Zirconium and Titanium Phosphate Coatings for Implants and Other Substrates
Porous TiP and ZrP coatings address the solubility and adhesion issues of calcium phosphate coatings by ensuring long-term stability and effective tissue integration, particularly for implants, through controlled synthesis methods.
Patent Information
- Application Number
- JP2023023982
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-02-09
- Filing Date
- 2023-02-20
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2039-02-08
AI Technical Summary
Existing implant coatings, particularly those based on calcium phosphates, face issues with solubility and adhesion, leading to reduced effectiveness in promoting tissue integration and stability over time, especially under acidic conditions, and there is a lack of effective coatings for soft tissue integration.
Development of porous coatings comprising titanium phosphate (TiP) and zirconium phosphate (ZrP) with controlled crystallinity and porosity, applied using water-in-oil emulsion methods to ensure strong adhesion and stability, maintaining hydrophilicity and promoting tissue integration.
The coatings provide long-term stability and enhanced integration with both bone and soft tissues, maintaining hydrophilicity and preserving the underlying substrate's morphology, thereby improving implant fixation and integration.
Smart Images

Figure 0007583848000002 
Figure 0007583848000003 
Figure 0007583848000004
Abstract
Description
[Technical field]
[0001] The present invention provides a coating that interacts favorably with biological tissues, such as bone and soft tissues. The coating is highly resistant to mechanical wear and acidic conditions, and can therefore be retained in vivo for extended periods of time. Another object of the present invention is to create hydrophilic surfaces that can be used in a variety of applications. More specifically, coatings of metal phosphates, such as zirconium phosphate and titanium phosphate, are described. [Background technology]
[0002] Implants are used in many areas of the human body. Dental screws, hip stems and spinal fusion cages are just a few examples of devices designed to integrate with bone tissue. Ostomy bag ports, bone anchored hearing aids and dental implant abutments are examples of devices designed to integrate with soft tissue.
[0003] The choice of implant material is of course very important for the successful integration of the implant into human tissue. Titanium was discovered in the 1950s to have an excellent ability to integrate with bone and stimulate the growth of new bone tissue, a phenomenon now called osseointegration. These properties and its high mechanical strength make titanium by far the most common implant material today. Ceramics such as zirconia and alumina-toughened zirconia osseointegrate slower than titanium, but are used in applications requiring extreme hardness and strength, such as hip cups and femoral heads. Some materials are classified as bioinert; they are accepted by the human body but are not integrated. Examples of such materials are polymers such as polyamide and polyetheretherketone (PEEK).
[0004] Bone is composed primarily of calcium phosphate compounds that are chemically and structurally very similar to the mineral hydroxyapatite (HA). To improve osseointegration, calcium phosphate coatings can be applied onto implant surfaces. Although the mechanism of action is not fully understood, it is generally believed that calcium phosphate induces bone growth by adsorbing proteins involved in the first steps of bone formation. At a later stage, the coating is gradually resorbed and used as a raw material to form new bone. The beneficial effects of materials such as tricalcium phosphate (TCP) and HA on bone tissue growth are well documented and they are used clinically in various medical applications such as bone scaffolding materials and implant coatings.
[0005] One important parameter of calcium phosphate biomaterials is their resorption rate in vivo. Endogenous bone resorption is a natural process, where old bone is constantly resorbed by osteoclasts and new bone is created by osteoblasts. This resorption releases calcium and phosphorus that can be used as raw material for new bone. Osteoclasts resorb bone by creating an acidic environment. HA has very low solubility at neutral pH, but dissolves rapidly below pH 4. Increased solubility under acidic conditions is also observed for other calcium phosphates, e.g., tricalcium phosphate or octacalcium phosphate. In thick (20-60 μm) calcium phosphate-based implant coatings, in vivo dissolution can reduce the integrity of the coating and cause detachment of large calcium phosphate particles, which in turn can lead to inflammatory reactions. In thin (less than 1 μm) coatings the amount of calcium phosphate is very low and in these coatings calcium phosphate acts more like a catalyst for bone growth rather than a raw material for bone growth (Meirelles et al. J. Biomed. Mater. Res. A 2 87 299-307). A thin coating means that it dissolves quickly in vivo, usually within a few weeks or months. After this time the first step of osseointegration is finished and the long-term stability of the implant depends on the properties of the substrate. If for any reason the thin coating dissolves much faster than desired, the efficiency of the coating is greatly reduced. If the substrate itself is a material with low integration ability, this can lead to a very low fixation strength of the implant, since there is a risk that connective tissue will form on the surface instead of bone. PEEK is an example of a bioinert material with low ability to form bone tissue. This makes it very important to ensure that the bone-stimulating coating is retained over time, at least over the first critical weeks of osseointegration.
[0006] Soft tissue is a broad term for structures within the human body, such as skin, tendons, fascia, and oral mucosa. Osseointegration is a mature field of research, and while the need for surfaces that integrate and heal with bone is well known, less is known about soft tissue integration. In general, surfaces that perform well for osseointegration also show good soft tissue integration. Thus, to achieve soft tissue integration, a surface should have a high affinity for proteins and a high surface area. Thus, titanium implants and HA-coated implants have been shown to have good soft tissue integration. Porous titanium dioxide (TiO2) and silicon dioxide (SiO2) coatings have also proven effective, as described in WO 02 / 087648.
[0007] As mentioned above, calcium phosphate minerals have increased solubility at acidic pH values, and absorption of calcium phosphate (CaP) coatings is a natural process in the human body. Another important parameter that influences in vivo absorption is the adhesion strength of the coating to the substrate. For polymeric materials, the bond strength of CaP coatings to the substrate is much weaker than for highly charged surfaces such as titanium. Thus, compared to coatings on titanium, coatings on polymers placed in vivo face a higher risk of peeling or delamination of the coating from the polymeric substrate, and a higher dissolution rate.
[0008] Zirconium and titanium phosphates (abbreviated as ZrP and TiP) are inorganic layered minerals that were originally discovered to have ion-exchange properties (K.A. Kraus et al., JACS, 78(3)694, 1956). Today, zirconium phosphates are commonly used in ion exchangers, fuel cells, and as catalytic materials in a variety of applications. Due to its high charge density, and ability to adsorb other molecules, ZrP has also been investigated as a vehicle for drug delivery, as a component in polymer composites and solar energy applications, to name a few. ZrP can be synthesized in aqueous solution by mixing a water-soluble Zr source, such as zirconyl chloride (ZrOCl2), with a phosphorus source, such as phosphoric acid (H3PO4). This results in the precipitation of amorphous or poorly crystalline ZrP. The resulting product can then be converted to a fully crystalline product by boiling in H3PO4 or hydrogen fluoride (HF). By varying the synthesis conditions, various polymorphs of ZrP can be obtained, for example, α-ZrP (Zr(HPO4)2H2O) and γ-ZrP (Zr(H2PO4)(PO4)2H2O). TiP can also be synthesized in aqueous solution by mixing Ti precursors with phosphoric acid. However, Ti precursors such as TiCl4 or titanium alkoxides hydrolyze in water to form TiO2, so the synthesis must be carried out in a way that prevents TiO2 formation.
