Surface-treated steel sheet
A surface-treated steel sheet with a zinc-based plating and urethane resin coating addresses the balance of economical efficiency, metallic appearance, and resistance to chemicals and weather by controlling peak ratios and incorporating melamine resin, achieving superior chemical penetration and weather resistance.
Patent Information
- Application Number
- JP2020122255
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-16
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-07-16
AI Technical Summary
Existing coated metal plates face challenges in achieving a balance between economical efficiency, metallic appearance, chemical penetration resistance, and weather resistance, with previous technologies either being too expensive or lacking sufficient barrier properties.
A surface-treated steel sheet with a zinc-based plating layer and a first coating film composed mainly of urethane resin, containing melamine resin as a hardening agent, with a thickness of 10 μm or less, and a specific ratio of aromatic ring and urethane bond peak heights, along with optional ultraviolet absorbers and light stabilizers, to enhance chemical and weather resistance.
The solution results in a steel sheet with improved economical efficiency, metallic appearance, and enhanced chemical penetration and weather resistance without using expensive resins like fluororesin.
Smart Images

Figure 0007583242000012 
Figure 0007583242000013 
Figure 0007583242000014
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface-treated steel sheet. [Background technology]
[0002] Instead of conventional painted products that are painted after processing, painted metal sheets covered with a coating film are being used for automobiles, home appliances, building materials, civil engineering, machinery, furniture, containers, etc. Such painted metal sheets are generally produced by applying paint to a metal sheet, cutting it, and press forming it.
[0003] Painted metal sheets are mainly used as exterior materials, and are exposed to various solvents and chemicals, so they often have solvent resistance and chemical resistance. Since they are exterior materials, many painted metal sheets are usually painted with a colored coating, and the thickness of the coating film is relatively thick due to the concealment properties of the color tone. On the other hand, in the case of a metallic painted metal sheet that directly uses the appearance of the metal sheet as the substrate, it is necessary to apply a clear coating that does not hide the design of the substrate. In such a case, by reducing the thickness of the clear coating film, the painted metal sheet will have an excellent metallic appearance. In addition, from the viewpoints of productivity and commerciality, the thinner the thickness of the clear coating film, the better.
[0004] In general, chemical resistance requires that the coating film does not deteriorate or discolor due to chemicals. However, when the coating film is thin, the problem is not that the coating film deteriorates due to chemicals, but that the chemicals penetrate to the interface between the coating film and the plating and dissolve the plating. In the case of colored coating, even if the metal discolors due to chemicals, it does not become an appearance abnormality, but the metal dissolution progresses and a corrosion product is generated, and the coating film becomes swollen due to the generated corrosion product, which becomes an appearance abnormality. On the other hand, in the case of clear coating, the appearance is considered abnormal when the metal discolors. In other words, in clear coating, it is necessary that the chemical components do not reach the metal. Such a characteristic is called chemical penetration resistance.
[0005] In addition, when used outdoors or even indoors in an environment exposed to sunlight, the deterioration of the coating film due to sunlight and the associated discoloration can become a problem. In other words, in order to expand the range of applications for coating films, it is necessary to suppress the discoloration of the coating film due to sunlight. This characteristic is called weather resistance.
[0006] Several examples of coated metal sheets with excellent chemical resistance have been reported in the past. For example, Patent Document 1 listed below discloses a method for coating a metal plate with a paint containing a solvent-soluble fluororesin as a main component.
[0007] Furthermore, Patent Document 2 listed below discloses a coated metal sheet having a coating film using a polyester resin with a high glass transition temperature, a polyester resin with a low glass transition temperature, and an aminoformaldehyde resin, and having excellent processability, contamination resistance, scratch resistance, and chemical resistance.
[0008] Furthermore, the following Patent Document 3 discloses a precoated metal having an upper layer coated with a polyacrylic resin and a lower layer coated with a polyester resin, which has excellent stain resistance, chemical resistance, weather resistance and processability.
[0009] Furthermore, Patent Document 4 below discloses a coated metal sheet having a coating film that is a mixture of a specific polyurethane resin and a polyester resin, and that has excellent processability, corrosion resistance (particularly edge corrosion resistance), chemical resistance, etc.
[0010] Furthermore, the following Patent Document 5 discloses a metal sheet having excellent bending workability, which has a coating film in which melamine resin particles having a particle size of 50 nm or less are dispersed.
[0011] Furthermore, the following Patent Document 6 discloses a technique for concentrating an aminoblastic resin on the surface layer of a coating film using an aminoblastic resin such as a melamine resin.
[0012] Patent Document 7 listed below discloses a coated metal sheet having a resin coating film formed on at least one surface of the metal sheet, the resin coating film including a first portion having a urethane bond skeleton and a second portion having a triazine ring skeleton. [Prior art documents] [Patent documents]
[0013] [Patent Document 1] Japanese Patent Application Publication No. 5-111675 [Patent Document 2] Japanese Patent Application Publication No. 7-331167 [Patent Document 3] Japanese Patent Application Publication No. 7-313929 [Patent Document 4] JP 2013-213281 A [Patent Document 5] JP 2005-53002 A [Patent Document 6] JP 2006-175815 A [Patent Document 7] Patent No. 6624346 Summary of the Invention [Problem to be solved by the invention]
[0014] However, the fluororesin used in the technique of Patent Document 1 is expensive and is not industrially preferable.
[0015] As in Patent Document 2, the use of the self-condensation reaction of melamine resin, a crosslinking agent, in the formation of a coating film using a solvent-based paint is suggested. However, what is disclosed therein does not take into consideration the conditions for surface thickening necessary for the formation of a barrier layer. In addition, the addition of an amine compound for surface thickening is also disclosed, but the effect is only to the extent of affecting the distribution density of the generated melamine self-condensation particles. Therefore, the structure of the coating film obtained under these conditions is such that coarse self-condensation particles of about 50 to 100 μm are dispersed in the coating film, and surface thickening is observed as the distribution density of the particles, and the effect of improving the chemical penetration resistance of the coating film is limited.
[0016] The polyacrylic resin used in the technology of Patent Document 3 is poor in processability, and when the coating film disclosed in Patent Document 3 is used as a clear coating film, the barrier property is insufficient and, further, the resistance to chemical penetration may be poor.
[0017] The coating film disclosed in the above Patent Document 4 does not have sufficient barrier properties, and furthermore may have poor resistance to chemical penetration.
[0018] When melamine resin particles are dispersed in a coating film as in the technique of Patent Document 5, the coating film may have poor resistance to chemical penetration.
[0019] In the technique disclosed in Patent Document 6, the particle size of the melamine resin particles in the coating film is large, and the barrier properties are insufficient, and furthermore, the resistance to chemical penetration may be poor.
[0020] A coating film having improved barrier properties and excellent resistance to chemical penetration can be obtained by forming a melamine resin thickened layer on the surface of the coating film as in the technology of Patent Document 7. However, the coating film of Patent Document 7 does not have sufficient weather resistance, and it may be difficult to use it in places exposed to sunlight.
[0021] As described above, the above Patent Documents 1 to 7 do not disclose any technology for obtaining a surface-treated steel sheet that is excellent in cost efficiency, metallic appearance, chemical penetration resistance, and weather resistance.
[0022] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a surface-treated steel sheet that is excellent in economy, metallic appearance, chemical penetration resistance and weather resistance. [Means for solving the problem]
[0023] As a result of intensive research into the above-mentioned problems, the present inventors have discovered a method for manufacturing a steel sheet having a zinc-based plating layer on at least one side thereof and a first coating film mainly composed of a urethane resin, the thickness of the first coating film being 10 μm or less, and an absorption peak at 1510±10 cm caused by an aromatic ring among absorption peaks determined by infrared spectroscopy. -1 The peak height of (I1) and 1533 ± 10 cm due to the urethane bond -1 They have come to the conclusion that by controlling the ratio I1 / I2 of the peak heights (I2) of the two peaks to be in the range of 0.9 to 1.2, it is possible to produce a surface-treated steel sheet that is excellent in cost efficiency, metallic appearance, chemical penetration resistance, and weather resistance. The gist of the present invention, which was completed based on these findings, is as follows.
[0024] (1) A surface-treated steel sheet according to one embodiment of the present invention has a zinc-based plating layer and a urethane resin-based coating layer on at least one side of the steel sheet. The coating contains 80% by mass or more of the melamine resin as a hardener. and a first coating film, the thickness of which is 10 μm or less, and among the absorption peaks determined by infrared spectroscopy, the absorption peak at 1510±10 cm due to an aromatic ring is -1 The peak height of (I1) and 1533 ± 10 cm due to the urethane bond -1 The peak height (I2) ratio I1 / I2 is 0.9 0 ~1.2 0 It is. (2) In the surface-treated steel sheet according to the above (1), the first coating film may contain at least one of the ultraviolet absorber and the light stabilizer. (3) The surface-treated steel sheet according to the above (2) may contain at least one of the ultraviolet absorber and the light stabilizer in a total amount of 0.5 to 2.0 mass %. (4) In the surface-treated steel sheet according to any one of the above aspects (1) to (3), the first coating film may have a first portion having a urethane bond skeleton and a second portion having a triazine ring skeleton, and the glass transition temperature of the first coating film may be 85° C. or more and 170° C. or less. When the second portion is stained with osmium oxide and observed at a magnification of 100,000 times using a transmission electron microscope, a dispersed-type second portion in which particles having a number-average particle size of 5 to 20 nm are dispersed and a concentrated-type second portion that is present at a position up to a depth of 15 nm from the surface of the first coating film, and in which particles having a number-average particle size of 5 nm or more are not observed independently, may be observed. (5) In the surface-treated steel sheet described in (4) above, N1 / N2, which is the ratio of the N concentration N1 at a depth position of 0.2 μm from the surface of the first coating film to the N concentration N2 at a depth position of 0.2 μm toward the first coating film from the interface between the first coating film and the zinc-based plated steel sheet, may be 1.2 or more. (6) The surface-treated steel sheet according to any one of the above aspects (1) to (5) may further include a second coating film between the first coating film and the zinc-based plating layer, and the glass transition temperature of the second coating film may be lower than or equal to the glass transition temperature of the first coating film. (7) In the surface-treated steel sheet according to any one of the above aspects (1) to (6), at least one of the first coating film and the second coating film may contain a colorant. (8) In the surface-treated steel sheet according to any one of the above aspects (1) to (7), a texture may be formed on the surface of at least one of the zinc-based plating layer and the steel sheet. Effect of the Invention
[0025] As described above, according to the present invention, it is possible to obtain a surface-treated steel sheet which is excellent in economy, metallic appearance, resistance to chemical penetration and weather resistance. [Brief description of the drawings]
[0026] [Figure 1A]FIG. 1 is a schematic diagram showing a surface-treated steel sheet according to an embodiment of the present invention (having only an upper coating film). [Figure 1B] FIG. 1 is a schematic diagram showing a surface-treated steel sheet according to an embodiment of the present invention (also having an underlayer coating film). [Figure 2A] FIG. 1 is a schematic diagram showing a surface-treated steel sheet according to an embodiment of the present invention (wherein an upper coating film is provided on both sides). [Figure 2B] FIG. 1 is a schematic diagram showing a surface-treated steel sheet according to an embodiment of the present invention (wherein an upper coating film and a lower coating film are provided on both sides). [Diagram 3] 4 is a schematic diagram showing a state of a second portion of the surface-treated steel sheet according to the present embodiment stained with osmium oxide and observed at a magnification of 100,000 times. FIG. [Figure 4] 1 is a flow chart showing an example of a flow of a method for producing a surface-treated steel sheet according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Hereinafter, a surface-treated steel sheet and a manufacturing method thereof according to the present embodiment will be described with reference to the drawings as appropriate. As shown in Fig. 1A, the surface-treated steel sheet 1 according to this embodiment has an upper layer coating film 13 as a first coating film on one side of a base steel sheet and a zinc-based plating layer (hereinafter, these may be collectively referred to as a zinc-based plated steel sheet 11). As shown in Fig. 1B, a lower layer coating film 15 may be provided as a second coating film between the zinc-based plated steel sheet 11 and the upper layer coating film 13.
