Coating solution for forming anti-glare film, anti-glare film and laminate having the same

A coating liquid using metal alkoxides and salts forms an anti-glare film with high refractive index, addressing safety and applicability issues in existing treatments, enhancing image display device visibility.

JP7583372B2Active Publication Date: 2024-11-14NISSAN CHEM CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021504042
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-01
Filing Date
2020-02-28
Publication Date
2024-11-14
Estimated Expiration
2040-02-28

AI Technical Summary

Technical Problem

Existing anti-glare treatments for image display devices, such as etching with chemicals or forming organic films, pose safety hazards and difficulty in application and adhesion, leading to issues with functional film applicability and damage.

Method used

A coating liquid containing specific metal alkoxides, metal salts, and solvents is used to form an anti-glare film with high refractive index, utilizing components like silicon, titanium, and zirconium alkoxides, along with metal salts and inorganic fine particles, to create a laminate with excellent anti-glare properties.

Benefits of technology

The solution enables the formation of an anti-glare film with superior anti-glare function and high refractive index, suitable for glass substrates, improving visibility in image display devices by reducing reflections.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583372000003
    Figure 0007583372000003
  • Figure 0007583372000004
    Figure 0007583372000004
  • Figure 0007583372000001
    Figure 0007583372000001
Patent Text Reader

Abstract

An anti-glare coating film formation coating liquid that contains the following components. Component (A): A first metal alkoxide represented by formula (I) or a hydrolyzate or partial condensate thereof. (I) R1 mM1(OR2)n-m. Component (B): A metal salt that includes a metal salt represented by formula (II) and / or an oxalate of M2 in formula (II). (II) M2(X)k. Solvent group (A): Glycol ethers that have a boiling point of less than 160°C or derivatives thereof; or ketones. Solvent group (B): Alcohols that have a boiling point of no more than 120°C. The symbols in formula 1 and formula 2 are defined in the description.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating liquid for forming an anti-glare coating which is excellent in anti-glare properties (anti-glare function) and can be formed on a glass substrate to form an anti-glare coating having a high refractive index, an anti-glare coating obtained from the coating liquid, and a laminate including the same. [Background technology]

[0002] Image display devices (liquid crystal displays, organic electroluminescence displays, plasma displays, etc.) equipped in various devices such as televisions, personal computers, and smartphones may experience a reduction in image visibility when external light such as indoor lighting (fluorescent lights, etc.) or sunlight is reflected on the display surface. One method for suppressing the reflection of external light is to apply an anti-glare treatment to the display surface of an image display device. The anti-glare treatment is a process for forming irregularities on the surface, and the formed irregularities provide the effect of diffusing and reflecting external light (anti-glare effect). Proposed methods for anti-glare treatment include etching the surface of a transparent substrate such as glass with a chemical such as hydrofluoric acid (see Patent Document 1), and forming an organic anti-glare film with an uneven surface (see Patent Document 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 5839134 [Patent Document 2] International Publication 2018 / 070426 Summary of the Invention [Problem to be solved by the invention]

[0004] However, in the process of etching the surface of a glass substrate with chemicals, the danger of the chemicals becomes an issue, and in the process of forming an organic anti-glare film on the surface, problems arise with the coatability onto the glass substrate and with the coatability and adhesion when forming an additional functional film on the film.

[0005] In view of the above, an object of the present invention is to provide a coating liquid for forming an anti-glare coating which is excellent in anti-glare properties (anti-glare function), can be formed on a glass substrate, and can form an anti-glare coating having a high refractive index, an anti-glare coating obtained from the coating liquid, and a laminate comprising the same. [Means for solving the problem]

[0006] As a result of intensive research by the present inventors in order to achieve the above object, the present invention has been completed as follows. That is, the present invention has the following constituent features. 1. A coating solution for forming an anti-glare coating containing the following components: Component (A): A first metal alkoxide represented by the following formula (I), a hydrolyzate thereof, or a partial condensate thereof. R 1 m M 1 (OR 2 ) n-m (I) (In the formula, M 1 R represents at least one metal selected from the group consisting of silicon (Si), titanium (Ti), tantalum (Ta), zirconium (Zr), boron (B), aluminum (Al), magnesium (Mg), tin (Sn) and zinc (Zn). 1 may be substituted with a hydrogen atom or a fluorine atom, and may be substituted with a halogen atom, a vinyl group, a glycidoxy group, a mercapto group, a methacryloxy group, an acryloxy group, an isopropyl group, S R represents a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a cyanate group, an amino group, or a ureido group and which may have a hetero atom. 2 represents an alkyl group having 1 to 5 carbon atoms, and n is M 1 represents a valence of 2 to 5. m is M 1 If the valence is 2, it is 0 or 1, M1 When the valence of is 3, it is 0 to 2, and M 1 When the valence of is 4, it is 0 to 3, and M 1 If the valence is 5, it is either 0 to 4.) Component (B): A metal salt represented by the following formula (II) and M in the following formula (II) 2 A metal salt containing at least one oxalate selected from the group consisting of the above. M 2 (X) k (II) (In the formula, M 2 represents at least one metal selected from the group consisting of aluminum (Al), indium (In), zinc (Zn), zirconium (Zr), bismuth (Bi), lanthanum (La), tantalum (Ta), yttrium (Y) and cerium (Ce); X represents chlorine, nitric acid, sulfuric acid, acetic acid, sulfamic acid, sulfonic acid, acetoacetic acid, acetylacetonate or a basic salt thereof; k represents M 2 Represents the valence of Solvent group (A): At least one selected from glycol ethers and their derivatives having a boiling point of less than 160° C., or ketones. Solvent group (B): At least one selected from alcohols having a boiling point of 120° C. or less. Effect of the Invention

