Glass for atomic cells, atomic cells, and method for manufacturing atomic cells
A glass composition with controlled molar volume and specific oxide ratios addresses helium penetration issues in atomic cells, ensuring stable oscillation frequency by enhancing He gas shielding and anodic bonding.
Patent Information
- Application Number
- JP2020097771
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-04
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-06-04
AI Technical Summary
Existing atomic cells using general glass are susceptible to helium gas penetration, leading to potential cell leakage and frequency fluctuations in atomic oscillators over time.
A glass composition with a molar volume of 26.0 cm³/mol or less, containing specific ratios of SiO₂, Al₂O₃, MgO, CaO, SrO, BaO, and minimal Li₂O, Na₂O, B₂O₃, and P₂O₅, which enhances He gas shielding and facilitates anodic bonding.
The proposed glass composition effectively prevents helium gas penetration, maintaining stable oscillation frequency in atomic oscillators by reducing cell leakage and ensuring airtightness.
Smart Images

Figure 0007583352000002 
Figure 0007583352000003 
Figure 0007583352000001
Abstract
Description
[Technical field]
[0001] The present invention relates to glass for an atomic cell used in an atomic oscillator or the like, an atomic cell, and a method for manufacturing an atomic cell. [Background technology]
[0002] Atomic clocks are equipped with atomic oscillators that oscillate based on the energy transition of alkali metal atoms such as cesium (Cs) and rubidium (Rb), and these atomic oscillators are known to have long-term, highly accurate oscillation characteristics. The operating principles of atomic oscillators are classified into several types, but atomic oscillators that utilize the quantum interference effect (CPT: Coherent Population Trapping) are known to have frequency stability that is about three orders of magnitude higher than that of quartz oscillators.
[0003] In such an atomic oscillator, an alkali metal vapor is sealed in the atomic cell, and in order to ensure the performance required for an atomic oscillator, a buffer gas such as neon (Ne) or argon (Ar) is further sealed in the atomic cell.
[0004] Patent Document 1 discloses an atomic cell sealed with glass by anodic bonding, and discloses that aluminosilicate glass, borosilicate glass, or quartz glass is used as the glass. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-87865 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the atomic cell using general glass disclosed in Patent Document 1 has a problem that helium (He) in the atmosphere penetrates from the outer surface of the glass to the inside and enters the atomic cell, that is, there is a problem in the shielding property of He gas, or the buffer gas present inside leaks to the outside of the cell, that is, there is a problem in that the frequency tends to fluctuate over time.
[0007] Therefore, an object of the present invention is to provide a glass for an atomic cell that is less susceptible to the change over time in the oscillation frequency of an atomic oscillator caused by the permeation of He gas. [Means for solving the problem]
[0008] As a result of extensive efforts, the present inventors have found that the shielding properties for He gas can be improved by defining the molar volume of glass, and propose this finding in the present invention.
[0009] More specifically, the glass of the present invention has a molar volume of 26.0 cm 3 The glass is characterized in that it is an atomic cell glass having a SiO2 content of 0.1 to 1.0 mole or less.
[0010] Furthermore, the glass for an atomic cell according to the present invention preferably contains, by mass %, 0.5 to 10% Li2O, which makes it easy to fabricate an atomic cell sealed with glass using an anodic bonding method.
[0011] Furthermore, the glass for an atomic cell according to the present invention preferably contains, in mass %, 50-70% SiO2, 10-30% Al2O3, 9-30% MgO+CaO+SrO+BaO, 0.5-10% Li2O, 0-3% Na2O, and 0-3% B2O3 as a glass composition.
[0012] The glass for an atomic cell according to the present invention preferably contains, in mass %, 9 to 30% MgO+CaO as a glass composition.
[0013] The glass for an atomic cell according to the present invention preferably has a glass composition in which the mass ratio of CaO / MgO is 1.0 or less.
[0014] It is preferable that the glass for an atomic cell according to the present invention does not substantially contain B2O3.
