Metallic pipe for oil well and method for manufacturing the same

A resin-coated metal pipe for oil wells with copper phthalocyanine enhances torque-on-shoulder resistance and seizure resistance, addressing environmental concerns while ensuring high torque performance, particularly for large diameters.

JP7583817B2Active Publication Date: 2024-11-14NIPPON STEEL CORPORATION +2
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2022543940
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-20
Filing Date
2021-08-16
Publication Date
2024-11-14
Estimated Expiration
2041-08-16

AI Technical Summary

Technical Problem

Existing metal pipes for oil wells face challenges in maintaining high torque performance, especially for large diameters, due to issues with torque-on-shoulder resistance, and conventional solutions using compound grease with heavy metal powders pose environmental concerns.

Method used

A metal pipe for oil wells with a resin coating containing resin, solid lubricating powder, and copper phthalocyanine applied on the pin and box contact surfaces, enhancing torque-on-shoulder resistance and seizure resistance without using heavy metal powders.

Benefits of technology

The resin coating with copper phthalocyanine improves high torque performance, allowing large-diameter oil well metal pipes to be fastened securely and reduces environmental impact by eliminating the need for heavy metal-containing compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583817000008
    Figure 0007583817000008
  • Figure 0007583817000009
    Figure 0007583817000009
  • Figure 0007583817000010
    Figure 0007583817000010
Patent Text Reader

Abstract

A metal pipe for an oil well according to the present disclosure can be fastened with a high torque even when the metal pipe has a large diameter. A metal pipe (1) for an oil well according to the present disclosure comprises a pipe main body (10) including a first end portion (10A) and a second end portion (10B). The pipe main body (10) includes a pin (40) formed to the first end portion (10A) and a box (50) formed to the second end portion (10B). The pin (40) includes a pin contact surface (400) including a male screw portion (41), and the box (50) includes a box contact surface (500) including a female screw portion (51). The metal pipe (1) for an oil well according to the present disclosure further comprises a resin film (100) containing a resin, a solid lubricant powder, and copper phthalocyanine on at least one of the pin contact surface (400) and the box contact surface (500).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a metallic oil well pipe and a method for manufacturing the metallic oil well pipe. [Background technology]

[0002] Metallic oil well pipes are used for the mining of oil fields and natural gas fields (hereinafter, oil fields and natural gas fields are also collectively referred to as "oil wells"). Metallic oil well pipes have threaded joints. Specifically, at an oil well mining site, a plurality of metallic oil well pipes are connected to form an oil well pipe connection, typically casing or tubing. An oil well pipe connection is formed by screwing metallic oil well pipes together. Inspection may be performed on the oil well pipe connection. When inspection is performed, the oil well pipe connection is pulled up and unscrewed. Then, the metallic oil well pipe is removed from the oil well pipe connection by unscrewing, and inspected. After inspection, the metallic oil well pipes are screwed together again, and reused as part of the oil well pipe connection.

[0003] The metal oil well pipe includes a pin and a box. The pin has a pin contact surface including a male thread portion on the outer peripheral surface of the end of the metal oil well pipe. The box has a box contact surface including a female thread portion on the inner peripheral surface of the end of the metal oil well pipe. In this specification, the male thread portion and the female thread portion are collectively referred to as "thread portion". The pin contact surface may further include a pin unthreaded metal contact portion including a pin seal surface and a pin shoulder surface. Similarly, the box contact surface may further include a box unthreaded metal contact portion including a box seal surface and a box shoulder surface.

[0004] When a metal pipe for oil well use is screwed and unscrewed, the pin contact surface and the box contact surface are repeatedly subjected to strong friction. Therefore, the pin contact surface and the box contact surface are prone to galling (irreparable seizure) when screwed and unscrewed repeatedly. Therefore, metal pipe for oil well use is required to have sufficient durability against friction, i.e., excellent seizure resistance.

[0005] Conventionally, compound grease containing heavy metal powder, called dope, has been used to improve the seizure resistance of oil well metal pipes. The seizure resistance of oil well metal pipes can be improved by applying compound grease to the pin contact surface and / or box contact surface. However, the heavy metal powders such as Pb, Zn, and Cu contained in the compound grease may have an adverse effect on the environment. For this reason, there is a demand for the development of oil well metal pipes that have excellent seizure resistance without using compound grease.

[0006] Techniques for improving the seizure resistance of metal pipes for oil wells have been proposed, for example, in WO 2014 / 042144 (Patent Document 1) and WO 2017 / 047722 (Patent Document 2).

[0007] The composition disclosed in Patent Document 1 is a composition for forming a solid coating on the surface of a threaded joint of a metal pipe for oil wells. The composition is a composition in which a powdered organic resin that is at least partially soluble in a dipolar aprotic solvent is contained in a mixed solvent containing water and a dipolar aprotic solvent. In the composition, the powdered organic resin exists in a dissolved or dispersed state in the mixed solvent.

[0008] The composition disclosed in Patent Document 2 is a composition for forming a solid lubricant coating on threaded joints of metal pipes for oil wells. The composition contains a binder, a lubricant additive, a rust inhibitor, and a plasticizer. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. 2014 / 042144 [Patent Document 2] International Publication No. 2017 / 047722 Summary of the Invention [Problem to be solved by the invention]

[0010] Meanwhile, various sizes (diameters) of oil well metal pipes are used. Therefore, it is desirable that the fastening between the oil well metal pipes is difficult to loosen, regardless of the size of the oil well metal pipes. Here, a high fastening torque is set in advance for the large-diameter oil well metal pipes so that the fastened oil well metal pipes do not loosen.

[0011] When a large-diameter metal pipe for oil wells is fastened with a high torque, it is desirable that the high-torque performance is high. High high-torque performance means that the torque-on-shoulder resistance is large. The torque-on-shoulder resistance means the difference between the yield torque at which a part of the metal pipe for oil wells yields and the shouldering torque at which the interference between the metal pipes for oil wells increases rapidly. On the other hand, even if the techniques disclosed in Patent Document 1 and Patent Document 2 are used, there are cases where the torque-on-shoulder resistance is small. In this case, it is difficult to fasten a large-diameter metal pipe for oil wells with a high torque.

[0012] An object of the present disclosure is to provide a metal oil well pipe that can be fastened with a high torque even if it has a large diameter, and a manufacturing method for the metal oil well pipe. [Means for solving the problem]

[0013] The metal pipe for oil well use according to the present disclosure comprises: a tube body including a first end and a second end; The tube body includes: A pin formed on the first end; a box formed at the second end; The pin is a pin contact surface including an external thread; The box includes: a box contact surface including an internal thread; The oil well metal pipe further comprises: At least one of the pin contact surface and the box contact surface is provided with a resin coating containing resin, solid lubricant powder, and copper phthalocyanine.

[0014] The method for producing a metal pipe for oil well according to the present disclosure includes the steps of: providing a metal oil well pipe comprising a pipe body including a pin including a pin contact surface including a male thread portion and a box including a box contact surface including a female thread portion; applying a composition containing a resin, a solid lubricant powder, and copper phthalocyanine onto at least one of the pin contact surface and the box contact surface; and a step of curing the applied composition to form a resin coating. Effect of the Invention

[0015] The metal pipe for oil well use according to the present disclosure can be fastened with a high torque even if it has a large diameter. The manufacturing method of the metal pipe for oil well use according to the present disclosure can manufacture the above-mentioned metal pipe for oil well use. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a diagram showing the relationship between the rotation speed and torque of a metal oil well pipe having a shoulder portion when the metal oil well pipe is fastened. [Figure 2A] FIG. 2A is a graph showing the relationship between the content of phthalocyanine copper in a resin coating and high torque performance. [Figure 2B] FIG. 2B is a partially enlarged view of the diagram showing the relationship between the content of phthalocyanine copper in the resin coating shown in FIG. 2A and high torque performance. [Diagram 3] FIG. 3 is a configuration diagram showing an example of the metallic oil well pipe according to this embodiment. [Figure 4] FIG. 4 is a partial cross-sectional view showing a cross section (longitudinal cross section) parallel to the pipe axial direction of the coupling for the metal pipe for oil well shown in FIG. [Diagram 5] FIG. 5 is a cross-sectional view of a portion of the metallic pipe for oil well use shown in FIG. 4 in the vicinity of a pin, taken along a line parallel to the axial direction of the metallic pipe for oil well use. [Figure 6] FIG. 6 is a cross-sectional view of a portion of the metallic pipe for oil well use shown in FIG. 4 in the vicinity of the box, taken along a line parallel to the axial direction of the metallic pipe for oil well use. [Figure 7]FIG. 7 is a partial cross-sectional view showing a cross section (longitudinal cross section) parallel to the pipe axis direction of a coupling for a metal pipe for oil wells according to this embodiment, which is different from FIG. [Figure 8] FIG. 8 is a configuration diagram of an integral type metal oil well pipe according to this embodiment. [Figure 9] FIG. 9 is an enlarged view of the pin contact surface shown in FIG. [Figure 10] FIG. 10 is an enlarged view of the box contact surface shown in FIG. [Figure 11] FIG. 11 is an enlarged view of the pin contact surface according to this embodiment, which is different from FIG. [Figure 12] FIG. 12 is an enlarged view of the pin contact surface according to this embodiment, which is different from FIGS. [Figure 13] FIG. 13 is an enlarged view of the pin contact surface according to this embodiment, which is different from FIGS. [Figure 14] FIG. 14 is a diagram showing the relationship between the plating layer, the content of copper phthalocyanine, and the result of a Bowden test, which is an index of seizure resistance. [Figure 15] FIG. 15 is an enlarged view of the box contact surface according to this embodiment, which is different from FIG. [Figure 16] FIG. 16 is an enlarged view of the pin contact surface according to this embodiment, which is different from FIGS. [Figure 17] FIG. 17 is an enlarged view of the pin contact surface according to this embodiment, which is different from FIGS. 9, 11, 12, 13 and 16. [Figure 18] FIG. 18 is an enlarged view of the pin contact surface according to this embodiment, which is different from FIGS. 9, 11, 12, 13, 16 and 17. [Figure 19] FIG. 19 is a diagram for explaining the torque-on-shoulder resistance ΔT in the example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, the present embodiment will be described in detail with reference to the drawings. In the drawings, the same or corresponding parts are designated by the same reference characters and their description will not be repeated.

[0018] The present inventors have conducted various studies on the relationship between a metal oil well pipe and a make-up torque, and have obtained the following findings.

[0019] [High torque performance] When metal pipes for oil wells are fastened together, an optimal torque for completing the fastening is determined in advance. FIG. 1 is a diagram showing the relationship between the rotation speed of the metal pipe for oil wells and the torque when the metal pipe for oil wells having a shoulder portion is fastened. Referring to FIG. 1, when the metal pipe for oil wells is screwed, the torque increases gradually in proportion to the rotation speed at first. When the screw is further tightened, the shoulder portions come into contact with each other. The torque at this time is called shouldering torque Ts. After the shouldering torque Ts is reached, when the screw is further tightened, the torque increases rapidly in proportion to the rotation speed. When the torque reaches a predetermined value (fastening torque To), the fastening is completed. At the fastening torque To, the metal seal portions interfere with each other with an appropriate surface pressure. In this case, the metal pipe for oil wells can obtain high airtightness. When the screw is further tightened excessively after the fastening torque To is reached, the torque reaches the yield torque Ty, and the pin and the box partially yield. In this specification, the difference between the shouldering torque Ts and the yield torque Ty is referred to as the torque-on-shoulder resistance ΔT.

[0020] Another type of oil well metal pipe is one that has no shoulder and has a wedge thread. In the case of such an oil well metal pipe with a wedge thread, the relationship between the rotation speed and torque of the oil well metal pipe is as shown in Figure 1, similar to the case of the oil well metal pipe with a shoulder.

[0021] Here, the wedge thread refers to a thread having the following structure. In the male thread of the wedge thread, the width of the thread gradually narrows along the helical winding of the thread as the pin is screwed in, and the width of the thread groove gradually widens along the helical winding of the thread. Furthermore, in the female thread of the wedge thread, the width of the thread groove gradually narrows along the helical winding of the thread as the box is screwed in, and the width of the thread gradually widens along the helical winding of the thread. In the case of a metal oil well pipe having a wedge thread, as the screw is tightened, the load flank surfaces of the male thread and the female thread come into contact with each other, and the stab flank surfaces come into contact with each other, causing locking (interference fit). The torque at which locking occurs is also called locking torque or locked flank torque.

