Coating material for electrode active material of magnesium secondary battery and magnesium secondary battery using same
A novel solid electrolyte composition with an amorphous structure addresses conductivity and stability issues in magnesium secondary batteries by preventing electrolyte decomposition at the electrode interface, thereby stabilizing the battery and enhancing its performance.
Patent Information
- Application Number
- JP2023128492
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-28
- Filing Date
- 2023-08-07
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-02-19
AI Technical Summary
Existing magnesium secondary batteries face challenges in achieving high magnesium ion conductivity and stability due to the decomposition of electrolytes at the electrode-electrolyte interface, particularly at high charging potentials.
A novel solid electrolyte composition of Mg x Zr y (P.O. z ) 2 (0
The solution enhances magnesium ion conductivity and prevents electrolyte decomposition, stabilizing the secondary battery and extending its lifespan by suppressing oxidative and reductive reactions at the electrode interface.
Smart Images

Figure 0007583414000001 
Figure 0007583414000002 
Figure 0007583414000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a solid electrolyte and a magnesium secondary battery using the same. [Background technology]
[0002] In recent years, there has been a growing expectation for the practical application of magnesium secondary batteries, which have a higher theoretical capacity density than conventional lithium-ion batteries.
[0003] Patent Document 1 discloses a solid electrolyte made of an oxide containing magnesium, silicic acid, and zirconium.
[0004] Non-Patent Document 1 discloses a solid electrolyte made of an oxide containing magnesium, phosphate, and zirconium, and reports that the conductivity of magnesium ions is improved by adding zirconium to magnesium phosphate.
[0005] Moreover, it is generally known that magnesium phosphate consisting only of crystalline portions does not provide magnesium ion conductivity. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2018-107106 A [Non-patent literature]
[0007] [Non-Patent Document 1] S. Ikeda et. al., Solid State Ionics 23 (1987) 125-129. Summary of the Invention [Problem to be solved by the invention]
[0008] The present disclosure provides a novel solid electrolyte capable of conducting magnesium ions and a secondary battery using the same.
Means for Solving the Problems
[0009] The present disclosure provides Mg x Zr y (PO z )2 (0 < x ≤ 3.5, 0 ≤ y < 1.5, 3 ≤ z ≤ 4.25), which has a composition and contains an amorphous portion, a solid electrolyte.
Advantages of the Invention
[0010] According to the present disclosure, a novel solid electrolyte capable of conducting magnesium ions and a secondary battery using the same can be provided.
Brief Description of the Drawings
[0011] [Figure 1] FIG. 1 is a cross-sectional view schematically showing a configuration example of a secondary battery according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a diagram showing an example of the configuration of a reaction apparatus for manufacturing a solid electrolyte according to an embodiment of the present disclosure. [Figure 3A] FIG. 3A is a flowchart showing an example of a method for manufacturing a solid electrolyte according to an embodiment of the present disclosure. [Figure 3B] FIG. 3B is a flowchart showing another example of a method for manufacturing a solid electrolyte according to an embodiment of the present disclosure. [Figure 3C] FIG. 3C is a flowchart showing another example of a method for manufacturing a solid electrolyte according to an embodiment of the present disclosure. [Figure 3D] FIG. 3D is a flowchart showing another example of a method for manufacturing a solid electrolyte according to an embodiment of the present disclosure. [Figure 4] FIG. 4 is a schematic cross-sectional view showing a configuration example of a secondary battery according to the first embodiment. [Diagram 5] FIG. 5 is a schematic cross-sectional view showing the configuration of Modification 1 of the secondary battery according to the first embodiment. [Figure 6] Figure 6 is a schematic cross-sectional view showing the configuration of Modification 2 of the secondary battery according to the first embodiment. [Figure 7] Figure 7 is a schematic cross-sectional view showing the configuration of Modification 3 of the secondary battery according to the first embodiment. [Figure 8] Figure 8 is a schematic cross-sectional view showing the configuration of Modification 4 of the secondary battery according to the first embodiment. [Figure 9] Figure 9 is a schematic cross-sectional view showing the configuration of Modification 5 of the secondary battery according to the first embodiment. [Figure 10] Figure 10 is a schematic cross-sectional view showing a configuration example of the secondary battery according to the second embodiment. [Figure 11] Figure 11 is a schematic cross-sectional view showing the configuration of Modification 1 of the secondary battery according to the second embodiment. [Figure 12] Figure 12 is a schematic cross-sectional view showing the configuration of Modification 2 of the secondary battery according to the second embodiment. [Figure 13] Figure 13 is a diagram showing the XRD diffraction patterns of the solid electrolytes of Examples 1 and 2. [Figure 14] Figure 14 is a diagram showing the XRD diffraction patterns of the solid electrolytes of Examples 3 and 4. [Figure 15] Figure 15 is a diagram showing the relationship between temperature and ionic conductivity for the solid electrolytes of Examples 1 to 4.
Embodiments for Carrying Out the Invention
[0012] (Overview of an Aspect According to the Present Disclosure) The solid electrolyte according to the first aspect of the present disclosure is Mg x Zr y (PO z )2 (where 0 < x ≤ 3.5, 0 ≤ y < 1.5, 3 ≤ z ≤ 4.25), and includes an amorphous portion.
[0013] According to the first aspect, a solid electrolyte exhibiting excellent magnesium ion conductivity can be realized.
[0014] In a second aspect of the present disclosure, for example, in the solid electrolyte according to the first aspect, the composition is Mg x (PO z )2 (3 ≦ x ≦ 3.5, 3 ≦ z ≦ 4.25) may be represented. According to such a configuration, a solid electrolyte exhibiting excellent magnesium ion conductivity can be realized.
[0015] In a third aspect of the present disclosure, for example, in the solid electrolyte according to the first aspect, the composition is Mg x Zr y (PO z )2 (0 < x < 3.5, 0 < y < 1.5, 3 ≦ z ≦ 4.25) may be represented. According to such a configuration, the structural stability of magnesium phosphate can be improved.
[0016] The coating material for the electrode active material of the magnesium secondary battery according to the fourth aspect of the present disclosure is a coating material for covering the electrode active material of the magnesium secondary battery, wherein the coating material contains any one of the solid electrolytes of the first to third aspects.
[0017] In a fifth aspect of the present disclosure, for example, in the coating material for the electrode active material of the magnesium secondary battery according to the fourth aspect, the electrode active material may be a positive electrode active material.
[0018] In a sixth aspect of the present disclosure, for example, in the coating material for the electrode active material of the magnesium secondary battery according to the fourth aspect, the electrode active material may be a negative electrode active material.
[0019] According to the fourth to sixth aspects, it is possible to prevent the decomposition of the electrolytic solution due to the transfer of electrons at the contact surface between the electrode and the electrolytic solution.
[0020] The electrode material of the magnesium secondary battery according to the seventh aspect of the present disclosure is electrode active material particles, a surface layer covering the electrode active material particles, and The surface layer contains the coating material for an electrode active material of a magnesium secondary battery according to the fourth embodiment.
[0021] In an eighth aspect of the present disclosure, for example, in the electrode material for the magnesium secondary battery according to the seventh aspect, the electrode active material particles may be positive electrode active material particles.
[0022] In a ninth aspect of the present disclosure, for example, in the electrode material for the magnesium secondary battery according to the seventh aspect, the electrode active material particles may be negative electrode active material particles.
[0023] The electrode layer of the magnesium secondary battery according to the tenth aspect of the present disclosure is The electrode material comprises any one of the seventh to ninth aspects.
[0024] According to the seventh to tenth aspects, the surfaces of the electrode active material particles are not exposed or are unlikely to be exposed in the gaps between the electrode active material particles, and therefore, for example, even if the gaps are filled with the electrolyte, oxidative or reductive decomposition of the electrolyte can be more effectively suppressed.
[0025] The electrode layer of the magnesium secondary battery according to the eleventh aspect of the present disclosure is an electrode active material layer including electrode active material particles; A surface layer provided on one main surface of the electrode active material layer and containing the coating material for an electrode active material of a magnesium secondary battery according to the fourth aspect; It is equipped with:
[0026] In a twelfth aspect of the present disclosure, for example, in the electrode layer of the magnesium secondary battery according to the eleventh aspect, the electrode active material particles may be positive electrode active material particles.
[0027] In a thirteenth aspect of the present disclosure, for example, in the electrode layer of the magnesium secondary battery according to the eleventh aspect, the electrode active material particles may be negative electrode active material particles.
[0028] According to the eleventh to thirteenth aspects, it is possible to prevent decomposition of the electrolyte solution caused by the transfer of electrons at the contact surface between the electrode and the electrolyte solution.
[0029] The electrode of the magnesium secondary battery according to the fourteenth aspect of the present disclosure is An electrode layer according to any one of the tenth to thirteenth aspects; a current collector supporting the electrode layer and in electrical contact with the electrode layer; It is equipped with:
[0030] According to the fourteenth aspect, the electrode can be easily manufactured.
[0031] A magnesium secondary battery according to a fifteenth aspect of the present disclosure includes: An electrode according to a fourteenth embodiment; an electrolyte solution containing a non-aqueous solvent and a magnesium salt dissolved in the non-aqueous solvent; It is equipped with:
[0032] According to the fifteenth aspect, decomposition of the electrolyte can be suppressed while maintaining the electrical characteristics of the secondary battery, resulting in a stable secondary battery with a longer life.
[0033] Hereinafter, the embodiment will be described in further detail with reference to the drawings.
[0034] The following descriptions are all comprehensive or specific examples. The numerical values, compositions, shapes, film thicknesses, electrical characteristics, secondary battery structures, electrode materials, etc. shown below are merely examples and are not intended to limit the present disclosure. In addition, components not described in the independent claims showing the highest concept are optional components.
[0035] (Embodiment) [1. Solid electrolyte] In the following, the solid electrolyte used in the secondary battery will be mainly described, but the application of the solid electrolyte of the present disclosure is not limited thereto. The solid electrolyte may be used in an electrochemical device such as an ion concentration sensor, for example.
[0036] [1-1. Configuration of Solid Electrolyte] Divalent magnesium ions have a stronger electrostatic interaction with anions in the solid electrolyte compared to monovalent lithium ions, and thus are less likely to diffuse in the solid electrolyte. Therefore, in a solid electrolyte that conducts magnesium ions, it is desirable to improve the ionic conductivity.
[0037] In contrast, the inventors of the present invention have found the following novel solid electrolyte.
[0038] The solid electrolyte according to this embodiment is Mg x Zr y (PO z )2 (where 0 < x ≤ 3.5, 0 ≤ y < 1.5, 3 ≤ z ≤ 4.25), and includes an amorphous portion.
[0039] The "solid electrolyte" in the present disclosure is not limited to those that strictly satisfy the above general formula, and also includes those that contain trace amounts of impurities in addition to the constituent elements represented by the general formula.
[0040] The "amorphous" in the present disclosure is not limited to substances that do not have a complete crystal structure, and also includes substances that have crystalline regions within the range of short-range order. An amorphous substance means, for example, a substance that does not show sharp peaks derived from crystals and shows broad peaks derived from amorphous in X-ray diffraction (XRD).
[0041] "The solid electrolyte includes an amorphous portion" means that at least a part of the solid electrolyte is amorphous. From the perspective of the conduction characteristics of magnesium ions, all of the solid electrolyte may be amorphous. When the solid electrolyte is in particle form, all of the particles made of the solid electrolyte may be amorphous. When the solid electrolyte is in thin film form, all of the thin films made of the solid electrolyte may be amorphous.
[0042] The solid electrolyte according to the present embodiment may not include a crystalline portion. The solid electrolyte according to the present embodiment may be substantially composed of an amorphous portion, or may include only an amorphous portion. This increases the spacing between the atoms and / or ions constituting the solid electrolyte. This increases the space in which the magnesium ions can move, and the electrostatic attraction that the magnesium ions receive from the surrounding ions can be further reduced. As a result, the solid electrolyte can exhibit excellent magnesium ion conduction characteristics.
[0043] For example, when the solid electrolyte is a thin film, X-ray diffraction measurement is performed at multiple arbitrary positions of the thin film. If no sharp peak is observed at any position, the solid electrolyte can be determined to be entirely amorphous, to be substantially composed of an amorphous portion, or to include only an amorphous portion.
[0044] The solid electrolyte according to this embodiment can exhibit excellent magnesium ion conductivity, which is believed to be due to the following reasons.