[0015] It is preferable that the glass for an atomic cell according to the present invention does not substantially contain P2O5.
[0016] It is preferable that the glass for an atomic cell according to the present invention does not substantially contain Na2O.
[0017] The atom cell according to the present invention includes a cell body having a first main surface and a second main surface facing each other and having a through hole penetrating between the first main surface and the second main surface, a first window portion provided on the first main surface of the cell body and closing one side of the through hole, and a second window portion provided on the second main surface of the cell body and closing the other side of the through hole, wherein the first window portion and the second window portion are made of an atomic cell glass configured according to the present invention.
[0018] In the atom cell according to the present invention, it is preferable that the glass for the atom cell constitutes at least one of a light entrance surface and a light exit surface of the atom cell.
[0019] In the atom cell according to the present invention, the cell body is preferably made of glass.
[0020] In the atomic cell according to the present invention, it is preferable that the cell body, the first window portion, and the second window portion have the same glass composition.
[0021] The manufacturing method of an atom cell according to the present invention is a manufacturing method of an atom cell configured according to the present invention, and includes the steps of: placing the first window portion on the first main surface of the cell body and joining the cell body and the first window portion; placing an alkali metal in the through hole; placing the second window portion on the second main surface of the cell body, joining the cell body and the second window portion, and sealing the inside of the through hole.
[0022] In the method for manufacturing an atomic cell according to the present invention, it is preferable that the cell body, the first window portion, and the second window portion are bonded to each other by anodic bonding. Effect of the Invention
[0023] According to the present invention, it is possible to provide a glass for an atomic cell that is less susceptible to change over time in the oscillation frequency of an atomic oscillator due to permeation of He gas. [Brief description of the drawings]
[0024] [Figure 1] FIG. 1 is a schematic perspective view showing an atom cell according to an embodiment of the present invention. [Diagram 2] 2 is a schematic cross-sectional view of a portion taken along line AA in FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] Preferred embodiments will be described below. However, the following embodiments are merely examples, and the present invention is not limited to the following embodiments. In addition, in the drawings, components having substantially the same functions may be referred to by the same reference numerals.
[0026] (Atomic cell glass) The atomic cell glass of the present invention has a molar volume of 26.0 cm 3 The reason for limiting the molar volume of the glass as described above is as follows.
[0027] The molar volume of glass is an index that indicates the structural density of the glass, and is an element that makes it difficult for He in the atmosphere to penetrate from the glass surface through the inside to the inside of the atomic cell. This makes it even more difficult for the oscillation frequency of the atomic oscillator to change over time. The molar volume of glass is 26.0 cm 3 / mol or less, preferably 25.5 cm 3 / mol or less, more preferably 25.0 cm 3 / mol or less, more preferably 24.5 cm 3 / mol or less, particularly preferably 24.0 cm 3 The lower limit of the molar volume of the atomic cell glass is preferably 19.0 cm 3 / mol or more, more preferably 20.0 cm 3 / mol or more.
[0028] By adjusting the glass composition as follows, the molar volume is 26.0 cm 3 In the description of the content of each component, "%" means "mass %" unless otherwise specified.
[0029] Li2O is a component that significantly lowers the melting temperature and softening point of glass, and also enables anodic bonding as a mobile component in glass. The content of Li2O is preferably 0.5 to 10%, more preferably 1 to 8%, further preferably 1.5 to 7%, and particularly preferably 2 to 6%. If the Li2O content is too low, the melting temperature of the glass becomes unduly high, and the amount of Li ions, which is a mobile component, is small, making anodic bonding significantly difficult. On the other hand, if the Li2O content is too high, the Li component precipitates from the glass surface (alkali blowing), and the weather resistance and acid resistance of the glass significantly decrease.
[0030] SiO2 is a component that forms the network of glass, and therefore stabilizes glass and enhances weather resistance and acid resistance. The content of SiO2 is preferably 50 to 70%, more preferably 52 to 67%, further preferably 54 to 65%, and particularly preferably 56 to 63%. If the content of SiO2 is too low, the weather resistance and acid resistance tend to decrease. On the other hand, if the content of SiO2 is too high, the melting temperature of the glass increases, increasing the manufacturing cost, and devitrification (unintended crystals) precipitates from the glass, causing problems in anodic bonding.
