Bulky nonwoven fabric with improved compressibility and recovery

A non-crimpable cross-section design in bicomponent fibers for nonwoven fabrics addresses the limitations of crimped fibers by enabling high bulkiness and recovery, improving compressibility and resilience for absorbent sanitary products.

JP7582943B2Active Publication Date: 2024-11-13REIFENHAUSER GMBH & CO MASCHFAB +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021529117
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-11-23
Filing Date
2019-11-22
Publication Date
2024-11-13
Estimated Expiration
2039-11-22

AI Technical Summary

Technical Problem

Existing nonwoven fabrics made from crimped or curled fibers with asymmetric cross-sections face limitations in achieving high bulkiness and recovery properties, particularly in applications requiring compressibility and resilience, such as absorbent sanitary products, due to the uniform crimping and regular contraction forces that restrict their ability to form irregular shapes.

Method used

A nonwoven fabric composed of endless filaments with a non-crimpable cross-section, utilizing bicomponent fibers where the second polymeric material extends longitudinally and forms the surface, allowing for irregular contraction forces that create a bulky, resilient structure with enhanced compressibility and recovery properties.

Benefits of technology

The non-crimpable cross-section design results in a fabric that can be compressed at low pressures and fully recovers upon release, offering improved structural softness, elasticity, and void volume, enhancing the performance of absorbent sanitary products by improving fluid management and user comfort.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582943000013
    Figure 0007582943000013
  • Figure 0007582943000014
    Figure 0007582943000014
  • Figure 0007582943000015
    Figure 0007582943000015
Patent Text Reader

Abstract

A nonwoven fabric and a method for making the nonwoven fabric are disclosed, comprising at least one layer comprising endless filaments, the nonwoven fabric comprising: - consisting of at least a first polymeric material (A) and a second polymeric material (B) having a lower melting point than the first polymeric material A, - said second polymeric material (B) extends in the longitudinal direction of said filaments and forms at least a part of the surface of said filaments; - said at least one layer of said endless filaments comprises interfilament bonds formed from a second polymeric material (B), all components of said filaments being arranged in a non-crimped configuration across the cross section of the filaments, and said nonwoven fabric has a structural softness of at least 80 (mm 4 mm 2 g -2 )
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a high-loft spunmelt-type nonwoven fabric having enhanced compressibility and recovery properties, comprising multicomponent fibers having a non-crimped cross-section. More specifically, the present invention relates to a nonwoven fabric comprising at least one layer comprising endless filaments, the nonwoven fabric comprising: - consisting of at least a first polymeric material and a second polymeric material having a lower melting point than the first polymeric material A, - the second polymeric material extends longitudinally of the filament and forms at least a portion of the surface of the filament; - at least one layer of said endless filaments comprises interfilament bonds formed from a second polymeric material.The present invention also relates to a method for producing such a nonwoven fabric. [Background technology]

[0002] Those skilled in the art understand the benefits of multicomponent crimped or curled fibers, for example, with asymmetric (crimped) cross-sections. It is well known in the industry that when certain combinations of polymers are arranged in a fiber with a suitable configuration, known as a crimped cross-section, the fiber will either crimp immediately after spinning—self-crimping—or have a certain level of potential crimp that can be induced by activation, e.g., heat activation. It is also well known that certain polymer composition combinations offer excellent softness and flexibility, while certain other polymer combinations are even more suitable for good recovery. For example, patent WO2018059610, filed September 3, 2016, describes the use of PET / PE compositions in an eccentric core / sheath configuration to create a bulky layer with a good combination of compressibility and recovery.

[0003] Those skilled in the art also recognize that, for certain applications, similar materials can be produced using advanced carding techniques. Carding is a well-known process consisting of several manufacturing steps in which fibers are first produced, then cut into short (staple) fibers, optionally processed and aligned to form fibrous layers, and then bonded. Spunmelt processing, on the other hand, is a line process in which the final nonwoven fabric is formed from endless filaments in a single step. Carded materials are produced from staple fibers, and the large number of ends of these fibers arranged in the warp and weft directions of the nonwoven layer may be undesirable for certain applications. Summary of the Invention

[0004] The object of the present invention is to achieve a high-loft nonwoven fabric that can be compressed at a relatively low pressure and can recover when the pressure is released.

[0005] These and several other drawbacks of the prior art are overcome by a nonwoven fabric comprising at least one layer containing endless filaments, said nonwoven fabric comprising: - consisting of at least a first polymeric material and a second polymeric material having a lower melting point than said first polymeric material, - the second polymeric material extends longitudinally of the filament and forms at least a portion of the surface of the filament; - the at least one layer of the endless filaments comprises interfilament bonds formed from a second polymeric material; all components of said filament are arranged in a non-crimped configuration across the cross section of the filament; The ratio of the length of the filament to the length of the fabric is greater than 1.2:1, and the proportion of fibers is at least 20% or more; The ratio of the length of the filament to the length of the fabric is greater than 1.5:1, and the proportion of fibers is at least 10% or more; At least 10% of the fibers have a ratio of the filament length to the fabric length of less than 2.5:1.

[0006] These drawbacks are also overcome by a nonwoven fabric consisting of at least one layer containing endless filaments, said nonwoven fabric comprising: - consisting of at least a first polymeric material and a second polymeric material having a lower melting point than the first polymeric material, - the second polymeric material extends longitudinally of the filament and forms at least a portion of the surface of the filament; - at least one layer of said endless filaments includes interfilament bonds formed from a second polymeric material; - The structural softness of the nonwoven fabric is 80 (m 4 mm 2 g -2 ) or more, preferably 100 (m 4 mm 2 g -2 ) or more, preferably 110 (m 4 mm 2 g -2 ) or more, more preferably 120 (m 4 mm 2 g -2 ) or more, more preferably 130 (m 4 mm 2 g -2 ) or more, more preferably 140 (m 4 mm 2 g -2 ) or more, most preferably 150 (m 4 mm 2 g -2 ) or more, and is calculated using the following formula: TIFF0007582943000001.tif1999, - Thickness is the thickness of the nonwoven structure in mm, - basis weight is the basis weight of said nonwoven structure in grams per square meter, - the recovery rate is the ratio (Tr) / (Ts), where (Ts) is the initial thickness of the nonwoven structure at a preload of 0.5 kPa and (Tr) is the recovered thickness of the nonwoven structure measured after applying and subsequently releasing a load of 2.5 kPa; - Compression ratio is the difference in mm between the initial thickness of the nonwoven structure and the thickness of the nonwoven structure when subjected to a load of 5 N.

[0007] Preferably, the first polymeric material and / or the second polymeric material consists of or comprises as a major component a polymeric material selected from the group consisting of polyester, polyolefin, polylactic acid, polyester copolymer, polylactic acid copolymer, and mixtures thereof; and the first polymeric material and the second polymeric material are different.

[0008] Also preferably, the filaments have a core / sheath structure, with the first polymer material forming the core and the second polymer material forming the sheath.

[0009] The mass ratio of the first polymer material to the second polymer material is 50:50 to 90:10.

[0010] The basis weight is at least 5 gsm, preferably at least 10 gsm, more preferably at least 20 gsm, more preferably at least 30 gsm, advantageously at least 40 gsm, and preferably at most 200 gsm, preferably at most 150 gsm, preferably at most 100 gsm, most preferably at most 80 gsm.

[0011] Advantageously, the median fiber diameter of said filaments is 5 microns or more; preferably 10 microns or more; preferably 15 microns or more; most preferably 20 microns or more; and 50 microns or less; preferably 40 microns or less; most preferably 35 microns or less.

[0012] Preferably, the void volume of said layer is 65% or more; preferably 75% or more; more preferably 80% or more; more preferably 84% or more; more preferably 86% or more; more preferably 88% or more; most preferably 90% or more.

[0013] The above-mentioned drawbacks of the prior art are overcome by a method for producing nonwoven fabrics, which method comprises: 1. A method comprising the steps of: a) melting and feeding at least a first polymeric material and a second polymeric material having a lower melting point than the first polymeric material into a nozzle of a spinning beam configured to form an endless filament having all components arranged in a non-crimped configuration across the cross section of the filament, the second polymeric material extending longitudinally of the filament and forming at least a portion of the surface of the filament, and wherein the filament speed is in the range of 3000 to 5500 m / min; b) cooling the formed filaments with a fluid medium at a temperature in the range of 10 to 90°C and drawing the filaments at a drawdown ratio in the range of 200 to 1300 to bring at least the first polymeric material (A) into a metastable crystalline state; c) laying the filaments onto a forming belt to form a nonwoven filamentary batt; d) heating the nonwoven filamentary batt to a temperature in the range of 80-200°C to activate shrinkage of the nonwoven filamentary batt and convert at least the polymeric material (A) to a more stable crystalline state.

[0014] Preferably, after step c) and before step d), the method further comprises a step of pre-compacting the nonwoven filamentary batt, said pre-compacting being carried out by heating the filaments to a temperature in the range of 80 to 180°C, preferably 90 to 150°C, most preferably 110 to 140°C, to partially soften the polymer material (B) and adhere the polymer material (B) between at least some of the filaments that intersect with each other.

[0015] Preferably, in step b), the filaments are cooled and stretched in a first zone using a fluid medium having a temperature in the range of 10 to 90°C, preferably 15 to 80°C, most preferably 15 to 70°C, and then cooled and stretched in a second zone using a fluid medium having a temperature in the range of 10 to 80°C, preferably 15 to 70°C, most preferably 15 to 45°C.

[0016] According to a preferred embodiment, in step d), the nonwoven filamentary batt is heated by exposing the batt to air at a temperature in the range of 80-200°C, preferably 100-160°C, for a time of 20-5000 ms, preferably 30-3000 ms, most preferably 50-1000 ms, the air being moved into and / or along the batt at an initial velocity in the range of 0.1-2.5 m / s, preferably 0.3-1.5 m / s.

[0017] Preferably, in step d), the nonwoven filamentary batt is heated so that it shrinks in the machine direction and the cross direction by not more than 20%, preferably not more than 15%, more preferably not more than 13%, more preferably not more than 11%, and most preferably not more than 9%, and its thickness increases by not less than 20%, preferably not less than 40%, more preferably not more than 60%, and most preferably not less than 100%.

[0018] In step d), the nonwoven filamentary batt may be heated to soften the polymeric material and bond it between at least some of the intersecting filaments. Alternatively, after step d), the nonwoven filamentary batt is heated to soften the polymeric material and bond it between the intersecting filaments. The heating after step d) of bonding the polymeric material (B) is carried out using an omega drum bonding device, or a flat belt bonding device, or a multi-drum bonding means, and / or by moving air through and / or along the nonwoven filamentary batt for 200 to 20,000 ms, preferably 200 to 15,000 ms, and most preferably 200 to 10,000 ms, wherein the air temperature is in the range of 100°C to 250°C, preferably 120°C to 220°C, and the initial velocity is 0.2 to 4.0 m / s, preferably 0.4 to 1.8 m / s.

[0019] Preferably, the first polymeric material and / or the second polymeric material consists of or comprises as a major component a polymeric material selected from the group consisting of polyester, polyolefin, polylactic acid, polyester copolymer, polylactic acid copolymer and mixtures thereof; the first polymeric material and the second polymeric material are different.

[0020] When carrying out the method of the present invention, the drawdown ratio is advantageously in the range of 300-800.

[0021] The above-mentioned drawbacks of the prior art are overcome by an absorbent sanitary product comprising a nonwoven fabric as defined above, said nonwoven fabric forming at least one of the top sheet, acquisition and distribution layers, absorbent core, back sheet, and attachment area for mechanical sealing.

[0022] Advantageously, the top sheet and the acquisition and distribution layer are adhered to one another.

[0023] More preferably, the topsheet and acquisition and distribution layer are an integral material.

[0024] More preferably, the pores of said nonwoven fabric are at least partially filled with particles of superabsorbent polymer.

[0025] More preferably, the backsheet and the attachment area are of one piece material.

[0026] definition The term "acquisition / distribution layer" or "ADL" generally refers to a layer of material, typically a nonwoven fabric, in absorbent sanitary products, located between the topsheet and the absorbent core. This layer is designed to rapidly acquire and / or distribute fluid from the topsheet to the core. This layer is also sometimes referred to as a "wicking layer," "surge layer," "supplementary layer," or "distribution layer." Articles are known that have an ADL layer consisting of one sublayer (an adhesive batt). Articles are also known that have two or more sublayers. Ideally, one sublayer primarily serves to rapidly draw fluid away from the topsheet and distribute it throughout the layer toward the core and / or other directions. The other sublayer(s) should reduce the tendency of fluid to move from the core back toward the first sublayer and topsheet, i.e., reduce or prevent rewetting of the topsheet. These sublayers typically do not contain superabsorbent material. Hereinafter, the term "supplementary-distribution layer" ("ADL") will be used to refer to the layer that resides between the top sheet and the absorbent core and provides these acquisition and distribution functions, regardless of the number of fibrous sublayers (batts) that form this layer.

