Multilayer ceramic capacitor and its manufacturing method

By adjusting the magnesium content in the side margin portions of multilayer ceramic capacitors to form regions with varying magnesium compositions, the capacitor's reliability is improved through enhanced breakdown voltage and moisture resistance, addressing the void-related issues in ultra-small and high-capacity designs.

JP7582731B2Active Publication Date: 2024-11-13SAMSUNG ELECTRO MECHANICS CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2018203644
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-08-09
Filing Date
2018-10-30
Publication Date
2024-11-13
Estimated Expiration
2038-10-30

AI Technical Summary

Technical Problem

Existing multilayer ceramic capacitors face issues with reduced reliability due to voids at the interface between the ceramic body and side margin portions, leading to low breakdown voltage and moisture resistance, which are exacerbated in ultra-small and high-capacity designs.

Method used

The solution involves adjusting the content of magnesium (Mg) in the side margin portions of the multilayer ceramic capacitor to form two regions with different magnesium compositions, where the content in the region adjacent to the internal electrodes is higher, thereby controlling the oxide layer length and improving the breakdown voltage and moisture resistance.

Benefits of technology

This approach enhances the breakdown voltage and moisture resistance reliability by minimizing voids and ensuring better adhesion between electrodes, thus improving the overall performance of ultra-small and high-capacity capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582731000001
    Figure 0007582731000001
  • Figure 0007582731000002
    Figure 0007582731000002
  • Figure 0007582731000003
    Figure 0007582731000003
Patent Text Reader

Abstract

To provide a multilayer ceramic capacitor and a method of manufacturing the same.SOLUTION: There is provided a multilayer ceramic capacitor including: a ceramic body including dielectric layers and having first and second surfaces opposing each other, third and fourth surfaces connecting the first and second surfaces, and fifth and sixth surfaces connected to the first to fourth surfaces and opposing each other; a plurality of internal electrodes disposed at the inside of the ceramic body, exposed to the first and second surfaces, and each having one end exposed to the third or fourth surface; and first and second side margin portions disposed on end portions of the internal electrodes exposed to the first and second surfaces. Each of the first and second side margin portions is divided into a first region adjacent to an outer side surface of the side margin portion and a second region adjacent to the internal electrodes exposed to the first and second surfaces, and a content of magnesium (Mg) contained in the second region is larger than that of magnesium (Mg) contained in the first region.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a multilayer ceramic capacitor and a manufacturing method thereof, which can improve reliability by controlling the length of an oxide layer of an internal electrode by adjusting the magnesium (Mg) content contained in a side margin portion. [Background technology]

[0002] Typically, electronic components using ceramic materials, such as capacitors, inductors, piezoelectric elements, varistors, or thermistors, comprise a ceramic body made of ceramic material, an internal electrode formed inside the body, and an external electrode provided on the surface of the ceramic body so as to be connected to the internal electrode.

[0003] In recent years, as electronic products have become smaller and more multifunctional, chip components have also tended to become smaller and more functional. This has led to a demand for multilayer ceramic capacitors that are small yet have high capacitance.

[0004] In order to reduce the size and increase the capacitance of multilayer ceramic capacitors, it is necessary to maximize the effective electrode area (increase the effective volume fraction required to achieve capacitance).

[0005] In order to realize a small-sized and high-capacity multilayer ceramic capacitor as described above, when manufacturing a multilayer ceramic capacitor, the internal electrodes are exposed in the width direction of the body, thereby maximizing the area of ​​the internal electrodes in the width direction through a margin-free design, and after manufacturing such a chip, a margin portion is separately attached to the exposed electrode surface in the width direction of the chip before firing to complete the process.

[0006] However, in the above method, during the process of forming the side margin portion, many voids are generated at the interface where the ceramic body and the side margin portion come into contact, which may reduce reliability.

[0007] In addition, voids formed at the interface where the ceramic body and side margins come into contact cause electric field concentration, which results in a problem of a lower breakdown voltage (BDV).

[0008] Furthermore, the voids may cause a decrease in the sintered density of the outer surface, resulting in a decrease in the reliability of moisture resistance.

[0009] Therefore, research is needed to prevent the decrease in breakdown voltage (BDV) and humidity resistance reliability in ultra-small and high-capacity products. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Korean Patent Publication No. 2010-0136917 Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention aims to provide a multilayer ceramic capacitor and a manufacturing method thereof that can improve reliability by controlling the length of the oxide layer of the internal electrode by adjusting the magnesium (Mg) content in the side margin portion. [Means for solving the problem]

[0012] One embodiment of the present invention provides a multilayer ceramic capacitor including: a ceramic body including a dielectric layer, the ceramic body having first and second surfaces opposing each other, third and fourth surfaces connecting the first and second surfaces, and fifth and sixth surfaces connected to the first to fourth surfaces and opposing each other; a plurality of internal electrodes disposed within the ceramic body and exposed to the first and second surfaces, the plurality of internal electrodes having one end exposed to the third or fourth surface; and first and second side margin portions disposed on ends of the internal electrodes exposed to the first and second surfaces, the first and second side margin portions being divided into a first region adjacent to outer surfaces of the side margin portions and a second region adjacent to the internal electrodes exposed to the first and second surfaces, and the second region having a higher magnesium (Mg) content than the first region.