[0007] By using the coating liquid for forming an anti-glare film of the present invention, it is possible to form an anti-glare film that is excellent in anti-glare properties (anti-glare function), can be formed on a glass substrate, and has a high refractive index. [Brief description of the drawings]

[0008] [Figure 1] 1 is an image of the antiglare coated substrate obtained in Example 2, observed using a three-dimensional white light interference microscope Contour GT. [Diagram 2] 1 is an image of the antiglare coated substrate obtained in Comparative Example 2, observed using a three-dimensional white light interference microscope Contour GT. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Each component contained in the coating solution for forming an antiglare film of the present invention will be described in detail below.

[0010] <Component (A)> The component (A) contained in the coating liquid for forming an antiglare film of the present invention is a first metal alkoxide represented by the following formula (I), a hydrolyzate thereof, or a partial condensate thereof. R 1 m M 1 (OR 2 ) n-m (I) In the formula, M 1 represents at least one metal selected from the group consisting of silicon (Si), titanium (Ti), tantalum (Ta), zirconium (Zr), boron (B), aluminum (Al), magnesium (Mg), tin (Sn) and zinc (Zn). Among these, silicon, titanium, zirconium, aluminum and tin are preferred from the viewpoints of availability and storage stability of the composition. R 1 may be substituted with a hydrogen atom or a fluorine atom, and may be substituted with a halogen atom, a vinyl group, a glycidoxy group, a mercapto group, a methacryloxy group, an acryloxy group, an isopropyl group, S It represents a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a cyanate group, an amino group or a ureido group and which may have a heteroatom. Among these, from the viewpoints of availability and stability, a vinyl group, a mercapto group, a methacryloxy group, an acryloxy group and a ureido group are preferred as the substituent, and a hydrocarbon group having 1 to 10 carbon atoms is preferred. R 2 represents an alkyl group having 1 to 5 carbon atoms, and among these, from the viewpoints of easy availability and the storage stability of the composition, those having 1 to 4 carbon atoms are preferred. n is M 1 represents a valence of 2 to 5. m is M 1 If the valence is 2, it is 0 or 1, M 1 When the valence of is 3, it is 0 to 2, and M 1 When the valence of is 4, it is 0 to 3, and M1 When the valence is 5, it is any one of 0 to 4.

[0011] The component (A) contained in the coating liquid for forming an antiglare film of the present invention is preferably a partial condensate of silicon alkoxide, titanium alkoxide or zirconium alkoxide. 1 Examples of the metal alkoxide include partial condensates of a metal alkoxide represented by the formula (I) in which the metal alkoxide is selected from silicon (Si), titanium (Ti), tantalum (Ta) and zirconium (Zr).

[0012] <Ingredient (B)> The component (B) contained in the coating liquid for forming an antiglare film of the present invention is a metal salt represented by the following formula (II) and M 2 The metal salt contains at least one metal salt selected from the group consisting of oxalates of the above. M 2 (X) k (II) In the formula, M 2 represents at least one metal selected from the group consisting of aluminum (Al), indium (In), zinc (Zn), zirconium (Zr), bismuth (Bi), lanthanum (La), tantalum (Ta), yttrium (Y) and cerium (Ce). X represents chlorine, nitric acid, sulfuric acid, acetic acid, sulfamic acid, sulfonic acid, acetoacetic acid, acetylacetonate or a basic salt thereof. Among these, nitrates of aluminum, indium and cerium are preferred from the viewpoints of availability and storage stability of the composition. k is M 2 Represents the valence of.

