Method for manufacturing wide filter substrate
The use of core-sheath type composite long fibers with controlled heating and pressure application addresses the challenge of uniform fluffing in wide spunbond nonwoven fabrics, ensuring consistent fluffing properties and improved production efficiency.
Patent Information
- Application Number
- JP2020199314
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-01
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-12-01
AI Technical Summary
Existing methods for producing wide spunbond nonwoven fabrics for filter base materials face challenges in achieving uniform fluffing properties across the width, leading to uneven surfaces and reduced efficiency when using heating rolls longer than 4 m.
A method involving core-sheath type composite long fibers with specific melting points and viscosities, combined with controlled heating and pressure application using rolls with convex surfaces, ensures uniform fusion and fixation of fibers, resulting in a wide filter base material with consistent fluffing properties.
The method produces a filter base material with uniform fluffing properties across the width, enhancing production efficiency and preventing uneven fluffiness, especially in the center, thus improving the effectiveness of dust removal.
Smart Images

Figure 0007582657000001 
Figure 0007582657000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a filter substrate having a surface that is resistant to fluffing, and in particular to a method for producing a filter substrate that, when a wide-width filter substrate is produced, has equal resistance to fluffing in the width direction. [Background technology]
[0002] Conventionally, spunbond nonwoven fabrics with a relatively high basis weight have been used as filter substrates for filters for industrial dust collectors, etc. Specifically, spunbond nonwoven fabrics have been used in which the constituent fibers are core-sheath type composite long fibers made of polyethylene terephthalate with a high melting point and a sheath component made of a copolymer polyester with a low melting point, and the constituent fibers are partially pressure-bonded to each other by softening or melting the copolymer polyester (Patent Document 1).
[0003] When dust accumulates on the surface of a dust collector filter during use and the pressure loss exceeds a predetermined value, the dust is brushed off with a pulse jet or compressed air. However, if the filter surface is fluffy, the dust becomes entangled in the fluff and is difficult to brush off. Therefore, filter substrates used in dust collector filters and the like are required to have a surface that is less likely to become fluffy.
[0004] The technique described in Patent Document 1 proposes preventing surface fluffing by passing a fiber fleece between a pair of heating rolls and fusing and fixing the core-sheath type composite long fibers constituting the surface layer to obtain a spunbonded nonwoven fabric. This method is also effective for single-width (about 1 m) or double-width (about 2 m) fiber fleece, but for wide-width (about 4 m or more) fiber fleece exceeding double width, the surface fluffiness in the width direction of the obtained wide-width spunbonded nonwoven fabric is not uniform. That is, when a wide-width fiber fleece is passed between a pair of heating rolls, a heating roll having an axial length of 4 m or more must be used, and the surface fluffiness is particularly poor in the central part of the obtained spunbonded nonwoven fabric. This is because if the axial length of the heating roll is long, it becomes difficult to apply a uniform pressure in the axial direction to the fiber fleece, especially in the central part of the heating roll.
[0005] [Patent Document 1] JP 2005-7268 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a method for producing a filter substrate having a relatively uniform fluffiness across the width, even when a wide fiber fleece is passed between a pair of heated rolls to obtain a wide filter substrate made of a spunbonded nonwoven fabric. [Means for solving the problem]
[0007] The present invention relates to The following configuration requirements: That is, the present invention solves the above problem by adopting a core component of polyethylene terephthalate. It consists of The sheath component has a lower melting point than the polyethylene terephthalate. It has a melting point of 220℃ to 240℃, and Relative viscosity ηR1.35~1.42 The isophthalic acid is copolymerized in an acid component at 6 to 12 mol %. Copolymer polyester The cross section is a six-leaf core-sheath type. It is made of core-sheath type composite long fiber and its width is 4~5m. The weight is 120g / m2 ~350g / m 2 The present invention relates to a method for producing a filter substrate, characterized in that the sheet-like fiber fleece described above is passed between a pair of heated rolls having an axial length of 4 to 5 m to soften or melt the sheath component of the core-sheath type composite long fibers, thereby fusion-fixing the core-sheath type composite long fibers to each other.
