Manufacturing method of reed fiber

By cutting and chemically treating reed stalks to preserve antibacterial components, the method effectively produces reed fibers that maintain their inherent antibacterial properties, facilitating the production of paper and yarns with sustained antibacterial effects.

JP7583486B2Active Publication Date: 2024-11-14ATELIER MAY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024026073
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-09-29
Filing Date
2024-02-23
Publication Date
2024-11-14
Estimated Expiration
2044-02-23

AI Technical Summary

Technical Problem

Existing methods for producing reed fibers from native reeds fail to retain the inherent antibacterial properties of reeds, leading to economic inefficiencies and difficulty in commercializing products with antibacterial appeal.

Method used

A method involving cutting reed stalks into predetermined lengths and immersing them in a 0.8 wt% sodium hydroxide solution at 20 to 30°C for 12 to 72 hours to remove lignin while preserving antibacterial components, followed by defibration and dehydration to obtain reed fibers.

Benefits of technology

The produced reed fibers retain their antibacterial properties, enabling the creation of paper products and blended yarns with sustained antibacterial effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583486000001
    Figure 0007583486000001
  • Figure 0007583486000002
    Figure 0007583486000002
Patent Text Reader

Abstract

To provide a manufacturing method of a reed fiber for obtaining a fiber from a reed stem without loosing antibacterial activity that a reed plant has intrinsically.SOLUTION: A manufacturing method of a reed fiber includes: a cutting step of cutting a reed stem to obtain a reed stem chip of a prescribed length; and a treating step of chemically treating the cut reed stem chips by soaking in a sodium hydroxide solution of a concentration of 0.8 wt% or over at a water temperature of 20 to 30°C for 12 to 72 hours to separate lignin in the reed stem chips.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing reed fibers using reed plants as a raw material. [Background technology]

[0002] Reeds are plants of the grass family that grow naturally on the banks of swamps and rivers. They are perennial plants, but the stems above ground, which grow in six months, die in winter. On the other hand, the underground stems do not die and new stems grow the following year. Reeds are an abundant, renewable natural resource found worldwide. They grow naturally on riverbeds and create reed beds, but are periodically cut for river maintenance. Regular cutting helps to maintain healthy reed beds that spread across riverbeds and other areas.

[0003] Although cut reed stalks are used as roofing materials or reed mats, and are also used in some areas as material for woodwind instrument reeds, from the perspective of economic efficiency, most cut reeds are disposed of by incineration, etc. Because reed beds have few economic uses, their protection has not been given much importance, and river improvement work has resulted in insufficient flooding, and at one time the reed beds were in danger of becoming extinct.

[0004] However, in recent years, with the trend of aiming for a sustainable society, economically rational means of utilizing reeds, which have been disposed of up until now, are being explored. Research is also being conducted from the perspective of whether plant fibers can be extracted from reeds and used industrially and economically as raw materials for paper, thread, cloth, etc. For example, Patent Document 1 discloses a technology for separating cellulose components, which are reed fibers, from naturally growing reeds, following the method of separating bamboo fibers from bamboo, and manufacturing nonwoven fabrics by blending them into yarn. In addition, a technology is disclosed for imparting antibacterial properties to the obtained reed fibers by immersing them in bamboo antibacterial extract or an aqueous solution of hinokitiol. However, the process of manufacturing paper, thread, cloth, etc. from reeds is less economically rational in terms of manufacturing costs compared to already industrially established methods, and it has been difficult to make appealing products.

[0005] Hydrolyzable tannins, which have antibacterial properties and have gallic acid (3,4,5-trihydroxybenzoic acid) as the basic skeleton, are known to be contained in many plants, such as Hamamelis, a plant of the Witch Hazel family, tea leaves, and oak bark, and their antibacterial properties have been extensively studied. For example, Non-Patent Document 1 discloses a study on the use of gallic acid and the like as an antibacterial agent, assuming a hot water extract of the leaves of Eucalyptus saligna, a type of eucalyptus. It is said that such antibacterial hydrolyzable tannins are also contained in native reeds.

