Tin-containing lithium phosphorus sulfide and its manufacturing method
A tin-containing lithium phosphorus sulfide with enhanced ionic conductivity and reduced hydrogen sulfide generation addresses the limitations of existing sulfide electrolytes, improving battery performance and safety in lithium ion secondary batteries.
Patent Information
- Application Number
- JP2021039391
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-11
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-03-11
AI Technical Summary
Existing lithium-ion secondary batteries face challenges with low ionic conductivity and hydrogen sulfide generation in sulfide solid electrolytes, particularly when exposed to moisture, limiting their safety and performance in large-scale applications.
Development of a tin-containing lithium phosphorus sulfide with a specific composition and crystal structure, represented by the formula xLi n1 SnS m1 ·(1-x)Li n2 P.S. m2, which enhances ionic conductivity and reduces hydrogen sulfide generation through mechanical milling and optional heat treatment.
The tin-containing lithium phosphorus sulfide improves ionic conductivity to 4.5×10 -4 ~1.0×10 -3 Scm -1 at room temperature and 9.0×10 -4 ~3.0×10 -3 Scm -1 at 60°C, while significantly reducing hydrogen sulfide generation, making it suitable for use as a solid electrolyte in lithium ion secondary batteries.
Smart Images

Figure 0007584138000004 
Figure 0007584138000005 
Figure 0007584138000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a tin-containing lithium phosphorus sulfide and a method for producing the same. [Background technology]
[0002] Lithium-ion secondary batteries have been attracting attention as high-energy density batteries, and their applications are expanding not only to portable devices (small consumer applications) but also to stationary applications such as in-vehicle and social infrastructure. One of the demands for these large-scale lithium-ion secondary batteries is the improvement of safety. Ordinary lithium-ion secondary batteries (hereafter abbreviated as liquid-based) use organic electrolytes, which contain large amounts of flammable low-boiling-point solvents (dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, etc.) that fall under the second petroleum of Class 4 of the Fire Service Act as viscosity reducers, raising concerns about battery ignition and smoke. Although companies are making efforts to improve safety, if the components are changed, that is, the electrolyte is changed to a less flammable solid electrolyte, and a dramatic improvement in safety and energy density can be achieved in the material composition, it will be possible to reduce costs for safety considerations, which will be extremely useful from an industrial perspective.
[0003] There are two types of solid electrolytes: polymer electrolytes and inorganic electrolytes. Currently, polymer electrolytes have low ionic conductivity below room temperature, and sufficient battery operation similar to that of liquid electrolytes cannot be expected unless the temperature is above 60°C.
[0004] On the other hand, inorganic electrolytes include oxides and sulfides, and although oxides have high ionic conductivity, they have low moldability and are brittle, making it difficult to build batteries using press alone. On the other hand, sulfide solid electrolytes have higher ionic conductivity than current organic electrolytes, and some of them are considered promising as solid electrolytes to replace electrolytes.
[0005] However, although sulfide solid electrolytes have high ionic conductivity and excellent moldability, they react with moisture in the air when exposed to the air to generate hydrogen sulfide. In contrast, when Sn is used as an electrolyte constituent element, it is difficult to react with moisture in the air (see, for example, Non-Patent Document 1). For example, Non-Patent Document 2 describes the synthesis of orthorhombic Li4SnS4 by heat treating Li2S, Sn, and S in a quartz ampoule. In addition, Non-Patent Document 3 describes the generation of hexagonal Li4SnS4 by mechanochemically treating Li2S and SnS2. Non-Patent Document 4 describes that a crystal obtained by substituting 20% of P in Li3PS4 with Sn has a higher ionic conductivity than Li3PS4 crystal. [Prior art documents] [Non-patent literature]
[0006] [Non-Patent Document 1] Energy Environ.Sci.,7(2014)1053. [Non-Patent Document 2] Chem.Mater.,24(2012)2211-2219. [Non-Patent Document 3] Inorg.Chem.,57(2018)9925-9930. [Non-Patent Document 4] Adv. Mater.,33(2021)2006577. Summary of the Invention [Problem to be solved by the invention]
[0007] However, the ionic conductivity of the orthorhombic Li4SnS4 produced by the solid-phase method as in Non-Patent Document 2 and the hexagonal Li4SnS4 synthesized by the mechanochemical treatment as in Non-Patent Document 3 is not sufficiently high, and the ionic conductivity of the powder compact at room temperature is 10 -5 Scm -1To that extent. Although it has been reported in Non-Patent Document 4 that the ionic conductivity is improved for crystals, the case where a part of P is substituted with Sn has not been investigated for Li3PS4 glass, which is generally used as an electrolyte for all-solid-state batteries.
[0008] The present invention has been made in view of the above-described state of the prior art, and its main object is to provide a compound that can be used as a solid electrolyte for a lithium-ion secondary battery, which can improve ionic conductivity and reduce the amount of hydrogen sulfide generated.
Means for Solving the Problems
[0009] The inventors of the present invention have conducted intensive studies to achieve the above-described object. As a result, they have found that a specific tin-containing lithium phosphorus sulfide can improve ionic conductivity and reduce the amount of hydrogen sulfide generated. The present invention has been further studied and completed based on such findings. That is, the present invention includes the following configurations.
[0010] Item 1. General formula (1): xLi n1 SnS m1 ·(1-x)Li n2 PS m2 (1) [In the formula, n1, n2, m1, m2, and x satisfy 3.0 ≦ n1 ≦ 5.0; 2.0 ≦ n2 ≦ 4.0; 3.0 ≦ m1 ≦ 5.0; 3.0 ≦ m2 ≦ 5.0; 0.00 < x < 0.40.] A tin-containing lithium phosphorus sulfide having a composition represented by the formula.
