Surface-treated steel sheet
The surface-treated steel sheet with optimized resin particle distribution and chemical conversion coating on both sides addresses the issues of scratches and corrosion by minimizing direct contact and enhancing adhesion and barrier properties, achieving improved resistance to surface contact flaws and corrosion.
Patent Information
- Application Number
- JP2024523984
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-09-27
- Filing Date
- 2023-09-27
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2043-09-27
AI Technical Summary
Existing surface-treated steel sheets face issues with scratches and corrosion due to contact between surfaces during coil winding and processing, particularly when one surface has a thinner colored film layer than the other, and existing solutions like using soft urethane or fluororesin beads for scratch resistance compromise corrosion resistance.
A surface-treated steel sheet with a zinc plating layer and two colored film layers on both sides, where the ratio and thickness of resin particles in each layer are optimized to minimize direct contact and enhance scratch resistance while maintaining corrosion resistance, using acrylic resin particles and a chemical conversion coating for improved adhesion and barrier properties.
The solution significantly improves scratch resistance and corrosion resistance by optimizing the film structure, reducing direct contact between surfaces and enhancing the adhesion and barrier properties of the film layers.
Smart Images

Figure 0007583349000009 
Figure 0007583349000010 
Figure 0007583349000011
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface-treated steel sheet. [Background technology]
[0002] Surface-treated steel sheets, such as organic resin-coated plated steel sheets (also called pre-coated steel sheets), which are zinc-based plated steel sheets coated with an organic resin film on the surface thereof, have come to be used for home appliances, building materials, automobiles, etc., in place of post-painted products that were conventionally painted after forming. These surface-treated steel sheets are made by coating rust-proofed steel sheets or plated steel sheets with a colored organic film, and have the characteristics of being beautiful, workable, and having good corrosion resistance. These surface-treated steel sheets are often used as materials for home appliances, building materials, automobiles, etc., without being further painted after being pressed. For this reason, such surface-treated steel sheets are required to have excellent scratch resistance so as not to lose their beauty during processing. For this reason, various techniques have been proposed in the past to improve the scratch resistance and other properties of surface-treated steel sheets.
[0003] For example, the following Patent Document 1 discloses a precoated metal sheet for electronic and electrical devices that is excellent not only in scratch resistance but also in corrosion resistance and conductivity. This precoated metal sheet is formed by providing a chemical conversion coating on the surface of a metal sheet having a specified surface roughness, and then providing a resin coating having a thickness of 0.4 to 2.0 μm and containing urethane beads or fluororesin beads having an average particle size of 1.0 to 10 μm on one side, and providing a resin coating having a thickness of 0.2 to 2.0 μm and containing urethane beads or fluororesin beads having an average particle size of 0.1 to 6.0 μm on the other side. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2010-5545 A Summary of the Invention [Problem to be solved by the invention]
[0005] Here, various surface-treated steel sheets, including the precoated metal sheet disclosed in the above Patent Document 1, are generally produced by providing a desired coating film on a metal sheet as a base material in a continuous coating line. Examples of the metal sheet as a base material include steel sheets including various plated steel sheets, aluminum sheets, aluminum alloy sheets, etc. The metal sheet provided with the desired coating film is wound into a coil at the end of the continuous coating line and transported to a customer.
[0006] In such a coil state, one side of the surface coating of the surface-treated steel sheet comes into contact with the other side. In this case, there are problems such as scratches due to contact during coil winding, blocking during coil storage, i.e., the coatings on the front and back are pressed together under a certain pressure, and pressure marks, i.e., the shape of one side is transferred to the other side. In addition, there is also a problem that scratches are caused by contact between one side and the other side when handling the cut metal sheet during processing at the customer's site. Furthermore, from the viewpoint of cost reduction, etc., colored coating layers are provided on both sides of the metal sheet as the base material with different thicknesses, and the thickness on one side is sometimes made thinner than the thickness on the other side. In this case, there is also a problem that it is necessary to ensure the scratch resistance of the other side.
[0007] In this regard, the above-mentioned Patent Document 1 discloses a problem that the resin film on the opposite side of the metal film that is mixed to give electrical conductivity to the resin film is damaged when the resin film is coiled up. The technology described in the above-mentioned Patent Document 1 suppresses damage to the resin film when the resin film is coiled up by providing a resin film containing resin beads on both sides of the metal plate. However, from the viewpoint of scratch resistance to optical disks, the material of the resin particles is limited to soft urethane beads or fluororesin beads with excellent slipperiness. In addition, from the viewpoint of ensuring electrical conductivity, the thickness of the resin film needs to be 2.0 μm or less. Therefore, there is room for improvement in achieving both scratch resistance, resistance to surface contact scratches, and corrosion resistance.
[0008] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a surface-treated steel sheet having good corrosion resistance, which further improves scratch resistance, in particular, resistance to surface contact scratches caused by contact between one surface and the other surface. [Means for solving the problem]
[0009] In order to solve the above problems, the inventors conducted intensive research and came up with the idea that it may be possible to further improve scratch resistance by differentiating the coating film configuration on one side and the other side of a steel sheet, which led to the completion of the present invention. The gist of the present invention, which was completed based on this concept, is as follows.
[0010] (1) A steel sheet comprising a zinc-containing plating layer located on both surfaces of the steel sheet, a first colored film layer located on the plating layer on one surface of the steel sheet, and a second colored film layer located on the plating layer on the other surface of the steel sheet, wherein the ratio of the film thickness of the second colored film layer to the film thickness of the first colored film layer is 0.1 or more and 0.5 or less, the first colored film layer and the second colored film layer contain resin particles, and when a cross section of the first colored film layer cut in the film thickness direction is observed, the length of the observed resin particles in the film thickness direction of the first colored film layer is the ratio of the number of the resin particles having a thickness equal to or greater than the film thickness of the first colored coating layer to the number of all the observed resin particles is 1% or more and 30% or less when the thickness of the resin particles is taken as the thickness of the resin particles; and when a cross section of the second colored coating layer is observed, the ratio of the number of the resin particles having a thickness equal to or greater than the film thickness of the second colored coating layer to the number of all the observed resin particles is 50% or more and 100% or less when the length of the observed resin particles in the film thickness direction of the second colored coating layer is taken as the thickness of the resin particles. (2) The surface-treated steel sheet according to (1), wherein, when a cross-section of the first colored coating layer is observed, a first observation length is a length of 1000 μm in a direction perpendicular to the thickness direction of the first colored coating layer, and a first occupation length is a sum of lengths of portions corresponding to the resin particles in a direction perpendicular to the thickness direction when a portion occupied by the resin particles within the first observation length is projected in the thickness direction, the ratio of the first occupation length to the first observation length is 15% or more and 40% or less; and a second observation length is a length of 1000 μm in a direction perpendicular to the thickness direction of the second colored coating layer, and a second occupation length is a sum of lengths of portions corresponding to the resin particles in a direction perpendicular to the thickness direction when a portion occupied by the resin particles within the second observation length is projected in the thickness direction, the ratio of the second occupation length to the second observation length is 5% or more and 15% or less. (3) The surface-treated steel sheet according to (1) or (2), wherein the first colored coating layer has a thickness of 3 μm or more and 10 μm or less. (4) The surface-treated steel sheet according to (1) or (2), wherein the thickness of the resin particles contained in the first colored coating layer is less than twice the thickness of the first colored coating layer, and the thickness of the resin particles contained in the second colored coating layer is less than three times the thickness of the second colored coating layer. (5) The surface-treated steel sheet according to (1) or (2), wherein the resin particles are acrylic resin particles. (6) The surface-treated steel sheet according to (1) or (2), wherein the film-forming components of the first colored coating layer and the second colored coating layer have a glass transition temperature Tg of 30°C or higher and 70°C or lower. (7) The surface-treated steel sheet according to (1) or (2), further comprising a chemical conversion coating layer between the plating layer and the first colored coating layer on one side of the steel sheet, and between the plating layer and the second colored coating layer on the other side of the steel sheet. (8) The surface-treated steel sheet according to (1) or (2), wherein the resin particles have an average particle size of 3 μm or more and 15 μm or less. Effect of the Invention
[0011] As described above, according to the present invention, it is possible to provide a surface-treated steel sheet having good corrosion resistance, in which the scratch resistance is further improved, in particular the resistance to surface contact scratches caused by contact between one surface and the other surface. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is an explanatory diagram showing a schematic structure of a surface-treated steel sheet according to an embodiment. [Diagram 2] FIG. 2 is an explanatory diagram of the thickness of resin particles when a cross section of a surface-treated steel sheet according to an embodiment is observed. [Diagram 3] FIG. 2 is an explanatory diagram of the occupied length of resin particles when a cross section of a surface-treated steel sheet according to an embodiment is observed. [Figure 4] FIG. 2 is an explanatory diagram of the occupied length of resin particles when a cross section of a surface-treated steel sheet according to an embodiment is observed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In this specification and the drawings, components having substantially the same functional configurations are designated by the same reference numerals, and duplicated explanations will be omitted.
