Lithium secondary battery

The lithium secondary battery design with a smaller positive electrode active material layer and a functional layer on the solid electrolyte's surfaces addresses inefficiencies in charge/discharge efficiency by preventing short circuits and reducing electrolyte decomposition, leading to improved battery performance.

JP7582453B2Active Publication Date: 2024-11-13NISSAN MOTOR CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023511076
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-03
Filing Date
2022-03-23
Publication Date
2024-11-13
Estimated Expiration
2042-03-23

AI Technical Summary

Technical Problem

Existing lithium deposition type lithium secondary batteries do not achieve sufficient charge/discharge efficiency despite advancements in technology.

Method used

A lithium secondary battery design with a positive electrode active material layer smaller than the solid electrolyte layer, incorporating a functional layer with electronic insulation and lithium ion conductivity on the solid electrolyte's main surface facing the negative electrode current collector and side surfaces, and a pressure member to prevent lithium metal contact with the positive electrode active material layer.

Benefits of technology

This configuration enhances charging and discharging efficiency by preventing short circuits and reducing reductive decomposition of the solid electrolyte, thereby improving the battery's overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582453000004
    Figure 0007582453000004
  • Figure 0007582453000005
    Figure 0007582453000005
  • Figure 0007582453000006
    Figure 0007582453000006
Patent Text Reader

Abstract

Provided is a lithium secondary battery comprising: a power generation element including a positive electrode in which a positive electrode active material layer containing a positive electrode active material capable of absorbing and releasing lithium ions is disposed on a surface of a positive electrode collector, a negative electrode which has a negative electrode collector and in which lithium metal is deposited on the negative electrode collector during charging, and a solid electrolyte layer which is interposed between the positive electrode and the negative electrode and which contains a solid electrolyte; and a pressing member that presses with a predetermined pressure the power generation element in a layering direction. The lithium secondary battery, wherein: when the power generation element is viewed in plan view, at least a portion of an outer peripheral edge of the positive electrode active material layer is positioned more toward the inside than an outer peripheral edge of the solid electrolyte layer; and a first functional layer, which has electron insulating properties and lithium ion conducting properties and which is more stable than the solid electrolyte in terms of reductive decomposition caused by contact with the lithium metal, is provided to at least a portion of a primary surface of the solid electrolyte layer opposing the negative electrode collector and to at least a portion of a side surface of the solid electrolyte layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lithium secondary battery. [Background technology]

[0002] In recent years, there has been a strong desire to reduce carbon dioxide emissions in order to combat global warming. In the automobile industry, there are high hopes for a reduction in carbon dioxide emissions through the introduction of electric vehicles (EVs) and hybrid electric vehicles (HEVs), and the development of non-aqueous electrolyte secondary batteries, such as motor drive secondary batteries, which hold the key to putting these vehicles to practical use, is being actively pursued.

[0003] Secondary batteries for driving motors are required to have extremely high output characteristics and high energy compared to consumer lithium-ion secondary batteries used in mobile phones, notebook computers, etc. Therefore, lithium-ion secondary batteries, which have the highest theoretical energy of all practical batteries, have attracted attention and are currently being rapidly developed.

[0004] Currently, lithium-ion secondary batteries in widespread use use flammable organic electrolytes as electrolytes, and for these liquid-based lithium-ion secondary batteries, stricter safety measures against leakage, short circuits, overcharging, etc. are required than for other batteries.

[0005] In recent years, therefore, research and development into all-solid-state lithium secondary batteries that use oxide- or sulfide-based solid electrolytes has been actively conducted. A solid electrolyte is a material that is mainly composed of ion conductors that can conduct ions in a solid state. For this reason, in principle, all-solid-state lithium secondary batteries do not have the various problems caused by flammable organic electrolytes that occur in conventional liquid-based lithium-ion secondary batteries. In addition, in general, the use of high-potential, large-capacity positive electrode materials and large-capacity negative electrode materials can significantly improve the output density and energy density of the battery.

[0006] Conventionally, as one type of all-solid-state lithium secondary battery, a so-called lithium precipitation type battery is known in which lithium metal is precipitated on a negative electrode current collector during charging (see, for example, JP 2019-61867 A). In the charging process of such a lithium precipitation type all-solid-state lithium secondary battery, lithium metal is precipitated between a solid electrolyte layer and a negative electrode current collector. In the lithium secondary battery described in JP 2019-61867 A, an electrolyte layer interposed between a positive electrode containing lithium and a negative electrode containing lithium is composed of an electrolyte layer made of a first electrolyte and a second electrolyte containing iodine provided between the electrolyte layer and the negative electrode, and is configured so that the ion conductivity of the second electrolyte is smaller than the ion conductivity of the first electrolyte. According to JP 2019-61867 A, by adopting such a configuration, even if the interface between the electrolyte layer and the negative electrode is not flat, uneven precipitation of lithium is eliminated and the generation of dendrites is suppressed. As a result, it is believed that the variation in internal resistance and the decrease in discharge capacity caused by the growth of lithium dendrites are improved, making it possible to provide a lithium battery with excellent charge and discharge characteristics. Summary of the Invention [Problem to be solved by the invention]

[0007] However, according to the studies of the present inventors, it has been found that even if the technology described in JP 2019-61867 A is used, there are still cases where sufficient charge / discharge efficiency cannot be achieved.

[0008] Therefore, an object of the present invention is to provide a means for further improving the charge / discharge efficiency in a lithium deposition type lithium secondary battery. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to solve the above problems, and as a result, have found that in a secondary battery including a lithium deposition-type power generating element and a pressure member that presses the power generating element in a stacking direction, the above problems can be solved by making the positive electrode active material layer slightly smaller than the solid electrolyte layer and providing a predetermined functional layer on at least a part of a main surface of the solid electrolyte layer that faces the negative electrode current collector and on at least a part of a side surface of the solid electrolyte layer, thereby completing the present invention.

[0010] That is, one aspect of the present invention relates to a lithium secondary battery including a power generating element having a positive electrode in which a positive electrode active material layer containing a positive electrode active material capable of absorbing and releasing lithium ions is disposed on the surface of a positive electrode current collector, a negative electrode having a negative electrode current collector and in which lithium metal is deposited on the negative electrode current collector during charging, and a solid electrolyte layer containing a solid electrolyte interposed between the positive electrode and the negative electrode, and a pressing member for pressing the power generating element with a predetermined pressure in the stacking direction. In the lithium secondary battery, when the power generating element is viewed in plan, at least a part of the outer circumferential edge of the positive electrode active material layer is located inside the outer circumferential edge of the solid electrolyte layer. The lithium secondary battery is also characterized in that a first functional layer having electronic insulation and lithium ion conductivity and being more stable than the solid electrolyte in terms of reductive decomposition due to contact with the lithium metal is provided on at least a part of the main surface of the solid electrolyte layer facing the negative electrode current collector and at least a part of the side surface of the solid electrolyte layer. Effect of the Invention

[0011] According to the present invention, the charge / discharge efficiency of a lithium deposition type lithium secondary battery can be further improved. [Brief description of the drawings]