[0011] Item 2. The tin-containing lithium phosphorus sulfide according to Item 1, which has crystals.
[0012] Item 3. The tin-containing lithium phosphorus sulfide according to Item 2, which has peaks at at least five positions of 17.5°, 18.1°, 25.9°, 29.1°, and 29.8° within a tolerance range of ±0.4° in the range of diffraction angle 2θ = 10° to 80° in the X-ray diffraction pattern by CuKα rays.
[0013] Item 4. The tin-containing lithium phosphorus sulfide according to Item 2 or 3, which has at least two peaks at 22.0° and 22.6° within a diffraction angle 2θ range of 10° to 80° in an X-ray diffraction pattern using CuKα rays, within a tolerance of ±0.2°, and has a ratio of the peak intensity at 22.6° to the peak intensity at 22.0° (peak intensity at 22.6° / peak intensity at 22.0°) of 0.90 to 1.4.
[0014] Item 5. The tin-containing lithium phosphorus sulfide according to any one of Items 2 to 4, having a β-Li3PS4 type crystal structure.
[0015] Item 6. The tin-containing lithium phosphorus sulfide according to Item 1, which has no peak within a diffraction angle range of 2θ=10° to 80° in an X-ray diffraction diagram using CuKα rays.
[0016] Item 7. A method for producing a tin-containing lithium phosphorus sulfide according to any one of items 1 to 6, A process of using a raw material containing lithium sulfide, tin sulfide and phosphorus sulfide as a raw material and subjecting it to a mechanical milling process. A manufacturing method comprising:
[0017] Item 8. The method according to item 7, wherein the amount of the lithium sulfide used is 4.5 to 16.0 moles per mole of the tin sulfide.
[0018] Item 9. The method according to item 7 or 8, wherein the amount of the phosphorus sulfide used is 0.80 to 5.0 moles per mole of the tin sulfide.
[0019] Item 10. The method according to any one of Items 7 to 9, wherein a heat treatment is carried out after the mechanical milling treatment.
[0020] Item 11. A solid electrolyte for a lithium ion secondary battery, comprising the tin-containing lithium phosphorus sulfide according to any one of items 1 to 6.
[0021] Item 12. A lithium ion secondary battery using the tin-containing lithium phosphorus sulfide according to any one of items 1 to 6, or the solid electrolyte for lithium ion secondary batteries according to item 11. Effect of the Invention
[0022] INDUSTRIAL APPLICABILITY The tin-containing lithium phosphorus sulfide of the present invention is useful as a solid electrolyte for lithium ion secondary batteries capable of improving ionic conductivity and reducing the amount of hydrogen sulfide generated. [Brief description of the drawings]
[0023] [Figure 1] 1 shows X-ray diffraction patterns of the powders obtained in Examples 1 to 3 and Comparative Examples 1 to 8. [Diagram 2] 1 shows Raman spectra of the powders obtained in Examples 1 to 3 and Comparative Examples 1 to 8. [Diagram 3] 1 is a graph showing the ionic conductivity of pellets using the powders obtained in Examples 1 to 3 and Comparative Examples 1 to 8. [Figure 4] 1 is a graph showing the results of differential scanning calorimetry of the powders obtained in Examples 1 to 3 and Comparative Examples 1 to 3 and 8. [Diagram 5] 1 shows X-ray diffraction patterns of the powders obtained in Examples 4 to 6 and Comparative Examples 9 to 12. [Figure 6] 1 is a graph showing the ionic conductivity of pellets using the powders obtained in Examples 1 to 6 and Comparative Examples 1 to 3 and 9 to 11. [Figure 7] 1 is a graph showing the temperature dependence of ionic conductivity of the powders obtained in Examples 1 to 6 and Comparative Examples 1 and 9. [Figure 8] 1 shows the state during measurement of the amount of hydrogen sulfide gas generated in Test Example 7. [Figure 9] 11 is a graph showing the measurement results of the amount of hydrogen sulfide gas generated in Test Example 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] In this specification, "comprising" is a concept that encompasses any of "comprise", "consist essentially of", and "consist of".
[0025] Also, in this specification, when a numerical range is indicated as "A to B", it means A or more and B or less.
[0026] 1. Tin-containing lithium phosphorus sulfide The tin-containing lithium phosphorus sulfide of the present invention is General formula (1): xLi n1 SnS m1 ·(1 - x)Li n2 PS m2 [ (1) ] [Wherein, n1, n2, m1, m2 and x satisfy 3.0 ≤ n1 ≤ 5.0; 2.0 ≤ n2 ≤ 4.0; 3.0 ≤ m1 ≤ 5.0; 3.0 ≤ m2 ≤ 5.0; 0.00 < x < 0.40. ] It has a composition represented by.
[0027] That is, the tin-containing lithium phosphorus sulfide of the present invention may be crystalline or glassy. In any case, the ionic conductivity can be improved and the amount of hydrogen sulfide generated can be reduced. Among them, the crystalline form can further improve the ionic conductivity. In this specification, the glass of the above composition means one that does not have a distinct (for example, half-value width less than 1° etc.) peak in the range of diffraction angle 2θ = 10° to 80° in the X-ray diffraction pattern by CuKα rays.