[0006] However, with conventional techniques, such as that described in Patent Document 1, for extracting reed fibers from native reeds and turning them into paper products, thread, fabric, etc., the antibacterial properties of the reed-derived components were lost by the time the products were made. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2022-102994 A [Non-patent literature]

[0008] [Non-Patent Document 1] Report of the Tokyo University Forestry Experiment Station, 137, 41-51 (2017) Inagaki et al. "Study on the antibacterial spectrum of gallic acids, the main components of Eucalyptus saligna leaves, for their utilization" Summary of the Invention [Problem to be solved by the invention]

[0009] In light of the above situation, the inventors have repeatedly investigated whether it is possible to effectively utilize virgin reeds to create products that retain the antibacterial components derived from the reeds, thereby creating products that feature their antibacterial properties. As a result of continuing to review the process, they have arrived at the present invention.

[0010] In view of the above circumstances, the present invention aims to provide a manufacturing method for extracting and fibrous reed fibers without losing the antibacterial activity inherent to reeds, antibacterial reed fibers obtained by this method, and antibacterial paper products and blended yarns made from the reeds. [Means for solving the problem]

[0011] In order to solve the above problems, the present invention provides a method for producing reed fiber from reed plants, comprising the steps of: Reed stems Length within the range of 10 to 100 mm The main feature of this method is that it includes a step of cutting the reed stalk pieces into reed stalk pieces, and a step of immersing the cut reed stalk pieces in a sodium hydroxide solution having a concentration of 0.8 wt % or more at a water temperature of 20 to 30°C for 12 to 72 hours to separate the lignin in the reed stalk pieces. Effect of the Invention

[0012] The reed fiber obtained by the reed fiber manufacturing method of the present invention retains the antibacterial activity inherent to reeds, and the paper products and blended yarns made from this reed fiber also retain the antibacterial activity.

[0013] Because the above-mentioned antibacterial effect utilizes the inherent properties of reeds, it is believed that not only will the specific fungi that are targeted by the antibacterial effect be different, but the antibacterial effect will also last longer than if antibacterial components were added later to the extracted fibers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention will be described in detail below by showing a specific manufacturing method, but the present invention is not limited to the embodiment shown below. The manufacturing method of reed fiber in the present invention mainly consists of the felling / crushing process, cutting process, bagging process, retching process, water washing process, fiber defibration process, sorting process, and dehydration / drying process shown below, but the important process for obtaining reed fiber that retains antibacterial components derived from reeds is the retching process.

[0015] (Logging and crushing process) First, reeds growing naturally in the reed beds, preferably those that are at least 10 months old, are cut down. Reeds that are less than 10 months old are still in the process of growing, and it is preferable to let them grow sufficiently before cutting them down. Cutting can be done manually or with a power source such as a harvester. To make processing easier in the later process, it is preferable to crush the stems of the cut reeds with a hammer or roller.

[0016] (Cutting process) The crushed reed stems are cut into pieces of a predetermined size prior to the subsequent chemical retching process. The length of the cut reeds is preferably 10 to 100 mm, more preferably 20 to 60 mm. The length does not need to be uniform, and it is sufficient that the length of each reed stem piece is within a predetermined preferred range. Cutting may be done manually, but a general cutting machine can also be used.

[0017] In general, it is more efficient to cut the reeds to a specified length after removing lignin by retching and softening the plant fibers. However, in the reed fiber manufacturing method of the present invention, chemical retching is performed in the subsequent retching step, which reduces the strength of the reeds so as not to lose the reeds' inherent antibacterial properties. For this reason, the reeds are cut to a specified size to form reed stem pieces prior to the retching step, so that the entire reed stem pieces can be quickly and thoroughly immersed in the retching solution. In the manufacturing method of the present invention, the main cutting step is performed prior to the retching step, so there is no need to perform the crushing step or the step of aligning the reeds to a specified length after the retching step.

