuits, or may be made of a flexible resin such as polyethylene terephthalate, polyimide, or polyethylene naphthalate.
[0040] In the LED module 30, as shown in FIG. 2, the LED element 10 is mounted on the wiring portion 22 via a solder layer 23 in a conductive manner.
[0041] There is no particular limit to the size of the LED module 30, but a diagonal length of about 50 inches to 200 inches is generally considered to be preferable from the viewpoint of cost performance. As described above, a plurality of LED modules 30 for self-luminous display bodies can be joined in a matrix on the same plane to form a light-emitting surface of a self-luminous display body such as a large-sized micro LED display device 100. For example, a micro LED television with a large screen with a diagonal length of 600 inches can be formed by joining 100×100 LED modules 30 with a diagonal length of 6 inches vertically and horizontally.
[0042] (LED element) The LED element 10, which is mounted on the wiring board 20 and constitutes the LED module 30 for a self-luminous display, is a light-emitting element that utilizes light emission at a PN junction where a P-type semiconductor and an N-type semiconductor are joined. A structure in which a P-type electrode and an N-type electrode are provided on the upper and lower surfaces of the element, and a structure in which both a P-type electrode and an N-type electrode are provided on one surface of the element have been proposed. Either structure of the LED element 10 can be used in the LED display device 100 of the present invention, but a minute-sized LED element such as the LED element disclosed as a "chip-shaped electronic component" in JP-A-2006-339551 is particularly preferably used. The LED element disclosed in the document is said to have a width x depth x height size of approximately 25 μm x 15 μm x 2.5 μm.
[0043] The LED element 10 preferably includes an LED light-emitting chip 11 and a resin cover 12 covering the LED light-emitting chip 11. The resin cover 12 is made of an organic insulating material such as epoxy resin, silicon resin, polyimide resin, etc., and among these, epoxy resin is particularly preferably used. The resin cover 12 made of epoxy resin not only protects the LED light-emitting chip 11 from physical impact, but also suppresses total reflection of light into the semiconductor due to the difference in refractive index between the semiconductor constituting the LED light-emitting chip 11 and air, thereby enhancing the light-emitting efficiency of the LED element 10. The encapsulant sheet 1 is preferably used as an encapsulant to be mounted on the micro LED display device 100 because it is made of an olefin resin that has excellent adhesion to epoxy resin.
[0044] In the self-luminous display of the present invention, an LED element including an LED chip and a resin cover covering the LED chip, the LED element having a width and depth of 300 μm or less and a height of 200 μm or less, can be preferably used. In this case, the LED elements are preferably arranged at intervals of 0.03 mm or more and 100 mm or less.
[0045] Furthermore, in the self-luminous display of the present invention, an LED element including an LED light-emitting chip and a resin cover covering the LED light-emitting chip, and an extremely small LED element having a width and depth of 50 μm or less and a height of 10 μm or less, can be more preferably used. In this case, the arrangement interval of the LED elements is preferably 0.03 mm or more and 100 mm or less. Specifically, such a mounting mode of the LED elements is also a standard mounting mode of the LED elements in a micro LED television.
[0046] (Sealant sheet for self-luminous displays) The encapsulant sheet of the present invention is a resin sheet that can be particularly preferably used as a resin sheet for covering a small number of light-emitting elements in a "self-luminous display" and laminating it on a wiring board. The encapsulant sheet for this self-luminous display is a sheet-shaped member formed by forming an encapsulant composition having an olefin-based resin as a base resin. The encapsulant sheet of the present invention may be a single-layer film, but may also be a multilayer film composed of a core layer and skin layers disposed on both sides of the core layer. The multilayer film in this specification refers to a film or sheet having a structure having at least a skin layer formed on at least one of the outermost layers, preferably both outermost layers, and a core layer that is a layer other than the skin layer.
