Method for producing thermoplastic resin film

By applying a phenyl-group compound with controlled viscosity to the T-die lip, the method addresses resin adhesion and streak issues in thermoplastic resin films, ensuring consistent film quality during prolonged production.

JP7583637B2Active Publication Date: 2024-11-14KURARAY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021022023
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-15
Publication Date
2024-11-14
Estimated Expiration
2041-02-15

AI Technical Summary

Technical Problem

Conventional methods for producing thermoplastic resin films suffer from the occurrence of white streaks due to resin adhesion to the T-die lip, which is exacerbated by silicone oil deterioration and deformation of the lip shape during long-term production, leading to poor film appearance.

Method used

Applying a compound with a phenyl group and specific viscosity properties to the T-die lip, ensuring the viscosity ratio between the compound and thermoplastic resin composition satisfies certain conditions to prevent resin adhesion and streak formation during continuous film production.

Benefits of technology

The method effectively suppresses white streaks in thermoplastic resin films during long-term production by maintaining the compound's applicability and preventing resin adhesion, resulting in improved film quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583637000006
    Figure 0007583637000006
  • Figure 0007583637000001
    Figure 0007583637000001
  • Figure 0007583637000002
    Figure 0007583637000002
Patent Text Reader

Abstract

To provide a method for producing a thermoplastic resin film, which is capable of suppressing white streaks occurring in a film flow direction even in long-term continuous production.SOLUTION: There is provided a method for producing a film comprising a step of extruding a thermoplastic resin composition (II) in a molten state from a T-die lip coated with a compound (I) having a phenyl group and a viscosity of 0.005 to 2.0 Pa s at 25°C, in which a viscosity of the compound (I) and a viscosity of the thermoplastic resin composition (II) satisfy the following relational formulas (1) and (2): formula (1); PII>PI-1, formula (2); PII>PI-2, in which PI-1: a viscosity of the compound (I) after heating for 24 hours at T-die temperature, PI-2: a viscosity of the compound (I) after heating for 48 hours at a temperature 30°C lower than T-die temperature, PII: a viscosity of the thermoplastic resin composition (II) at T-die temperature.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a thermoplastic resin film by melt extrusion. [Background technology]

[0002] Thermoplastic resin films are used for optical and decorative applications because they have excellent optical properties such as high transparency and low birefringence, and can be easily formed into films by melt molding. One of the common methods for forming thermoplastic resin films is to feed a thermoplastic resin composition as a raw material from a hopper to an extruder, heat and melt it, and then extrude it from a die to form a film. However, this method has a problem in that streaks occur in the flow direction of the film. The occurrence of streaks in the film not only impairs the surface condition, but also causes poor appearance when a coating layer is applied to the film surface in optical and decorative applications.

[0003] As a method for suppressing the occurrence of such streaks, Patent Document 1 proposes a method of forming a T-die lip in a specific shape to prevent the resin from adhering to the lip and suppress the occurrence of streaks. Patent Document 2 shows that applying silicone oil to the die reduces low molecular weight substances originating from thermoplastic resin that adhere to the lower surface of the die and cause streaks. Patent Document 3 shows a method of suppressing black streaks (streaks that appear black due to indirect reflected light) and die lines using a static mixer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-255453 A [Patent Document 2] JP 2002-307523 A [Patent Document 3] JP 2017-185760 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, with the above-mentioned conventional technology, the lip shape changes every time the T-die is disassembled and the lip is cleaned repeatedly, making it difficult to prevent resin from adhering to the lip for a long period of time. Also, simply applying silicone oil can cause streaks due to the deterioration of the silicone oil. As a result, it was not possible to improve the white streaks (streaks that appear white due to indirect reflected light) that occur in the flow direction of the film. The present invention has been made in consideration of these circumstances, and aims to provide a method for producing a thermoplastic resin film that can suppress the occurrence of white streaks in the flow direction of the film even during long-term continuous production. [Means for solving the problem]

[0006] As a result of extensive investigations aimed at solving the above-mentioned problems, the inventors discovered that by applying a compound that contains a phenyl group and has specific thermal properties to a T-die, the occurrence of white streaks can be suppressed even during long periods of continuous production, and thus completed the present invention.

[0007] The present invention relates to the following items [1] to [6]. [1] A method for producing a film, comprising the step of extruding a molten thermoplastic resin composition (II) from a T-die lip coated with a compound (I) having a phenyl group and a viscosity of 0.005 to 2.0 [Pa s] at 25°C, A method for producing a thermoplastic resin film, characterized in that the viscosity of the compound (I) and the viscosity of the thermoplastic resin composition (II) satisfy the following relational expressions (1) and (2): P II >P I-1 (1) P II >P I-2 (2) P I-1 : Viscosity of the compound (I) after heating at die temperature for 24 hours P I-2 : Viscosity of the compound (I) after heating for 48 hours at a temperature 30°C lower than the die temperature P II : Viscosity of the thermoplastic resin composition (II) at die temperature

[0008] [2] The method for producing a film according to [1] above, wherein the compound (I) is a silicone oil, and the phenyl group is directly bonded to a silicon atom other than a terminal of the silicone oil. [3] P. II and the above P I-1 But, P II / P I-1 The method for producing a thermoplastic resin film according to the above [1] or [2], wherein the relationship of [4] The method for producing a thermoplastic resin film according to any one of [1] to [3] above, wherein the thermoplastic resin composition (II) contains a (meth)acrylic resin (A).

[0009] [5] The method for producing a thermoplastic resin film according to any one of [1] to [4] above, wherein the thermoplastic resin composition (II) contains (meth)acrylic polymer particles (B) having a multilayer structure. [6] The method for producing a thermoplastic resin film according to any one of [1] to [5] above, wherein the thermoplastic resin composition (II) has a viscosity of 200 to 2,000 Pa s at 270°C and a shear rate of 122 / sec. Effect of the Invention

[0010] According to the present invention, it is possible to provide a method for producing a thermoplastic resin film that can suppress the occurrence of white streaks in the machine direction of the film even during long-term continuous production. [Brief description of the drawings]

[0011] [Figure 1] 1 is a diagram showing one embodiment of a method for producing a thermoplastic resin film of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The method for producing a thermoplastic resin film of the present invention is a method for producing a film, comprising a step of extruding a molten thermoplastic resin composition (II) from a T-die lip to which a compound (I) having a phenyl group and a viscosity of 0.005 to 2.0 [Pa s] at 25°C has been applied, and is characterized in that the viscosity of the compound (I) and the viscosity of the thermoplastic resin composition (II) satisfy the following relational expressions (1) and (2): P II >P I-1 (1) P II >P I-2 (2) P I-1 : Viscosity of the compound (I) after heating at die temperature for 24 hours P I-2 : Viscosity of the compound (I) after heating for 48 hours at a temperature 30°C lower than the die temperature P II : Viscosity of the thermoplastic resin composition (II) at die temperature

[0013] The present inventors have found that by using a compound having a phenyl group as compound (I), the coatability onto a T-die is improved and compound (I) is less likely to deteriorate on the T-die lip for a long period of time. Furthermore, they have found that by making the viscosity of compound (I) after heating at the T-die temperature for 24 hours smaller than the viscosity of thermoplastic resin composition (II) at the T-die temperature and making the viscosity of compound (I) after heating at a temperature 30°C lower than the T-die temperature for 48 hours smaller than the viscosity of thermoplastic resin composition (II), solidification of compound (I) is easily suppressed, the surface of the film does not deform even when the thermoplastic resin composition (II) extruded from the T-die lip comes into contact with compound (I), the occurrence of white streaks can be suppressed, and the occurrence of white streaks when film production is continued can be suppressed. In the present invention, the "T-die temperature" refers to the set temperature of the T-die (the set temperature of the extruder).

[0014] <Compound (I)> In the present invention, compound (I) is a compound having a phenyl group and a viscosity of 0.005 to 2.0 [Pa s] at 25° C. Since compound (I) is a compound having a phenyl group, the coatability onto a T-die is improved, and the compound remains on the T-die lip for a long time without being altered, making it possible to produce a film for a long time while suppressing the occurrence of white streaks. In addition, since the compound (I) is applied to the T-die, it is preferable that the compound (I) has a role as a mold release agent. By having the property of a mold release agent, it is possible to prevent low molecular weight components contained in the thermoplastic resin composition (II) from adhering to the T-die lip. In addition, even under conditions in which the resin discharge amount is not constant at the start of film formation, it is possible to suppress the thermoplastic resin composition (II) from adhering to the T-die lip, so that the occurrence of white streaks can be further suppressed.