[0008] The core-sheath type composite continuous fiber used in the present invention has a core component made of polyethylene terephthalate. The polyethylene terephthalate has a melting point of about 256°C and a relative viscosity ηR of about 1.38. The melting point is the temperature at which an extreme value is obtained on the melting endothermic curve measured at a temperature rise rate of 20°C / min using a PerkinElmer DSC-2 differential scanning calorimeter. The relative viscosity ηR is measured by using a solution of an equal mixture of phenol and tetrachloroethane as a solvent and measuring the relative viscosity ηR at 100 cm 3 0.5 g of polyethylene terephthalate sample was dissolved in the solution, and the measurement was carried out at a temperature of 20°C.
[0009] The sheath component of the core-sheath type composite long fiber used in the present invention is formed of a copolymer polyester whose melting point is lower than that of the polyethylene terephthalate forming the core component. By making the melting point of the sheath component lower than that of the core component, only the sheath component is melted or softened, that is, the core component maintains its original fiber form, and the core-sheath type composite long fiber is fused and fixed to each other. The melting point of the sheath component is specifically 220°C to 240°C. The relative viscosity ηR of the sheath component is 1.35 to 1.42. If the relative viscosity ηR exceeds 1.42, the fluidity of the sheath component when softened or melted decreases, which is not preferable. If the relative viscosity ηR is less than 1.35, the fluidity of the sheath component when softened or melted becomes too high, and the copolymer polyester is likely to adhere to the heating roll, which is not preferable. In other words, when the sheath component is softened or melted, the relative viscosity ηR at which the sheath component has appropriate fluidity is 1.35 to 1.42.
[0010] The copolymerized polyester is obtained by adding a third component as an acid component and polymerizing it. As the third component, isophthalic acid is used. The amount of the third component added is 6 to 12 mol % in the acid component. By adjusting the amount of the third component added and the molecular weight of the copolymerized polyester, a copolymerized polyester having a relative viscosity ηR of 1.35 to 1.42 can be obtained.
[0011] The sheath-core composite continuous fiber is a six-leaf sheath-core type having a cross section as shown in Figure 1. That is, the sheath components, each consisting of six elliptical cylinders, are arranged at equal intervals around the periphery of a roughly cylindrical core component, parallel to the axial direction of the core component. The core component is the white part in the center, and the sheath component is the dark black part. The fineness of the sheath-core composite continuous fiber is about 1.5 to 5.0 decitex.
[0012] The core-sheath type composite long fibers are accumulated in a sheet shape to obtain a fiber fleece. The width of this fiber fleece is as wide as 4 to 5 m. By making the fiber fleece wide, a filter substrate made of a wide spunbond nonwoven fabric can be obtained, improving production efficiency. The basis weight of the fiber fleece is 120 to 350 g / m 2 The basis weight of the filter substrate made of the obtained spunbonded nonwoven fabric is 120 to 350 g / m 2 The weight is 120g / m 2 If the weight is less than 350 g / m, the rigidity of the filter substrate tends to decrease, making it difficult to brush off the dust accumulated on the filter. 2 If the thickness exceeds this range, heat is less likely to be conducted to the inside when passing through heated rolls, and delamination tends to occur easily when the filter is folded to produce a pleated filter.
[0013] After obtaining a wide fiber fleece, it is passed between a pair of heating rolls having an axial length of 4 to 5 m. The length of the heating rolls is set to 4 to 5 m in order to apply heat and pressure over the entire width of the fiber fleece. As the pair of heating rolls, a pair of heating smooth rolls, a pair of heating uneven rolls, or one of the heating uneven rolls and the other of the heating smooth roll is used. The surface temperature of the heating roll is set to a temperature at which only the sheath component of the core-sheath type composite long fiber softens or melts. Specifically, the surface temperature of the heating roll is about 210°C to 220°C, depending on the linear pressure. The linear pressure is about 400 to 700 N / cm.
