Curable resin composition, coating material and article
A curable resin composition with a specific polyester polyol and acrylic polyol blend addresses the limitations of existing acrylic resin coatings by providing improved adhesion, water resistance, and chemical resistance, suitable for automotive and industrial coatings.
Patent Information
- Application Number
- JP2024540765
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-14
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2044-03-14
AI Technical Summary
Existing acrylic resin compositions for coatings lack excellent adhesion, water resistance, and chemical resistance, particularly in applications requiring good appearance and texture, such as automobile paints.
A curable resin composition comprising a polyester polyol derived from a polyhydric carboxylic acid with 20 mol% aliphatic dicarboxylic acid and a polyhydric alcohol with 20 mol% diols, combined with an acrylic polyol, achieving a specific ester group concentration for improved chemical resistance and appearance.
The composition provides a cured coating film with excellent adhesion, water resistance, and chemical resistance, suitable for automotive and industrial applications, enhancing durability and appearance.
Smart Images

Figure 0007582568000001 
Figure 0007582568000002 
Figure 0007582568000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable resin composition, a coating material, and an article. [Background technology]
[0002] Conventionally, acrylic resin compositions have been used in applications such as paints, inks, adhesives, and synthetic leather due to their excellent chemical resistance, weather resistance, flexibility, and adhesion. In particular, in paint applications, they are used in fields such as automobiles, home appliances, and building materials. In these fields, coating films that are excellent in appearance (thickness) are required in addition to adhesion to plastic substrates and chemical resistance (sunscreen resistance, alcohol resistance) assuming actual use.
[0003] As a coating composition that gives a good coating film thickness, a two-liquid mixed coating composition has been proposed that contains, as a base, at least one of an oxidatively polymerizable unsaturated fatty acid and an alkyd resin having an oxidatively polymerizable group, and a copolymer of an acrylic copolymer and a silicone having at least one of a hydroxyl group and an alkoxysilyl group (see, for example, Patent Document 1). However, systems that use this unsaturated fatty acid or alkyd resin have a problem of poor chemical resistance, such as sunscreen resistance. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5688523 specification Summary of the Invention [Problem to be solved by the invention]
[0005] The problem to be solved by the present invention is to provide a curable resin composition that can give a cured coating film that is excellent in appearance (thickness), adhesion, water resistance, and chemical resistance; a coating material; and an article having a cured coating film of the coating material. [Means for solving the problem]
[0006] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have found that a curable resin composition containing a specific polyester polyol and an acrylic polyol can provide a cured coating film that is excellent in appearance (thickness), adhesion, water resistance, and chemical resistance, and have completed the present invention.
[0007] That is, the present invention relates to a curable resin composition comprising a polyester polyol (A) which is a reaction product of a polyvalent carboxylic acid (a1) and a polyhydric alcohol (a2) and an acrylic polyol (B), wherein the polyvalent carboxylic acid (a1) contains 20 mol % or more of an aliphatic dicarboxylic acid (a1-1) having a linear alkyl group having 4 to 10 carbon atoms, the polyhydric alcohol (a2) contains 20 mol % or more of one or more diols (a2-1) selected from the group consisting of ethylene glycol, diethylene glycol, 1,2-propanediol, and 1,3-propanediol, and contains 5 to 20 mol % of a trifunctional or higher alcohol (a2-2), and the ester group concentration of the polyester polyol (A) is 6 to 11 mmol / g. Effect of the Invention
[0008] The curable resin composition of the present invention can give a cured coating film that is excellent in appearance (thickness), adhesion, water resistance, and chemical resistance, and can therefore be suitably used in various coating materials for automobile exteriors, automobile repairs, plastics, industrial machinery, building materials, wooden floors, and the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The curable resin composition of the present invention is a resin composition containing a polyester polyol (A) which is a reaction product of a polybasic carboxylic acid (a1) and a polyhydric alcohol (a2), and an acrylic polyol (B), in which the polybasic carboxylic acid (a1) contains 20 mol % or more of an aliphatic dicarboxylic acid (a1-1) having a linear alkyl group having 4 to 10 carbon atoms, the polyhydric alcohol (a2) contains 20 mol % or more of one or more diols (a2-1) selected from the group consisting of ethylene glycol, diethylene glycol, 1,2-propanediol, and 1,3-propanediol, and contains 5 to 20 mol % of a trifunctional or higher alcohol (a2-2), and the polyester polyol (A) has an ester group concentration of 6 to 11 mmol / g.