[0022] In this specification, unless otherwise specified, there is no distinction between the locking torque and the shouldering torque, and they are referred to as the shouldering torque Ts. In the case of a metal oil well pipe having a wedge thread, as in the case of a metal oil well pipe having a shoulder portion, if the threads are further tightened after the shouldering torque Ts is reached, the torque increases rapidly in proportion to the rotation speed. In other words, at the shouldering torque Ts, the interference between the metal oil well pipes increases rapidly. If the threads are further tightened, the make-up torque To is reached. If the threads are further tightened excessively after the make-up torque To is reached, the yield torque Ty is reached and parts of the pin and the box yield.

[0023] As described above, a high tightening torque To is set for a large-diameter metal pipe for oil wells. However, when the tightening torque To is set high, a part of the pin and the box may yield before the tightening torque To is reached, causing plastic deformation. If the torque-on-shoulder resistance ΔT is large, the screw can be further tightened after the shouldering torque Ts is reached. Therefore, if the torque-on-shoulder resistance ΔT is large, even a large-diameter metal pipe for oil wells can be tightened with a high torque. In this case, the metal pipe for oil wells is less likely to loosen. Here, in this specification, high high torque performance means that the torque-on-shoulder resistance ΔT is large. In this specification, a large-diameter metal pipe for oil wells means a metal pipe for oil wells having an outer diameter of 254 mm (10 inches) or more.

[0024] In order to increase the torque-on-shoulder resistance ΔT, it is effective to reduce the shouldering torque Ts or increase the yield torque Ty. However, it is generally known that the shouldering torque Ts and the yield torque Ty behave in a similar manner. For example, if the friction coefficient of the surface of the metal pipe for oil wells is reduced in order to reduce the shouldering torque Ts, not only the shouldering torque Ts but also the yield torque Ty will decrease. In this case, a part of the pin or box may yield before the fastening torque To is reached. Also, if the friction coefficient of the surface of the metal pipe for oil wells is increased in order to increase the yield torque Ty, not only the yield torque Ty but also the shouldering torque Ts will increase. In this case, the shoulder portion may not come into contact even when the fastening torque To is reached.

[0025] Compared with ordinary to small diameter metal pipes for oil wells, large diameter metal pipes for oil wells are required to have higher high torque performance. Therefore, the present inventors have studied a method for improving the high torque performance even of large diameter metal pipes for oil wells. As a result, the following findings have been obtained.

[0026] Fig. 2A is a diagram showing the relationship between the content of phthalocyanine copper in the resin coating and high torque performance. Fig. 2A was obtained from the results of Example 1 described later. In Example 1, a so-called large-diameter (outer diameter 273.05 mm (10.75 inches), wall thickness: 12.570 mm (0.495 inches)) oil well metal pipe was used.

[0027] The horizontal axis of FIG. 2A indicates the content (mass%) of phthalocyanine copper in the resin coating. The vertical axis of FIG. 2A indicates torque-on-shoulder resistance ΔT. Torque-on-shoulder resistance ΔT is a relative value compared to the torque-on-shoulder resistance ΔT when using a dope specified in API (American Petroleum Institute) standard Bull 5A2 (1998), which is set at 100. In FIG. 2A, a white circle (◯) indicates that phthalocyanine copper was contained in the resin coating, and a black circle (●) indicates that phthalocyanine copper was not contained in the resin coating.

[0028] 2A, when the resin coating contains phthalocyanine copper, the torque-on-shoulder resistance ΔT is increased compared to when the resin coating does not contain phthalocyanine copper. In other words, when the resin coating contains phthalocyanine copper, the high torque performance is improved. In this case, even a large-diameter metal pipe for oil wells can be fastened with a high torque.

[0029] Fig. 2B is a partially enlarged view of the relationship between the content of phthalocyanine copper in the resin coating and the high torque performance. With reference to Fig. 2B, if the content of phthalocyanine copper in the resin coating is adjusted to 0.2 mass% or more, the high torque performance of the metal pipe for oil well use is further improved.

[0030] The metallic oil well pipe according to the present embodiment, which has been completed based on the above findings, and the method for manufacturing the metallic oil well pipe are outlined below.

[0031] [1] A metal pipe for oil wells, comprising: a tube body including a first end and a second end; The tube body includes: A pin formed on the first end; a box formed at the second end; The pin is a pin contact surface including an external thread; The box includes: a box contact surface including an internal thread; The oil well metal pipe further comprises: a resin coating containing a resin, a solid lubricant powder, and phthalocyanine copper on at least one of the pin contact surface and the box contact surface; Metal pipes for oil wells.

[0032] The metal pipe for oil wells according to the present embodiment has a resin coating containing phthalocyanine copper. Therefore, even if the metal pipe for oil wells has a large diameter, it can be fastened with a high torque. The metal pipe for oil wells according to the present embodiment can also be applied to metal pipes for oil wells of normal to small diameters. The metal pipe for oil wells according to the present embodiment can be fastened with a necessary and sufficient torque even when applied to metal pipes for oil wells of normal to small diameters.

[0033] [2] The metal pipe for oil well use according to [1], The resin coating is Contains 0.2 to 30.0% by mass of phthalocyanine copper; Metal pipes for oil wells.

[0034] In this case, the high torque performance of the metal oil well pipe is further improved.

[0035] [3] The metal pipe for oil well use according to [2], The resin coating is 0.2 to 30.0 mass% of phthalocyanine copper; 60 to 90% by mass of the resin; and 1 to 30 mass % of the solid lubricant powder. Metal pipes for oil wells.

[0036] [4] The metal pipe for oil well use according to [2] or [3], The resin coating is Contains 0.2 to 9.0% by mass of phthalocyanine copper; Metal pipes for oil wells.

[0037] In this case, the metal oil well pipe has high resistance to seizure in addition to high torque performance.

[0038] [5] The metal pipe for oil well use according to any one of [1] to [4], further comprising: a plating layer is provided between the resin coating and at least one of the pin contact surface and the box contact surface; Metal pipes for oil wells.

[0039] [6] The metal pipe for oil well use according to any one of [1] to [4], further comprising: a chemical conversion coating is provided between at least one of the pin contact surface and the box contact surface and the resin coating; Metal pipes for oil wells.

[0040] [7] The metal pipe for oil well use according to [5], further comprising: A chemical conversion coating is provided between the plating layer and the resin coating. Metal pipes for oil wells.

[0041] [8] The metal pipe for oil well use according to any one of [1] to [7], The resin coating further comprises: Contains anti-rust pigments, Metal pipes for oil wells.

[0042] [9] The metal pipe for oil well use according to any one of [1] to [8], At least one of the pin contact surface and the box contact surface is a surface that has been subjected to one or more treatments selected from the group consisting of blast treatment and pickling. Metal pipes for oil wells.

[0043]

[10] The metal pipe for oil well use according to any one of [1] to [9], The resin is At least one resin selected from the group consisting of epoxy resin, phenol resin, acrylic resin, urethane resin, polyester resin, polyamideimide resin, polyamide resin, polyimide resin, and polyetheretherketone resin. Metal pipes for oil wells.

[0044]

[11] The metal pipe for oil well use according to any one of [1] to

[10] , The solid lubricant powder is At least one selected from the group consisting of graphite, zinc oxide, boron nitride, talc, molybdenum disulfide, tungsten disulfide, graphite fluoride, tin sulfide, bismuth sulfide, organic molybdenum, a thiosulfate compound, and polytetrafluoroethylene; Metal pipes for oil wells.

[0045]

[12] [1] -

[11] The metal pipe for oil well use according to any one of the above, The pin contact surface further includes a pin seal surface and a pin shoulder surface. The box contact surface further includes a box seal surface and a box shoulder surface. Metal pipes for oil wells.

[0046]

[13] A method for producing a metal pipe for oil well use according to the present invention, comprising the steps of: providing a metal oil well pipe comprising a pipe body including a pin including a pin contact surface including a male thread portion and a box including a box contact surface including a female thread portion; applying a composition containing a resin, a solid lubricant powder, and copper phthalocyanine onto at least one of the pin contact surface and the box contact surface; and curing the applied composition to form a resin coating. A manufacturing method for metal pipes for oil wells.

[0047] The metallic oil well pipe according to this embodiment will be described in detail below.

[0048] [Configuration of metal pipe for oil wells] First, the configuration of the metal pipe for oil well use of the present embodiment will be described. The metal pipe for oil well use has a well-known configuration. There are T&C type metal pipe for oil well use and integral type metal pipe for oil well use. Each type of metal pipe for oil well use will be described in detail below.

[0049] [When the oil well metal pipe 1 is T&C type] Fig. 3 is a configuration diagram showing an example of a metal pipe for oil well use 1 according to the present embodiment. Fig. 3 is a configuration diagram of a so-called T&C (Threaded and Coupled) metal pipe for oil well use 1. Referring to Fig. 3, the metal pipe for oil well use 1 includes a pipe main body 10.

[0050] The pipe body 10 extends in the pipe axis direction. A cross section of the pipe body 10 perpendicular to the pipe axis direction is circular. The pipe body 10 includes a first end 10A and a second end 10B. The first end 10A is the end opposite to the second end 10B. In the T&C type metal pipe for oil wells 1 shown in FIG. 3, the pipe body 10 includes a pin pipe body 11 and a coupling 12. The coupling 12 is attached to one end of the pin pipe body 11. More specifically, the coupling 12 is fastened to one end of the pin pipe body 11 by a screw.

[0051] Fig. 4 is a partial cross-sectional view showing a cross section (longitudinal cross section) parallel to the pipe axis direction of the coupling 12 of the metal pipe for oil well use 1 shown in Fig. 3. With reference to Figs. 3 and 4, the pipe body 10 includes a pin 40 and a box 50. The pin 40 is formed at a first end portion 10A of the pipe body 10. When fastening, the pin 40 is inserted into a box 50 of another metal pipe for oil well use 1 (not shown) and fastened to the box 50 of the other metal pipe for oil well use 1 by a screw.

[0052] The box 50 is formed at the second end 10B of the pipe body 10. During fastening, the pin 40 of another metal pipe for oil well use 1 is inserted into the box 50, and fastened to the pin 40 of the other metal pipe for oil well use 1 by a screw.

[0053] [About the configuration of pin 40] Fig. 5 is a cross-sectional view parallel to the pipe axis direction of the metal pipe for oil wells 1, showing a portion near the pin 40 of the metal pipe for oil wells 1 shown in Fig. 4. The dashed line portion in Fig. 5 shows the configuration of a box 50 of another metal pipe for oil wells 1 when fastening to another metal pipe for oil wells 1. Referring to Fig. 5, the pin 40 has a pin contact surface 400 on the outer circumferential surface of the first end 10A of the pipe body 10. When fastening to another metal pipe for oil wells 1, the pin contact surface 400 is screwed into the box 50 of the other metal pipe for oil wells 1, and comes into contact with a box contact surface 500 (described later) of the box 50.

[0054] The pin contact surface 400 includes at least the male thread portion 41 formed on the outer circumferential surface of the first end portion 10A. The pin contact surface 400 may further include a pin seal surface 42 and a pin shoulder surface 43. In FIG. 5, the pin shoulder surface 43 is disposed on the tip surface of the first end portion 10A, and the pin seal surface 42 is disposed on the outer circumferential surface of the first end portion 10A, closer to the tip side of the first end portion 10A than the male thread portion 41. That is, the pin seal surface 42 is disposed between the male thread portion 41 and the pin shoulder surface 43. The pin seal surface 42 is provided in a tapered shape. Specifically, the outer diameter of the pin seal surface 42 gradually decreases from the male thread portion 41 toward the pin shoulder surface 43 in the longitudinal direction (pipe axis direction) of the first end portion 10A.

[0055] When fastening with another metal pipe for oil wells 1, the pin seal surface 42 comes into contact with a box seal surface 52 (described later) of a box 50 of the other metal pipe for oil wells 1. More specifically, when fastening, the pin 40 is inserted into the box 50 of the other metal pipe for oil wells 1, so that the pin seal surface 42 comes into contact with the box seal surface 52. Then, when the pin 40 is further screwed into the box 50 of the other metal pipe for oil wells 1, the pin seal surface 42 comes into close contact with the box seal surface 52. As a result, when fastening, the pin seal surface 42 comes into close contact with the box seal surface 52 to form a seal based on metal-metal contact. Therefore, the airtightness of the metal pipes for oil wells 1 fastened to each other can be improved.