[0013] Another embodiment of the present invention includes the steps of: preparing a first ceramic green sheet on which a plurality of first internal electrode patterns are formed at predetermined intervals and a second ceramic green sheet on which a plurality of second internal electrode patterns are formed at predetermined intervals; laminating the first ceramic green sheet and the second ceramic green sheet so that the first internal electrode patterns and the second internal electrode patterns intersect, thereby forming a ceramic green sheet laminate body; cutting the ceramic green sheet laminate body so that ends of the first internal electrode patterns and the second internal electrode patterns have side surfaces exposed in the width direction; The present invention provides a method for manufacturing a multilayer ceramic capacitor, the method including: forming first and second side margin portions on side surfaces where ends of first and second internal electrode patterns are exposed; and manufacturing a ceramic body including dielectric layers and first and second internal electrodes by firing the cut multilayer body, wherein the first and second side margin portions are divided into a first region adjacent to outer surfaces of the side margin portions and a second region adjacent to the first and second internal electrodes, and the second region has a higher magnesium (Mg) content than the first region. [Effects of the Invention]

[0014] According to one embodiment of the present invention, the first and second side margin portions are divided into a first region adjacent to the outer surfaces of the side margin portions and a second region adjacent to the internal electrodes exposed on the first and second surfaces of the ceramic body. The magnesium (Mg) content in the second region is adjusted to be higher than the magnesium (Mg) content in the first region, thereby increasing the breakdown voltage (BDV) and improving reliability.

[0015] Specifically, by adjusting the magnesium (Mg) content in the side margin region adjacent to the width direction of the ceramic body, the length of the oxide layer at the tip of the internal electrode exposed to the width direction of the ceramic body can be controlled, thereby increasing the breakdown voltage (BDV) and improving moisture resistance reliability. [Brief explanation of the drawings]

[0016] [Figure 1] 1 is a schematic perspective view showing a multilayer ceramic capacitor according to an embodiment of the present invention; [Figure 2] FIG. 2 is a perspective view showing the appearance of the ceramic body of FIG. [Figure 3] 3 is a perspective view showing the ceramic green sheet laminate body of FIG. 2 before firing. FIG. [Figure 4] FIG. 3 is a side view seen from the direction A in FIG. 2. [Figure 5a] 5A to 5C are cross-sectional views schematically illustrating a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention. [Figure 5b] 5A to 5C are cross-sectional views schematically illustrating a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention. [Figure 5c] 5A to 5C are cross-sectional views schematically illustrating a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention. [Figure 5d] 10 is a perspective view schematically illustrating a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention. [Figure 5e] 5A to 5C are cross-sectional views schematically illustrating a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention. [Figure 5f] 5A to 5C are cross-sectional views schematically illustrating a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention. [Figure 6] 1 is a graph comparing breakdown voltages (BDV) according to an embodiment of the present invention and a comparative example. DETAILED DESCRIPTION OF THE INVENTION

[0017] Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. However, the embodiments of the present invention can be modified into various other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those having average knowledge in the art. Therefore, the shapes and sizes of elements in the drawings may be enlarged or reduced (or highlighted or simplified) for clearer explanation.

[0018] FIG. 1 is a schematic perspective view showing a multilayer ceramic capacitor according to an embodiment of the present invention.

[0019] FIG. 2 is a perspective view showing the appearance of the ceramic body of FIG.

[0020] FIG. 3 is a perspective view showing the ceramic green sheet laminate body of FIG. 2 before firing.

[0021] FIG. 4 is a side view seen from the direction A in FIG.

[0022] 1 to 4, the multilayer ceramic capacitor 100 according to the present embodiment includes a ceramic body 110, a plurality of internal electrodes 121, 122 formed inside the ceramic body 110, and external electrodes 131, 132 formed on the outer surface of the ceramic body 110.

[0023] The ceramic body 110 may have a first surface 1 and a second surface 2 facing each other, a third surface 3 and a fourth surface 4 connecting the first surface and the second surface, and a fifth surface 5 and a sixth surface 6 which are the upper and lower surfaces.

[0024] The first surface 1 and the second surface 2 can be defined as surfaces that face each other in the width direction of the ceramic body 110, the third surface 3 and the fourth surface 4 can be defined as surfaces that face each other in the length direction, and the fifth surface 5 and the sixth surface 6 can be defined as surfaces that face each other in the thickness direction.

[0025] The shape of the ceramic body 110 is not particularly limited, but may be a rectangular parallelepiped shape as shown in the drawing.

[0026] The plurality of internal electrodes 121, 122 formed inside the ceramic body 110 have one end exposed to the third surface 3 or the fourth surface 4 of the ceramic body.

[0027] The internal electrodes 121 and 122 may be a pair of a first internal electrode 121 and a second internal electrode 122 having different polarities.

[0028] One end of the first internal electrode 121 may be exposed to the third surface 3 , and one end of the second internal electrode 122 may be exposed to the fourth surface 4 .

[0029] The other ends of the first internal electrode 121 and the second internal electrode 122 are formed at a predetermined distance from the third surface 3 or the fourth surface 4.

[0030] First and second external electrodes 131 and 132 are formed on the third and fourth surfaces 3 and 4 of the ceramic body and can be electrically connected to the internal electrodes, respectively.

[0031] The multilayer ceramic capacitor 100 according to one embodiment of the present invention includes a plurality of internal electrodes 121, 122 disposed inside the ceramic body 110, exposed to the first and second surfaces 1, 2, and having one end exposed to the third surface 3 or the fourth surface 4, and a first side margin portion 112 and a second side margin portion 113 disposed on the ends of the internal electrodes 121, 122 exposed to the first surface 1 and the second surface 2.

[0032] A plurality of internal electrodes 121 and 122 are formed inside the ceramic body 110. Ends of the internal electrodes 121 and 122 are exposed to a first surface 1 and a second surface 2, which are surfaces in the width direction of the ceramic body 110, and a first side margin portion 112 and a second side margin portion 113 are disposed on the exposed ends.

[0033] The average thickness of the first side margin portion 112 and the second side margin portion 113 may be not less than 2 μm and not more than 10 μm.