[0010] The polyester polyol (A) is a reaction product of a polyvalent carboxylic acid (a1) and a polyhydric alcohol (a2), and is obtained by a known condensation reaction.
[0011] It is important that the polyvalent carboxylic acid (a1) contains 20 mol % or more of an aliphatic dicarboxylic acid (a1-1) having a linear alkyl group having 4 to 10 carbon atoms, since this gives a coating film with excellent thickness.
[0012] Examples of the aliphatic dicarboxylic acid (a1-1) having a linear alkyl group having 4 to 10 carbon atoms include succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, maleic acid, fumaric acid, etc., and methyl esters and acid chlorides of these aliphatic dicarboxylic acids, with succinic acid and sebacic acid being more preferred. These aliphatic dicarboxylic acids (a1-1) can be used alone or in combination of two or more.
[0013] In the present invention, the dicarboxylic acid includes anhydrides of the dicarboxylic acid.
[0014] As the polyvalent carboxylic acid (a1), a polyvalent carboxylic acid (a1-2) other than the dicarboxylic acid (a1-1) can be used in combination.
[0015] The other polycarboxylic acids (a1-2) include aliphatic dicarboxylic acids other than the dicarboxylic acids (a1-1), alicyclic dicarboxylic acids, aromatic dicarboxylic acids, etc. These polycarboxylic acids (a1-2) can be used alone or in combination of two or more.
[0016] Examples of the aliphatic dicarboxylic acid other than the dicarboxylic acid (a1-1) include decanedicarboxylic acid and dimer acid.
[0017] Examples of the alicyclic dicarboxylic acid include 1,3-cyclopentanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid.
[0018] Examples of the aromatic dicarboxylic acid include terephthalic acid, isophthalic acid, orthophthalic acid, naphthalenedicarboxylic acid, biphenyldicarboxylic acid, 1,2-bis(phenoxy)ethane-p,p'-dicarboxylic acid, p-hydroxybenzoic acid, p-(2-hydroxyethoxy)benzoic acid, trimellitic acid, and pyromellitic acid.
[0019] The aliphatic dicarboxylic acid (a1-1) having a linear alkyl group having 4 to 10 carbon atoms in the polyvalent carboxylic acid (a1) is preferably contained in an amount of 30 to 90 mol % since this further improves the thickness of the resulting coating film.
[0020] It is important that the polyhydric alcohol (a2) contains 20 mol % or more of one or more diols (a2-1) selected from the group consisting of ethylene glycol, diethylene glycol, 1,2-propanediol, and 1,3-propanediol, in order to obtain a coating film with excellent thickness.
[0021] Furthermore, since a coating film having excellent chemical resistance can be obtained from the polyhydric alcohol (a2), it is important that the polyhydric alcohol (a2) contains 5 to 20 mol % of a tri- or higher functional alcohol (a2-2).
[0022] Examples of the trifunctional or higher alcohol (a2-2) include aliphatic polyol compounds such as trimethylolethane, trimethylolpropane, glycerin, hexanetriol, and pentaerythritol; aromatic polyol compounds such as trihydroxybenzene; and polyether-modified polyol compounds obtained by ring-opening polymerization of the aliphatic polyol compounds or aromatic polyol compounds with cyclic ether compounds such as ethylene oxide, propylene oxide, tetrahydrofuran, ethyl glycidyl ether, propyl glycidyl ether, butyl glycidyl ether, phenyl glycidyl ether, and allyl glycidyl ether. These trifunctional or higher alcohols (a2-2) can be used alone or in combination of two or more.
