Processes for the depolymerization of polyethylene terephthalate (PET)

The described process efficiently depolymerizes PET into DMT and MEG using methanol and sodium methoxide, addressing inefficiencies in existing methods by achieving high yields and handling larger particle sizes and impurities with reduced energy consumption.

JP7583733B2Active Publication Date: 2024-11-149449710カナダインク
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021555542
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-20
Filing Date
2020-03-18
Publication Date
2024-11-14
Estimated Expiration
2040-03-18

AI Technical Summary

Technical Problem

Existing methods for depolymerizing polyethylene terephthalate (PET) are inefficient in handling larger particle sizes and require high energy consumption, leading to suboptimal yields of dimethyl terephthalate (DMT) and monoethylene glycol (MEG), and there is a need for a process that can handle impurities and achieve high yields with lower energy input.

Method used

A process involving the use of methanol and sodium methoxide to depolymerize PET, where a first portion of methanol is mixed with PET, followed by the addition of sodium methoxide and subsequent portions of methanol, allowing for the formation of DMT and MEG, with specific conditions on time, temperature, and methanol concentration to enhance yield and efficiency.

Benefits of technology

The process achieves high yields of DMT and MEG, up to 99 mol% and 95 mol% respectively, while accommodating larger particle sizes and varying impurity levels, with improved energy efficiency and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present disclosure relates to forming dimethyl terephthalate (DMT) and monoethylene glycol (MEG). The present invention also relates to depolymerizing polyethylene terephthalate (PET) and recovering dimethyl terephthalate (DMT) and monoethylene glycol (MEG) using sodium methoxide as a catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] cross reference This patent application claims the benefit of U.S. Provisional Patent Application No. 62 / 821,270, filed March 20, 2019, which is incorporated by reference in its entirety herein.

[0002] The present disclosure relates to the formation of dimethyl terephthalate (DMT) and monoethylene glycol (MEG) from polyethylene terephthalate (PET). [Background technology]

[0003] The market for polyethylene terephthalate (PET) bottle resin has experienced strong growth as PET resin replaces carbonated soft drink glasses, water bottles and food containers.

[0004] Dimethyl terephthalate (DMT) is used primarily in the production of polyethylene terephthalate (PET) for fibers, films, container plastics and specialty plastic applications.

[0005] The largest polyester segment is the textile market, where it is used to make clothing, household textiles such as sheets and curtains, carpets and rugs, and industrial products such as tire cord, seat belts, hoses and ropes. PET film is used in electrical applications such as dielectric metal foil capacitors, and for food packaging. Summary of the Invention

[0006] Disclosed herein is a process for depolymerizing polyethylene terephthalate (PET) contained in a feedstock to form dimethyl terephthalate (DMT) and monoethylene glycol (MEG), the process comprising: (i) combining a feedstock comprising polyethylene terephthalate (PET) and a first portion of methanol to form a first mixture; (ii) adding sodium methoxide to the first mixture; (iii) mixing; (iv) adding a second portion of methanol, thereby forming a second mixture; The process forms dimethyl terephthalate (DMT) and monoethylene glycol (MEG).

[0007] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first portion of methanol is between about 0.1 kg and about 0.5 kg per kg of feedstock.

[0008] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first portion of methanol is about 0.3 kg per kg of feedstock.

[0009] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 15 minutes to about 120 minutes.

[0010] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 60 minutes.

[0011] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out at a temperature between about 50° C. and about 100° C.

[0012] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out at a temperature between about 60°C and about 90°C.

[0013] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out at a temperature of about 60° C.

[0014] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out at a temperature of about 80° C.

[0015] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 10 minutes to about 120 minutes.

[0016] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 30 minutes.

[0017] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out at a temperature between about 40° C. and about 100° C.

[0018] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is conducted at a temperature between about 85° C. and about 90° C.

[0019] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided to maintain a sodium methoxide concentration of the second mixture between about 0.2% and about 5.0% by weight.

[0020] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided to maintain a sodium methoxide concentration of the second mixture between about 0.5% and about 1.5% by weight.

[0021] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided to maintain a sodium methoxide concentration of the second mixture at about 0.7 wt.%.

[0022] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided at a predetermined time in multiple fractions.

[0023] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), a first fraction of the second portion of methanol is provided about 1 minute to about 60 minutes after the addition of sodium methoxide.

[0024] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 30 minutes after the addition of sodium methoxide.

[0025] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first fraction of the second portion of methanol is between about 50 g / kg of feedstock and about 100 g / kg of feedstock.

[0026] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 30 minutes to about 90 minutes after the addition of sodium methoxide.

[0027] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 60 minutes after the addition of sodium methoxide.

[0028] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the second fraction of the second portion of methanol is between about 100 g / kg of feedstock and about 200 g / kg of feedstock.

[0029] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), a third fraction of the second portion of methanol is provided about 60 minutes to about 120 minutes after the addition of sodium methoxide.

[0030] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), a third fraction of the second portion of methanol is provided about 90 minutes after the addition of sodium methoxide.

[0031] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the third fraction of the second portion of methanol is between about 100 g per kg of feedstock and about 200 g per kg of feedstock.

[0032] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is fed continuously.

[0033] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is continuously fed at a rate between about 50 g / h / kg feedstock and about 100 g / h / kg feedstock.