[0015] The viscosity of the compound (I) at 25°C is 0.005 to 2.0 [Pa·s]. If the viscosity is more than 2.0 [Pa·s], the handling property at room temperature of about 25°C is reduced, and as a result, it becomes difficult to apply the compound uniformly to the T-die lip. On the other hand, if the viscosity is less than 0.005 [Pa·s], the handling property can be ensured, but there are problems that the compound volatilizes during film formation, making it difficult to exert the effect of suppressing white streaks for a long time, and that the flash point is low, making it difficult to ensure safety. From these viewpoints, the viscosity of the compound (I) at 25°C is preferably 0.01 to 1.5 [Pa·s], more preferably 0.02 to 1.0 [Pa·s], and even more preferably 0.03 to 0.6 [Pa·s]. The viscosity of compound (I) in the present invention refers to the viscosity at a shear rate of 100 [1 / s], and specifically, can be measured by the method described in the Examples.

[0016] The present invention is further characterized in that the compound (I) and the thermoplastic resin composition (II) satisfy the following relational expressions (1) and (2). P II >P I-1 (1) P II >P I-2 (2) P I-1 : Viscosity of the compound (I) after heating at die temperature for 24 hours P I-2 : Viscosity of the compound (I) after heating for 48 hours at a temperature 30°C lower than the die temperature P II : Viscosity of the thermoplastic resin composition (II) at die temperature

[0017] In the present invention, P II and P I-1 But, P II >P I-1 By satisfying [relationship formula (1)], the viscosity of the compound (I) does not increase even when the film is continuously produced for a long period of time, and the occurrence of white streaks in the thermoplastic resin composition (II) extruded as a film can be suppressed. II and P I-1 , P II / P I-1 It is preferable that the relationship of >100 is satisfied, and P II / P I-1 It is more preferable that the relationship satisfies >500, and P II / P I-1 It is more preferable that the relationship of P II / P I-1 It is even more preferable that the relationship satisfies >10,000, and P II / P I-1 It is particularly preferred that the relationship be satisfied. II / P I-1 When P is greater than the lower limit, the viscosity of compound (I) is sufficiently low, so that the occurrence of white streaks in the produced film can be more effectively suppressed. II / P I-1 There is no particular upper limit, but it may be 100,000 or 500,000.

[0018] In the present invention, P II and P I-2 But, P II >P I-2By satisfying the above condition, the thermoplastic resin composition (II) discharged from the T-die is prevented from being damaged by the compound (I) applied to the T-die. II and P I-2 , P II / P I-2 It is preferable that the relationship of >100 is satisfied, and P II / P I-2 It is more preferable that the relationship satisfies >500, and P II / P I-2 It is more preferable that the relationship of P II / P I-2 It is even more preferable that the relationship satisfies >10,000, and P II / P I-2 It is particularly preferred that the relationship be satisfied. II / P I-2 There is no particular upper limit, but it may be 100,000 or 500,000.

[0019] The method of applying the compound (I) to the T-die lip is not particularly limited, but the compound (I) may be applied by soaking a rag or the like in the compound (I), or the compound (I) may be applied by spraying. Alternatively, the compound (I) may be mixed with a solvent and then applied by the above method, and the solvent may be removed by volatilization.

[0020] The coating amount of the compound (I) is 0.03 to 3 mg / cm based on the coating surface of the T-die lip. 2 is preferably 0.03 to 2 mg / cm 2 When the coating amount is equal to or more than the lower limit, the effect of suppressing white streaks can be sufficiently obtained, whereas when the coating amount is equal to or less than the upper limit, the balance between the production cost and the obtained effect is improved.

[0021] From the viewpoint of the safety of the production process, the compound (I) is preferably selected such that the relationship between the flash point (Ta) and the T die temperature (Tt) satisfies Ta≧Tt+20(° C.), and more preferably Ta≧Tt+30(° C.).

[0022] There are no particular limitations on the compound (I) so long as it satisfies the above-mentioned properties. Examples include fluorine-based resins and silicone oils, and among these, silicone oils are preferred. As the silicone oil having phenyl group, phenyl-modified silicone, alkyl-modified silicone, polyether-modified silicone, carboxy-modified silicone, etc. can be used, and phenyl-modified silicone is particularly preferred, and among them, the one in which phenyl group is directly bonded to the silicon atom other than the end of silicone oil is more preferred.The silicone oil in which phenyl group is directly bonded to the silicon atom other than the end of silicone oil has excellent applicability to T-die, and is easy to remain on T-die lip for a long time, so that it can obtain the effect of suppressing white streaks for a long time.

[0023] The phenyl-modified silicone preferably has a phenyl modification rate of 3 to 50%. When the phenyl modification rate is within the above range, compound (I) is more likely to remain on the T-die lip for a long period of time. From this viewpoint, the phenyl modification rate is more preferably 10 to 50%, and even more preferably 10 to 40%. The phenyl modification rate is the number of phenyl groups relative to the total number of phenyl groups and methyl groups bonded to silicon atoms, expressed as a percentage.

[0024] Examples of commercially available products of compound (I) include "TSF4300", "TSF437", "TSF433", and "TSF431" manufactured by Momentive Performance Materials Japan, LLC; "SH510" manufactured by DuPont Toray Specialty Materials Co., Ltd.; "KF-50", "KF-54", and "KF-56A" manufactured by Shin-Etsu Chemical Co., Ltd.; and "WACKER SILICONE FLUID AP 100-1000" manufactured by Wacker Asahi Kasei Silicone Co., Ltd.

[0025] <Thermoplastic resin composition (II)> The thermoplastic resin composition (II) used in the present invention is not particularly limited as long as it contains a thermoplastic resin. From the viewpoint of easily suppressing the occurrence of die lines and from the viewpoint of producing a film suitable for optical applications and the like, however, it is preferably an amorphous thermoplastic resin composition, and among these, it is particularly preferably a resin composition containing a (meth)acrylic resin (A), i.e., a (meth)acrylic resin composition. In the present invention, "(meth)acrylic" means acrylic and / or methacrylic.

[0026] The (meth)acrylic resin (A) used in the present invention is not particularly limited, but preferably contains a structural unit derived from methyl methacrylate and, if necessary, a structural unit derived from an acrylic acid ester. Examples of acrylic acid esters that can be used in the (meth)acrylic resin (A) include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, s-butyl acrylate, t-butyl acrylate, amyl acrylate, isoamyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, pentadecyl acrylate, dodecyl acrylate, cyclohexyl acrylate, norbornenyl acrylate, isobornyl acrylate, benzyl acrylate, phenoxyethyl acrylate, 2-hydroxyethyl acrylate, 2-ethoxyethyl acrylate, glycidyl acrylate, allyl acrylate, and phenyl acrylate. Among these, alkyl acrylates in which the alkyl group has 1 to 6 carbon atoms are preferred.

[0027] The amount of structural units derived from methyl methacrylate in the (meth)acrylic resin (A) is preferably 85 to 100% by mass, and more preferably 90 to 100% by mass, from the viewpoint of improving the mechanical strength of the thermoplastic resin film. When the (meth)acrylic resin (A) contains a structural unit derived from an acrylic ester, the amount thereof in the (meth)acrylic resin (A) is preferably 0.01 to 15 mass %, more preferably 0.1 to 10 mass %, from the viewpoint of improving the thickness accuracy of the thermoplastic resin film.

[0028] The glass transition temperature of the (meth)acrylic resin (A) used in the present invention is preferably 95° C. or higher, more preferably 100° C. or higher, and even more preferably 105° C. or higher. When the glass transition temperature is equal to or higher than the lower limit, the thickness precision of the thermoplastic resin film is improved. The glass transition temperature of the (meth)acrylic resin (A) used in the present invention is usually 130° C. or lower. The glass transition temperature of the (meth)acrylic resin (A) can be measured in accordance with JIS K7121:2012. When the (meth)acrylic resin (A) has a plurality of glass transition temperatures, it is sufficient that at least one of the glass transition temperatures satisfies the above range, it is preferable that the plurality of glass transition temperatures satisfies the above range, and it is more preferable that all of the glass transition temperatures satisfy the above range.