[0028] When the tin-containing lithium phosphorus sulfide of the present invention contains crystals, the crystallinity of the tin-containing lithium phosphorus sulfide is evaluated by an X-ray diffraction pattern. In the present invention, the X-ray diffraction pattern is obtained by the powder X-ray diffraction measurement method, and the following measurement conditions: X-ray source: CuKα 40 kV - 40 mA Measurement conditions: 2θ = 10° to 80°, 0.1° step, scanning speed 5 seconds / step It is measured under.
[0029] When the tin-containing lithium phosphorus sulfide of the present invention contains crystals, it is preferable that the tin-containing lithium phosphorus sulfide has peaks at at least five positions, namely, 17.5°, 18.1°, 25.9°, 29.1°, and 29.8°, within the range of diffraction angles 2θ=10° to 80° in an X-ray diffraction diagram using CuKα rays, with an allowable range of ±0.4° (particularly ±0.3°). That is, the tin-containing lithium phosphorus sulfide of the present invention has peaks in the ranges of 17.1° to 17.9° (particularly 17.2° to 17.8°), 17.7° to 18.5° (particularly 17.8° to 18.4°), 25.5° to 26.3° (particularly 25.6° to 26.2°), 28.7° to 29.5° (particularly 28.8° to 29.4°), and 29.4° to 30.2° (particularly 29.5° to 30.1°) within the range of diffraction angle 2θ=10° to 80° in an X-ray diffraction diagram using CuKα rays. In addition, in the case of lithium phosphorus sulfide that does not contain lithium tin sulfide, if heat treatment is not performed, there is no peak in the range of diffraction angle 2θ = 10 ° to 80 ° in the X-ray diffraction diagram by CuKα rays, and it is glass, and in the case of lithium tin sulfide that does not contain lithium phosphorus sulfide, there is no peak at 29.1 ° and 29.8 °.
[0030] When the tin-containing lithium phosphorus sulfide of the present invention contains crystals, it is preferable that the peaks at 17.5°, 18.1°, and 29.1° have similar peak intensities within the range of diffraction angle 2θ=10° to 80° in an X-ray diffraction diagram using CuKα rays.
[0031] When the tin-containing lithium phosphorus sulfide of the present invention contains crystals, it is desirable that the tin-containing lithium phosphorus sulfide of the present invention has at least two peaks at 22.0° and 22.6° within a range of diffraction angle 2θ=10° to 80° in an X-ray diffraction diagram by CuKα radiation, with a tolerance of ±0.2°. In other words, the tin-containing lithium phosphorus sulfide of the present invention has peaks in the ranges of 21.8° to 22.2° and 22.4° to 22.8° within a range of diffraction angle 2θ=10° to 80° in an X-ray diffraction diagram by CuKα radiation.
[0032] When the tin-containing lithium phosphorus sulfide of the present invention contains crystals, within the range of diffraction angles 2θ=10° to 80° in an X-ray diffraction diagram using CuKα rays, the ratio of the peak intensity at 22.6° to the peak intensity at 22.0° (peak intensity at 22.6° / peak intensity at 22.0°) is preferably 0.90 to 1.4, and more preferably 1.0 to 1.3.
[0033] When the tin-containing lithium phosphorus sulfide of the present invention contains crystals, depending on the crystallinity, within the range of diffraction angle 2θ=10° to 80° in an X-ray diffraction diagram using CuKα rays, the diffraction angle 2θ may have a peak at at least one (particularly all) of 19.8°, 39.3°, 40.3°, 44.8°, 47.4°, and 56.5° within an allowable range of ±0.4° (particularly ±0.3°). That is, the tin-containing lithium phosphorus sulfide of the present invention can have peaks in the ranges of 19.4° to 20.2° (particularly 19.5° to 20.1°), 38.9° to 39.7° (particularly 39.0° to 39.6°), 39.9° to 40.7° (particularly 40.0° to 40.6°), 44.4° to 45.2° (particularly 44.5° to 45.1°), 47.0° to 47.8° (particularly 47.1° to 47.7°), and 56.1° to 56.9° (particularly 56.2° to 56.8°) within the range of diffraction angle 2θ=10° to 80° in the X-ray diffraction diagram by CuKα rays. This also suggests that the lithium phosphorus sulfide is neither a lithium tin sulfide containing lithium phosphorus sulfide nor a lithium tin sulfide containing lithium phosphorus sulfide.
[0034] The crystal structure of the tin-containing lithium phosphorus sulfide of the present invention, when it contains crystals, preferably has a β-Li3PS4 type crystal structure. The β-Li3PS4 type crystal structure means that it has a crystal structure identical or similar to β-Li3PS4, although it is acceptable for it to have a composition other than β-Li3PS4.
[0035] The tin-containing lithium phosphorus sulfide of the present invention preferably has the above characteristics, but is preferably a tin-containing lithium phosphorus sulfide having the general formula (1): xLi n1 SnS m1 (1-x)Lin2 PS m2 (1) [wherein, n1, n2, m1, m2 and x satisfy 3.0 ≤ n1 ≤ 5.0; 2.0 ≤ n2 ≤ 4.0; 3.0 ≤ m1 ≤ 5.0; 3.0 ≤ m2 ≤ 5.0; 0.00 < x < 0.40.] It has a composition represented by the following.
[0036] In general formula (1), n1 represents the amount of lithium in lithium tin sulfide in the tin-containing lithium phosphorus sulfide of the present invention, and 3.0 ≤ n1 ≤ 5.0, preferably 3.5 ≤ n1 ≤ 4.5, more preferably 3.8 ≤ n1 ≤ 4.2. By setting n1 within this range, the iodine-containing lithium tin sulfide of the present invention becomes stable. When n1 is 4.0, the tin-containing lithium phosphorus sulfide of the present invention is the most stable and has high crystallinity.