[0014] <About surface-treated steel sheet 1> Hereinafter, a surface-treated steel sheet according to an embodiment of the present invention will be described in detail with reference to Fig. 1. Fig. 1 is an explanatory diagram that shows a schematic structure of the surface-treated steel sheet according to this embodiment.
[0015] <Overall structure of surface-treated steel sheet 1> As shown in FIG. 1, the surface-treated steel sheet 1 according to the present embodiment has a steel sheet 10 as a substrate, a plating layer 20 provided on the surface of the steel sheet 10, and a colored coating layer 30 located on the surface of the plating layer 20. As shown in FIG. 1, it is preferable that the steel sheet 1 further has a chemical conversion coating layer 40 between the plating layer 20 and the colored coating layer 30. The plating layer 20, the colored coating layer 30, and the chemical conversion coating layer 40 are provided on both sides of the steel sheet 10. That is, a first plating layer 20a, a first colored coating layer 30a, and a first chemical conversion coating layer 40a are respectively formed on one side (first side 10a) of the steel sheet 10, which corresponds to the upper side in the figure. Moreover, on the other surface (second surface 10b) which corresponds to the lower surface in the figure, a second plating layer 20b, a second colored coating layer 30b, and a second chemical conversion coating layer 40b are formed.
[0016] <About Steel Plate 10> The steel plate 10 as the substrate is not particularly limited, and various steel plates 10 can be used depending on the mechanical strength required for the surface-treated steel plate 1. Examples of such steel plates 10 include various steel plates 10 such as Al-killed steel, extra-low carbon steel containing Ti, Nb, etc., and high-strength steel in which extra-low carbon steel further contains strengthening elements such as P, Si, Mn, etc.
[0017] Furthermore, the thickness of the steel plate 10 according to this embodiment is not particularly limited and may be appropriately set depending on the mechanical strength required for the surface-treated steel plate 1, and may be, for example, about 0.2 mm to 10.0 mm.
[0018] <Regarding plating layer 20> The type of plating in the plating layer 20 of the surface-treated steel sheet 1 according to this embodiment is not particularly limited. For example, a zinc-based plating can be used as the plating type. Examples of such zinc-based plating include zinc-nickel alloy plating, galvannealed hot-dip plating, aluminum-zinc alloy plating, zinc-aluminum-magnesium alloy plating, zinc-vanadium composite plating, and zinc-zirconium composite plating.
[0019] Among such zinc-based platings, zinc-aluminum-magnesium alloy plating is particularly preferred, and zinc-aluminum-magnesium-silicon alloy plating containing 4 to 22 mass% Al, 1 to 10 mass% Mg, 0.0001 to 2.0000 mass% Si, with the remainder being Zn and impurities, is more preferred.
[0020] [Al:4~22% by mass] By setting the Al content to 4 mass% or more, it is possible to further improve the corrosion resistance of the steel sheet. The Al content is more preferably 5 mass% or more. On the other hand, by setting the Al content to 22 mass% or less, it is possible to further improve the corrosion resistance of the steel sheet while suppressing saturation of the corrosion resistance improvement effect as described above. The Al content is more preferably 16 mass% or less.
[0021] [Mg:1~10% by mass] By setting the Mg content to 1 mass% or more, it is possible to further improve the corrosion resistance of the steel sheet. The Mg content is more preferably 2 mass% or more. On the other hand, by adjusting the Mg concentration in the plating bath used to form the plating layer 20 so that the Mg content in the plating layer 20 after production is 10 mass% or less, it is possible to stabilize the generation of dross in the plating bath and stably produce a plated steel sheet. In this specification, the plated steel sheet refers to a steel sheet 10 having a plating layer 20 formed on the surface thereof. It is more preferable to adjust the Mg concentration in the plating bath used to form the plating layer 20 so that the Mg content in the plating layer 20 after production is 5 mass% or less.
[0022] [Si:0.0001~2.0000% by mass] By setting the Si content to 0.0001% by mass or more, it is possible to further improve the adhesion of the plating layer 20 (more specifically, the adhesion between the base steel sheet 10 and the plating layer 20). On the other hand, by setting the Si content to 2.0000% by mass or less, it is possible to further improve the adhesion of the plating layer 20 while suppressing saturation of the adhesion improving effect of the plating layer 20. The Si content is more preferably 1.6000% by mass or less.
[0023] Furthermore, the zinc-containing plating layer 20 may contain elements such as Fe, Sb, Pb, etc., either alone or in combination, in an amount of 1 mass % or less in place of a portion of the remaining Zn.
[0024] An example of a plated steel sheet having a plating layer 20 having the above-mentioned chemical composition is a molten zinc-aluminum-magnesium-silicon alloy plated steel sheet (e.g., "Super Dima (registered trademark)" manufactured by Nippon Steel Corporation), such as a plated steel sheet having a Zn-11%Al-3%Mg-0.2%Si alloy plating layer.
[0025] The plating layer 20 as described above can be manufactured, for example, as follows. First, the surface of the prepared steel sheet 10 is subjected to pretreatment such as cleaning and degreasing as necessary. Thereafter, the steel sheet 10 that has been pretreated as necessary is immersed in a hot-dip plating bath having a desired chemical composition, and the steel sheet 10 is removed from the plating bath. In this plating operation, plating may be performed by either a continuous coil plating method or a plating method for a single cut sheet.
[0026] The temperature of the hot dip plating bath varies depending on the composition, but is preferably in the range of 400 to 500°C, for example.
[0027] The coating weight of the coating layer 20 can be controlled by adjusting the lifting speed of the steel sheet 10, the flow rate and flow rate of the wiping gas ejected from the wiping nozzle provided above the coating bath, etc. The coating weight of the coating layer 20 is 30 g / m in total on both sides of the steel sheet 10. 2or more (i.e., 15 g / m per side) 2 It is preferable that the coating weight is 30 g / m or more. 2 By setting the coating weight at or above this level, it is possible to reliably ensure the corrosion resistance of the zinc-based plated steel sheet 10. More preferably, the coating weight is 40 g / m2 in total on both sides of the steel sheet 10. 2 On the other hand, the coating weight of the plating is 600 g / m2 or less in total on both sides of the steel sheet 10 (i.e., 300 g / m2 per side). 2 It is preferable that the coating weight is 600 g / m or less. 2 By setting the thickness to 550 g / m or less, it is possible to further improve the corrosion resistance while ensuring the smoothness of the surface of the Zn-containing plating layer 13. More preferably, the plating coverage is 550 g / m in total on both sides of the steel sheet 10. 2 The following is the result.
[0028] After adjusting the coating weight of the hot-dip coating, the steel sheet is cooled. At this time, the cooling conditions are not particularly limited.
[0029] <About the colored film layer 30> The colored coating layer 30 is a coating layer colored to a desired color by containing a color pigment. The surface-treated steel sheet 1 according to this embodiment includes, as the colored coating layer 30, a first colored coating layer 30a formed on the first surface 10a of the steel sheet 10 and a second colored coating layer 30b formed on the second surface 10b. Hereinafter, when describing a configuration common to the first colored coating layer 30a and the second colored coating layer 30b, they may be collectively referred to simply as the colored coating layer 30.
