Polyamide-cellulose resin composition

A resin composition with polyamide, polyphenylene ether, and cellulose nanofibers addresses the challenges of thermal expansion and water absorption in automobile parts, providing low specific gravity and high rigidity, suitable for large exterior components.

JP7583007B2Active Publication Date: 2024-11-13ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2022173000
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-13
Filing Date
2022-10-28
Publication Date
2024-11-13
Estimated Expiration
2040-10-23

AI Technical Summary

Technical Problem

Existing resin materials, such as polypropylene and polyamide/polyphenylene ether alloys, do not adequately address the need for low specific gravity, high rigidity, low thermal expansion, and low water absorption, which are essential for replacing metal parts in automobile components, particularly in vertical and large exterior parts, due to issues like high thermal expansion, warping, and water absorption.

Method used

A resin composition comprising polyamide as a continuous phase, a second polymer such as polyphenylene ether or a crystalline/amorphous resin forming a dispersed phase, and cellulose nanofibers, with specific ratios and modifications to enhance compatibility and reduce thermal expansion and water absorption.

Benefits of technology

The resin composition achieves a balance of low specific gravity, high rigidity, and low thermal expansion, while minimizing water absorption, making it suitable for large automobile exterior parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583007000013
    Figure 0007583007000013
  • Figure 0007583007000014
    Figure 0007583007000014
  • Figure 0007583007000015
    Figure 0007583007000015
Patent Text Reader

Abstract

The present invention provides a resin composition that achieves a particularly high degree of compatibility between low specific gravity, high rigidity, and low linear expansion coefficient, a resin composition that simultaneously achieves low specific gravity, high rigidity, low thermal expansion coefficient, and low water absorption, or a resin composition that achieves a high degree of compatibility between the contradictory properties of low specific gravity, high toughness, and low thermal expansion. [Solution] In one aspect, a resin composition is provided which includes a first polymer forming a continuous phase, a second polymer forming a dispersed phase, and cellulose, wherein the first polymer is a polyamide, and the second polymer is at least one polymer selected from the group consisting of crystalline resins having a melting point of 60°C or higher and amorphous resins having a glass transition point of 60°C or higher.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition containing polyamide and cellulose. [Background technology]

[0002] Thermoplastic resins are light and have excellent processing properties, and are therefore widely used in many areas, including automotive parts, electrical and electronic parts, office equipment housings, and precision parts. In particular, in the automotive industry, metal parts have long been replaced by resin parts to improve fuel efficiency. In recent years, the shift to electric vehicles has been rapidly promoted in areas such as China and Europe, and the development of electric vehicles has become more active. As a result, reducing the weight of vehicles is becoming an urgent issue in order to extend the driving range of electric vehicles. Replacing metal parts with resin parts is an effective way to reduce the weight of automobiles, and automobile manufacturers are stepping up their efforts in this area, as the use of resin for exterior parts with large volumes in particular contributes greatly to weight reduction.

[0003] Polypropylene-based materials are widely used for plastic exterior parts, mainly bumpers, etc. For fenders, which are vertical parts, the use of polyamide / polyphenylene ether alloy materials as described in Patent Document 1 is being considered in terms of rigidity, heat resistance, etc. Furthermore, in order to further improve dimensional accuracy, Patent Documents 2 and 3, for example, have considered blending inorganic fillers. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2002 / 094936 [Patent Document 2] International Publication No. 2006 / 077818 [Patent Document 3] JP 2006-199748 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, polypropylene-based materials are not suitable for plate-shaped vertical components (door panels, fenders, etc.) because they do not have sufficient room temperature rigidity and high temperature rigidity. In addition, although polyamide / polyphenylene ether-based alloy materials have sufficient rigidity for use in fenders, etc., the alloy materials have the problem of having a high thermal expansion coefficient (approximately 90 ppm / K).

[0006] Automobiles are expected to be driven in a variety of driving environments. For example, the difference in part surface temperature between extreme cold and the desert can be as much as 100°C. In the case of the thermal expansion coefficient of the alloy material, for example, a part with a length of 70 cm will have a dimensional variation of approximately 6 mm. In this case, in order to avoid contact with adjacent parts due to thermal expansion, it becomes necessary to prepare a gap of several millimeters in advance. This is a major challenge for passenger cars, which place importance on design.

[0007] One possible technique for suppressing the thermal expansion coefficient is to incorporate inorganic fillers. However, the materials obtained by this technique have new problems, such as the weight reduction effect achieved by using resin components being lost due to the addition of inorganic fillers with high specific gravity, reduced impact strength, warping or anisotropy in the product, and poor stability of physical properties, and therefore the technology has not yet been widely adopted.

[0008] On the other hand, horizontal parts of an automobile (e.g., bonnet, roof, etc.) are large and require further improvements in thermal expansion and anisotropy, and the reality is that the replacement of metal parts with resin parts has not progressed.

[0009] In recent years, reinforced resins using cellulose such as cellulose nanofibers (CNF) as a filler have been studied. Cellulose-reinforced polyamides, particularly cellulose nanofiber-reinforced polyamides, have the advantages of low specific gravity, high rigidity (especially high rigidity at high temperatures), and low thermal expansion coefficient, but further improvement in these performances is required. In addition, cellulose nanofiber-reinforced polyamides have the problem of high water absorption while having low specific gravity, high rigidity, and low thermal expansion coefficient. High water absorption in cellulose-reinforced resins can cause deterioration of physical properties due to water absorption, deformation of molded bodies due to dimensional changes, etc. That is, at the present time, a material that simultaneously achieves low specific gravity, high rigidity, low thermal expansion coefficient, and low water absorption has not been obtained. In addition, in order to replace metal members with resin members, a resin composition that has low specific gravity while also achieving high toughness and low thermal expansion, which are contradictory properties, is also required, but at the present time, such a resin composition has not been obtained.

[0010] An object of the present invention is to provide a resin composition that solves the above problems and achieves a high degree of compatibility between low specific gravity, high rigidity, and low linear expansion coefficient. Another object of the present invention is to provide a resin composition that simultaneously achieves low specific gravity, high rigidity, low thermal expansion coefficient, and low water absorption. Another object of the present invention is to provide a resin composition that achieves a high degree of compatibility between the contradictory properties of high toughness and low thermal expansion while having a low specific gravity, or while having a low specific gravity and low physical property anisotropy. [Means for solving the problem]

[0011] The present disclosure includes the following aspects. First Embodiment [1] A resin composition comprising a first polymer forming a continuous phase, a second polymer forming a dispersed phase, and cellulose, the first polymer is a polyamide; The second polymer is at least one polymer selected from the group consisting of a crystalline resin having a melting point of 60° C. or higher and a non-crystalline resin having a glass transition point of 60° C. or higher. Resin composition. [2] A resin composition comprising polyamide, polyphenylene ether, and cellulose nanofibers, The resin composition, wherein the polyamide forms a continuous phase and the polyphenylene ether forms a dispersed phase. [3] The resin composition according to aspect 2, wherein the amount of the polyphenylene ether is 30 parts by mass to 150 parts by mass per 100 parts by mass of the polyamide. [4] The resin composition according to aspect 2 or 3, wherein at least a part of the polymer present in the dispersed phase has an acidic functional group. [5] The resin composition according to any one of the above aspects 2 to 4, wherein the polyphenylene ether is present as dispersed particles having a number average particle size of 3 μm or less in a continuous phase of the polyamide. [6] the polyphenylene ether is present as dispersed particles in a continuous phase of the polyamide; The resin composition according to any one of the above-mentioned aspects 2 to 5, wherein the dispersed particles have a volume ratio of particles having a particle diameter of 1 μm or more of 30 volume % or less. [7] The resin composition according to any one of Aspects 2 to 6, further comprising an elastomer. [8] The resin composition according to claim 7, wherein the polyphenylene ether forms a continuous phase and the elastomer forms a dispersed phase within the dispersed phase of the polyphenylene ether. [9] The resin composition according to aspect 7 or 8, wherein the elastomer is at least one selected from the group consisting of an ethylene-α-olefin copolymer, a block copolymer of an aromatic vinyl compound and a conjugated diene compound, and a hydrogenated product of a block copolymer of an aromatic vinyl compound and a conjugated diene compound.

[10] The resin composition according to any one of the above aspects 7 to 9, wherein the elastomer is an acid anhydride-modified elastomer.

[11] The resin composition according to any one of Aspects 7 to 10, wherein the elastomer is a mixture of an elastomer having an acidic functional group and an elastomer not having an acidic functional group.

[12] The resin composition according to any one of Aspects 2 to 11 above, wherein more than 50% by mass of the cellulose nanofibers are present in the polyamide phase.

[13] The resin composition according to any one of aspects 2 to 12 above, wherein the orientation degree of cellulose nanofibers in the center of a multipurpose test piece obtained by molding the resin composition in accordance with ISO 294-1 is 0.45 or less as determined by small-angle X-ray scattering.

[14] The resin composition according to any one of Aspects 2 to 13, wherein the amount of the cellulose nanofibers is 0.1 to 30% by mass, based on 100% by mass of the resin composition.

[15] The resin composition according to any one of Aspects 2 to 14, wherein the cellulose nanofibers are hydrophobized cellulose nanofibers.

[16] The resin composition according to claim 15, wherein the hydrophobized cellulose nanofibers are acetylated cellulose nanofibers.

[17] The resin composition according to any one of aspects 2 to 16, wherein the cellulose nanofibers have a weight average molecular weight (Mw) of 100,000 or more and a ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) of 6 or less.

[18] The resin composition according to any one of Aspects 2 to 17, wherein the cellulose nanofibers have an average alkali-soluble polysaccharide content of 12% by mass or less and a crystallinity of 60% or more.

[19] The resin composition according to any one of Aspects 1 to 18, wherein the polyamide is one or more selected from the group consisting of polyamide 6, polyamide 10, polyamide 11, polyamide 12, polyamide 66, polyamide 610, polyamide 612, polyamide 6 / 6I, polyamide 66 / 6I, polyamide 6I, and mixtures thereof.

[20] The viscosity number (V) of the polyamide when measured in 96% by weight sulfuric acid according to ISO 307 N20. The resin composition according to any one of the above embodiments 1 to 19, wherein the molecular weight of the polymer is 200 or less.

[21] The resin composition according to any one of the above aspects 1 to 20, further comprising a saponified ethylene-vinyl ester copolymer.

[22] The resin composition according to any one of the above aspects 1 to 21, further comprising an antioxidant.

[23] The resin composition according to any one of the above aspects 1 to 22, further comprising a colorant.

[24] The resin composition according to any one of the above aspects 1 to 23, having a thermal expansion coefficient of 50 ppm / K or less at 20° C. to 100° C.

[25] A molded article made of the resin composition according to any one of the above aspects 1 to 24.

[26] An automobile exterior part made of the resin composition according to any one of the above embodiments 1 to 24.

[0012] Second Embodiment [1] Polyamide, One or more elastomers selected from the group consisting of aromatic vinyl compound-conjugated diene compound block copolymers and derivatives thereof, and cellulose, A resin composition comprising: the polyamide and the elastomer are phase-separated, A resin composition, wherein more than 50% by mass of the cellulose is present in the polyamide phase. [2] The resin composition according to claim 1, wherein the polyamide forms a continuous phase and the elastomer forms a dispersed phase. [3] The resin composition according to aspect 1 or 2, wherein the polyamide is at least one selected from the group consisting of polyamide 6, polyamide 10, polyamide 11, polyamide 12, polyamide 66, polyamide 610, polyamide 612, polyamide 6 / 6I, polyamide 66 / 6I, polyamide 6I, and mixtures thereof. [4] Viscosity number (V) of polyamide measured in 96% sulfuric acid according to ISO 307 N 4. The resin composition according to any one of the above embodiments 1 to 3, wherein the molecular weight of the polymer is 200 or less. [5] The resin composition according to any one of the above aspects 1 to 4, wherein the amount of the elastomer is 1 to 50 parts by mass per 100 parts by mass of the polyamide. [6] The resin composition according to any one of the above aspects 1 to 5, wherein the derivative includes an acid-modified product of an aromatic vinyl compound-conjugated diene compound block copolymer. [7] The resin composition according to claim 6, wherein the elastomer is a mixture of a polymer having an acidic functional group and a polymer not having an acidic functional group. [8] The elastomer is present as dispersed particles in a polyamide continuous phase; A resin composition according to any one of the above embodiments 1 to 7, wherein the dispersed particles have a number average particle diameter of 3 μm or less. [9] The elastomer is present as dispersed particles in a polyamide continuous phase; The resin composition according to any one of the above embodiments 1 to 8, wherein the dispersed particles have a volume ratio of particles having a particle size of 1 μm or more of 30 volume % or less.

[10] The resin composition according to any one of the above aspects 1 to 9, wherein the amount of cellulose is 0.1 to 30% by mass, based on 100% by mass of the resin composition.

[11] The resin composition according to any one of the above aspects 1 to 10, wherein the cellulose is a cellulose nanofiber having a diameter of 50 to 1000 nm and a length (L) / diameter (D) ratio of 30 or more, a cellulose nanocrystal having a diameter of 100 nm or less and a length (L) / diameter (D) ratio of less than 30, or a cellulose microfiber having a diameter of more than 1 μm to 50 μm, or a mixture of two or more of these.

[12] The resin composition according to the above embodiment 11, wherein the amount of the cellulose microfibers is 0.1 to 20% by mass, based on 100% by mass of the resin composition.

[13] The resin composition according to any one of the above aspects 1 to 12, wherein the cellulose is a hydrophobized cellulose.

[14] The resin composition according to any one of the above aspects 1 to 13, wherein the hydrophobized cellulose is acetylated cellulose.

[15] The resin composition according to any one of the above aspects 1 to 14, further comprising a conductive carbon-based filler.

[16] The resin composition according to any one of the above aspects 1 to 15, further comprising an antioxidant.

[17] The resin composition according to any one of the above aspects 1 to 16, further comprising a colorant.

[18] The resin composition according to any one of the above aspects 1 to 17, having a thermal expansion coefficient of 60 ppm / K or less at 20° C. to 100° C.

[19] A molded article made of the resin composition according to any one of the above aspects 1 to 18.

[20] An automobile exterior part made of the resin composition according to any one of the above embodiments 1 to 18.

[0013] Third Embodiment [1] Polyamide, Saponified ethylene-vinyl ester copolymers, and cellulose, A resin composition comprising: [2] The resin composition according to the above-mentioned embodiment 1, wherein the amount of the saponified ethylene-vinyl ester copolymer is 1 to 100 parts by mass per 100 parts by mass of the polyamide. [3] The resin composition according to the above-mentioned embodiment 1 or 2, wherein the amount of the saponified ethylene-vinyl ester copolymer is 50 to 5,000 parts by mass per 100 parts by mass of cellulose. [4] The resin composition according to any one of the above aspects 1 to 3, wherein the amount of the cellulose is 0.1 to 30% by mass, based on 100% by mass of the resin composition. [5] The resin composition according to any one of the above aspects 1 to 4, wherein the polyamide forms a continuous phase. [6] The resin composition according to any one of Aspects 1 to 5, wherein the polyamide is at least one selected from the group consisting of polyamide 6, polyamide 10, polyamide 11, polyamide 12, polyamide 66, polyamide 610, polyamide 612, polyamide 6 / 6I, polyamide 66 / 6I, polyamide 6I, and mixtures thereof. [7] The viscosity number (V) of the polyamide when measured in 96% by weight sulfuric acid according to ISO 307 N 7. The resin composition according to any one of the above embodiments 1 to 6, wherein the molecular weight of the polymer is 200 or less. [8] The resin composition according to any one of the above aspects 1 to 7, further comprising an elastomer. [9] The resin composition according to claim 8, wherein the elastomer is at least one selected from the group consisting of an ethylene-α-olefin copolymer, a block copolymer of an aromatic vinyl compound and a conjugated diene compound, and a hydrogenated product of a block copolymer of an aromatic vinyl compound and a conjugated diene compound.

[10] The resin composition according to aspect 8 or 9, wherein the amount of the elastomer is 1 to 50 parts by mass per 100 parts by mass of the polyamide.

[11] The resin composition according to any one of the above aspects 8 to 10, wherein the elastomer is an acid anhydride-modified elastomer.

[12] The resin composition according to any one of Aspects 8 to 11 above, wherein the elastomer is a mixture of a polymer having an acidic functional group and a polymer not having an acidic functional group.

[13] The resin composition according to any one of the above aspects 1 to 12, wherein the ratio of vinyl alcohol units is 60 mol % or more relative to 100 mol % of all monomer units constituting the saponified ethylene-vinyl ester copolymer.

[14] The resin composition according to any one of the above aspects 1 to 13, wherein the cellulose is a cellulose nanofiber having a diameter of 50 to 1000 nm and a length (L) / diameter (D) ratio of 30 or more, a cellulose nanocrystal having a diameter of 100 nm or less and a length (L) / diameter (D) ratio of less than 30, or a cellulose microfiber having a diameter of more than 1 μm to 50 μm, or a mixture of two or more of these.

[15] The resin composition according to claim 14, wherein the amount of the cellulose microfibers is 0.1 to 20% by mass, based on 100% by mass of the resin composition.

[16] The resin composition according to any one of the above aspects 1 to 15, wherein the cellulose is a hydrophobized cellulose.

[17] The resin composition according to claim 16, wherein the hydrophobized cellulose is acetylated cellulose.

[18] The resin composition according to any one of the above aspects 1 to 17, further comprising a polyphenylene ether.

[19] The resin composition according to any one of the above aspects 1 to 18, further comprising an antioxidant.

[20] The resin composition according to any one of the above aspects 1 to 19, further comprising a colorant.

[21] The resin composition according to any one of the above aspects 1 to 20, having a linear thermal expansion coefficient of 70 ppm / K or less at 20° C. to 100° C.

[22] The resin composition according to any one of the above aspects 1 to 21, having a tensile break strain of 10% or more.

[23] A molded article made of the resin composition according to any one of the above aspects 1 to 22.

[24] An automobile exterior part made of the resin composition according to any one of the above embodiments 1 to 22. Effect of the Invention

[0014] According to one aspect of the present invention, it is possible to provide a resin composition which achieves a high degree of compatibility between low specific gravity, high rigidity, and low linear expansion coefficient, and according to another aspect of the present invention, it is possible to provide a resin composition which simultaneously achieves low specific gravity, high rigidity, low thermal expansion coefficient, and low water absorption, and according to another aspect of the present invention, it is possible to provide a resin composition which achieves a high degree of compatibility between the contradictory properties of high toughness and low thermal expansion while having a low specific gravity, or while having a low specific gravity and low physical anisotropy. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a microscopic image showing an example of a cellulose nanofiber. [Diagram 2] FIG. 2 is a microscopic image showing an example of cellulose nanocrystals. [Diagram 3] FIG. 3 is a microscopic image showing an example of cellulose microfibers. [Figure 4] FIG. 4 is an explanatory diagram of a method for calculating the IR index 1730 and the IR index 1030. As shown in FIG. [Diagram 5] FIG. 5 is an explanatory diagram of a method for calculating the average substitution degree of hydroxyl groups in cellulose. [Figure 6]FIG. 6 is a schematic diagram showing the shape of a fender produced for fender evaluation in the examples and comparative examples. [Figure 7] FIG. 7 is a diagram showing positions from which test pieces were taken out for fender evaluation in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, exemplary embodiments of the present invention (hereinafter, abbreviated as "present embodiments") will be described, but the present invention is not limited to these embodiments. Note that, unless otherwise specified, the characteristic values ​​of the present disclosure are values ​​measured by the method described in the [Examples] section of the present disclosure or a method that is understood to be equivalent to the above by a person skilled in the art.

[0017] ≪Resin composition≫ This embodiment includes the following first to third embodiments. The first embodiment includes a first polymer forming a continuous phase, a second polymer forming a dispersed phase (hence a polymer different from the first polymer), and cellulose. In one aspect, the first polymer is a polyamide, and the second polymer is at least one polymer selected from the group consisting of a crystalline resin having a melting point of 60°C or higher and an amorphous resin having a glass transition point of 60°C or higher. In such a resin composition, low specific gravity, high rigidity, and low thermal expansion coefficient can be particularly highly compatible.

[0018] In the present disclosure, in one embodiment, a crystalline resin is a resin that exhibits an endothermic peak due to crystalline melting when heated from 23° C. at a heating rate of 10° C. / min using a differential scanning calorimeter (DSC). In the present disclosure, in one embodiment, an amorphous resin is a resin that does not have an endothermic peak due to crystalline melting when the temperature is increased from 23° C. at a heating rate of 10° C. / min using a differential scanning calorimeter (DSC). In the present disclosure, an elastomer, in one embodiment, is a substance (specifically, a natural or synthetic polymer substance) that is elastic at room temperature (23° C.). In one embodiment, being elastic means that the storage modulus at 23° C. and 10 Hz measured by dynamic viscoelasticity measurement is 1 MPa or more and 100 MPa or less.

[0019] In one aspect of the first embodiment, the resin composition includes polyamide, polyphenylene ether, and cellulose nanofiber. In the resin composition, the polyamide and polyphenylene ether are phase-separated, with the polyamide forming a continuous phase and the polyphenylene ether forming a dispersed phase. With such a phase structure, the high water absorption, which is a drawback of the cellulose nanofiber-reinforced polyamide, is compensated for by the water absorption reducing effect of the polyphenylene ether without impairing various properties inherent to the polyamide (particularly, high heat resistance, low linear expansion coefficient, etc.), and further, the advantages of the polyphenylene ether, such as high rigidity (particularly high rigidity in a high temperature range) and low specific gravity, can be satisfactorily exhibited. Therefore, the resin composition can have a low specific gravity, high rigidity, a low thermal expansion coefficient, and low water absorption.

[0020] In one embodiment, at least a part of the polymer (e.g., polyphenylene ether) present in the dispersed phase has an acidic functional group. The acidic modified group of the dispersed phase, for example, polyphenylene ether, reacts with the amino terminal of the polyamide to moderately improve the compatibility between the continuous phase and the dispersed phase, thereby reducing the dispersion size of the dispersed phase and suppressing interfacial peeling between the continuous phase and the dispersed phase. This is advantageous in that the above-mentioned advantages due to the coexistence of the continuous phase and the dispersed phase are more effectively exhibited. And, cellulose (e.g., cellulose nanofiber) inherently has a higher affinity for polyamide than, for example, polyphenylene ether, so it is mainly present in the polyamide phase. This is considered to be due to hydrogen bonds between cellulose and polyamide. Cellulose (particularly cellulose nanofiber) contributes to the low linear expansion coefficient and high rigidity (particularly high rigidity in a high temperature region) of the resin composition. Thus, according to the resin composition of the first embodiment, a resin composition can be provided in which high rigidity, low thermal expansion coefficient, low specific gravity, and low water absorption are simultaneously achieved while using cellulose (particularly cellulose nanofiber).

[0021] The second embodiment provides a resin composition including one or more elastomers selected from the group consisting of polyamide, aromatic vinyl compound-conjugated diene compound block copolymers and derivatives thereof (hereinafter also referred to as the elastomer of the second embodiment), and cellulose. In one aspect, the polyamide and the elastomer are phase-separated. In one aspect, more than 50 mass% of the cellulose is present in the polyamide phase. In a typical aspect, the resin composition has a two-phase structure of a polyamide phase and an elastomer phase. Although it is not excluded that the resin composition of the second embodiment has three or more phases, this disclosure mainly describes a resin composition related to a two-phase structure of a polyamide phase and an elastomer phase, which is a typical aspect of the second embodiment. The resin composition according to the second embodiment may have high toughness and low linear expansion. In one aspect, the resin composition can have high fluidity that can also be used for the production of large molded bodies, and can further provide a molded body that is substantially free of partial strength defects.

[0022] The phase morphology of the resin composition of the second embodiment may be a morphology in which the polyamide forms a continuous phase and the elastomer forms a dispersed phase, a morphology in which the polyamide forms a dispersed phase and the elastomer forms a continuous phase, or a morphology in which both the polyamide and the elastomer form continuous phases (i.e., a co-continuous phase structure). The morphology in which the polyamide forms a continuous phase and the elastomer forms a dispersed phase is preferred in terms of satisfactorily exhibiting heat resistance as a composition and achieving high rigidity and low linear expansion.

[0023] Generally, cellulose has a high affinity with polyamides because of its hydrophilicity, and may also have an affinity with polymers that are at least partially acid-modified (i.e., at least a portion of which has an acidic functional group). It is also believed that finely divided cellulose may be entangled in highly viscous elastomer components. On the other hand, it is known that cellulose that has been hydrophobized as described below has a lower hydrophilicity, and therefore its location in the resin composition changes depending on the kneading conditions.