[0012] [Figure 1] 1 is a cross-sectional view showing a schematic overall structure of a stacked-type (internal parallel connection type) all-solid-state lithium secondary battery (stacked-type secondary battery) according to one embodiment of the present invention. [Diagram 2]2 is an enlarged cross-sectional view of a unit cell layer of a stacked secondary battery according to one embodiment of the present invention, which corresponds to the configuration of an evaluation cell produced in Example 1 described later. [Diagram 3] 3 is an enlarged cross-sectional view of a unit cell layer showing a modified example of a stacked secondary battery according to the present invention, which corresponds to the configuration of an evaluation cell produced in Example 5 described later. [Figure 4] 1 is a perspective view of a stacked secondary battery according to one embodiment of the present invention; [Diagram 5] FIG. 5 is a side view seen from a direction A shown in FIG. [Figure 6] 6 is an enlarged cross-sectional view of a unit cell layer showing a modified example of a stacked secondary battery according to the present invention, which corresponds to the configuration of an evaluation cell produced in Example 2 described later. [Figure 7] 7 is an enlarged cross-sectional view of a unit cell layer showing a modified example of a stacked secondary battery according to the present invention, which corresponds to the configuration of an evaluation cell produced in Example 3 described later. [Figure 8] 1 is a perspective view showing the appearance of a stacked secondary battery according to one embodiment of the present invention; [Figure 9] 9 is an enlarged cross-sectional view of a unit cell layer showing a modified example of a stacked secondary battery according to the present invention, which corresponds to the configuration of an evaluation cell produced in Example 4 described later. [Figure 10] 10 is an enlarged cross-sectional view of a unit cell layer showing an example of a stacked-type secondary battery not according to the present invention, which corresponds to the configuration of an evaluation cell produced in Comparative Example 1 described later. [Figure 11] 11 is an enlarged cross-sectional view of a unit cell layer showing an example of a stacked-type secondary battery not according to the present invention, which corresponds to the configuration of an evaluation cell produced in Comparative Example 2 described later. [Figure 12] 12 is an enlarged cross-sectional view of a unit cell layer showing an example of a stacked-type secondary battery not according to the present invention, which corresponds to the configuration of an evaluation cell produced in Comparative Example 3 described later. [Figure 13] 13 is an enlarged cross-sectional view of a unit cell layer showing an example of a stacked-type secondary battery not according to the present invention, which corresponds to the configuration of an evaluation cell produced in Comparative Example 4 described later. [Figure 14] 14 is an enlarged cross-sectional view of a unit cell layer showing a modified example of a stacked secondary battery according to the present invention, which corresponds to the configuration of an evaluation cell produced in Example 14 described later. [Figure 15] 15 is an enlarged cross-sectional view of a unit cell layer showing a modified example of a stacked secondary battery according to the present invention, which corresponds to the configuration of an evaluation cell produced in Example 18 described later. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] One embodiment of the present invention is a lithium secondary battery comprising: a positive electrode formed by disposing a positive electrode active material layer containing a positive electrode active material capable of absorbing and releasing lithium ions on a surface of a positive electrode current collector; a negative electrode having a negative electrode current collector and in which lithium metal is deposited on the negative electrode current collector during charging; and a solid electrolyte layer interposed between the positive electrode and the negative electrode and containing a solid electrolyte; and a pressurizing member for pressing the power generating element with a predetermined pressure in a stacking direction, wherein, when the power generating element is viewed in plan, at least a part of the outer circumferential edge of the positive electrode active material layer is located inside the outer circumferential edge of the solid electrolyte layer, and a first functional layer having electronic insulation and lithium ion conductivity and being more stable than the solid electrolyte in terms of reductive decomposition due to contact with the lithium metal is provided on at least a part of a main surface of the solid electrolyte layer facing the negative electrode current collector and at least a part of a side surface of the solid electrolyte layer. The lithium secondary battery according to this embodiment can further improve the charge and discharge efficiency in a lithium deposition type lithium secondary battery.

[0014] The present embodiment will be described below with reference to the drawings, but the technical scope of the present invention should be determined based on the description of the claims, and is not limited to the following embodiment. Note that the dimensional ratios in the drawings are exaggerated for the convenience of explanation and may differ from the actual ratios.

[0015] FIG. 1 is a cross-sectional view showing a schematic overall structure of a stacked type (internal parallel connection type) all-solid-state lithium secondary battery (hereinafter, also simply referred to as a "stacked type secondary battery") according to one embodiment of the present invention. The stacked type secondary battery 10a shown in FIG. 1 has a structure in which a substantially rectangular power generating element 21, in which a charge / discharge reaction actually proceeds, is sealed inside a laminate film 29 that is a battery exterior body. Note that FIG. 1 shows a cross section of the stacked type secondary battery during charging, and therefore, a negative electrode active material layer 13 made of lithium metal is present between the negative electrode current collector 11' and the solid electrolyte layer 17. In addition, a restraining pressure is applied to the stacked type secondary battery 10a by a pressure member in the stacking direction of the power generating element 21 (not shown). Therefore, the volume of the power generating element 21 is kept constant.

[0016] As shown in FIG. 1, a power generating element 21 of a stacked secondary battery 10a of this embodiment has a configuration in which a negative electrode in which a negative electrode active material layer 13 containing lithium metal is arranged on both sides of a negative electrode collector 11′, a solid electrolyte layer 17, and a positive electrode in which a positive electrode active material layer 15 containing a lithium transition metal composite oxide is arranged on both sides of a positive electrode collector 11″ are stacked. Specifically, the negative electrode, the solid electrolyte layer, and the positive electrode are stacked in this order such that one negative electrode active material layer 13 and an adjacent positive electrode active material layer 15 face each other with the solid electrolyte layer 17 interposed therebetween. As a result, the adjacent negative electrode, solid electrolyte layer, and positive electrode constitute one unit cell layer 19. Therefore, the stacked secondary battery 10a shown in FIG. 1 can also be said to have a configuration in which a plurality of unit cell layers 19 are stacked and electrically connected in parallel.

[0017] A negative current collector 25 and a positive current collector 27 which are electrically connected to the electrodes (negative and positive) are attached to the negative current collector 11' and the positive current collector 11", respectively, and are structured to be sandwiched between the ends of the laminate film 29 and led out of the laminate film 29. The negative current collector 25 and the positive current collector 27 may be attached to the negative current collector 11' and the positive current collector 11" of the electrodes by ultrasonic welding, resistance welding, or the like, respectively, via a negative terminal lead and a positive terminal lead (not shown) as necessary.

[0018] FIG. 2 is an enlarged cross-sectional view of a single cell layer 19 of a stacked secondary battery according to an embodiment of the present invention. As shown in FIG. 2, the single cell layer 19 constituting the stacked secondary battery 10a according to this embodiment has a positive electrode constituted by a positive electrode current collector 11" and a positive electrode active material layer 15 disposed on the surface thereof. A solid electrolyte layer 17 containing a solid electrolyte is disposed on the surface of the positive electrode active material layer 15 opposite to the positive electrode current collector 11". Here, in the embodiment shown in FIG. 2, the outer peripheral edge portion of the solid electrolyte layer 17 extends to the side surface of the positive electrode active material layer 15 over its entire circumference. As a result, the positive electrode active material layer 15 is configured to be one size smaller than the solid electrolyte layer 17. That is, when the power generating element 21 is viewed in plan, the entire circumference of the outer peripheral end of the positive electrode active material layer 15 is configured to be located inside the outer peripheral end of the solid electrolyte layer 17. With this configuration, even if the lithium metal constituting the negative electrode active material layer 13 is pushed out from the outer peripheral end of the solid electrolyte layer 17 toward the positive electrode active material layer 15 by the restraining pressure of the pressing member, the lithium metal is less likely to come into contact with the side surface of the positive electrode active material layer 15. As a result, the effect of preventing a short circuit is further enhanced. Note that the "side surface of the positive electrode active material layer" means the surface of the positive electrode active material layer that is not in contact with the positive electrode current collector and does not face the negative electrode current collector. Here, as shown in FIG. 3, the outer peripheral edge portion of the solid electrolyte layer 17 does not have to extend to the side surface of the positive electrode active material layer 15. However, even in this case, as shown in FIG. 3, when the power generating element 21 is viewed in plan, at least a part of the outer peripheral end of the positive electrode active material layer 15 needs to be configured to be located inside the outer peripheral end of the solid electrolyte layer 17. This is because even if the lithium metal constituting the negative electrode active material layer 13 is pushed out from the outer peripheral edge of the solid electrolyte layer 17 toward the positive electrode active material layer 15 due to the restraining pressure of the pressure member, the lithium metal is less likely to come into contact with the side surface of the positive electrode active material layer 15, and a short circuit can be prevented.