[0018] (Rettching process) Generally, the retching process is a process for extracting plant fibers from plants, in which the lignin that bonds to cellulose, the main component of plant fibers, is removed to facilitate the subsequent defibration process. When a chemical method is used, such as using a sodium hydroxide solution as the retching solution, it is called chemical retching. In the manufacturing method of the present invention, chemical retching is selected as the retching method, and the conditions are made strict. This removes the lignin contained in the reed, but allows the antibacterial components that are naturally contained in the reed to be retained in the reed fibers.

[0019] In the manufacturing method of the present invention, since the reeds are cut into reed stem pieces of a predetermined length in the cutting step, it is preferable to bag a predetermined number of reeds before immersing them in the retching solution in order to facilitate the work in the retching step. There are no particular limitations on the bags used for the bags, such as hemp bags, as long as they can easily pass through the retching solution and are resistant to the alkaline solution used in this step.

[0020] The conditions for the retching process in the manufacturing method of the present invention to remove a significant amount of lignin from the reed stalk pieces while not losing the antibacterial activity inherent to the reed are as follows. The retching solution is a sodium hydroxide solution of 0.8 wt% or more. The temperature and time for immersing the bagged reed stalk pieces in the solution (preferably) are a water temperature of 20 to 30°C and an immersion time of 12 to 72 hours. If the water temperature is higher or the time is longer than the above conditions, the antibacterial properties derived from the reed are lost. On the other hand, if the concentration is lower, the water temperature is lower, or the time is shorter than the above conditions, the lignin cannot be sufficiently removed, causing problems in the subsequent fiberization process and poor workability. In addition, when the concentration of the sodium hydroxide solution is 1.5 wt% or more, the work efficiency is the same, but the pH concentration of the wastewater after the retching process becomes higher, which is not preferable because it only increases the environmental load. The above conditions can be set to a certain degree of freedom within their respective ranges, but care must be taken, particularly when the concentration of the sodium hydroxide solution is too high, as this will change the properties of the resulting reed fiber.

[0021] (Water washing process) After the retching process, the reed stem pieces are washed and neutralized by exposing them to water. Washing can be done by immersing them in stored water and changing the water several times, or by using running water. The pH of the washing water can be measured to determine whether the reed stem pieces have been sufficiently neutralized.

[0022] (defibration process) The neutralized reed stalk pieces are defibrated to obtain reed fiber. Defibration is the process of loosening the fibers without breaking them to obtain fiber, and is generally carried out using a machine called a disc refiner. There are various mechanisms for defibration using disc refiners, one of which is to pass the raw material between two rotating grinding plates.

[0023] (Separation process) The reed fibers obtained in the fiber defibration process are sorted by length and used as raw materials for applications appropriate to their length. For example, long fibers with a length of 10 mm or more are suitable as fiber raw materials for spinning and blended yarn. On the other hand, short fibers with a length of less than 10 mm are suitable for pulp for paper products.

[0024] (Dehydration / drying process) The separated reed fibers are dehydrated using a dehydrator. At this time, the long fibers are loosened after dehydration and before drying to prevent them from sticking together. When loosening the reed fibers, care must be taken not to cut the fibers. In this regard, since reed fibers are more brittle than the fibers obtained from wood, using mechanical means such as a compressor will result in a large amount of breakage. For this reason, at present, the most efficient way to loosen the long reed fibers is by hand.

[0025] The dehydrated short fibers and the long fibers that have been loosened after dehydration are then dried. Methods for drying include using a hot air dryer or fan, or drying in the sun. However, when using a hot air dryer, care must be taken as using too high a temperature can result in the reed fibers losing their antibacterial properties. For this reason, drying by blowing air or drying in the sun is the preferred method of drying. Powders produced during the dehydration and drying process can be used as raw materials for papermaking. Furthermore, other residues produced during the above manufacturing processes can be used as soil conditioners or compost.

