Release Film
A release film with an aromatic polyester resin and controlled molecular orientation addresses the issue of low peeling angles in flexible circuit board manufacturing, enhancing release properties and reducing defects in automated processes.
Patent Information
- Application Number
- JP2020571733
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-25
- Filing Date
- 2020-09-17
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-09-17
AI Technical Summary
Conventional release films used in the manufacturing of flexible circuit boards, especially in roll-to-roll methods, face challenges with low peeling angles and require excessive force for peeling, leading to potential defects due to adhesive penetration and reduced mold releasability as circuit boards become thinner.
A release film with a release layer containing an aromatic polyester resin, characterized by an orientation function f of 0.35 or more, achieved through surface treatments like friction treatment and controlled molecular orientation, enhances the film's release properties.
The film exhibits improved release properties, reducing peeling force and preventing adhesive penetration, suitable for high-speed, automated manufacturing processes like RtoR methods, while maintaining flexibility and conformability to irregular surfaces.
Smart Images

Figure 0007583614000001 
Figure 0007583614000002 
Figure 0007583614000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a release film. [Background technology]
[0002] 2. Description of the Related Art Release films are used in the manufacturing processes of printed wiring boards, flexible circuit boards, multilayer printed wiring boards, and the like. In the manufacturing process of a flexible circuit board, a coverlay film is heat-pressed and bonded to a flexible circuit board body on which a copper circuit is formed via a thermosetting adhesive or a thermosetting adhesive sheet. At this time, by disposing a release film between the coverlay film and the heat-press plate, it is possible to prevent the coverlay film and the heat-press plate from adhering to each other, and also to prevent problems such as the adhesive seeping out and interfering with the plating process of the electrode portion (for example, Patent Documents 1 and 2).
[0003] In recent years, release films made of multiple layers including a release layer and a cushion layer have also been used to ensure performance such as releasability and ability to conform to unevenness (embedding ability) in response to the thinning of L / S (line / space) on flexible circuit boards. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-283862 [Patent Document 2] JP 2009-132806 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, as flexible circuit boards become thinner, release films are required to have further improved releasability. In addition, in recent years, the manufacturing of flexible circuit boards has also become automated using the roll-to-roll (RtoR) method and the like. In the RtoR method, the flexible circuit board body and release film, etc., which are unwound from a roll, are transported between heat press plates, heat press bonded, and then wound up on the roll again. In such an RtoR method, when the release film is peeled off from the flexible circuit board after heat press bonding, the peel angle tends to be low. Therefore, when a conventional release film is used, a larger force may need to be applied during peeling, which may lead to defects. Therefore, release films are required to have further improved releasability.
[0006] An object of the present invention is to provide a release film which has better releasability than conventional films and can be suitably used in the production of flexible circuit boards by the roll-to-roll method. [Means for solving the problem]
[0007] The present invention is a release film having at least one release layer, wherein the release layer contains an aromatic polyester resin and has an orientation function f of 0.35 or more calculated by the following formula (1) based on an infrared absorption spectrum measured by a total reflection measurement method.
[0008]
number
[0009] In formula (1), A1 represents the absorption intensity due to C=O stretching motion in the incident direction (first direction) in which the absorption due to C=O stretching motion is greatest, and A2 represents the absorption intensity due to C=O stretching motion in the direction perpendicular to the first direction (second direction). The present invention will be described in detail below.
[0010] The heat pressing process in the manufacture of flexible circuit boards may be performed at a temperature of 160 to 180°C for the purpose of softening and hardening the adhesive. The present inventors have found that in the temperature range corresponding to the softening and hardening of the adhesive, the adhesive of the coverlay film to be laminated is more likely to permeate into the release film, which causes a decrease in releasability. As a result of further intensive research, they have found that the permeation of the adhesive into the film can be suppressed and the releasability can be improved by sufficiently orienting the molecules on the extreme surface of the release layer of the release film, thereby completing the present invention.
[0011] The release film of the present invention has at least one release layer. The release layer has an orientation function f of 0.35 or more, which is calculated by the above formula (1) based on an infrared absorption spectrum measured by total reflection measurement. The orientation function f of the release layer surface can be calculated from the measured value of the infrared absorption spectrum obtained by infrared spectroscopy (IR) measured by total reflection measurement (ATR method).
[0012] Infrared spectroscopy (IR) is one of the most common analytical methods for organic matter and has been widely used for a long time. In the attenuated total reflection (ATR) method, the surface condition of a sample can be analyzed by using light totally reflected at the interface between a prism (a high refractive index medium transparent in the infrared range) and the sample. After the prism and the sample are brought into contact, the infrared light transmitted through the prism is totally reflected at the interface with the sample. During this total reflection, a small amount of infrared light penetrates the sample side, so by detecting the totally reflected light, it is possible to obtain an infrared absorption spectrum (FT-IR spectrum) of the sample surface (a few μm deep). In particular, the ATR method using a germanium prism can analyze the condition of the very surface (less than 1 μm) of the sample.