[0034] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the ratio of sodium methoxide to polyethylene terephthalate (PET) is between about 1:2 and about 1:28 (mol / mol).

[0035] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the ratio of sodium methoxide to polyethylene terephthalate (PET) is between about 1:5 and about 1:20 (mol / mol).

[0036] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the ratio of sodium methoxide to polyethylene terephthalate (PET) is between about 1:10 and about 1:20 (mol / mol).

[0037] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the ratio of sodium methoxide to polyethylene terephthalate (PET) is between about 1:10 and about 1:15 (mol / mol).

[0038] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), dimethyl terephthalate is obtained in a yield of at least about 90 mol%.

[0039] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), dimethyl terephthalate is obtained in a yield of at least about 95 mol%.

[0040] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), dimethyl terephthalate is obtained in a yield of at least about 99 mol%.

[0041] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), monoethylene glycol is obtained in a yield of at least about 80 mol %.

[0042] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), monoethylene glycol is obtained in a yield of at least about 85 mol%.

[0043] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), monoethylene glycol is obtained in a yield of at least about 90 mol %.

[0044] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), a feedstock comprising polyethylene terephthalate (PET) is provided in the form of particles.

[0045] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the average particle size is between about 0.1 mm and about 20 mm.

[0046] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the average particle size is between about 5 mm and about 10 mm.

[0047] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the average particle size is up to about 6 mm.

[0048] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the average particle size is up to about 8 mm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0049] Dimethyl terephthalate (DMT) is used in the production of polyesters such as polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT) and polybutylene terephthalate (PBT). Because DMT is volatile, it is an intermediate in some schemes for recycling PET, for example from plastic bottles. Hydrogenation of DMT gives the diol 1,4-cyclohexanedimethanol, a useful monomer in forming polyester resins.

[0050] DMT has been produced in a number of ways. Traditionally, and still commercially valuable today, it is the direct esterification of terephthalic acid. Alternatively, it is prepared from paraxylene via methyl paratoluate, alternating with a step of oxidation and methyl esterification. The process for producing DMT from paraxylene and methanol consists of four main steps: oxidation, esterification, distillation, and crystallization. A mixture of paraxylene and p-toluate esters is oxidized with air in the presence of a transition metal catalyst (Co / Mn). The acid mixture from the oxidation is esterified with methanol to produce an ester mixture. The crude ester mixture is distilled to remove any heavy boilers and residues produced, and the lighter esters are recycled to the oxidation step. The raw DMT is then crystallized to remove DMT isomers, residual acids, and aromatic aldehydes.

[0051] Improvements in recycling PET to produce DMT and MEG: The expanding use of PET in the packaging and textile (carpet and other textile) industries requires highly efficient, low energy, high yield and cost-effective methods for forming DMT and MEG from PET.

[0052] feedstock Described herein is a process for depolymerizing polyethylene terephthalate (PET) contained in a feedstock to form dimethyl terephthalate (DMT) and monoethylene glycol (MEG).

[0053] In some embodiments, the feedstock containing polyethylene terephthalate also contains contaminants, including other polymers (e.g., polyethylene, polypropylene, polyvinyl chloride (PVC), polycarbonate (PC), polyvinylidene chloride (PVDC), and polyamides), paper, stains, dirt, ethylene vinyl alcohol (EVOH), ethylene vinyl acetate (EVA), cellulose, adhesives, or combinations thereof. In some embodiments, the feedstock contains between about 5% and about 30% contaminants.

[0054] Mishra et al. (Kinetic and thermodynamic study of methanolysis of poly(ethylene terephthalate) waste powder Polym. Int. 52:337-342(2003)) shows that the larger the particle size of the PET flakes, the less likely the depolymerization will proceed. Mishra et al. documented an optimal particle size of 127.5 μm. There is a need for a depolymerization process that can use larger particle size feedstocks. In some embodiments, the polyethylene terephthalate (PET)-containing feedstock is provided in the form of particles. In some embodiments, the average particle size is between about 0.1 mm and about 20 mm. In some embodiments, the average particle size is between about 5 mm and about 10 mm. In some embodiments, the average particle size is up to about 5 mm. In some embodiments, the average particle size is up to about 6 mm. In some embodiments, the average particle size is up to about 7 mm. In some embodiments, the average particle size is up to about 8 mm. In some embodiments, the average particle size is up to about 9 mm. In some embodiments, the average particle size is up to about 10 mm. In some embodiments, the average particle size is up to about 11 mm. In some embodiments, the average particle size is up to about 12 mm. In some embodiments, the average particle size is up to about 13 mm. In some embodiments, the average particle size is up to about 14 mm. In some embodiments, the average particle size is up to about 15 mm. In some embodiments, the average particle size is up to about 16 mm. In some embodiments, the average particle size is up to about 17 mm. In some embodiments, the average particle size is up to about 18 mm. In some embodiments, the average particle size is up to about 19 mm. In some embodiments, the average particle size is up to about 20 mm.

[0055] DMT Described herein is a process for depolymerizing polyethylene terephthalate (PET) contained in a feedstock to form dimethyl terephthalate (DMT) and monoethylene glycol (MEG).

