Graphite dispersion and positive electrode composition using same

The graphite dispersion liquid with polyvinyl acetal improves dispersibility and reduces viscosity, addressing uneven distribution issues in lithium-ion batteries, enhancing cycle and self-discharge characteristics.

JP7583780B2Active Publication Date: 2024-11-14MITSUBISHI PENCIL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022195821
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-12-07
Publication Date
2024-11-14
Estimated Expiration
2042-12-07

AI Technical Summary

Technical Problem

Existing graphite dispersions for lithium-ion batteries have high viscosity, leading to poor yield and uneven distribution of conductive agents and active materials, which affects cycle characteristics, self-discharge characteristics, and electrode resistance.

Method used

A graphite dispersion liquid containing graphite, a solvent, and polyvinyl acetal with specific peak intensity ratios, which reduces viscosity and enhances dispersibility, allowing uniform distribution of conductive agents and active materials.

Benefits of technology

The solution achieves low viscosity for uniform distribution, maintaining high cycle and self-discharge characteristics without affecting electrode resistance, suitable for high-efficiency lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583780000001
    Figure 0007583780000001
  • Figure 0007583780000002
    Figure 0007583780000002
  • Figure 0007583780000003
    Figure 0007583780000003
Patent Text Reader

Abstract

To provide a graphite dispersion liquid which is desirably used for an electrode for a positive electrode such as a lithium ion secondary battery, and a material for a lithium ion battery positive electrode.SOLUTION: A graphite dispersion liquid includes graphite, a solvent, and polyvinyl acetal expressed by the following expression (I). The ratio of the peak intensity when the FT-IR spectrum obtained by an ATR technique of polyvinyl acetal is 2950 cm-1 to the peak intensity when the FT-IR spectrum is 1650 cm-1 is at least 50 and the mass average molecule amount measured by gel permeation chromatography is 100,000 at most. (In the expression, each of l, m, and n is a positive value, and R is an alkyl group with 1-20 carbons.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a graphite dispersion liquid suitably used for an electrode for a positive electrode such as a lithium ion secondary battery, and a composition for a positive electrode electrode using the same.

Background Art

[0002] In recent years, with the spread of electronic devices and mobility considering environmental aspects, the lithium ion battery market has attracted attention. A lithium ion battery includes a negative electrode containing an active material that reversibly allows lithium ions to enter and exit, a positive electrode, and a non-aqueous electrolyte that immerses them. The positive electrode is manufactured by coating an electrode slurry composed of an active material, a conductive material, and a binder on a current collector such as an aluminum foil.

[0003] Conventionally, the use of a high specific surface area carbon material, particularly graphite (graphite particles), in non-aqueous secondary batteries including lithium ion batteries has been studied. In particular, it is known to form an intercalation compound in graphite and use the intercalation compound as a secondary battery electrode material, and many techniques have been disclosed.

[0004] For example, Patent Document 1 describes "a secondary battery having a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte, wherein a non-carbonaceous material is used as an active material of the positive electrode, and the BET specific surface area A (m / g) of the active material of the negative electrode is in the range of 0.1 < A < 100, and the values of the crystal thickness Lc (Å) and the true density ρ (g / cm in X-ray diffraction 3 ) satisfy the conditions 1.80 < ρ < 2.18, 15 < Lc and 120ρ - 227 < Lc < 120ρ - 189, and a secondary battery using a carbonaceous material in this range." This Patent Document 1 further discloses Li + ​It is described that when ions and the like are to be taken in, the carbonaceous material has better properties if it has a certain degree of disordered structure, and further, it is described that if the surface area of ​​the carbon material is small, it is difficult for the electrochemical reaction to proceed smoothly on the electrode surface, which is undesirable, and that if the specific surface area is too large, deterioration in characteristics such as cycle life characteristics, self-discharge characteristics, and current efficiency characteristics is observed, which is undesirable.

[0004] Furthermore, Patent Document 2 describes a conductive additive, which has a particle thickness of 0.5 nm to 30 nm and a specific surface area of ​​50 m 2 / g or more, a carbon material other than the flake graphite, a dispersant, a binder, etc.

[0005] Patent Document 3 also describes a conductive agent for electrodes of lithium ion batteries, which (1) has a band intensity ratio of a Raman spectrum measured by Raman spectroscopy using an argon laser that satisfies the following relationship: G band (1580 cm -1 ) Intensity / D band (1360cm -1 ) intensity] ≥ 8, and (2) the G band (1580 cm ) of the Raman spectrum measured by Raman spectroscopy using an argon laser is satisfied. -1 ) half width (G-FWHM) is 15 to 22 cm -1 The document discloses a conductive agent characterized by containing exfoliated graphite having the following characteristics, and it is disclosed that the thickness of the basal plane of the exfoliated graphite particles, as measured by a field emission scanning electron microscope (FE-SEM), is preferably 5 to 50 nm. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Publication No. 4-24831 (claims, examples, etc.) [Patent Document 2] JP 2014-182873 A (claims, examples, etc.) [Patent Document 3] International Publication No. 2021 / 107094 (Claims, Examples, etc.) Summary of the Invention [Problem to be solved by the invention]

[0007] However, all of the carbonaceous materials and flaky graphite still have high viscosities, which means that the yields in the manufacturing processes of graphite dispersions and electrode compositions (electrode dispersions) are insufficient, and the pressure loss during liquid transport is large, making it difficult to increase the solid content. It is stated that the exfoliated graphite in Patent Document 2 preferably does not have reactive functional groups. In this case, adsorption of a dispersant becomes difficult when dispersing the graphite in various solvents, including water, making it impossible to achieve a low viscosity. In fact, the composition described here is a "paste" and is presumed to be a composition with extremely high viscosity. Normally, when a high-viscosity "paste" is used, adding a conductive agent or active material, such as carbon nanotubes, to the paste later does not cause a problem of the already high viscosity increasing further. However, the current situation is that it becomes difficult to uniformly disperse the conductive agent and active material when coating the paste to form an electrode, which can adversely affect cycle characteristics, self-discharge characteristics, and the resistance value of the electrode itself. In addition, the fluidity in the coating machine piping and coating section is still insufficient, so the current collector foil Defects in the electrode occur due to improper application of the electrode dispersion to the electrode, resulting in insufficient electrode adhesion. In some cases, the yield could not be achieved.