[0009] Initial reports on ZrP synthesis used simple precipitation in aqueous solutions without structure-directing agents to control particle growth. More recent work has focused on increasing the specific surface area and particle size, often through the use of surfactant systems or other soft templates. Jimenez-Jimenez et al. (Adv. Mater. 1998, (10), 10, 812-815) described the synthesis of ZrP in a surfactant-assisted system using cetyltrimethylammonium (CTMA) bromide as a structure-directing agent. The result was a 250-320m 2 A semicrystalline powder with a specific surface area of 1000 nm / g is obtained, but no method for producing a surface coating is described.
[0010] Yuko et al. (Langmuir 22(23), 2006, 9469-9472) disclose the preparation of ordered mesoporous zirconium phosphate films on silicon substrates by spin-coating using a mixture of zirconium isopropoxide, triethyl phosphate, Pluronic P123 triblock copolymer, nitric acid, ethanol and water. The film thickness was about 275 nm. The film had high proton conductivity.
[0011] WO 03 / 069712 discloses a proton conducting ceramic membrane. The membrane comprises a substrate having a coating thereon, the substrate being selected from woven or non-woven non-conductive fibers. The fibers may be glass fibers, ceramic fibers or a combination thereof. The coating comprises particles of zirconium phosphate having a particle size of less than 5000 nm, preferably 1-100 nm or 10-100 nm. The coating may also comprise agglomerates of zirconium phosphate particles, the agglomerates having a size of 1 μm or more, preferably 1-25 μm.
[0012] Korean Patent No. 10-2012-0137710 A discloses an antibacterial coating composition comprising an antibacterial compound and a porous material. The porous material may be selected from zeolite, potassium phosphate, zirconium phosphate and silica gel.
[0013] WO 2014 / 048555 describes a procedure in which a zirconium oxide surface is reacted with an acidic sodium phosphate solution to form a monolayer of phosphate ions on the surface with a thickness of less than 1.0 nm. In this example, the resulting phosphate ion layer was found to adhere very well to the ZrO2 substrate. However, this layer is not a porous ZrP or TiP coating.
[0014] US 2003 / 0157349 discloses an osteoconductive material consisting of a composite coating of metal hydroxide with surface species such as -ZrOH or -TiOH on the metal surface. The coating is immersed in a phosphate buffer and heat treated to form a phosphate layer on the metal hydroxide. The coating consists of phosphate disposed on the metal hydroxide and does not contain nano-sized ZrP or TiP.
[0015] A similar approach to forming a sensor by first creating a coating of ZrO2 on a glass surface and then applying a phosphoric acid solution to the ZrO2 coating to create a layer of phosphate on the ZrO2 coating has been described by X. Bai et al. (J. Environ. Monit., 2009, 11, 326-329). Note that although the authors describe this as a "ZrP coating", it is a phosphate ion coating on top of a ZrO2 layer, as in WO 2014 / 048555. The thickness of this ZrO2 / phosphate coating is listed as 0.9 μm.
[0016] WO 2005 / 123579 describes the production of nanosized calcium phosphates in the form of coatings or as powders. This coating method is capable of producing very thin (<150 nm) layers of nanosized calcium phosphates. The synthesis of the particles is carried out by dissolving the precursors in an acidic liquid crystal phase and crystallization is initiated by slowly increasing the pH with ammonia. The liquid crystal phase acts as a structure directing system that restricts the growth of the calcium phosphate so that nanosized crystals are produced. This method is not suitable for the production of ZrP or TiP, since these materials precipitate at low pH values and the addition of the precursors to the liquid crystal phase initiates an immediate reaction between the precursors, leading to uncontrolled crystal growth.
[0017] The literature also describes products consisting of a thin film of ZrP crystals embedded in a polymer matrix, for example by M. Wong et al. (Nature Comm. DOI: 10.1038 / ncomms4589), who describe an epoxy / α-ZrP composite, or by TC Huang et al. (RSC Adv., 2017, 7, 9908-9913), who describe a polyurethane / α-ZrP composite. These materials can be applied as thin coatings on a surface, but the coating is not pure ZrP, but consists of ZrP crystals surrounded by a polymer matrix.
[0018] There remains a need for alternative implants that include coatings that promote tissue integration. Summary of the Invention
[0019] The present invention provides a substrate comprising a coating on a surface thereof, the coating comprising titanium phosphate, zirconium phosphate or a mixture thereof, and the substrate is an implant suitable for in vivo use.
[0020] Preferably the coating is a porous coating, preferably having pores with a longest dimension of from 1 to 100 nm, and preferably the coating comprises titanium phosphate, zirconium phosphate or a mixture thereof.
[0021] The coating is preferably amorphous or has a low degree of crystallinity and preferably is continuous.
[0022] The coating typically has a thickness of about 1 to about 1000 nm. The ZrP and / or TiP in the coating has a thickness of about 5 to about 400 nm as measured by nitrogen adsorption. 2 It is preferable that the specific surface area is 100 / g.
[0023] In another embodiment, the present invention provides a substrate comprising a porous coating on a surface thereof, the coating comprising titanium phosphate, zirconium phosphate or a mixture thereof, the coating having a thickness of from 1 to 99 nm. Preferably, the coating comprises titanium phosphate, zirconium phosphate or a mixture thereof. The coating is a porous coating, preferably having pores with a longest dimension of from 1 to 100 nm.
[0024] The coating typically has a thickness of about 1 to about 1000 nm. The ZrP and / or TiP in the coating has a thickness of about 5 to about 400 nm as measured by nitrogen adsorption. 2 It is preferable that the specific surface area is 100 / g.
[0025] Preferably, the coating is amorphous or has a low degree of crystallinity, and preferably, the coating is continuous.
[0026] The present invention also provides a first method for forming a coating comprising or consisting of zirconium phosphate on a surface of a substrate, the method comprising: a) mixing a first water-in-oil emulsion containing a zirconium precursor with a second water-in-oil emulsion containing a phosphate precursor, reacting the zirconium precursor and the phosphate precursor together to form a dispersion of nano-sized zirconium phosphate particles; b) applying the dispersion to a surface of a substrate; c) optionally creating a uniform layer of the dispersion on the surface of the substrate; and d) removing any other components of the dispersion to form a coating of zirconium phosphate on the surface of the substrate.
[0027] Alternatively to the above method, step a) above can be replaced by step a1): a1) adding a phosphate precursor to a water-in-oil emulsion containing a zirconium precursor or adding a zirconium precursor to a water-in-oil emulsion containing a phosphate precursor and reacting the zirconium precursor and the phosphate precursor together to form a dispersion of nano-sized zirconium phosphate particles.
[0028] The present invention further provides a second method for forming a coating comprising or consisting of titanium phosphate on a surface of a substrate, the method comprising: e) adding a titanium precursor to the water-in-oil emulsion containing the phosphate precursor and reacting the titanium precursor and the phosphate precursor together to form a dispersion of nano-sized titanium phosphate particles; f) applying the dispersion to a surface of a substrate; g) optionally creating a uniform layer of the dispersion on the surface of the substrate; and h) removing any other components of the dispersion to form a coating of titanium phosphate on the surface of the substrate.
[0029] The present invention further provides a third method for forming a coating comprising or consisting of titanium and / or zirconium phosphate on a surface of a substrate, the method comprising: a) mixing a solution comprising zirconium and / or titanium precursors in an organic (non-aqueous) solvent with a water-in-oil emulsion comprising phosphate precursors, and reacting the zirconium and / or titanium precursors and the phosphate precursors together to form a dispersion of nano-sized zirconium phosphate and / or titanium phosphate particles; b) applying the dispersion to a surface of a substrate; c) optionally producing a uniform layer of the dispersion on a substrate; and d) removing any other components of the dispersion to form a coating of zirconium phosphate and / or titanium phosphate on the substrate.