[0029] The weight average molecular weight of the (meth)acrylic resin (A) is preferably 60,000 to 150,000. When the weight average molecular weight is equal to or more than the lower limit, the mechanical properties are improved, and when it is equal to or less than the upper limit, the viscosity is lowered and the processability is improved. From the above viewpoints, the weight average molecular weight is more preferably 70,000 to 120,000, and further preferably 80,000 to 100,000. The weight average molecular weight of the (meth)acrylic resin (A) can be measured by the method described in the Examples.

[0030] The method for producing the (meth)acrylic resin (A) is not particularly limited, and it can be produced by known polymerization methods such as radical polymerization, anionic polymerization, etc. There are no particular limitations on the production conditions, and the desired (meth)acrylic resin (A) can be obtained by appropriately adjusting the polymerization temperature, polymerization time, the type and amount of the chain transfer agent, the type and amount of the polymerization initiator, etc.

[0031] The content of the (meth)acrylic resin (A) in the thermoplastic resin composition (II) of the present invention is preferably 60 mass % or more, more preferably 70 mass % or more, and even more preferably 75 mass % or more, from the viewpoint of improving the transparency of the thermoplastic resin film.

[0032] <(Meth)acrylic polymer particles (B) having a multilayer structure> The thermoplastic resin composition (II) used in the present invention preferably contains (meth)acrylic polymer particles (B) having a multilayer structure (hereinafter also simply referred to as "polymer particles (B)"). In the present invention, when the thermoplastic resin composition (II) contains the (meth)acrylic polymer particles (B) having a multilayer structure, the effects of the present invention are particularly easily obtained. The reason for this is presumed to be as follows. When small lumps (which may be in a molten state) originating from the thermoplastic resin composition (II) containing the (meth)acrylic polymer particles (B) having a multilayer structure are generated on the T-die lip, the polymer particles (B) are contained in the lumps at a relatively high concentration, and it is assumed that these polymer particles (B) will aggregate over time, which will cause white streaks, but in the present invention, the compound (I) applied to the T-die is present so as to surround the polymer particles (B), which is believed to prevent the aggregation of the polymer particles (B). It is assumed that this makes it possible to more effectively suppress the generation of white streaks on the thermoplastic resin composition (II).

[0033] The (meth)acrylic polymer particles (B) having a multilayer structure are not particularly limited as long as they have a multilayer structure, and for example, an acrylic polymer having a core-shell multilayer structure can be mentioned. In addition, the number of layers constituting the multilayer structure is not particularly limited, and it may be two layers or three layers or more. Among these, from the viewpoint of improving the impact resistance of the thermoplastic resin film, the polymer particles (B) are preferably acrylic polymers having a core-shell multilayer structure, more specifically, acrylic polymers having a core-shell multilayer structure consisting of three layers: a core (inner layer), an inner shell (middle layer), and an outer shell (outer layer). In the present invention, the acrylic polymer having a core-shell multilayer structure consisting of three layers refers to an acrylic polymer in which the core and the inner shell, and the inner shell and the outer shell are each composed of different polymers. When a resin composition containing the acrylic polymer having a core-shell multilayer structure consisting of three layers is melt-kneaded, all or a part of the outer shell is fused and united with the (meth)acrylic resin (A) to form a matrix, and the matrix contains core-shell particles consisting of two layers, a core and an inner shell.

[0034] Hereinafter, an acrylic polymer having a core-shell multilayer structure consisting of three layers, a core (inner layer), an inner shell (middle layer), and an outer shell (outer layer), will be described in detail. The polymer constituting the core will be referred to as "polymer (a)", the polymer constituting the inner shell as "polymer (b)", and the polymer constituting the outer shell as "polymer (c)".

[0035] [Polymer (a): Polymer constituting the core] The polymer (a) is preferably a polymer containing a structural unit derived from methyl methacrylate, a structural unit derived from an alkyl acrylate, a structural unit derived from a grafting agent, and, if necessary, a structural unit derived from a crosslinking agent. In the present invention, the grafting agent means a monomer having two or more different polymerizable groups, and the crosslinking agent means a monomer having two or more of the same type of polymerizable groups (excluding the grafting agent).

[0036] The alkyl acrylate used in the polymer (a) is not particularly limited, but the number of carbon atoms in the alkyl group is preferably 1 to 8, more preferably 1 to 6. When the number of carbon atoms in the alkyl group in the alkyl acrylate is within the above range, the thermal decomposition resistance of the (meth)acrylic polymer particles (B) having a multilayer structure is improved, and the hot water whitening resistance and boiling water whitening resistance of the thermoplastic resin film are improved. Specific examples of the alkyl acrylate include methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, s-butyl acrylate, t-butyl acrylate, n-butyl methyl acrylate, n-heptyl acrylate, 2-ethylhexyl acrylate, and n-octyl acrylate. These can be used alone or in combination of two or more. Among these, methyl acrylate is particularly preferred from the above viewpoint.

[0037] It is preferable that the polymer (a) contains a structural unit derived from a grafting agent for the purpose of chemically bonding the polymer (a) and the polymer (b) and for the purpose of assisting the formation of a crosslinked structure of the polymer (a). Examples of the grafting agent used in the polymer (a) include allyl methacrylate, allyl acrylate, mono- or di-allyl maleate, mono- or di-allyl fumarate, crotyl acrylate, and crotyl methacrylate, etc. These grafting agents can be used alone or in combination of two or more. Among these, allyl methacrylate is preferred from the viewpoints of improving the bonding ability between the polymer (a) and the polymer (b) and improving the stress whitening resistance and transparency of the thermoplastic resin film.

[0038] The polymer (a) may contain a structural unit derived from a crosslinking agent for the purpose of forming a crosslinked structure in the polymer (a) and for the purpose of forming a graft structure between the polymer (a) and the polymer (b). Examples of the crosslinking agent used in the polymer (a) include diacryl compounds, dimethacrylic compounds, diallyl compounds, divinyl compounds, diene compounds, trivinyl compounds, etc. More specifically, ethylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, divinylbenzene, trivinylbenzene, ethylene glycol diallyl ether, propylene glycol diallyl ether, butadiene, etc. These crosslinking agents can be used alone or in combination of two or more.

[0039] The amount of structural units derived from methyl methacrylate in the polymer (a) is preferably 40 to 98.99 mass%, more preferably 45 to 96.9 mass%, of the total structural units of the polymer (a). When the amount of structural units derived from methyl methacrylate is equal to or more than the lower limit, the weather resistance of the thermoplastic resin film is improved, and when the amount is equal to or less than the upper limit, the impact resistance of the thermoplastic resin film is improved.

[0040] The amount of structural units derived from alkyl acrylate in polymer (a) is preferably 1 to 59 mass %, more preferably 3 to 55 mass %, of the total structural units of polymer (a). When the amount of structural units derived from alkyl acrylate is equal to or more than the lower limit, the thermal decomposition resistance of the multilayered (meth)acrylic polymer particles (B) is improved, and when the amount is equal to or less than the upper limit, the hot water whitening resistance and boiling water whitening resistance of the thermoplastic resin film are improved.

[0041] The amount of the structural units derived from the grafting agent in the polymer (a) is preferably 0.01 to 1 mass %, more preferably 0.1 to 0.5 mass %, based on the total structural units of the polymer (a). When the amount of the structural units derived from the grafting agent is equal to or more than the lower limit, the bonding strength between the polymer (a) and the polymer (b) is improved, and when the amount is equal to or less than the upper limit, the impact resistance of the thermoplastic resin film is improved.

[0042] The amount of the structural units derived from the crosslinking agent in the polymer (a) is preferably 0 to 0.5% by mass, more preferably 0 to 0.2% by mass, based on the total amount of the structural units in the polymer (a). When the amount of the structural units derived from the crosslinking agent is within the above range, the impact resistance of the thermoplastic resin film is improved.