[0019] In the embodiment shown in FIG. 2, a first functional layer 18 is provided on the entire main surface of the solid electrolyte layer 17 facing the negative electrode current collector 11′ and on the entire side surface of the solid electrolyte layer 17. The "side surface of the solid electrolyte layer" means a surface of the solid electrolyte layer that does not face either the positive electrode active material layer or the negative electrode current collector during discharge when the negative electrode active material layer 13 made of lithium metal is not present. The first functional layer 18 is a layer having electronic insulation and lithium ion conductivity. The first functional layer 18 is characterized in that it is more stable than the solid electrolyte constituting the solid electrolyte layer 17 with respect to reductive decomposition due to contact with lithium metal. In the embodiment shown in FIG. 2, the first functional layer 18 is made of lithium fluoride (LiF). By disposing such a first functional layer on the side surface of the solid electrolyte layer, even when the lithium metal deposited on the surface of the negative electrode current collector during charging is pushed out from the outer peripheral edge of the solid electrolyte layer by the restraining pressure of the pressing member, contact between the solid electrolyte layer and the negative electrode active material layer is prevented, and deterioration of the solid electrolyte layer due to reductive decomposition is suppressed. In addition, since the effective area of ​​the lithium metal facing the positive electrode active material layer via the first functional layer and the solid electrolyte layer is increased, there is an advantage that the charge / discharge efficiency is further improved.

[0020] Further, in the embodiment shown in FIG. 2, the negative electrode current collector 11' is configured to be slightly smaller than the solid electrolyte layer 17. The negative electrode current collector 11' is configured to be slightly larger than the positive electrode active material layer 15. That is, when the power generating element 21 is viewed in plan, the entire circumference of the outer periphery of the negative electrode current collector 11' is located inside the outer periphery of the solid electrolyte layer 17 and outside the outer periphery of the positive electrode active material layer 15. With this configuration, it is possible to prevent the occurrence of a short circuit caused by the negative electrode active material layer 13 made of lithium metal going beyond the outer periphery of the solid electrolyte layer 17 and wrapping around to the positive electrode active material layer 15 side while suppressing the occurrence of dendrites made of lithium metal at the end of the negative electrode. However, depending on the case, the negative electrode current collector 11' may be configured to be the same size as or slightly larger than the solid electrolyte layer 17, or may be configured to be the same size as or slightly smaller than the positive electrode active material layer 15.

[0021] Fig. 4 is a perspective view of a stacked secondary battery according to one embodiment of the present invention, and Fig. 5 is a side view seen from direction A shown in Fig. 4.

[0022] As shown in Fig. 4 and Fig. 5, the stacked secondary battery 100 according to this embodiment includes the power generating element 21 sealed in the laminate film 29 shown in Fig. 1, two metal plates 200 sandwiching the power generating element 21 sealed in the laminate film 29, and a bolt 300 and a nut 400 as fastening members. The fastening members (bolt 300 and nut 400) have a function of fixing the power generating element 21 sealed in the laminate film 29 in a sandwiched state between the metal plates 200. As a result, the metal plates 200 and the fastening members (bolt 300 and nut 400) function as pressure members that press (restrain) the power generating element 21 in its stacking direction. The pressure members are not particularly limited as long as they are members that can press the power generating element 21 in its stacking direction. As the pressure members, a combination of a plate made of a material having rigidity such as the metal plate 200 and the above-mentioned fastening members is typically used. As for the fastening members, in addition to the bolts 300 and nuts 400, tension plates or the like that fix the ends of the metal plates 200 so as to restrain the power generating element 21 in the stacking direction may be used.

[0023] The lower limit of the load applied to the power generating element 21 (restraint pressure in the stacking direction of the power generating element) is, for example, 0.1 MPa or more, preferably 1 MPa or more, more preferably 3 MPa or more, and even more preferably 5 MPa or more. The upper limit of the restraint pressure in the stacking direction of the power generating element is, for example, 100 MPa or less, preferably 70 MPa or less, more preferably 40 MPa or less, and even more preferably 10 MPa or less.

[0024] The main components of the above-mentioned stacked secondary battery 10a will now be described.

[0025] [Positive electrode current collector] The positive electrode current collector is a conductive member that functions as a flow path for electrons that are discharged from the positive electrode toward an external load or flow from a power source toward the positive electrode as the battery reaction (charge / discharge reaction) progresses. There is no particular limitation on the material that constitutes the positive electrode current collector. For example, metals and conductive resins can be used as the material that constitutes the positive electrode current collector. There is no particular limitation on the thickness of the positive electrode current collector, but an example is 10 to 100 μm.

[0026] [Cathode active material layer] The positive electrode constituting the lithium secondary battery according to this embodiment has a positive electrode active material layer containing a positive electrode active material capable of absorbing and releasing lithium ions. The positive electrode active material layer 15 is disposed on the surface of a positive electrode current collector 11″ as shown in FIG. 1.

[0027] The positive electrode active material is not particularly limited as long as it is a material that can release lithium ions during the charging process of the secondary battery and absorb lithium ions during the discharging process. An example of such a positive electrode active material is one that contains an M1 element and an O element, and the M1 element contains at least one element selected from the group consisting of Li, Mn, Ni, Co, Cr, Fe, and P. An example of such a positive electrode active material is LiCoO 2 , LiMnO 2 , LiNiO 2 , Li(Ni-Mn-Co)O 2 Layered rock salt active materials such as LiMn 2 O 4 , LiNi 0.5 Mn 1.5 O 4 Spinel-type active materials such as LiFePO 4 , LiMnPO 4 Olivine-type active materials such as Li 2 FeSiO 4 , Li 2 MnSiO 4 Examples of oxide active materials other than those mentioned above include Si-containing active materials such as Li 4 Ti 5 O 12 , LiVO 2In some cases, two or more kinds of positive electrode active materials may be used in combination. Of course, a positive electrode active material other than the above may be used. In a preferred embodiment, the positive electrode active material layer 15 constituting the lithium secondary battery according to this embodiment is made of a layered rock salt type active material containing lithium and cobalt (for example, Li(Ni-Mn-Co)O 2 ).

[0028] The content of the positive electrode active material in the positive electrode active material layer is not particularly limited, but is, for example, preferably in the range of 30 to 99 mass %, more preferably in the range of 40 to 90 mass %, and even more preferably in the range of 45 to 80 mass %.

[0029] In the lithium secondary battery according to this embodiment, the positive electrode active material layer 15 preferably further contains a solid electrolyte. Examples of the solid electrolyte include a sulfide solid electrolyte, a resin solid electrolyte, and an oxide solid electrolyte. As the solid electrolyte, a material having a desired bulk modulus can be appropriately selected according to the degree of volume expansion accompanying charge and discharge of the electrode active material used.

[0030] In a preferred embodiment of the secondary battery according to the present invention, the solid electrolyte preferably includes a resin solid electrolyte from the viewpoint of being able to better follow the volume change of the electrode active material accompanying charging and discharging. Examples of such a resin solid electrolyte include fluororesins, polyethylene oxide, polyacrylonitrile, polyacrylate, and derivatives and copolymers thereof. Examples of fluororesins include fluororesins containing vinylidene fluoride (VdF), hexafluoropropylene (HFP), tetrafluoroethylene (TFE), and derivatives thereof as constituent units. Specifically, examples of such fluororesins include homopolymers such as polyvinylidene fluoride (PVdF), polyhexafluoropropylene (PHFP), and polytetrafluoroethylene (PTFE), and binary copolymers such as copolymers of VdF and HFP.