[0026] (Application to paper products) The reed fiber obtained by the manufacturing method of the present invention can be used like pulp for paper products that retain the antibacterial component derived from reeds. Reed fiber can be made into paper products (reed paper) through a normal papermaking process. It can also be made into 100% reed paper made only from reed fiber. On the other hand, it can be mixed with pulp obtained from other wood and used as reed fiber mixed reed paper. However, in order to exert the antibacterial properties derived from reeds, it is necessary to use reed fiber as 30 wt% or more of the paper raw material. The paper manufacturing process is roughly divided into a pulping process, a raw material preparation process, and a papermaking process. When manufacturing reed fiber mixed reed paper, reed fiber can be mixed with other wood in any of these processes to make paper. However, in order to make paper while maintaining the antibacterial component derived from reeds, it is preferable to mix pulp and reed fiber after the raw material preparation process and before the papermaking process. This is because the antibacterial component derived from reeds is likely to fall off when reed fiber goes through the pulping process or raw material preparation process. Also, as the proportion of reed fiber increases, the paper product will feel rougher, but if this is viewed as part of the texture, it does not impair the functionality of the paper product. For this reason, reed paper made from 100% reed fiber can also be used industrially.

[0027] (Blended yarn, application to fabric products) The reed fiber obtained by the manufacturing method of the present invention can be blended with other raw fibers such as cotton and spun into a blended yarn that retains the antibacterial component derived from reed. The blended yarn obtained can be woven into a fabric that retains the antibacterial component derived from reed through a general weaving process. The optimal ratio of reed fiber in the raw material of the blended yarn is 30 to 80 wt%. In order to exert the antibacterial properties derived from reed, it is necessary for the raw material to be 30 wt% or more of reed fiber. On the other hand, a blended yarn with more than 80 wt% of reed fiber does not have the strength generally required and is easily broken, making it difficult to fully exert the performance as a thread.

[0028] (Antibacterial ingredient) The present invention is aimed at producing reed fiber and paper products, blended yarns or cloth products using the reed fiber by a method that does not impair the antibacterial component contained in the raw material, the virgin reed. Specifically, the antibacterial component contained in the virgin reed is a hydrolyzable tannin having a gallic acid skeleton. Tannin is a general term for polyphenol compounds contained in the leaves, fruits, seeds, roots, etc. of plants, and is not a term that indicates a specific chemical structure. The specific chemical structure of the tannin contained in the virgin reed has not been clarified at present. Therefore, in the examples of the present invention described below, the presence of tannin derived from the virgin reed is not directly confirmed in the reed fiber and its products, but rather, whether or not they exhibit antibacterial properties is confirmed to confirm the effect of the present invention and to infer the presence of tannin derived from the virgin reed. EXAMPLES

[0029] (Changes due to concentration of retching solution) Several reeds over 10 months old that grow naturally in the Yodo River system were cut down. They were crushed by rolling and then cut to lengths of 50 mm ± 5 mm to produce reed stem pieces. These reed stem pieces were packed in groups of about 10, and chemical retching was carried out using four different concentrations of sodium hydroxide solution, as shown in Table 1. The retching conditions other than concentration were as follows: 50 g of reed stem pieces, water temperature 30°C, water volume 1 L, soaking time 41 hours.

[0030] After retching, each reed stalk piece was washed with water until the pH reached 7. From the washed reed stalk pieces, branches that could not be defibrated were removed and the pieces were defibrated using a disc refiner (KRK High Concentration Disc Refiner, product number No. 2500-I, manufactured by Kumagai Riki Kogyo Co., Ltd.). The defibrated reed fibers were evaluated. Table 1 summarizes the concentration (weight percent) of the sodium hydroxide aqueous solution used for retching, as well as the hardness of the reed stalk pieces after retching, the amount of branches that could not be defibrated, the fibers after defibration, and the presence or absence of antibacterial properties.

[0031] [Table 1]

[0032] From Table 1, it can be seen that in chemical retching, in the case of experiment number 1 where the concentration of the sodium hydroxide aqueous solution was 0.5 wt%, workability was poor and there were many branches that could not be defibrated, making it impractical. On the other hand, in the cases of experiment numbers 2-6 where the concentration of the sodium hydroxide aqueous solution was 0.8 wt% or more, workability was good, there were few branches that could not be defibrated, and it can be seen that it is economically feasible.