[0047] The thickness of the encapsulant sheet may be 50 μm or more and 1000 μm or less, preferably 50 μm or more and 500 μm or less, and more preferably 50 μm or more and 300 μm or less. In addition, when the LED element to be covered is an extremely small LED element with a height of 10 μm or less, the thickness of the encapsulant sheet is preferably 25 μm or more and 100 μm or less. When the thickness of the encapsulant sheet is 50 μm or more, the LED element can be sufficiently protected from external impact. On the other hand, when the thickness of the encapsulant sheet is 1000 μm or less, sufficient molding properties can be exhibited. Specifically, during the heat press processing in the state in which the LED element is covered, the resin constituting the encapsulant sheet can sufficiently go around the unevenness of the LED module surface and perform good lamination without gaps. In addition, in the self-luminous display body after integration, the light transmittance of the encapsulation layer made of the encapsulant sheet can be sufficiently ensured.
[0048] The encapsulant sheet has a Vicat softening point of more than 60° C. and not more than 90° C., preferably more than 70° C. and not more than 90° C. By making the encapsulant sheet have a Vicat softening point of more than 60° C., it is possible to suppress the occurrence of blocking during the manufacturing process of a self-luminous display using the encapsulant sheet, thereby contributing to improving the productivity of the self-luminous display. Furthermore, by making the temperature range 90° C. or less, it is possible to maintain the molding properties required for an encapsulant sheet for a self-luminous display.
[0049] More specifically, it is preferable to optimize the Vicat softening point of the encapsulant sheet more strictly according to the melting point of the encapsulant sheet. Specifically, when the melting point of the encapsulant sheet is in a relatively low range of 50°C to less than 70°C, the Vicat softening point is preferably in the range of 60°C to less than 70°C in order to suppress excessive flow during heat press processing. When the melting point is in a relatively high range of 70°C or more, the Vicat softening point is preferably in the range of 70°C to 90°C in order to maintain good molding properties during heat press processing.
[0050] In this specification, the "Vicat softening point" of the encapsulant sheet refers to a value of the Vicat softening point of the encapsulant sheet after completion of sheet formation in which an encapsulant composition containing a resin component and other additives is formed into a sheet by a molding method such as extrusion melt molding, measured in accordance with ASTM D1525.
[0051] In addition, the resin sheet constituting the sealing material sheet for a self-luminous display body has a melt mass flow rate (MFR) at 190° C. of 0.1 g / 10 min or more and less than 12.0 g / 10 min, preferably 0.1 g / 10 min or more and less than 5.0 g / 10 min, and more preferably 0.1 g / 10 min or more and less than 0.5 g / 10 min. By making the MFR of the sealing material sheet 0.1 g / 10 min or more, the sealing material sheet for a self-luminous display body can be provided with the molding properties required.
[0052] Moreover, by making the MFR less than 12.0 g / 10 min, the uniformity of the thickness of the encapsulant sheet after heat pressing for integration into a self-luminous display device can be maintained at an extremely high level. In a self-luminous display such as the micro LED display device 100, the encapsulant sheet laminated on the light-emitting surface side of the LED element is required to have a particularly uniform thickness. This is because even a slight difference in thickness between the center and the edge of the encapsulant sheet causes the encapsulant sheet to become lenticular, which has an unintended and undesirable effect on the display quality of the micro LED display device.
[0053] In addition, by having the MFR of the encapsulant sheet be less than 12.0 g / 10 min, the fluidity of the material resin composition is reduced, and high-temperature film formation is possible during sheet extrusion molding, which is advantageous in that productivity is improved. Film formation at high temperatures makes it possible to reduce the torque of the extruder, making sheet molding easier. In addition, in the case of film formation at high temperatures, neck-in during sheet molding can be suppressed, making it possible to mold a wide sheet, and when a sheet is obtained, it is in a high-temperature molten state in the extruder, so gels and the like are less likely to occur, and unevenness is less likely to occur on the surface of the sheet, making it easy to obtain a good appearance.
[0054] In addition, when the MFR of the encapsulant is 12.0 g / 10 min or more, crosslinking is required with a crosslinking agent or the like to provide heat creep resistance, and the heat press processing conditions also need to be set individually according to the MFR, whereas when the MFR of the encapsulant is less than 12.0 g / 10 min, crosslinking is not required and the press conditions can be set in common. From these points of view, it is preferable that the encapsulant sheet has an MFR of less than 12.0 g / 10 min.
