RELEASE FILM AND METHOD FOR MANUFACTURING RELEASE FILM

A release film with a controlled residual strain orientation index minimizes wrinkles during heating, enhancing the manufacturing process of flexible circuit boards by preventing defects.

JP7583660B2Active Publication Date: 2024-11-14SEKISUI CHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021057586
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-30
Publication Date
2024-11-14
Estimated Expiration
2041-03-30

AI Technical Summary

Technical Problem

Release films used in the manufacturing of flexible circuit boards wrinkle during hot press adhesion, leading to defects on the circuit board.

Method used

A release film with a standard deviation of residual strain orientation index of 10,000 or less, obtained through polarized light microscopy analysis, is developed to minimize uneven shrinkage and wrinkle formation during heating.

Benefits of technology

The release film effectively reduces wrinkle formation during heating, ensuring high-quality manufacturing of flexible circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583660000002
    Figure 0007583660000002
  • Figure 0007583660000003
    Figure 0007583660000003
  • Figure 0007583660000004
    Figure 0007583660000004
Patent Text Reader

Abstract

To provide a release film less likely to cause wrinkles during heating, and a method for manufacturing the release film.SOLUTION: A release film includes at least one release layer. A standard deviation of a residual strain orientation index obtained by analyzing a polarizing microscopic observation image of the release film is 10,000 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a release film. The present invention also relates to a method for producing the release film. [Background technology]

[0002] 2. Description of the Related Art Release films are used in the manufacturing processes of printed wiring boards, flexible circuit boards, multilayer printed wiring boards, and the like. In the manufacturing process of a flexible circuit board, a coverlay film is heat-pressed to a flexible circuit board body on which a copper circuit is formed via a thermosetting adhesive or a thermosetting adhesive sheet. At this time, by disposing a release film between the coverlay film and the heat-press plate, it is possible to prevent the coverlay film and the heat-press plate from adhering to each other, and also to prevent problems such as the adhesive seeping out and interfering with the plating process of the electrode portion (for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 5-283862 [Patent Document 2] JP 2009-132806 A Summary of the Invention [Problem to be solved by the invention]

[0004] Such release films have the problem that they wrinkle when used in a hot press. If wrinkles occur in the release film during hot press bonding, the wrinkles may be transferred to the flexible circuit board, which may lead to defects.

[0005] An object of the present invention is to provide a release film that is less likely to wrinkle when heated, and a method for producing the release film. [Means for solving the problem]

[0006] The present invention is a release film having at least one release layer, in which the standard deviation of the residual strain orientation index obtained by analyzing an image of the release film observed under a polarizing microscope is 10,000 or less. The present invention will be described in detail below.

[0007] The present inventors have studied the cause of wrinkles occurring during heating, and have found that residual stress (strain) applied to the release film during the manufacturing process causes uneven shrinkage due to the residual strain during heating, resulting in wrinkles. The present inventors have studied ways to suppress the concentration or orientation of such residual strain (disperse the residual strain), and have considered using the standard deviation of the residual strain orientation index obtained by analyzing a polarized microscope image of the release film as an index showing the degree of concentration or orientation of the residual strain. The present inventors have found that the occurrence of wrinkles during heating can be suppressed by adjusting the standard deviation of the residual strain orientation index obtained by analyzing a polarized microscope image of the release film to a certain value or less, and have completed the present invention.

[0008] The release film of the present invention is a release film having at least one release layer, and the upper limit of the standard deviation of the residual strain orientation index obtained by analyzing an image of the release film observed under a polarizing microscope is 10,000. The standard deviation of the residual strain orientation index is an index showing the degree of concentration or orientation of the residual strain (stress applied in the manufacturing process) of the release film. If the standard deviation of the residual strain orientation index is 10,000 or less, the degree of concentration or orientation of the residual strain of the release film is small, and uneven shrinkage caused by the residual strain during heating can be suppressed, so that the release film is less likely to wrinkle when heated. The preferred upper limit of the standard deviation of the residual strain orientation index is 5,000, and the more preferred upper limit is 4,000. The lower limit of the standard deviation of the residual strain orientation index is not particularly limited, and the closer to 0, the smaller the degree of concentration or orientation of the residual strain of the release film, so this is preferable.