[0034] According to one embodiment of the present invention, the ceramic body 110 may be composed of a laminate in which a plurality of dielectric layers 111 are stacked, and a first side margin portion 112 and a second side margin portion 113 disposed on both sides of the laminate.

[0035] The plurality of dielectric layers 111 may be in a sintered state, and may be integrated to the extent that the boundaries between adjacent dielectric layers are not recognizable.

[0036] The length of the ceramic body 110 corresponds to the distance from the third surface 3 to the fourth surface 4 of the ceramic body.

[0037] The length of the dielectric layer 111 defines the distance between the third face 3 and the fourth face 4 of the ceramic body.

[0038] Although not limited thereto, according to one embodiment of the present invention, the length of the ceramic body may be 400 to 1400 μm, more specifically, the length of the ceramic body may be 400 to 800 μm or 600 to 1400 μm.

[0039] Internal electrodes 121 and 122 may be formed on the dielectric layer 111, and the internal electrodes 121 and 122 may be formed inside the ceramic body by sintering with one dielectric layer sandwiched therebetween.

[0040] 3, a first internal electrode 121 is formed on the dielectric layer 111. The first internal electrode 121 is not formed over the entire length of the dielectric layer. That is, one end of the first internal electrode 121 may be formed at a predetermined distance from the fourth surface 4 of the ceramic body, and the other end of the first internal electrode 121 may be formed up to and exposed to the third surface 3.

[0041] The end of the first internal electrode exposed on the third surface 3 of the ceramic body is connected to the first external electrode 131 .

[0042] Unlike the first internal electrode, one end of the second internal electrode 122 is formed at a predetermined distance from the third surface 3, and the other end of the second internal electrode 122 is exposed to the fourth surface 4 and connected to the second external electrode 132.

[0043] The internal electrodes may be stacked in 400 layers or more to achieve a high-capacity multilayer ceramic capacitor, but the number of layers is not necessarily limited to this.

[0044] The dielectric layer 111 may have the same width as the first internal electrode 121. That is, the first internal electrode 121 may be formed over the entire dielectric layer 111 in the width direction.

[0045] Although not limited thereto, according to one embodiment of the present invention, the width of the dielectric layer and the width of the internal electrode may be 100 to 900 μm, more specifically, the width of the dielectric layer and the width of the internal electrode may be 100 to 500 μm or 100 to 900 μm.

[0046] As the ceramic body becomes smaller, the thickness of the side margin portion can affect the electrical characteristics of the multilayer ceramic capacitor. According to one embodiment of the present invention, the thickness of the side margin portion is formed to be 10 μm or less, thereby improving the characteristics of the miniaturized multilayer ceramic capacitor.

[0047] That is, by forming the thickness of the side margin portion to 10 μm or less, the overlapping area of ​​the internal electrodes that form the capacitance can be maximized, thereby realizing a multilayer ceramic capacitor with a high capacitance and a small size.

[0048] The ceramic body 110 may be composed of an active portion that contributes to forming the capacitance of the capacitor, and upper and lower cover portions that serve as upper and lower margin portions formed above and below the active portion, respectively.

[0049] The active portion can be formed by repeatedly stacking a plurality of first and second internal electrodes 121 and 122 with a dielectric layer 111 sandwiched therebetween.

[0050] The upper and lower cover portions may have the same material and structure as the dielectric layer 111, except that they do not include internal electrodes.

[0051] That is, the upper and lower cover parts may include a ceramic material, for example, a barium titanate (BaTiO3) based ceramic material.

[0052] The upper and lower cover parts may each have a thickness of 20 μm or less, but are not necessarily limited thereto.

[0053] In one embodiment of the present invention, the internal electrodes and the dielectric layers are cut and formed simultaneously, and the widths of the internal electrodes and the dielectric layers may be the same, as will be described in more detail below.

[0054] In this embodiment, the width of the dielectric layer is formed to be the same as the width of the internal electrodes, so that ends of the internal electrodes 121 and 122 can be exposed on the first and second surfaces of the ceramic body 110 in the width direction.

[0055] A first side margin portion 112 and a second side margin portion 113 may be formed on both widthwise sides of the ceramic body 110 where the ends of the internal electrodes 121 and 122 are exposed.

[0056] The thickness of the first side margin portion 112 and the second side margin portion 113 may be 10 μm or less. As the thickness of the first side margin portion 112 and the second side margin portion 113 is smaller, the overlapping area of ​​the internal electrodes formed in the ceramic body may become relatively larger.

[0057] The thickness of the first side margin portion 112 and the second side margin portion 113 is not particularly limited as long as it is a thickness that can prevent short-circuiting of the internal electrodes exposed on the side surface of the ceramic body 110, and may be, for example, 2 μm or more.

[0058] If the thickness of the first and second side margin portions is less than 2 μm, the mechanical strength against external impact may be reduced, and if the thickness of the first and second side margin portions is more than 10 μm, the overlapping area of ​​the internal electrodes may be relatively reduced, making it difficult to ensure high capacitance of the multilayer ceramic capacitor.

[0059] To maximize the capacitance of multilayer ceramic capacitors, methods such as thinning the dielectric layers, increasing the number of layers of thinned dielectric layers, and improving the coverage of the internal electrodes have been considered.

[0060] Also, a method has been considered for increasing the overlapping area of ​​the internal electrodes that form the capacitance.

[0061] In order to increase the overlapping area of ​​the internal electrodes, it is necessary to minimize the marginal area where no internal electrodes are formed.

[0062] In particular, as multilayer ceramic capacitors become smaller, the area of ​​the margins needs to be minimized in order to increase the overlapping area of ​​the internal electrodes.