[0045] The solid electrolyte according to this embodiment is composed of coordination polyhedra and magnesium ions inserted between these coordination polyhedra in the short-range order region. The coordination polyhedron is basically an octahedron in which six oxygen ions are coordinated around a phosphorus atom, and the composition formula is phosphate ion (PO4) 3- However, some compounds have the formula P x O 1+3x Ions indicated by or P x O 1+3x The solid electrolyte according to the present embodiment may be present in a form in which oxygen is released from the phosphorus, and phosphorus and the remaining oxygen form a double bond. The solid electrolyte according to the present embodiment may exhibit high conductivity because it has a deficiency of atoms constituting a coordination polyhedron and / or a deficiency of magnesium atoms.
[0046] In the above general formula, x representing the composition ratio of magnesium satisfies 0 < x ≤ 3. As a result, the solid electrolyte may have a deficiency of magnesium atoms. Due to this deficiency, magnesium ions become more likely to move. Therefore, the conductivity of magnesium ions in the solid electrolyte can be improved. Also, the solid electrolyte may partially contain a magnesium oxide layer, and in this case, 0 < x ≤ 3.5 is satisfied. Due to the presence of this magnesium oxide layer, the space through which magnesium ions pass can be widened. Note that when magnesium oxide is contained at a composition ratio of 1 / 2 mol with respect to 1 mol of Mg3(PO4)2, it is assumed that x = 3.5. If more than 1 / 2 mol of magnesium oxide is contained with respect to 1 mol of Mg3(PO4)2, the conductivity of magnesium ions may decrease. Therefore, the appropriate content of magnesium oxide is 1 / 2 mol or less.
[0047] Furthermore, zirconium may be added in the above general formula within a range satisfying 0 ≤ y < 1.5. Thereby, the structure of the solid electrolyte is stabilized and the stability against temperature changes is increased. Also, since a sufficient carrier density of magnesium ions is ensured, the solid electrolyte can have excellent magnesium ion conduction characteristics. When zirconium is added, a part of the magnesium ions is substituted with zirconium ions. However, not only such a form but also a form in which zirconium oxide (ZrO2) is partially contained may be acceptable.
[0048] In the above general formula, z representing the composition ratio of oxygen satisfies 3 ≤ z ≤ 4. As a result, the solid electrolyte may have a deficiency of oxygen atoms. Due to this deficiency, the electrostatic attraction force exerted by oxygen ions on magnesium ions is weakened. Therefore, the conductivity of magnesium ions in the solid electrolyte can be improved.
[0049] z may further satisfy 4 < z ≤ 4.25. Oxygen does not necessarily form an octahedron with six-fold coordination around the phosphorus atom. For example, a part of oxygen may form magnesium oxide. As a result, a sufficient amount of oxygen vacancies can be ensured, and the amorphization of the solid electrolyte can be easily controlled. Therefore, the solid electrolyte can have excellent magnesium ion conduction characteristics, and the conductivity of magnesium ions in the solid electrolyte can be improved. When magnesium oxide is contained in a composition ratio of 1 / 2 mol per 1 mol of Mg3(PO4)2, z is assumed to be 4.25. If more than 1 / 2 mol of magnesium oxide is contained per 1 mol of Mg3(PO4)2, the conductivity of magnesium ions may decrease. Therefore, the appropriate content of magnesium oxide is 1 / 2 mol or less.
[0050] From the above, the solid electrolyte according to this embodiment is Mg x (PO z )2 (3 ≤ x ≤ 3.5, 3 ≤ z ≤ 4.25) may have a composition represented by. According to such a composition, the conductivity of magnesium ions can be more sufficiently improved.
[0051] Also, the solid electrolyte according to this embodiment is Mg x Zr y (PO z )2 (0 < x < 3.5, 0 < y < 1.5, 3 ≤ z ≤ 4.25) may have a composition represented by. According to such a composition, the structural stability of magnesium phosphate can be improved.
[0052] The solid electrolyte contains an amorphous part. As a result, the distance between the atoms and / or ions constituting the solid electrolyte increases. Thereby, the space in which magnesium ions can move expands, and the electrostatic attraction received by the magnesium ions from the surrounding ions can be reduced. As a result, the solid electrolyte can exhibit excellent magnesium ion conduction characteristics.
[0053] The solid electrolyte contains an amorphous portion, and therefore can be formed as a thin film. The thickness of the solid electrolyte may be, for example, 100 nm or more and 20 μm or less, or may be 2 μm or less. This can reduce the resistance value against the conduction of magnesium ions while suppressing the generation of pinholes in the solid electrolyte.
[0054] [1-2. Manufacturing method of solid electrolyte] The solid electrolyte of the present embodiment may be formed, for example, by a physical deposition method or a chemical deposition method. Examples of the physical deposition method include sputtering, vacuum evaporation, ion plating, and pulsed laser deposition (PLD). Examples of the chemical deposition method include atomic layer deposition (ALD), chemical vapor deposition (CVD), liquid phase film formation, sol-gel method, metal organic decomposition (MOD), spray pyrolysis (SPD), doctor blade method, spin coating, and printing technology. Examples of the CVD method include plasma CVD, thermal CVD, and laser CVD. The liquid phase film formation method is, for example, wet plating, and examples of wet plating include electrolytic plating, immersion plating, and electroless plating. Examples of the printing technology include inkjet method and screen printing. However, the method of forming the solid electrolyte is not limited to these methods.
[0055] [1-3. Secondary battery] An example of the secondary battery according to this embodiment will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view that illustrates a schematic configuration example of a secondary battery 10 according to this embodiment.
[0056] The secondary battery 10 includes a substrate 11, a positive electrode current collector 12, a positive electrode 13, a solid electrolyte 14, a negative electrode 15, and a negative electrode current collector 16. The solid electrolyte 14 may be disposed between the positive electrode 13 and the negative electrode 15, and an intermediate layer may be provided therebetween. Magnesium ions can move between the positive electrode 13 and the negative electrode 15 through the solid electrolyte 14.
[0057] The substrate 11 may be an insulating substrate or a conductive substrate. The substrate 11 may be any substrate that does not change when an inorganic layer or an organic layer is formed thereon. Examples of the substrate 11 include a glass substrate, a plastic substrate, a polymer film, a silicon substrate, a metal plate, a metal foil sheet, and a laminate of these. The substrate 11 may be a commercially available substrate or may be manufactured by a known method.
[0058] The positive electrode current collector 12 is composed of an electronic conductor that does not undergo a chemical change with the ion conductor contained in the positive electrode 13 within the range of the operating voltage of the secondary battery 10. The operating voltage of the positive electrode current collector 12 with respect to the standard redox potential of magnesium may be, for example, within the range of +2.5 V to +4.5 V. The material of the positive electrode current collector 12 is, for example, a metal or an alloy. More specifically, the material of the positive electrode current collector 12 may be a metal or an alloy containing at least one metal element selected from the group consisting of copper, chromium, nickel, titanium, platinum, gold, aluminum, tungsten, iron, and molybdenum. The material of the positive electrode current collector 12 may be, for example, aluminum, an aluminum alloy, platinum, or gold in terms of electrical conductivity, resistance to ion conductors, and redox potential.
[0059] The positive electrode current collector 12 may be formed of a transparent conductive film. Examples of the transparent conductive film include indium tin oxide (ITO), indium zinc oxide (IZO), fluorine-doped tin oxide (FTO), antimony-doped tin oxide (ATO), indium oxide (In2O3), tin oxide (SnO2), and Al-containing ZnO.
[0060] The positive electrode current collector 12 may be a laminated film in which the above-mentioned metals and / or transparent conductive films are laminated.
[0061] The positive electrode 13 contains a positive electrode active material capable of absorbing and releasing magnesium ions. Examples of the positive electrode active material include metal oxides, polyanion salt compounds, sulfides, chalcogenide compounds, and hydrides. Examples of metal oxides include transition metal oxides and magnesium composite oxides. Examples of transition metal oxides include V2O5, MnO2, and MoO3. Examples of magnesium composite oxides include MgCoO2 and MgNiO2. Examples of polyanion salt compounds include MgCoSiO4, MgMnSiO4, MgFeSiO4, MgNiSiO4, MgCo2O4, and MgMn2O4. Examples of sulfides include Mo6S8. Examples of chalcogenide compounds include Mo9Se 11 Examples include:
[0062] The positive electrode active material is, for example, crystalline. Positive electrode 13 may contain two or more types of positive electrode active materials.
[0063] The positive electrode 13 may contain a conductive material and / or a binder, if necessary.
[0064] The conductive material is not particularly limited as long as it is an electron conductive material. Examples of the conductive material include carbon materials, metals, and conductive polymers. Examples of the carbon material include graphite, acetylene black, carbon black, ketjen black, carbon whiskers, needle coke, and carbon fibers. Examples of graphite include natural graphite and artificial graphite. Examples of natural graphite include lump graphite and flake graphite. Examples of metals include copper, nickel, aluminum, silver, and gold. These materials may be used alone or in combination. The material of the conductive material may be, for example, carbon black or acetylene black from the viewpoints of electron conductivity and coatability.
[0065] The binder is not particularly limited as long as it plays a role in binding the active material particles and the conductive material particles. Examples of the binder include fluorine-containing resin, thermoplastic resin, ethylene propylene diene monomer (EPDM) rubber, sulfonated EPDM rubber, and natural butyl rubber (NBR). Examples of the fluorine-containing resin include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), and fluororubber. Examples of the thermoplastic resin include polypropylene and polyethylene. These materials may be used alone or in combination. The binder may be, for example, a water dispersion of cellulose or styrene butadiene rubber (SBR).
[0066] Examples of the solvent for dispersing the positive electrode active material, the conductive material, and the binder include N-methylpyrrolidone, dimethylformamide, dimethylacetamide, methyl ethyl ketone, cyclohexanone, methyl acetate, methyl acrylate, diethylenetriamine, N,N-dimethylaminopropylamine, ethylene oxide, and tetrahydrofuran. For example, a thickener may be added to the dispersant. Examples of the thickener include carboxymethylcellulose and methylcellulose.
[0067] The positive electrode 13 is formed, for example, as follows. First, a positive electrode active material, a conductive material, and a binder are mixed. Next, a suitable solvent is added to this mixture, thereby obtaining a paste-like positive electrode material. Next, this positive electrode material is applied to the surface of a positive electrode current collector and dried. In this way, the positive electrode 13 is obtained. The positive electrode material may be compressed to increase the electrode density.
[0068] The positive electrode 13 may be in the form of a thin film. The thickness of the positive electrode 13 may be, for example, 500 nm or more and 20 μm or less.
[0069] The solid electrolyte 14 is the same as the solid electrolyte described above, and therefore a description thereof will be omitted.
[0070] The negative electrode 15 contains a negative electrode active material capable of absorbing and releasing magnesium ions. Examples of the negative electrode active material include metals, alloys, sulfides, carbon, organic compounds, inorganic compounds, metal complexes, and organic polymer compounds. Examples of metals include magnesium, tin, bismuth, and antimony. The alloy is, for example, an alloy of magnesium and at least one selected from aluminum, silicon, gallium, zinc, tin, manganese, bismuth, and antimony.
[0071] Negative electrode 15 may contain two or more types of negative electrode active materials.
[0072] The negative electrode 15 may contain a conductive material and / or a binder, as necessary. The conductive material, binder, solvent, and thickener in the negative electrode 15 may be the same as those described for the positive electrode 13.
[0073] The negative electrode 15 may be in the form of a thin film. The thickness of the negative electrode 15 may be, for example, 500 nm or more and 20 μm or less.
[0074] The negative electrode current collector 16 is composed of an electronic conductor that does not undergo chemical change with the ionic conductor contained in the negative electrode 15 within the range of the operating voltage of the secondary battery 10. The operating voltage of the negative electrode current collector 16 with respect to the standard reduction potential of magnesium may be within the range of, for example, 0 V to +1.5 V. The material of the negative electrode current collector 16 may be any of those described for the positive electrode current collector 12.
[0075] The positive electrode current collector 12, the positive electrode 13, the solid electrolyte 14, the negative electrode 15, and the negative electrode current collector 16 can each be formed by the chemical deposition method or the physical deposition method described above.
[0076] The shape of the secondary battery 10 in a top view may be, for example, rectangular, circular, elliptical, or hexagonal. The structure of the secondary battery 10 may be cylindrical, square, button, coin, or flat.
[0077] Various embodiments of the solid electrolyte and the method for manufacturing the solid electrolyte are exemplified below. The materials, compositions, film thicknesses, shapes, properties, steps of the manufacturing method, and the order of these steps shown in the present disclosure are merely examples. Multiple steps of the manufacturing method may be performed simultaneously or at different times.
[0078] [2. Manufacturing equipment] 2 shows an example of the configuration of a manufacturing apparatus 21 for forming a solid electrolyte membrane by the ALD method according to one embodiment. The manufacturing apparatus 21 includes a reactor 22, a controller 35, a first precursor supply unit 23, a second precursor supply unit 24, a third precursor supply unit 25, an oxygen supply unit 33, and a purge gas supply unit 34.