[0013] In the infrared spectroscopy analysis by the total reflection measurement method in the present invention, polarization measurement is performed. Specifically, s-polarized light (polarized light perpendicular to the incident plane) is irradiated to obtain a spectrum. First, for the release layer of the release film to be measured, infrared absorption spectra (FT-IR spectra) by the total reflection measurement method (ATR method) are obtained for various polarization directions. That is, the polarization direction of the infrared light in a plane parallel to the film surface is changed by changing the incident angle (azimuth angle) of the infrared light by changing the orientation of the film, etc., and measurement is performed. From the FT-IR spectrum in each direction obtained, the direction in which the absorption due to the C=O stretching motion is the largest is set as the first direction, and the absorption intensity A1 due to the C=O stretching motion in the first direction is obtained. Next, the direction perpendicular to the first direction is set as the second direction, and the absorption intensity A2 in the second direction is obtained. The obtained A1 and A2 can be substituted into the above formula (1) to calculate the orientation function f. Here, the absorption due to the C=O stretching motion is at a wave number of 1700 to 1720 cm -1 In the present invention, the absorption intensity due to the C=O stretching motion is a value normalized by the absorption due to the stretching vibration of the benzene ring. The absorption due to the stretching vibration of the benzene ring is a peak in the range of wave numbers from 1400 to 1420 cm. -1 In other words, the absorption intensity due to the C=O stretching motion is the absorption peak in the wavenumber range of 1400 to 1420 cm -1 The wavenumber for the maximum value in the range of 1700 to 1720 cm -1 In addition, if there is no maximum value within the above wave number range, the maximum value within the range is treated as the maximum value in that range. -1 The absorption peak in the range of 1600 to 1800 cm is calculated using the wavenumber of 1600 to 1800 cm. -1 The baseline is the section (wave number 1600 cm -1 Absorption intensity at wavenumber 1800cm -1 The baseline is the line connecting the absorption intensities at wavenumbers 1400 to 1420 cm. -1 The absorption peak in the range of 1360 to 1425 cm was calculated using the wavenumber of 1360 to 1425 cm. -1The baseline is the section (wave number 1360 cm -1 Absorption intensity at wavenumber 1425cm -1 The straight line connecting the absorption intensities at each point is used as the baseline. As an infrared absorption spectrum measuring device, for example, FT / IR6600 (manufactured by JASCO) can be used.
[0014] The orientation function indicates the orientation state of the molecules, with no orientation being "0" and perfect orientation being "1." The orientation function f of the release layer surface is calculated based on an infrared absorption spectrum measured by total reflection measurement, and therefore represents the orientation state of the molecules on the release layer surface of the release film. As can be understood from the above formula (1) and the above polarization measurement (the method for determining the absorption intensities A1 and A2), the molecular orientation referred to here means that the molecules as a whole are oriented in one arbitrary direction in a plane parallel to the film surface. In addition, the orientation function itself does not necessarily distinguish between crystalline and amorphous regions, and also includes the influence of the molecular orientation in the amorphous region. The release film of the present invention can exhibit high releasability by having the orientation function f of the release layer surface of 0.35 or more. This is believed to be because the molecules on the extreme surface of the release layer of the release film are sufficiently oriented, thereby reducing the free volume of the molecules, making it difficult for the adhesive to penetrate into the release film even when the temperature becomes high during the heat press process. The orientation function f of the release layer surface is preferably 0.40 or more, more preferably 0.43 or more, and even more preferably 0.45 or more.
[0015] The method for making the orientation function f of the release layer surface 0.35 or more is not particularly limited, but possible methods include reducing the arithmetic mean roughness Ra of the release layer before surface treatment, adjusting the molding (film formation) conditions of the release film, the method and conditions of the surface treatment, etc. More specifically, examples include performing a friction treatment at a high temperature, increasing the elongation stress during film formation, etc.
[0016] By reducing the arithmetic mean roughness Ra of the release layer before the surface treatment, the orientation function f of the release layer surface can be increased. The reason is unclear, but can be presumed as follows. For example, when performing surface treatment by friction treatment, if the arithmetic mean roughness Ra is relatively large, the unevenness of the release layer surface inhibits changes in physical properties and uniform treatment, and the degree of surface change by the friction treatment decreases. On the other hand, if the arithmetic mean roughness Ra is sufficiently small, it is considered that the unevenness of the release layer surface inhibits changes in physical properties and uniform treatment little, and the surface can be sufficiently changed by the friction treatment. The arithmetic mean roughness Ra of the surface of the release layer before the surface treatment can be, for example, 0.30 μm or less. In addition, the arithmetic mean roughness Ra of the release layer before the surface treatment needs only to be small during the surface treatment. Even if the arithmetic mean roughness Ra becomes large after the surface treatment as a result of embossing the surface of the release layer as described below, the orientation function itself is not significantly affected. The arithmetic mean roughness Ra of the surface of the release layer before the surface treatment is the arithmetic mean roughness Ra in accordance with JIS B 0601:2013, and can be measured, for example, using a Surftest SJ-301 manufactured by Mitutoyo Corporation.
