Skin material, skin material composite, method for producing skin material and method for producing skin material composite
The skin material with through holes and recessed portions addresses the lack of unique design and breathability in conventional synthetic leather by enhancing air permeability and offering a novel aesthetic through varying hole sizes and shapes, combined with a cushion layer.
Patent Information
- Application Number
- JP2020160876
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-25
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-09-25
AI Technical Summary
Conventional synthetic leather materials lack a unique design effect when viewed from a distance, and existing three-dimensional skin materials do not focus on achieving novel designs, while also failing to provide high air permeability and breathability equivalent to natural leather.
A skin material with through holes penetrating the thickness direction, featuring varying hole sizes and shapes, recessed portions with a depth of 0.2 mm or more, and a combination of perforated and non-perforated regions, along with a cushion layer, to enhance air permeability and achieve a distinctive design.
The skin material achieves high air permeability and a novel design that differs from conventional materials, providing a unique appearance and improved breathability through a simple manufacturing process.
Smart Images

Figure 0007583568000003 
Figure 0007583568000004 
Figure 0007583568000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a skin material, a skin material composite, a method for manufacturing a skin material, and a method for manufacturing a skin material composite. [Background technology]
[0002] Synthetic resin skin materials, which have excellent durability, are widely used in place of natural leather and fiber sheets for automobile interior parts such as instrument panels, door trims, seats, and ceilings, railway car and aircraft interior parts such as trims, seats, and ceilings, furniture, shoes, footwear, bags, interior and exterior components for building decoration, clothing covering materials and linings, wall covering materials, etc. For example, with regard to automobile interior parts, as vehicles become more luxurious, it has become important to impart a luxurious feel to interior covering materials. There is also a demand for breathability equal to or greater than that of natural leather. Conventionally, perforated skin materials have been known in which a laminated sheet used as synthetic leather is perforated to provide it with moisture permeability, breathability, and design features, thereby creating a dot pattern of through holes with a diameter of about 1 mm.
[0003] Such perforated covering materials have attracted attention as materials that are both breathable and attractive, and are used, for example, as covering materials for automobile seats. However, the holes formed in the synthetic leather for purposes such as ventilation are uniform in shape and arranged regularly and evenly over the entire surface of the synthetic leather, and further improvement is required from the standpoint of improving design.
[0004] With the aim of improving the design of perforated skin materials, a perforated leather-like sheet has been proposed in which the presence of a nonwoven fabric on the inner surface of the through holes formed in the synthetic leather is made visible, thereby emphasizing the design of the through holes (see Patent Document 1). A decorative sheet has been proposed in which a laminated sheet has a colored layer and an opaque skin layer with a hue different from that of the colored layer, and a plurality of holes are provided that penetrate at least the colored layer and the opaque skin layer and allow the color of the colored layer to be visually recognized when viewed from the skin layer side (see Patent Document 2). This decorative sheet is said to exhibit a design effect not seen in conventional decorative sheets, in that the hue of the colored layer present below can be seen through the through holes depending on the angle at which the through holes are viewed. Furthermore, as a skin material that achieves a different design from conventional ones, a three-dimensional skin material with deeper recesses and projections than the commonly used synthetic leather that has shallow recesses and projections like leather has been proposed (see Patent Document 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-34355 A [Patent Document 2] Japanese Patent Application Publication No. 11-256483 [Patent Document 3] International Publication No. 2019 / 065758 Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the skin layers as described in Patent Documents 1 and 2, a unique design effect can be obtained when the through-hole and its surrounding area are visually confirmed, but when the skin material is used over a wide area such as an automobile seat, there is a problem that it is difficult to improve the design in terms of the appearance when viewed from a distance. For example, when riding in an automobile seat, the seat is viewed from a distance of about 30 cm, making it difficult to confirm the color tone inside the through-hole. Furthermore, the synthetic resin skin material described in Patent Document 3 provides a skin material having a three-dimensional shape with deep projections and recesses, but does not focus on achieving a novel design. Nowadays, people's values are becoming more diverse, and new designs that differ from conventional designs are being demanded for perforated skin materials that are designed to provide breathability.
[0007] An object of the embodiments of the present invention is to provide a skin material which has through holes, is highly breathable, and can achieve a new design different from that of conventionally known skin materials, and a skin material composite including the skin material. An object of another embodiment of the present invention is to provide a method for producing a skin material, which can produce, in a simple process, a skin material that has through holes, is highly breathable, and can achieve new designs different from those of conventionally known skin materials, and a method for producing a skin material composite including the skin material. [Means for solving the problem]
[0008] Means for solving the above problems include the embodiments shown below. <1> A skin material comprising at least a skin layer, the skin material having a plurality of through holes penetrating the skin material in a thickness direction, and a recess having a depth of 0.2 mm or more on at least one surface of the skin layer.
[0009] <2> The through holes are regularly arranged over the entire surface of the skin layer. <1> The skin material according to claim 1. <3> The through holes include a plurality of types of through holes having different sizes or shapes when the skin layer is viewed in plan. <1> or <2> The skin material according to claim 1. <4> When the skin material is viewed from above, it has a perforated region having through holes and a non-perforated region having no through holes. <1> ~ <3> 13. A skin material according to any one of claims 1 to 12. <5> Only the perforated area has a recess having a depth of 0.2 mm or more. <4> The skin material according to claim 1. <6> Only the non-perforated region has the recess having a depth of 0.2 mm or more. <4> The skin material according to claim 1. <7> The surface of the skin layer has a base fabric on the side opposite to the side having a recess with a depth of 0.2 mm or more. <1> ~ <6> 13. The skin material according to claim 12,
[0010] <8> <1> ~ <7> and a cushion layer, in this order, wherein the skin has the recessed portion having a depth of 0.2 mm or more on a surface opposite to a surface having the cushion layer.
[0011] <9> A method for producing a skin material, comprising the steps of: forming a skin material substrate having at least a skin layer; forming a plurality of through holes in the skin material substrate; and contacting one surface of the skin material substrate with an embossing roll or an embossing plate to form recesses having a depth of 0.2 mm or more. <10> A method for producing a skin material composite, comprising the steps of: forming a skin material substrate having at least a skin layer; forming a plurality of through holes in the skin material substrate; bonding a cushion layer to a surface of the skin material substrate opposite to the surface having the skin layer; and contacting an embossing roll or an embossing plate with the surface having the skin layer of the skin material substrate bonded to the cushion layer, to form recesses having a depth of 0.2 mm or more. Effect of the Invention
[0012] According to the embodiments of the present invention, it is possible to provide a skin material that has through holes, is highly breathable, and can achieve a new design different from that of conventionally known skin materials, and a skin material composite including the skin material. According to another embodiment of the present invention, it is possible to provide a method for producing a skin material, which can produce, in a simple process, a skin material that has through holes, is highly breathable, and can achieve a new design different from that of conventionally known skin materials, and a method for producing a skin material composite including the skin material. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a schematic plan view showing an example of an arrangement of regularly arranged through holes, in which the through holes are located at the lattice points of a square lattice in plan view. [Diagram 2]FIG. 1 is a schematic diagram showing an example of an arrangement of regularly-arranged through holes, and is a schematic plan view of an embodiment in which the through holes are arranged in overlapping hexagons of similar shapes but different sizes. [Diagram 3] FIG. 1 is a schematic plan view showing an example of a method for checking perforated and non-perforated regions in a skin material of the present disclosure. [Figure 4] FIG. 4 is a schematic plan view showing an example of a method for checking perforated and non-perforated regions in a skin material according to the present disclosure, according to an embodiment different from that shown in FIG. 3. [Diagram 5] FIG. 5(A) is a plan view showing a skin material of Example 1 which is a first aspect of the skin material of the present disclosure, and FIG. 5(B) is a schematic cross-sectional view showing the skin material of Example 1. [Figure 6] FIG. 6(A) is a plan view showing a skin composite of Example 2 which is a first embodiment of the skin composite of the present disclosure, and FIG. 6(B) is a schematic cross-sectional view showing the skin composite of Example 2. [Figure 7] FIG. 7(A) is a plan view showing a skin material of Example 3 which is a second embodiment of the skin material of the present disclosure, and FIG. 7(B) is a schematic cross-sectional view showing the skin material of Example 3. [Figure 8] FIG. 8(A) is a plan view showing a skin composite of Example 4, which is a second embodiment of the skin composite of the present disclosure, and FIG. 8(B) is a schematic cross-sectional view showing the skin composite of Example 4. [Figure 9] FIG. 9(A) is a plan view showing a skin material of Example 5, which is the third embodiment of the skin material of the present disclosure, and FIG. 9(B) is a schematic cross-sectional view showing the skin material of Example 5. [Figure 10] FIG. 10(A) is a plan view showing a skin composite of Example 6, which is the third embodiment of the skin composite of the present disclosure, and FIG. 10(B) is a schematic cross-sectional view showing the skin composite of Example 6. [Figure 11] FIG. 11(A) is a plan view showing a skin material of Example 7, which is the fourth embodiment of the skin material of the present disclosure, and FIG. 11(B) is a schematic cross-sectional view showing the skin material of Example 7. [Figure 12]FIG. 12(A) is a plan view showing a skin composite of Example 8, which is the fourth embodiment of the skin composite of the present disclosure, and FIG. 12(B) is a schematic cross-sectional view showing the skin composite of Example 8. [Figure 13] FIG. 13(A) is a plan view showing a through hole pattern of a conventional skin material having through holes of the same circular shape and the same diameter in accordance with Comparative Example 1, and FIG. 13(B) is a schematic cross-sectional view of the skin material of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] In the present disclosure, a numerical range described using "to" indicates a numerical range that includes the numerical values before and after "to" as the lower and upper limits. In the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in the present disclosure. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples. Also, in the present disclosure, combinations of two or more preferred aspects are more preferred aspects. In the present disclosure, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved. In this disclosure, components shown with the same reference numerals in each drawing are meant to be the same components. It should be noted that the drawings are merely schematic illustrations of examples of the embodiments of the present disclosure, and the dimensional ratios in each drawing do not necessarily represent the actual dimensional ratios.
[0015] Hereinafter, in this disclosure, the skin material composite may be simply referred to as the "composite." In this disclosure, the skin material has a sheet-like form, the maximum area of the sheet-like skin material is referred to as the "face" of the skin material, and the length of the cross section perpendicular to the "face" direction of the skin material is referred to as the "thickness" of the skin material. The "through hole" of the skin material means a hole that passes through the sheet-like skin material in the thickness direction. Therefore, when the skin material has a single-layer structure consisting of only a skin layer, it means a hole that passes through the skin layer, and when the skin material has a multi-layer structure having a skin layer on a base fabric, for example, it means a hole that passes through the skin layer and the base fabric. In this disclosure, the "depth of a recess" refers to the distance from the surface of the skin layer in an area where no recesses are formed in the skin to the bottom of a recess formed in the skin. In this disclosure, a sheet-like skin precursor having at least a skin layer and before the through-holes and recesses having a depth of 0.2 mm or more are formed is referred to as a "skin substrate." In this disclosure, the "skin" refers to a finished skin in which the through-holes and recesses having a depth of 0.2 mm or more are formed in the skin substrate.
[0016] The skin material, composite, and manufacturing method thereof according to the present disclosure will be described in detail below with reference to specific examples. The specific examples shown below are one embodiment of the present disclosure, and the present disclosure is not limited to the specific examples shown below, and various modifications can be made without departing from the spirit of the present disclosure.
[0017] [Skin material] The skin material of the present disclosure is a skin material comprising at least a skin layer, the skin material having a plurality of through holes penetrating the skin material in a thickness direction, and at least one surface of the skin layer having a recess having a depth of 0.2 mm or more. The through holes function as ventilation holes for the skin material. The skin material serving as the base material for forming the through-holes is not particularly limited in terms of layer structure, materials for forming the layers, etc., except that it has a skin layer as a decorative layer. Examples of skin materials include natural leather, artificial leather, synthetic leather, decorative films used in the interiors of vehicles and buildings, etc. The synthetic leather includes so-called PVC leather having a skin layer containing polyvinyl chloride (PVC). The skin material may have a single-layer structure consisting of only a skin layer, or may have a multi-layer structure including other layers such as a base fabric, an adhesive layer, and an intermediate layer in addition to the skin layer. The skin material of the present disclosure exhibits a unique appearance due to a combination of a plurality of through holes in the skin material and recesses having a depth of 0.2 mm or more formed on the surface of the skin material.