[0030] The present invention further provides a method of increasing the hydrophilicity of a surface of a substrate, the method comprising forming a coating on the surface of the substrate using any of the methods of the present invention described above. Preferably, the substrate is a polymeric substrate, more preferably PEEK.
[0031] The present invention also provides a coated substrate obtainable by any of the processes of the present invention.
[0032] The substrate can be an implant such as a dental screw, a hip stem, a spinal fusion cage, an ostomy bag port, a bone anchored hearing aid, a dental implant abutment, and an external fixation device. The substrate can also be a structure where a hydrophilic surface is desirable, such as a sensor or a component of a medical device. [Brief description of the drawings]
[0033] [Figure 1a] SEM image of the inventive ZrP coating on a titanium disk using a Pluronic L64 / p-xylene / water system. Scale bar = 200 nm. [Figure 1b] SEM image of the inventive ZrP coating on a titanium disk using a Triton X-100 / 1-hexanol / cyclohexane / water system. Scale bar = 200 nm. [Diagram 2] SEM image of the inventive TiP coating on a titanium disk. Scale bar = 100 nm. [Diagram 3] SEM images at low and high magnification of a blasted PEEK screw coated with ZrP according to the present invention, scale bars = 200 μm and 200 nm. [Figure 4] Total amount of ZrP (calculated as the sum of atomic % Zr and P) determined by XPS for ZrP disks immersed in acetic acid or sonicated in water. [Diagram 5]Calcium content of uncoated and ZrP coated PEEK and titanium disks immersed in Simulated Body Fluid (SBF) as measured by XPS. [Figure 6] Contact angle measurements on uncoated and ZrP-coated PEEK after 1 and 2 weeks in a simulated salt water solution. [Figure 7] SEM image of a PEEK disk first coated with ZrP and then coated with nanosized HA. Scale bar = 500 nm. [Figure 8] Removal torque values of blasted PEEK implants (uncoated and ZrP coated) 6 weeks after implantation in rabbit tibias. [Figure 9] Liquid adsorption of water on dental implant screws after different storage times. ●=heat treated, ■=ZrP coated, ▲=HA coated. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] Unless otherwise indicated, the following description applies to any type of substrate and to any embodiment of the present invention.
[0035] The coatings of the present invention are formed from titanium phosphate (TiP) and / or zirconium phosphate (ZrP). Preferably, they are formed directly on the surface of the substrate without an intervening layer or coating. Acidic phosphate-based materials such as ZrP or TiP strongly interact with surfaces that can form bonds with phosphate groups. Thus, the coatings have high adhesion strength not only to metals such as titanium and zirconium, but also to ceramics such as ZrO2 and Al2O3, and polymers such as PEEK. Like HA, ZrP strongly adsorbs to proteins and amino acids, but one notable difference between HA and ZrP is their stability at different pHs. HA is stable under basic conditions and begins to dissolve at low pH values, while ZrP behaves in the opposite way, being stable at low pH values but beginning to dissolve under basic conditions. This makes ZrP highly resistant to the acidic environment that occurs during the natural dissolution process in the human body. TiP has similar properties to ZrP in terms of protein adsorption and stability in acidic conditions, but TiP has a higher solubility at alkaline pH values. Thus, ZrP and TiP coatings last long term in vivo, eg, are essentially permanent.
[0036] ZrP or TiP implant coatings are resistant to acidic conditions and have a high tendency for protein adsorption. Furthermore, coatings with features in the nanometer range increase the surface energy and specific surface area of the underlying substrate, thus improving protein adhesion. Such coatings also increase the hydrophilicity of the substrate, whether it is a polymer such as PEEK or a metal such as titanium. Hydrophilic surfaces are desirable for osseointegration and soft tissue integration, but are also attractive for other applications, as they help to prevent air bubble formation in sensors and increase wetting in catheters, for example. The coating can be made very thin and continuous, allowing it to follow the underlying structure of the implant and thereby preserve the topography of the implant surface. Many commercially available implants have a surface roughness in the micrometer range (arithmetic mean height of the surface (S a) are typically machined to have a roughness of 0.5-2 μm, so coatings on these surfaces must be thin to maintain micron-sized roughness.
[0037] Materials such as ZrP or TiP are more brittle than polymers or metals, and this difference in mechanical properties can cause problems if the coating is too thick. For example, when a coated polymer material is subjected to a bending force, the dimensional deformation is quite different between the coating and the polymer substrate. For a given shape, the flexibility of any material increases as its thickness decreases, so a thin coating is more resilient to bending than a thicker coating. Therefore, if the substrate is a polymer or metal substrate, it is advantageous to have a relatively thin ZrP or TiP coating.
[0038] Base material The coating can be applied to any suitable substrate, including, but not limited to, substrates made from metals such as titanium and its alloys, zirconium and its alloys, stainless steel, tantalum, NiTi alloys, and cobalt-chromium alloys; ceramics such as alumina, zirconia, alumina-reinforced zirconia, and Si3N4; graphitic materials such as graphene and pyrocarbon; silicon; and polymers such as polypropylene, polyethylene, polysulfone (PSU), polyetherketoneketone (PEKK), poly(styrene), poly(carbonate), poly(ethylene terephthalate), and PEEK. Preferred substrates include titanium and its alloys, zirconium and its alloys, stainless steel, tantalum, NiTi alloys, cobalt-chromium alloys, alumina, zirconia, alumina-reinforced zirconia, pyrocarbon, polysulfone (PSU), polyetherketoneketone (PEKK), poly(styrene), poly(carbonate), and PEEK. More preferred substrates include titanium and its alloys, stainless steel, zirconia, alumina toughened zirconia, pyrocarbon and PEEK, most preferably PEEK.
[0039] The preferred substrate is in the form of an implant for in vivo use. In the case of an implant, the substrate is preferably biocompatible. Suitable implants include dental screws, hip stems, spinal fusion cages, ostomy bag ports, bone-anchored hearing aids, dental implant abutments and external fixation devices. To accelerate integration after implantation in the human or animal body, implants with rough surfaces are preferred. Preferred substrates for implants include titanium and its alloys, stainless steel, cobalt-chromium alloys, zirconia, alumina-reinforced zirconia, pyrocarbon and PEEK, most preferably PEEK.
[0040] The ZrP and TiP coatings of the present invention are hydrophilic. Thus, the substrate can be any device or component for which it is beneficial to have a hydrophilic surface. Preferred substrates that are made hydrophilic include polymeric substrates, especially PEEK substrates. For example, the formation of air bubbles can distort measurements using sensors. Since air bubbles tend to adhere to hydrophobic surfaces, making the surface of the sensor hydrophilic by coating with ZrP and / or TiP according to the present invention can help prevent air bubbles from forming. Other substrates for which a hydrophilic surface may be preferred include catheters, tubes, nozzles and cables, for example cables made of polymeric materials such as PEEK. Thus, further preferred substrates are sensors or sensor components, catheters and tubes.
[0041] The coated substrates of the present invention may also be useful in membrane separations, optical devices, electronic devices including membrane electrode assemblies, and fuel cells.
[0042] coating The coating may be present over the entire surface of the substrate or over only a portion of the surface. For implants, it is preferred that at least 25% (by area) of the body-facing surface of the implant is coated, more preferably at least 40%, at least 50% or at least 70%.