[0031] Al2O3 is a component that stabilizes glass and improves weather resistance and acid resistance. The content of Al2O3 is preferably 10 to 30%, more preferably 12 to 28%, further preferably 15 to 25%, and particularly preferably 18 to 23%. If the content of Al2O3 is too low, the weather resistance and acid resistance are reduced, and devitrified substances are precipitated from the molten glass during melting, which causes problems with anodic bonding. On the other hand, if the content of Al2O3 is too high, devitrified substances are precipitated from the molten glass during melting, which causes problems with anodic bonding. There is also a risk of melting becoming difficult.
[0032] Na2O is a component that lowers the melting temperature and softening point of glass and, as a mobile component in glass, enables anodic bonding. However, if the Na2O content is too high, the Na component precipitates from the glass surface (alkali blowing), and the weather resistance and acid resistance of the glass decrease. The Na2O content is preferably 0 to 3%, more preferably 0 to 2%, and even more preferably 0 to 1%, and it is particularly preferable that the Na2O content is substantially zero. Here, "substantially zero" means that the content in the glass composition is 1000 ppm or less.
[0033] In addition, the effect as a movable component is greatest in the order of Li2O and Na2O. Therefore, when anodic bonding is performed, it is preferable to preferentially select Li2O as long as it does not impede other properties of the glass (meltability, stability, weather resistance, acid resistance, etc.).
[0034] Alkaline earth oxides MgO, CaO, SrO, and BaO have the effect of lowering the molar volume of glass, and therefore are components that make it difficult for He in the atmosphere to penetrate from the glass surface through the inside to the inside of the atomic cell. In addition, alkaline earth oxides are components that lower the melting temperature and softening point of glass, but also stabilize glass. In particular, in the case of LAS-based glass that is based on SiO2, Al2O3, and Li2O, there is a risk that devitrification becomes difficult due to precipitation of devitrified matter during melting, and even if it is possible to form the glass, there is a risk that crystals will precipitate from the glass when heat is applied to the formed glass, which will have a significant adverse effect on the anodic bondability. Therefore, in the present invention, the effect of alkaline earth oxides is important. The content of MgO+CaO+SrO+BaO is preferably 9 to 30%, more preferably 10 to 25%, even more preferably 11 to 22%, and particularly preferably 12 to 20%. If the content of MgO+CaO+SrO+BaO is too low, the melting temperature of the glass becomes high, making it difficult to melt, and the glass becomes significantly unstable, making it difficult to vitrify. On the other hand, if the content of MgO+CaO+SrO+BaO is too high, the glass becomes unstable and its weather resistance and acid resistance decrease. Here, MgO+CaO+SrO+BaO refers to the total content of MgO, CaO, SrO, and BaO in the glass.
[0035] MgO is a component that lowers the melting temperature and softening point of glass, but also stabilizes glass. In addition, it has the effect of lowering the molar volume of glass, so that He in the atmosphere is less likely to penetrate from the surface of the glass through the inside to the inside of the atomic cell. The content of MgO is preferably 5 to 25%, more preferably 7 to 23%, further preferably 8 to 20%, and particularly preferably 9 to 18%. If the content of MgO is too small, the melting temperature of the glass becomes high, making it difficult to melt, and the glass becomes significantly unstable, making it difficult to vitrify. On the other hand, if the content of MgO is too high, the glass becomes unstable and the weather resistance and acid resistance of the glass decrease.