[0018] The skin substrate before the through holes and recesses are formed is not particularly limited in terms of the material constituting the skin substrate, the layer structure of the skin substrate, etc., except that the skin substrate has a skin layer. The skin substrate becomes the skin of the present disclosure by forming the through holes and recesses with a depth of 0.2 mm or more.
[0019] <Epidermal layer> The surface layer of the skin material may be natural leather, or may be a synthetic resin surface layer formed by containing a synthetic resin. When natural leather is used as the skin layer, the skin material may be a single-layer skin material consisting of natural leather as the skin layer, or a multi-layer skin material having a base fabric on the side opposite to the grain side, which is the surface of the natural leather as the skin layer. Among these, from the viewpoint of better processability and design freedom, it is preferable that the surface layer contains a synthetic resin. There is no particular limitation on the synthetic resin contained in the surface layer, and it can be appropriately selected depending on the purpose. Examples of synthetic resins contained in the surface layer include urethane resin, polyvinyl chloride resin (PVC), acrylic resin, fluororesin, polyester resin, etc. Among these, urethane resin and PVC are preferred from the viewpoint of the retention of recesses formed in the surface layer.
[0020] Examples of polyurethanes that can be contained in the skin layer include polycarbonate-based polyurethanes, polyether-based polyurethanes, polyester-based polyurethanes, and modified products thereof, etc. Among these, polycarbonate-based polyurethanes are preferred from the viewpoint that the skin material of the present disclosure is used for applications requiring long-term durability, such as automotive interior materials and chairs. The polyurethane that can be contained in the surface layer can be appropriately selected from water-based polyurethanes, solvent-free polyurethanes, and solvent-based polyurethanes.
[0021] The PVC that can be contained in the skin layer can be any PVC that is generally used for skin materials, without any particular limitations.Specific examples include PVC homopolymers with an average degree of polymerization of 650 to 2000, preferably about 650 to 1800, and further copolymers of vinyl chloride with ethylene, vinyl acetate, methacrylic acid ester, etc., mainly made of PVC. Furthermore, mixed resins of the above-mentioned PVC homopolymers and copolymers containing structural units derived from vinyl chloride with polyester resins, epoxy resins, acrylic resins, vinyl acetate resins, urethane resins, acrylonitrile, styrene-butadiene copolymer resins, partially saponified vinyl alcohol, etc. can be used.
[0022] When the skin layer contains a synthetic resin, it may contain only one type of synthetic resin, or may contain two or more types of synthetic resin. In addition to the synthetic resin as the main material, the composition for forming the skin layer (hereinafter sometimes referred to as the skin layer-forming composition) may contain known additives for the purpose of imparting various functions such as improving the appearance and feel to the skin layer, as long as the effects of the present disclosure are not impaired. The synthetic resin as the main material refers to a synthetic resin contained in an amount of 50% by mass or more based on the total amount of the skin layer-forming composition.
[0023] Examples of additives that may be contained in the skin layer-forming composition include plasticizers, stabilizers, crosslinking agents, crosslinking accelerators, fillers, colorants, film-forming assistants, flame retardants, and foaming agents. For example, the design of the resulting skin material can be improved by adding a colorant to the skin layer. The flame retardancy of the skin material can be improved by adding a known flame retardant such as a phosphorus-based, halogen-based, or inorganic metal-based flame retardant to the skin layer. When PVC is used as the synthetic resin, the processability and the feel of the resulting skin layer can be improved by adding a plasticizer.
[0024] There is no particular limitation on the method for forming the surface layer, and the surface layer can be provided by applying a surface layer forming method used for known synthetic leathers and surface materials. The surface layer can be formed, for example, by preparing a composition for forming a surface layer containing a resin and, if desired, other components such as a colorant and a solvent, and molding the resulting composition for forming a surface layer. The composition for forming the surface layer can be prepared by dissolving the resin in a solvent. Examples of the solvent that can be used for preparing the composition for forming the surface layer include dimethylformamide (DMF), methyl ethyl ketone (MEK), isopropyl alcohol (IPA), toluene, and the like, and a mixed solvent of two or more of these. Hereinafter, the solvents may be referred to by the above-mentioned abbreviations.
[0025] The surface layer can be formed by forming a film from a composition for forming a surface layer by a known film forming method such as a calendar method, a paste processing method, or a melt extrusion method. The skin layer can be formed by applying the composition for forming the skin layer onto a release paper. As the release paper, either a release paper for transferring a grain pattern or a smooth release paper can be used. By using the release paper for transferring a grain pattern, a concave-convex pattern called a grain pattern can be formed on the surface of the skin layer.
[0026] The thickness of the skin layer is appropriately selected depending on the intended use of the skin material. When the skin material has a single-layer structure consisting of only a skin layer, the thickness of the skin layer after drying is preferably 0.45 mm to 1.8 mm, and more preferably 0.9 mm to 1.2 mm, from the viewpoint that the necessary strength of the skin layer is easily maintained after perforation processing. When the skin material has a multi-layer structure having a skin layer on the base fabric surface, the thickness of the skin layer after drying is preferably 0.25 mm to 0.8 mm from the viewpoints of recess formability and strength. When there are two or more skin layers, the thickness of the skin layer refers to the total thickness of the multiple skin layers. The thickness of the base layer, the thickness of the skin material described below, the base fabric contained in the skin material, and other optional layers can be measured by observing a cut surface obtained by cutting the skin material perpendicular to the surface direction. In the present disclosure, the thickness of the skin layer is determined by measuring the thickness of five randomly selected points on the cut surface of the skin layer or a skin material having a skin layer, and calculating the arithmetic average of the thicknesses. The thicknesses of the skin material and other layers of the skin material can also be measured in the same manner. Therefore, in this disclosure, the thickness of each layer in the skin material refers to the thickness of each layer after it has been dried.
[0027] The skin material of the present disclosure may have a single-layer structure consisting of only a skin layer, or may have a multi-layer structure including layers other than the skin layer.
[0028] <Base fabric> From the viewpoint of improving strength and flexibility, the skin material of the present disclosure may further have, in addition to the skin layer, a base fabric on the surface of the skin layer opposite the side having the recess with a depth of 0.2 mm or more. A multi-layered skin material having a base fabric and a skin layer is a skin material having a basic structure that is widely used for synthetic leather, artificial leather, and the like.
[0029] There are no particular limitations on the base fabric, so long as it has the necessary strength and flexibility, and the resulting skin material has the desired stretchability. Examples of fibers used for the base fabric include synthetic fibers such as polyester, polyamide, polyacrylonitrile, and polyvinyl alcohol, and natural fibers such as cotton and hemp, and may be selected according to the purpose.
[0030] The base fabric may be any of woven fabric, knitted fabric, and nonwoven fabric. Among these, knitted fabric is preferred from the viewpoint of better processability of the skin material, particularly better formability of recesses. Examples of knitted fabrics include warp knitted tricot knitted fabrics, double raschel knitted fabrics, circular knitted pique knitted fabrics, interlock knitted fabrics, mocrody knitted fabrics, and weft knitted fabrics, with interlock knitted fabrics, which are a type of double-sided knitting, being more preferred.
[0031] The basis weight of the base fabric used for the skin material is set to 30 g / m from the viewpoints of better moldability, appearance after molding, and texture. 2~400g / m 2 is preferred, and 30 g / m 2 ~300g / m 2 is more preferred. In the case of a knitted fabric, for example, the basis weight of the base fabric can be adjusted by the structure of the knitted fabric, the thickness of the fibers used in knitting, the structure, the density of the fibers, and the like.
[0032] The thickness of the base fabric used for the skin material is preferably 0.2 mm to 1.4 mm, and more preferably 0.2 mm to 1.0 mm, from the viewpoints of better molding processability, and better appearance and feel after molding.
[0033] The skin material may further have an optional layer, if necessary, in addition to the skin layer and the base fabric that is provided as desired. The optional layer may include an adhesive layer, a foamed resin layer, a surface treatment layer, an intermediate layer, etc.
[0034] The thickness of the skin material is appropriately selected depending on the intended use of the skin material. From the viewpoint that the necessary strength of the skin layer is easily maintained after perforation processing, the thickness of the skin layer is preferably 0.45 mm to 1.8 mm, and more preferably 0.9 mm to 1.2 mm. In the present disclosure, the thickness of the skin material substrate refers to the thickness of the skin layer itself when the skin material has a single-layer structure consisting of only a skin layer, and refers to the total thickness of the skin material in a multi-layer structure when the skin material has a multi-layer structure including, for example, an optional layer such as a base fabric in addition to the skin layer. According to the investigations of the present inventors, it has been confirmed that there is no change in the thickness of the skin material after the through holes are provided, compared to the thickness of the skin material base material before the through holes are provided. The method of manufacturing the skin material, for example, the method of drilling through holes in the skin material and the method of forming recesses in the skin material, will be described in detail later.
[0035] <any layer> (1. Adhesive layer) The skin material of the present disclosure may have an adhesive layer. For example, when the skin material has a base fabric, the adhesive layer may be provided between the skin layer and the base fabric to improve the adhesion between the base fabric and the skin layer. Also, when an optional layer is provided between the skin layer and the base fabric, the adhesive layer can improve the adhesion between the optional layer formed adjacent to the base fabric and the base fabric. The adhesive constituting the adhesive layer is not particularly limited, and examples thereof include adhesives containing resins such as urethane resins, polyvinyl chloride, polyvinylidene chloride, polystyrene, and acrylic resins. Examples of the urethane resin contained in the adhesive include resins selected from polycarbonate-based polyurethanes, polyether-based polyurethanes, polyester-based polyurethanes, and modified versions of these. Among these, from the viewpoint of improving the various performances required of the skin material, adhesives containing urethane resin or polyvinyl chloride resin are preferred, and adhesives containing polycarbonate-based polyurethane are more preferred. From the viewpoint of improving adhesion between the base fabric and the adjacent layer and improving moldability, the resin contained in the adhesive preferably has a 100% modulus at 20°C of 1.0 MPa to 6.0 MPa, and more preferably 1 MPa to 3 MPa. The thickness of the adhesive is preferably from 2.0 μm to 80.0 μm, and more preferably from 25.0 μm to 60.0 μm, from the viewpoints of further improving the adhesion between adjacent layers and improving the texture. The thickness of the adhesive layer can be controlled by the amount of adhesive applied.
[0036] (2. Surface treatment layer) The skin material of the present disclosure may have a surface treatment layer. For example, when the skin material of the present disclosure has a base fabric, the surface treatment layer may be provided on the surface of the skin layer opposite to the surface on the base fabric side. The surface treatment layer is generally provided on the outermost surface of the skin material for the purpose of improving at least one of the appearance, texture (feel), and abrasion resistance of the skin material. Examples of the resin contained in the surface treatment layer include polyurethane, acrylic resin, fluororesin, polyvinyl chloride resin, etc., and from the viewpoint of further improving abrasion resistance and texture, it is preferable to contain polyurethane as the main component. The polyurethane may be a polycarbonate-based polyurethane, a polyether-based polyurethane, a polyester-based polyurethane, or a modified product thereof. From the viewpoint of various performances required of the skin material, it is preferable that the surface treatment layer contains a polycarbonate-based polyurethane.