[0055] In this specification, the "MFR" of an encapsulant sheet refers to the MFR of an encapsulant sheet after completion of sheeting by forming an encapsulant composition containing a resin component and other additives into a sheet by a molding method such as extrusion melt molding, measured under conditions of 190°C and a load of 2.16 kg in accordance with JIS K7210. In addition, when the encapsulant sheet is a multilayer film, the MFR is measured by the above-mentioned process while the encapsulant sheet is in a multilayer state in which all layers are laminated together, and the measured value obtained is regarded as the MFR value of the multilayer encapsulant sheet.
[0056] The base resin of the encapsulant composition forming the encapsulant sheet can be selected from a wide range of olefin-based thermoplastic resins as long as the Vicat softening point and MFR are within the above ranges. Among them, polyethylene resins such as low-density polyethylene resins (LDPE), linear low-density polyethylene resins (LLDPE), and metallocene linear low-density polyethylene resins (M-LLDPE) can be preferably used. In this specification, the term "base resin" refers to the resin that has the largest content ratio among the resin components of a resin composition containing the base resin.
[0057] The density of the polyethylene resin used as the base resin of the encapsulant composition is 0.870 g / cm 3 More than 0.910g / cm 3 It is sufficient if it is less than or equal to 0.895 g / cm 3 More than 0.905g / cm 3 The density of the base resin of the encapsulant composition is 0.910 g / cm 3 By setting the density to 0.890 g / cm or less, the adhesion of the sealing material sheet to a wiring board or the like can be maintained within a preferable range. 3 By adjusting the above, the encapsulant sheet can be provided with necessary and sufficient heat resistance without undergoing a crosslinking treatment.
[0058] Here, one of the features of the encapsulant sheet of the present invention is that it is a thermoplastic encapsulant that does not require crosslinking treatment after film formation. As such an encapsulant sheet that does not require crosslinking treatment, a "weakly crosslinked encapsulant" obtained by weakly crosslinking a polyethylene-based encapsulant composition can also be used. "Weak crosslinking" is a crosslinking treatment technology related to a method for producing an encapsulant, the details of which are disclosed in International Publication No. 2011 / 152314, and is a technology in which a film of an encapsulant composition is formed while proceeding with very weak crosslinking while maintaining the gel fraction at 0%. In this specification, the encapsulant that has been weakly crosslinked and formed into a film through this weak crosslinking treatment is referred to as a "weakly crosslinked encapsulant". In addition, the weakly crosslinked encapsulant has been subjected to the weak crosslinking treatment at the time of film formation, and substantially no crosslinking agent remains after film formation. Therefore, a separate crosslinking treatment is not required in the manufacturing process of the self-luminous display.
[0059] This weakly cross-linked encapsulant has a density of 0.870 g / cm 3 More than 0.890g / cm 3 The sealing material composition for the light-receiving side sealing material, which contains the following polyethylene-based resin as a base resin and a very small amount of a crosslinking agent, can be obtained by carrying out the above-mentioned weak crosslinking treatment during film formation in the process of film formation by a conventionally known method.
[0060] It is more preferable that the encapsulant composition contains a certain amount of a silane copolymer (hereinafter also referred to as "silane-modified polyethylene resin") obtained by copolymerizing an α-olefin and an ethylenically unsaturated silane compound as a comonomer in each encapsulant composition as necessary. The silane-modified polyethylene resin is obtained by graft polymerization of an ethylenically unsaturated silane compound as a side chain to a linear low-density polyethylene resin (LLDPE) or the like that serves as a main chain. Such a graft copolymer increases the degree of freedom of the silanol group that contributes to the adhesive force, and therefore can improve the adhesiveness of the encapsulant sheet 1 to other members in the solar cell module. The content of this silane-modified polyethylene resin in the encapsulant composition is preferably 2% by mass or more and 20% by mass or less in the encapsulant composition for the core layer, and 5% by mass or more and 40% by mass or less in the encapsulant composition for the skin layer. In particular, it is more preferable that the encapsulant composition for the skin layer contains 10% or more of silane-modified polyethylene. The amount of silane modification in the silane-modified polyethylene resin is preferably about 1.0% by mass or more and 3.0% by mass or less. The preferred range of the content of the silane-modified polyethylene resin in the encapsulant composition is based on the premise that the amount of silane modification is within this range, and it is desirable to appropriately fine-tune the content depending on the variation of the amount of modification.