[0024] In the first embodiment, the ratio of cellulose (cellulose nanofiber in a specific embodiment) present in the polyamide phase among the cellulose (cellulose nanofiber in a specific embodiment) in the resin composition, and in the second embodiment, the ratio of cellulose present in the polyamide phase among the cellulose in the resin composition, each have a lower limit of preferably more than 50% by mass, more preferably 60% by mass, more preferably 70% by mass, even more preferably 75% by mass, even more preferably 80% by mass, and most preferably 100% by mass (i.e., substantially all of the cellulose is present in the polyamide phase). When the ratio is within the above-mentioned range, in the first embodiment, low thermal expansion and high rigidity can be more highly compatible, or in the second embodiment, various contradictory properties such as low thermal expansion, low anisotropy, and high toughness can be compatible. The upper limit of the ratio may be, for example, 99% by mass or 98% by mass from the viewpoint of ease of production of the resin composition.

[0025] As an example of a method for confirming that more than 50% by mass of the cellulose in the resin composition in the first embodiment (cellulose nanofiber in a specific embodiment) and the cellulose in the resin composition in the second embodiment are present in the polyamide phase, for example, the resin composition is photographed with a transmission electron microscope, and the area of ​​the cellulose present in the polyamide phase and the area of ​​the cellulose present in the other phase (for example, the polyphenylene ether in the first embodiment or the elastomer phase in the second embodiment) are confirmed. The above method is useful, for example, when the abundance ratio of cellulose is significantly different between the polyamide phase and the other phase and quantification is not required. On the other hand, when quantification is required, the resin composition is sliced ​​to a thickness of about 0.1 to 2 μm to obtain a film-like sample. The sample is immersed in a solvent (for example, chloroform, toluene, etc.) that dissolves the components of the other phase (for example, the polyphenylene ether component or the elastomer component) but does not dissolve the polyamide to elute the other phase, and the eluate is concentrated and then ultracentrifuged to separate the cellulose present in the other phase, and then washed with the solvent at least three times, dried, and the amount of cellulose present in the other phase is measured.

[0026] The third embodiment provides a resin composition containing polyamide, a saponified ethylene-vinyl ester copolymer, and cellulose. The resin composition according to the third embodiment can have a low linear thermal expansion coefficient even when molded into a large molded product, for example, because the cellulose is stably finely dispersed in the polyamide phase. In addition, the resin composition can have a high tensile break strain (i.e., high toughness) due to the contribution of the saponified ethylene-vinyl ester copolymer. The resin composition according to this embodiment has the above-mentioned excellent properties and can therefore be suitably used for various molded articles, particularly various large parts (for example, automobile exterior parts, etc.).

[0027] Next, each component that can be used in this embodiment will be described in detail.

[0028] <First polymer (polyamide)> The polyamide used in the first to third embodiments includes polycondensates of dibasic acid and diamine, ring-opening polymers of cyclic lactam, polycondensates of aminocarboxylic acid, and copolymers and blends thereof. More specifically, aliphatic polyamides such as polyamide 6, polyamide 10, polyamide 11, polyamide 12, polyamide 46, polyamide 66, polyamide 610, and polyamide 612, aromatic polyamide resins such as polymetaxylene adipamide (polyamide MXD6), polyhexamethylene terephthalamide (polyamide 6T), and polyhexamethylene isophthalamide (polyamide 6I), and copolymers and blends such as polyamide 6 / 6I, polyamide 66 / 6I, polyamide 6 / 6T, polyamide 66 / 6T, polyamide 6 / 66 / 6T, polyamide 6 / 66 / 6I, polyamide 9T, and polyamide 10T can be used. Among these, polyamide 6, polyamide 10, polyamide 11, polyamide 12, polyamide 66, polyamide 610, polyamide 612, polyamide 6 / 6I, polyamide 66 / 6I, polyamide 6I, and mixtures thereof are particularly preferred, and polyamide 6, polyamide 66, polyamide 610, polyamide 612, polyamide 6I, and mixtures thereof are most preferred.

[0029] In the first to third embodiments, the terminal carboxyl group concentration of the polyamide is not particularly limited, but the lower limit is preferably 5 μmol / g, 10 μmol / g, 20 μmol / g, 25 μmol / g, or 30 μmol / g. The upper limit of the terminal carboxyl group concentration is preferably 150 μmol / g, 100 μmol / g, or 80 μmol / g.

[0030] In the first to third embodiments, the terminal amino group concentration of the polyamide is not particularly limited, but the lower limit is preferably 20 μmol / g or 30 μmol / g, and the upper limit is preferably 150 μmol / g, 100 μmol / g, or 80 μmol / g.

[0031] In the polyamides of the first to third embodiments, the carboxyl end group ratio to the total end groups ([COOH] / [total end groups]) is preferably 0.20 to 0.95. The lower limit of the carboxyl end group ratio is more preferably 0.3, more preferably 0.35, even more preferably 0.40, and most preferably 0.45. The upper limit of the carboxyl end group ratio is more preferably 0.90, even more preferably 0.85, and most preferably 0.80. The carboxyl end group ratio is preferably 0.20 or more from the viewpoint of dispersibility of cellulose in the resin composition, and is preferably 0.95 or less from the viewpoint of the color tone of the resulting resin composition.

[0032] The terminal group concentration of the polyamide can be adjusted by a known method, for example, by adding a terminal regulator that reacts with the terminal group, such as a diamine compound, a monoamine compound, a dicarboxylic acid compound, a monocarboxylic acid compound, an acid anhydride, a monoisocyanate, a monoacid halide, a monoester, or a monoalcohol, to the polymerization solution so that the terminal group concentration is a predetermined value during polymerization of the polyamide.

[0033] Examples of the terminal regulator that reacts with the terminal amino group include aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid; alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid; aromatic monocarboxylic acids such as benzoic acid, toluic acid, α-naphthalenecarboxylic acid, β-naphthalenecarboxylic acid, methylnaphthalenecarboxylic acid, and phenylacetic acid; and mixtures of a plurality of terminal regulators selected from the above. Among these, from the viewpoints of reactivity, stability of the blocked terminal, and cost, one or more terminal regulators selected from the group consisting of acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, and benzoic acid are preferred, and acetic acid is most preferred.

[0034] Examples of the terminal regulator that reacts with the terminal carboxyl group include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, etc., alicyclic monoamines such as cyclohexylamine, dicyclohexylamine, etc., aromatic monoamines such as aniline, toluidine, diphenylamine, naphthylamine, etc., and any mixtures thereof. Among these, one or more terminal regulators selected from the group consisting of butylamine, hexylamine, octylamine, decylamine, stearylamine, cyclohexylamine, and aniline are preferred in terms of reactivity, boiling point, stability of the blocked terminal, cost, etc.

[0035] The concentrations of these amino end groups and carboxyl end groups are as follows: 1 From the viewpoints of accuracy and simplicity, it is preferable to determine the concentration of each end group from the integral value of the characteristic signal corresponding to each end group by H-NMR. As a method for determining the concentration of these end groups, the method described in JP-A-7-228775 is specifically recommended. When using this method, deuterated trifluoroacetic acid is useful as a measurement solvent. 1 The number of H-NMR scans must be at least 300, even when an instrument with sufficient resolution is used. Alternatively, the concentration of the terminal group can be measured by a titration method as described in JP-A-2003-055549. However, in order to minimize the influence of additives, lubricants, etc., 1 Quantitation by H-NMR is more preferred.

[0036] The degree of polymerization of the polyamide is not particularly limited, but from the viewpoint of ordinary injection molding processability, the viscosity number (V) of the polyamide measured in sulfuric acid with a concentration of 96% by mass in accordance with ISO307 is preferably 1.0 or more. N) is preferably 200 or less. A more preferred upper limit is 180, even more preferred is 150, even more preferred is 140, and most preferred is 130. By keeping it within the above range, it is possible to maintain the flowability during molding of the molded product at an appropriate level and reduce molding distortion, thereby suppressing the anisotropy of the actual molded product. The lower limit of the viscosity number is not particularly limited, but is preferably 50, more preferably 60, more preferably 65, and most preferably 70, from the viewpoint of obtaining good impact resistance.

[0037] The polyamide in the present embodiment may be a mixture of multiple different types of polyamides. When multiple types of polyamides are used as a mixture, the various characteristic values ​​of the polyamide may be average values ​​of the multiple types.

[0038] The method for polymerizing the polyamide is not particularly limited, and may be any of melt polymerization, interfacial polymerization, solution polymerization, bulk polymerization, solid-phase polymerization, and combinations thereof. Among these, melt polymerization is more preferably used from the viewpoint of polymerization controllability.

[0039] In addition, for the purpose of improving the heat resistance stability of the polyamide resin, known metal stabilizers such as those described in JP-A-1-163262 may be used. Particularly preferred examples of metal stabilizers include CuI, CuCl2, copper acetate, and cerium stearate. In addition, alkali metal halide salts such as potassium iodide and potassium bromide can also be suitably used. Of course, these may be added in combination. The preferred blending amount of the metal stabilizer and / or alkali metal halide salt is 0.001 to 5 parts by mass in total relative to 100 parts by mass of polyamide. From the viewpoint of heat aging resistance, it is preferable that the blending amount is not less than the lower limit, and from the viewpoint of maintaining high toughness, it is preferable that the blending amount is not more than the upper limit.

[0040] Furthermore, in addition to the above, known additives that can be added to polyamides may be added in an amount of, for example, less than 10 parts by mass per 100 parts by mass of polyamide.

[0041] In the first to third embodiments, the ratio of polyamide to 100 mass% of the resin composition is preferably 30 mass% or more, or 35 mass% or more, or 40 mass% or more, from the viewpoint of obtaining advantages such as high heat resistance and low linear expansion coefficient due to the polyamide phase, and is preferably 90 mass% or less, or 80 mass% or less, or 70 mass% or less, or 60 mass% or less, from the viewpoint of obtaining advantages due to other components in the resin composition.

[0042] <Second Polymer> In one embodiment, the resin composition includes a second polymer in addition to a polyamide as a first polymer. The second polymer is a polymer different from the first polymer. In one embodiment, the second polymer is at least one polymer selected from the group consisting of a crystalline resin having a melting point of 60° C. or higher and an amorphous resin having a glass transition point of 60° C. or higher.

[0043] Examples of the crystalline resin include crystalline polyolefin resins such as polyethylene and polypropylene, crystalline polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polylactic acid, and polybutylene succinate, crystalline polyacetal resins such as polyoxymethylene, and saponified ethylene-vinyl ester copolymers. Among these, saponified ethylene-vinyl ester copolymers are preferred in terms of achieving high toughness. The crystalline resin may be, for example, the saponified ethylene-vinyl ester copolymer of the third embodiment.

[0044] The melting point of the crystalline resin is 60° C. or higher in one embodiment, preferably 100° C. or higher, or 150° C. or higher, or 180° C. or higher, and preferably 350° C. or lower, or 300° C. or lower, or 280° C. or lower. In the present disclosure, the melting point means the peak top temperature of an endothermic peak that appears when the temperature is increased from 23° C. at a rate of 10° C. / min using a differential scanning calorimeter (DSC). When two or more endothermic peaks appear, the melting point refers to the peak top temperature of the lowest temperature peak.

[0045] Examples of the amorphous resin include amorphous polyolefin resins such as polymethylene pentene and cyclic polyolefin, amorphous polyvinyl resins such as polystyrene and polyvinyl chloride, polycarbonate resins, polyacrylic resins, polyarylate resins, polysulfone resins, polyphenylene ether resins, polyphenylene sulfide resins, polyether sulfone resins, polyketone resins, polyphenylene ether ketone resins, and polyimide resins. Among these, polyphenylene ether resins are preferred in terms of achieving low specific gravity and high rigidity. The amorphous resin may be, for example, the polyphenylene ether of the first embodiment.

[0046] The glass transition point of the amorphous resin is 60° C. or higher in one embodiment, preferably 100° C. or higher, or 150° C. or higher, or 180° C. or higher, and preferably 350° C. or lower, or 300° C. or lower, or 280° C. or lower. In the present disclosure, the glass transition point means the peak top temperature at which the storage modulus is greatly reduced and the loss modulus is maximized when measured using a dynamic viscoelasticity measuring device while increasing the temperature at a rate of 2° C. / min from -100° C. and applying a frequency of 10 Hz. When two or more peaks of the loss modulus appear, the peak top temperature refers to the peak top temperature of the lowest temperature peak.

[0047] In one embodiment, the amount of the second polymer relative to 100 parts by mass of the first polymer, polyamide, is, from the viewpoint of obtaining the advantages of the resin other than polyamide, preferably 1 part by mass or more, or 5 parts by mass or more, or 10 parts by mass or more, and from the viewpoint of obtaining the advantages inherent to the polyamide, in one embodiment, is 100 parts by mass or less, and preferably 80 parts by mass or less, or 60 parts by mass or less, or 40 parts by mass or less.

[0048] <Polyphenylene Ether of First Embodiment> In one aspect of the first embodiment, the resin composition includes polyphenylene ether. In the second and third embodiments, the resin composition may further include polyphenylene ether. The polyphenylene ether is represented by the following general formula (1): [ka] (In formula (1), R 1 , R 2 , R 3 , and R 4 are each independently a monovalent group selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 7 carbon atoms, a phenyl group, a haloalkyl group, an aminoalkyl group, a hydrocarbyloxy group, or a halohydrocarbyloxy group in which at least two carbon atoms separate the halogen atom from the oxygen atom, and n is an integer of 20 or more. It has a structure represented by the following formula:

[0049] In the above formula (1), R 1 , R 2 , R 3 , and R 4 Examples of the halogen atom represented by the formula (I) include a fluorine atom, a chlorine atom, a bromine atom, etc., and a chlorine atom and a bromine atom are preferred.

[0050] In the above formula (1), R 1 , R 2 , R 3 , and R 4 The "alkyl group" represented by the formula (I) represents a linear or branched alkyl group having preferably 1 to 6 carbon atoms, more preferably 1 to 3 carbon atoms, and examples thereof include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, etc. Methyl and ethyl are preferred, and methyl is more preferred.

[0051] In the above formula (1), R 1 , R 2 , R 3 , and R 4The alkyl group represented by the formula (I) may be substituted with one or more substituents at substitutable positions. Examples of such substituents include halogen atoms (e.g., fluorine atoms, chlorine atoms, bromine atoms), alkyl groups having 1 to 6 carbon atoms (e.g., methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl), aryl groups (e.g., phenyl, naphthyl), alkenyl groups (e.g., ethenyl, 1-propenyl, 2-propenyl), alkynyl groups (e.g., ethynyl, 1-propynyl, 2-propynyl), aralkyl groups (e.g., benzyl, phenethyl), alkoxy groups (e.g., methoxy, ethoxy), and the like.

[0052] In the above formula (1), n ​​may be 20 or more, or 100 or more, or 200 or more, and may be 2000 or less, or 1000 or less, or 400 or less.

[0053] The polyphenylene ether is not particularly limited, and known ones may be used. For example, poly(2,6-dimethyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), poly(2,6-dichloro-1,4-phenylene ether), etc. may be mentioned, and further, polyphenylene ether copolymers such as 2,6-dimethylphenol and other phenols (e.g., 2,3,6-trimethylphenol or 2-methyl-6-butylphenol) may also be used. Among the above, poly(2,6-dimethyl-1,4-phenylene ether) and copolymers of 2,6-dimethylphenol and 2,3,6-trimethylphenol are preferred, and poly(2,6-dimethyl-1,4-phenylene ether) is more preferred. These polyphenylene ethers may be used alone or in combination of two or more kinds.

[0054] The intrinsic viscosity [η] of the polyphenylene ether is preferably 0.1 dl / g or more, or 0.2 dl / g or more, or 0.3 dl / g or more from the viewpoint of obtaining a resin composition with high rigidity, and is preferably 1.0 dl / g or less, or 0.7 dl / g or less, or 0.6 dl / g or less, or 0.5 dl / g or less from the viewpoint of imparting good fluidity to the resin composition. The intrinsic viscosity is a value measured in chloroform at 25°C.

[0055] In one embodiment, the polyphenylene ether is present in the dispersed phase, and at least a portion of the polyphenylene ether may be acid-modified by reacting the polyphenylene ether with a modifying agent (e.g., α,β-unsaturated carboxylic acid and its derivatives, etc.).

[0056] Examples of α,β-unsaturated carboxylic acids include monobasic acids such as (meth)acrylic acid, crotonic acid, isocrotonic acid, furan acid, pentenoic acid, vinylacetic acid, and angelic acid; dibasic acids such as maleic acid, chloromaleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, and endo-cis-bicyclo[2,2,1]hept-5-ene-2,3-dicarboxylic acid (nadic acid); and tribasic acids such as citric acid and aconitic acid.

[0057] Examples of the derivatives of α,β-unsaturated carboxylic acids include acid halides, amides, imides, acid anhydrides, and esters of the above-mentioned α,β-unsaturated carboxylic acids. For example, malenyl chloride, acrylamide, maleimide, N-phenylmaleimide, N-methylmaleimide, N-ethylmaleimide, maleic anhydride, itaconic anhydride, glutaconic anhydride, citraconic anhydride, nadic anhydride, aconic anhydride, methyl (meth)acrylate, monomethyl maleate, dimethyl maleate, diethyl itaconate, dibutyl citraconate, glycidyl (meth)acrylate, and diglycidyl maleate. Among these, examples of preferred modifiers include maleic acid, citric acid, itaconic acid, itaconic anhydride, and maleic anhydride, and more preferably, citric acid and maleic anhydride.

[0058] The degree of acid modification of polyphenylene ether is preferably 0.01% or more, or 0.1% or more, or 0.2% or more, or 0.25% or more from the viewpoint of obtaining the advantages of the combined use of polyamide and polyphenylene ether by dispersing polyphenylene ether in the polyamide phase with a relatively small dispersion size, and is preferably 10% or less, or 5% or less, or 2% or less, or 1% or less, or 0.7% or less, or 0.6% or less from the viewpoint of obtaining the advantages of high rigidity and low water absorption by using polyphenylene ether. The polyphenylene ether of the present disclosure may be a mixture of two or more polymers having different acid modification degrees. In this case, it is preferable that the degree of acid modification of the entire polyphenylene ether in the resin composition is within the above range. The above acid modification degree is an addition rate calculated from infrared spectroscopy measurement. When the acid functional group is derived from maleic anhydride, a mixture of polyphenylene ether and maleic anhydride is used to obtain the 1790 cm -1 After preparing a calibration curve for the peak at 1790 cm for maleic anhydride-modified polyphenylene ether, -1 The addition rate is calculated from the peak intensity.

[0059] Examples of the method for modifying polyphenylene ether with an acid include a method of reacting a modifier with polyphenylene ether in a fluid state (for example, by melting, or dispersing or dissolving in a solvent), a method of reacting a modifier with powdered polyphenylene ether in the presence of a modifier at a temperature below the glass transition point of polyphenylene ether, etc. Examples of the method for reacting a modifier with polyphenylene ether in a fluid state include a method of melt-kneading polyphenylene ether and a modifier at 250°C to 350°C for 5 seconds to 30 minutes using a roll mill, Banbury mixer, extruder, etc., and a method of dissolving polyphenylene ether in an organic solvent (for example, toluene, xylene, decalin, tetralin, etc.), adding a modifier, and heating. An example of a method for reacting a modifier with powdered polyphenylene ether is a method in which predetermined amounts of polyphenylene ether and modifier are charged into a stirring device capable of high-speed stirring, and the temperature of the contents is maintained at 160°C to 200°C for at least 30 seconds or more by the shear heat generated by high-speed stirring and / or heat transfer from the jacket.

[0060] The reaction may be carried out in the presence of a radical initiator. Examples of the radical initiator include organic peroxides (benzoyl peroxide, dicumyl peroxide, di-tert-butyl peroxide, tert-butylcumyl peroxide, cumene hydroperoxide, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3, etc.) and azo compounds (azobisisobutylnitrile, dimethylazoisobutyrate, etc.). The amount of the radical initiator used may be, for example, 0.01 to 10 parts by mass relative to 100 parts by mass of polyphenylene ether.

[0061] In one embodiment, the polyphenylene ether may be a mixture of polyphenylene ether having an acidic functional group and polyphenylene ether not having an acidic functional group. The mixing ratio of the polyphenylene ether having an acidic functional group and the polyphenylene ether not having an acidic functional group, when the total of both is 100 mass%, is preferably 10 mass% or more, more preferably 20 mass% or more, even more preferably 30 mass% or more, and most preferably 40 mass% or more, from the viewpoint of obtaining the advantages of high rigidity and low water absorption of the resin composition and from the viewpoint of increasing affinity with cellulose nanofibers. The upper limit is not particularly limited, and substantially all of the polyphenylene ether may be polyphenylene ether having an acidic functional group, but from the viewpoint of not causing problems in fluidity when melted, it is desirable to be 80 mass% or less.

[0062] The phase containing polyphenylene ether may form a particulate dispersed phase (dispersed particles) in the resin composition. In this case, the dispersed particle diameter is preferably 3 μm or less, more preferably 2 μm or less, and most preferably 1 μm or less, as a number average particle diameter. The lower limit is not particularly limited, but is, for example, 0.01 μm. From the viewpoint of high toughness and physical property stability, it is preferable to set it within the above-mentioned range.

[0063] The phase containing polyphenylene ether preferably has a high uniformity of the dispersed particle diameter. From this viewpoint, the volume ratio of dispersed particles having a particle diameter of 1 μm or more to the total dispersed particles of polyphenylene ether is preferably 30% by volume or less. The upper limit is more preferably 25% by volume, even more preferably 20% by volume, even more preferably 15% by volume, and most preferably 10% by volume. In the volume-based dispersed particle diameter distribution, even if there are only a few coarse particles, the volume ratio of dispersed particles having a particle diameter of 1 μm or more is suddenly expressed as being large. When the volume ratio is within the above range, the uniformity of the dispersed particle diameter is high, which is preferable. From the viewpoint of ease of production of the resin composition, the volume ratio may be, for example, 2% by volume or more, or 5% by volume or more.

[0064] Methods for increasing the uniformity of the dispersed particle size of the phase containing polyphenylene ether include a method in which the components of the resin composition are extrusion-kneaded to produce a resin composition, and the polyphenylene ether is finely dispersed by imparting high shear strain to the components by increasing the screw rotation speed during extrusion kneading; a method in which extensional flow strain is imparted to the components by arranging screw parts having uniformly spaced narrow clearances, such as a seal ring; and a method in which a molten polymer is passed through a special narrow slit and extensional flow strain is imparted at the slit. Any of these methods may be used, but since the method of imparting high shear causes a significant rise in the polymer temperature during processing, the method using extensional flow strain is more preferable.

[0065] The method of observing the dispersion form includes a method of cutting a resin composition in the form of a molded body, pellets, etc. into ultrathin slices, staining the polyamide phase with phosphotungstic acid, etc., and observing it with a transmission electron microscope, a method of uniformly polishing the surface of a resin composition in the form of a molded body, pellets, etc., immersing it in a solvent that selectively dissolves only polyphenylene ether, extracting the polyphenylene ether, and observing it with a scanning electron microscope, etc. The obtained image is binarized with an image analyzer, and the diameters of the dispersed particles (at least 500 randomly selected) of the dispersed phase are calculated as the circle equivalent diameter, and the particle diameters of each particle are counted, so that the number average particle diameter of the dispersed particles and the volume ratio of particles having a predetermined particle diameter (for example, the above-mentioned particle diameter of 1 μm or more) can be calculated.

[0066] In the first embodiment, the ratio of polyphenylene ether to 100 mass% of the resin composition is preferably 10 mass% or more, or 20 mass% or more, or 30 mass% or more, from the viewpoint of obtaining the advantages of high rigidity, low specific gravity, and low water absorption due to the polyphenylene ether phase, and is preferably 60 mass% or less, or 50 mass% or less, or 40 mass% or less, from the viewpoint of obtaining the advantages of other components in the resin composition.

[0067] In addition, the amount of polyphenylene ether per 100 parts by mass of polyamide is preferably 30 parts by mass or more, or 40 parts by mass or more, or 50 parts by mass or more, from the viewpoint of obtaining the above-mentioned advantages of the polyphenylene ether phase well, and is preferably 150 parts by mass or less, or 120 parts by mass or less, or 100 parts by mass or less, from the viewpoint of facilitating the existence of the polyphenylene ether phase as a dispersed phase in the polyamide phase.

[0068] <Elastomer of the First Embodiment> In the first embodiment, the resin composition may have an elastomer phase in addition to the first and second polymers, and in one aspect, may have an elastomer phase in addition to the polyamide phase and the polyphenylene ether phase. The elastomer constituting the elastomer phase is a material (specifically, a natural or synthetic polymer material) that is elastic at room temperature (23°C). When the elastomer phase is further present, the toughness and elongation (especially elongation in a low temperature environment) of the resin composition become good, which is preferable.