[0037] The method for producing the surface treatment layer is not particularly limited, and the surface treatment layer is formed by applying a composition for forming the surface treatment layer obtained by dissolving the above-mentioned resin in an appropriate solvent, or a surface treatment agent composition containing the above-mentioned resin in the form of an aqueous emulsion or dispersion, to the surface of the epidermis layer. When preparing the composition for forming the surface treatment layer, examples of non-aqueous organic solvents that can be used to dissolve the resin include dimethylformamide (DMF), methyl ethyl ketone (MEK), isopropyl alcohol (IPA), toluene, etc., and mixed solvents of two or more of these. The aqueous emulsion resin or dispersion resin is a resin dispersion in which the resin is contained in a uniform emulsion state in an aqueous medium or a non-aqueous organic solvent (or dispersion medium). Examples of the aqueous medium used in the resin dispersion include water, alcohol, and a mixed medium of two or more of these. The non-aqueous solvent used in the resin dispersion can be the same as the above-mentioned solvents.
[0038] The surface treatment layer may contain other components in addition to the above-mentioned resin and solvent (dispersion medium). Examples of other components include a crosslinking agent, an organic filler, a lubricant, a flame retardant, etc. For example, when the surface treatment layer contains an organic filler, a lubricant, etc., the surface material is given a smooth feel and the abrasion resistance is further improved.
[0039] From the viewpoint of obtaining a sufficient effect of improving the abrasion resistance and texture of the skin material, the thickness of the surface treatment layer is preferably in the range of 1.0 μm to 10.0 μm, and more preferably in the range of 1.0 μm to 7.5 μm.
[0040] <Through hole> The skin material of the present disclosure has a plurality of through holes that penetrate the skin material in the thickness direction. The shape of the through hole, specifically, the shape of the through hole when viewed in plan from the skin layer side of the skin material, is not particularly limited, and can be any shape according to the desired design. The shape of the through holes in the skin material in a plan view may be selected from a circle, an ellipse, a polygon, a star, an irregular shape, and the like. It should be noted that when a radial shape such as a polygon or star is used, stress is likely to be concentrated at the acute apexes, making the material more susceptible to tearing, and so from the standpoint of maintaining the strength of the skin material, circular and elliptical shapes are preferred, and from the standpoint of freedom of design, a circular shape is more preferred. If the through holes are polygonal, star-shaped, or the like, stress is likely to concentrate at the apex, which may cause the skin material to be easily torn from the apex when applied to a substrate. From the viewpoint of achieving a skin material with better strength, therefore, apex-free shapes such as circular or elliptical shapes are preferred, with circular shapes being more preferred.
[0041] From the viewpoint of achieving a higher level of compatibility between the design provided by the through holes and the strength maintenance of the skin material, the diameter of the through holes is preferably 0.5 mm to 2.0 mm, and more preferably 1.0 mm to 1.5 mm, in terms of the equivalent circular diameter obtained by converting the area of the through holes in the skin layer into the diameter of a circle having the same area. From the same viewpoint, the porosity of the skin material is preferably 3% to 15%, and more preferably 5% to 10%. The porosity of the skin material means the ratio of the total area of a plurality of through holes present in a certain region to the area of the skin material when the skin material is viewed in plan from the skin layer side.
[0042] There is no particular limitation on the method for forming through holes in the skin material, and known methods can be used. Examples of the method for forming through holes include a punching method using a punching die and a laser punching method, and from the viewpoint of process simplicity, a punching method using a punching die is preferred. Note that when forming through holes of complex shapes such as irregular, star-shaped, or petal-shaped, the laser punching method is also effective.
[0043] <Concave portions with a depth of 0.2 mm or more> The skin material of the present disclosure has a recess having a depth of 0.2 mm or more on at least one surface of the skin layer. The skin material of the present disclosure achieves a distinctive design by combining the through-hole and the recess having a depth of 0.2 mm or more formed on the surface of the skin layer. The "depth of the recess" refers to the distance from the surface of the skin layer in an area where no recess is formed in the skin to the bottom of the recess formed in the skin. A specific method for measuring the depth of the recess will be described later. The depth of the recesses formed in the skin layer is 0.2 mm or more, and preferably 0.25 mm or more. There is no particular upper limit to the depth, but from the viewpoint of the strength and flexibility of the skin material, it can be 1.0 mm or less. In the skin material of the present disclosure, novel designs not previously available can be achieved by controlling the number, arrangement positions, etc. of the through holes and recesses with a depth of 0.2 mm or more. A recess depth of 0.2 mm or more is preferable because the presence of the recess is easily confirmed even when viewed from a distance from the skin material, and the novel design when combined with the through hole is easily recognized.
[0044] There is no particular limitation on the shape of the recesses formed in the skin layer in plan view. For example, in the case of continuous band-like recesses, the width of the recesses is preferably 10 mm to 50 mm, more preferably 13 mm to 40 mm, from the viewpoint of the tendency of affecting the appearance. Here, the width of the recesses refers to the distance perpendicular to the longitudinal direction of the skin material of the continuous band-like recesses when the recesses are viewed in plan view.
[0045] There is no particular limitation on the method for forming the recesses in the skin material, and known surface processing methods can be applied. From the viewpoint of the formability of the recesses and the simplicity of the process, it is preferable to apply embossing using an embossing roll or embossing plate. By controlling the height, shape, and arrangement position of the protrusions of the embossing roll or embossing plate, recesses having any depth and shape can be formed on the surface of the skin material having the skin layer.
[0046] In the skin material of the present disclosure, by adjusting the shape, hole diameter (hole size), number of holes, position of the holes, depth of recesses with a depth of 0.2 mm or more, size of the recesses in a plan view, position of the recesses, area of the recesses, etc., it is possible to provide a skin material with novel designs.
[0047] <Through hole arrangement> The through holes in the skin material may be regularly arranged over the entire surface of the skin layer. Here, the "regularly arranged" through holes refers to a state in which the through holes are arranged at equal intervals when the skin material is viewed in plan from the skin layer side, or a state in which the same pattern formed by a plurality of through holes is repeatedly arranged. FIG. 1 shows an example of a state in which through holes are arranged at equal intervals. FIG. 1 is a schematic plan view showing an example of an arrangement of regularly arranged through holes, and is a schematic plan view of an embodiment in which through holes 10 are arranged at the lattice points of a square lattice in a plan view. The square lattice shown in FIG. 1 is a virtual line showing the arrangement positions of the through holes 10, and by having the through holes 10 at the lattice points of the square lattice, the through holes 10 are arranged regularly at equal intervals. FIG. 1 shows an embodiment in which the through holes 10 are arranged at the lattice points of the square lattice, but in the case of a triangular lattice, the through holes are also arranged regularly by having the through holes at the lattice points of the triangular lattice.
[0048] Fig. 2 is a schematic diagram showing an example of an arrangement of regularly arranged through holes, and is a schematic plan view of an embodiment in which the through holes are arranged in a state of overlapping hexagons of similar shapes but different sizes. Fig. 2 shows a repetition of a hexagonal pattern formed by a plurality of through holes 12A, 12B, and 12C. The "regularly arranged" in the present disclosure includes cases where figures of the same pattern in plan view are repeatedly arranged in the same size or similar shapes of different sizes as shown in Fig. 2, without being limited to hexagons.
[0049] The through holes may include a plurality of types of through holes having different sizes or shapes when the skin layer is viewed in plan. In the embodiment shown in Fig. 2, the through holes constituting the hexagonal pattern include three types of through holes of different sizes, namely, a circular through hole 12A in a plan view, a circular through hole 12B having a diameter smaller than that of the through hole 12A, and a through hole 12C having a diameter even smaller than that of the through hole 12B. The through holes 12A, 12B, and 12C of different sizes are combined to form a hexagonal pattern, and a hexagonal pattern of through holes 12B having a diameter larger than that of the through hole 12C is formed outside the hexagonal pattern of through holes 12C, and a hexagonal pattern of through holes 12A having a diameter larger than that of the through hole 12B is formed outside the hexagonal pattern of through holes 12C, forming similar hexagonal patterns, which are regularly repeated to form a design. In Fig. 2, a plurality of hexagonal patterns are arranged in a plan view, which are formed by combining a plurality of through holes 12A, 12B, and 12C of different sizes. The hexagonal patterns are arranged in the width direction in a line symmetrical direction to the repeating pattern arranged in the length direction, and a unique design is expressed. By forming a hexagonal pattern by combining a plurality of through holes of different sizes, a more distinctive design is expressed by the through holes than by repeating patterns of through holes of the same size.
[0050] 2, there are three types of through holes with different hole diameters, but there may be two types of hole sizes, or there may be four or more types of through holes with different sizes. In addition, there may be multiple types of through holes with different shapes but the same size, for example, the same area in a plan view of the through holes, or there may be multiple types of through holes with different sizes and shapes.
[0051] The skin material of the present disclosure may have, when viewed in plan, a perforated region having through holes and a non-perforated region having no through holes.
[0052] A "perforated region" having through-holes and a "non-perforated region" having no through-holes in the present disclosure will be described with reference to the drawings. In the skin material of the present disclosure, a "perforated region" having through holes refers to a region that forms a series of polygons of a certain size and the same shape when adjacent through holes that are located at the shortest distance from each other are connected with a straight line. When a region that forms a series of polygons of a certain size and the same shape when the centers (hereinafter also referred to as center points) of the through holes in a plan view are connected with a straight line has polygons of multiple sizes, the region that forms the smaller polygon in area is defined as the "perforated region". In addition, when the skin material of the present disclosure has through holes of different shapes or the same shape but different diameters, the size of the polygon is determined by the distance between the center points of the through holes in a plan view of the imaginary line connecting the through holes. In the following description, unless otherwise specified, the arrangement of the through holes refers to the arrangement when the skin layer side of the skin material is viewed in plan.
[0053] 3 shows an embodiment in which a certain size of square is formed continuously when the through holes are connected by a straight line. The "perforated regions" where multiple squares are formed continuously are indicated by the symbols A-1 and A-2, and the "non-perforated regions" are indicated by the symbols B-1, B-2, and B-3. In Figure 3, A-1 and A-2, in which multiple squares are formed in succession, are "perforated regions" in the present disclosure, while B-1, in which no squares are formed even though the periphery is surrounded by a perforated region, B-2, in which squares are formed but not continuous, and B-3, in which squares are formed in succession but the squares are larger, are "non-perforated regions" in the present disclosure. Fig. 4 shows an embodiment in which equilateral triangles of a certain size are formed continuously when the through holes are connected by a straight line. In Fig. 4, A-3 where equilateral triangles are formed continuously is a "perforated region", and B-4 and B-5 where equilateral triangles are not formed continuously are "non-perforated regions". The skin materials having the through-hole patterns shown in FIG. 3 and FIG. 4 both correspond to skin materials having perforated regions and non-perforated regions. In the skin material shown in Fig. 2, which shows an example of an arrangement of regularly-spaced through holes, similar regular hexagons are formed by overlapping circular through holes of different sizes. In the embodiment shown in Fig. 2, the area occupied by the largest regular hexagon is the "perforated area", including the area where smaller similar regular hexagons are formed.
[0054] <Skin material composite> The skin material composite of the present disclosure is a skin material composite comprising the above-described skin material of the present disclosure and a cushion layer, in this order, and the skin material has a recess having a depth of 0.2 mm or more on the surface opposite to the side having the cushion layer.
[0055] (skin material) The configuration of the skin material in the composite is the same as that of the skin material of the present disclosure described above, and preferred examples are also the same. However, in the case of a composite having a cushion layer, the depth of the recess formed on the side of the skin material opposite to the side having the cushion layer, i.e., on the surface of the skin material facing the skin layer, is 0.2 mm or more. In the composite body of the present disclosure, by having a cushion layer with good elasticity, recesses having a depth of 0.2 mm or more can be formed more easily, and recesses having greater depths can also be formed.
[0056] (Cushion layer) The cushion layer is a layer formed from a synthetic resin having excellent elasticity, and there are no particular limitations on the synthetic resin used as long as the required elasticity can be achieved. Among these, from the viewpoint of light weight and good elasticity, a layer made of a synthetic resin foam is preferable. The cells in the foam may be open cells, closed cells, or may contain both. Examples of synthetic resins that can be used to form the cushion layer include polyurethane, polyvinyl chloride, polyolefin, and the like. From the viewpoint of elasticity, polyurethane is preferred, and soft polyurethane is more preferred.