[0037] In general formula (1), m1 represents the amount of sulfur in lithium tin sulfide in the tin-containing lithium phosphorus sulfide of the present invention, and 3.0 ≤ m1 ≤ 5.0, preferably 3.5 ≤ m1 ≤ 4.5, more preferably 3.8 ≤ m1 ≤ 4.2. By setting m1 within this range, the tin-containing lithium phosphorus sulfide of the present invention becomes stable. When m1 is 4.0, the tin-containing lithium phosphorus sulfide of the present invention is the most stable and has high crystallinity.
[0038] In general formula (1), n2 represents the amount of lithium in lithium phosphorus sulfide in the tin-containing lithium phosphorus sulfide of the present invention, and 2.0 ≤ n2 ≤ 4.0, preferably 2.5 ≤ n2 ≤ 3.5, more preferably 2.8 ≤ n2 ≤ 3.2. By setting n2 within this range, the tin-containing lithium phosphorus sulfide of the present invention becomes stable. When n2 is 3.0, the tin-containing lithium phosphorus sulfide of the present invention is the most stable and has high crystallinity.
[0039] In the general formula (1), m2 represents the amount of sulfur in the lithium phosphorus sulfide in the tin-containing lithium phosphorus sulfide of the present invention, and 3.0 ≤ m2 ≤ 5.0, preferably 3.5 ≤ m2 ≤ 4.5, more preferably 3.8 ≤ m2 ≤ 4.2. By setting m2 within this range, the tin-containing lithium phosphorus sulfide of the present invention becomes stable. When m2 is 4.0, the tin-containing lithium phosphorus sulfide of the present invention is the most stable and has high crystallinity.
[0040] In the general formula (1), x represents the ratio of lithium tin sulfide to lithium phosphorus sulfide in the tin-containing lithium phosphorus sulfide of the present invention, and 0.00 < x < 0.40, preferably 0.050 ≤ x ≤ 0.35, more preferably 0.070 ≤ x ≤ 0.33, still more preferably 0.090 ≤ x ≤ 0.31. When x is 0.00, the ionic conductivity decreases, and since it does not contain Sn, there are concerns from the perspective of safety. Also, when x is 0.40 or more, the ionic conductivity decreases compared to the case where x is 0.00. From the perspective of ionic conductivity, glasses with a composition of 0.050 ≤ x ≤ 0.15 (particularly 0.070 ≤ x ≤ 0.13) are preferred, and from the perspective of the balance between moisture resistance and ionic conductivity, crystals with a composition of 0.25 ≤ x ≤ 0.35 (particularly 0.27 ≤ x ≤ 0.33) are preferred.
[0041] In addition, the tin-containing lithium phosphorus sulfide of the present invention has an ionic conductivity at room temperature of 4.5×10 -4 ~1.0×10 -3 S cm -1 (particularly 7.0×10 -4 ~1.0×10 -3 S cm -1 ) and preferably has an ionic conductivity at 60 °C of 9.0×10 -4 ~3.0×10 -3 S cm -1 (particularly 2.0×10 -3 ~3.0×10 -3 S cm -1 ). The ionic conductivity of the tin-containing lithium phosphorus sulfide of the present invention is measured by the AC impedance method using blocking electrodes.
[0042] The tin-containing lithium phosphorus sulfide of the present invention satisfies the above-mentioned conditions, but may contain other impurities as long as the performance of the tin-containing lithium phosphorus sulfide is not impaired. Examples of such impurities include metals such as transition metals and typical metals that may be mixed into the raw materials; carbon and oxygen that may be mixed into the raw materials and during production. Furthermore, impurities may include residual materials from the raw materials (lithium sulfide (Li2S), tin sulfide (SnS2), phosphorus sulfide (P2S5), etc.) and products other than the target product of the present invention. The amount of these impurities may be within a range that does not impair the performance of the tin-containing lithium phosphorus sulfide described above, and is usually preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less, based on the total amount of the tin-containing lithium phosphorus sulfide that satisfies the above-mentioned conditions as 100% by mass. However, since lithium sulfide affects ion conductivity, it is preferable that it is not contained, or if it is contained, it is only in a very small amount.
[0043] When these impurities are present, in addition to the peaks in the X-ray diffraction diagram described above, diffraction peaks may be present depending on the impurities.
[0044] 2. Manufacturing method of tin-containing lithium phosphorus sulfide The tin-containing lithium phosphorus sulfide of the present invention can be obtained by subjecting a suitable raw material to a mechanical milling treatment.
[0045] for example, A process of using a raw material containing lithium sulfide, tin sulfide and phosphorus sulfide as a raw material and subjecting it to a mechanical milling process. The manufacturing method can be obtained by the method.
[0046] Mechanical milling, also known as mechanochemical processing, is a method of grinding and mixing raw materials while applying mechanical energy. According to this method, the raw materials are ground and mixed by applying mechanical impact and friction, so that lithium sulfide, tin sulfide, and phosphorus sulfide come into vigorous contact with each other and are finely divided, causing a reaction of the raw materials. In other words, mixing, grinding, and reaction occur simultaneously. Therefore, it is possible to more reliably react the raw materials without heating them to high temperatures. By using mechanical milling, a metastable crystal structure that cannot be obtained by normal heat treatment can be obtained.