[0009] The polarizing microscope observation image of the release film can be taken under the following conditions using a polarizing microscope (e.g., Olympus Corporation's "BX53M" and "OLYMPUS Stream Basic ver2.4"). The image is taken while avoiding areas with scratches, etc., and the image file is saved in TIFF format without compression. Differential interference slider: Yes Magnification: 4x Exposure conditions: Auto mode Sensitivity: ISO200 Exposure compensation: 0 Resolution: 1920 x 1440 (Field of view: 3.55716 mm x 2.64942 mm) Aspect Ratio: Standard White balance mode: Auto (high)

[0010] The obtained polarizing microscope image can be analyzed, for example, using software (for example, software "ImageJ ver1.52p" manufactured by NIH, plug-in "OrientationJ ver2.0.4", etc.) as described below. First, the obtained polarizing microscope observation image is converted to an 8-bit image using "ImageJ ver1.52p". Next, the five images are analyzed (brightness analysis) using "Orientation Distribution" in "OrientationJ ver2.0.4" under the conditions of Local Window σ: 4 pixels, Gradient: Cubic Spline. In the histogram obtained by the analysis, the horizontal axis is "Orientation in Degrees" and the vertical axis is "Distribution of orientation", and the value on the vertical axis is the "residual strain orientation index". The obtained data on the "residual strain orientation index" is imported into the software "Microsoft Office Standard 2016 Excel" and its standard deviation is calculated. In addition, five images taken at any five points on the release film are used to calculate the standard deviation. In other words, the standard deviation of the "residual strain orientation index" is calculated for each of the five images, and the average value is adopted.

[0011] In the release film of the present invention, the maximum value of the residual strain orientation index obtained by analyzing an image of the release film observed under a polarizing microscope is not particularly limited, but the preferred upper limit is 40,000. If the maximum value of the residual strain orientation index is 40,000 or less, the degree of concentration or orientation of the residual strain in the release film becomes smaller, and the release film becomes less likely to wrinkle when heated. A more preferable upper limit of the maximum value of the residual strain orientation index is 30,000.

[0012] In the release film of the present invention, the difference between the maximum and minimum values ​​of the residual strain orientation index obtained by analyzing an image of the release film observed under a polarizing microscope is not particularly limited, but a preferred upper limit is 30,000. If the difference between the maximum and minimum values ​​of the residual strain orientation index is 30,000 or less, the degree of concentration or orientation of the residual strain in the release film becomes smaller, and the release film becomes less susceptible to wrinkles when heated. A more preferable upper limit of the difference between the maximum and minimum values ​​of the residual strain orientation index is 15,000. The lower limit of the difference between the maximum and minimum values ​​of the residual strain orientation index is not particularly limited, but the smaller the difference, the smaller the degree of concentration or orientation of the residual strain in the release film, and therefore it is preferable.

[0013] The method for adjusting the standard deviation, maximum value, and difference between the maximum value and minimum value of the residual strain orientation index to the above range is not particularly limited, and examples include a method of selecting a resin that constitutes the release film and then adjusting the conditions for producing the release film. Specifically, for example, in a method for producing a release film having a step (1) of preparing an original film having at least one release layer and a step (2) of embossing the surface of the release layer in the obtained original film (after cooling), a method of embossing the surface of the release layer at a high temperature when forming the original film in the above step (1) can be mentioned. In addition, in the embossing treatment in the above step (2), a method of increasing heat transmission from the metal roll by lowering the linear speed, a method of increasing the metal roll temperature (heating temperature), a method of increasing the Rz of the metal roll, etc. can also be mentioned. According to these methods, the concentration or orientation of the residual strain of the release film can be suppressed (residual strain can be dispersed). Among them, the method of lowering the linear speed, increasing the metal roll temperature (heating temperature), or increasing the Rz of the metal roll in the embossing treatment in the above step (2) is preferable because it can further suppress the concentration or orientation of the residual strain.

[0014] The resin constituting the release layer is not particularly limited, but polyester, polyolefin or polystyrene is preferred because it improves the releasability of the release film. The polyester preferably contains an aromatic polyester resin. The polyolefin preferably contains poly(4-methyl-1-pentene) or an alicyclic olefin resin. The polystyrene preferably contains a polystyrene resin having a syndiotactic structure. In particular, the release layer more preferably contains an aromatic polyester resin, since it has excellent conformability to irregularities and excellent anti-bleeding properties of the adhesive formed on the coverlay film.