[0031] In another preferred embodiment of the secondary battery according to this embodiment, the solid electrolyte preferably contains S element and is a sulfide solid electrolyte that exhibits excellent lithium ion conductivity and can better follow the volume change of the electrode active material during charge and discharge. More preferably, it contains Li element, M element and S element, and the M element is a sulfide solid electrolyte containing at least one element selected from the group consisting of P, Si, Ge, Sn, Ti, Zr, Nb, Al, Sb, Br, Cl and I. Even more preferably, it is a sulfide solid electrolyte containing S element, Li element and P element. The sulfide solid electrolyte may have a Li 3 PS 4 skeleton, and may have a Li 4 P 2 S 7 skeleton, and may have a Li 4 P 2 S 6 skeleton. Examples of the sulfide solid electrolyte having a Li 3 PS 4 skeleton include, for example, LiI-Li 3 PS 4 , LiI-LiBr-Li 3 PS 4 , Li 3 PS 4 . Examples of the sulfide solid electrolyte having a Li 4 P 2 S 7 skeleton include, for example, the Li-P-S-based solid electrolyte called LPS. Examples of the sulfide solid electrolyte also include, for example, Li (4-x) Ge (1- x) P x S 4 (where x satisfies 0 < x < 1), such as LGPS, may be used. More specifically, for example, LPS (Li 2 S-P 2 S 5 ), Li 7 P 3 S 11 , Li 3.2 P 0 .96 S, Li 3.25 Ge 0.25 P 0.75 S4 , Li 10 GeP 2 S 12 , or Li 6 P.S. 5 X (wherein X is Cl, Br or I). 2 SP 2 S 5 " The statement is from Li 2 S and P 2 S 5 The sulfide solid electrolyte is preferably LPS (LiPS) from the viewpoint that it has high ionic conductivity and low bulk modulus and can follow the volume change of the electrode active material caused by charging and discharging. 2 SP 2 S 5 ), Li 6 P.S. 5 X (wherein X is Cl, Br or I), Li 7 P 3 S 11 , Li 3.2 P 0.96 S and Li 3 P.S. 4 is selected from the group consisting of:

[0032] The content of the solid electrolyte in the positive electrode active material layer is not particularly limited, but is, for example, preferably in the range of 1 to 70 mass %, more preferably in the range of 10 to 60 mass %, and even more preferably in the range of 20 to 55 mass %.

[0033] The positive electrode active material layer may further contain at least one of a conductive assistant and a binder in addition to the positive electrode active material and the solid electrolyte. The thickness of the positive electrode active material layer varies depending on the configuration of the intended lithium secondary battery, but is preferably within a range of, for example, 0.1 to 1000 μm, and more preferably 40 to 100 μm.

[0034] [Solid electrolyte layer] The solid electrolyte layer is a layer interposed between the positive electrode active material layer and the negative electrode current collector during discharge, and contains a solid electrolyte (usually as a main component). The specific form of the solid electrolyte contained in the solid electrolyte layer is the same as that described above, so a detailed description will be omitted here.

[0035] The content of the solid electrolyte in the solid electrolyte layer is, for example, preferably in the range of 10 to 100 mass%, more preferably in the range of 50 to 100 mass%, and even more preferably in the range of 90 to 100 mass%, based on the total mass of the solid electrolyte layer. The solid electrolyte layer may further contain a binder in addition to the above-mentioned solid electrolyte. The thickness of the solid electrolyte layer varies depending on the configuration of the intended lithium secondary battery, but is, for example, preferably in the range of 0.1 to 1000 μm, and more preferably 10 to 40 μm.

[0036] As described above with reference to FIG. 2, from the viewpoint of preventing a short circuit caused by contact between the negative electrode active material layer and the positive electrode active material layer, it is preferable that at least a part (preferably the entire circumference) of the outer peripheral edge of the solid electrolyte layer extends to the side surface of the positive electrode active material layer. In a more preferred embodiment, the outer peripheral edge of the solid electrolyte layer extends to the positive electrode current collector, thereby covering the entire side surface of the positive electrode active material layer, which is particularly effective in preventing a short circuit. In this case, the outer peripheral end of the solid electrolyte layer covering the side surface of the positive electrode active material layer may be arranged to be approximately parallel to the side surface of the positive electrode active material layer, or may be arranged in a tapered shape so as to be inclined at a certain angle thereto (for example, see FIG. 9).

[0037] [Negative electrode current collector] The negative electrode current collector is a conductive member that functions as a flow path for electrons that are discharged from the negative electrode toward the power source as the battery reaction (charge / discharge reaction) progresses, or that flow from an external load toward the negative electrode. There is no particular limitation on the material that constitutes the negative electrode current collector. For example, metals and conductive resins can be used as the material that constitutes the negative electrode current collector. There is no particular limitation on the thickness of the negative electrode current collector, but an example is 10 to 100 μm.

[0038] [Negative electrode active material layer] The lithium secondary battery according to the present embodiment is a so-called lithium precipitation type in which lithium metal is precipitated on the negative electrode current collector during the charging process. The layer made of lithium metal precipitated on the negative electrode current collector during the charging process is the negative electrode active material layer of the lithium secondary battery according to the present embodiment. Therefore, the thickness of the negative electrode active material layer increases with the progress of the charging process, and the thickness of the negative electrode active material layer decreases with the progress of the discharging process. The negative electrode active material layer does not need to exist during full discharge, but in some cases, a negative electrode active material layer made of a certain amount of lithium metal may be disposed during full discharge. The thickness of the negative electrode active material layer (lithium metal layer) during full charge is not particularly limited, but is usually 0.1 to 1000 μm.

[0039] [First functional layer] In the lithium secondary battery according to this embodiment, a first functional layer is provided on at least a part (preferably the entirety of the main surface) of the solid electrolyte layer facing the negative electrode current collector, and on at least a part (preferably the entirety of the side surface) of the solid electrolyte layer. This first functional layer is a layer having electronic insulation and lithium ion conductivity. In addition, the first functional layer must be more stable than the solid electrolyte with respect to reductive decomposition caused by contact with lithium metal. Here, "more stable than the solid electrolyte with respect to reductive decomposition caused by contact with lithium metal" means that when comparing the tendency of the solid electrolyte constituting the solid electrolyte layer to be reductively decomposed by contact with lithium metal and the tendency of the constituent material of the first functional layer to be reductively decomposed by contact with lithium metal, the latter tendency is smaller. Whether or not the constituent material of the first functional layer satisfies this condition can be determined by determining whether or not the current flowing through the first functional layer is smaller than the current flowing through the solid electrolyte layer when a voltage is swept near 0 V [vs. Li / Li+] using cyclic voltammetry with each of the solid electrolyte layer and the first functional layer as the working electrode and lithium metal as the counter electrode.

[0040] By disposing such a first functional layer on the side of the solid electrolyte layer, even when the lithium metal deposited on the surface of the negative electrode current collector during charging is pushed out from the outer peripheral end of the solid electrolyte layer by the restraining pressure of the pressing member, the contact between the solid electrolyte layer and the negative electrode active material layer is prevented, and deterioration due to reductive decomposition of the solid electrolyte layer is suppressed. In addition, since the effective area of ​​the lithium metal facing the positive electrode active material layer through the first functional layer and the solid electrolyte layer is larger, there is an advantage that the charge and discharge efficiency is further improved. Here, whether or not the first functional layer of the lithium secondary battery according to this embodiment is disposed can be determined, for example, by confirming whether or not a layer corresponding to the first functional layer exists on the main surface and side of the solid electrolyte layer by SEM-EDX observation of the cross section of the lithium secondary battery, and then analyzing the composition by elemental analysis or the like. In addition, if it is difficult to determine by the above method because the first functional layer is thin, it is also possible to determine by analyzing the layer corresponding to the first functional layer while performing etching by the XPS method.

[0041] The material of the first functional layer as described above is not particularly limited, and any material that satisfies the above conditions can be suitably used. For example, the first functional layer may be made of lithium halide (lithium fluoride (LiF), lithium chloride (LiCl), lithium bromide (LiBr), lithium iodide (LiI)), lithium ion conductive polymer, composite metal oxide represented by Li-MO (M is one or more metal elements selected from the group consisting of Mg, Au, Al, Sn, and Zn), and Li-Ba-TiO 3It is preferable that the first functional layer contains one or more materials selected from the group consisting of composite oxides. All of these materials are particularly stable against reductive decomposition due to contact with lithium metal, and are therefore suitable as constituent materials for the first functional layer. In particular, when the first functional layer contains lithium halide, the rate characteristics of the battery can be improved. This is believed to be because the activation barrier when lithium ions diffuse through the solid electrolyte layer and the first functional layer during charging and discharging is lowered, thereby improving the interfacial diffusion rate of lithium ions and ensuring a sufficient contact area between the first functional layer and the negative electrode active material layer (metallic lithium layer).