[0036] CaO is a component that lowers the melting temperature and softening point of glass, but also stabilizes glass. In addition, it has the effect of lowering the molar volume of glass, so that it is a component that makes it difficult for He in the atmosphere to penetrate from the surface of the glass through the inside to the inside of the atomic cell. The CaO content is preferably 0 to 15%, more preferably 0.5 to 12%, further preferably 1 to 10%, and particularly preferably 3 to 8%. If the CaO content is too small, the melting temperature of the glass becomes high, making it difficult to melt, and the glass becomes significantly unstable, making it difficult to vitrify. On the other hand, if the CaO content is too high, the glass becomes unstable and the weather resistance and acid resistance of the glass decrease.
[0037] SrO is a component that lowers the melting temperature and softening point of glass, but also stabilizes glass. In addition, it has the effect of lowering the molar volume of glass, so that He in the atmosphere is less likely to penetrate from the surface of the glass through the inside to the inside of the atomic cell. The content of SrO is preferably 0 to 10%, more preferably 0.1 to 8%, further preferably 0.5 to 5%, and particularly preferably 1 to 3%. If the content of SrO is too small, the melting temperature of the glass becomes high, making it difficult to melt, and the glass becomes significantly unstable, making it difficult to vitrify. On the other hand, if the content of SrO is too large, the glass becomes unstable and the weather resistance and acid resistance of the glass decrease. In addition, it inhibits the mobility of Li ions in the glass, so that the anodic bondability is significantly deteriorated.
[0038] BaO is a component that lowers the melting temperature and softening point of glass, but also stabilizes glass. In addition, BaO has the effect of lowering the molar volume of glass, so that He in the atmosphere is less likely to penetrate from the surface of the glass through the inside to the inside of the atomic cell. The content of BaO is preferably 0 to 8%, more preferably 0.1 to 5%, further preferably 0.5 to 3%, and particularly preferably 1 to 2%. If the content of BaO is too small, the melting temperature of the glass increases, making it difficult to melt, and the glass becomes significantly unstable, making it difficult to vitrify. On the other hand, if the content of BaO is too large, the glass becomes unstable and the weather resistance and acid resistance of the glass decrease. In addition, the mobility of Li ions in the glass is inhibited, so that the anodic bondability is significantly deteriorated.
[0039] From the viewpoint of effectively performing anodic bonding while keeping the molar volume low, it is preferable to select MgO and CaO as the alkaline earth oxides, as long as other properties of the glass (meltability, stability, weather resistance, acid resistance, etc.) are not impaired. The content of MgO+CaO in the glass is preferably 9 to 30%, more preferably 10 to 25%, further preferably 11 to 22%, and particularly preferably 12 to 20%. If the content of MgO+CaO is too small, the melting temperature of the glass becomes high, making it difficult to melt, and the glass becomes significantly unstable, making it difficult to vitrify. On the other hand, if the content of MgO+CaO is too high, the glass becomes unstable and the weather resistance and acid resistance of the glass decrease. Here, MgO+CaO refers to the total content of MgO and CaO in the glass.
[0040] Furthermore, from the viewpoint of effectively performing anodic bonding while keeping the molar volume low, the mass ratio "CaO / MgO" obtained by dividing the CaO content in the glass by the MgO content is preferably 1.0 or less, more preferably 0.8 or less, even more preferably 0.6 or less, and particularly preferably 0.4 or less.
[0041] B2O3 is a glass network forming component, and therefore stabilizes glass and enhances weather resistance and acid resistance. However, since it is a component that significantly increases the molar volume of glass, it significantly reduces the shielding ability against He gas. The content of B2O3 is preferably 0 to 3%, more preferably 0 to 2%, and even more preferably 0 to 1%, and it is particularly preferable that it is substantially not contained. Here, "substantially not contained" means that the content in glass is 1000 ppm or less.
[0042] P2O5 is a component that stabilizes glass because it is a component that forms a glass network. However, it is a component that increases the molar volume of glass, and therefore reduces the shielding ability for He gas. The content of P2O5 is preferably 0 to 5%, more preferably 0 to 2%, and even more preferably 0 to 1%, and it is particularly preferable that it is substantially not contained. Here, "substantially not contained" means that the content in the glass is 1000 ppm or less.