[0028] Furthermore, as shown typically in Figures 2A and 2B, in the surface-treated steel sheet 1 according to this embodiment, the upper layer coating film 13 may be provided on both sides of the zinc-based plated steel sheet 11, or the upper layer coating film 13 and the lower layer coating film 15 may be provided on both sides of the zinc-based plated steel sheet 11.
[0029] The configuration of the surface-treated steel sheet 1 according to this embodiment is not limited to the configuration shown in Figures 1A to 2B. For example, a configuration in which an upper coating film 13 and an underlayer coating film 15 are provided on one side of a zinc-based plated steel sheet 11, and an upper coating film 13 or an underlayer coating film 15 is provided on the other side of the zinc-based plated steel sheet 11, can also be realized.
[0030] The upper layer coating film 13, which is an example of the first coating film, is mainly composed of a urethane resin and may include a first portion having a urethane bond skeleton (hereinafter also referred to as a "urethane portion") and a second portion having a triazine ring skeleton (hereinafter also referred to as a "triazine portion") The glass transition temperature of the upper layer coating film 13 may be 85°C or higher and 170°C or lower. Furthermore, as shown diagrammatically in FIG. 3, when the second portion having a triazine ring skeleton is stained with osmium oxide and observed at a magnification of 100,000 times using a transmission electron microscope, it may contain both a dispersed-type second portion (symbol 101 in FIG. 3) in which particles with a number-average particle size of 5 nm or more are dispersed, and a concentrated-type second portion (symbol 103 in FIG. 3) which is present at a position up to a depth of 15 nm from the surface of the upper layer coating film 13 and in which particles with a number-average particle size of 5 nm or more are densely packed together such that individual particles cannot be observed independently. That is, the upper layer coating 13 may contain a triazine portion in addition to the urethane portion corresponding to the above-mentioned urethane resin, and this triazine portion may have triazine granules 101 (dispersed second portion) dispersed as particles having a number-average particle size of 5 nm or more, and concentrated portions 103 (concentrated second portion) located at a depth of 15 nm from the surface of the upper layer coating 13 and agglomerated in a layer rather than existing independently as particles having a number-average particle size of 5 nm or more.
[0031] The surface-treated steel sheet 1 according to the present embodiment has the above-mentioned configuration, and is excellent in metallic appearance, chemical penetration resistance, and weather resistance without using expensive resins such as fluororesins. The reason for this is presumed to be as follows.
[0032] The main component of the upper layer coating film 13 is a urethane resin. Urethane resin is known to have excellent chemical penetration resistance. In addition, in order to increase the glass transition temperature of the coating film and further improve the chemical penetration resistance, it is effective to introduce aromatic rings, which are rigid molecular structures, into the urethane resin. On the other hand, the aromatic rings in the urethane resin react and discolor when exposed to energy such as sunlight. In other words, the more aromatic rings in the urethane resin, the better the chemical penetration resistance, but the worse the weather resistance. These chemical penetration resistance and weather resistance are superior as the upper layer coating film 13 is thicker. However, to obtain an excellent metallic appearance, the film thickness needs to be 10 μm or less. Under such constraints, by controlling the ratio of aromatic rings and urethane bonds in the upper layer coating film 13, it has become possible to simultaneously achieve the metallic appearance, which was a challenge, as well as chemical penetration resistance and weather resistance.
[0033] In order to set the glass transition temperature to 85°C or more and 170°C or less, the urethane portion needs to have a considerably high glass transition temperature. When the urethane portion has a high glass transition temperature, a high cohesive force is generated in the urethane portion when the upper layer coating film 13 is formed. As a result, the triazine portion does not condense alone, but is dispersed in the urethane portion, and the urethane portion and the triazine portion tend to bond preferentially. The triazine portion, which has high solvent resistance, bonds with the urethane portion to form a three-dimensional network structure. As a result, the barrier property (i.e., resistance to chemical penetration) of the upper layer coating film 13 is enhanced. In order to obtain such characteristics, in this embodiment, the glass transition temperature of the upper layer coating film 13 is preferably set to 85°C or more and 170°C or less.
[0034] In addition, the triazine moieties form domains in the upper coating film 13 and disperse in a granular form (reference numeral 101 in FIG. 3), and also thicken at the surface of the upper coating film 13 to form thickened portions 103, so that the triazine moieties, which have high solvent resistance, enhance the solvent resistance of the upper coating film 13. Furthermore, as described above, if a high cohesive force is generated in the urethane moiety when the upper coating film 13 is formed, the urethane moiety and the triazine moiety tend to bond preferentially, and as shown diagrammatically in FIG. 3, the fine granular triazine moieties (hereinafter also referred to as "triazine granules 101") are thickened at the surface of the upper coating film 13. From this point of view as well, the solvent resistance of the upper coating film 13 is further improved.
[0035] When the fine granular triazine moieties (triazine granules 101) are concentrated in the surface layer of the topcoat 13, light scattering by the triazine moieties is suppressed, improving the transparency of the topcoat 13 and making it easier to visually recognize the gloss of the underlying zinc-based plated steel sheet 11 from the outside. This also improves the metallic appearance of the surface-treated steel sheet 1 according to this embodiment.
[0036] As outlined above, it is presumed that the surface-treated steel sheet 1 of this embodiment, due to its configuration as described above, has excellent metallic appearance, chemical penetration resistance, and solvent resistance without the use of expensive resins such as fluororesins.
[0037] Hereinafter, each component of the surface-treated steel sheet 1 according to this embodiment will be described in detail.
[0038] <About zinc-based coated steel sheets 11> The surface-treated steel sheet 1 according to this embodiment has a steel sheet and a zinc-based plating layer (zinc-based plated steel sheet), and various generally known zinc-based plated steel sheets can be used as the zinc-based plated steel sheet 11. Specifically, it refers to plated steel sheets in which zinc or an alloy of zinc and another metal is plated on the surface of the steel sheet, such as zinc-plated steel sheet, zinc-nickel alloy plated steel sheet, hot-dip alloyed zinc-plated steel sheet, aluminum-zinc alloy plated steel sheet, zinc-aluminum-magnesium alloy plated steel sheet, etc. The zinc-based plated steel sheet may be any of hot-dip galvanized steel sheet, electrolytic zinc-plated steel sheet, etc.
[0039] Furthermore, the surface of the galvanized steel sheet 11 (i.e., the surface of the steel sheet and / or the surface of the zinc-based plating layer) may be formed with various textures such as matte finish, roughness, streaks (hairline), cloth grain (satin), hammered finish, etc., in order to further improve the design of the surface-treated steel sheet 1 according to this embodiment. In the surface-treated steel sheet 1 according to this embodiment, the transparency of the upper coating film 13 is improved by the above-mentioned configuration, so that even if the above-mentioned texture is formed on the surface of the galvanized steel sheet 11, the metallic feel evoked by such texture is easily visible from the outside.
[0040] <About the top layer coating 13> As mentioned above, the upper coating film 13 of the surface-treated steel sheet 1 according to this embodiment mainly contains a urethane resin, has a coating thickness of 10 μm or less, and exhibits an absorption peak of 1510±10 cm due to an aromatic ring among absorption peaks determined by infrared spectroscopy. -1 The peak height of 1533 ± 10 cm due to the urethane bond (I1) -1 The peak height (I1 / I2) is 0.9 to 1.2.
[0041] The urethane resin constituting the upper coating film 13 has an aromatic ring and a urethane bond in its resin skeleton. When such a coating film is analyzed by infrared spectroscopy, the infrared spectroscopy wavelength is 1510±10 cm -1 The size of the absorption peak (I1) that appears at 1533±10 cm is proportional to the aromatic ring ratio in the resin. -1The magnitude of the absorption peak (I2) that appears in is proportional to the ratio of urethane bonds contained in the resin. In other words, I1 / I2 means the ratio of the number of aromatic rings to the number of urethane bonds in the resin. As mentioned above, the upper layer coating film 13 of the surface-treated steel sheet 1 according to this embodiment may contain, in addition to a urethane portion (a first portion having a urethane bond skeleton), a triazine portion (a second portion having a triazine ring skeleton).