[0023] As the polyhydric alcohol (a2), a polyhydric alcohol (a2-3) other than the diol (a2-1) and the tri- or higher functional alcohol (a2-2) can be used in combination.
[0024] Examples of the other polyhydric alcohols (a2-3) include 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 2-ethyl-1,3-propanediol, 2-methyl-1,4-butanediol, 2-ethyl-2-methyl-1,3-propanediol, 2-ethylbutane-1,4-butanediol, 2,3-dimethyl-1,4-butanediol, 3-methyl-1,5-pentanediol, 2,4- Aliphatic diols such as dimethyl-1,5-pentanediol, 3,3-dimethylpentane-1,5-diol, 2,2-diethyl-1,3-propanediol, 3-propylpentane-1,5-diol, 2,2-diethyl-1,4-butanediol, 2,4-diethyl-1,5-pentanediol, 2,2-dipropyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, and 2,5-diethyl-1,6-hexanediol; alicyclic structure-containing diol compounds such as cyclohexanediol and cyclohexanedialcohol; aromatic ring-containing diol compounds such as biphenol and bisphenol; polyether diol; polycarbonate diol, etc. These other polyhydric alcohols (a2-3) can be used alone or in combination of two or more kinds.
[0025] It is important that the ester group concentration of the polyester polyol (A) is 6 to 11 mmol / g in terms of the balance between the chemical resistance of the resulting coating film and the compatibility with the acrylic polyol (B).
[0026] The ester group concentration (mmol / g) refers to the number of millimoles of ester groups in 1 g of the polyester polyol (A), and is determined, for example, by a calculated value from the charged amount.
[0027] The hydroxyl value of the polyester polyol (A) is preferably from 50 to 250 mgKOH / g, since this leads to a better balance between the chemical resistance of the resulting coating film and the compatibility with the acrylic polyol (B).
[0028] The number average molecular weight of the polyester polyol (A) is preferably 800 to 5,000, since this further improves the balance between the chemical resistance of the resulting coating film and the compatibility with the acrylic polyol (B).
[0029] In the present invention, the hydroxyl value and acid value are measured in accordance with JIS test method K 0070-1992, and the average molecular weight is a value calculated in terms of polystyrene based on gel permeation chromatography (hereinafter abbreviated as "GPC") measurement.
[0030] The acrylic polyol (B) can be obtained, for example, by copolymerizing an unsaturated monomer (b1) having a hydroxyl group and another unsaturated monomer (b2).
[0031] Examples of the unsaturated monomer (b1) having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxy-n-butyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-n-butyl (meth)acrylate, 3-hydroxy-n-butyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, glycerin mono(meth)acrylate, polyoxyethylene mono(meth)acrylate, polyoxypropylene mono(meth)acrylate, polyoxybutylene mono(meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, polycaprolactone-modified hydroxyethyl mono(meth)acrylate, etc. These unsaturated monomers (b1) having a hydroxyl group can be used alone or in combination of two or more.
[0032] Examples of the other unsaturated monomers (b2) include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, β-carboxyethyl (meth)acrylate, ω-carboxy-polycaprolactone mono(meth)acrylate, 2-(meth)acryloyloxyethyl succinate, and 2-(meth)acryloyloxyethyl hexahydrophthalic acid; unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid, and half esters of these unsaturated dicarboxylic acids. unsaturated monomers having a carboxyl group, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylates having a hydrocarbon group such as butyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, behenyl (meth)acrylate, cyclohexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and benzyl (meth)acrylate; acrylamide, N,N-dimethyl (meth)acrylamide, (meth)acrylonitrile, 3-(meth)acryloylpropyltrimethoxysilane, N,N-dimethylaminoethyl (meth)acrylate, glycidyl (meth)acrylate, 2-(meth)acryloyloxyethyl acid phosphate, styrene, α-methylstyrene, p-methylstyrene, and p-methoxystyrene. These other unsaturated monomers (b2) can be used alone or in combination of two or more kinds.