[0043] TiO2 is a component that improves the weather resistance and acid resistance of glass. The content of TiO2 is preferably 0 to 5%, more preferably 0.1 to 4%, further preferably 0.5 to 3%, and particularly preferably 1 to 2%. If the content of TiO2 is too high, the viscosity (softening point, etc.) of the glass increases, and the glass becomes thermally unstable, and the glass is easily devitrified when melted.
[0044] ZnO is a component that forms the skeleton of glass. The content of ZnO is preferably 0 to 5%, more preferably 0.1 to 3%, further preferably 0.5 to 2%, and particularly preferably 1 to 2%. When the content of ZnO is large, devitrification particles caused by ZnO are easily precipitated, which increases the liquidus temperature and therefore the melting cost.
[0045] K2O is a component that lowers the melting temperature and softening point of glass. The content of K2O is 0 to 3%, preferably 0.1 to 2%, and more preferably 0.2 to 1%. If the content of K2O is too low, the melting temperature of the glass becomes unduly high. On the other hand, if the content of K2O is too high, alkali components precipitate from the glass surface (alkali blowing), and the weather resistance and acid resistance of the glass decrease.
[0046] (Atomic Cell) Fig. 1 is a schematic perspective view showing an atomic cell according to one embodiment of the present invention, Fig. 2 is a schematic cross-sectional view of a portion taken along line AA in Fig. 1.
[0047] As shown in FIGS. 1 and 2, the atomic cell 1 includes a cell body 2, a first window portion 3, and a second window portion 4.
[0048] The cell body 2 has a first main surface 2a and a second main surface 2b opposed to each other. The cell body 2 is provided with a through hole 5 penetrating from the first main surface 2a to the second main surface 2b.
[0049] In this embodiment, the shape of the cell body 2 is a rectangular parallelepiped. The shape of the cell body 2 may be, for example, a cylindrical shape, and is not particularly limited. In this embodiment, the shape of the through-hole 5 is also a cylindrical shape. The shape of the through-hole 5 may also be, for example, a rectangular parallelepiped, and is not particularly limited.
[0050] In this embodiment, the cell body 2 is made of glass. This increases the transmittance of light emitted from the light source, allowing the alkali metal to be irradiated effectively. However, the cell body 2 may be made of metal, quartz, silicon, etc.
[0051] A first window portion 3 is provided on the first main surface 2a of the cell body 2. The first window portion 3 is provided so as to close one side of the through hole 5 of the cell body 2. In addition, a second window portion 4 is provided on the second main surface 2b of the cell body 2. The second window portion 4 is provided so as to close the other side of the through hole 5 of the cell body 2.
[0052] In this embodiment, the first window portion 3 and the second window portion 4 each have a rectangular plate shape. The shapes of the first window portion 3 and the second window portion 4 are not particularly limited and may each be a disk shape as long as they can close the through hole 5.
[0053] The first window 3 and the second window 4 are made of the glass for an atom cell of the present invention. The glass for an atom cell of the present invention has a molar volume of 26.0 cm 3 / mol or less.
[0054] The atomic cell 1 is a container in which an alkali metal or a buffer gas is sealed, and the vapor-like alkali metal or the buffer gas is sealed in the through-hole 5 of the atomic cell 1 for use. In the atomic cell 1 in which the alkali metal or the buffer gas is sealed in the through-hole 5, light emitted from a light source (not shown) is incident on the light-entering surface 1a of the first window 3. The light incident on the light-entering surface 1a is irradiated on the alkali metal in the through-hole 5 and is emitted from the light-exiting surface 1b of the second window 4. The light emitted from the light-exiting surface 1b is incident on a photodetector (not shown) to obtain a signal. The alkali metal may be cesium (Cs) or rubidium (Rb). The buffer gas may be neon or argon.