[0042] The upper coating film 13 may contain at least one of an ultraviolet absorber and a light stabilizer. By containing at least one of an ultraviolet absorber and a light stabilizer in the upper coating film 13, ultraviolet rays are absorbed in the coating film, and resin decomposition in the coating film can be suppressed. Secondary resin decomposition caused by ultraviolet rays reflected on the plating surface can also be suppressed. The types of ultraviolet absorbers and light stabilizers that can be contained in the upper coating film 13 are not particularly limited, and known ones can be used. Specifically, examples of ultraviolet absorbers include benzophenone-based, benzotriazole-based, and cyanoacrylate-based agents. Examples of light stabilizers include hindered amine-based compounds. When the upper coating film 13 contains at least one of an ultraviolet absorber and a light stabilizer, the total content is preferably 0.5 to 2.0 mass %. This is because the total content of 0.5 to 2.0 mass % absorbs ultraviolet rays and suppresses decomposition of the resin.
[0043] Each part of the upper coating film 13 will be described below. The urethane bond skeleton of the urethane moiety in the upper coating film 13 can be confirmed by analyzing the upper coating film 13 by Fourier transform infrared spectroscopy and detecting a vibration peak attributable to the urethane bond.
[0044] The triazine ring skeleton of the triazine moiety is a skeleton derived from a triazine ring contained in a melamine resin, that is, the triazine moiety is a moiety derived from a triazine ring contained in a melamine resin.
[0045] As mentioned earlier with reference to Figure 3, when the triazine portion is stained with osmium oxide and observed at 100,000 times magnification using a transmission electron microscope, a dispersed-type second portion in which particles having a number-average particle size of 5 to 20 nm are dispersed, and a concentrated-type second portion which is located at a position up to a depth of 15 nm from the surface of the upper layer coating 13 and in which the particles are densely packed, so that particles having a number-average particle size of 5 nm or more are not observed individually, are observed.
[0046] Here, the thickened portion 103 in this embodiment is present within a range extending from the surface of the top coating film 13 to a depth d (15 nm) toward the zinc-based plated steel sheet 11, as shown diagrammatically in Figure 3. The phrase "the triazine moieties are concentrated in the surface layer of the upper coating film 13" means that granular triazine moieties (i.e., triazine granules 101) are unevenly distributed in a layer on the surface side of the upper coating film 13 opposite the interface with the zinc-based plated steel sheet 11. In other words, this means that the region of the granular triazine moieties unevenly distributed in a layer constitutes the surface layer of the upper coating film 13. Here, "the triazine moieties are unevenly distributed in a layered manner to form concentrated portion 103" means that the average concentration (average content) of the triazine moieties in the region where the triazine moieties are unevenly distributed is 1.2 times or more the average concentration of the triazine moieties in the region other than the unevenly distributed portion.
[0047] Here, the triazine moiety in this embodiment is dispersed in the upper coating film 13 in the form of particles having a number-average particle size of 5 nm or more and 20 nm (in other words, the number-average particle size of the triazine particles 101 is 5 nm or more and 20 nm or less), and is concentrated in the surface layer within a depth of 15 nm from the surface of the upper coating film 13 (in other words, the depth d in Figure 3 is 15 nm or less).
[0048] Here, the fact that the triazine moieties are concentrated in the surface layer within a depth of 15 nm from the surface of the topcoat 13 means that a region of granular triazine moieties distributed unevenly in a layer on the surface side of the topcoat 13 opposite the interface with the zinc-based plated steel sheet 11 is present within a depth of 15 nm from the surface of the topcoat 13. In other words, this means that the region of granular triazine moieties distributed unevenly in a layer constitutes the surface layer of the topcoat 13 and has a thickness of 15 nm or less.
[0049] When the number average particle diameter of the granular triazine moieties (i.e., triazine granules 101) is less than 5 nm, the chemical penetration resistance may decrease. On the other hand, when the number average particle diameter of the granularly dispersed triazine moieties exceeds 20 nm, the metallic appearance and chemical penetration resistance of the surface-treated steel sheet 1 may decrease, or the metallic appearance, chemical penetration resistance and processability may decrease. Here, when the processability of the surface-treated steel sheet 1 decreases, cracks or the like occur in the upper coating film 13, and the chemical penetration resistance and solvent resistance also decrease. From the viewpoint of the metallic appearance and chemical penetration resistance, the number average particle diameter of the granularly dispersed triazine moieties (triazine granules 101) is more preferably 5 nm or more and 15 nm or less.
[0050] Furthermore, when the granular triazine moieties are not concentrated on the surface of the upper coating film 13 (i.e., when the concentrated portion 103 does not exist), the metallic appearance and chemical penetration resistance may be deteriorated. Furthermore, when the granular triazine moieties are concentrated to a depth of more than 15 nm from the surface of the upper coating film 13 (i.e., when the concentrated portion 103 exists at a depth of more than 15 nm from the surface of the upper coating film 13), the workability may be deteriorated. When the workability of the surface-treated steel sheet 1 is deteriorated, cracks or the like are generated in the upper coating film 13, and the chemical penetration resistance is also deteriorated.
[0051] It is preferable that a plurality of thickened parts 103 are formed in the upper layer coating film 13. By forming a plurality of thickened parts 103, the barrier property is further improved and suitable chemical resistance can be obtained. In order to form the thickened parts 103, the heating method in the upper layer coating film formation step described later is important. This point will be described later.
[0052] Here, in the top layer coating 13 of this embodiment, the ratio N1 / N2 of the N concentration N1 (unit: mass %) at a depth position of 0.2 μm from the surface of the top layer coating 13 to the N concentration N2 (unit: mass %) at a depth position of 0.2 μm toward the top layer coating 13 from the interface between the top layer coating 13 and the zinc-based plated steel sheet 11 is 1.2 or more. By setting N1 / N2 to 1.2 or more, it is possible to more reliably improve the metallic appearance and the solvent resistance. N1 / N2 is more preferably 1.5 or more and 10 or less.
[0053] Next, various methods for analyzing the triazine moiety in the upper coating film 13 will be described. First, the top coating film 13 to be analyzed is stained with osmium oxide. This selectively stains the triazine moieties in the top coating film 13. Next, the coating film stained with osmium oxide is cut in the film thickness direction using a microtome, focused ion beam processing device, or the like to prepare a coating film sample whose cross section can be observed. Next, the thin film sample is observed at a magnification of 100,000 times using a transmission electron microscope. In this observation, the triazine moieties in the thin film sample are observed as black in STEM-BF (bright field) images and as white in STEM-HAADF (dark field) images.
[0054] The above-mentioned analytical method can confirm the triazine moiety in the upper layer coating film 13. The triazine moiety in the upper layer coating film 13 can also be confirmed by analyzing the coating film by energy dispersive X-ray spectroscopy or Fourier transform infrared spectroscopy to detect nitrogen and osmium or to detect a vibration peak assigned to a triazine ring.
[0055] The thickness of the region where the granular triazine moieties are concentrated (i.e., the thickness of the concentrated portion (concentrated second portion) 103 which is a region where the granular triazine moieties are unevenly distributed in a layer) is a value measured by the following method. As described above, a thin film sample is observed at a magnification of 100,000 times using a transmission electron microscope to obtain a STEM-BF (bright field) image. The obtained STEM-BF (bright field) image is binarized. Then, in the obtained binarized image, the thicknesses of the layered regions observed as black from the surface of the upper coating film 13 are measured at any 20 points, and the average value is calculated as the thickness of the region where the granular triazine moieties are concentrated. The position where the concentrated portion 103 exists can be specified by focusing on the position of the lower end (interface on the zinc-based plated steel sheet 11 side) of the thickness of the concentrated portion 103 obtained as described above in the binarized image. When a layer of black regions is observed on the surface of the upper coating film 13, it is deemed that the granular triazine moieties are concentrated on the surface of the upper coating film 13.
[0056] The number average particle diameter of the granular triazine moieties (the number average particle diameter of the triazine granules 101) is a value measured by the following method. As described above, a thin film sample is observed at a magnification of 100,000 times using a transmission electron microscope to obtain a STEM-BF (bright field) image. The obtained STEM-BF (bright field) image is binarized, for example, with a threshold value of 120. Then, the circle equivalent diameter of the granular regions observed as black in the obtained binarized image is calculated using the formula: circle equivalent diameter=2(area / π). 0.5 The "area" in this formula refers to the area of the granular regions observed as black. This calculation of the equivalent circle diameter is then carried out for 20 arbitrarily selected granular regions, and the average value is taken as the number-average particle diameter of the granular triazine moieties.
[0057] The average concentration of triazine moieties concentrated on the surface side of the upper coating film 13 can be measured as follows: That is, the distribution of N element concentration in the depth direction from the surface side of the upper coating film 13 toward the zinc-based plated steel sheet is measured, and N1 / N2, which is the ratio between the N element concentration N1 at a position 0.2 μm away from the outermost layer and the N element concentration N2 at a position 0.2 μm away from the boundary with the zinc-based plated steel sheet or lower coating film, is calculated. The elemental analysis in the depth direction can be carried out by a known method, for example, glow discharge optical emission spectroscopy (GD-OES), Auger electron spectroscopy (AES), or the like.
[0058] Next, the glass transition temperature (Tg) of the upper coating film 13 will be described. The glass transition temperature of the upper layer coating film 13 is preferably 85°C or higher and 170°C or lower. If the glass transition temperature of the upper layer coating film 13 is lower than 85°C, the chemical penetration resistance of the surface-treated steel sheet 1 may decrease. On the other hand, if the glass transition temperature of the upper layer coating film 13 exceeds 170°C, the workability and weather resistance of the surface-treated steel sheet 1 may decrease. If the workability of the surface-treated steel sheet 1 decreases, cracks or the like will occur in the upper layer coating film 13, and the chemical penetration resistance will also decrease. From the viewpoint of chemical penetration resistance and weather resistance (particularly from the viewpoint of chemical penetration resistance), the glass transition temperature of the upper layer coating film 13 is preferably 100°C or higher and 160°C or lower, more preferably 110°C or higher and 150°C or lower.
[0059] Furthermore, when the surface-treated steel sheet 1 according to this embodiment has an underlayer coating film 15, the glass transition temperature of the upper layer coating film 13 is preferably equal to or higher than the glass transition temperature of the underlayer coating film 15. When the glass transition temperature of the upper layer coating film 13 is lower than the glass transition temperature of the underlayer coating film 15, the adhesion between the upper layer coating film 13 and the underlayer coating film 15 decreases, and the chemical penetration resistance may decrease.