[0027] The term "batt" refers to material in the form of filaments as it appears prior to bonding, a process that can be carried out in various ways, such as through-air bonding or calendering. The "batt" is made up of individual filaments, between which the bond between each other is usually not yet fixed, even if the filaments have been pre-bonded / pre-consolidated in a specific way. Here, this pre-consolidation occurs during or immediately after the laying of the filaments in the spunlay process. However, this pre-consolidation still allows a significant number of filaments to move freely and rearrange. The "batt" may also consist of several layers formed by the accumulation of filaments from several spinning beams in the spunlay process.

[0028] The term "filament" refers primarily to endless fibers, while the term "staple fibers" refers to fibers that have been cut to a predetermined length.

[0029] The term "interfilament bond" refers to a bond that connects two filaments, usually in an area where the filaments cross each other or locally approach or abut each other. The bond may connect more than two filaments or connect two portions of the same filament.

[0030] The term "monocomponent filament" refers to a filament formed from a single polymer or polymer blend, as distinguished from bicomponent or multicomponent filaments.

[0031] "Multicomponent fiber or filament" refers to a fiber or filament having a cross-section composed of multiple discrete segments, each of which is composed of a different polymer component or a different mixture of polymer components, or a polymer component or a mixture of polymer components. The term "multicomponent fiber / filament" includes, but is not limited to, "bicomponent fiber / filament." The different components of a multicomponent fiber are arranged in more or less distinct regions across the cross-section of the fiber and extend continuously along the length of the fiber. The overall cross-section of a multicomponent fiber may be divided into subsections of the different components in any shape or arrangement, such as coaxial subsections, core-sheath subsections, side-by-side subsections, radial subsections, or sea-islands subsections. The cross-section of a bicomponent filament having a "core-sheath structure" is composed of two discrete segments, each composed of a polymer or polymer mixture, with the sheath polymer or polymer mixture component surrounding the core polymer or polymer mixture component.

[0032] The unit of "fiber diameter" is expressed in μm. The terms "grams of fiber per 9000 m (denier or den)" or "grams of fiber per 10000 m" (dTex) are used to describe the fineness or coarseness of the fibers, which is related to their diameter (assuming they are circular) by the density of the material(s) employed.

[0033] "Film" means a skin-like or membrane-like layer of material formed from one or more polymers, not consisting primarily of a fabric-like structure of consolidated polymeric fibers and / or other fibers.

[0034] "MACHINE DIRECTION" (MD) - In the context of nonwoven textile manufacturing and nonwoven textile materials, machine direction (MD) refers to the direction along the textile material that is generally parallel to the direction of advancement of the textile material through the manufacturing line that produces the textile material.

[0035] "Cross Direction" (CD) - With respect to the manufacture of nonwoven textile materials and nonwoven textile materials, cross direction (CD) means the direction along the textile material that is generally perpendicular to the direction of advancement of the textile material through the manufacturing line that produces the textile material.

[0036] "Nonwoven" or "nonwoven fabric" or "nonwoven fabric" means a manufactured sheet or fabric of directionally or randomly oriented fibers that are first formed into a batt and then consolidated by friction, bundling, or adhesion, and bonded thermally (e.g., air-through bonding, calendar bonding, ultrasonic bonding, etc.), chemically (e.g., by use of adhesives), mechanically (e.g., hydroentanglement, etc.), or a combination thereof. The term does not include fabrics woven, knitted, or sewn from yarns or filaments. Fibers may be of natural or synthetic origin, may be staple or continuous filaments, and may be formed in situ. Commercially available fibers range in diameter from less than about 0.001 mm to more than about 0.2 mm and exist in several different forms: staple fibers (known as staple fibers or chopped fibers), continuous single fibers (filaments or monofilaments), untwisted bundles of continuous filaments (tows), and twisted bundles of continuous filaments (yarns). Nonwoven fabrics can be formed from staple fibers by many processes including, but not limited to, meltblowing, spunbonding, spunmelt, solvent spinning, electrospinning, carding, film attenuation, melt film attenuation, air-laying, dry-laying, wet-laying, and combinations of these processes known in the art. The basis weight of a nonwoven fabric is typically expressed in grams per square meter (gsm).

[0037] As used herein, the term "absorbent hygiene product" refers to a product or aid that absorbs or contains bodily exudates; more specifically, to a product or aid that is placed against or adjacent to the user's body for the purpose of absorbing and containing various bodily exudates. Absorbent hygiene products include disposable diapers, diaper pants, incontinent adult underwear and pads, feminine hygiene products, nursing pads, disposable changing pads, bibs, bandages, and the like. The term "exudates," as used herein, refers to urine, blood, vaginal secretions, breast milk, sweat, and feces.

[0038] As used herein, the term "layer" refers to a subcomponent or element of a fabric. A "layer" may be in the form of multiple fibers made on a single beam, or on two or more successive beams that produce substantially the same fibers. For example, two successively aligned spunbond beams of substantially the same setting and polymer composition can together produce one layer. In contrast, two spunbond beams, for example, if one produces monocomponent fibers and the other produces bicomponent fibers, will form two distinctly different layers. The composition of a layer can be determined by knowing the individual settings and components of the resin (polymer) compositions used to form the layer, or by analyzing the nonwoven itself, for example, using an optical microscope or SEM microscope, or by analyzing the composition used to make the fibers of the layer using DSC or NMR methods.

[0039] The "spunbond" process is a nonwoven manufacturing system that involves the direct conversion of polymers into continuous filaments, integrating the conversion of the filaments into randomly arranged laid filaments to form a nonwoven batt, and then bonding the nonwoven batt to form a nonwoven fabric. Bonding can be accomplished by a variety of methods, such as air-through bonding, calendaring, etc.

[0040] "Activation" in this specification refers to a process in which a fiber or filament or fiber structure that is in a metastable state (e.g., not crystallized in the lowest possible energy state) is heated and then slowly cooled to transform the metastable state into some other more stable state (e.g., a different crystallized phase).

[0041] As used herein, the term "crimpable cross section" refers to a multicomponent fiber in which multiple components with different shrinkage properties are arranged across its cross section, and when heated above an activation temperature and then slowly cooled, the fibers will crimp, causing them to follow the shrinkage force vector. This results in a so-called helical crimp when the fibers are released, but when the fibers are contained in a fibrous layer, the ideal helix will not form due to the inter-fiber adhesion. For multicomponent fibers, the center of mass of each individual component in the fiber cross section can be determined (taking into account their area / position in the cross section). Without being bound by theory, the inventors believe that the center of mass of all the areas of each component is Contains the same A fiber is considered non-crimped when the center of mass is approximately the same point. For example, for a circular bicomponent fiber with a central core / sheath structure, the center of mass is at the center of the cross section (see Figure 2).

[0042] As used herein, the term "compressibility" refers to the distance in millimeters (mm) that a nonwoven fabric will compress under a load as defined by the "resilience" measurement.

[0043] The term "spinneret capillary density [1000 / m]" in this specification refers to the number of capillaries arranged in the spinneret per meter of CD distance.

[0044] As used herein, the term "filament speed" refers to a value calculated from the filament fiber diameter, throughput, and polymer density.

[0045] As used herein, the term "drawdown ratio" refers to the value calculated by dividing the capillary cross-sectional area by the filament cross-sectional area. To calculate the filament cross-sectional area, the fiber fineness, measured based on the apparent diameter, is used. Other non-circular cross-sections cannot be calculated using this method, and therefore require analysis of SEM images showing the actual cross-section.

[0046] In this specification, the term "cooling air / polymer of ratio rate " refers to the calculated value obtained by dividing the mass flow rate of the cooling air by the mass flow rate of the polymer.

[0047] Preferred embodiments of the present invention will now be described in more detail with reference to the accompanying schematic drawings, in which: [Brief explanation of the drawings]

[0048] [Figure 1] Filament Shape [Figure 2] Non-crimped cross section [Figure 3] Omni-directionality of filaments within layers according to exemplary embodiments of the present invention [Figure 4] Shrinkage of Example 2F compared to shrinkage of Example 4 [Figure 5] SEM micrographs of core / sheath fiber cross sections before and after activation [Figure 6a] Example of filament paths in fabrics according to the invention [Figure 6b] Example of filament paths in fabrics according to the invention [Figure 6c] Example of filament paths in fabrics according to the invention [Figure 7] Micrograph of multiple fiber layers with different crimp levels [Figure 8] Fabric Cross Section - Example 7C (Crimped Fiber) [Figure 9] Fabric Cross Section - Examples 5A+D (Examples in Accordance with the Invention) [Figure 10] Fabric Cross Section - Fabrics According to Exemplary Embodiments of the Invention [Figure 11A]A manufacturing line suitable for carrying out a method according to an exemplary embodiment of the present invention [Figure 11B] A manufacturing line suitable for carrying out a method according to an exemplary embodiment of the present invention [Figure 12] "Ratio of filament length to fabric length" - Example image to compare with b)

[0049] MODE FOR CARRYING OUT THE INVENTION The object of the present invention is to achieve a high-loft nonwoven fabric that can be compressed at relatively low pressure and recovers upon release. Those skilled in the art will be aware of various ways to achieve such a material using crimped fibers. However, the present inventors have found a surprising solution to the problem of achieving this effect using endless fibers with a non-crimped cross section.

[0050] According to the present invention, the nonwoven fabric comprises at least one layer formed from endless filaments having a predominantly non-crimped cross section. The fibers can be multicomponent, preferably bicomponent. Without being bound by theory, the inventors believe that the center of gravity of the surface formed by a component across the fiber cross section is equal to the center of gravity of each of the surfaces of the other components. Contains the same When they are in approximately the same position, the cross section is considered to be non-crimped.

[0051] For example, a layer according to the present invention may be composed primarily of endless filaments having circular cross sections, trilobal cross sections, star cross sections, etc. (See Figure 1.) Those skilled in the art will be aware of many possible shapes of fiber cross sections that do not substantially crimp upon cooling, nor do they have any latent crimp, but which may be activated by heating the fiber and subsequent cooling.

[0052] For example, the endless filament can be a multicomponent filament, with the layout of the components in the cross section being core / sheath (concentric circles) with the center of gravity of the component regions at one location within the filament cross section, a compartmentalized pie, or any other layout (Figure 2).

[0053] Preferably, layers according to the present invention are formed from bicomponent core / sheath filaments having a round or trilobal shape.

[0054] According to the present invention, the endless filaments are formed from two or more components, one of which provides a certain level of strength and toughness required for the recovery properties, while the other component provides softness and may also provide adhesion between the individual filaments to maintain the cohesive structure. For example, the first component can be selected from the group of polyesters (e.g., aromatic polyesters such as polyethylene terephthalate (PET) or aliphatic polyesters such as polylactic acid (PLA)), polyamides, polyurethanes, or copolymers or suitable mixtures thereof. It is within the scope of the present invention for the first component to consist of or essentially consist of a plastic from the group of polyesters, which also includes polyester copolymers (coPET) or polylactic acid copolymers (COPLA). Preferably, polyethylene terephthalate (PET) or polylactic acid (PLA) is used as the polyester.

[0055] For example, the second component can be selected from the group of polyolefins (i.e., polypropylene or polyethylene), low-melting polymers, copolymers or mixtures of suitable polymers. It is within the scope of the present invention for the second component to consist of or essentially consist of plastics from the group of polyesters, which also includes polyester copolymers (coPET) or polylactic acid copolymers (COPLA). Preferably, polyethylene (PE) is used as the polyolefin.

[0056] Preferred combinations of components for the bicomponent filaments of the nonwoven layer according to the invention are PET / PE, PET / PP, PET / CoPET, PLA / COPLA, PLA / PE, and PLA / PP.

[0057] Preferred bicomponent filaments have a ratio of the mass of the first component to the mass of the second component of 50:50 to 90:10.

[0058] In other embodiments, the components may include additives to modify filament properties. For example, the core may include color pigments or, for example, nucleating agents. Those skilled in the art will recognize that specific combinations of nucleating agents can significantly alter polymer crystallization and shrinkage behavior (e.g., as shown by Gajanan in U.S. Pat. No. 5,753,736, filed in 1995). On the other hand, for example, simple titanium dioxide, often used as a white colorant, produces only negligible changes in polymer behavior, which can be easily offset, if necessary, by slight adjustments to process conditions.

[0059] The sheath can include, for example, color pigments and surface modifiers (e.g., to achieve a silky feel or texture). Those skilled in the art will realize many other options based on the requirements of a particular application.

[0060] In other embodiments, the components can contain specific amounts of different polymers. For example, a first component (e.g., core) can contain a specific, minor amount of the polymer(s) of the second component (e.g., sheath), or vice versa; a second component (e.g., sheath) can contain, for example, a minor amount of the polymer(s) of the first component (e.g., core). Specific content levels can be used for the correct polymer combination. For example, Moore teaches that blending polyester with up to 10% polypropylene results in stable fibers (U.S. Application No. 2012088424, filed by 3M Innovative Properties, Inc.).