[0014] The uneven roll has convex and concave portions on its peripheral surface. The shape of the convex portions is arbitrary, and for example, uneven rolls having spiral, stripe or dot-shaped convex portions are used. In particular, when an uneven roll and a smooth roll are combined to form a pair of heating rolls, it is preferable to use an uneven roll having dot-shaped convex portions uniformly arranged on the roll surface. The area of the tip surface of the dot-shaped convex portions (the surface that comes into contact with the fiber fleece) is 0.1 to 1.0 mm 2 The density of the dot-like protrusions is preferably about 4 to 80 pieces / cm. 2 The total area of the tip faces of the projections is preferably 5 to 40% of the area of the peripheral surface of the roll, and more preferably 10 to 30%.
[0015] The fiber fleece is passed between a pair of heating rolls. This heats and pressurizes the fiber fleece, softening or melting the sheath components of the core-sheath type composite long fibers. The core-sheath type composite long fibers are then fused and fixed to each other to obtain a filter substrate. In particular, when a pair of heating rolls is used in combination with a concave-convex roll and a smooth roll, the sheath components of the core-sheath type composite long fibers in the fiber fleece that come into contact with the convex portions soften or melt, and a filter substrate having partial regions in which the long fibers are fused and fixed to each other can be obtained.
[0016] The obtained filter substrate can be processed in various ways to produce a filter. For example, it can be cut to a predetermined size and attached with a support to produce a filter. It can also be folded to form pleats and used as a pleated filter. Effect of the Invention
[0017] According to the production method of the present invention, it is possible to obtain a filter substrate made of a wide spunbonded nonwoven fabric having uniform fluffiness in the width direction, thereby improving the production efficiency of the filter substrate. EXAMPLES
[0018] Example 1 As the core component, polyethylene terephthalate with a melting point of 256°C and a relative viscosity ηR of 1.38 was prepared. On the other hand, as the sheath component, a copolymer polyester with a melting point of 230°C and a relative viscosity ηR of 1.37 was prepared. The core component and sheath component were fed to a conjugate melt spinning device so that the ratio of core component to sheath component was 6:4 (mass ratio), and conjugate melt spinning was performed at a spinning temperature of 290°C to spin a six-leaf core-sheath type conjugate long fiber having a cross section as shown in Figure 1. The spun long fiber group was pulled by an air sucker at a speed of about 5000 m / min and then opened, and the long fiber group was accumulated on a moving collection conveyor to obtain a fiber fleece with a width of 4.3 m. The basis weight of this fiber fleece was 260 g / m 2 The fineness of the long fibers was 3.0 decitex.
[0019] The fiber fleece was passed through a pair of heated rolls consisting of a heated uneven roll and a heated smooth roll, each having an axial length of 4.5 m. The heated uneven roll had dot-like projections uniformly arranged over the entire roll, and the tip surface area of the projections was 0.5 mm 2 , the density of the protrusions is 25 / cm 2 The total area of the tip surfaces of the convex parts was 13% of the peripheral area of the roll. The surface temperatures of the uneven roll and the smooth roll were heated to 210°C, and the linear pressure applied to the fiber fleece was 590N / cm. 2A filter substrate approximately 4 m wide was obtained.
[0020] Example 2 A filter substrate was obtained in the same manner as in Example 1, except that a copolymer polyester having a melting point of 230°C and a relative viscosity ηR of 1.40 was used as the sheath component instead of the copolymer polyester having a melting point of 230°C and a relative viscosity ηR of 1.37.
[0021] Comparative Example 1 A filter substrate was obtained in the same manner as in Example 1, except that a copolymer polyester having a melting point of 230°C and a relative viscosity ηR of 1.44 was used as the sheath component instead of the copolymer polyester having a melting point of 230°C and a relative viscosity ηR of 1.37.