[0033] (Manufacturing of reed fiber) Several reeds over 10 months old that grow naturally in the Yodo River system were cut down. They were crushed by rolling and then cut to lengths of 50 mm ± 5 mm to produce reed stem pieces. These reed stem pieces were packed in groups of about 10 and subjected to chemical retching under the following conditions: 50 g reed stem pieces, 1.0 wt% sodium hydroxide aqueous solution, water temperature 30°C, water volume 1 L, soaking time 41 hours.

[0034] After retching, each reed stem piece was washed with water until the pH reached approximately 7. From the washed reed stem pieces, branches that could not be defibrated were removed and the pieces were defibrated using a disc refiner (KRK High Concentration Disc Refiner, product number No. 2500-I, manufactured by Kumagai Riki Kogyo Co., Ltd.). Of the defibrated reed fibers, those less than 10 mm in length were separated into short fibers, and those 10 mm or longer were separated into short fibers. Both the short and long fibers were dehydrated using a dehydrator. After dehydration, the long fibers were disintegrated by hand. Then, both the short and long fibers were dried using a blower.

[0035] (Manufacturing of reed paper) The reed fiber short fibers obtained above (30 wt%) and virgin wood pulp (70 wt%) were mixed to produce pulp raw material, and reed paper containing 30 wt% reed fiber was produced through a papermaking process.

[0036] (Blended Yarn Manufacturing) The above-obtained long reed fiber (30 wt%) and cotton fiber (70 wt%) were blended and spun to produce a blended yarn containing 30 wt% reed fiber.

[0037] (Antibacterial properties confirmation test derived from reeds) Antibacterial tests were conducted on the reed paper containing 30 wt% reed fiber, the blended yarn containing 30 wt% reed fiber, and the reed stalks themselves for reference. The tests were conducted according to the bacterial liquid absorption method described in "Antibacterial test methods and antibacterial effects of textile products" specified in JIS-L-1902. According to this test, an antibacterial activity value of 2.2 or higher is considered to have antibacterial properties.

[0038] As a result, the antibacterial activity value of the reed paper containing 30 wt% reed fiber was 5.9, the antibacterial activity value of the blended yarn containing 30 wt% reed fiber was 3.8, and the antibacterial activity value of the reed stalk itself was 6.0. This shows that reed stalks inherently have high antibacterial activity, and according to the manufacturing method of the present invention, even if they are mixed in a specified ratio to produce paper products or blended yarn, the antibacterial activity derived from the reed remains, so the product itself exhibits antibacterial properties.

[0039] (Antibacterial performance evaluation of reed fiber: Additional information) Sample preparation [Sample A] Several reeds over 10 months old that grow naturally in the Yodo River system were felled. They were crushed by rolling them. Chemical retching was then carried out. The conditions for chemical retching were 5L of water, 2wt% sodium hydroxide aqueous solution, 28℃ water temperature, and 72 hours of immersion time. After retching, the reed stalks were washed with water until the pH reached 7. They were crushed again with a roller, then cut into pieces of 50mm±5mm, and defibrated using a disc refiner (KRK high-density disc refiner, product number No. 2500-I, manufactured by Kumagai Riki Kogyo Co., Ltd.) to obtain sample A, which is reed fiber.

[0040] [Sample B] Several reeds over 10 months old that grow naturally in the Yodo River system were felled. They were crushed by rolling, then cut into lengths of 50 mm ± 5 mm to produce reed stalk pieces, which were then packed in bags of approximately 10 pieces each. These were then subjected to chemical retching. The conditions for chemical retching were 5 L of water, 1 wt% sodium hydroxide aqueous solution concentration, 28°C water temperature, and 72 hours of immersion time. After retching, the reed stalk pieces were washed with water until the pH reached approximately 7. The washed reed stalk pieces were defibrated using a disc refiner (KRK High Concentration Disc Refiner, product number No. 2500-I, manufactured by Kumagai Riki Kogyo Co., Ltd.) to obtain fiber B.