[0079] The reactor 22 is, for example, a process chamber.
[0080] The first precursor supply unit 23 supplies a first precursor into the reactor 22. The first precursor contains magnesium. The first precursor supply unit 23 is, for example, a bottle that stores the first precursor.
[0081] The second precursor supply unit 24 supplies a second precursor into the reactor 22. The second precursor contains phosphorus that constitutes phosphoric acid. The second precursor supply unit 24 is, for example, a bottle that stores the second precursor.
[0082] The third precursor supply unit 25 supplies a third precursor into the reactor 22. The third precursor contains zirconium. The third precursor supply unit 25 is, for example, a bottle that stores the third precursor.
[0083] The manufacturing apparatus 21 includes a first pipe P1 extending from a first precursor supply unit 23 to the reactor 22, a second pipe P2 extending from a second precursor supply unit 24 to the reactor 22, and a third pipe P3 extending from a third precursor supply unit 25 to the reactor 22.
[0084] The oxygen supply unit 33 supplies any one of oxygen gas, HO gas, and ozone gas, or a combination of these gases, into the reactor 22. The purge gas supply unit 34 supplies a purge gas into the reactor 22, thereby purging gas remaining in the reactor 22 and adjusting the degree of vacuum in the reactor 22.
[0085] The manufacturing apparatus 21 shown in FIG. 2 further includes auxiliary gas supply units 27 to 32, mass flow controllers 26a to 26e, valves V1 to V8, manual valves MV1 to MV3, and a needle valve NV.
[0086] The controller 35 controls, for example, the valves V1 to V8 and the mass flow controllers 26a to 26e. The controller 35 includes, for example, a memory and a processor. The controller 35 includes, for example, a semiconductor device, a semiconductor integrated circuit (IC), an LSI (large scale integration), or an electronic circuit that is a combination of these. The LSI or IC may be integrated into one chip, or multiple chips may be combined. For example, each functional block may be integrated into one chip. The LSI or IC may be called, for example, a system LSI, a VLSI (very large scale integration), or a ULSI (ultra large scale integration) depending on the degree of integration.
[0087] Commercially available products can be applied depending on the type of the target solid electrolyte membrane as the manufacturing apparatus 21. Examples of commercially available manufacturing apparatuses include Savannah Systems, Fiji Systems, and Phoenix Systems (all manufactured by Ultratech / Cambridge NanoTech), ALD-series (manufactured by Showa Shinku Co., Ltd.), TFS 200, TFS 500, TFS 120P400A, and P800 (all manufactured by Beneq), OpAL and FlexAL (all manufactured by Oxford Instruments), InPassion ALD 4, InPassion ALD 6, and InPassion ALD 8 (all manufactured by SoLay Tec), AT-400 ALD System (manufactured by ANRIC TECHNOLOGIES), and LabNano and LabNano-PE (all manufactured by Ensure NanoTech). When a commercially available product is used as the manufacturing apparatus 21, for example, a program for executing the various flows described below can be stored in the memory of the controller 35, and the processor in the controller 35 can be made to execute this program, thereby forming the manufacturing apparatus 21 according to this embodiment.
[0088] [3. Manufacturing method] In the following, as an example of the method for producing a solid electrolyte membrane according to the present embodiment, a method for producing the solid electrolyte membrane using the production apparatus 21 will be described. Note that the solid electrolyte membrane and the production method thereof in the present disclosure are not limited to a specific production apparatus. Each step of the production method in the present disclosure may be performed based on a predetermined program stored in the production apparatus, or may be performed by manually operating the production apparatus.
[0089] [3-1. Overall flow] 3A is a flow chart showing an example of a method for producing a solid electrolyte membrane according to an embodiment. The method shown in FIG. 3A includes a step S1 of supplying a first precursor containing magnesium into the reactor 22, a step S2 of supplying any one of oxygen gas, H2O gas, and ozone gas, or a combination thereof, into the reactor 22, a step S3 of supplying a second precursor containing phosphorus into the reactor 22, and a step S4 of supplying any one of oxygen gas, H2O gas, and ozone gas, or a combination thereof, into the reactor 22. This method further includes, for example, a step of supplying a purge gas into the reactor 22. In addition, in the supply of oxygen in the steps S2 and S4, each gas may be turned into plasma.
[0090] The order, timing, and number of times each step is performed are not particularly limited. For example, the flow shown in FIG. 3A may be repeatedly performed. For example, multiple steps may be performed simultaneously. For example, step S1 is performed at least once before step S2 or S4. For example, steps S1 and S3 are performed in different periods.
[0091] In the case of the sequence shown in FIG. 3A, in step S2, a first precursor is oxidized in step S2. This results in magnesium oxide. In step S3, a phosphorus-containing precursor is bonded onto the magnesium oxide. In step S4, the phosphorus precursor is oxidized. This results in a solid electrolyte membrane.
[0092] Alternatively, step S2 may be omitted, and the precursors supplied in steps S1 and S3 may be oxidized simultaneously in step S4.
[0093] [3-2. Preparation] Before starting the production of the solid electrolyte membrane, a substrate is placed in the reactor 22 .
[0094] Examples of the substrate material include metal, metal oxide, resin, glass, and ceramics. The metal may be, for example, Au. The metal oxide may be, for example, a metal composite oxide. Examples of the resin include polyester, polycarbonate, fluororesin, and acrylic resin. Examples of the glass include soda-lime glass and quartz glass. Examples of the ceramic include aluminum oxide, silicon, gallium nitride, sapphire, and silicon carbide. For example, a thermal oxide film (SiO2) having a thickness of 400 nm may be formed on a Si substrate.
[0095] The temperature inside the reactor 22 is not particularly limited, and may be 100° C. or more and 500° C. or less, or 120° C. or more and 300° C. or less. By setting the temperature inside the reactor 22 to 500° C. or less, film formation proceeds well. When the first precursor and / or the second precursor contains carbon, the precursor can be appropriately oxidized by setting the temperature inside the reactor 22 to 100° C. or more.
[0096] [3-3. Supply of the first precursor] In step S1, a first precursor containing magnesium is supplied into the reactor 22. For example, in FIG.
[0097] The temperature of the first precursor supply part 23 is not particularly limited, and may be 50° C. or higher and 190° C. or lower when the vapor pressure of the first precursor is low.
[0098] In step S1, the manual valve MV1 may be opened to supply an auxiliary gas from the auxiliary gas supply unit 27 toward the reactor 22. The auxiliary gas pushes the first precursor released from the first precursor supply unit 23 into the first pipe P1 into the reactor 22. The flow rate of the auxiliary gas is not particularly limited, and may be 20 ml / min or more and 60 ml / min or less, or 30 ml / min or more and 55 ml / min or less.
[0099] In step S1, depending on the type of the first precursor, the valve V2 may be opened to supply an auxiliary gas from the auxiliary gas supply unit 28 to the reactor 22. The auxiliary gas pushes the first precursor into the reactor 22. The flow rate of this auxiliary gas may be controlled by the mass flow controller 26a. The flow rate of this auxiliary gas is not particularly limited, and may be 1 ml / min or more and 30 ml / min or less, or 5 ml / min or more and 20 ml / min or less.
[0100] The temperature of the auxiliary gas supplied from the auxiliary gas supply units 27, 28 is not particularly limited, and may be 50°C or higher and 300°C or lower, or 100°C or higher and 280°C or lower.
[0101] In step S1, the flow rate of the first precursor may be controlled by adjusting the opening of the needle valve NV, for example, from 10 to 60%.
[0102] The auxiliary gas supplied from the auxiliary gas supply units 27 and 28 may be the same as that exemplified in the description of step S1.
[0103] The first precursor is not particularly limited, and examples thereof include bis(cyclopentadienyl)magnesium (Cp2Mg), bis(methylcyclopentadienyl)magnesium (MeCp2Mg), and bis(ethylcyclopentadienyl)magnesium (EtCp2Mg). These may be used alone or in combination of two or more.
[0104] Step S1 is terminated by closing valve V1. The duration of step S1 corresponds to, for example, the time from when valve V1 is opened to when it is closed. Step S1 is not particularly limited, and may be about 0.01 seconds or more and 10 seconds or less, about 0.05 seconds or more and 8 seconds or less, or about 0.1 seconds or more and 5 seconds or less.
[0105] [3-4. Oxygen supply] In step S2, any one of oxygen gas, HO gas, and ozone gas, or a combination thereof is supplied into the reactor 22. For example, in FIG. 2, the valve V7 is opened to supply any one of oxygen gas, HO gas, and ozone gas, or a combination thereof from the oxygen supply unit 33 into the reactor 22.
[0106] The oxygen gas and H2O gas may contain oxygen radicals generated by, for example, plasma processing. Plasma ALD can increase reactivity and lower the temperature of the system.
[0107] Ozone gas may be generated, for example, by supplying oxygen gas to an OT-020 ozone generator (manufactured by Ozone Technology).
[0108] The flow rate of any one of oxygen gas, HO gas, and ozone gas, or a combination of these gases, is controlled by a mass flow controller 26d, and may be, for example, 20 to 60 ml / min, or 30 to 50 ml / min. The concentration of any one of oxygen gas, HO gas, and ozone gas, or a combination of these gases is not particularly limited, and may be, for example, 100%. The temperature of any one of oxygen gas, HO gas, and ozone gas, or a combination of these gases is not particularly limited, and may be, for example, 50°C to 300°C, or 100°C to 280°C.
[0109] Step S2 is terminated by closing valve V7. The duration of step S2 corresponds to the time from when valve V7 is opened to when it is closed. The duration of step S2 is not particularly limited, and may be about 0.1 to 15 seconds, about 0.2 to 10 seconds, or about 0.2 to 8 seconds.
[0110] [3-5. Supply of the second precursor] In step S3, a second precursor containing a network former is supplied into the reactor 22. For example, in FIG.
[0111] The temperature of the second precursor supply part 24 is not particularly limited, and may be 1° C. or higher and 60° C. or lower, or 5° C. or higher and 50° C. or lower, when the vapor pressure of the second precursor is high.
[0112] In step S3, the manual valve MV2 may be opened to supply an auxiliary gas from the auxiliary gas supply unit 29 toward the reactor 22. The auxiliary gas pushes the second precursor released from the second precursor supply unit 24 into the second pipe P2 into the reactor 22. The flow rate of this auxiliary gas is not particularly limited and may be 20 ml / min or more and 60 ml / min or less, or 25 ml / min or more and 50 ml / min or less. In step S3, the flow rate of the second precursor may be controlled by adjusting the aperture of the needle valve NV. The aperture of the needle valve NV is, for example, 10 to 60%.
[0113] In step S3, depending on the type of the second precursor, the valve V4 may be opened to supply an auxiliary gas from the auxiliary gas supply unit 30 to the reactor 22. The auxiliary gas pushes the second precursor into the reactor 22. The flow rate of this auxiliary gas may be controlled by the mass flow controller 26b. The temperature of the auxiliary gas supplied from the auxiliary gas supply units 29 and 30 is not particularly limited and may be 100°C or higher and 300°C or lower, or 120°C or higher and 280°C or lower.
[0114] The auxiliary gas is, for example, an inert gas. Examples of the inert gas include argon gas and nitrogen gas. The auxiliary gas may be one type of gas or a mixture of two or more types of gases.
[0115] The network former means an atom or a group of atoms (i.e., radicals) that can form a network structure by bonding directly or indirectly to each other, or that already form a network structure. The network structure is the framework of the oxide. The network former may be, for example, a part of a molecule that constitutes the second precursor, and the other part of the molecule may be cleaved off when the network structure is formed. The network former contains phosphorus.
[0116] The second precursor is not particularly limited, and may be, for example, a phosphorus-containing compound. Examples of the phosphorus-containing compound include tris(dimethylamino)phosphine (TDMAP), trimethylphosphine (TMP), triethylphosphine (TEP), and tert-butylphosphine (TBP). These may be used alone or in combination of two or more.
[0117] Step S3 is terminated by closing valve V3. The duration of step S3 is not particularly limited, and may be about 0.01 seconds or more and 10 seconds or less, about 0.05 seconds or more and 8 seconds or less, or about 0.1 seconds or more and 5 seconds or less.
[0118] [3-6. Oxygen supply] In step S4, any one of oxygen gas, H2O gas, and ozone gas, or a combination of these gases, is supplied into the reactor 22. The gas types and method are the same as those in step S2, so a description thereof will be omitted.