[0056] In FIG. 5, the pin shoulder surface 43 is disposed on the tip surface of the first end portion 10A. That is, in the pin 40 shown in FIG. 5, the male thread portion 41, the pin seal surface 42, and the pin shoulder surface 43 are disposed in this order from the center of the pipe body 10 toward the first end portion 10A. When fastening with another metal pipe for oil wells 1, the pin shoulder surface 43 faces and contacts a box shoulder surface 53 (described later) of a box 50 of the other metal pipe for oil wells 1. More specifically, when fastening, the pin 40 is inserted into the box 50 of the other metal pipe for oil wells 1, so that the pin shoulder surface 43 contacts the box shoulder surface 53. This allows a high torque to be obtained when fastening. Also, the positional relationship between the pin 40 and the box 50 in the fastened state can be stabilized.

[0057] It should be noted that the pin contact surface 400 of the pin 40 includes at least the male thread portion 41. In other words, the pin contact surface 400 may include the male thread portion 41, and not include the pin seal surface 42 and the pin shoulder surface 43. The pin contact surface 400 may include the male thread portion 41 and the pin shoulder surface 43, and not include the pin seal surface 42. The pin contact surface 400 may include the male thread portion 41 and the pin seal surface 42, and not include the pin shoulder surface 43.

[0058] [About the composition of Box 50] Fig. 6 is a cross-sectional view parallel to the pipe axis direction of the metal pipe for oil wells 1, showing a portion near the box 50 of the metal pipe for oil wells 1 shown in Fig. 4. The dashed line portion in Fig. 6 shows the configuration of the pin 40 of another metal pipe for oil wells 1 when fastening to another metal pipe for oil wells 1. Referring to Fig. 6, the box 50 has a box contact surface 500 on the inner peripheral surface of the second end portion 10B of the pipe body 10. When fastening to another metal pipe for oil wells 1, the pin 40 of the other metal pipe for oil wells 1 is screwed into the box contact surface 500, and the box contact surface 500 comes into contact with the pin contact surface 400 of the pin 40.

[0059] The box contact surface 500 includes at least a female thread portion 51 formed on the inner circumferential surface of the second end portion 10B. During fastening, the female thread portion 51 meshes with the male thread portion 41 of the pin 40 of another metal pipe for oil well 1.

[0060] The box contact surface 500 may further include a box seal surface 52 and a box shoulder surface 53. In FIG. 6, the box seal surface 52 is disposed on the inner circumferential surface of the second end portion 10B closer to the pipe body 10 than the female thread portion 51. That is, the box seal surface 52 is disposed between the female thread portion 51 and the box shoulder surface 53. The box seal surface 52 is tapered. Specifically, the inner diameter of the box seal surface 52 gradually decreases from the female thread portion 51 toward the box shoulder surface 53 in the longitudinal direction (pipe axial direction) of the second end portion 10B.

[0061] When fastening with another metal pipe for oil wells 1, the box seal surface 52 comes into contact with the pin seal surface 42 of the pin 40 of the other metal pipe for oil wells 1. More specifically, when fastening, the pin 40 of the other metal pipe for oil wells 1 is screwed into the box 50, so that the box seal surface 52 comes into contact with the pin seal surface 42, and when further screwed, the box seal surface 52 comes into close contact with the pin seal surface 42. As a result, when fastening, the box seal surface 52 comes into close contact with the pin seal surface 42 to form a seal based on metal-metal contact. Therefore, the airtightness of the metal pipes for oil wells 1 fastened to each other can be improved.

[0062] The box shoulder surface 53 is disposed closer to the pipe body 10 than the box seal surface 52. That is, in the box 50, the box shoulder surface 53, the box seal surface 52, and the female thread portion 51 are disposed in this order from the center of the pipe body 10 toward the tip of the second end 10B. When fastening with another metal pipe for oil wells 1, the box shoulder surface 53 faces and contacts the pin shoulder surface 43 of the pin 40 of the other metal pipe for oil wells 1. More specifically, when fastening, the pin 40 of the other metal pipe for oil wells 1 is inserted into the box 50, so that the box shoulder surface 53 contacts the pin shoulder surface 43. This allows a high torque to be obtained when fastening. Also, the positional relationship between the pin 40 and the box 50 in the fastened state can be stabilized.

[0063] The box contact surface 500 includes at least an internal thread portion 51. During fastening, the internal thread portion 51 of the box contact surface 500 of the box 50 corresponds to and contacts the external thread portion 41 of the pin contact surface 400 of the pin 40. The box seal surface 52 corresponds to and contacts the pin seal surface 42. The box shoulder surface 53 corresponds to and contacts the pin shoulder surface 43.

[0064] When the pin contact surface 400 includes the male threads 41 and does not include the pin seal surface 42 and the pin shoulder surface 43, the box contact surface 500 includes the female threads 51 and does not include the box seal surface 52 and the box shoulder surface 53. When the pin contact surface 400 includes the male threads 41 and the pin shoulder surface 43 and does not include the pin seal surface 42, the box contact surface 500 includes the female threads 51 and the box shoulder surface 53 and does not include the box seal surface 52. When the pin contact surface 400 includes the male threads 41 and the pin seal surface 42 and does not include the pin shoulder surface 43, the box contact surface 500 includes the female threads 51 and the box seal surface 52 and does not include the box shoulder surface 53.

[0065] The pin contact surface 400 may include a plurality of male thread portions 41, a plurality of pin seal surfaces 42, or a plurality of pin shoulder surfaces 43. For example, in the pin contact surface 400 of the pin 40, the pin shoulder surface 43, the pin seal surface 42, the male thread portion 41, the pin seal surface 42, the pin shoulder surface 43, the pin seal surface 42, and the male thread portion 41 may be arranged in this order from the tip of the first end portion 10A toward the center of the pipe body 10. In this case, in the box contact surface 500 of the box 50, the female thread portion 51, the box seal surface 52, the box shoulder surface 53, the box seal surface 52, the female thread portion 51, the box seal surface 52, and the box shoulder surface 53 are arranged in this order from the tip of the second end portion 10B toward the center of the pipe body 10.

[0066] 5 and 6 show a so-called premium joint in which the pin 40 includes the male thread portion 41, the pin seal surface 42, and the pin shoulder surface 43, and the box 50 includes the female thread portion 51, the box seal surface 52, and the box shoulder surface 53. However, as described above, the pin 40 may include the male thread portion 41 and not include the pin seal surface 42 and the pin shoulder surface 43. In this case, the box 50 includes the female thread portion 51, but not the box seal surface 52 and the box shoulder surface 53. FIG. 7 shows an example of a metal pipe for oil well 1 in which the pin 40 includes the male thread portion 41, but not the pin seal surface 42 and the pin shoulder surface 43, and the box 50 includes the female thread portion 51, but not the box seal surface 52 and the box shoulder surface 53.

[0067] [When the oil well metal pipe 1 is an integral type] The metal pipe for oil well use 1 shown in Figures 3, 4 and 7 is a so-called T&C type metal pipe for oil well use 1 in which a pipe body 10 includes a pin pipe body 11 and a coupling 12. However, the metal pipe for oil well use 1 of the present embodiment may be an integral type instead of a T&C type.

[0068] FIG. 8 is a configuration diagram of an integral type metal pipe for oil wells 1 according to this embodiment. Referring to FIG. 8, the integral type metal pipe for oil wells 1 includes a pipe body 10. The pipe body 10 includes a first end 10A and a second end 10B. The first end 10A is disposed on the opposite side to the second end 10B. As described above, in the T&C type metal pipe for oil wells 1, the pipe body 10 includes a pin pipe body 11 and a coupling 12. That is, in the T&C type metal pipe for oil wells 1, the pipe body 10 is configured by fastening two separate members (the pin pipe body 11 and the coupling 12). In contrast, in the integral type metal pipe for oil wells 1, the pipe body 10 is integrally formed.

[0069] The pin 40 is formed at a first end 10A of the pipe body 10. When fastening, the pin 40 is inserted into and screwed into a box 50 of another integral type metal pipe for oil wells 1, and is fastened to the box 50 of the other integral type metal pipe for oil wells 1. The box 50 is formed at a second end 10B of the pipe body 10. When fastening, the pin 40 of the other integral type metal pipe for oil wells 1 is inserted into and screwed into the box 50, and is fastened to the pin 40 of the other integral type metal pipe for oil wells 1.

[0070] The configuration of the pin 40 of the integral type metal pipe for oil wells 1 is the same as that of the pin 40 of the T&C type metal pipe for oil wells 1 shown in FIG. 5. Similarly, the configuration of the box 50 of the integral type metal pipe for oil wells 1 is the same as that of the box 50 of the T&C type metal pipe for oil wells 1 shown in FIG. 6. In FIG. 8, the pin shoulder surface 43, the pin seal surface 42, and the male thread portion 41 are arranged in this order from the tip of the first end 10A toward the center of the pipe body 10 in the pin 40. Therefore, in the box 50, the female thread portion 51, the box seal surface 52, and the box shoulder surface 53 are arranged in this order from the tip of the second end 10B toward the center of the pipe body 10. However, like the pin contact surface 400 of the pin 40 of the T&C type metal pipe for oil wells 1, the pin contact surface 400 of the pin 40 of the integral type metal pipe for oil wells 1 only needs to include at least the male thread portion 41. Similarly to the box contact surface 500 of the box 50 of the T&C type metal pipe for oil wells 1, the box contact surface 500 of the box 50 of the integral type metal pipe for oil wells 1 may include at least the female thread portion 51.

[0071] In short, the metal oil well pipe 1 of the present embodiment may be of the T&C type or the integral type.

[0072] [Resin coating] The metal pipe for oil well use 1 according to the present embodiment is provided with a resin coating 100 on at least one of the pin contact surface 400 and the box contact surface 500. FIG. 9 is an enlarged view of the pin contact surface 400 shown in FIG. 5. FIG. 10 is an enlarged view of the box contact surface 500 shown in FIG. 6. As shown in FIGS. 9 and 10, the metal pipe for oil well use 1 according to the present embodiment may be provided with the resin coating 100 on both the pin contact surface 400 and the box contact surface 500. However, the metal pipe for oil well use 1 according to the present embodiment may be provided with the resin coating 100 on only one of the pin contact surface 400 or the box contact surface 500. For example, as shown in FIG. 9, when the resin coating 100 is provided on the pin contact surface 400, the resin coating 100 may not be provided on the box contact surface 500. Also, as shown in FIG. 10, when the resin coating 100 is provided on the box contact surface 500, the resin coating 100 may not be provided on the pin contact surface 400. In other words, the metal oil well pipe 1 according to this embodiment has the resin coating 100 on the pin contact surface 400 and / or the box contact surface 500 .

[0073] The resin coating 100 is a solid coating containing a resin, a solid lubricant powder, and copper phthalocyanine. The resin and the solid lubricant powder can be selected independently. The resin, the solid lubricant powder, and the copper phthalocyanine contained in the resin coating 100 according to the present embodiment will be described in detail below.

[0074] [resin] The resin contained in the resin coating 100 according to this embodiment is not particularly limited. However, when the metal oil well pipe 1 is fastened, the surface of the resin coating 100 is scraped off and wear powder is generated. Therefore, in order to stably obtain the wear resistance (coating life) and high torque performance of the resin coating 100, it is preferable to use a resin that has high adhesion to the base and appropriate hardness. The resin that has high adhesion to the base and appropriate hardness is, for example, one or more types selected from the group consisting of epoxy resin, phenol resin, acrylic resin, urethane resin, polyester resin, polyamideimide resin, polyamide resin, polyimide resin, and polyetheretherketone resin.

[0075] Preferably, the resin is one or two selected from the group consisting of epoxy resins and acrylic resins.

[0076] The resin content in the resin coating 100 is, for example, 60 to 90% by mass. In this case, the moldability, seizure resistance, and high torque performance of the resin coating 100 can be more stably improved. The lower limit of the resin content is preferably 62% by mass, more preferably 63% by mass, and even more preferably 65% ​​by mass. The upper limit of the resin content is preferably 88% by mass, and more preferably 86% by mass.

[0077] [Solid lubricating powder] The solid lubricant powder contained in the resin coating 100 according to this embodiment is not particularly limited. The solid lubricant powder is, for example, one or more selected from the group consisting of graphite, zinc oxide, boron nitride, talc, molybdenum disulfide, tungsten disulfide, graphite fluoride, tin sulfide, bismuth sulfide, organic molybdenum, a thiosulfate compound, and polytetrafluoroethylene.

[0078] Preferably, the solid lubricant powder is one or more selected from the group consisting of graphite, polytetrafluoroethylene, and molybdenum disulfide, and more preferably, the solid lubricant powder is polytetrafluoroethylene.

[0079] The content of the solid lubricant powder in the resin coating 100 is, for example, 1 to 30 mass %. In this case, the moldability and seizure resistance of the resin coating 100 can be more stably improved. The lower limit of the content of the solid lubricant powder is preferably 2 mass %, more preferably 5 mass %. The upper limit of the content of the solid lubricant powder is preferably 25 mass %, more preferably 20 mass %.