[0015] The aromatic polyester resin is not particularly limited, but crystalline aromatic polyester resin is preferred.Specific examples include polyethylene terephthalate resin, polybutylene terephthalate resin, polyhexamethylene terephthalate resin, polyethylene naphthalate resin, polybutylene naphthalate resin, terephthalic acid butanediol polytetramethylene glycol copolymer, etc.These aromatic polyester resins may be used alone or in combination of two or more.Among them, polybutylene terephthalate resin is preferred from the viewpoint of balance of heat resistance, releasability, conformability to unevenness, wrinkle suppression during heating, etc. Also preferred is a mixed resin of a polybutylene terephthalate resin and a block copolymer of polybutylene terephthalate and an aliphatic polyether. The aliphatic polyether is not particularly limited, and examples thereof include polyethylene glycol, polydiethylene glycol, polypropylene glycol, and polytetramethylene glycol.

[0016] From the viewpoint of film forming properties, the aromatic polyester resin has a melt volume flow rate of 30 cm 3 / 10min or less is preferable, and 20cm 3 It is more preferable that the melt volume flow rate is equal to or less than 1000000 / min. The melt volume flow rate can be measured in accordance with ISO1133 at a measurement temperature of 250° C. and a load of 2.16 kg.

[0017] Among the above aromatic polyester resins, commercially available examples include "Pelprene (registered trademark)" (manufactured by Toyobo Co., Ltd.), "Hytrel (registered trademark)" (manufactured by DuPont-Toray Co., Ltd.), "Duranex (registered trademark)" (manufactured by Polyplastics Co., Ltd.), and "Novaduran (registered trademark)" (manufactured by Mitsubishi Engineering Plastics Corporation).

[0018] The poly(4-methyl-1-pentene)-containing polyolefin preferably contains 90% by weight or more of poly(4-methyl-1-pentene) resin. As the poly(4-methyl-1-pentene) resin, for example, a commercially available product such as TPX (registered trademark) manufactured by Mitsui Chemicals, Inc. can be used.

[0019] The alicyclic olefin resin is an olefin resin having a cyclic aliphatic hydrocarbon in the main chain or side chain, and from the standpoint of heat resistance, strength, etc., thermoplastic saturated norbornene resin is preferred. Examples of the thermoplastic saturated norbornene resin include resins obtained by hydrogenating ring-opening polymers or ring-opening copolymers of norbornene monomers (after modification such as maleic acid addition or cyclopentadiene addition, if necessary). Other examples include resins obtained by addition polymerization of norbornene monomers, resins obtained by addition polymerization of norbornene monomers and olefin monomers such as ethylene or α-olefin, and resins obtained by addition polymerization of norbornene monomers and cyclic olefin monomers such as cyclopentene, cyclooctene, and 5,6-dihydrodicyclopentadiene. Furthermore, modified products of these resins are also included.

[0020] The polystyrene containing the polystyrene-based resin having a syndiotactic structure preferably contains 70% by weight or more and 90% by weight or less of the polystyrene-based resin having a syndiotactic structure. A polystyrene resin having a syndiotactic structure is a resin having a stereoregular structure in which phenyl groups and substituted phenyl groups, which are side chains, are alternately positioned in opposite directions relative to the main chain formed from carbon-carbon sigma bonds.

[0021] The polystyrene resin having the syndiotactic structure is not particularly limited. For example, polystyrene having a syndiotacticity of 75% or more in racemic diad or 30% or more in racemic pentad, poly(alkylstyrene), poly(arylstyrene), poly(halogenated styrene), poly(halogenated alkylstyrene), poly(alkoxystyrene), poly(vinyl benzoate ester), etc. can be mentioned. In addition, hydrogenated polymers of these, mixtures of these, copolymers containing these as main components, etc. can be mentioned. The polystyrene resin having the syndiotactic structure can be commercially available, such as XAREC (registered trademark) manufactured by Idemitsu Kosan Co., Ltd.

[0022] The release layer may contain a mixed resin containing polybutylene terephthalate resin and an elastomer. The elastomer is not particularly limited, and may be, for example, a block copolymer of polybutylene terephthalate and an aliphatic polyether. The aliphatic polyether is not particularly limited, and may be, for example, polyethylene glycol, polydiethylene glycol, polypropylene glycol, polytetramethylene glycol, etc.