[0119] [3-7. Supply of purge gas] In steps S11 to S14 of supplying a purge gas, the purge gas is supplied into the reactor 22, thereby purging gas remaining in the reactor 22. For example, in FIG. 2, the valve V8 is opened to supply the purge gas from the purge gas supply unit 34 into the reactor 22.
[0120] The flow rate of the purge gas is controlled by the mass flow controller 26e and may be, for example, 20 ml / min to 60 ml / min, or 30 ml / min to 50 ml / min. The temperature of the purge gas is not particularly limited and may be 100°C to 300°C, or 120°C to 280°C.
[0121] The purging steps S11 to S14 may be performed, for example, each time each of the steps S1 to S4 is completed, or each time a specific step among the steps S1 to S4 is completed. Alternatively, the purging steps S11 to S14 may be performed simultaneously with at least one of the steps S1 to S4. For example, in order to sufficiently exhaust gas in the reactor 22, the purging steps may be continuously performed as a background process from the start to the end of the formation of the solid electrolyte membrane.
[0122] The duration of each of the purge steps S11 to S14 is not particularly limited, and may be about 0.1 seconds to 60 seconds, or about 5 seconds to 30 seconds.
[0123] The purge gas is, for example, an inert gas. Examples of the inert gas include argon gas and / or nitrogen gas. The purge gas may be one type of gas or a mixture of two or more types of gases.
[0124] [3-8. Reactor vacuum level and piping temperature] In the method for producing a solid electrolyte membrane according to this embodiment, the degree of vacuum may be controlled within the reactor 22. For example, in FIG. 2, the degree of vacuum within the reactor 22 can be controlled by adjusting the opening of the exhaust manual valve MV4.
[0125] The degree of vacuum can be set according to the type of solid electrolyte membrane. For example, it may be 0.1 Torr or more and 8.0 Torr or less, or 0.5 Torr or more and 5.0 Torr or less. By setting the degree of vacuum to 0.1 Torr or more, for example, the first precursor is continuously supplied into the reactor 22, and the first precursor is sufficiently oxidized. Therefore, for example, when the first precursor contains carbon, the amount of carbon in the solid electrolyte membrane can be reduced by sufficient oxidation. By setting the degree of vacuum to 8.0 Torr or less, for example, the supply amount of the second precursor can be appropriately controlled. The degree of vacuum of the reactor can be measured, for example, by a Pirani gauge (TPR280 DN16 ISO-KF: manufactured by PFEIFFER VACUUM).
[0126] In the method for manufacturing a solid electrolyte membrane according to this embodiment, the temperature of each pipe may be set, for example, as follows.
[0127] 2, the temperature of the first pipe P1 and the temperature of the second pipe P2 are set to be higher than the boiling point or sublimation temperature of the first precursor and higher than the boiling point or sublimation temperature of the second precursor. For example, when the first precursor is bis(ethylcyclopentadienyl)magnesium, the boiling point is about 65° C. When the second precursor is tris(dimethylamino)phosphine, the boiling point is about 48 to 50° C.
[0128] For example, the temperature of the first pipe P1 and the temperature of the second pipe P2 are higher than the temperature of the first precursor supply part 23 and higher than the temperature of the second precursor supply part 24. This makes it possible to prevent the first precursor from solidifying in the first pipe P1 and to prevent the second precursor from solidifying in the second pipe P2.
[0129] The temperature of the first pipe P1 and the temperature of the second pipe P2 may be 55° C. or more higher than the temperature of the first precursor supply part 23 and 55° C. or more higher than the temperature of the second precursor supply part 24. The temperature of the first pipe P1 and the temperature of the second pipe P2 may be 60° C. or more higher than the temperature of the first precursor supply part 23 and 60° C. or more higher than the temperature of the second precursor supply part 24.
[0130] For example, when the temperature of the first precursor supply part 23 is 60°C and the temperature of the second precursor supply part 24 is 40°C, the temperatures of the first pipe P1 and the second pipe P2 may be set to about 180°C.
[0131] [3-9. Manufacturing method of magnesium phosphate membrane] FIG. 3B is a flowchart showing an example of a method for producing a solid electrolyte membrane according to an embodiment. The method shown in FIG. 3B includes a step S1 of supplying a first precursor into the reactor 22, a step S2 of supplying oxygen gas, H2O gas, and ozone gas, or a combination thereof, into the reactor 22, a step S3 of supplying a second precursor into the reactor 22, a step S4 of supplying oxygen gas, H2O gas, and ozone gas, or a combination thereof, steps S11 to S14 of supplying a purge gas into the reactor 22, and a step S5 of determining whether the number of repetitions has reached a predetermined set value. As a result, a cycle including steps S1 to S5 and S11 to S14 is repeated multiple times. In FIG. 3B, the description of the items described with reference to FIG. 3A may be omitted.
[0132] In the manufacturing method shown in FIG. 3B, after steps S1 to S4 are completed, purging steps S11 to S14 are performed, respectively.
[0133] 3B, in step S5, it is determined whether the number of repetitions has reached a set number. If the number of repetitions has not reached the predetermined set value (NO in step S5), the process returns to step S1. If the number of repetitions has reached the predetermined set value (YES in step S5), the formation of the solid electrolyte membrane is completed.
[0134] The number of cycle repetitions is not particularly limited and is appropriately set depending on, for example, the thickness of the target solid electrolyte membrane, the type of the first precursor, and the type of the second precursor. The number of cycle repetitions may be, for example, about 2 to 8000, or about 5 to 3000. For example, when the thickness of the solid electrolyte membrane is set to about 500 nm, the number of cycle repetitions may be set to 1000 to 3000. Alternatively, when the thickness of the solid electrolyte membrane is set to 50 nm or less, the number of cycle repetitions may be set to 300 or less.
[0135] The thickness of the solid electrolyte membrane according to the present embodiment is not particularly limited. The thickness of the solid electrolyte membrane may be, for example, 5 μm or less, 2 μm or less, 550 nm or less, or 300 nm or less. The thickness of the solid electrolyte membrane may be, for example, 200 nm or less, 150 nm or less, 110 nm or less, 100 nm or less, or 50 nm or less. The lower limit of the thickness of the solid electrolyte membrane is not particularly limited, and may be 0.1 nm or 1 nm.
[0136] In the example shown in Fig. 3B, steps S1 to S4 are each performed once in one cycle. However, the number of times each step is performed in one cycle is not limited to this. In addition, the number of times and timing of performing the purge step are not limited to the example shown in Fig. 3B.
[0137] Whether to continue or terminate the formation of the solid electrolyte membrane may be determined based on a condition other than the number of repetitions. For example, the formation of the solid electrolyte membrane may be terminated when the elapsed time reaches a predetermined value, or when the thickness of the solid electrolyte membrane reaches a predetermined value.
[0138] The composition ratio of each element in the solid electrolyte film can be controlled, for example, by the flow rate of the first precursor, the duration of the pulse of the first precursor, the flow rate of the second precursor, the duration of the pulse of the second precursor, and the duration of the pulse of the purge gas. The composition ratio of each element in the solid electrolyte film may be controlled, for example, by setting the amount of the precursor with the lowest vapor pressure and setting the flow rates and pulse durations of the other elements based on this.
[0139] Furthermore, as shown in FIG. 3C, after the number of repetitions reaches a set value in step S5, steps S1 to S12 may be performed.
[0140] [3-10. Manufacturing method of magnesium phosphate membrane with added zirconium] Fig. 3D is a flow chart showing an example of a method for producing a solid electrolyte membrane according to an embodiment. In the production method shown in Fig. 3D, an example of a production method for a magnesium phosphate membrane to which zirconium is added is described. Note that the description of the matters described with reference to Figs. 3A to 3C may be omitted.
[0141] Since the steps other than the supply of the third precursor in step SS3 are similar to those described with reference to FIGS. 3A to 3C, only the supply of the third precursor in step SS3 will be described.
[0142] In step SS3, a third precursor containing zirconium is supplied into the reactor 22. For example, in FIG.
[0143] The temperature of the third precursor supply part 25 is not particularly limited, and may be 50° C. or higher and 190° C. or lower when the vapor pressure of the third precursor is low.
[0144] In step SS3, the manual valve MV3 may be opened to supply an auxiliary gas from the auxiliary gas supply unit 31 toward the reactor 22. The auxiliary gas pushes the third precursor released from the third precursor supply unit 25 into the third pipe P3 into the reactor 22. The flow rate of the auxiliary gas is not particularly limited, and may be 20 ml / min or more and 60 ml / min or less, or 30 ml / min or more and 55 ml / min or less.
[0145] In step SS3, depending on the type of the third precursor, the valve V6 may be opened to supply an auxiliary gas from the auxiliary gas supply unit 32 to the reactor 22. The auxiliary gas pushes the third precursor into the reactor 22. The flow rate of this auxiliary gas may be controlled by the mass flow controller 26c. The flow rate of this auxiliary gas is not particularly limited, and may be 1 ml / min or more and 30 ml / min or less, or 5 ml / min or more and 20 ml / min or less.
[0146] The temperature of the auxiliary gas supplied from the auxiliary gas supply parts 31 and 32 is not particularly limited, and may be 50° C. or higher and 300° C. or lower, or 100° C. or higher and 280° C. or lower.
[0147] In step SS3, the flow rate of the third precursor may be controlled by adjusting the opening of the needle valve NV, for example, from 10 to 60%.
[0148] The auxiliary gas supplied from the auxiliary gas supply units 31 and 32 may be the same as that exemplified in the description of step S1.
[0149] The third precursor is not particularly limited, and examples thereof include tetrabutoxyzirconium, tetrakisethylmethylaminozirconium, and tetraethoxyzirconium. These may be used alone or in combination of two or more.
[0150] Step SS3 is terminated by closing valve V5. The duration of step SS3 corresponds to, for example, the time from when valve V5 is opened to when it is closed. Step SS3 is not particularly limited, and may be about 0.01 seconds or more and 10 seconds or less, about 0.05 seconds or more and 8 seconds or less, or about 0.1 seconds or more and 5 seconds or less.
[0151] Fig. 3D is a flow chart showing an example of a method for manufacturing a solid electrolyte membrane according to the embodiment. The manufacturing method shown in Fig. 3D includes a step SS1 of supplying a first precursor into the reactor 22, a step SS2 of supplying oxygen gas, H2O gas, and ozone gas, or a combination thereof, into the reactor 22, a step SS3 of supplying a third precursor into the reactor 22, a step SS4 of supplying oxygen gas, H2O gas, and ozone gas, or a combination thereof, a step SS5 of supplying a second precursor into the reactor 22, a step SS6 of supplying oxygen gas, H2O gas, and ozone gas, or a combination thereof, steps SS11 to SS16 of supplying a purge gas into the reactor 22, and a step SS7 of determining whether the number of repetitions has reached a predetermined set value. Thus, a cycle including steps SS1 to SS7 and SS11 to SS16 is repeated multiple times. In FIG. 3D, the description of the matters described with reference to FIGS. 3A to 3C may be omitted.
[0152] In the manufacturing method shown in FIG. 3D, after steps SS1 to SS6 are completed, purge steps SS11 to SS16 are performed, respectively.
[0153] In the example shown in Fig. 3D, it is determined whether the number of repetitions reaches a set number in step SS7. If the number of repetitions does not reach the predetermined set value (NO in step SS7), the process returns to step SS1, and if the number of repetitions reaches the predetermined set value (YES in step SS7), the formation of the solid electrolyte membrane is completed.
[0154] The number of cycle repetitions is not particularly limited and is appropriately set depending on, for example, the intended thickness of the solid electrolyte membrane and the types of the first to third precursors. The number of cycle repetitions may be, for example, about 2 to 8000, or about 5 to 3000. For example, when the thickness of the solid electrolyte membrane is set to about 500 nm, the number of cycle repetitions may be set to 1000 to 3000. Alternatively, when the thickness of the solid electrolyte membrane is set to 50 nm or less, the number of cycle repetitions may be set to 300 or less.
[0155] The thickness of the solid electrolyte membrane according to the present embodiment is not particularly limited. The thickness of the solid electrolyte membrane may be, for example, 5 μm or less, 2 μm or less, 550 nm or less, or 300 nm or less. The thickness of the solid electrolyte membrane may be, for example, 200 nm or less, 150 nm or less, 110 nm or less, 100 nm or less, or 50 nm or less. The lower limit of the thickness of the solid electrolyte membrane is not particularly limited, and may be 0.1 nm or 1 nm.
[0156] In the example shown in Fig. 3D, steps SS1 to SS6 are each performed once in one cycle. However, the number of times each step is performed in one cycle is not limited to this. In addition, the number of times and timing of performing the purge step are not limited to the example shown in Fig. 3D.