[0080] [Phthalocyanine copper] The resin coating 100 according to this embodiment contains phthalocyanine copper. Phthalocyanine copper is the most important substance for achieving high torque performance in the metal pipe for oil well 1 according to this embodiment. Phthalocyanine copper is a phthalocyanine (C 32 H 18 N8) is copper ion (Cu 2+ The chemical formula for copper phthalocyanine is shown below.

[0081] [ka]

[0082] If the resin coating 100 contains phthalocyanine copper, the high torque performance of the metal pipe for oil well use 1 is improved. The details of the reason for this are not clear. However, it has been proven by the examples described later that the torque-on-shoulder resistance ΔT, which is the difference between the yield torque Ty and the shouldering torque Ts, is increased by the inclusion of phthalocyanine copper in the resin coating 100 according to this embodiment. Therefore, the metal pipe for oil well use 1 according to this embodiment can be fastened with a high torque even if it has a large diameter.

[0083] The content of phthalocyanine copper in the resin coating 100 according to this embodiment is not particularly limited. That is, even if the resin coating 100 contains even a small amount of phthalocyanine copper, the effect of improving the high torque performance of the metal pipe for oil well use 1 can be obtained to some extent. The lower limit of the content of phthalocyanine copper in the resin coating 100 may be 0.1 mass %. On the other hand, if the content of phthalocyanine copper in the resin coating 100 is 0.2 mass % or more, the high torque performance of the metal pipe for oil well use 1 is further improved. Therefore, in this embodiment, the lower limit of the content of phthalocyanine copper in the resin coating 100 is preferably 0.1 mass %, more preferably 0.2 mass %, and even more preferably 0.4 mass %.

[0084] If the content of phthalocyanine copper in the resin coating 100 according to this embodiment is 30.0% by mass or less, the dispersibility of phthalocyanine copper is improved. Therefore, a preferable upper limit of the content of phthalocyanine copper in the resin coating 100 is 30.0% by mass. Furthermore, if the content of phthalocyanine copper in the resin coating 100 according to this embodiment is 9.0% by mass or less, the metal pipe for oil well 1 will have improved high torque performance as well as improved seizure resistance. Therefore, the upper limit of the content of phthalocyanine copper in the resin coating 100 may be 9.0% by mass.

[0085] In view of the above, the upper limit of the phthalocyanine copper content in the resin coating 100 according to this embodiment is preferably 30.0 mass%, more preferably 14.0 mass%, even more preferably 12.0 mass%, even more preferably 10.0 mass%, even more preferably 9.0 mass%, and even more preferably 6.0 mass%.

[0086] [Seizure resistance] In the metal pipe for oil well use 1 according to this embodiment, if the upper limit of the content of phthalocyanine copper in the resin coating 100 is further adjusted, not only the high torque performance but also the seizure resistance of the metal pipe for oil well use 1 can be improved. This point will be specifically explained below with reference to a table.

[0087] Table 1 shows the content of phthalocyanine copper in the resin coating 100 and the results of the Bowden test, which is an index of seizure resistance. Table 1 is an excerpt of the results of Example 2 described later. In Example 2, a resin coating 100 containing phthalocyanine copper in the content shown in Table 1 was formed on the surface of the steel plate of each test number. Furthermore, a Bowden test was performed using the steel plate of each test number on which the resin coating 100 was formed. In the Bowden test, a steel ball was slid on the surface of the resin coating 100 of the steel plate of each test number to determine the friction coefficient. Table 1 shows the content of phthalocyanine copper in the resin coating 100 of each test number and the number of slides until the friction coefficient exceeds 0.3. Note that the greater the number of slides until the friction coefficient exceeds 0.3, the higher the seizure resistance.

[0088] [Table 1]

[0089] Referring to Table 1, when the content of phthalocyanine copper in the resin coating 100 is 0.2 to 9.0 mass%, the number of sliding movements until the friction coefficient exceeds 0.3 increases compared to when the content of phthalocyanine copper in the resin coating 100 is 0.1 mass% and when the content of phthalocyanine copper in the resin coating 100 is 10.0 mass%. In other words, when the content of phthalocyanine copper in the resin coating 100 is 0.2 to 9.0 mass%, not only the high torque performance of the metal pipe for oil well 1 but also the seizure resistance is improved.

[0090] [Other ingredients] The resin coating 100 according to this embodiment may further contain components other than those described above. The other components are, for example, one or more selected from the group consisting of a rust inhibitor, a preservative, and an antioxidant. The rust inhibitor is, for example, one or more selected from the group consisting of aluminum tripolyphosphate, aluminum phosphite, and calcium ion-exchanged silica. A commercially available water repellent may be used as the rust inhibitor.

[0091] The resin coating 100 according to the present embodiment may be a single layer or may include multiple layers. "Includes multiple layers" means that the resin coating 100 is laminated in two or more layers in the radial direction of the metal pipe for oil well 1. The resin coating 100 can be formed by laminating two or more layers by repeatedly applying and curing a composition for forming the resin coating 100. The resin coating 100 may be formed directly on at least one of the pin contact surface 400 and the box contact surface 500, or may be formed after performing a base treatment described later on the pin contact surface 400 and / or the box contact surface 500. When the resin coating 100 includes multiple layers, any one of the resin coatings 100 may contain each component within the above range, or all of the multiple resin coatings 100 may contain each component within the above range. Preferably, the resin coating 100 includes an anti-rust resin coating. In the present embodiment, the anti-rust resin coating has any configuration. That is, the rust-preventive resin coating may not be formed on the metal oil well pipe 1 according to this embodiment. The rust-preventive resin coating will be described in detail below.

[0092] [Anti-rust resin coating] The metal pipe for oil well use 1 according to this embodiment may further include an anti-rust resin coating in the resin coating 100 formed on at least one of the pin contact surface 400 and the box contact surface 500. The anti-rust resin coating contains an anti-rust pigment and an acrylic silicone resin. The anti-rust pigment is, for example, one or more selected from the group consisting of aluminum tripolyphosphate, aluminum phosphite, zinc-rich primer (JIS K5552 (2010)), and micaceous iron oxide. The acrylic silicone resin may be a commercially available acrylic silicone resin. For example, the commercially available acrylic silicone resin is the acrylic silicone resin ACRYDIC manufactured by DIC Corporation. When the resin coating 100 of the metal pipe for oil well use 1 includes the anti-rust resin coating 70, the corrosion resistance of the metal pipe for oil well use 1 is enhanced.

[0093] The content of the anti-rust pigment in the anti-rust resin coating is, for example, 5 to 30 mass %. The content of the acrylic silicone resin in the anti-rust resin coating is, for example, 50 to 80 mass %. The anti-rust resin coating may contain other components in addition to the anti-rust pigment and the acrylic silicone resin. The other components are, for example, one or more selected from the group consisting of a pigment, an antifoaming agent, a leveling agent, and a fibrous filler. The content of the other components in the anti-rust resin coating is, for example, 0 to 20 mass % in total.

[0094] As described above, the rust-preventive resin coating is included in the resin coating 100. Specifically, Fig. 11 is an enlarged view of the pin contact surface 400 according to this embodiment, which is different from Fig. 9. Referring to Fig. 11, the metal pipe for oil well 1 includes the resin coating 100 formed on the pin contact surface 400, an rust-preventive resin coating 70, and an upper layer 60 of the resin coating 100. In this case, the upper layer 60 of the resin coating 100 contains a resin, a solid lubricant powder, and phthalocyanine copper, and the rust-preventive resin coating 70, which is the lower layer of the resin coating 100, contains an anti-rust pigment and an acrylic silicone resin.

[0095] The arrangement of the rust-preventive resin coating 70 in the metal pipe for oil well use 1 according to this embodiment is not limited to that shown in FIG. 11. Although not shown, the metal pipe for oil well use 1 may include the rust-preventive resin coating 70 in the resin coating 100 formed on the box contact surface 500, similarly to FIG. 11. The rust-preventive resin coating 70 may also be included only in the resin coating 100 formed on the pin contact surface 400, and not included in the resin coating 100 formed on the box contact surface 500. The rust-preventive resin coating 70 may further be included only in the resin coating 100 formed on the box contact surface 500, and not included in the resin coating 100 formed on the pin contact surface 400. The rust-preventive resin coating 70 may further be included in both the resin coating 100 formed on the pin contact surface 400 and the resin coating 100 formed on the box contact surface 500.

[0096] In this embodiment, the rust-preventive resin coating 70 may be included in the resin coating 100 formed on a plating layer described later, or may be included in the resin coating 100 formed on a chemical conversion coating described later. That is, in this embodiment, the rust-preventive resin coating 70 may be formed on the pin contact surface 400, may be formed on the box contact surface 500, may be formed on the plating layer described later, or may be formed on the chemical conversion coating described later.

[0097] The resin coating 100 may be disposed as an outermost layer on the pin contact surface 400 and / or the box contact surface 500. When the metal oil well pipe 1 is fastened, a liquid lubricant may be further applied on the resin coating 100.

[0098] [Resin coating thickness] The thickness of the resin coating 100 is not particularly limited. The thickness of the resin coating 100 is, for example, 1 to 100 μm. In this case, the high torque performance of the metal pipe for oil well 1 can be more stably improved. The lower limit of the thickness of the resin coating 100 is preferably 2 μm, more preferably 5 μm, and even more preferably 10 μm. The upper limit of the thickness of the resin coating 100 is preferably 80 μm, more preferably 70 μm, more preferably 60 μm, and even more preferably 50 μm.

[0099] [Method of measuring resin coating] The thickness of the resin coating 100 is measured by the following method. A probe of an electromagnetic induction type film thickness gauge is brought into contact with the pin contact surface 400 or the box contact surface 500 on which the resin coating 100 is formed. The probe has an electromagnet, and when a magnetic body is brought close, electromagnetic induction occurs, and the voltage changes depending on the distance between the probe and the magnetic body. The thickness of the resin coating 100 is obtained from the change in the voltage. The measurement points are 12 points (12 points at 0°, 30°, 60°, 90°, 120°, 150°, 180°, 210°, 240°, 270°, 300°, and 330°) in the circumferential direction of the metal pipe for oil well 1. The arithmetic average of the measurement results at the 12 points is defined as the thickness of the resin coating 100.

[0100] The resin coating 100 may be formed directly on the pin contact surface 400 or the box contact surface 500, in contact with the pin contact surface 400 or the box contact surface 500. The metal pipe for oil well 1 may further include another coating between the pin contact surface 400 or the box contact surface 500 and the resin coating 100. The other coating is, for example, one or more coatings selected from the group consisting of a plating layer and a chemical conversion coating.

[0101] [Optional configuration] [Plating layer] The metal pipe for oil well use 1 according to this embodiment may further include a plating layer between the resin coating 100 and at least one of the pin contact surface 400 and the box contact surface 500. In the metal pipe for oil well use 1 according to this embodiment, the plating layer may have any configuration. That is, in the metal pipe for oil well use 1 according to this embodiment, the plating layer may not be formed.

[0102] FIG. 12 is an enlarged view of the pin contact surface 400 according to the present embodiment, which is different from FIG. 9 and FIG. 11. In FIG. 12, the plating layer 80 is disposed between the pin contact surface 400 and the resin coating 100. Specifically, in FIG. 12, the plating layer 80 is formed on the pin contact surface 400, and the resin coating 100 is formed on the plating layer 80. However, the arrangement of the plating layer 80 is not limited to FIG. 12. Although not shown, for example, the plating layer 80 may be disposed between the box contact surface 500 and the resin coating 100. For example, the plating layer 80 may be disposed between the pin contact surface 400 and the resin coating 100, and neither the resin coating 100 nor the plating layer 80 may be disposed on the box contact surface 500. For example, the plating layer 80 may be disposed between the pin contact surface 400 and the resin coating 100, and the plating layer 80 may be disposed between the box contact surface 500 and the resin coating 100.

[0103] In this embodiment, a rust-preventive resin coating 70 may further be provided on the plating layer 80. Specifically, Fig. 13 is an enlarged view of the pin contact surface 400 according to this embodiment, which is different from Figs. 9, 11, and 12. Referring to Fig. 13, the plating layer 80 may be disposed between the pin contact surface 400 and the resin coating 100, and the resin coating 100 may include the rust-preventive resin coating 70 and an upper layer 60 of the resin coating 100.