[0061] The silane-modified polyethylene resin can be produced, for example, by the method described in JP-A-2003-46105. By using the resin as a component of an encapsulant composition for solar cell modules, it is possible to produce solar cell modules that are excellent in strength, durability, etc., as well as in weather resistance, heat resistance, water resistance, light resistance, wind pressure resistance, hail resistance, and other properties, and that further have extremely excellent heat fusion properties without being affected by manufacturing conditions such as heat compression bonding used to produce the solar cell module, and that are suitable for a variety of applications, making it possible to stably produce solar cell modules at low cost. EXAMPLES
[0062] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0063] <Production of sealing material sheet for self-luminous display body> The following encapsulant compositions prepared for each Example and Comparative Example were formed into sheets using a film forming machine having a φ30 mm extruder and a 200 mm wide T-die at an extrusion temperature of 210° C., a take-up speed of 1.1 m / min, and a film thickness of 400 μm to produce encapsulant sheets for each Example and Comparative Example. Regarding the cooling roll and rubber roll immediately below the T-die, the cooling roll was a chrome-plated cooling roll with a surface roughness of Rz 1.5 μm, and the rubber roll was a silicone rubber roll with a hardness of 70 degrees.
[0064] (Sealing material sheet of Example 1 (1-1 to 1-2)) The following base resin 1 was mixed with 100 parts by mass of the following additive resin 1 (weather resistance master batch) and 20 parts by mass of the following additive resin 2 (silane-modified polyethylene resin) in a ratio of 5 parts by mass to 100 parts by mass of the following base resin 1, to obtain an encapsulant composition for molding the encapsulant sheet of Example 1 (1-1 to 1-2). Base Resin 1 :Density 0.901g / cm 3 A metallocene-based linear low-density polyethylene resin (M-LLDPE) with a melting point of 93°C and an MFR of 2.0g / 10min at 190°C. Additive resin 1 (weather resistant masterbatch) :Density 0.919g / cm 3 For 100 parts by mass of low-density polyethylene resin with MFR of 3.5 g / 10 min at 190°C, KEMISTAB62 (HALS): 0.6 parts by mass, KEMISORB12 (UV absorber): 3.5 parts by mass, and KEMISORB79 (UV absorber): 0.6 parts by mass. Additive resin 2 (Silane-modified polyethylene resin) :Density 0.900g / cm 3 A silane-modified polyethylene resin was obtained by mixing 2 parts by mass of vinyltrimethoxysilane and 0.15 parts by mass of dicumyl peroxide as a radical generator (reaction catalyst) with 100 parts by mass of a metallocene-based linear low-density polyethylene resin having an MFR of 2.0 g / 10 min, and melting and kneading the mixture at 200°C. The density of this additive resin 2 was 0.901 g / cm. 3, MFR is 1.0g / 10min.
[0065] (Sealing material sheet of Example 2 (2-1 to 2-2)) The following base resin 2 was mixed with 100 parts by mass of the above-mentioned additive resin 1 (weather resistance master batch) and 20 parts by mass of the above-mentioned additive resin 2 (silane-modified polyethylene resin) in a ratio of 5 parts by mass to 100 parts by mass of the below-mentioned base resin 2 to obtain an encapsulant composition for molding the encapsulant sheet of Example 2 (2-1 to 2-2). Base resin 2: Density 0.898g / cm 3 A metallocene-based linear low-density polyethylene resin (M-LLDPE) with an MFR of 3.5 g / 10 min at 190°C.