[0042] There is no particular limitation on the average thickness of the first functional layer, and it is sufficient that the first functional layer is disposed with a thickness that can exhibit the above-mentioned functions. However, if the average thickness of the first functional layer is too large, it increases the internal resistance, which causes a decrease in charge / discharge efficiency. For this reason, the average thickness of the first functional layer is preferably smaller than the average thickness of the solid electrolyte layer. Also, if the average thickness of the first functional layer is too small, the protective effect of providing the first functional layer may not be sufficiently obtained. From these viewpoints, the average thickness of the first functional layer is preferably 0.5 nm to 20 μm, and more preferably 5 nm to 10 μm. The "average thickness" of the first functional layer means a value calculated as the arithmetic average value of thicknesses measured at several to several tens of different points on the first functional layer constituting the lithium secondary battery. From the viewpoint of further improving the rate characteristics of the battery, the arithmetic mean roughness (Ra; measured in accordance with JIS B 0601:2013) of the main surface of the first functional layer facing the negative electrode current collector is preferably less than 1 μm, more preferably 100 nm or less, even more preferably 50 nm or less, particularly preferably 20 nm or less, and most preferably 10 nm or less. On the other hand, there is no particular restriction on the lower limit of Ra, but in practice it is 1 nm or more.

[0043] [Insulation layer] In the lithium secondary battery according to this embodiment, as shown in FIG. 6, when the power generating element 21 is viewed in plan, it is preferable that at least a part of the outer peripheral edge of the positive electrode active material layer 15 is located inside the outer peripheral edge of the positive electrode current collector 11'', and an insulating layer 20 made of an electronic insulating material is arranged on the surface of the positive electrode current collector 11'' on the side of the solid electrolyte layer 17 on which the positive electrode active material layer 15 is not arranged. With this configuration, even when the lithium metal deposited on the surface of the negative electrode current collector during charging is pushed out from the outer peripheral edge of the solid electrolyte layer by the restraining pressure of the pressing member, the contact between the positive electrode active material layer 15 and the negative electrode active material layer 13 is prevented, and the occurrence of a short circuit is suppressed. In the embodiment shown in FIG. 6, the insulating layer 20 is arranged so that the entire side surface of the positive electrode active material layer 15 is covered with the insulating layer 20. In this way, if at least a part of the outer peripheral edge of the solid electrolyte layer 17 extends to at least a part of the side surface of the positive electrode active material layer 15, and at least a part of the outer periphery of the positive electrode active material layer 15 is covered by one or more of the solid electrolyte layer 17, the first functional layer 18, and the insulating layer 20, the cycle durability of the battery is significantly improved, which is preferable. In such a configuration, it is more preferable that the first functional layer contains a material (e.g., a lithium ion conductive polymer) having a Young's modulus of less than 100 MPa. With such a configuration, the first functional layer can sufficiently follow the expansion and contraction of the positive electrode active material layer during charging and discharging, and exposure of the side surface of the positive electrode active material layer and the occurrence of a short circuit due to this can be prevented. As a result, the cycle durability of the battery can be improved. However, as in the embodiment shown in FIG. 7, the insulating layer 20 may be arranged so that a part of the side surface of the positive electrode active material layer 15 is exposed.

[0044] The material of the insulating layer as described above is not particularly limited, and any material that satisfies the above conditions can be suitably used. An example of the material of the insulating layer is a material in which inorganic powder such as aluminum oxide, zirconium oxide, silicon oxide, and SB-Na-based glass frit is dispersed in the solid electrolyte constituting the solid electrolyte layer. However, the material of the insulating layer is preferably a resin material or a rubber material. Since these materials are highly durable and elastic, even if internal stress occurs in the region where the insulating layer is formed, the insulating layer can be stretched without breaking, thereby effectively preventing the occurrence of a short circuit. Examples of such resin materials include polyolefin resins such as polyethylene (e.g., low-density polyethylene, high-density polyethylene, etc.), polypropylene, and other such polyolefin resins, polyester resins such as polyethylene terephthalate (PET), polyvinyl chloride resins, acrylic resins, methacrylic resins, acrylonitrile-butadiene-styrene resins, vinyl acetate resins, ethylene-vinyl acetate resins, styrene-butadiene resins, and other such thermoplastic resins; silicone resins, urethane resins, melamine resins, thermosetting acrylic resins, urea resins, phenolic resins, resorcinol resins, alkylresorcinol resins, epoxy resins, and thermosetting polyesters, and other such thermosetting resins. Examples of rubber materials include latex rubber, chloroprene rubber (CR), styrene-butadiene rubber (SBR), ethylene-propylene-diene rubber (EPDM), acrylonitrile-butadiene rubber (NBR), and other such rubbers.

[0045] [Second functional layer] In the lithium secondary battery according to this embodiment, as shown in FIG. 15, it is preferable that a second functional layer 23 containing an element capable of being alloyed with lithium or a compound containing the element is further provided on at least a part of the main surface of the first functional layer 18 facing the negative electrode current collector 11'. With such a configuration, the cycle durability of the battery can be further improved. This is because the second functional layer 23 is interposed between the first functional layer 18 and the negative electrode current collector 11', and thus the energy required for lithium ions to precipitate as metallic lithium during the charging process can be reduced, and as a result, charging and discharging can be performed at a higher current density. Here, examples of the element capable of being alloyed with lithium contained in the second functional layer include at least one selected from the group consisting of gold, silver, zinc, magnesium, aluminum, platinum, silicon, tin, bismuth, indium, and palladium. The second functional layer can be composed of a compound containing these elements as well as a simple substance of these elements. Examples of such compounds include SiO x or SnO x and the like, and alloys containing transition metal elements such as Ni-Si alloys, Ti-Si alloys, Mg-Sn alloys, Fe-Sn alloys, etc. Among these, it is preferable to contain the above elements as simple substances, and it is more preferable to contain silver, zinc, or magnesium as simple substances.

[0046] Although the above description has been given with reference to an example in which the secondary battery according to the present embodiment is an all-solid-state lithium secondary battery, the lithium secondary battery according to the present embodiment may not be an all-solid-state type. That is, the solid electrolyte layer may further contain a conventionally known liquid electrolyte (electrolytic solution). There is no particular restriction on the amount of liquid electrolyte (electrolytic solution) that can be contained in the solid electrolyte layer, but it is preferable that the amount is such that the shape of the solid electrolyte layer formed by the solid electrolyte is maintained and the liquid electrolyte (electrolytic solution) does not leak. As the liquid electrolyte (electrolytic solution), a solution having a form in which a conventionally known lithium salt is dissolved in a conventionally known organic solvent is used. The liquid electrolyte (electrolytic solution) may further contain additives other than the organic solvent and the lithium salt. These additives may be used alone or in combination of two or more. In addition, the amount of additives used in the electrolyte solution can be appropriately adjusted. EXAMPLES

[0047] The present invention will be described in more detail below with reference to examples. However, the technical scope of the present invention is not limited to the following examples. In the following, the operations were performed in a glove box. Furthermore, the instruments and devices used in the glove box were thoroughly dried in advance.

[0048] <Example 1> [Preparation of evaluation cell] (Preparation of positive electrode) First, LiNi as the positive electrode active material 0.8 Mn 0.1 Co 0.1 O 2 , acetylene black as a conductive additive, and a sulfide solid electrolyte (LPS(Li 2 SP 2 S 5)) were weighed out to a mass ratio of 50:30:20, mixed in an agate mortar in a glove box, and then further mixed and stirred in a planetary ball mill. 2 parts by mass of styrene-butadiene rubber (SBR) were added to 100 parts by mass of the obtained mixed powder, and mesitylene was added as a solvent to prepare a positive electrode active material slurry. Next, the positive electrode active material slurry prepared above was applied to the surface of an aluminum foil as a positive electrode current collector, dried, and pressed to form a positive electrode active material layer (thickness 50 μm), and a positive electrode was produced.

[0049] (Preparation of solid electrolyte layer and first functional layer) Sulfide solid electrolyte (LPS(Li 2 SP 2 S 5 )) 100 parts by mass, 2 parts by mass of styrene-butadiene rubber (SBR) was added, and mesitylene was added as a solvent to prepare a solid electrolyte slurry. Next, the solid electrolyte slurry prepared above was applied to the surface of a stainless steel foil as a support, and dried to obtain a solid electrolyte layer (thickness 30 μm) as a free-standing film. After that, a first functional layer (thickness 20 nm) made of lithium fluoride (LiF) was formed by sputtering on one main surface and the entire side surface of the obtained solid electrolyte layer.