[0013] <Other ingredients> The coating liquid for forming an antiglare film of the present invention may contain other components in addition to the above-mentioned components, such as inorganic fine particles, metalloxane oligomers, metalloxane polymers, leveling agents, surfactants, and the like. As the inorganic fine particles, silica fine particles, alumina fine particles, titania fine particles, magnesium fluoride fine particles, etc. are preferable, and a colloidal solution of these inorganic fine particles is particularly preferable. This colloidal solution may be one in which inorganic fine particle powder is dispersed in a dispersion medium, or may be a commercially available colloidal solution. In the present invention, by incorporating inorganic fine particles, it becomes possible to impart a surface shape and other functions to the anti-glare coating film to be formed. The inorganic fine particles preferably have an average particle size of 0.001 to 0.2 μm, and more preferably 0.001 to 0.1 μm. Examples of the dispersion medium for the inorganic fine particles include water and organic solvents. From the viewpoint of improving the stability of the coating solution for forming an antiglare film, the colloidal solution is preferably adjusted to have a pH or pKa of 1 to 10, more preferably 2 to 7. Examples of organic solvents used as dispersion media for colloidal solutions include alcohols such as methanol, ethanol, propanol, butanol, ethylene glycol, propylene glycol, butanediol, pentanediol, 2-methyl-2,4-pentanediol, diethylene glycol, dipropylene glycol, and ethylene glycol monopropyl ether; ketones such as methyl ethyl ketone and methyl isobutyl ketone; aromatic hydrocarbons such as toluene and xylene; amides such as dimethylformamide, dimethylacetamide, and N-methyl-2-pyrrolidone; esters such as ethyl acetate, butyl acetate, and γ-butyrolactone; and ethers such as tetrahydrofuran and 1,4-dioxane. Among these, alcohols and ketones are preferred. These organic solvents can be used as dispersion media either alone or in combination of two or more.

[0014] <Solvent group (A)> The solvent group (A) contained in the coating liquid for forming an antiglare film of the present invention is at least one selected from glycol ethers and their derivatives having a boiling point of less than 160° C., or ketones. Specifically, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol Examples of suitable ethers include glycol ethers and derivatives thereof, such as ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dipropyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol dimethyl ether, and propylene glycol diethyl ether; and ketones, such as acetone, methyl ethyl ketone, and methyl isobutyl ketone. Among these, from the viewpoint of coating stability, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol diethyl ether, ethylene glycol dipropyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, and methyl isobutyl ketone are preferred.

[0015] <Solvent group (B)> The solvent group (B) contained in the coating liquid for forming an antiglare film of the present invention is at least one selected from alcohols having a boiling point of 120° C. or less. Specific examples include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, and 2-methyl-2-propanol. Among these, from the viewpoint of storage stability of the composition, methanol, ethanol, 2-propanol, 2-butanol, and 2-methyl-1-propanol are preferred.

[0016] <Other solvents> The coating solution for forming an antiglare film of the present invention may contain solvents other than the solvent groups (A) and (B) (hereinafter also referred to as other solvents) as necessary from the viewpoint of the stability of the coating solution.

[0017] Examples of other solvents include alcohols such as hexanol, heptanol, octanol, nonanol, decanol, undecanol, dodecanol, and diacetone alcohol; glycols such as ethylene glycol, diethylene glycol, dipropylene glycol, 2-methyl-2,4-pentanediol, propanediol, butanediol, pentanediol, hexanediol, and heptanediol; ethylene glycol monobutyl ether, ethylene glycol dibutyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, propylene glycol dipropyl ether, and propylene glycol diisopropyl ether. Examples of the glycol ethers include diethylene glycol dibutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, and diethylene glycol dibutyl ether; esters such as methyl acetate, ethyl acetate, and ethyl lactate; N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, γ-butyrolactone, dimethylsulfoxide, tetramethylurea, hexamethylphosphotriamide, m-cresol, and tetrahydrofuran.Among these, from the viewpoints of availability and storage stability of the composition, ethylene glycol, diethylene glycol, 2-methyl-2,4-pentanediol, propanediol, butanediol, ethylene glycol monobutyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, N-methyl-2-pyrrolidone, N,N-dimethylformamide, and tetrahydrofuran are preferably used.

[0018] <Coating liquid for forming anti-glare film and anti-glare film> The coating solution for forming an antiglare coating film of the present invention is a coating solution for forming an antiglare coating film, which comprises a first metal alkoxide represented by the above formula (I) and a metal salt represented by the above formula (II) and M 2 The compound is obtained by hydrolysis and condensation in an organic solvent in the presence of at least one metal salt selected from the group consisting of oxalates of the above, and then adding a suitable solvent. The solvents of the solvent groups (A) and (B) are added during the hydrolysis and condensation and / or in the subsequent solvent addition step. In this case, other solvents may also be added as necessary. Metal atom of metal alkoxide (M 1 ) and the metal atom of the metal salt (M 2 The content ratio of M is 0.01 or less in terms of molar ratio. 2 / (M 1 +M 2)≦0.7. If this value is less than 0.01, the mechanical strength of the resulting coating is insufficient, which is undesirable. On the other hand, if it exceeds 0.7, the adhesion of the metal oxide layer to a substrate such as a glass substrate decreases. Furthermore, when the metal oxide layer is fired at a low temperature of 450° C. or less, the chemical resistance of the resulting metal oxide layer also tends to decrease. When the metal alkoxide contained in the coating composition contains multiple types of metal atoms, the above metal atoms (M 1 ) means the total of a plurality of metal atoms, and when the metal salt contained in the coating composition contains a plurality of metal atoms, the metal atoms (M 2 ) means the total of multiple types of metal atoms.