[0017] The arithmetic mean roughness Ra of the surface of the release layer before the surface treatment can be influenced by the conditions during film formation. For example, when the resin constituting the release layer is melt-extruded and the molten resin is cooled, the following methods can be used. That is, a method of using a cooling roll having a smoother surface and transferring the roll surface shape to the film, or a method of adjusting the elongation stress applied to the molten resin during cooling so as to be large, etc. can be mentioned. In addition, fine adjustment can be made by changing the line speed or temperature. In addition, a process such as hot pressing (press annealing) can be added.
[0018] Examples of the surface treatment include friction treatment, heat treatment, uniaxial stretching or biaxial stretching. These surface treatments may be used alone or in combination of two or more. Among them, friction treatment is preferred because it can efficiently treat only the very surface of the release layer.
[0019] The method of the friction treatment is not particularly limited, but the friction treatment can be performed using a friction treatment device (for example, a polishing treatment device manufactured by Yamagata Kikai Co., Ltd., model YCM-150M) and using a woven fabric as the surface material of the friction treatment material. The method of the heat treatment is not particularly limited, but may be a method of passing the film between rolls heated to a certain temperature, a method of heating the film with a heater, or the like. The method for the uniaxial or biaxial stretching treatment is not particularly limited, and a method in which the formed film is stretched at a certain temperature can be used.
[0020] When friction treatment is performed as the above surface treatment, the work energy amount En (kJ) can be calculated by the following formula (3).
[0021]
number
[0022] In formula (3), Ar is the area (m 2 ), J represents the amount of work per unit time required for rubbing treatment (KJ / min), W represents the width (m) of the film to be rubbing treated, and LS represents the line speed (m / min), which is the speed at which the film passes through the rubbing treatment device.
[0023] When friction treatment is performed as the surface treatment, the work energy amount En (kJ) can be, for example, 300 to 900 kJ.
[0024] When friction treatment is performed as the surface treatment, the friction treatment can be performed in a heated state. By performing the friction treatment at a high temperature, it becomes easier to make the orientation function f of the release layer surface 0.35 or more. The heating temperature in the friction treatment can be, for example, 30 to 70°C.
[0025] The forming (film-forming) conditions of the release film can be, for example, adjusted so that the elongation stress applied to the molten resin during cooling is increased. By doing so, the orientation function f of the release layer surface can be easily set to 0.35 or more. In order to increase the value of the orientation function f, it is preferable to increase the elongation stress, for example, an air knife method can be used.
[0026] The release layer preferably has an arithmetic mean roughness Ra of 2 μm or more on the surface. By having the arithmetic mean roughness Ra of the release layer of 2 μm or more on the surface, it is possible to prevent air bubbles from being trapped at the interface when the release film is placed between the coverlay film and the heat press plate, thereby improving wrinkle resistance. The arithmetic mean roughness Ra of the release layer is more preferably 3 μm or more, and even more preferably 4 μm or more. The upper limit of the arithmetic mean roughness Ra of the release layer is not particularly limited, but is preferably 5 μm or less. The arithmetic mean roughness Ra of the surface of the release layer can be adjusted by the film-forming conditions and the embossing conditions (such as the shape of the shaping die and the processing speed). As described above, when the surface treatment is a friction treatment, in order to make the orientation function f of the release layer surface 0.35 or more, it is preferable that the arithmetic mean roughness Ra of the surface of the release layer is small during the surface treatment. However, even if the arithmetic mean roughness Ra is increased by subjecting the surface of the release layer to embossing or the like after the surface treatment, the orientation function itself is not significantly affected.
[0027] The release layer preferably has an orientation function g calculated by the following formula (2) based on an infrared absorption spectrum by a transmission method, which is smaller than the orientation function f of the surface of the release layer. If the orientation function of the entire release layer is higher than necessary, the flexibility of the entire release film decreases, and the ability to follow unevenness decreases, which may cause voids to occur during hot press bonding or increase the width of the adhesive seeping out. By adjusting the orientation of the release layer other than the extreme surface, the release layer can have a high orientation function value at the extreme surface while having a moderate orientation as a whole release layer. With this configuration, the release film becomes even more excellent in both releasability and ability to follow unevenness.
[0028] The orientation function g of the entire release layer can be calculated from the measured value of the infrared absorption spectrum obtained by infrared spectroscopy (IR) by the transmission method. In the transmission method, not only the surface of the sample but also the state of the entire sample (the part through which infrared rays pass) can be analyzed. The orientation function g of the entire release layer based on the infrared absorption spectrum by the transmission method is preferably 0.35 or less.