[0008] Therefore, the present invention provides a novel graphite dispersion having good dispersibility and also provides a method for dispersing Li +The present invention aims to provide a positive electrode composition that can uniformly disperse exfoliated graphite without adversely affecting the transfer of ions such as ions or the reduction in the resistance value of the electrode, and that can uniformly distribute a conductive agent and an active material when applied to form an electrode using a dispersion with low viscosity, while maintaining high cycle characteristics and self-discharge characteristics and without adversely affecting the resistance value of the electrode itself, and that is suitable as a material for the positive electrode of a lithium ion battery such as a highly efficient lithium ion battery. [Means for solving the problem]

[0009] As a result of extensive research, the present inventors have found that the above problems can be solved by the following means. That is, the present invention is as follows: <Aspect 1> The graphite dispersion of the present invention contains at least graphite, a solvent, and a polyvinyl acetal represented by the following formula (I), and the polyvinyl acetal has a peak at 1650 cm in an FT-IR spectrum obtained by an ATR method. -1 Peak intensity at 2950cm -1 The ratio of the peak intensities at the peaks is 50 or more. [ka] (In the formula, l, m, and n are positive numbers, and R is an alkyl group having 1 to 20 carbon atoms.) <Aspect 2> 2. The graphite dispersion according to claim 1, wherein a 10% by mass solution of the polyvinyl acetal in NMP has an absorbance at 320 nm of 0.50 or more. <Aspect 3> 3. The graphite dispersion according to claim 1, wherein a 10 mass % solution of the polyvinyl acetal in NMP has a viscosity of 21.0 mPa·s or more and 31.0 mPa·s or less at a shear rate of 76.6 / s. <Aspect 4> 3. The graphite dispersion according to claim 1, wherein the polyvinyl acetal has a mass average molecular weight of 100,000 or less. <Aspect 5> The positive electrode composition of the present invention is characterized by containing at least the graphite dispersion liquid according to aspect 1 or 2 and a positive electrode active material, and the mass of the graphite is 0.1 to 6.0 parts by mass per 100 parts by mass of the positive electrode active material. [Effects of the Invention]

[0010] According to the present invention, Li + The present invention provides a graphite dispersion that uniformly disperses graphite without adversely affecting the transfer of ions such as ions or the reduction in the resistance value of the electrode, and that has a low viscosity, allowing a conductive agent and an active material to be uniformly distributed when the dispersion is applied to form an electrode, and that does not adversely affect the resistance value of the electrode itself while maintaining high cycle characteristics and self-discharge characteristics. This graphite dispersion is suitable for producing battery electrodes for highly efficient lithium ion batteries and the like, and in particular is suitable for use in positive electrodes for lithium ion secondary batteries and the like, and a positive electrode composition that can be suitably used in lithium ion batteries and the like using the same. The objects and advantages of the invention will be realized and attained by means of the elements and combinations particularly pointed out in the claims. Both the foregoing general description and the following detailed description are exemplary and explanatory and are not restrictive of the invention as claimed. DETAILED DESCRIPTION OF THE INVENTION

[0011] The following describes in detail the embodiments of the present invention. However, please note that the technical scope of the present invention is not limited to the embodiments described in detail below, but extends to the inventions set forth in the claims and their equivalents. Furthermore, the present invention can be implemented based on the contents disclosed in this specification and common general technical knowledge in the relevant field (including design matters and obvious matters).

[0012] <Graphite dispersion> The graphite dispersion of the present invention contains at least graphite, a solvent, and a polyvinyl acetal represented by the following formula (I), and has a peak at 1650 cm in an FT-IR (Fourier transform infrared spectroscopy) spectrum of the polyvinyl acetal obtained by attenuated total reflection (ATR) measurement method. -1 Peak intensity at 2950cm -1 The ratio of the peak intensities is 50 or more.

[0013] [ka] (In the formula, l, m, and n are positive numbers, and R is an alkyl group having 1 to 20 carbon atoms.)

[0014] In this specification, "2950 cm -1 The peak near 2950 cm -1 200cm in front and behind -1 , front and rear 150cm -1 , front and rear 100cm -1 , front and back 50cm -1 , or 30cm -1 It means the largest peak in the region of 3450 cm. -1 "Peaks near 1650cm" and "1650cm -1 Regarding the "peak in the vicinity of 2950 cm" -1 "A peak in the vicinity of the X-Y (mass % or μm, etc.)" should be interpreted in the same way as "a peak in the vicinity of the X-Y (mass % or μm, etc.)." Furthermore, "X to Y (mass % or μm, etc.)" means "X (mass % or μm, etc.) or more and Y (mass % or μm, etc.) or less." In the present invention, the attenuated total reflectance (ATR) method was performed using diamond as the crystal, and using a sample that had been dried for three days in an environment with a dew point temperature of minus 30°C before measurement.