[0056] In some embodiments, DMT contains less than about 10% impurities (w / w). In some embodiments, DMT contains less than about 9% impurities (w / w). In some embodiments, DMT contains less than about 8% impurities (w / w). In some embodiments, DMT contains less than about 7% impurities (w / w). In some embodiments, DMT contains less than about 6% impurities (w / w). In some embodiments, DMT contains less than about 5% impurities (w / w). In some embodiments, DMT contains less than about 4% impurities (w / w). In some embodiments, DMT contains less than about 3% impurities (w / w). In some embodiments, DMT contains less than about 2% impurities (w / w). In some embodiments, DMT contains less than about 1% impurities (w / w). In some embodiments, DMT contains less than about 0.5% impurities (w / w). In some embodiments, DMT contains less than about 0.4% impurities (w / w). In some embodiments, the DMT contains less than about 0.3% impurities (w / w). In some embodiments, the DMT contains less than about 0.2% impurities (w / w). In some embodiments, the DMT contains less than about 0.1% impurities (w / w).

[0057] In some embodiments, the DMT is less than about 250 ppm of any metal, less than about 240 ppm of any metal, less than about 230 ppm of any metal, less than about 220 ppm of any metal, less than about 210 ppm of any metal, less than about 200 ppm of any metal, less than about 190 ppm of any metal, less than about 180 ppm of any metal, less than about 170 ppm of any metal, less than about 160 ppm of any metal, less than about 150 ppm of any metal, less than about 140 ppm of any metal, less than about 130 ppm of any metal, less than about 120 ppm of any metal, less than about 110 ppm of any metal, less than about 100 ppm of any metal, less than about 90 ppm of any metal, less than about 80 ppm of any metal, less than about 70 ppm of any metal, less than about 60 ppm of any metal, less than about 50 ppm of any metal, less than about 40 ppm of any metal, less than about 30 ppm of any metal, less than about 20 ppm of any metal. , less than about 10 ppm of any metal, less than about 5 ppm of any metal, less than about 4 ppm of any metal, less than about 3 ppm of any metal, less than about 2 ppm of any metal, less than about 1 ppm of any metal, less than about 0.9 ppm of any metal, less than about 0.8 ppm of any metal, less than about 0.7 ppm of any metal, less than about 0.6 ppm of any metal, less than about 0.5 ppm of any metal, less than about 0.4 ppm of any metal, less than about 0.3 ppm of any metal, less than about 0.2 ppm of any metal, less than about 0.1 ppm of any metal, less than about 0.09 ppm of any metal, less than about 0.08 ppm of any metal, less than about 0.07 ppm of any metal, less than about 0.06 ppm of any metal, less than about 0.05 ppm of any metal, less than about 0.04 ppm of any metal, less than about 0.03 ppm of any metal, less than about 0.02 ppm of any metal, or less than about 0.01 ppm of any metal.

[0058] In some embodiments, the DMT is less than about 10 ppm sodium methoxide, less than about 5 ppm sodium methoxide, less than about 4 ppm sodium methoxide, less than about 3 ppm sodium methoxide, less than about 2 ppm sodium methoxide, less than about 1 ppm sodium methoxide, less than about 0.9 ppm sodium methoxide, less than about 0.8 ppm sodium methoxide, less than about 0.7 ppm sodium methoxide, less than about 0.6 ppm sodium methoxide, less than about 0.5 ppm sodium methoxide, less than about 0.4 ppm sodium methoxide, less than about 0.3 ppm sodium methoxide, pm of sodium methoxide, less than about 0.2 ppm of sodium methoxide, less than about 0.1 ppm of sodium methoxide, less than about 0.09 ppm of sodium methoxide, less than about 0.08 ppm of sodium methoxide, less than about 0.07 ppm of sodium methoxide, less than about 0.06 ppm of sodium methoxide, less than about 0.05 ppm of sodium methoxide, less than about 0.04 ppm of sodium methoxide, less than about 0.03 ppm of sodium methoxide, less than about 0.02 ppm of sodium methoxide, or less than about 0.01 ppm of sodium methoxide.

[0059] In some embodiments, DMT is obtained in a yield between about 50 mol% and about 99 mol%. In some embodiments, DMT is obtained in a yield between about 60 mol% and about 99 mol%. In some embodiments, DMT is obtained in a yield between about 70 mol% and about 99 mol%. In some embodiments, DMT is obtained in a yield between about 80 mol% and about 99 mol%. In some embodiments, DMT is obtained in a yield between about 85 mol% and about 99 mol%. In some embodiments, DMT is obtained in a yield between about 90 mol% and about 99 mol%. In some embodiments, DMT is obtained in a yield of at least about 50 mol%. In some embodiments, DMT is obtained in a yield of at least about 55 mol%. In some embodiments, DMT is obtained in a yield of at least about 60 mol%. In some embodiments, DMT is obtained in a yield of at least about 65 mol%. In some embodiments, DMT is obtained in a yield of at least about 70 mol%. In some embodiments, DMT is obtained in a yield of at least about 75 mol%. In some embodiments, DMT is obtained in a yield of at least about 80 mol%. In some embodiments, DMT is obtained in a yield of at least about 85 mol%. In some embodiments, DMT is obtained in a yield of at least about 90 mol%. In some embodiments, DMT is obtained in a yield of at least about 95 mol%. In some embodiments, DMT is obtained in a yield of at least about 99 mol%.

[0060] MEG Described herein is a process for depolymerizing polyethylene terephthalate (PET) contained in a feedstock to form dimethyl terephthalate (DMT) and monoethylene glycol (MEG).