[0023] The proportion of the polybutylene terephthalate resin in the resin constituting the release layer is not particularly limited, but is preferably 75% by weight or more. If the proportion of the polybutylene terephthalate resin is 75% by weight or more, the release property of the release film is improved. A more preferable lower limit of the proportion of the polybutylene terephthalate resin in the resin constituting the release layer is 80% by weight.

[0024] The release layer may contain a rubber component. When the release layer contains a rubber component, the ability to conform to the irregularities of the release film is improved. The rubber component is not particularly limited, and examples thereof include natural rubber, styrene-butadiene copolymer, polybutadiene, polyisoprene, acrylonitrile-butadiene copolymer, ethylene-propylene copolymer (EPM, EPDM), polychloroprene, butyl rubber, acrylic rubber, silicone rubber, urethane rubber, etc. Examples of the rubber component include olefin-based thermoplastic elastomer, styrene-based thermoplastic elastomer, vinyl chloride-based thermoplastic elastomer, ester-based thermoplastic elastomer, amide-based thermoplastic elastomer, etc.

[0025] The release layer may contain a stabilizer. The stabilizer is not particularly limited, and examples thereof include hindered phenol-based antioxidants and heat stabilizers. The hindered phenol-based antioxidant is not particularly limited, and examples thereof include 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 3,9-bis{2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)-propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, and the like. The heat stabilizer is not particularly limited, and examples thereof include tris(2,4-di-t-butylphenyl)phosphite, trilauryl phosphite, 2-t-butyl-α-(3-t-butyl-4-hydroxyphenyl)-p-cumenylbis(p-nonylphenyl)phosphite, dimyristyl 3,3'-thiodipropionate, distearyl 3,3'-thiodipropionate, pentaerythryl tetrakis(3-laurylthiopropionate), ditridecyl 3,3'-thiodipropionate, and the like.

[0026] The release layer may further contain conventionally known additives such as fibers, inorganic fillers, flame retardants, ultraviolet absorbing agents, antistatic agents, inorganic substances, and salts of higher fatty acids.

[0027] The thickness of the release layer is not particularly limited, but the preferred lower limit is 10 μm, and the preferred upper limit is 40 μm. If the thickness of the release layer is 10 μm or more, the heat resistance of the release film is improved. If the thickness of the release layer is 40 μm or less, the conformability of the release film to the unevenness is improved. The more preferred lower limit of the thickness of the release layer is 15 μm, and the more preferred upper limit is 30 μm.

[0028] The release film of the present invention may have a single-layer structure constituted only of the release layer, or may have a multi-layer structure containing layers other than the release layer.

[0029] The release film of the present invention preferably further comprises a cushion layer, which improves the ability of the release film to conform to unevenness. When the release film of the present invention has the cushion layer, it is sufficient that the release film has at least one release layer and a cushion layer, and may have a two-layer structure or a three-layer structure or more. In particular, it is preferable that the release film has a structure in which a release layer is provided on both sides of the cushion layer. In this case, the release layers on both sides may have the same resin composition or different resin compositions, and the release layers on both sides may have the same thickness or different thicknesses. Furthermore, the release film of the present invention may have a structure in which the release layer and the cushion layer are in direct contact with each other and integrated together, or may have a structure in which the release layer and the cushion layer are integrated together via an adhesive layer.

[0030] The resin constituting the cushion layer is not particularly limited, but it is preferable that the cushion layer contains the resin constituting the release layer. The cushion layer contains the resin constituting the release layer, so that the adhesion between the release layer and the cushion layer is improved. The cushion layer more preferably contains the main component resin of the release layer, and further preferably contains the main component resin of the release layer and a polyolefin resin. Here, the main component resin of the release layer means the resin with the highest content among the resins contained in the release layer.

[0031] The content of the resin constituting the release layer in the cushion layer is not particularly limited, but the preferred lower limit is 10% by weight, and the preferred upper limit is 50% by weight. If the content of the resin constituting the release layer is 10% by weight or more, the adhesion between the release layer and the cushion layer is improved. If the content of the resin constituting the release layer is 50% by weight or less, the flexibility of the cushion layer is sufficient, and the ability to follow the unevenness of the release film is improved. The more preferred lower limit of the content of the resin constituting the release layer is 20% by weight, and the even more preferred lower limit is 25% by weight. The more preferred upper limit of the content of the resin constituting the release layer is 40% by weight, and the even more preferred upper limit is 35% by weight.