[0019] The solid content concentration in the coating solution for forming an anti-glare coating is preferably in the range of 0.5 to 20 mass % in terms of solid content, calculated as metal oxide for the metal alkoxide and metal salt. If the solid content exceeds 20 mass %, the storage stability of the coating composition deteriorates, and it becomes difficult to control the thickness of the anti-glare coating. On the other hand, if the solid content is 0.5 mass % or less, the thickness of the anti-glare coating obtained is thin, and multiple coatings are required to obtain the desired thickness.

[0020] The coating solution for forming an antiglare coating film is a solution of a first metal alkoxide (e.g., silicon alkoxide or titanium alkoxide) represented by the above formula (I) in the presence of a metal salt represented by the above formula (II) and M 2The antiglare coating is obtained by hydrolysis and condensation in an organic solvent in the presence of at least one metal salt (e.g., aluminum salt) selected from the group consisting of oxalates of silicon alkoxide, titanium alkoxide, or silicon alkoxide and titanium alkoxide. The amount of water used for hydrolysis of silicon alkoxide, titanium alkoxide, or silicon alkoxide and titanium alkoxide is preferably 0.5 to 24 in terms of molar ratio with respect to the total number of moles of silicon alkoxide, titanium alkoxide, or silicon alkoxide and titanium alkoxide. More preferably, it is 0.5 to 20. When the molar ratio (amount of water (moles) / (total number of moles of metal alkoxide)) is 0.5 or less, hydrolysis of the metal alkoxide becomes insufficient, which is undesirable because it reduces the film-forming property and the strength of the antiglare coating obtained. In addition, when the molar ratio is more than 24, polycondensation continues to proceed, which is undesirable because it reduces storage stability. The same applies when other metal alkoxides are used.

[0021] When other metal alkoxides are used, it is preferable to select the same conditions for the amount of water added.

[0022] In the hydrolysis process when preparing a coating solution for forming an antiglare coating film, if the coexisting metal salt (e.g., aluminum salt) is a hydrate salt, the moisture content of the metal salt (e.g., aluminum salt) is involved in the reaction, so it is necessary to take into account the moisture content of the metal salt (e.g., aluminum salt) relative to the amount of water used for hydrolysis.

[0023] The coating liquid for forming an antiglare coating is produced by hydrolysis and condensation of a metal alkoxide, and the refractive index of the resulting antiglare coating can be adjusted within a predetermined range by selecting the composition of the metal alkoxide. For example, when silicon alkoxide and titanium alkoxide are selected as the metal alkoxide, the refractive index of the resulting antiglare coating can be adjusted within a predetermined range described below, specifically within a range of 1.45 to 2.1, by adjusting the mixing ratio. From the viewpoint of antireflection of the laminate including the antiglare coating of the present invention, the refractive index of the antiglare coating of the present invention is preferably 1.48 to 1.8.

[0024] In other words, when the refractive index required for the anti-glare coating film after coating and baking the coating liquid for forming the anti-glare coating film is determined, it is possible to determine the composition molar ratio of silicon alkoxide and titanium alkoxide according to the refractive index. This composition molar ratio is arbitrary, but for example, the refractive index of the anti-glare coating film from the coating liquid for forming the anti-glare coating film obtained by hydrolyzing only silicon alkoxide is about 1.45. And, the refractive index of the metal oxide layer from the coating composition obtained by hydrolyzing only titanium alkoxide is about 2.1. Therefore, when it is desired to set the refractive index of the anti-glare coating film between 1.45 and 2.1, it is possible to manufacture the coating composition by using silicon alkoxide and titanium alkoxide in a predetermined ratio according to the refractive index value within that range.

[0025] The refractive index of the resulting anti-glare coating can also be adjusted by using other metal alkoxides.

[0026] Furthermore, the refractive index of the anti-glare coating can be adjusted by selecting the film formation conditions in addition to the composition conditions, thereby realizing a desired refractive index value of the anti-glare coating.

[0027] That is, when an anti-glare coating is produced by baking a coating film of a coating liquid for forming an anti-glare coating, the refractive index of the anti-glare coating varies according to the baking temperature. In this case, the higher the baking temperature, the higher the refractive index of the anti-glare coating can be. Therefore, by selecting an appropriate baking temperature, it is possible to adjust the refractive index of the anti-glare coating obtained. In addition, when the heat resistance of the substrate and the like is taken into consideration, the baking temperature is preferably in the range of 100°C to 300°C, and more preferably in the range of 150°C to 250°C.