[0061] In some embodiments, MEG contains less than about 10% impurities (w / w). In some embodiments, MEG contains less than about 9% impurities (w / w). In some embodiments, MEG contains less than about 8% impurities (w / w). In some embodiments, MEG contains less than about 7% impurities (w / w). In some embodiments, MEG contains less than about 6% impurities (w / w). In some embodiments, MEG contains less than about 5% impurities (w / w). In some embodiments, MEG contains less than about 4% impurities (w / w). In some embodiments, MEG contains less than about 3% impurities (w / w). In some embodiments, MEG contains less than about 2% impurities (w / w). In some embodiments, MEG contains less than about 1% impurities (w / w). In some embodiments, MEG contains less than about 0.5% impurities (w / w). In some embodiments, MEG contains less than about 0.4% impurities (w / w). In some embodiments, MEG contains less than about 0.3% impurities (w / w). In some embodiments, MEG contains less than about 0.2% impurities (w / w). In some embodiments, MEG contains less than about 0.1% impurities (w / w).

[0062] In some embodiments, MEG is obtained in a yield between about 50 mol% and about 99 mol%. In some embodiments, MEG is obtained in a yield between about 60 mol% and about 99 mol%. In some embodiments, MEG is obtained in a yield between about 70 mol% and about 99 mol%. In some embodiments, MEG is obtained in a yield between about 80 mol% and about 99 mol%. In some embodiments, MEG is obtained in a yield between about 85 mol% and about 99 mol%. In some embodiments, MEG is obtained in a yield between about 90 mol% and about 99 mol%. In some embodiments, MEG is obtained in a yield of at least about 50 mol%. In some embodiments, MEG is obtained in a yield of at least about 55 mol%. In some embodiments, MEG is obtained in a yield of at least about 60 mol%. In some embodiments, MEG is obtained in a yield of at least about 65 mol%. In some embodiments, MEG is obtained in a yield of at least about 70 mol%. In some embodiments, MEG is obtained in a yield of at least about 75 mol%. In some embodiments, MEG is obtained in a yield of at least about 80 mol%. In some embodiments, MEG is obtained in a yield of at least about 85 mol%. In some embodiments, MEG is obtained in a yield of at least about 90 mol%. In some embodiments, MEG is obtained in a yield of at least about 95 mol%. In some embodiments, MEG is obtained in a yield of at least about 99 mol%.

[0063] Sodium Methoxide Described herein is a process for depolymerizing polyethylene terephthalate (PET) contained in a feedstock to form dimethyl terephthalate (DMT) and monoethylene glycol (MEG).

[0064] In some embodiments, the processes described herein include a catalytic amount of sodium methoxide. In some embodiments, the processes described herein include a substoichiometric amount of sodium methoxide.

[0065] "Substoichiometric amount," as used herein, is used to indicate the usage of less than a stoichiometric amount of material. The term is used interchangeably herein with "catalytic amount." In some embodiments, the substoichiometric amount is about 95% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 90% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 85% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 80% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 75% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 70% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 65% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 60% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 55% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 50% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 45% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 40% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 35% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 30% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 25% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 20% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 15% or less of the stoichiometric amount. In some embodiments, the substoichiometric amount is about 10% or less of the stoichiometric amount.

[0066] "Stoichiometric amount," as used herein, is used to indicate that the amount of material used is equal to the number of ester bonds present in the polyester.

[0067] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the ratio of sodium methoxide to polyethylene terephthalate (PET) is between about 1:2 and about 1:28 (mol / mol). In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the ratio of sodium methoxide to polyethylene terephthalate (PET) is between about 1:5 and about 1:20 (mol / mol). In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the ratio of sodium methoxide to polyethylene terephthalate (PET) is between about 1:10 and about 1:20 (mol / mol). In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the ratio of sodium methoxide to polyethylene terephthalate (PET) is between about 1:10 and about 1:15 (mol / mol).

[0068] Process for depolymerization Described herein is a process for depolymerizing polyethylene terephthalate (PET) contained in a feedstock to form dimethyl terephthalate (DMT) and monoethylene glycol (MEG), the process comprising: (i) combining a feedstock comprising polyethylene terephthalate (PET) and a first portion of methanol to form a first mixture; (ii) adding sodium methoxide to the first mixture; (iii) mixing; (iv) adding a second portion of methanol, thereby forming a second mixture; The process forms dimethyl terephthalate (DMT) and monoethylene glycol (MEG).

[0069] Process (i) In some embodiments, the processes described herein include pretreating polyethylene terephthalate (PET) with a first portion of a methanol solvent that swells the polyethylene terephthalate (PET) prior to the addition of sodium methoxide.

[0070] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first portion of methanol is between about 0.1 kg and about 0.5 kg per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first portion of methanol is between about 0.2 kg and about 0.4 kg per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first portion of methanol is between about 0.1 kg and about 0.3 kg per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first portion of methanol is between about 0.3 kg and about 0.5 kg per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first portion of methanol is about 0.1 kg per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first portion of methanol is about 0.2 kg per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first portion of methanol is about 0.3 kg per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first portion of methanol is about 0.4 kg per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first portion of methanol is about 0.5 kg per kg of feedstock.