[0060] The glass transition temperature of the upper coating film 13 is preferably at least 5° C. higher than the glass transition temperature of the lower coating film 15. When the difference between the glass transition temperature of the upper coating film 13 and the glass transition temperature of the lower coating film 15 is at least 5° C., the adhesion between the upper coating film 13 and the lower coating film 15 becomes even better, and chemical penetration resistance is likely to be further improved.
[0061] Furthermore, it is more preferable that the glass transition temperature of the upper layer coating film 13 is higher by 10° C. or more and 50° C. or less than that of the lower layer coating film 15. When the glass transition temperature of the upper layer coating film 13 is higher by 10° C. or more than that of the lower layer coating film 15, chemical penetration resistance is easily improved. On the other hand, when the glass transition temperature of the upper layer coating film 13 is higher by 50° C. or less than that of the lower layer coating film 15, a decrease in coating hardness is easily suppressed.
[0062] Here, the glass transition temperature (Tg) is a value measured by the following method. First, the coating film to be measured is peeled off or scraped off to prepare a measurement sample. Then, the glass transition temperature is determined by using the measurement sample according to the differential scanning calorimetry (DSC method) of the transition temperature measurement method for plastics (JIS K7121 1987).
[0063] It is preferable that the upper coating film 13 does not contain at least one metal complex compound selected from aluminum and titanium. Here, examples of at least one metal complex compound selected from zinc, aluminum, and titanium include zinc stearate, zinc gluconate, zinc picolinate, zinc citrate, zinc acetylacetonate, aluminum acetate, aluminum stearate, aluminum ethylate, aluminum isopropylate, aluminum triisoporoxide, aluminum ethylacetoacetate diisopropylate, aluminum trisethylacetoacetate, aluminum tris(acetylacetate), aluminum oxide isopropoxy, and the like. Examples of suitable additives include side trimer, titanium tetraisopropoxide, titanium tetra normal butoxide, titanium butoxide dimer, titanium tetra 2-ethylhexoxide, titanium diisopropoxybis(acetylacetonate), titanium tetraacetylacetonate, titanium dioctyloxybis(octylene glycolate), titanium diisopropoxybis(ethylacetoacetate), titanium diisopropoxybis(triethanol aminate), titanium lactate ammonium salt, titanium lactate, polyhydroxytitanium stearate, etc. This is because if the upper layer coating film 13 contains at least one metal complex compound selected from aluminum and titanium, the chemical resistance of the upper layer coating film 13 will deteriorate.
[0064] <About the undercoat 15> In the surface-treated steel sheet 1 according to this embodiment, the underlayer coating film 15 is not particularly limited, and may be a well-known resin coating film such as a polyurethane resin, an epoxy resin, an acrylic resin, a polyester resin, a phenolic resin, a polyolefin resin, an alkyd resin, a melamine resin, a silicone resin, etc. When forming such a resin coating film, it is also possible to use a well-known additive such as a silane coupling agent.
[0065] Among these resin coatings, from the viewpoints of metallic appearance, chemical penetration resistance, and solvent resistance, the underlayer coating 15 is preferably a resin coating having at least a first portion having a urethane bond skeleton (hereinafter also referred to as a "urethane portion") and preferably further containing a portion having at least either an epoxy group or a siloxane bond skeleton (hereinafter, the portion having an epoxy group is also referred to as an "epoxy portion" and the portion having a siloxane bond skeleton is also referred to as a "siloxane portion"). Moreover, the underlayer coating 15 preferably contains, in addition to the above-mentioned urethane portion, a compound having one or more elements selected from the group consisting of P, V, Ti, Si, and Zr.
[0066] Here, since the urethane portion further has an anionic functional group, the dispersibility of the urethane portion in aqueous media (water-based paint) is improved, and the film-forming properties of the underlayer coating film 15 are enhanced, which improves the adhesion between the underlayer coating film 15 and the zinc-based plated steel sheet 11 and enhances the barrier properties (i.e., resistance to chemical penetration) of the underlayer coating film 15.
[0067] Furthermore, the inclusion of a urethane moiety and at least one of an epoxy group and a siloxane bond skeleton also improves the chemical penetration resistance of the underlayer coating film 15. Furthermore, by making the underlayer coating film 15 a resin coating film having at least a urethane moiety, the transparency of the underlayer coating film 15 is improved and the metallic appearance is also improved.
[0068] Furthermore, a compound having one or more elements selected from the group consisting of P, V, Ti, Si, and Zr generally functions as a rust inhibitor, and such a compound may be contained in the underlayer coating film 15. By containing such a compound in the underlayer coating film 15, it becomes possible to further improve the corrosion resistance of the surface-treated steel sheet 1.
[0069] Next, each part included in the undercoat film 15 will be described. Examples of anionic functional groups that are preferably contained in the urethane moiety include a carboxylic acid group (carboxy group) and a sulfonic acid group (sulfo group). On the other hand, the urethane bond skeleton of the urethane moiety is a skeleton derived from a polyurethane resin. In other words, the urethane moiety is a moiety derived from a polyurethane resin, and can further have an anionic functional group.
[0070] The epoxy moiety having an epoxy group is a moiety derived from an epoxy resin. In other words, the epoxy group of the epoxy moiety is an epoxy group residue that has not reacted with the urethane moiety derived from the polyurethane resin. The siloxane bond skeleton of the siloxane moiety is a skeleton derived from a silicone resin having a siloxane bond or a silane coupling agent capable of generating a siloxane bond.
[0071] The urethane bond skeleton of the urethane moiety, the epoxy group of the epoxy moiety, and the siloxane bond skeleton of the siloxane moiety in the underlayer coating 15 can be confirmed by analyzing the underlayer coating 15 by energy dispersive X-ray spectroscopy or Fourier transform infrared spectroscopy to detect elements constituting the corresponding bonds or functional groups, or to detect vibration peaks attributed to the corresponding bonds or functional groups. The presence of a compound having one or more elements selected from the group consisting of P, V, Ti, Si, and Zr in the underlayer coating 15 can be confirmed by whether or not the elements contained in such a compound are detected by energy dispersive X-ray spectroscopy.
[0072] Next, the glass transition temperature of the undercoat film 15 will be described. The glass transition temperature of the lower coating film 15 is preferably equal to or lower than the glass transition temperature of the upper coating film 13. The glass transition temperature of the lower coating film 15 is more preferably within the range of 80°C or higher and 170°C or lower, and is equal to or lower than the glass transition temperature of the upper coating film 13. If the glass transition temperature of the lower coating film 15 is lower than 80°C, the chemical penetration resistance may decrease. On the other hand, if the glass transition temperature of the lower coating film 15 exceeds 170°C, the processability may decrease. If the processability decreases, cracks may occur in the lower coating film 15, and the chemical penetration resistance and solvent resistance may also decrease. From the viewpoint of chemical penetration resistance and solvent resistance (particularly from the viewpoint of chemical penetration resistance), the glass transition temperature of the lower coating film 15 is more preferably equal to or lower than the glass transition temperature of the upper coating film 13, and is within the range of 100°C or higher and 170°C or lower.
[0073] <About the film thickness of the upper coating film 13 and the lower coating film 15> In the surface-treated steel sheet 1 according to this embodiment, the thickness of the upper coating film 13 as described above is set to 10 μm or less. If the thickness of the upper coating film 13 exceeds 10 μm, the transparency of the upper coating film 13 decreases, and the metallic appearance may be deteriorated. On the other hand, the lower limit of the thickness of the upper coating film 13 is not particularly set, but may be set to 0.5 μm or more from the viewpoint of chemical penetration resistance. From the viewpoint of metallic appearance and chemical penetration resistance, the thickness of the upper coating film 13 is more preferably 3 μm or more and 8 μm or less.
[0074] In addition, in the surface-treated steel sheet 1 according to this embodiment, when an underlayer coating film 15 is provided in addition to the upper layer coating film 13, the thickness of the underlayer coating film 15 is preferably 0.1 μm or more and 3 μm or less. By setting the thickness of the underlayer coating film 15 to 0.1 μm or more and 3 μm or less, it becomes possible to further improve the chemical penetration resistance while maintaining the metallic appearance. From the viewpoint of chemical penetration resistance, the thickness of the underlayer coating film 15 is more preferably more than 0.3 μm and 2 μm or less.
[0075] <Coloring agent in upper coating film 13 and / or lower coating film 15> In the surface-treated steel sheet 1 according to this embodiment, the above-mentioned upper coating film 13 and / or lower coating film 15 may contain a colorant. By adding a colorant to the upper coating film 13 and / or lower coating film 15, the color tone of the product can be adjusted, making it possible to apply the product to a wide variety of applications.
[0076] Here, when a texture is present on the surface of the zinc-based plated steel sheet, it is preferable to disperse the coloring pigment in the above-mentioned upper coating film 13. If the pigment is dispersed in the lower coating film 15, the film thickness in the recesses present on the surface of the zinc-based plated steel sheet becomes relatively large, which may conceal the formed texture.
[0077] <Specific configurations of the upper coating film 13 and the lower coating film 15> In the surface-treated steel sheet 1 according to the present embodiment, the upper layer coating film 13 is preferably a resin coating film (e.g., a resin coating film containing a crosslinked product of a polyurethane resin and a water-soluble melamine resin) obtained by curing an upper layer paint containing a polyurethane resin (a) having a glass transition temperature of 75°C or more and 160°C or less, a water-soluble melamine resin (b) which is a triazine ring-containing water-soluble curing agent, and an aqueous solvent. The resin coating film formed from such an upper layer paint has a glass transition temperature of 85°C or more and 170°C or less as a whole. In this case, the water-soluble melamine resin (b) exists in the form of particles dispersed in the upper layer coating film 13 and in the form concentrated on the surface side of the upper layer coating film 13. In addition, when an underlayer coating film 15 is further provided between the upper layer coating film 13 and the zinc-based plated steel sheet 11, the glass transition temperature of the polyurethane resin (a) is preferably equal to or higher than the glass transition temperature of a polyurethane resin (c) contained in the underlayer coating film 15 as described below.