[0104] In the present embodiment, the type of the plating layer 80 is not particularly limited. The plating layer 80 is, for example, selected from the group consisting of a Zn plating layer, a Ni plating layer, a Cu plating layer, a Zn-Ni alloy plating layer, a Zn-Co alloy plating layer, and a Ni-W alloy plating layer. When the plating layer 80 is a Zn-Ni alloy plating layer, the chemical composition of the Zn-Ni alloy plating layer is, for example, 10 to 20 mass % Ni, and the balance is Zn and impurities. When the plating layer 80 is a Cu plating layer, the chemical composition of the Cu plating layer is, for example, Cu and impurities.

[0105] When the metal oil well pipe 1 according to this embodiment has the plating layer 80 on the pin contact surface 400 and / or the box contact surface 500, the seizure resistance of the metal oil well pipe 1 is further improved.

[0106] FIG. 14 is a diagram showing the relationship between the plating layer 80, the content of phthalocyanine copper, and the results of the Bowden test, which is an index of seizure resistance. FIG. 14 was obtained from Example 2 described later. The horizontal axis of FIG. 14 indicates the content of phthalocyanine copper in the resin coating 100. The vertical axis of FIG. 14 indicates the number of sliding movements until the friction coefficient exceeds 0.3. In Example 2, a steel ball was slid on the surface of the steel sheet on which the plating layer 80 and / or the resin coating 100 was formed, and the number of sliding movements until the friction coefficient exceeds 0.3 was measured. The higher the number of sliding movements until the friction coefficient exceeds 0.3, the higher the seizure resistance. In FIG. 14, a white circle (◯) indicates that the plating layer 80 was not formed on the surface of the steel sheet, and only the resin coating 100 was formed. In FIG. 14, a square (□) indicates that a Zn-Ni alloy plating layer was formed on the surface of the steel sheet, and the resin coating 100 was formed thereon. 14, the metal pipe for oil well use 1 having a Zn-Ni alloy plating layer requires a larger number of sliding cycles until the friction coefficient exceeds 0.3, compared with the metal pipe for oil well use 1 not having the plating layer 80. In this manner, the metal pipe for oil well use 1 having the plating layer 80 formed on the pin contact surface 400 and / or the box contact surface 500 has further improved seizure resistance.

[0107] [Thickness of plating layer] The thickness of the plating layer 80 is not particularly limited. The thickness of the plating layer 80 is, for example, 1 to 30 μm. In this case, the seizure resistance of the metal pipe for oil well 1 can be more stably improved. The lower limit of the thickness of the plating layer 80 is preferably 2 μm, more preferably 3 μm, and further preferably 4 μm. The upper limit of the thickness of the plating layer 80 is preferably 20 μm, and more preferably 10 μm.

[0108] [Method of measuring plating layer thickness] The thickness of the plating layer 80 is measured by the following method. A probe of an electromagnetic induction type film thickness measuring instrument is brought into contact with the pin contact surface 400 or the box contact surface 500 on which the plating layer 80 is formed. The probe is brought into contact with the portion of the pin contact surface 400 or the box contact surface 500 from which the resin coating 100 has been removed. The probe has an electromagnet, and when a magnetic body is brought close, electromagnetic induction occurs, and the voltage changes depending on the distance between the probe and the magnetic body. The thickness of the plating layer 80 is obtained from the change in the voltage. The measurement points are 12 points (12 points at 0°, 30°, 60°, 90°, 120°, 150°, 180°, 210°, 240°, 270°, 300°, and 330°) in the circumferential direction of the metal pipe for oil well 1. The arithmetic average of the measurement results at the 12 points is taken as the thickness of the plating layer 80.

[0109] [Chemical conversion coating] The metal pipe for oil well use 1 according to this embodiment may further include a chemical conversion coating between the resin coating 100 and at least one of the pin contact surface 400 and the box contact surface 500. In the metal pipe for oil well use 1 according to this embodiment, the chemical conversion coating may be of any configuration. That is, in the metal pipe for oil well use 1 according to this embodiment, the chemical conversion coating may not be formed.

[0110] FIG. 15 is an enlarged view of the box contact surface 500 according to the present embodiment, which is different from FIG. 10. In FIG. 15, a conversion coating 90 is disposed between the box contact surface 500 and the resin coating 100. Specifically, in FIG. 15, the conversion coating 90 is formed on the box contact surface 500, and the resin coating 100 is formed on the conversion coating 90. However, the arrangement of the conversion coating 90 is not limited to FIG. 15. Although not shown, for example, the conversion coating 90 may be disposed between the pin contact surface 400 and the resin coating 100, and neither the resin coating 100 nor the conversion coating 90 may be disposed on the box contact surface 500. For example, the conversion coating 90 may be disposed between the pin contact surface 400 and the resin coating 100, and the conversion coating 90 may be disposed between the box contact surface 500 and the resin coating 100.

[0111] In this embodiment, an anti-rust resin coating 70 may further be provided on the chemical conversion coating 90. Specifically, Fig. 16 is an enlarged view of a pin contact surface 400 according to this embodiment, which is different from Figs. 9, 11, 12, and 13. Referring to Fig. 16, the chemical conversion coating 90 is disposed between the pin contact surface 400 and the resin coating 100, and the resin coating 100 may include an anti-rust resin coating 70 and an upper layer 60 of the resin coating 100.

[0112] The pin contact surface 400 and the box contact surface 500 according to this embodiment may further include both the plating layer 80 and the chemical conversion coating 90. Fig. 17 is an enlarged view of the pin contact surface 400 according to this embodiment, which is different from Figs. 9, 11, 12, 13, and 16. In Fig. 17, the plating layer 80 is disposed on the pin contact surface 400, the chemical conversion coating 90 is disposed on the plating layer 80, and the resin coating 100 is disposed on the chemical conversion coating 90. In other words, when the plating layer 80 is provided, the metal pipe for oil well 1 includes the chemical conversion coating 90 between the plating layer 80 and the resin coating 100.

[0113] The arrangement of the plating layer 80 and the chemical conversion coating 90 in the metal pipe for oil well 1 according to the present embodiment is not limited to that shown in FIG. 17. However, when the plating layer 80 and the chemical conversion coating 90 are arranged between the pin contact surface 400 and the resin coating 100, the chemical conversion coating 90 may be arranged on the plating layer 80, and the resin coating 100 may be arranged on the chemical conversion coating 90. When the plating layer 80 is not arranged between the pin contact surface 400 and the resin coating 100, the chemical conversion coating 90 may be arranged on the pin contact surface 400, and the resin coating 100 may be arranged on the chemical conversion coating 90. Similarly, when the plating layer 80 and the chemical conversion coating 90 are provided between the box contact surface 500 and the resin coating 100, the chemical conversion coating 90 may be arranged on the plating layer 80, and the resin coating 100 may be arranged on the chemical conversion coating 90. In addition, when no plating layer 80 is provided between the box contact surface 500 and the resin coating 100, a chemical conversion coating 90 may be placed on the box contact surface 500, and the resin coating 100 may be placed on the chemical conversion coating 90.

[0114] In this embodiment, when the plating layer 80 and the chemical conversion coating 90 are provided, the anti-rust resin coating 70 may be provided on the chemical conversion coating 90. Specifically, Fig. 18 is an enlarged view of the pin contact surface 400 according to this embodiment, which is different from Figs. 9, 11, 12, 13, 16, and 17. Referring to Fig. 18, the plating layer 80 may be disposed on the pin contact surface 400, the chemical conversion coating 90 may be disposed on the plating layer 80, and the resin coating 100 may be disposed on the chemical conversion coating 90, and the resin coating 100 may include the anti-rust resin coating 70 and an upper layer 60 of the resin coating 100.

[0115] In this embodiment, the type of the chemical conversion coating 90 is not particularly limited. The chemical conversion coating 90 is, for example, selected from the group consisting of a phosphate conversion coating, an oxalate conversion coating, a borate conversion coating, and a chromate coating. From the viewpoint of adhesion of the resin coating 100, a phosphate conversion coating is preferable. Here, the phosphate is, for example, one or more selected from the group consisting of manganese phosphate, zinc phosphate, iron manganese phosphate, or zinc calcium phosphate. The chemical conversion coating 90 may be a chromate coating. The chromate coating may be formed by a known method. The chromate coating preferably does not contain hexavalent chromium.

[0116] When the metal pipe for oil well use 1 according to this embodiment has the chemical conversion coating 90 on the pin contact surface 400 and / or the box contact surface 500, the seizure resistance of the metal pipe for oil well use 1 is further improved. The chemical conversion coating 90 enhances the adhesion of the resin coating 100 thereon by an anchor effect. This enhances the seizure resistance of the metal pipe for oil well use 1. With reference to Example 3 described later, the metal pipe for oil well use 1 having the chemical conversion coating 90 has a greater number of sliding strokes until the friction coefficient exceeds 0.3 than the metal pipe for oil well use 1 not having the chemical conversion coating 90. In this way, the metal pipe for oil well use 1 having the chemical conversion coating 90 formed on the pin contact surface 400 and / or the box contact surface 500 has a further improved seizure resistance.

[0117] The metal pipe for oil well use 1 of this embodiment may have the resin coating 100 on at least one of the pin contact surface 400 and the box contact surface 500. As described above, the arrangement of the plating layer 80, the chemical conversion coating 90, and the rust-preventive resin coating 70 on the pin contact surface 400 may be the same as or different from that on the box contact surface 500. The metal pipe for oil well use 1 may further have other coatings as necessary.

[0118] [Surface preparation] In the metal pipe for oil well use 1 according to the present embodiment, at least one of the pin contact surface 400 and the box contact surface 500 may be a surface that has been subjected to a surface treatment. That is, in the present embodiment, the surface treatment is an optional step, and neither the pin contact surface 400 nor the box contact surface 500 may be a surface that has been subjected to a surface treatment. If the surface treatment is performed, the surface treatment is, for example, one or more selected from the group consisting of blasting and pickling. If the surface treatment is performed, the surface roughness of the pin contact surface 400 and / or the box contact surface 500 is increased. Therefore, the adhesion of the resin coating 100, the plating layer 80 and / or the chemical conversion coating 90 formed thereon is increased. As a result, the seizure resistance of the metal pipe for oil well use 1 is increased.

[0119] [Chemical composition of the tube body] The chemical composition of the pipe body 10 of the metal pipe for oil well use 1 according to the present embodiment is not particularly limited. The metal pipe for oil well use 1 according to the present embodiment is characterized by the resin coating 100. Therefore, in the present embodiment, the steel type of the pipe body 10 of the metal pipe for oil well use 1 is not particularly limited.

[0120] The pipe body 10 may be formed of, for example, carbon steel, stainless steel, alloys, etc. That is, the metal pipe for oil wells may be a steel pipe made of an Fe-based alloy, or an alloy pipe represented by a Ni-based alloy pipe. Here, the steel pipe is, for example, a low-alloy steel pipe, a martensitic stainless steel pipe, a duplex stainless steel pipe, etc. On the other hand, among alloy steels, high-alloy steels such as Ni-based alloys and duplex stainless steels containing alloy elements such as Cr, Ni, and Mo have high corrosion resistance. Therefore, if these high-alloy steels are used as the pipe body 10, excellent corrosion resistance can be obtained in a corrosive environment containing hydrogen sulfide, carbon dioxide, etc.

[0121] [Manufacturing method] A method for producing the metal oil well pipe 1 according to this embodiment will be described below.

[0122] The method for manufacturing the metal oil well pipe 1 according to the present embodiment includes a preparation step, a coating step, and a hardening step. The hardening step is carried out after the coating step.

[0123] [Preparation process] In the preparation step, a metal pipe for oil well use 1 is prepared, which includes a pipe body 10 including a pin 40 including a pin contact surface 400 including a male thread portion 41, and a box 50 including a box contact surface 500 including a female thread portion 51. As described above, the metal pipe for oil well use 1 according to this embodiment has a well-known configuration. That is, in the preparation step, it is sufficient to prepare a metal pipe for oil well use 1 having a well-known configuration.

[0124] [Coating process] In the coating step, a composition containing a resin, a solid lubricant powder, and phthalocyanine copper is coated onto at least one of the pin contact surface 400 and the box contact surface 500. The composition is a composition for forming the resin coating 100 described above. The composition contains a resin, a solid lubricant powder, and phthalocyanine copper. The composition for forming the resin coating 100, excluding the solvent, is the same as the composition of the resin coating 100 described above.

[0125] The solventless composition can be produced, for example, by heating the resin to a molten state, adding the solid lubricant powder and copper phthalocyanine, and kneading the mixture. All of the components may be mixed in powder form to produce a powder mixture.