[0028] In addition, when the coating solution for forming an anti-glare film contains titanium alkoxide, if the coating film is irradiated with ultraviolet (UV) rays before baking, the refractive index of the resulting anti-glare film will vary. Specifically, the higher the amount of ultraviolet irradiation, the higher the refractive index of the anti-glare film can be. Therefore, it is possible to select whether or not to irradiate with ultraviolet rays in order to achieve a desired refractive index. In the case of an anti-glare film, if the desired refractive index can be achieved by selecting conditions such as the composition, ultraviolet irradiation is not necessary. In addition, in the case of irradiating with ultraviolet rays, it is possible to adjust the refractive index of the anti-glare film by selecting the amount of irradiation. In the case where ultraviolet irradiation is necessary to obtain a desired refractive index in the anti-glare film, for example, a high-pressure mercury lamp can be used. In addition, when a high-pressure mercury lamp is used, the total light irradiation is 1000 mJ / cm2 in terms of 365 nm. 2 The preferred dose is 3000 mJ / cm or more. 2 ~10000mJ / cm 2 The irradiation amount is more preferably 10 ...

[0029] However, when the coating solution for forming an anti-glare coating contains a titanium alkoxide component, the viscosity gradually increases when stored at room temperature. Although there is no concern that this will cause a major problem in practical use, when precisely controlling the thickness of the anti-glare coating, careful management of temperature and other factors is required. In addition, this increase in viscosity becomes more noticeable as the composition ratio of titanium alkoxide in the coating composition increases. This is thought to be because titanium alkoxide has a higher hydrolysis rate than silicon alkoxide and the like, and the condensation reaction is faster.

[0030] In the case where the coating solution for forming an antiglare film contains a titanium alkoxide component, in order to reduce the change in viscosity, for example, a method of mixing the metal salt with a solvent such as alcohol and then hydrolyzing the silicon alkoxide and titanium alkoxide can be mentioned. In this method, the stability of the condensate is improved by subsequently mixing glycol or a derivative thereof, and a coating solution for forming an antiglare film with less change in viscosity can be obtained.

[0031] The coating solution for forming an antiglare coating film described above can be made into fine droplets and applied to a substrate to obtain a metal oxide coating film having antiglare properties. Examples of the coating method include spray coating, mist coating, and inkjet coating, and among these, spray coating and inkjet coating are preferred.

[0032] <Laminate> The laminate of the present invention can be obtained by applying and baking the coating liquid for forming an antiglare coating onto various substrates including a glass substrate to form an antiglare coating. On this antiglare coating, various functional films such as an antireflection film can be formed according to the functions required for the laminate. Here, the anti-reflection film refers to a film that has the effect of reducing reflectance and reduces glare caused by reflected light, and when used in an image display device, can improve the transmittance of light from the image display device and improve the visibility of the image display device. The configuration of the anti-reflection film is not particularly limited as long as it can suppress the reflection of light. For example, the anti-reflection film may be a film having a lower refractive index than the anti-glare coating (hereinafter, also referred to as a low refractive index film). An example of a material constituting the low refractive index film is polysiloxane having a silicon atom to which a fluorine-containing organic group is bonded. Methods for forming an anti-reflection film include coating the surface of an adhesion layer formed on the anti-glare coating film or other functional film by spin coating, dip coating, casting, slit coating, spray coating, electrostatic spray deposition (ESD), or the like, followed by heat treatment as necessary, or coating the surface of the adhesion layer by chemical vapor deposition (CVD), sputtering, physical vapor deposition (PLD), or the like. Furthermore, the laminate of the present invention may further have an anti-soiling film laminated on the anti-glare coating or the anti-reflection film. The anti-soiling film is a film that suppresses adhesion of organic or inorganic substances to the surface, or a film that has the effect of allowing the adhesion of organic or inorganic substances to be easily removed by cleaning such as wiping even if the organic or inorganic substances adhere to the surface. The thickness of the antifouling film is not particularly limited, but when the antifouling film is made of a fluorine-containing organosilicon compound film, the film thickness is preferably 2 to 20 nm, more preferably 2 to 15 nm, and even more preferably 2 to 10 nm. If the film thickness is 2 nm or more, the antifouling layer will be uniformly covered, and will be practical from the viewpoint of abrasion resistance. In addition, if the film thickness is 20 nm or less, the optical properties such as the haze value of the antiglare coated substrate when the antifouling film is formed are good.

[0033] The anti-glare coated substrate has an in-plane standard deviation of haze of 1 to 40%, and more preferably 1 to 30%. Within this range, when the anti-glare coated substrate is visually observed by the user, it appears to have a uniform anti-glare film treatment, and is excellent in aesthetics. In addition, the touch feeling due to the unevenness of the anti-glare film is not impaired.