[0066] (Sealing material sheet of Example 3 (3-1 to 3-2)) The following base resin 3 was mixed with 100 parts by mass of the above-mentioned additive resin 1 (weather resistance master batch) and 20 parts by mass of the above-mentioned additive resin 2 (silane-modified polyethylene resin) in a ratio of 5 parts by mass to 100 parts by mass of the below-mentioned base resin 3 to obtain an encapsulant composition for molding the encapsulant sheet of Example 3 (3-1 to 3-2). Base resin 3: Density 0.905g / cm 3 A metallocene-based linear low-density polyethylene resin (M-LLDPE) with an MFR of 3.5 g / 10 min at 190°C.
[0067] (Sealing material sheet of Example 4 (4-1 to 4-2)) The following base resin 4 was mixed with 100 parts by mass of the above-mentioned additive resin 1 (weather resistance master batch) and 20 parts by mass of the above-mentioned additive resin 2 (silane-modified polyethylene resin) in a ratio of 5 parts by mass to 100 parts by mass of the below-mentioned base resin 4 to obtain an encapsulant composition for molding the encapsulant sheet of Example 4 (4-1 to 4-2). Base resin 4: Density 0.919g / cm 3 A metallocene-based linear low-density polyethylene resin (M-LLDPE) with an MFR of 3.5 g / 10 min at 190°C.
[0068] (Sealing material sheet of Example 5 (5-1 to 5-2)) The following base resin 5 was mixed with 97 parts by mass of the above-mentioned additive resin 1 (weather resistance agent master batch 1-2) and 5 parts by mass of the above-mentioned additive resin 2 (silane-modified polyethylene resin) in a ratio of 5 parts by mass to obtain an encapsulant composition for molding the encapsulant sheet of Example 5 (5-1 to 5-2), which is a weakly crosslinked encapsulant sheet. Base resin 5: 0.880g / cm 3 A compound pellet obtained by impregnating 100 parts by mass of M-LLDPE pellets having an MFR of 3.5 g / 10 min at 190°C with 0.041 parts by mass of 2,5-dimethyl-2,5-di(t-butylperoxy)hexane.
[0069] <Production of sealing materials> The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0070] (Sealing material sheet of Comparative Example 1 (1-1 to 1-2)) The following base resin 6 was mixed with 100 parts by mass of the above-mentioned additive resin 1 (weather resistance master batch) and 20 parts by mass of the above-mentioned additive resin 2 (silane-modified polyethylene resin) in a ratio of 5 parts by mass to 100 parts by mass of the below-mentioned base resin 6, to obtain an encapsulant composition for molding the encapsulant sheet of Comparative Example 1 (1-1 to 1-2). Base resin 6: Density 0.880g / cm 3 A metallocene-based linear low-density polyethylene resin (M-LLDPE) with an MFR of 2.2 g / 10 min at 190°C.
[0071] (Sealing material sheet of Comparative Example 2) The following base resin 7 was mixed with 100 parts by mass of the above-mentioned additive resin 1 (weather resistance master batch) and 10 parts by mass of the above-mentioned additive resin 2 (silane-modified polyethylene resin) in a ratio of 3 parts by mass to 10 parts by mass of the below-mentioned base resin 7 to obtain an encapsulant composition for molding the encapsulant sheet of Comparative Example 2. Base resin 7: Density 0.910g / cm 3 A metallocene-based linear low-density polyethylene resin (M-LLDPE) having an MFR of 15.0 g / 10 min at 190°C.
[0072] (Sealing material sheet of Comparative Example 3) The following base resin 8 was mixed with 100 parts by mass of the above-mentioned additive resin 1 (weather resistance master batch) and 20 parts by mass of the above-mentioned additive resin 2 (silane-modified polyethylene resin) in a ratio of 5 parts by mass to 100 parts by mass of the below-mentioned base resin 8, to obtain an encapsulant composition for molding the encapsulant sheet of Comparative Example 2. Base resin 8: Density 0.913g / cm 3 A metallocene-based linear low-density polyethylene resin (M-LLDPE) with an MFR of 2.4 g / 10 min at 190°C.