[0055] The feature of this embodiment is that the molar volume of the atomic cell glass constituting the first window portion 3 and the second window portion 4 is 26.0 cm 3 Thus, the molar volume of the first window portion 3 and the second window portion 4 is 26.0 cm3 / mol or less. 3 / mol or less, He in the atmosphere is unlikely to penetrate into the atomic cell through the glass. In addition, buffer gases such as neon and argon sealed inside the atomic cell 1 are unlikely to escape from the cell. Therefore, in the atomic cell 1, it is possible to make it difficult for the oscillation frequency of the atomic oscillator to change over time.
[0056] In the present invention, the molar volume of the atomic cell glass is preferably 25.5 cm 3 / mol or less, more preferably 25.0 cm3 / mol or less, more preferably 24.5 cm 3 / mol or less, particularly preferably 24.0 cm 3 / mol or less. When the molar volume of the atomic cell glass is within the above numerical range, He in the atmosphere is unlikely to penetrate from the glass surface through the inside to the atomic cell. This makes it even more difficult for the oscillation frequency of the atomic oscillator to change over time. The lower limit of the molar volume of the atomic cell glass is preferably 19.0 cm3. 3 / mol or more, more preferably 20.0 cm 3 / mol or more.
[0057] In addition, since the Li2O content of the atomic cell glass constituting the first window portion 3 and the second window portion 4 is 0.5% or more, anodic bonding can be easily performed at a relatively low temperature of 320° C. or less. Therefore, the atomic cell 1 can provide an atomic cell with excellent adhesiveness and airtightness.
[0058] The average thermal expansion coefficient of the atomic cell glass at 30°C to 300°C is, for example, 30×10 -7 / ℃ or more, 120×10 -7 / ℃ or less.
[0059] In this embodiment, both the first window portion 3 and the second window portion 4 have a molar volume of 26.0 cm 3 The glass is made of an atomic cell glass having a molar volume of 26.0 cm3 / mol or less. However, at least one of the first window portion 3 and the second window portion 4 is made of an atomic cell glass having a molar volume of 26.0 cm3 / mol or less. 3 At least one of the light entrance surface 1a and the light exit surface 1b may be made of an atomic cell glass having a molar volume of 26.0 cm3 / mol or less. 3 In particular, the portion of at least one of the first window portion 3 and the second window portion 4 facing the through hole 5 which is the portion for sealing the alkali metal may be made of an atomic cell glass having a molar volume of 26.0 cm3 or less. 3 The cell glass may be composed of an atomic cell glass having a molecular weight of 1 / mol or less.
[0060] Moreover, the cell body 2 preferably has the same glass composition as the first window 3 and the second window 4. More preferably, the cell body 2 has substantially the same glass composition as the first window 3 and the second window 4. That is, the cell body 2 is also preferably made of the glass for atomic cells of the present invention. In this case, He in the atmosphere is more unlikely to enter the inside of the atomic cell. Also, the buffer gas sealed inside the atomic cell 1 is more unlikely to escape from the cell. Therefore, it is possible to make it more difficult for the oscillation frequency of the atomic oscillator to change over time. In the present invention, glasses having "same glass composition" refer to glasses in which the top three components with the highest content among the components contained as a glass composition are the same. In the present invention, glasses having "substantially the same glass composition" include glasses in which the components contained as a glass composition are the same, and the difference in the content of each component of one glass relative to the composition of the other glass is within the range of +5% to -5%.
[0061] An example of a method for manufacturing the atomic cell 1 will now be described.
[0062] (Method of manufacturing the atomic cell) In the manufacturing method of the atomic cell 1, first, the cell body 2, the first window portion 3, and the second window portion 4 are prepared. The through-hole 5 of the cell body 2 can be formed by, for example, drilling or ultrasonic processing. The diameter of the through-hole 5 is not particularly limited.
[0063] Next, the first main surface 2a of the cell body 2 and the first window portion 3 are anodically bonded. Next, an alkali metal is put into the through hole 5 of the cell body 2, and the second main surface 2b of the cell body 2 and the second window portion 4 are anodically bonded. In addition, when anodically bonding the second main surface 2b of the cell body 2 and the second window portion 4, a buffer gas is introduced into the through hole 5, and the anodically bonding is performed in this buffer gas atmosphere. As the buffer gas, an inert gas such as neon or argon can be used. In addition, after the anodically bonding, the alkali metal can be gasified by heating and used. In other words, in the present invention, the alkali metal in the atomic cell 1 may be in a state such as a solid before gasification, or may be in a gasified state. In addition, the alkali metal may be directly sealed inside the atomic cell 1 in a gaseous state.