[0034] <Application> The anti-glare coated substrate of the present invention is not particularly limited in its application. Specific examples include transparent parts for vehicles (headlight covers, side mirrors, front transparent substrates, side transparent substrates, rear transparent substrates, instrument panel surfaces, etc.), meters, architectural windows, show windows, displays (notebook computers, monitors, LCDs, PDPs, ELDs, CRTs, PDAs, etc.), LCD color filters, touch panel substrates, pickup lenses, optical lenses, eyeglass lenses, camera parts, video parts, CCD cover substrates, optical fiber end faces, projector parts, copier parts, solar cell transparent substrates (cover glass, etc.), mobile phone windows, backlight unit parts (light guide plates, cold cathode fluorescent tubes, etc.), backlight unit parts liquid crystal brightness enhancement films (prisms, semi-transparent films, etc.), liquid crystal brightness enhancement films, organic EL light emitting element parts, inorganic EL light emitting element parts, phosphor light emitting element parts, optical filters, end faces of optical parts, lighting lamps, lighting fixture covers, amplified laser light sources, anti-reflection films, polarizing films, agricultural films, etc. EXAMPLES

[0035] The present invention will be described in more detail below with reference to examples, but is not limited to these. The abbreviations used below are as follows: TEOS: Tetraethoxysilane F13: Tridecafluorooctyltrimethoxysilane UPS: γ-ureidopropyltriethoxysilane MPMS: 3-methacryloxypropyltrimethoxysilane TTE:Tetraethoxytitanium TIPT: Titanium tetraisopropoxide AN: Aluminum nitrate nonahydrate MeOH: Methanol EtOH: Ethanol IPA: Isopropanol BCS: Butyl cellosolve PGME: Propylene glycol monomethyl ether PGMEA: Propylene glycol monomethyl ether acetate PG: Propylene glycol HG: 2-methyl-2,4-pentanediol

[0036] <Synthesis Example 1> In a 200 mL flask, AN (2.9 g), water (2.7 g), and EtOH (50.3 g) were added and stirred to obtain an AN solution. TEOS (23.1 g) was added to the AN solution and stirred at room temperature for 30 minutes. Then, TTE (8.4 g) and EtOH (12.6 g) were added and stirred at room temperature for another 30 minutes to obtain solution K1.

[0037] <Synthesis Example 2> In a 200 mL flask, AN (2.9 g), water (2.6 g), and EtOH (50.6 g) were added and stirred to obtain an AN solution. TEOS (21.2 g) was added to the AN solution and stirred at room temperature for 30 minutes. Then, TTE (10.0 g) and EtOH (12.7 g) were added and stirred at room temperature for another 30 minutes to obtain solution K2.

[0038] <Synthesis Example 3> In a 200 mL flask, AN (2.8 g), water (2.6 g), and EtOH (51.2 g) were added and stirred to obtain an AN solution. TEOS (17.7 g) was added to the AN solution and stirred at room temperature for 30 minutes. Then, TTE (12.9 g) and EtOH (12.8 g) were added and stirred at room temperature for another 30 minutes to obtain solution K3.

[0039] <Synthesis Example 4> In a 200 mL flask, AN (2.9 g), water (2.7 g), EtOH (24.3 g), and IPA (24.3 g) were added and stirred to obtain an AN solution. TEOS (23.1 g) was added to the AN solution and stirred at room temperature for 30 minutes. Then, TIPT (10.5 g), EtOH (6.1 g), and IPA (6.1 g) were added and stirred at room temperature for another 30 minutes to obtain solution K4.

[0040] <Synthesis Example 5> TEOS (34.7 g) and MeOH (33.0 g) were added to a 200 mL four-neck flask equipped with a reflux condenser and stirred, and MeOH (16.4 g), water (15.0 g), and 60% aqueous nitric acid solution (0.9 g) were added thereto and stirred for 30 minutes in an ice bath at 10° C. After that, the mixture was refluxed for 3 hours and allowed to cool to room temperature to obtain solution K5.

[0041] <Synthesis Example 6> TEOS (29.0 g), F13 (10.5 g), and MeOH (27.9 g) were added to a 200 mL four-neck flask equipped with a reflux condenser and stirred, and MeOH (14.0 g), water (15.0 g), and oxalic acid (0.8 g) were added thereto and stirred for 30 minutes in an ice bath at 10°C. After that, the mixture was stirred at 65°C for 2 hours, and then UPS (1.4 g) and MeOH (1.4 g) were added and reacted at 65°C for another 2 hours. After that, the mixture was allowed to cool to room temperature to obtain solution K6.

[0042] <Synthesis Example 7> In a 200 mL flask, AN (2.8 g), water (2.5 g), and EtOH (51.0 g) were added and stirred to obtain an AN solution. TEOS (15.9 g) and MPMS (2.1 g) were added to the AN solution and stirred at room temperature for 30 minutes. Then, TTE (12.9 g) and EtOH (12.8 g) were added and stirred at room temperature for another 30 minutes to obtain solution K7.