[0071] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 15 minutes to about 120 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 15 minutes to about 90 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 15 minutes to about 60 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 30 minutes to about 120 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 60 minutes to about 120 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 45 minutes to about 90 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 45 minutes to about 60 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 60 minutes to about 90 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 15 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 20 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 25 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 30 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 35 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 40 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 45 minutes.In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 50 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 55 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 60 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 65 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 70 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 75 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 80 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 85 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 90 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 95 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 100 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 105 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 110 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 115 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is carried out for about 120 minutes.

[0072] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature between about 25° C. and about 100° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature between about 25° C. and about 60° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature between about 25° C. and about 80° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature between about 50° C. and about 100° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature between about 60° C. and about 90° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 25° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 30° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 35° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 40° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 45° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 50° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 55° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 60° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 65° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 70° C.In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 75° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 80° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 85° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 90° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 95° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (i) is performed at a temperature of about 100° C.

[0073] Process (iii) In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 10 minutes to about 120 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 10 minutes to about 90 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 10 minutes to about 60 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 10 minutes to about 45 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 10 minutes to about 30 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 30 minutes to about 120 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 60 minutes to about 120 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 90 minutes to about 120 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 10 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 15 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 20 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 25 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 30 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 35 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 40 minutes.In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 45 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 50 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 55 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 60 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 65 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 70 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 75 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 80 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 85 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 90 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 95 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 100 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 105 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 110 minutes. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 115 minutes.In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is carried out for about 120 minutes.

[0074] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature between about 40° C. and about 100° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature between about 50° C. and about 100° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature between about 60° C. and about 100° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature between about 70° C. and about 100° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature between about 80° C. and about 100° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature between about 85° C. and about 90° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature of about 40° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature of about 45° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature of about 50° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature of about 55° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature of about 60° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature of about 65° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature of about 70° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature of about 75° C.In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature of about 80° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature of about 85° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature of about 90° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature of about 95° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iii) is performed at a temperature of about 100° C.

[0075] Process (iv) In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), methanol is consumed during the process for depolymerization to form dimethyl terephthalate (DMT). In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), a second portion of methanol is added.

[0076] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided to maintain the sodium methoxide concentration of the second mixture between about 0.2% and about 5.0% by weight. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided to maintain the sodium methoxide concentration of the second mixture between about 0.2% and about 4.0% by weight. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided to maintain the sodium methoxide concentration of the second mixture between about 0.2% and about 3.0% by weight. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided to maintain the sodium methoxide concentration of the second mixture between about 0.2% and about 2.0% by weight. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided to maintain the sodium methoxide concentration of the second mixture between about 0.2% and about 1.5% by weight. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided to maintain the sodium methoxide concentration of the second mixture between about 0.5% and about 1.0% by weight. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided to maintain the sodium methoxide concentration of the second mixture at about 0.7% by weight.In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the sodium methoxide concentration of the second mixture is about 0.2 wt%, about 0.3 wt%, about 0.4 wt%, about 0.5 wt%, about 0.6 wt%, about 0.7 wt%, about 0.8 wt%, about 0.9 wt%, about 1 wt%, about 1.1 wt%, about 1.2 wt%, about 1.3 wt%, about 1.4 wt%, about 1.5 wt%, about 1.6 wt%, about 1.7 wt%, about 1.8 wt%, about 1.9 wt%, about 2 wt%, about 2.1 wt%, about 2.2 wt%, about 2.3 wt%, about A second portion of methanol is provided to maintain the mixture at about 2.4 wt%, about 2.5 wt%, about 2.6 wt%, about 2.7 wt%, about 2.8 wt%, about 2.9 wt%, about 3 wt%, about 3.1 wt%, about 3.2 wt%, about 3.3 wt%, about 3.4 wt%, about 3.5 wt%, about 3.6 wt%, about 3.7 wt%, about 3.8 wt%, about 3.9 wt%, about 4 wt%, about 4.1 wt%, about 4.2 wt%, about 4.3 wt%, about 4.4 wt%, about 4.5 wt%, about 4.6 wt%, about 4.7 wt%, about 4.8 wt%, about 4.9 wt%, or about 5 wt%.

[0077] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature between about 25° C. and about 100° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature between about 25° C. and about 60° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature between about 25° C. and about 80° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature between about 50° C. and about 100° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature between about 60° C. and about 90° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 25° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 30° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 35° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 40° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 45° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 50° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 55° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 60° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 65° C.In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 70° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 75° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 80° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 85° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 90° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 95° C. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is performed at a temperature of about 100° C.

[0078] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is carried out for a total time between about 1 hour and about 10 hours. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is carried out for a total time between about 1 hour and about 8 hours. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is carried out for a total time between about 1 hour and about 5 hours. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is carried out for a total time between about 4 hours and about 6 hours. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), step (iv) is carried out for a total time between about 3 hours and about 7 hours.

[0079] Sequential addition In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), in step (iv), the second portion of methanol is provided sequentially at a predetermined time. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), in step (iv), the second portion of methanol is provided at a predetermined time in a plurality of fractions. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided in 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 fractions. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided in 1, 2, 3, 4, or 5 fractions. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided in 1, 2, or 3 fractions. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided in 2 or 3 fractions. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided in two fractions. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided in three fractions. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided in four fractions. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided in five fractions. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided in six fractions. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided in seven fractions. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided in eight fractions.In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided in 9 fractions. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is provided in 10 fractions.