[0064] It is preferable to polish the bonding surfaces beforehand when anodically bonding the cell body 2 to the first window portion 3 and the second window portion 4. In this case, the surface roughness Ra of the bonding surfaces is preferably 0.3 nm or less, more preferably 0.2 nm or less, and further preferably 0.1 nm or less.
[0065] Furthermore, when anodically bonding the cell body 2 to the first window portion 3 and the second window portion 4, the bonding can be made even stronger by further applying pressure. The pressure during the application of pressure is preferably 1 MPa or less, more preferably 0.8 MPa or less, and further preferably 0.5 MPa or less. The lower limit of the pressure during the application of pressure is preferably 0.01 MPa.
[0066] The heating temperature in the anodic bonding is preferably 320° C. or less, 300° C. or less, particularly preferably 250° C. or less, which is the temperature at which cesium azide, the Cs source, begins to release Cs gas.
[0067] In this embodiment, the cell body 2, the first window portion 3, and the second window portion 4 are all made of glass, so that the atomic cell 1 can be manufactured simply and efficiently and can be firmly joined at a low temperature. Furthermore, the cell body 2, the first window portion 3, and the second window portion 4 have the same thermal expansion coefficient, so that the airtightness can be further improved.
[0068] The glass for atomic cells and the atomic cell of the present invention can be used, for example, in an atomic oscillator that uses the quantum interference effect of two types of light with different wavelengths to cause an alkali metal to undergo a resonant transition. However, the glass and the atomic cell may also be used in an atomic oscillator that uses the double resonance phenomenon of light and microwaves to cause an alkali metal to undergo a resonant transition, and are not particularly limited. In either case, the oscillation frequency of the atomic oscillator can be made less susceptible to change over time.
[0069] The present invention will be described below based on examples, but the present invention is not limited to these examples.
[0070] (Examples 1 to 7 and Comparative Examples 1 to 2) Glasses for atomic cells of Examples 1 to 7 and Comparative Examples 1 and 2 shown in Table 1 below were prepared.
[0071] Specifically, a glass batch was prepared by mixing various oxides, carbonates, etc. to obtain the glass composition shown in Table 1 below, which was then placed in a platinum crucible and melted at 1400 to 1500°C for 6 hours, after which the molten glass was poured into a stainless steel mold and molded. The glass thus obtained was then annealed by holding it at 650°C for 1 hour.
[0072] Thereafter, the density of the obtained glass was measured by Archimedes' method.
[0073] Furthermore, the average thermal expansion coefficient in the temperature range of 30 to 300° C. was measured using a push rod type thermal expansion coefficient measuring device.
[0074] The molar volume was then calculated from the formula weight of the glass composition and the density of the glass.
[0075] Then, a window made of the obtained glass was placed on the main surface of the cell body made of the obtained glass, and the cell body and the window were anodically bonded. Then, an alkali metal was placed in the through hole. Furthermore, another window made of the obtained glass was placed on the main surface of the cell body opposite to the above, and the cell body and the window were anodically bonded to seal the through hole, thereby producing an atomic cell. The anodic bonding was performed at 320°C, 300°C, and 250°C with an applied voltage of 1000V.
[0076] After that, the airtightness of the atomic cell was evaluated as follows. A low-viscosity red ink was dripped along the interface of the anodic bond of the fabricated atomic cell, and the bonded interface was set to be perpendicular to the ground surface. After 72 hours, the bonded interface was observed with an optical microscope (200x). The bonded interface was observed from the perpendicular direction, and the red ink was marked as "good" when it had permeated less than 10% of the bonded interface area, marked as "good" when it had permeated 10-90% of the bonded interface area, and marked as "bad" when it had permeated 90-100% of the bonded interface area.