[0063] According to this embodiment, the internal electrodes are formed across the entire width of the dielectric layer, and the thickness of the side margins is set to 10 μm or less, so that the overlapping area of ​​the internal electrodes is large.

[0064] Generally, the higher the dielectric layer density, the thinner the dielectric layers and internal electrodes become. Therefore, short circuits between the internal electrodes can occur frequently. Furthermore, if the internal electrodes are formed only on a portion of the dielectric layers, a step is generated by the internal electrodes, which can reduce the accelerated life and reliability of the insulation resistance.

[0065] However, according to the present embodiment, even if thin-film internal electrodes and dielectric layers are formed, the internal electrodes are formed across the entire width of the dielectric layers, so that the overlapping area of ​​the internal electrodes is increased, thereby increasing the capacitance of the multilayer ceramic capacitor.

[0066] Furthermore, by reducing the steps due to the internal electrodes, the accelerated life of the insulation resistance is improved, thereby providing a multilayer ceramic capacitor with excellent capacitance characteristics and reliability.

[0067] According to one embodiment of the present invention, the first and second side margin portions 112, 113 are divided into first regions 112a, 113a adjacent to the outer surfaces of the side margin portions 112, 113 and second regions 112b, 113b adjacent to the internal electrodes 121, 122 exposed to the first surface 1 and the second surface 2 of the ceramic body 110, and the magnesium (Mg) content in the second regions 112b, 113b is higher than the magnesium (Mg) content in the first regions 112a, 113a.

[0068] The first and second side margin portions 112 and 113 arranged on the sides of the ceramic body 110 are divided into two regions having different compositions. In this case, the magnesium (Mg) content in the second regions 112b and 113b is adjusted to be higher than the magnesium (Mg) content in the first regions 112a and 113a, thereby increasing the breakdown voltage (BDV) and improving reliability.

[0069] Specifically, the length of the oxide layer at the tip of the internal electrode exposed on the side surface in the width direction of the ceramic body can be controlled by adjusting the magnesium (Mg) content in the second regions 112b and 113b of the side margin portion adjacent to the internal electrodes 121 and 122 exposed on the first surface 1 and the second surface 2 of the ceramic body 110. This can increase the breakdown voltage (BDV) and improve the moisture resistance reliability.

[0070] Generally, during the process of forming the side margin, many voids are generated at the interface where the ceramic body and the side margin contact each other, which can reduce reliability.

[0071] In addition, voids formed at the interface where the ceramic body and side margins come into contact cause electric field concentration, which results in a problem of a lower breakdown voltage (BDV).

[0072] Furthermore, the voids may cause a decrease in the sintered density of the outer surface, resulting in a decrease in the reliability of moisture resistance.

[0073] According to one embodiment of the present invention, by adjusting the magnesium (Mg) content in the second regions 112b, 113b of the side margin portion adjacent to the internal electrodes 121, 122 exposed on the first surface 1 and the second surface 2 of the ceramic body 110, an oxide layer can be formed in the voids generated at the interface where the ceramic body and the side margin portion come into contact.

[0074] As mentioned above, when an oxide layer is formed in the voids generated at the interface where the ceramic body and side margins come into contact, insulation is ensured and the concentration of electric fields can be alleviated, thereby increasing the breakdown voltage (BDV) and reducing short circuits.

[0075] In addition, the first and second side margin portions 112, 113 arranged on the sides of the ceramic body 110 are divided into two regions having different compositions, and in this case, the magnesium (Mg) content contained in each region is made different, thereby increasing the density of the first and second side margin portions 112, 113 and improving moisture resistance characteristics.

[0076] Specifically, by adjusting the magnesium (Mg) content in the second regions 112b, 113b of the first and second side margin portions 112, 113 to be greater than the magnesium (Mg) content in the outer first regions 112a, 113a, the density of the first regions 112a, 113a of the side margin portions 112, 113 can be improved, thereby improving the moisture resistance characteristics.

[0077] In particular, by reducing the magnesium (Mg) content in the first regions 112a, 113a of the first and second side margin portions 112, 113 adjacent to the outer surfaces of the side margin portions 112, 113, the adhesion strength between the first external electrode 131 and the second external electrode 132 can be improved.

[0078] The magnesium (Mg) content in the second regions 112b and 113b can be adjusted to be greater than the magnesium (Mg) content in the first regions 112a and 113a by varying the composition of the dielectric material for forming the ceramic body and the composition of the dielectric material for forming the first and second side margin portions during the manufacturing process of the multilayer ceramic capacitor.

[0079] That is, when the magnesium (Mg) content in the composition of the dielectric for forming the first and second side margin portions is increased, different from the composition of the dielectric for forming the ceramic body, and the magnesium (Mg) content is adjusted by diffusion during the sintering and firing process, the magnesium (Mg) content in the second regions 112b and 113b can be adjusted to be higher than the magnesium (Mg) content in the first regions 112a and 113a.

[0080] This can reduce the electric field concentrated at the tip of the internal electrode, preventing dielectric breakdown, which is one of the main defects of the multilayer ceramic capacitor, and improving the reliability of the multilayer ceramic capacitor.

[0081] According to an embodiment of the present invention, the magnesium (Mg) content of the second regions 112b and 113b is set to be equal to or greater than the titanium (Ti) content of the first and second side margin portions. 100 moles The amount of the hydroxybenzoate may be 10 moles or more and 30 moles or less relative to the hydroxybenzoate.

[0082] The magnesium (Mg) content of the second regions 112b and 113b is 100 molesBy adjusting the mole ratio to be 10 moles or more and 30 moles or less with respect to the total mole ratio, it is possible to increase the breakdown voltage (BDV) and improve the moisture resistance reliability.