[0050] (Preparation of evaluation cells) The solid electrolyte layer on which the first functional layer was formed was transferred by cold isostatic pressing (CIP) to the positive electrode active material layer side of the positive electrode prepared above, so that the exposed surface of the solid electrolyte layer faces the positive electrode active material layer. At this time, the pressing pressure during the CIP treatment was controlled so that the outer peripheral edge of the solid electrolyte layer extends to the middle of the side surface of the positive electrode active material layer over the entire circumference. Finally, a stainless steel foil was laminated as a negative electrode current collector on the exposed surface of the first functional layer to prepare an evaluation cell (lithium precipitation type all-solid-state lithium secondary battery) having the form shown in FIG. 2 except that there is no negative electrode active material layer.

[0051] [Evaluation of evaluation cells (measurement of charge / discharge efficiency)] A positive electrode lead and a negative electrode lead were connected to the positive electrode current collector and the negative electrode current collector of the evaluation cell prepared above, respectively, and two cycles of charge and discharge were performed under the following charge and discharge test conditions. At this time, the following charge and discharge test was performed while applying a restraining pressure of 5 [MPa] in the stacking direction of the evaluation cell using a pressure member.

[0052] (Charge / discharge test conditions) 1) Charge / discharge conditions [Voltage range] 3.0~4.3V [Charging process] CCCV (0.01C cutoff) [Discharge process]CC [Charge / discharge rate] 0.2C (After charging and discharging, rest for 30 minutes each.) 2) Evaluation temperature: 298K (25℃).

[0053] The evaluation cell was charged from 3.0 V to 4.3 V at 0.2 C (0.01 C cutoff) in the charging process (when lithium metal precipitates on the negative electrode current collector) in a thermostatic chamber set to the above evaluation temperature using a charge-discharge tester. The cell was then discharged from 4.3 V to 3.0 V at 0.2 C in the constant current (CCCV) mode during the discharging process (when lithium metal on the negative electrode current collector dissolves). Here, 1 C refers to the current value at which the battery is fully charged (100% charged) when charged for 1 hour at that current value. Here, the charge capacity (battery capacity at the time of charging) and discharge capacity (battery capacity at the time of discharging) were measured during the charge-discharge process of the evaluation cell. The charge-discharge efficiency (coulombic efficiency) was calculated as the ratio of the battery capacity at the time of discharging to the battery capacity at the time of charging in the second cycle.

[0054] As a result, the charge / discharge efficiency in this example was 99%.

[0055] <Example 2> An evaluation cell having the configuration shown in Fig. 6 was produced in the same manner as in Example 1 described above, except that a resin layer (insulating layer) made of polyethylene terephthalate (PET) was disposed on the surface of the outer peripheral portion of the positive electrode current collector so as to surround the outer periphery (the entire exposed side surface) of the positive electrode active material layer. The charge / discharge efficiency (Coulombic efficiency) was calculated in the same manner as above, and the charge / discharge efficiency in this example was 99%.

[0056] <Example 3> An evaluation cell having the configuration shown in Fig. 7 except that no negative electrode active material layer was present was produced by the same method as in Example 2 described above, except that a resin layer made of polyethylene terephthalate (PET) was disposed on the surface of the outer peripheral portion of the positive electrode current collector so as to surround the outer periphery (a part of the exposed side surface) of the positive electrode active material layer, and the sputtering conditions were controlled so that the outer peripheral portion of the first functional layer extended all the way around to the middle of the side surface of the solid electrolyte layer. The charge / discharge efficiency (Coulombic efficiency) was calculated by the same method as above, and the charge / discharge efficiency in this example was 99%.

[0057] <Example 4> The solid electrolyte layer before the formation of the first functional layer was transferred to the positive electrode active material layer side of the positive electrode by cold isostatic pressing (CIP). At this time, the transfer conditions were controlled so that the width of the solid electrolyte layer arranged on the side of the positive electrode active material layer widens toward the positive electrode current collector side while the solid electrolyte layer covers the entire exposed surface and side of the positive electrode active material layer as shown in FIG. 9. Then, the evaluation cell shown in FIG. 9 except that the negative electrode active material layer was not present was obtained by the same method as in Example 1 described above, except that the first functional layer (thickness 20 nm) made of lithium fluoride (LiF) was formed by sputtering on one main surface and the entire side of the obtained solid electrolyte layer. Then, the charge / discharge efficiency (Coulomb efficiency) was calculated by the same method as above, and the charge / discharge efficiency in this example was 99%.

[0058] <Example 5> An evaluation cell having the configuration shown in Fig. 3 except that no negative electrode active material layer was present was produced by the same method as in Example 1 described above, except that the pressing pressure during the CIP treatment was controlled so that the outer peripheral edge of the solid electrolyte layer did not extend all the way to the side surface of the positive electrode active material layer, and the sputtering conditions were controlled so that the outer peripheral edge of the first functional layer extended all the way to the middle of the side surface of the solid electrolyte layer. The charge / discharge efficiency (Coulombic efficiency) was calculated by the same method as above, and the charge / discharge efficiency in this example was 99%.

[0059] In addition, for each of the above-mentioned Examples 1 to 5, the thickness of the first functional layer was changed from 20 nm to 5 nm, 100 nm, 250 nm, 1 μm, 5 μm, or 15 μm, and similar evaluation cells were fabricated and the charge / discharge efficiency was measured. As a result, it was confirmed that the same results as above were obtained in all cases.

[0060] <Comparative Example 1> A test cell having the configuration shown in FIG. 10 was produced by the same method as in Example 5 described above, except that the sputtering conditions were controlled so that the outer peripheral edge of the first functional layer did not extend to the side surface of the solid electrolyte layer over the entire circumference. The charge / discharge efficiency (Coulomb efficiency) was calculated by the same method as above, and the charge / discharge efficiency in this comparative example was 83%. When the test cell was disassembled and observed after the charge / discharge test, it was confirmed that the side surface of the solid electrolyte layer had deteriorated and discolored. In this comparative example, the first functional layer was not arranged so as to extend to the side surface of the solid electrolyte layer. For this reason, it is considered that the lithium metal deposited on the surface of the negative electrode current collector during charging is pushed out from the outer peripheral end of the solid electrolyte layer by the restraining pressure of the pressing member and comes into contact with the side surface of the solid electrolyte layer as shown in FIG. 10, and the solid electrolyte constituting the solid electrolyte layer is degraded by reduction decomposition, and the internal resistance increases, resulting in a decrease in the charge / discharge efficiency.

[0061] <Comparative Example 2> A resin layer (insulating layer) made of polyethylene terephthalate (PET) was arranged on the surface of the outer periphery of the positive electrode current collector so as to surround the outer periphery (the entire exposed side surface) of the positive electrode active material layer and so that the height of the insulating layer was greater than the thickness of the positive electrode active material layer. An evaluation cell was produced in the same manner as in Comparative Example 1 described above, except that the negative electrode active material layer was not present. When a charge / discharge test was performed using the same method as above, a short circuit occurred and the charge / discharge efficiency could not be measured. When the evaluation cell after the charge / discharge test was disassembled and observed, it was confirmed that cracks had occurred in the outer periphery of the solid electrolyte layer. In this comparative example, an insulating layer that is higher than the thickness of the positive electrode active material layer is provided. For this reason, it is believed that internal stress was generated at the interface between the insulating layer and the solid electrolyte layer due to the restraining pressure, which caused cracks to occur in the outer periphery of the solid electrolyte layer, which caused the short circuit.

[0062] <Comparative Example 3> A test cell was produced in the same manner as in Example 3 except that the sputtering conditions were controlled so that the outer peripheral edge of the first functional layer did not extend to the side of the solid electrolyte layer over the entire circumference, and the size of the positive electrode active material layer was made the same as the size of the solid electrolyte layer, and an evaluation cell was produced in the same manner as in Example 3 except that the negative electrode active material layer was not present. Then, when a charge / discharge test was performed using the same method as above, a short circuit occurred and the charge / discharge efficiency could not be measured. In this comparative example, the size of the positive electrode active material layer is made the same as the size of the solid electrolyte layer. Therefore, when the lithium metal precipitated on the surface of the negative electrode current collector during charging is pushed out from the outer peripheral end of the solid electrolyte layer by the restraining pressure of the pressing member, the lithium metal easily comes into contact with the side of the positive electrode active material layer. It is believed that a short circuit occurred as a result.