[0073] <Vicat softening point of sealing material sheet> The Vicat softening point of each of the encapsulant sheets of the Examples and Comparative Examples was measured in accordance with ASTM D 1525. The results are shown in Table 1.
[0074] <MFR of encapsulant sheet> The MFR of each of the encapsulant sheets of the Examples and Comparative Examples was measured in accordance with JIS K7210 under conditions of 190° C. and a load of 2.16 kg. The results are shown in Table 1.
[0075] <Evaluation Example 1: Blocking resistance> The blocking resistance of each of the encapsulant sheets of the Examples and Comparative Examples was evaluated by the following test method. [Blocking resistance test] (Test Method) The blocking property of each of the encapsulant sheets in the Examples and Comparative Examples was measured in accordance with ASTM D395 using a blocking tester, a CO-201 permanent deformation tester (constant load type) manufactured by Tester Sangyo Co., Ltd. A load of 5 kg was applied using a large test piece of 29 mmφ, and the cooling roll surface side during film formation was aligned with the rubber roll surface side. Each of the encapsulant sheets was cut to a size of 5 x 5 cm and sandwiched between the large test pieces of 29 mmφ. The sheets were placed in a 40°C, 90% humidity oven for 48 hours, and the blocking state after 24 hours at 23°C, 50% was confirmed. (Evaluation Criteria) A: Peeling occurred without applying any force. B: Force was applied when peeling. C: When force was applied during peeling, it was observed that part of one of the sealing materials laminated on the peeled surface was dislocated to the other and adhered thereto. The evaluation results are shown in Table 1 as "blocking resistance."
[0076] <Evaluation Example 2: Molding property> For each of the encapsulant sheets of the Examples and Comparative Examples, the molding properties for various uneven surfaces were evaluated by the following test method. [Creating a module for molding test] Sample 1 (marked as "minor" in the module unevenness column in Table 1) An LED module was prepared in which micro-sized LED elements, 25 μm wide × 15 μm deep × 2.5 μm high, were arranged at a pitch of 2 mm on the surface of a glass epoxy wiring board measuring 200 × 300 mm. A 300 μm-thick encapsulant sheet of any one of the examples or comparative examples was laminated on the surface of the module on which the LED elements were arranged. Furthermore, a 50 μm-thick ethylene tetrafluoroethylene (ETFE) film that had been corona-treated on one side was laminated on top of the encapsulant sheet as a surface protection film. A vacuum lamination process was then performed using a vacuum laminator used for manufacturing solar cell modules under conditions of a temperature of 150°C, a vacuum drawing time of 5 minutes, a press holding time of 10 minutes, and an upper chamber pressure of 70 KPa, to produce a module (sample 1) for a molding property test. Sample 2 (marked as "small" in the module unevenness table in Table 1) A molding test module (sample 2) was fabricated using the same materials and method as sample 1, except that the size of the LED elements was 100 μm wide x 200 μm deep x 100 μm high, and the arrangement pitch was 10 mm. [Molding test] Each of the test modules was visually observed and the molding characteristics were evaluated according to the following evaluation criteria. (Evaluation Criteria) A: The encapsulant sheet perfectly conforms to the unevenness of the LED element mounting surface. No voids were observed. B: 2mm 2Up to 3 bubbles were observed. C: A part of the encapsulant sheet does not completely conform to the unevenness of the LED element arrangement surface facing it, Some lamination defects (voids) were formed near the elements. The evaluation results are shown in Table 1 as "molding property."