[0057] Methods for forming a cushion layer on a urethane resin skin material include a method of adhering a cushion layer-forming material to the urethane resin skin material, and a method of applying a precursor of the cushion layer-forming material to the urethane resin skin material. The cushion layer may be formed, for example, by forming a foam raw material (a precursor of the material for forming the cushion layer) into a synthetic resin foam in advance and then adhering the foam raw material to form the cushion layer, or by applying a foam raw material (a precursor of the material for forming the cushion layer) containing a synthetic resin or a precursor of a synthetic resin directly to a urethane resin skin material and foaming it on the skin material to form a synthetic resin foam containing air bubbles. In particular, from the viewpoint of good cushioning properties and processability, it is preferable to use a synthetic resin foam as the cushion layer forming material for forming the cushion layer, and it is more preferable to use a soft polyurethane foam material having continuous cells.
[0058] The flexible polyurethane foam material is formed by reacting and foaming a foam raw material containing polyols, polyisocyanates, a blowing agent, and a catalyst. The flexible polyurethane foam material in the present disclosure refers to a material that contains polyurethane containing bubbles, is lightweight, generally has an open cell structure in which cells are interconnected, is flexible, and has recovery properties against pressure or deformation.
[0059] In the present disclosure, the flexible polyurethane foam material used to form the cushion layer is preferably a flexible slab polyurethane foam obtained by a slab foaming method. According to the slab foaming method, the mixed and stirred foam raw material (reaction mixture) is discharged onto a belt conveyor, and while the belt conveyor is moving, the foam raw material reacts at room temperature and atmospheric pressure, and naturally foams to produce a soft polyurethane foam. The formed flexible polyurethane foam is sliced to a predetermined thickness to obtain a flexible polyurethane foam material for forming the cushion layer.
[0060] The cushion layer may be formed by a known method for forming a synthetic resin layer containing air bubbles therein, such as a method in which a foam raw material (precursor of a material for forming a cushion layer) containing a foaming agent and a synthetic resin or a synthetic resin precursor is applied to the base fabric side of the skin material, and then the foam is foamed and cured to form a cushion layer made of a synthetic resin foam (material for forming a cushion layer); or a method in which a shear force is applied to an uncured urethane resin precursor to cause mechanical foaming, and a urethane resin precursor (precursor of a material for forming a cushion layer) containing air bubbles is applied to the base fabric side of the skin material, and the urethane resin is cured to form a cushion layer.
[0061] The soft polyurethane foam material that forms the cushion layer is an elastic material, but when compressed within a certain temperature range, it can maintain its shape, i.e., can undergo plastic deformation. The plastic deformation temperature of the soft polyurethane foam material is preferably 130°C or higher, and more preferably 150°C or higher. When the plastic deformation temperature is 130° C. or higher, the moldability when forming recesses in the composite and the shape retention of the recesses after molding are further improved. The upper limit of the plastic deformation temperature is a temperature lower than the temperature at which the flexible polyurethane foam material thermally decomposes and melts, and from the viewpoint of productivity, it is preferably 250° C. or lower.
[0062] The density of the cushion layer is 15kg / m 3 ~100kg / m 3and preferably in the range of 18 kg / m 3 ~60kg / m 3 It is more preferable that the range is .
[0063] There is no particular limitation on the thickness of the cushion layer, but from the viewpoint of facilitating the formation of deep recesses, it is preferable that the thickness of the cushion layer is greater than the thickness of the skin material described above. In particular, from the viewpoint of easily exhibiting appropriate cushioning properties and providing better processability when forming deep recesses, the thickness of the cushion layer containing voids is generally preferably 1 mm to 15 mm, and more preferably 3 mm to 10 mm. The composite may have only one cushion layer or may have multiple cushion layers. When multiple cushion layers are included, the total thickness of the cushion layers is preferably within the preferred thickness range of the cushion layer described above.
[0064] There is no particular restriction on the method for bonding the skin material and the cushion layer. Examples of the bonding method include a method of bonding the skin material and the cushion layer using an adhesive and a method of bonding by a frame lamination method. The frame lamination method is a method in which the surface of the polyurethane foam material, which is the cushion layer, is heated by a flame (frame) such as a burner, the surface of the polyurethane foam material is thermally melted, the surface of the skin material opposite to the side having the skin layer is brought into contact with the melted portion, and the skin material is pressurized and cooled to bond the skin material and the cushion layer. The frame lamination method will be described in detail below. When an adhesive is used for bonding, a method of forming the adhesive layer, which is an optional layer described in the skin material, between the cushion layer and the skin material may be applied using the adhesive used for forming the adhesive layer. From the viewpoint of better productivity, when a soft polyurethane foam material is used as the cushion layer, it is preferable to adhere the surface material and the cushion layer by a frame lamination method.
[0065] (Concave depth of 0.2 mm or more) The skin material in the composite body of the present disclosure has a recess having a depth of 0.2 mm or more on the surface opposite to the side having the cushion layer. The depth of the recess formed in the composite is 0.2 mm or more, preferably 1.0 mm or more, and more preferably 1.5 mm or more. There is no particular upper limit to the depth, but from the viewpoint of the strength and flexibility of the composite, it can be 6.0 mm or less. In the composite of the present disclosure, novel designs not previously available can be achieved by controlling the number, arrangement positions, etc. of the through holes and recesses with a depth of 0.2 mm or more that the skin material has. In the composite body of the present disclosure, a recess having a depth of 0.2 mm or more provided on the skin side in combination with the through-holes realizes a distinctive design.
[0066] There is no particular limitation on the method for forming the recesses on the surface of the skin layer side of the composite, and any known surface processing method can be used. As in the above-mentioned formation of the recesses in the skin material, it is preferable to apply embossing using an embossing roll or embossing plate.
[0067] Hereinafter, an embodiment of the skin material of the present disclosure will be described with reference to the drawings as appropriate. Components indicated by the same reference numerals in each drawing in this disclosure are the same components. Note that descriptions of configurations and reference numerals that are duplicated in each drawing may be omitted. Also, the dimensional ratios in each drawing do not necessarily represent the actual dimensional ratios.
[0068] Fig. 5(A) is a plan view showing a first embodiment of the skin material of the present disclosure, and Fig. 5(B) is a schematic cross-sectional view showing the first embodiment of the skin material of the present disclosure. The skin material 14 shown in Fig. 5(A) and Fig. 5(B) has a plurality of through holes 10 of the same circular shape and size in plan view. 5(A) indicates the length direction of the skin 14 (the direction in which the skin is conveyed during production). Arrows in the following drawings also indicate the length direction of the skin. As shown in the plan view of Fig. 5(A), circular through-holes 10 of the same shape and size are formed at regular intervals over the entire surface of the skin layer in the skin material 14. In the longitudinal direction of the skin material, band-like recesses 16 with a depth of 0.25 mm are formed at regular intervals. As shown in the schematic cross-sectional view of FIG. 5(B), the skin material 14 has a skin layer 22 containing a synthetic resin on one side of a base fabric 18 via an adhesive layer 20, and has a plurality of through holes 10 that penetrate the skin material 14 in the thickness direction. The skin material 14 of the first embodiment of the present disclosure has a plurality of through holes 10 formed regularly over the entire surface of the skin material 14, i.e., on both the surface on which the recesses 16 are formed and the surface on which the recesses 16 are not formed, and the through holes 10 and the band-shaped recesses form a unique design. Here, the depth of the recess in the skin material refers to the distance α from the surface of the skin layer 22 in an area where no recess is formed in the skin material 14 (indicated by a dashed line in FIG. 5(B)) to the bottom of the recess formed in the skin material. In this embodiment, the depth of the recess is 0.25 mm. The depth α of the recesses in the skin material can be measured by observing a cut surface of the skin material cut perpendicularly to the surface direction. That is, the depth can be measured from the difference in thickness between the skin material in the region without the recesses and the skin material in the region where the recesses are formed. The depth of the recesses can be measured by a photograph of the cut surface taken with an electron microscope. In the present disclosure, the arithmetic average of the depths of the recesses at five randomly selected points on the skin material as a sample is used, as in the method for measuring the thickness of the skin layer or skin material.
[0069] Fig. 6(A) is a plan view showing a first embodiment of the composite of the present disclosure, and Fig. 6(B) is a schematic cross-sectional view showing the first embodiment of the composite of the present disclosure. The composite 24 shown in Fig. 6 has a plurality of through-holes 10 of the same circular shape and the same size in plan view. As shown in the schematic cross-sectional view of Fig. 6(B), the composite 24 has a skin material 14 having a plurality of through-holes 10 penetrating in the thickness direction, and a cushion layer 26. The skin material 14 in the composite 24 shown in Fig. 6(B) has the same layer structure as the first embodiment of the skin material of the present disclosure shown in Figs. 5(A) and 5(B), and is a skin material 14 having a skin layer 22 containing a synthetic resin on one surface of a base fabric 18 via an adhesive layer 20. Here, the depth of the composite recess refers to the distance β from the surface of the skin layer 22 in an area where no recess is formed in the skin material 14 of the composite 24 (shown by a dashed line in FIG. 6(B)) to the bottom of the recess formed in the skin material, and in this embodiment, the depth of the recess is 1.5 mm. The depth β of the recesses in the composite can be measured in the same manner as the depth α of the recesses in the skin material. That is, the depth can be measured by measuring the difference in thickness between the area of the composite that does not have a recess and the area where a recess is formed on a cut surface obtained by cutting the composite perpendicularly to the surface direction. The measurement can be performed using an electron microscope photograph of the cut surface of the composite.
[0070] Fig. 7(A) is a plan view showing a second embodiment of the skin material of the present disclosure, and Fig. 7(B) is a schematic cross-sectional view showing the second embodiment of the skin material of the present disclosure. Skin material 28 shown in Fig. 7(A) and Fig. 7(B) is circular in plan view and has three types of through holes 12A, 12B, and 12C of different sizes. As shown in the plan view of FIG. 7(A), three different sizes of circular through-holes 12A, 12B, and 12C are formed in the skin 28, and the through-holes of each size are regularly arranged in a strip shape at equal intervals parallel to the length of the skin 28, and the skin 28 also has a strip-shaped region without a through-hole in the length direction. In addition, the skin 28 has strip-shaped recesses 16A, 16B, and 16C with a depth of 0.2 mm formed at regular intervals in the length direction. In the skin 28 shown in FIG. 7(A) and FIG. 7(B), the recess 16A has a region with a through-hole and a region without a through-hole, the recess 16B is entirely a region with a through-hole, and the recess 16C has a region with a through-hole and a region without a through-hole, and the area of the region without a through-hole is larger than the area of the region without a through-hole in the recess 16A. As shown in the schematic cross-sectional view of FIG. 7(B), the layer structure of the skin material 28 has a skin layer 22 containing a synthetic resin on one side of a base fabric 18 via an adhesive layer 20, and has a plurality of through holes 12A, 12B and 12C penetrating the skin material 14 in the thickness direction, and has the same layer structure as the skin material 14 shown in FIG. 5(B) except that the through holes have different sizes. In the skin material 28 of the second embodiment of the present disclosure, the arrangements of the through holes 12A, 12B and 12C of different sizes in the recesses 16A, 16B and 16C formed in the skin layer parallel to the longitudinal direction of the skin material 28 are different from each other, thereby forming a distinctive design of the skin material 28. In the second embodiment of the skin material, the depth of the recesses is 0.20 mm.