[0069] In one aspect of the first embodiment, the resin composition has a polyamide phase (continuous phase) and a polyphenylene ether phase (dispersed phase). When an elastomer is further used, the elastomer inherently has a higher affinity for polyphenylene ether than polyamide, so that the elastomer phase can be distributed in the polyphenylene ether phase (i.e., the polyphenylene ether phase is the continuous phase and the elastomer phase is the dispersed phase). That is, in the resin composition further containing an elastomer, the polyphenylene phase is dispersed in the polyamide phase with a relatively small size, and the elastomer phase is further dispersed in the polyphenylene phase. To obtain such a dispersed form, for example, a polyamide, a polyphenylene ether having an acidic functional group, and an elastomer not having an acidic functional group can be used.

[0070] Also, an elastomer phase may be dispersed in a polyamide phase, and a first polymer phase or a polyphenylene ether phase may be distributed in the elastomer phase. To obtain such a dispersed form, for example, a polyamide, a polyphenylene ether having no acidic functional group, and an elastomer having an acidic functional group may be used.

[0071] Also, the second polymer phase or polyphenylene ether phase and the elastomer phase can be separately distributed in the polyamide phase. To obtain such a dispersion form, for example, a polyamide, a second polymer having an acidic functional group or a polyphenylene ether having an acidic functional group, and an elastomer having an acidic functional group can be used.

[0072] Even when an elastomer phase is further present, the preferred example of the dispersion size of the polyphenylene ether phase may be the same as described above. The elastomer phase may be present as dispersed particles in the polyphenylene ether phase, or may be present as dispersed particles in the polyamide phase. In this case, the preferred dispersed particle size is preferably 3 μm or less, more preferably 2 μm or less, and most preferably 1 μm or less, as the number average particle size. The lower limit is not particularly limited, but is, for example, 0.01 μm. From the viewpoint of exhibiting good toughness and elongation, it is preferable to set it within the above-mentioned range.

[0073] In the elastomer, it is preferable that the uniformity of the dispersed particle size is high. From this viewpoint, it is preferable that the volume ratio of dispersed particles having a particle size of 3 μm or more to the total dispersed particles of the elastomer is 30 volume % or less. The upper limit is more preferably 25 volume %, further preferably 20 volume %, further more preferably 15 volume %, and most preferably 10 volume %. From the viewpoint of ease of production of the resin composition, the above volume ratio may be, for example, 2 volume % or more, or 5 volume % or more. As a method for increasing the uniformity of the dispersed particle size of the elastomer, a method of producing a resin composition by extrusion kneading the blending components of the resin composition, and finely dispersing the elastomer by applying high shear strain to the blending components by increasing the screw rotation speed during extrusion kneading can be mentioned.

[0074] Specific examples of the elastomer include natural rubber, conjugated diene compound polymers, aromatic compound-conjugated diene copolymers, hydrogenated aromatic compound-conjugated diene copolymers, polyolefins, polyester-based elastomers, polyurethane-based elastomers, polyamide-based elastomers, and elastomers having a core-shell structure. In one embodiment, the elastomer is a different type of polymer from polyamide (i.e., not a polyamide elastomer). Among these, from the viewpoint of ease of the modification reaction of the acidic functional group described below, aromatic compound-conjugated diene copolymers and hydrogenated products thereof, polyolefins, and elastomers having a core-shell structure are preferred. As the aromatic compound-conjugated diene copolymers and hydrogenated products thereof, aromatic compound-conjugated diene block copolymers and hydrogenated products thereof are more preferred, and as the polyolefins, copolymers of ethylene and α-olefins are more preferred.

[0075] In one embodiment, the elastomer is at least one selected from the group consisting of an ethylene-α-olefin copolymer, a block copolymer of an aromatic vinyl compound and a conjugated diene compound, and a hydrogenated product of a block copolymer of an aromatic vinyl compound and a conjugated diene compound.

[0076] In the present disclosure, the aromatic compound-conjugated diene block copolymer is a block copolymer composed of a polymer block (A) mainly made of an aromatic vinyl compound and a polymer block (B) mainly made of a conjugated diene compound. From the viewpoint of impact strength expression, a block copolymer in which the bonding type of each block is AB type, ABA type, or ABAB type is preferable, and an ABA type or ABAB type is more preferable.

[0077] The mass ratio of the aromatic vinyl compound unit to the conjugated diene compound unit in the block copolymer is preferably 10 / 90 to 70 / 30. More preferably, it is 15 / 85 to 55 / 45, and most preferably 20 / 80 to 45 / 55. Furthermore, these may be blended with two or more different mass ratios of the aromatic vinyl compound to the conjugated diene compound. Specific examples of the aromatic vinyl compound include styrene, α-methylstyrene, vinyltoluene, etc., and one or more compounds selected from these are used, among which styrene is particularly preferred.

[0078] Specific examples of the conjugated diene compound include butadiene, isoprene, piperylene, 1,3-pentadiene, etc., and one or more compounds selected from these are used, but among these, butadiene, isoprene, and combinations thereof are preferred, and butadiene is particularly preferred. When butadiene is used as the conjugated diene compound of the block copolymer, the microstructure of the polybutadiene block portion preferably has a 1,2-vinyl content or a total amount of the 1,2-vinyl content and the 3,4-vinyl content of 5 to 80% on a molar basis, more preferably 10 to 50%, and most preferably 15 to 40%, from the viewpoint of suppressing crystallization of the soft segment.

[0079] The aromatic compound-conjugated diene block copolymer is a block copolymer composed of a polymer block mainly made of an aromatic vinyl compound and a polymer block mainly made of a conjugated diene compound, and is a block copolymer that has not been subjected to a hydrogenation treatment. The hydrogenated product of the block copolymer of an aromatic vinyl compound and a conjugated diene compound refers to a block copolymer of an aromatic vinyl compound and a conjugated diene compound, which is hydrogenated to control the aliphatic double bonds of the polymer block mainly made of a diene compound in the range of more than 0% to 100%. From the viewpoint of suppressing thermal deterioration during processing, the hydrogenation rate of the hydrogenated product of the block copolymer is preferably 50% or more, more preferably 80% or more, and most preferably 98% or more, and from the viewpoint of low temperature toughness, it is preferably 50% or less, more preferably 20% or less, and most preferably 0% (i.e., a block copolymer of an aromatic vinyl compound and a conjugated diene compound).

[0080] In addition, the molecular weight of each of the block copolymer of an aromatic vinyl compound and a conjugated diene compound and its hydrogenated product is preferably a number average molecular weight (Mn) of 10,000 to 500,000, and most preferably 40,000 to 250,000, from the viewpoint of achieving both impact strength and fluidity. In the present disclosure, the number average molecular weight is a value measured using a gel permeation chromatography device, chloroform as a solvent, at a measurement temperature of 40°C, and converted into polystyrene standard, unless otherwise specified.

[0081] These aromatic vinyl compound-conjugated diene compound block copolymers may be used in a mixture of two or more types of copolymers having different bond types, different molecular weights, different aromatic vinyl compound types, different conjugated diene compound types, different 1,2-vinyl contents or the total amount of 1,2-vinyl content and 3,4-vinyl content, different aromatic vinyl compound component contents, different hydrogenation rates, etc. In a mixture of copolymers having different hydrogenation rates, the preferred hydrogenation rate of the mixture is as described above.

[0082] As the polyolefin, from the viewpoint of impact resistance, an ethylene-α-olefin copolymer can be suitably used. Examples of monomers that can be copolymerized with ethylene units include aliphatic substituted vinyl monomers such as propylene, butene-1, pentene-1, 4-methylpentene-1, hexene-1, heptene-1, octene-1, nonene-1, decene-1, undecene-1, dodecene-1, tridecene-1, tetradecene-1, pentadecene-1, hexadecene-1, heptadecene-1, octadecene-1, nonadecene-1, or eicosene-1, isobutylene, and aromatic vinyl monomers such as styrene and substituted styrene, ester vinyl monomers such as vinyl acetate, acrylic acid esters, methacrylic acid esters, glycidyl acrylic acid esters, glycidyl methacrylic acid esters, and hydroxyethyl methacrylic acid esters, acrylamide, allylamine, vinyl-p-aminobenzene, and nitrogen-containing vinyl monomers such as acrylonitrile, and dienes such as butadiene, cyclopentadiene, 1,4-hexadiene, and isoprene.

[0083] Preferably, it is a copolymer of ethylene and one or more α-olefins having 3 to 20 carbon atoms, more preferably a copolymer of ethylene and one or more α-olefins having 3 to 16 carbon atoms, and most preferably a copolymer of ethylene and one or more α-olefins having 3 to 12 carbon atoms. From the viewpoint of impact resistance, the molecular weight of the ethylene-α-olefin copolymer is preferably 10,000 or more, more preferably 10,000 to 100,000, and even more preferably 20,000 to 60,000, as measured by a gel permeation chromatography measuring device using 1,2,4-trichlorobenzene as a solvent at 140°C and using polystyrene standards. From the viewpoint of impact resistance, the molecular weight distribution (weight average molecular weight / number average molecular weight: Mw / Mn) is preferably 3 or less, and even more preferably 1.8 to 2.7.

[0084] Moreover, the preferred content of ethylene units in the ethylene-α-olefin copolymer is 30 to 95% by mass based on the total amount of the ethylene-α-olefin copolymer, from the viewpoint of ease of handling during processing.

[0085] These preferred ethylene-α-olefin copolymers can be produced, for example, by the production methods described in JP-B-4-12283, JP-A-60-35006, JP-A-60-35007, JP-A-60-35008, JP-A-5-155930, JP-A-3-163088, and U.S. Pat. No. 5,272,236.

[0086] In the present disclosure, the elastomer having a core-shell structure includes a core-shell type elastomer having a core that is a particulate rubber and a shell that is a glassy graft layer formed on the outside of the core. As the rubber component as the core, butadiene rubber, acrylic rubber, silicone-acrylic composite rubber, etc. can be suitably used. As the shell, a glassy polymer such as styrene resin, acrylonitrile-styrene copolymer, acrylic resin, etc. can be suitably used. Among these, from the viewpoint of compatibility with polyamide, an elastomer having a core-shell structure having a butadiene rubber core and an acrylic resin shell can be suitably used.

[0087] In one embodiment, at least a part of the elastomer has an acidic functional group. In this disclosure, the term "an elastomer has an acidic functional group" means that the acidic functional group is added to the molecular skeleton of the elastomer via a chemical bond. In this disclosure, the term "acidic functional group" means a functional group capable of reacting with a basic functional group, and specific examples thereof include a hydroxyl group, a carboxyl group, a carboxylate group, a sulfo group, and an acid anhydride group.

[0088] From the viewpoint of compatibility with a second polymer having an acidic functional group or a polyphenylene ether having an acidic functional group, the amount of acidic functional groups added in the elastomer is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 0.2% by mass or more, and preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less, based on 100% by mass of the elastomer. The number of acidic functional groups is a value obtained by measuring a calibration curve sample in which an acidic substance is mixed in advance with an infrared absorption spectrometer, and measuring the sample based on a calibration curve prepared using the characteristic absorption band of the acid.

[0089] Examples of elastomers having an acidic functional group include elastomers having a core-shell structure having a shell layer formed using acrylic acid or the like as a copolymerization component, and elastomers which are modified products obtained by grafting an α,β-unsaturated dicarboxylic acid or a derivative thereof to an ethylene-α-olefin copolymer, polyolefin, aromatic compound-conjugated diene copolymer, or a hydrogenated aromatic compound-conjugated diene copolymer containing acrylic acid or the like as a monomer, in the presence or absence of a peroxide.

[0090] In a preferred embodiment, the elastomer is an anhydride modified elastomer.

[0091] Among these, modified products obtained by grafting an α,β-unsaturated dicarboxylic acid or a derivative thereof onto a polyolefin, an aromatic compound-conjugated diene copolymer, or a hydrogenated aromatic compound-conjugated diene copolymer in the presence or absence of a peroxide are more preferred, and among these, modified products obtained by grafting an α,β-unsaturated dicarboxylic acid or a derivative thereof onto an ethylene-α-olefin copolymer, or a hydrogenated aromatic compound-conjugated diene block copolymer in the presence or absence of a peroxide are particularly preferred.

[0092] Specific examples of the α,β-unsaturated dicarboxylic acid and its derivatives include maleic acid, fumaric acid, maleic anhydride, and fumaric anhydride, with maleic anhydride being particularly preferred.

[0093] In one embodiment, the elastomer may be a mixture of an elastomer having an acidic functional group and an elastomer not having an acidic functional group. When the total of the elastomer having an acidic functional group and the elastomer not having an acidic functional group is 100% by mass, the mixing ratio of the elastomer having an acidic functional group is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and most preferably 40% by mass or more, from the viewpoint of maintaining high toughness and physical property stability of the resin composition. There is no particular upper limit, and substantially all of the elastomer may be an elastomer having an acidic functional group, but from the viewpoint of not causing problems in flowability, it is desirable to have 80% by mass or less.

[0094] In the first embodiment, when an elastomer phase is further present, the ratio of the elastomer to 100 mass% of the resin composition is preferably 3 mass% or more, or 5 mass% or more, or 8 mass% or more, from the viewpoint of favorably improving the toughness and elongation of the resin composition, and is preferably 40 mass% or less, or 30 mass% or less, or 10 mass% or less, from the viewpoint of increasing the rigidity and decreasing the thermal expansion coefficient of the resin composition.

[0095] When the elastomer phase is further present, the amount of elastomer per 100 parts by mass of the total of the polyamide and the second polymer or polyphenylene ether is, from the viewpoint of favorably improving the toughness and elongation of the resin composition, preferably 1 part by mass or more, or 2 parts by mass or more, or 3 parts by mass or more, or 4 parts by mass or more, or 5 parts by mass or more, and from the viewpoint of increasing the rigidity and decreasing the thermal expansion coefficient of the resin composition, preferably 50 parts by mass or less, or 40 parts by mass or less, or 35 parts by mass or less, or 30 parts by mass or less, or 25 parts by mass or less.

[0096] When the elastomer phase is further present, the amount of elastomer per 100 parts by mass of the second polymer or polyphenylene ether is preferably 10 parts by mass or more, or 15 parts by mass or more, or 20 parts by mass or more, from the viewpoint of favorably improving the toughness and elongation of the resin composition, and is preferably 100 parts by mass or less, or 80 parts by mass or less, or 70 parts by mass or less, or 50 parts by mass or less, or 40 parts by mass or less, from the viewpoint of easily causing the elastomer phase to exist as a dispersed phase in the second polymer phase or polyphenylene ether phase.

[0097] <Elastomer of the second embodiment> In a second embodiment, the resin composition contains an aromatic compound-conjugated diene compound block copolymer (i.e., a block copolymer composed of a polymer block (A) mainly composed of an aromatic vinyl compound and a polymer block (B) mainly composed of a conjugated diene compound) and / or an elastomer which is a derivative thereof (i.e., a substance which is an elastic body at room temperature (23°C) (specifically, a natural or synthetic polymer substance)). A block copolymer in which the bonding type of each block is any of AB type, ABA type, and ABAB type is preferred from the viewpoint of impact strength expression, and more preferably, the ABA type or ABAB type. In addition, the derivative of an aromatic compound-conjugated diene compound block copolymer means a polymer which has a different structure due to modification, hydrogenation, or the like while retaining the main structure of the block copolymer, and in one embodiment, it is a modified product (e.g., an acid modified product, etc.) and / or a hydrogenated product of an aromatic compound-conjugated diene compound block copolymer.

[0098] Suitable examples of the structure of the block copolymer, and the structures of the aromatic vinyl compound unit and the conjugated diene compound unit in the block copolymer and the mass ratio thereof may be the same as those described for the block copolymer in the first embodiment.

[0099] In the resin composition according to the second embodiment, it was unexpectedly found that the aromatic vinyl compound-conjugated diene compound block copolymer and / or the elastomer which is a derivative thereof can impart high toughness and low thermal expansion coefficient to the resin composition. Although not wishing to be bound by theory, it is believed that the aromatic vinyl compound-conjugated diene compound block copolymer and its derivatives have low molecular mobility because the molecules can be crosslinked by the double bonds in the molecules. In the resin composition including the combination of polyamide and elastomer, the elastomer forms domains and contributes to improving toughness, while it is more likely to thermally expand than polyamide, and therefore is a factor in increasing the thermal expansion of the resin composition. However, according to the elastomer of the second embodiment, it is believed that the thermal expansion of the resin composition can be suppressed low due to the crosslinking of the elastomer molecules as described above. In this way, the resin composition including the elastomer of the second embodiment can unexpectedly have the contradictory properties of high toughness and low thermal expansion to a high degree.

[0100] In addition, when the elastomer contains an acid-modified product, the formation of crosslinks between the molecules as described above also contributes to suppressing the reaction between cellulose and acidic functional groups. In this case, there is an advantage that the increase in the thermal expansion coefficient of the resin composition due to the adhesion of the elastomer to the cellulose (i.e., the decrease in the effect of reducing the thermal expansion coefficient due to the difficulty of making the cellulose exist mainly in the polyamide phase) is unlikely to occur.

[0101] The number average molecular weight (Mn) of each of the aromatic vinyl compound-conjugated diene compound block copolymer and its derivative is preferably from 10,000 to 500,000, and more preferably from 40,000 to 250,000, from the viewpoint of achieving both impact strength and fluidity.

[0102] In one embodiment, the derivative of the aromatic vinyl compound-conjugated diene compound block copolymer includes an acid-modified product of the block copolymer. In one embodiment, the acidic functional group of the present disclosure is added to the molecular skeleton of the block copolymer via a chemical bond.

[0103] The acid-modified product may be a product obtained by grafting an α,β-unsaturated dicarboxylic acid or a derivative thereof to an aromatic vinyl compound-conjugated diene compound block copolymer or a hydrogenated product thereof in the presence or absence of a peroxide. In a preferred embodiment, the acid-modified product is an acid anhydride-modified product. Specific examples of the α,β-unsaturated dicarboxylic acid and its derivatives include maleic acid, fumaric acid, maleic anhydride, and fumaric anhydride, and among these, maleic anhydride is particularly preferred.

[0104] The elastomer may be a mixture of a polymer having an acidic functional group and a polymer not having an acidic functional group, or may be composed of a polymer having an acidic functional group. When the total of the polymer having an acidic functional group (acid-modified product) and the polymer not having an acidic functional group (non-acid-modified product) is taken as 100% by mass, the ratio of the acid-modified product is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and most preferably 40% by mass or more, from the viewpoint of obtaining a good toughness improving effect by the elastomer of the second embodiment. The upper limit of the ratio of the acid-modified product is not particularly limited, and the elastomer of the second embodiment may be substantially composed of only the acid-modified product, but from the viewpoint of not causing a problem in the flowability of the resin composition, it is desirable to have the ratio of 80% by mass or less.

[0105] From the viewpoint of compatibility with polyamide, the amount of acidic functional groups in the acid-modified product is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 0.2% by mass or more, and preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 2% by mass or less. The number of acidic functional groups is a value obtained by measuring a calibration curve sample in which an acidic substance is mixed in advance with an infrared absorption spectrometer, and measuring the sample based on a calibration curve prepared using the characteristic absorption band of the acid.

[0106] In one aspect, the amount of acidic functional groups relative to 100% by mass of the total amount of the elastomer of the second embodiment is preferably within the range exemplified above as the amount of acidic functional groups in the acid-modified product.

[0107] In the resin composition, the amount of elastomer relative to 100 parts by mass of polyamide is preferably within the range of 1 to 50 parts by mass. The upper limit is more preferably 40 parts by mass, more preferably 35 parts by mass, even more preferably 30 parts by mass, and most preferably 25 parts by mass. In order to maintain good rigidity and heat resistance of the resin composition, it is desirable to set the amount below the above upper limit. The lower limit is more preferably 2 parts by mass, even more preferably 3 parts by mass, even more preferably 4 parts by mass, and most preferably 5 parts by mass. In order to increase the toughness and physical property stability of the resin composition, it is preferable to set the amount above the above lower limit.

[0108] When the elastomer phase forms a particulate dispersed phase (dispersed particles) in the resin composition, the dispersed particle diameter is preferably within the same range as the elastomer phase of the first embodiment, from the viewpoint of high toughness and physical property stability.

[0109] It is preferable that the elastomer has a high uniformity of the dispersed particle diameter. From this viewpoint, it is preferable that the volume ratio of dispersed particles having a particle diameter of 1 μm or more to the total dispersed particles of the elastomer is 30 volume % or less. The upper limit is more preferably 25 volume %, further preferably 20 volume %, even more preferably 15 volume %, and most preferably 10 volume %. In the volume-based dispersed particle diameter distribution, even if there are only a few coarse particles, the volume ratio of dispersed particles having a particle diameter of 1 μm or more is suddenly expressed as being large. When the above volume ratio is within the above range, the uniformity of the dispersed particle diameter is high, which is preferable. From the viewpoint of ease of production of the resin composition, the above volume ratio may be, for example, 2 volume % or more, or 5 volume % or more.

[0110] A method for improving the uniformity of the dispersed particle size of the elastomer includes producing a resin composition by extrusion kneading the blended components of the resin composition, and increasing the screw rotation speed during extrusion kneading to apply high shear strain to the blended components, thereby finely dispersing the elastomer.

[0111] Methods for observing the dispersion form include cutting a resin composition in the form of a molded body, pellets, etc. into ultrathin slices, staining the polyamide phase with phosphotungstic acid, etc., and observing with a transmission electron microscope, and a method for uniformly leveling the surface of a resin composition in the form of a molded body, pellets, etc., immersing it in a solvent that selectively dissolves only the elastomer, extracting the elastomer, and observing with a scanning electron microscope. The obtained image is binarized with an image analyzer, and the diameters of the dispersed particles (at least 500 randomly selected) in the dispersed phase are calculated as the equivalent circle diameter, and the particle diameters of each particle are counted, so that the number average particle diameter of the dispersed particles and the volume ratio of particles with a predetermined particle diameter (for example, the above-mentioned particle diameter of 1 μm or more) can be calculated.

[0112] In the second embodiment, the resin composition may further contain an elastomer component other than the aromatic vinyl compound-conjugated diene compound block copolymer and / or a derivative thereof, as long as the advantages of the present invention are not impaired.

[0113] <Saponified ethylene-vinyl ester copolymer according to the third embodiment> In the third embodiment, the resin composition includes a saponified ethylene-vinyl ester copolymer. In the first and second embodiments, the resin composition may further include a saponified ethylene-vinyl ester copolymer. The saponified ethylene-vinyl ester copolymer has excellent strength and dimensional stability, and has a hydroxyl group and excellent affinity with polyamide and cellulose, which can impart a high breaking strain (i.e., excellent toughness) to a resin composition containing polyamide and cellulose. The saponified ethylene-vinyl ester copolymer is also advantageous in that it does not impair the advantages brought about by cellulose, that is, the advantages of low specific gravity and excellent reduction effect of the linear thermal expansion coefficient and physical property anisotropy of the resin composition. Therefore, the resin composition of the third embodiment can have a unique advantage of achieving a high degree of compatibility between the contradictory properties of high toughness and low thermal expansion.

[0114] The saponified ethylene-vinyl ester copolymer is a compound obtained by adding an alkaline salt to a copolymer obtained by copolymerizing ethylene and a vinyl ester to saponify the copolymer, and contains ethylene units and vinyl alcohol units. The saponified ethylene-vinyl ester copolymer may contain vinyl ester units as non-saponified sites, but in a typical embodiment, it is substantially free of vinyl ester units.

[0115] In 100 mol% of all monomer units constituting the saponified ethylene-vinyl ester copolymer, the ratio of vinyl alcohol units (specifically, structural units generated by saponification of vinyl ester units) is, from the viewpoint of obtaining a good effect of improving the breaking strain of the resin composition, preferably 60 mol% or more, or 65 mol% or more, or 70 mol% or more, or 74 mol% or more, or 76 mol% or more, and, from the viewpoint of containing a suitable amount of ethylene units in the saponified ethylene-vinyl ester copolymer, it is preferably 95 mol% or less, or 90 mol% or less, or 80 mol% or less.

[0116] The ratio of ethylene units in 100 mol% of all monomer units constituting the saponified ethylene-vinyl ester copolymer is preferably 5 mol% or more, or 10 mol% or more, or 20 mol% or more from the viewpoints of processability, water absorbency, etc. during the production of the resin composition, and is preferably 40 mol% or less, or 35 mol% or less, or 30 mol% or less, or 26 mol% or less, or 24 mol% or less from the viewpoint of obtaining a good effect of improving the breaking strain of the resin composition.

[0117] In the 100 mol% of all monomer units in the saponified ethylene-vinyl ester copolymer, the ratio of vinyl ester units (specifically, units that are not saponified during saponification after copolymerization of ethylene and vinyl ester) is preferably 20 mol% or less, 10 mol% or less, 5 mol% or less, or 1 mol% or less, from the viewpoint of obtaining the advantages of the saponified ethylene-vinyl ester copolymer. The ratio is ideally 0 mol%, but from the viewpoint of ease of production of the saponified ethylene-vinyl ester copolymer, it may be, for example, 0.01 mol% or more, 0.1 mol% or more, or 0.5 mol% or more.