[0043] The polymer (a) and the polymer (b) described later are preferably insoluble in a solvent such as acetone, i.e., grafted. When the polymer (a) and the polymer (b) are grafted, the polymer (a) and the polymer (b) are present as particles having a two-layer structure in the matrix of the polymer (c) described later, which is preferable because it improves the impact resistance of the thermoplastic resin film.

[0044] [Polymer (b): Polymer constituting the inner shell] The polymer (b) is preferably a polymer containing a structural unit derived from an alkyl acrylate, a structural unit derived from a grafting agent, and, if necessary, a structural unit derived from an aromatic vinyl compound and a structural unit derived from a crosslinking agent.

[0045] Examples of the alkyl acrylate used in the polymer (b) include the alkyl acrylates exemplified for the polymer (a). From the viewpoints of improving the thermal decomposition resistance of the (meth)acrylic polymer particles (B) having a multilayer structure and improving the hot water whitening resistance and boiling water whitening resistance of the thermoplastic resin film, n-butyl acrylate is particularly preferred.

[0046] Examples of the aromatic vinyl compound used in the polymer (b) include aromatic vinyl compounds such as styrene, α-methylstyrene, p-methylstyrene, and m-methylstyrene, and from the viewpoint of improving the thermal decomposition resistance of the (meth)acrylic polymer particles (B) having a multilayer structure, styrene is preferred.

[0047] In addition, examples of the grafting agent used for the polymer (b) include the grafting agents exemplified for the polymer (a) above. From the viewpoint of improving the bonding ability between the polymer (a) and the polymer (b) and improving the stress whitening resistance and transparency of the thermoplastic resin film, allyl methacrylate is preferred.

[0048] Examples of the crosslinking agent used for the polymer (b) include the crosslinking agents exemplified for the polymer (a) above. From the viewpoint of forming a crosslinked structure in the polymer (b) and between the polymer (a) and the polymer (b), preferred are diacrylic compounds, dimethacrylic compounds, diallyl compounds, divinyl compounds, and the like.

[0049] The amount of the structural units derived from alkyl acrylate in polymer (b) is preferably 70 to 99.5 mass %, more preferably 80 to 99 mass %, of the total structural units in polymer (b). When the amount of the structural units derived from alkyl acrylate is equal to or more than the lower limit, the impact resistance of the thermoplastic resin film is improved, and when the amount is equal to or less than the upper limit, the stress whitening resistance and transparency of the thermoplastic resin film are improved.

[0050] The amount of structural units derived from an aromatic vinyl compound in the polymer (b) is preferably 0 to 29% by mass, more preferably 0 to 20% by mass, based on the total amount of structural units in the polymer (b). When the amount of structural units derived from methyl methacrylate is within the above range, the impact resistance of the thermoplastic resin film is improved.

[0051] The amount of structural units derived from the grafting agent in the polymer (b) is preferably 0.5 to 5 mass %, more preferably 1 to 4 mass %, based on the total structural units of the polymer (b). When the amount of structural units derived from the grafting agent is equal to or more than the lower limit, the stress whitening resistance of the thermoplastic resin film is improved. On the other hand, when the amount is equal to or less than the upper limit, the impact resistance of the thermoplastic resin film is improved.

[0052] The amount of the structural units derived from the crosslinking agent in the polymer (b) is preferably 0 to 5 mass %, more preferably 0 to 2 mass %, based on the total amount of the structural units in the polymer (b). When the amount of the structural units derived from the crosslinking agent is within the above range, the impact resistance of the thermoplastic resin film is improved.

[0053] In the present invention, the polymer (b) is preferably softer than the polymer (a) and the polymer (c). When the polymer (b) is softer than the polymer (a) and the polymer (c), the impact resistance is improved.

[0054] [Polymer (c): Polymer constituting the outer shell] The polymer (c) is preferably a polymer containing a structural unit derived from methyl methacrylate and a structural unit derived from an alkyl acrylate. Examples of the alkyl acrylate used in the polymer (c) include the alkyl acrylates exemplified for the polymer (a). Methyl acrylate is particularly preferred from the viewpoints of improving the thermal decomposition resistance of the (meth)acrylic polymer particles (B) having a multilayer structure and improving the hot water whitening resistance and boiling water whitening resistance of the thermoplastic resin film.

[0055] The amount of structural units derived from methyl methacrylate in polymer (c) is preferably 80 to 99 mass %, more preferably 85 to 98 mass %, of the total structural units of polymer (c). When the amount of structural units derived from methyl methacrylate is equal to or more than the lower limit, the stress whitening resistance of the thermoplastic resin film is improved. On the other hand, when the amount is equal to or less than the upper limit, the thermal decomposition resistance of the thermoplastic resin film is improved.

[0056] The amount of the structural units derived from alkyl acrylate in the polymer (c) is preferably 1 to 19 mass %, more preferably 2 to 15 mass %, based on the total amount of structural units in the polymer (c). When the amount of the structural units derived from alkyl acrylate is equal to or more than the lower limit, the thermal decomposition resistance of the (meth)acrylic polymer particles (B) having a multilayer structure is improved, and when the amount is equal to or more than the lower limit, the stress whitening resistance of the thermoplastic resin film is improved.

[0057] It is preferable that the polymer (c) is soluble in a solvent such as acetone, i.e., is not crosslinked. When the polymer (c) is not crosslinked, when the (meth)acrylic polymer particles (B) having a multilayer structure consisting of the polymer (a), the polymer (b) and the polymer (c) are used, the polymer (c) forms a matrix in which the particles consisting of the polymer (a) and the polymer (b) are present, and the ease of production of the thermoplastic resin film is improved.

[0058] [Mass ratio of polymer (a), polymer (b) and polymer (c)] The amount of polymer (a) in the (meth)acrylic polymer particles (B) having a multilayer structure is preferably 1 to 50% by mass, more preferably 5 to 45% by mass, and even more preferably 10 to 40% by mass. When the amount of polymer (a) is equal to or more than the lower limit, the thermal stability and productivity of the thermoplastic resin film are improved. On the other hand, when the amount of polymer (a) is equal to or less than the upper limit, the impact resistance and flexibility of the thermoplastic resin film are improved.

[0059] The amount of polymer (b) in the (meth)acrylic polymer particles (B) having a multilayer structure is preferably 20 to 60% by mass, more preferably 25 to 55% by mass, and even more preferably 30 to 50% by mass. When the amount of polymer (b) is equal to or more than the lower limit, the thermal stability and productivity of the thermoplastic resin film are improved. On the other hand, when the amount of polymer (b) is equal to or less than the upper limit, the impact resistance and flexibility of the thermoplastic resin film are improved.

[0060] The amount of polymer (c) in the (meth)acrylic polymer particles (B) having a multilayer structure is preferably 5 to 40% by mass, more preferably 10 to 35% by mass, and even more preferably 15 to 30% by mass. When the amount of polymer (c) is equal to or more than the lower limit, the flowability of the (meth)acrylic polymer particles (B) having a multilayer structure and the moldability of the thermoplastic resin film are improved. When the amount of polymer (c) is equal to or less than the upper limit, the impact resistance and stress whitening resistance of the thermoplastic resin film are improved.

[0061] [Method for producing (meth)acrylic polymer particles (B) having a multilayer structure] The method for producing the (meth)acrylic polymer particles (B) having a multilayer structure used in the present invention is not particularly limited. For example, the particles can be obtained as a latex by successively forming a polymer (a) in a primary polymerization, a polymer (b) in a secondary polymerization, and a polymer (c) in a tertiary polymerization, using a seed emulsion polymerization method.

[0062] The polymerization initiator used in the production of the (meth)acrylic polymer particles (B) having a multilayer structure is not particularly limited, and examples thereof include water-soluble inorganic initiators such as potassium persulfate and ammonium persulfate; redox initiators obtained by combining an inorganic initiator with a sulfite or a thiosulfate; and redox initiators obtained by combining an organic peroxide with a ferrous salt or sodium sulfoxylate. The polymerization initiator may be added to the reaction system all at once at the start of polymerization, or may be added to the reaction system in portions at the start of polymerization and during polymerization, taking into consideration the reaction rate, etc. The amount of the polymerization initiator used can be appropriately set, for example, so that the average particle size of the (meth)acrylic polymer particles (B) having a multilayer structure falls within the range described below.