[0022] Comparative Example 2 A filter substrate was obtained in the same manner as in Comparative Example 1, except that the surface temperatures of the uneven roll and the smooth roll were changed to 215°C.
[0023] Comparative Example 3 A filter substrate was obtained in the same manner as in Comparative Example 1, except that the surface temperatures of the uneven roll and the smooth roll were changed to 220° C. However, copolymerized polyester, fiber pieces, etc. were attached to the uneven roll surface, and continuous production was not possible. Therefore, the fuzziness evaluation described below was not performed.
[0024] [Evaluation of fuzziness] From the filter substrate having a width of about 4 m obtained in Examples 1 and 2 and Comparative Examples 1 and 2, circular pieces having a diameter of 13 cm were taken from the positions a, b, c, d, e, and f shown in FIG. 2 across the width. Then, a hole having a diameter of about 6 mm was drilled in the center of the circular piece to prepare a test piece. Using this test piece, the fuzziness was evaluated according to JIS L 1913 6.6.2, the tapered method. When the test piece was attached to the sample holder, it was attached so that the surface in contact with the smooth roll was rubbed by the abrasive wheel. The abrasive wheel used was No. CS-10, the load applied was 500 g, and the number of rubs was 100. Then, the fuzziness was evaluated on a 5-point scale, with the most severe fuzz being grade 1 and the almost no fuzz being grade 5. The results are shown in Table 1.
[0025] [Table 1] ━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━ Fuzziness (grade) ━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━ abcdef ━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━ Example 1 4.5 4.5 3.5 4.0 4.5 4.5 Example 2 4.0 3.0 3.0 3.0 3.5 4.0 Comparative Example 1 4.0 1.5 1.0 1.0 2.0 4.0 Comparative Example 2 4.5 4.5 2.0 2.0 3.5 4.5 ━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━
[0026] As is clear from a comparison between Examples 1 and 2 and Comparative Examples 1 and 2, the filter substrates obtained by the methods of Examples 1 and 2 show less change in fuzziness across the width of the wide filter substrate, compared to the filter substrates obtained by the methods of Comparative Examples 1 and 2. [Brief description of the drawings]
[0027] [Figure 1] 1 is a schematic diagram showing an example of a cross section of a core-sheath type conjugated continuous fiber used in the present invention. [Diagram 2] FIG. 2 is a partial plan view showing the location where test pieces were taken from a wide filter substrate to evaluate fuzziness in the examples and comparative examples.
Claims
1. The core component is made of polyethylene terephthalate, the sheath component has a melting point of 220°C to 240°C, which is lower than that of the polyethylene terephthalate, and a relative viscosity ηR of 1.35 to 1.42, and is made of an isophthalic acid copolymerized polyester in which 6 to 12 mol % of isophthalic acid is copolymerized in the acid component; A method for producing a filter substrate, comprising: passing a sheet-like fiber fleece having a width of 4 to 5 m and a basis weight of 120 g / m2 to 350 g / m2, the sheet being composed of sheath-core composite long fibers having a hexapole sheath-core cross section, between a pair of heated rolls having an axial length of 4 to 5 m, softening or melting the sheath component of the sheath-core composite long fibers, thereby fusion-fixing the core-sheath composite long fibers to each other.
2. 2. The method for producing a filter substrate according to claim 1, wherein one of the pair of heating rolls is an uneven roll and the other is a smooth roll.
3. A method for producing a pleated filter, comprising folding the filter substrate obtained by the method according to claim 1 to form pleats.
Citation Information
Patent Citations
Nonwoven fabric, primary base cloth for tufted carpet, tufted carpet, base material for filter and filter
JP1997273063A
Ultrafine staple-containing composite nonwoven fabric and its production
JP2000017558A
Polyester-based filament nonwoven fabric
JP2005105434A