[0071] Fig. 8(A) is a plan view showing a second embodiment of the composite of the present disclosure, and Fig. 8(B) is a schematic cross-sectional view showing the second embodiment of the composite of the present disclosure. The composite 30 shown in Fig. 8 has a plurality of through-holes 12A, 12B, and 12C that are circular in plan view and have different sizes. As shown in the schematic cross-sectional view of FIG. 8(B), the composite body 30 has a skin material 28 having a plurality of through-holes 12A, 12B, and 12C penetrating in the thickness direction, and a cushion layer 26. The skin material 28 in the composite 30 shown in FIG. 8(B) has the same layer structure as the second embodiment of the skin material of the present disclosure shown in FIGS. 7(A) and 7(B), and is a skin material 28 having a skin layer 22 containing a synthetic resin on one side of a base fabric 18 via an adhesive layer 20. In the composite 30 of the second embodiment, the recess depth is 1.0 mm. The composite 30 shown in Figs. 8(A) and 8(B) is circular in plan view, and has three types of through-holes 12A, 12B, and 12C of different sizes. As in the plan view of FIG. 7(A), the composite 30 shown in FIG. 8(A) has three different sizes of circular through holes 12A, 12B, and 12C formed therein, and the through holes of each size are regularly arranged in a strip shape at equal intervals parallel to the length direction of the skin layer, and there is also a strip-shaped region in the length direction that has no through holes. In addition, in the length direction of the composite 30, recesses 16A, 16B, and 16C with a depth of 1.0 mm are formed in strip shape at regular intervals. The design of the composite 30 shown in FIG. 8(A) and FIG. 8(B) in plan view is the same as that of the skin material 28 shown in FIG. 7(A) and FIG. 7(B) except for the depth of the recesses. The arrangement of the through holes 12A, 12B, and 12C of different sizes in the recesses 16A, 16B, and 16C formed in the skin layer parallel to the length direction of the composite 30 is different from each other, so that the composite 30 has a distinctive design. In the composite 30 of the second embodiment, the recess depth is 1.0 mm.
[0072] Fig. 9(A) is a plan view showing a third embodiment of the skin material of the present disclosure, and Fig. 9(B) is a schematic cross-sectional view showing the third embodiment of the skin material of the present disclosure. The skin material 32 shown in Fig. 9(A) and Fig. 9(B) has a plurality of through holes 10 of the same circular shape and size in plan view. 9(A) shows a third embodiment of a skin material 32 in which circular through holes 10 of the same shape and size are formed at regular intervals parallel to the longitudinal direction of the skin layer, and regions having through holes are formed at regular intervals between regions not having through holes 10. That is, the skin material 32 has regions having through holes and regions not having through holes. The skin material of the present disclosure may have recesses having a depth of 0.2 mm or more only in the non-perforated areas.
[0073] As described above, in the skin material 32, circular through-holes 10 of the same shape and size are formed regularly and at equal intervals parallel to the longitudinal direction of the skin layer, and regions having through-holes are formed at regular intervals between regions not having through-holes 10. Then, in the longitudinal direction of the skin material 32, only in the non-perforated regions not having through-holes 10, band-shaped recesses 16 having a depth of 0.2 mm are formed. In the skin material 32, recesses are formed in the areas where the through holes 10 are not formed, and therefore no through holes 10 are formed in the areas where the recesses 16 are formed. In a plan view, the skin material 32 has areas where no recesses are formed, in which the through holes 10 are regularly and repeatedly arranged at equal intervals, and recesses with a depth of 0.2 mm that do not have through holes 10. For this reason, the skin material 32 forms a distinctive design due to the arrangement of the recesses and through holes. As shown in the schematic cross-sectional view of FIG. 9(B), the skin material 32 has a skin layer 22 containing a synthetic resin on one side of a base fabric 18 via an adhesive layer 20, and has a plurality of through holes 10 penetrating the skin material 32 in the thickness direction. The layer structure of the skin material 32 is the same as that of the skin material 14 of the first embodiment of the present disclosure, except for the positions of the through holes and the depth of the recesses.
[0074] Fig. 10(A) is a plan view showing a third embodiment of the composite of the present disclosure, and Fig. 10(B) is a schematic cross-sectional view showing the third embodiment of the composite of the present disclosure. The composite 34 shown in Fig. 10(A) and Fig. 10(B) has a plurality of through-holes 10 of the same circular shape and the same size in plan view. As shown in the schematic cross-sectional view of Fig. 10(B), the composite 34 has a skin material 32 having a plurality of through-holes 10 penetrating in the thickness direction, and a cushion layer 26. The skin material 32 in the composite 34 shown in Fig. 10(B) has the same layer structure as the third embodiment of the skin material of the present disclosure shown in Figs. 9(A) and 9(B), and is a skin material 14 having a skin layer 22 containing a synthetic resin on one surface of a base fabric 18 via an adhesive layer 20. The depth of the recess in the composite 34 is 3.0 mm.
[0075] Similar to the plan view of Fig. 9(A), the composite 34 shown in Fig. 10(A) has a plurality of through-holes 10 of the same circular shape and the same size in plan view, and the through-holes 10 are regularly and repeatedly arranged only in the non-recessed regions of the composite 34. That is, the recesses 16 are formed only in the non-perforated regions, and the bottom surfaces of the recesses 16 are visually observed as a smooth surface. The composite 34 shown in Figures 10(A) and 10(B) has a distinctive design in that only in the areas of the composite 34 where the multiple regularly-repeated through holes 10 are not formed, i.e., in the non-perforated areas, there are recesses with a depth of 3.0 mm, the bottom of which reaches beyond the interface between the skin material and the cushioning layer.
[0076] Fig. 11(A) is a plan view showing a fourth embodiment of the skin material of the present disclosure, and Fig. 11(B) is a schematic cross-sectional view showing the fourth embodiment of the skin material of the present disclosure. The skin material 36 shown in Fig. 11(A) and Fig. 11(B) has a plurality of through holes 10 of the same circular shape and size in plan view. 11(A) shows a fourth embodiment of a skin material 36 in which circular through holes 10 of the same shape and size are formed regularly and at equal intervals parallel to the longitudinal direction of the skin layer, and regions having through holes are formed at regular intervals between regions not having through holes 10. That is, the skin material 36 has regions having through holes and regions not having through holes. The skin material of the present disclosure may have recesses with a depth of 0.2 mm or more only in the perforated areas.
[0077] In the longitudinal direction of the skin material 36, circular through-holes 10 of the same shape and size are regularly and evenly spaced in parallel with the longitudinal direction of the skin layer, and the regions having through-holes are formed at regular intervals through regions not having through-holes 10. In the longitudinal direction of the skin material 36, a band-shaped recess 16 having a depth of 0.20 mm is formed only in the perforated region having the through-holes 10. In the skin material 36, the through-holes 10 are formed only in the regions where the recesses 16 are formed, and therefore the through-holes 10 are visible in the region of the bottom surface of the recesses 16. In the regions where the through-holes 10 are not formed, i.e., the non-perforated regions, the recesses 16 are not formed. In the skin material 36, when viewed from above, the through-holes 10 are regularly and repeatedly arranged at regular intervals only in the regions where the recesses 16 are formed, and the regions where the recesses 16 are not formed do not have the through-holes 10, and a smooth skin layer is visible. For this reason, the skin material 36 forms a distinctive design due to the arrangement of the recesses 16 and the through-holes 10. As shown in the schematic cross-sectional view of FIG. 11(B), skin material 36 has a skin layer 22 containing a synthetic resin on one side of base fabric 18 via an adhesive layer 20, and has a plurality of through holes 10 penetrating skin material 36 in the thickness direction. The layer structure of skin material 36 is the same as that of skin material 14 of the first embodiment of the present disclosure, except for the positions of the through holes.
[0078] Fig. 12(A) is a plan view showing a fourth embodiment of the composite of the present disclosure, and Fig. 12(B) is a schematic cross-sectional view showing the fourth embodiment of the composite of the present disclosure. The composite 38 shown in Fig. 12(A) and Fig. 12(B) has a plurality of through-holes 10 of the same circular shape and the same size in plan view. As shown in the schematic cross-sectional view of Fig. 12(B), a composite 38 has a skin material 36 having a plurality of through-holes 10 penetrating in the thickness direction, and a cushion layer 26. The skin material 36 in the composite 38 shown in Fig. 12(B) has the same layer structure as the fourth embodiment of the skin material of the present disclosure shown in Figs. 11(A) and 11(B), and is a skin material 36 having a skin layer 22 containing a synthetic resin on one surface of a base fabric 18 via an adhesive layer 20. The depth of the recess in the composite 38 is 3.0 mm.
[0079] Similar to the plan view of Fig. 11(A), a plurality of through holes 10 of the same circular shape and size in plan view are regularly and repeatedly arranged at regular intervals in the composite 38 shown in Fig. 12(A). The recesses 16 of the composite 38 are formed only in the regions where the through holes 10 are formed, i.e., the perforated regions, and the through holes 10 are not formed in the non-perforated regions, and the regions where the recesses 16 are not formed are visually observed as a smooth surface. In the composite 38 shown in Figures 12(A) and 12(B), recesses 16 having a depth of 3.0 mm, with the bottom reaching a depth beyond the interface between the skin material and the cushioning layer, are formed only in the area where there are a plurality of regularly repeated through holes 10, and there are no recesses in the non-perforated area. Since there are no through holes on the convex surface on the skin material 36 side of the composite 38, a distinctive design is formed.
[0080] In both the skin material and the composite body having a skin material of the present disclosure, a variety of distinctive designs can be formed by combining the arrangement of the through holes when the skin material is viewed in plan and the recesses of specific depths formed on the surface. That is, by combining the size, shape, and arrangement of the through holes, the area in which the through holes are arranged, and the size and formation area of the recesses of a specific depth in various ways, a skin material and a composite body having through holes, high breathability, and distinctive design properties can be obtained. Thus, in the skin material and composite body of the present disclosure, the combination of through holes and recesses can impart a unique and excellent design to the skin material and the composite body having the skin material and having good cushioning properties, and the range of applications is wide. In the skin material of the present disclosure, by selecting the through holes and recesses of a specific depth, in addition to the breathability inherent to the through holes and the improved feel due to the presence of the recesses, it is possible to impart a unique design to the skin material and composite material, making it suitable for a variety of applications.
[0081] There is no particular limitation on the method for producing the skin material of the present disclosure. First, a skin material is prepared, and any of the known methods of drilling a plurality of through holes penetrating the skin material in the thickness direction, and of forming recesses in the skin material or a composite can be used. Examples of methods for forming through holes in a skin material include a punching method in which a punching die such as a punching roll or a flat punch die is used to punch through holes having a desired diameter at desired intervals in the skin material, and a method in which a skin material substrate is perforated using a laser. The skin material of the present disclosure is preferably produced by the method for producing a skin material of the present disclosure described below, since this makes it possible to more easily and efficiently produce a skin material having a distinctive design.
[0082] [Method of manufacturing skin material] The method for producing a skin material according to the present disclosure includes the steps of: forming a skin material substrate having at least a skin layer (Step I); forming a plurality of through holes in the skin material substrate (Step II); and contacting one surface of the skin material substrate with an embossing roll or embossing plate to form recesses having a depth of 0.2 mm or more (Step III).
[0083] The method for producing a skin material according to the present disclosure may include other steps, if desired, in addition to steps I, II, and III. Other steps may include, for example, a step of applying an adhesive between the base fabric and the skin layer to form an adhesive layer (step (IV)), and a step of forming a surface treatment layer on the surface of the skin layer opposite the base fabric side (step (V)). Each step of the manufacturing method of the present disclosure will be described in detail.
[0084] [Step I: Forming a skin substrate having at least a skin layer] The skin material substrate has at least a skin layer, and optionally has any layers such as a base fabric, an adhesive layer, etc. In order to form the skin material substrate, first, a skin layer-forming composition layer may be formed using a composition for forming a skin layer (hereinafter, sometimes referred to as a skin layer-forming composition). In addition to the synthetic resin that is the main material, the composition for forming the surface layer may contain known additives for the purpose of imparting various functions to the surface layer, such as improving the appearance and feel, as long as the effects of the present disclosure are not impaired. The synthetic resin that can be used in the composition for forming the surface layer is as explained above in the section on the surface layer. Examples of synthetic resins that can be contained in the composition for forming a surface layer include urethane resins, PVC, acrylic resins, fluororesins, and polyester resins, with urethane resins and PVC being preferred. When the skin layer-forming composition contains a synthetic resin, it may contain only one type of synthetic resin, or may contain two or more types of synthetic resin. The synthetic resin serving as the main material refers to a synthetic resin contained in an amount of 50% by mass or more based on the total amount of the composition for forming the skin layer. Examples of additives that may be contained in the skin layer-forming composition include plasticizers, stabilizers, crosslinking agents, crosslinking accelerators, fillers, colorants, film-forming assistants, flame retardants, and foaming agents.