[0063] From the viewpoint of obtaining the (meth)acrylic polymer particles (B) having a multilayer structure as a latex, it is preferable to use an emulsifier. There is no particular limitation on the emulsifier, but examples thereof include anionic emulsifiers such as long-chain alkyl sulfonates, sulfosuccinic acid alkyl ester salts, and alkylbenzene sulfonates; nonionic emulsifiers such as polyoxyethylene alkyl ethers and polyoxyethylene nonylphenyl ether; nonionic and anionic emulsifiers such as polyoxyethylene nonylphenyl ether sulfates such as sodium polyoxyethylene nonylphenyl ether sulfate, polyoxyethylene alkyl ether sulfates such as sodium polyoxyethylene alkyl ether sulfate, and alkyl ether carboxylates such as sodium polyoxyethylene tridecyl ether acetate. The amount of the emulsifier used can be appropriately set so that the average particle size of the (meth)acrylic polymer particles (B) having a multilayer structure falls within the range described below.

[0064] In the present invention, a chain transfer agent can be used in each polymerization step in order to adjust the molecular weight of the (meth)acrylic polymer particles (B) having a multilayer structure. In particular, in the third polymerization step, the chain transfer agent can be added to the reaction system to adjust the molecular weight of the polymer (c). The chain transfer agent used in producing the (meth)acrylic polymer particles (B) having a multilayer structure is not particularly limited, and examples thereof include alkyl mercaptans such as n-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, and n-hexadecyl mercaptan; xanthogen disulfides such as dimethyl xanthogen disulfide and diethyl xanthogen disulfide; thiuram disulfides such as tetrathiuram disulfide; and halogenated hydrocarbons such as carbon tetrachloride and ethylene bromide.

[0065] The amount of the chain transfer agent used can be appropriately set within a range that allows the polymer to be adjusted to a predetermined molecular weight in each polymerization. The amount of the chain transfer agent used in the tertiary polymerization varies depending on the amount of the polymerization initiator used in the tertiary polymerization, and is preferably 0.05 to 2 parts by mass, more preferably 0.08 to 1 part by mass, based on 100 parts by mass of the total amount of the monomers used in the tertiary polymerization, specifically, methyl methacrylate and alkyl acrylate.

[0066] In the above-mentioned production method, the first polymerization, the second polymerization, and the third polymerization may be carried out in sequence in one polymerization tank, or the first polymerization, the second polymerization, and the third polymerization may be carried out in sequence in different polymerization tanks, but it is preferable to carry out each polymerization in sequence in one polymerization tank. The temperature of the reaction system during the polymerization is preferably 30 to 120°C, more preferably 50 to 100°C.

[0067] Each of the polymerizations can be carried out by mixing the monomers, specifically methyl methacrylate, alkyl acrylate, grafting agent and crosslinking agent in the above ratio and supplying them to the reaction system. There is no particular restriction on the rate at which the monomers are supplied to the reaction system, but it is preferable to supply them at a rate of preferably 0.05 to 10 mass% / min, more preferably 0.1 to 8 mass% / min, and even more preferably 0.2 to 7 mass% / min, based on the total amount of the monomers used in each polymerization. Supplying them at the above rate can prevent the generation of undesirable polymer aggregates and the adhesion of polymer scale to the reaction tank, and can prevent appearance defects such as fish eyes that may occur due to the inclusion of polymer aggregates or polymer scale.

[0068] The latex obtained by the above method can be coagulated by a known method. Examples of the coagulation method include freeze coagulation method, salting out coagulation method, acid precipitation coagulation method, etc. Among these, the freeze coagulation method is preferred because it does not require the addition of a coagulant that is an impurity for the (meth)acrylic polymer particles (B) having a multilayer structure.

[0069] It is preferable to thoroughly wash and dehydrate the slurry obtained by solidification. By washing and dehydrating the slurry, water-soluble components such as emulsifiers and catalysts can be removed from the slurry. The washing and dehydration of the slurry can be performed, for example, using a filter press, a belt press, a Ginner type centrifuge, a screw decanter type centrifuge, etc. From the viewpoint of productivity and washing efficiency, it is preferable to use a screw decanter type centrifuge. It is preferable to wash and dehydrate the slurry at least twice. The more times the washing and dehydration are performed, the lower the remaining amount of water-soluble components. From the viewpoint of productivity, it is preferable that the number of times the washing and dehydration is performed is three or less.

[0070] Furthermore, it is preferable to dry the obtained slurry. The drying of the slurry is preferably carried out so that the moisture content of the (meth)acrylic polymer particles (B) having a multilayer structure obtained by the above-mentioned method is preferably less than 0.2% by mass, more preferably less than 0.1% by mass. The higher the moisture content, the more likely it is that an ester hydrolysis reaction will occur in the (meth)acrylic polymer particles (B) having a multilayer structure during melt extrusion molding, and carboxyl groups will be generated in the molecular chain, which will result in the generation of streaks in the thermoplastic resin film.

[0071] The average particle size of the (meth)acrylic polymer particles (B) having a multilayer structure is preferably 0.01 μm or more, more preferably 0.04 μm or more, even more preferably 0.05 μm or more, particularly preferably 0.07 μm or more, and preferably 0.35 μm or less, more preferably 0.30 μm or less. If the average particle size is too large, the stress whitening resistance of the thermoplastic resin film tends to decrease. The average particle size is determined by the method described in the Examples based on the light scattering method.

[0072] The content of the (meth)acrylic polymer particles (B) having a multilayer structure is preferably 5 to 50 parts by mass, more preferably 10 to 40 parts by mass, and even more preferably 15 to 30 parts by mass, per 100 parts by mass of the (meth)acrylic resin (A), from the viewpoint of improving the mechanical strength and processability of the thermoplastic resin film.

[0073] <Optional ingredients> The thermoplastic resin composition (II) used in the present invention may contain known additives such as ultraviolet absorbers, antioxidants, light stabilizers, plasticizers, polymer processing aids, lubricants, dyes, and pigments, as necessary. When the thermoplastic resin composition (II) contains an additive, the content thereof in the thermoplastic resin composition (II) is preferably 20 mass % or less. The additives may be added, for example, to the thermoplastic resin composition (II) molten in a film molding machine, or may be dry blended with the pelletized thermoplastic resin composition (II), or may be added when the (meth)acrylic polymer particles (B) and / or the (meth)acrylic resin (A) having a multilayer structure are pelletized (masterbatch method).

[0074] The thermoplastic resin composition (II) used in the present invention preferably contains an ultraviolet absorbing agent. For example, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol] can be mentioned as an example of the ultraviolet absorbing agent. The content of the ultraviolet absorbing agent is preferably 0.05 to 5 parts by mass based on 100 parts by mass of the total amount of the (meth)acrylic resin (A) and the polymer particles (B).

[0075] The viscosity of the thermoplastic resin composition (II) used in the present invention at 270°C and a shear rate of 122 / sec is preferably 200 to 2,000 Pa·s. The viscosity is more preferably 250 Pa·s or more, and even more preferably 300 Pa·s or more. Also, it is more preferably 1,500 Pa·s or less, and even more preferably 1,200 Pa·s or less. When the viscosity of the thermoplastic resin composition (II) is within the above range, it is possible to maintain a good melt tension in melt extrusion molding, to easily obtain a good film, and to maintain good mechanical properties such as breaking strength of the obtained film. The viscosity of the thermoplastic resin composition (II) refers to a value measured by the method described in the examples.

[0076] The method for producing a thermoplastic resin film of the present invention can be carried out, for example, by the apparatus shown in FIG. In the apparatus of Fig. 1, first, a thermoplastic resin composition (II) which is a raw material resin is melted in an extruder 1. Next, the molten thermoplastic resin composition (II) passes through a gear pump 2, is filtered through a polymer filter 3, passes through a static mixer 4, and is discharged in a sheet form from a T-die 5. The discharged molten resin is pressed between a roll 6 and a roll 7 and formed into a desired thickness. Thereafter, the thermoplastic resin film is wound up, for example, in a roll form.