[0078] When a polyester resin is used instead of a polyurethane resin, the polyester resin has inferior chemical resistance to the polyurethane resin, so that the thickness of the upper coating film must be increased in order to obtain the same chemical resistance. If the thickness of the upper coating film becomes too thick, it is not preferable because the desired metallic appearance cannot be obtained when the upper coating film is made into a clear coating film.
[0079] In addition, when the underlayer coating film 15 is provided on the surface-treated steel sheet 1 according to this embodiment, the underlayer coating film 15 is specifically a resin coating film (for example, a crosslinked mixture of the polyurethane resin (c) and the epoxy resin (d)) obtained by curing an underlayer paint containing at least one of a polyurethane resin (c) having a glass transition temperature equal to or lower than the glass transition temperature of the polyurethane resin (a) of the upper layer coating film 13, an epoxy resin (d), a silane coupling agent (e), and a rust inhibitor (f) containing one or more elements selected from the group consisting of P, V, Ti, Si, and Zr, and an aqueous solvent. a resin coating film containing a crosslinked product of polyurethane resin (c), epoxy resin (d) and a silane coupling agent (e); a resin coating film containing a crosslinked product of polyurethane resin (c), epoxy resin (d) and a silane coupling agent (e) and a rust inhibitor (f); a resin coating film containing a crosslinked product of polyurethane resin (c) and a silane coupling agent (e); a resin coating film containing a crosslinked product of polyurethane resin (c) and a silane coupling agent (e) and a rust inhibitor (f); a resin coating film containing a crosslinked product of polyurethane resin (c) and a silane coupling agent (e) and a rust inhibitor (f), a resin coating film containing a polyurethane resin (c) and a rust inhibitor (f), etc.
[0080] The surface-treated steel sheet 1 according to this embodiment has been described in detail above. The surface-treated steel sheet 1 according to the embodiment as described above can be used for automobiles, home appliances, building materials, civil engineering, machinery, furniture, containers, and the like.
[0081] (Regarding the manufacturing method of surface-treated steel sheets) Next, an example of a method for producing a surface-treated steel sheet according to this embodiment will be described in detail with reference to Fig. 4. Fig. 4 is a flow chart showing an example of the flow of the method for producing a surface-treated steel sheet according to this embodiment. The method for producing the surface-treated steel sheet according to the present embodiment is not limited to the method described below. The following production method is one example for producing the surface-treated steel sheet according to the present embodiment.
[0082] The manufacturing method of the surface-treated steel sheet according to this embodiment is a manufacturing method of a surface-treated steel sheet 1 having at least an upper layer coating film 13 on at least one side of a predetermined zinc-based plated steel sheet 11. As shown in Fig. 4 as an example, the manufacturing method of this surface-treated steel sheet includes a texture forming step (step S101) of forming a predetermined texture on the surface of the zinc-based plated steel sheet 11 as necessary, an underlayer coating film forming step (step S103) of forming an underlayer coating film 15 on the zinc-based plated steel sheet 11 as necessary, and an upper layer coating film forming step (step S105) of forming an upper layer coating film 13 on the zinc-based plated steel sheet 11 or the underlayer coating film 15.
[0083] Here, the texture forming process and the underlayer coating film forming process may be performed as necessary. For example, when manufacturing a surface-treated steel sheet 1 in which an upper layer coating film 13 is formed on a zinc-based plated steel sheet 11 having no texture, etc., only step S105 of the three processes shown in Figure 4 is performed.
[0084] In the manufacturing method of the surface-treated steel sheet shown in Fig. 4, the most important step is the upper layer coating film forming step (step S105). This upper layer coating film forming step is a step of coating an upper layer paint (such an upper layer paint is an example of a first paint) containing a polyurethane resin (a) containing an anionic functional group and having a glass transition temperature of 75°C or more and 160°C or less, a water-soluble melamine resin (b) which is a triazine ring-containing water-soluble curing agent, and an aqueous solvent on a zinc-based plated steel sheet 11 (on the lower layer coating film 15 when the lower layer coating film 15 is formed on the zinc-based plated steel sheet 11), and then heating and cooling the zinc-based plated steel sheet on which the upper layer paint has been applied, thereby forming an upper layer coating film 13.
[0085] The manufacturing method of the surface-treated steel sheet according to the present embodiment can manufacture the surface-treated steel sheet according to the present embodiment (i.e., the surface-treated steel sheet having excellent metallic appearance, chemical penetration resistance, and solvent resistance) while suppressing costs by the above-mentioned technique. The reason for this is presumed to be as follows.
[0086] First, in general, when a coating film is formed using a paint containing a polyurethane resin and a water-soluble melamine resin, the melamine resin has poor compatibility with the polyurethane resin and therefore is difficult to coexist with the polyurethane resin, resulting in a phenomenon in which the self-condensed particles of the melamine resin become larger and the melamine resin becomes concentrated on the surface layer of the coating film.
[0087] In contrast, in the manufacturing method of the surface-treated steel sheet according to the present embodiment, the polyurethane resin (a) containing an anionic functional group is adopted, so that the polyurethane resin (a) and the water-soluble melamine resin (b), which is a water-soluble curing agent containing a triazine ring, are uniformly mixed and coexist in the aqueous medium. When the upper layer paint in such a state is formed on the zinc-based plated steel sheet 11 (or on the lower layer coating film 15) and heated, the autogenous shrinkage of the water-soluble melamine resin (b) is suppressed, and the reaction between the water-soluble melamine resin (b) and the polyurethane resin (a) occurs preferentially. Furthermore, when the vaporization (drying) of the aqueous solvent proceeds due to heating, the polyurethane resin (a) is in a molten state. When the polyurethane resin (a) is in a molten state, the viscosity increases due to the high glass transition temperature of 75°C or more and 160°C or less, resulting in a high cohesive force and a decrease in the diffusion speed of the melamine resin (b). This suppresses the autogenous shrinkage of the water-soluble melamine resin (b), and the reaction between the water-soluble melamine resin (b) and the polyurethane resin (a) occurs preferentially.
[0088] In this way, the melamine resin (b) that has low compatibility with the polyurethane resin (a) is concentrated toward the surface layer of the coating film, but the self-shrinkage of the water-soluble melamine resin (b) is suppressed, and the melamine resin (b) reacts preferentially with the polyurethane resin (a). However, since the self-shrinkage of the water-soluble melamine resin (b) is not completely suppressed, the reaction product of the water-soluble melamine resin (b) reacted with the polyurethane resin (a) and the reaction product resulting from the self-shrinkage of the water-soluble melamine resin (b) coexist in the upper coating film 13. As a result, the portion derived from the water-soluble melamine resin (b) is present in the form of particles dispersed in the upper coating film 13 and in the form concentrated on the surface layer of the upper coating film 13. Moreover, as described above, when the upper coating film 13 is formed, the polyurethane resin (a) generates a high cohesive force, and the reaction between the water-soluble melamine resin (b) and the polyurethane resin (a) occurs preferentially. As a result, the micronized granular water-soluble melamine resin (b) thickens on the surface of the upper coating film 13 to form thickened portion 103 as shown in Figure 3, while the micronized granular water-soluble melamine resin (b) that does not thicken on the surface of the upper coating film 13 forms triazine granules 101 as shown in Figure 3.
[0089] In addition, when providing the underlayer coating film 15, by forming the underlayer coating film 15 using a polyurethane resin (c) having a glass transition temperature of 80° C. or more and 160° C. or less and a lower glass transition temperature than the polyurethane resin (a), it is possible to realize high adhesion between the upper layer coating film 13 and the underlayer coating film 15. Furthermore, by employing the polyurethane resin (a) containing an anionic functional group, the dispersibility of the urethane moiety in the aqueous medium (aqueous paint) is improved, so that the film-forming property of the upper layer coating film 13 is improved and high adhesion between the upper layer coating film 13 and the underlayer coating film 15 is realized.
[0090] As outlined above, it is presumed that the manufacturing method of the surface-treated steel sheet according to this embodiment can produce the surface-treated steel sheet according to this embodiment (i.e., the surface-treated steel sheet having excellent metallic appearance, chemical penetration resistance, and solvent resistance) while keeping costs down.
[0091] Hereinafter, the method for producing a surface-treated steel sheet according to this embodiment will be described in detail.
[0092] <About the top layer coating process> Although the flow is opposite to that shown in FIG. 4, the upper layer coating film forming step will be described in detail below first. In the upper layer coating film forming step, first, an upper layer paint, which is an example of a first paint, is prepared. The upper layer paint contains a polyurethane resin (a), a water-soluble melamine resin (b) which is a water-soluble curing agent containing a triazine ring, and an aqueous solvent.
[0093] [About polyurethane resin (a)] The polyurethane resin (a) is a polyurethane resin that contains an anionic functional group and has a glass transition temperature of 75° C. or more and 160° C. or less. In addition, in the surface-treated steel sheet according to this embodiment, when not only the upper layer coating film 13 but also the lower layer coating film 15 is formed, the glass transition temperature of the polyurethane resin (a) is preferably equal to or higher than the glass transition temperature of the polyurethane resin (c) used in the lower layer coating film 15.
[0094] In order to obtain a high glass transition temperature (85°C or higher and 170°C or lower) in the upper layer coating film 13 as mentioned above, it is suitable to use a polyurethane resin having a urethane bond; for example, a polyester resin with a high glass transition temperature is difficult to manufacture. In addition, since a polyurethane resin with a high glass transition temperature has a very high melt viscosity, it is difficult to apply (form a coating film) unless a paint dispersed in an aqueous medium is used. For this reason, by imparting an anionic functional group to the polyurethane resin, it becomes possible to disperse it in an aqueous medium together with the water-soluble melamine resin.
[0095] The polyurethane resin (a) can be obtained, for example, by reacting a polyhydric alcohol such as ethylene glycol, propylene glycol, diethylene glycol, 1,6-hexanediol, neopentyl glycol, triethylene glycol, bisphenol hydroxypropyl ether, glycerin, trimethylolethane, or trimethylolpropane with a diisocyanate compound such as hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, tolylene diisocyanate, or diphenylmethane diisocyanate, and then chain-extending the resulting mixture with a diamine or the like and dispersing the resulting mixture in water.