[0047] Specifically, the mechanical milling treatment can involve mixed pulverization using a mechanical pulverizing device such as a ball mill, a bead mill, a rod mill, a vibration mill, a disk mill, a hammer mill, or a jet mill.
[0048] There is no particular limitation on the lithium sulfide (Li2S, etc.) used as a raw material, and commercially available lithium sulfide can be used. In particular, it is preferable to use lithium sulfide with high purity. In addition, since lithium sulfide is mixed and pulverized by mechanical milling, there is no limitation on the particle size of the lithium sulfide used, and commercially available powdered lithium sulfide can usually be used.
[0049] There is no particular limitation on the tin sulfide (SnS, SnS2, etc.) used as a raw material, and any commercially available tin sulfide can be used. In particular, it is preferable to use a high-purity tin sulfide. In addition, since the tin sulfide is mixed and pulverized by mechanical milling, there is no limitation on the particle size of the tin sulfide used, and commercially available powdered tin sulfide can usually be used.
[0050] There is no particular limitation on the phosphorus sulfide (P2S5, P4S3, P4S5, P4S7, etc.) used as a raw material, and any commercially available phosphorus sulfide can be used. In particular, it is preferable to use one with high purity. In addition, since the phosphorus sulfide is mixed and pulverized by mechanical milling, there is no particular limitation on the particle size of the phosphorus sulfide used, and commercially available powdered phosphorus sulfide can usually be used.
[0051] The mixing ratio of these raw materials can be adjusted so as to be the same as the desired composition of the tin-containing lithium phosphorus sulfide.
[0052] Specifically, the amount of lithium sulfide used is preferably 4.5 to 16.0 mol, and more preferably 4.2 to 15.8 mol, per mol of tin sulfide.
[0053] The amount of phosphorus sulfide used is preferably 0.80 to 5.0 mol, and more preferably 1.0 to 4.8 mol, per mol of tin sulfide.
[0054] There are no particular limitations on the temperature at which mechanical milling is performed. However, from the viewpoint of preventing sulfur from volatilizing and preventing the previously reported crystal phase from being generated, it is preferable to perform mechanical milling at 100°C or less, preferably at 20 to 40°C.
[0055] The time for the mechanical milling treatment is not particularly limited, and the mechanical milling treatment can be performed for any time until the desired tin-containing lithium phosphorus sulfide is precipitated.
[0056] For example, the mechanical milling process can be carried out with an energy amount of about 0.1 to 100 kWh / kg of raw material mixture within a processing time range of about 0.1 to 200 hours. Note that this mechanical milling process can also be carried out in multiple steps with breaks in between as necessary.
[0057] By the above-mentioned mechanical milling treatment, the target tin-containing lithium phosphorus sulfide of the present invention can be obtained as a fine powder.
[0058] The thus obtained tin-containing lithium phosphosulfide of the present invention can be further heat-treated. When heat-treated, it can be performed at, for example, 200 to 300° C. In addition, when a glass tin-containing lithium phosphosulfide is obtained by the mechanical milling treatment, it can be crystallized by heat-treating it at the above temperature, and a crystalline tin-containing lithium phosphosulfide can be obtained.
[0059] 3. Applications of tin-containing lithium phosphorus sulfide The above-mentioned tin-containing lithium phosphorus sulfide of the present invention can improve ionic conductivity and reduce the amount of hydrogen sulfide generated as described above, and is therefore useful as an ion conductor (particularly a solid electrolyte), and is particularly preferably used as a solid electrolyte for lithium ion secondary batteries.
[0060] When the tin-containing lithium phosphosulfide of the present invention is used as a solid electrolyte for a lithium ion secondary battery, the structure of the lithium ion secondary battery of the present invention (particularly, an all-solid-state lithium ion secondary battery) can be the same as that of a known lithium ion secondary battery, except that the tin-containing lithium phosphosulfide of the present invention is used as a solid electrolyte.
[0061] For example, known positive electrode active materials such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), lithium iron phosphate (LiFePO4), vanadium oxide-based materials, and sulfur-based materials can be used as the positive electrode, and a positive electrode mixture containing this positive electrode active material, the tin-containing lithium phosphorus sulfide of the present invention, and a conductive agent and a binder as necessary can be supported on a positive electrode current collector such as Al, Ni, stainless steel, or carbon cloth. As the conductive agent, for example, carbon materials such as graphite, coke, carbon black, and acicular carbon can be used. In addition, as the binder, for example, materials such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyimide (PI), polyamide, polyamideimide, polyacrylic, styrene butadiene rubber (SBR), styrene-ethylene-butylene-styrene copolymer (SEBS), and carboxymethyl cellulose (CMC) can be used alone or in combination of two or more.
[0062] As the negative electrode, known negative electrode active materials such as metallic lithium, carbon-based materials (activated carbon, graphite, etc.), silicon, silicon oxide, Si-SiO-based materials, and lithium titanium oxide are used, and a positive electrode mixture containing this negative electrode active material, the tin-containing lithium phosphorus sulfide of the present invention, and a conductive agent and a binder as necessary can be supported on a negative electrode current collector such as Al, Ni, stainless steel, or carbon cloth. As the conductive agent, for example, carbon materials such as graphite, coke, carbon black, and acicular carbon can be used. As the binder, for example, materials such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyimide (PI), polyamide, polyamideimide, polyacrylic, styrene butadiene rubber (SBR), styrene-ethylene-butylene-styrene copolymer (SEBS), and carboxymethylcellulose (CMC) can be used alone or in combination of two or more. As the electrolyte, a conventionally used electrolyte can also be used in combination.