[0043] A thin coating is desirable to maintain the underlying surface morphology. A thick coating may exhibit a tendency to crack or delaminate relative to the substrate. Thus, preferably, when the substrate is an implant, the coating thickness is 1000 nm or less, such as about 1 to about 1000 nm or about 5 to about 1000 nm. The lower limit of the thickness is preferably at least about 1 nm, more preferably at least about 3 nm, even more preferably at least about 5 nm, such as at least about 10 nm. The upper limit of the thickness is preferably about 500 nm or less, more preferably about 300 nm or less, even more preferably about 250 nm or less, such as about 200 nm or less. More preferably, the coating thickness is in the range of about 5 to about 150 nm or about 5 to about 100 nm. Most preferably, the coating thickness is about 10 to about 40 nm. The range obtained by combining any of the above lower limits with any of the above upper limits is also included in the present invention.
[0044] For other types of substrates, the coating thickness is less than 100 nm, preferably about 1 to about 99 nm. The lower thickness limit is preferably at least about 1 nm, more preferably at least about 3 nm, even more preferably at least about 5 nm, for example at least about 10 nm. The upper thickness limit is preferably about 95 nm or less, more preferably about 80 nm or less, even more preferably about 40 nm or less. More preferably, the coating thickness is in the range of about 5 to about 95 nm or about 5 to about 80 nm. Most preferably, the coating thickness is about 10 to about 40 nm. Ranges obtained by combining any of the above lower limits with any of the above upper limits are also included in the present invention.
[0045] Preferably, the specific surface area of the ZrP and / or TiP in the coating, as measured via nitrogen adsorption and using the Brunauer-Emmett-Teller (BET) model, is between about 5 and about 400 m. 2 More preferably, the specific surface area is about 50 to about 350 m 2More preferably, the specific surface area is in the range of about 100 to about 250 m / g. 2 / g range. The specific surface area of the ZrP and / or TiP in the coating cannot be measured directly. Rather, it can be measured by calcining (burning) a portion of the coating dispersion and analyzing the resulting powder.
[0046] The coating of the present invention is preferably porous. By porous, it is meant that the coating is capable of absorbing gas or liquid. Preferably, the coating has pores with a longest dimension of about 1 to about 100 nm. As used herein, a coating formed from particles of ZrP or TiP is also considered to be porous if there is space between adjacent particles in the coating, thereby allowing for the absorption of gas or liquid. Pore size can be measured using SEM and image analysis. Specific surface area also serves as an indirect measure of the porosity of the coating. A higher specific surface area generally corresponds to a more porous coating.
[0047] As mentioned above, many implants have roughened surfaces to accelerate in vivo integration. The present invention makes it possible to create very thin coatings that preserve the underlying surface morphology of the substrate, thus allowing features in the micrometer range to be coated without significantly changing the roughness.
[0048] Measuring the thickness of a coating can be done in several ways. For very thin coatings, between 1 and 10 nm thick, X-ray photoelectron spectroscopy (XPS) can be used to estimate the thickness. XPS measures the atomic content from the top 10 nm of the substrate, so if the coating is homogeneous and uniformly distributed, the XPS measurement, which returns a signal from the underlying substrate, will indicate a coating thickness in the range of 1 to 10 nm. For relatively thick coatings, for example >10 nm to <100 nm, the thickness can be measured, for example, by dissolving the coating in a strongly alkaline medium and measuring the atomic content of the extracted medium using inductively coupled plasma atomic emission spectroscopy (ICP-AES). Another way to measure coatings in this thickness range is by performing a milling and lift-out procedure followed by transmission electron microscopy (TEM) analysis. For relatively thick coatings (>100 nm), the thickness can be measured by examining a cross-section of the coated substrate using a scanning electron microscope (SEM).
[0049] Preferably, the coating is formed from amorphous or low crystalline ZrP and / or TiP. Amorphous or low crystalline ZrP or TiP can be optionally converted to highly crystalline ZrP or TiP by suitable treatment. Methods for converting amorphous or low crystalline ZrP or TiP to highly crystalline materials are known in the art. However, conversion to highly crystalline ZrP or TiP generally requires treatment with boiling phosphoric acid or boiling hydrofluoric acid, or heat treatment. Therefore, it is not suitable unless the substrate can withstand the treatment conditions.
[0050] method The present invention also provides a method for forming a ZrP and / or TiP coating on a substrate, and a method for improving or increasing the hydrophilicity of a substrate.
[0051] The present invention provides a first method for forming a coating comprising or consisting of zirconium phosphate on a surface of a substrate, the method comprising: a) mixing a first water-in-oil emulsion comprising a zirconium precursor and optionally a surfactant with a second water-in-oil emulsion comprising a phosphate precursor and optionally a surfactant, reacting the zirconium precursor and the phosphate precursor together to form a dispersion of nano-sized zirconium phosphate particles; b) applying the dispersion to a surface of a substrate, preferably by dripping, spraying or immersing the substrate in the dispersion; c) optionally forming a uniform layer of the dispersion on the surface of the substrate, preferably by rotating the substrate, capillary extraction, using a gravimetric force, or applying a stream of compressed gas onto the substrate; and d) removing any other components of the dispersion, preferably by heat treatment, plasma treatment, liquid extraction or a combination thereof, to form a coating of zirconium phosphate on the surface of the substrate.
[0052] Alternatively to the above method, step a) above can be replaced by step a1): a1) adding a phosphate precursor to a water-in-oil emulsion comprising a zirconium precursor and optionally a surfactant, or adding a zirconium precursor to a water-in-oil emulsion comprising a phosphate precursor and optionally a surfactant, and reacting the zirconium precursor and the phosphate precursor together to form a dispersion of nano-sized zirconium phosphate particles.
[0053] The present invention further provides a second method for forming a coating comprising or consisting of titanium phosphate on a surface of a substrate, the method comprising: e) adding the titanium precursor to a water-in-oil emulsion containing the phosphate precursor and optionally a surfactant, and reacting the titanium precursor and the phosphate precursor together to form a dispersion of nano-sized titanium phosphate particles; f) applying the dispersion to a surface of a substrate, preferably by dripping, spraying or immersing the substrate in the dispersion; g) optionally forming a uniform layer of the dispersion on the surface of the substrate, preferably by rotating the substrate, capillary extraction, using gravimetry, or applying a stream of compressed gas onto the substrate; and h) removing any other components of the dispersion, preferably by heat treatment, plasma treatment, liquid extraction or a combination thereof, to form a coating of titanium phosphate on the surface of the substrate.
[0054] The present invention further provides a third method for forming a coating comprising or consisting of titanium and / or zirconium phosphate on a surface of a substrate, the method comprising: a) mixing a solution comprising zirconium and / or titanium precursors and optionally a surfactant in an organic (non-aqueous) solvent with a water-in-oil emulsion comprising a phosphate precursor and a surfactant, reacting the zirconium and / or titanium precursors and the phosphate precursor together to form a dispersion of nano-sized zirconium phosphate and / or titanium phosphate particles; b) applying the dispersion onto a solid surface, preferably by dripping, spraying or immersing a substrate in the dispersion; c) optionally forming a uniform layer of the dispersion on the substrate, preferably by using rotation, capillary extraction, gravimetry, or applying a stream of compressed gas onto the substrate; and d) removing any other components of the dispersion, preferably by heat treatment, plasma treatment, liquid extraction or a combination thereof, to form a coating of zirconium phosphate and / or titanium phosphate on the substrate.