[0080] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the mixture is blended between the addition of each fraction.

[0081] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 1 minute to about 60 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 15 minutes to about 45 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 1 minute after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 5 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 10 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 15 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 20 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 25 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 30 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 35 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 40 minutes after the addition of sodium methoxide.In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 45 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 50 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 55 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the first fraction of the second portion of methanol is provided about 60 minutes after the addition of sodium methoxide.

[0082] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first fraction of the second portion of methanol is between about 10 g / kg feedstock and about 100 g / kg feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first fraction of the second portion of methanol is between about 50 g / kg feedstock and about 100 g / kg feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first fraction of the second portion of methanol is between about 50 g / kg feedstock and about 80 g / kg feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first fraction of the second portion of methanol is about 10 g / kg feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first fraction of the second portion of methanol is about 20 g / kg feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first fraction of the second portion of methanol is about 30 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first fraction of the second portion of methanol is about 40 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first fraction of the second portion of methanol is about 50 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first fraction of the second portion of methanol is about 60 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first fraction of the second portion of methanol is about 70 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first fraction of the second portion of methanol is about 80 g per kg of feedstock.In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first fraction of the second portion of methanol is about 90 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the first fraction of the second portion of methanol is about 100 g per kg of feedstock.

[0083] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 30 minutes to about 90 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 45 minutes to about 75 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 30 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 35 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 40 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 45 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 50 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 55 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 60 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 65 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 70 minutes after the addition of sodium methoxide.In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 75 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 80 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 85 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second fraction of the second portion of methanol is provided about 90 minutes after the addition of sodium methoxide.

[0084] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the second fraction of the second portion of methanol is between about 100 g / kg of feedstock and about 200 g / kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the second fraction of the second portion of methanol is between about 100 g / kg of feedstock and about 150 g / kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the second fraction of the second portion of methanol is about 100 g / kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the second fraction of the second portion of methanol is about 110 g / kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the second fraction of the second portion of methanol is about 120 g / kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the second fraction of the second portion of methanol is about 130 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the second fraction of the second portion of methanol is about 140 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the second fraction of the second portion of methanol is about 150 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the second fraction of the second portion of methanol is about 160 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the second fraction of the second portion of methanol is about 170 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the second fraction of the second portion of methanol is about 180 g per kg of feedstock.In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the second fraction of the second portion of methanol is about 190 g / kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the second fraction of the second portion of methanol is about 200 g / kg of feedstock.

[0085] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 60 minutes to about 120 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 90 minutes to about 120 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 60 minutes to about 90 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 60 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 65 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 70 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 75 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 80 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 85 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 90 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 95 minutes after the addition of sodium methoxide.In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 100 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 105 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 110 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 115 minutes after the addition of sodium methoxide. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the third fraction of the second portion of methanol is provided about 120 minutes after the addition of sodium methoxide.

[0086] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the third fraction of the second portion of methanol is between about 100 g / kg of feedstock and about 200 g / kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the third fraction of the second portion of methanol is between about 100 g / kg of feedstock and about 150 g / kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the third fraction of the second portion of methanol is about 100 g / kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the third fraction of the second portion of methanol is about 110 g / kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the third fraction of the second portion of methanol is about 120 g / kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the third fraction of the second portion of methanol is about 130 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the third fraction of the second portion of methanol is about 140 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the third fraction of the second portion of methanol is about 150 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the third fraction of the second portion of methanol is about 160 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the third fraction of the second portion of methanol is about 170 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the third fraction of the second portion of methanol is about 180 g per kg of feedstock.In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the third fraction of the second portion of methanol is about 190 g per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the amount of the third fraction of the second portion of methanol is about 200 g per kg of feedstock.

[0087] Continuous addition In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), in step (iv), the second portion of methanol is supplied continuously.

[0088] In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is continuously fed at a rate between about 50 g / h per kg of feedstock and about 100 g / h per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is continuously fed at a rate between about 50 g / h per kg of feedstock and about 90 g / h per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is continuously fed at a rate between about 50 g / h per kg of feedstock and about 80 g / h per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is continuously fed at a rate between about 50 g / h per kg of feedstock and about 70 g / h per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is continuously fed at a rate of about 50 g / h per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is continuously fed at a rate of about 60 g / h per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is continuously fed at a rate of about 70 g / h per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is continuously fed at a rate of about 80 g / h per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is continuously fed at a rate of about 90 g / h per kg of feedstock. In some embodiments of the process for depolymerizing polyethylene terephthalate (PET), the second portion of methanol is continuously fed at a rate of about 100 g / h per kg of feedstock.

[0089] Specific Terms The section headings used herein are for organizational purposes only and are not to be construed as limiting the subject matter described.

[0090] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood in the art to which the claimed subject matter belongs. In the event that there are a plurality of definitions for terms herein, those in this section prevail.

[0091] It will be understood that the general description and detailed description are merely exemplary and explanatory and are not limiting of any of the subject matter claimed. In this application, the use of the singular includes the plural unless specifically stated otherwise. It should be noted that as used in this specification and the appended claims, the singular forms "a", "an" and "the" include the plural unless the context clearly indicates otherwise. In this application, the use of "or" means "and / or" unless specifically stated otherwise. Furthermore, the use of the term "including" as well as other forms such as "include", "includes" and "included" is not limiting.