[0032] The polyolefin resin is not particularly limited, and examples thereof include polyethylene resins (e.g., high-density polyethylene, low-density polyethylene, linear low-density polyethylene), polypropylene resins, ethylene-vinyl acetate copolymers, etc. Also included are ethylene-acrylic monomer copolymers such as ethylene-methyl methacrylate copolymers, ethylene-ethyl acrylate copolymers, and ethylene-acrylic acid copolymers. These polyolefin resins may be used alone or in combination of two or more. Among them, polypropylene resins are preferred because they easily achieve both conformability to irregularities and heat resistance.

[0033] The content of the polyolefin resin in the cushion layer is not particularly limited, but the preferred lower limit is 50% by weight, and the preferred upper limit is 90% by weight. If the content of the polyolefin resin is 50% by weight or more, the flexibility of the cushion layer is sufficient, and the ability to follow the unevenness of the release film is improved. If the content of the polyolefin resin is 90% by weight or less, the adhesion between the release layer and the cushion layer is improved. The more preferred lower limit of the content of the polyolefin resin is 60% by weight, and even more preferred lower limit is 65% by weight. The more preferred upper limit of the content of the polyolefin resin is 80% by weight, and even more preferred upper limit is 75% by weight.

[0034] The cushion layer may further contain a resin such as polystyrene, polyvinyl chloride, polyamide, polycarbonate, polysulfone, or polyester. The cushion layer may further contain additives such as fibers, inorganic fillers, flame retardants, ultraviolet absorbing agents, antistatic agents, inorganic substances, and salts of higher fatty acids.

[0035] The cushion layer may have a single-layer structure made of a single layer, or a multi-layer structure made of a laminate of multiple layers. When the cushion layer has a multi-layer structure, the multiple layers may be laminated together via an adhesive layer.

[0036] The thickness of the cushion layer is not particularly limited, but the preferred lower limit is 15 μm, and the preferred upper limit is 200 μm. If the thickness of the cushion layer is 15 μm or more, the ability to follow the unevenness of the release film is improved. If the thickness of the cushion layer is 200 μm or less, the exudation of resin from the cushion layer that occurs at the film end during heat press bonding can be suppressed. The more preferred lower limit of the thickness of the cushion layer is 30 μm, and the more preferred upper limit is 150 μm.

[0037] The method for producing the release film of the present invention is not particularly limited.From the viewpoint of adjusting the standard deviation, maximum value, and difference between maximum value and minimum value of the residual strain orientation index within the above range, the method for producing the release film of the present invention preferably includes a step (1) of producing an original film having at least one release layer, and a step (2) of embossing the surface of the release layer in the obtained original film (after cooling).Such a method for producing a release film is also one of the present inventions. In addition, depending on the conditions when embossing the surface of the release layer at high temperature when forming the original film in the above step (1), the standard deviation of the residual strain orientation index can be adjusted to the above range even without performing the above step (2), and the release film becomes less likely to wrinkle when heated.

[0038] In the above step (1), the method for producing the raw film is not particularly limited, and examples thereof include a water-cooled or air-cooled coextrusion inflation method, a coextrusion T-die method for forming a film, a solvent casting method, and a hot press molding method. In the case of a structure having the release layers on both sides of the cushion layer, a method of preparing a film to be one of the release layers, laminating a film to be the cushion layer on this film by extrusion lamination, and then dry laminating a film to be the other release layer can be used. Also, a method of dry laminating a film to be one of the release layers, a film to be the cushion layer, and a film to be the other release layer can be used. Among these, the co-extrusion T-die method is preferred because it allows excellent control of the thickness of each layer.