[0015] Each component of the present invention will be described below. Graphite The graphite (graphite particles) used in the present invention may have at least one shape or characteristic selected from the group consisting of scaly, flaky, spherical, expanded, flaked, flaked scaly, and graphene (obtained by chemical vapor deposition, pyrolysis, mechanical exfoliation, chemical treatment, etc.) (either alone or in combination; the same applies hereinafter). These shapes and characteristics may overlap, e.g., flaked scaly graphite.

[0016] Examples of commercially available scaly graphite that can be used include SP-270, J-SP-α, JB-5 (all manufactured by Nippon Graphite Co., Ltd.), FT-7J (manufactured by Fuji Graphite Co., Ltd.), and NOCSP. Examples of commercially available flake graphite that can be used include CMX-40, JSP-α, UP-5α, UP-10-α, UP-5N, and UP-50N (all manufactured by Nippon Graphite Co., Ltd.). Examples of commercially available spherical graphite include CGB-6, CGB-6R, CGB-20, and CGC-50 (all manufactured by Nippon Graphite Co., Ltd.). Examples of commercially available expanded graphite that can be used include FS-5 (manufactured by Higashi Nippon Carbon Co., Ltd.). In the present invention, it is particularly preferable to use scaly graphite or exfoliated expanded graphite, since this can reduce the sheet resistance of the positive electrode material to which the graphite dispersion is added.

[0017] There is no problem if the average particle size of the graphite used in the above shape is 2 to 50 μm from the beginning, but even if it is larger than this, for example, by being pulverized in the dispersion step, the average particle size after dispersion will be 2 to 50 μm, more preferably 3 to 30 μm, even more preferably 4 to 20 μm, and even more preferably 5 to 10 μm, which will be preferable properties for a dispersion liquid for battery electrodes, etc.

[0018] The average particle size used herein is selected appropriately depending on the size of the graphite in question. For graphite less than approximately 1 μm, it is the histogram average particle size (D50) value based on the scattering intensity distribution measured by dynamic light scattering. For particles 1 μm or larger, it is the median diameter (D50) value calculated on a volume basis by laser diffraction. Measurement by dynamic light scattering can be performed, for example, using a DelsaMax CORE (Beckman Coulter). Measurement by laser diffraction can be performed, for example, using a particle size distribution analyzer MT3300II (Microtrack Bell Corporation). This average particle size of graphite refers to secondary particles formed by stacking or spherical aggregation of flake graphite particles, and can be measured by suspending the graphite in any solution.

[0019] The content of these graphites can be set to a suitable content depending on the application, and is not particularly limited. For example, when used in an electrode composition such as a conductive slurry, an electrode slurry for a secondary battery, or an electrode (positive electrode) for a secondary battery, the content thereof may be 0.1 mass % or more, 0.2 mass % or more, 0.4 mass % or more, 0.6 mass % or more, or 0.8 mass % or more, relative to the total mass of the graphite dispersion, in terms of exerting the effects of the present invention, achieving both high stability and conductive performance, and viscosity during dispersion production. The content may also be 20 mass % or less, 15 mass % or less, 10 mass % or less, or 8 mass % or less.

[0020] <solvent> As the solvent, any organic solvent can be used, for example, a protic polar solvent or an aprotic polar solvent. These solvents can be used alone or in combination.

[0021] The protic polar liquid medium is generally a solvent containing acidic hydrogen, and examples of the protic polar liquid medium include phenol-based liquid media, monohydric alcohol-based liquid media, and polyhydric alcohol-based liquid media.

[0022] As the phenol-based liquid medium, for example, cresols can be used. Examples of monohydric alcohol liquid media that can be used include ethanol, n-propanol, isopropanol, n-butanol, isobutanol, tert-butyl alcohol, 1-pentanol, isamyl alcohol, sec-amyl alcohol, 3-pentanol, tert-amyl alcohol, and n-hexanol.

[0023] Examples of polyhydric alcohol liquid media that can be used include glycol liquid media such as propylene glycol, triethylene glycol, tetraethylene glycol, diglyme, and polyethylene glycol having a molecular weight of 600 or less, and glycerin.

[0024] The aprotic polar liquid medium is generally a solvent that does not contain acidic hydrogen. Examples of the aprotic polar liquid medium include N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone. The use of rolidone is preferred from the viewpoint of its affinity with polyvinyl acetal.

[0025] <Polyvinyl acetal> The polyvinyl acetal in the graphite dispersion of the present invention is comprised of the following formula: [ka] (In the formula, l, m, and n are positive numbers, and R is an alkyl group having 1 to 20 carbon atoms.)

[0026] The polyvinyl acetal of the present invention has a peak at 1650 cm measured by FT-IR. -1 Intensity of the peak near 2950 cm -1 The ratio of the peak intensities at This ratio may be 50 or greater, 55 or greater, 60 or greater, 65 or greater, 70 or greater, 75 or greater, 80 or greater, 85 or greater, 90 or greater, 95 or greater, or 100 or greater.

[0027] I don't want to be bound by theory, but this 1650cm -1 The intensity of the peak at 2950 cm increases due to the proportion of acetyl groups, i.e., the value of m in the above formula (1). -1 The intensity of the peak at is considered to be high due to the ratio of the sum of the acetal group and the acetyl group, i.e., the sum of the values ​​of - and m in the above formula (1). Therefore, the ratio of the intensities of the above peaks is considered to indicate that the proportion of the acetal group is relatively high. The FT-IR (Fourier transform infrared spectroscopy) spectrum of this polyvinyl acetal obtained by attenuated total reflectance (ATR) measurement was at 1650 cm -1 Peak intensity at 2950cm -1 If the ratio of the peak intensities is less than 50, the effect of the present invention will not be exhibited, which is not preferable.