[0118] The saponification degree of the saponified ethylene-vinyl ester copolymer is preferably 90 mol% or more, or 95 mol% or more, or 99 mol% or more from the viewpoint of improving the breaking strain of the resin composition. From the viewpoint of ease of production of the saponified ethylene-vinyl ester copolymer, the saponification degree may be, for example, 99.99 mol% or less, or 99.9 mol% or less, or 99.5 mol% or less. The saponification degree is calculated as the number of vinyl alcohol units in the saponified ethylene-vinyl ester copolymer divided by the total number of vinyl alcohol units and vinyl ester units.

[0119] The amount of each structural unit in the saponified ethylene-vinyl ester copolymer can be confirmed by a nuclear magnetic resonance (NMR) method.

[0120] The saponified ethylene-vinyl ester copolymer may contain additional structural units in addition to the ethylene unit, the vinyl alcohol unit and the vinyl ester unit, as long as the effect of the present invention is not impaired. Examples of the additional structural units include olefins such as propylene, 1-butene, and isobutene; hydroxyl-containing α-olefins such as 2-propen-1-ol, 3-buten-1-ol, 4-penten-1-ol, 5-hexen-1-ol, 3,4-dihydroxy-1-butene, and 5-hexen-1,2-diol; acylated or esterified products thereof; and the like. Examples of the esterified products include 3,4-diacyloxy-1-butene, particularly 3,4-diacetoxy-1-butene.Further, hydroxyalkyl vinylidenes such as 2-methylenepropane-1,3-diol and 3-methylenepentane-1,5-diol; hydroxyalkyl vinylidene diacetates such as 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane and 1,3-dibutyronyloxy-2-methylenepropane; unsaturated acids or salts thereof such as acrylic acid, methacrylic acid, crotonic acid, (anhydrous) phthalic acid, (anhydrous) maleic acid, (anhydrous) itaconic acid, and the like, and mono- or dialkyl esters having 1 to 18 carbon atoms; acrylamide, N-alkylacrylamide having 1 to 18 carbon atoms, N,N-dimethylacrylamide, 2-acrylamidopropanesulfonic acid or salts thereof, acrylamidopropyldimethylamine or its acid salt or its quaternary salt; methacrylamide, N-alkylmethacrylamide having 1 to 18 carbon atoms, N,N-dimethylmethacrylamide, Examples of the vinyl silanes include acrylamide, 2-methacrylamidopropanesulfonic acid or a salt thereof; methacrylamidepropyldimethylamine, its acid salt or its quaternary salt; N-vinylamides such as N-vinylpyrrolidone, N-vinylformamide, N-vinylacetamide, etc.; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl ethers such as alkyl vinyl ethers, hydroxyalkyl vinyl ethers, alkoxyalkyl vinyl ethers having 1 to 18 carbon atoms; vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, vinyl bromide, etc.; vinyl silanes such as trimethoxyvinylsilane; allyl acetate, allyl chloride, trimethyl-(3-acrylamido-3-dimethylpropyl)-ammonium chloride, acrylamido-2-methylpropanesulfonic acid, vinyl ethylene carbonate, glycerin monoallyl ether, etc. In 100 mol % of all monomer units constituting the saponified ethylene-vinyl ester copolymer, the molar ratio of the additional structural unit is preferably 20 mol % or less, 15 mol % or less, or 10 mol % or less. The molar ratio may be, for example, 1 mol % or more, 3 mol % or more, or 5 mol % or more.

[0121] The method for producing the saponified ethylene-vinyl ester copolymer is not limited, and the ethylene monomer and the vinyl ester monomer may be radically polymerized by a known polymerization method (for example, solution polymerization method), and then saponified by a known saponification method.

[0122] Examples of vinyl ester monomers include aliphatic vinyl esters and aromatic vinyl esters. Specific preferred examples of vinyl esters include vinyl acetate, vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl versatate, and vinyl benzoate.

[0123] For the saponification, for example, at least one alkaline salt selected from the group consisting of sodium hydroxide and potassium hydroxide can be used.

[0124] The saponified ethylene-vinyl ester copolymer may be a commercially available product, such as Soarnol V2504 (ethylene ratio 25 mol%), Soarnol DT2904 (ethylene ratio 29 mol%), Soarnol DC3212 (ethylene ratio 32 mol%) (all available from Mitsubishi Chemical Holdings Corporation), EVAL M100B (ethylene ratio 24 mol%), EVAL L104B (ethylene ratio 27 mol%), EVAL C109B (ethylene ratio = 35 mol%) (all available from Kuraray Co., Ltd.).

[0125] In the resin composition, the amount of the saponified ethylene-vinyl ester copolymer per 100 parts by mass of polyamide is, from the viewpoint of obtaining a good effect of improving the breaking strain, preferably 1 part by mass or more, or 5 parts by mass or more, or 10 parts by mass or more, or 20 parts by mass or more, or 30 parts by mass or more, and from the viewpoint of toughness, preferably 100 parts by mass or less, or 80 parts by mass or less, or 60 parts by mass or less, or 50 parts by mass or less, or 40 parts by mass or less.

[0126] The phase morphology of the resin composition may be such that the polyamide forms a continuous phase and the saponified ethylene-vinyl ester copolymer forms a dispersed phase, such that the polyamide forms a dispersed phase and the saponified ethylene-vinyl ester copolymer forms a continuous phase, or such that both the polyamide and the saponified ethylene-vinyl ester copolymer form continuous phases (i.e., a co-continuous phase structure). The form in which the polyamide forms a continuous phase and the saponified ethylene-vinyl ester copolymer forms a dispersed phase is preferred in terms of favorable heat resistance and high toughness of the composition.

[0127] In the resin composition, the amount of the saponified ethylene-vinyl ester copolymer per 100 parts by mass of cellulose is, from the viewpoint of obtaining a good effect of improving breaking strain, preferably 50 parts by mass or more, or 100 parts by mass or more, or 200 parts by mass or more, or 300 parts by mass or more, and from the viewpoints of molding processability and cost, preferably 5,000 parts by mass or less, or 1,000 parts by mass or less, or 700 parts by mass or less, or 500 parts by mass or less.

[0128] <Elastomer of the third embodiment> In the third embodiment, the resin composition may further include an elastomer. When the resin composition includes an elastomer, the phase form of the resin composition may be a form in which the polyamide forms a continuous phase and the elastomer forms a dispersed phase, a form in which the polyamide forms a dispersed phase and the elastomer forms a continuous phase, or a form in which both the polyamide and the elastomer form a continuous phase (i.e., a bicontinuous phase structure), but the form in which the polyamide forms a continuous phase and the elastomer forms a dispersed phase is preferred in terms of exhibiting good heat resistance as a composition and achieving high rigidity and low linear expansion.

[0129] The lower limit of the ratio of cellulose present in a phase other than the elastomer phase is preferably more than 50% by mass, or 60% by mass or more, or 70% by mass or more, or 75% by mass or more, or 80% by mass or more, or 100% by mass (i.e., substantially all of the cellulose is present in the polyamide phase) from the viewpoint of simultaneously and highly achieving the contradictory properties of low thermal expansion, low anisotropy, and high toughness. The above ratio may be, for example, 99% by mass or less, or 98% by mass or less from the viewpoint of ease of production of the resin composition.

[0130] As an example of a method for confirming that more than 50% by mass of cellulose is present in a phase other than the elastomer phase, for example, when the ratio of cellulose present in the phase other than the elastomer phase is significantly different from that in the elastomer phase, it can be easily confirmed by photographing the resin composition with a transmission electron microscope and confirming the amount of cellulose present in the phase other than the elastomer phase and the amount of cellulose present in the elastomer phase without the need for quantification. If quantification is required, the resin composition is sliced ​​to a thickness of about 0.1 to 2 μm to obtain a film-like sample. The sample is immersed in a solvent (e.g., chloroform, toluene, etc.) that dissolves elastomer components but does not dissolve components other than the elastomer phase to elute the elastomer phase, and the eluate is concentrated and then ultracentrifuged to separate the cellulose present in the elastomer phase, followed by washing with the solvent at least three times, drying, and measuring the amount of cellulose present in the elastomer phase.

[0131] In addition, methods for observing the phase morphology of a resin composition include a method of cutting a resin composition in the form of a molded body, pellets, etc. into ultrathin slices, staining the polyamide phase with phosphotungstic acid, etc., and then observing with a transmission electron microscope, a method of uniformly leveling the surface of a resin composition in the form of a molded body, pellets, etc., immersing it in a solvent that selectively dissolves only the elastomer, extracting the elastomer, and observing with a scanning electron microscope, etc. The size of the dispersed phase (for example, dispersed particles described later) can be determined by binarizing the obtained image with an image analyzer, calculating the diameters of at least 500 randomly selected particles as the circle equivalent diameter, and counting the particle diameters of each particle.

[0132] The elastomer contributes to further improving the toughness of the resin composition. The molecular structure, various properties (molecular weight, etc.) and preferred examples of the usage mode (blending amount, etc.) of the elastomer may be the same as those exemplified as the elastomers of the first and second embodiments, and the aromatic compound-conjugated diene copolymer and its hydrogenated product exemplified in the first embodiment, polyolefin, and elastomer having a core-shell structure are preferred. As the aromatic compound-conjugated diene copolymer and its hydrogenated product exemplified in the first embodiment, the aromatic compound-conjugated diene block copolymer and its hydrogenated product exemplified in the first embodiment are more preferred, and as the polyolefin, a copolymer of ethylene and α-olefin is more preferred.

[0133] The elastomer preferably has an acidic functional group at least in a part thereof. Specific examples of the elastomer having an acidic functional group may be the same as those exemplified in the first and second embodiments. The amount of the acidic functional group added in the elastomer may be the same as those exemplified in the first and second embodiments from the viewpoint of compatibility with the polyamide.

[0134] For example, the amount of elastomer in the resin composition relative to 100 parts by mass of polyamide is preferably 1 part by mass or more, or 2 parts by mass or more, or 3 parts by mass or more, or 4 parts by mass or more, or 5 parts by mass or more from the viewpoint of improving the toughness and physical property stability of the resin composition, and is preferably 50 parts by mass or less, or 40 parts by mass or less, or 35 parts by mass or less, or 30 parts by mass or less, or 25 parts by mass or less from the viewpoint of improving the rigidity and heat resistance of the resin composition.

[0135] The elastomer may form a particulate dispersed phase (dispersed particles) in the resin composition. In this case, the dispersed particle size may be the same as that of the elastomer of the first and second embodiments from the viewpoint of obtaining a favorable effect of improving the toughness and physical property stability of the resin composition by the elastomer and from the viewpoint of ease of production of the resin composition.

[0136] It is preferable that the dispersed particle size of the elastomer is highly uniform in order to obtain a good effect of improving the properties of the resin composition. The preferred volume ratio of dispersed particles having a particle size of 1 μm or more in the total dispersed particles of the elastomer and the method for adjusting the same may be the same as those of the elastomer of the second embodiment.

[0137] It is believed that the aromatic vinyl compound-conjugated diene compound block copolymer and its hydrogenated product have low molecular mobility because the molecules can be crosslinked by the double bonds in the molecule. In a resin composition containing a combination of a polyamide and an elastomer, the elastomer forms domains and contributes to improving toughness, while it is more susceptible to thermal expansion than polyamide, which increases the thermal expansion of the resin composition. However, it is believed that the aromatic vinyl compound-conjugated diene compound block copolymer and its hydrogenated product can suppress the thermal expansion of the resin composition to a low level due to the crosslinking of the elastomer molecules. Such an elastomer is advantageous in achieving both high toughness and low linear thermal expansion.

[0138] In addition, when the elastomer contains an acid-modified product, the formation of crosslinks between the molecules as described above also contributes to suppressing the reaction between cellulose and acidic functional groups. In this case, there is also an advantage that the increase in the linear thermal expansion coefficient of the resin composition due to the adhesion of the elastomer to the cellulose (i.e., the decrease in the effect of reducing the thermal expansion coefficient due to the difficulty of making the cellulose exist mainly in the polyamide phase) is unlikely to occur.

[0139] <Cellulose> [Cellulose of the first embodiment] In a first embodiment, the resin composition contains cellulose. In one embodiment, the cellulose contains fibrous cellulose, and in one embodiment, the cellulose is fibrous cellulose. In one embodiment, the cellulose contains cellulose nanofiber, and in one embodiment, the cellulose is nanofiber. Examples of raw materials for cellulose include natural cellulose and regenerated cellulose. As natural cellulose, wood pulp obtained from wood species (broadleaf or coniferous trees), non-wood pulp obtained from non-wood species (bamboo, hemp-based fiber, bagasse, kenaf, linter, etc.), and refined pulp thereof (refined linter, etc.) can be used. As non-wood pulp, cotton-derived pulp including cotton linter pulp, hemp-derived pulp, bagasse-derived pulp, kenaf-derived pulp, bamboo-derived pulp, straw-derived pulp, etc. can be used. Cotton-derived pulp, hemp-derived pulp, bagasse-derived pulp, kenaf-derived pulp, bamboo-derived pulp, and straw-derived pulp each include cellulose made from purified pulp obtained from raw materials such as cotton lint, cotton linter, hemp-based abaca (e.g., from Ecuador or the Philippines), zaisal, bagasse, kenaf, bamboo, straw, etc., through a refining process such as delignification by cooking treatment, a bleaching process, etc.

[0140] For example, cellulose nanofibers can be obtained by treating the above-mentioned pulp with hot water of 100° C. or higher to hydrolyze and weaken the hemicellulose portion, and then defibrating the pulp by a pulverization method using a high-pressure homogenizer, microfluidizer, ball mill, disk mill, etc. In one embodiment, the diameter of the cellulose nanofiber is 2 to 1000 nm, preferably 4 nm or more, or 5 nm or more, or 10 nm or more, or 15 nm or more, or 20 nm or more, or 50 nm or more, or 100 nm or more, and preferably 500 nm or less, or 450 nm or less, or 400 nm or less, or 350 nm or less, or 300 nm or less, or 250 nm or less, or 200 nm or less.

[0141] In the first embodiment, the length, diameter, and L / D ratio of each cellulose are determined by diluting an aqueous dispersion of cellulose with a water-soluble solvent (e.g., water, ethanol, tert-butanol, etc.) to 0.01 to 0.1% by mass, dispersing the cellulose using a high-shear homogenizer (e.g., manufactured by IKA, trade name "Ultra Turrax T18") under processing conditions: rotation speed 25,000 rpm x 5 minutes, casting the homogenized sample on mica, and air-drying the sample to be measured, and measuring the length (L) and diameter (D) of 100 randomly selected fibrous substances in an observation field adjusted in magnification so that at least 100 fibrous substances are observed, and the ratio (L / D) is calculated. The number average value of the length (L), the number average value of the diameter (D), and the number average value of the ratio (L / D) are calculated for cellulose.

[0142] The length, diameter, and L / D ratio of the cellulose in the resin composition described below can be confirmed by measuring the solid resin composition as a measurement sample using the above-mentioned measurement method. Alternatively, the length, diameter, and L / D ratio of the cellulose in the resin composition can be confirmed by dissolving the resin components in the resin composition in an organic or inorganic solvent that can dissolve the resin components of the resin composition, separating the cellulose, thoroughly washing with the solvent, and then replacing with a water-soluble solvent (e.g., water, ethanol, tert-butanol, etc.), preparing a 0.01 to 0.1 mass% dispersion, and redispersing with a high-shear homogenizer (e.g., IKA, product name "Ultra Turrax T18"). The redispersion can be confirmed by casting the redispersion on mica, air-drying it, and measuring it as a measurement sample using the above-mentioned measurement method. At this time, the cellulose to be measured is measured on 100 or more randomly selected pieces.

[0143] The crystallinity of cellulose is preferably 55% or more. When the crystallinity is in this range, the mechanical properties (strength, dimensional stability) of the cellulose itself are high, so that when the cellulose is dispersed in a resin, the strength and dimensional stability of the resin composition tend to be high. A more preferable lower limit of the crystallinity is 60%, even more preferably 70%, and most preferably 80%. There is no particular upper limit for the crystallinity of cellulose, and the higher the better, but from the viewpoint of production, a preferable upper limit is 99%.

[0144] Alkali-soluble polysaccharides such as hemicellulose and acid-insoluble components such as lignin are present between the microfibrils and between the microfibril bundles of plant-derived cellulose. Hemicellulose is a polysaccharide composed of sugars such as mannan and xylan, and plays a role in binding the microfibrils together by hydrogen bonding with cellulose. Lignin is a compound having an aromatic ring, and is known to be covalently bonded to hemicellulose in the cell walls of plants. If there is a large amount of impurities such as lignin remaining in the cellulose, discoloration may occur due to heat during processing. Therefore, from the viewpoint of suppressing discoloration of the resin composition during extrusion processing and molding processing, it is desirable to set the crystallinity of the cellulose within the above-mentioned range.

[0145] The degree of crystallinity here, when the cellulose is cellulose type I crystal (derived from natural cellulose), is calculated from the diffraction pattern (2θ / deg. is 10 to 30) obtained by measuring a sample by wide-angle X-ray diffraction using the Segal method, according to the following formula: Crystallinity (%) = ([diffraction intensity due to the (200) plane at 2θ / deg. = 22.5] - [diffraction intensity due to amorphous matter at 2θ / deg. = 18]) / [diffraction intensity due to the (200) plane at 2θ / deg. = 22.5] × 100

[0146] When the cellulose is cellulose II type crystal (derived from regenerated cellulose), the degree of crystallinity can be calculated from the absolute peak intensity h0 at 2θ=12.6° assigned to the (110) plane peak of cellulose II type crystal in wide-angle X-ray diffraction and the peak intensity h1 from the baseline at this interplanar spacing, according to the following formula: Crystallinity (%) =h1 / h0 ×100

[0147] Known crystalline forms of cellulose include type I, type II, type III, and type IV, among which type I and type II are particularly widely used, and type III and type IV are obtained on a laboratory scale but are not widely used on an industrial scale. The cellulose of the present disclosure is preferably cellulose containing cellulose type I crystals or cellulose type II crystals, since it has relatively high structural mobility and by dispersing the cellulose in a resin, a resin composition having a lower linear expansion coefficient and superior strength and elongation during tensile and bending deformation can be obtained, and more preferably cellulose containing cellulose type I crystals and having a crystallinity of 55% or more.

[0148] In addition, the degree of polymerization of cellulose is preferably 100 or more, more preferably 150 or more, more preferably 200 or more, more preferably 300 or more, more preferably 400 or more, and preferably 3500 or less, more preferably 3300 or less, more preferably 3200 or less, more preferably 3100 or less, and more preferably 3000 or less.

[0149] From the viewpoint of processability and mechanical property expression, it is desirable that the degree of polymerization of cellulose is within the above-mentioned range. From the viewpoint of processability, it is preferable that the degree of polymerization is not too high, and from the viewpoint of mechanical property expression, it is desirable that the degree of polymerization is not too low.

[0150] The degree of polymerization of cellulose means the average degree of polymerization measured according to the reduced specific viscosity method using a copper ethylenediamine solution described in the Verification Test (3) of the "Japanese Pharmacopoeia Commentary, 15th Edition (published by Hirokawa Shoten)."

[0151] In one embodiment, the weight average molecular weight (Mw) of the cellulose is 100,000 or more, more preferably 200,000 or more. The ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight (Mn) is 6 or less, preferably 5.4 or less. The larger the weight average molecular weight, the fewer the number of terminal groups of the cellulose molecule. In addition, since the ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight represents the width of the molecular weight distribution, the smaller the Mw / Mn, the fewer the number of terminals of the cellulose molecule. Since the terminals of the cellulose molecules are the starting points of thermal decomposition, when the weight average molecular weight of the cellulose molecules is not only large but also has a narrow molecular weight distribution width, a particularly high heat-resistant cellulose and a resin composition containing cellulose and a resin can be obtained. The weight average molecular weight (Mw) of the cellulose may be, for example, 600,000 or less, or 500,000 or less, from the viewpoint of the availability of the cellulose raw material. From the viewpoint of ease of production of cellulose, the ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight (Mn) may be, for example, 1.5 or more, or 2 or more. Mw can be controlled within the above range by selecting a cellulose raw material having an Mw appropriate for the purpose, performing physical and / or chemical treatment on the cellulose raw material appropriately within a moderate range, and the like. Mw / Mn can also be controlled within the above range by selecting a cellulose raw material having an Mw / Mn appropriate for the purpose, performing physical and / or chemical treatment on the cellulose raw material appropriately within a moderate range, and the like. In both the control of Mw and the control of Mw / Mn, examples of the physical treatment include dry or wet grinding using a microfluidizer, ball mill, disk mill, etc., physical treatment that applies mechanical forces such as impact, shear, shear, and friction using a crusher, homomixer, high-pressure homogenizer, ultrasonic device, etc., and examples of the chemical treatment include digestion, bleaching, acid treatment, and regenerated cellulose.

[0152] The weight average molecular weight and number average molecular weight of cellulose referred to here are values ​​determined by dissolving cellulose in N,N-dimethylacetamide containing added lithium chloride and then subjecting the cellulose to gel permeation chromatography using N,N-dimethylacetamide as a solvent.

[0153] Methods for controlling the degree of polymerization (i.e., average degree of polymerization) or molecular weight of cellulose include hydrolysis. The hydrolysis promotes depolymerization of amorphous cellulose inside the cellulose, decreasing the average degree of polymerization. At the same time, the hydrolysis removes impurities such as hemicellulose and lignin in addition to the amorphous cellulose described above, making the inside of the fiber porous. This makes the cellulose more susceptible to mechanical treatment in a process of applying mechanical shear force to the cellulose, such as during the kneading process described below, and makes the cellulose more easily pulverized.

[0154] The hydrolysis method is not particularly limited, and examples thereof include acid hydrolysis, alkali hydrolysis, hydrothermal decomposition, steam explosion, and microwave decomposition. These methods may be used alone or in combination of two or more. In the acid hydrolysis method, for example, α-cellulose obtained as pulp from a fibrous plant is used as a cellulose raw material, and this is dispersed in an aqueous medium, and an appropriate amount of a protonic acid, a carboxylic acid, a Lewis acid, a heteropoly acid, etc. is added, and the mixture is heated while stirring, so that the average degree of polymerization can be easily controlled. The reaction conditions such as temperature, pressure, and time at this time vary depending on the cellulose type, cellulose concentration, acid type, acid concentration, etc., but are appropriately adjusted so that the desired average degree of polymerization is achieved. For example, a condition in which cellulose is treated for 10 minutes or more at 100°C or higher under pressure using an aqueous mineral acid solution of 2% by mass or less can be exemplified. Under these conditions, the catalyst component such as acid penetrates into the inside of the cellulose, promoting hydrolysis, reducing the amount of catalyst component used, and making subsequent purification easier. The dispersion of the cellulose raw material during hydrolysis may contain, in addition to water, a small amount of an organic solvent within a range that does not impair the effects of the present invention.

[0155] Alkali-soluble polysaccharides that cellulose may contain include hemicellulose, β-cellulose, and γ-cellulose. Alkali-soluble polysaccharides are understood by those skilled in the art as components obtained as the alkali-soluble portion of holocellulose obtained by solvent extraction and chlorine treatment of plants (e.g., wood) (i.e., components obtained by removing α-cellulose from holocellulose). Alkali-soluble polysaccharides are polysaccharides containing hydroxyl groups and have poor heat resistance, and may cause inconveniences such as decomposition when exposed to heat, yellowing during heat aging, and a decrease in the strength of cellulose. Therefore, it is preferable that the content of alkali-soluble polysaccharides in cellulose is low.

[0156] In one embodiment, the average content of alkali-soluble polysaccharides in cellulose is preferably 20% by mass or less, or 18% by mass or less, or 15% by mass or less, or 12% by mass or less, or 11% by mass or less, or 8% by mass or less, based on 100% by mass of cellulose, from the viewpoint of obtaining good dispersibility of cellulose. The above content may be 1% by mass or more, or 2% by mass or more, or 3% by mass or more, or 6% by mass or more, from the viewpoint of ease of production of cellulose. In one embodiment, the average content of alkali-soluble polysaccharides in the cellulose raw material may be 13% by mass or less, or 12% by mass or less, or 11% by mass or less, or 8% by mass or less, and is most preferably 0% by mass, but may be, for example, 3% by mass or more, or 6% by mass or more, from the viewpoint of ease of availability of the cellulose raw material.

[0157] The average alkali-soluble polysaccharide content can be determined by the method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000), by subtracting the α-cellulose content from the holocellulose content (Wise method). This method is understood in the industry as a method for measuring the amount of hemicellulose. The alkali-soluble polysaccharide content is calculated three times for each sample, and the number average of the calculated alkali-soluble polysaccharide contents is taken as the average alkali-soluble polysaccharide content.

[0158] In one embodiment, the average content of acid-insoluble components in cellulose is preferably 10% by mass or less, 5% by mass or less, or 3% by mass or less, based on 100% by mass of cellulose, from the viewpoint of avoiding a decrease in heat resistance of cellulose and the associated discoloration. From the viewpoint of ease of production of cellulose, the content may be 0.1% by mass or more, 0.2% by mass or more, or 0.3% by mass or more.