[0083] The magnesium (Mg) content of the second regions 112b and 113b is 100 moles If the content is less than 10 moles, an oxide layer is not sufficiently formed in the voids generated at the interface where the ceramic body and the side margin contact, which may result in a lower breakdown voltage (BDV) and an increase in short circuit defects.

[0084] Meanwhile, the content of magnesium (Mg) in the second regions 112b and 113b is smaller than that of titanium (Ti) contained in the first and second side margin portions. 100 moles If the amount exceeds 30 moles, the sinterability may be reduced, resulting in problems such as non-uniform distribution of reliability and breakdown voltage (BDV).

[0085] According to one embodiment of the present invention, the dielectric layer 111 has a thickness of 0.4 μm or less, and the internal electrodes 121 and 122 have a thickness of 0.4 μm or less, thereby providing an ultra-small multilayer ceramic capacitor.

[0086] When a thin dielectric layer and an internal electrode are applied, with the dielectric layer 111 having a thickness of 0.4 μm or less and the internal electrodes 121 and 122 having a thickness of 0.4 μm or less, as in one embodiment of the present invention, the reliability problem caused by voids occurring at the boundary between the ceramic body and the side margin portion is a very important issue.

[0087] That is, in the case of the conventional multilayer ceramic capacitor, there was no significant problem in reliability even if the magnesium (Mg) content of each region of the side margin portion included in the multilayer ceramic capacitor was not adjusted as in the embodiment of the present invention.

[0088] However, in products in which thin-film dielectric layers and internal electrodes are applied, such as in one embodiment of the present invention, the magnesium (Mg) content in each region of the side margin must be adjusted to prevent BDV and reduced reliability due to voids generated at the interface where the ceramic body and the side margin contact.

[0089] That is, in one embodiment of the present invention, the content of magnesium (Mg) in the second regions 112b and 113b is less than the content of titanium (Ti) in the first and second side margin portions. 100 moles By adjusting the ratio of the SiO2 to be 10 moles or more and 30 moles or less, the breakdown voltage (BDV) can be increased and the moisture resistance reliability can be improved even when the thickness of the dielectric layer 111 and the first and second internal electrodes 121, 122 is a thin film of 0.4 μm or less.

[0090] However, the above thin film does not mean that the thickness of the dielectric layer 111 and the first and second internal electrodes 121, 122 is 0.4 μm or less, but can be understood as the concept of including a dielectric layer and internal electrodes that are thinner than conventional products.

[0091] Meanwhile, the width of the first regions 112a and 113a may be 12 μm or less, and the width of the second regions 112b and 113b may be 3 μm or less, but is not necessarily limited thereto.

[0092] Referring to Figure 4, the ratio of the thickness tc1 of the first or second side margin region contacting the end of the centrally located internal electrode among the plurality of internal electrodes 121, 122 to the thickness tc2 of the first or second side margin region contacting the end of the outermost internal electrode may be 1.0 or less.

[0093] There is no particular lower limit to the ratio of the thickness tc2 of the first or second side margin region that contacts the end of the internal electrode that is located at the outermost side to the thickness tc1 of the first or second side margin region that contacts the end of the internal electrode that is located in the central portion, but it is preferable that it be 0.9 or more.

[0094] According to one embodiment of the present invention, unlike conventional techniques, the first or second side margin portion is formed by attaching a ceramic green sheet to the side of the ceramic body, so that the thickness of each position of the first or second side margin portion is uniform.

[0095] That is, conventionally, the side margins have been formed by coating or printing ceramic slurry, which has resulted in significant variations in thickness from position to position in the side margins.

[0096] Specifically, conventionally, the thickness of the first or second side margin region that contacts the end of the internal electrode arranged in the center of the ceramic body has been made thicker than the thickness of other regions.

[0097] For example, in the past, the ratio of the thickness of the first or second side margin region that contacts the end of the internal electrode located at the outermost position to the thickness of the first or second side margin region that contacts the end of the internal electrode located in the central portion was less than 0.9, resulting in a large variation.

[0098] In the conventional case where the thickness of the side margin portion varies greatly depending on the position, the side margin portion occupies a large portion of a multilayer ceramic capacitor of the same size, making it impossible to ensure a large size for the capacitance forming portion, and making it difficult to ensure high capacitance.

[0099] In contrast, in one embodiment of the present invention, the average thickness of the first and second side margin portions 112, 113 is 2 μm or more and 10 μm or less, and the ratio of the thickness tc2 of the first or second side margin portion region that contacts the end of the internal electrode located at the outermost position to the thickness tc1 of the first or second side margin portion region that contacts the end of the internal electrode located in the center of the plurality of internal electrodes 121, 122 is 0.9 or more and 1.0 or less, so that the thickness of the side margin portion is thin and there is little variation in thickness, and therefore a large size can be ensured for the capacitance forming portion.

[0100] This makes it possible to realize a high-capacity multilayer ceramic capacitor.

[0101] Meanwhile, referring to FIG. 4, the ratio of the thickness tc1 of the first or second side margin region contacting the end of the centrally located internal electrode among the plurality of internal electrodes 121, 122 to the thickness tc3 of the first or second side margin region contacting the corner of the ceramic body 110 may be 1.0 or less.

[0102] It is preferable that the lower limit of the ratio of the thickness tc3 of the first or second side margin region that contacts the corner of the ceramic body 110 to the thickness tc1 of the first or second side margin region that contacts the end of the internal electrode arranged in the central portion is 0.9 or more.

[0103] Due to the above-mentioned characteristics, there is little variation in thickness between regions of the side margin portion, so that the size of the capacitance forming portion can be secured to be large, thereby making it possible to realize a multilayer ceramic capacitor with a high capacitance.