[0157] Whether to continue or terminate the formation of the solid electrolyte membrane may be determined based on a condition other than the number of repetitions. For example, the formation of the solid electrolyte membrane may be terminated when the elapsed time reaches a predetermined value, or when the thickness of the solid electrolyte membrane reaches a predetermined value.
[0158] The composition ratio of each element in the solid electrolyte film can be controlled by, for example, the flow rate of the first precursor, the duration of the pulse of the first precursor, the flow rate of the second precursor, the duration of the pulse of the second precursor, the flow rate of the third precursor, the duration of the pulse of the third precursor, and the duration of the pulse of the purge gas. The composition ratio of each element in the solid electrolyte film may be controlled, for example, by setting the amount of the precursor with the lowest vapor pressure and setting the flow rates and pulse durations of the other elements based on this.
[0159] Furthermore, similarly to FIG. 3C, after the number of repetitions in step SS7 reaches a set value, steps SS1 to SS12, or steps SS1 to SS14 may be performed.
[0160] Regarding the temperature settings of the piping and precursor supplying parts, for example, when the temperature of the first precursor supplying part 23 is 60°C, the temperature of the second precursor supplying part 24 is 40°C, and the temperature of the third precursor supplying part 25 is 50°C, the temperatures of the first pipe P1, the second pipe P2, and the third pipe P3 may be set to approximately 180°C.
[0161] [4. Solid electrolyte membrane] An example of the structure of the solid electrolyte membrane according to the present embodiment will be described. Note that the solid electrolyte membrane according to the present embodiment may be manufactured by, for example, the manufacturing method described above.
[0162] The solid electrolyte membrane according to this embodiment contains a network former containing phosphorus and magnesium.
[0163] The solid electrolyte membrane according to this embodiment has an amorphous structure, and is characterized by the absence of specific peaks indicating crystal growth in analysis using an X-ray diffraction device (XRD). This expands the space through which magnesium ions pass, improving the conductivity of magnesium ions.
[0164] Furthermore, the solid electrolyte membrane according to the present embodiment may contain zirconium in addition to the phosphorus-containing network former and magnesium, which improves the stability of the material and suppresses decomposition due to heat or application of voltage.
[0165] [4-1. Secondary battery] The solid electrolyte membrane according to the present embodiment can be used as a solid electrolyte for a secondary battery. For example, the secondary battery according to the present embodiment includes a positive electrode, a negative electrode, and a solid electrolyte containing the above-mentioned oxynitride. The positive electrode includes a positive electrode current collector and a positive electrode active material. The negative electrode includes a negative electrode current collector and a negative electrode active material.
[0166] The secondary battery may be, for example, an all-solid-state secondary battery. In this case, a solid electrolyte membrane may be sandwiched between a positive electrode and a negative electrode. By applying a voltage between the positive electrode and the negative electrode, ion conduction occurs in the solid electrolyte membrane. The current collector material of the positive electrode and the negative electrode may be a material having electrical conductivity. Examples of the material having electrical conductivity include metals. Examples of the metals include Au, Pt, Al, Ag, Cu, Mg, Ni, Ti, and Fe. Examples of the material having electrical conductivity include alloys containing at least one of the above metals. Examples of the alloys include Au-Mg alloys, Ca-Mg alloys, Mg-Ni alloys, Ca-Ni alloys, Mg-Zn alloys, and Al-Mg alloys.
[0167] In the secondary battery, the solid electrolyte may be only a solid electrolyte membrane, or may be a laminate in which a solid electrolyte membrane is laminated with other membranes. Examples of other membranes include sulfides and halides. The solid electrolyte does not have to be a membrane, and may be, for example, a powder. Therefore, what is described as a "solid electrolyte membrane" in this embodiment can be appropriately read as an explanation of an "oxide."
[0168] In this embodiment, the coating material for electrode active material of magnesium secondary battery is a material for coating the electrode active material. The coating material for electrode active material of magnesium secondary battery has a solid electrolyte containing magnesium phosphate or magnesium phosphate with added zirconium, as represented by the above general formula. This makes it possible to prevent decomposition of the electrolyte due to electron transfer at the contact surface between the electrode and the electrolyte.
[0169] The positive electrode may have an uneven surface, and the solid electrolyte may be a coating covering the uneven surface. The negative electrode may have an uneven surface, and the solid electrolyte may be a coating covering the uneven surface. This allows the contact area between the electrode and the solid electrolyte to be increased, and the reaction between the electrode and the solid electrolyte to be activated. The coating of the solid electrolyte is formed, for example, by the above-mentioned ALD, so that it has a conformal shape that follows the uneven surface. This allows the formation of a solid electrolyte with less process variation. At least one of the positive electrode and the negative electrode may have, for example, a porous shape, and the solid electrolyte may have a shape that follows the uneven surface caused by this porosity.
[0170] For example, the positive electrode active material may be made of active material particles, and the solid electrolyte may be a coating covering the surfaces of each of the active material particles. The negative electrode active material may be made of active material particles, and the solid electrolyte may be a coating covering the surfaces of each of the active material particles. This makes it possible to increase the contact area between the active material and the solid electrolyte, and to activate the reaction between the active material and the solid electrolyte. For example, according to the above-mentioned ALD, in each process, the raw material gas can penetrate between the active material particles, and thus a solid electrolyte film covering the surfaces of each of the particles can be formed.
[0171] Alternatively, the solid electrolyte may be formed as a film on the positive electrode current collector or the negative electrode current collector.
[0172] The secondary battery according to the present embodiment is not limited to an all-solid-state secondary battery. The secondary battery may have, for example, a liquid electrolyte in addition to a solid electrolyte.
[0173] The standard electrode potential of magnesium is -2.36V. This value is more noble than the standard electrode potential of lithium, -3.05V. Therefore, the electrolyte of a magnesium ion secondary battery is required to have higher oxidation resistance than the electrolyte of a conventional lithium ion secondary battery. For example, a charging potential of 4.00V based on magnesium corresponds to a charging potential of 4.69V based on lithium. This charging potential is high enough that the electrolyte of a conventional lithium ion secondary battery is oxidized and decomposed. Therefore, when the charging potential of the positive electrode based on magnesium exceeds 4V, a higher oxidation resistance is required that exceeds the range that can be assumed in a conventional lithium ion secondary battery. However, there are few electrolytes that meet such requirements in magnesium ion secondary batteries. In particular, no electrolyte has been reported that meets such requirements when the potential of the positive electrode exceeds 4V during charging.
[0174] The present inventors have focused on the fact that the electrolyte decomposes due to the exchange of electrons between the positive electrode and the electrolyte and / or between the negative electrode and the electrolyte, and have conceived of the secondary battery described below.
[0175] (Drawings and definitions of terms) The present disclosure will be described with reference to certain embodiments and drawings, but the disclosure is not limited thereto, but only by the claims. The drawings are schematic and non-limiting only. In the drawings, the size and shape of some components may be exaggerated and not drawn to scale for illustrative purposes. The dimensions and relative dimensions do not necessarily correspond to actual realizations of the present disclosure.
[0176] In this disclosure, the terms "first" and "second" are used to distinguish between similar components, not to describe a temporal or spatial order, and thus "first" and "second" are interchangeable where appropriate.
[0177] In this disclosure, the terms "top," "bottom," and the like are used for descriptive purposes and do not necessarily describe relative positions. These terms are interchangeable under appropriate circumstances, and various embodiments are capable of operation in other orientations than those described or illustrated herein.
[0178] In this disclosure, the term “X disposed on Y” means that X is in contact with Y, and does not limit the relative positional relationship between X and Y to a particular orientation.
[0179] Among the components described in this disclosure, any components that are not recited in an independent claim indicating a top-level concept are described as optional components.
[0180] (First embodiment) [4-2. Structure of magnesium secondary battery using electrolyte] FIG. 4 is a schematic cross-sectional view showing the configuration of the secondary battery 1000 according to the first embodiment.
[0181] The secondary battery 1000 includes a positive electrode 100, a negative electrode 200, an electrolytic solution 300, and a solid electrolyte layer 400. The negative electrode 200 and the positive electrode 100 face each other and are electrically separated from each other via a gap. The solid electrolyte layer 400 covers the positive electrode 100. The electrolytic solution 300 is filled in the space between the positive electrode 100 and the negative electrode 200. The secondary battery 1000 is charged and discharged by the movement of magnesium ions between the positive electrode 100 and the negative electrode 200.
[0182] The secondary battery 1000 may further include, for example, a separator (not shown) that separates the solid electrolyte layer 400 and the negative electrode 200. In this case, the electrolyte solution 300 may be impregnated into the separator.
[0183] The shape of the secondary battery 1000 is not limited to the example shown in FIG. 4, and may be, for example, a sheet type, a coin type, a button type, a laminated type, a cylindrical type, a flat type, or a rectangular type.
[0184] [4-3. Positive electrode] The positive electrode 100 includes a positive electrode current collector 110 and a positive electrode active material layer 120. The positive electrode active material layer 120 is disposed on the positive electrode current collector 110, and includes positive electrode active material particles 130. In other words, the positive electrode active material particles 130 are disposed on the positive electrode current collector 110. The upper surface of the positive electrode active material layer 120 is an uneven surface defined by the positive electrode active material particles 130.
[0185] The positive electrode current collector 110 is, for example, a metal sheet or a metal film. The positive electrode current collector 110 may be porous or non-porous. Examples of metal materials include aluminum, aluminum alloys, stainless steel, titanium, and titanium alloys. A carbon material such as carbon may be applied to the surface of the positive electrode current collector 110. Alternatively, the positive electrode current collector 110 may be a transparent conductive film. Examples of the transparent conductive film include indium tin oxide (ITO), indium zinc oxide (IZO), fluorine-doped tin oxide (FTO), antimony-doped tin oxide (ATO), indium oxide (In2O3), tin oxide (SnO2), and zinc oxide containing Al.
[0186] The positive electrode active material particles 130 are, for example, a metal oxide containing magnesium and a transition metal, a metal sulfide containing magnesium and a transition metal, a polyanion salt compound containing magnesium and a transition metal, or a fluorinated polyanion salt compound containing magnesium and a transition metal, and the transition metal is selected from, for example, Mn, Co, Cr, V, Ni, and Fe. These materials can absorb and release magnesium ions.
[0187] Examples of the material of the positive electrode active material particles 130 include MgMO (wherein M is at least one selected from Mn, Co, Cr, Ni, and Fe), MgMO (wherein M is at least one selected from Mn, Co, Cr, Ni, and Al), MgMSiO (wherein M is at least one selected from Mn, Co, Ni, and Fe), and Mg x M y AO z Fw (However, M is a transition metal, Sn, Sb or In, A is P, Si or S, 0 < x ≤ 2, 0.5 ≤ y ≤ 1.5, z is 3 or 4, 0.5 ≤ w ≤ 1.5).
[0188] Note that the positive electrode active material particles 130 are not limited to the above materials. For example, they may not contain magnesium. For example, the positive electrode active material particles 130 may be graphite fluoride, a metal oxide, or a metal halide. The metal oxide and the metal halide may contain, for example, at least one selected from scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, and zinc. For example, the positive electrode active material particles 130 may be a sulfide such as Mo6S8, or a chalcogenide compound such as Mo9Se 11 and may be a chalcogenide compound such as Mo9Se.
[0189] The positive electrode active material particles 130 may be, for example, a material having an electrode potential with respect to magnesium metal greater than +4V. In this case, the secondary battery 1000 can realize a capacity exceeding 4V while suppressing the oxidative decomposition of the electrolytic solution 300. Examples of such materials include MgNiSiO4 and MgCoSiO4.
[0190] In addition to the above materials, a conductive material and / or a binder may be added to the positive electrode active material layer 120 as necessary. As the conductive material and / or the binder, those described in the above [1-3. Secondary battery] can be appropriately used.
[0191] The positive electrode 100 is formed, for example, as follows. First, the positive electrode active material particles 130, the conductive material, and the binder are mixed. Next, an appropriate solvent is added to this mixture to obtain a paste-like positive electrode mixture. Next, this positive electrode mixture is applied to the surface of the positive electrode current collector 110 and dried. Thereby, the positive electrode 100 is obtained. Note that the dried positive electrode mixture may be rolled together with the positive electrode current collector 110 in order to increase the electrode density.
[0192] The positive electrode 100 may be in the form of a thin film. The thickness of the positive electrode 100 may be, for example, 500 nm or more and 20 μm or less.
[0193] [4-4. Negative electrode] The negative electrode 200 includes a negative electrode current collector 210 and a negative electrode active material layer 220. The negative electrode active material layer 220 is disposed on the negative electrode current collector 210 and includes a negative electrode active material particles 230. In other words, the negative electrode active material particles 230 are disposed on the negative electrode current collector 210. The lower surface of the negative electrode active material layer 220 is an uneven surface defined by the negative electrode active material particles 230.