[0030] As shown in FIG. 1, the colored coating layer 30 contains a film-forming component 301 and resin particles 303. When the surface-treated steel sheet 1 is cut in a cross section in the thickness direction of the colored coating layer 30 and observed (hereinafter referred to as cross-sectional observation), at least a part of the resin particles 303 in both the first colored coating layer 30a and the second colored coating layer 30b has a thickness equal to or greater than the thickness of the first colored coating layer 30a or the second colored coating layer 30b. In other words, the number of the resin particles 303 having a thickness equal to or greater than the thickness of the colored coating layer 30 is contained at a desired number ratio (described later) relative to the number of all the resin particles 303 observed in the cross-sectional observation. By providing the colored coating layer 30 containing the resin particles 303 having a thickness equal to or greater than the thickness of the colored coating layer 30, the resin particles 303 protruding from the surface of the colored coating layer 30 are present. As a result, when the colored coating layer 30 comes into contact with a surface, the contact is not made by the entire colored coating layer 30, but by the resin particles 303. In other words, the contact with a surface is not by surface contact with the entire colored coating layer 30, but by point contact with the resin particles 303 protruding from the colored coating layer 30. This makes it possible to improve the scratch resistance (more specifically, resistance to surface contact scratches) of the surface-treated steel sheet 1 according to this embodiment.
[0031] The cross-section observation can be performed, for example, as follows: The surface-treated steel sheet 1 is embedded in a room-temperature drying epoxy resin in a direction perpendicular to the coating thickness direction, and the embedded surface is mechanically polished and then observed with a SEM (scanning electron microscope).
[0032] 1, the colored coating layer 30 is provided such that the thickness Tb of the second colored coating layer 30b is thinner than the thickness Ta of the first colored coating layer 30a. Specifically, the ratio Tb / Ta of the thickness Tb of the second colored coating layer 30b to the thickness Ta of the first colored coating layer 30a is 0.1 or more and 0.5 or less. By setting the ratio Tb / Ta within this range, it is possible to achieve a desired ratio in number of resin particles 303 having a thickness equal to or greater than the thickness of the colored coating layer 30 in cross-sectional observation described below.
[0033] In this embodiment, the thickness Ta of the first colored coating layer 30a is preferably 3.0 μm or more. The thickness Tb of the second colored coating layer 30b is preferably 0.3 μm or more based on the above ratio Tb / Ta. This can further improve the resistance to surface contact scratches. The thickness Ta of the first colored coating layer 30a is more preferably 4.0 μm or more. On the other hand, the thickness Ta of the first colored coating layer 30a is preferably 10.0 μm or less. By setting the thickness Ta of the first colored coating layer 30a to 10.0 μm or less, it is possible to suppress the occurrence of coating defects such as popping while suppressing costs, and to obtain a stable appearance. The thickness Ta of the first colored coating layer 30a is more preferably 8.0 μm or less. The upper limit of the thickness Tb of the second colored coating layer is determined based on the above ratio Tb / Ta from the upper limit value of the thickness Ta of the first colored coating layer 30a.
[0034] The thicknesses (Ta, Tb) of the colored coating layer 30 can be measured by observing a cross section. The thicknesses are measured at a number of arbitrary positions (e.g., 10 positions) in each of the first colored coating layer 30a and the second colored coating layer 30b, and the average value of the obtained thicknesses is taken as the thickness (Ta, Tb).
[0035] Next, the thickness of the resin particles 303 when observed in a cross section will be described with reference to Fig. 2. Fig. 2 is an explanatory diagram for describing the thickness of the resin particles 303 when the cross section of the surface-treated steel sheet 1 according to this embodiment is observed.
[0036] In FIG. 2, the thickness of the resin particles 303 refers to the length of each resin particle 303 in the thickness direction of the colored coating layer 30 (the double-ended arrows shown on the resin particles 303 in FIG. 2). More specifically, for the flat resin particles 303a that are tilted in FIG. 2, the resin particles 303a are projected in a direction perpendicular to the thickness direction (the direction of the dashed line in FIG. 2), and the length in the thickness direction in the projection is regarded as the length in the thickness direction, which is defined as the thickness of the resin particles 303a. Hereinafter, the thickness of the resin particles 303 contained in the first colored coating layer 30a is referred to as the first thickness Ga. The thickness of the resin particles 303 contained in the second colored coating layer 30b is referred to as the second thickness Gb.
[0037] In this embodiment, the ratio of the number of resin particles 303 having a first thickness Ga (Ga≧Ta) equal to or greater than the film thickness Ta of the first colored coating layer 30a to the number of all resin particles 303 within the observation field in cross-sectional observation of the first colored coating layer 30a is 1% or more and 30% or less. On the other hand, the ratio of the number of resin particles 303 having a second thickness Gb (Gb≧Tb) equal to or greater than the film thickness Tb of the second colored coating layer 30b to the number of all resin particles 303 within the observation field in cross-sectional observation of the second colored coating layer 30b is 50% or more and 100% or less. As shown in FIG. 2, the resin particles 303 having a thickness equal to or greater than the film thickness of the colored coating layer 30 protrude from the surface of the colored coating layer 30.
[0038] The proportion of resin particles 303 having a first thickness Ga that is equal to or greater than the thickness Ta of the first colored coating layer 30a (Ga≧Ta) to the number of all resin particles 303 within the observation field in cross-sectional observation of the first colored coating layer 30a, and the proportion of resin particles 303 having a second thickness Gb that is equal to or greater than the thickness Tb of the second colored coating layer 30b to the number of all resin particles 303 within the observation field in cross-sectional observation of the second colored coating layer 30b are calculated by observing a total of 500 μm or more in a direction perpendicular to the thickness direction of the colored coating layer 30a and the colored coating layer 30b, respectively.
[0039] In this embodiment, the ratio of the number of resin particles 303 having a second thickness Gb (Gb≧Tb) equal to or greater than the thickness Tb of the second colored coating layer 30b is greater than the ratio of the number of resin particles 303 having a first thickness Ga (Ga≧Ta) equal to or greater than the thickness Ta of the first colored coating layer 30a. This results in a sufficient number of resin particles 303 protruding from the second colored coating layer 30b. Therefore, even when the first colored coating layer 30a and the second colored coating layer 30b come into contact with each other, surface contact between the two coatings is significantly suppressed. As a result, scratches caused by surface contact between the two coatings, blocking during coil storage, pressure marks, and the like can be suppressed.
[0040] When the ratio of the number of resin particles 303 having a first thickness Ga (Ga≧Ta) equal to or greater than the thickness Ta of the first colored coating layer 30a is less than 1%, or when the ratio of the number of resin particles 303 having a second thickness Gb (Gb≧Tb) equal to or greater than the thickness Tb of the second colored coating layer 30b is less than 50%, the effect of suppressing surface contact between the first colored coating layer 30a and the second colored coating layer 30b is insufficient, and therefore the effect of suppressing surface contact defects is insufficient. The ratio of the number of resin particles 303 having a first thickness Ga (Ga≧Ta) equal to or greater than the thickness Ta of the first colored coating layer 30a to the number of all resin particles 303 within the observation field in cross-sectional observation of the first colored coating layer 30a is preferably 3% or more, more preferably 5% or more. Furthermore, the ratio of the number of resin particles 303 having a second thickness Gb (Gb≧Tb) equal to or greater than the film thickness Tb of the second colored coating layer 30b to the number of all resin particles 303 within the observation field in cross-sectional observation of the second colored coating layer 30b is preferably 55% or more, and more preferably 60% or more.
[0041] Furthermore, when the proportion of the number of resin particles 303 having a first thickness Ga equal to or greater than the film thickness Ta of the first colored coating layer 30a (Ga≧Ta) exceeds 30%, the processing adhesion decreases due to the excessive number of resin particles 303 protruding from the surface of the colored coating layer 30. Processing adhesion refers to the ability of a coating such as the colored coating layer 30 to remain in close contact without peeling off in the processed area.