[0077] <Extruder> As an extruder for melting and extruding the thermoplastic resin composition (II), for example, a single screw extruder, a twin screw extruder, a multi-screw extruder, etc. can be used. In the present invention, the extruder is preferably equipped with a vent mechanism in order to remove volatile matters generated when mixing the thermoplastic resin composition (II). As the screw of the extruder, a screw with a barrier flight or a mixing section can be used. From the viewpoint of obtaining sufficient plasticization and mixing state of the thermoplastic resin composition (II), the L / D of the screw (L represents the cylinder length of the extruder, and D represents the cylinder inner diameter) is preferably 10 or more, more preferably 20 or more, even more preferably 25 or more, and preferably 100 or less, more preferably 50 or less, and even more preferably 40 or less. By having the L / D be equal to or more than the lower limit, the thermoplastic resin composition (II) can be sufficiently plasticized and mixed. In addition, by having the L / D be equal to or less than the upper limit, mixing is possible while suppressing decomposition of the thermoplastic resin composition (II) due to shear heat generation.

[0078] The temperature of the extruder (set temperature of the cylinder) when the thermoplastic resin is in a molten state depends on the type, composition, glass transition temperature, etc. of the thermoplastic resin used, but is preferably 150°C or higher, more preferably 180°C or higher, and preferably 310°C or lower, more preferably 280°C or lower. By setting the cylinder temperature to the lower limit or higher, the thermoplastic resin composition (II) can be sufficiently melted. On the other hand, by setting the cylinder temperature to the upper limit or lower, low-boiling decomposition products, scorching, gelation, etc. generated by decomposition due to thermal degradation of the thermoplastic resin composition (II) can be suppressed.

[0079] <Gear pump> In the present invention, a gear pump may be installed after the extruder in order to compensate for pressure loss in a polymer filter or a static mixer, which will be described later. There are no particular limitations on the gear pump, but an inverter-controlled gear pump is preferred. By using an inverter-controlled gear pump, pulsation of the flow rate of the molten resin discharged from the extruder can be suppressed. The resin pressure at the inlet of the gear pump is preferably 10 MPa or less, and more preferably 8 MPa or less. When the resin pressure at the inlet of the gear pump is equal to or less than the upper limit, extrusion defects are less likely to occur even when the number of static mixer elements is increased. The lower limit of the resin pressure is preferably 1 MPa or more, and more preferably 3 MPa or more. When the resin pressure at the inlet of the gear pump is equal to or more than the lower limit, fluctuations in the resin discharge rate of the gear pump are reduced.

[0080] <Polymer filter> In the present invention, it is preferable to use a polymer filter between the gear pump and the static mixer. The polymer filter preferably comprises a filter element part for filtering the thermoplastic resin composition (II) and a housing part for introducing and discharging the molten resin. The filter element may be of a disk type or a cylindrical type, with the cylindrical type being preferred since it allows a large filtration area per element and is therefore cost-effective. A cylindrical filter element usually comprises a filtration section that filters a fluid from its outer peripheral surface, a hollow section through which the filtered fluid flows, a discharge section at an end section that discharges the fluid from the hollow section, and a tip section of the filter element. Examples of cylindrical filter elements include tube types and candle types, and among these, candle-type filter elements are preferred. There is no particular limitation on the shape of the candle-type filter element, and a wave type, pleated type, etc. can be used. The pleats in the pleated type may extend in the radial direction of the filter element, or may be so-called spiral pleats that extend obliquely to the radial direction and have a curved or arched cross-sectional shape.

[0081] The filtration accuracy of the filter element is preferably 5 μm or more, more preferably 8 μm or more, and preferably 50 μm or less, more preferably 30 μm or less. When the filtration accuracy is within the above range, it is possible to improve the balance between productivity and the suppression of contamination with foreign matter. In particular, when the filtration accuracy is equal to or more than the lower limit, it is possible to suppress thermal deterioration caused by shear heat generated when passing the thermoplastic resin composition (II) in a molten state. On the other hand, when the filtration accuracy is equal to or less than the upper limit, it is possible to effectively remove foreign matter.

[0082] <Static mixer> In the present invention, a static mixer is used for the purpose of efficiently stirring and mixing a highly viscous fluid (paste) by laminar flow while minimizing pressure loss. In the present invention, the number of unit mixing elements (number of elements) in the static mixer is preferably 9 to 30. If the number of elements is less than the lower limit, the uniformity of the temperature of the thermoplastic resin composition (II) and the uniformity of each blended component may decrease. If the number of elements exceeds the upper limit, the surface area of ​​the elements increases, and deteriorated resin may adhere to the element surface, leading to a decrease in film quality. From these viewpoints, the number of elements is more preferably 10 or more, even more preferably 11 or more, and more preferably 28 or less, even more preferably 25 or less, and even more preferably 20 or less. The arrangement of elements is preferably a static mixer in which right elements, which are rectangular plates twisted 180 degrees to the right inside the pipe, and left elements, which are rectangular plates twisted 180 degrees to the left inside the pipe, are alternately arranged. By arranging each element as described above, effective mixing can be achieved while minimizing shearing.

[0083] The length Le of each element of the static mixer of the present invention varies depending on the scale of operation, but is generally, from the viewpoint of suppressing thermal degradation due to retention of the thermoplastic resin composition (II), preferably 30 mm or more, more preferably 40 mm or more, and preferably 160 mm or less, and more preferably 100 mm or less. From the same viewpoint, the diameter De of each element of the static mixer is preferably 25 mm or more, more preferably 30 mm or more, and preferably 110 mm or less, and more preferably 80 mm or less. Furthermore, the ratio Le / De of the length Le to the diameter De per element of the static mixer of the present invention is preferably 1.2 or more, more preferably 1.3 or more, from the viewpoint of suppressing thermal deterioration due to retention of the thermoplastic resin composition (II), and is preferably 1.8 or less, more preferably 1.7 or less.

[0084] It is not necessary for all elements of a static mixer to be connected in a row; they may be divided into multiple pipes and connected together. However, since the mixing effect of the static mixer decreases if the number of divisions is increased, it is desirable to install at least five elements in a row.

[0085] The temperature of the thermoplastic resin composition (II) just before entering the static mixer and the temperature of the thermoplastic resin composition (II) just after passing through the static mixer vary depending on the glass transition temperature of the thermoplastic resin used, but is preferably 230° C. or higher, more preferably 250° C. or higher, and preferably 300° C. or lower, more preferably 280° C. or lower. By making the temperature of the thermoplastic resin composition (II) equal to or higher than the lower limit, the viscosity of the thermoplastic resin composition (II) can be reduced, and the pressure loss can be reduced. On the other hand, by making the temperature of the thermoplastic resin composition (II) equal to or lower than the upper limit, it is possible to suppress decomposition of the resin due to shear heat generation.

[0086] <Tダイ> The T-die used in the present invention is not particularly limited, and any known die can be used, such as a manifold die, a fishtail die, a coat hanger die, etc. In order to stabilize the thickness, it is preferable to use an automatically adjusting die equipped with a mechanism for automatically adjusting the lip opening bolt by measuring the thickness of the formed film.

[0087] The T-die temperature is preferably 100 to 200° C. higher than the glass transition temperature of the thermoplastic resin. By being in the above range, the effect of being able to mold the molten resin smoothly when it comes into contact with the roll can be obtained. From these viewpoints, the T-die temperature is more preferably 110 to 190° C. higher than the glass transition temperature of the thermoplastic resin, and further preferably 120 to 180° C. higher than the glass transition temperature of the thermoplastic resin.

[0088] <role> In the production method of the present invention, from the viewpoint of improving the surface smoothness and thickness accuracy of the thermoplastic resin film, it is preferable to take up and clamp the molten material extruded from the T-die using a mirror-finished roll or mirror-finished belt, preferably made of metal. Examples of the mirror-finished roll made of metal include an elastic metal roll and a rigid metal roll, and from the viewpoint of improving the surface smoothness of the thermoplastic resin film, it is preferable to use a combination of an elastic metal roll and a rigid metal roll. When a mirror-finished roll or mirror-finished belt is used, the pressing pressure is preferably 0.5 MPa or more, more preferably 1.0 MPa or more, from the viewpoint of improving the surface smoothness of the thermoplastic resin film. The upper limit of the pressing pressure is usually 5.0 MPa.