[0033] The content of the unsaturated monomer (b1) having a hydroxyl group in the unsaturated monomer raw material of the acrylic polyol (B) is preferably 0.5 to 40 mass %, more preferably 1.5 to 35 mass %, in order to further improve the balance between chemical resistance and adhesion.
[0034] The content of the unsaturated monomer having a carboxyl group in the unsaturated monomer raw material of the acrylic polyol (B) is preferably 0.1 to 15% by mass since this further improves the chemical resistance.
[0035] In the present invention, "(meth)acrylic acid" refers to either or both of methacrylic acid and acrylic acid, "(meth)acrylate" refers to either or both of methacrylate and acrylate, and "(meth)acryloyl" refers to either or both of methacryloyl and acryloyl.
[0036] The acrylic polyol (B) can be produced by a known polymerization method using the monomer (b1) having a hydroxyl group and the other monomer (b2) as raw materials. However, a solution radical polymerization method is preferred because it is simple.
[0037] The method for producing the acrylic polyol (B) by the solution radical polymerization method includes a method in which each monomer as a raw material is dissolved in a solvent and / or the polyester polyol (A) and a polymerization reaction is carried out in the presence of a polymerization initiator. From the viewpoint of improving compatibility, it is preferable to carry out the polymerization reaction in the presence of the polyester polyol (A).
[0038] Examples of the solvent include hydrocarbon solvents such as toluene, xylene, cyclohexane, n-hexane, and octane; alcohol solvents such as methanol, ethanol, iso-propanol, n-butanol, iso-butanol, sec-butanol, and ethylene glycol monomethyl ether; ester solvents such as methyl acetate, ethyl acetate, n-butyl acetate, isobutyl acetate, and amyl acetate; and ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone. These solvents can be used alone or in combination of two or more.
[0039] Examples of the polymerization initiator include azo compounds such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), and azobiscyanovaleric acid; organic peroxides such as tert-butyl peroxypivalate, tert-butyl peroxybenzoate, tert-butyl peroxy-2-ethylhexanoate, di-tert-butyl peroxide, cumene hydroperoxide, benzoyl peroxide, and tert-butyl hydroperoxide; and inorganic peroxides such as hydrogen peroxide, ammonium persulfate, potassium persulfate, and sodium persulfate. These polymerization initiators can be used alone or in combination of two or more kinds. The polymerization initiator is preferably used in an amount of 0.1 to 10% by mass based on the total amount of monomers that are raw materials for the acrylic polyol (A).
[0040] In addition to the polymerization initiator, a chain transfer agent such as lauryl mercaptan, octyl mercaptan, 2-mercaptoethanol, octyl thioglycolate, 3-mercaptopropionic acid, or α-methylstyrene dimer can also be used, if necessary.
[0041] The weight average molecular weight (Mw) of the mixture of the polyester polyol (A) and the acrylic polyol (B) is preferably 8,000 to 150,000.
[0042] The curable resin composition of the present invention contains the polyester polyol (A) and the acrylic polyol (B). The mass ratio (A / B) of the polyester polyol (A) to the acrylic polyol (B) is preferably 10 / 90 to 70 / 30, and more preferably 15 / 85 to 60 / 40, in order to improve the balance between thickness and chemical resistance.
[0043] The hydroxyl value of the solid content of the curable resin composition of the present invention is preferably from 30 to 150 mgKOH / g, since this further improves the balance between chemical resistance and adhesion.
[0044] The acid value of the solid content of the curable resin composition of the present invention is preferably from 0.5 to 20 mgKOH / g, since this further improves the balance between chemical resistance, adhesion and water resistance.
[0045] The method for mixing the polyester polyol (A) and the acrylic polyol (B) is not particularly limited, but from the viewpoint of improving compatibility, a method in which the acrylic polyol (B) is synthesized in the presence of the polyester polyol (A) is preferred.