[0126] The solvent-type composition can be produced, for example, by dissolving or dispersing the resin, the solid lubricant powder, and the phthalocyanine copper in a solvent and mixing them. The solvent is, for example, water, alcohol, or an organic solvent. The solvent may contain a small amount of a surfactant. The ratio of the solvent is not particularly limited. The ratio of the solvent may be adjusted so that the composition has an appropriate viscosity depending on the application method. The ratio of the solvent is, for example, 40 to 60% by mass, assuming that the total of all components other than the solvent is 100% by mass.

[0127] The method of applying the composition onto the pin contact surface 400 and / or the box contact surface 500 is not particularly limited, and may be a well-known method. In the case of a solvent-free composition, for example, the composition can be applied onto the pin contact surface 400 and / or the box contact surface 500 using a hot melt method. In the hot melt method, the composition is heated to melt the resin and put into a low-viscosity fluid state. The fluidized composition is sprayed from a spray gun having a temperature retention function. The method of applying the composition onto the pin contact surface 400 and / or the box contact surface 500 may be brush coating, immersion, or the like, instead of spray coating. The heating temperature of the composition is preferably 10 to 50° C. higher than the melting point of the resin.

[0128] In the case of a solvent-based composition, for example, the composition in a solution state can be applied by spraying onto the pin contact surface 400 and / or the box contact surface 500. In this case, the viscosity of the composition is adjusted so that it can be sprayed under an environment of normal temperature and pressure. The method of applying the composition onto the pin contact surface 400 and / or the box contact surface 500 may be brushing, dipping, or the like, instead of spraying.

[0129] [Curing process] In the curing step, the applied composition is cured to form the resin coating 100. In the case of a solventless composition, the composition applied on at least one of the pin contact surface 400 and the box contact surface 500 is cooled, and the molten composition is cured to form the solid resin coating 100. In this case, the cooling method is not particularly limited and may be a well-known method. The cooling method is, for example, air cooling and air cooling. In the case of a solvent-type composition, the composition applied on at least one of the pin contact surface 400 and the box contact surface 500 is dried, and the composition is cured to form the solid resin coating 100. In this case, the drying method is not particularly limited and may be a well-known method. The drying method is, for example, natural drying, low-temperature air drying, and vacuum drying. In addition, when the resin is a thermosetting resin, the composition may be cured by a heat curing treatment to form the solid resin coating 100.

[0130] Through the above-mentioned manufacturing process, the metal oil well pipe 1 of the present embodiment is manufactured.

[0131] [Optional manufacturing process] The method for producing the metal oil well pipe 1 of the present embodiment may further include one or more of a plating layer forming step, a chemical conversion treatment step, a rust-preventive resin coating forming step, and a surface preparation step. All of these steps are optional. Therefore, these steps may not be performed.

[0132] [Plating layer formation process] The method for manufacturing the metal pipe for oil well 1 according to the present embodiment may further include a plating layer forming step before the coating step. When the plating layer forming step is performed, a plating layer 80 is formed on at least one of the pin contact surface 400 and the box contact surface 500.

[0133] The method for forming the plating layer 80 is not particularly limited, and may be a well-known method. The plating layer 80 may be formed by electrolytic plating or electroless plating. For example, when a Zn-Ni alloy plating layer is formed by electrolytic plating, the plating bath contains zinc ions and nickel ions. The plating bath preferably contains 1 to 100 g / L of zinc ions and 1 to 50 g / L of nickel ions. The electrolytic plating conditions are, for example, plating bath pH: 1 to 10, plating bath temperature: 20 to 60° C., and current density: 1 to 100 A / dm 2 and treatment time: 0.1 to 50 minutes. For example, when a Cu plating layer is formed by electrolytic plating, it can be carried out by a well-known method.

[0134] [Chemical conversion treatment process] The method for manufacturing the metal oil well pipe 1 according to the present embodiment may further include a chemical conversion treatment step before the coating step. When the chemical conversion treatment step is performed, a chemical conversion coating 90 is formed on at least one of the pin contact surface 400 and the box contact surface 500.

[0135] The method of the chemical conversion treatment is not particularly limited, and may be a well-known method. The chemical conversion treatment may be selected from the group consisting of, for example, phosphate conversion treatment, oxalate conversion treatment, borate conversion treatment, and chromate treatment. As the treatment liquid for the chemical conversion treatment, an acidic phosphate conversion treatment liquid for general zinc-plated materials may be used. As the treatment liquid, for example, a zinc phosphate-based conversion treatment containing 1 to 150 g / L of phosphate ions, 3 to 70 g / L of zinc ions, 1 to 100 g / L of nitrate ions, and 0 to 30 g / L of nickel ions may be used. As the treatment liquid, a manganese phosphate-based conversion treatment liquid commonly used for oil well metal pipes 1 may also be used. As the treatment liquid, a commercially available chromate treatment liquid may also be used. The liquid temperature of the treatment liquid is, for example, room temperature to 100° C. The treatment time for the chemical conversion treatment may be appropriately set according to the desired film thickness, and is, for example, 0.5 to 15 minutes. In order to promote the formation of the chemical conversion coating 90, surface conditioning may be performed before the chemical conversion treatment. The surface conditioning refers to a treatment of immersing the plate in a surface conditioning aqueous solution containing colloidal titanium. When a chemical conversion treatment step is carried out, it is preferable to wash the plate with water or hot water after the chemical conversion treatment and then dry the plate.

[0136] As described above, in the metal pipe for oil well use 1 according to this embodiment, the chemical conversion coating 90 is formed on any one of the pin contact surface 400, the box contact surface 500, or the plating layer 80. That is, in the manufacturing method for the metal pipe for oil well use 1 according to this embodiment, when both the plating layer forming step and the chemical conversion treatment step are performed, the plating layer forming step is followed by the chemical conversion treatment step, and then the coating step is performed.

[0137] [Rust-preventive resin film formation process] The method for manufacturing the metal pipe for oil well 1 according to the present embodiment may further include a rust-preventive resin coating forming step before the coating step. When the rust-preventive resin coating forming step is performed, the rust-preventive resin coating 70 is formed on at least one of the pin contact surface 400, the box contact surface 500, the plating layer 80, and the chemical conversion coating 90.

[0138] The method for forming the rust-preventive resin coating 70 is not particularly limited, and may be a well-known method. The rust-preventive resin coating 70 can be formed, for example, by applying a composition containing an anti-rust pigment and an acrylic silicone resin onto at least one of the pin contact surface 400, the box contact surface 500, the plating layer 80, and the chemical conversion coating 90, and curing the composition. The application method is not particularly limited, and may be spray application, brush application, or immersion. The composition for forming the rust-preventive resin coating 70 may contain a solvent. The composition for forming the rust-preventive resin coating 70, excluding the solvent, is the same as the composition of the rust-preventive resin coating 70 described above. The curing method is, for example, natural drying, low-temperature air drying, and heat drying.

[0139] As described above, in the metal pipe for oil well use 1 according to this embodiment, the rust-preventive resin coating 70 is formed on any one of the pin contact surface 400, the box contact surface 500, the plating layer 80, or the chemical conversion coating 90. That is, in the manufacturing method for the metal pipe for oil well use 1 according to this embodiment, when the plating layer forming step, the chemical conversion treatment step, and the rust-preventive resin coating forming step are all performed, the plating layer forming step, the chemical conversion treatment step, and the rust-preventive resin coating forming step are performed in this order, and then the coating step is performed.

[0140] [Surface preparation process] The method for producing the metal pipe for oil well use 1 according to the present embodiment may further include a surface preparation step before the coating step. When a coating layer forming step is performed, the method for producing the metal pipe for oil well use 1 may include a surface preparation step before the coating layer forming step. When a chemical conversion treatment step is performed, the method for producing the metal pipe for oil well use 1 may include a surface preparation step before the chemical conversion treatment step. When a rust-preventive resin coating forming step is performed, the method for producing the metal pipe for oil well use 1 may include a surface preparation step before the rust-preventive resin coating forming step. In the surface preparation step, for example, pickling and / or blasting are performed. In addition, an alkaline degreasing treatment may be performed.

[0141] When performing the pickling treatment, the pin contact surface 400 and / or the box contact surface 500 are immersed in a strong acid solution such as sulfuric acid, hydrochloric acid, nitric acid, hydrofluoric acid, or a mixed acid thereof to increase the surface roughness of the pin contact surface 400 and / or the box contact surface 500. When performing the blasting treatment, for example, sandblasting is performed in which a blasting material (abrasive) is mixed with compressed air and projected onto the pin contact surface 400 and / or the box contact surface 500. In this case, the surface roughness of the pin contact surface 400 and / or the box contact surface 500 is increased.

[0142] The plating layer forming process, chemical conversion process, and base treatment process described above may be the same or different processes performed on the pin contact surface 400 and the box contact surface 500. Moreover, these processes may be performed only on the pin contact surface 400 or only on the box contact surface 500.

[0143] The metal pipe for oil well use 1 according to the present embodiment is manufactured by the above steps. However, the above-mentioned manufacturing method is only one example of the manufacturing method of the metal pipe for oil well use 1 according to the present embodiment, and the manufacturing method is not limited to this. The metal pipe for oil well use 1 according to the present embodiment may be manufactured by other methods. EXAMPLES

[0144] In Example 1, the resin coating 100 was formed on the pin contact surface 400 or the box contact surface 500 of the metal pipe for oil well use 1, and the high torque performance and seizure resistance were evaluated. Specifically, in Example 1, a metal pipe for oil well use VAM21 (registered trademark) HT (outer diameter 273.05 mm (10.75 inches), wall thickness: 12.570 mm (0.495 inches)) manufactured by Nippon Steel Corporation was used. The steel type of the metal pipe for oil well use was SM2535M110 steel (C≦0.03%, Si:≦0.50%, Mn≦1.0%, Cu≦1.5%, Ni: 29.5 to 36.5%, Cr: 24.0 to 27.0%, balance: Fe and impurities).

[0145] A plating layer and a resin coating including a rust-preventive resin coating were appropriately formed on the contact surfaces of the boxes of test numbers 1 to 12 to prepare metal pipes for oil wells including pins and boxes of test numbers 1 to 12. The "plating layer" column in Table 2 shows the plating layer formed. "-" in the "plating layer" column in Table 2 means that a plating layer was not formed. The plating layers formed all had a thickness of 8 μm. The thickness of the plating layer was measured using an electromagnetic film thickness meter SDM-picоR manufactured by Sanko Electronics Laboratory Co., Ltd., and was performed by the above-mentioned method. The "rust-preventive resin coating" column in Table 2 shows whether or not a rust-preventive resin coating was formed. "Formed" in the "rust-preventive resin coating" column in Table 2 means that a rust-preventive resin coating was formed. "-" in the "rust-preventive resin coating" column in Table 2 means that a rust-preventive resin coating was not formed. The rust-preventive resin coating formed was the same as the rust-preventive resin coating of test numbers 32 and 33 in Example 4 described later.

[0146] Furthermore, the "Resin Coating" column in Table 2 indicates whether or not a resin coating was formed. "Formed" in the "Resin Coating" column in Table 2 means that a resin coating was formed. "-" in the "Resin Coating" column in Table 2 means that a resin coating was not formed. In addition, in test numbers 1 to 9 and 11 to 12, the formed resin coatings all had a thickness of 20 μm. In test number 10, the thickness of the resin coating was 20 μm, excluding the thickness of the rust-preventive resin coating. The thickness of the resin coating was measured using an electromagnetic coating thickness meter SDM-picоR manufactured by Sanko Electronics Laboratory Co., Ltd., by the method described above. In test numbers 2 to 9 and 11 to 12, the resin coatings were all formed on the surface of the above-mentioned plating layer.

[0147] In addition, in test number 1, a plating layer was not formed. Therefore, in test number 1, a resin film was formed directly on the box contact surface. Furthermore, in test number 10, an upper layer of a resin film was formed on the rust-preventive resin film. That is, in test number 10, the resin film was a multi-layered film. For each test number, the content of phthalocyanine copper in the formed resin film is shown in Table 2. The formed resin film further contained 1 to 30 mass% polytetrafluoroethylene (PTFE) as a solid lubricant powder, and the remainder contained epoxy resin as a resin. In Table 2, "-" in the "Content of phthalocyanine copper" column means that a resin film was not formed or that the formed resin film did not contain phthalocyanine copper. In test number 12, the formed resin film did not contain phthalocyanine copper. In test number 12, the resin film contained 8.6 mass% Cr2O3 instead of phthalocyanine copper. The resin coating of Test No. 12 further contained 1 to 30 mass % polytetrafluoroethylene (PTFE) as a solid lubricant powder, and the remainder contained an epoxy resin as a resin.