[0029]
number
[0030] In the infrared spectroscopy analysis by the transmission method in the present invention, polarization measurement is performed. Specifically, s-polarized light (polarized light perpendicular to the incident surface) is irradiated to obtain a spectrum. First, infrared absorption spectra (FT-IR spectra) by the transmission method are obtained for various polarization directions for the release layer of the release film to be measured. That is, the measurement is performed by changing the polarization direction of infrared light in a plane parallel to the film surface by changing the orientation of the film, etc. In addition, in the transmission method, infrared light is made to be perpendicularly incident on the target measurement surface of the sample. From the FT-IR spectrum in each direction obtained, the direction in which the overtone absorption due to the C=O stretching motion is the largest is set as the third direction, and the overtone absorption intensity A3 due to the C=O stretching motion in the third direction is obtained. Next, the direction perpendicular to the first direction is set as the fourth direction, and the overtone absorption intensity A4 due to the C=O stretching motion in the fourth direction is obtained. The obtained A3 and A4 can be substituted into the above formula (2) to calculate the orientation function g. Here, the overtone absorption due to the C=O stretching motion is a wave number of 3420 to 3440 cm -1 In the present invention, the overtone absorption intensity due to the C=O stretching motion is a value normalized by the absorption due to the stretching vibration of the benzene ring. The absorption due to the stretching vibration of the benzene ring is a peak in the range of wave numbers from 1400 to 1420 cm. -1 In other words, the overtone absorption intensity due to C=O stretching motion is the absorption peak in the wavenumber range of 1400 to 1420 cm -1 The wavenumber for the maximum value in the range 3420-3440 cm -1 In addition, if there is no maximum value within the above wave number range, the maximum value within the range is treated as the maximum value in that range. -1 The absorption peak in the range of 3370 to 3470 cm was calculated using the wavenumber of 3370 to 3470 cm. -1 The baseline is the section (wave number 3370 cm -1 Absorption intensity at wavenumber 3470cm -1 The baseline is the line connecting the absorption intensities at wavenumbers 1400 to 1420 cm. -1 The absorption peak in the range of 1360 to 1425 cm was calculated using the wavenumber of 1360 to 1425 cm.-1 The baseline is the section (wave number 1360 cm -1 Absorption intensity at wavenumber 1425cm -1 The straight line connecting the absorption intensities at each point is used as the baseline. As an infrared absorption spectrum measuring device, for example, FT / IR6600 (manufactured by JASCO) can be used.
[0031] The method of adjusting the orientation function g of the entire release layer is not particularly limited, but like the method of adjusting the orientation function f of the surface of the release layer, it is possible to reduce the arithmetic mean roughness Ra of the release layer before the surface treatment, adjust the molding (film formation) conditions of the release film, and adjust the method and conditions of the surface treatment. By adjusting as described above, it is possible to keep the orientation function g of the entire release layer at a relatively small value while increasing the orientation function f of the surface of the release layer. On the other hand, when the film is stretched in the film manufacturing process, the molecules constituting the film are oriented under the influence of the stretching, regardless of whether they are on the surface or inside of the release layer. Therefore, it is difficult for the film manufactured through the stretching process to have a configuration in which the orientation of the surface of the release layer is high and the orientation of the entire release layer is low.
[0032] The release layer contains an aromatic polyester resin, which improves the releasability of the release film. The aromatic polyester resin is not particularly limited, but crystalline aromatic polyester resin is preferred.Specific examples include polyethylene terephthalate resin, polybutylene terephthalate resin, polyhexamethylene terephthalate resin, polyethylene naphthalate resin, polybutylene naphthalate resin, terephthalic acid butanediol polytetramethylene glycol copolymer, etc.These aromatic polyester resins may be used alone or in combination of two or more.Among them, polybutylene terephthalate resin is preferred from the viewpoint of balance of heat resistance, releasability, conformability to unevenness, etc. Also preferred is a mixed resin of a polybutylene terephthalate resin and a block copolymer of polybutylene terephthalate and an aliphatic polyether. The aliphatic polyether is not particularly limited, and examples thereof include polyethylene glycol, polydiethylene glycol, polypropylene glycol, and polytetramethylene glycol.
[0033] From the viewpoint of film forming properties, the aromatic polyester resin has a melt volume flow rate of 30 cm 3 / 10min or less is preferable, and 20cm 3 It is more preferable that the melt volume flow rate is equal to or less than 1000000 / min. The melt volume flow rate can be measured in accordance with ISO1133 at a measurement temperature of 250° C. and a load of 2.16 kg.
[0034] Among the above aromatic polyester resins, commercially available examples include "Pelprene (registered trademark)" (manufactured by Toyobo Co., Ltd.), "Hytrel (registered trademark)" (manufactured by DuPont-Toray Co., Ltd.), "Duranex (registered trademark)" (manufactured by Polyplastics Co., Ltd.), and "Novaduran (registered trademark)" (manufactured by Mitsubishi Engineering Plastics Corporation).
[0035] The release layer may contain a mixed resin containing polybutylene terephthalate resin and an elastomer. The elastomer is not particularly limited, and may be, for example, a block copolymer of polybutylene terephthalate and an aliphatic polyether. The aliphatic polyether is not particularly limited, and may be, for example, polyethylene glycol, polydiethylene glycol, polypropylene glycol, polytetramethylene glycol, etc.
[0036] The proportion of the polybutylene terephthalate resin in the resin constituting the release layer is not particularly limited, but is preferably 75% by weight or more. If the proportion of the polybutylene terephthalate resin is 75% by weight or more, the release property of the release film is improved. A more preferable lower limit of the proportion of the polybutylene terephthalate resin in the resin constituting the release layer is 80% by weight.