[0085] The composition for forming the skin layer can be prepared by dissolving the resin in a solvent or dispersing the resin in a dispersion medium. Examples of the solvent that can be used to prepare the composition for forming the skin layer include DMF, MEK, IPA, toluene, and the like, and a mixed solvent of two or more of these. The solvent used to prepare the composition for forming the skin layer is appropriately selected in relation to the synthetic resin contained in the composition.
[0086] The method for forming the surface layer is not particularly limited, and the surface layer can be provided by applying a method for forming a surface layer used for known synthetic leather and surface materials. When natural leather is used, the natural leather can be used as the surface layer as it is. The surface layer can be formed, for example, by preparing a composition for forming a surface layer containing a resin and, if desired, other components such as a colorant and a solvent, and molding the resulting composition for forming a surface layer.
[0087] The skin layer-forming composition layer can be formed by forming the skin layer-forming composition into a film by a known film-forming method such as a calendar method, a paste processing method, or a melt extrusion method. The skin layer can be formed by applying the composition for forming the skin layer onto a release paper. As the release paper, either a release paper for transferring a grain pattern or a smooth release paper can be used. By using the release paper for transferring a grain pattern, a concave-convex pattern called a grain pattern can be formed on the surface of the skin layer.
[0088] The amount of the composition for forming a surface layer applied onto the release paper is appropriately selected depending on the intended use of the surface material. When the skin material is a multi-layered skin material having a base fabric, the thickness of the composition layer for forming the skin layer is preferably an amount that results in a film thickness of 0.25 mm to 0.8 mm after drying. Also, when the skin layer is formed by the above-mentioned extrusion method or the like, it is preferable to form the film under conditions that result in a film thickness of 0.25 mm to 0.8 mm after drying.
[0089] In the case where the skin material substrate has a layer other than the skin layer, it is also a preferred embodiment that the layer is adhered to the skin material substrate before drying the layer of the skin layer-forming composition. For example, when preparing a skin material substrate having a base fabric and using release paper, the base fabric may be attached to the side of the skin layer-forming composition layer opposite the release paper side, the skin layer-forming composition layer may be heated and cured, and the release paper may be peeled off to form a skin material substrate as a laminate of the skin layer and the base fabric. The base fabric may be the same as that described in the section on the skin material. When the skin material substrate is formed by bonding the skin layer and the base fabric, the base fabric may be bonded to one surface of the skin layer. The side of the base fabric that contacts the surface layer may be subjected to a nap raising treatment by a conventional method, which improves the adhesion between the surface layer and the base fabric. The adhesion may be performed by pressing a layer of the composition for forming an epidermis layer onto a base fabric before the composition for forming an epidermis layer is completely cured, and then curing the layer, or by forming an optional adhesive layer on the base fabric and adhering the epidermis layer to the base fabric via the adhesive layer. When the adhesive layer is formed, an optional step of forming an adhesive layer (step (IV)) described below may be performed after step (I) and prior to step (II). The adhesive for forming the adhesive layer, the preferred thickness of the adhesive layer, etc. are as described above. The heat curing of the skin layer-forming composition layer can be carried out by a conventional method. The heating temperature is preferably in the range of 50° C. to 190° C., and more preferably in the range of 70° C. to 170° C. The heating time is appropriately selected depending on the type of synthetic resin contained in the skin layer, the thickness of the skin layer, etc. In general, it is preferable to mature and harden the composition under the above temperature conditions for 12 hours to 72 hours. After the skin layer has hardened, a skin material substrate having the skin layer and the base fabric can be obtained. If a release paper is used to form the skin layer, the release paper can be peeled off after the skin layer has hardened.
[0090] As one of the preferred embodiments of step (I), the following embodiment in which a skin substrate is formed using release paper can be mentioned. More specifically, an embodiment includes a method in which a layer of a composition for forming a skin layer is formed on a release paper, a base fabric is attached to the side of the composition layer for forming a skin layer opposite the release paper side, the composition layer for forming a skin layer is heat-cured, and the release paper is peeled off to form a skin material substrate as a laminate of the skin layer and the base fabric.
[0091] [Step II: Forming a plurality of through holes in the skin substrate] In step II, through holes are formed in the skin substrate obtained in step I. There is no particular limitation on the method for forming the through holes, and any known method for boring through holes in skin materials, synthetic leather, etc. can be used. Examples of a method for forming the through holes include a punching method using a punching die and a laser punching method. For example, when forming through-holes of complex shapes such as irregular, star-shaped, or petal-shaped, the laser drilling method is effective. From the viewpoint of the simplicity of the through-hole forming process, a perforation method using a punching die is preferred. By forming through-holes using a punching die equipped with punching pins in a conventional manner, through-holes can be easily and efficiently formed in a regular arrangement. For example, by arranging punching pins at lattice points on the die table of a punching die, a plurality of through holes can be formed in the skin material in a square lattice or triangular lattice pattern. Moreover, a repeated pattern of hexagons can be formed by arranging a plurality of punching pins in a shape of overlapping hexagons on the mold table as shown in Fig. 2. The punching device used to form the through holes may be equipped with a plurality of types of punching molds. By combining punching dies in which the same type of punching pins are arranged, or punching dies in which multiple different types of punching pins are arranged, and by controlling the timing of the up and down movement of each punching die, it is possible to easily manufacture multiple through holes having the same pattern or different patterns repeated at various pitches.
[0092] [Step III: contacting one surface of the skin substrate with an embossing roll or embossing plate to form recesses having a depth of 0.2 mm or more] In step III, an embossing roll or an embossing plate is brought into contact with one surface of the skin substrate obtained in step I, forming recesses having a depth of 0.2 mm or more. When the skin substrate is a multi-layered skin substrate having a skin layer and a base fabric, the recesses are formed by bringing the embossing roll or the embossing plate into contact with the surface of the skin substrate having the skin layer. A skin having through holes and recesses having a depth of 0.2 mm or more is obtained by subjecting the skin substrate obtained in step I to steps II and III. The preferred depth of the recesses in the skin is as described above.
[0093] In the method of producing a skin material according to the present disclosure, either step II or step III may be performed first. That is, first, through holes may be formed in the skin material substrate obtained in step I (step II), and then recesses having a depth of 0.2 mm or more may be formed (step III), or recesses having a depth of 0.2 mm or more may be formed in the skin material substrate (step III), and then through holes may be formed (step II).
[0094] When an embossing roll is used to form recesses in the base material for a skin, the base material for a skin is heated and pressed between an embossing roll for shaping and a backup roll in an embossing machine having a pair of embossing rolls, thereby forming recesses having a depth of 0.2 mm or more in the base material for a skin. When forming recesses in the base material for the skin, if an embossing plate having convex portions for forming recesses formed on a flat plate is used, the base material for the skin is placed between the embossing plate and a backup plate in an embossing machine having an embossing plate, and heat and pressure are applied to form recesses having a depth of 0.2 mm or more in the base material for the skin. During embossing, a desired gap can be provided between the laminate and the embossing roll or embossing plate depending on the required design and thickness. When forming discontinuous recesses that are independent of each other, either an embossing roll or an embossing plate may be used. However, when forming continuous recesses in a band shape, for example, it is preferable to use an embossing roll from the viewpoint of process simplicity.
[0095] From the viewpoint of efficiency in forming the recesses, it is preferable to apply heating when forming the recesses. As a heating method, it is preferable to heat one surface of the skin material substrate to be pressed by the embossing roll or embossing plate, preferably the surface having the skin layer, with a heater or the like, and then to apply the shape of the recesses with the embossing roll or embossing plate. The embossing roll or embossing plate itself may be heated to impart the shape.
[0096] The processing conditions in the embossing machine are appropriately selected depending on the purpose. For example, in the case of embossing using an embossing roll, the heating temperature of the surface of the skin layer that comes into contact with the embossing roll is preferably in the range of 90° C. to 210° C., more preferably in the range of 130° C. to 170° C. The heating conditions of the heater that heats the embossing roll or embossing plate may be adjusted so that the surface temperature falls within the above range. The pressure during embossing is 0.1kgf / cm 2 ~50kgf / cm2 is preferable, and 1kgf / cm 2 ~20kgf / cm 2 More preferably, 1.5 kgf / cm 2 ~10kgf / cm 2 More preferably, it is 1 kgf / cm 2 can be converted to SI units of 9.80665 × 10 kPa. The processing speed is preferably 0.5 m / min to 20 m / min, more preferably 1 m / min to 10 m / min, and further preferably 1.5 m / min to 5 m / min. For example, in the case of embossing using an embossing plate, the heating temperature is preferably in the range of 90° C. to 210° C., more preferably 130° C. to 170° C., as the surface temperature on the urethane skin side of the laminate. The heater of the embossing plate may be adjusted so that the surface temperature falls within the above range. The pressure applied by the embossing plate is 0.1kgf / cm 2 ~50kgf / cm 2 is preferable, and 1kgf / cm 2 ~20kgf / cm 2 More preferably, 1.5 kgf / cm 2 ~10kgf / cm 2 is more preferred. The pressing time is preferably from 10 to 90 seconds, more preferably from 15 to 80 seconds, and even more preferably from 20 to 70 seconds. By subjecting the skin substrate obtained in step I to steps II and III, it is possible to obtain the skin of the present disclosure having through holes and recesses with a depth of 0.2 mm or more.
[0097] (Other processes) Step (IV) is an optional step of forming an adhesive layer. The adhesive layer is formed by applying an adhesive to the surface of the base fabric or the surface layer to form an adhesive layer, and then bonding the two together via the adhesive layer. The adhesive layer can be formed, for example, by applying an adhesive to the surface of the base fabric or the surface layer. In particular, it is preferable to apply an adhesive to the surface of the base fabric and dry it to form the adhesive layer. The adhesive used to form the adhesive layer that is provided if desired is as described in the section on the adhesive layer. Methods for applying the adhesive include a transfer method and a coating method. An adhesive is applied to the surface of the base fabric or the skin layer, and the applied adhesive layer is heated and dried to form an adhesive layer on one side of the base fabric or the thermoplastic resin layer.
[0098] Step (V) is an optional step of forming a surface treatment layer (e.g., a feel-improving layer) on the surface of the skin layer (the side of the skin layer opposite the base fabric side) to improve the feel and appearance. The step (V) is carried out by applying a composition for forming a surface treatment layer containing a resin onto the surface of the skin layer. The composition for forming a surface treatment layer can be applied by appropriately applying a known method. The surface treatment layer may be formed by a method appropriately selected from the following: coating by gravure printing, coating by a coating device such as a reverse coater or a direct coater, etc. Among these, the gravure printing method is preferred from the viewpoint of forming a more uniform layer. The details of the surface treatment layer are as described above.
[0099] The method for producing a skin material composite of the present disclosure includes the steps of forming a skin material substrate having at least a skin layer (step i), forming a plurality of through holes in the skin material substrate (step ii), laminating a cushion layer to the surface of the skin material substrate opposite the surface having the skin layer (step iii), and bringing an embossing roll or embossing plate into contact with the surface having the skin layer of the skin material substrate laminated with the cushion layer to form recesses having a depth of 0.2 mm or more (step iv). Here, the step of forming a plurality of through holes in the skin material substrate (step ii) may be performed after the step of bonding a cushion layer to the surface of the skin material substrate opposite to the surface having the skin layer (step iii). By forming the through holes in step ii after bonding the skin material and the cushion layer in step iii, a composite having through holes penetrating not only the skin material but also the cushion layer can be formed. A composite having through holes penetrating the skin material and the cushion layer has improved breathability.
[0100] The method for producing the composite of the present disclosure may include other steps, if desired, in addition to steps i, ii, iii, and iv. Other steps include the step of applying an adhesive between the base fabric and the skin layer to form an adhesive layer (step (IV)), and the step of forming a surface treatment layer on the surface of the skin layer opposite to the base fabric side (step (V)), which are already mentioned in the manufacturing method for the skin material of the present disclosure. Each step of the method for producing the composite of the present disclosure will be described in detail.