[0039] In the above step (1), from the viewpoint of adjusting the standard deviation, maximum value, and difference between the maximum value and minimum value of the residual strain orientation index within the above ranges, it is preferable to perform an embossing treatment on the surface of the release layer at a high temperature when forming the raw film as described above. At this time, the Rz of the metal roll used is not particularly limited, but from the viewpoint of adjusting the standard deviation, maximum value, and difference between the maximum value and the minimum value of the residual strain orientation index to the above range, the preferred lower limit is 10 μm, and the preferred upper limit is 50 μm. The more preferred lower limit of the Rz of the metal roll is 20 μm, and the more preferred upper limit is 40 μm. Under such conditions, the standard deviation of the residual strain orientation index can be adjusted to the above range without performing the above step (2), and the release film is less likely to wrinkle when heated. In addition, in the above step (1), it is preferable that the raw material resin is sufficiently melted. At this time, the resin temperature is not particularly limited, but is preferably not less than the melting point of the resin and not more than the decomposition temperature of the resin, and more specifically, for example, it is preferable that the temperature is 10 to 20° C. higher than the melting point of the resin. When the above step (2) is carried out, the Rz of the metal roll and the resin temperature in the above step (1) are not particularly limited, and do not have to satisfy the above ranges.

[0040] The method of the embossing treatment in the above step (2) is not particularly limited, and examples thereof include conventionally known methods such as an embossing roll method. Such embossing treatment can suppress the concentration or orientation of residual strain in the release film (disperse residual strain), improve the visibility and handleability (distinguishing between front and back and slipperiness) of the release film, and suppress blocking between the release films. The embossing treatment may be performed on both sides of the release film. By embossing both sides of the release film, the concentration or orientation of residual strain in the release film can be further suppressed, and the visibility, handleability, and blocking resistance of the release film can be further improved.

[0041] In the embossing process of step (2) above, from the viewpoint of adjusting the standard deviation, maximum value, and difference between the maximum value and minimum value of the residual strain orientation index within the above ranges, it is preferable to reduce the line speed, increase the metal roll temperature (heating temperature), or increase the Rz of the metal roll, as described above. In the embossing process of the above step (2), the line speed is not particularly limited, but from the viewpoint of adjusting the standard deviation, maximum value, and difference between the maximum value and the minimum value of the residual strain orientation index to the above range, the preferred lower limit is 3 m / min, the preferred upper limit is 30 m / min, the more preferred lower limit is 5 m / min, and the more preferred upper limit is 20 m / min. The metal roll temperature (heating temperature) is not particularly limited, but from the viewpoint of adjusting the standard deviation, maximum value, and difference between the maximum value and the minimum value of the residual strain orientation index to the above range, the preferred lower limit is 50 ° C, the preferred upper limit is 160 ° C, the more preferred lower limit is 100 ° C, and the more preferred upper limit is 140 ° C. The Rz of the metal roll used is not particularly limited, but from the viewpoint of adjusting the standard deviation, maximum value, and difference between the maximum value and the minimum value of the residual strain orientation index to the above range, the preferred lower limit is 30 μm, the preferred upper limit is 50 μm, the more preferred lower limit is 35 μm, and the more preferred upper limit is 40 μm.

[0042] The Rz of the metal roll in step (1) or (2) means the surface roughness Rz defined in JIS B0601:2001, and can be measured, for example, using a Surftest SJ-301 manufactured by Mitutoyo Corporation.

[0043] In the method for producing a release film of the present invention, a step (3) of rubbing the surface of the release layer in the obtained raw film may be performed. Such rubbing treatment can improve the releasability without impairing the ability of the release film to conform to unevenness, the suppression of wrinkles during heating, etc. The above step (3) may be carried out after the above step (2). However, from the viewpoint of improving releasability without impairing the ability of the release film to conform to the irregularities and the suppression of wrinkles during heating, it is preferable that the step (3) is carried out between the above steps (1) and (2).

[0044] The use of the release film of the present invention is not particularly limited, but it can be suitably used in the production processes of printed wiring boards, flexible circuit boards, multilayer printed wiring boards, and the like. Specifically, for example, in the manufacturing process of a flexible circuit board, the release film of the present invention can be used when hot press bonding a coverlay film to a flexible circuit board main body having a copper circuit formed thereon via a thermosetting adhesive or a thermosetting adhesive sheet. The release film of the present invention can also be suitably used in the production of flexible circuit boards by the RtoR method, which requires high releasability. Effect of the Invention

[0045] According to the present invention, it is possible to provide a release film that is less likely to wrinkle when heated. Also, according to the present invention, it is possible to provide a method for producing the release film. [Brief description of the drawings]