[0063] In addition, the tin-containing lithium phosphorus sulfide of the present invention can be formed into a layer by a conventional method using a known binder as necessary, and used as the electrolyte layer. As the binder, for example, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyimide (PI), polyamide, polyamideimide, polyacrylic, styrene butadiene rubber (SBR), styrene-ethylene-butylene-styrene copolymer (SEBS), carboxymethyl cellulose (CMC), and other materials can be used alone or in combination of two or more. In addition, as the electrolyte layer, it is also possible to use a combination of electrolyte layers that have been used conventionally.
[0064] The separator may be made of a material such as a polyolefin resin, such as polyethylene or polypropylene, a fluororesin, nylon, aromatic aramid, or inorganic glass, and may be in the form of a porous film, a nonwoven fabric, or a woven fabric.
[0065] Furthermore, a lithium ion secondary battery can be assembled in a conventional manner using other known battery components. In the present invention, the term "lithium ion secondary battery" is a concept that also includes a "lithium secondary battery" that uses metallic lithium as the negative electrode material.
[0066] The shape of the lithium ion secondary battery is not particularly limited, and may be any of cylindrical, rectangular, and the like. EXAMPLES
[0067] The present invention will be described in more detail below with reference to examples. However, it goes without saying that the present invention is not limited to the following examples.
[0068] In addition, the mechanical milling time may differ between the examples and comparative examples, but this is because the mechanical milling was performed until all of the lithium sulfide (Li2S) powder reacted, and the difference in the mechanical milling time is not a substantial difference. When all of the lithium sulfide (Li2S) powder reacts, the peak at 26.9° disappears within the range of diffraction angle 2θ=10° to 80° in the X-ray diffraction diagram using CuKα rays, with a tolerance of ±0.2°.
[0069] As shown in Fig. 1 of Test Example 1 described later, Examples 1 to 3 and Comparative Examples 1 to 3 are glasses that have no peaks within the diffraction angle 2θ range of 10° to 80° in the X-ray diffraction diagram using CuKα rays. On the other hand, Comparative Examples 4 to 8 have peaks at at least three positions, 25.6°, 28.0°, and 45.2°, within the allowable range of ±0.4° (especially ±0.3°), and are considered to have crystallinity and are hexagonal.
[0070] [Comparative Example 1: Synthesis of Li3PS4 glass powder] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium sulfide (Li2S) powder and phosphorus sulfide (P2S5) powder were weighed and mixed in a molar ratio of 3:1, and then mechanical milling was performed for 90 hours at 510 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 90 g (approximately 500 balls) of 4 mm diameter zirconia balls to obtain Li3PS4 powder. The mechanical milling was performed in an atmosphere-controlled overpot. The obtained powder of Li3PS4 composition is referred to as Li3PS4 glass powder for convenience.
[0071] [Example 1: Synthesis of 0.10Li4SnS4 0.90Li3PS4 glass powder] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium sulfide (Li2S) powder, tin sulfide (SnS2) powder, and phosphorus sulfide (P2S5) powder were weighed and mixed in a molar ratio of 73.8:4.8:21.4, respectively, and then mechanical milling was performed for 50 hours at 510 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 90 g (approximately 500 balls) of 4 mm diameter zirconia balls. The mechanical milling was performed in an atmosphere-controlled overpot. The obtained powder with the composition 0.10Li4SnS4·0.90Li3PS4 is referred to as 0.10Li4SnS4·0.90Li3PS4 glass powder for convenience.
[0072] [Example 2: Synthesis of 0.20Li4SnS4 0.80Li3PS4 glass powder] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium sulfide (Li2S) powder, tin sulfide (SnS2) powder, and phosphorus sulfide (P2S5) powder were weighed and mixed in a molar ratio of 72.7:9.1:18.2, respectively, and then mechanical milling was performed for 120 hours at 510 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 90 g (approximately 500 balls) of 4 mm diameter zirconia balls. The mechanical milling was performed in an atmosphere-controlled overpot. The obtained powder with the composition 0.20Li4SnS4·0.80Li3PS4 is referred to as 0.20Li4SnS4·0.80Li3PS4 glass powder for convenience.
[0073] [Example 3: Synthesis of 0.30Li4SnS4 0.70Li3PS4 glass powder] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium sulfide (Li2S) powder, tin sulfide (SnS2) powder, and phosphorus sulfide (P2S5) powder were weighed and mixed in a molar ratio of 71.7:13.1:15.2, respectively, and then mechanical milling was performed for 100 hours at 510 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 90 g (approximately 500 balls) of 4 mm diameter zirconia balls. The mechanical milling was performed in an overpot for controlling the atmosphere. The obtained powder with the composition 0.30Li4SnS4·0.70Li3PS4 is referred to as 0.30Li4SnS4·0.70Li3PS4 glass powder for convenience.
[0074] [Comparative Example 2: Synthesis of 0.40Li4SnS4·0.60Li3PS4 glass powder] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium sulfide (Li2S) powder, tin sulfide (SnS2) powder, and phosphorus sulfide (P2S5) powder were weighed and mixed in a molar ratio of 70.8:16.7:12.5, respectively, and then mechanical milling was performed for 100 hours at 510 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 90 g (approximately 500 balls) of 4 mm diameter zirconia balls. The mechanical milling was performed in an atmosphere-controlled overpot. The obtained powder with the composition 0.40Li4SnS4·0.60Li3PS4 is referred to as 0.40Li4SnS4·0.60Li3PS4 glass powder for convenience.