[0101] [Steps I and II] In the method for producing a composite according to the present disclosure, step i: a step of forming a substrate for a skin material, and step ii: a step of forming a plurality of through holes in the substrate for a skin material are the same as steps I and II, respectively, in the method for producing a skin according to the present disclosure described above, and therefore a description thereof will be omitted.
[0102] [Step iii: Step of bonding a cushion layer to the surface of the skin material substrate opposite to the surface layer] In step iii, a cushion layer is attached to the skin material substrate obtained in step i. When the skin material substrate is a multi-layered skin material having a skin layer and a base fabric, the cushion layer is attached to the surface opposite to the surface having the skin layer. When the marking material substrate is a single-layered structure consisting of only a skin layer, the cushion layer may be attached to one surface of the skin layer. In the case of a single-layered skin material, it is preferable to attach the cushion layer to the surface of the skin layer, for example, the surface opposite to the grain surface if the skin layer is made of natural leather. Methods for forming a cushion layer on a skin material include a method of adhering a cushion layer-forming material to the skin material, and a method of applying a precursor of the cushion layer-forming material (also called foam raw material) to a urethane resin skin material. Details of the material for forming the cushion layer are as described in the section explaining the cushion layer.
[0103] The cushion layer may be formed, for example, by foaming a foam raw material in advance by heating or the like, forming a synthetic resin foam, and then adhering the resulting synthetic resin foam to a skin material to form the cushion layer; alternatively, a foam raw material containing a synthetic resin or a synthetic resin precursor may be applied directly to a skin material and foamed on the skin material to form a cushion layer that is a synthetic resin foam containing air bubbles. In particular, from the viewpoint of good cushioning properties and processability, it is preferable to use a synthetic resin foam as the cushion layer forming material for forming the cushion layer, and it is more preferable to use a soft polyurethane foam material having continuous cells that can be applied to the frame lamination process described below.
[0104] The cushion layer-forming material formed in a sheet shape, preferably a soft polyurethane foam material, is attached to the fabric-bearing side of the skin material substrate obtained in step I. The cushion layer-forming material may be attached to the fabric-bearing side of the skin material substrate in which the through holes are formed, obtained in step ii.
[0105] Examples of the adhesion method for bonding the skin material substrate and the cushion layer include a method using the adhesive layer described above and a method using a frame lamination process. In the method of bonding using an adhesive layer, a method of forming an adhesive layer similar to that used for bonding the above-mentioned surface material and base fabric between the cushion layer and the surface material may be applied. From the viewpoint of better productivity, when a soft polyurethane foam material is used as the cushion layer, the step iii preferably includes a frame lamination step. The frame lamination process is a process in which the surface of the polyurethane foam material, which is the cushion layer, is heated with a flame (frame) from a burner or the like, the surface of the polyurethane foam material is thermally melted, and the melted area is brought into contact with the base fabric-bearing surface of the skin material substrate previously obtained in process i, or of the skin material substrate with through holes formed in process ii, and then pressurized and cooled, thereby bonding the skin material substrate and the cushion layer together. By using the frame lamination process to bond the skin material and the cushion layer, the skin material and the cushion layer are bonded together in a short time compared to a bonding method using an adhesive layer, which requires a process of applying an adhesive and drying and curing the adhesive. This improves the productivity of the composite. Furthermore, since there is no adhesive layer between the skin material substrate and the cushion layer, the thickness of the composite can be made thinner. This has the advantage that the formation of recesses with a depth of 0.2 mm or more can be performed more efficiently in step iv, which will be described later.
[0106] [Step iv: a step of contacting an embossing roll or an embossing plate with the side of the skin material substrate having the skin layer bonded to the cushion layer to form recesses having a depth of 0.2 mm or more] In step iv, an embossing roll or embossing plate is brought into contact with the surface layer side of the surface material substrate laminated with the cushion layer in step iii, to form recesses having a depth of 0.2 mm or more. The method for forming recesses having a depth of 0.2 mm or more can be carried out by contacting with an embossing roll or embossing plate, as in step III of the above-described method for producing a skin material according to the present disclosure. The depth of the recess formed in the composite is 0.2 mm or more, preferably 1.0 mm or more, and more preferably 1.5 mm or more. There is no particular upper limit to the depth, but from the viewpoint of the strength and flexibility of the composite, it can be 6.0 mm or less. In the manufacturing method of the composite of the present disclosure, the thickness of the composite is greater than that of the skin material alone, but because the composite has soft cushioning properties, a method of contacting an embossing roll or embossing plate can be used to form recesses with a depth of 0.2 mm or more, and even recesses with greater depths. The obtained composite can express a distinctive design by the through holes formed at least in the skin material of the composite and the deep recesses having a depth of 0.2 mm or more.
[0107] The recesses having a depth of 0.2 mm or more are formed by controlling the height of the protrusions on the embossing roll or embossing plate. From the viewpoint of facilitating the formation of deeper recesses, step iv is preferably an embossing process using an embossing plate, for example, by placing the skin substrate laminated with the cushion layer between a pair of dies consisting of a first die having an embossing die and a second die having no embossing die, and heating both the first die and the second die. When the convex portion of the embossing mold of the first die is pressed against the surface of the skin material substrate opposite the side having the cushion layer to form the concave portion, the tip of the convex portion of the embossing mold of the first die may be inserted from the skin material side to a depth of 0.2 mm or more to perform embossing.
[0108] When an embossing roll or an embossing plate is used to form recesses having a depth of 0.2 mm or more, it is preferable to heat at least one of the skin material, the embossing roll, or the embossing plate. The heating temperature of the embossing roll or embossing plate is preferably in the range of 130°C to 160°C, more preferably in the range of 135°C to 155°C, and even more preferably in the range of 140°C to 150°C. The second mold not having an embossing mold may be heated, and the heating temperature of the second mold in this case is preferably in the range of 140°C to 200°C, more preferably in the range of 150°C to 190°C, and even more preferably in the range of 170°C to 180°C. That is, the heating temperature of the first mold having the embossing mold is preferably lower than the heating temperature of the second mold not having the embossing mold.
[0109] The embossing conditions are a pressure of 20 kgf / cm 2 ~50kgf / cm 2 The heating time is preferably 10 to 90 seconds, and the pressure is 30 kgf / cm 2It is more preferable to apply pressure for about 20 to 60 seconds before and after. By setting the embossing conditions within the above ranges, recesses having a depth of 0.2 mm or more can be easily formed, and the recesses thus formed can retain their shape for a long period of time, resulting in the formation of a composite body with excellent durability.
[0110] In the manufacturing method of the composite of the present disclosure, any one of steps ii, iii, and iv may be performed first. That is, a cushion layer may be bonded to the skin substrate in which the through-holes have been formed in step ii (step iii), and then a recess having a depth of 0.2 mm or more may be formed (step iv), or the skin substrate and the cushion layer may be bonded together (step iii), and then a through-hole may be formed (step ii), and a recess having a depth of 0.2 mm or more may be formed (step iv), or the skin substrate and the cushion layer may be bonded together (step iii), and then a recess having a depth of 0.2 mm or more may be formed (step iv), and then a through-hole may be formed (step ii).
[0111] According to the manufacturing method of the skin material and composite body of the present disclosure, a combination of through holes and recesses having a depth of 0.2 mm or more makes it possible to manufacture skin materials and composite bodies with excellent design never before seen. EXAMPLES
[0112] The skin material and the manufacturing method thereof according to the present disclosure will be specifically described below with reference to examples, but the present disclosure is not limited to these. In the following description, unless otherwise specified, "%" representing the content and concentration means "% by mass."
[0113] Example 1 (1. Preparation of skin base material A) A polyurethane resin (a one-component polycarbonate-based polyurethane resin having a resin solid content of 20%) was diluted with a solvent (DMF) to prepare a composition for forming a surface layer. The obtained composition for forming a skin layer was applied to the surface of a release paper using a knife coater to form a composition layer for forming a skin layer on the surface of the release paper. The coating amount of the composition layer for forming a skin layer was set to an amount such that the thickness of the composition for forming a skin layer after drying was 0.9 mm. A knitted fabric as a base fabric was attached to the layer of the composition for forming a skin layer via an adhesive, and then the resulting mixture was aged and cured at 100° C. for 24 hours to obtain a skin material substrate A (Step I, Step IV).
[0114] (2. Formation of Through Holes) Through holes were formed in the skin material substrate A prepared above using a die having cylindrical punching pins with a diameter of 1.5 mm (Step II). The through holes were arranged as shown in Fig. 5(A), with circular through holes being regularly repeated. In this manner, a skin material substrate B having through holes was obtained. The thickness of the skin material substrate B was 0.9 mm.
[0115] (3. Formation of a recess with a depth of 0.2 mm or more) An embossing roll having protrusions 10.0 mm wide and 0.25 mm high was used to form band-like depressions continuous in the longitudinal direction on the surface of the skin substrate B obtained in step II opposite the side having the base fabric, thereby obtaining the skin material of Example 1 (step III). In this manner, a skin material of Example 1 was obtained, having a structure similar to that shown in the plan view of Fig. 5(A) and the schematic cross-sectional view of Fig. 5(B). The thickness of the skin material was 0.9 mm, the depth of the recesses was 0.25 mm, and the width of the recesses was 10.0 mm.
[0116] Example 2 (1. Preparation of skin base material A) The polyurethane resin was diluted with a solvent (DMF) to prepare a composition for forming a skin layer in the same manner as in Example 1. The obtained composition for forming a skin layer was applied to the surface of a release paper with a knife coater to form a composition layer for forming a skin layer on the surface of the release paper. A knitted fabric as a base fabric was attached to the layer of the composition for forming a skin layer via an adhesive, and then the resulting mixture was aged and cured at 100° C. for 24 hours to obtain a skin material substrate A (step i, step IV).
[0117] (2. Formation of Through Holes) In the skin material substrate A prepared above, through holes were formed using a die having cylindrical punching pins with a diameter of 1.5 mm (step ii). The through holes were arranged in a regularly repeated circular pattern as shown in FIG. 6(A). In this manner, a skin material substrate B with through holes formed therein was obtained. The thickness of the skin material substrate B was 0.9 mm.
[0118] (3. Formation of cushion layer) Density 20kg / m 3 A polyether polyester type soft urethane foam material obtained by the slab foaming method with a hardness of 98.1 (JIS K6400-2) and a compression set of 8% or less (JIS K6400-4) was sliced to a thickness of 1.8 mm to prepare a cushion layer. The skin material base material B and the cushion layer were attached to each other by frame lamination to form a laminate C of the skin material base material and the cushion layer (step iii). In step iii, the surface of the polyurethane foam material as the cushion layer was heated by a burner flame (frame) to melt the surface of the polyurethane foam material, and the base fabric surface of the laminate B was brought into contact with the melted portion, followed by cooling under pressure to bond the laminate B and the cushion layer together to obtain the laminate C. The thickness of the laminate C was 2.2 mm. This was because the thickness of the cushion layer became 1.3 mm as a result of the frame lamination process and pressure application.
[0119] (4. Formation of a recess with a depth of 0.2 mm or more) An embossing roll having a convex portion with a width of 13.7 mm and a height of 1.5 mm was used to form a continuous belt-like recess in the length direction on the surface of the laminate C obtained in step iii opposite to the cushion layer. In this way, a composite of Example 2 having a structure similar to that shown in the plan view of Figure 6(A) and the schematic cross-sectional view of Figure 6(B) was obtained (step iv). The thickness of the composite of Example 2 was 2.2 mm, the depth of the recess was 1.5 mm, and the width of the belt-like recess in plan view was 13.7 mm.
[0120] Example 3 A skin material of Example 3 having a configuration similar to that shown in the plan view of FIG. 7(A) and the schematic cross-sectional view of FIG. 7(B) was obtained in the same manner as in Example 1 except that in (2. Formation of through holes), through holes were formed in the skin material base A prepared above using a die having cylindrical punching pins of different sizes, 1.0 mm, 1.3 mm, and 1.5 mm in diameter (Step II), and in (3. Formation of recesses with a depth of 0.2 mm or more), recesses with a depth of 0.2 mm were formed using an embossing plate having protrusions with a width of 34.0 mm and a height of 0.20 mm (Step III).