[0148] [Table 2]

[0149] Box Contact Surface [Plating layer formation process] As shown in Table 2, a Zn-Ni alloy plating layer was formed by electroplating on the box contact surfaces of test numbers 2 to 9 and 11 to 12. The plating bath used was Dainjin Alloy N-PL (trademark) manufactured by Daiwa Kasei Co., Ltd. The thickness of the Zn-Ni alloy plating layer was 8 μm. The thickness of the plating layer was measured by the above-mentioned method using an electromagnetic film thickness meter SDM-picоR manufactured by Sanko Electronics Laboratory Co., Ltd. The electroplating conditions were plating bath pH: 6.5, plating bath temperature: 25°C, current density: 2 A / dm 2 The composition of the Zn-Ni alloy plating layer was Zn: 85% and Ni: 15%. Furthermore, a trivalent chromate film was formed on the obtained Zn-Ni alloy plating layer. The treatment liquid for forming the trivalent chromate film was Dynechromate TR-02 manufactured by Daiwa Kasei Co., Ltd. The conditions for the chemical conversion treatment were bath temperature: 25°C, pH: 4.0, and treatment time: 50 seconds.

[0150] [Coating process and curing process] As shown in Table 2, a resin film was formed on the box contact surface of test numbers 1 to 12. In test numbers 2 to 9, 11, and 12, a resin film was formed on the box contact surface on which a plating layer was formed. In test number 1, a resin film was formed directly on the box contact surface. In test number 10, an upper layer of a resin film was formed on the rust-preventive resin film. A composition for forming a resin film was spray-applied on the box contact surface, the Zn-Ni alloy plating layer, or the rust-preventive resin film, and cured. As described above, the components in the composition other than the solvent included polytetrafluoroethylene particles and phthalocyanine copper, and the remainder was epoxy resin. The composition further included a solvent. The solvent was a mixed solution of water, alcohol, and a surfactant. After the composition was spray-applied on the Zn-Ni alloy plating layer on the box surface, a heat curing treatment was performed at 210°C for 20 minutes to form a resin film. In test number 12, phthalocyanine copper was not used, and instead 8.6 mass% of Cr2O3 was used.

[0151] [Pin Contact Surface] The contact surfaces of the pins of test numbers 1 to 12 were finished by mechanical grinding. That is, as shown in Table 2, no plating layer or resin coating was formed on the contact surfaces of the pins of test numbers 1 to 12.

[0152] [High torque performance evaluation] The torque-on-shoulder resistance ΔT was measured using the metal oil well pipes having the pin contact surface and the box contact surface of test numbers 1 to 12. Specifically, the tightening torque value was gradually increased at a tightening speed of 10 rpm, and the test was terminated when the material yielded. The torque was measured during tightening, and a torque chart as shown in FIG. 19 was created. Ts in FIG. 19 means shouldering torque. MTV in FIG. 19 means the torque value where the line segment L intersects with the torque chart. The line segment L has the same slope as the slope of the linear region in the torque chart after shouldering, and is a straight line with 0.2% more rotations than the linear region. Usually, when measuring the torque-on-shoulder resistance, Ty (yield torque Ty) is used. However, in this embodiment, the yield torque Ty (the boundary between the linear region and the nonlinear region in the torque chart after shouldering) was unclear. Therefore, the MTV was defined using the line segment L. The difference between MTV and Ts was taken as the torque-on-shoulder resistance ΔT. The torque-on-shoulder resistance ΔT was calculated as a relative value, with the torque-on-shoulder resistance ΔT when the API standard dope was used being set at 100. The results are shown in the "High torque performance" column in Table 2.

[0153] [Repeated fastening test] A repeated make-up test was carried out with a make-up torque of 53,800 Nm using metal oil well pipes having pin contact surfaces and box contact surfaces of test numbers 1 to 12. Make-up was carried out until irreparable seizure occurred in the threaded portion (male threaded portion and / or female threaded portion) or until seizure occurred in the metal seal portion. The results are shown in the "M&B number of times (times)" column in Table 2. "-" in the "M&B number of times (times)" column in Table 2 indicates that a repeated make-up test was not carried out.

[0154] [Evaluation Results] Referring to Table 2, the metal pipes for oil wells of test numbers 1 to 10 were provided with a resin coating containing resin, solid lubricant powder and phthalocyanine copper on at least one of the pin contact surface and the box contact surface. Therefore, the torque-on-shoulder resistance ΔT of test numbers 1 to 10 was 100 or more, and showed excellent high torque performance.

[0155] Furthermore, the metal oil well pipes of test numbers 1 and 3 to 10 had a copper phthalocyanine content of 0.2 to 30.0 mass% in the resin coating, and therefore had higher torque-on-shoulder resistance ΔT than test number 2, which had a copper phthalocyanine content of less than 0.2 mass%.

[0156] On the other hand, the oil well metal pipe of test number 11 had a resin coating containing resin and solid lubricant powder formed on the box contact surface, but the resin coating did not contain phthalocyanine copper. As a result, the torque-on-shoulder resistance ΔT was 65, and the high torque performance was low.

[0157] The oil well metal pipe of test number 12 had a resin coating containing resin and solid lubricant powder formed on the box contact surface, but this resin coating did not contain phthalocyanine copper, but instead contained Cr2O3. As a result, the torque-on-shoulder resistance ΔT was 90, and the high torque performance was low. EXAMPLES

[0158] In Example 2, a resin coating was formed on the surface of a steel plate simulating a metal pipe for oil wells, and the seizure resistance was evaluated. Specifically, in Example 2, a cold-rolled steel plate (chemical composition: C≦0.15%, Mn≦0.60%, P≦0.100%, S≦0.050%, balance: Fe and impurities) was used.

[0159] The plating layers shown in Table 3 were appropriately formed on the surfaces of the steel sheets of test numbers 13 to 21. The "plating layer" column in Table 3 shows the plating layers formed. "-" in the "plating layer" column in Table 3 means that no plating layer was formed. The formed plating layers all had a thickness of 8 μm. A resin film was formed on the surfaces of the steel sheets of test numbers 13 to 17 and 21. In test numbers 18 to 20, a resin film was formed on the formed plating layer. The formed resin film all had a thickness of 20 μm. The thickness of the resin film was measured using an electromagnetic film thickness meter SDM-picоR manufactured by Sanko Electronics Laboratory Co., Ltd., and the average value of the thicknesses at nine points on the same evaluation surface was taken as the thickness of the resin film. Furthermore, the content of phthalocyanine copper in the formed resin film is shown in Table 3. The resin coating further contained 1 to 30 mass% polytetrafluoroethylene (PTFE) as a solid lubricant powder, and the remainder contained epoxy resin as a resin. In Table 3, "-" in the "Phthalocyanine copper content" column means that the resin coating did not contain phthalocyanine copper.

[0160] [Table 3]

[0161] [Plating layer formation process] A Zn-Ni alloy plating layer was formed on the surface of the steel sheets of test numbers 18 to 20 by electroplating. The plating bath used was Dainjin Alloy N-PL (trademark) manufactured by Daiwa Kasei Co., Ltd. The thickness of the Zn-Ni alloy plating layer was 8 μm. The thickness of the plating layer was measured using an electromagnetic film thickness meter SDM-picоR manufactured by Sanko Electronics Laboratory Co., Ltd., and the average value of thicknesses at nine points on the same evaluation surface was taken as the thickness of the plating layer. The electroplating conditions were plating bath pH: 6.5, plating bath temperature: 25°C, current density: 2 A / dm 2The composition of the Zn-Ni alloy plating layer was Zn: 85% and Ni: 15%. Furthermore, a trivalent chromate film was formed on the obtained Zn-Ni alloy plating layer. The treatment liquid for forming the trivalent chromate film was Dynechromate TR-02 manufactured by Daiwa Kasei Co., Ltd. The conditions for the chemical conversion treatment were bath temperature: 25°C, pH: 4.0, and treatment time: 50 seconds.

[0162] [Coating process and curing process] A resin coating was formed on the surface of the steel sheets of test numbers 13 to 21. Specifically, a composition for forming a resin coating was applied to the surface of the steel sheets of test numbers 13 to 21 with a bar coder and cured. In the composition, the components other than the solvent included solid lubricant particles and phthalocyanine copper, and the remainder was resin. In test numbers 13 to 21, an epoxy resin was used as the resin. In test numbers 13 to 21, polytetrafluoroethylene particles were used as the solid lubricant particles. The content of phthalocyanine copper was as shown in Table 3. The composition further included a solvent. As the solvent, a mixed solution of water, alcohol, and a surfactant was used. In the case where there was a plating layer, or on the plating layer (or the chemical conversion coating thereon), in the case where there was no plating layer, the composition was applied to the steel sheet surface with a bar coder, and then heat curing treatment was performed at 210°C for 20 minutes to form a resin coating.

[0163] [Bowden test] A Bowden test was performed using the steel plates of test numbers 13 to 21 on which the resin coating was formed to evaluate the seizure resistance. Specifically, a steel ball was slid on the surface of the resin coating of test numbers 13 to 21 to determine the friction coefficient. The steel ball had a diameter of 3 / 16 inches and a chemical composition equivalent to SUJ2 of the JIS standard. The load was 3 kgf (Hertz surface pressure: average 1.56 GPa). The sliding width was 10 mm, and the sliding speed was 4 mm / sec. The sliding was performed without oil application at room temperature. The friction coefficient μ of the steel ball during sliding was measured, and the number of sliding times (number of reciprocating movements, i.e., one reciprocating movement in a range of 10 mm was counted as "one time") until the friction coefficient μ exceeded 0.3 (corresponding to the friction coefficient between the resin coating and the steel ball) was measured. A Bowden type adhesion sliding tester manufactured by Shinko Engineering Co., Ltd. was used for the test. The results are shown in Table 3 in the column for the number of sliding strokes until the friction coefficient exceeded 0.3.

[0164] [Evaluation Results] Referring to Table 3, the steel plates of test numbers 13 to 20 were provided with a resin coating containing resin, solid lubricant powder, and copper phthalocyanine on the surface. Further referring to Table 3, the resin coating formed on the steel plates of test numbers 14 to 16 and 18 to 20 had a copper phthalocyanine content of 0.2 to 9.0 mass%. As a result, the steel plates of test numbers 14 to 16 and 18 to 20 had a greater number of sliding strokes until the friction coefficient exceeded 0.3, compared with test number 21, which did not contain copper phthalocyanine in the resin coating, and steel plates of test numbers 13 and 17, which had a copper phthalocyanine content outside the range of 0.2 to 9.0 mass% in the resin coating. That is, they showed excellent seizure resistance. EXAMPLES

[0165] In Example 3, a resin coating was formed on the surface of a steel plate simulating a metal oil well pipe, and the seizure resistance was evaluated in the same manner as in Example 2. Specifically, in Example 3, a cold-rolled steel plate (chemical composition: C≦0.15%, Mn≦0.60%, P≦0.100%, S≦0.050%, balance: Fe and impurities) was used.

[0166] The plating layers shown in Table 4 were appropriately formed on the surfaces of the steel sheets of test numbers 22 to 31. The "plating layer" column in Table 4 shows the plating layers formed. "-" in the "plating layer" column in Table 4 means that no plating layer was formed. The thickness of each of the plating layers formed was 8 μm. The thickness of the plating layer was measured using an electromagnetic film thickness meter SDM-picоR manufactured by Sanko Electronics Laboratory Co., Ltd., and the average value of the thickness at nine points on the same evaluation surface was taken as the thickness of the plating layer. A chemical conversion coating was formed on the surfaces of the steel sheets of test numbers 22 to 29 and 31. The "chemical conversion coating" column in Table 4 shows the formed chemical conversion coating. Table 5 shows the chemical conversion treatment solution, treatment temperature, and treatment time used to form the coatings A to D among the chemical conversion coatings in the "chemical conversion coating" column. The "trivalent chromate" in the "chemical conversion coating" column in Table 4 means that a trivalent chromate coating was formed. The trivalent chromate coating will be described later.

[0167] [Table 4]

[0168] [Table 5]

[0169] A resin film was formed on the plating layer or chemical conversion film of test numbers 22 to 31. The formed resin films all had a thickness of 20 μm. The thickness of the resin film was measured using an electromagnetic film thickness gauge SDM-picоR manufactured by Sanko Electronics Laboratory Co., Ltd., and the average value of the thicknesses at nine points on the same evaluation surface was taken as the thickness of the resin film. The formed resin film contained phthalocyanine copper in the amount shown in Table 4, and further contained 1 to 30 mass % of polytetrafluoroethylene (PTFE) as a solid lubricant powder, and the remainder contained epoxy resin as a resin.