[0061] Without being bound by theory, the inventors believe that the key feature for forming a fabric with the desired properties is achieved by the combination of two components. First, the component of the filaments forming the nonwoven structure according to the present invention, for example forming the core, consists of polymer A, which is capable of shrinking under certain conditions. During the fiber formation process, particularly during cooling and drawing, polymer A is designed to undergo a change due to subsequent activation. For example, polymer A is left in a metastable state (e.g., not crystallized in the lowest possible energy state), and then heated during activation, followed by slow cooling, which transforms the metastable state into some other, more stable state (e.g., a different crystalline phase with a smaller volume). This change generates an internal shrinkage force that is believed to have a vector in the direction of the fiber centerline.

[0062] Fiber diameters in spunmelt nonwovens are in the millimeter and / or sub-millimeter range; typically, the fibers are non-directional (see Figure 3), and they contact each other so that the interfiber free space is also typically in the millimeter and / or sub-millimeter range. The interfiber bonds oppose the internal force vector and form the first point of resistance against that vector. This resistance point may be referred to as the threshold resistance point for structural contraction. For example, a single fiber, when properly conditioned and activated, can form, for example, irregular bows or waves in all three dimensions. In contrast, a fiber confined to the surrounding structure of adjacent fibers does not have such freedom.

[0063] The layer according to the present invention is formed from bicomponent filaments, with the second component being polymer B, which has a lower melting point and preferably also provides other desirable properties such as softness, pleasant skin feel, and feel-enhancing properties. The contraction properties of polymer material A and polymer material B must be different, with polymer material B (preferably the material forming the sheath of the filament) preferably having a lower contraction capacity than polymer material A (preferably the material forming the core of the filament). As a result, the contraction forces acting within the two adjacent polymer materials are different. Without being bound by theory, the inventors believe that because polymer material A and polymer material B always have different characteristics, the internal contraction force vectors are never the same at the same time. This force non-uniformity creates a second threshold resistance point to contraction. This resistance point can also be defined as the threshold resistance point to fiber contraction. For example, significant differences are observed when comparing the behavior of a layer formed from a monocomponent filament (e.g., PET) and a layer formed from a bicomponent filament (e.g., PET / PP) under the same conditions. Two samples of the same size, produced under the same conditions, were both exposed to an activation temperature of 120°C for the same time. The monocomponent PET shrank into small, planar objects, whereas the PET / PP structure, in contrast, increased in volume (smaller decreases in the CD and MD, larger increases in the z-direction - see Table 1 and Figure 4). [Table 1]

[0064] The CD or MD shrinkage of a batt layer according to the present invention upon activation is 20% or less, preferably 15% or less, preferably 13% or less, more preferably 11% or less, more preferably 9% or less.

[0065] The z-direction increase of a batt layer according to the invention upon activation is 20% or more, preferably 40% or more, preferably 60% or more, preferably 80% or more, more preferably 100% or more.

[0066] Quite simply, the shrinkage level of a batt can be estimated by the shrinkage level of a single fiber.

[0067] The volume change of a batt layer according to the invention undergoing activation is positive; preferably the volume change is greater than 10%, preferably greater than 15%, more preferably greater than 20%.

[0068] Those skilled in the art will understand that delicate manufacturing processes such as spunbonding can also be affected by a variety of other conditions that can induce specific counter forces that oppose shrinkage of both the fibers and the structure.

[0069] It is well known in the industry that certain combinations of polymers with different shrinkage levels arranged in a so-called crimpable cross-section result in so-called crimps, which can be immediate self-crimping or latent crimping, and require activation of the fiber (e.g., heat activation) to exhibit the crimp.

[0070] Fibers with a crimpable cross-section develop a regular crimp, forming a so-called helical crimp. Quite simply, fibers with a crimpable cross-section tend to bend toward the higher shrinkage component, resulting in a nearly uniform helical crimp. In other words, a crimpable cross-section causes the internal force vectors of the first and second components to shift regularly toward each other. Without being bound by theory, we believe that the regularity of the shift is the primary reason for the regular crimp on a free single fiber. In contrast, according to our invention, and without being bound by theory regarding fibers with a non-crimpable cross-section, we believe that the lack of a regular shift of the internal contraction force vectors of the first and second components toward each other causes the fiber to form irregular bows or waves in any direction. Quite simply, fibers do not have a uniform tendency to bend toward any particular portion of their cross-section or periphery, resulting in an irregular final shape. After activation, the fiber cross-section remains largely non-crimpable. Please refer to Figure 5.

[0071] Without being bound by theory, the inventors believe that if the internal contraction force is weak and cannot exceed the fiber resistance point threshold of the reaction force, the fabric will remain unchanged. If the internal contraction force is strong enough to exceed all of the MD / CD resistance point thresholds of the reaction forces, the fabric will contract according to the MD / CD ratio and form a flat structure. If the internal contraction force is only strong enough to exceed the fiber contraction resistance point threshold but not strong enough to exceed the structural MD / CD contraction resistance point threshold, the fibers will bend like springs in various directions, facing the lowest structural resistance, primarily from the z-direction, and form the desired bulky structure. The desired internal fiber contraction force is higher than the fiber internal resistance point but lower than the structural MD-CD contraction resistance point threshold.

[0072] A layer according to the present invention is formed from a large number of fibers with many contact points with each other. At the millimeter and / or submillimeter scale, the inventors believe that fibers, or more preferably millimeter and / or submillimeter portions of fibers, are uniquely positioned to experience multiple forces uniquely combined during activation by adjacent fibers, resulting in a wide variety of filament shapes in the final structure. In contrast, fibers can remain almost entirely planar in the MD / CD plane. Alternatively, fibers can move "up" or "down" to form large 3D structures in all MD, CD, and z directions. Some examples are shown in Figure 6. Without being bound by theory, the inventors believe that, according to the present invention, the diversity of filament paths within the layer provides benefits to the final properties. According to the present invention, the layer is homogeneous on a macroscopic scale. The diverse filament morphologies and their interactions within the layer provide advantages of the present invention, allowing the layer to respond to external forces (e.g., pressure and release, or fluid flow through the fibers) in a desired manner.

[0073] Quite simply, the fiber path can be expressed as the ratio of "filament length to fabric length."

[0074] In the nonwoven fabric according to the invention: the proportion of fibres having a "filament length to fabric length" ratio of greater than 1.2:1 is 20% or greater, preferably the proportion of fibres having a "filament length to fabric length" ratio of greater than 1.2:1 is 30% or greater, preferably the proportion of fibres having a "filament length to fabric length" ratio of greater than 1.2:1 is 40% or greater, more preferably the proportion of fibres having a "filament length to fabric length" ratio of greater than 1.2:1 is 50% or greater; the proportion of fibres having a "filament length to fabric length" ratio of greater than 1.5:1 is 10% or greater, preferably the proportion of fibres having a "filament length to fabric length" ratio of greater than 1.5:1 is 15% or greater, preferably the proportion of fibres having a "filament length to fabric length" ratio of greater than 1.5:1 is 20% or greater, preferably the proportion of fibres having a "filament length to fabric length" ratio of greater than 1.5:1 is 25% or greater, more preferably the proportion of fibres having a "filament length to fabric length" ratio of greater than 1.5:1 is 30% or greater; the proportion of fibers with a "filament length to fabric length" ratio of greater than 200% is 5% or greater, preferably the proportion of fibers with a "filament length to fabric length" ratio of greater than 200% is 10% or greater, preferably the proportion of fibers with a "filament length to fabric length" ratio of greater than 200% is 15% or greater, more preferably the proportion of fibers with a "filament length to fabric length" ratio of greater than 200% is 20% or greater; In the nonwoven fabric according to the invention: the proportion of fibres having a "filament length to fabric length" ratio of less than 2.5:1 is 10% or more, preferably the proportion of fibres having a "filament length to fabric length" ratio of less than 2.5:1 is 20% or more, preferably the proportion of fibres having a "filament length to fabric length" ratio of less than 2.5:1 is 30% or more, preferably the proportion of fibres having a "filament length to fabric length" ratio of less than 2.5:1 is 40% or more, more preferably the proportion of fibres having a "filament length to fabric length" ratio of less than 2.5:1 is 50% or more; The proportion of fibers with a ratio of "filament length to fabric length" of less than 200% is 5% or more, preferably the proportion of fibers with a ratio of "filament length to fabric length" of less than 200% is 10% or more, preferably the proportion of fibers with a ratio of "filament length to fabric length" of less than 200% is 15% or more, and more preferably the proportion of fibers with a ratio of "filament length to fabric length" of less than 200% is 20% or more.

[0075] In contrast to the present invention, fibers with a crimpable cross-section tend to form regular shapes—helical crimps, in which the fibers essentially bend regularly toward the fiber made of the more contractile material. These fibers are also constrained by adjacent fibers; regular forces create a generally helical shape. Without being bound by theory, the inventors believe that the greater the internal contraction force, the greater the "crimps per length" of a single fiber, and therefore the more helical sections present in the fabric structure. In contrast, at lower crimp levels, e.g., less than 25 crimps per inch (each single "round" of formed helix greater than 1 mm in length), the free space between fiber contact points begins to become insufficient for proper helical section formation, while the reaction forces generated by fiber contact become relatively strong. It should be understood that the number of crimps provided is merely exemplary and may vary with various fiber compositions and / or manufacturing conditions. At less than about 15 crimps per inch (each single "round" where the length of the helix formed is greater than 2 mm), it is difficult to distinguish the helical sections, and at less than about 10 crimps per inch (each single "round" where the length of the helix formed is greater than about 2.5 mm), the structure appears completely irregular, as the regular forces within the fiber are completely overcome by counterforces, tending toward regular crimp formation as opposed to a shift in the internal contraction vector. However, it should be understood that there are different engines driving the bulky structure (crimped cross-section) that arises from a shift in the regular internal contraction vector, and the bulky structure that arises from irregular fiber contraction in the case of a non-crimped fiber cross-section. An example of the difference in structure based on crimp of Lyon fiber is shown in Figure 7 (described in the article Fiber Crimp Distribution in Nonwoven Structure by Kunal Singha and Mrinal Singha, 2013, available at http: / / article.sapub.org / 10.5923.j.fs.20130301.03.html).

[0076] While it is complicated to describe in a general way the structural differences that distinguish nonwoven fabrics according to the present invention from those formed from crimped fibers, particularly at low crimp levels, those skilled in the art can confidently determine the type of fabric they are examining. For example, compare the SEM cross-sectional images of Examples 7C (crimped) and 05A+D (according to the present invention) in Figures 7 and 8.

[0077] In the case of uncertainty, the layout of components in the fiber cross section is the most important factor. This layout can be known from the manufacturing setting or can be estimated by the "fiber cross section type estimation" method.

[0078] The layer according to the present invention combines several important properties, which need to be properly balanced. The layer itself should be thick, lofty, and bulky, which can be described by the thickness of the layer. The layer itself should not be tough; it should be pleasant and comfortable for the end user. For example, when used as an ADL in a hygienic absorbent product or as part of a garment, it should be soft, thick, and elastic. Therefore, when pressure is applied (e.g., when sitting), it should compress smoothly with low pressure. This can be expressed by the compressibility in length units (e.g., mm). Furthermore, when pressure is released, the layer itself should recover, i.e., it can be expressed by the recovery measurement. The balance of all the above properties can be expressed by structural softness. Structural softness = (thickness / basis weight) x recovery rate x (compression rate / basis weight) x 10e6 TIFF0007582943000003.tif1999 formula: The thickness is measured in millimeters (mm). Basis weight is measured in grams per square meter (gsm) Recovery rate is a unitless ratio Compression ratio in millimeters (mm) = Compression ratio (unitless ratio) x Thickness (mm) The structural flexibility of the layer according to the invention is 40 m 4 mm 2 g -2 More than 80m; preferably 4 mm 2 g-2 More than 100m; preferably 100m 4 mm 2 g -2 Above 110m, preferably 4 mm 2 g -2 More than 120m, preferably 4 mm 2 g -2 More than 130m, preferably 4 mm 2 g -2 More than 140m, preferably 4 mm 2 g -2 Above, 150m is advantageous 4 mm 2 g -2 That's all.

[0079] The basis weight of the layer according to the invention is at least 5 gsm, preferably at least 10 gsm, more preferably at least 20 gsm, more preferably at least 30 gsm, advantageously at least 40 gsm. The basis weight of the layer according to the invention is at most 200 gsm, preferably at most 150 gsm, preferably at most 100 gsm, most preferably at most 80 gsm.

[0080] The thickness of the layer according to the invention relative to the basis weight (thickness recalculated to 1 gsm = thickness (mm) / basis weight (gsm)) is 5e10 -3 More than 10e10 -3 More than 12e10 -3 That's all.

[0081] The recovery rate of the layer according to the invention is greater than or equal to 0.8 (corresponding to a recovery rate of 80% of the original thickness), preferably greater than or equal to 0.82, more preferably greater than or equal to 0.84, most preferably greater than or equal to 0.85.