[0092] Unless the context requires otherwise, throughout the specification and the following claims, the word "comprise" and variations thereof, such as "comprises" and "comprising," are to be construed in an open and inclusive sense, i.e., "including, but not limited to." Moreover, the headings provided herein are for convenience only and do not interpret the scope or meaning of the claimed invention.

[0093] As used in this specification and the appended claims, the singular forms "a," "an," and "the" include the plural unless the context clearly indicates otherwise. It should also be noted that the term "or" is generally used in its sense including "and / or" unless the context clearly indicates otherwise.

[0094] As used herein, the term "about" or "approximately" means within 10%, preferably within 10%, and more preferably within 5% of a given value or range.

[0095] As used herein, ambient temperature is a colloquial expression of the normal indoor temperature or the preferred indoor (air conditioned) temperature to which people are generally accustomed. Ambient temperature refers to a small range of temperatures, approximately 21° C., where the air does not feel hot or cold. In some embodiments, the ambient temperature is 25±5° C. In some embodiments, the ambient temperature is 18° C. In some embodiments, the ambient temperature is 19° C. In some embodiments, the ambient temperature is 20° C. In some embodiments, the ambient temperature is 21° C. In some embodiments, the ambient temperature is 22° C. In some embodiments, the ambient temperature is 23° C. In some embodiments, the ambient temperature is 24° C. In some embodiments, the ambient temperature is 25° C. In some embodiments, the ambient temperature is 26° C. In some embodiments, the ambient temperature is 27° C. In some embodiments, the ambient temperature is 28° C. In some embodiments, the ambient temperature is 29° C. In some embodiments, the ambient temperature is 30° C.

[0096] As used herein and in the appended claims, depolymerization refers to a process that breaks down a polymer into starting materials. Depolymerization is essentially the opposite of polymerization. In some embodiments, depolymerization is accomplished by methanolysis.

[0097] As used herein, the term "mol" when referring to PET is the molar amount, calculated using the unit molecular weight of "PET" of 192.17 g / mol.

[0098] Definitions of standard chemical terms can be found in reference works including, but not limited to, Carey and Sundberg, "Advanced Organic Chemistry 4th Ed." Vols. A (2000) and B (2001), Plenum Press, New York.

[0099] Working Example The following examples are intended to illustrate, but not limit, the disclosed embodiments.

[0100] Example 1: Depolymerization of PET by sequential addition of methanol To a 25 L reactor containing 10.00 kg of feedstock (PET fines), 3.00 kg of methanol were added. The medium was stirred and heated to 60° C. for 1 hour. The temperature was then increased to 85° C., after which sodium methoxide (30 kg per ton of feedstock) was added. The fractions of methanol were added as follows: 710 g were added 30 minutes after the addition of sodium methoxide, 1.21 kg were added after another 30 minutes, and the final 1.21 kg was added after another 30 minutes. After the addition of sodium methoxide, the reaction medium was stirred at 85° C. for a total of 8 to 10 hours. The yields of the reaction were 97% for DMT and 95% for MEG.

[0101] Example 2: Depolymerization of PET by partial removal of methanol and sequential addition of methanol To a 25 L reactor containing 10.00 kg of feedstock (PET fines), 6.00 kg of methanol were added. The medium was stirred and heated to 60° C. for 1 hour. Then, 3 kg of liquid was discharged and the temperature was increased to 85° C., after which sodium methoxide (30 kg per ton of feedstock) was added. The fractions of methanol were added as follows: 1.21 kg was added 30 minutes after the addition of sodium methoxide, 1.21 kg was added 30 minutes later, and the final 1.21 kg was added 30 minutes later. After the addition of sodium methoxide, the reaction medium was stirred at 85° C. for a total of 8 to 10 hours. The yields of the reaction were 87% for DMT and 83% for MEG.

[0102] Example 3: Depolymerization of PET by partial removal of methanol and addition of methanol once To a 25 L reactor containing 10.00 kg of feedstock (PET fines), 6.00 kg of methanol was added. The medium was stirred and heated to 60° C. for 1 hour. Then, 2.2 kg of liquid was discharged, the temperature was increased to 85° C., and sodium methoxide (30 kg per ton of feedstock) was added. After 30 minutes, 2.3 kg of methanol was added. After the addition of sodium methoxide, the reaction medium was stirred at 85° C. for a total of 8 to 10 hours. The yield of the reaction was 80% for DMT and 93% for MEG.

Claims

1. 1. A process for depolymerizing polyethylene terephthalate (PET) contained in a feedstock to form dimethyl terephthalate (DMT) and monoethylene glycol (MEG), the process comprising: (i) mixing a feedstock comprising polyethylene terephthalate (PET) and a first portion of methanol to form a first mixture; (ii) after step (i), adding sodium methoxide to the first mixture; (iii) mixing; (iv) adding a second portion of methanol, thereby forming a second mixture; forming said dimethyl terephthalate (DMT) and said monoethylene glycol (MEG) by said process.

2. The process of claim 1, wherein the amount of the first portion of methanol is from 0.1 kg per kg of feedstock to 0.5 kg per kg of feedstock.