[0046] The coating material of the present invention contains the curable resin composition of the present invention, and other compounding ingredients such as inorganic pigments, organic pigments, extender pigments, coloring pigments, high-brightness pigments, cellulose derivatives, waxes, surfactants, stabilizers, flow adjusters, dyes, leveling agents, rheology control agents, ultraviolet absorbers, antioxidants, plasticizers, antistatic agents, defoamers, viscosity adjusters, light resistance stabilizers, weather resistance stabilizers, heat resistance stabilizers, pigment dispersants, and curing agents can be used.
[0047] By using a polyisocyanate compound (C) as the curing agent, the coating film properties can be further improved. Examples of the polyisocyanate compound (C) include aromatic diisocyanate compounds such as tolylene diisocyanate, diphenylmethane diisocyanate, m-xylylene diisocyanate, and m-phenylene bis(dimethylmethylene) diisocyanate; and aliphatic or alicyclic diisocyanate compounds such as pentamethylene diisocyanate, hexamethylene diisocyanate, lysine diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 2-methyl-1,3-diisocyanatocyclohexane, 2-methyl-1,5-diisocyanatocyclohexane, 4,4'-dicyclohexylmethane diisocyanate, and isophorone diisocyanate.
[0048] Further, as the polyisocyanate compound, a prepolymer having an isocyanate group obtained by subjecting the above diisocyanate compound to an addition reaction with a polyhydric alcohol; a compound having an isocyanurate ring obtained by cyclizing and trimerizing the above diisocyanate compound; a polyisocyanate compound having a urea bond or a biuret bond obtained by reacting the above diisocyanate compound with water; a homopolymer of an acrylic monomer having an isocyanate group, such as 2-isocyanatoethyl (meth)acrylate, 3-isopropenyl-α,α-dimethylbenzyl isocyanate, or (meth)acryloyl isocyanate; or a copolymer having an isocyanate group obtained by copolymerizing the above acrylic monomer having an isocyanate group with a monomer such as another acrylic monomer, a vinyl ester compound, a vinyl ether compound, an aromatic vinyl monomer, or a fluoroolefin.
[0049] The above polyisocyanate compounds (C) can be used alone or in combination of two or more kinds.
[0050] The amount of the polyisocyanate compound (C) used is preferably such that the equivalent ratio (NCO / OH) of the isocyanate group (NCO) of the polyisocyanate compound (C) to the hydroxyl group (OH) of the curable resin composition is in the range of 0.2 to 2, more preferably 0.5 to 1.5.
[0051] Each of the above-mentioned raw materials used in the curable resin composition and coating material of the present invention may be a biomass raw material.
[0052] The method for applying the coating material of the present invention varies depending on the article to be coated, but examples include methods using a gravure coater, roll coater, comma coater, knife coater, air knife coater, curtain coater, kiss coater, shower coater, wheeler coater, spin coater, dipping, screen printing, spraying, applicator, bar coater, brush, etc.
[0053] Furthermore, the coating material of the present invention can be diluted with an organic solvent to adjust the viscosity to a level suitable for the above coating method. Examples of the organic solvent include aromatic hydrocarbon solvents such as toluene and xylene; alcohol solvents such as methanol, ethanol, isopropanol, t-butanol, propylene glycol monomethyl ether, propylene glycol normal propyl ether, ethylene glycol monobutyl ether, and diacetone alcohol; ester solvents such as ethyl acetate, butyl acetate, isobutyl acetate, normal propyl acetate, propylene glycol monomethyl ether acetate, and 3-ethoxyethyl propionate; and ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, and cyclohexanone. These solvents can be used alone or in combination of two or more.
[0054] The coating material of the present invention can provide a cured coating film that is excellent in appearance and various coating physical properties on the surface of various articles.
[0055] The coating composition of the present invention may be applied directly to the article to be coated, or a primer coating material suitable for the article to be coated may be applied first, and then the coating composition of the present invention may be applied.