[0077] <Evaluation Example 3: Film thickness uniformity> For each of the encapsulant sheets of the Examples and Comparative Examples, the uniformity of the film thickness after vacuum lamination in the above molding test was measured and evaluated using each of the above test modules according to the following test method. [Film thickness uniformity test] Each encapsulant sheet of the Examples and Comparative Examples was cut to 30×30 cm, and 50 μm of untreated ETFE was laminated as a release film on both sides thereof, and then a laminate of 30×30 cm and 3 mm thick glass was laminated on both sides thereof to form a laminate, and this laminate was subjected to a vacuum lamination process under the same conditions as in Evaluation Example 2. After cooling, the glass and ETFE were peeled off, and the thickness of the encapsulant was measured at two points, the center part and a point 2 cm from the corner toward the center, with a digital thickness meter, and the thickness uniformity was evaluated according to the following evaluation criteria. (Evaluation Criteria) A: The difference in thickness between the center and 2 cm from the corner is less than 12 microns (3%). B: The difference in thickness between the center and a point 2 cm from the corner is 12 microns (3%) or more and less than 32 microns (8%). C: The difference in thickness between the center and 2 cm from the corner is 32 microns (8%) or more. The evaluation results are shown in Table 1 as "film thickness uniformity."
[0078] [Table 1]
[0079] From Table 1, it can be seen that the encapsulant sheet of the present invention has sufficient molding properties for finely uneven surfaces and excellent film thickness uniformity, and is suitable for use in various self-luminous display devices such as micro LED televisions. [Explanation of symbols]
[0080] 1. Encapsulating material sheet 2 Display panel 10 LED elements 11 LED light emitting chip 12 Resin cover 20 Wiring board 21 Support substrate 22 Wiring section 23 Solder layer 30 LED module for self-luminous display 100, 100A, 100B Micro LED display device (self-luminous display)
Claims
1. A resin sheet having a metallocene-based linear low-density polyethylene resin as a base resin, The Vicat softening point is greater than 60°C and less than 90°C, The MFR at 190° C. is 0.1 g / 10 min or more and less than 12.0 g / 10 min, The thickness uniformity is less than 8% as measured by the thickness uniformity test described below. Sealing material sheet for self-luminous displays. (Thickness uniformity test) A 50 μm untreated ETFE is laminated as a release film on the front and back of a sealing material sheet cut to 30×30 cm, and then a 3 mm thick glass is laminated on the front and back to form a laminate, and this laminate is vacuum laminated under the same conditions. After cooling, the glass and ETFE are peeled off, and the thickness of the sealing material is measured with a digital thickness meter at the center and at a point 2 cm away from the corner toward the center. The thickness difference (%) at the above two points of the sealing material measured in this way is called "thickness uniformity".
2. The sealing material sheet according to claim 1, having an MFR at 190°C of less than 5.0 g / 10 min.
3. The sealing material sheet according to claim 2 , having an MFR at 190° C. of less than 0.5 g / 10 min.
4. a light-emitting module for a self-luminous display, the light-emitting module being configured by mounting a plurality of light-emitting elements on a wiring board; a sealing material that covers the light-emitting element and is laminated on a mounting surface of the wiring board on which the light-emitting element is mounted; A display panel laminated on a surface of the sealing material, The encapsulant is the encapsulant sheet according to claim 1 .
5. The self-luminous display according to claim 4 , wherein the light-emitting element is an LED element.
6. The LED element has an LED chip and a resin cover that covers the LED chip, The LED element has a width and a depth of 300 μm or less, and a height of 200 μm or less, 6. The self-luminous display according to claim 5, wherein the LED elements are arranged at intervals of 0.03 mm or more and 100 mm or less.
7. The width and depth of the LED element are both 50 μm or less, and the height is 10 μm or less, 7. The self-luminous display according to claim 6, wherein the LED elements are arranged at intervals of 0.05 mm to 5 mm.
8. 8. The self-luminous display according to claim 4, wherein a plurality of the light-emitting modules have a light-emitting surface formed by bonding the light-emitting modules together on the same plane, and the sealing material sheet is laminated on the light-emitting surface.
Citation Information
Patent Citations
Optical semiconductor sealing sheet and optical semiconductor element
JP2009084511A
Light emitting device and method of manufacturing the same
JP2011171357A
Thermosetting resin composition, and optical element comprising cured product of the same
JP2012126896A
Film-like sealing material for electronic device, sealing sheet for electronic device and electronic device
JP2014148584A
Light-emitting element reflection bank structure
JP2016503958A