[0037] The release layer may contain a rubber component. When the release layer contains a rubber component, the ability to conform to the irregularities of the release film is improved. The rubber component is not particularly limited, and examples thereof include natural rubber, styrene-butadiene copolymer, polybutadiene, polyisoprene, acrylonitrile-butadiene copolymer, ethylene-propylene copolymer (EPM, EPDM), polychloroprene, butyl rubber, acrylic rubber, silicone rubber, urethane rubber, etc. Examples of the rubber component include olefin-based thermoplastic elastomer, styrene-based thermoplastic elastomer, vinyl chloride-based thermoplastic elastomer, ester-based thermoplastic elastomer, amide-based thermoplastic elastomer, etc.
[0038] The release layer may contain a stabilizer. The stabilizer is not particularly limited, and examples thereof include hindered phenol-based antioxidants and heat stabilizers. The hindered phenol-based antioxidant is not particularly limited, and examples thereof include 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 3,9-bis{2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)-propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, and the like. The heat stabilizer is not particularly limited, and examples thereof include tris(2,4-di-t-butylphenyl)phosphite, trilauryl phosphite, 2-t-butyl-α-(3-t-butyl-4-hydroxyphenyl)-p-cumenylbis(p-nonylphenyl)phosphite, dimyristyl 3,3'-thiodipropionate, distearyl 3,3'-thiodipropionate, pentaerythryl tetrakis(3-laurylthiopropionate), ditridecyl 3,3'-thiodipropionate, and the like.
[0039] The release layer may further contain conventionally known additives such as fibers, inorganic fillers, flame retardants, ultraviolet absorbing agents, antistatic agents, inorganic substances, and salts of higher fatty acids.
[0040] The thickness of the release layer is not particularly limited, but the preferred lower limit is 10 μm, and the preferred upper limit is 40 μm. If the thickness of the release layer is 10 μm or more, the heat resistance of the release film is improved. If the thickness of the release layer is 40 μm or less, the conformability of the release film to the unevenness is improved. The more preferred lower limit of the thickness of the release layer is 15 μm, and the more preferred upper limit is 30 μm.
[0041] The release film of the present invention may have a single-layer structure constituted only of the release layer, or may have a multi-layer structure containing layers other than the release layer.
[0042] The release film of the present invention preferably further comprises a cushion layer, which improves the ability of the release film to conform to unevenness. When the cushion layer is included, the release film of the present invention may have at least one release layer and a cushion layer, and may have a two-layer structure or a three-layer structure or more. In particular, it is preferable to have a structure having a release layer on both sides of the cushion layer. In this case, the release layers on both sides may have the softening temperature as described above, or only the release layer on one side may have the softening temperature as described above. In addition, the release layers on both sides may have the same resin composition or different resin compositions. In addition, the release layers on both sides may have the same thickness or different thicknesses. Furthermore, the release film of the present invention may have a structure in which the release layer and the cushion layer are in direct contact with each other and integrated together, or may have a structure in which the release layer and the cushion layer are integrated together via an adhesive layer.
[0043] The resin constituting the cushion layer is not particularly limited, but it is preferable that the cushion layer contains the resin constituting the release layer. The cushion layer contains the resin constituting the release layer, so that the adhesion between the release layer and the cushion layer is improved. The cushion layer more preferably contains the main component resin of the release layer, and further preferably contains the main component resin of the release layer and a polyolefin resin. Here, the main component resin of the release layer means the resin with the highest content among the resins contained in the release layer.
[0044] The content of the resin constituting the release layer in the cushion layer is not particularly limited, but the preferred lower limit is 10% by weight, and the preferred upper limit is 50% by weight. If the content of the resin constituting the release layer is 10% by weight or more, the adhesion between the release layer and the cushion layer is improved. If the content of the resin constituting the release layer is 50% by weight or less, the flexibility of the cushion layer is sufficient, and the ability to follow the unevenness of the release film is improved. The more preferred lower limit of the content of the resin constituting the release layer is 20% by weight, and the even more preferred lower limit is 25% by weight. The more preferred upper limit of the content of the resin constituting the release layer is 40% by weight, and the even more preferred upper limit is 35% by weight.
[0045] The polyolefin resin is not particularly limited, and examples thereof include polyethylene resins (e.g., high-density polyethylene, low-density polyethylene, linear low-density polyethylene), polypropylene resins, ethylene-vinyl acetate copolymers, etc. Also included are ethylene-acrylic monomer copolymers such as ethylene-methyl methacrylate copolymers, ethylene-ethyl acrylate copolymers, and ethylene-acrylic acid copolymers. These polyolefin resins may be used alone or in combination of two or more. Among them, polypropylene resins are preferred because they easily achieve both conformability to irregularities and heat resistance.
[0046] The content of the polyolefin resin in the cushion layer is not particularly limited, but the preferred lower limit is 50% by weight, and the preferred upper limit is 90% by weight. If the content of the polyolefin resin is 50% by weight or more, the flexibility of the cushion layer is sufficient, and the ability to follow the unevenness of the release film is improved. If the content of the polyolefin resin is 90% by weight or less, the adhesion between the release layer and the cushion layer is improved. The more preferred lower limit of the content of the polyolefin resin is 60% by weight, and even more preferred lower limit is 65% by weight. The more preferred upper limit of the content of the polyolefin resin is 80% by weight, and even more preferred upper limit is 75% by weight.