[0089] When a mirror-finished roll or belt is used, the surface temperature is preferably 50 to 130°C, more preferably 60 to 100°C, from the viewpoint of improving the surface smoothness, haze, appearance, etc. of the thermoplastic resin film.

[0090] <Thickness> According to the present invention, for example, a thermoplastic resin film having a thickness of 20 to 200 μm can be obtained while suppressing the occurrence of white streaks. Furthermore, from the viewpoint of improving the handleability of the thermoplastic resin film and keeping costs low, the thickness of the thermoplastic resin film is preferably 25 to 180 μm, more preferably 30 to 150 μm, and even more preferably 35 to 100 μm. When the thickness is equal to or more than the lower limit, the rigidity is increased, and the handleability of the thermoplastic resin film is improved. Furthermore, when the thickness is equal to or less than the upper limit, the balance between the strength of the thermoplastic resin film and the production cost is improved.

[0091] <Applications of thermoplastic resin films> The thermoplastic resin film produced by the production method of the present invention can be used in the following various applications. For example, it can be used in the fields of construction and building materials such as the interior and exterior of automobiles, the interior and exterior of personal computers, the interior and exterior of mobile phones, the interior and exterior of solar cells, solar cell back sheets, road signs, bathroom equipment, flooring materials, road light-transmitting panels, lenses for paired glass, skylight windows, carports, lighting covers, sizing for building materials, microwave cooking containers (dishes), housings for home appliances, toys, sunglasses, stationery, etc. It can also be used as an alternative application for molded products using transfer foil sheets. The film is also suitable for optical applications, and can be used in known applications such as the front panels of liquid crystal screens of terminals such as mobile phones, smartphones, and tablets; liquid crystal light guide plates, diffusion plates, backsheets, reflective sheets, polarizing films, transparent resin sheets, retardation films, light diffusion films, prism sheets, optically isotropic films, polarizer protective films, and transparent conductive films as films for liquid crystal displays; in the information equipment field, for example, surface protective films; and in the periphery of organic EL devices as films for organic EL devices. EXAMPLES

[0092] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The measurement methods and the like in the examples are as follows.

[0093] [Measurement and evaluation methods] <Weight average molecular weight (Mw)> The weight average molecular weight (Mw) of the (meth)acrylic resin (A) was determined in terms of standard polystyrene by gel permeation chromatography (GPC) using the following measuring device and conditions: · Apparatus: Tosoh Corporation GPC device "HLC-8320" Separation column: Tosoh Corporation's "TSKgel SuperMultipore HZM-M" and "SuperHZ4000" are directly connected. Detector: Tosoh Corporation "RI-8020" Eluent: Tetrahydrofuran ·Eluent flow rate: 0.35ml / min Sample concentration: 8mg / 10ml Column temperature: 40℃

[0094] <Glass transition temperature (Tg)> The glass transition temperatures of the (meth)acrylic resin (A) and the thermoplastic resin composition (II) were measured in accordance with JIS K7121: 2012. That is, a sample was heated once to 200°C, then cooled to 30°C or lower, and then heated from 30°C to 200°C at a rate of 10°C / min, under which a DSC curve was measured by differential scanning calorimetry, and the midpoint glass transition temperature determined from the DSC curve measured during the second heating was taken as the glass transition temperature in the present invention.

[0095] <Average particle size> The average particle size of the (meth)acrylic polymer particles (B) having a multilayer structure was measured by diluting the latex containing the sample particles 200 times with water, and analyzing the diluted solution at 25° C. using a laser diffraction scattering type particle size distribution measuring device (manufactured by Horiba, Ltd., device name "LA-950V2") At this time, the absolute refractive indexes of the sample particles and water were set to 1.4900 and 1.3333, respectively.

[0096] <Viscosity of compound (I) after heating (heating and viscosity of silicone oil)> (1) Heating silicone oil 30 g of each of the silicone oils used in the Examples and Comparative Examples was added to a metal tray (width 140 mm, length 187 mm) and heated for 24 hours at the T-die temperature (set temperature) in an air atmosphere in a constant temperature incubator (manufactured by Yamato Scientific Co., Ltd., device name "DN410H"). Next, the viscosity (P I-1 ) was measured. Furthermore, silicone oil was prepared in the same manner as above and heated at a temperature 30°C lower than the T-die temperature (set temperature) for 48 hours. Then, the viscosity (P I-2 The results are shown in Table 1.

[0097] (2) Viscosity measurement method The viscosity was measured using a rotational rheometer (manufactured by TA Instruments, device name "ARES") at a shear rate of 100 [1 / s] with the temperature set according to each condition.

[0098] <Viscosity of Compound (I) at 25°C> The viscosity of compound (I) was measured at 25° C. in accordance with the method for measuring the viscosity of compound (I) after heating (viscosity of silicone oil).

[0099] <Viscosity of Thermoplastic Resin Composition (II) at T-Die Temperature> The viscosity (P II ) was measured using a Capillograph (Model 1D, manufactured by Toyo Seiki Seisakusho Co., Ltd., capillary diameter 1 mm, length 40 mm) under conditions of 270°C (T-die setting temperature) and a shear rate of 122 [1 / sec].

[0100] <Amount of white streaks> A 300 m long film produced by the method described below was pulled out from the end of the roll, and this was used as an evaluation sample. In a dark room, a black flannel cloth was hung on one side of the evaluation sample, and the other side was irradiated with indirect reflected light from a Polarion Light (Polarion, PS-NP1: HID light source, 35 W). Streaks in the flow direction of the film that appeared white due to the indirect reflected light were observed as white streaks and evaluated according to the following criteria. Evaluation was performed on two types of evaluation samples: a film produced 4 hours after the start of film production, and a film produced 24 hours after the start of film production. [Evaluation Criteria] 1 (Good): 2 or less white lines 2 (normal): 3 to 5 white lines 3 (bad): 6 or more white lines

[0101] <Production Example 1: Production of (meth)acrylic resin (A)> 99.3 parts by mass of methyl methacrylate and 0.7 parts by mass of methyl acrylate were added with 0.008 parts by mass of a polymerization initiator [2,2'-azobis(2-methylpropionitrile), hydrogen abstraction ability: 1%, 1-hour half-life temperature: 83°C] and 0.26 parts by mass of a chain transfer agent (n-octyl mercaptan) and dissolved to obtain 3,000 kg of a raw material liquid. 100 parts by mass of ion-exchanged water, 0.03 parts by mass of sodium sulfate, and 0.45 parts by mass of potassium polymethacrylate were mixed to obtain 6,000 kg of a mixed liquid. The mixed liquid and the raw material liquid (total of 9,000 kg) were charged into a pressure-resistant polymerization tank, and the temperature was raised to 70°C while stirring under a nitrogen atmosphere to start the polymerization reaction. After 3 hours had elapsed since the start of the polymerization reaction, the temperature was raised to 90°C, and stirring was continued for 1 hour to obtain a liquid in which a bead-like copolymer was dispersed. Although some polymer adhered to the walls of the polymerization tank or the stirring blades, there was no foaming, and the polymerization reaction proceeded smoothly. The obtained copolymer dispersion was washed with an appropriate amount of ion-exchanged water, and the bead-like copolymer was taken out using a bucket centrifuge and dried for 12 hours in a hot air dryer at 80°C to obtain bead-like (meth)acrylic resin (A). The resulting (meth)acrylic resin (A) had a methyl methacrylate unit content of 99.3 mass %, a methyl acrylate unit content of 0.7 mass %, a weight average molecular weight (Mw) of 92,000 and a glass transition temperature of 120°C.