[0159] The average acid-insoluble content is determined as a quantitative determination of the acid-insoluble content using the Clason method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000). This method is understood in the industry as a method for measuring the amount of lignin. The sample is stirred in a sulfuric acid solution to dissolve cellulose, hemicellulose, etc., and then filtered through a glass fiber filter paper, and the resulting residue corresponds to the acid-insoluble content. The acid-insoluble content is calculated from the weight of the acid-insoluble content, and the number average of the acid-insoluble content calculated for the three samples is taken as the average acid-insoluble content.

[0160] The cellulose may be chemically treated (e.g., oxidized or chemically modified with a modifying agent). As an example, fine cellulose fibers obtained by oxidizing cellulose fibers with 2,2,6,6-tetramethylpiperidine-1-oxyl radical as shown in Cellulose (1998) 5, 153-164, followed by washing and mechanical fiberization, may be used.

[0161] In the first embodiment, the ratio of cellulose (particularly the ratio of cellulose nanofibers) to 100 mass% of the resin composition is preferably 0.1 mass% or more, or 0.5 mass% or more, or 1 mass% or more, or 3 mass% or more, from the viewpoint of obtaining the advantages of the low linear expansion coefficient and high rigidity provided by cellulose, and is preferably 30 mass% or less, or 25 mass% or less, or 20 mass% or less, or 15 mass% or less, from the viewpoint of obtaining the advantages of the other components in the resin composition.

[0162] In the first embodiment, the ratio of cellulose (particularly the ratio of cellulose nanofibers) to 100 parts by mass of polyamide is, from the viewpoint of obtaining the advantages of low linear expansion coefficient and high rigidity provided by cellulose, preferably 1 part by mass or more, or 5 parts by mass or more, or 10 parts by mass or more, or 15 parts by mass or more, and, from the viewpoint of dispersing cellulose well in the polyamide phase, preferably 50 parts by mass or less, or 40 parts by mass or less, or 30 parts by mass or less, or 20 parts by mass or less.

[0163] <Cellulose of the second and third embodiments> The resin compositions according to the second and third embodiments contain cellulose. The cellulose may contain fibrous cellulose. The cellulose may contain cellulose nanofibers (CNF) having a diameter of 50 to 1000 nm and a length (L) / diameter (D) ratio of 30 or more, cellulose nanocrystals (CNC) having a diameter of 100 nm or less and a length (L) / diameter (D) ratio of less than 30, or cellulose microfibers (CMF) having a diameter of more than 1 μm to 50 μm, or a mixture thereof, and is preferably CNF, CNC, CMF, or a mixture thereof. Examples of such cellulose include natural cellulose and regenerated cellulose, as exemplified above.

[0164] Cellulose nanofibers (CNF) can be obtained by the procedure described in the first embodiment. In one aspect, the diameter of the CNF is 50 to 1000 nm. The diameter of the CNF is preferably 50 nm or more, more preferably 100 nm or more, more preferably 400 nm or less, and even more preferably 200 nm or less. In one aspect, the L / D of the CNF is 30 or more, preferably 50 or more, more preferably 80 or more, and even more preferably 100 or more, and preferably 5000 or less, more preferably 4000 or less, and even more preferably 3000 or less.

[0165] Figure 1 is a microscope image showing examples of cellulose nanofibers. It can be seen that all of the cellulose has a fibrous structure, a diameter of 50 to 1000 nm, and an L / D of 30 or more.

[0166] Cellulose nanocrystals (CNC) are crystalline cellulose that remains after cutting the above-mentioned pulp and dissolving the amorphous part of the cellulose in an acid such as hydrochloric acid or sulfuric acid. In one embodiment, the diameter of the CNC is 100 nm or less, preferably 80 nm or less, more preferably 70 nm or less, preferably 3 nm or more, more preferably 5 nm or more, and even more preferably 10 nm or more. In one embodiment, the length / diameter ratio (L / D ratio) of the CNC is less than 30, preferably 20 or less, more preferably 15 or less, and even more preferably 10 or less. In one embodiment, the L / D ratio is 1 or more, preferably 2 or more, more preferably 4 or more, and even more preferably 5 or more.

[0167] Figure 2 shows microscopic images of examples of cellulose nanocrystals (also called cellulose nanowhiskers or needle-shaped particulate cellulose), and Figure 2(B) is a partially enlarged view of Figure 2(A). It can be seen that all of the cellulose has a needle-shaped crystalline particulate structure, a diameter of 100 nm or less, and an L / D ratio of less than 30.

[0168] Cellulose microfiber (hereinafter sometimes referred to as CMF) refers to a relatively large-sized fibrous cellulose obtained by reducing the number of defibration steps in the process of producing CNF. In one embodiment, the diameter of the CMF is more than 1 μm to 50 μm. The diameter of the CMF is preferably 2 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, and preferably 45 μm or less, more preferably 40 μm or less, even more preferably 35 μm or less. The L / D of the CMF is preferably 30 or more, more preferably 50 or more, even more preferably 70 or more, and preferably 2000 or less, more preferably 1000 or less, even more preferably 500 or less. CMF can be obtained with about half the energy required to produce regular CNF.

[0169] Figure 3 shows micrographs of cellulose microfibers. It can be seen that all of the cellulose has a diameter of more than 1 μm to 50 μm and an L / D ratio of 30 or more.

[0170] The amount of cellulose relative to 100% by mass of the entire resin composition is preferably 0.1 to 30% by mass. More preferably, the upper limit of the amount of cellulose is 25% by mass, 20% by mass, or 15% by mass. More preferably, the lower limit of the amount of cellulose is 0.5% by mass, 1% by mass, or 3% by mass. From the viewpoint of suppressing the thermal expansion coefficient and obtaining good physical property stability, the amount is preferably within the above-mentioned range.

[0171] In the second and third embodiments, preferred aspects of the cellulose include, from the viewpoint of ensuring the stability of physical properties, the use of CNF alone, the use of CMF alone, the use of two types of CNF and CNC in combination, the use of two types of CNF and CMF in combination, the use of two types of CMF and CNC in combination, and the use of three types of CMF, CNF, and CNC in combination. More preferred aspects include the use of CMF alone, the use of two types of CNF and CNC in combination, the use of two types of CNF and CMF in combination, the use of two types of CMF and CNC in combination, and the use of three types of CMF, CNF, and CNC in combination.

[0172] When CNF and CMF are used in combination, the preferred ratio of CMF is 50 to 99% by mass when the total amount of cellulose is 100% by mass. The upper limit of the ratio is more preferably 97% by mass, even more preferably 95% by mass, even more preferably 93% by mass, and most preferably 90% by mass. The lower limit of the ratio is more preferably 55% by mass, even more preferably 60% by mass, and most preferably 70% by mass.

[0173] In addition, when CNF and CNC are used in combination, and when CMF and CNC are used in combination, the preferred ratio of CNC is 50 to 99% by mass when the total amount of cellulose is taken as 100% by mass. The upper limit of the ratio is more preferably 97% by mass, even more preferably 95% by mass, even more preferably 93% by mass, and most preferably 90% by mass. The lower limit of the ratio is more preferably 55% by mass, even more preferably 60% by mass, and most preferably 70% by mass.

[0174] In addition, when CMF, CNF, and CNC are used in combination, the preferred ratio of CNC is 50 to 99% by mass when the total amount of cellulose is 100% by mass. The upper limit of the ratio is more preferably 97% by mass, even more preferably 95% by mass, even more preferably 93% by mass, and most preferably 90% by mass. The lower limit of the ratio is more preferably 55% by mass, even more preferably 60% by mass, and most preferably 65% ​​by mass. Furthermore, when the total amount of cellulose other than CNC is 100% by mass, the preferred ratio of CMF is 50 to 99% by mass. The upper limit of the ratio is more preferably 97% by mass, even more preferably 95% by mass, even more preferably 93% by mass, and most preferably 90% by mass. The lower limit of the ratio is more preferably 55% by mass, even more preferably 60% by mass, and most preferably 70% by mass.

[0175] The amount of CNF relative to 100% by mass of the resin composition is preferably 0.1 to 20% by mass. When the amount of CNF is within the above range, it is possible to improve properties such as thermal expansion. The lower limit of the amount is more preferably 1% by mass, further preferably 2% by mass, even more preferably 3% by mass, and most preferably 5% by mass. The upper limit is more preferably 18% by mass, further preferably 16% by mass, further preferably 14% by mass, and most preferably 12% by mass.

[0176] Furthermore, the amount of CMF relative to 100% by mass of the resin composition is preferably 0.1 to 20% by mass. When the amount of CMF is within the above range, it is possible to improve properties such as tensile elongation and vibration fatigue properties. The lower limit of the amount is more preferably 1% by mass, further preferably 2% by mass, even more preferably 3% by mass, and most preferably 5% by mass. The upper limit is more preferably 18% by mass, further preferably 16% by mass, further preferably 14% by mass, and most preferably 12% by mass.

[0177] In the second and third embodiments, the length, diameter, and L / D ratio of each of the CNCs and CNFs are determined by dispersing each of the aqueous dispersions of CNCs and CNFs using a high-shear homogenizer (e.g., Nippon Seiki Co., Ltd., product name "Excel Auto Homogenizer ED-7") under processing conditions: rotation speed 15,000 rpm × 5 minutes, diluting the aqueous dispersion with pure water to 0.1 to 0.5 mass%, casting it on mica, and air-drying it to obtain a measurement sample, and measuring it with a high-resolution scanning microscope (SEM) or atomic force microscope (AFM). Specifically, the length (L) and diameter (D) of 100 randomly selected celluloses are measured in an observation field where the magnification is adjusted so that at least 100 celluloses are observed, and the ratio (L / D) is calculated. A ratio (L / D) of less than 30 is classified as CNC, and a ratio of 30 or more is classified as CNF. The number average value of the length (L), the number average value of the diameter (D), and the number average value of the ratio (L / D) were calculated for each of the CNCs and CNFs, and these were used as the length, diameter, and L / D ratio for each of the CNCs and CNFs. The length and diameter of the cellulose mentioned above are the number average values ​​of the 100 celluloses mentioned above.

[0178] CMF has a different size scale from CNC and CNF, and electron microscope is not suitable for measuring the length, diameter, L / D ratio, etc. of CMF, so the size of CMF is observed by another method. A low-concentration aqueous dispersion prepared so that the CMF is about 0.1% by mass is subjected to sufficient vibration in an ultrasonic cleaner or a dispersion treatment for 20 minutes in a dispersing machine (e.g., Despamill, manufactured by Asada Iron Works Co., Ltd.) to loosen the entanglements between the CMF, and then the aqueous dispersion is observed as it is under an optical microscope. The measurement and calculation methods are the same as those for CNF and CNC.

[0179] Alternatively, the length, diameter, and L / D ratio of each of the CMF, CNC, and CNF in the resin composition are measured by dissolving the polymer components in the composition in an organic or inorganic solvent capable of dissolving the polymer components of the composition, separating the cellulose, thoroughly washing with the solvent, and then replacing the solvent with pure water to prepare an aqueous dispersion. The cellulose concentration is then diluted with pure water to 0.1 to 0.5 mass%, and the measurement is performed by the method described above.

[0180] The average diameter of the CNCs as measured by volume average particle size is preferably 10 nm or more, more preferably 15 nm or more, even more preferably 20 nm or more, more preferably 40 nm or more, even more preferably 50 nm or more, and is preferably 1000 nm or less, more preferably 700 nm or less, more preferably 500 nm or less, even more preferably 300 nm or less. The average diameter of the CNFs, as determined by volume average particle size measurement, is preferably 20 nm or more, more preferably 40 nm or more, even more preferably 50 nm or more, and is preferably 1000 nm or less, more preferably 700 nm or less, even more preferably 500 nm or less.

[0181] The volume average particle diameter is a value obtained by a laser diffraction / scattering particle size distribution analyzer as the equivalent spherical diameter (volume average particle diameter) of particles when the cumulative volume is 50%. Specifically, a sample is mixed at 40% solids by mass in a planetary mixer (e.g., 5DM-03-R, manufactured by Shinagawa Kogyosho Co., Ltd., with a hook-type stirring blade) at 126 rpm for 30 minutes at room temperature and normal pressure, then suspended in pure water at a concentration of 0.5% by mass, and dispersed at a rotation speed of 15,000 rpm for 5 minutes using a high-shear homogenizer (e.g., manufactured by Nippon Seiki Co., Ltd., trade name "Excel Auto Homogenizer ED-7" processing condition), and centrifuged at a centrifugal force of 39,200 m 2 The supernatant was collected after centrifugation at 116,000m / s for 10 minutes. 2 The mixture is centrifuged at 1000 / s for 45 minutes, and the supernatant after centrifugation is collected. The volume-frequency particle size distribution obtained using this supernatant with a laser diffraction / scattering particle size distribution analyzer (e.g., Horiba, Ltd., trade name "LA-910" or trade name "LA-950", ultrasonic treatment for 1 minute, refractive index 1.20) is determined to be the cumulative 50% particle size (i.e., the spherical equivalent diameter of the particles when the cumulative volume is 50% of the total volume of the particles) as the volume-average particle size.

[0182] In the second and third embodiments, the crystallinity, crystal form, degree of polymerization, weight average molecular weight (Mw), ratio of weight average molecular weight to number average molecular weight (Mn) (Mw / Mn), average content of alkali-soluble polysaccharides, average content of acid-insoluble components, and methods for measuring and adjusting these may be the same as those exemplified in the first embodiment.

[0183] <Hydrophobicity of cellulose> The cellulose in the first to third embodiments may be cellulose hydrophobized by a hydrophobizing agent (also referred to as chemically modified cellulose in the present disclosure). Hydrophobization weakens hydrogen bonds between cellulose, contributing to fine dispersion, improving heat resistance as cellulose, making it possible to suppress deterioration due to kneading with resin, and making cellulose less likely to become the starting point of physical property defects. As the hydrophobizing agent (also referred to as a modifying agent in the present disclosure), a compound that reacts with the hydroxyl group of cellulose can be used, and examples of the hydrophobizing agent include an esterifying agent, an etherifying agent, and a silylating agent. In particular, an esterifying agent is preferred. In a preferred embodiment, the hydrophobization is acylation using an esterifying agent. As the esterifying agent, acid halides, acid anhydrides, and carboxylic acid vinyl esters are preferred. In a particularly preferred embodiment, the hydrophobization is acetylation.

[0184] The acid halide may be at least one selected from the group consisting of compounds represented by the following formula (1). R 1 -C(=O)-X (1) (In the formula, R 1 represents an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, a cycloalkyl group having 3 to 24 carbon atoms, or an aryl group having 6 to 24 carbon atoms, and X is Cl, Br, or I. Specific examples of acid halides include, but are not limited to, acetyl chloride, acetyl bromide, acetyl iodide, propionyl chloride, propionyl bromide, propionyl iodide, butyryl chloride, butyryl bromide, butyryl iodide, benzoyl chloride, benzoyl bromide, and benzoyl iodide. Among them, acid chlorides can be preferably used in terms of reactivity and handling. In addition, in the reaction of acid halides, one or more alkaline compounds may be added to act as a catalyst and neutralize the by-product acidic substances. Specific examples of alkaline compounds include, but are not limited to, tertiary amine compounds such as triethylamine and trimethylamine; and nitrogen-containing aromatic compounds such as pyridine and dimethylaminopyridine.

[0185] As the acid anhydride, any suitable acid anhydride can be used. For example, Saturated aliphatic monocarboxylic acid anhydrides, such as acetic acid, propionic acid, (iso)butyric acid, and valeric acid; unsaturated aliphatic monocarboxylic acid anhydrides, such as (meth)acrylic acid and oleic acid; Alicyclic monocarboxylic acid anhydrides such as cyclohexanecarboxylic acid and tetrahydrobenzoic acid; Aromatic monocarboxylic acid anhydrides such as benzoic acid and 4-methylbenzoic acid; Examples of dibasic carboxylic acid anhydrides include saturated aliphatic dicarboxylic acid anhydrides such as succinic anhydride and adipic acid, unsaturated aliphatic dicarboxylic acid anhydrides such as maleic anhydride and itaconic anhydride, alicyclic dicarboxylic acid anhydrides such as 1-cyclohexene-1,2-dicarboxylic acid anhydride, hexahydrophthalic anhydride and methyltetrahydrophthalic anhydride, and aromatic dicarboxylic acid anhydrides such as phthalic anhydride and naphthalic anhydride; Examples of polybasic carboxylic acid anhydrides having three or more bases include polycarboxylic acids (anhydrides) such as trimellitic anhydride and pyromellitic anhydride. In addition, in the reaction of an acid anhydride, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.

[0186] The vinyl carboxylate may be represented by the following formula (1): R-COO-CH=CH2…Formula (1) Preferred is a vinyl carboxylate represented by the formula: {wherein R is any one of an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, and an aryl group having 6 to 24 carbon atoms.} The vinyl carboxylate is more preferably at least one selected from the group consisting of vinyl acetate, vinyl propionate, vinyl butyrate, vinyl caproate, vinyl cyclohexanecarboxylate, vinyl caprylate, vinyl caprate, vinyl laurate, vinyl myristate, vinyl palmitate, vinyl stearate, vinyl pivalate, vinyl octylate, divinyl adipate, vinyl methacrylate, vinyl crotonate, vinyl pivalate, vinyl octylate, vinyl benzoate, and vinyl cinnamate. In the esterification reaction with a vinyl carboxylate, one or more catalysts selected from the group consisting of alkali metal hydroxides, alkaline earth metal hydroxides, alkali metal carbonates, alkaline earth metal carbonates, alkali metal hydrogencarbonates, primary to tertiary amines, quaternary ammonium salts, imidazole and derivatives thereof, pyridine and derivatives thereof, and alkoxides may be added.

[0187] Examples of the alkali metal hydroxides and alkaline earth metal hydroxides include sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, barium hydroxide, etc. Examples of the alkali metal carbonates, alkaline earth metal carbonates, and alkali metal hydrogen carbonates include lithium carbonate, sodium carbonate, potassium carbonate, cesium carbonate, magnesium carbonate, calcium carbonate, barium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, cesium hydrogen carbonate, etc.

[0188] The primary, secondary and tertiary amines refer to primary, secondary and tertiary amines, and specific examples thereof include ethylenediamine, diethylamine, proline, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,3-propanediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, tris(3-dimethylaminopropyl)amine, N,N-dimethylcyclohexylamine and triethylamine.

[0189] Examples of imidazole and its derivatives include 1-methylimidazole, 3-aminopropylimidazole, and carbonyldiimidazole.

[0190] Examples of pyridine and its derivatives include N,N-dimethyl-4-aminopyridine and picoline.

[0191] Examples of the alkoxide include sodium methoxide, sodium ethoxide, and potassium t-butoxide.

[0192] The carboxylic acid may be at least one selected from the group consisting of compounds represented by the following formula (1). R-COOH …(1) (In the formula, R represents an alkyl group having 1 to 16 carbon atoms, an alkenyl group having 2 to 16 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, or an aryl group having 6 to 16 carbon atoms.)

[0193] Specific examples of carboxylic acids include at least one selected from the group consisting of acetic acid, propionic acid, butyric acid, caproic acid, cyclohexane carboxylic acid, caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, pivalic acid, methacrylic acid, crotonic acid, pivalic acid, octylic acid, benzoic acid, and cinnamic acid.

[0194] Among these carboxylic acids, at least one selected from the group consisting of acetic acid, propionic acid, and butyric acid, and particularly acetic acid, is preferred from the viewpoint of reaction efficiency. In addition, in the reaction of carboxylic acid, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.

[0195] Among these esterification reactants, at least one selected from the group consisting of acetic anhydride, propionic anhydride, butyric anhydride, vinyl acetate, vinyl propionate, vinyl butyrate, and acetic acid, and among these, acetic anhydride and vinyl acetate are preferred from the viewpoint of reaction efficiency.

[0196] When obtaining hydrophobized cellulose nanofibers, there is no particular limitation on the method for pulverizing natural cellulose raw materials to reduce the fiber diameter, but it is preferable to make the defibration processing conditions (method of applying a shear field, magnitude of the shear field, etc.) more efficient. In particular, by impregnating a cellulose raw material having a cellulose purity of 85% by mass or more with a defibration solution containing an aprotic solvent, cellulose swelling occurs in a short time, and the cellulose is pulverized by only applying slight stirring and shear energy. Then, hydrophobized cellulose nanofibers can be obtained by adding a cellulose modifying agent immediately after defibration. This method is preferable from the viewpoints of production efficiency and purification efficiency (i.e., high cellulose purity of hydrophobized cellulose nanofibers) and physical properties of the resin composition.

[0197] Examples of the aprotic solvent include alkyl sulfoxides, alkyl amides, pyrrolidones, etc. These solvents may be used alone or in combination of two or more kinds.

[0198] Examples of the alkyl sulfoxides include di-C1-4 alkyl sulfoxides such as dimethyl sulfoxide (DMSO), methyl ethyl sulfoxide, and diethyl sulfoxide.

[0199] Examples of the alkylamides include N,N-diC1-4 alkylformamides such as N,N-dimethylformamide (DMF) and N,N-diethylformamide; and N,N-diC1-4 alkylacetamides such as N,N-dimethylacetamide (DMAc) and N,N-diethylacetamide.

[0200] Examples of pyrrolidones include pyrrolidones such as 2-pyrrolidone and 3-pyrrolidone; and N-C1-4 alkylpyrrolidones such as N-methyl-2-pyrrolidone (NMP).

[0201] These aprotic solvents can be used alone or in combination. Among these aprotic solvents (numbers in parentheses indicate the number of donors), DMSO (29.8), DMF (26.6), DMAc (27.8), NMP (27.3), etc., especially DMSO, can be used to more efficiently produce hydrophobic cellulose nanofibers with a high thermal decomposition onset temperature. The mechanism of this action is not entirely clear, but it is presumed to be due to the uniform micro-swelling of the fiber raw material in the aprotic solvent.

[0202] When cellulose raw materials swell in aprotic solvents, the aprotic solvent quickly penetrates and swells the fibrils that make up the raw materials, causing the microfibrils to become finely defibrated. After this state is created, chemical modification is performed to homogeneously hydrophobize the entire fine fiber, which is presumably the result of high heat resistance. Furthermore, these microfibrillated, chemically modified fine fibers maintain a high degree of crystallinity, and when combined with resin, they can achieve high mechanical properties and excellent dimensional stability (especially a significant reduction in the linear thermal expansion coefficient).

[0203] When obtaining hydrophobic cellulose nanofibers, cellulose nanofibers that have been finely divided (defibrated) and hydrophobized can be obtained using devices that apply collision shear, such as planetary ball mills and bead mills, devices that apply a rotational shear field that induces cellulose fibrillation, such as disc refiners and grinders, or devices that can perform the functions of kneading, stirring, and dispersion with high efficiency, such as various kneaders and planetary mixers.

[0204] The degree of hydrophobicity (degree of modification) of cellulose is expressed as the average degree of substitution of hydroxyl groups (also referred to as DS, the average number of hydroxyl groups substituted per glucose, which is the basic structural unit of cellulose). In one embodiment, the DS of the chemically modified cellulose is preferably 0.01 or more and 2.0 or less. If the DS is 0.01 or more, a resin composition containing chemically modified cellulose with a high thermal decomposition onset temperature can be obtained. On the other hand, if the DS is 2.0 or less, an unmodified cellulose skeleton remains in the chemically modified cellulose, so that a resin composition containing chemically modified cellulose having both high tensile strength and dimensional stability derived from cellulose and high thermal decomposition onset temperature derived from chemical modification can be obtained. The DS is more preferably 0.05 or more, even more preferably 0.1 or more, particularly preferably 0.2 or more, and most preferably 0.3 or more, and more preferably 1.8 or less, even more preferably 1.5 or less, particularly preferably 1.2 or less, and most preferably 1.0 or less.

[0205] In the reflection infrared absorption spectrum of hydrophobized cellulose, the peak position of the absorption band changes depending on the type of hydrophobic modification group. From the change in peak position, it is possible to determine which absorption band the peak is based on, and to identify the modification group. In addition, the modification rate can be calculated from the peak intensity ratio between the peak derived from the modification group and the peak derived from the cellulose skeleton.