[0043] <Synthesis Example 8> In a 200 mL flask, AN (2.8 g), water (2.5 g), and EtOH (38.3 g) were added and stirred to obtain an AN solution. TEOS (16.8 g) was added to the AN solution and stirred at room temperature for 30 minutes. Then, TTE (12.9 g) and EtOH (12.8 g) were added and stirred at room temperature for another 30 minutes. Then, UPS (1.1 g) and EtOH (12.8 g) were added and stirred at room temperature for 30 minutes. Solution K8 was obtained.

[0044] <Preparation Example 1> To 60 g of the K1 solution, PGME (10 g) and EtOH (30 g) were added to obtain a solution KL1.

[0045] <Preparation Examples 2 to 7> PGME (30 g) and EtOH (10 g) were added to solutions K2 to K5 and K7 to K8 (60 g) to obtain solutions KL2 to KL5 and KL7 to KL8, respectively.

[0046] <Preparation Example 8> To the K1 solution (60 g) was added EtOH (40 g) to obtain a solution KM1.

[0047] <Preparation Example 9> To the K1 solution (60 g), HG (10 g), BCS (10 g), and IPA (20 g) were added to obtain a solution KM2.

[0048] <Preparation Example 10> To the K5 solution (60 g), PGMEA (30 g) and MeOH (10 g) were added to obtain a solution KM3.

[0049] <Preparation Example 11> To the K6 solution (20 g), PG (5 g) and MeOH (75 g) were added to obtain a solution KL6.

[0050] [Spray application] Spray coating was carried out using the following equipment and conditions. Equipment name: API-240-3D spray coater manufactured by Apiros <Coating Condition I> Nozzle height: 100mm, Y-axis pitch: 5mm, Air pressure: 560kPa, Liquid flow rate: 2cc / min, Nozzle speed: 170mm / sec <Coating Conditions II> Nozzle height: 100mm, Y-axis pitch: 5mm, Air pressure: 560kPa, Liquid flow rate: 2cc / min, Nozzle speed: 250mm / sec <Coating Condition III> Nozzle height: 100mm, Y-axis pitch: 7mm, Air pressure: 560kPa, Liquid flow rate: 4.9cc / min, Nozzle speed: 400mm / sec

[0051] [Firing conditions] The coating was dried on a hot plate at 70°C for 3 minutes and then baked in a hot air circulating oven at 200°C for 30 minutes.

[0052] [Discharge stability] When the ink could be discharged without clogging, it was rated as ◯, and when clogging occurred during application, it was rated as ×.

[0053] [HAZE, total light transmittance] A soda lime glass substrate was used, and a film was formed by spray coating under coating condition I or II. The haze and total light transmittance of the obtained substrate with the coating were measured using a haze meter HZ-V3 manufactured by Suga Test Instruments Co., Ltd.

[0054] [Surface observation] A soda-lime glass substrate was used, and a film was formed by spray coating under coating condition I or II. The obtained substrate with the film was observed with a 3D white light interference microscope Contour GT manufactured by Bruker Japan Ltd.

[0055] [Refractive index] A silicon substrate (100) was used as the substrate, and solutions KL2 to KL5, KL7 to KL8, and KM2 were spin-coated to form films so that the film thickness after baking would be 100 nm, and the films were dried on a hot plate at 70°C for 3 minutes and baked in a hot air circulating oven at 200°C for 30 minutes. The refractive index at a wavelength of 633 nm was measured using an ellipsometer (Mizojiri Optical Co., Ltd., DVA-FLVW) using the obtained substrate with the coating.

[0056] [Table 1]

[0057] As shown in Table 1, in Examples 1 to 7 and 11 to 12, ejection stability was maintained. In addition, the haze value increased, and an uneven shape was observed on the surface from the interference microscope image. This suggests that an anti-glare coating was formed. In Comparative Example 1, since the solvent (A) component was not included, the ejection stability was poor, clogging occurred in the nozzle, and film formation was difficult. In Comparative Example 2, since the solvent was at 150°C or higher, haze did not increase, and the surface was observed to be flat even in interference microscope images, and antiglare properties were not expressed.

[0058] [LR film production] KL2 to KL4 and KM3 were spray-coated on glass substrates under coating condition II to form films, thereby producing substrates with antiglare coatings. The refractive index was measured using KM3 and found to be 1.43. In addition, the haze of the substrate on which the film was formed using KM3 was 10.

[0059] On the above-mentioned antiglare coated substrate, an antireflection layer was formed by spray coating KL6 under coating condition III.

[0060] [Reflectance] Using the prepared substrate, the reflectance was measured in the wavelength range of 380 nm to 800 nm at a light incidence angle of 5° using a UV-3600 ultraviolet-visible-near infrared spectrophotometer manufactured by Shimadzu Corporation, and the average luminous reflectance was calculated from the obtained spectral reflectance curve in accordance with JIS R 3106.