[0042] The ratio of the number of resin particles 303 having a first thickness Ga (Ga≧Ta) equal to or greater than the thickness Ta of the first colored coating layer 30a to the number of all resin particles 303 within the observation field in cross-sectional observation of the first colored coating layer 30a is preferably 20% or less, more preferably 15% or less. The upper limit of the ratio of the number of resin particles 303 having a second thickness Gb (Gb≧Tb) equal to or greater than the thickness Tb of the second colored coating layer 30b is not particularly limited and may be 100%. The ratio of the number of resin particles 303 having a second thickness Gb (Gb≧Tb) equal to or greater than the thickness Tb of the second colored coating layer 30b to the number of all resin particles 303 within the observation field in cross-sectional observation of the second colored coating layer 30b is preferably 95% or less, more preferably 90% or less.
[0043] In the first colored film layer 30a, the content of the resin particles 303 is preferably 3% by mass or more based on the total content of the film-forming component 301 and the resin particles 303. This makes it possible to further improve the scratch resistance. The content of the resin particles 303 in the first colored film layer 30a is more preferably 5% by mass or more. On the other hand, the content of the resin particles 303 in the first colored film layer 30a is preferably 40% by mass or less based on the total content of the film-forming component 301 and the resin particles 303. This makes it possible to further improve the scratch resistance. If the content of the resin particles 303 in the first colored film layer 30a exceeds 40% by mass, the ratio of the film-forming component in the colored film is low, the barrier property of the film is reduced, and it becomes difficult to achieve the desired corrosion resistance. The content of the resin particles 303 in the first colored film layer 30a is more preferably 35% by mass or less.
[0044] In addition, the content of the resin particles 303 in the second colored film layer 30b is preferably 3% by mass or more based on the total content of the film-forming component 301 and the resin particles 303. This makes it possible to further improve the scratch resistance. The content of the resin particles 303 in the second colored film layer 30b is more preferably 5% by mass or more. On the other hand, the content of the resin particles 303 in the second colored film layer 30b is preferably 40% by mass or less based on the total content of the film-forming component 301 and the resin particles 303. This makes it possible to further improve the scratch resistance. If the content of the resin particles 303 in the second colored film layer 30b exceeds 40% by mass, the ratio of the film-forming component in the colored film is low, the barrier property of the film is reduced, and it becomes difficult to achieve the desired corrosion resistance. The content of the resin particles 303 in the second colored film layer 30b is more preferably 35% by mass or less.
[0045] Next, as a preferred configuration of the surface-treated steel sheet 1 according to this embodiment, the occupation length of the resin particles 303 will be described with reference to Fig. 3 and Fig. 4. Fig. 3 and Fig. 4 are explanatory diagrams for explaining the occupation length of the resin particles 303 when the cross section of the surface-treated steel sheet 1 according to this embodiment is observed.
[0046] In FIG. 3, when the cross section of the first colored coating layer 30a is observed, the observation range in the direction perpendicular to the film thickness direction of the first colored coating layer 30a is defined as the first observation length L1. Furthermore, within the range of the first observation length L1, the parts p1, p2, p3, p4, and p5 occupied by the resin particles 303 are projected in the film thickness direction. According to this projection, the parts p1 and p2 and the parts p4 and p5 partially overlap, and a projection P1 corresponding to the parts p1 and p2, a projection P2 corresponding to the part p3, and a projection P3 corresponding to the parts p4 and p5 are obtained. The sum P1+P2+P3 of the lengths of these projections P1, P2, and P3 is defined as the first occupation length D1. At this time, it is preferable that the ratio (D1 / L1×100) of the first occupation length D1 to the first observation length L1 is 15% or more and 40% or less.
[0047] Similarly, in FIG. 4, when the cross section of the second colored coating layer 30b is observed, the observation range in the direction perpendicular to the film thickness direction of the second colored coating layer 30b is defined as the second observation length L2. Furthermore, within the range of the second observation length L2, the portions p6, p7, p8, p9, and p10 occupied by the resin particles 303 are projected in the film thickness direction. According to this projection, the portions p6 and p7 and the portions p9 and p10 partially overlap, and a projection P4 corresponding to the portions p6 and p7, a projection P5 corresponding to the portion p8, and a projection P6 corresponding to the portions p9 and p10 are obtained. The sum P4+P5+P6 of the lengths of these projections P4, P5, and P6 is defined as the second occupation length D2. At this time, it is preferable that the ratio (D2 / L2×100) of the second occupation length D2 to the second observation length L2 is 5% or more and 15% or less. The first observation length L1 and the second observation length L2 are each 1000 μm.
[0048] By setting the ratio of the first occupation length D1 to the first observation length L1 to 15% or more, it is possible to further improve the scratch resistance. The ratio of the first occupation length D1 to the first observation length L1 is more preferably 20% or more. On the other hand, by setting the ratio of the first occupation length D1 to the first observation length L1 to 40% or less, it is possible to further improve the corrosion resistance. If the ratio of the first occupation length D1 to the first observation length L1 exceeds 40%, the ratio of the film-forming component 301 in the first colored film layer 30a decreases, the barrier properties of the film decrease, and it may be difficult to achieve the desired corrosion resistance. The ratio of the first occupation length D1 to the first observation length L1 is more preferably 35% or less.
[0049] By setting the ratio of the second occupation length D2 to the second observation length L2 to 5% or more, it is possible to further improve the scratch resistance. The ratio of the second occupation length D2 to the second observation length L2 is more preferably 7% or more. On the other hand, it is preferable to set the ratio of the second occupation length D2 to the second observation length L2 to 15% or less. This makes it possible to further improve the scratch resistance. The reason is that, from a certain point of view, the second surface 10b of the steel sheet 10 is thinner than the first surface 10a, so when the ratio of the second occupation length D2 to the second observation length L2 exceeds 15%, the ratio of resin particles with a particle diameter equal to or greater than the film thickness on the second surface 10b is large. When the ratio of resin particles with a particle diameter equal to or greater than the film thickness is large, it is difficult to hold the resin particles in the film, and the resin particles 303 are easily detached from the second surface 10b during surface contact, which may become the starting point of scratches. From another perspective, when the ratio of the second occupation length D2 to the second observation length L2 exceeds 15%, the effect of improving scratch resistance becomes saturated, while the ratio of the film-forming component 301 in the second colored coating layer 30b decreases, reducing the barrier properties of the coating, which may make it difficult to achieve the desired corrosion resistance on the second side 10b of the steel sheet 10. From the viewpoint of further improving the scratch resistance or further improving the corrosion resistance on the second side 10b of the steel sheet 10, the ratio of the second occupation length D2 to the second observation length L2 is more preferably 13% or less.
[0050] The film-forming component 301 of the colored film layer 30 according to this embodiment can be any material that functions as a binder for the resin particles 303. However, from the viewpoint of ease of production and cost, it is preferable to use various organic resins. Examples of such film-forming components 301 include acrylic resins, polyester resins, urethane resins, and fluorine resins. In addition, when resin particles made of organic resins are used as the resin particles 303, it is preferable to select the same type of resin as the resin particles as the film-forming component 301. This improves the affinity between the film-forming component 301 and the resin particles 303, and it is possible to further improve the scratch resistance and adhesion of the colored film layer 30.
[0051] Moreover, the film-forming component 301 according to this embodiment is preferably an organic resin having a glass transition temperature Tg of 30° C. or higher. By using a resin having a glass transition temperature Tg as described above as the film-forming component 301, the colored coating layer 30 has a more appropriate hardness, and the scratch resistance (particularly, scratch resistance) of the surface-treated steel sheet 1 can be further improved.
[0052] The glass transition temperature Tg of the film-forming component 301 is preferably 35° C. or higher, and more preferably 40° C. or higher. On the other hand, the upper limit of the glass transition temperature Tg is not particularly specified, but if it exceeds 70° C., the processability may decrease. Therefore, the glass transition temperature Tg of the film-forming component 301 is preferably 70° C. or lower.