[0028] In addition, the polyvinyl acetal of the present invention has a peak at 3400 cm measured by FT-IR. -1 Intensity of the peak at 2950 cm -1 The ratio of the intensities of the peaks at 3400 cm to 3400 cm may preferably be 2.0 or more, 2.5 or more, or 3.0 or more. -1 The intensity of the peak at is considered to be high due to the proportion of hydroxyl groups, i.e., the value of n in the above formula (1). Therefore, a high intensity ratio is considered to indicate a relatively high proportion of acetal groups.

[0029] It is believed that the relatively large proportion of acetal groups makes the polyvinyl acetal as a whole more hydrophobic, thereby resulting in a high affinity for graphite. As a result, the graphite dispersion can be easily dispersed at low shear rates, e.g., 0.1 s.l.s.-1 The viscosity at the time of the reaction can be reduced.

[0030] The graphite dispersion of the present invention having such polyvinyl acetal, 0.1 s -1 Viscosity at 1000s -1 is preferably 1000 or less, 900 or less, 800 or less, 700 or less, 600 or less, or 550 or less.

[0031] Here, in measuring the viscosity ratio above, the shear rate is set to 0.1 s -1 Viscosity at 0.1 s -1 From the 1000s -1 The shear rate was then changed logarithmically from 1000 s-1 to 0.1 s-1 over 20 seconds, and the viscosity was measured over a total of 40 seconds. The viscosity at 20 seconds was measured at a shear rate of 1000 s-1. -1 The viscosity was measured at 40 seconds and the shear rate was 0.1 s -1 The viscosity was measured.

[0032] The content of the acetal group in the polyvinyl acetal of the present invention may be 70% by mass or more, 75% by mass or more, 80% by mass or more, 81% by mass or more, 82% by mass or more, or 83% by mass or more, based on the mass of the polyvinyl acetal.

[0033] The number of carbon atoms in the alkyl group constituting R in the above formula (1) is not particularly limited, but may be 1 or more, 3 or more, 5 or more, 7 or more, or 9 or more, and may be 20 or less, 18 or less, 16 or less, 14 or less, or 12 or less. In particular, the polyvinyl acetal in the present invention is The alkyl group constituting the R may be polyvinyl butyral having 4 carbon atoms. stomach.

[0034] The absorbance at 320 nm of a 10% by mass NMP solution of polyvinyl acetal in the present invention From the viewpoints of the viscosity and stability over time of the dispersion, the absorbance may be preferably 0.25 or more, 0.30 or more, 0.35 or more, 0.40 or more, 0.45 or more, 0.50 or more, 0.55 or more, 0.60 or more, or 0.65 or more, with 0.50 or more being preferred from the viewpoint of improving dispersibility. The absorbance may be 0.90 or less, 0.85 or less, 0.80 or less, 0.75 or less, or 0.70 or less. In measuring the absorbance, the absorbance of NMP is used as a blank.

[0035] The viscosity of a 10 mass % NMP solution of the polyvinyl acetal of the present invention at a shear rate of 76.6 mPa·s may be 10.0 mPa·s or more, 15.0 mPa·s or more, 20.0 mPa·s or more, or 21.0 mPa·s or more, or may be 70.0 mPa·s or less, 65 mPa·s or less, 60.0 mPa·s or less, 55.0 mPa·s or less, 50 mPa·s, 45.0 mPa·s or less, 40.0 mPa·s or less, 35.0 mPa·s or less, 33.0 mPa·s or less, 3.0 mPa·s or less, or 30.0 mPa·s or less. This viscosity can be measured using a cone-plate viscometer for a measurement time of 60 seconds.

[0036] The weight-average molecular weight of the polyvinyl acetal of the present invention, as measured by gel permeation chromatography, is preferably 100,000 or less to further enhance the effects of the present invention. This weight-average molecular weight may be 90,000 or less, 85,000 or less, 80,000 or less, 75,000 or less, 70,000 or less, 65,000 or less, 60,000 or less, 55,000 or less, or 50,000 or less. Such a weight-average molecular weight reduces the viscosity of the polyvinyl acetal solution, thereby suppressing aggregation of the resulting graphite. This weight-average molecular weight may be 10,000 or more, 15,000 or more, 20,000 or more, 25,000 or more, 30,000 or more, 35,000 or more, or 40,000 or more. The weight-average molecular weight obtained by gel permeation chromatography is a converted value obtained using polystyrene as the standard polymer.

[0037] The polyvinyl acetal content may be 0.1% by mass or more, 0.3% by mass or more, 0.5% by mass or more, 0.7% by mass or more, or 0.9% by mass or more, and may be 10.0% by mass or less, 8.0% by mass or less, 5.0% by mass or less, 3.0% by mass or less, 2.7% by mass or less, 2.4% by mass or less, 2.1% by mass or less, 1.8% by mass or less, or 1.5% by mass or less, based on the total mass of the graphite dispersion.