[0121] Example 4 A composite of Example 4 having a configuration similar to that shown in the plan view of FIG. 8(A) and the schematic cross-sectional view of FIG. 8(B) was obtained in the same manner as in Example 2, except that in (2. Formation of through holes), through holes were formed in the skin material base A prepared above using a die having cylindrical punching pins of different sizes, 1.0 mm, 1.3 mm, and 1.5 mm in diameter (step ii), and in (4. Formation of recesses with a depth of 0.2 mm or more), recesses with a depth of 1.0 mm were formed using an embossing plate having protrusions with a width of 47.0 mm and a height of 1.0 mm (step iv).
[0122] Example 5 In (2. Formation of through holes), through holes were formed in the skin base material A prepared above using a die having cylindrical punching pins with a diameter of 1.5 mm in the arrangement shown in FIG. 9(A) (Step II), and in (3. Formation of recesses with a depth of 0.2 mm or more), recesses with a depth of 0.2 mm were formed using an embossing roll having a protrusion with a width of 34.0 mm and a height of 0.20 mm (Step III). Except for this, a skin material of Example 5 having the same configuration as the plan view of FIG. 9(A) and the schematic cross-sectional view of FIG. 9(B) was obtained in the same manner as in Example 1. In the skin material of Example 5, recesses were formed in the non-perforated region. The thickness of the skin material of Example 5 was 0.9 mm, the depth of the recesses was 0.2 mm, and the width of the recesses was 34.0 mm.
[0123] Example 6 (1. Preparation of skin base material A) The polyurethane resin was diluted with a solvent (DMF) to prepare a composition for forming a skin layer in the same manner as in Example 1. The obtained composition for forming a skin layer was applied to the surface of a release paper with a knife coater to form a composition layer for forming a skin layer on the surface of the release paper. A knitted fabric as a base fabric was attached to the layer of the composition for forming a skin layer via an adhesive, and then the resulting mixture was aged and cured at 100° C. for 24 hours to obtain a skin material substrate A (step i, step IV).
[0124] (2. Formation of Through Holes) Through holes were formed in the skin material substrate A prepared above using a die having cylindrical punching pins with a diameter of 1.5 mm (step ii). The through holes were arranged in a regularly repeated circular pattern as shown in Fig. 10(A). In this manner, a skin material substrate B having through holes was obtained. The thickness of the skin material substrate B was 0.9 mm.
[0125] (3. Formation of cushion layer) Density 20kg / m 3 A polyether polyester type soft urethane foam material obtained by the slab foaming method was sliced to a thickness of 5.5 mm to form a cushion layer. The skin base material B and the cushion layer were laminated together by frame lamination to form a laminate C of the skin base material B and the cushion layer. (Step iii) The thickness of the laminate C was 5.9 mm. This was because the thickness of the cushion layer became 5.0 mm through frame lamination and pressure application.
[0126] (4. Formation of a recess with a depth of 0.2 mm or more) An embossing roll having a convex portion with a width of 47.0 mm and a height of 3.0 mm was used to form a continuous band-like concave portion in the length direction on the surface of the laminate C obtained in step iv opposite to the side having the base fabric, to obtain a composite of Example 6 (step iv). In the composite of Example 6, the concave portions were formed in the non-perforated regions. The thickness of the composite of Example 6 was 5.9 mm, the depth of the concave portion was 3.0 mm, and the width of the concave portion was 47.0 mm.
[0127] Example 7 In (2. Formation of through holes), through holes were formed in the arrangement shown in FIG. 11(A) using a die having a cylindrical punching pin with a diameter of 1.5 mm in the skin material base material A prepared above (Step II), and in (3. Formation of recesses with a depth of 0.2 mm or more), recesses with a depth of 0.2 mm were formed using an embossing plate having a protrusion with a width of 34.0 mm and a height of 0.20 mm (Step III). Except for this, a skin material of Example 7 having a structure similar to that shown in the plan view of FIG. 11(A) and the schematic cross-sectional view of FIG. 11(B) was obtained in the same manner as in Example 1. In the skin material of Example 7, recesses were formed only in the perforated area. The thickness of the skin material of Example 7 was 0.9 mm, the depth of the recesses was 0.2 mm, and the width of the recesses was 34.0 mm.
[0128] Example 8 In (2. Formation of through holes), a die having a cylindrical punching pin with a diameter of 1.5 mm was used to form through holes arranged as shown in FIG. 12(A) (step ii), and in (4. Formation of recesses with a depth of 0.2 mm or more), an embossed plate having a protrusion with a width of 47.0 mm and a height of 3.0 mm was used to form recesses with a depth of 3.0 mm (step iv). Except for this, a composite of Example 8 having a configuration similar to that shown in the plan view of FIG. 12(A) and the schematic cross-sectional view of FIG. 12(B) was obtained in the same manner as in Example 6. In the composite of Example 8, recesses were formed only in the perforated region. The thickness of the composite of Example 8 was 5.9 mm, the depth of the recess was 3.0 mm, and the width of the recess was 47.0 mm.
[0129] Comparative Example 1 (1. Preparation of Laminate A) The polyurethane resin was diluted with a solvent (DMF) to prepare a composition for forming a skin layer in the same manner as in Example 1. The obtained composition for forming a skin layer was applied to the surface of a release paper with a knife coater to form a composition layer for forming a skin layer on the surface of the release paper. A knitted fabric as a base fabric was attached to the layer of the composition for forming a skin layer via an adhesive, and then the resulting mixture was aged and cured at 100° C. for 24 hours to obtain a skin material substrate A (Step I, Step IV).
[0130] (2. Formation of Through Holes) Through holes were formed in the skin material base material A prepared above using a die having cylindrical punching pins with a diameter of 1.5 mm (Step II). FIG. 13(A) is a plan view showing the through hole pattern of a conventional skin material 40 having through holes of the same circular shape and the same diameter in accordance with Comparative Example 1, and FIG. 13(B) is a schematic cross-sectional view of the skin material of Comparative Example 1. As shown in FIG. 13(B), the skin material of Comparative Example 1 has a skin layer 22 on a base fabric 18 via an adhesive layer 20, and has circular through-holes 10 arranged in a regularly repeated pattern. The layer structure of the skin material is the same as that of the skin material of Example 1. In the skin material of Comparative Example 1, the through holes are arranged in a regularly repeated manner as shown in Fig. 13(A). In this manner, a skin material of Comparative Example 1 was obtained, which has a structure similar to that shown in the plan view of Fig. 13(A) and the schematic cross-sectional view of Fig. 13(B), has through holes, and has no recesses with a depth of 0.2 mm or more. The thickness of the skin material of Comparative Example 1 was 0.9 mm.
[0131] Comparative Example 2 A skin material of Comparative Example 2 was obtained in the same manner as in Example 1, except that, when forming recesses on the surface of the skin material substrate B obtained in step II opposite the side having the base fabric, an embossing roll having protrusions 5.0 mm wide and 0.1 mm high was used to form band-like recesses that were continuous in the longitudinal direction (step III). In this way, a skin material of Comparative Example 2 was obtained, which had a layer structure similar to that shown in the schematic cross-sectional view of Fig. 5(B) except that the depth and width of the formed recesses differed from those shown in the plan view of Fig. 5(A). The thickness of the skin material was 0.9 mm, the depth and width of the recesses were 0.1 mm and 5.0 mm, respectively.
[0132] Comparative Example 3 A composite of Comparative Example 3 was obtained in the same manner as in Example 2, except that, when forming recesses on the surface of the laminate C of the skin material and the cushioning layer obtained in step iii, opposite the side having the base fabric, an embossing roll having protrusions 5.0 mm wide and 0.1 mm high was used to form band-like recesses that were continuous in the longitudinal direction (step iv). In this way, a composite of Comparative Example 3 was obtained, which had a layer structure similar to that shown in the schematic cross-sectional view of Fig. 6(B) except that the depth and width of the recesses formed were different from those shown in the plan view of Fig. 6(A). The thickness of the skin material of the composite of Comparative Example 3 was 2.2 mm, the depth and width of the recesses were 0.1 mm, and 5.0 mm, respectively.
[0133] [Evaluation of the skin material and the skin material composite] The obtained skin materials and composites were evaluated according to the following criteria. The results are shown in Tables 1 and 2.
[0134] 1. Design The obtained skin material and composite were visually observed in plan view and evaluated according to the following evaluation criteria: The skin layer having uniform through-holes of Comparative Example 1 was evaluated as a conventional product (standard). A: It has a distinctive design that is different from conventional products. B: Appearance is the same as the conventional product
[0135] [Table 1]
[0136] [Table 2]
[0137] As is clear from Tables 1 and 2, when the appearances of the skin materials of Examples 1, 3, 5 and 7 and the composites of Examples 2, 4, 6 and 8 were observed, they all exhibited appearances with distinctive designs not seen before. On the other hand, the skin material of Comparative Example 1, which had a through hole but no recesses, the skin material of Comparative Example 2, which had no recesses with a depth of 0.2 mm or more, and the composite of Comparative Example 3, which had no recesses with a depth of 0.2 mm or more, all failed to achieve an appearance with a distinctive design that was different from the conventional products. [Explanation of symbols]
[0138] 10 Through hole 12A, 12B, 12C through hole 14, 28, 32, 36 Skin material 16, 16A, 16B, 16C recess 18 Base fabric 20 Adhesive layer 22 Epidermal layer 24, 30, 34, 38 Skin material composite (composite) 26 Cushioning layer 40 Comparative skin material α Distance indicating the depth of the recess β Distance indicating the depth of the recess
Claims
1. A skin material having at least a skin layer, The skin material has a plurality of through holes passing through the skin material in a thickness direction, At least one surface of the skin layer has a recess having a depth of 0.2 mm or more, The skin material, wherein the recess is a band-like recess having a width of 10 mm to 50 mm that is continuous in the longitudinal direction when viewed in a plan view.
2. The skin material according to claim 1 , wherein the through holes are regularly arranged over the entire surface of the skin layer.
3. The skin material according to claim 1 or 2, wherein the through holes include a plurality of types of through holes having different sizes or shapes when the skin layer is viewed in plan.
4. 4. The skin material according to claim 1, wherein the skin material has, in a plan view, a perforated region having through holes and a non-perforated region having no through holes.
5. 5. The skin material according to claim 4, wherein the recesses having a depth of 0.2 mm or more are formed only in the perforated area.
6. 5. The skin material according to claim 4, wherein the recesses having a depth of 0.2 mm or more are formed only in the non-perforated region.
7. 7. The skin material according to claim 1, further comprising a base fabric on a surface of the skin layer opposite to a surface having a recess having a depth of 0.2 mm or more.
8. A skin material composite comprising the skin material according to any one of claims 1 to 7 and a cushion layer in this order, The skin material has the recess having a depth of 0.2 mm or more on a surface opposite to the surface having the cushion layer.
9. forming a skin material substrate having at least a skin layer; forming a plurality of through holes in the skin material substrate; and contacting one surface of the skin substrate with an embossing roll or an embossing plate to form a continuous band-like recess in the longitudinal direction having a depth of 0.2 mm or more and a width of 10 mm to 50 mm in plan view.
10. forming a skin material substrate having at least a skin layer; forming a plurality of through holes in the skin material substrate; A step of bonding a cushion layer to a surface of the skin material substrate opposite to a surface layer having the skin layer; and contacting an embossing roll or embossing plate with the side of the skin material substrate laminated with the cushion layer, the side having the skin layer, to form band-like recesses having a depth of 0.2 mm or more and a width of 10 mm to 50 mm in a plan view that are continuous in the longitudinal direction.
Citation Information
Patent Citations
JP1973020850B1
JP1973020851B1
Synthetic leather for heat press mold
JP1981112579A
Synthetic leather and its production
JP1998025668A
Decorative laminated sheet
JP1999256483A