[0096] Suitable examples of such polyurethane resin (a) include polyether polyurethane resin (polyurethane resin having a polyether skeleton), polyester polyurethane resin (polyurethane resin having a polyester skeleton), polyether polyester polyurethane resin (polyurethane resin having a polyether skeleton and a polyester skeleton), etc. Coating films using these polyurethane resins tend to have improved chemical penetration resistance and solvent resistance.
[0097] The polyether polyurethane resin, polyester polyurethane resin, and polyether polyester polyurethane resin can be obtained by using at least one of polyether polyol and polyester polyol as the polyhydric alcohol. Examples of polyether polyols include polyethylene glycol, polyoxyethylene glycol, polyoxypropylene glycol, polytetramethylene glycol, and copolymers thereof. Furthermore, polyester polyols can be obtained, for example, by reacting a dibasic acid, such as terephthalic acid, isophthalic acid, adipic acid, azelaic acid, or sebacic acid, or a dialkyl ester of a dibasic acid, with a glycol, such as ethylene glycol, propylene glycol, diethylene glycol, butylene glycol, neopentyl glycol, 1,6-hexane glycol, 3-methyl-1,5-pentanediol, 3,3'-dimethylolheptane, polyoxyethylene glycol, polyoxypropylene glycol, or polytetramethylene ether glycol. Moreover, polyester polyols can be obtained, for example, by ring-opening polymerization of lactones such as polycaprolactone, polyvalerolactone, and poly(β-methyl-γ-valerolactone).
[0098] The glass transition temperature of the polyurethane resin (a) is 75°C or higher and 160°C or lower. If the glass transition temperature of the polyurethane resin (a) is lower than 75°C, the chemical penetration resistance decreases. On the other hand, if the glass transition temperature of the polyurethane resin (a) is higher than 160°C, the processability decreases. If the processability decreases, cracks or the like occur in the upper layer coating film 13, and the chemical penetration resistance and solvent resistance also decrease. From the viewpoint of chemical penetration resistance and solvent resistance (particularly from the viewpoint of chemical penetration resistance), the glass transition temperature of the polyurethane resin (a) is preferably 100°C or higher and 160°C or lower.
[0099] The glass transition temperatures of various resins including the polyester resin can be measured according to the differential scanning calorimetry (DSC) method of measuring the glass transition temperature of plastics (JIS K7121 1987).
[0100] [About water-soluble melamine resin (b)] As the water-soluble melamine resin (b) which is a triazine ring-containing water-soluble curing agent, a generally known water-soluble melamine resin (imino-type melamine resin, methylol-type melamine resin, fully alkyl-etherified melamine resin, etc.) can be used. Examples of commercially available water-soluble melamine resins include water-soluble melamine resins manufactured by Nippon Carbide Corporation, Allnex Corporation, DIC Corporation, etc.
[0101] As the water-soluble melamine resin (b) as described above, it is particularly preferable to use a melamine resin containing an imino group (imino-type melamine resin). By using a melamine resin containing an imino group, the granular water-soluble melamine resin is easily concentrated on the surface layer of the upper coating film 13, so that the solvent resistance is easily improved.
[0102] The term "water-soluble" refers to a dissolution amount of the target substance in 100 parts by mass of water at 25° C. of 5 parts by mass or more (preferably 10 parts by mass or more).
[0103] [About the film formation method (coating method)] In the upper layer coating film forming step, the method for forming (applying) the upper layer paint on the zinc-based plated steel sheet 11 or the lower layer coating film 15 is not particularly limited, and for example, well-known film forming (applying) methods such as roll coating, wringer roll coating, air spraying, airless spraying, immersion, etc. can be used. Furthermore, it is more preferable to form the film in a continuous coating line called a coil coating line or sheet coating line equipped with a film forming device (applicator) for carrying out these well-known film forming (applying) methods, since this improves the efficiency of the coating work and enables mass production.
[0104] [Heating method (baking method) and cooling method] In the upper layer coating film forming step, after the upper layer paint is formed (applied) on the zinc-based plated steel sheet 11 or the lower layer coating film 15, the method of heating the upper layer paint film is not particularly limited, and for example, a generally known device such as a hot air oven, a direct flame oven, a far infrared oven, an induction heating oven, etc. can be used. By heating the upper layer paint film, the aqueous solvent present in the upper layer paint film dries, and then the polyurethane resin (a) and the water-soluble melamine resin (b) react with each other to form the upper layer coating film 13.
[0105] On the other hand, the method for cooling the upper coating film 13 after heating is not particularly limited, but well-known methods such as water cooling (spraying, submersion in water, etc.) and air cooling (spraying nitrogen gas, etc.) can be used.
[0106] In the upper layer coating film forming step, it is particularly preferable to heat the upper layer coating film 13 under conditions such that the heating time from the start of heating to the maximum temperature after the formation of the upper layer paint is 1 second or more and 30 seconds or less, and to cool the upper layer coating film 13 under conditions such that the cooling time from the maximum temperature to 30° C. is 0.1 seconds or more and 5 seconds or less. Here, the heating time and the cooling time are measured by detecting the temperature of the zinc-based plated steel sheet with a thermocouple.
[0107] When the upper layer coating is heated for a short time of 1 to 30 seconds as described above after the coating, the autogenous shrinkage of the water-soluble melamine resin (b) is further suppressed, and when the upper layer coating is cooled for a short time of 0.1 to 5 seconds as described above, the diffusion of the water-soluble melamine resin (b) is suppressed. As a result, the water-soluble melamine resin (b) reacted with the polyurethane resin (a) forms a domain, and is dispersed in the upper layer coating 13 as particles having a number-average particle size of 5 to 20 nm, and is likely to be concentrated in the surface layer within a depth of 15 nm from the surface of the upper layer coating 13. This makes it easier to further improve the metallic appearance, chemical penetration resistance, and solvent resistance of the manufactured surface-treated steel sheet 1.
[0108] Here, if the heating time is less than 1 second, the reaction between the polyurethane resin (a) and the water-soluble melamine resin (b) becomes insufficient, and the chemical penetration resistance and solvent resistance may decrease. On the other hand, if the heating time exceeds 30 seconds, the water-soluble melamine resin (b) becomes more likely to self-condense, the self-condensed particles become larger, and the phenomenon of the coating film being concentrated toward the surface layer occurs, and the metallic appearance and chemical penetration resistance of the produced surface-treated steel sheet 1 may decrease.
[0109] Furthermore, if the cooling time is less than 0.1 seconds, the cooling is performed too quickly, which may result in cracks in the upper coating film 13. On the other hand, if the cooling time exceeds 5 seconds, the water-soluble melamine resin (b) may diffuse, and the metallic appearance and chemical penetration resistance of the produced surface-treated steel sheet 1 may deteriorate.
[0110] From the viewpoints of metallic appearance, resistance to chemical penetration, and resistance to solvents, the heating time is preferably 1 second or more and 20 seconds or less, and from the same viewpoint, the cooling time is preferably 0.1 seconds or more and 2 seconds or less.
[0111] The maximum temperature reached and the holding time thereof are not particularly limited. A maximum temperature reached that is equal to or higher than the boiling point of the aqueous solvent may be appropriately set according to the aqueous solvent used, and the holding time may be set to, for example, about 0.1 seconds or more and 5 seconds or less.
[0112] Furthermore, when forming a plurality of thickened portions 103 in the upper layer coating 13, the upper layer coating 13 is first heated to a temperature of 40 to 100°C for 1 to 20 seconds. Next, the upper layer coating 13 is heated to a temperature of over 200°C for 1 to 10 seconds. After that, the upper layer coating 13 is cooled. By forming the upper layer coating 13 in this manner, thickened portions 103 are formed not only in the surface layer but also at depths other than the surface layer.
[0113] The upper layer coating film forming step according to this embodiment has been described in detail above.
[0114] <About the undercoat coating process> Next, the undercoat film forming step in the method for producing a surface-treated steel sheet according to this embodiment will be described. In the manufacturing method of the surface-treated steel sheet according to this embodiment, there are no particular restrictions on the underlayer coating film formation process, and the underlayer coating film 15 can be formed by a well-known method using a well-known underlayer paint as an example of a second paint.
[0115] Among known methods, from the viewpoints of metallic appearance, chemical penetration resistance, and solvent resistance, the underlayer coating film formation step is preferably a step of forming an underlayer coating film 15 on at least one surface of a zinc-based plated steel sheet 11 by applying an underlayer paint containing at least one of a polyurethane resin (c) containing an anionic functional group and having a glass transition temperature equal to or lower than the glass transition temperature of the polyurethane resin (a), an epoxy resin (d), a silane coupling agent (e), and a rust inhibitor (f) containing one or more elements selected from the group consisting of P, V, Ti, Si, and Zr, and an aqueous solvent, and heating and cooling the resulting film.
[0116] [About polyurethane resin (c)] As mentioned above, the glass transition temperature of the polyurethane resin (c) is preferably equal to or lower than the glass transition temperature of the polyurethane resin (a). When the glass transition temperature of the polyurethane resin (c) is equal to or lower than the glass transition temperature of the polyurethane resin (a), the adhesion between the lower coating film 15 and the upper coating film 13 is improved, and the chemical penetration resistance is further improved.
[0117] The glass transition temperature of the polyurethane resin (c) is preferably within a range of 80°C to 160°C, and is lower than the glass transition temperature of the polyurethane resin (a) (preferably lower than the glass transition temperature of the polyurethane resin (a) by 5°C or more). If the glass transition temperature of the polyurethane resin (c) is lower than 80°C, the chemical penetration resistance may decrease. On the other hand, if the glass transition temperature of the polyurethane resin (c) is higher than 160°C, the processability may decrease. If the processability decreases, cracks or the like may occur in the lower layer coating film 15, and the chemical penetration resistance and solvent resistance also decrease. From the viewpoint of chemical penetration resistance and solvent resistance (particularly from the viewpoint of chemical penetration resistance), the glass transition temperature of the polyurethane resin (c) is preferably within a range of 100°C to 160°C.
[0118] The polyurethane resin (c) may be a polyurethane resin containing a polyurethane resin having a glass transition temperature of 80° C. or more and 160° C. or less, and a polyurethane resin having a glass transition temperature of 20° C. or more and 60° C. or less. By using polyurethane resins having different glass transition temperatures and adjusting the glass transition temperature of the polyurethane resin (c), it becomes easier to further improve the chemical penetration resistance.