[0082] The compressibility of a layer according to the invention per gsm of layer basis weight is at least 0.25 microns (0.00025 mm), preferably at least 0.75 microns (0.00075 mm), preferably at least 1.25 microns (0.00125 mm), more preferably at least 1.75 microns (0.00175 mm). Thus, for example, the compressibility of a 100 gsm layer is at least 25 microns (0.025 mm), preferably at least 75 microns (0.075 mm), preferably at least 125 microns (0.125 mm), more preferably at least 175 microns (0.175 mm).

[0083] The modulus of elasticity of the layer according to the invention is 5% or more, preferably 8% or more, more preferably 10% or more, more preferably 13% or more, more preferably 15% or more.

[0084] Most preferably, layers according to the invention are comprised of filaments having a median fiber diameter of 5 microns or greater; preferably 10 microns or greater; preferably 15 microns or greater; advantageously 20 microns or greater. In exemplary embodiments, layers according to the invention are comprised of filaments having a median fiber diameter of 50 microns or less, preferably 40 microns or less, advantageously 35 microns or less.

[0085] Fiber thickness and fiber thickness distribution can affect many other parameters. For example, certain applications can utilize a homogeneous fiber thickness distribution, i.e., where the fibers are approximately the same, the vector forces among them are approximately equal, and the final fabric is approximately homogeneous. Such materials are advantageous, for example, in hygiene applications. For example, certain other applications can utilize a wide fiber thickness distribution, i.e., where there are thick and thin samples within the fabric. Without being bound by theory, the inventors believe that, from a certain level, the vector forces of thick fibers are much stronger than those of thin fibers, and therefore the thick fibers become the dominant activators, forming the final state of the nonwoven fabric, while the vector forces of thin fibers can be suppressed. A final structure in which thick fibers form a sort of internal skeleton may be advantageous, for example, for filtration. Combinations of thick and thin fibers can be produced using mixed filaments (e.g., mixed spunbond as described in Mitsui Chemicals Inc. application WO2009145105) or using continuous beams under conditions where the batts from each beam remain open enough to allow the thick and thin fibers to fuse into a single structure.

[0086] In another embodiment of this invention, a layer is defined by its void volume, which is defined as the volume percentage of the total volume of void space in the material relative to the bulk occupied by the material. Those skilled in the art will recognize that void volume can be measured in many different ways. For purposes of this report, the reported void volume is calculated from known basis weight (gsm), average polymer density, and known bulk (1 square meter of fabric thickness or caliper).

[0087] According to the invention, the void volume of the layer is 65% or more; preferably 75% or more; more preferably 80% or more; more preferably 84% or more; more preferably 86% or more; more preferably 88% or more; advantageously 90% or more.

[0088] In another embodiment of the present invention, as shown in a microscopic image (FIG. 10), a thick, elastic, and bulky nonwoven structure comprises numerous single filament loops and / or loop bundles protruding outward from the surface. Without being bound by theory, the inventors believe that these surface "hairs" have at least two functions: For example, in applications such as acquisition-distribution layers, these hairs serve to interconnect the thick, elastic ADL structure with the topsheet on one side and with the absorbent core underlying the ADL on the other side. This interconnection of the fibrous structures of the layers in the absorbent product improves fluid transport within the layers into the absorbent core. b. For example, in applications requiring direct contact with the user's skin, these hairs improve the tactile softness and make the fabric more comfortable to the touch and / or wear. For example, in hygiene applications, this advantage can be appreciated in soft, thick and elastic top and / or back sheets. For example, in protective clothing, the sheet can be used on the side facing the user's skin.

[0089] Disposable absorbent sanitary products, such as diapers, panty diapers, or pads, are comprised of numerous fibrous elements formed from nonwoven materials. Examples of such nonwoven elements include topsheets, backsheets, stand-up leg gathers, attachment areas for mechanical "hook and loop" closures, etc. In some absorbent sanitary products, the typical absorbent core formed from a mixture of cellulosic fluff pulp and superabsorbent polymers has been replaced with nonwoven layers containing superabsorbent polymer particles adhered to or intercalated between these layers by various means, such as adhesives, ultrasonic welding, heat welding, etc.

[0090] The high loft nonwoven fabrics / structures according to the present invention can be produced in a wide range of basis weights. Relatively light weight nonwoven fabrics between 5 and 35 gsm exhibit ideal properties for the outer layers of absorbent sanitary products, such as topsheets and backsheets, due to their outstanding softness, flexibility, and elasticity, which are mechanical requirements for materials that will remain in contact with human skin.

[0091] The significant loft and open surface structure of nonwoven fabrics according to the present invention provide a perfect "loopy" surface as an "attachment area" for the "hooks" on the sealing means of mechanical fasteners. Materials according to the present invention can be used not only as an attachment area on a backsheet, but can also form part of the surface of the backsheet. In the latter case, the backsheet and attachment area become a unitary material that fulfills both functions: "backsheet" and "attachment area." Nonwoven attachment areas in absorbent articles are described, for example, in U.S. Patent Application No. 2018318153 filed by Procter & Gamble.

[0092] Nonwoven fabrics according to the present invention, manufactured at high basis weights, such as 36-120 gsm, offer excellent properties as "acquisition and distribution layers" in absorbent hygiene products. The excellent shape memory, which benefits the resilience and recovery of the structure, can improve the management of liquid (e.g., urine) flow in absorbent products, especially in cases of multiple wetting, such as overnight. The "use of a supplemental distribution layer" in absorbent articles is described, for example, in U.S. Patent Application No. 2018296402 filed by Procter & Gamble.

[0093] The topsheet and ADL, both formed in accordance with the present invention, are combined to form a unitary material that forms the interface with the wearer's skin and the surge management element underlying the topsheet. These two layers of the unitary material can be manufactured separately and then adhered to each other, or they can be manufactured as a multi-layer material in one step. Unitary topsheets and absorbent articles are described, for example, in U.S. Patent Application No. 2018311082 filed by Procter & Gamble.

[0094] The open structure of the nonwoven material according to the invention results in a very high void volume. These void spaces of the fibrous structure, called pores, can be used as containers for superabsorbent polymer particles. Those skilled in the art will know how to introduce the particles into the fibrous structure, for example by applying vibration.

[0095] The present invention relates to a method for producing a nonwoven fabric from continuous filaments, in particular from continuous filaments of a thermoplastic material. In the context of the present invention, a nonwoven fabric layer formed or composed of continuous filaments is used. It is known that continuous filaments, due to their semi-endless length, are significantly different from staple fibers, which have a much shorter length, for example 10 mm to 60 mm.

[0096] A preferred embodiment of the present invention is characterized in that at least one nonwoven layer is formed as a spunbond nonwoven fabric by a spunbonding process. The nonwoven fabric can be formed from several layers. This embodiment of the present invention is particularly advantageous. The multicomponent or bicomponent filaments of the nonwoven fabric layer are spun using a spinning device or spinneret and then preferably passed through a cooling device for cooling. In the cooling device, the filaments are conveniently cooled using a fluid medium, in particular cooling air. It is within the scope of the present invention to then pass the spun filaments through a drawing device to draw the filaments. The drawn filaments are then accumulated on a tray, preferably laid on a moving forming belt, to form a nonwoven batt. In particular, by adjusting the parameters controlling the drawdown ratio, filaments with controlled shrinkage can be formed in the nonwoven layer. According to a preferred embodiment of the present invention, a sprinkler device is installed between the drawing device and the accumulation location as a storage device for managing the laying of the filaments. It is within the scope of the present invention to use at least one sprinkler device having side walls that diverge and are opposite each other in the direction of filament flow. A particularly preferred embodiment of the invention is characterized in that the drive units of the cooling device and the stretching device are designed as a closed system, in which there is no supply of cooling medium or cooling air to the cooling device, nor is there any external air supply, and such a closed system has proven itself to be excellent in the production of nonwoven fabrics.

[0097] It has been found that the technical problem of the present invention with regard to original shrinkage is solved particularly reliably and effectively when using the closing unit described, at least in addition to the particularly preferred embodiment of a spraying device between the stretching device and the storage area. The shrinkage capacity of nonwoven sheets produced by the spunbonding process is determined by the parameters drawdown ratio, cooling air / polymer ratio, and the like. of ratio rate , and it has already been shown that the filament speed can be very specifically adjusted or controlled.

[0098] As previously defined, a spunbond process is one in which a polymer is directly converted into continuous filaments and then the filaments are randomly laid down in a collection location to form a nonwoven layer composed of these filaments. The spunbond process defines both the properties of the single filaments as well as the properties of the final nonwoven fabric. It is not always possible to use the finished nonwoven fabric to determine the various properties and states of the individual filaments, such as rheological properties, polymer structure properties, and shrinkage, present during the individual nonwoven fabric manufacturing steps. In general, the shrinkage of a nonwoven layer determines its ability to produce a high-bulk nonwoven fabric by utilizing the shrinkage of single filaments to increase the relative thickness of the filament batt without disrupting the fabric structure and / or significantly changing the length and width of the filament batt.

[0099] It is within the scope of the present invention that the shrinkage capacity of the fibers is defined by using different raw materials in the composition of the continuous filaments, and / or by setting different process conditions in the production of the continuous filaments of the nonwoven fabric, and / or by using different filament cross-sectional shapes for the continuous filaments, and / or by adjusting the mass ratio between the different input materials, and / or by arranging the continuous filaments in different orientations.

[0100] A particularly preferred embodiment of the method according to the invention features nonwoven fabrics made from multicomponent filaments, especially bicomponent filaments with a substantially non-crimping cross section, in a core-sheath configuration or other bicomponent fibers with a substantially non-crimping configuration (Figure 2). It is essential that the multicomponent or bicomponent configuration does not generate internal forces within the filaments that can initiate regular crimping or curling of the filaments.

[0101] The first component of the filament, for example forming the core, consists of a polymer material A that is shrinkable under certain conditions. The second component of the filament, for example forming the sheath, consists of a polymer material B that is different from polymer material A. For example, the filaments comprise different polymers or polymer mixtures. Advantageously, according to a preferred embodiment of the invention, the difference between the melting points of polymer material A and polymer material B is greater than 5°C, preferably greater than 10°C. The first component can be selected from the group of polyesters (for example derived from aromatic polyesters such as polyethylene terephthalate (PET) or from aliphatic polyesters such as polylactic acid (PLA)), polyamides, polyurethanes, or copolymers or suitable mixtures thereof. It is within the scope of the present invention for the first component to consist of or essentially consist of a plastic from the group of polyesters, which also includes polyester copolymers (coPET) and polylactic acid copolymers (COPLA). It is preferred to use polyethylene terephthalate (PET) or polylactic acid (PLA) as polyester.

[0102] The second component can be selected from the group of polyolefins (i.e., polypropylene or polyethylene), low-melting polymers, copolymers or mixtures of suitable polymers. It is within the scope of the present invention for the second component to consist of or essentially consist of a plastic from the group of polyesters, which also includes polyester copolymers (coPET) or polylactic acid copolymers (COPLA). It is preferred to use polyethylene (PE) as polyolefin. Preferred combinations of components of bicomponent filaments in the nonwoven layer according to the present invention are PET / PE, PET / PP, PET / CoPET, PLA / COPLA, PLA / PE and PLA / PP.

[0103] Preferred bicomponent filaments have a ratio of the mass of the first component to the mass of the second component of 50:50 to 90:10. In the context of the process according to the invention, the mass ratio of the core-sheath configuration can be freely changed during production without shutting down the machine.

[0104] Filaments with a non-crimping cross-section offer manufacturing advantages over crimping filaments, as they allow for the achievement of bulkier, softer, thicker, and more elastic materials. Unlike non-crimping fibers, it is not easy to control filaments that exhibit (self-)crimping during manufacturing. Most filament types with a crimping cross-section undergo crimping during the laying process and / or upon activation. These filaments move relative to one another during the crimping process, and therefore can easily come into contact with or become entangled with one another, or in other words, interfere with one another. Therefore, the design of nonwoven layers made of self-crimping filaments tends to be limited by the uneven fiber distribution caused by the relative movement of the filaments. The resulting workarounds often involve reduced throughput, slower production speeds, and special intermediate processing steps to secure the filaments together.

[0105] Because the present invention does not utilize self-crimping filaments, a much more uniform lay-down can be achieved, which allows for the lowest possible basis weight while maintaining the desired fabric properties and / or allows for faster production line speeds with higher throughput. The use of non-crimping filaments makes the process much easier to control and reduces the manufacturing costs of the spinning nozzle / spinning beam.

[0106] It is within the scope of the present invention to thermally pre-bond, i.e., pre-consolidate, thermally activate, and heat-bond the resulting nonwoven layer. Heat activation and bonding are preferably carried out with the aid of at least one hot fluid and / or by contact with a hot surface. The hot surface may in particular be part of a roller. Heat activation is preferably carried out under conditions that result in uniform shrinkage over the entire surface of the fibrous layer. Heat activation can be carried out in a hot air box or by passing the vat through an oven. Heat activation and bonding can also be carried out by ultraviolet light, microwaves, and / or laser irradiation. It should be emphasized that heat bonding in the context of this "in-line" process can be carried out immediately after the upstream process steps are completed, or both process steps, heat activation and bonding, can be "off-line" and thus separated from the upstream process steps. Thus, heat activation can, in principle, be carried out "off-line" at a different time and place. Therefore, the nonwoven fabric, which is not yet heat-activated and therefore not very bulky, can be transported to another processing location in a simple and space-saving manner.