[0038] <Other polymers> Polymers other than polyvinyl acetal can be used, for example, as binders. Polymers can be used. Examples of such polymers include various emulsion-type or solution-type polymers, such as fluorine-based polymers such as polyvinylidene fluoride (PVdF), tetrafluoroethylene-hexafluoropropylene polymer (FEP), tetrafluoroethylene-perfluoroalkyl vinyl ether polymer (PFA), and polytetrafluoroethylene (PTFE), elastomer-based polymers such as ethylene-propylene-diene copolymer (EPDM), nitrile-butadiene rubber (NBR), and styrene-butadiene rubber (SBR), and acrylic polymers.

[0039] The polymer may be a natural polymer such as a polysaccharide or a synthetic polymer, and may be used as a thickener.

[0040] Examples of polysaccharides that can be used include gum arabic, tragacanth gum, guar gum, locust bean gum, alginic acid, carrageenan, gelatin, xanthan gum, welan gum, succinoglycan, diutan gum, dextran, methylcellulose, ethylcellulose, hydroxyethylcellulose, carboxymethylcellulose, starch glycolic acid, and salts thereof. Of these, carboxymethylcellulose is preferred from the viewpoint of dispersion stability.

[0041] Examples of synthetic polymers that can be used include water-soluble resins such as polyvinylpyrrolidone, polyvinyl methyl ether, polyacrylic acid and its salts, polyethylene oxide, vinyl acetate-polyvinylpyrrolidone copolymer, styrene-acrylic acid copolymer and its salts, and isobutylene-maleic anhydride copolymer and its salts.

[0042] As the polymer, for example, nonionic dispersants such as polyalkylene oxides, polyvinyl ethers, chitins, chitosans, starch, etc. These polymers may be used as dispersing aids.

[0043] The polymer may be a dispersant. Examples of the polymer that can be used include nonionic or anionic dispersants and polysaccharides. Examples of the nonionic dispersant that can be used include the above-mentioned dispersing aids or polyvinylpyrrolidone. Examples of the anionic dispersant that can be used include acrylic resins such as styrene-acrylic resins, urethane resins, polyester resins, polyvinyl chloride resins, and epoxy resins.

[0044] The total content of other polymers may be 0.5% by weight or more, 1.0% by weight or more, 1.5% by weight or more, 2.0% by weight or more, or 2.2% by weight or more, and may be 15.0% by weight or less, 12.0% by weight or less, 10.0% by weight or less, 8.0% by weight or less, 6.0% by weight or less, 5.0% by weight or less, 4.5% by weight or less, 4.0% by weight or less, 3.5% by weight or less, 3.0% by weight or less, or 2.5% by weight or less, based on the total weight of the graphite dispersion.

[0045] <Proton concentration regulator> As the optional proton concentration adjuster, for example, at least one of ammonia, urea, monoethanolamine, diethanolamine, triethanolamine, aminomethylpropanol, alkali metal salts of carbonate or phosphoric acid such as sodium tripophosphate or sodium carbonate, and alkali metal hydroxides such as sodium hydroxide can be used.

[0046] <Preservatives> As optional preservatives, at least one of phenol, sodium omadine, sodium pentachlorophenol, 1,2-benzisothiazolin-3-one, 2,3,5,6-tetrachloro-4(methylphenyl)pyridine, alkali metal salts of benzoic acid, sorbic acid or dehydroacetic acid, benzimidazole compounds, alcohols such as phenoxyethanol, glycols such as 1,3-pentanediol, etc. can be used.

[0047] The graphite dispersion of the present invention can be produced, for example, by adding at least the graphite, a solvent, the optional components that are added as needed, and the polyvinyl acetal having the specific physical properties represented by formula (I) as the balance (remaining components), followed by stirring and mixing, and then carrying out a dispersing step. The dispersion treatment of the above-mentioned dispersion liquid can be carried out using, for example, an ultrasonic disperser, mixers such as a disperser, a homomixer, a rotation-revolution mixer, a Henschel mixer, or a planetary mixer, a (high-pressure) homogenizer, a paint conditioner, colloid mills, media-type dispersers such as a bead mill, a cone mill, a ball mill, a sand mill, an attritor, a pearl mill, or a Coball mill, media-less dispersers such as a wet jet mill or a thin film rotary high-speed mixer, or other dispersing devices such as a roll mill, but is not limited to these. Preferable dispersing devices include a (high-pressure) homogenizer, a thin film rotary high-speed mixer, a bead mill, etc., from the viewpoint of stability and dispersion efficiency.

[0048] The graphite dispersion of the present invention thus constituted contains at least graphite, a solvent, and the polyvinyl acetal represented by the above formula (I), and has a peak at 1650 cm in the FT-IR spectrum of the polyvinyl acetal obtained by the ATR method. -1 Peak intensity at 2950cm -1 By using a peak intensity ratio of 50 or more, Li +The graphite dispersion can be uniformly dispersed without adversely affecting the transfer of ions such as ions or the decrease in the resistance value of the electrode, and the low viscosity of the dispersion allows the conductive agent and active material to be uniformly distributed when the dispersion is applied to form an electrode, and furthermore, the graphite dispersion can be obtained which is suitable for producing battery electrodes for highly efficient lithium ion batteries and the like, without adversely affecting the resistance value of the electrode itself, while maintaining high cycle characteristics and self-discharge characteristics.

[0049] 《Positive electrode composition》 The positive electrode composition of the present invention contains at least the graphite dispersion and a positive electrode active material, and is characterized in that the mass of the graphite is 0.1 parts by mass or more and 6 parts by mass or less per 100 parts by mass of the positive electrode active material. The positive electrode composition of the present invention, which contains the graphite dispersion of the present invention having good dispersibility, can achieve good sheet resistance, capacity retention rate, and cycle retention rate.