[0119] Specific examples of the polyurethane resin (c) include the various polyurethane resins exemplified as the polyurethane resin (a).
[0120] [About epoxy resin (d)] Examples of the epoxy resin (d) include bisphenol A type epoxy resin, bisphenol F type epoxy resin, novolac type epoxy resin, aliphatic type epoxy resin, etc. Among these resins, aliphatic type epoxy resin is particularly preferable as the epoxy resin (d) because it is less likely to discolor due to baking.
[0121] The specific type of these epoxy resins (d) is not particularly limited, and various commercially available epoxy resins (d) can be used. In addition, epoxy resins (d) having a glass transition temperature within the above range can be synthesized in-house and used as appropriate.
[0122] [About silane coupling agent (e)] Silane coupling agent (e) is not particularly limited, and various known silane coupling agents can be used. Examples of such silane coupling agents include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, bis(trimethoxysilylpropyl)amine, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 3-glycidoxypropylmethyldiethoxysilane. By including such a silane coupling agent in the lower layer coating, it is possible to further improve the chemical penetration resistance of the lower layer coating film 15.
[0123] [About rust inhibitors (f)] In the underlayer coating film forming step according to this embodiment, a rust inhibitor containing at least one element selected from the group consisting of P, V, Ti, Si, and Zr can be used as the rust inhibitor (f). By including such a rust inhibitor (f) in the underlayer paint, it is possible to improve the corrosion resistance of the underlayer coating film 15.
[0124] Examples of the P-containing compound that functions as a rust inhibitor (f) include phosphoric acids such as orthophosphoric acid, metaphosphoric acid, pyrophosphoric acid, triphosphoric acid, tetraphosphoric acid, and salts thereof; phosphonic acids such as aminotri(methylenephosphonic acid), 1-hydroxyethylidene-1,1-diphosphonic acid, ethylenediaminetetra(methylenephosphonic acid), diethylenetriaminepenta(methylenephosphonic acid), and salts thereof; and organic phosphoric acids such as phytic acid and salts thereof.
[0125] Examples of compounds containing V that function as the rust inhibitor (f) include vanadium pentoxide, metavanadic acid, ammonium metavanadate, sodium metavanadate, vanadium oxytrichloride, vanadium trioxide, vanadium dioxide, vanadium oxysulfate, vanadium oxyacetylacetonate, vanadium acetylacetonate, vanadium trichloride, and phosphomolybdic acid. In addition, a pentavalent vanadium compound reduced to a tetravalent or divalent form by an organic compound having at least one functional group selected from the group consisting of a hydroxyl group, a carbonyl group, a carboxyl group, a primary to tertiary amino group, an amide group, a phosphoric acid group, and a phosphonic acid group, a salt of an oxovanadium cation and an inorganic acid anion such as hydrochloric acid, nitric acid, phosphoric acid, or sulfuric acid, or an organic acid anion such as formic acid, acetic acid, propionic acid, butyric acid, or oxalic acid, or a chelate of an organic acid and a vanadyl compound such as vanadyl glycolate or vanadyl dehydroascorbate can be used.
[0126] Examples of compounds containing Ti that function as a rust inhibitor (f) include potassium titanium oxalate, titanyl sulfate, titanium chloride, titanium lactate, titanium isopropoxide, isopropyl titanate, titanium ethoxide, titanium 2-ethyl-1-hexanolate, tetraisopropyl titanate, tetra-n-butyl titanate, titania sol, and titanium hydrofluoric acid or a salt thereof.
[0127] Examples of compounds containing Si that function as a rust inhibitor (f) include colloidal silica such as SNOWTEX C, SNOWTEX O, SNOWTEX N, SNOWTEX S, SNOWTEX UP, SNOWTEX PS-M, SNOWTEX PS-L, SNOWTEX 20, SNOWTEX 30, SNOWTEX 40 (all manufactured by Nissan Chemical Industries, Ltd.), Adelite AT-20N, Adelite AT-20A, Adelite AT-20Q (all manufactured by Asahi Denka Kogyo Co., Ltd.), and gas-phase silica such as Aerosil 50, Aerosil 130, Aerosil 200, Aerosil 300, Aerosil 380, Aerosil TT600, Aerosil MOX80, Aerosil MOX170 (all manufactured by Nippon Aerosil Co., Ltd.).
[0128] Examples of Zr-containing compounds that function as the rust inhibitor (f) include zirconyl nitrate, zirconyl acetate, zirconyl sulfate, ammonium zirconium carbonate, potassium zirconium carbonate, sodium zirconium carbonate, zirconium acetate, zirconium hydrofluoric acid, and salts thereof.
[0129] [Film formation method (coating method), heating method (baking method) and cooling method] In the lower layer coating film forming step, there is no particular limitation on the method for forming and heating the lower layer paint on at least one surface of the zinc-based plated steel sheet 11 and then cooling it, and for example, various film forming methods (painting methods), heating methods, and cooling methods can be used as described in the upper layer coating film forming step. In addition, there is no particular limitation on the maximum temperature reached, heating time, holding time, and cooling time of the zinc-based plated steel sheet 11 coated with the lower layer paint, and these may be set appropriately.
[0130] <Other ingredients> In the manufacturing method of the surface-treated steel sheet according to this embodiment, both the upper layer paint and the lower layer paint may contain well-known additives such as wax, leveling agent, defoamer, thickener, dispersant, etc. That is, in the surface-treated steel sheet according to this embodiment, both the upper layer coating film 13 and the lower layer coating film 15 may contain these well-known additives.
[0131] <About the texture formation process> In the manufacturing method of the surface-treated steel sheet according to the present embodiment, various textures such as matte finish, roughness, streaks (hairline), cloth grain (satin), hammered texture, etc. may be formed as necessary on the surface of the zinc-based plated steel sheet 11 to which the above-mentioned top layer paint is applied. By forming such textures in advance on the surface of the zinc-based plated steel sheet 11, it is possible to further improve the design of the surface-treated steel sheet according to the present embodiment.
[0132] Here, the method and device used for forming the above-mentioned various textures are not particularly limited, and various known methods and devices can be appropriately used.
[0133] The method for producing a surface-treated steel sheet according to this embodiment has been described in detail above. EXAMPLES
[0134] The surface-treated steel sheet and the method for manufacturing the surface-treated steel sheet according to the present invention will be described in more detail below with reference to examples and comparative examples. Note that the examples shown below are merely examples of the surface-treated steel sheet and the method for manufacturing the surface-treated steel sheet according to the present invention, and the surface-treated steel sheet and the method for manufacturing the surface-treated steel sheet according to the present invention are not limited to the examples below.
[0135] (Test Example 1) <Zinc-based coated steel sheet (base sheet)> The following zinc-based plated steel sheets (base sheets) were used: hot-dip galvanized steel sheet "NS Silver Zinc (registered trademark)" (hereinafter referred to as "GI") manufactured by Nippon Steel Corporation; electrolytic galvanized steel sheet "NS Zincoat (registered trademark)" (hereinafter referred to as "EG") manufactured by Nippon Steel Corporation; zinc-nickel alloy plated steel sheet "NS Zinclite (registered trademark)" (hereinafter referred to as "ZL") manufactured by Nippon Steel Corporation; zinc-iron alloy plated steel sheet "NS Silver Alloy (registered trademark)" (hereinafter referred to as "GA"); zinc-aluminum-magnesium-silicon alloy plated steel sheet "Super Dima (registered trademark)" (hereinafter referred to as "SD") manufactured by Nippon Steel Corporation; and zinc-aluminum-magnesium alloy plated steel sheet "ZAM (registered trademark)" (hereinafter referred to as "ZAM") manufactured by Nippon Steel Corporation. The thickness of each zinc-based plated steel sheet was 0.6 mm.
[0136] The plating weight of ZL is 20g / m per side. 2 The amount of nickel in the plating layer was 12 mass%. The plating weight of GI, SD, GL, and ZAM was 60 g / m per side. 2The plating weight of GA was 45 g / m2 per side. 2 The plating weight of EG was 20 g / m per side. 2 It was. In some examples and comparative examples, a hairline texture was formed on the surface of a zinc-based plated steel sheet.
[0137] <Paint> In this test example, a surface-treated steel sheet was prepared on one side of the above-mentioned zinc-based plated steel sheet (original sheet) in a single-layer structure having only an upper layer coating film as shown in Fig. 1A, or a two-layer structure having an underlayer coating film and an upper layer coating film as shown in Fig. 1B. The polyurethane resin and water-soluble melamine resin used in preparing the upper layer coating are shown in Table 1 below. Similarly, the polyester resin, water-soluble melamine resin, silane coupling agent, and colorant used in preparing the lower layer coating are shown in Table 2 below.
[0138] <Top layer paint> 1,3-bis(isocyanatemethyl)cyclohexane (145g), dimethylolpropionic acid (20g), neopentyl glycol (15g), polyurethane diol (75g) with different aromatic ring numbers in the molecular chain, and acetonitrile (64g) as a solvent were added, and the mixture was heated to 75°C under a nitrogen atmosphere and stirred for 3 hours. After confirming that the reaction solution had reached the required amine equivalent, the reaction solution was cooled to 40°C, and then 30g of triethylamine (boiling point 89°C) was added to obtain an acetonitrile solution of polyurethane prepolymer. 300g of this solution was dispersed in 700g of water using a homodisper to form an emulsion, and the solution was kept at 40°C, and 35.6g of ethylenediaminehydrazine monohydrate was added as a chain extender to cause a chain extension reaction. Next, the reaction solution was placed at 50°C and a reduced pressure of 150mmHg to distill off the acetonitrile used in the synthesis of the polyurethane prepolymer, to obtain self-made polyurethane resins 1 to 5. The top layer paint was made by adding a curing agent, an ultraviolet absorber, a light stabilizer, and a colorant to these homemade polyurethane resins and commercially available resins as the main resins. Sumisorb 200 (manufactured by Sumika Chemtex Co., Ltd.) was used when adding an ultraviolet absorber to the top layer paint. Adeka STAB LA-77G (manufactured by ADEKA Co., Ltd.) was used when adding a light stabilizer to the top layer paint. Used. The formulations of each upper layer paint are shown in Tables 3A to 3C. <Lower paint> The formulations of the undercoat paint are shown in Tables 4A to 4C.