[0194] The negative electrode current collector 210 is, for example, a metal sheet or a metal film. The negative electrode current collector 210 may be porous or non-porous. Examples of metal materials include aluminum, aluminum alloys, stainless steel, titanium, and titanium alloys. A carbon material such as carbon may be applied to the surface of the negative electrode current collector 210.
[0195] Examples of the negative electrode active material particles 230 include metals, carbon, metal oxides, carbon intercalation compounds, and sulfides. The negative electrode active material particles 230 contain, for example, magnesium metal or an alloy containing magnesium. Alternatively, the negative electrode active material particles 230 may be a material capable of absorbing and releasing magnesium ions.
[0196] Examples of materials for the negative electrode active material particles 230 include magnesium, tin, bismuth, antimony, and magnesium alloys. The magnesium alloys contain, for example, magnesium and at least one selected from tin, bismuth, titanium, manganese, lead, antimony, aluminum, silicon, gallium, and zinc.
[0197] In addition to the above materials, a conductive material and / or a binder may be added as necessary to the negative electrode active material layer 220. The conductive material, binder, solvent, and thickener in the negative electrode active material layer 220 can be appropriately selected from the materials described for the positive electrode active material layer 120.
[0198] The negative electrode 200 can be formed by a method similar to the method for forming the positive electrode 100 described above.
[0199] The negative electrode 200 may be in the form of a thin film. The thickness of the negative electrode 200 may be, for example, 500 nm or more and 20 μm or less.
[0200] [4-5.Solid electrolyte layer] The solid electrolyte layer 400 covers the positive electrode active material layer 120. The solid electrolyte layer 400 contains a coating material for a positive electrode active material of a magnesium secondary battery. This separates the positive electrode active material layer 120 and the electrolyte solution 300 from each other by the solid electrolyte layer 400, making it possible to avoid direct contact between the positive electrode active material layer 120 and the electrolyte solution 300. This makes it possible to prevent decomposition of the electrolyte solution due to the transfer of electrons at the contact surface between the positive electrode and the electrolyte solution.
[0201] More specifically, the solid electrolyte layer 400 is provided on one main surface of the positive electrode active material layer 120 including the positive electrode active material particles 130, and is a layer that covers the positive electrode active material particles 130 collectively. In other words, the solid electrolyte layer 400 is a layer that covers the positive electrode active material layer 120. The solid electrolyte layer 400 is formed along the uneven surface defined by the positive electrode active material particles 130. The positive electrode active material coating material of the magnesium secondary battery covers the positive electrode active material layer 120 including the positive electrode active material particles 130, thereby forming the solid electrolyte layer 400. In this specification, the "solid electrolyte layer 400" may be referred to as the "surface layer 400". The solid electrolyte layer 400 is an example of a surface layer provided on one main surface of the positive electrode active material layer.
[0202] The positive electrode may further include a solid electrolyte layer 400. In that case, the positive electrode includes a positive electrode current collector 110 and a positive electrode layer. The positive electrode layer has a positive electrode active material layer 120 including positive electrode active material particles 130, and a solid electrolyte layer 400.
[0203] The method for producing the solid electrolyte layer 400 may be the same as the method described above in [1-2. Method for producing a solid electrolyte], for example.
[0204] The solid electrolyte layer 400 may be in a powder form or a lump form. The solid electrolyte may include an amorphous portion. The thickness of the solid electrolyte layer 400 may be, for example, 1 nm or more and 50 nm or less. When the solid electrolyte layer 400 includes an amorphous portion, the solid electrolyte layer 400 is easily formed along the uneven surface of the positive electrode active material layer 120.
[0205] [4-6. Electrolyte] The electrolyte solution 300 fills the space between the positive electrode 100 and the negative electrode 200. The electrolyte solution 300 may further fill the gaps between the positive electrode active material particles 130, or may fill the gaps between the negative electrode active material particles 230.
[0206] The electrolyte 300 is a liquid containing a non-aqueous solvent and a magnesium salt dissolved in the non-aqueous solvent, and is capable of moving magnesium ions in response to an electric field.
[0207] Examples of non-aqueous solvent materials include cyclic ethers, chain ethers, cyclic carbonates, chain carbonates, cyclic carboxylates, chain carboxylates, pyrocarbonates, phosphates, borates, sulfates, sulfites, cyclic sulfones, chain sulfones, nitriles, and sultones.
[0208] Examples of cyclic ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, and crown ethers and derivatives thereof. Examples of the chain ethers include 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl, and derivatives thereof.
[0209] Examples of cyclic carbonates include ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, fluoroethylene carbonate, 4,5-difluoroethylene carbonate, 4,4,4-trifluoroethylene carbonate, fluoromethylethylene carbonate, trifluoromethylethylene carbonate, 4-fluoropropylene carbonate, 5-fluoropropylene carbonate, and derivatives thereof. Examples of chain carbonates include dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, and derivatives thereof.
[0210] Examples of cyclic carboxylic acid esters include γ-butyrolactone, γ-valerolactone, γ-caprolactone, ε-caprolactone, α-acetolactone, and derivatives thereof. Examples of chain carboxylic acid esters include methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, and derivatives thereof.
[0211] Examples of pyrocarbonate esters include diethylpyrocarbonate, dimethylpyrocarbonate, di-tert-butyldicarbonate, and derivatives thereof. Examples of phosphate esters include trimethylphosphate, triethylphosphate, hexamethylphosphoramide, and derivatives thereof. Examples of borate esters include trimethylborate, triethylborate, and derivatives thereof. Examples of sulfate esters include trimethylsulfate, triethylsulfate, and derivatives thereof. Examples of sulfite esters include ethylene sulfite and derivatives thereof.
[0212] Examples of cyclic sulfones include sulfolane and its derivatives. Examples of linear sulfones include alkyl sulfones and its derivatives. Examples of nitriles include acetonitrile, valeronitrile, propionitrile, trimethylacetonitrile, cyclopentanecarbonitrile, adiponitrile, pimelonitrile and its derivatives. Examples of sultones include 1,3-propane sultone and its derivatives.
[0213] As the solvent, only one of the above substances may be used, or two or more of them may be used in combination.
[0214] Examples of magnesium salts include MgBr2, MgI2, MgCl2, Mg(AsF6)2, Mg(ClO4)2, Mg(PF6)2, Mg(BF4)2, Mg(CF3SO3)2, Mg[N(CF3SO2)2]2, Mg(SbF6)2, Mg(SiF6)2, Mg[C(CF3SO2)3]2, Mg[N(FSO2)2]2, Mg[N(C2F5SO2)2]2, MgB 10 Cl 10 , MgB 12 Cl 12 , Mg[B(C6F5)4]2, Mg[B(C6H5)4]2, Mg[N(SO2CF2CF3)2]2, Mg[BF3C2F5]2, and Mg[PF3(CF2CF3)3]2. As the magnesium salt, only one of the above substances may be used, or two or more of them may be used in combination.
[0215] The electrolyte solution 300 is, for example, filled in the space between the positive electrode 100 and the negative electrode 200 facing each other in an exterior (not shown), and impregnates the positive electrode 100, the solid electrolyte layer 400, and the negative electrode 200.
[0216] [4-7.Effects] In the case of a conventional secondary battery without a solid electrolyte layer, as described above, electrons are transferred at the contact surface between the positive electrode and the electrolyte, which may cause the electrolyte to decompose. On the other hand, the secondary battery 1000 has a solid electrolyte layer 400 that covers the positive electrode 100. Therefore, it is possible to suppress the movement of electrons between the positive electrode 100 and the electrolyte 300 while allowing the movement of magnesium ions between the positive electrode 100 and the electrolyte 300. Therefore, it is possible to suppress the decomposition of the electrolyte 300 while maintaining the electrical characteristics of the secondary battery 1000. As a result, the secondary battery 1000 can be stabilized and its life can be extended.
[0217] Note that the solid electrolyte layer 400 does not have to completely prevent contact between the positive electrode 100 and the electrolytic solution 300. For example, it is sufficient that the contact area between the positive electrode 100 and the electrolytic solution 300 is reduced compared to a configuration without the solid electrolyte layer 400.
[0218] In particular, when the charging potential of the positive electrode 100 exceeds 4 V during charging of the secondary battery 1000, the effect of suppressing decomposition of the electrolyte 300 is more significant. For example, electrolyte materials that were thought to be unusable in the region where the charging potential exceeds 4 V can be used in the secondary battery 1000. For example, non-aqueous solvents used in conventional lithium ion secondary batteries can be adopted as non-aqueous solvents for high-capacity alkaline earth metal ion secondary batteries. Therefore, the freedom of material selection for the secondary battery 1000 is increased.
[0219] In the secondary battery 1000, the electrolytic solution 300 and the solid electrolyte layer 400 can function as an electrolyte. For example, by adjusting the distance between the negative electrode 200 and the solid electrolyte layer 400 and the film thickness of the solid electrolyte layer 400, the electrolytic solution 300 can be made to function as a main component of the electrolyte. This can realize a secondary battery having an electrolyte with superior electrical properties compared to, for example, a secondary battery in which the electrolyte is entirely solid (i.e., an all-solid-state secondary battery).
[0220] In the secondary battery 1000, the solid electrolyte layer 400 can be manufactured more easily than, for example, the surface layer 400c described below. Furthermore, for example, when the positive electrode active material layer 120 contains a conductive material, the solid electrolyte layer 400 can cover the conductive material in addition to the positive electrode active material particles 130. Therefore, the solid electrolyte layer 400 can also suppress the reaction between the conductive material and the electrolyte solution 300.
[0221] Furthermore, when the electrolyte comes into contact with the positive electrode in a magnesium ion secondary battery, there is a risk that a magnesium compound (e.g., magnesium oxide) will precipitate at the contact surface between the electrolyte and the positive electrode. This precipitate is a passive film that inhibits the movement of magnesium ions between the positive electrode and the electrolyte. Therefore, there is a risk that the deposited passive film will prevent the magnesium ion secondary battery from being able to perform charge and discharge operations.
[0222] However, this problem of passive film does not occur in lithium ion secondary batteries. It is known that lithium compounds precipitate in lithium ion secondary batteries. However, this precipitate has ion conductivity and does not hinder the movement of lithium ions.
[0223] Therefore, when the secondary battery 1000 is a magnesium ion secondary battery, the solid electrolyte layer 400 covers the positive electrode 100, thereby suppressing the generation of a passivation film on the positive electrode 100, thereby ensuring stable charge and discharge operation of the secondary battery 1000.
[0224] [5. Various Modifications] [5-1. Variation 1] FIG. 5 is a schematic cross-sectional view showing the configuration of a secondary battery 1000a as Modification 1 of the secondary battery according to the first embodiment.
[0225] The secondary battery 1000a includes a positive electrode 100, a negative electrode 200, an electrolytic solution 300, a solid electrolyte layer 400, and a solid electrolyte layer 500. The solid electrolyte layer 500 covers the negative electrode 200. The components of the secondary battery 1000a, except for the solid electrolyte layer 500, are similar to the corresponding components of the secondary battery 1000, and therefore will not be described.
[0226] The solid electrolyte layer 500 covers the negative electrode active material layer 220. The solid electrolyte layer 500 contains a coating material for a negative electrode active material of a magnesium secondary battery. This separates the negative electrode active material layer 220 and the electrolyte solution 300 from each other by the solid electrolyte layer 500, and direct contact between the negative electrode active material layer 220 and the electrolyte solution 300 can be avoided. This makes it possible to prevent decomposition of the electrolyte solution due to the transfer of electrons at the contact surface between the negative electrode and the electrolyte solution.
[0227] The solid electrolyte layer 500 is provided on one main surface of the negative electrode active material layer 220 including the negative electrode active material particles 230, and is a layer that covers the negative electrode active material particles 230 collectively. In other words, the solid electrolyte layer 500 is a layer that covers the negative electrode active material layer 220. The solid electrolyte layer 500 is formed along the uneven surface defined by the negative electrode active material particles 230. The negative electrode active material coating material of the magnesium secondary battery covers the negative electrode active material layer 220 including the negative electrode active material particles 230, thereby forming the solid electrolyte layer 500. In this specification, the "solid electrolyte layer 500" may be referred to as the "surface layer 500". The solid electrolyte layer 500 is an example of a surface layer provided on one main surface of the negative electrode active material layer.