[0206] When the modifying group is an acyl group, the degree of acyl substitution (DS) can be calculated from the reflection infrared absorption spectrum of the esterified cellulose based on the peak intensity ratio between the peak derived from the acyl group and the peak derived from the cellulose skeleton. The peak of the absorption band of C=O based on the acyl group is at 1730 cm -1 The absorption band of CO based on the cellulose backbone appears at 1030 cm -1 The DS of esterified cellulose is calculated by plotting a correlation graph between the DS obtained from solid-state NMR measurement of esterified cellulose (described later) and the modification ratio (IR index 1030), which is defined as the ratio of the peak intensity of the absorption band of C=O based on the acyl group to the peak intensity of the absorption band of CO in the cellulose backbone chain, and then calculating a calibration curve from the correlation graph. Degree of substitution DS = 4.13 × IR index (1030) It can be found by using

[0207] In addition, when it is difficult to perform an appropriate measurement using the reflection infrared absorption spectrum, solid-state NMR is used. The method for calculating the DS of esterified cellulose by solid-state NMR is as follows for frozen and crushed esterified cellulose: 13 C solid-state NMR measurement was performed, and the intensity can be calculated using the area intensity (Inf) of a signal assigned to one carbon atom derived from the modifying group relative to the total area intensity (Inp) of signals assigned to carbons C1-C6 derived from the pyranose ring of cellulose, which appear in the range from 50 ppm to 110 ppm, using the following formula. DS = (Inf) x 6 / (Inp) For example, when the modifying group is an acetyl group, the signal at 23 ppm assigned to -CH3 may be used.

[0208] Use 13 The conditions for the C solid-state NMR measurement are, for example, as follows: Equipment:Bruker Biospin Avance500WB Frequency: 125.77MHz Measurement method: DD / MAS method Waiting time: 75sec NMR sample tube: 4mmφ Accumulation times: 640 times (approx. 14 hours) MAS: 14,500Hz Chemical shift reference: glycine (external reference: 176.03 ppm)

[0209] <Antioxidants> In the first to third embodiments, the resin composition may further contain an antioxidant. The antioxidant is advantageous in that it suppresses thermal degradation of each component (e.g., polyphenylene ether, elastomer, and / or saponified ethylene-vinyl ester copolymer) when the resin composition is melt-kneaded at a high temperature equal to or higher than the melting point of the polyamide. The antioxidant may be one or more selected from the group consisting of hindered phenol-based antioxidants, hindered amine-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, benzotriazole-based antioxidants, benzophenone-based antioxidants, triazine-based antioxidants, salicylic acid ester-based antioxidants, and p-phenylenediamine-based antioxidants. For example, in the third embodiment, hindered phenol-based antioxidants and phosphorus-based antioxidants are particularly preferred.

[0210] Hindered phenol antioxidants include 2,4-bis[(laurylthio)methyl]-o-cresol, 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl), 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl), 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2,6-di-t-butyl-4-nonylphenol, 2,2'-isobutylidene-bis-(4,6-dimethyl-phenol), 4,4'-butyl- Examples of the phenolic compounds include 2,2'-thiodiethyl bis-(2-t-butyl-5-methylphenol), 2,2'-thio-bis-(6-t-butyl-4-methylphenol), 2,5-di-t-amyl-hydroquinone, 2,2'-thiodiethyl bis-(3,5-di-t-butyl-4-hydroxyphenyl)-propionate, 1,1,3-tris-(2'-methyl-4'-hydroxy-5'-t-butylphenyl)-butane, 2,2'-methylene-bis-(6-(1-methyl-cyclohexyl)-p-cresol), 2,4-dimethyl-6-(1-methyl-cyclohexyl)-phenol, N,N-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), etc. In addition, oligomer type and polymer type compounds having a hindered phenol structure can also be used.

[0211] Specific examples include ADK STAB AO-20, AO-30, AO-40, AO50, AO60, AO80, and AO320 manufactured by ADEKA CORPORATION; KEMINOX101, 179, 76, and 9425 manufactured by Chemipro Corporation; IRGANOX1010, 1035, 1076, 1098, 1135, 1330, 1726, 1425WL, 1520L, 245, 259, 3114, 5057, and 565 manufactured by BASF Ltd.; and Cyanox CY-1790 and CY-2777 manufactured by Sun Chemical Co., Ltd.

[0212] Hindered amine antioxidants include bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(N-methyl-2,2,6,6-tetramethyl-4-piperidyl)sebacate, N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl)-1,6-hexamethylenediamine, and 2-methyl-2-(2,2,6,6-tetramethyl-4-piperidyl)amino. -N-(2,2,6,6-tetramethyl-4-piperidyl)propionamide, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)(1,2,3,4-butanetetracarboxylate, poly[{6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethyl {(2,2,6,6-tetramethyl-4-piperidyl)imino}], poly[(6-morpholino-1,3,5-triazine-2,4-diyl){(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethine{(2,2,6,6-tetramethyl-4-piperidyl)imino}], polycondensate of dimethyl succinate and 1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine, N,N'-4,7-tetrakis[4,6-bis{N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino}-1,3,5-triazine-2-yl]-4,7-diazadecane-1,10-diamine, etc. In addition, oligomer type and polymer type compounds having a hindered amine structure can also be used.

[0213] Specific examples include ADK STAB LA-52, LA-57, LA-63P, LA-68, LA-72, LA-77Y, LA-77G, LA-81, LA-82, LA-87, LA-402F, and LA-502XP manufactured by ADEKA CORPORATION; KAMISTAB 29, 62, 77, 29, and 94 manufactured by Chemipro Chemical Co., Ltd.; Tinuvin 249, TINUVIN 111FDL, 123, 144, 292, and 5100 manufactured by BASF Corporation; and Cyasorb UV-3346, UV-3529, and UV-3853 manufactured by Sun Chemical Co., Ltd.

[0214] Examples of phosphorus antioxidants include tris(isodecyl)phosphite, tris(tridecyl)phosphite, phenyl isooctyl phosphite, phenyl isodecyl phosphite, phenyl di(tridecyl)phosphite, diphenyl isooctyl phosphite, diphenyl isodecyl phosphite, diphenyl tridecyl phosphite, triphenyl phosphite, tris(nonylphenyl)phosphite, 4,4'isopropylidenediphenol alkyl phosphite, trisnonylphenyl phosphite, tris(2,4-di-t-butylphenyl)phosphite, tris(biphenyl)phosphite, distearyl pentaerythritol diphosphite, di(2,4-di-t-butylphenyl)pentaerythritol Examples of the phosphite include tetratridecyl diphosphite, di(nonylphenyl)pentaerythritol diphosphite, phenyl bisphenol A pentaerythritol diphosphite, tetratridecyl 4,4'-butylidene bis(3-methyl-6-t-butylphenol) diphosphite, hexatridecyl 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane triphosphite, 3,5-di-t-butyl-4-hydroxybenzyl phosphite diethyl ester, sodium bis(4-t-butylphenyl) phosphite, sodium-2,2-methylene-bis(4,6-di-t-butylphenyl)-phosphite, 1,3-bis(diphenoxyphosphonyloxy)-benzene, and ethyl bis(2,4-ditert-butyl-6-methylphenyl) phosphite. Other oligomer and polymer type compounds having a phosphite structure can also be used.

[0215] Specific examples include ADK STAB PEP-36, PEP-8, HP-10, ADK STAB 2112, 1178, 1500, C, 3013, and TPP manufactured by ADEKA CORPORATION, IRGAFOS168 manufactured by BASF Corporation, and HostanoxP-EPQ manufactured by Clariant Chemicals K.K.

[0216] Examples of sulfur-based antioxidants include 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,4-bis[(octylthio)methyl]-o-cresol, 2,4-bis[(laurylthio)methyl]-o-cresol, 2,2-bis{[3-(dodecylthio)-1-oxopropoxy]methyl}propane-1,3-diylbis[3-(dodecylthio)propionate], 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], etc. In addition, oligomer and polymer type compounds having a thioether structure can also be used.

[0217] Specific examples include ADK STAB AO-412S and AO-503 manufactured by ADEKA CORPORATION, and KEMINOXPLS manufactured by Chemipro Chemicals Co., Ltd.

[0218] As the benzotriazole-based antioxidant, oligomer-type and polymer-type compounds having a benzotriazole structure can be used.

[0219] Specific examples include ADK STAB LA-29, LA-31RG, LA-32, LA-36, -412S manufactured by ADEKA CORPORATION, KEMISORB71, 73, 74, 79, 279 manufactured by Chemipro Chemical Co., Ltd., TINUVIN PS, 99-2, 384-2, 900, 928, 1130 manufactured by BASF Corporation, and the like.

[0220] Benzophenone-based antioxidants include 2-hydroxy-4-methoxybenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-n-octoxybenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 2-hydroxy-4-octadecyloxybenzophenone, 2,2'dihydroxy-4-methoxybenzophenone, 2,2'dihydroxy-4,4'-dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2-hydroxy-4-methoxy-5-sulfobenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, etc. In addition, oligomer type and polymer type compounds having a benzophenone structure can also be used.

[0221] Specific examples include ADK STAB 1413 manufactured by ADEKA CORPORATION, K EMISORB10, 11, 11S, 12, and 111 manufactured by Chemipro Chemical Co., Ltd., and UV-12 and UV-329 manufactured by Sun Chemical Co., Ltd.

[0222] Examples of triazine-based antioxidants include 2,4-bis(allyl)-6-(2-hydroxyphenyl)1,3,5-triazine, etc. In addition, oligomer-type and polymer-type compounds having a triazine structure can also be used.

[0223] Specific examples include ADK STAB LA-46 and F70 manufactured by ADEKA CORPORATION, KEMISORB102 manufactured by Chemipro Chemicals Co., Ltd., TINUVIN 400, 405, 460, 477, and 479 manufactured by BASF Corporation, and CYASORB UV-1164 manufactured by Sun Chemical Co., Ltd.

[0224] Examples of salicylic acid ester antioxidants include phenyl salicylate, p-octylphenyl salicylate, p-tert-butylphenyl salicylate, etc. In addition, oligomer type and polymer type compounds having a salicylic acid ester structure can also be used.

[0225] These antioxidants may be used alone or in combination of two or more kinds in any ratio as required.

[0226] The content of the antioxidant is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, even more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, based on 100% by mass of the resin composition, from the viewpoint of suppressing thermal deterioration of the resin composition. From the viewpoint of suppressing deterioration of the balance of the physical properties of the resin composition, the content is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 2% by mass or less.

[0227] <Conductive carbon-based filler> In the first to third embodiments, the resin composition may further contain a conductive carbonaceous filler. This makes it possible to obtain a conductive resin composition. Preferred conductive carbonaceous fillers include carbon black, carbon fiber, graphite, graphene, carbon nanotubes, and the like. These may also function as colorants. The conductive carbonaceous fillers may be in the form of granules, flakes, or fibers. Specific examples of preferred conductive carbonaceous fillers include conductive carbon black, carbon nanotubes (CNT), carbon fiber, graphite, and the like, and among these, conductive carbon black and CNT are most preferred.

[0228] In the first and second embodiments, the dibutyl phthalate (DBP) absorption of the conductive carbon black is preferably 250 ml / 100 g or more, more preferably 300 ml / 100 g or more, and even more preferably 350 ml / 100 g or more. In the present disclosure, the DBP absorption is a value measured by a method defined in ASTM D2414. The upper limit of the DBP absorption is not particularly limited, but may be, for example, 400 ml / 100 g or less from the viewpoint of availability. Furthermore, the conductive carbon black is preferably a carbon black having a BET surface area of ​​200 m 2 / g or more is preferable, and 400m 2The upper limit of the BET surface area is not particularly limited, but from the viewpoint of availability, it is preferably, for example, 2000 m 2 / g or less. DBP absorption is 250 ml / 100 g or more, and / or BET surface area is 200 m 2 / g or more, the conductive carbon black is generally used for coloring (usually, the above-mentioned DBP absorption is less than 250 ml / 100 g and the BET surface area is 200 m 2 / g), good electrical conductivity can be achieved with a small amount of addition.

[0229] In the third embodiment, the dibutyl phthalate (DBP) absorption of the conductive carbon black is preferably 20 ml / 100 g or more, more preferably 30 ml / 100 g or more, and even more preferably 50 ml / 100 g or more. The upper limit of the DBP absorption is not particularly limited, but may be, for example, 400 ml / 100 g or less from the viewpoint of availability. Furthermore, the conductive carbon black is preferably one having a BET surface area of ​​20 m 2 / g or more is preferable, and 40m 2 The upper limit of the BET surface area is not particularly limited, but from the viewpoint of availability, it is preferably, for example, 2000 m 2 / g or less.

[0230] In the first to third embodiments, commercially available conductive carbon black includes Ketjenblack EC-600JD and the like.

[0231] Carbon nanotubes (CNTs) are carbon-based fibers with a fiber diameter of 100 nm or less and a hollow structure. CNTs include both single-walled carbon nanotubes, whose tube walls are made of a single layer of carbon, and multi-walled nanotubes, whose tube walls are made of multiple layers of carbon.

[0232] The conductive carbonaceous filler may be treated with any of various known coupling agents and / or sizing agents to improve its adhesion to the resin and / or its handling properties.

[0233] The amount of the conductive carbonaceous filler is preferably 0.1 to 10% by mass when the entire resin composition is taken as 100% by mass. The upper limit is more preferably 8% by mass, even more preferably 6% by mass, and most preferably 3% by mass. The lower limit is more preferably 0.3% by mass, even more preferably 0.5% by mass, and most preferably 0.8% by mass. In order to maintain a stable balance between the conductivity and fluidity of the resin composition, it is desirable to keep the amount within the above range.

[0234] <Agglomeration inhibitor> In the first to third embodiments, the resin composition may further contain an aggregation inhibitor. Since cellulose has a property of agglomerating in a drying process and being difficult to redisperse, it is preferable to use an aggregation inhibitor to improve the redispersibility of cellulose when melt-kneaded with a resin. By increasing the redispersibility, the mechanical properties and stability of the resulting resin composition can be improved. It is preferable to add the aggregation inhibitor to a cellulose aqueous dispersion, and then dry it while applying shear to obtain a cellulose powder.

[0235] The preferred amount of the aggregation inhibitor is 2 to 100 parts by mass relative to 100 parts by mass of cellulose in the resin composition. The lower limit is more preferably 4 parts by mass, even more preferably 5 parts by mass, and most preferably 6 parts by mass. The upper limit is more preferably 80 parts by mass, even more preferably 60 parts by mass, and most preferably 40 parts by mass. In order to improve the dispersibility of cellulose in the resin and to improve the stability of physical properties, it is desirable to keep the amount within the above range.

[0236] The aggregation inhibitor can be at least one selected from the group consisting of surfactants, organic compounds having a boiling point of 100° C. or higher, and resins having a chemical structure capable of highly dispersing cellulose.

[0237] The surfactant may have a chemical structure in which a moiety having a hydrophilic substituent and a moiety having a hydrophobic substituent are covalently bonded, and may be one that is used for various purposes such as food, industrial, etc. For example, the following may be used alone or in combination of two or more:

[0238] The surfactant may be any of anionic surfactants, nonionic surfactants, amphoteric surfactants, and cationic surfactants. From the viewpoint of affinity with cellulose, however, anionic surfactants and nonionic surfactants are preferred, and nonionic surfactants are more preferred.

[0239] Among the above, from the viewpoint of affinity with cellulose, surfactants having a polyoxyethylene chain, a carboxyl group, or a hydroxyl group as a hydrophilic group are preferred, polyoxyethylene-based surfactants (polyoxyethylene derivatives) having a polyoxyethylene chain as a hydrophilic group are more preferred, and nonionic polyoxyethylene derivatives are even more preferred. The polyoxyethylene chain length of the polyoxyethylene derivative is preferably 3 or more, more preferably 5 or more, even more preferably 10 or more, and particularly preferably 15 or more. The longer the chain length, the higher the affinity with cellulose, but in terms of the balance with coating properties, the upper limit is preferably 60 or less, more preferably 50 or less, even more preferably 40 or less, particularly preferably 30 or less, and most preferably 20 or less.

[0240] Among the above-mentioned surfactants, the hydrophobic group of alkyl ether type, alkyl phenyl ether type, rosin ester type, bisphenol A type, β-naphthyl type, styrenated phenyl type, and hardened castor oil type can be preferably used because they have high affinity with resin. The preferred alkyl chain length (in the case of alkyl phenyl, the number of carbon atoms excluding the phenyl group) is preferably 5 or more, more preferably 10 or more, even more preferably 12 or more, and particularly preferably 16 or more. When the resin is polyolefin, the higher the carbon number, the higher the affinity with the resin, so there is no upper limit, but from the viewpoint of handleability, the upper limit is preferably 30 or less, more preferably 25 or less.

[0241] Among these hydrophobic groups, those having a cyclic structure or those having a bulky and multifunctional structure are preferred. As those having a cyclic structure, alkylphenyl ether type, rosin ester type, bisphenol A type, β-naphthyl type, and styrenated phenyl type are preferred, and as those having a multifunctional structure, hydrogenated castor oil type is preferred. Among these, rosin ester type and hydrogenated castor oil type are particularly more preferred.

[0242] In addition, organic compounds with a boiling point of 100°C or higher may be effective as a non-surfactant dispersion medium. Examples of such organic compounds include polyethylene glycol, polypropylene glycol, and organic compounds having a glycerin structure. In addition, depending on the type of resin, for example, when the resin is a polyolefin, high-boiling organic solvents such as liquid paraffin and decalin are effective. In addition, when the resin is a polar resin such as nylon and polyacetate, it may be effective to use a solvent similar to the aprotic solvent that can be used in producing cellulose, such as dimethyl sulfoxide.

[0243] <Coloring agent> In the first to third embodiments, the resin composition may further contain a colorant. Among them, organic colorants are advantageous in that they have the effect of improving the toughness of the resin composition. Examples of organic colorants include azine compounds (such as nigrosine), aniline black, cyanine compounds (such as phthalocyanine and naphthalocyanine), porphyrin, perylene, quaterrylene, metal complexes, azo dyes, anthraquinone, squaric acid derivatives, immonium dyes, and the like, and nigrosine is particularly preferred. Nigrosine is a component known to those skilled in the art as a black azine condensation mixture, and those described in the Colour Index as CISOLVENT BLACK 5, CISOLVENT BLACK 7, and the like are known. Specific examples of nigrosine include triphenazine oxazine and phenazine azine. Examples of commercially available Nigrosine products include Nubian Black PA-9801, Nubian Black PA-9800, and Nubian Black PA-0800 (all available from Orient Chemical Industry Co., Ltd.). Nigrosine not only functions as a colorant, but also has the effect of delaying the crystallization of polyamide during the production of a resin composition, particularly during cooling after melt kneading, and therefore can improve the toughness of the resin composition and suppress the occurrence of defects, thereby reducing the variation in toughness of the resin composition.

[0244] The content of nigrosine in 100% by mass of the resin composition is preferably 0.001% by mass or more, or 0.01% by mass or more, or 0.03% by mass or more, from the viewpoint of obtaining the above-mentioned effects by using nigrosine well, and is preferably 1% by mass or less, or 0.5% by mass or less, or 0.3% by mass or less, from the viewpoint of dimensional stability.

[0245] <Other ingredients> In the first to third embodiments, the resin composition may contain, as other components, additives such as, for example, a fine fiber filler component made of a highly heat-resistant organic polymer other than cellulose (for example, fibrillated fiber or fine fiber of aramid fiber); a compatibilizer; a plasticizer; polysaccharides such as starches and alginic acid; natural proteins such as gelatin, glue, and casein; inorganic compounds such as zeolite, ceramics, talc, silica, metal oxides, and metal powders; fragrances; pigments; flow regulators; leveling agents; conductive agents; antistatic agents; ultraviolet absorbers; ultraviolet dispersants; and deodorants. The content ratio of the above other components in the resin composition is appropriately selected within a range in which the desired effects of the present invention are not impaired.

[0246] <Production of resin composition> There is no particular limitation on the method for producing the resin compositions of the first to third embodiments, but specific examples include the following methods: Using a single-screw or twin-screw extruder, a mixture of a first polymer (i.e., polyamide), a second polymer (e.g., polyphenylene ether), cellulose (e.g., cellulose nanofiber), and an arbitrary elastomer (first embodiment), a mixture of a polyamide, an elastomer, and a cellulose (second embodiment), or a mixture of a polyamide, a saponified ethylene-vinyl ester copolymer, and a cellulose, and an arbitrary elastomer (third embodiment) is melt-kneaded, extruded into a strand shape, and cooled and solidified in a water bath to obtain a pellet-shaped molded product; using a single-screw or twin-screw extruder, melt-kneaded in the same manner, extruded into a rod or cylinder shape, and cooled to obtain an extrusion molded product; and using a single-screw or twin-screw extruder, melt-kneaded, and extruded from a T-die to obtain a sheet or film-shaped molded product.

[0247] <Shape of resin composition> The resin compositions of the first to third embodiments can be provided in various shapes. Specifically, resin pellets, sheets, fibers, plates, rods, etc. can be mentioned, but the resin pellet shape is more preferable from the viewpoint of ease of post-processing and ease of transportation. In this case, preferred pellet shapes include round, elliptical, and cylindrical shapes, which differ depending on the cutting method during extrusion processing. Pellets cut by a cutting method called underwater cutting are often round, pellets cut by a cutting method called hot cutting are often round or elliptical, and pellets cut by a cutting method called strand cutting are often cylindrical. In the case of round pellets, the preferred size is 1 mm or more and 3 mm or less in terms of pellet diameter. In the case of cylindrical pellets, the preferred diameter is 1 mm or more and 3 mm or less, and the preferred length is 2 mm or more and 10 mm or less. It is desirable to set the above diameter and length to be equal to or more than the lower limit from the viewpoint of operational stability during extrusion, and it is desirable to set them to be equal to or less than the upper limit from the viewpoint of biting into the molding machine in post-processing.

[0248] The resin compositions of the first to third embodiments can be used as various resin molded products. There is no particular limitation on the manufacturing method of the resin molded product, and any manufacturing method may be used, but injection molding, extrusion molding, blow molding, inflation molding, foam molding, etc. can be used. Among these, injection molding is most preferable from the viewpoint of design and cost.

[0249] <Characteristics of resin composition> In the resin compositions of the first to third embodiments, from the viewpoint of eliminating strength defects of the obtained molded article, it is preferable to set the coefficient of variation CV of the tensile breaking strength to 10% or less. The coefficient of variation here is expressed as a percentage obtained by dividing the standard deviation (σ) by the arithmetic mean (μ) and multiplying the result by 100, and is a unitless number that indicates relative variation. CV = (σ / μ) × 100 Here, μ and σ are given by the following equations.

[0250]

number

[0251] The number of samples (n) used to calculate the coefficient of variation CV of the tensile breaking strength is preferably at least 10, and more preferably 15 or more, in order to make it easier to find defects.

[0252] A more preferable upper limit of the coefficient of variation is 9%, further preferably 8%, more preferably 7%, further more preferably 6%, and most preferably 5%. A preferable lower limit is zero, but from the viewpoint of ease of production, it is preferably 0.1%.

[0253] Localized strength defects in conventional resin molded products are thought to be caused by uneven distribution of fillers, formation of voids, etc. One method for evaluating the susceptibility of these strength defects to form is to carry out tensile tests on multiple test pieces and check the presence and number of variations in breaking strength.

[0254] For example, if there are unevenly dispersed filler areas or voids in molded structural parts such as automobile bodies, door panels, and bumpers, when a large stress is applied instantaneously to the molded part, or when a small stress such as vibration is applied repeatedly, the stress will be concentrated and the molded part will be destroyed, which will reduce the reliability of the product.

[0255] Until now, it has been difficult to predict structural defects that may occur in actual products at the testing stage, and methods such as checking defective areas in the product with a microscope have been used. However, observations with a microscope are extremely microscopic, and cannot comprehensively evaluate the entire test piece or the entire product.

[0256] In the course of various investigations, the present inventors have found that there is a correlation between the coefficient of variation of tensile breaking strength and the proportion of structural defects in a product.

[0257] To explain in more detail, for example, if a material has a homogeneous internal structure and does not have voids, the stress at which the material breaks will be almost the same for multiple samples when tensile tests are performed on the samples, and the coefficient of variation will be very small. However, for materials that have internal non-uniformities, voids, etc., the stress at which a sample breaks will be significantly different from the stress of the other samples. The degree to which there are many samples that exhibit a stress different from the stress of the other samples can be clarified by using a measure called the coefficient of variation.

[0258] For example, in the case of a material that does not have a yield strength, a sample with an internal defect breaks at a lower strength than the other samples. In the case of a material that has a yield strength, after reaching yield, it often breaks on the way to necking, and a sample with an internal defect tends to break at a higher strength than the other samples. Although there are differences in behavior, the possibility of occurrence of strength defects in actual products can be predicted by the measure of the coefficient of variation of the tensile breaking strength.

[0259] It is considered that the dispersion state and dispersion position of cellulose in the composition have a large effect on the coefficient of variation of tensile breaking strength. In addition, for example, in the case of the polyamide / elastomer alloy of the second embodiment, the elastomer phase and the interface layer between the elastomer and the polyamide are important sites for stabilizing physical properties. For example, if cellulose is localized at the interface between the dispersed phase and the continuous phase, or in the dispersed phase, the localized portion becomes a stress concentration point, and the stability of physical properties decreases. In other words, stably dispersing cellulose in the polyamide phase is advantageous for the stability of physical properties.