[0053] The glass transition temperature Tg can be determined, for example, by a method of TMA (thermomechanical analysis) in which a needle is inserted into the surface of a coating to be measured in the direction of the coating thickness and a constant temperature change is applied to measure the change in thermal expansion of the coating to be measured, or by a method of DMA (dynamic viscoelastic analysis) in which a coating to be measured that has been peeled off from a substrate is subjected to a constant temperature change while being subjected to periodic deformation to analyze the viscoelasticity.
[0054] The resin particles 303 of the colored coating layer 30 according to this embodiment are preferably resin particles made of organic resin. By using such resin particles, the toughness and ductility of the resin particles can mitigate the impact applied to the colored coating layer 30, and the scratch resistance can be further improved. Examples of such resin particles include acrylic resin particles, polyester resin particles, urethane resin particles, fluorine resin particles, silicone resin particles, and polyolefin resin particles, but it is more preferable to use acrylic resin particles. In addition, the color pigment contained in the colored coating layer 30 itself may function as the above-mentioned resin particles 303.
[0055] In this embodiment, the resin particles 303 may have a thickness equal to or greater than the thickness of the colored coating layer 30, or may not. Therefore, the resin particles 303 used have a particle diameter that varies. The average particle diameter is preferably 3 to 15 μm. The resin particles 303 having the above-mentioned average particle diameter can further improve the scratch resistance of the surface-treated steel sheet 1. Here, the average particle diameter of the resin particles 303 means an average value calculated from the circle-equivalent diameter of each resin particle observed by cross-sectional observation, unlike the thickness of the resin particles 303 defined above. Specifically, the average particle diameter of the resin particles 303 may be determined by measuring the particle diameters of the resin particles 303 observed at any multiple positions (for example, 10 positions) in cross-sectional observation, and the average value of the obtained multiple particle diameters may be used as the average particle diameter of the resin particles 303. The resin particles 303 having a particle diameter that varies includes a case where multiple resin particles 303 with no particle diameter variation are mixed and used.
[0056] In addition, the thickness Ga of the resin particles 303 contained in the first colored coating layer 30a is less than 2.0 times the thickness Ta of the first colored coating layer, and the thickness of the resin particles 303 contained in the second colored coating layer 30b is less than 2.0 times the thickness Ta of the first colored coating layer. It is preferable that the thickness Gb of the resin 3 is less than 3.0 times the thickness Tb of the second colored coating layer. The above-mentioned relationship between the thickness of the resin particles 303 and the film thickness of the colored coating layer 30 makes it possible to further improve the scratch resistance of the surface-treated steel sheet 1. The thickness Ga of the resin particles 303 contained in the first colored coating layer 30a is preferably less than 1.5 times the film thickness Ta of the first colored coating layer. Moreover, the thickness Gb of the resin particles 303 contained in the second colored coating layer 30b is preferably less than 2.5 times the film thickness Tb of the second colored coating layer.
[0057] ◇Other components in the colored coating layer 30 The colored coating layer 30 according to this embodiment may further contain a crosslinking agent in addition to the components described above.
[0058] By further containing a crosslinking agent in the colored coating layer 30 according to this embodiment, it is possible to further improve the barrier properties of the colored coating layer 30 itself, and to further improve the scratch resistance and corrosion resistance of the surface-treated steel sheet 1. In particular, by containing at least one of a melamine resin and an isocyanate resin as a crosslinking agent in the colored coating layer 30, it is possible to further improve the scratch resistance and corrosion resistance of the surface-treated steel sheet 1. The content of such a crosslinking agent is preferably about 10 to 40 mass % in the film-forming component 301, for example.
[0059] The color pigment contained in the color coating layer 30 is not particularly limited, and various known pigments can be used appropriately depending on the color tone desired for the color coating layer 30. Examples of such color pigments include aluminum pigments, carbon black, TiO2, etc. The content of the pigment may be appropriately set, for example, about 3 to 60 mass%.
[0060] The colored coating layer 30 can be formed by applying a paint composition containing the components constituting the colored coating layer 30 as described above onto the surface of the steel sheet 10, onto the plated surface, onto the surface of the steel sheet 10 having the chemical conversion coating 40, or onto the plated surface having the chemical conversion coating 40, and then baking and curing at a temperature of 150° C. or higher and lower than 300° C. If the baking temperature is lower than 150° C., the bake hardening may be insufficient, and the corrosion resistance and scratch resistance of the coating may decrease, whereas if the baking temperature is 300° C. or higher, thermal degradation of the resin components may occur, and processability may decrease.
[0061] The coating composition as described above can be applied by a generally known coating method, such as roll coating, curtain flow coating, air spray, airless spray, immersion, bar coating, brush coating, etc. Among such coating methods, roll coating is particularly preferred.
[0062] Furthermore, the colored coating layer 30 may further contain additives such as anti-rust pigments, surface-modified metal powders or glass powders, dispersants, leveling agents, waxes, aggregates, and dilution solvents, as necessary, within the scope that does not impair the above-mentioned effects.
[0063] When an anti-rust pigment is contained, the content is preferably, for example, 1 to 15 mass %. In addition, the anti-rust pigment used may be any of various known anti-rust pigments.
[0064] ◇Hardness of colored film layer 30 The colored coating layer 30 preferably has a Vickers hardness of 10 to 70 Hv measured at a depth of 3 / 4 of the coating thickness from the surface (the test load is set according to the hardness of the colored coating layer 30 so as to achieve a desired depth of penetration). The Vickers hardness is measured using a Universal Hardness Tester (manufactured by Fisher Instruments). The hardness is measured from the coating surface at any 10 points under the above-mentioned depth of penetration, regardless of whether the resin particles 303 are present or not, and the average of the 10 measured values is calculated. The colored coating layer 30 has the above-mentioned Vickers hardness, which makes it possible to further improve the scratch resistance. The Vickers hardness of the colored coating layer 30 is more preferably 15 to 65 Hv.
[0065] <About the chemical conversion coating layer 40> The chemical conversion coating layer 40 according to this embodiment is a coating layer that can be located between the steel sheet 10 and the colored coating layer 30, and is a layer formed by so-called chemical conversion treatment.
[0066] A detailed configuration of the chemical conversion coating layer 40 according to this embodiment may include, for example, a configuration containing one or more selected from the group consisting of resin, silane coupling agent, zirconium compound, silica, phosphoric acid and its salt, fluoride, vanadium compound, and tannin or tannic acid. The inclusion of these substances further improves the film-forming properties after application of the chemical conversion coating solution, the barrier properties (density) of the coating against corrosive factors such as moisture and corrosive ions, and the coating adhesion to the plating surface, thereby contributing to raising the corrosion resistance of the coating.
[0067] In particular, when the chemical conversion coating layer 40 contains one or more of a silane coupling agent or a zirconium compound, a cross-linked structure is formed within the chemical conversion coating layer 40, and the bond with the plating surface is also strengthened, making it possible to further improve the adhesion and barrier properties of the coating.
[0068] Furthermore, when the chemical conversion coating layer 40 contains one or more of silica, phosphoric acid and its salts, fluorides, and vanadium compounds, these function as inhibitors and form a precipitate film or a passivation film on the plating or steel surface, thereby making it possible to further improve corrosion resistance.
[0069] In the following, the components that may be contained in the chemical conversion coating layer 40 as described above will be described in detail with reference to examples.
[0070] [resin] The resin is not particularly limited, and known organic resins such as polyester resin, polyurethane resin, epoxy resin, phenol resin, acrylic resin, polyolefin resin, etc. can be used. In order to further improve adhesion to the plated steel sheet for precoated steel sheet, it is preferable to use at least one resin having a forced site or a polar functional group in the molecular chain (polyester resin, urethane resin, epoxy resin, acrylic resin, etc.). The resin may be used alone or in combination of two or more kinds.
[0071] The resin content in the chemical conversion coating layer 40 is, for example, preferably 0 mass% or more, and more preferably 1 mass% or more, relative to the coating solid content. The resin content in the chemical conversion coating layer 40 is, for example, preferably 85 mass% or less, more preferably 60 mass% or less, and even more preferably 40 mass% or less, relative to the coating solid content. If the resin content exceeds 85 mass%, the proportion of other coating constituent components decreases, and performance required of the coating other than corrosion resistance may decrease.