[0050] In the positive electrode composition of the present invention, the mass of graphite per 100 parts by mass of the positive electrode active material is 0.1 parts by mass or more, 0.3 parts by mass or more, 0.5 parts by mass or more, 0.7 parts by mass or more, or 0.9 parts by mass or more, and is 6.0 parts by mass or less, 5.5 parts by mass or less, 5.0 parts by mass or less, 4.5 parts by mass or less, 4.0 parts by mass or less, 3.5 parts by mass or less, 3.0 parts by mass or less, 2.5 parts by mass or less, 2.0 parts by mass or less, or 1.7 parts by mass or less.

[0051] The positive electrode composition may contain a polymer other than polyvinyl acetal, such as those mentioned above for the carbon nanotube dispersion.

[0052] The positive electrode composition may further contain a solvent, and the solvents mentioned above for the graphite dispersion may be used.

[0053] The positive electrode composition may also contain other conductive materials, such as carbon-based conductive materials other than graphite. The conductive material may be, for example, a carbon-based conductive material, such as at least one selected from carbon fibers, carbon particles, and carbon nanotubes.

[0054] Examples of carbon fibers include, but are not limited to, milled fibers and chopped fibers, which may be used alone or in combination. The average length of the carbon fibers can be 1 μm or more, 3 μm or more, 5 μm or more, 10 μm or more, or 15 μm or more, and can be 100 μm or less, 70 μm or less, 50 μm or less, or 30 μm or less.

[0055] Examples of carbon particles include carbon black such as acetylene black and ketjen black, which may be used alone or in combination. The shape of the carbon particles is not particularly limited, and may be, for example, flat, array-like, spherical, or the like.

[0056] The average particle size of carbon particles can be 100 nm or more, 200 nm or more, 300 nm or more, 500 nm or more, 700 nm or more, 1 μm or more, 2 μm or more, or 3 μm or more, and can be 20 μm or less, 15 μm or less, 10 μm or less, or 7 μm or less. The average particle size used herein is appropriately selected depending on the size of the target carbon particles. For particles less than approximately 1 μm, it is the histogram mean particle size (D50) value based on the scattering intensity distribution measured by dynamic light scattering. For particles 1 μm or larger, it is the median diameter (D50) value calculated on a volume basis by laser diffraction. Measurement by dynamic light scattering can be performed, for example, using a DelsaMax CORE (Beckman Coulter, Inc.). Measurement by laser diffraction can be performed, for example, using a particle size distribution analyzer MT330011 (Microtrac BELL Corporation).

[0057] The content of the carbonaceous conductive material in the positive electrode composition (electrode layer-forming non-aqueous dispersion) may be 1.0 mass % or more, 1.5 mass % or more, 2.0 mass % or more, or 2.5 mass % or more, based on the total mass of the composition (electrode layer-forming non-aqueous dispersion), and may be 15.0 mass % or less, 12.0 mass % or less, 10.0 mass % or less, 8.0 mass % or less, 6.0 mass % or less, 5.0 mass % or less, 4.5 mass % or less, 4.0 mass % or less, 3.5 mass % or less, or 3.0 mass % or less.

[0058] Known carbon nanotubes can be used as carbon nanotubes. The average particle diameter of carbon nanotubes can be 100 nm or more, 200 nm or more, 300 nm or more, 500 nm or more, 700 nm or more, 1 μm or more, 2 μm or more, or 3 μm or more, and can be 20 μm or less, 15 μm or less, 10 μm or less, or 7 μm or less. Here, the average particle diameter used in this specification is appropriately selected depending on the size of the carbon nanotubes in question. For particles less than approximately 1 μm, it is the histogram mean particle diameter (D50) value based on the scattering intensity distribution measured by dynamic light scattering. For particles 1 nm or larger, it is the median diameter (D50) value calculated on a volume basis by laser diffraction. Measurement by dynamic light scattering can be performed, for example, using a DelsaMax CORE (Beckman Coulter, Inc.). Measurement by laser diffraction can be performed, for example, using a particle size distribution analyzer MT300011 (Microtrac BELL Corporation). The average particle diameter of carbon nanotubes refers to secondary particles formed by single carbon nanotube fibers forming bundles or strands, and can be measured by suspending the carbon nanotubes in any solution.

[0059] Examples of the positive electrode active material include metal compounds such as metal oxides and metal sulfides that can be doped or intercalated with lithium ions, and conductive polymers. Examples include oxides of transition metals such as Fe, Co, Ni, and Mn, composite oxides with lithium, and inorganic compounds such as transition metal sulfides. Specific examples include MnO, VO, and VO. 13 , transition metal oxide powders such as TiO2, layered lithium nickel oxide, lithium cobalt oxide, lithium manganate, spinel-structured lithium manganate, ternary lithium materials (NCM), such as LiNiO 0.8 Co 0.1 Mn 0.1Examples of such materials include composite oxide powders of lithium and transition metals such as O2, lithium iron phosphate materials, which are phosphate compounds with an olivine structure, and transition metal sulfide powders such as TiS2 and FeS. Conductive polymers such as polyaniline, polyacetylene, polypyrrole, and polythiophene can also be used. Mixtures of the above inorganic and organic compounds may also be used.

[0060] The content of the positive electrode active material may be 40% by mass or more, 45% by mass or more, 50% by mass or more, 53% by mass or more, or 55% by mass or more, and may be 80% by mass or less, 75% by mass or less, or 70% by mass or less, relative to the mass of the positive electrode composition.