[0047] The cushion layer may further contain a resin such as polystyrene, polyvinyl chloride, polyamide, polycarbonate, polysulfone, or polyester. The cushion layer may further contain additives such as fibers, inorganic fillers, flame retardants, ultraviolet absorbing agents, antistatic agents, inorganic substances, and salts of higher fatty acids.
[0048] The cushion layer may have a single-layer structure made of a single layer, or a multi-layer structure made of a laminate of multiple layers. When the cushion layer has a multi-layer structure, the multiple layers may be laminated together via an adhesive layer.
[0049] The thickness of the cushion layer is not particularly limited, but the preferred lower limit is 15 μm, and the preferred upper limit is 200 μm. If the thickness of the cushion layer is 15 μm or more, the ability to follow the unevenness of the release film is improved. If the thickness of the cushion layer is 200 μm or less, the exudation of resin from the cushion layer that occurs at the film end during heat press bonding can be suppressed. The more preferred lower limit of the thickness of the cushion layer is 30 μm, and the more preferred upper limit is 150 μm.
[0050] The method for producing the release film of the present invention is not particularly limited, and examples thereof include a method in which a film is first prepared by a water-cooled or air-cooled coextrusion inflation method, a coextrusion T-die method, a solvent casting method, a hot press molding method, or the like, and then the above-mentioned surface treatment is performed. In the case of a structure having the release layers on both sides of the cushion layer, a method of preparing a film to be one of the release layers, laminating the cushion layer on this film by extrusion lamination, and then dry laminating the other release layer can be used. Also, a method of dry laminating the film to be one of the release layers, the film to be the cushion layer, and the film to be the other release layer can be used. Among these, the co-extrusion T-die method is preferred because it allows excellent control of the thickness of each layer.
[0051] By subjecting the thus obtained film to the above-mentioned surface treatment, the orientation function f of the surface of the release layer can be made to be 0.35 or more. After the surface treatment, it is preferable to emboss the surface of the release layer. If the surface treatment is performed, even if the arithmetic mean roughness Ra of the surface of the release layer is increased by embossing, the wrinkle resistance can be improved while maintaining the release property without significantly changing the orientation function itself.
[0052] The use of the release film of the present invention is not particularly limited, but it can be suitably used in the production processes of printed wiring boards, flexible circuit boards, multilayer printed wiring boards, and the like. Specifically, for example, in the manufacturing process of a flexible circuit board, the release film of the present invention can be used when hot press bonding a coverlay film to a flexible circuit board main body having a copper circuit formed thereon via a thermosetting adhesive or a thermosetting adhesive sheet. Since the release film of the present invention has extremely excellent releasability, it can also be suitably used in the production of flexible circuit boards by the RtoR method, which requires high releasability. Effect of the Invention
[0053] According to the present invention, it is possible to provide a release film which has better releasability than conventional ones and can be suitably used in the production of flexible circuit boards by the roll-to-roll method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0054] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0055] Example 1 (1) Preparation of films Polybutylene terephthalate resin (PBT) was used as the resin constituting the release layers (release layers a and b). 75 parts by weight of polypropylene resin (PP) and 25 parts by weight of polybutylene terephthalate resin (PBT) (main component resin of the release layer) were used as the resin constituting the cushion layer. The resin constituting the release layer and the resin constituting the cushion layer were co-extruded in three layers at a T-die width of 400 mm using an extruder (GM Engineering, GM30-28 (screw diameter 30 mm, L / D 28)), and the extruded molten resin was cooled by a cooling roll (temperature 90°C, arithmetic mean surface roughness Ra 0.1 μm). This resulted in a three-layer film having a release layer a (thickness 20 μm) and a release layer b (thickness 30 μm) on both sides of the cushion layer (thickness 50 μm). During cooling, the contact time between the molten resin and the cooling roll was 1.0 second, and the elongation stress when cooling the molten resin by the cooling roll was 450 kPa.
[0056] The above tensile stress is expressed by the following formula (4).
[0057]
number
[0058] The strain rate and the extensional viscosity of the molten resin are expressed by the following formulas (5) and (6), respectively.
[0059]
number
[0060]
number
[0061] In equation (5), V is the roll speed (m / s), V0 is the flow velocity of the molten resin at the die exit (m / s), and L is the distance from the die exit to the contact point of the molten resin with the roll (m).
[0062] The arithmetic mean roughness Ra of the surface of the release layer a (before the friction treatment) of the obtained film was measured using a Mitutoyo Surftest SJ-301 in accordance with JIS B 0601:2013, and was found to be 0.24 μm.
[0063] (2) Film surface treatment While the obtained film was being fed by a roll, the surface of the release layer a was subjected to friction treatment using a friction treatment device (a polishing treatment device manufactured by Yamagata Kikai Co., Ltd., model YCM-150M) and a woven fabric as the surface material of the friction treatment material, thereby obtaining a release film. During the friction treatment, a surface treatment roll was placed between the feed roll and the take-up roll, and the surface treatment roll was pressed against the film to apply a load to the film. The ratio of the rotation speed of the take-up roll to the rotation speed of the feed roll was adjusted to generate a tension of 400 N / m in the unwinding direction of the film. The work energy amount En applied during the friction treatment was 350 kJ.