[0056] Examples of materials for the article to be coated include various metals such as iron, copper, zinc, aluminum, magnesium, etc. and their alloys; various plastics such as polycarbonate, acrylonitrile-butadiene-styrene copolymer, PC-ABS polymer alloy, polymethyl methacrylate, polyethylene terephthalate, polyamide, polypropylene, etc., and fiber-reinforced plastics in which these plastics are filled with fillers such as glass fibers; and wood.
[0057] Examples of articles having a cured coating film formed using the paint of the present invention include interior and exterior materials for various vehicles such as automobiles and railway cars; interior and exterior materials for buildings such as industrial machinery, exterior walls, roofs, glass, decorative panels, and wooden floors; civil engineering components such as soundproof walls and drainage ditches; housings for home appliances such as televisions, refrigerators, washing machines, and air conditioners; housings for electronic devices such as personal computers, smartphones, mobile phones, digital cameras, and game consoles; and housings for office automation equipment such as printers and facsimiles. EXAMPLES
[0058] The present invention will be described in more detail below with reference to specific examples. The hydroxyl value and acid value were measured in accordance with JIS test method K 0070-1992. The average molecular weight (Mw) was measured under the following GPC measurement conditions.
[0059] [GPC measurement conditions] Measurement equipment: High-speed GPC equipment (Tosoh Corporation "HLC-8220GPC") Column: The following columns manufactured by Tosoh Corporation were used, connected in series. "TSKgel G5000" (7.8mm I.D. x 30cm) x 1 "TSKgel G4000" (7.8mm I.D. x 30cm) x 1 "TSKgel G3000" (7.8mm I.D. x 30cm) x 1 "TSKgel G2000" (7.8mmI.D. x 30cm) x 1 Detector: RI (differential refractometer) Column temperature: 40℃ Eluent: tetrahydrofuran (THF) Flow rate: 1.0mL / min Injection volume: 100 μL (sample concentration 4 mg / mL in tetrahydrofuran solution) Standard sample: A calibration curve was prepared using the following monodisperse polystyrene.
[0060] (monodisperse polystyrene) "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-5000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation
[0061] (Synthesis Example 1: Production of polyester polyol (A-1)) 61 parts by mass of ethylene glycol, 314 parts by mass of diethylene glycol, 92 parts by mass of trimethylolpropane, 379 parts by mass of succinic acid, and 154 parts by mass of isophthalic acid were added to a reaction vessel equipped with a stirrer, a condenser, and a thermometer. An esterification reaction was carried out for 12 hours at 200 to 250°C while stirring under a nitrogen stream, and 148.9 parts by mass of condensed water was removed to obtain polyester polyol (A-1). The number average molecular weight (Mn) of this polyester polyol (A-1) was 1,416, the hydroxyl value was 115 mgKOH / g, and the acid value was 7.1 mgKOH / g. Ester group concentration [mmol / g] = (number of moles of carboxyl groups [mol]) / (mass of polyester polyol [g]) × 1000 =8.273 / 851.1×1000[mmol / g] =9.72[mmol / g]
[0062] (Synthesis Examples 2 to 6: Production of Polyester Polyols (A-2) to (A-6)) Polyester polyols (A-2) to (A-6) were obtained in the same manner as in Synthesis Example 1, except that the raw materials used in Synthesis Example 1 were changed as shown in Table 1.
[0063] (Synthesis Examples 7 to 10: Production of Polyester Polyols (RA-1) to (RA-4)) Polyester polyols (RA-1) to (RA-4) were obtained in the same manner as in Synthesis Example 1, except that the raw materials used in Synthesis Example 1 were changed as shown in Table 2.
[0064] The resin compositions and property values of the polyester polyols (A-1) to (A-6) obtained above are shown in Tables 1 and 2.
[0065] [Table 1]
[0066] [Table 2]
[0067] The resin compositions and property values of the polyester polyols (RA-1) to (RA-4) obtained above are shown in Table 3.