[0107] The desired level of fabric / batt pre-consolidation depends heavily on the process conditions. It is important to correctly set the level of inter-fiber cohesion within the batt and thereby control the level of batt cohesion based on the requirements of the next manufacturing step. In the case of line processes with belt activation, the desired level of cohesion is rather low, and cohesion is only necessary to prevent tearing or thinning caused by undesirable large fiber movements during the activation step. In special cases, for example, when multiple fibers themselves provide very good cohesion, either in contact with each other or with the underlying layer due to, for example, their cross-sectional shape, entanglement rate, or material composition, the batt cohesion may be sufficiently good even without thermal pre-consolidation. In other cases, for example, when the process is divided into two steps or when the pre-consolidated batt is transported, for example in the form of a roll, before full activation, the desired level of cohesion may be significantly higher, and therefore the pre-consolidation level may also need to be significantly higher. Those skilled in the art, familiar with the process conditions for textiles, will readily recognize the level of pre-consolidation required for a particular example of the conditions.

[0108] The activation temperature preferably ranges between the glass transition temperature and the softening point (Vicat softening point ISO DEN 306) of component(s) A, preferably the core component. It should be understood that an optimum activation temperature can be selected for a given composition of components.

[0109] The present invention provides a high-loft nonwoven fabric formed using filaments with regulated or controlled shrinkage. Shrinkage occurs uniformly throughout the batt, and therefore the process should provide uniform nonwoven fabric properties that ensure uniform and controlled shrinkage.

[0110] In the cooling device, the filaments are conveniently cooled by a fluid medium, especially cooling air. As already mentioned, the potential shrinkage of the filaments must be uniformly distributed over the entire length, width, and thickness of the final nonwoven fabric. The shrinkage characteristics depend on the drawdown ratio, cooling air / polymer ratio, and the of ratio rate , and can be improved by adjusting the filament speed, so that in the present invention these parameters are approximately uniform for each individual filament.

[0111] It is within the scope of the present invention that the formed nonwoven fabric consists of several layers each formed on a spunbond beam (1), it being understood that a plurality of layers are superimposed and transported together on at least one forming belt (2) to a final bonding device (3).

[0112] Filaments (4) are spun from the spinneret (5). The filament arrangement is optimized in a staggered pattern to ensure that each filament has a very similar mass and very similar cooling air temperature. The spinnerets vary not only in the number of capillaries, but also in their capillary diameter (d) and length (l). The length (l) is typically calculated as a multiple of the capillary diameter and, for this application, ranges from 2 to 10 l / d. The number of capillaries must be selected based on the desired filament spinning speed, along with the desired final filament diameter and the desired or planned total polymer throughput. The number of capillaries ranges from 800 to 7,000 per meter, with filament diameters ranging from 8 to 45 μm. The capillary diameter and filament speed are selected to produce an appropriate level of shrinkage in the final filament. The filament speed should be defined as 3000 to 5500 m / min, and the capillary diameter should be 200 to 1000 μm. As a result, for circular capillaries, the drawdown ratio suitable for the manufacturing process is 200 to 1300, which is desirable for line manufacturability. For circular capillaries, the drawdown ratio more suitable for the manufacturing process is 300 to 800. Non-circular capillaries usually exhibit relatively high drawdown ratios, which depend greatly on the capillary shape and the surface area to volume ratio. The volume and temperature of the cooling air are set to achieve an appropriate drawdown ratio and cooling conditions. The cooling air / polymer ratio has been identified as 20 to 45, which is useful in this invention. The volume and temperature of the cooling air are controlled by a cooling device (6). The temperature can be set to 10 to 90°C, preferably 15 to 80°C, so that the shrinkage rate can be controlled by the cooling conditions. The cooling conditions determine the rate at which the filaments are cooled from their melting point at the time of spinning to their glass transition point. For example, increasing the temperature of the cooling air will slow the cooling of the filaments. To achieve the necessary and useful temperature range of the cooling air, as in the present invention, it is actually easier to manage the temperature range by dividing the cooling device into two different zones whose temperatures can be controlled independently. In the first zone (6a) close to the spinneret, the temperature can be set to 10°C to 90°C, preferably 15°C to 80°C, and most preferably 15°C to 70°C. In the second zone (6b) close to the first zone, the temperature can be set to 10°C to 80°C, preferably 15°C to 70°C, and most preferably 15°C to 45°C.

[0113] The filaments are then led to the drawdown zone (7). The filaments are drawn down by the tensile force generated by the cooling air velocity. The amount of cooling air and the adjustable geometry of the drawdown zone convert the air velocity into a filament velocity. The filament velocity defines the filament diameter together with the polymer throughput. The potential shrinkage is a function of the filament velocity, the drawdown ratio, and the cooling air / polymer ratio. of ratio rate Controlled by:

[0114] In the next step, the filaments are guided to a spreading device (8) with side walls that diverge in the direction of filament flow. These walls are adjustable in such a way that a uniform nonwoven fabric is achieved in which the single filaments form a filament laying array oriented in all directions in the MD / CD plane.

[0115] It has been found that filament lay-down is influenced by the air that guides the filaments in the spreader. The air can be adjusted to create arrangements ranging from a clear zigzag lay-down arrangement to circular loops and even elliptical structures with CD orientation. The filaments are laid down on the forming belt and transported to at least one pre-compaction device (9). Cooling air passes through the filament lay-down layer and the forming belt and moves out of the process. The amount of suction air can be adjusted to assist in the filament lay-down and ensure that the filament batt is fixed firmly on the forming belt. The pre-compaction device is located close to the spreader. The filament batt is controlled by suction air on its way from the spreader to the pre-compaction device. Pre-compaction of the filament batt is achieved by hot air.

[0116] The energy delivered to the filament vat controls the filaments to only partially soften or pre-melt, creating good cohesion between the individual filaments. Good cohesion of the filaments allows the filament vat to be transported on the forming belt without further assistance from other devices and without being affected by conveying forces or being destroyed / damaged. This pre-consolidation process is also sufficient to transfer the filament vat into another laying area on a multi-beam production line. The energy delivered to the filaments is not sufficient to activate filament contraction.

[0117] The method of the present invention describes a balance of pre-compacting parameters, pre-compacting temperature, pre-compacting air velocity, and pre-compacting time, which is understood to be the time during which the filament batt is treated with pre-compacting air.

[0118] It is recommended that the pre-consolidation time of the batt is 1 to 10,000 ms, preferably 2 to 1,000 ms, and most preferably 4 to 200 ms.

[0119] The pre-compression air speed used in this pre-compression device can be adjusted in the range of 0.1 to 10 m / s, preferably 0.8 to 4 m / s. The pre-compression temperature is recommended to be 80°C to 200°C, preferably 100°C to 180°C. In one embodiment, the pre-compression temperature is 90°C to 150°C, particularly 110°C to 140°C. According to a preferred embodiment, the nonwoven layer of bicomponent filaments has a core component made of polyethylene terephthalate (PET) and a sheath component made of polyolefin, particularly polyethylene or polypropylene, in which the pre-compression temperature is preferably 110°C to 160°C, particularly 120°C to 150°C. In one embodiment, the nonwoven layer is made of bicomponent filaments having a core component made of polyethylene terephthalate (PET) and a sheath component made of polyethylene terephthalate copolymer (CoPET), in which the pre-compression temperature is preferably 110°C to 180°C. When the nonwoven layer is made of bicomponent filaments having a core component made of polylactic acid (PLA) and a sheath component made of polyolefin, especially polyethylene or polypropylene, the pre-consolidation temperature is preferably between 80°C and 130°C.

[0120] Further along the production line from the spraying device, the filament batt is conveyed to at least one activation unit (10). The filaments are activated by hot air. It has been found that the actual shrinkage of the shrinkable component of the filaments is a function of the temperature of the shrinkable component of the filaments and the duration of temperature exposure. The rate of the shrinkage process depends on the temperature of the shrinkable component of the filaments. In the present invention, the process is controlled to slowly induce shrinkage, so that the force induced into the filament batt from the shrinkage is lower than the cohesive force between the filaments. This process control results in a cohesive and uniform nonwoven structure with a reduced filament structural density and also increases the thickness of the nonwoven.

[0121] One embodiment of the present invention is to combine the process steps of pre-compaction and activation in a combined pre-compaction and activation device by controlling the pre-compaction and / or activation time, the pre-compaction and / or activation air speed, and the pre-compaction and / or activation temperature.

[0122] This innovative method describes the balance of activation parameters: activation temperature, activation air speed, and activation time. Activation time is understood as the time during which the filament batt is treated with activation air. These parameters can be varied within the aforementioned ranges to set the ideal combination of activation time, activation temperature, and activation air speed, corresponding to the potential shrinkage level of the filament.

[0123] The activation time of the bat is recommended to be 20 to 5000 ms, preferably 30 to 3000 ms, and most preferably 50 to 1000 ms.

[0124] The activation air speed used in this activation unit can be adjusted within a range of 0.1 to 2.5 m / s, preferably 0.3 to 1.5 m / s. The activation temperature for thermal activation is recommended to be 80 to 200°C, preferably 100 to 160°C. In one embodiment, the activation temperature is 90 to 140°C, particularly 110 to 130°C. According to a preferred embodiment, the nonwoven layer of bicomponent filaments has a core component made of polyethylene terephthalate (PET) and a sheath component made of polyolefin, particularly polyethylene or polypropylene, and the activation temperature is preferably 90 to 140°C, particularly 100 to 140°C. In one embodiment, the nonwoven layer is made of bicomponent filaments having a core component made of polyethylene terephthalate (PET) and a sheath component made of polyethylene terephthalate copolymer (CoPET), and the activation temperature is preferably 120 to 160°C. When the nonwoven layer is made of bicomponent filaments having a core component made of polylactic acid (PLA) and a sheath component made of polyolefin, especially polyethylene or polypropylene, the activation temperature is preferably between 80°C and 140°C.

[0125] The innovative method of the present application provides for a final bonding step in which the filament batt is treated with hot air in a bonding device (3). The bonding device bonds all of the single and / or multiple layers of filament batt together without significantly reducing the thickness of the filament batt and without creating a significant bonding gradient across the thickness of the nonwoven. The remaining thickness and elasticity of the nonwoven are affected by the bonding temperature, which must be high enough to achieve the desired bond between the nonwoven fibers without softening and disintegrating the filament batt. The bonding device must match the bonding temperature and adhesive force to the filament batt to the desired process effect, which has a low softening point and low force but is sufficient to affect the integrity of the nonwoven filament batt. This can be achieved with several different devices, such as omega drum bonding devices, flat belt bonding devices, and multi-drum bonding means.

[0126] The bonded nonwoven fabric is finally wound up on a winder (11). If the surface properties of the nonwoven fabric are to be modified, for example to improve fluid transport or moisture absorption performance, a spray device or kiss roll can be placed between the forming belt and the final bonding device, or between the final bonding device and the winder.

[0127] One embodiment of the present invention is to combine the activation and bonding process steps by controlling the activation and / or bonding time, activation and / or bonding air speed, and activation and / or bonding temperature of the bonding device.

[0128] The method of the present invention describes a balance of bonding parameters: bonding temperature, bonding air velocity, and bonding time. Bonding time is understood to be the time during which the filament batt is treated with bonding air. These parameters can be varied within the aforementioned ranges to achieve an ideal combination of bonding time, bonding temperature, and bonding air velocity, depending on the connection ability of the filament batt.

[0129] It is recommended that the bonding time of the batt is 200 to 20,000 ms, preferably 200 to 15,000 ms, and most preferably 200 to 10,000 ms.

[0130] The adhesive air speed used in this adhesive unit device can be adjusted within the range of 0.2 to 4.0 m / s, preferably 0.4 to 1.8 m / s. The adhesive temperature for thermal bonding is recommended to be 100°C to 250°C, preferably 120°C to 220°C. In one embodiment, the adhesive temperature is 90°C to 140°C, particularly 110°C to 130°C.

[0131] According to a preferred embodiment, the nonwoven layer of bicomponent filaments has a core component made of polyethylene terephthalate (PET) and a sheath component made of polyolefin, in particular polyethylene or polypropylene; the bonding temperature is preferably 90°C to 140°C, in particular 100°C to 140°C. In one embodiment, the nonwoven layer is made of bicomponent filaments, the core component is formed from polyethylene terephthalate (PET) and the sheath component is formed from polyethylene terephthalate copolymer (CoPET), and the bonding temperature is preferably 140°C to 230°C.

[0132] When the nonwoven layer is made of bicomponent filaments with a core component made of polylactic acid (PLA) and a sheath component made of polyolefin, especially polyethylene or polypropylene, the bonding temperature is preferably 80°C to 140°C. The aforementioned temperature ranges can be used for different individual processes, whereby the bonding air temperature and bonding air speed are within the aforementioned ranges but at different levels in different areas of the bonding device.