[0061] [Table 2]

[0062] In Examples 8 to 10, the provision of an antireflection layer suppressed surface reflection. In Comparative Example 3, although antiglare properties were exhibited, the refractive index was low, so that the provision of an antireflection layer did not produce much of an effect of suppressing reflection. [Industrial Applicability]

[0063] By using the coating solution for forming an anti-glare film of the present invention, it is possible to provide an anti-glare film having excellent anti-glare properties (anti-glare function), which can be formed on a glass substrate, and which has a high refractive index, and a laminate having the same, which can contribute to improving the display quality of image display devices (liquid crystal displays, organic EL displays, plasma displays, etc.) provided in various devices such as televisions, personal computers, and smartphones.

Claims

1. A coating solution for forming an anti-glare coating containing the following components: Component (A): A first metal alkoxide represented by the following formula (I), its hydrolysate, or its partial condensate. R 1 m M 1 (OR 2 ) n-m (I) (In the formula, M 1 R represents at least one metal selected from the group consisting of silicon (Si), titanium (Ti), tantalum (Ta), zirconium (Zr), boron (B), aluminum (Al), magnesium (Mg), tin (Sn) and zinc (Zn). 1 is selected from a hydrogen atom, a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms, and the hydrogen atom of the hydrocarbon group may be substituted with a halogen atom, a vinyl group, a glycidoxy group, a mercapto group, a methacryloxy group, an acryloxy group, an isocyanate group, an amino group, or a ureido group, and may have a hetero atom. 2 represents an alkyl group having 1 to 5 carbon atoms, and n is M 1 represents a valence of 2 to 5; m represents M 1 When the valence is 2, it is 0 or 1, M 1 When the valence of is 3, it is 0 to 2, and M 1 When the valence of is 4, it is any one of 0 to 3, and M 1 When the valence is 5, it is any one of 0 to 4.) Component (B): A metal salt represented by the following formula (II) and M in the following formula (II) 2 A metal salt containing at least one oxalate selected from the group consisting of the above. M 2 (X) k (II) (In the formula, M 2represents at least one metal selected from the group consisting of aluminum (Al), indium (In), zinc (Zn), zirconium (Zr), bismuth (Bi), lanthanum (La), tantalum (Ta), yttrium (Y) and cerium (Ce); X represents chlorine, nitric acid, sulfuric acid, acetic acid, sulfamic acid, sulfonic acid, acetoacetic acid, acetylacetonate or a basic salt thereof; k represents M 2 Represents the valence of Solvent group (A): At least one selected from glycol ethers and derivatives thereof, or ketones, having a boiling point of less than 160°C, and at least one selected from the group consisting of ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol diethyl ether, ethylene glycol dipropyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, and methyl isobutyl ketone. Solvent group (B): at least one selected from alcohols, excluding the solvents included in the solvent group (A), and having a boiling point of 120° C. or lower. However, when the component (A) contains a titanium alkoxide, it further contains a silicon alkoxide.

2. The metal atom (M 1 ) and the metal atom (M 2 The content ratio of M) in terms of molar ratio is 0.01≦M 2 / (M 1 +M 2 2. The coating solution for forming an anti-glare film according to claim 1, wherein the coating liquid satisfies the above-mentioned formula (1).

3. The coating liquid for forming an antiglare film according to claim 1, wherein the solvent group (B) is at least one selected from the group consisting of methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, and 2-methyl-2-propanol.

4. 2. The coating liquid for forming an anti-glare film according to claim 1, wherein the content of the solvent group (A) is 5 to 70% by mass of the total solvent.

5. M of formula (I) 1 The coating solution for forming an antiglare film according to claim 1, wherein is silicon, titanium, zirconium, aluminum or tin.

6. 2. The coating liquid for forming an anti-glare film according to claim 1, wherein the component (A) is a partial condensate of silicon alkoxide, titanium alkoxide, or zirconium alkoxide.

7. M of the formula (II) 2 The coating solution for forming an antiglare film according to claim 1, wherein is aluminum, indium or cerium.

8. A method for producing an anti-glare coating, comprising applying the coating liquid for forming an anti-glare coating according to claim 1 to a substrate by spray coating.

9. An anti-glare coating film obtained from the coating liquid for forming an anti-glare coating film according to claim 1.

10. The antiglare coating according to claim 9, which has a refractive index of 1.48 to 1.

8.

11. A laminate comprising the antiglare coating according to claim 9 or 10.

12. The laminate according to claim 11, wherein the in-plane standard deviation of the haze of the laminate is 1 to 40%.

13. A laminate comprising the antiglare coating according to claim 9 or 10 and an antireflection film laminated thereon.

Citation Information

Patent Citations

  • FM stereo demodulating circuit

    JP1983039134A

  • Coating composition and production thereof

    JP1990258646A

  • Method for producing coating composition for lens of spectacles

    JP2002105398A

  • Method of manufacturing antidazzle film and method of manufacturing antidazzle antireflection film

    JP2003337204A

  • Method for manufacturing antireflective optical article and siloxane resin composition

    JP2010085579A