[0075] [Comparative Example 3: Synthesis of 0.50Li4SnS4·0.50Li3PS4 glass powder] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium sulfide (Li2S) powder, tin sulfide (SnS2) powder, and phosphorus sulfide (P2S5) powder were weighed and mixed in a molar ratio of 70.0:20.0:10.0, respectively, and then mechanical milling was performed for 100 hours at 510 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 90 g (approximately 500 balls) of 4 mm diameter zirconia balls. The mechanical milling was performed in an atmosphere-controlled overpot. The obtained powder with the composition 0.50Li4SnS4·0.50Li3PS4 is referred to as 0.50Li4SnS4·0.50Li3PS4 glass powder for convenience.
[0076] [Comparative Example 4: Synthesis of hexagonal 0.60Li4SnS4 0.40Li3PS4 powder] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium sulfide (Li2S) powder, tin sulfide (SnS2) powder, and phosphorus sulfide (P2S5) powder were weighed and mixed in a molar ratio of 69.2:23.1:7.7, respectively, and then mechanical milling was performed for 60 hours at 510 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 90 g (approximately 500 balls) of 4 mm diameter zirconia balls. The mechanical milling was performed in an atmosphere-controlled overpot. The obtained powder with the composition 0.60Li4SnS4·0.40Li3PS4 is referred to as hexagonal 0.60Li4SnS4·0.40Li3PS4 powder for convenience.
[0077] [Comparative Example 5: Synthesis of hexagonal 0.70Li4SnS4 0.30Li3PS4 powder] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium sulfide (Li2S) powder, tin sulfide (SnS2) powder, and phosphorus sulfide (P2S5) powder were weighed and mixed in a molar ratio of 68.5:25.9:5.6, respectively, and then mechanical milling was performed for 60 hours at 510 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 90 g (approximately 500 balls) of 4 mm diameter zirconia balls. The mechanical milling was performed in an atmosphere-controlled overpot. The obtained powder with the composition 0.70Li4SnS4·0.30Li3PS4 is referred to as hexagonal 0.70Li4SnS4·0.30Li3PS4 powder for convenience.
[0078] [Comparative Example 6: Synthesis of hexagonal 0.80Li4SnS4 0.20Li3PS4 powder] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium sulfide (Li2S) powder, tin sulfide (SnS2) powder, and phosphorus sulfide (P2S5) powder were weighed and mixed in a molar ratio of 67.8:28.6:3.6, respectively, and then mechanical milling was performed for 20 hours at 510 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 90 g (approximately 500 balls) of 4 mm diameter zirconia balls. The mechanical milling was performed in an atmosphere-controlled overpot. The obtained powder with the composition 0.80Li4SnS4·0.20Li3PS4 is referred to as hexagonal 0.80Li4SnS4·0.20Li3PS4 powder for convenience.
[0079] [Comparative Example 7: Synthesis of hexagonal 0.90Li4SnS4 0.10Li3PS4 powder] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium sulfide (Li2S) powder, tin sulfide (SnS2) powder, and phosphorus sulfide (P2S5) powder were weighed and mixed in a molar ratio of 67.3:31.0:1.7, respectively, and then mechanical milling was performed for 20 hours at 510 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 90 g (approximately 500 balls) of 4 mm diameter zirconia balls. The mechanical milling was performed in an atmosphere-controlled overpot. The obtained powder with the composition 0.90Li4SnS4·0.10Li3PS4 is referred to as hexagonal 0.90Li4SnS4·0.10Li3PS4 powder for convenience.
[0080] [Comparative Example 8: Synthesis of hexagonal Li4SnS4 powder] In a glove box with an argon atmosphere (not exposed to air), commercially available lithium sulfide (Li2S) powder and tin sulfide (SnS2) powder were weighed and mixed in a molar ratio of 2:1, and then mechanical milling was performed for 10 hours at 510 rpm in a ball mill (Fritsch P-7, Classic Line) using a 45 mL zirconia container containing 90 g (about 500 balls) of 4 mm diameter zirconia balls to obtain Li4SnS4 powder. The mechanical milling was performed in an overpot for controlling the atmosphere. The obtained powder of Li4SnS4 composition is referred to as hexagonal Li4SnS4 powder for convenience.
[0081] [Test Example 1: X-ray diffraction (part 1)] X-ray diffraction (XRD) using CuKα radiation was measured for the powders obtained in Examples 1 to 3 and Comparative Examples 1 to 8. The results are shown in Figure 1. In the XRD measurement, a polymeric air-protected folder was used to prevent the prepared samples from being exposed to the air.
[0082] In the X-ray diffraction diagram shown in FIG. 1, hexagonal Li4SnS4 crystals remain in the range of x = 0.60 to 1.00, but in the range of x = 0.00 to 0.50, almost no crystals remain and it can be seen that the material is a glass.
[0083] [Test Example 2: Raman Spectroscopic Analysis] Raman spectroscopic analysis was performed on the powders obtained in Examples 1 to 3 and Comparative Examples 1 to 8. The Raman spectroscopic analysis was performed under the following measurement conditions: Laser wavelength: 532nm Exposure time: 5 or 10 seconds Number of times: 8 The results are shown in FIG. 2. In Comparative Examples 1 and 8, the PS4 3- Unit and SnS4 4- A Raman band that can be assigned to the Li3PS4 unit was observed. 3- It was found that the intensity of the Raman bands attributable to the Li4SnS4 unit decreased. On the other hand, as the ratio of Li4SnS4 decreased from Comparative Example 8, the intensity of the SnS4 4- The intensity of the Raman bands attributable to the unit was found to decrease and shift slightly to the lower wavenumber side, suggesting that the SnS4 tetrahedrons in the electrolyte structure are distorted.