[0104] 5a to 5f are cross-sectional and perspective views schematically illustrating a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention.

[0105] According to another embodiment of the present invention, a method for manufacturing a ceramic green sheet includes the steps of: preparing a first ceramic green sheet on which a plurality of first internal electrode patterns are formed at predetermined intervals and a second ceramic green sheet on which a plurality of second internal electrode patterns are formed at predetermined intervals; laminating the first ceramic green sheet and the second ceramic green sheet so that the first internal electrode patterns and the second internal electrode patterns intersect with each other to form a ceramic green sheet laminate body; cutting the ceramic green sheet laminate body so that ends of the first internal electrode patterns and the second internal electrode patterns have side surfaces exposed in a width direction; The present invention provides a method for manufacturing a multilayer ceramic capacitor, the method including: forming first and second side margin portions on side surfaces where ends of the first and second internal electrode patterns are exposed; and manufacturing a ceramic body including dielectric layers and first and second internal electrodes by firing the cut multilayer body, wherein the first and second side margin portions are divided into a first region adjacent to outer surfaces of the side margin portions and a second region adjacent to the first and second internal electrodes, and the second region has a higher magnesium (Mg) content than the first region.

[0106] Hereinafter, a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention will be described.

[0107] 5a, a plurality of stripe-shaped first internal electrode patterns 221 are formed at predetermined intervals on a ceramic green sheet 211. The plurality of stripe-shaped first internal electrode patterns 221 may be formed parallel to each other.

[0108] The ceramic green sheet 211 may be formed of a ceramic paste containing ceramic powder, an organic solvent, and an organic binder.

[0109] The ceramic powder is a material having a high dielectric constant, and may be, but is not limited to, a barium titanate (BaTiO3)-based material, a lead complex perovskite-based material, or a strontium titanate (SrTiO3)-based material, and is preferably barium titanate (BaTiO3) powder. When the ceramic green sheet 211 is fired, it becomes the dielectric layer 111 that constitutes the ceramic body 110.

[0110] The stripe-shaped first internal electrode pattern 221 may be formed by an internal electrode paste containing a conductive metal, such as, but not limited to, nickel (Ni), copper (Cu), palladium (Pd), or an alloy thereof.

[0111] The method for forming the stripe-shaped first internal electrode pattern 221 on the ceramic green sheet 211 is not particularly limited, but may be formed by a printing method such as screen printing or gravure printing.

[0112] Although not shown, a plurality of stripe-shaped second internal electrode patterns 222 may be formed on another ceramic green sheet 211 at predetermined intervals.

[0113] Hereinafter, the ceramic green sheet on which the first internal electrode pattern 221 is formed will be referred to as a first ceramic green sheet, and the ceramic green sheet on which the second internal electrode pattern 222 is formed will be referred to as a second ceramic green sheet.

[0114] Next, as shown in FIG. 5b, the first and second ceramic green sheets may be alternately laminated so that the stripe-shaped first internal electrode patterns 221 and the stripe-shaped second internal electrode patterns 222 are cross-laminated.

[0115] Thereafter, the first internal electrode 121 can be formed by the stripe-shaped first internal electrode pattern 221, and the second internal electrode 122 can be formed by the stripe-shaped second internal electrode pattern 222.

[0116] According to another embodiment of the present invention, the thickness td of the first and second ceramic green sheets is 0.6 μm or less, and the thickness te of the first and second internal electrode patterns is 0.5 μm or less.

[0117] The present invention is characterized by an ultra-small, high-capacity multilayer ceramic capacitor having a dielectric layer thickness of 0.4 μm or less and an internal electrode thickness of 0.4 μm or less, wherein the thickness td of the first and second ceramic green sheets is 0.6 μm or less, and the thickness te of the first and second internal electrode patterns is 0.5 μm or less.

[0118] Figure 5c is a cross-sectional view showing a ceramic green sheet laminated body 220 in which first and second ceramic green sheets are laminated according to one embodiment of the present invention, and Figure 5d is a perspective view showing a ceramic green sheet laminated body 220 in which first and second ceramic green sheets are laminated.

[0119] Referring to Figures 5c and 5d, first ceramic green sheets on which a plurality of parallel stripe-shaped first internal electrode patterns 221 are printed and second ceramic green sheets on which a plurality of parallel stripe-shaped second internal electrode patterns 222 are printed are alternately stacked with each other.

[0120] More specifically, the first ceramic green sheet may be laminated so that the center of the stripe-shaped first internal electrode pattern 221 printed on the first ceramic green sheet overlaps with the spacing between the stripe-shaped second internal electrode patterns 222 printed on the second ceramic green sheet.

[0121] 5d, the ceramic green sheet laminated body 220 may be cut across the plurality of stripe-shaped first internal electrode patterns 221 and the plurality of stripe-shaped second internal electrode patterns 222. That is, the ceramic green sheet laminated body 220 may be cut into laminated bodies 210 along cutting lines C1-C1 and C2-C2 that are perpendicular to each other.

[0122] More specifically, the stripe-shaped first internal electrode pattern 221 and the stripe-shaped second internal electrode pattern 222 can be divided into a plurality of internal electrodes having a certain width by cutting them lengthwise. At this time, the laminated ceramic green sheets are also cut together with the internal electrode patterns. As a result, the dielectric layer can be formed to have the same width as the width of the internal electrodes.

[0123] Furthermore, it is possible to cut along the cutting line C2-C2 to match the size of each individual ceramic body. That is, before forming the first side margin portion and the second side margin portion, the rod-shaped laminate body is cut along the cutting line C2-C2 to match the size of each individual ceramic body, thereby forming a plurality of laminate bodies 210.