[0068] [Table 3]
[0069] (Example 1: Production of curable resin composition (1)) A flask equipped with a cooling tube, a thermometer, a dropping funnel, and a stirrer was charged with 200 parts by mass of polyester polyol (A-1) and 600 parts by mass of n-butyl acetate, and the internal temperature was raised to 100 ° C. Then, a mixture of 370.4 parts by mass of methyl methacrylate, 160.0 parts by mass of n-butyl methacrylate, 245.6 parts by mass of 2-hydroxyethyl methacrylate, 24.0 parts by mass of methacrylic acid, 160 parts by mass of n-butyl acetate, and 32 parts by mass of t-butylperoxy-2-ethylhexanoate was dropped over 3 hours. Then, the polymerization reaction was carried out for 15 hours while maintaining the internal temperature at 100 ° C. Then, 250 parts by mass of n-butyl acetate was added to obtain the desired curable resin composition (1). The weight average molecular weight (Mw) of the obtained resin was 25,540, the hydroxyl value of the solid content was 128 mgKOH / g, and the acid value of the solid content was 17.1 mgKOH / g.
[0070] (Examples 2 to 6: Production of curable resin compositions (2) to (6)) Curable resin compositions (2) to (6) were obtained in the same manner as in Example 1, except that the raw materials used in Example 1 were changed as shown in Table 4.
[0071] (Comparative Examples 1 to 4: Production of Curable Resin Compositions (R1) to (R4)) Except for changing the raw materials used in Example 1 as shown in Table 5, the same procedure as in Example 1 was carried out to obtain curable resin compositions (R1) to (R4).
[0072] The resin compositions and property values of the curable resin compositions (1) to (6) obtained above are shown in Table 4.
[0073] [Table 4]
[0074] Table 5 shows the resin compositions and property values of the curable resin compositions (R1) to (R4) obtained above.
[0075] [Table 5]
[0076] The abbreviations in the table are as follows. MMA: Methyl methacrylate BMA: n-Butyl methacrylate HEMA: 2-hydroxyethyl methyl methacrylate MAA: Methacrylic acid
[0077] [Paint preparation] The curable resin composition obtained above and a curing agent (Sumika Covestro Urethane Co., Ltd.'s "Sumijul N-3300", a polyisocyanate compound) were mixed uniformly. The blending ratio of the curable resin composition and the curing agent was set so that the equivalent of the hydroxyl group in the curable resin composition and the equivalent of the isocyanate group in the curing agent were 1:1. Next, the paint was prepared by diluting with a mixed solvent (butyl acetate / diacetone alcohol / isobutyl acetate / ethyl acetate = 30 / 30 / 30 / 10 (mass ratio)) so that the viscosity was 9 to 10 seconds (23 ° C.) in "Viscosity Cup NK-2" manufactured by Anest Iwata Corporation.
[0078] [Preparation of cured coating film X for evaluation] The coating material obtained above was spray-coated onto an ABS (acrylonitrile-butadiene-styrene copolymer) substrate (50 mm × 70 mm × 1 mm) so that the film thickness after drying would be 15 to 25 μm, and the coating was dried by heating in a dryer at 80°C for 30 minutes, and then dried at 25°C for 7 days to produce cured coating film X for evaluation.
[0079] [Preparation of cured coating film Y for evaluation] The coating material obtained above was spray-coated onto a PC (polycarbonate) substrate (50 mm × 70 mm × 1 mm) so that the film thickness after drying would be 20 to 30 μm, and the coating was dried by heating in a dryer at 80°C for 30 minutes, and then dried at 25°C for 7 days to produce cured coating film Y for evaluation.