[0133] The present invention is based on the finding that nonwoven fabrics according to the invention can be designed to be relatively bulky and thus relatively thick, while still retaining sufficient stability. The layers according to the invention exhibit excellent elasticity after being subjected to load or pressure. These advantageous properties can be achieved if the nonwoven fabric has a relatively low basis weight.

[0134] The method of the present invention is further characterized by the advantage that it allows the continuous production of nonwoven fabrics in a simple manner at relatively high production rates without interrupting the process. The parameters for producing nonwoven fabrics are highly variable and flexible and can be adjusted during the process, allowing for the production of variable end products without interrupting the process. Furthermore, the parameters of the pre-consolidation, activation, and bonding steps can be easily modified.

[0135] The method of the present invention can be carried out in a simple "in-line" manner, but can also be easily carried out "off-line" if necessary. Pre-consolidation, shrinkage activation, and final bonding can therefore be separated without any problems from the actual laminate production. In summary, it is remarkable that innovative fabrics with highly advantageous 3D structured surfaces of large volume and thickness can be produced in a simple, inexpensive, and cost-effective manner while still satisfying the compressive strength of the fabric. Various parameters of the nonwoven fabric or the resulting nonwoven layer can be changed during the manufacturing process and can be flexibly adjusted.

[0136] Example According to the present invention, layers can be produced, for example, in a laboratory line at the Center of Polymer Systems, Zlín Tomáš Beta University, Czech Republic. The laboratory line, model LBS-300, can produce spunbond or meltblown fibers of mono- or bi-compositions. The extrusion system of this model, consisting of two extruders, can heat the polymer up to 450°C. Spunbond fibers can be produced using a spunbond die with 72 holes (0.35 mm diameter; 1.4 mm length) in a square area of ​​6 x 6 cm. There are several configurations for the bicomponent die: core / sheath, side-by-side, compartmental pie, or sea-island. The system is open; the extension air pressure of the inlet system can be up to 150 kPa. The filaments can be collected as is or laid on a belt at speeds of 0.7 to 12 m / min. The final product width is up to 10 cm. The total processing rate can be set between 0.02 and 2.70 kg / h. The final product basis weight is between 30 and 150 g / m 2There is also the option of using calender rolls to bond the batts at temperatures up to 250°C. This laboratory line was used to manufacture the layers described in Examples 1 to 4.

[0137] A standard stationary oven was used to model laboratory air-through bonding (Examples 1-4). Due to the significant differences in heat transfer conditions that exist between a still atmosphere oven and an airflow through the fabric, and the heat lost when the oven is opened and closed, a 5-minute activation time was used.

[0138] Example 1 - Example according to the present invention The nonwoven fabrics consisted of non-crimped, core / sheath bicomponent filaments with a core / sheath mass ratio of 70:30. The core was made of PLA (Ingeo, Nature Works) and the sheath was made of PP (Tatren HT 2511, Slovnaft). The nonwoven fabrics were produced on a laboratory line at the Center of Polymer Systems, Zlín Tomáš Beta University. The core extruder was heated to a maximum of 240°C (with three zones heated to 195°C, 220°C, and 240°C, respectively), and the sheath extruder was heated to a maximum of 235°C (with three zones heated to 200°C, 215°C, and 235°C, respectively). The spinning beam temperature was set to 240°C. The polymer throughput was set to 0.25 g / min / capillary. The filaments were cooled with air at a temperature of 20°C. The inlet pressures are listed in Table 2. The inlet pressure for Examples 1A, 1C, 1E, and 1F was 100 kPa, the inlet pressure for Example 1B was 50 kPa, and the inlet pressure for Example 1D was 150 kPa. The fibers were collected on a moving belt; the gsm of the batt was 130 g / m 2 The batts from the belt were cut into test specimens measuring 10 x 7 cm. Each sample was carefully transferred to a separate oven and activated for 5 minutes at a set temperature, as shown in Table 2 for each of Examples 1A-1F. [Table 2] Examples 1B, 1C, and 1D demonstrate the potential for controlling shrinkage levels through the amount of fiber draw force (inlet pressure). Cooling is the same in all three examples. Without being bound by theory, we believe that the draw force serves to induce a range of metastable crystalline states in the filaments, some of which are more desirable for thickening than others. A weak draw force can result in a relatively low tenacity fiber, potentially reducing the final thickness of the fabric. On the other hand, a strong draw force sets the induced crystallization to undergo volumetric change, resulting in a lower shrinkage force upon activation, again reducing the final thickness. A moderate draw force, as shown in Example 1C, maximizes not only the final fabric thickness but also structural softness. Optimal conditions can be achieved by adjusting the filament speed and drawdown ratio. Examples 1A, 1C, 1E and 1F show the possibility of controlling the shrinkage level by the activation temperature. Under these correct conditions, it can be seen that the best final thickness is achieved for the sample activated at 140°C (+155%), however, the material according to the invention is complex and the key evaluation parameter is structural flexibility, and the best samples are activated at 120°C.

[0139] Example 2 - Example according to the present invention The nonwoven fabrics consisted of non-crimped, core / sheath bicomponent filaments with a core / sheath mass ratio of 70:30. The core was made of PET (Invista 5520-type resin) and the sheath was made of PP (Slovnaft Tatren HT 2511). The nonwoven fabrics were produced in a laboratory line at the Center of Polymer Systems, Zlín Tomáš Beta University. The core extruder was heated to a maximum of 340°C (with three zones heated to 340°C, 335°C, and 325°C, respectively), and the sheath extruder was heated to a maximum of 235°C (with three zones heated to 200°C, 215°C, and 235°C, respectively). The spinning beam temperature was set to 305°C. The polymer throughput was set to 0.25 g / min / capillary. The filaments were cooled with air at a temperature of 20°C. The inlet pressures are shown in Table 3. Fiber is collected on a moving belt; the gsm of the batt is 75 g / m 2 The batts from the belt were cut into test specimens measuring 10 x 7 cm. Each specimen was carefully transferred to a separate oven and activated at the set temperature for 5 minutes. The different temperatures corresponding to Examples 2A to 2F are shown in Table 3.

[0140] Example 3 - Example according to the present invention The nonwoven fabrics consisted of non-crimped, core / sheath bicomponent filaments with a core / sheath mass ratio of 70:30. The core was made of PET (Invista 5520 type resin), and the sheath was made of a blend of 95% PP (Slovnaft Tatren HT 2511) and 5% white masterbatch (PolyOne CC10084467BG). The nonwoven fabrics were produced on a laboratory line at the Center of Polymer Systems, Zlín Tomáš Beta University. The core extruder was heated to a maximum of 340°C (with three zones heated to 340°C, 335°C, and 325°C, respectively), and the sheath extruder was heated to a maximum of 235°C (with three zones heated to 200°C, 215°C, and 235°C, respectively). The spinning beam temperature was set at 305°C. The polymer throughput was set at 0.25 g / min / capillary. The filaments were cooled with air at a temperature of 20°C. The inlet pressures are shown in Table 3. The fibers were collected on a moving belt; the gsm of the batt was 75 g / m2 The batts from the belt were cut into test specimens measuring 10 x 7 cm. Each specimen was carefully transferred to a separate oven and activated at the set temperature for 5 minutes. The temperatures are shown in Table 3.

[0141] Example 4 - Comparative Example The nonwoven fabric has a non-crimping cross-sectional layout and consists of bicomponent core / sheath filaments, both of which are made of PET (Invista 5520 type resin). The nonwoven fabric was produced in a laboratory line at the Centre of Polymer Systems, Zlín Tomáš Beta University. The extruder was heated to a maximum of 340°C (three zones heated to 340°C, 335°C, and 325°C, respectively). The temperature of the spinning beam was set to 305°C. The polymer throughput was set to 0.25g / min / capillary. The filaments were cooled with air at a temperature of 20°C. The inlet pressure is shown in Table 3. The fibers were collected on a moving belt; the gsm of the batt was 75g / m². 2 The batts from the belt were cut into test specimens measuring 10 x 7 cm. Each specimen was carefully transferred to a separate oven and activated at the set temperature for 5 minutes. The temperatures are shown in Table 3. [Table 3] Examples 2C and 3 demonstrate the same principle as Examples 1B-D above. Examples 2A-F demonstrate the possibility of controlling the level of shrinkage through activation temperature. With these correct conditions, it is clear that the sample activated at 140°C (+51%) gave the best final thickness, and this temperature was also the best in terms of structural flexibility. Example 3 and Comparative Example 4 demonstrate the importance of the correct sheath material in materials according to the invention. It can be clearly seen that the PET / PET materials behave very differently upon activation, which leads to different shrinkage levels (see Figure 4). The sample according to the invention increased in volume by 47% and also showed good elasticity and recovery figures. In contrast, the PET / PET sample lost 56% in volume and shrunk into a slightly bent, rigid piece with no measurable elasticity or recovery figures. Also, the filament length could not be measured. Note that, as with Examples 1A-E above, Examples 2A-F have CD and MD shrinkage levels below 10%. In contrast, the increase in thickness is much greater than the decrease in CD and MD. Examples 2F and 3 achieve very good values ​​of structural softness while also achieving acceptable levels of CD and MD shrinkage (15%). It should be noted that the PET used in Examples 2 to 4 contained a small amount of TiO2 (used as a matting agent by the polymer manufacturer). In contrast, the PLA used in Example 1 did not contain any TiO2. According to an exemplary embodiment of the present invention, one or two layers can be produced in-line, for example on a pilot line at Reifenhaeuser Reicofil GmbH in Troisdorf, Germany. This line was used to produce the nonwoven fabrics described in the following examples according to the present invention, i.e., Examples 5, 6, 8, 9, 10, and 11, with the following standard settings: Pre-compaction wind speed: 2.3 m / s Activated wind speed 1.3[m / s] Adhesive wind speed 1.3[m / s] Quenching air temperature 20[℃]. The pilot line is equipped with two BiCo spunbond beams, each with two extruders equipped with BiCo coathanger dies. The extrusion system allows for the processing of a variety of polymers at temperatures up to 350°C, with a specific total throughput per beam ranging from 80 to 450 kg / h / m. Multiple spinnerets with various capillary densities and capillary geometries are available. Using a spin pack with a Hills melt distribution system, virtually any imaginable cross section can be produced on the 1.1-m-wide spinneret, in addition to the standard cross sections described in this invention. The cooling, stretching, and forming equipment is today's industry standard, accommodating a wide range of cooling and drawing conditions and ensuring the formation of an excellent, uniform filament batt. The forming belt runs at production speeds of up to 400 m / min. The nonwoven layer from the first spunbond beam passes through optional in-line pre-consolidation, activation, and / or bonding equipment before the layer from the second beam is laid on top of the first beam. The second beam is equipped with optional in-line equipment for pre-consolidation, activation, and bonding similar to the first beam. The pre-bonded or final bonded product may be wound on an in-line slitter rewinder or may be bonded in-line with a drum bonding means before winding. Kiss-roll surfactant treatments to modify the surface properties of the nonwoven are available in-line or off-line.

[0142] Example 5 - Example according to the present invention The nonwoven fabrics were produced on a single circular core / sheath bicomponent spunbond beam. The core / sheath mass ratio was 70 / 30. The core was made from PET (Invista 5520 type resin) and the sheath was made from PE (Dow ASPUN 6834). The process conditions and final fabric parameters for each of Examples 5A to 5D are shown in Table 4 below. Activation and bonding were performed on a single machine with an activation zone and a bonding zone. [Table 4] Examples 5A to 5D show the effect of cooling air / polymer on the final fabric properties. of ratio rateThe results show the importance of the drawing ratio, drawdown ratio, and filament speed. It can be seen that with increasing drawing and cooling, fabric thickness, fiber diameter, and even structural softness decrease, while the mechanical properties of the final product improve.

[0143] Example 6 - Example according to the present invention The nonwoven fabrics were produced on two circular core-sheath bicomponent spunbond beams. The core / sheath mass ratio was 70 / 30. The core was made from PET (Invista 5520 type resin) and the sheath was made from PE (Dow ASPUN 6834). The process conditions and final fabric parameters for each of Examples 6A to 6D are shown in Table 5 below. Activation and bonding were performed on a single machine with an activation zone and a bonding zone. [Table 5]

[0144] Example 7 - Comparative Example The nonwoven fabrics consisted of circular eccentric core / sheath bicomponent filaments arranged in a crimped cross-section, with the core made of PET and the sheath made of PE. The fabrics were hot-air bonded. The fabric parameters for Examples 7A-7C are shown in Table 6 below. [Table 6] Examples 7A-C represent single-layer nonwoven fabrics with comparable polymer compositions. However, these fibers have a crimpable cross-section and crimp, as seen in the fabric cross-section in Figure 8 compared to the cross-section of the example (5A+D) according to the present invention - Figure 9. The structural softness of the examples is significantly lower compared to Examples 5 and 6, as is the fabric thickness.