[0064] (3) Calculation of the orientation function f of the release layer surface The release layer a of the obtained release film was subjected to infrared spectroscopy (IR) by the ATR method using a germanium prism. In a plane parallel to the film surface, the flow direction during film molding was set to 0°, and infrared light (s-polarized) was irradiated so that the polarization direction was in each direction from 0° to 170° in 10° increments, and an infrared absorption spectrum (FT-IR spectrum) was obtained in each direction. Absorption due to C=O stretching motion (wavelength 1700 to 1720 cm -1 The direction in which the C=O stretching motion is the largest was defined as the first direction, and the absorption intensity A1 due to the C=O stretching motion in the first direction was determined. Next, the direction perpendicular to the first direction was defined as the second direction, and the absorption intensity A2 due to the C=O stretching motion in the second direction was determined. The obtained A1 and A2 were substituted into the above formula (1) to calculate the orientation function f.
[0065] (4) Calculation of the orientation function g of the entire release layer The release layer a of the obtained release film was subjected to infrared spectroscopy (IR) by a transmission method. In a plane parallel to the film surface, the flow direction during film molding was set to 0°, and infrared light (s-polarized) was incident so that the polarization direction was in each direction from 0° to 170° in 10° increments, and an infrared absorption spectrum (FT-IR spectrum) was obtained in each direction. Overtone absorption due to C=O stretching motion (wavelength 3420 to 3440 cm -1 The direction in which the C=O stretching motion is the largest was defined as the third direction, and the overtone absorption intensity A3 due to the C=O stretching motion in the third direction was determined. Next, the direction perpendicular to the third direction was defined as the fourth direction, and the overtone absorption intensity A4 due to the C=O stretching motion in the fourth direction was determined. The obtained A3 and A4 were substituted into the above formula (2) to calculate the orientation function g.
[0066] (Examples 2 to 6, Comparative Examples 1 to 4) In Examples 2 to 4 and Comparative Examples 1 to 3, release films were obtained in the same manner as in Example 1, except for the cooling method of the molten resin and the elongation stress during cooling. In Comparative Examples 1 to 4, the arithmetic mean roughness Ra of the surface of the release layer a was adjusted by adjusting the arithmetic mean roughness Ra of the cooling roll surface, the line speed, and the temperature. In Examples 5, 6, and Comparative Example 4, a stretching process was performed instead of a friction process as a post-treatment. More specifically, a film was first produced in the same manner as in Example 1 to obtain a three-layered film having a release layer a (thickness 60 μm) and a release layer b (thickness 90 μm) on both sides of a cushion layer (thickness 150 μm). Then, uniaxial stretching was performed three times in the flow direction with a longitudinal stretching roll heated to 80 degrees. In this way, a three-layered film having a release layer a (thickness 20 μm) and a release layer b (thickness 30 μm) on both sides of a cushion layer (thickness 50 μm) was obtained. In addition, for Examples 2, 4 and 6, the surface that had been subjected to the surface treatment was then embossed to obtain a release film. Specifically, the film after the friction treatment was fed with a roll while being pressed with an embossing roll (arithmetic mean surface roughness Ra 8 μm, temperature 160° C., linear pressure 50 kg / cm) to emboss the surface on the release layer a side. The surface on the release layer a side of the obtained release film was measured for the arithmetic mean surface roughness Ra of the release layer a (before friction treatment) using Mitutoyo Surf Test SJ-301 in accordance with JIS B 0601:2013.
[0067] (evaluation) The release films obtained in the examples and comparative examples were evaluated by the following methods. The results are shown in Table 1.
[0068] (1) Evaluation of releasability The epoxy adhesive surface of the coverlay film (CISV-2535, manufactured by Nikkan Kogyo Co., Ltd.) cut into a 200 mm square was overlapped with the surface of the release layer a of the obtained release film. Next, using a slide type vacuum heater press (MKP-3000v-MH-ST, manufactured by Mikado Technos Co., Ltd.), pressing was performed at a pressure of 30 kgf, 180°C, and 5 minutes, and then cured for one day under conditions of 23°C and 50% RH. After that, an evaluation sample with a width of 30 mm and a length of 150 mm was cut out from the cured sample, and the peel force (gf / cm) of this evaluation sample was measured using Tensilon (STA-1150, manufactured by A&D Co., Ltd.) at a peel speed of 500 mm / min and a peel angle of 180°.