[0055] The present invention further provides a method of increasing the hydrophilicity of a surface of a substrate, the method comprising forming a coating on the surface of the substrate using any of the methods of the present invention described above.
[0056] In the method of the present invention, nano-size refers to particles having a longest dimension between 1 and 100 nm.
[0057] Preferably, each of the starting emulsions and solutions for use in the methods of the present invention also contains one or more surfactants.
[0058] The titanium precursor may be any suitable titanium salt or compound that can be dissolved in a suitable organic solvent, such as titanium tetrachloride (TiCl4), titanium ethoxide, titanium isopropoxide, and titanium diisopropoxide bis(acetylacetonate). Many titanium compounds, including TiCl4 and titanium isopropoxide, hydrolyze to form titanium dioxide when in contact with water. Therefore, it is important to avoid premature contact of the titanium precursor with water in the synthesis of titanium phosphate coatings. Therefore, the preferred titanium precursor is a compound that is soluble in an organic solvent. Titanium salts or compounds that are insoluble in water, such as titanium dioxide, titanium sulfate, titanium carbide, or titanium phosphate, are not suitable for use as precursors.
[0059] The zirconium precursor can be any suitable zirconium salt or compound, including zirconium tetrachloride (ZrCl4), zirconyl oxychloride, zirconyl nitrate, zirconium ethoxide, zirconium isopropoxide, and zirconium diisopropoxide bis(acetylacetonate). When used in the first method, the zirconium precursor should be water-soluble so that it is present in the water phase of the water-in-oil emulsion. Suitable water-soluble precursors include zirconium tetrachloride, zirconyl oxychloride, and zirconyl nitrate. When used in the third method, the zirconium precursor should be soluble in an organic solvent. Suitable organic-soluble precursors include zirconium ethoxide, zirconium isopropoxide, and zirconium diisopropoxide bis(acetylacetonate).
[0060] The phosphorus precursor may be phosphoric acid (H3PO4), Na3PO4, Na2HPO4, NaH2PO4, K3PO4, K2HPO4, KH2PO4, phosphorous acid (H3PO3), hypophosphorous acid (H3PO2), or a phosphite ester such as triethyl phosphite. Preferably, the phosphorus precursor is water soluble so that it is present in the aqueous phase of a water-in-oil emulsion.
[0061] The metal precursors and phosphate precursors can be used in any suitable molar ratio to provide, for example, a molar ratio of Zr to phosphate of about 1:1 to about 1:3, or a molar ratio of titanium to phosphate of about 1:2.
[0062] The water-in-oil emulsions used in the method of the invention are preferably microemulsions. Emulsions typically contain surfactants, although any surfactant-stabilized system with nano-sized aqueous domains could potentially be used. Microemulsions generally contain a dispersed phase present as droplets or domains of about 1-100 nm in diameter, for example about 10-50 nm in diameter, dispersed within a continuous phase. In water-in-oil microemulsions, water forms the dispersed phase and an organic solvent (oil) that is immiscible or substantially immiscible with water forms the continuous phase. Surfactants are usually present at the interface between the dispersed and continuous phases to help stabilize the emulsion (K. Holmberg et al. Surfactants and Polymers in aqueous solutions, Wiley, ISBN 0-471-49883-1). One beneficial property of microemulsions is their ability to wet and spread on almost any surface, whether it is a polar and hydrophilic surface such as titanium or a non-polar and hydrophobic surface such as PEEK.
[0063] Without being bound by theory, it is believed that the dispersed water domains, preferably covered by surfactant, in the starting water-in-oil emulsion act as nano-sized (e.g., having diameters in the range of about 1 to about 100 nm) reaction vessels that prevent the growing particles of ZrP or TiP from colliding and growing into larger aggregates, resulting in a dispersion in which the water domains contain dispersed nano-sized ZrP or TiP particles.
[0064] Emulsions for use in the method of the present invention can be formed using various surfactant / solvent / water combinations.Surfactants suitable for use in the method herein include, but are not limited to, nonionic surfactants, such as poly(propylene oxide) (PPO)-poly(ethylene oxide) (PEO) surfactants, such as PEO-PPO-PEO and PPO-PEO-PPO surfactants, alcohol ethoxylates (C-EO), polysorbates, linear alcohols, fatty acid amides, alkylphenol ethoxylates and polyglycerol alkyl ethers, anionic surfactants, such as alkyl phosphates, alkyl sulfonates and alkyl sulfates, and cationic surfactants, such as quaternary ammonium salts.Preferred surfactants include poly(ethylene oxide)-poly(propylene oxide)-poly(ethylene oxide) (PEO-PPO-PEO) block copolymers Pluronic L64 and Pluronic P84, and alkylphenol ethoxylates. Suitable alkylphenol ethoxylates include those available from The Dow Chemical Company under the Triton trademark, such as Triton X-100, which has a CAS Registry Number of 9002-93-1 and is characterized by the formula: [ka] In the formula, n is 9 to 10.
[0065] Suitable organic solvents for making the starting emulsion or solution include any solvent that is immiscible or substantially immiscible with water, such as aliphatic, aromatic and cyclic hydrocarbons, alcohols, esters, ethers, ketones and mixtures thereof. Preferred organic solvents include p-xylene, cyclohexane and hexadecane and combinations thereof.
[0066] When two different emulsions, or an emulsion and an organic solution, are used in the methods disclosed herein, it is preferred that the same organic solvent is used in both, as well as the same surfactant be used in both.
[0067] In the mixing step of the method of the present invention, mixing should be continued for a sufficient time for the metal precursor and phosphate precursor to react together to form TiP or ZrP. Typically, mixing should continue for about 5 to about 24 hours, preferably about 6 hours, to ensure that the reaction is complete. ZrP and TiP are insoluble in water and the organic solvents used, and therefore precipitate to produce a colloidal dispersion of ZrP and / or TiP. As used herein, colloidal dispersion refers to particles dispersed in a liquid and having a size of about 1 to about 1000 nm.
[0068] Application of the dispersion to the surface of the substrate can be done using any technique known in the art, including spraying, dip coating, or by dropwise application. Equipment such as a spin coater can be used to control the thickness of the coating liquid layer by removing excess coating dispersion and spreading the liquid to create a uniform layer on any desired surface of the substrate.
[0069] Once the coating dispersion is applied to the substrate, the components of the dispersion other than TiP or ZrP, such as water, organic solvent and any surfactant, must be removed to leave only the layer of zirconium phosphate or titanium phosphate. This causes the nano-sized particles of ZrP and / or TiP to aggregate or fuse together to form a continuous porous coating. Drying can be used to remove the water and any organic solvent, but other methods may be required to remove any surfactant present. A convenient method to remove all other components is to use a heat treatment at a temperature high enough to burn off the surfactant and evaporate the water and organic solvent. Heat treatment can also increase the adhesion between the phosphate compound and the substrate, and has the added benefit of providing a sterile coated substrate, making it attractive that the coating process can be carried out in an industrial environment. Because the layer of the coating dispersion is very thin, the heat treatment can be carried out in a short period of time, such as about 5 to about 10 minutes or less. This short heat treatment does not affect the mechanical properties of the substrate material. Suitable temperatures for heat treatment are about 300 to about 550°C for metals such as titanium and about 300 to about 350°C for polymers such as PEEK.