[0041] Preparation of test bacteria solution Staphylococcus aureus (ATCC 6538P) was cultured in 2xYT broth at 35°C for 24 hours with shaking. The culture was collected by centrifugation and the turbidity (OD 600 The bacteria were suspended in sterile water so that the bacterial count was approximately 1.0. This suspension was diluted 10-fold with sterile water to prepare a microbial suspension. 1.0 mL of this microbial suspension was mixed with 0.5 mL of 10-fold diluted normal bouillon medium and 8.5 mL of sterile water to prepare a test bacterial solution.

[0042] Sample preparation 0.4 g of the test samples (samples A and B) and a nonwoven fabric to be used as a comparison (control) were placed in 50 mL glass vials, sterilized in an autoclave (121°C, 15 minutes), and then dried overnight in a dryer at 55°C to prepare the test samples.

[0043] Antibacterial testing 0.2 mL of the test bacteria liquid was added to the test sample, and the container was covered and incubated at 35°C for a certain period of time. After a certain period of time, each test sample was collected, and 20 mL of SCDLP medium was added to wash out the microorganisms. This procedure was carried out twice, with the test samples collected 6, 12, and 24 hours later in the first procedure, and 12, 18, and 24 hours later in the second procedure. The washed-out liquid was serially diluted 10-fold with sterile water, and 0.1 mL of the undiluted solution and each diluted solution were applied to a standard agar medium, and then incubated at 35°C for 48 hours. In addition, 1.0 mL of the undiluted washed-out liquid was added to a standard agar medium by the pour method, and incubated in the same manner. After incubation, the number of colonies that had grown was counted to calculate the number of viable bacteria. The number of viable bacteria at each incubation time was the average of the values ​​obtained from all test samples (three or more samples) obtained in two tests. The change over time in the number of viable bacteria obtained for each sample is shown in Table 2.

[0044] [Table 2]

[0045] From Table 2, in the control, almost no change in viable cell count over time was observed. In sample A, a decrease in viable cell count was observed from 18 hours. In sample B, a decrease in viable cell count was observed from 12 hours. It can be seen that sample B is more effective at reducing viable cell count than sample A. [Industrial Applicability]

[0046] As described above, the reed fiber manufacturing method of the present invention makes it possible to obtain paper products, blended yarns, and even fabrics that retain the antibacterial properties inherent to reeds, making it a method with high industrial applicability.

Claims

1. A method for producing reed fiber by obtaining fiber from reed without losing the antibacterial activity inherent to the reed plant, comprising the steps of: A cutting process for cutting the reed stems into pieces having a length within a range of 10 to 100 mm; and a retching process in which the cut reed stalk pieces are immersed in a sodium hydroxide solution having a concentration of 0.8 wt % or more at a water temperature of 20 to 30° C. for 12 to 72 hours to separate the lignin in the reed stalk pieces. Manufacturing method.

2. 2. The method according to claim 1, wherein a predetermined number of reed stem pieces obtained in the cutting step are packed in a liquid-permeable and alkali-resistant bag, and then subjected to the retching step.

3. In a method for manufacturing paper products, the steps are pulping, raw material preparation, and papermaking in that order. After the raw material preparation process and before the papermaking process, pulp obtained from other wood materials is mixed with the reed fibers obtained by the manufacturing method according to claim 1, and then the papermaking process is carried out. In addition, in the above-mentioned mixing, the reed fiber is added in an amount of 30 wt% or more relative to the total amount of the papermaking raw material. This method obtains reed paper, which is paper containing reed fibers, and produces a paper product while maintaining the antibacterial component derived from reeds.

4. A method for producing a blended yarn by spinning a plurality of plant fiber raw materials, comprising the steps of: A method for producing a blended yarn by adding reed fiber obtained by the method described in claim 1 as a fiber raw material in an amount of 30 to 80 wt % relative to the total raw material, and spinning the blended yarn while maintaining the antibacterial properties derived from the reed.

Citation Information

Patent Citations

  • Water absorptive paper product

    JP2000262431A

  • Waste water treatment apparatus, column, and waste water treatment method

    JP2014057919A

  • Reed fine fiber, spun yarn thereof, and non-woven fabric

    JP2022102994A

  • Rush microfiber, rush spun yarn, and method for producing rush microfiber