[0145] Example 8 - Example according to the present invention The nonwoven fabrics were produced from two circular core-sheath bicomponent spunbond beams. The core / sheath weight ratio was 70 / 30. The core was made from PET (Invista 5520 type resin) and the sheath was made from coPET (Invista 701k type). The process conditions and final fabric parameters for Examples 8A and 8B are listed in Table 7 below. Activation and bonding were performed in-line on the belt using separate activation and bonding equipment.

[0146] Example 9 - Example according to the present invention The nonwoven fabrics were produced on two circular core-sheath bicomponent spunbond beams. The core / sheath mass ratio was 70 / 30. The core was made from PET (Invista 5520 type resin) and the sheath was made from coPET (Invista 701k type). The process conditions and final fabric parameters for Examples 9A-9C are shown in Table 7 below. Activation was performed in a single step, and bonding was performed in a second step on a different machine. For Example 9A+B, bonding was performed immediately after in-line activation on a drum. For Example 9C, bonding was performed on a different machine a few days after offline activation on a drum. [Table 7] Examples 8 and 9 demonstrate the importance of the bonding conditions. Example 8 focuses on high structural flexibility. Because the sheath polymer melting point is higher than in the previous examples, the optimum bonding temperature is higher than the core activation temperature. The bonding temperature used (155°C) is close to the optimum activation temperature, but does not achieve the optimum bonding level. It also results in low mechanical properties. In contrast, Example 9 focuses on the optimum bonding level, with good mechanical properties but low thickness and structural flexibility. Example 9C simulates the possibility of separating the "activation" and "bonding" process steps from each other, and is bonded offline. After activation, the product is wound and transported to a separate location, where it is unwound and the final bonding takes place. Besides bonding temperature and time, other parameters, especially the pressure during the bonding stage (including pressure from air throughput, pressure from nonwoven fabric tension, pressure from auxiliary guide rollers, etc.), can also affect the final thickness and reduce structural flexibility. The difference between Examples 9A+B and 9C not only represents the online / offline possibility, but also the influence of different bonding settings.

[0147] Example 10 - Example according to the present invention The nonwoven fabrics were produced on two trilobal core-sheath bicomponent spunbond beams. The core / sheath mass ratio was 70 / 30. The core was made from PET (Invista 5520 type resin) and the sheath was made from coPET (Invista 701k type). The process conditions and final fabric parameters are shown in Table 8 below. Activation and bonding were performed on a single machine with activation and bonding zones.

[0148] Example 11 - Example according to the present invention The nonwoven fabrics were produced on two circular core-sheath bicomponent spunbond beams. The core / sheath weight ratio was 70 / 30. The core was made from PET (Invista 5520 type resin) and the sheath was made from coPET (Trevira RT5032 type). The process conditions and final fabric parameters for Examples 11A and 11B are shown in Table 8 below. Activation and bonding were performed on a single machine with an activation zone and a bonding zone. [Table 8] Example 10 demonstrates the possibility of using different non-circular filaments. Examples 11A+B demonstrate the possibility of also using spinnerets with higher capillary densities.

[0149] Example 12 - Comparative Example The nonwoven samples selected for comparison were manufactured using the brand "TWE Hygiene" manufactured by TWE gtoup. This nonwoven is made of short bicomponent fibers of the core-sheath type, with the core made of PET and the sheath made of PE (previously, reasonable guesses have been made as to the materials of these samples, but no in-depth laboratory analysis of the materials has been performed). The fabrics were manufactured using the carding technique and consolidated by hot air bonding. The fabric parameters for each of Examples 12A to 12C are shown in Table 9 below. [Table 9]

[0150] The objective of the present invention is to achieve a high-loft nonwoven fabric that can be compressed with relatively low pressure and recover when released. Those skilled in the art will recognize that modern worsted materials may also be suitable as a result of long-term development. On the other hand, worsted materials are made from staple fibers, and the high number of fiber ends running across the nonwoven layer may be undesirable for certain applications. Examples 12A-C show the properties of three commercially available worsted fabrics designated for hygiene applications. Comparing this set of samples with the present invention samples made with comparative polymer compositions, it can be seen that the elasticity of the worsted material is slightly higher than that of the present invention, but due to its thinner thickness, its compressibility is equal to or less than that of the present invention. Therefore, the actual feel and touch of the material, which is soft, thick, and elastic, is equal to or better than that of the material of the present invention.

[0151] Test Method The basis weight of nonwoven fabrics is measured according to the European standard test EN ISO 9073-1:1989 (based on WSP130.1). Ten nonwoven fabric layers are used for the measurement, with a sample area of ​​10 × 10 cm. 2 is.

[0152] The "thickness" or "edge spacing" of nonwoven materials is measured in accordance with European Standard Test EN ISO 9073-2:1995 (based on WSP120.6) with the following modifications: 1. Materials should be measured on samples taken from the production site without being subjected to higher forces and without being left under pressure (e.g. on a product roll) for more than one day; otherwise, the material should be allowed to lie freely on a surface for at least 24 hours before measurement. 2. The total weight of the weighted upper arm of the device is 130g.

[0153] In this specification, the "recovery" of bulkiness after pressure refers to the ratio of the thickness of the dough after the load is released to the original thickness of the dough. The thickness of the dough is measured according to EN ISO 9073-2:1995, applying a preload of 0.5 kPa. The recovery measurement procedure consists of the following steps: 1. Prepare a 10 x 10 cm fabric sample for measurement. 2.Measure the thickness of one piece of fabric. 3. Apply a preload force of 0.5 kPa (Ts) and measure the thickness of the five stacked fabrics. 4. Place the five stacked dough sheets on a thickness gauge (2.5 kPa) for 5 minutes. 5. Release the load and wait 5 minutes. 6. Apply a preload force of 0.5 kPa (Tr) and measure the thickness of the five stacked pieces of fabric. 7. Calculate the recovery rate according to the following formula: Recovery rate = Tr / Ts (unitless) Ts = original sample thickness Tr = thickness of the restored sample

[0154] As used herein, "compressibility" refers to the distance in mm that a nonwoven fabric is compressed by the load defined in the "elasticity" measurement. Compressibility can also be calculated as modulus of elasticity (unitless) x thickness (mm). The "elasticity" of a nonwoven fabric is measured according to European Standard Test EN ISO 964-1, modified as follows: 1. Measure the thickness of one layer of fabric. 2. Prepare a stack of fabric samples with a total thickness of at least 4 mm, and optimally 5 mm. The stack of fabric contains at least one layer of fabric. 3. Measure the thickness of the stacked fabric samples. 4. A force of 5 N is applied to the overlapped nonwoven sample at a loading rate of 5 mm / min. 5.Measure the clamp travel distance. 6. Calculate the elasticity according to the formula: R (unitless) = T1 (mm) / T0 (mm) or R(%) = T1(mm) / T0(mm) x 100% T1 = Clamp travel distance under a 5N load [mm] = Degree of compression of the stacked fabric T0 = ​​thickness (according to EN ISO 9073-2:1995, using a preload force of 1.06 N) [mm].

[0155] The "filament length to fabric length ratio" can be measured in three different ways. a) The length of the filament is measured by stretching it so that it extends along the line without crimping. This method works better the weaker the bond. b) For fabrics bonded to a given level, it is not possible to use method a) to measure the length of the filaments, so the following estimates may be used: a. Take a photograph of the layer being evaluated at a magnification that allows the fibers to be clearly seen. b. Select a single fiber and mark its path through the photograph, or at least a portion of the photograph. c. Measure the length of the fiber marked on the photograph and estimate its actual length. d. Measure the length of the fabric where you marked the fiber. e. Calculate the ratio (percentage) of the estimated filament length to the fabric length for at least 20 fibers. c) In fabrics using the "Method for determining geometric fiber statistics of nonwoven materials": a. Geometric depiction of the analytical fabric measures 8 mm in the MD and 8 mm in the CD, maintaining the full thickness of the sample in the z direction. b. Only fibers entering one side of the cut sample area and exiting the other side are of interest. c. At least 20 filaments must be measured. d. Calculate the ratio (percentage) of filament length to fabric length.

[0156] The "type of fiber cross section" can be determined from the process conditions defined by the fiber forming die. If the process conditions are unknown, the following estimates can be used: A sample of the fabric is taken and photographs of the cross sections of at least 20 fibres are made. The cross sections are taken in the free parts of the fibres, not in adhesive positions or in contact with other fibres where deformation is expected. For each cross section, the surface of the component is marked on the image, separating each component. The centre of mass of each component is determined based on the determination of the centre of gravity or geometric centre of a planar object, and its position is recorded using a Cartesian coordinate system with the geometric centre of the fibre cross section as centre [0;0]. The deflection (D) of the centre of mass of each component in each fibre cross section is calculated according to the following formula: D = absolute value (x × y), where x and y are the coordinates of the center of mass. If one of the values ​​of x and y is 0 and the other is not 0, the sample is excluded from the evaluation. Calculate the mean and standard deviation for each component. A fiber is considered non-crimped if the ratio of ((average deflection) + (standard deviation)) to the total fiber cross-sectional surface is less than 5%. If the ratio of ((average deflection) - (standard deviation)) to the total fiber cross-sectional surface is less than 5%, the fiber is predicted to be non-crimped.

[0157] The "median fiber diameter" within a layer is expressed in SI units - micrometers (μm) or nanometers (nm). To determine the median, samples of the nonwoven fabric must be taken from at least three locations at least 5 cm apart. For each sample, the diameters of at least 50 individual fibers must be measured for each layer observed. For example, an optical microscope or an electron microscope (depending on the fiber diameters measured) can be used. If the fiber diameter of one sample differs significantly from the other two, the entire sample should be discarded and a new one prepared. For circular fibers, the diameter is measured as the diameter of the fiber's cross section. For other fiber shapes (e.g., hollow fibers or trilobal fibers), the surface area of ​​the cross section of each measured fiber is determined and recalculated for a circle with the same surface area. The diameter of this theoretical circle is the fiber diameter. The measurements for each layer of all three samples are compiled into a set of values ​​from which the median is then determined. The set should be such that at least 50% of the fibres have a diameter less than the median and at least 50% of the fibres have a diameter greater than or equal to the median. To determine the median value for a given set of samples, it is sufficient to order the values ​​according to size and take the value in the middle of the list. If the set has an even number of items, the median is usually determined as the arithmetic mean of the values ​​at positions N / 2 and N / 2+1.

[0158] As used herein, the term "void volume" refers to the total amount of void space in a material relative to the volume occupied by the material. The bulk of the material is equal to the bulk of the nonwoven fabric and can be calculated from the fabric thickness (edge ​​spacing) using the following formula: Bulk amount (m 3 )=end face spacing (mm) / 1000×1×1 The total amount of void space in a material can be calculated using the following formula: Void space = bulk (m 3 ) - Massive volume (m 3 ) The total mass volume can be calculated using the following formula: Massive volume (m 3 )=Basic weight (g / m 2 ) / 1000 / mass density (kg / m 3 ) where the mass density can be calculated from known composition or measured according to the standard ISO 1183-3:1999. Therefore, the void volume can be calculated using the following formula: Void content (%) = 1-(Basic weight (g / m 2 )×end distance (mm)) / mass density (kg / m 3 )×100%