[0046] [Figure 1] 1 is a polarizing microscope image of the release film obtained in Example 1. [Diagram 2]1 is a histogram obtained from a polarizing microscope observation image of the release film obtained in Example 1. [Diagram 3] 1 is an observation image of the release film obtained in Example 1 after a heating test. [Figure 4] 1 is a polarizing microscope image of the release film obtained in Comparative Example 4. [Diagram 5] 1 is a histogram obtained from a polarizing microscope observation image of the release film obtained in Comparative Example 4. [Figure 6] 1 is an observation image of the release film obtained in Comparative Example 4 after a heating test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0047] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0048] Example 1 (1) Preparation of resin composition A resin composition for a release layer was obtained by mixing 70 parts by weight of polybutylene terephthalate resin (PBT) and 30 parts by weight of a copolymer of polybutylene terephthalate and polytetramethylene glycol (PBT / PTMG copolymer). On the other hand, 20 parts by weight of polybutylene terephthalate resin (PBT) (main component resin of the release layer), 40 parts by weight of polypropylene resin (PP), and 40 parts by weight of ethylene-methyl methacrylate copolymer (EMMA) were mixed to obtain a resin composition for the cushion layer.

[0049] (2) Process (1) (raw film production process) The resin composition for the release layer and the resin composition for the cushion layer were co-extruded in three layers at a T-die width of 400 mm using an extruder (GM Engineering, GM30-28 (screw diameter 30 mm, L / D 28)). This resulted in a three-layered raw film having a release layer (thickness 25 μm on one side) on both sides of a cushion layer (thickness 70 μm). During co-extrusion, the extruded resin was pinched at a resin temperature of 250° C. with a metal roll (Rz=0.03 μm) and a pinch roll (Rz=5 μm) at a pressure of 0.2 MPa to form a film, thereby embossing the surface of the release layer.

[0050] (3) Step (2) (Embossing step) The obtained raw film was pressed with an embossing machine (manufactured by Yuri Roll Co., Ltd.) at a pressure of 2 MPa to emboss the surface of the release layer, thereby obtaining a release film. During the embossing process, a metal roll (Rz=40 μm) was used, the linear speed was 5 m / min, and the metal roll temperature (heating temperature) was 110° C.

[0051] (4) Calculation of the standard deviation, maximum value, and difference between the maximum value and the minimum value of the residual strain orientation index Polarizing microscope observation images of the release film were taken under the following conditions using a polarizing microscope (Olympus Corporation, "BX53M" and "OLYMPUS Stream Basic ver2.4") Note that images were taken while avoiding areas with scratches, etc., and the image files were saved in TIFF format without compression. Differential interference slider: Yes Magnification: 4x Exposure conditions: Auto mode Sensitivity: ISO200 Exposure compensation: 0 Resolution: 1920 x 1440 (Field of view: 3.55716 mm x 2.64942 mm) Aspect Ratio: Standard White balance mode: Auto (high)

[0052] The obtained polarizing microscope images were analyzed using software (NIH, software "ImageJ ver1.52p", plug-in "OrientationJ ver2.0.4") as described below. First, the obtained polarizing microscope observation image was converted to an 8-bit image using "ImageJ ver1.52p". Next, five images were analyzed (brightness analysis) using "Orientation Distribution" in "OrientationJ ver2.0.4" under the conditions of Local Window σ: 4 pixels, Gradient: Cubic Spline. In the histogram obtained by the analysis, the horizontal axis was "Orientation in Degrees" and the vertical axis was "Distribution of orientation", and the value on the vertical axis was taken as the "residual strain orientation index". The obtained data on the "residual strain orientation index" was imported into the software "Microsoft Office Standard 2016 Excel" and its standard deviation was calculated. In addition, five images taken at any five points on the release film were used to calculate the standard deviation. In other words, the standard deviation of the "residual strain orientation index" was calculated for each of the five images, and the average value was adopted. In the same manner as the standard deviation, the maximum value of the "residual strain orientation index" and the difference between the maximum value and the minimum value were calculated using the software "Microsoft Office Standard 2016 Excel".

[0053] (Examples 2 to 7, Comparative Examples 1 to 5) A release film was obtained in the same manner as in Example 1, except that the conditions of step (1) (raw film preparation step) and step (2) (embossing step) were changed as shown in Table 1. Fig. 1 shows a polarizing microscope image of the release film obtained in Example 1, and Fig. 2 shows a histogram obtained from the polarizing microscope image of the release film obtained in Example 1. Similarly, Fig. 4 shows a polarizing microscope image of the release film obtained in Comparative Example 4, and Fig. 5 shows a histogram obtained from the polarizing microscope image of the release film obtained in Comparative Example 4.