[0080] [Adhesion evaluation] The cured coating film for evaluation obtained above was cut with a cutter to make 1 mm wide squares, so that the number of squares was 100. Next, cellophane tape was applied so as to cover all the squares, and the operation of quickly peeling it off was repeated four times, and the adhesion was evaluated according to the following criteria based on the number of squares remaining that were adhered. ○:100 pieces △:70~99 pieces ×: 69 or less
[0081] [Evaluation of water-resistant adhesion] The cured coating film for evaluation obtained above was immersed in water at 40° C. for 240 hours, and then the same procedure as in the adhesion evaluation above was carried out to evaluate the water-resistant adhesion according to the following criteria. ○:100 pieces △:70~99 pieces ×: 69 or less
[0082] [Evaluation of chemical resistance] A chemical (Neutrogena, Ultra Sheer Dry Touch Sunscreen, SPF 55) was applied to the cured coating obtained above at 20 mg / cm2, and then dried in a dryer at 55°C for 4 hours. The coating surface was then washed with a neutral detergent and left at room temperature for 24 hours, after which the chemical resistance was evaluated according to the following criteria. ◎: No trace ○: Some traces △: Traces present ×: The base material of the substrate is exposed
[0083] [Appearance evaluation] The thickness of the cured coating film for evaluation obtained above was evaluated visually. ◎: Very meaty feel 〇: Strong meaty feel △: Weak meatiness ×: No meaty feeling
[0084] The evaluation results of the paints (1) to (6) obtained above are shown in Table 6.
[0085] [Table 6]
[0086] The evaluation results of the paints (R1) to (R4) obtained above are shown in Table 7.
[0087] [Table 7]
[0088] It was confirmed that the cured coating films obtained from the curable resin compositions of the present invention in Examples 1 to 6 were excellent in appearance (thickness), adhesion, water resistance, and chemical resistance.
[0089] On the other hand, in Comparative Example 1, the amount of the tri- or higher functional alcohol (a2-2) in the polyhydric alcohol (a2) was less than the lower limit of the present invention, but it was confirmed that the chemical resistance of the cured coating film was insufficient.
[0090] Comparative Example 2 is an example in which the ester group concentration of the polyester polyol (A) is higher than the upper limit of the present invention, but it was confirmed that the compatibility with the acrylic polyol (B) was poor and the appearance of the cured coating film was insufficient.
[0091] In Comparative Example 3, the amount of diol (a2-1) in the polyhydric alcohol (a2) was less than the lower limit of the present invention, but it was confirmed that the appearance of the cured coating film was insufficient.
[0092] Comparative Example 4 is an example in which the amount of the aliphatic dicarboxylic acid (a1-1) in the polyvalent carboxylic acid (a1) is less than the lower limit of the present invention, but it was confirmed that the appearance of the cured coating film was insufficient.
Claims
1. A curable resin composition comprising a polyester polyol (A) which is a reaction product of a polyvalent carboxylic acid (a1) and a polyhydric alcohol (a2), and an acrylic polyol (B), wherein the mass ratio (A / B) of the polyester polyol (A) to the acrylic polyol (B) is 10 / 90 to 70 / 30, the polyvalent carboxylic acid (a1) contains 20 mol% or more of an aliphatic dicarboxylic acid (a1-1) having a linear alkyl group having 4 to 10 carbon atoms, the polyhydric alcohol (a2) contains 20 to 80 mol% of one or more diols (a2-1) selected from the group consisting of ethylene glycol, diethylene glycol, 1,2-propanediol, and 1,3-propanediol, and contains 5 to 20 mol% of a trifunctional or higher alcohol (a2-2), and the ester group concentration of the polyester polyol (A) is 6 to 11 mmol / g.
2. 2. The curable resin composition according to claim 1, having a hydroxyl value of the solid content of 30 to 150 mgKOH / g.
3. A coating material comprising the curable resin composition according to claim 1 or 2 and a polyisocyanate compound (C).
4. An article having a cured coating film of the coating material according to claim 3.
Citation Information
Patent Citations
JP1974055788A
Film-forming hydrophilic resin and coating material composition
JP1998338719A
Method for producing aqueous resin dispersion
JP2004149593A
Adhesive layer and adhesive sheet
JP2022079443A
Polyester polyol resin and coating
WO2018084062A1