[0124] That is, the rod-shaped laminate can be cut along cutting lines that are formed between the centers of the overlapping first internal electrodes and the overlapping second internal electrodes and have the same predetermined interval, so that one ends of the first internal electrodes and the second internal electrodes can be alternately exposed on the cut surface.

[0125] Thereafter, a first side margin portion and a second side margin portion may be formed on the first and second side surfaces of the laminated body 210 .

[0126] Next, as shown in FIG. 5e, a first side margin portion 212 and a second side margin portion (not shown) can be formed on the first and second side surfaces of the laminated body 210, respectively.

[0127] Specifically, the first side margin portion 212 is formed by placing the ceramic green sheet 212 for the side surface on top of a punched elastic material 300 made of rubber.

[0128] Next, the multilayer body 210 is rotated by 90 degrees so that the first side surface of the multilayer body 210 faces the side surface ceramic green sheet 212, and then the multilayer body 210 is pressed and adhered to the side surface ceramic green sheet 212.

[0129] When the laminated body 210 is pressed against the side ceramic green sheet 212 to transfer the side ceramic green sheet 212 to the laminated body 210, the rubber punching elastic material 300 allows the side ceramic green sheet 212 to be formed up to the corners of the side of the laminated body 210, and the remaining portion can be cut off.

[0130] FIG. 5F shows that the ceramic green sheets 212 for side surfaces are formed up to the corners of the side surfaces of the laminated body 210.

[0131] Thereafter, the laminated body 210 can be rotated to form a second side margin portion on the second side surface of the laminated body 210 .

[0132] Next, the multilayer body 210 having the first and second side margin portions formed on both sides thereof may be calcined and fired to form a ceramic body including the dielectric layers and the first and second internal electrodes.

[0133] Thereafter, external electrodes may be formed on a third side surface of the ceramic body where the first internal electrode is exposed and a fourth side surface of the ceramic body where the second internal electrode is exposed.

[0134] According to another embodiment of the present invention, the ceramic green sheets for side surfaces are thin and have little variation in thickness, so that the size of the capacitance forming portion can be secured to be large.

[0135] Specifically, the average thickness of the first and second side margin portions 112, 113 after firing is 2 μm or more and 10 μm or less, and there is little variation in thickness from position to position, so that the size of the capacitance forming portion can be secured to be large.

[0136] This makes it possible to realize a high-capacity multilayer ceramic capacitor.

[0137] Other features that are the same as those in the embodiment of the present invention described above will not be described here to avoid redundancy.

[0138] The present invention will be described in more detail below by way of experimental examples. However, these examples are merely for the purpose of concretely understanding the invention, and the scope of the present invention is not limited to these experimental examples.

[0139] [Experimental Example] According to one embodiment of the present invention, a comparative example in which a conventional side margin portion is formed and an example in which a side margin portion including first and second regions with different magnesium (Mg) contents is formed were prepared.

[0140] Then, a ceramic green sheet laminate body was formed so that the internal electrodes were exposed in the width direction and side ceramic green sheets could be attached to the electrode exposed portions of the green chip without margins to form side margin portions, as in the above comparative example and example.

[0141] While applying a constant temperature and pressure under conditions that minimized deformation of the chip, ceramic green sheets for forming the side surfaces were attached to both sides of the ceramic green sheet laminate body, and a multilayer ceramic capacitor green chip with 0603 size (width x length x height: 0.6mm x 0.3mm x 0.3mm) was produced.

[0142] The multilayer ceramic capacitor test pieces thus fabricated were calcined in a nitrogen atmosphere at 400°C or less, and then sintered at a firing temperature of 1200°C or less and with a hydrogen concentration of 0.5% H2 or less. Electrical properties such as appearance defects, insulation resistance, and moisture resistance were then comprehensively checked.

[0143] FIG. 6 is a graph comparing breakdown voltages (BDV) between the examples of the present invention and the comparative examples.

[0144] In FIG. 6, Comparative Example 1 is a conventional multilayer ceramic capacitor structure in which there is no difference in the magnesium (Mg) content contained in the side margin portions, Examples 1 and 2 are cases in which the magnesium (Mg) content contained in the second regions 112b and 113b of the first and second side margin portions 112 and 113 adjacent to the first and second internal electrodes 121 and 122 is 10 moles and 30 moles, respectively, and Comparative Example 2 is a case in which the magnesium (Mg) content contained in the second regions 112b and 113b of the first and second side margin portions 112 and 113 adjacent to the first and second internal electrodes 121 and 122 is 50 moles.

[0145] It can be seen that in Examples 1 and 2, the breakdown voltage (BDV) is increased compared to Comparative Example 1, which is a conventional multilayer ceramic capacitor.

[0146] In the case of Comparative Example 2, although the breakdown voltage (BDV) increases, the distribution is uneven, and the distribution of the moisture resistance reliability is also uneven. Therefore, in the present invention, it is preferable that the magnesium (Mg) content contained in the second regions 112b, 113b of the first and second side margin portions 112, 113 is 30 moles or less.