[0139] [Table 1]
[0140] [Table 2]
[0141] [Table 3A]
[0142] [Table 3B]
[0143] [Table 3C]
[0144] [Table 4A]
[0145] [Table 4B]
[0146] [Table 4C]
[0147] <Preparation of surface-treated steel sheet> Various zinc-based plated steel sheets were degreased by immersing them for 10 seconds in an aqueous solution containing 2 mass % of FC-4336 (manufactured by Nippon Parkerizing Co., Ltd.) at a temperature of 60° C., rinsed with water, and then dried.
[0148] Next, the underlayer paint prepared as described above was applied to each of the plates using a roll coater. In an induction heating furnace into which hot air was blown, the underlayer paint film was heated (dried and cured) under the conditions that the maximum temperature of the metal plate reached was 150°C and the heating time from the start of heating to the maximum temperature reached was 5 seconds. One second after the maximum temperature reached, water was sprayed onto the painted metal plate, and the plate was water-cooled under the conditions that the cooling time from the maximum temperature reached to 30°C was 1 second. The maximum temperature was maintained for 1 second during heating.
[0149] Next, the upper layer paint prepared as described above was applied to each of the plates using a roll coater. In an induction heating furnace into which hot air was blown, the maximum temperature of the metal plate, the heating time from the start of heating to the maximum temperature, and the holding time at 40 to 100°C were adjusted, and the film of the upper layer paint was heated (dried and cured). One second after the maximum temperature was reached, water was sprayed onto the coated metal plate, and the plate was water-cooled under conditions that the cooling time from the maximum temperature to 30°C was one second. The holding time at the maximum temperature during heating was set to one second.
[0150] For each of the produced surface-treated steel sheet samples, the thickness (enrichment depth) of the surface thickened portion and the number-average particle size (particle size) of the granular triazine moiety (water-soluble melamine resin) in the upper coating film were measured according to the method described above. In addition, N1 / N2, which is the ratio of the N concentration N1 at a depth of 0.2 μm from the surface of the first coating film to the N concentration N2 at a depth of 0.2 μm on the first coating film side from the interface between the first coating film and the metal sheet, was measured according to the method described above. In addition, the surface thickened area was stained with osmium oxide and observed at 100,000 times magnification using a transmission electron microscope to determine whether melamine particles of 5 nm or more were observed, using the method previously described.
[0151] The ratio of aromatic rings and urethane bonds contained in the coating was estimated for each of the samples of surface-treated steel sheets produced. Specifically, the coating was analyzed from the surface of the surface-treated steel sheets using a Fourier transform infrared spectrophotometer (FT-IR, PerkinElmer Frontier) and the 1510±10 cm -1 The peak height of (I1) and 1533 ± 10 cm due to the urethane bond -1 The peak height (I2) of each peak was then calculated. The ratio of these peak heights (I1 / I2) was then calculated.
[0152] For each of the produced surface-treated steel sheet samples, the glass transition temperature (Tg) of each coating film was measured according to the method already described.
[0153] <Evaluation method> Each of the produced surface-treated steel sheets was evaluated according to the following criteria.
[0154] [Metal appearance] A clear paint was applied to a hairline stainless steel plate as specified in JIS G4305:2012. A commercially available polyester / melamine paint (NSC200HQ, manufactured by Nippon Paint Industrial Coatings Co., Ltd.) was used as the clear paint, and the paint was applied using a bar coater. The stainless steel plate to which the paint was applied was then baked and cured for 30 seconds in a hot air oven. Using this process, several types of comparison samples with different coating thicknesses were prepared. The metallic feel of the test sample was then compared with that of these comparison samples, and the metallic feel of the test sample was evaluated based on the following evaluation criteria. A rating of 3 or higher was deemed to be acceptable.
[0155] (Evaluation Criteria) 5: Stainless steel (unpainted) with an equivalent or superior metallic feel 4: Stainless steel (coating thickness 5μm) equivalent 3: Stainless steel (coating thickness 10 μm) equivalent 2: Stainless steel (coating thickness 30 μm) equivalent 1: No metallic feel
[0156] [Chemical penetration resistance test] Each of the produced surface-treated steel sheets was cut into a width of 5 cm, and all edges were protected with Nitoflon (registered trademark) tape to produce samples, which were then immersed in 5% sulfuric acid water at 20°C for 24 hours and the degree of discoloration was evaluated on a 5-point scale. A rating of 3 or higher was considered to be acceptable.
[0157] (Evaluation Criteria) 5: No discoloration 4: Very slight discoloration 3: Slightly discolored 2: Many discolorations 1: Significant discoloration and peeling of paint
[0158] [Weather resistance] The specimen was exposed to carbon arc light for 500 hours using a Sunshine Weather Meter (manufactured by Suga Test Instruments). Water was sprayed on the specimen for 12 minutes per hour to simulate rain. The color tone before and after the test was measured using the CIELAB (JIS Z8729) L * ,a * ,b * The color system was measured using a Konica Minolta CR-400 spectrophotometer, and the color difference ΔE * was calculated. ΔE * The evaluation was done on a 5-point scale according to the criteria. A rating of 3 or above was considered a pass.
[0159] (Evaluation Criteria) 5:ΔE * <= 1.0 4:ΔE * <=3.0 3:ΔE * <= 5.0 2:ΔE * <= 10.0 1:ΔE * >10.0
[0160] [Processability test] Each of the manufactured surface-treated steel sheets was cut to a width of 5 cm and subjected to 2T bending in an atmosphere at 20°C according to the test method in accordance with JIS G3312. Specifically, two coated sheets identical to the test pieces were sandwiched inside each other, and the surfaces on which the upper and lower coating films were formed were placed on the outside, and the sheets were bent at 180 degrees in close contact. The cracks in the coating were evaluated on a four-level scale of A (excellent), B, C, and D (poor). Evaluation criteria of A, B, and C were judged to be acceptable.
[0161] (Evaluation Criteria) A: No cracks B: Slightly cracked C: Many cracks D: Many cracks and peeling paint
[0162] [Stain resistance test] Each of the manufactured surface-treated steel sheets was coated with red magic ink (Teranishi Chemical Industry Co., Ltd.), wiped off with ethanol after 24 hours, and the ink traces were evaluated on a 5-point scale. For those with significant traces, a CR-400 made by Konica Minolta was used to measure the redness of the steel sheets before and after the test. * The difference (Δa * ) and evaluated as follows. A rating of 3 or more was considered to be acceptable.
[0163] (Evaluation Criteria) 5: No marks left 4: Slight marks remain 3:Δa * is greater than 1 and less than or equal to 3 2:Δa * More than 3 and less than 5 1:Δa * More than 5
[0164] The levels and evaluation results of each of the produced surface-treated steel sheets are shown in Tables 5A to 5C.
[0165] [Table 5A]
[0166] [Table 5B]
[0167] [Table 5C]
[0168] As is clear from Table 5 above, the surface-treated steel sheets corresponding to the examples of the present invention are excellent in metallic appearance, chemical penetration resistance, solvent resistance and processability. [Explanation of symbols]
[0169] 1. Surface-treated steel sheets 11 Zinc-plated steel sheet 13 Upper layer coating (first coating) 15 Lower layer coating (second coating) 101 Triazine granules (dispersed second part) 103 Enriched part (enriched type second part)
Claims
1. Steel plate; a zinc-based plating layer provided on at least one surface of the steel sheet; a first coating film containing 80 mass % or more of a urethane resin as a main component and further containing a melamine resin as a curing agent, and having a film thickness of 10 μm or less; Equipped with Among the absorption peaks obtained by measuring the surface of the first coating film by infrared spectroscopy, 1510±10 cm due to aromatic rings -1 Peak height (I 1 ) and 1533 ± 10 cm due to urethane bonds -1 Peak height (I 2 ) ratio I 1 / I 2 is between 0.90 and 1.20 A surface-treated steel sheet characterized by:
2. 2. The surface-treated steel sheet according to claim 1, wherein the first coating film contains at least one of an ultraviolet absorber and a light stabilizer.
3. 3. The surface-treated steel sheet according to claim 2, wherein the first coating film contains at least one of the ultraviolet absorber and the light stabilizer in a total amount of 0.5 to 2.0 mass %.
4. the first coating film has a first portion having a urethane bond skeleton and a second portion having a triazine ring skeleton, The glass transition temperature of the first coating film is 85° C. or higher and 170° C. or lower, When the second portion is stained with osmium oxide and observed at a magnification of 100,000 times using a transmission electron microscope, a dispersed-type second portion in which particles having a number-average particle size of 5 to 20 nm are dispersed, and a concentrated-type second portion which is present at a position up to a depth of 15 nm from the surface of the first coating film and in which no particles having a number-average particle size of 5 nm or more are independently observed, are observed. The surface-treated steel sheet according to any one of claims 1 to 3.
5. The surface-treated steel sheet according to claim 4, characterized in that N1 / N2, which is the ratio of N concentration N1 at a depth position of 0.2 μm from the surface of the first coating film to N concentration N2 at a depth position of 0.2 μm toward the first coating film from the interface between the first coating film and the zinc-based plated steel sheet, is 1.2 or more.
6. A second coating film is further provided between the first coating film and the zinc-based plating layer, The glass transition temperature of the second coating film is equal to or lower than the glass transition temperature of the first coating film. The surface-treated steel sheet according to any one of claims 1 to 5.
7. 7. The surface-treated steel sheet according to claim 1, wherein at least one of the first coating film and the second coating film contains a colorant.
8. The surface-treated steel sheet according to any one of claims 1 to 7, characterized in that a texture is formed on a surface of at least one of the zinc-based plating layer and the steel sheet.
Citation Information
Patent Citations
Method for coating metallic sheet
JP1993111675A
Precoat metal and roll painting method thereof
JP1995313929A
Coating composition and metal plate coated therewith
JP1995331167A
Precoated metal sheet excellent in bending processability
JP2005053002A
Coated metal sheet excellent in processability and antistaining properties
JP2006175815A