[0159] "Method for determining geometric fiber statistics of nonwoven fabrics" This paper describes a software-based method for analyzing nonwoven material samples to characterize their geometric properties. The method uses a machine learning approach to identify the individual fibers present in the sample, followed by a geometric analysis of these fibers to obtain statistics suitable for characterizing the material. The resulting analysis workflow provides fiber orientation and density distribution. This analysis workflow was developed by Math2Market and is part of the GeoDict Digital Teaching Materials Laboratory. Step 1: Obtain a 3D μCT image of the sample First, a μCT scanner digitizes the nonwoven sample to obtain a 3D image. The 3D image consists of a uniform Cartesian grid, with each grid cell (volume element, or voxel) storing the X-ray attenuation of the corresponding part of the sample. Depending on the material and the μCT system configuration, pores typically exhibit the lowest attenuation (smallest grayscale values), while material phases have larger values. Step 2: Cut out the μCT image and separate the material from the pore space For further analysis, the grayscale images are noise-filtered using the Non-Local Means approach [1]. The images are then binarized using a global threshold derived by the Otsu algorithm [2]. After binarization, each image voxel is classified as containing either pores or fiber material. Voxels with gray values ​​below the threshold are classified as pores. All other voxels are classified as fiber material. Both noise filtering and thresholding operations use the ImportGeo module of GeoDict software. Step 3: Analyze the material density distribution Furthermore, the material density distribution in the Z direction is calculated electronically. For each slice of the image (at a given depth Z), the material density is calculated electronically as the number of voxels of white material divided by the total number of voxels in the slice. This analysis is performed using the MatDict module in GeoDict. Step 4: Applying neural networks to identify fiber centerlines A major challenge in identifying individual fibers in μCT images is that fibers are not spatially separated at contact locations after binarization, which leads to undersegmentation, where multiple objects (fibers) are incorrectly classified as a single fiber. To isolate fibers, Math2Market developed an approach that identifies fiber centerline curves. These centerlines are depicted in a binary voxel image of the same size as the original image. In this image, voxels that are within approximately 1-2 voxels of the fiber center are marked. To this end, we use a neural network-based semantic segmentation approach [3]. Images are analyzed by considering 3D sliding input windows that move across the image. For each input window, we define an output window that is smaller than the input window and centered on the input window. The neural network analyzes the binary voxel values ​​of the input window and generates a prediction for each voxel in the output window. The prediction determines whether a voxel in the output window is part of a centerline or not. Combining the results of all these output windows results in a binary image that classifies each material voxel in the original image. This image transformation is performed by GeoDict's FiberFind-AI module using Tensorflow [4]. Step 5: Create training data for the neural network To train a neural network to perform the above transformation, Math2Market creates several artificial 3D images of the nonwoven material using GeoDict's probabilistic FiberGeo structure generation module. This module generates an analytical geometric description of the fibers as a series of line segments. At the same time, this module outputs a binary image of the fiber structure equivalent to the binarization result in step 2. Similarly, by changing the fiber diameter in analytical depiction to about 2-3 voxels, it is possible to obtain a centerline image corresponding to the artificial fiber structure. These paired images (fiber and centerline) are then used to train a neural network to convert fiber images into centerline images. The network effectively learns to "shrink" the fiber down to its centerline curve. Step 6: Trace the fiber centerline to obtain a geometric description of the fiber After shrinking the fibers to their respective centerlines, we assume that the centerlines are not touching each other. Next, we separate the individual centerlines from each other by analyzing the connected components of the centerline image, assuming that each component corresponds to the centerline of one fiber. We define a connected component as the subset of material voxels that are all the same color and that cannot be expanded by adding touching voxels of the same color. For each centerline, we trace a curve across a set of voxels to obtain a geometric description of the corresponding fiber in the form of a series of connected line segments (polylines). This process is also part of Geodict's FiberFind-AI. Step 7: Electronically calculate the fiber orientation distribution histogram To obtain the orientation distribution in any plane (e.g., the XY plane), we first project each fiber segment onto that plane and electronically calculate the angles within the plane. Next, we electronically calculate this orientation histogram across all segment angles. Finally, we visualize this orientation histogram using a polar plot, where the radius at a certain angle is proportional to the frequency of occurrence of the corresponding orientation. This analysis is then repeated for the remaining two planes (XZ and YZ).

[0160] Industrial applicability The present invention can be used wherever a high loft nonwoven fabric with enhanced compressibility and recovery is required - for example, in the hygiene industry as various portions of absorbent hygiene products (e.g., baby diapers, incontinence products, feminine hygiene products, changing pads, etc.), or in healthcare as parts of protective clothing, surgical cover sheets, underlayments, and other barrier material products. Further, industrial applications include, for example, as parts of protective clothing, filtration, thermal insulation, packaging, sound absorption, the shoe industry, automotive, furniture, etc. The present invention can be used advantageously in particular in applications where improved fabric loft, compressibility, and recovery are required in combination with the requirement for endless fibers.

Claims

1. A nonwoven fabric comprising at least one layer containing endless filaments, the nonwoven fabric comprising: - consisting of at least a first polymeric material (A) and a second polymeric material (B) having a lower melting point than the first polymeric material A, - said second polymeric material (B) extends in the longitudinal direction of said filaments and forms at least a part of the surface of said filaments; said filaments have a median fiber diameter of 5 microns or more and 50 microns or less; said first polymeric material (A) consists of or comprises as a major component a polymeric material selected from the group consisting of polyester, polylactic acid, polyester copolymers, polylactic acid copolymers and mixtures thereof; and said second polymeric material (B) consists of or comprises as a major component a polymeric material selected from the group consisting of polyolefins; - said at least one layer of said endless filaments comprises interfilament bonds formed from a second polymeric material (B), all of said filament components are arranged in a non-crimping configuration in which the centers of gravity of each of said filament components are in substantially the same position, including the same, in the cross-section of the filament, and said nonwoven fabric has a structural softness of 80 (m 4 mm 2 g -2 ) or more, and is calculated using the following formula: In the ceremony, - thickness is the thickness of the nonwoven structure, expressed in mm, measured according to the European standard test EN ISO 9073-2: 1995 (based on WSP 120.6) modified as follows:

1. The material should be measured on samples taken from the manufacturing site without being exposed to higher forces and without being left under pressure for more than one day, otherwise the material should be allowed to lie freely on the surface for at least 24 hours before measurement; 2. The total weight of the weighted upper arm of the device is 130g. - basis weight is the basis weight of the nonwoven structure in grams per square meter, measured according to the European standard test EN ISO 9073-1:1989 (based on WSP130.1); the recovery rate is the ratio (Tr) / (Ts), where (Ts) is the initial thickness of the nonwoven structure measured according to the European standard test EN ISO 9073-2: 1995 with a preload of 0.5 kPa and (Tr) is the recovered thickness of the nonwoven structure measured according to the European standard test EN ISO 9073-2: 1995 with a preload of 0.5 kPa after the application and subsequent release of a load of 2.5 kPa; - the compressibility is expressed in mm as the difference between the initial thickness of the nonwoven structure and its thickness when subjected to a load of 5 N, measured according to the European standard test EN ISO 964-1, modified as follows:

1. Measure the thickness of one layer of fabric.

2. Prepare a layered dough sample having a total thickness of at least 4 mm, and preferably 5 mm, the layered dough including at least one dough sheet; 3. Measure the thickness of the stacked fabric samples.

4. Apply a force of 5 N to the stacked nonwoven samples at a loading rate of 5 mm / min.

5. Measure the clamp travel distance.

6. Calculate the elasticity according to the following formula: R (unitless) = T1 (mm) / T0 (mm), or R (%) = T1 (mm) / T0 (mm) x 100%, T1 = Clamp travel distance under a load of 5 N [mm] = degree of compression of the stacked fabric, T0 = ​​thickness (in accordance with EN ISO 9073-2:1995, using a preload force of 1.06 N) [mm] A nonwoven fabric characterized by:

2. The ratio of the filament length to the nonwoven fabric length is greater than 1.2:1, and the proportion of fibers is 20% or more, The nonwoven fabric according to claim 1, characterized in that the ratio is measured by cutting a piece of the nonwoven fabric, measuring 8 mm in the MD and 8 mm in the CD while maintaining the full thickness in the z direction, measuring at least 20 filaments entering from one side of the cut fabric and exiting from the other side, and calculating the ratio between the length of the filament and the length of the cut fabric.

3. The ratio of the filament length to the nonwoven fabric length is greater than 1.5:1, and the proportion of fibers is 10% or more; The nonwoven fabric according to claim 1 or 2, characterized in that the ratio is measured by cutting a piece of the nonwoven fabric, measuring 8 mm in the MD and 8 mm in the CD while maintaining the full thickness in the z direction, measuring at least 20 filaments entering from one side of the cut fabric and exiting on the other side, and calculating the ratio between the length of the filament and the length of the cut fabric.

4. The ratio of the filament length to the fabric length of the nonwoven fabric is less than 2.5:1, and the ratio of the fibers is 10% or more, The nonwoven fabric according to any one of claims 1 to 3, characterized in that the ratio is measured by cutting a piece of the nonwoven fabric at 8 mm in MD and 8 mm in CD while maintaining the overall thickness in the z direction, measuring at least 20 filaments entering from one side of the cut fabric and exiting from the other side, and calculating the ratio between the length of the filament and the length of the cut fabric.

5. The nonwoven fabric according to any one of claims 1 to 4, characterized in that the filaments have a core / sheath structure, the first polymer material (A) forming the core and the second polymer material (B) forming the sheath.

6. The nonwoven fabric according to any one of claims 1 to 5, characterized in that a mass ratio of the first polymer material (A) to the second polymer material (B) is from 50:50 to 90:

10.

7. The nonwoven fabric according to any one of claims 1 to 6, characterized in that the basis weight is at least 5 gsm and at most 200 gsm.

8. The nonwoven fabric according to any one of claims 1 to 7, characterized in that the void volume of said layer is 65% or more.

9. A method for producing a nonwoven fabric, comprising the steps of: a) melting and feeding at least a first polymeric material (A) and a second polymeric material (B) having a melting point lower than that of the first polymeric material (A) to a nozzle of a spinning beam, the first polymeric material (A) being made of or comprising as a main component a polymeric material selected from the group consisting of polyester, polylactic acid, polyester copolymer, polylactic acid copolymer, and mixtures thereof, and the second polymeric material (B) being made of or comprising as a main component a polymeric material selected from the group consisting of polyolefins, the difference between the melting points of the first polymeric material (A) and the second polymeric material (B) being greater than 5°C, the nozzle being configured to form endless filaments in which all components are arranged in a non-crimped configuration in which the centers of gravity of each component of the filament are in substantially the same position in the cross section of the filament, including the same, the second polymeric material (B) extending in the longitudinal direction of the filament and forming at least a portion of the surface of the filament, and the filament spinning speed is in the range of 3000 to 5500 m / min; b) cooling the formed filaments with a fluid medium, which is cooling air at a temperature in the range of 10-90° C. and drawing the filaments at a drawdown ratio in the range of 200-1300 to bring at least the first polymeric material (A) into a metastable crystalline state, the metastable crystalline state being the lowest possible energy state of the first polymeric material (A) that is not crystallized, and the calculated value of the mass flow rate of the cooling air divided by the mass flow rate of the polymer is between 20 and 45; c) laying the filaments onto a forming belt to form a nonwoven filamentary batt; d) heating the nonwoven filamentary batt at a temperature in the range of 80-200° C. by exposing it to air at a temperature of 80-200° C. for a period of 20-5000 ms to activate shrinkage of the nonwoven filamentary batt and convert at least the polymeric material (A) to a more stable crystalline state. The method includes:

10. 10. The method of claim 9, further comprising the step of pre-bonding the nonwoven filamentary batt after step c) and before step d), said pre-bonding being performed by heating the filaments to a temperature in the range of 80-180°C to partially soften said polymeric material (B) and bond said polymeric material (B) between at least some of the mutually crossing filaments.

11. 11. The method according to claim 9 or 10, characterized in that in step b) the filaments are cooled and drawn in a first zone using a fluid medium having a temperature in the range of 10-90°C and then cooled and drawn in a second zone using a fluid medium having a temperature in the range of 10-80°C.

12. 11. The method of claim 10, wherein the air is moved into and / or along the bat at an initial velocity in the range of 0.1 to 2.5 m / s.

13. 12. The method according to claim 9, wherein in step d) the nonwoven filamentary batt is heated such that it shrinks by less than 20% in the machine direction and in the cross direction and increases in thickness by more than 20%.

14. 13. The method according to claim 9, wherein in step d) the nonwoven filamentary batt is heated so that the polymeric material (B) softens and bonds the polymeric material (B) between at least some of the filaments that cross each other.

15. 14. The method according to claim 9, further comprising heating the nonwoven filamentary batt after step d) so that the polymeric material (B) softens and bonds the polymeric material (B) between at least some of the mutually crossing filaments.

16. 16. The method according to claim 15, characterized in that the heating after step d) of bonding the polymeric material (B) is carried out using an Omega drum bonding device, or a flat belt bonding device, or a multi-drum bonding means, and / or by moving air through and / or along the nonwoven filamentary batt for a time of 200-20000 ms, the air temperature being in the range of 100°C to 250°C and the initial velocity being in the range of 0.2-4.0 m / s.

17. 17. The method of any one of claims 9 to 16, wherein the drawdown ratio is in the range of 300 to 800.

18. An absorbent sanitary article comprising a nonwoven fabric according to any one of claims 1 to 8, characterized in that the nonwoven fabric forms at least one of the top sheet, the acquisition and distribution layer, the absorbent core, the back sheet, and the attachment area for mechanical sealing.

19. 20. The absorbent sanitary article of claim 18, wherein said nonwoven fabric forms at least one of said topsheet and said acquisition and distribution layer, said topsheet and said acquisition and distribution layer being bonded to one another.

20. 20. An absorbent sanitary article according to claim 18 or 19, characterized in that the nonwoven forms the topsheet and the acquisition and distribution layer, the topsheet and the acquisition and distribution layer being an integral material.

21. 21. An absorbent sanitary article according to claim 18, 19 or 20, characterized in that the nonwoven fabric forms the core, the pores of the nonwoven fabric being at least partially filled with particles of superabsorbent polymer.

22. 21. The absorbent sanitary article according to any one of claims 18 to 20, characterized in that the nonwoven fabric forms the back sheet and the wearing area, the back sheet and the wearing area being an integral material.

Citation Information

Patent Citations

  • Nonwoven fabric

    JP2014070317A

  • Acoustically absorbing textile composite

    JP2018171907A

  • Molded nonwoven fabric

    JP2018522149A

  • High density nonwoven filter media

    US5855784A

  • Nonwoven fabric of long fibers and absorbent articles made from the same

    WO1998056969A1