[0054] <Evaluation> The release films obtained in the examples and comparative examples were evaluated as follows. The results are shown in Table 1.

[0055] (1) Evaluation of wrinkles caused by heating (1-1) Making the underlay A coverlay film (NIKKAN INDUSTRY CO., LTD., CISV-2535) cut to a 200 mm square was placed on top of a 300 mm square piece of cushion paper, and pressed for 6 minutes at 30 kgf pressure and 180°C using a sliding vacuum heater press (MIKADO TECHNOS CO., LTD., MKP-3000v-MH-ST).

[0056] (1-2) Sample preparation The obtained release film was cut to a size of 60 mm x 120 mm. The release film was wrapped around a SUS plate weighing about 200 g and measuring 63 mm x 63 mm x 6 mm at room temperature, and both ends were fixed with tape. The tape used in this case is preferably one that can withstand heat of 180°C.

[0057] (1-3) Heating test The underlay prepared above was placed on a hot plate (manufactured by AS ONE, ND-2) and heated at a set temperature of 180°C. After the actual temperature measured on the monitor reached 180°C and was sufficiently stabilized, the sample prepared above was placed on the underlay and heated for 5 minutes. After that, the sample was removed from the hot plate and underlay, and immediately thereafter, the tape was gently removed so as not to tear the release film, and the release film was removed from the SUS plate. The release film was left to stand until it reached room temperature. 3 and 6 show examples of observation images of the release film after such a heating test. Fig. 3 is an observation image of the release film obtained in Example 1 after the heating test, and no wrinkles are observed. Fig. 6 is an observation image of the release film obtained in Comparative Example 4 after the heating test, and wrinkles are generated due to heating.

[0058] (1-4) Wrinkle measurement The release film after the heating test was placed on a glass plate, and weights were placed on both ends of the release film to make it stick tightly to the glass plate. Using a Mitutoyo Surf Test SJ-301, λc was set to 8 mm and the range to 350 μm, and the surface roughness Rz of the release film was measured in accordance with JIS B0601:2001. Measurements were performed at five arbitrary locations, and the three largest values ​​among the five measured values ​​were adopted, and their average value was taken as (A). The same measurement was performed on the release film before the heating test, and the average value obtained was designated as (B). The value (A) / (B) was calculated, and if the solution (C) was 2.00 or less, it was judged as ◯, and if it exceeded 2.00, it was judged as ×. Note that (C) was rounded off to the third decimal place.

[0059] [Table 1] [Industrial Applicability]

[0060] According to the present invention, it is possible to provide a release film that is less likely to wrinkle when heated. Also, according to the present invention, it is possible to provide a method for producing the release film.

Claims

1. A release film having at least one release layer, The standard deviation of the residual strain orientation index obtained by analyzing the polarizing microscope observation image of the release film is 10,000 or less. A release film characterized by:

2. 2. The release film according to claim 1, wherein the maximum value of the residual strain orientation index obtained by analyzing an image of the release film observed under a polarizing microscope is 40,000 or less.

3. 3. The release film according to claim 1, wherein the difference between the maximum and minimum values ​​of the residual strain orientation index obtained by analyzing an image of the release film observed under a polarizing microscope is 30,000 or less.

4. 4. The release film according to claim 1, 2 or 3, wherein the release layer contains an aromatic polyester resin.

5. 5. The release film according to claim 4, wherein the aromatic polyester resin contains a polybutylene terephthalate resin.

6. 6. The release film according to claim 5, wherein the polybutylene terephthalate resin accounts for 75% by weight or more of the resin constituting the release layer.

7. A method for producing the release film according to claim 1, 2, 3, 4, 5 or 6, comprising the steps of: A step (1) of preparing a raw film having at least one release layer; and (2) a step of embossing the surface of the release layer in the obtained raw film. A method for producing a release film comprising the steps of:

Citation Information

Patent Citations

  • Manufacture of laminated printed board

    JP1993283862A

  • Release film and manufacturing method of circuit substrate

    JP2008246882A

  • Mold release film

    JP2009132806A

  • Multilayer release film

    JP2015058691A

  • Release film for adhesive sheet, and adhesive sheet laminate

    JP2020066174A