[0260] In the first to third embodiments, various methods can be mentioned as a method for stably dispersing cellulose in a polyamide phase. For example, in the first embodiment, various approaches can be mentioned, such as a method for optimizing the composition ratio of polyamide to the sum of polyphenylene ether and any elastomer, a method for optimizing the amount of acidic functional groups of polyphenylene ether and any elastomer, a method for optimizing the end group concentration of polyamide, a method for optimizing the order of addition during kneading of cellulose, a method for weakening the affinity between polyphenylene ether and cellulose or increasing the affinity between polyamide and cellulose by adding an optimal surfactant or the like, a method for melt-mixing polyamide and cellulose in advance to prepare a master batch, a method for optimizing the screw arrangement during extrusion processing, and a method for optimizing the resin viscosity by controlling the temperature during processing. In addition, for example, in the second embodiment, various approaches can be mentioned, such as a method of optimizing the composition ratio of polyamide and elastomer, a method of optimizing the amount of acidic functional groups in the elastomer, a method of optimizing the terminal group concentration of the polyamide, a method of optimizing the order of addition during kneading of cellulose, a method of weakening the affinity between the elastomer and cellulose or increasing the affinity between the elastomer and polyamide by adding an optimal surfactant or the like, a method of melt-mixing polyamide and cellulose in advance to prepare a master batch, a method of optimizing the screw arrangement during extrusion processing, and a method of optimizing the resin viscosity by controlling the temperature during processing.

[0261] In addition to the above, the heat resistance of cellulose is improved and structural defects caused by thermal degradation during kneading with a resin are prevented from occurring, thereby increasing the stability of physical properties.

[0262] Any of these approaches may be adopted to stably disperse cellulose in the polyamide phase. Setting the coefficient of variation CV of the tensile breaking strength to 10% or less can greatly contribute to eliminating strength defects of the obtained molded article, and has the effect of significantly improving the reliability of the strength of the molded article.

[0263] In the resin compositions of the first to third embodiments, the tensile yield strength tends to be dramatically improved compared to the thermoplastic resin alone. The ratio of the tensile yield strength of the resin composition to the tensile yield strength of the thermoplastic resin alone taken as 1.0 is preferably 1.1 times or more, more preferably 1.15 times or more, even more preferably 1.2 times or more, and most preferably 1.3 times or more. The upper limit of the ratio is not particularly limited, but from the viewpoint of ease of production, it is preferably, for example, 5.0 times, more preferably 4.0 times.

[0264] Since the resin compositions of the first to third embodiments contain cellulose, they can exhibit low thermal expansion without increasing the specific gravity. Specifically, the thermal expansion coefficient of the resin composition in the temperature range of 20°C to 100°C is preferably 70 ppm / K or less, more preferably 60 ppm / K or less, more preferably 50 ppm / K or less, more preferably 45 ppm / K or less, even more preferably 40 ppm / K or less, and most preferably 35 ppm / K or less. The lower limit of the thermal expansion coefficient is not particularly limited, but from the viewpoint of ease of production, it is preferably, for example, 5 ppm / K, more preferably 10 ppm / K.

[0265] In the resin compositions of the first to third embodiments, the cellulose can be stably finely dispersed in the polyamide phase, and the composition can have a feature that the variation in the linear expansion coefficient in a large molded product is small. Specifically, the composition can have a feature that the variation in the linear expansion coefficient measured using test pieces taken from different parts of the large molded product is very low.

[0266] When the dispersion of cellulose in the resin composition is non-uniform and the linear expansion coefficient differs greatly from one part to another, the molded product is likely to suffer from defects such as distortion or warping due to temperature changes. Moreover, this defect is caused by differences in thermal expansion and is a failure mode that occurs reversibly when the temperature rises or falls. Therefore, it can be a failure mode with potential danger that cannot be recognized by checking at room temperature.

[0267] The magnitude of variation in the linear expansion coefficient can be expressed by the coefficient of variation of the linear expansion coefficient of measurement samples obtained from different parts of the body. The coefficient of variation here is calculated in the same way as explained above in the section on the coefficient of variation of the tensile breaking strength.

[0268] The coefficient of variation of the linear expansion coefficient in the resin compositions of the first to third embodiments is preferably 15% or less. The upper limit of the coefficient of variation is more preferably 13%, further preferably 11%, even more preferably 10%, further more preferably 9%, and most preferably 8%. The lower limit is preferably zero, but is preferably 0.1% from the viewpoint of ease of production.

[0269] The number of samples (n) used to calculate the coefficient of variation of the linear expansion coefficient is desirably at least 10 in order to reduce the influence of data errors and the like.

[0270] <Tensile breaking strain> In the first embodiment, the tensile breaking strain of the resin composition is preferably 10% or more, or 20% or more, or 30% or more, or 40% or more, or 50% or more. Such a resin composition is preferable because it has excellent toughness. The tensile breaking strain of the resin composition is preferably high, but from the viewpoint of ease of production of the resin composition, it may be, for example, 500% or less, 200% or less, or 100% or less. The tensile breaking strain is a value obtained as the strain at break when a tensile test is performed on a strip test piece having a length of 70 mm, a width of 10 mm, and a thickness of 2 mm using a tensile tester at a temperature of 23° C., a relative humidity of 50%, a chuck distance of 40 mm, and a tensile speed of 5 mm / min.

[0271] In the second and third embodiments, the tensile break strain of the resin composition is preferably 10% or more, or 20% or more, or 30% or more, or 40% or more, or 50% or more. Such a resin composition is preferable because it has excellent toughness. The tensile break strain of the resin composition is preferably high, but from the viewpoint of ease of production of the resin composition, it may be, for example, 500% or less, 200% or less, or 100% or less. The tensile break strain is a value obtained as the arithmetic average of five data points of strain at break when a tensile test is performed on an ISO 37 type 3 test piece using a tensile tester at a temperature of 23°C and a relative humidity of 50% at a tensile speed of 5 mm / min.

[0272] The resin compositions according to the first to third embodiments have the advantage of small physical property anisotropy. In the center of a multipurpose test piece obtained by molding the resin composition in accordance with ISO294-1, the degree of orientation of cellulose (particularly the degree of orientation of cellulose nanofibers) determined by small-angle X-ray scattering is preferably 0.45 or less, or 0.40 or less, or 0.35 or less, or 0.30 or less, or 0.25 or less, or 0.20 or less, in terms of small physical property anisotropy. The smaller the degree of orientation, the more preferable it is, but from the viewpoint of ease of production of the resin composition, it may be, for example, 0.01 or more, or 0.05 or more, or 0.10 or more. EXAMPLES

[0273] More specific embodiments of the present invention will be described below with reference to examples, but the present invention is not limited to these examples in any way.

[0274] -Example I (first embodiment)- ≪Materials used≫ <Polyamide> (1) Polyamide 6 (PA6) Carboxyl end group ratio: ([COOH] / [total end groups]) = 0.7 Viscosity number (VN) of polyamide measured in 96% sulfuric acid according to ISO307 = 95 (2) Polyamide 66 (PA66) Carboxyl end group ratio: ([COOH] / [total end groups]) = 0.6 Viscosity number (VN) of polyamide measured in 96% sulfuric acid according to ISO307 = 118 (3) Polyamide 610 (PA610) Carboxyl end group ratio: ([COOH] / [total end groups]) = 0.5 Viscosity number (VN) of polyamide measured in 96% sulfuric acid according to ISO307 = 115 (4) Polyamide 12 (PA12) Carboxyl end group ratio: ([COOH] / [total end groups]) = 0.6 Viscosity number (VN) of polyamide measured in 96% sulfuric acid according to ISO307 = 98

[0275] <Polyphenylene ether (amorphous resin)> (1) Polyphenylene ether (hereinafter simply referred to as PPE) Poly(2,6-dimethyl-1,4-phenylene ether) Intrinsic viscosity [η]: 0.40 dl / g, glass transition temperature: 210°C (2) Maleic anhydride modified polyphenylene ether (hereinafter simply referred to as m-PPE) To 100 parts by mass of PPE, 0.1 parts by mass of radical initiator and 1.5 parts by mass of maleic anhydride were added, and the mixture was melt-kneaded using a twin-screw extruder at a cylinder temperature of 320° C. The maleic anhydride addition rate of m-PPE was 0.5%, and the glass transition point was 210° C.

[0276] <Elastomer> (1) Maleic anhydride modified styrene-ethylene butylene-styrene block copolymer (hereinafter simply referred to as m-SEBS) To Tuftec H1052 (Asahi Kasei Corporation), a styrene-ethylenebutylene-styrene block copolymer with a bound styrene content of 20% by mass, 0.15 parts by mass of a radical initiator and 1.4 parts by mass of maleic anhydride were added, and the mixture was melt-kneaded using a twin-screw extruder at a cylinder temperature of 230° C. The maleic anhydride addition rate of m-SEBS was 0.9%, the MFR (230° C., 2.16 kgf) was 8 g / 10 min, and the glass transition point was −48° C. (2) Maleic anhydride modified ethylene-octene copolymer (hereinafter simply referred to as m-EOR) Fusabond MN-493D (DowDuPont) MFR(190℃, 2.16kgf)=1.2g / 10min Octene content = 28% by mass Melting point = 55°C (DSC method: heating rate 10°C / min) Glass transition temperature = -55℃ (3) Styrene-ethylene butylene-styrene block copolymer (hereinafter simply referred to as SEBS) Taipole 6151 (TSRC Taiping Corporation) Styrene content = 33% by mass Weight average molecular weight = 270,000 Glass transition temperature = -48℃

[0277] (4) Styrene-butadiene-styrene block copolymer (hereinafter simply referred to as SBS1) Asaprene T-437 (Asahi Kasei Corporation) Styrene content = 30% by mass MFR(200℃, 5kgf)=2g / 10min Glass transition temperature = -75℃ (5) Styrene-butadiene-styrene block copolymer (hereinafter simply referred to as SBS2) Tufprene A (Asahi Kasei Corporation) Styrene content = 40% by mass MFR(200℃, 5kgf)=13g / 10min Glass transition temperature = -75℃ (6) Styrene-butadiene-styrene block copolymer (hereinafter simply referred to as SBS3) Tufprene T-438 (Asahi Kasei Corporation) Styrene content = 35% by mass MFR(200℃, 5kgf)=25g / 10min Glass transition temperature = -75℃

[0278] <Antioxidants> Irganox 1010 (BASF Japan Ltd.)

[0279] <Hydrophobic CNF> (defibration process) The raw material, linter pulp, was stirred in dimethyl sulfoxide (DMSO) at room temperature for 1 hour at 500 rpm using a single-shaft mixer (Imex DKV-1 φ125 mm dissolver).The mixture was then fed to a bead mill (Imex NVM-1.5) using a hose pump and circulated for 120 minutes using only DMSO to obtain a defibrated slurry.

[0280] (Defibrillation and acetylation process) Then, 11 parts by mass of vinyl acetate and 1.63 parts by mass of sodium bicarbonate were added to the bead mill device per 100 parts by mass of the defibrated slurry, and the device was further circulated for 60 minutes to obtain a hydrophobic CNF slurry.

[0281] During circulation operation, the rotation speed of the bead mill was 2500 rpm and the peripheral speed was 12 m / s. The beads used were made of zirconia and had a diameter of 2.0 mm, and the filling rate was 70% (the slit gap of the bead mill at this time was 0.6 mm). During circulation operation, the slurry temperature was controlled at 40°C using a chiller to absorb heat generated by friction.

[0282] To the obtained hydrophobized CNF slurry, 192 parts by mass of pure water was added per 100 parts by mass of defibrated slurry, and after thorough stirring, it was concentrated in a dehydrator. The obtained wet cake was dispersed again in the same amount of pure water, stirred, and concentrated, and this washing procedure was repeated a total of five times.

[0283] When the properties of the obtained hydrophobized CNF (in the form of a wet cake or a porous sheet) were evaluated, the degree of acyl substitution DS (degree of acetylation) was 0.9, the crystallinity was 75%, the average fiber diameter was 65 nm, L / D was 30 or more (about 450), Mw was 340,000, the Mw / Mn ratio was 5.4, and the average content rate of alkali-soluble polysaccharides was 3.4% by mass.

[0284] To 100 parts by mass of the obtained aqueous dispersion of hydrophobized CNF (solid content rate: 10% by mass), 5 parts by mass of PEG20000 was added, and then the mixture was vacuum dried at about 40 °C using a stirrer of the revolution and rotation type (High Vis Mix 2P-1 manufactured by Primix Corporation) to obtain a hydrophobized CNF powder.

[0285] ≪Evaluation method≫ <Evaluation of polymer> [Melting point] Regarding the polymer pellets, when the temperature was raised from 23 °C at a rate of 10 °C / min using a differential scanning calorimeter (DSC8500 manufactured by PERKINELMER), the peak top temperature of the endothermic peak that appeared was measured. When two or more endothermic peaks appeared, the peak top temperature of the peak on the lowest temperature side was taken as the melting point.

[0286] [Glass transition point] Regarding the central part of a plate-shaped multipurpose test piece obtained by molding the polymer in accordance with ISO294-1, when the temperature was raised from -100 °C at a rate of 2 °C / min using a dynamic viscoelasticity measuring device (ARES G2 manufactured by TA Instruments) and measured under the conditions of an applied frequency of 10 Hz, the temperature at the peak top of the peak where the storage elastic modulus decreased significantly and the loss elastic modulus became maximum was measured. When two or more peaks of the loss elastic modulus appeared, the peak top temperature of the peak on the lowest temperature side was taken as the glass transition point.

[0287] <Evaluation of CNF> [Production of porous sheet] First, the wet cake was added to tert-butanol, and further dispersed using a mixer or the like until no aggregates were formed. The concentration was adjusted to 0.5% by mass per 0.5 g of CNF solids. 100 g of the resulting tert-butanol dispersion was filtered on filter paper, dried at 150°C, and the filter paper was peeled off to obtain a sheet. The air resistance of this sheet was 10 g / m2. 2 The porous sheets with a permeability of 100 sec / 100 ml or less were used as measurement samples. The basis weight W (g / m2) of the sample left standing for one day in an environment of 23°C and 50% RH 2 After measuring the air permeability, the air permeability resistance R (sec / 100ml) was measured using an Oken air permeability tester (manufactured by Asahi Seiko Co., Ltd., model EG01). 2 The value per unit area was calculated. Weight 10g / m 2 Air resistance per unit (sec / 100ml) = R / W x 10

[0288] [Acyl Substitution Degree (DS)] The infrared spectrum of the porous sheet at five points was measured by the ATR-IR method using a Fourier transform infrared spectrophotometer (FT / IR-6200 manufactured by JASCO Co., Ltd.) The infrared spectrum measurement was performed under the following conditions. Number of times accumulated: 64 times, Wavenumber resolution: 4cm -1 , Measurement wave number range: 4000~600cm -1 , ATR crystal: Diamond, Incident angle: 45° From the obtained IR spectrum, the IR index was calculated according to the following formula (1): IR index = H1730 / H1030 (1) In the formula, H1730 and H1030 are at 1730 cm -1 , 1030cm -1 (absorption band of CO stretching vibration of cellulose backbone chain) -1 and 1500cm -1The line connecting the -1 and 1500cm -1 The line connecting these points is taken as the baseline, and the absorbance is calculated when this baseline is taken as 0. Then, the average degree of substitution at each measurement site was calculated from the IR index according to the following formula (2), and the average value was taken as DS. DS = 4.13 × IR index (2)

[0289] [Crystallization degree] The porous sheet was subjected to X-ray diffraction measurement, and the crystallinity was calculated according to the following formula. Crystallinity (%)=[I (200) -I (amorphous) ] / I (200) ×100 I (200) : Diffraction peak intensity due to 200 plane (2θ=22.5°) in cellulose I crystal I (amorphous) : The halo peak intensity due to the amorphous phase in cellulose I crystals, which is the peak intensity at an angle 4.5° lower than the diffraction angle of the 200 plane (2θ=18.0°) (X-ray diffraction measurement conditions) Equipment: MiniFlex (Rigaku Corporation) Operation axis 2θ / θ Source CuKα Measurement method: Continuous Voltage 40kV Current 15mA Starting angle 2θ=5° End angle 2θ=30° Sampling width 0.020° Scan speed: 2.0° / min Sample: A porous sheet is attached onto the sample holder.

[0290] [Average fiber diameter, L / D] The wet cake was diluted to 0.01% by mass with tert-butanol, dispersed using a high-shear homogenizer (IKA, product name "Ultra Turrax T18") at 25,000 rpm for 5 minutes, cast onto mica, air-dried, and measured with a high-resolution scanning microscope. The magnification was adjusted so that at least 100 cellulose fibers could be observed, and the length (L), major axis (D), and ratio of these were determined for 100 randomly selected cellulose fibers, and the arithmetic average of the 100 cellulose fibers was calculated.

[0291] [Weight average molecular weight (Mw), number average molecular weight (Mn) and Mw / Mn ratio] 0.88 g of the porous sheet was weighed, cut into small pieces with scissors, lightly stirred, 20 mL of pure water was added, and left for one day. Next, the water and solids were separated by centrifugation. Next, 20 mL of acetone was added, lightly stirred, and left for one day. Next, the acetone and solids were separated by centrifugation. Next, 20 mL of N,N-dimethylacetamide was added, lightly stirred, and left for one day. N,N-dimethylacetamide and solids were separated again by centrifugation, then 20 mL of N,N-dimethylacetamide was added, lightly stirred, and left for one day. N,N-dimethylacetamide and solids were separated by centrifugation, and 19.2 g of N,N-dimethylacetamide solution prepared so that lithium chloride was 8 mass percent was added to the solids, stirred with a stirrer, and visually confirmed to be dissolved. The solution in which cellulose was dissolved was filtered through a 0.45 μm filter, and the filtrate was used as a sample for gel permeation chromatography. The apparatus and measurement conditions used are as follows. Equipment: Tosoh HLC-8120 Column: TSKgel SuperAWM-H (6.0mm I.D. x 15cm) x 2 Detector: RI detector Eluent: N,N-dimethylacetamide (lithium chloride 0.2%) Flow rate: 0.6mL / min Calibration curve: Pullulan conversion

[0292] [Average content of alkali-soluble polysaccharides] The alkali-soluble polysaccharide content was calculated by subtracting the α-cellulose content from the holocellulose content (Wise method) according to the method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pp. 92-97, 2000) for CNF. The alkali-soluble polysaccharide content was calculated three times for each sample, and the number average of the calculated alkali-soluble polysaccharide contents was taken as the average alkali-soluble polysaccharide content of the CNF.

[0293] <Fender's evaluation> [Fender molding] The pellets thus obtained were used in an injection molding machine with a maximum clamping pressure of 4000 tons, the cylinder temperature of which was set to 260°C, and a predetermined mold (cavity volume: approximately 1400 cm) capable of molding a fender having the shape shown in the schematic diagrams of Figures 6 and 7 was molded. 3 , average thickness: 2mm, projected area: approx. 7000cm 2 The fenders were molded using a hot runner: 1), number of gates: 5-point gate, and a mold temperature of 80°C.

[0294] [Polyamide phase ratio in CNF] With reference to Figure 7, a sample cut from the position (9) of the fender was observed under a transmission electron microscope to confirm the area (CNFp) indicating the amount of cellulose present in the polyamide phase and the area (CNFo) indicating the amount of cellulose present in the other phases. At this time, the polyamide phase and the other phases were each appropriately stained with a known staining agent so that the cellulose could be clearly confirmed. The polyamide phase ratio of CNF was calculated using the following formula. Polyamide phase ratio of CNF = CNFp / (CNFp+CNFo)

[0295] [Water absorption rate] Referring to FIG. 7, a small flat test piece measuring 10 mm long, 10 mm wide, and 2 mm thick was cut from the fender at position (10) into a square of approximately 10 mm. The weight (Wb) of the test piece before water absorption was measured. The test piece was immersed in 80°C hot water for 17 hours, then exposed to 80°C and 57 RH% conditions in a constant temperature and humidity chamber for 100 hours, and then left in a constant temperature and humidity chamber at 23°C and 50 RH% for 24 hours. The weight (Wa) of the test piece after water absorption was measured. The water absorption rate was calculated using the following formula. Water absorption rate=(Wa-Wb) / Wb×100

[0296] [Linear expansion coefficient] Referring to Figure 7, a rectangular test piece measuring 10 mm in the resin flow direction, 5 mm in the direction perpendicular to the resin flow direction, and 2 mm thick was taken from the fender at position (1). The expansion rate in the resin flow direction during molding was measured in the measurement temperature range of -10°C to 120°C in accordance with ISO11359-2, and the expansion coefficient between 20°C and 100°C was calculated. Prior to the measurement, the piece was left to stand in a 120°C environment for 5 hours for annealing.

[0297] [Linear expansion anisotropy] Regarding the linear expansion coefficient, the expansion rate in the direction perpendicular to the flow direction of the resin during molding was measured in the measurement temperature range of -10°C to 120°C in accordance with ISO11359-2, and the expansion coefficient was calculated between 20°C and 100°C. Prior to the measurement, the sample was left to stand in a 120°C environment for 5 hours for annealing. The linear expansion anisotropy was calculated by the following formula. Linear expansion anisotropy = Linear expansion coefficient in the direction of resin flow during molding / Linear expansion coefficient in the direction perpendicular to the direction of resin flow during molding

[0298] [Tensile strain at break] Referring to Figure 7, a rectangular test piece measuring 70 mm in the resin flow direction, 10 mm in the direction perpendicular to the resin flow direction, and 2 mm thick was taken from the fender at position (2). A tensile test was performed using a tensile testing machine (Shimadzu Corporation, Autograph AG-IS) with a chuck distance of 40 mm, a tensile speed of 5 mm / min, and 23°C and 50% RH. The strain at break was recorded as the tensile break strain.

[0299] [Cellulose orientation] The resin composition was molded in accordance with ISO294-1 to obtain a plate-shaped multipurpose test piece. X-rays were irradiated perpendicularly to the plate surface at the center of the plate, and the orientation degree of cellulose was determined by small-angle X-ray scattering. Specifically, a one-dimensional scattering profile was obtained by circular averaging of the two-dimensional scattering pattern obtained by small-angle X-ray scattering measurement, and after background correction, a one-dimensional scattering profile was obtained by circular averaging of the two-dimensional scattering pattern obtained by small-angle X-ray scattering measurement. <q<0.07 nm -1 The azimuth angle dependence of the scattering intensity in the range of q = 4πsinθ / λ (λ: wavelength of X-ray, 2θ: scattering angle). Based on this result, the degree of orientation is calculated as follows: <p2>was calculated.

[0300] Considering three perpendicular axes, and assuming that the angles between the cellulose fiber axis direction and each of the three axes are α, β, and γ, the following equation holds:

number

[0301] If the angle between the flow direction during molding of the multipurpose test piece and the cellulose fiber axis is α and the cellulose is considered symmetrical around the flow direction, the following equation holds:

number

[0302] Since scattering from the cellulose surface occurs in the β direction perpendicular to α, <cos 2 β> can be calculated using the following formula.

number

[0303] Therefore, the degree of orientation of the cellulose fiber axis <p2>is expressed by the following formula:

number

[0304] In this case, if the flow direction is completely oriented <p2>is 1, and in the case of no orientation it is 0.

[0305] (Small angle X-ray scattering measurement conditions) Equipment: Rigaku NANOPIX X-ray wavelength: 0.154nm Optical system: Point collimation (1st: 0.55mmφ, 2nd: Open, guard: 0.35mmφ) Detector: HyPix-6000 (2D semiconductor detector) Camera length: 1312mm Exposure time: 15 min / sample Environment around the sample cell: Air Test piece arrangement: Multipurpose test pieces are arranged so that the flow direction of the resin composition during molding is the left-right direction. X-ray incidence direction: perpendicular to the plate surface of the multi-purpose test piece

[0306] <Composite manufacturing> [Extruder Design] A twin-screw extruder (TEM SX series extruder manufactured by Toshiba Machine Co., Ltd.) with 13 cylinder blocks and an L / D of 52 was used. A side feed port was installed in cylinder 5 to enable the supply of raw materials from that position, and a vent port for reducing pressure and suction was installed in cylinder 12 to enable the removal of volatile components and coexisting air.

[0307] The screw configuration was as follows: cylinders 1-2 were used as conveying screws, cylinders 3-4 were used as premixing zones with two clockwise kneading discs (feed type kneading discs: hereinafter referred to as RKD), followed by one neutral kneading disc (non-conveying type kneading disc: hereinafter referred to as NKD), followed by a counterclockwise screw, and cylinder 5, which was a side feed zone, was used as a conveying screw, and cylinders 6-7 were used as melt kneading zones with one RKD, two NKDs, followed by one counterclockwise screw. Cylinders 8-9 were used as conveying screws, and cylinder 10 was used as a kneading zone with one RKD, followed by one NKD, followed by a counterclockwise screw. Cylinders 11-13 were used as conveying screws, and were used as devolatilization zones.