[0061] The positive electrode composition suitable for lithium ion batteries and the like configured as described above contains the graphite dispersion described above, and by setting the mass of graphite to be 0.1 parts by mass or more and 6 parts by mass or less per 100 parts by mass of the positive electrode active material, the active material can be uniformly distributed, and the cycle characteristics and self-discharge characteristics are maintained at a high level without adversely affecting the resistance value of the electrode itself, etc., and a positive electrode composition suitable for lithium ion battery positive electrode dispersions, which are suitable for producing battery electrodes for highly efficient lithium ion batteries and the like, can be obtained. [Example]

[0062] The present invention will be specifically explained by means of Production Examples, Examples and Comparative Examples, but the present invention is not limited to these.

[0063] <<Production Examples 1 to 9: Preparation of Graphite Dispersion>> (Production Example 1) A graphite dispersion (total amount: 100% by mass) of Example 1 was prepared by dispersing 6.0 parts by mass of graphite (UP-5N, manufactured by Nippon Graphite Co., Ltd.), 3.0 parts by mass of polyvinyl butyral A (PVB-A), and 91.0 parts by mass of N-methyl-2-pyrrolidone as a solvent using a high-pressure homogenizer (dispersion pressure: 100 MPa, 10 passes).

[0064] <Production Examples 2 to 9> In Production Example 2, a graphite dispersion of Production Example 2 was prepared in the same manner as Production Example 1, except that the graphite was replaced with 6.0 parts by mass of another graphite (CGB-6R, manufactured by Nippon Graphite Co., Ltd.). In Production Examples 3 to 9, graphite dispersions were prepared in the same manner as Production Example 1, except that the same amounts of each dispersant shown in Table 1 below were used instead of PVB-A. PVB-B, PVB-C, PVB-D, PVB-E, PVB-F, PVB-G: Polyvinyl butyral, VP: Polyvinylpyrrolidone

[0065] The estimated proportions of functional groups in PVB-B and PVB-F are as follows: PVB-B: Polyvinyl butyral containing 83% butyral by mass, 3% acetyl by mass, and 14% vinyl alcohol by mass PVB-F: Polyvinyl butyral containing 78% butyral by mass, 3% acetyl by mass, and 19% vinyl alcohol by mass

[0066] <Evaluation of each physical property of dispersants> <FT-IR intensity> For each PVB, the FT-IR spectrum was measured and the -1 Near 2950cm -1 Around 1650cm -1 The peak intensity values ​​around the peak were obtained, and the predetermined intensity ratio was calculated based on these values. The measurement was performed using the ATR method and a diamond crystal. In addition, each PVB was dried for three days in an environment with a dew point temperature of minus 30°C before measurement.

[0067] <Absorbance and Viscosity> A 10% by mass solution of each dispersant in N-methylpyrrolidone was prepared, and the absorbance of this solution was measured at 320 nm, with the absorbance of N-methylpyrrolidone used as a blank. The viscosity of this solution was measured using a cone-plate viscometer at a shear rate of 76.6 / s for a measurement time of 60 seconds.

[0068] <Mass average molecular weight> The weight average molecular weight of each dispersant was measured by gel permeation chromatography. The weight average molecular weight was determined by converting the weight average molecular weight to polystyrene as a standard polymer.

[0069] <Evaluation of the physical properties of graphite dispersions: Viscosity> Each of the prepared graphite dispersions and the dispersions for positive electrodes obtained using the same in the following Examples and Comparative Examples were measured using a rheometer (Anton Paar Co., Ltd. Modular Compact Rheometer MCR102, diameter 50 mm, 2° cone) at a sample temperature of 25°C and a shear rate of 0.1 s -1 and 1000s -1 The viscosity at each point was measured. Shear rate 0.1s -1 From the 1000s -1 The shear rate was then changed to 1000 s using a logarithmic ramp over 20 s. -1 to 0.1 seconds -1 The viscosity was measured over a total of 40 seconds by changing the shear rate to 1000 s with a logarithmic gradient over 20 seconds. -1 The viscosity was measured at 40 seconds and the shear rate was 0.1 s -1 The viscosity was measured at 1000 kJ / min. The stability over time is 0.1s after 7 days at 25°C from the time of production. -1 Viscosity, and 1000s -1 The viscosity of each dispersion was measured at 0.1 s. -1 Viscosity, and 1000s -1 The value obtained by dividing the value by the viscosity was defined as the viscosity ratio over time, and the stability over time was evaluated according to the following evaluation criteria. Evaluation criteria: ◎: 0.1s -1 Viscosity ratio over time and 1000s -1 The viscosity ratio over time is 0.7 to 1.3. ○: 0.1s -1 viscosity ratio over time or 1000s -1 Either the viscosity ratio over time is less than 0.7 or greater than 1.3. △:0.1s -1 Viscosity ratio over time or 1000s-1 The viscosity ratio over time is either less than 0.7 or greater than 1.3.

[0070] [Table 1]

[0071] *1 to *2 in Table 1 above are as follows. *1: UP-5N (average particle size: 5 μm, manufactured by Nippon Graphite Co., Ltd.) *2: CGB-6R (average particle size: 6 μm, manufactured by Nippon Graphite Co., Ltd.)

[0072] As is clear from the results in Table 1 above, when Production Examples 1 to 4 are compared with Production Examples 5 to 9, the graphite dispersions of Production Examples 1 to 4 have a 0.1s -1 Viscosity / 1000s -1 Since the viscosity ratio was kept low, it was confirmed that the graphite was uniformly dispersed, and that there was little increase or decrease in the viscosity ratio over time, making this a graphite dispersion with excellent stability.