[0070] Another method to remove the organic and aqueous components of the coating dispersion is to perform an extraction using a suitable solvent such as isopropanol or p-xylene to remove the surfactant and solvent. This method is particularly suitable for materials that cannot withstand high temperature processing, such as low melting point polymers.
[0071] Yet another method of removing the organic and aqueous components of the coating dispersion is to use a plasma cleaning device. By treating the implant surface with an ionized gas (plasma) in a vacuum chamber, any organic components of the dispersion, such as surfactants, can be completely oxidized and removed while the water and organic solvents evaporate.
[0072] One advantage of the methods of the present invention is that they can be used to form a coating, preferably a continuous coating, over the entire exposed surface of a substrate, such as a substrate with a complex shape.This is particularly advantageous for implants made from polymers, since implants made from polymers often have complex shapes and it may be difficult to coat the entire surface using conventional techniques.Because the methods of the present invention are wet chemical techniques, they are very suitable for use in coating complex structures that are 3D printed (additive manufacturing) or for coating structures such as metal foams, as opposed to line of sight techniques such as chemical vapor deposition, physical vapor deposition or plasma spraying.
[0073] As mentioned before, many implants have a rough surface to accelerate integration. The method of the invention makes it possible to create very thin coatings that allow coating features in the micrometer range without significantly changing the roughness. The thickness of the coating can be varied, for example, by changing the concentration of precursors in the starting emulsion or solution, by changing the rotation speed during the spin-coating procedure, and / or by applying compressed air during the spin-coating procedure. Another way to control the thickness on porous structures, such as 3D printed structures or metal foams, is to remove a certain amount of the coating microemulsion from the structure by capillary extraction before the drying step. In this method, the coated substrate is placed on a porous material that has the ability to extract the coating liquid from the coated substrate. Depending on the material, pore size and thickness of the porous material, the amount of coating liquid extracted can vary, which affects the thickness of the coating layer after drying.
[0074] The TiP and / or ZrP coatings render the surface of the substrate to which they are applied hydrophilic for polymers, or superhydrophilic (water contact angle <10°) for metals. Thus, the present invention further provides a method of increasing the hydrophilicity of the surface of a substrate, the method comprising forming a coating on the surface of the substrate using any of the methods of the present invention described above.
[0075] Although porous coatings are preferred for implants, non-porous coatings can also be used. Non-porous coatings can be formed on substrates using chemical vapor deposition, physical vapor deposition or plasma spray techniques. However, these techniques are line-of-sight techniques that may not be suitable for coating rough surfaces, 3D printed structures or complex structures such as metal foams.
[0076] TiP and ZrP coatings may be functionalized after formation, for example, by adding additional coating layers and / or active compounds. The active compounds may be adsorbed by the coating or attached to the coating. Suitable active compounds include substances that stimulate bone growth or prevent bacterial growth. Substances that can stimulate bone tissue growth include, but are not limited to, bone morphogenetic proteins (BMPs), bisphosphonates, calcium phosphates, calcium ions, and magnesium ions. It is also possible to functionalize the coating with the attachment of substances that prevent bacterial growth, including, but are not limited to, antibiotics such as gentamicin or chlorhexidine, endogenous substances such as defensins, or inorganic antibiotics such as silver or zinc.
[0077] Functionalization can be carried out by immersing the coated substrate in a solution or dispersion of the desired active compound or mixture of active compounds.
[0078] Additional coating layers may be deposited on the TiP or ZrP coating using known techniques for coating substrates. For example, a layer of hydroxyapatite or other calcium phosphate may be deposited using the method of WO 2005 / 123579. Preferred additional coating layers include amorphous calcium phosphate, monocalcium phosphate, dicalcium phosphate, tricalcium phosphate, tetracalcium phosphate, hydroxyapatite, octacalcium phosphate or mixtures thereof, more preferably hydroxyapatite. In this way, a composite coating may be created on the implant, where the top layer is absorbed in a few months and stimulates bone growth, and the bottom layer of TiP or ZrP serves as a stable substrate that is not absorbed over time.
[0079] The present invention includes any and all combinations of the preferred features disclosed herein. In particular, any preferred feature of the coated substrate is also a preferred feature of the coated substrate obtainable by the method of the present invention.
[0080] example The following are non-limiting examples of the present invention. Abbreviation: PBS - Phosphate Buffered Saline Sa - arithmetic mean height of the surface SBF-Simulated body fluid
[0081] Example 1a. Preparation of ZrP coating dispersion In beaker 1, the following ingredients were mixed to form a microemulsion: 17.5g Pluronic L64 (BASF) 53.75g p-xylene (Sigma-Aldrich) 3.75g H2O 0.500g ZrCl4 (Sigma-Aldrich)
[0082] In beaker 2, the following ingredients were mixed to form a microemulsion: 17.5g Pluronic L64 (BASF) 53.75g p-xylene (Sigma-Aldrich) 3.75g H2O 0.495g H3PO4 85% (Fluka)
[0083] The contents of Beaker 2 were poured into Beaker 1 and the resulting mixture was placed on a magnetic stirrer for 24 hours. The resulting dispersion was translucent with slight haze.
[0084] Example 1b. Preparation of alternative ZrP coating dispersions In beaker 1, the following ingredients were mixed to form a microemulsion: 12.5g Triton X-100(Sigma-Aldrich) 3.1g 1-hexanol (Sigma-Aldrich) 23.5g cyclohexane 3.40ml H2O 0.626g ZrOCl2*8H2O
[0085] In beaker 2, the following ingredients were mixed to form a microemulsion: 12.5g Triton X-100(Sigma-Aldrich) 3.1g 1-hexanol (Sigma-Aldrich) 23.5g cyclohexane 3.40ml H2O 0.448g H3PO4 85% (Fluka)
[0086] The contents of Beaker 2 were poured into Beaker 1 and the resulting mixture was placed on a magnetic stirrer for 24 hours. The resulting dispersion was translucent and slightly hazy.
[0087] Example 2. Preparation of TiP coating dispersion In beaker 1, the following ingredients were mixed to form a solution: 17.5g Pluronic L64 (BASF) 53.75g p-xylene (Sigma-Aldrich) 0.500g Titanium isopropoxide (Sigma-Aldrich)
[0088] In beaker 2, the following ingredients were mixed to form a microemulsion: 17.55g Pluronic L64 (BASF) 53.75g p-xylene (Sigma-Aldrich) 7.5g H2O 0.406g H3PO4 85% (Fluka)
[0089] The contents of Beaker 2 were poured into Beaker 1 and the resulting mixture was placed on a magnetic stirrer for 24 hours. The resulting dispersion was translucent with slight haze.
[0090] Example 3a. Application of nano-sized ZrP coatings on titanium disks A titanium disk with a diameter of 6 mm and a thickness of 2 mm was roughened using grade 400 sandpaper and then washed with isopropanol, 1 M HNO3, and water. The disk was placed on a spin-coating apparatus, after which 85 μl of the coating dispersion prepared in Example 1a was added. The disk was then spun at 2200 rpm for 3 seconds using the spin-coating apparatus. The disk was allowed to dry at room temperature and then placed in an oven set at 450 °C in an oxygen-enriched atmosphere for 5 minutes. After heat treatment, the disk was cooled to room temperature and analyzed by SEM and XPS. An SEM image of the coated disk is shown in Figure 1a (scale bar = 200 nm). As can be seen from this high magnification image, the coating has a porous appearance, with pore sizes ranging from 10 to 30 nm.