[0308] [Example 1-1] A mixture of 34.3 parts by mass (pbw) of m-PPE and 14.3 parts by mass of hydrophobized CNF (including 4.3 parts by mass of PEG 20000) was fed and kneaded from cylinder 1 of an extruder set at water-cooling cylinder 1, 300° C., and 250° C. The mixture was extruded into a strand shape by cutting the strand with a strand cutter to obtain m-PPE / hydrophobized CNF master batch pellets. A mixture of 51.4 parts by mass of PA6 and 48.6 parts by mass of m-PPE / hydrophobized CNF master batch was fed from cylinder 1 of the extruder, which was cooled by water and the other cylinders were set at 250°C, kneaded, and extruded into a strand shape. The strand was cut with a strand cutter to obtain hydrophobized CNF composite pellets. The composition of the obtained composite is shown in Table 1.

[0309] [Example 1-2] Cylinder 1 was water-cooled, cylinder 3 was set at 300°C, and the other cylinders were set at 250°C. 34.3 parts by mass of m-PPE was fed through cylinder 1 of an extruder, and further a mixture of 51.4 parts by mass of PA6 and 14.3 parts by mass of hydrophobic CNF was fed through the side feed port of cylinder 5 and kneaded to obtain hydrophobic CNF composite pellets.

[0310] [Examples 1-3] A mixture of 51.4 parts by mass of PA6 and 14.3 parts by mass of hydrophobic CNF was fed and kneaded from cylinder 1 of an extruder, with cylinder 1 cooled by water and the other cylinders set at 250° C., and extruded into a strand shape. The strand was cut with a strand cutter to obtain PA / hydrophobic CNF master batch pellets. A mixture of 34.3 parts by mass of m-PPE and 65.7 parts by mass of PA / hydrophobized CNF master batch was fed from cylinder 1 of the extruder, with cylinder 1 set to water cooling, cylinder 3 set to 300°C, and the other cylinders set to 250°C, and kneaded and extruded into a strand shape. The strand was cut with a strand cutter to obtain hydrophobized CNF composite pellets. The composition of the obtained composite is shown in Table 1.

[0311] [Examples 1-4] A mixture of 51.4 parts by mass of PA6, 34.3 parts by mass of m-PPE, and 14.3 parts by mass of hydrophobic CNF was fed from cylinder 1 of an extruder, with cylinder 1 set to water cooling, cylinder 3 set to 300° C., and the other cylinders set to 250° C., and kneaded and extruded into a strand shape. The strand was cut with a strand cutter to obtain hydrophobic CNF composite pellets.

[0312] [Comparative Example 1-1] Pellets were obtained in the same manner as in Example 1-4, except that no hydrophobic CNF was used and the materials were kneaded to obtain the composition shown in Table 1.

[0313] [Comparative Example 1-2] Pellets were obtained in the same manner as in Example 1-4, except that the cylinder 3 was set to 250° C., m-PPE was not used, and kneading was performed so as to obtain the composition shown in Table 1.

[0314] [Reference example 1-1] Pellets were obtained in the same manner as in Example 1-4, except that the cylinder 3 was set to 250° C. and kneading was performed so as to obtain the composition shown in Table 1. The composition of the obtained composite is shown in Table 2.

[0315] [Examples 1-5] Cylinder 1 was water-cooled, cylinder 3 was set at 300°C, and the other cylinders were set at 250°C. A mixture of 40 parts by mass of m-PPE and 10 parts by mass of SEBS was fed through cylinder 1 of an extruder, and 50 parts by mass of PA6 was further fed through the side feed port of cylinder 5 and kneaded to obtain resin pellets. A mixture of 87.5 parts by mass of resin pellets and 14.3 parts by mass of hydrophobic CNF was fed from cylinder 1 of the extruder, which was water-cooled and the other cylinders were set at 250°C, kneaded, and extruded into a strand shape. The strand was cut with a strand cutter to obtain hydrophobic CNF composite pellets. The composition of the obtained composite is shown in Table 2.

[0316] [Examples 1-6] Hydrophobized CNF composite pellets were obtained in the same manner as in Example 1-5, except that a mixture of 30 parts by mass of PPE, 10 parts by mass of m-PPE, and 10 parts by mass of SEBS was fed from cylinder 1.

[0317] [Examples 1-7 and 1-8] Hydrophobized CNF composite pellets were obtained in the same manner as in Examples 1-5, except that the materials were kneaded to obtain the composition shown in Table 2.

[0318] [Examples 1-9] Hydrophobized CNF composite pellets were obtained in the same manner as in Example 1-5, except that a mixture of 40 parts by mass of m-PPE and 10 parts by mass of SEBS was fed from cylinder 1, and then a mixture of 45 parts by mass of PA6 and 5 parts by mass of m-EOR was fed and kneaded from the side feed port of cylinder 5.

[0319] [Examples 1-10] Cylinder 1 was set to water cooling, cylinder 3 to 300°C, and the other cylinders to 250°C. A mixture of 50 parts by mass of PA6, 40 parts by mass of m-PPE, 10 parts by mass of SBS1, and 0.2 parts by mass of an antioxidant was fed through cylinder 1 of an extruder and kneaded to obtain resin pellets. A mixture of 87.5 parts by mass of resin pellets and 14.3 parts by mass of hydrophobic CNF was fed and kneaded from cylinder 1 of an extruder, with cylinder 1 cooled by water and the other cylinders set at 250° C., and extruded into a strand shape. The strand was cut with a strand cutter to obtain hydrophobic CNF composite pellets.

[0320] [Examples 1-11 to 1-20] Hydrophobized CNF composite pellets were obtained in the same manner as in Examples 1-10, except that the materials were kneaded to obtain the compositions shown in Tables 2 and 3.

[0321] [Table 1]

[0322] [Table 2]

[0323] [Table 3]

[0324] -Example II (Second embodiment)- ≪Materials used≫ <Polyamide> Carboxy-terminated polyamide 6 (hereinafter referred to simply as PA6) UBE Nylon 1013B (Ube Industries, Ltd.) The amino end group ratio is ([NH2] / ([NH2]+[COOH]))=0.4 Viscosity number (VN) of polyamide measured in 96% by weight sulfuric acid = 95

[0325] <Elastomer> [Elastomers with acidic functional groups] Tufprene T912 (Asahi Kasei Corporation) (hereinafter referred to simply as m-SBS) Maleic anhydride modified styrene-butadiene-styrene block copolymer Bound styrene content = 40% by mass Maleic anhydride addition rate = 0.2 mass% Glass transition temperature = -75℃

[0326] Fusabond MN-493D (DowDuPont) (hereinafter referred to simply as m-EOR) Maleic anhydride modified ethylene-octene copolymer MFR(190℃, 2.16kgf)=1.2g / 10min Octene content = 28% by mass Melting point = 55°C (DSC method: heating rate 10°C / min) Glass transition temperature = -55℃ Maleic anhydride addition rate = 1.0 mass%

[0327] [Elastomers without acidic functional groups] Asaprene T-411 (Asahi Kasei Corporation) (hereinafter referred to simply as SBS) Styrene-butadiene-styrene block copolymer Bound styrene content = 30% by mass Glass transition temperature = -75℃

[0328] <Antioxidants> Irganox 1010 (BASF Japan Ltd.) was used. <Coloring agent> Organic colorant: NUBIANBLACK PA9801 (Orient Chemical Industry Co., Ltd.) Inorganic colorant: Carbon black #52 (Mitsubishi Chemical Holdings Corporation)

[0329] <Cellulose> The same hydrophobic CNF powder was used as prepared in Example I (first embodiment). The properties of the hydrophobic CNF (wet cake) were evaluated and found to be 65 nm in diameter, 30 or more in L / D (approximately 450), 340,000 in weight average molecular weight (Mw), and 0.9 in acetylation degree.

[0330] Evaluation method [Length, diameter, L / D of hydrophobic CNF] The wet cake was suspended in pure water at a concentration of 1% by mass, and dispersed using a high-shear homogenizer (manufactured by Nippon Seiki Co., Ltd., product name "Excel Auto Homogenizer ED-7", processing conditions: rotation speed 15,000 rpm x 5 minutes). The aqueous dispersion was then diluted with pure water to 0.1 to 0.5% by mass, cast onto mica, and air-dried. The ratio (L / D) of the length (L) to the diameter (D) of the particle image obtained when the particle was measured with an atomic force microscope (AFM) was determined, and the average value of 100 to 150 particles was calculated.

[0331] [Confirmation of the continuous phase] The pellets thus obtained were immersed in chloroform to check for any change in shape. Since no particular change occurred in either the Examples or Comparative Examples carried out this time, it was determined that the polyamide formed a continuous phase.

[0332] [Polyamide phase ratio of cellulose] The obtained composition was sliced ​​to a thickness of 1 μm using an ultramicrotome to obtain a film-like sample, which was then immersed in chloroform to elute the elastomer phase, and the eluate was concentrated and ultracentrifuged to separate the cellulose, which was then washed with chloroform and ultracentrifuged three times. The remaining cellulose was dried to determine the amount of cellulose present in the elastomer phase. The amount obtained was subtracted from the amount charged, and the ratio obtained by dividing the amount by the amount of cellulose charged was expressed as a percentage, which was the polyamide phase ratio of cellulose.

[0333] [Number average particle size of dispersed elastomer particles and volume ratio of dispersed particles with a particle size of 1 μm or more] The composition thus obtained was photographed using a transmission electron microscope. The number average diameter (i.e., dispersed particle diameter) of 500 dispersed particles in the dispersed phase of the elastomer and the volume ratio of dispersed particles having a particle diameter of 1 μm or more were calculated.

[0334] [Thermal expansion (coefficient of thermal expansion)] A sample with a length of 10 mm, width of 4 mm, and thickness of 2 mm was cut out from the center of the test piece (ISO 37 type 3) using a precision cut saw. In accordance with ISO11359-2, the expansion rate in the direction of resin flow during molding (MD direction, length direction of the sample) was measured at a measurement temperature range of -10℃ to 120℃, and the coefficient of thermal expansion (hereinafter referred to as CTE) between 20℃ and 100℃ was measured. MD Prior to the measurement, the sample was left to stand in an environment of 120° C. for 5 hours for annealing.

[0335] [Toughness Tensile Breaking Strain] Tensile tests were performed on test pieces (ISO 37 type 3) using a tensile testing machine (Shimadzu Corporation, Autograph AG-IS) at a temperature of 23°C and a relative humidity of 50%, with a tensile speed of 5 mm / min. The arithmetic average of five data points of strain at tensile break was used as an index of toughness.

[0336] <Extrusion conditions> [Extruder Design] Cylinder 1 of the twin-screw extruder (TEM SX series extruder manufactured by Toshiba Machine Co., Ltd.) with 13 cylinder blocks and an L / D of 52 was water-cooled, cylinders 2 to 4 were set at 150°C, and cylinder 5 to the die at 250°C. A vent port for reducing pressure and suction was installed in cylinder 12, allowing the removal of volatile components and coexisting air.

[0337] The screw configuration was as follows: cylinders 1-2 were used as conveying screws, cylinder 3 was provided with three clockwise kneading discs (feed type kneading discs: hereinafter sometimes simply referred to as RKDs) to form a pre-mixing zone, cylinder 4 was used as a conveying screw, and cylinders 5-6 were provided with one RKD, two neutral kneading discs (non-conveying type kneading discs: hereinafter sometimes simply referred to as NKDs), and one counterclockwise screw to form a melt-kneading zone. Cylinders 7-9, which were side feed zones, were used as conveying screws, and cylinder 10 was provided with two RKDs, three NKDs, and a counterclockwise screw to form a kneading zone. Cylinders 11-13 were used as conveying screws, and were used as a devolatilization zone. In addition, a die having two holes with a diameter of 3 mm was attached to the die.

[0338] <Production of resin composition> [Examples 2-1 to 2-6, Comparative Examples 2-1 to 2-2] Using an extruder of the same design, the materials were mixed in the ratios shown in Table 4, melt-kneaded at a screw speed of 300 rpm, and pelletized, after which various evaluations were carried out. The results are shown in Table 4. In the table, the column indicating parts by mass indicates the preparation recipe, the middle column indicating mass % indicates the composition, and the bottom column indicates the physical properties.

[0339] From the results shown in the table, each Example using an aromatic vinyl compound-conjugated diene compound block copolymer or its derivative elastomer showed high breaking strain (i.e., good toughness) and low thermal expansion coefficient, whereas Comparative Example 2-1 using an ethylene-octene copolymer as the elastomer showed a poor thermal expansion coefficient, and Comparative Example 2-2 using no elastomer showed a poor breaking strain. Furthermore, when Examples 2-4, 2-5, and 2-6 using a colorant were compared with Example 2-1 not using a colorant, the results showed that Examples 2-4, 2-5, and 2-6 showed higher breaking strain.

[0340] [Table 4]

[0341] Example III (third embodiment) ≪Materials used≫ <Polyamide> PA6: UBE Nylon 1013B (Ube Industries, Ltd.) Carboxy-rich polyamide 6 The amino end group ratio is ([NH2] / ([NH2]+[COOH]))=0.4 Viscosity number (VN) of polyamide measured in 96% by weight sulfuric acid = 95

[0342] <Elastomer> [Elastomers with acidic functional groups] m-EOR: Fusabond MN-493D (DowDuPont) Maleic anhydride modified ethylene-octene copolymer MFR(190℃, 2.16kgf)=1.2g / 10min Octene content = 28% by mass Melting point = 55°C (DSC method: heating rate 10°C / min) Glass transition temperature = -55℃ Maleic anhydride addition rate = 1.0 mass%

[0343] m-SBS: Tufprene T912 (Asahi Kasei Corporation) Maleic anhydride modified styrene-butadiene-styrene block copolymer Bound styrene content = 40% by mass Maleic anhydride addition rate = 0.2 mass% Glass transition temperature = -75℃

[0344] [Elastomers without acidic functional groups] SBS: Asaprene T-411 (Asahi Kasei Corporation) Styrene-butadiene-styrene block copolymer Bound styrene content = 30% by mass Glass transition temperature = -75℃

[0345] <Saponified ethylene-vinyl ester copolymer> EVOH-1: Soarnol V2504 (Mitsubishi Chemical Holdings Corporation) Ethylene composition=25 mol%, vinyl alcohol composition=75 mol%, melting point=195°C, glass transition point=63°C EVOH-2: EVAL M100B (Kuraray Co., Ltd.) Ethylene composition=24 mol%, vinyl alcohol composition=76 mol%, melting point=195°C, glass transition point=60°C EVOH-3: EVAL L104B (Kuraray Co., Ltd.) Ethylene composition=27 mol%, vinyl alcohol composition=73 mol%, melting point=190°C, glass transition point=63°C EVOH-4: Soarnol DT2904 (Mitsubishi Chemical Holdings Corporation) Ethylene composition=29 mol%, vinyl alcohol composition=71 mol%, melting point=188°C, glass transition point=62°C EVOH-5: Soarnol DC3212 (Mitsubishi Chemical Holdings Corporation) Ethylene composition=32 mol%, vinyl alcohol composition=68 mol%, melting point=183°C, glass transition point=61°C EVOH-6: EVAL C109B (Kuraray Co., Ltd.) Ethylene composition=35 mol%, vinyl alcohol composition=65 mol%, melting point=177°C, glass transition point=58°C

[0346] <Other ingredients> Antioxidant: Irganox 1010 (BASF Japan Ltd.) Organic colorant: NUBIANBLACK PA9801 (Orient Chemical Industry Co., Ltd.) Inorganic colorant: Carbon black #CB960 (Mitsubishi Chemical Holdings Corporation)

[0347] <Cellulose nanofiber> [Preparation Example 1] Cellulose nanofiber (hereinafter referred to as CNF) The linter pulp was cut and then heated in hot water of 120°C or higher for 3 hours using an autoclave, and the refined pulp from which the hemicellulose portion had been removed was squeezed and highly shortened and fibrillated by beating so that the solid content in pure water was 1.5% by mass, and then defibrated at the same concentration using a high-pressure homogenizer (operating pressure: 10 times at 85 MPa) to obtain defibrated cellulose. Here, the beating process used a disc refiner, and the pulp was treated with a beating blade with high cutting function (hereinafter referred to as cutting blade) for 4 hours, and then beaten for an additional 1.5 hours using a beating blade with high defibration function (hereinafter referred to as defibration blade). The properties of the obtained CNF were evaluated and it was found that the diameter was 90 nm and the L / D ratio was more than 30 (approximately 300).

[0348] To the obtained aqueous dispersion of CNF, 5 parts by mass of PEG20000 was added per 100 parts by mass of CNF, and then the mixture was vacuum dried at approximately 40°C using a revolution / rotation type mixer (Hivismix 2P-1, manufactured by Primix Corporation) to obtain CNF powder.

[0349] [Preparation Example 2] Acetylated cellulose nanofiber (hereinafter referred to as acetylated CNF) The same hydrophobized CNF powder was used as prepared in Examples I and II (first and second embodiments). The properties of the acetylated CNF (wet cake) were evaluated, and the diameter was 65 nm, the L / D was 30 or more (about 450), the weight average molecular weight (Mw) was 340,000, and the degree of acetylation was 0.9.

[0350] [Preparation Example 3] Acetylated cellulose microfiber (hereinafter referred to as acetylated CMF) The same procedure as in Preparation Example 1 was carried out to obtain a defibrated slurry, except that the treatment with the high-pressure homogenizer in Preparation Example 1 was carried out twice. The obtained defibrated slurry was treated in the same manner as in the defibration and acetylation steps in Preparation Example 2. The properties of the obtained acetylated CMF were evaluated and found to be 12 μm in diameter and L / D of 30 or more (approximately 200).

[0351] To the obtained aqueous dispersion of acetylated CMF (solid content: 10% by mass), 5 parts by mass of PEG20000 was added per 100 parts by mass of acetylated CMF, and the mixture was then vacuum dried at approximately 40°C using a revolution / rotation type mixer (Hivismix 2P-1, manufactured by Primix Corporation) to obtain acetylated CMF powder.

[0352] Evaluation method [Weight average molecular weight (Mw) and acetylation degree] Measurement was carried out in the same manner as in Example I (first embodiment), except that a powder was used instead of a porous sheet.

[0353] [Length, diameter, L / D of CNF, acetylated CNF, and acetylated CMF] The wet cake was suspended in pure water at a concentration of 1% by mass, and dispersed using a high-shear homogenizer (manufactured by Nippon Seiki Co., Ltd., product name "Excel Auto Homogenizer ED-7", processing conditions: rotation speed 15,000 rpm x 5 minutes). The aqueous dispersion was then diluted with pure water to 0.1 to 0.5% by mass, cast onto mica, and air-dried. The ratio (L / D) of the length (L) to the diameter (D) of the particle image obtained when the particle was measured with an atomic force microscope (AFM) was determined, and the average value of 100 to 150 particles was calculated.

[0354] [Confirmation of the continuous phase] The same procedure as in Example II (second embodiment) was used for confirmation. Since no particular changes occurred in either the examples or comparative examples carried out this time, it was determined that the polyamide formed a continuous phase.

[0355] [Linear thermal expansion coefficient] The measurement was performed in the same manner as in Example II (second embodiment).

[0356] [Tensile strain at break] A tensile test was carried out in the same manner as in Example II (second embodiment), and five pieces of data on the strain at tensile break were obtained. The number average value of the break strain at the five points was used as an index of toughness, and the break strain range, which is the difference between the maximum and minimum values ​​among the five points, was used as an index of toughness variation.

[0357] <Extrusion conditions> [Extruder Design] A similar extruder design was used as in Example II (second embodiment).

[0358] <Production of resin composition> [Examples 3-1 to 3-16, Comparative Examples 3-1 to 3-3] The materials were mixed in the ratios shown in Tables 5 and 6 using an extruder of the same design, melt-kneaded at a screw speed of 300 rpm, and pelletized, after which various evaluations were carried out. The results are shown in Tables 5 and 6. In the table, the column indicating parts by mass indicates the preparation recipe, the middle column indicating mass % indicates the composition, and the bottom column indicates the physical properties.

[0359] From the results shown in the table, each example including polyamide, saponified ethylene-vinyl ester copolymer, and cellulose nanofiber showed high breaking strain (i.e., good toughness) and low linear thermal expansion coefficient, whereas each comparative example not including saponified ethylene-vinyl ester copolymer or polyamide showed poor breaking strain. In addition, comparing Example 3-5 using acetylated CNF with Example 3-12 using CNF, Example 3-5 using acetylated CNF showed smaller toughness variation. Furthermore, comparing Examples 3-13, 3-14, and 3-15 using a colorant with Example 3-5 not using a colorant, Examples 3-13, 3-14, and 3-15 showed smaller toughness variation.

[0360] [Table 5]

[0361] [Table 6] [Industrial Applicability]

[0362] The resin composition according to this embodiment may have excellent properties that are particularly suitable for use in large parts. That is, the resin composition according to the first embodiment may have low specific gravity, high rigidity, low thermal expansion coefficient, and low water absorption, and therefore may be suitably used in various large part applications. The resin compositions according to the second and third embodiments may have a high degree of compatibility between the contradictory properties of high toughness and low thermal expansion, and may have sufficient physical property stability to withstand practical use, and therefore may be suitably used in applications requiring high physical properties over a wide temperature range (such as the field of exterior material applications for automobiles, which are large parts).

Claims

1. polyamide, Saponified ethylene-vinyl ester copolymer, and cellulose, A resin composition comprising: The cellulose is a fibrous cellulose having a diameter of 2 nm to 1000 nm, the amount of the saponified ethylene-vinyl ester copolymer is 1 part by mass to 50 parts by mass relative to 100 parts by mass of the polyamide; The amount of the cellulose is 0.1% by mass to 15% by mass relative to 100% by mass of the resin composition.

2. The resin composition according to claim 1, wherein the amount of the saponified ethylene-vinyl ester copolymer is 50 to 5,000 parts by mass per 100 parts by mass of cellulose.

3. The resin composition according to claim 1 or 2, wherein the polyamide forms a continuous phase.

4. The resin composition according to any one of claims 1 to 3, wherein the polyamide is at least one selected from the group consisting of polyamide 6, polyamide 10, polyamide 11, polyamide 12, polyamide 66, polyamide 610, polyamide 612, polyamide 6 / 6I, polyamide 66 / 6I, polyamide 6I, and mixtures thereof.

5. The viscosity number (V) of the polyamide when measured in 96% by weight sulfuric acid in accordance with ISO 307 N 5. The resin composition according to claim 1, wherein the molecular weight of the polymer is 200 or less.

6. The resin composition according to any one of claims 1 to 5, further comprising an elastomer.

7. The resin composition according to claim 6, wherein the elastomer is at least one selected from the group consisting of an ethylene-α-olefin copolymer, a block copolymer of an aromatic vinyl compound and a conjugated diene compound, and a hydrogenated product of a block copolymer of an aromatic vinyl compound and a conjugated diene compound.

8. The resin composition according to claim 6 or 7, wherein the amount of the elastomer is 1 to 50 parts by mass per 100 parts by mass of polyamide.

9. The resin composition according to any one of claims 6 to 8, wherein the elastomer is an acid anhydride-modified elastomer.

10. The resin composition according to any one of claims 6 to 9, wherein the elastomer is a mixture of a polymer having an acidic functional group and a polymer not having an acidic functional group.

11. The resin composition according to any one of claims 1 to 10, wherein the ratio of vinyl alcohol units is 60 mol% or more relative to 100 mol% of all monomer units constituting the saponified ethylene-vinyl ester copolymer.

12. The resin composition according to any one of claims 1 to 11, wherein the cellulose is a cellulose nanofiber having a diameter of 50 to 1000 nm and a length (L) / diameter (D) ratio of 30 or more.

13. The resin composition according to any one of claims 1 to 12, wherein the cellulose is a hydrophobized cellulose.

14. The resin composition according to claim 13, wherein the hydrophobized cellulose is an acetylated cellulose.

15. The resin composition according to any one of claims 1 to 14, further comprising a polyphenylene ether.

16. The resin composition according to any one of claims 1 to 15, further comprising an antioxidant.

17. The resin composition according to any one of claims 1 to 16, further comprising a colorant.

18. The resin composition according to any one of claims 1 to 17, having a linear thermal expansion coefficient of 70 ppm / K or less at 20 ° C. to 100 ° C.

19. The resin composition according to any one of claims 1 to 18, having a tensile break strain of 10% or more.

20. A molded article made of the resin composition according to any one of claims 1 to 19.

21. An automobile exterior part comprising the resin composition according to any one of claims 1 to 19.

Citation Information

Patent Citations

  • Stabilized polyacetal composition

    JP1992505470A

  • Resin composition for manufacture of automobile exterior parts

    JP2004230926A

  • Method for producing resin composition

    JP2006199748A

  • Method for producing thermoplastic resin composition

    JP2006273984A

  • Resin molded product for painting

    JP2007284647A