[0069] (2) Evaluation of wrinkle resistance CCL (20cm x 20cm, polyimide thickness 25μm, copper foil 35μm), coverlay (20cm x 20cm, polyimide thickness 15μm, epoxy resin adhesive layer 25μm), and release film were stacked in this order from the bottom up. After aligning the position between the press dies preheated to 180℃ using a sliding vacuum heater press (MKP-3000V-WH-ST, Mikado Technos), pressing was started (it took about 10 seconds from placement to actually applying pressure). Under vacuum conditions, 50kg / cm 2 A flexible circuit board (FPC) evaluation sample consisting of the CCL and coverlay was produced by pressing the CCL and coverlay at 0.8 V for 2 minutes. The FPC evaluation sample and the release film were then removed, and the release film was peeled off, after which the number of wrinkles transferred onto the coverlay surface was measured. The number of wrinkles was evaluated as "◎" when there were 0 wrinkles, "○" when there were 1 to 10 wrinkles, "△" when there were 11 to 20 wrinkles, and "×" when there were 21 or more wrinkles. When the number of wrinkles is 20 or less, it can be said that the film has sufficient wrinkle resistance as a release film when manufacturing a flexible circuit board. More preferably, the number of wrinkles is 10 or less.
[0070] (3) Evaluation of embeddability CCL (20cm x 20cm, polyimide thickness 25μm, copper foil 35μm), coverlay with holes (20cm x 20cm, polyimide thickness 15μm, epoxy resin adhesive layer 25μm), and release film were stacked in this order from the bottom up. After aligning the position between the press dies preheated to 180℃ using a sliding vacuum heater press (MKP-3000V-WH-ST, Mikado Technos), pressing was started (it took about 10 seconds from placement to actually applying pressure). Under vacuum conditions, 50kg / cm 2 A flexible circuit board (FPC) evaluation sample consisting of the CCL and coverlay was produced by pressing the CCL and coverlay at 0.8 V for 2 minutes. The FPC evaluation sample and the release film were then removed, and the release film was peeled off, after which the distance (μm) that the adhesive had seeped out was measured. A seepage distance of 40 μm or less was evaluated as "◎", a seepage distance of more than 40 μm and less than 50 μm was evaluated as "◯", and a seepage distance of more than 50 μm was evaluated as "×". When the seepage is 50 μm or less, it can be said that the film has sufficient embedding properties as a release film when manufacturing flexible circuit boards.
[0071] [Table 1] [Industrial Applicability]
[0072] According to the present invention, it is possible to provide a release film which has better releasability than conventional ones and can be suitably used in the production of flexible circuit boards by the roll-to-roll method.
Claims
1. A release film having at least one release layer and a cushion layer, The release layer contains an aromatic polyester resin, The cushion layer has a resin content of 20% by weight or more that constitutes the release layer, A release film having an orientation function f of 0.35 or more, which is calculated based on an infrared absorption spectrum measured by a total reflection method and is calculated using the following formula (1): [0010] In formula (1), A1 represents the absorption intensity due to C=O stretching motion in the incident direction (first direction) in which the absorption due to C=O stretching motion is greatest, and A2 represents the absorption intensity due to C=O stretching motion in a direction perpendicular to the first direction (second direction).
2. The release film according to claim 1, characterized in that the release layer has an orientation function g calculated by the following formula (2) based on an infrared absorption spectrum by a transmission method, which is smaller than the orientation function f of the surface of the release layer. [0025] In formula (2), A3 represents the overtone absorption intensity due to C=O stretching motion in the incident direction (third direction) in which absorption due to C=O stretching motion is greatest, and A4 represents the overtone absorption intensity due to C=O stretching motion in the direction perpendicular to the first direction (fourth direction).
3. A release film having at least one release layer, the release layer containing an aromatic polyester resin, and having an orientation function f calculated based on an infrared absorption spectrum measured by a total reflection measurement method according to the following formula (1) of 0.35 or more: The release layer has a surface arithmetic mean roughness Ra of 2 μm or more. [0030] In formula (1), A1 represents the absorption intensity due to C=O stretching motion in the incident direction (first direction) in which the absorption due to C=O stretching motion is greatest, and A2 represents the absorption intensity due to C=O stretching motion in a direction perpendicular to the first direction (second direction).
4. 4. The release film according to claim 1, 2 or 3, wherein the aromatic polyester resin contains a polybutylene terephthalate resin.
5. 5. The release film according to claim 4, wherein the proportion of polybutylene terephthalate resin in the resin constituting the release layer is 75% by weight or more.
6. A release film as described in claim 1, 2, 3, 4 or 5, characterized in that it has a structure in which release layers are arranged on both sides of the cushion layer.
7. 7. The release film according to claim 1, 2, 3, 4, 5 or 6, which is used in the production of flexible circuit boards by a roll-to-roll method.
8. 8. The release film according to claim 1, wherein the release layer has an arithmetic mean roughness Ra of 0.30 μm or less before the surface treatment.
9. A method for producing the release film according to claim 1, 2, 3, 4, 5, 6, 7 or 8, comprising the steps of: A step of surface treating the release film is included, The arithmetic mean roughness Ra of the surface of the release layer before the surface treatment is 0.30 μm or less. A method for producing a release film.
Citation Information
Patent Citations
Manufacture of laminated printed board
JP1993283862A
Mold release film
JP2009132806A
Mold release film, and method for producing semiconductor device-sealed body
JP2014213493A
Multilayer release film
JP2015058691A
Release film and use method of release film
JP2016068371A