[0091] Example 3b. Application of nano-sized ZrP coatings on titanium disks To study the appearance of coating dispersions with different compositions, a titanium disk with a diameter of 6 mm and a thickness of 2 mm was roughened using sandpaper grade 400 and then washed with isopropanol, 1 M HNO3, and water. The disk was placed on a spin-coating apparatus, after which 85 μl of the coating dispersion prepared in Example 1b was added. The disk was then spun at 2200 rpm for 3 seconds using the spin-coating apparatus. The disk was dried at room temperature and then placed in an oven set at 450° C. in an oxygen-enriched atmosphere for 5 minutes. After heat treatment, the disk was cooled to room temperature and analyzed by SEM and XPS. An SEM image of the coated disk is shown in FIG. 1b (scale bar=200 nm). As can be seen from this image, the coating has a similar appearance to the coating dispersion described in Example 1a.
[0092] Example 4. Application of nano-sized TiP coatings on titanium discs A titanium disk with a diameter of 6 mm and a thickness of 2 mm was roughened and cleaned according to Example 3. The disk was placed on a spin-coating apparatus, after which 85 μl of the coating dispersion prepared in Example 2 was added. The disk was then spun at 3000 rpm for 10 seconds using the spin-coating apparatus. The disk was heat treated according to Example 3a. The disk was cooled to room temperature and analyzed by SEM and XPS. An SEM image of the coated disk is shown in FIG. 2 (scale bar=100 nm). As can be seen, the coating has a similar appearance to the ZrP coating, with a porous foam-like structure. The pore size is in the same range as the ZrP coating. At the top of this image, machined stripes are visible, and interestingly, these patterns continue through the coated area, indicating that the coating follows the underlying topography.
[0093] Example 5. Application of nano-sized ZrP coating on PEEK screw A PEEK screw (machined from PEEK-Optima (Invibio Ltd)) with a diameter of 3.5 mm and a length of 4 mm was blasted to a roughness (Sa) of 1.1 μm using an absorbent blasting medium (hydroxyapatite, RBM WAS 180-300, Medical Group Corp, France). The roughness before blasting was 0.55 μm (Sa). The implant was coated by dissolving the RBM medium and applying 85 μl of the coating dispersion prepared in Example 1a onto the implant and spinning at 2500 rpm and 5 seconds on a spin-coating device. The implant screw was dried at room temperature and then placed in an oven set at 340° C. in an oxygen-enriched atmosphere for 5 minutes. After heat treatment, the screw was cooled to room temperature and analyzed by SEM and XPS. SEM images of the coated screw at low magnification (40X) and high magnification (40000X) are shown in FIG. 3. At low magnification (top image, scale bar 200 μm), the coating is not visible, indicating that the topography does not change at this size level. At high magnification (bottom image, scale bar 200 nm), the coating can be seen as a porous layer on top of the substrate.
[0094] Example 6. Investigation of adhesion and acid resistance of ZrP coatings. Machined PEEK screws of 3.5 mm and 4 mm diameter were coated according to the parameters used in Example 5. One group of screws was immersed in a beaker of 200 ml water and sonicated for 5 minutes. Another group was immersed in a beaker of 200 ml acetic acid at pH 4. The screws were washed, dried and analyzed by XPS. The results are shown in Figure 4 (total amount of ZrP measured using XPS, calculated as the sum of atomic % Zr and P). As this shows, the ZrP coating was not affected by the sonication or exposure to acidic pH.
[0095] Example 7. Investigation of the mineralization properties of ZrP coatings Titanium and PEEK discs with a diameter of 6 mm and a thickness of 2 mm were roughened and cleaned as described in Example 3a. The titanium discs were coated using the parameters described in Example 3a. The PEEK discs were coated by spinning at 2500 rpm for 3 seconds and at a temperature of 325°C for 5 minutes in an oxygen atmosphere. The discs were then immersed in Dulbecco's PBS (1x) with Ca&Mg (simulated body fluid) from PAA Cell Culture Company. After 24 hours, the discs were removed from the SBF bath and rinsed thoroughly with Type 1 (ultrapure) water. The discs were dried and then analyzed by XPS. The amount of calcium measured for the various samples using XPS is shown in Figure 5. As can be seen from this figure, no calcium was detected in the untreated PEEK. 2.8% calcium was detected in the ZrP coated discs. As a comparison, titanium discs were also included in this study and the amount of calcium in these discs was about twice the amount detected for the ZrP coated PEEK discs (5.6%). This indicates that the ZrP coating on the PEEK substrate produces a surface that induces mineralization, a property known to be critical for bone cell growth.
[0096] Example 8. Investigation of coating stability and hydrophilicity of ZrP coatings on PEEK discs immersed in simulated saline water PEEK disks with a diameter of 6 mm and a thickness of 2 mm were roughened and cleaned according to Example 3a. Half of the disks were coated with ZrP as described in Example 3a, and the other half was left uncoated and used as a control sample. The disks were immersed in a salt solution designed to mimic the composition of natural seawater, containing 24.615 g / l NaCl, 4.105 g / l Na2SO4, 11.06 g / l MgCl2·6H2O, and 1.558 g / l CaCl2·2H2O. The solution was adjusted to pH 8 using 0.2 M NaOH solution. Half of the disks were coated with ZrP, and the other half was left uncoated and used as a control sample. After 1 and 2 weeks, the disks were removed from the salt solution. The disks were washed with Type 1 water, dried, and the water contact angle was analyzed. The results of this analysis are shown in Figure 6. As can be seen, before immersion in the saline solution, the ZrP coated disk was hydrophilic with a contact angle of about 45°, whereas the uncoated disk was hydrophobic with a contact angle of about 110°. The difference in contact angle between the coated and uncoated disks was almost the same after 1 week and 2 weeks. The coated disks maintained their hydrophilicity with a contact angle of 45-50°, whereas the uncoated disks were hydrophobic with a contact angle of 90-100°. This indicates that the hydrophilicity was maintained in the ZrP coated samples.
[0097] Example 9. Preparation of ZrP and HA combination coatings A PEEK disk with a diameter of 6 mm and a thickness of 2 mm was roughened and cleaned as described in Example 3a. The PEEK disk was placed on a spin-coating apparatus, after which 75 μl of the coating dispersion described in Example 1a was added. Using the spin-coating apparatus, the disk was spun at 1300 rpm for 3 seconds. The disk was dried at 120° C. for 10 minutes and then cooled at room temperature for 5 minutes. The disk was then placed in a furnace set at 325° C. in an air-fed atmosphere for 5 minutes. After heat treatment, the disk was cooled to room temperature.
[0098] The coated PEEK was again placed on the spin-coating apparatus and the above process was repeated, except that the coating dispersion used was the one described in Example 2 of WO 2005 / 123579. After heat treatment, the disk was cooled to room temperature and analyzed by XPS. This analysis showed 8.8% Ca and 5.5% P along with traces of Zr, indicating that the CaP coating behaved similarly to one formed directly on the titanium substrate. An SEM image of the disk is shown in Figure 7 (scale bar = 500 nm). As can be seen, the HA layer follows the structure underlying the ZrP layer and forms a thin layer of uniform needle-like HA crystals on top of the ZrP coating.