3. The process of claim 1, wherein the amount of the first portion of methanol is 0.3 kg per kg of feedstock.

4. The process of claim 1, wherein step (i) is carried out for 15 minutes to 120 minutes.

5. The process of claim 1, wherein step (i) is carried out for 60 minutes.

6. The process of claim 1, wherein step (i) is carried out at a temperature of from 50°C to 100°C.

7. The process of claim 1, wherein step (i) is carried out at a temperature of from 60°C to 90°C.

8. The process of claim 1, wherein step (i) is carried out at a temperature of 60°C.

9. The process of claim 1, wherein step (i) is carried out at a temperature of 80°C.

10. The process according to any one of claims 1 to 9, wherein step (iii) is carried out for a period of from 10 minutes to 120 minutes.

11. The process according to any one of claims 1 to 10, wherein step (iii) is carried out for 30 minutes.

12. The process according to any one of claims 1 to 11, wherein step (iii) is carried out at a temperature of from 40°C to 100°C.

13. The process according to any one of claims 1 to 12, wherein step (iii) is carried out at a temperature of from 85°C to 90°C.

14. 14. The process of any one of claims 1 to 13, wherein the second portion of methanol is provided to maintain a sodium methoxide concentration of the second mixture between 0.2 wt% and 5.0 wt%.

15. 15. The process of any one of claims 1 to 14, wherein the second portion of methanol is provided to maintain a sodium methoxide concentration of the second mixture between 0.5% and 1.5% by weight.

16. 16. The process of any one of claims 1 to 15, wherein the second portion of methanol is provided to maintain a sodium methoxide concentration of the second mixture at 0.7 wt%.

17. The process of claim 1, wherein the second portion of the methanol is delivered at a predetermined time in multiple fractions.

18. The process of claim 17, wherein a first fraction of the second portion of the methanol is provided between 1 minute and 60 minutes after the addition of the sodium methoxide.

19. The process of claim 18, wherein a first fraction of the second portion of the methanol is provided 30 minutes after the addition of the sodium methoxide.

20. The process of claim 18 or 19, wherein the amount of the first fraction of the second portion of the methanol is from 50 g per kg of feedstock to 100 g per kg of feedstock.

21. The process of claim 17, wherein a second fraction of the second portion of the methanol is provided 30 minutes to 90 minutes after the addition of the sodium methoxide.

22. The process of claim 17, wherein a second fraction of the second portion of the methanol is provided 60 minutes after the addition of the sodium methoxide.

23. The process of claim 21 or 22, wherein the amount of the second fraction of the second portion of the methanol is from 100 g per kg of feedstock to 200 g per kg of feedstock.

24. 24. The process of any one of claims 17 to 23, wherein a third fraction of the second portion of methanol is provided 60 minutes to 120 minutes after the addition of the sodium methoxide.

25. The process of claim 17, wherein a third fraction of the second portion of the methanol is provided 90 minutes after the addition of the sodium methoxide.

26. The process of claim 24 or 25, wherein the amount of the third fraction of the second portion of methanol is from 100 g per kg of feedstock to 200 g per kg of feedstock.

27. The process of any one of claims 1 to 16, wherein the second portion of the methanol is supplied continuously.

28. The process of claim 27, wherein the second portion of the methanol is continuously supplied at a rate of from 50 g / h per kg of feedstock to 100 g / h per kg of feedstock.

29. The process of any one of claims 1 to 28, wherein the ratio of sodium methoxide to polyethylene terephthalate (PET) is 1:2 to 1:28 (mol / mol).

30. The process of any one of claims 1 to 29, wherein the ratio of sodium methoxide to polyethylene terephthalate (PET) is from 1:5 to 1:20 (mol / mol).

31. The process of any one of claims 1 to 30, wherein the ratio of sodium methoxide to polyethylene terephthalate (PET) is 1:10 to 1:20 (mol / mol).

32. The process of any one of claims 1 to 31, wherein the ratio of sodium methoxide to polyethylene terephthalate (PET) is 1:10 to 1:15 (mol / mol).

33. The process of any one of claims 1 to 32, wherein the dimethyl terephthalate is obtained in a yield of at least 90 mol%.

34. The process of any one of claims 1 to 32, wherein the dimethyl terephthalate is obtained in a yield of at least 95 mol%.

35. The process of any one of claims 1 to 32, wherein the dimethyl terephthalate is obtained in a yield of at least 99 mol%.

36. 36. The process of any one of claims 1 to 35, wherein the monoethylene glycol is obtained in a yield of at least 80 mol %.

37. 36. The process of any one of claims 1 to 35, wherein the monoethylene glycol is obtained in a yield of at least 85 mol %.

38. 36. The process of any one of claims 1 to 35, wherein the monoethylene glycol is obtained in a yield of at least 90 mol %.

39. The process of any one of claims 1 to 38, wherein the feedstock containing the polyethylene terephthalate (PET) is supplied in particulate form.

40. 40. The process of claim 39, wherein the average particle size is from 0.1 mm to 20 mm.

41. 41. The process of claim 39 or 40, wherein the average particle size is from 5 mm to 10 mm.

42. The process according to any one of claims 39 to 41, wherein the average particle size is up to 6 mm.

43. The process according to any one of claims 39 to 41, wherein the average particle size is up to 8 mm.

Citation Information

Patent Citations

  • FR01081681A1

  • Monomerization of polyethylene terephthalate

    JP2000072720A

  • METHOD FOR PRODUCING BIS-beta-HYDROXYETHYL TEREPHTHALATE

    JP2003055300A

  • Cosmetic

    JP2008063305A

  • Method for producing polyester monomer from polyester

    JP2012116779A