[0102] <Production Example 2: Production of (meth)acrylic polymer particles (B) having a multilayer structure> According to the following procedure, an acrylic polymer having a core-shell multilayer structure consisting of three layers, a core (inner layer), an inner shell (middle layer), and an outer shell (outer layer), was produced. (1) Synthesis of the inner layer In a reactor equipped with a stirrer, a thermometer, a nitrogen gas inlet tube, a monomer inlet tube and a reflux condenser, 1,050 parts by mass of ion-exchanged water, 0.3 parts by mass of sodium polyoxyethylene tridecyl ether acetate and 0.7 parts by mass of sodium carbonate (total 2,100 kg) were charged, and the inside of the reactor was fully replaced with nitrogen gas. Then, the inside temperature was set to 80°C, 0.25 parts by mass of potassium persulfate was added, and the mixture was stirred for 5 minutes. 245 parts by mass of a monomer mixture consisting of 95.4% by mass of methyl methacrylate, 4.4% by mass of methyl acrylate and 0.2% by mass of allyl methacrylate was continuously added dropwise over 60 minutes. After the dropwise addition, the polymerization reaction was continued for another 30 minutes so that the polymerization conversion rate was 98% or more.

[0103] (2) Synthesis of the middle layer Next, 0.32 parts by mass of potassium persulfate was added to the reactor and stirred for 5 minutes. After that, 315 parts by mass of a monomer mixture consisting of 80.5% by mass of n-butyl acrylate, 17.5% by mass of styrene, and 2% by mass of allyl methacrylate was continuously dripped over 60 minutes. After the dripping was completed, the polymerization reaction was continued for another 30 minutes so that the polymerization conversion rate was 98% or more.

[0104] (3) Synthesis of the outer layer Next, 0.14 parts by mass of potassium persulfate was added to the reactor and stirred for 5 minutes. After that, 140 parts by mass of a monomer mixture consisting of 95.2% by mass of methyl methacrylate, 4.4% by mass of methyl acrylate, and 0.4% by mass of n-octyl mercaptan was continuously dripped over 30 minutes. After the dripping was completed, the polymerization reaction was continued for another 60 minutes so that the polymerization conversion rate was 98% or more.

[0105] After obtaining a latex containing the (meth)acrylic polymer particles (B) having a multi-layer structure by the above-mentioned operations, the latex containing the (meth)acrylic polymer particles (B) having a multi-layer structure was frozen and solidified. Then, it was washed with water and dried to obtain the (meth)acrylic polymer particles (B) having a multi-layer structure. The average particle size of the particles was 0.23 μm.

[0106] <Example 1> A thermoplastic resin film was produced using the apparatus shown in FIG. Specifically, 80 parts by mass of the (meth)acrylic resin (A) produced in Production Example 1, 20 parts by mass of the (meth)acrylic polymer particles (B) having a multilayer structure produced in Production Example 2, and 2 parts by mass of Adeka STAB LA-31 (manufactured by Adeka Corporation) as an ultraviolet absorber were mixed in a Henschel mixer. Next, mixing was performed using a vented twin-screw extruder with a set temperature (cylinder set temperature) of 260°C and a screw diameter of 58 mm to obtain a thermoplastic resin composition (II). The glass transition temperature of the thermoplastic resin composition (II) was 120°C. The thermoplastic resin composition (II) was melted using a vented single screw extruder with a screw diameter of 90 mm (L / D=34) set at 265°C (temperature was the cylinder's set temperature), extruded in the form of a film from a T-die (temperature 270°C: set temperature) with a lip width of 1850 mm and a lip opening of 0.6 mm at a discharge speed of 180 kg / h, and pressed between two rolls (temperature: 90°C, pressure 1.6 MPa) to obtain a thermoplastic resin film ((meth)acrylic resin film) with a thickness of 75 μm, width of 1500 mm, and rolled up to 300 m at a line speed of 20 m / min. A spur-toothed external gear pump (manufactured by Toshiba Machine Co., Ltd.) was used as the gear pump, and the inlet pressure was 5 MPa. The polymer filter consisted of four candle filters with a filtering accuracy of 10 μm, which were arranged in parallel. The static mixer had 16 elements and an Le / De ratio of 1.5 (Le = 57 mm, De = 38 mm). 2 ml of silicone oil (methylphenyl silicone, manufactured by Shin-Etsu Chemical Co., Ltd., product name: KF-54) represented by the following formula (1) as compound (I) was impregnated into a waste cloth and applied to the die lip. The temperature of the thermoplastic resin composition (II) immediately before entering the static mixer and the temperature of the thermoplastic resin composition (II) immediately after passing through the static mixer were both adjusted to 270°C, and the temperature up to the T-die thereafter was also set to 270°C to produce a film. The produced film was evaluated for white streaks by the above-mentioned method. The thickness of the obtained thermoplastic resin film was 75 μm.

[0107] [ka] In formula (1), x and y represent integers (the same applies hereinafter).

[0108] <Comparative Example 1> A film was produced in the same manner as in Example 1, except that a silicone oil represented by the following formula (2) (dimethyl silicone, manufactured by Shin-Etsu Chemical Co., Ltd., product name: KF96-100CS) was used instead of the silicone oil used in Example 1. The evaluation results are shown in Table 1.

[0109] [ka]

[0110] <Comparative Example 2> A film was produced in the same manner as in Example 1, except that a silicone oil represented by the following formula (3) (aralkyl-modified silicone, manufactured by Shin-Etsu Chemical Co., Ltd., product name: KF410) was used instead of the silicone oil used in Example 1. The evaluation results are shown in Table 1. The compound solidified after heating for 48 hours at a temperature 30°C lower than the T-die temperature (P II <P I-2 ) Therefore, it is expected that die lines will occur if used in film production.

[0111] [ka]

[0112] <Comparative Example 3> A film was produced in the same manner as in Example 1, except that a silicone oil represented by the following formula (4) (silicone modified at both ends with phenol, manufactured by Shin-Etsu Chemical Co., Ltd., product name: KF2201) was used instead of the silicone oil used in Example 1. The evaluation results are shown in Table 1. This compound solidified after heating for 48 hours at a temperature 30°C lower than the T-die temperature (PII <P I-2 ) Therefore, it is expected that die lines will occur if used in film production. In the formula (4), R represents an alkylene chain.

[0113] [ka]

[0114] [Table 1]

[0115] The details of the descriptions in Table 1 are as follows: P I-1 : Viscosity of the compound (I) after heating at die temperature for 24 hours P I-2 : Viscosity of the compound (I) after heating for 48 hours at a temperature 30°C lower than the die temperature P II : Viscosity of the thermoplastic resin composition (II) at die temperature

[0116] According to the method for producing a thermoplastic resin film of the present invention, the occurrence of white streaks in the machine direction of the film can be suppressed. [Explanation of symbols]

[0117] 1. Extruder 2 Gear pump 3. Polymer Filter 4. Static Mixer 5 T-die 6 Rolls(1) 7 Rolls(2)

Claims

[Claim 1] The method for producing a film includes a step of extruding a molten thermoplastic resin composition (II) from a T-die lip coated with a compound (I) having a phenyl group and a viscosity of 0.005 to 2.0 [Pa s] at 25°C, A method for producing a thermoplastic resin film, characterized in that the viscosity of the compound (I) and the viscosity of the thermoplastic resin composition (II) satisfy the following relational expressions (1) and (2): P II >P I-1 (1) P II >P I-2 (2) P I-1 : Viscosity of the compound (I) after heating at T die temperature for 24 hours P I-2 : Viscosity of the compound (I) after heating for 48 hours at a temperature 30° C. lower than the T-die temperature P II : Viscosity of the thermoplastic resin composition (II) at T die temperature the compound (I) is a silicone oil, the phenyl group is directly bonded to a silicon atom other than a terminal of the silicone oil, The P II and the P I-1 satisfy a relationship of P II / P I-1 > 100, The thermoplastic resin composition (II) contains a (meth)acrylic resin (A), the thermoplastic resin composition (II) contains (meth)acrylic polymer particles (B) having a multilayer structure, The thermoplastic resin composition (II) has a viscosity of 200 to 2,000 Pa s at 270°C and a shear rate of 122 / sec. A method for producing a thermoplastic resin film.

Citation Information

Patent Citations

  • Molding mouthpiece

    JP1988049416A

  • Polyolefin resin composition

    JP2000319458A

  • Thermoplastic resin film and method for manufacturing the same

    JP2002307523A

  • Method of manufacturing extrusion molding of thermoplastic resin and film molded by the manufacturing method