[0063] <Comparative Example 4> A cell for evaluation having the configuration shown in FIG. 13 was produced by the same method as in Comparative Example 1 described above, except that the pressing pressure during the CIP treatment was controlled so that the outer peripheral edge of the solid electrolyte layer extended halfway to the side of the positive electrode active material layer over the entire circumference, and that the components other than the negative electrode current collector of the power generating element were sealed with a sealant (epoxy resin). Then, when a charge / discharge test was performed by the same method as above, a short circuit occurred and the charge / discharge efficiency could not be measured. In this comparative example, even if it was sealed with epoxy resin, the lithium metal precipitated on the surface of the negative electrode current collector during charging was pushed out from the outer peripheral end of the solid electrolyte layer by the restraining pressure of the pressurizing member, and reached the side of the positive electrode active material layer through the gap between the epoxy resin and the solid electrolyte layer. It is considered that a short circuit occurred as a result.

[0064] <Example 6> An evaluation cell was fabricated in the same manner as in Example 1 above, except that the thickness of the first functional layer was changed to 40 nm.

[0065] <Example 7> An evaluation cell was produced in the same manner as in Example 6 above, except that the constituent material of the first functional layer was changed from lithium fluoride to lithium bromide (LiBr).

[0066] <Example 8> An evaluation cell was fabricated in the same manner as in Example 6 above, except that the constituent material of the first functional layer was changed from lithium fluoride to lithium chloride (LiCl).

[0067] <Example 9> An evaluation cell was produced in the same manner as in Example 6 above, except that the constituent material of the first functional layer was changed from lithium fluoride to lithium iodide (LiI).

[0068] <Example 10> The constituent material of the first functional layer was changed from lithium fluoride to lithium carbonate (Li 2 CO 3) An evaluation cell was produced in the same manner as in Example 6 above, except that the above-mentioned procedure was changed to the above-mentioned procedure in Example 6.

[0069] <Example 11> The constituent material of the first functional layer was changed from lithium fluoride to lithium oxide (Li 2 Except for changing the above-mentioned condition, the evaluation cell was produced in the same manner as in Example 6.

[0070] <Example 12> An evaluation cell was produced in the same manner as in Example 8 above, except that the thickness of the first functional layer was changed to 10 μm.

[0071] <Example 13> A slurry was prepared by dispersing lithium chloride powder in an appropriate amount of mesitylene, adding 1% by mass of SBR to the lithium chloride, and mixing. The evaluation cell was produced in the same manner as in Example 8, except that the slurry was applied and dried to form a first functional layer (thickness 2 μm).

[0072] [Measurement of the arithmetic mean roughness (Ra) of the surface of the first functional layer] The arithmetic mean roughness (Ra) of the main surface of the first functional layer facing the negative electrode current collector was measured in accordance with JIS B 0601: 2013. The results are shown in Table 1 below.

[0073] [Evaluation of evaluation cells (measurement of charge rate characteristics)] A positive electrode lead and a negative electrode lead were connected to the positive electrode current collector and the negative electrode current collector of the evaluation cells prepared in the above Examples 6 to 13, respectively, and three cycles of charge and discharge treatment were performed at 1.0C or 0.2C according to the same charge and discharge test conditions as above, except that the evaluation temperature was changed to 333K (60°C). Then, the percentage [%] of the charge capacity (1.0C) at the third cycle relative to the charge capacity (0.2C) at the third cycle was calculated to obtain the charge rate characteristics. The results are shown in Table 1 below.

[0074] [Table 1]

[0075] From the results shown in Table 1, it can be seen that Examples 6 to 9 in which the first functional layer contains lithium halide exhibit superior charge rate characteristics compared to Examples 10 and 11 in which the first functional layer is composed of a material other than lithium halide. It can also be seen that it is particularly preferable for the first functional layer to be composed of LiBr, LiCl, or LiI. Furthermore, from a comparison of Examples 8, 12, and 13, it can be seen that a lithium secondary battery with superior charge rate characteristics can be obtained when the arithmetic mean roughness (Ra) of the main surface of the first functional layer facing the negative electrode current collector is less than 1 μm (preferably 20 nm or less, more preferably 10 nm or less).

[0076] <Example 14> A first functional layer (thickness 2 μm) was formed by applying a solution of polyethylene glycol (PEG (polyethylene oxide; PEO); number average molecular weight 200,000) dissolved in an appropriate amount of water and drying it. At this time, the size of the first functional layer was controlled so that the outer peripheral edge of the first functional layer covered the entire side surface of the solid electrolyte layer and the side surface of the positive electrode active material layer over the entire circumference. Apart from these points, an evaluation cell was produced in the same manner as in Example 3 described above, with the exception that there was no negative electrode active material layer, as shown in FIG. 14. The Young's modulus of the first functional layer was measured by a spherical indentation test and was found to be 70 MPa.

[0077] <Comparative Example 5> An evaluation cell was produced in the same manner as in Example 14 above, except that the first functional layer was not formed.

[0078] <Example 15> An evaluation cell was produced in the same manner as in Example 14 above, except that no insulating layer was formed.

[0079] <Example 16> A solution of polyethylene glycol (PEG (polyethylene oxide; PEO); number average molecular weight 200,000) dissolved in an appropriate amount of water was applied and dried to form a first functional layer (thickness 2 μm). At this time, the size of the first functional layer was controlled so that the first functional layer was positioned as shown in Figure 7. Other than these, the evaluation cell was produced using the same method as in Example 3 described above.

[0080] <Example 17> The material of the first functional layer was changed from polyethylene glycol to an aluminum metal film (thickness 20 nm). In this case, the first functional layer made of an aluminum metal film was formed by sputtering before arranging the negative electrode current collector after transferring the solid electrolyte layer so that the exposed surface of the solid electrolyte layer faces the positive electrode active material layer. Except for these, the evaluation cell was produced by the same method as in Example 14 described above. The Young's modulus of the first functional layer was measured by a spherical indentation test and was found to be 70 GPa.

[0081] [Evaluation of evaluation cells (measurement of charge / discharge cycle characteristics)] A positive electrode lead and a negative electrode lead were connected to the positive electrode current collector and the negative electrode current collector of the evaluation cells produced in the above Examples 14 to 17 and Comparative Example 5, respectively, and the charge / discharge process was repeatedly performed under the same charge / discharge test conditions as those used to measure the charge / discharge efficiency above, except that the evaluation temperature was changed to 333 K (60° C.) and the voltage range was changed to 2.5 to 4.3 V, and the number of cycles that could be charged and discharged before a short circuit occurred was measured. The results are shown in Table 2 below.

[0082] [Table 2]

[0083] From the results shown in Table 2, it can be seen that the charge-discharge cycle characteristics are improved when an insulating layer is disposed on the surface of the positive electrode current collector on the solid electrolyte layer side where the positive electrode active material layer is not disposed, the outer peripheral edge of the solid electrolyte layer extends to the side surface of the positive electrode active material layer, and the outer periphery of the positive electrode active material layer is covered by the solid electrolyte layer, the first functional layer, or the insulating layer. It can also be seen that the charge-discharge cycle characteristics are improved when the first functional layer is composed of a lithium ion conductive polymer (e.g., polyethylene glycol) having a small Young's modulus (specifically, less than 100 MPa) or the like.

[0084] <Example 18> The material of the first functional layer was changed from lithium fluoride to lithium chloride, and the thickness of the first functional layer was changed to 100 nm. In addition, before laminating the stainless steel foil as the negative electrode current collector on the exposed surface of the first functional layer, a second functional layer made of silver was formed by sputtering on the entire surface of the negative electrode current collector on the first functional layer side. Except for these, an evaluation cell was produced in the same manner as in Example 1 described above, except that there was no negative electrode active material layer, as shown in FIG. 15.