[0073] (Examples 1 to 4 and Comparative Examples 1 to 5: Positive Electrode Compositions) Each of the graphite dispersions obtained in Production Examples 1 to 9 was dispersed using a planetary mixer according to the blending compositions shown in Table 2 below, to prepare a dispersion for a positive electrode, which would serve as a composition (material) for a positive electrode. The obtained dispersion for positive electrode, which becomes each of the positive electrode compositions, was measured by the same viscosity measurement method as for the graphite dispersion described above. -1 and 1000s -1 The viscosity and viscosity ratio at each time point were measured. Furthermore, the coating stability, electrode sheet resistance (KΩ / □), capacity retention rate after 10 C discharge (%), and capacity retention rate after 100 cycles were measured using the following evaluation methods. The evaluation results are shown in Table 2 below.

[0074] <Method for evaluating coating stability> The resulting positive electrode dispersion was applied to aluminum foil at a wet film thickness of 100 μm using a comma coater with a coating width of 200 mm. Streaks that appeared on the resulting coating film and were 10 mm or longer were evaluated according to the following criteria. When multiple streaks appeared, the total length of each streak was used as the standard. Evaluation criteria: ◎: No streaks longer than 10 mm were present. ○: The total length of the muscle was 10 mm or more and less than 50 mm. △: The total length of the muscle was 50 mm or more and less than 100 mm. ×: The total length of the muscle was 100 mm or more.

[0075] <Electrode sheet resistance> The obtained positive electrode dispersion was applied to one side of a PET film (Lumira #100-T60, manufactured by Toray Industries, Inc.) with an applicator so that the liquid film was 50 μm thick, and then dried at room temperature for 30 minutes, followed by further drying at 80° C. for 5 minutes to obtain an electrode layer. The sheet resistance of the produced electrode layer was measured using an apparatus consisting of a four-point probe with a probe spacing of 10 mm and a Milliohm HiTester 3227 (manufactured by Hioki E.E. Corporation).

[0076] <Capacity retention rate after 10C charge / discharge> The obtained dispersion for positive electrode was applied to aluminum foil with a wet film thickness of 100 μm using a comma coater with a coating width of 200 mm, and dried in a drying oven at 100°C for 5 minutes to prepare five coin secondary batteries. The capacity retention rate after 10C charge / discharge was evaluated by calculating the average value of five coin secondary batteries using the formula "B / A x 100" from the capacity (A) and the discharge capacity (B) when subsequently charged / discharged at a charge / discharge rate of 10 CI.

[0077] In this coin secondary battery, a carbonate-based solvent was used as the electrolyte, a polypropylene separator was used, and metallic lithium was used as the counter electrode. <100 cycle maintenance rate> Five coin secondary batteries were fabricated under the same conditions as above, and the initial discharge capacity (A) and the 100th discharge capacity (B) after 100 charge / discharge cycles at 1C were calculated using the formula: The 100 cycle retention rate was evaluated according to the following criteria by calculating the average value of five coin secondary batteries using the formula "B / A x 100". Evaluation criteria: ◎: 98% or more ○: 95% or more to less than 98% △: 85% to less than 95% ×: Less than 85%

[0078] [Table 2]

[0079] As is clear from the results in Table 2 above, the positive electrode compositions using the graphite dispersions of Examples 1 to 4, which are within the scope of the present invention, were found to have better coating stability, electrode sheet resistance, capacity retention rate, and cycle retention rate than the positive electrode compositions using the graphite dispersions of Comparative Examples 1 to 5, which are outside the scope of the present invention. [Industrial Applicability]

[0080] The graphite dispersion and the positive electrode composition using the same are excellent in stability and conductivity, and are particularly suitable for producing electrodes for lithium-ion secondary batteries and the like. They can be suitably used for producing positive electrodes and can achieve excellent battery performance that can withstand repeated charge and discharge over a long period of time.

Claims

1. The polyvinyl acetal contains at least graphite, a solvent, and a polyvinyl acetal represented by the following formula (I), and has a peak at 1650 cm in the FT-IR spectrum obtained by the ATR method of the polyvinyl acetal. -1 Peak intensity at 2950 cm -1 and a mass average molecular weight measured by gel permeation chromatography of 100,000 or less. [Formula 1] (In the formula, l, m, and n are positive numbers, and R is an alkyl group having 1 to 20 carbon atoms.)

2. 2. The graphite dispersion for a positive electrode according to claim 1, wherein a 10 mass % solution of the polyvinyl acetal in NMP has an absorbance at 320 nm of 0.50 or more.

3. 3. The graphite dispersion for a positive electrode according to claim 1, wherein a 10 mass % solution of the polyvinyl acetal in NMP has a viscosity of 21.0 mPa·s or more and 31.0 mPa·s or less at a shear rate of 76.6 / s.

4. 3. The graphite dispersion for a positive electrode according to claim 1, wherein the polyvinyl acetal has a mass average molecular weight Mw of 30,000 to 50,000.

5. 3. A positive electrode composition comprising at least the graphite dispersion liquid for a positive electrode according to claim 1 or 2 and a positive electrode active material, wherein a mass of the graphite is 0.1 to 6.0 parts by mass per 100 parts by mass of the positive electrode active material.

Citation Information

Patent Citations

  • Test device

    JP1992024831A

  • Carbon black dispersion

    JP2011184664A

  • Nonaqueous secondary battery electrode-forming material, nonaqueous secondary battery electrode, and nonaqueous secondary battery

    JP2014182873A

  • Binder for power storage device electrode