[0072] [Silane coupling agents] Examples of the silane coupling agent include γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropylmethyldiethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropyltriethoxy ...triethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltriethoxysil Dipropylmethyldiethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltriethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropylmethyldiethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-glycidoxypropyltriethoxy Silane, gamma-glycidoxypropylmethyldiethoxysilane, gamma-mercaptopropyltrimethoxysilane, gamma-mercaptopropylmethyldimethoxysilane, gamma-mercaptopropyltriethoxysilane, gamma-mercaptopropylmethyldiethoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, vinyltriacetoxysilane, gamma-chloropropyltrimethoxysilane, gamma-chloropropylmethyldimethoxysilane, gamma-chloropropyltriethoxysilane, gamma-chloropropyl dimethyldiethoxysilane, hexamethyldisilazane, γ-anilinopropyltrimethoxysilane, γ-anilinopropylmethyldimethoxysilane, γ-anilinopropyltriethoxysilane, γ-anilinopropylmethyldiethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, vinyltriethoxysilane, vinylmethyldiethoxysilane, octadecyldimethyl[3-(trimethoxysilyl)propyl]ammonium chloride, octadecyldimethyl[3-(methyldimethoxysilyl)propyl]ammonium chloride,Examples of suitable silane coupling agents include octadecyldimethyl[3-(triethoxysilyl)propyl]ammonium chloride, octadecyldimethyl[3-(methyldiethoxysilyl)propyl]ammonium chloride, γ-chloropropylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, methyltrichlorosilane, dimethyldichlorosilane, and trimethylchlorosilane. The amount of silane coupling agent added to the chemical conversion coating layer 40 can be, for example, 2 to 80 g / L. If the amount of silane coupling agent added is less than 2 g / L, the adhesion to the plating surface may be insufficient, and the processing adhesion of the coating film may decrease. If the amount of silane coupling agent added is more than 80 g / L, the cohesive force of the chemical conversion coating layer may be insufficient, and the processing adhesion of the coating film layer may decrease. The silane coupling agents exemplified above may be used alone or in combination of two or more.
[0073] [Zirconium compounds] Examples of the zirconium compound include zirconium normal propylate, zirconium normal butylate, zirconium tetraacetylacetonate, zirconium monoacetylacetonate, zirconium bisacetylacetonate, zirconium monoethylacetoacetate, zirconium acetylacetonate bisethylacetoacetate, zirconium acetate, zirconium monostearate, zirconium carbonate, zirconium ammonium carbonate, zirconium potassium carbonate, and zirconium sodium carbonate. The amount of the zirconium compound added to the chemical conversion coating layer 40 can be, for example, 2 to 80 g / L. If the amount of the zirconium compound added is less than 2 g / L, the adhesion to the plating surface may be insufficient, and the processing adhesion of the coating layer may be reduced. If the amount of the zirconium compound added is more than 80 g / L, the cohesive force of the chemical conversion coating layer 40 may be insufficient, and the processing adhesion of the coating layer may be reduced. Such zirconium compounds may be used alone or in combination of two or more kinds.
[0074] [silica] As the silica, for example, commercially available silica gel such as "Snowtex N", "Snowtex C", "Snowtex UP", and "Snowtex PS" manufactured by Nissan Chemical Industries, Ltd., "Adelite AT-20Q" manufactured by ADEKA Corporation, powdered silica such as Aerosil #300 manufactured by Nippon Aerosil Co., Ltd., or equivalent to these commercially available silicas can be used. The silica can be appropriately selected according to the required performance of the precoated plated steel sheet. The amount of silica added in the chemical conversion treatment agent for forming the chemical conversion treatment film layer 40 is preferably, for example, 1 to 40 g / L. If the amount of silica added is less than 1 g / L, the processing adhesion of the film layer may decrease, and if the amount of silica added is more than 40 g / L, the effects of processing adhesion and corrosion resistance are likely to be saturated, which is uneconomical.
[0075] [Phosphoric acid and its salts] Examples of phosphoric acid and its salts include phosphoric acids such as orthophosphoric acid, metaphosphoric acid, pyrophosphoric acid, triphosphoric acid, and tetraphosphoric acid, and their salts, ammonium salts such as triammonium phosphate and diammonium hydrogen phosphate, phosphonic acids such as aminotri(methylenephosphonic acid), 1-hydroxyethylidene-1,1-diphosphonic acid, ethylenediaminetetra(methylenephosphonic acid), and diethylenetriaminepenta(methylenephosphonic acid), and their salts, and organic phosphoric acids such as phytic acid and their salts. Examples of phosphoric acid salts other than ammonium salts include metal salts with Na, Mg, Al, K, Ca, Mn, Ni, Zn, Fe, and the like. Phosphoric acid and its salts may be used alone or in combination of two or more.
[0076] The content of phosphoric acid and its salts is, for example, preferably 0% by mass or more, and more preferably 1% by mass or more, based on the solid content of the coating. The content of phosphoric acid and its salts is, for example, preferably 20% by mass or less, and more preferably 10% by mass or less, based on the solid content of the coating. If the content of phosphoric acid and its salts exceeds 20% by mass, the coating becomes brittle, and the processing followability of the coating when the surface-treated steel sheet 1 is formed may decrease.
[0077] [Fluoride] Examples of the fluoride include ammonium zirconate fluoride, ammonium silicofluoride, ammonium titanium fluoride, sodium fluoride, potassium fluoride, calcium fluoride, lithium fluoride, titanium hydrofluoric acid, zirconate hydrofluoric acid, etc. Such fluorides may be used alone or in combination of two or more.
[0078] The fluoride content is, for example, preferably 0% by mass or more, and more preferably 1% by mass or more, based on the solid content of the coating. The fluoride content is, for example, preferably 20% by mass or less, and more preferably 10% by mass or less, based on the solid content of the coating. If the fluoride content exceeds 20% by mass, the coating becomes brittle, and the processing followability of the coating when the surface-treated steel sheet 1 is formed may decrease.
[0079] [Vanadium compounds] Examples of vanadium compounds include vanadium compounds obtained by reducing pentavalent vanadium compounds such as vanadium pentoxide, metavanadic acid, ammonium metavanadate, sodium metavanadate, and vanadium oxytrichloride to divalent to tetravalent vanadium compounds with a reducing agent, vanadium trioxide, vanadium dioxide, vanadium oxysulfate, vanadium oxyoxalate, vanadium oxyacetylacetonate, vanadium acetylacetonate, vanadium trichloride, phosphovanadomolybdic acid, vanadium sulfate, vanadium dichloride, and vanadium oxide, and other vanadium compounds having an oxidation number of 4 to 2. Such vanadium compounds may be used alone or in combination of two or more.
[0080] The content of the vanadium compound is, for example, preferably 0% by mass or more, more preferably 1% by mass or more, based on the solid content of the coating. The content of the vanadium compound is, for example, preferably 20% by mass or less, more preferably 10% by mass or less, based on the solid content of the coating. If the content of the vanadium compound exceeds 20% by mass, the coating becomes brittle, and the processing followability of the coating when the surface-treated steel sheet 1 is formed may decrease.
[0081] [Tannin or tannic acid] Tannin or tannic acid may be either hydrolyzable tannin or condensed tannin. Examples of tannin and tannic acid include hammeta tannin, Chinese gall tannin, gall tannin, myrobalan tannin, dividivi tannin, algarovila tannin, valonia tannin, and catechin. The amount of tannin or tannic acid added to the chemical conversion coating 40 may be 2 to 80 g / L. If the amount of tannin or tannic acid added is less than 2 g / L, the adhesion to the plating surface may be insufficient, and the processing adhesion of the coating may be reduced. If the amount of tannin or tannic acid added is more than 80 g / L, the cohesive force of the chemical conversion coating may be insufficient, and the processing adhesion of the coating may be reduced.