[0170] [Plating layer formation process] A Zn-Ni alloy plating layer was formed on the surface of the steel sheets of test numbers 30 and 31 by electroplating. The plating bath used was Dainjin Alloy N-PL (trademark) manufactured by Daiwa Kasei Co., Ltd. The thickness of the Zn-Ni alloy plating layer was 8 μm. The thickness of the plating layer was measured using an electromagnetic film thickness meter SDM-picоR manufactured by Sanko Electronics Laboratory Co., Ltd., and the average value of thicknesses at nine points on the same evaluation surface was taken as the thickness of the plating layer. The electroplating conditions were plating bath pH: 6.5, plating bath temperature: 25°C, current density: 2 A / dm 2 and treatment time: 18 minutes. The composition of the Zn-Ni alloy plating layer was Zn: 85% and Ni: 15%.

[0171] [Chemical film formation process] Chemical conversion coatings were formed on the surfaces of the steel sheets or plating layers of test numbers 22 to 29 and 31. Specifically, the chemical conversion treatment solutions shown in Table 5 were used for the coatings A to D. Dynechromate TR-02, manufactured by Daiwa Kasei Co., Ltd., was used as the treatment solution for forming the trivalent chromate coating. The conditions for the chemical conversion treatments for the coatings A to D were as shown in Table 5. The conditions for the chemical conversion treatment for forming the trivalent chromate coating were a bath temperature of 25°C, pH of 4.0, and a treatment time of 50 seconds.

[0172] [Coating process and curing process] A resin film was formed on the surface of the plating layer or chemical conversion coating of test numbers 22 to 31. Specifically, a composition for forming a resin film was applied to the surface of the plating layer or chemical conversion coating of test numbers 22 to 31 with a bar coder, and cured. In the composition, the components other than the solvent contained solid lubricant particles and phthalocyanine copper, and the remainder was resin. In test numbers 22 to 31, an epoxy resin was used as the resin. In test numbers 22 to 31, polytetrafluoroethylene particles were used as the solid lubricant particles. The content of phthalocyanine copper was as shown in Table 4. The composition further contained a solvent. A mixed solution of water, alcohol, and a surfactant was used as the solvent. The composition was applied with a bar coder on the chemical conversion coating when there was a chemical conversion coating, and on the plating layer when there was no chemical conversion coating, and then heat curing treatment was performed at 210 ° C for 20 minutes to form a resin film.

[0173] [Pin-on-disk test] The steel plates of test numbers 22 to 31 on which the resin coating was formed were used to evaluate the seizure resistance by a pin-on-disk type sliding tester. Specifically, the steel ball was pressed with 60 N against the steel plates of test numbers 22 to 31 attached to a rotating disk, and the rotating disk was rotated at 100 rpm. The rotating disk was rotated in only one direction. The sliding of the steel ball against the resin coating by rotating the rotating disk was performed without oil application at room temperature. The friction coefficient μ of the steel ball during sliding was measured, and the sliding distance (m) until the friction coefficient μ exceeded 0.6 (corresponding to the friction coefficient between the resin coating and the steel ball) was measured. The results are shown in the column of sliding distance until the friction coefficient exceeded 0.6 in Table 4.

[0174] [Evaluation Results] Referring to Table 4, the steel plates of test numbers 22 to 31 were provided on the surface with a resin coating containing resin, solid lubricant powder, and copper phthalocyanine. Further referring to Table 4, the resin coating formed on the steel plates of test numbers 22 to 31 had a copper phthalocyanine content of 0.2 to 9.0 mass %. As a result, the sliding distance until the friction coefficient exceeded 0.6 was long. In other words, excellent seizure resistance was demonstrated.

[0175] The steel plates of test numbers 22 to 29 and 31 had a chemical conversion coating below the resin coating. As a result, the sliding distance until the friction coefficient exceeded 0.6 was longer than that of the steel plate of test number 30 that did not have a chemical conversion coating below the resin coating. In other words, they showed even better seizure resistance.

[0176] The steel sheets of test numbers 22 to 29 were provided with coatings A to D as chemical conversion coatings. As a result, compared with the steel sheet of test number 31 provided with a trivalent chromate coating as a chemical conversion coating, the sliding distance until the friction coefficient exceeded 0.6 was longer. In other words, they showed even better seizure resistance. EXAMPLES

[0177] In Example 4, a resin coating was formed on the surface of a steel plate simulating a metal pipe for oil wells, and the seizure resistance was evaluated. Specifically, in Example 4, a cold-rolled steel plate (chemical composition: C≦0.15%, Mn≦0.60%, P≦0.100%, S≦0.050%, balance: Fe and impurities) was used.

[0178] A resin coating including a rust-preventive resin coating or a resin coating shown in Table 6 was formed on the surfaces of the steel sheets of test numbers 32 to 34. "Formed" in the "rust-preventive resin coating" column in Table 6 indicates that a rust-preventive resin coating was formed on the steel sheet surface. "-" in the "rust-preventive resin coating" column in Table 6 indicates that a rust-preventive resin coating was not formed on the steel sheet surface.

[0179] [Table 6]

[0180] [Rust-preventive resin film formation process] A rust-preventive resin film was formed on the surface of the steel plates of test numbers 32 and 33. The composition for forming the rust-preventive resin film contained 8 mass% of an anti-rust pigment and 70 mass% of an acrylic silicone resin. The composition for forming the rust-preventive resin film further contained a solvent. The composition for forming the rust-preventive resin film was spray-applied to the surface of the steel plates of test numbers 32 and 33, and cured by natural drying. The thickness of the rust-preventive resin film of test number 32 was 13 μm, and the thickness of the rust-preventive resin film of test number 33 was 11 μm. The thickness of the rust-preventive resin film was measured using an electromagnetic film thickness gauge SDM-picоR manufactured by Sanko Electronics Laboratory Co., Ltd., and the average value of the thicknesses at nine points on the same evaluation surface was taken as the thickness of the resin film.

[0181] [Coating process and curing process] For test numbers 32 and 33, an upper layer of the resin coating was formed on the surface of the rust-preventive resin coating. For test number 34, a resin coating was formed on the surface of the steel plate. Specifically, a composition for forming a resin coating was applied with a bar coder onto the surface of the steel plate or the surface of the rust-preventive resin coating of test numbers 32 to 34, and cured. In the composition, the components other than the solvent contained solid lubricant particles and phthalocyanine copper, and the remainder was resin. As the resin, an epoxy resin was used. As the solid lubricant particles, polytetrafluoroethylene particles were used. The content of phthalocyanine copper was as shown in Table 6. The composition further contained a solvent. As the solvent, a mixed solution of water, alcohol, and a surfactant was used. The composition was applied with a bar coder onto the rust-preventive resin coating when there was a rust-preventive resin coating, or onto the surface of the steel plate when there was no rust-preventive resin coating, and then heat curing treatment was performed at 210 ° C for 20 minutes to form a resin coating. The formed resin coating contained 1 to 30 mass % polytetrafluoroethylene (PTFE) as a solid lubricant powder, and the remainder contained epoxy resin as a resin.

[0182] The thickness of the resin coating of test number 32 was 35.5 μm, the thickness of the resin coating of test number 33 was 33.0 μm, and the thickness of the resin coating of test number 34 was 26.8 μm. As mentioned above, the resin coatings of test numbers 32 and 33 included an anti-rust resin coating. In other words, the thickness of the upper layer of the resin coating of test number 32 was 22.5 μm, and the thickness of the upper layer of the resin coating of test number 33 was 22.0 μm. The thickness of the resin coating was measured using an electromagnetic thickness meter SDM-picоR manufactured by Sanko Electronics Laboratory Co., Ltd., and the average value of thicknesses at nine points on the same evaluation surface was taken as the thickness of the resin coating.

[0183] [Salt spray test] A salt spray test (SST) was conducted using the steel plates with test numbers 32 to 34 on which a resin coating was formed. For the salt spray test, a salt-dry-wet combined cycle tester CY90 manufactured by Suga Test Instruments Co., Ltd. was used. The salt spray test was conducted in accordance with JIS Z 2371 (2015). The test conditions were a spray NaCl concentration of 5±0.5% and a spray volume of 1.5±0.5mL / h / 80cm. 2The temperature was 35±2° C., and the pH was 6.5 to 7.2 during the test. In this example, the time when the resin film blistered was defined as the rusting time. The rusting time (hours) for each test number obtained is shown in Table 6.

[0184] [Evaluation Results] Referring to Table 6, the steel plates of test numbers 32 to 34 were provided on the surface with a resin coating containing a resin, a solid lubricant powder, and copper phthalocyanine.

[0185] The steel sheets of test numbers 32 and 33 had a rust-preventive resin coating in the resin coating. As a result, it took longer for rust to appear than the steel sheet of test number 34, which did not have a rust-preventive resin coating in the resin coating. In other words, they showed excellent corrosion resistance.

[0186] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments without departing from the spirit of the present disclosure. [Explanation of symbols]

[0187] 1 Metal pipe for oil well 10 Tube body 10A 1st end 10B 2nd end 11 pin body 12 Coupling 40 pin 41 Male thread 42 Pin seal surface 43 Pin shoulder surface 50 Box 51 Female thread 52 Box seal surface 53 Box Shoulder Surface 70 Anti-rust resin coating 80 Plating layer 90 Chemical conversion coating 100 Resin coating 400 pin contact surface 500 Box Contact Surface

Claims

1. A metal pipe for oil wells, comprising: a tube body including a first end and a second end; The tube body includes: a pin formed on the first end; a box formed at the second end; The pin is a pin contact surface including an external thread; The box includes: a box contact surface including an internal thread; The oil well metal pipe further comprises: a resin coating containing a resin, a solid lubricant powder, and 0.2 to 30.0 mass % of phthalocyanine copper on at least one of the pin contact surface and the box contact surface; The solid lubricant powder is one or more selected from the group consisting of graphite, zinc oxide, boron nitride, talc, molybdenum disulfide, tungsten disulfide, graphite fluoride, tin sulfide, bismuth sulfide, organic molybdenum, a thiosulfate compound, and polytetrafluoroethylene; Metal pipes for oil wells.

2. The metal pipe for oil well according to claim 1, The resin coating is 0.2 to 30.0% by mass of phthalocyanine copper; 60 to 90% by weight of the resin; and 1 to 30 mass % of the solid lubricant powder. Metal pipes for oil wells.

3. The metal pipe for oil well according to claim 1 or 2, The resin coating is Contains 0.2 to 9.0% by mass of phthalocyanine copper; Metal pipes for oil wells.

4. The metal pipe for oil well use according to any one of claims 1 to 3, further comprising: a plating layer is provided between the resin coating and at least one of the pin contact surface and the box contact surface; Metal pipes for oil wells.

5. The metal pipe for oil well use according to any one of claims 1 to 3, further comprising: a chemical conversion coating is provided between at least one of the pin contact surface and the box contact surface and the resin coating; Metal pipes for oil wells.

6. The metal oil well pipe according to claim 4, further comprising: A chemical conversion coating is provided between the plating layer and the resin coating. Metal pipes for oil wells.

7. The metal pipe for oil well according to any one of claims 1 to 6, The resin coating further comprises: Contains anti-rust pigments, Metal pipes for oil wells.

8. The metal pipe for oil well according to any one of claims 1 to 7, At least one of the pin contact surface and the box contact surface is a surface that has been subjected to one or more treatments selected from the group consisting of blast treatment and pickling. Metal pipes for oil wells.

9. The metal pipe for oil well according to any one of claims 1 to 8, The resin is At least one resin selected from the group consisting of epoxy resin, phenol resin, acrylic resin, urethane resin, polyester resin, polyamideimide resin, polyamide resin, polyimide resin, and polyetheretherketone resin. Metal pipes for oil wells.

10. The metal pipe for oil well according to any one of claims 1 to 9, The pin contact surface further includes a pin seal surface and a pin shoulder surface. The box contact surface further includes a box seal surface and a box shoulder surface. Metal pipes for oil wells.

11. A method for producing a metal oil well pipe according to claim 1, providing a metal oil well pipe comprising a pipe body including a pin including a pin contact surface including a male thread portion and a box including a box contact surface including a female thread portion; applying a composition containing a resin, a solid lubricant powder, and copper phthalocyanine onto at least one of the pin contact surface and the box contact surface; and curing the applied composition to form a resin coating. A manufacturing method for metal pipes for oil wells.

Citation Information

Patent Citations

  • Special-purpose protection dope for petroleum pipe / drill pipe and its preparation method and construction method

    CN101240137A

  • Eccentric wear resisting powder paint of oil well pipe

    CN102329553A

  • Lubricant composition and method

    JP1999507678A

  • Threaded fittings for steel pipes

    JP2008527249A

  • Photocurable composition suitable for rust prevention of threaded joint for steel pipes