[0228] The negative electrode 200 includes a negative electrode current collector 210 and a negative electrode active material layer 220. The negative electrode active material layer 220 is disposed on the negative electrode current collector 210 and includes a negative electrode active material particle 230. In other words, the negative electrode active material particle 230 is disposed on the negative electrode current collector 210. The upper surface of the negative electrode active material layer 220 is an uneven surface defined by the negative electrode active material particle 230. The negative electrode may further include a solid electrolyte layer 500. In that case, the negative electrode includes the negative electrode current collector 210 and a negative electrode layer. The negative electrode layer has the negative electrode active material layer 220 including the negative electrode active material particle 230, and the solid electrolyte layer 500.
[0229] The method for producing the solid electrolyte layer 500 may be the same as the method described above in [1-2. Method for producing a solid electrolyte], for example.
[0230] The solid electrolyte layer 500 may be in a powder form or in a lump form. The solid electrolyte may include an amorphous portion. The thickness of the solid electrolyte layer 500 may be, for example, 1 nm or more and 20 μm or less, or may be 5 nm or more and 50 nm or less. When the solid electrolyte layer 500 includes an amorphous portion, the solid electrolyte layer 500 is easily formed along the uneven surface of the negative electrode active material layer 220.
[0231] The secondary battery 1000a exhibits the effects attributable to the solid electrolyte layer 500 in addition to the various effects described in the above [4-7. Effects]. The effects attributable to the solid electrolyte layer 500 can be understood by appropriately replacing the "positive electrode collector 110", the "solid electrolyte layer 400", and the "positive electrode 100" with the "negative electrode collector 210", the "solid electrolyte layer 500", and the "negative electrode 200" in the description of the above [4-7. Effects]. In short, the solid electrolyte layer 500 can suppress the reductive decomposition of the electrolyte solution 300 by suppressing contact between the negative electrode 200 and the electrolyte solution 300. In addition, the solid electrolyte layer 500 can suppress the generation of a passivation film on the negative electrode 200.
[0232] [5-2. Variation 2] FIG. 6 is a schematic cross-sectional view showing the configuration of a secondary battery 1000b as Modification 2 of the secondary battery according to the first embodiment.
[0233] The secondary battery 1000b includes a positive electrode 100, a negative electrode 200, an electrolytic solution 300, and a solid electrolyte layer 500. That is, the secondary battery 1000b has a configuration in which the solid electrolyte layer 400 is removed from the secondary battery 1000a. Each component of the secondary battery 1000b is similar to the corresponding component of the secondary battery 1000, and therefore description thereof will be omitted.
[0234] The secondary battery 1000b exhibits the same effects as those attributable to the solid electrolyte layer 500 described above in [5-1. Modification 1].
[0235] [5-3. Variation 3] FIG. 7 is a schematic cross-sectional view showing the configuration of a secondary battery 1000c as the third modification of the secondary battery according to the first embodiment.
[0236] The secondary battery 1000c includes a positive electrode 100, a negative electrode 200a, an electrolytic solution 300, and a solid electrolyte layer 400. The negative electrode 200a includes a negative electrode current collector 210 and a negative electrode active material layer 220a. The components of the secondary battery 1000c, except for the negative electrode active material layer 220a, are similar to the corresponding components of the secondary battery 1000, and therefore will not be described.
[0237] The negative electrode active material layer 220a is a flat layer disposed on the negative electrode current collector 210. The material of the negative electrode active material layer 220a can be selected from, for example, the various materials listed in [4-4. Negative Electrode] above. The negative electrode active material layer 220a can be formed by, for example, a physical deposition method or a chemical deposition method.
[0238] The secondary battery 1000c has the same effects as those described above in [4-7. Effects].
[0239] [5-4. Variation 4] FIG. 8 is a schematic cross-sectional view showing the configuration of a secondary battery 1000d as the fourth modification of the secondary battery according to the first embodiment.
[0240] The secondary battery 1000d includes a positive electrode 100, a negative electrode 200a, an electrolytic solution 300, a solid electrolyte layer 400, and a solid electrolyte layer 500a. The components of the secondary battery 1000d, except for the solid electrolyte layer 500a, are similar to the corresponding components of the secondary battery 1000c, and therefore will not be described.
[0241] The solid electrolyte layer 500a is a flat layer disposed on the negative electrode active material layer 220a. The material and the method for forming the solid electrolyte layer 500a are as described above in [4-5. Solid electrolyte layer].
[0242] The secondary battery 1000d provides the same effects as those described above in [5-1. Modification 1].
[0243] [5-5. Variation 5] FIG. 9 is a schematic cross-sectional view showing the configuration of a secondary battery 1000e as the fifth modification of the secondary battery according to the first embodiment.
[0244] The secondary battery 1000e includes a positive electrode 100, a negative electrode 200a, an electrolytic solution 300, and a solid electrolyte layer 500a. That is, the secondary battery 1000e has a configuration in which the solid electrolyte layer 400 is removed from the secondary battery 1000d. Each component of the secondary battery 1000e is similar to the corresponding component of the secondary battery 1000d, and therefore description thereof will be omitted.
[0245] The secondary battery 1000e exhibits the same effects as those attributable to the solid electrolyte layer 500 described above in [5-2. Modification 2].
[0246] Second embodiment [6-1. Structure of secondary batteries] FIG. 10 is a schematic cross-sectional view showing the configuration of a secondary battery 2000 according to the second embodiment.
[0247] The secondary battery 2000 has a similar configuration to the secondary battery 1000 described in the first embodiment, except for the positive electrode 100c and the solid electrolyte coating 400c.
[0248] In the second embodiment, the secondary battery 2000 includes a positive electrode material. The positive electrode material includes positive electrode active material particles 130 and a solid electrolyte coating 400c that coats the positive electrode active material particles 130. The solid electrolyte coating 400c includes a coating material for a positive electrode active material of a magnesium secondary battery. Since the solid electrolyte coating 400c coats the positive electrode active material particles 130, the surfaces of the positive electrode active material particles are not exposed or are unlikely to be exposed in the gaps between the positive electrode active material particles. Therefore, for example, even if the electrolyte fills these gaps, the oxidative decomposition of the electrolyte can be more effectively suppressed. In this specification, the "solid electrolyte coating 400c" may be referred to as the "surface layer 400c".
[0249] The positive electrode 100c includes a positive electrode current collector 110 and a positive electrode active material layer 120c. The positive electrode active material layer 120c is disposed on the positive electrode current collector 110 and includes positive electrode active material particles 130. The surfaces of the positive electrode active material particles 130 are covered with a solid electrolyte coating 400c. With this configuration, the movement of electrons between the positive electrode active material particles 120c and the electrolyte 300 can be suppressed. As a result, the oxidative decomposition of the electrolyte 300 can be suppressed. In addition, the solid electrolyte coating 400c can suppress the generation of a passivation film on the positive electrode 100c by coating the surfaces of the positive electrode active material particles 130. The solid electrolyte coating 400c is an example of a surface layer that covers the positive electrode active material particles.
[0250] [6-2. Positive electrode and solid electrolyte coating] The secondary battery 2000 is similar to that described in the first embodiment except for the shape of the solid electrolyte and the method of forming the solid electrolyte and the positive electrode, and therefore the description thereof is omitted. Specifically, the material of the solid electrolyte coating 400c can be selected from the various materials listed in [4-5. Solid electrolyte layer] of the first embodiment, for example.
[0251] The solid electrolyte coating 400c may be in a powder form or a thin film form. If the solid electrolyte coating 400c is in a thin film form, it is easily formed along the shape of the positive electrode active material particles 130, and the coverage is improved. The thickness of the solid electrolyte coating 400c may be, for example, 1 nm or more and 200 nm or less.
[0252] The positive electrode 100c and the solid electrolyte coating 400c are formed, for example, as follows.
[0253] First, the surface of the positive electrode active material particles 130 is coated with a solid electrolyte to form a solid electrolyte coating 400c. The coated positive electrode active material particles 130 are then mixed with a conductive material and a binder. Next, a suitable solvent is added to this mixture, thereby obtaining a paste-like positive electrode mixture. Next, this positive electrode mixture is applied to the surface of the positive electrode current collector 110 and dried. In this way, the positive electrode 100c is obtained.
[0254] The solid electrolyte coating 400c may be formed, for example, by depositing a solid electrolyte material by the above-mentioned physical deposition method or chemical deposition method while moving the positive electrode active material particles 130. Alternatively, the solid electrolyte coating 400c may be formed, for example, by a sol-gel method or the above-mentioned liquid phase film formation method.
[0255] [6-3. Effects] The secondary battery 2000 has various effects similar to those described in the first embodiment. Specifically, these effects can be understood by appropriately replacing "solid electrolyte layer 400" with "solid electrolyte coating 400c" in the description of [4-7. Effects] of the first embodiment.
[0256] In the secondary battery 2000, each of the positive electrode active material particles 130 is covered with a solid electrolyte coating 400c. Therefore, the surface of the positive electrode active material particles 130 is not exposed, or is unlikely to be exposed, in the gaps between the positive electrode active material particles 130. Therefore, even if the electrolyte solution 300 fills these gaps, for example, the oxidative decomposition of the electrolyte solution 300 can be more effectively suppressed. In addition, the solid electrolyte coating 400c can effectively suppress the generation of a passivation film on the positive electrode 100c.
[0257] [6-4. Various Modifications] [6-4-1. Variation 1] FIG. 11 is a schematic cross-sectional view showing the configuration of a secondary battery 2000a as Modification 1 of the secondary battery according to the second embodiment.
[0258] The secondary battery 2000a has the same configuration as the secondary battery 2000, except for the negative electrode 200c and the solid electrolyte coating 500c.
[0259] In the first modification, the secondary battery 2000a includes a negative electrode material. The negative electrode material includes a negative electrode active material particle 230 and a solid electrolyte coating 500c that coats the negative electrode active material particle 230. The solid electrolyte coating 500c includes a coating material for a negative electrode active material of a magnesium secondary battery. Since the solid electrolyte coating 500c coats the negative electrode active material particle 230, the surface of the negative electrode active material particle is not exposed or is unlikely to be exposed in the gaps between the negative electrode active material particles. Therefore, even if the electrolyte fills these gaps, for example, the reductive decomposition of the electrolyte can be more effectively suppressed. In this specification, the "solid electrolyte coating 500c" may be referred to as the "surface layer 500c".
[0260] The negative electrode 200c includes a negative electrode current collector 210 and a negative electrode active material layer 220c. The negative electrode active material layer 220c is disposed on the negative electrode current collector 210 and includes negative electrode active material particles 230. The surfaces of the negative electrode active material particles 230 are covered with a solid electrolyte coating 500c. With this configuration, it is possible to suppress the transfer of electrons between the negative electrode active material particles 230 and the electrolyte solution 300. As a result, it is possible to suppress the reductive decomposition of the electrolyte solution 300. In addition, the solid electrolyte coating 500c can suppress the generation of a passivation film on the negative electrode 200c by coating the surfaces of the negative electrode active material particles 230. The solid electrolyte coating 500c is an example of a surface layer that covers the negative electrode active material particles.
[0261] The material of the solid electrolyte coating 500c can be selected from, for example, the materials described in [4-5. Solid electrolyte layer] of the first embodiment. The solid electrolyte coating 500c may be in a powder form or a thin film form. If the solid electrolyte coating 500c is in a thin film form, it is easily formed along the shape of the negative electrode active material particles 230, and the coverage is improved. The thickness of the solid electrolyte coating 500c may be, for example, 1 nm or more and 200 nm or less.
[0262] The method for forming the negative electrode 200c and the solid electrolyte coating 500c may be the same as the method described above in [6-2. Positive electrode and solid electrolyte coating], for example.
[0263] In addition to the various effects described in the above [6-3. Effects], the secondary battery 2000a exhibits effects attributable to the solid electrolyte coating 500c. The effects attributable to the solid electrolyte coating 500c can be understood by appropriately replacing the "solid electrolyte layer 400" and the "positive electrode 100" in the description of the above [4-7. Effects] with the "solid electrolyte coating 500c" and the "negative electrode 200c", respectively.
[0264] In the secondary battery 2000a, each of the negative electrode active material particles 230 is covered with a solid electrolyte coating 500c. Therefore, even if the electrolyte solution 300 fills the gaps between the negative electrode active material particles 230, the reductive decomposition of the electrolyte solution 300 can be more effectively suppressed. In addition, the solid electrolyte coating 500c can effectively suppress the generation of a passivation film on the negative electrode 200c.
[0265] [6-4-2. Variation 2] FIG. 12 is a schematic cross-sectional view showing the configuration of a secondary battery 2000b as Modification 2 of the secondary battery according to the second embodiment.
[0266] The secondary battery 2000b has a configuration in which the solid electrolyte film 400c is removed from the secondary battery 2000a. Each component of the secondary battery 2000b is similar to the corresponding component of the secondary battery 2000a, and therefore a description thereof will be omitted.