[0082] Furthermore, an acid, an alkali, or the like may be added to the chemical conversion treatment agent used to form the chemical conversion coating layer 40 in order to adjust the pH, within a range that does not impair performance.
[0083] The chemical conversion treatment agent containing the above-mentioned various components is applied to one or both sides of the steel sheet 10 and then dried to form the chemical conversion coating layer 40. In the surface-treated steel sheet 1 according to this embodiment, the chemical conversion treatment agent is applied to one or both sides at a concentration of 10 mg / m 2 It is preferable to form the above chemical conversion coating layer 40 on the plating layer 20. The coating weight of the chemical conversion coating layer 40 is more preferably 20 mg / m 2 More preferably, it is 50 mg / m 2 The above is true for the surface-treated steel sheet 1 according to this embodiment. 2 It is preferable to form the following chemical conversion coating layer 40 on the plating layer 20. The coating weight of the chemical conversion coating layer 40 is more preferably 800 mg / m 2 More preferably, it is 600 mg / m or less. 2 The thickness of the chemical conversion coating layer 40 corresponding to this amount of adhesion will vary depending on the components contained in the chemical conversion treatment agent, but will generally be about 0.01 to 1 μm. The thickness of the chemical conversion coating layer 40 can be measured by cross-sectional observation, similar to the thickness of the colored coating layer 30. EXAMPLES
[0084] The surface-treated steel sheet 1 according to the present invention will be specifically described below with reference to examples and comparative examples. Note that the examples shown below are merely examples of the surface-treated steel sheet 1 according to the present invention, and the surface-treated steel sheet 1 according to the present invention is not limited to the following examples.
[0085] (1) Galvanized steel sheet Five types of metal sheets, A1 to A5, shown in Table 1 below, were prepared. Steel sheets with a thickness of 0.7 mm were used as the substrates for the plated metal sheets. Furthermore, chromate-free conversion coating (CT-E300 / Nihon Parkerizing Co., Ltd.) was applied to these metal sheets at a concentration of 60 mg / m 2The plating steel sheets were also prepared. The treatment solution used for the chemical conversion treatment contained a silane coupling agent as a component, and the coating layer formed by the chemical conversion treatment functions as a chemical conversion coating layer. The presence or absence of chemical conversion treatment is shown in Tables 6 and 7 below.
[0086] (2) Preparation of colored paint A colored coating material used for forming a colored coating layer was prepared. As a binder resin functioning as a film-forming component, a resin equivalent to the resin shown in Table 2 below was prepared. For each resin solution, a melamine-based curing agent (equivalent to Cymel 303 / manufactured by Allnex) was prepared as a curing agent at a solid content ratio of 30 mass%. Furthermore, as resin particles, particles equivalent to those shown in Table 3 below were prepared. Furthermore, as color pigments, aluminum pigments, titanium oxide, and carbon black (CB) equivalent to those shown in Table 4 below were prepared. Furthermore, as rust-preventive pigments, compounds shown in Table 5 below were prepared. These coating compositions were mixed in the predetermined particle sizes and amounts shown in Tables 6 and 7 below to prepare colored coating materials.
[0087] (3) Sample preparation The colored coating material prepared as described above was applied to both sides of a plated steel sheet using a roll coater, and the sheet was heated to a maximum reached temperature (PMT) of 200°C to form a colored coating layer. The thickness of the colored coating layer thus produced was measured by cross-sectional observation in accordance with the method previously described, and the results are shown in Tables 6 and 7. In Tables 6 and 7, the "proportion (%) of the thickness or more" refers to the proportion (%) of the number of resin particles 303 in the colored coating layer 30a that have a thickness Ga (Ga≧Ta) equal to or greater than the thickness Ta of the colored coating layer 30a, and refers to the proportion (%) of the number of resin particles 303 in the colored coating layer 30b that have a thickness Gb (Gb≧Tb) equal to or greater than the thickness Tb of the colored coating layer 30b.
[0088] (4) Evaluation of samples The performance of each sample prepared by the above method was evaluated based on the following criteria. The evaluation results are shown in Table 8 below.
[0089] <Surface contact scratch resistance> The surface contact scratch resistance was evaluated by the following method. The prepared sample was cut into two pieces of 50 mm square, and one piece was fixed with the colored coating layer 30a facing up. The other piece was placed on top of the first piece with the colored coating layer 30b facing down, and the sample was subjected to a pressure of 8.5 kgf / cm 2 After rotating the specimen by 90 degrees while being pressurized under the condition of 1 kgf (1 kgf is approximately 9.8 N), the condition of the colored coating layer 30a was evaluated according to the following criteria, with a score of 2 or higher being considered a pass.
[0090] Evaluation criteria for surface contact scratch resistance 5: Almost no peeling of the coating is observed, and some or almost no change in gloss due to pressure is observed. 4: Very slight peeling of the coating is observed, and some gloss change due to pressure is observed. 3: Slight peeling of the coating is observed, and some gloss changes due to pressure are observed. 2: Slight peeling of the coating is observed, and gloss change due to pressure is observed. 1: Paint peeling is observed, and significant gloss change due to pressure is observed.
[0091] <Corrosion resistance> The corrosion resistance was evaluated based on the following criteria: After the end faces of the test plates were sealed with tape, a salt spray test (SST) in accordance with JIS Z 2371 was carried out for 72 hours, and the occurrence of rust was observed and evaluated based on the following criteria, with a score of 2 or higher being considered a pass.
[0092] Corrosion resistance evaluation criteria 5: White rust occurs on less than 1% of the surface area and red rust does not occur. 4: White rust occurs on an area of 1% or more but less than 3%. Red rust does not occur. 3: The area of white rust is between 3% and 4% and no red rust occurs. 2: The area of white rust is between 4% and 5% and no red rust occurs. 1: White rust has appeared on 5% or more of the surface area, or red rust has appeared.
[0093] <Scratch resistance> As a reference performance, scratch resistance was evaluated by the following coin scratch test. A coin was inclined at an angle of 45 degrees and contacted with the colored film layer 30a of the prepared sample, and scratched with a load of 500 g. The scratches made with each load were evaluated according to the following criteria, and a score of 2 or more was considered to be a pass.
[0094] Evaluation criteria for scratch resistance 5: No peeling of the coating or change in gloss was observed. 4: No peeling of the coating is observed, but slight changes in gloss are observed. 3: Slight peeling of the coating film and change in gloss are observed. 2: Partial peeling of the coating is observed, and changes in gloss are observed. 1: The coating has completely peeled off.
[0095] <Pressure mark resistance> As a reference performance, the pressure mark resistance was evaluated based on the following criteria. The prepared samples were cut into one each of 70 mm square and 50 mm square. The 70 mm square sample was fixed with the colored coating layer 30a facing up, and the 50 mm square sample was placed on top of it with the colored coating layer 30b facing down, and pressure was applied at 50°C and 10 MPa for 5 minutes. After the two samples were separated, the condition of the colored coating layer 30a of the 70 mm square sample was evaluated based on the following criteria, and a score of 2 or more was considered to be acceptable.
[0096] Evaluation criteria for pressure mark resistance 4: Completely invisible when observed from the front or at an angle. 3: It is not visible when observed from the front, but a slight change in gloss of the pressured area is visible when observed from an oblique position. 2: It is not visible when observed from the front, but the change in gloss of the pressed area can be seen when observed from an oblique position. 1: The change in gloss of the entire pressured area is visible when observed from the front or from an oblique position.
[0097] <Processing adhesion> As a reference performance, the processing adhesion was evaluated based on the following criteria. The prepared samples were bent 90 degrees with an inner radius of 1 mm in a 20°C atmosphere, and then a tape peeling test was carried out on the outside of the bent part. The appearance of the tape peeled part was evaluated based on the following criteria, and a score of 2 or more was considered to be a pass.
[0098] Evaluation criteria for adhesion of processed parts 4: Almost no peeling of the coating is observed. 3: Slight peeling of the coating is observed. 2: Partial peeling of the coating is observed. 1: Paint peeling is observed overall.