[0085] <Example 19> An evaluation cell was prepared in the same manner as in Example 18 described above, except that a dispersion liquid prepared by dispersing silver powder in an appropriate amount of mesitylene was spray-coated onto the entire surface of the negative electrode current collector on the side of the first functional layer, and then dried to form a second functional layer.

[0086] <Example 20> An evaluation cell was produced in the same manner as in Example 18, except that a dispersion liquid in which silver powder was dispersed in an appropriate amount of mesitylene was spray-coated on the area of ​​the surface of the first functional layer on the negative electrode current collector side facing the negative electrode current collector, and then dried to form a second functional layer. Note that in the obtained evaluation cell, the silver particles constituting the second functional layer were present not only between the first functional layer and the negative electrode current collector, but also inside the first functional layer.

[0087] <Example 21> An evaluation cell was prepared in the same manner as in Example 18 described above, except that a second functional layer made of silver was formed by sputtering over the entire surface of the first functional layer on the negative electrode current collector side before the solid electrolyte layer on which the first functional layer was formed was transferred to the positive electrode active material layer side of the positive electrode.

[0088] <Example 22> An evaluation cell was produced in the same manner as in Example 19 described above, except that in producing the second functional layer, the silver powder was changed to magnesium powder.

[0089] <Example 23> An evaluation cell was produced in the same manner as in Example 19 described above, except that in producing the second functional layer, the silver powder was changed to zinc powder.

[0090] <Example 24> An evaluation cell was prepared in the same manner as in Example 4 described above, except that before the solid electrolyte layer on which the first functional layer was formed was transferred to the positive electrode active material layer side of the positive electrode, a dispersion liquid prepared by dispersing silver powder in an appropriate amount of mesitylene was spray-coated onto the entire surface of the first functional layer on the negative electrode current collector side, and then dried to form a second functional layer made of silver on the entire surface of the first functional layer on the negative electrode current collector side.

[0091] [Evaluation of evaluation cells (measurement of charge / discharge cycle characteristics)] A positive electrode lead and a negative electrode lead were connected to the positive electrode current collector and the negative electrode current collector of the evaluation cells prepared in the above-mentioned Examples 18 to 24 and the above-mentioned Example 1, respectively, and 30 cycles of charge and discharge treatment were performed under the same charge and discharge test conditions as those used to measure the charge and discharge efficiency above, except that the evaluation temperature was changed to 333K (60°C) and the charge and discharge rate was changed to 1.0C. Then, the percentage [%] of the discharge capacity at the 30th cycle relative to the discharge capacity at the 1st cycle was calculated to obtain the charge and discharge cycle capacity retention rate. The results are shown in Table 3 below.

[0092] [Table 3]

[0093] The results shown in Table 3 show that the charge-discharge cycle characteristics are improved when a second functional layer containing an element capable of alloying with lithium or a compound containing such an element is further provided on the main surface of the first functional layer facing the negative electrode current collector.

[0094] This application is based on Japanese Patent Application No. 2021-055645 filed on March 29, 2021, and Japanese Patent Application No. 2022-032266 filed on March 3, 2022, the contents of which are incorporated by reference in their entirety into this specification.

Claims

1. a positive electrode including a positive electrode active material layer disposed on a surface of a positive electrode current collector, the positive electrode active material layer containing a positive electrode active material capable of absorbing and releasing lithium ions; a negative electrode having a negative electrode current collector on which lithium metal is deposited during charging; a solid electrolyte layer interposed between the positive electrode and the negative electrode and containing a sulfide solid electrolyte; and a pressure member that applies a predetermined pressure to the power generating element in a stacking direction, when the power generating element is viewed in plan, at least a part of an outer circumferential edge of the positive electrode active material layer is located inside an outer circumferential edge of the solid electrolyte layer, and an outer circumferential edge of the negative electrode current collector is located inside an outer circumferential edge of the solid electrolyte layer and outside an outer circumferential edge of the positive electrode active material layer; a first functional layer that has electronic insulation and lithium ion conductivity, and is more stable than the solid electrolyte with respect to reductive decomposition due to contact with lithium metal, is provided on at least a part of a main surface of the solid electrolyte layer facing the negative electrode current collector and on at least a part of a side surface of the solid electrolyte layer.

2. 2. The lithium secondary battery according to claim 1, wherein at least a portion of an outer periphery of the solid electrolyte layer extends to at least a portion of a side surface of the positive electrode active material layer.

3. The first functional layer is preferably made of lithium fluoride (LiF), lithium chloride (LiCl), lithium bromide (LiBr), lithium iodide (LiI), a lithium ion conductive polymer, a composite metal oxide represented by Li-M-O (M is one or more metal elements selected from the group consisting of Mg, Au, Al, Sn, and Zn), and Li-Ba-TiO 3 3. The lithium secondary battery according to claim 1, comprising one or more materials selected from the group consisting of composite oxides.

4. 4. The lithium secondary battery of claim 3, wherein the first functional layer comprises lithium fluoride (LiF), lithium chloride (LiCl), lithium bromide (LiBr), or lithium iodide (LiI).

5. The lithium secondary battery according to any one of claims 1 to 4, wherein the average thickness of the first functional layer is 0.5 nm to 20 µm.

6. The lithium secondary battery according to claim 5, wherein the average thickness of the first functional layer is 5 nm to 10 μm.

7. The lithium secondary battery according to any one of claims 1 to 6, wherein the first functional layer has a main surface facing the negative electrode current collector with an arithmetic mean roughness (Ra) of less than 1 µm.

8. When the power generating element is viewed in plan, at least a part of an outer circumferential edge of the positive electrode active material layer is located inside an outer circumferential edge of the positive electrode current collector, 8. The lithium secondary battery according to claim 1, wherein an insulating layer made of an electronic insulating material is disposed on a surface of the positive electrode current collector on the side of the solid electrolyte layer on which the positive electrode active material layer is not disposed.

9. 9. The lithium secondary battery according to claim 8, wherein at least a part of an outer periphery of the solid electrolyte layer extends to at least a part of a side surface of the positive electrode active material layer, and at least a part of the outer periphery of the positive electrode active material layer is covered by one or more of the solid electrolyte layer, the first functional layer, and the insulating layer.

10. The lithium secondary battery of claim 9 , wherein the first functional layer comprises a material having a Young's modulus of less than 100 MPa.

11. The lithium secondary battery of claim 10 , wherein the first functional layer comprises a lithium ion conductive polymer.

12. The lithium secondary battery according to any one of claims 1 to 11, further comprising a second functional layer including an element capable of being alloyed with lithium or a compound containing the element, on at least a part of a main surface of the first functional layer facing the negative electrode current collector.

13. 13. The lithium secondary battery according to claim 12, wherein the element capable of alloying with lithium includes at least one selected from the group consisting of gold, silver, zinc, magnesium, aluminum, platinum, silicon, tin, bismuth, indium, and palladium.

14. The solid electrolyte contained in the solid electrolyte layer is Li2 S -P 2 S 5 , Li 6 P.S. 5 X (wherein X is Cl, Br or I), Li 7 P 3 S 11 , Li 3.2 P 0.96 S and Li 3 P.S. 4 The lithium secondary battery according to any one of claims 1 to 13, selected from the group consisting of:

15. The lithium secondary battery according to any one of claims 1 to 14, wherein the positive electrode active material layer further contains a sulfide solid electrolyte.

16. The lithium secondary battery according to claim 15 , wherein an average thickness of the first functional layer is smaller than an average thickness of the solid electrolyte layer.

17. The lithium secondary battery according to any one of claims 1 to 16, wherein the content of the sulfide solid electrolyte in the solid electrolyte layer is 90 to 100 mass%.

Citation Information

Patent Citations

  • Solid battery

    JP2006179241A

  • All-solid-state lithium battery

    JP2014120265A

  • Lithium solid type secondary battery, and method for manufacturing the same

    JP2016012495A

  • All-solid battery, and method for manufacturing the same

    JP2020009619A

  • Solid-state lithium battery, solid-state lithium battery module, and method for producing solid-state lithium battery