[0077] The atomic cell was then used to evaluate the shielding properties of He gas. 5 The atoms / cm s atoms is the detection limit of He gas permeability, and if it is below the detection limit, the shielding effect of He gas is high. The He gas permeability was evaluated by measuring at 30°C using gas chromatography.
[0078] [Table 1]
[0079] From Table 1, the glasses of Examples 1 to 7 have a molar volume of 26.0 cm 3 / mol or less, and the helium permeability is 10 5 The molar volume of the glasses of Comparative Examples 1 and 2 was 26.0 cm 3 / mol, helium permeability exceeds 10 5The shielding properties of He gas were poor because the ion concentration exceeded the limit of 1000 keV / cm s atoms.
[0080] Therefore, it was confirmed that when the glasses of Examples 1 to 7 were used, an atomic cell in which the oscillation frequency of the atomic oscillator is unlikely to change over time due to high He gas shielding properties was obtained. [Explanation of symbols]
[0081] 1...Atomic cell 1a...Light incident surface 1b…Idemitsu surface 2. Cell body 2a…First main surface 2b…Second main surface 3…First window section 4…Second window section 5...Through hole
Claims
1. Molar volume is 23.8 cm 3 / mol or less, and the glass composition contains, in mass %, 50% to 70% SiO 2 , 10% to 30% Al 2 O 3 , 9 to 30% MgO+CaO+SrO+BaO, 0.5% to 10% Li 2 O , 0 to 3% Na 2 O , and 0 to 1.5% B 2 O 3 .
2. The glass for an atomic cell according to claim 1, containing 9 to 30 mass% of MgO + CaO.
3. 3. The glass for an atomic cell according to claim 1, wherein a mass ratio of CaO / MgO is 1.0 or less.
4. In reality, B 2 O 3 The glass for an atom cell according to any one of claims 1 to 3, which does not contain
5. In effect, P 2 O 5 The glass for an atom cell according to any one of claims 1 to 4, which does not contain
6. Substantially Na 2 The glass for an atom cell according to any one of claims 1 to 5, which does not contain O.
7. A cell body having a first main surface and a second main surface opposed to each other and having a through hole penetrating between the first main surface and the second main surface; a first window portion provided on a first main surface of the cell body and closing one side of the through hole; a second window portion provided on a second main surface of the cell body and closing the other side of the through hole; Equipped with An atom cell, wherein the first window portion and the second window portion are made of the glass for atom cells according to any one of claims 1 to 6.
8. The atom cell according to claim 7 , wherein the atom cell glass constitutes at least one of a light entrance surface and a light exit surface of the atom cell.
9. The atomic cell according to claim 7 or 8, wherein the cell body is made of glass.
10. The atomic cell according to any one of claims 7 to 9, wherein the cell body, the first window portion and the second window portion have substantially the same glass composition.
11. A method for producing an atom cell according to any one of claims 7 to 10, comprising the steps of: disposing the first window portion on the first main surface of the cell body and joining the cell body and the first window portion; disposing an alkali metal in the through hole; a step of disposing the second window portion on the second main surface of the cell body, joining the cell body and the second window portion, and sealing the inside of the through hole; A method for manufacturing an atomic cell comprising:
12. The method for manufacturing an atomic cell according to claim 11 , wherein the cell body and the first window portion are joined by an anodic bonding method, and the cell body and the second window portion are joined by an anodic bonding method.
Citation Information
Patent Citations
Flat panel display device containing borosilicate glass rich in alumina and alkal earth metal
JP1993193980A
Atomic frequency reference cell and its manufacture
JP1994204586A
Glass cell, liquid crystal device, and manufacturing method of these
JP2015215502A
Frequency signal generation device and frequency signal generation system
JP2019087865A
Vapor cell comprising electro-optic function for chip-scale atomic clock, and method for manufacturing sealed container for chipscale instrument
US20180212612A1