[0099] [Table 1]
[0100] [Table 2]
[0101] [Table 3]
[0102] [Table 4]
[0103] [Table 5]
[0104] [Table 6]
[0105] [Table 7]
[0106] [Table 8]
[0107] As is clear from Table 8 above, the samples corresponding to the examples of the present invention exhibited excellent resistance to surface contact scratches and also exhibited excellent corrosion resistance, while the samples corresponding to the comparative examples of the present invention were inferior in the evaluation of either resistance to surface contact scratches or corrosion resistance, and did not achieve both resistance to surface contact scratches and corrosion resistance.
[0108] Although the preferred embodiment of the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention.
[0109] The embodiments disclosed herein are illustrative and not restrictive in all respects. The above embodiments may be omitted, substituted, or modified in various forms without departing from the scope of the appended claims, the technical scope of the present invention as described below, and the spirit thereof. For example, the components of the above embodiments can be arbitrarily combined within a range that does not impair the effects of the components. Furthermore, the arbitrary combination naturally provides the actions and effects of each of the components in the combination, and also provides other actions and effects that are obvious to a person skilled in the art from the description of this specification.
[0110] In addition, the effects described in this specification are merely explanatory or exemplary, and are not limiting. In other words, the technology according to the present invention may achieve other effects that are apparent to a person skilled in the art from the description of this specification, in addition to or in place of the above effects.
[0111] The following configurations also fall within the technical scope of the present invention. (1) a zinc-containing coating layer located on both surfaces of a steel sheet; a first colored coating layer located on the plating layer on one surface of the steel sheet; a second colored coating layer located on the plating layer on the other surface of the steel sheet; Equipped with a ratio of a thickness of the second colored coating layer to a thickness of the first colored coating layer is 0.1 or more and 0.5 or less; the first colored coating layer and the second colored coating layer contain resin particles, When observing a cross section of the first colored coating layer cut in the thickness direction, When the length of the observed resin particle in the thickness direction of the first colored coating layer is defined as the thickness of the resin particle, the ratio of the number of the resin particles having a thickness equal to or greater than the film thickness of the first color coating layer to the number of all the resin particles observed is 1% or more and 30% or less, When observing a cross section of the second colored coating layer cut in the thickness direction, When the length of the observed resin particle in the thickness direction of the second colored coating layer is defined as the thickness of the resin particle, the ratio of the number of the resin particles having a thickness equal to or greater than the film thickness of the second colored coating layer to the number of all the observed resin particles is 50% or more and 100% or less; Surface treated steel sheet. (2) when a cross section of the first colored coating layer is observed, a length of 1000 μm in a direction perpendicular to the film thickness direction of the first colored coating layer is defined as a first observation length, and a portion occupied by the resin particles within the first observation length is projected in the film thickness direction, and the sum of lengths of the portions corresponding to the resin particles in the direction perpendicular to the film thickness direction is defined as a first occupation length, the ratio of the first occupation length to the first observation length being 15% or more and 40% or less, The surface-treated steel sheet according to (1) above, wherein a second observation length is a length of 1000 μm in a direction perpendicular to the film thickness direction of the second colored coating layer, and a second occupation length is the sum of the lengths in a direction perpendicular to the film thickness direction of the portions corresponding to the resin particles when the portions occupied by the resin particles within the second observation length are projected in the film thickness direction, and the ratio of the second occupation length to the second observation length is 5% or more and 15% or less. (3) The surface-treated steel sheet according to (1) or (2) above, wherein the first colored coating layer has a thickness of 3 μm or more and 10 μm or less. (4) the thickness of the resin particles contained in the first colored coating layer is less than twice the thickness of the first colored coating layer; The surface-treated steel sheet according to any one of the above (1) to (3), wherein the thickness of the resin particles contained in the second colored coating layer is less than three times the thickness of the second colored coating layer. (5) The surface-treated steel sheet according to any one of the above (1) to (4), wherein the resin particles are acrylic resin particles. (6) The surface-treated steel sheet according to any one of (1) to (5) above, wherein the film-forming components of the first colored film layer and the second colored film layer have a glass transition temperature Tg of 30°C or higher and 70°C or lower. (7) The surface-treated steel sheet according to any one of (1) to (6) above, further comprising a chemical conversion coating layer between the plating layer and the first colored coating layer on one side of the steel sheet, and between the plating layer and the second colored coating layer on the other side of the steel sheet. (8) The surface-treated steel sheet according to any one of the above (1) to (7), wherein the resin particles have an average particle size of 3 μm or more and 15 μm or less. [Explanation of symbols]
[0112] 1. Surface-treated steel sheets 10 steel plate 20 Plating layer 30 Colored film layer 40 Chemical conversion coating layer 301 Film-forming components 303 Resin particles
Claims
1. a zinc-containing coating layer located on both surfaces of the steel sheet; a first colored coating layer located on the plating layer on one surface of the steel sheet; a second colored coating layer located on the plating layer on the other surface of the steel sheet; Equipped with a ratio of a thickness of the second colored coating layer to a thickness of the first colored coating layer is 0.1 or more and 0.5 or less; the first colored film layer and the second colored film layer contain resin particles, When observing a cross section of the first colored coating layer cut in the thickness direction, When the length of the observed resin particle in the thickness direction of the first colored coating layer is defined as the thickness of the resin particle, the ratio of the number of the resin particles having a thickness equal to or greater than the film thickness of the first colored coating layer to the number of all the resin particles observed is 1% or more and 30% or less, When a cross section of the second colored coating layer cut in the thickness direction is observed, When the length of the observed resin particle in the thickness direction of the second colored coating layer is defined as the thickness of the resin particle, the ratio of the number of the resin particles having a thickness equal to or greater than the film thickness of the second colored coating layer to the number of all the observed resin particles is 50% or more and 100% or less; Surface treated steel sheet.
2. when a cross section of the first colored coating layer is observed, a length of 1000 μm in a direction perpendicular to a thickness direction of the first colored coating layer is defined as a first observation length, and a portion occupied by the resin particles within the first observation length is projected in the thickness direction, the total length of the portion corresponding to the resin particles in a direction perpendicular to the thickness direction is defined as a first occupation length, and a ratio of the first occupation length to the first observation length is 15% or more and 40% or less, 2. The surface-treated steel sheet according to claim 1, wherein a second observation length is a length of 1000 μm in a direction perpendicular to the film thickness direction of the second colored coating layer, and a second occupation length is a sum of lengths in a direction perpendicular to the film thickness direction of a portion corresponding to the resin particle when a portion occupied by the resin particle within the second observation length is projected in the film thickness direction, and the ratio of the second occupation length to the second observation length is 5% or more and 15% or less.
3. The surface-treated steel sheet according to claim 1 or 2, wherein the first colored coating layer has a thickness of 3 μm or more and 10 μm or less.
4. the thickness of the resin particles contained in the first colored coating layer is less than twice the thickness of the first colored coating layer; 3. The surface-treated steel sheet according to claim 1, wherein the thickness of the resin particles contained in the second colored coating layer is less than three times the thickness of the second colored coating layer.
5. The surface-treated steel sheet according to claim 1 or 2, wherein the resin particles are acrylic resin particles.
6. 3. The surface-treated steel sheet according to claim 1, wherein the film-forming components of the first colored film layer and the second colored film layer have a glass transition temperature Tg of 30°C or higher and 70°C or lower.
7. 3. The surface-treated steel sheet according to claim 1, further comprising a chemical conversion coating layer between the plating layer and the first colored coating layer on one surface of the steel sheet, and between the plating layer and the second colored coating layer on the other surface of the steel sheet.
8. The surface-treated steel sheet according to claim 1 or 2, wherein the resin particles have an average particle size of 3 μm or more and 15 μm or less.
Citation Information
Patent Citations
Heating odorless lubricating steel panel
JP1996156178A
Galvanized steel sheet with organic coating, excellent in lubricity
JP1996174758A
Lubricity resin coating metal plate with excellent processability and coating film adhesive properties
JP1997187881A
Precoated metallic plate for electronic / electrical equipment
JP2010005545A
Organic resin coating plated steel plate
JP2017061750A