[0099] Example 10. In vivo testing of osseointegration properties of ZrP-coated PEEK implants PEEK screws were blasted and coated according to Example 5. Machined PEEK implants, blasted PEEK and ZrP coated implants, all with the same screw geometry macro-geometry, were then implanted into the tibiae of seven rabbits. After six weeks of healing of the implants, the animals were sacrificed and the removal torque of the implants was measured using a Tohnichi torque gauge. The removal torque values (in Ncm) of the various groups are shown in Figure 8. It can be seen that the blasting treatment increased the fixation strength of the implants from 6.9 Ncm for the rotated implants to 9.1 Ncm for the blasted implants. Coating with ZrP increased the fixation strength to 13.5 Ncm. Statistical significance (Mann-Whitney U) was p(0.05) for ZrP coated screws vs. blasted screws. This indicates that the ZrP coating transforms the bioinert PEEK surface into an osseointegrating surface.
[0100] Example 11. Investigation of hydrophilicity during storage Acid-etched dental implants with a roughness of about 1.0 μm (Sa) were coated with ZrP using the coating dispersion described in Example 1a, using a temperature of 450° C. in an oxygen-enriched atmosphere for the heat treatment. In a second test group, the same type of implants were coated with HA according to WO 2005 / 123579. In a third test group, the same type of implants were heat treated using the same temperature as the ZrP and HA treated implants. All implants were placed in glass vials and stored for 1, 2, 4, 8 and 12 weeks. After each period, the liquid sorption was measured. A separate glass vial was used for each implant and each time, i.e., the implants were discarded after the liquid sorption measurement. The liquid sorption was measured by lowering the implants into a beaker containing type 1 water until the bottom three threads were below the water surface. The implants were then allowed to absorb water for 30 seconds, after which the implants were lifted so that no part of the implant touched the water surface. The implants were then placed on an analytical balance and the weight was recorded. By comparing the weight of the implants before and after immersion, it was possible to calculate the weight of adsorbed water. The results of these measurements are shown in Figure 9 (●=heat treated (HT), ■=ZrP coated, ▲=HA coated). As can be seen in Figure 9, the screws treated with ZrP and HA retained their hydrophilicity over time. The heat treated screws were initially hydrophilic, but this hydrophilicity decreased during storage.
Claims
1. 1. A method for forming a coating comprising or consisting of zirconium phosphate on a surface of a substrate, the method comprising: a) mixing a first water-in-oil emulsion containing a zirconium precursor with a second water-in-oil emulsion containing a phosphate precursor and reacting the zirconium precursor and the phosphate precursor together to form a dispersion of nano-sized zirconium phosphate particles, wherein the zirconium precursor is a zirconium salt or compound of zirconium tetrachloride (ZrCl4), zirconyl oxychloride, zirconyl nitrate, zirconium ethoxide, zirconium isopropoxide, or zirconium diisopropoxide bis(acetylacetonate), and the phosphate precursor is phosphoric acid (H3PO4), Na3PO4, Na2HPO4, NaH2PO4, K3PO4, K2HPO4, KH2PO4, phosphorous acid (H3PO3), hypophosphorous acid (H3PO4), or a combination thereof; 3PO2), or a phosphite ester), b) applying the dispersion to the surface of the substrate; c) optionally creating a uniform layer of said dispersion on said surface of said substrate; and d) removing any other components of said dispersion to form said coating of zirconium phosphate on said surface of said substrate.
2. 1. A method for forming a coating comprising or consisting of zirconium phosphate on a surface of a substrate, the method comprising: a1) adding a phosphate precursor to a water-in-oil emulsion containing a zirconium precursor or adding a zirconium precursor to a water-in-oil emulsion containing a phosphate precursor, and reacting the zirconium precursor and the phosphate precursor together to form a dispersion of nano-sized zirconium phosphate particles, wherein the zirconium precursor is a zirconium salt or compound of zirconium tetrachloride (ZrCl4), zirconyl oxychloride, zirconyl nitrate, zirconium ethoxide, zirconium isopropoxide, or zirconium diisopropoxide bis(acetylacetonate), and the phosphate precursor is phosphoric acid (H3PO4), Na3PO4, Na2HPO4, NaH2PO4, K3PO4, K2HPO4, KH2PO4, phosphorous acid (H3PO3), ), hypophosphorous acid (H 3 PO 2 ), or a phosphite ester); b) applying the dispersion to the surface of the substrate; c) optionally creating a uniform layer of said dispersion on said surface of said substrate; and d) removing any other components of said dispersion to form said coating of zirconium phosphate on said surface of said substrate.
3. 1. A method for forming a coating comprising or consisting of titanium phosphate on a surface of a substrate, the method comprising: e) adding a titanium precursor to a water-in-oil emulsion containing a phosphate precursor and reacting the titanium precursor and the phosphate precursor together to form a dispersion of nano-sized titanium phosphate particles, wherein the phosphate precursor is phosphoric acid (H3PO4), Na3PO4, Na2HPO4, NaH2PO4, K3PO4, K2HPO4, KH2PO4, phosphorous acid (H3PO3), hypophosphorous acid (H3PO2), or a phosphorous acid ester, and the titanium precursor is a titanium salt or compound of titanium tetrachloride (TiCl4), titanium ethoxide, titanium isopropoxide, and titanium diisopropoxide bis(acetylacetonate); f) applying the dispersion to the surface of the substrate; g) optionally creating a uniform layer of said dispersion on said surface of said substrate; and h) removing any other components of said dispersion to form said coating of titanium phosphate on said surface of said substrate.
4. 1. A method for forming a coating comprising or consisting of titanium and / or zirconium phosphate on a surface of a substrate, the method comprising: a) mixing a solution containing a zirconium and / or titanium precursor in an organic solvent with a water-in-oil emulsion containing a phosphate precursor and reacting the zirconium and / or titanium precursor with the phosphate precursor together to form a dispersion of nano-sized zirconium phosphate and / or titanium phosphate particles, wherein the zirconium precursor is a zirconium salt or compound of zirconium tetrachloride (ZrCl4), zirconyl oxychloride, zirconyl nitrate, zirconium ethoxide, zirconium isopropoxide, or zirconium diisopropoxide bis(acetylacetonate); the titanium precursor is a titanium salt or compound of titanium tetrachloride (TiCl4), titanium ethoxide, titanium isopropoxide, and titanium diisopropoxide bis(acetylacetonate); the phosphate precursor is phosphoric acid (H3PO4), Na3PO4, Na2HPO4, NaH2 ... PO4, K3PO4, K2HPO4, KH2PO4, phosphorous acid (H3PO3), hypophosphorous acid (H3PO2), or a phosphite ester); b) applying the dispersion to the surface of the substrate; c) optionally forming a uniform layer of said dispersion on said substrate; and d) removing any other components of said dispersion to form said coating of zirconium phosphate and / or titanium phosphate on said substrate.
5. 5. The method of claim 1, wherein the substrate is made of polyetheretherketone.
6. 6. The method of claim 1, further comprising forming an additional coating comprising calcium phosphate.
7. (A) the calcium phosphate is amorphous calcium phosphate, monocalcium phosphate, dicalcium phosphate, tricalcium phosphate, tetracalcium phosphate, hydroxyapatite, octacalcium phosphate or a mixture thereof, preferably hydroxyapatite; and / or (B) the additional coating is formed on the coating comprising or consisting of titanium phosphate and / or zirconium phosphate; The method according to claim 6.
8. The method of claim 1 , wherein the substrate is an implant for in vivo use.
Citation Information
Patent Citations
Compound implant
JP1993057010A
Titanium implant and method for manufacturing the same
JP2010505586A
A method for manufacturing an implant with a modified surface and an implant manufactured thereby.
JP2010533708A