[0267] The secondary battery 2000b exhibits the same effects as those attributable to the solid electrolyte coating 500c described above in [6-4-1. Modification 1].
[0268] [6-4-3. Other variations] The secondary batteries 2000, 2000a, and 2000b described above may be combined with any one of the secondary batteries 1000, 1000a, 1000b, 1000c, 1000d, and 1000e described in the first embodiment.
[0269] For example, the negative electrode 200 of the secondary battery 2000 may be replaced with the negative electrode 200a described in [5-3. Modification 3] of the first embodiment, and further, the solid electrolyte layer 500a described in [5-4. Modification 4] of the first embodiment may be added.
[0270] [7. Experimental Results] Various examples of the solid electrolyte membrane according to this embodiment will be described. [7-1. Example 1] The magnesium phosphate membrane of Example 1 was produced using the production apparatus 21 shown in Fig. 2. Here, a production method similar to the flow shown in Fig. 3B was carried out.
[0271] The first precursor supply part 23 and the second precursor supply part 24 were precursor bottles (manufactured by Japan Advanced Chemicals Ltd.). The reactor 22, the sample holder in the reactor 22, the first precursor supply part 23, the second precursor supply part 24, and various piping were made of stainless steel (SUS316). Ribbon heaters were wrapped around the reactor 22, the first precursor supply part 23, the second precursor supply part 24, and various piping, and each part was heated by heating the ribbon heater. The temperature of each part was measured by a thermocouple, and the temperature was controlled by a temperature controller. The mass flow controllers 26a to 26e and the valves V1 to V8 were controlled using a sequencer (MELSEC-Q; manufactured by Mitsubishi Electric Corporation) and a control program (manufactured by Nippon Spread Co., Ltd.). The needle valve NV was a bellows-sealed valve (SS-4VMG; manufactured by Swagelok). The degree of vacuum in the reactor 22 was measured by a Pirani gauge (TPR280 DN16 ISO-KF; manufactured by PFEIFFER VACUUM). The degree of vacuum in the reactor 22 during the deposition was adjusted to 10 -1 Pa to 10 3 Controlled by Pa.
[0272] The substrate was a glass substrate on which Au electrodes were formed. The Au electrodes were comb-shaped with a pitch of 5 μm. The glass substrate with the Au electrodes was placed in the reactor 22. The first precursor was bis(ethylcyclopentadienyl)magnesium, and the second precursor was tris(dimethylamino)phosphine (TDMAP). The purge gas was argon gas. The oxygen supply unit 33 was capable of supplying oxygen gas. The temperature in the reactor 22 was set to 250° C. The temperature of the first precursor supply unit 23 was set to 40° C. The temperature of the second precursor supply unit 24 was set to 40° C. The temperature of the first pipe P1 was set to 170° C. The temperatures of all pipes other than the first pipe P1 and the second pipe P2 were set to 200° C. The flow rates of the oxygen gas and the purge gas were set to 50 ml / min. The manual valves MV1 and MV2 were constantly open, and the flow rate of the auxiliary gas from the auxiliary gas supply units 27 and 29 was set to 50 ml / min. The opening of the needle valve NV was 50%.
[0273] Prior to step S1 shown in FIG. 3B, the following preparatory steps were carried out.
[0274] Valve V8 was opened, and purge gas was supplied from the purge gas supply unit 34 into the reactor 22 for about 1800 seconds, and then valve V8 was closed. Next, valve V7 was opened, and oxygen gas was supplied from the oxygen supply unit 33 into the reactor 22 for 6 seconds, and then valve V7 was closed. Thereafter, a purge step was performed for 8 seconds. After the preparation step, the repeat cycle shown in FIG. 3B was performed 1000 times. Composition analysis was performed using an XPS device (Quamtera SXM; manufactured by ULVAC-PHI, Inc.), and the composition formula of Example 1 was found to be Mg 3.1 (PO 3.1 )2.
[0275] [7-2. Example 2] A magnesium phosphate film according to Example 2 was produced under the same conditions as Example 1, except that the temperature inside the reactor 22 during film formation was set to 125° C. As a result of composition analysis using an XPS device, the composition formula of Example 2 was Mg 3.1 (PO3.0 )2.
[0276] [7-3. Example 3] The zirconium-added magnesium phosphate membrane of Example 3 was produced using the production apparatus 21 shown in Fig. 2. Here, a production method similar to the flow shown in Fig. 3D was carried out.
[0277] The first precursor supply part 23, the second precursor supply part 24, the third precursor supply part 25, and the third precursor supply part 26 were precursor bottles (manufactured by Japan Advanced Chemicals Ltd.). The reactor 22, the sample holder in the reactor 22, the first precursor supply part 23, the second precursor supply part 24, the third precursor supply part 25, and various piping were made of stainless steel (SUS316). Ribbon heaters were wrapped around the reactor 22, the first precursor supply part 23, the second precursor supply part 24, the third precursor supply part 25, and various piping, and each part was heated by heating the ribbon heater. The temperature of each part was measured by a thermocouple, and the temperature was controlled by a temperature controller. The mass flow controllers 26a to 26e and the valves V1 to V8 were controlled by a sequencer (MELSEC-Q; manufactured by Mitsubishi Electric Corporation) and a control program (manufactured by Nippon Spread Co., Ltd.). The needle valve NV was a bellows seal valve (SS-4VMG; manufactured by Swagelok). The degree of vacuum in the reactor 22 was measured by a Pirani gauge (TPR280 DN16 ISO-KF; manufactured by PFEIFFER VACUUM). The degree of vacuum in the reactor 22 during the deposition was adjusted to 10 -1 Pa to 10 3 Controlled by Pa.
[0278] The substrate was a glass substrate on which Au electrodes were formed. The Au electrodes were comb-shaped with a pitch of 5 μm. The glass substrate with the Au electrodes was placed in the reactor 22. The first precursor was bis(ethylcyclopentadienyl)magnesium, the second precursor was tris(dimethylamino)phosphine (TDMAP), and the third precursor was tetrakisethylmethylaminozirconium. The purge gas was argon gas. The oxygen supply unit 33 was capable of supplying oxygen gas. The temperature in the reactor 22 was set to 250° C. The temperature of the first precursor supply unit 23 was set to 40° C. The temperature of the second precursor supply unit 24 was set to 40° C., and the temperature of the third precursor supply unit 25 was set to 45° C. The temperatures of the first pipe P1, the second pipe P2, and the third pipe P3 were set to 170° C. The temperatures of all pipes other than the pipes P1 to P3 were set to 200° C. The flow rates of oxygen gas and purge gas were set to 50 ml / min. Manual valves MV1 to MV3 were always open, and the flow rates of auxiliary gas from auxiliary gas supply units 27, 29, and 31 were set to 50 ml / min. The opening of needle valve NV was 50%.
[0279] Prior to step SS1 shown in FIG. 3D, the following preparation steps were carried out.
[0280] Valve V8 was opened, and purge gas was supplied from the purge gas supply unit 34 into the reactor 22 for about 1800 seconds, and then valve V8 was closed. Next, valve V7 was opened, and oxygen gas was supplied from the oxygen supply unit 33 into the reactor 22 for 6 seconds, and then valve V7 was closed. Thereafter, a purge step was performed for 8 seconds. After the preparation step, the repeat cycle shown in FIG. 3D was performed 1000 times. Composition analysis was performed using an XPS device (Quamtera SXM; manufactured by ULVAC-PHI, Inc.), and the composition formula of Example 3 was found to be Mg 2.5 Zr 0.9 (PO 3.6 )2.
[0281] [7-4. Example 4] A magnesium phosphate film containing zirconium according to Example 4 was produced under the same conditions as Example 3, except that the temperature inside the reactor 22 during film formation was set to 125° C. As a result of composition analysis using an XPS device, the composition formula of Example 4 was Mg 2.4 Zr 1.0 (PO 3.5 )2.
[0282] [7-5. Structural analysis of magnesium phosphate membrane and magnesium phosphate membrane with added zirconium] The crystallinity of the solid electrolytes of Examples 1 to 4 was evaluated by X-ray diffraction (XRD). In Examples 1 and 2, the solid electrolytes formed on a glass substrate, and in Examples 3 and 4, the solid electrolytes formed on a silicon substrate with a thermal oxide film were used as samples. The structure of the samples was analyzed by the θ-2θ method of wide-angle X-ray diffraction using an XRD device (SmartLab: manufactured by Rigaku Corporation). As shown in Figures 13 and 14, the solid electrolytes of Examples 1 to 4 were amorphous. The broad peak seen around θ=20 to 30° in Figure 13 is due to the quartz substrate, and the peak around θ=45 to 55° in Figure 14 is due to the silicon substrate.
[0283] [7-6. Measurement of ionic conductivity] The ionic conductivity of the magnesium phosphate membranes to which magnesium phosphate and zirconium were added according to Examples 1 to 4 was measured using an electrochemical measurement device (Modulab; manufactured by Solartrom Analytical).
[0284] FIG. 15 shows the temperature dependence of ion conductivity of the magnesium phosphate membranes according to Examples 1 to 4 and the magnesium phosphate membrane with zirconium added. The black circles represent the measurement results of Example 1, the white circles represent the measurement results of Example 2, the black squares represent the measurement results of Example 3, and the white squares represent the measurement results of Example 4. As shown in FIG. 15, the conductivity was high in Examples 2 and 4, which had low film formation temperatures. The reason for this is presumed to be as follows. As shown in FIGS. 13 and 14, the magnesium phosphate membranes according to Examples 1 to 4 and the magnesium phosphate membrane with zirconium added all had an amorphous structure. When the film formation temperature was low, a more sparse membrane was formed, which is thought to ensure space for magnesium ions to pass through, resulting in high conductivity of magnesium ions.
[0285] Furthermore, when comparing the magnesium phosphate membrane of Example 2 and the magnesium phosphate membrane of Example 4 to which zirconium has been added, the magnesium ion conductivity was comparable in the low temperature region, whereas the magnesium ion conductivity of the magnesium phosphate membrane of Example 4 to which zirconium has been added was higher in the high temperature region. This is because, whereas magnesium phosphate starts to decompose at about 500°C, the addition of zirconium to magnesium phosphate improves the thermal stability of the solid electrolyte membrane, thereby making it possible to suppress this decomposition. In other words, this is because the structural stability of magnesium phosphate is improved by the addition of zirconium to magnesium phosphate. [Industrial Applicability]
[0286] The solid electrolyte according to the present disclosure is useful, for example, for producing an all-solid-state secondary battery.
Claims
1. A coating material for covering an electrode active material of a magnesium secondary battery, The coating material is Mg x (P.O. z ) 2 (3≦x≦3.5, 3≦z≦4.25) and including an amorphous portion, Coating material for electrode active materials in magnesium secondary batteries.
2. The electrode active material is a positive electrode active material. The coating material for an electrode active material of a magnesium secondary battery according to claim 1.
3. The electrode active material is a negative electrode active material. The coating material for an electrode active material of a magnesium secondary battery according to claim 1.
4. Electrode active material particles; a surface layer covering the electrode active material particles; Equipped with The surface layer includes the coating material for an electrode active material of a magnesium secondary battery according to claim 1. Electrode material for magnesium secondary batteries.
5. The electrode active material particles are positive electrode active material particles. The electrode material for a magnesium secondary battery according to claim 4.
6. The electrode active material particles are negative electrode active material particles. The electrode material for a magnesium secondary battery according to claim 4.
7. An electrode layer of a magnesium secondary battery comprising the electrode material according to claim 4.
8. an electrode active material layer including electrode active material particles; A surface layer provided on one main surface of the electrode active material layer, the surface layer including the coating material for an electrode active material of a magnesium secondary battery according to claim 1; An electrode layer of a magnesium secondary battery comprising:
9. The electrode active material particles are positive electrode active material particles. The electrode layer of a magnesium secondary battery according to claim 8.
10. The electrode active material particles are negative electrode active material particles. The electrode layer of a magnesium secondary battery according to claim 8.
11. An electrode layer according to claim 7 or 8; a current collector supporting the electrode layer and in electrical contact with the electrode layer; An electrode for a magnesium secondary battery comprising:
12. An electrode according to claim 11; an electrolyte solution containing a non-aqueous solvent and a magnesium salt dissolved in the non-aqueous solvent; Equipped with Magnesium secondary battery.
Citation Information
Patent Citations
Polyanion active materials and method of forming the same
JP2013030484A
Secondary battery
JP2018098172A
Solid electrolyte and secondary battery using the same
JP2018107106A
Positive electrode active material and aqueous magnesium ion secondary battery using the same
JP2018163800A
Interface layer for solid-state battery and method for manufacturing the same
JP2018502416A