[0147] Although the embodiments of the present invention have been described in detail above, it will be apparent to those skilled in the art that the scope of the present invention is not limited thereto, and that various modifications and variations are possible within the scope of the technical idea of ​​the present invention described in the claims. [Explanation of symbols]

[0148] 110 Ceramic body 111 Dielectric layer 112 First side margin 113 Second side margin 121 1st internal electrode 122 2nd internal electrode 131 1st external electrode 132 2nd external electrode

Claims

1. a ceramic body including a dielectric layer, the ceramic body having first and second surfaces facing each other, third and fourth surfaces connecting the first and second surfaces, and fifth and sixth surfaces connected to the first to fourth surfaces and facing each other; a plurality of internal electrodes disposed inside the ceramic body, exposed to the first and second surfaces, and having one end exposed to the third or fourth surface; a first side margin portion and a second side margin portion disposed on ends of the internal electrodes exposed on the first surface and the second surface, the first side margin portion and the second side margin portion are divided into a first region adjacent to an outer surface of the side margin portion and a second region adjacent to the internal electrodes exposed to the first surface and the second surface, the first region contains magnesium (Mg), and a content of magnesium (Mg) contained in the second region is greater than a content of magnesium (Mg) contained in the first region; The multilayer ceramic capacitor, wherein the content of magnesium (Mg) in the second region is 10 moles or more and 30 moles or less with respect to 100 moles of titanium (Ti) contained in the first side margin portion and the second side margin portion.

2. 2. The multilayer ceramic capacitor according to claim 1, wherein a ratio of a thickness of the first side margin region or the second side margin region that contacts an end of an internal electrode that is arranged at the outermost side to a thickness of the first side margin region or the second side margin region that contacts an end of an internal electrode that is arranged at a center among the plurality of internal electrodes is 0.9 or more and 1.0 or less.

3. 3. The multilayer ceramic capacitor according to claim 1, wherein a ratio of a thickness of the first side margin region or the second side margin region that contacts an end of an internal electrode arranged in a central portion among the plurality of internal electrodes to a thickness of the first side margin region or the second side margin region that contacts a corner of the ceramic body is 0.9 or more and 1.0 or less.

4. 4. The multilayer ceramic capacitor according to claim 1, wherein the thickness of the dielectric layers is 0.4 μm or less, and the thickness of the internal electrodes is 0.4 μm or less.

5. 5. The multilayer ceramic capacitor according to claim 1, wherein the first side margin portion and the second side margin portion have an average thickness of 2 [mu]m or more and 10 [mu]m or less.

6. 6. The multilayer ceramic capacitor according to claim 1, wherein the width of the first region is 12 μm or less, and the width of the second region is 3 μm or less.

7. A multilayer ceramic capacitor described in any one of claims 1 to 6, wherein the first side margin portion and the second side margin portion are each formed using one ceramic green sheet.

8. manufacturing a first ceramic green sheet having a plurality of first internal electrode patterns formed at predetermined intervals and a second ceramic green sheet having a plurality of second internal electrode patterns formed at predetermined intervals; forming a ceramic green sheet laminate body by stacking the first ceramic green sheet and the second ceramic green sheet such that the first internal electrode pattern and the second internal electrode pattern cross each other; cutting the ceramic green sheet laminate body so that ends of the first internal electrode pattern and the second internal electrode pattern have exposed side surfaces in a width direction; forming a first side margin portion and a second side margin portion on the side surfaces where the ends of the first internal electrode pattern and the second internal electrode pattern are exposed; and firing the cut multilayer body to manufacture a ceramic body including dielectric layers and first and second internal electrodes, the first side margin portion and the second side margin portion are divided into a first region adjacent to an outer surface of the side margin portion and a second region adjacent to the first and second internal electrodes within the layer, the first region contains magnesium (Mg), and a content of magnesium (Mg) contained in the second region is greater than a content of magnesium (Mg) contained in the first region; a content of magnesium (Mg) in the second region is 10 moles or more and 30 moles or less relative to 100 moles of titanium (Ti) contained in the first side margin portion and the second side margin portion.

9. 9. The method for manufacturing a multilayer ceramic capacitor according to claim 8, wherein the first and second ceramic green sheets have a thickness of 0.6 μm or less, and the first and second internal electrode patterns have a thickness of 0.5 μm or less.

10. 9. The method for manufacturing a multilayer ceramic capacitor according to claim 8, wherein a ratio of a thickness of the first side margin portion or the second side margin portion region contacting an end of an internal electrode arranged at the outermost side to a thickness of the first side margin portion or the second side margin portion region contacting an end of an internal electrode arranged at a center of the first and second internal electrodes is 0.9 or more and 1.0 or less.

11. 9. The method for manufacturing a multilayer ceramic capacitor according to claim 8, wherein the ratio of the thickness of the first side margin portion or the second side margin portion region contacting the end of the internal electrode arranged in the center of the first and second internal electrodes to the thickness of the first side margin portion or the second side margin portion region contacting the corner of the ceramic green sheet laminate body is 0.9 or more and 1.0 or less.

12. The method for manufacturing a multilayer ceramic capacitor according to claim 8 , wherein the first side margin portion and the second side margin portion have an average thickness of 2 μm to 10 μm.

13. The method for manufacturing a multilayer ceramic capacitor according to claim 11, wherein the width of the first region is 12 μm or less, and the width of the second region is 3 μm or less.

14. 4. The multilayer ceramic capacitor according to claim 1, wherein the internal electrodes have a thickness of 0.4 [mu]m or less.

15. 4. The multilayer ceramic capacitor according to claim 1, wherein the dielectric layer has a thickness of 0.4 [mu]m or less.

16. A method for manufacturing a multilayer ceramic capacitor as described in Claim 8, wherein the step of forming the first side margin portion and the second side margin portion is a step of forming the first side margin portion and the second side margin portion using one ceramic green sheet each.

Citation Information

Patent Citations

  • Method for manufacturing laminated ceramic electronic part

    JP2008153309A

  • Multi-layered ceramic electronic component

    JP2009016796A

  • Multilayer ceramic capacitor and manufacturing method therefor

    JP2014068000A

  • Multilayer ceramic electronic component

    JP2014096551A

  • Multilayer ceramic capacitor and method of manufacturing the same

    JP2014204114A