[0084] In addition, in Example 3 and Comparative Examples 2 to 5, the PS4 3- Unit and SnS4 4- Both units were observed, and the intensities of the Raman bands of both were approximately the same in Comparative Example 3 in particular. From this, it is presumed that PS4 tetrahedrons and SnS4 tetrahedrons coexist when x is 0.3 to 0.7.
[0085] [Test Example 3: Measurement of ionic conductivity of solid electrolyte pellets (part 1)] 100-120 mg of the powders obtained in Examples 1-3 and Comparative Examples 1-8 were uniformly filled into a molding machine with a diameter of 10 mm, and uniaxially molded at 360 MPa for 5 minutes to produce pellets with a thickness of 0.6-0.8 mm and a diameter of 10 mm. The resistance of these pellets at 25°C (room temperature) and 60°C was measured by an AC impedance method, and the ionic conductivity σ at 25°C (room temperature) and 60°C was calculated from the resistance. The results are shown in FIG. 3 and Table 1.
[0086] [Table 1]
[0087] As a result, the ionic conductivity tended to increase with increasing lithium phosphosulfide composition, but the increasing tendency slowed down under the condition of x = 0.50 or less, where vitrification occurs. However, when x = 0.10, the ionic conductivity at room temperature and 60 °C was specifically higher than when x = 0.00, which consists only of lithium phosphosulfide, or when the other compositions were used.
[0088] [Test Example 4: Differential Scanning Calorimetry] Differential scanning calorimetry was performed on the powders obtained in Examples 1 to 3 and Comparative Examples 1 to 3 and 8. The differential scanning calorimetry was performed under the following measurement conditions: Measurement temperature range: Room temperature to 500℃ Heating rate: 10℃ / min The results are shown in FIG. 4. In Examples 1 to 3 and Comparative Examples 1 to 3, which contain Li3PS4 in their composition, an exothermic peak was observed in the range of 200 to 280°C, whereas in Example 8, which consists only of hexagonal Li4SnS4, an exothermic peak was observed at a higher temperature of around 340°C. From the results in FIG. 4, a crystalline powder was obtained by heat-treating Examples 1 to 3 and Comparative Examples 1 to 3, which are glass powders, at a temperature higher than the temperature at which the exothermic peak was observed. The crystalline powder obtained by heat-treating the glass powder is called a glass ceramic powder. Furthermore, the composition does not change due to the heat treatment, and the obtained glass ceramic has the same composition as glass.
[0089] [Comparative Example 9: Synthesis of Li3PS4 glass ceramic powder] The Li3PS4 glass powder obtained in Comparative Example 1 was heated from room temperature to 250°C at 2°C / min, heat-treated at 250°C for 2 hours, and then allowed to cool to obtain Li3PS4 glass ceramic powder.
[0090] [Example 4: Synthesis of 0.10Li4SnS4 0.90Li3PS4 glass ceramic powder] The 0.10Li4SnS4·0.90Li3PS4 glass powder obtained in Example 1 was heated from room temperature to 230°C at 2°C / min, heat-treated at 230°C for 2 hours, and then allowed to cool to obtain 0.10Li4SnS4·0.90Li3PS4 glass ceramic powder.
[0091] [Example 5: Synthesis of 0.20Li4SnS4 0.80Li3PS4 glass-ceramic powder] The 0.20Li4SnS4·0.80Li3PS4 glass powder obtained in Example 2 was heated from room temperature to 250°C at 2°C / min, heat-treated at 250°C for 2 hours, and then allowed to cool to obtain 0.20Li4SnS4·0.80Li3PS4 glass ceramic powder.
[0092] [Example 6: Synthesis of 0.30Li4SnS4 0.70Li3PS4 glass ceramic powder] The 0.30Li4SnS4·0.70Li3PS4 glass powder obtained in Example 3 was heated from room temperature to 270°C at 2°C / min, heat-treated at 270°C for 2 hours, and then allowed to cool to obtain 0.30Li4SnS4·0.70Li3PS4 glass ceramic powder.
[0093] [Comparative Example 10: Synthesis of 0.40Li4SnS4·0.60Li3PS4 glass ceramic powder] The 0.40Li4SnS4·0.60Li3PS4 glass powder obtained in Comparative Example 2 was heated from room temperature to 280°C at 2°C / min, heat-treated at 280°C for 2 hours, and then allowed to cool to obtain 0.40Li4SnS4·0.60Li3PS4 glass ceramic powder.
[0094] [Comparative Example 11: Synthesis of 0.50Li4SnS4·0.50Li3PS4 glass ceramic powder] The 0.50Li4SnS4·0.50Li3PS4 glass powder obtained in Comparative Example 3 was heated from room temperature to 250°C at 2°C / min, heat-treated at 250°C for 2 hours, and then allowed to cool to obtain 0.50Li4SnS4·0.50Li3PS4 glass ceramic powder.
[0095] [Comparative Example 12: Synthesis of orthorhombic Li4SnS4 powder] The hexagonal Li4SnS4 powder obtained in Comparative Example 8 was heated from room temperature to 390°C at 2°C / min, heat-treated at 390°C for 2 hours, and then allowed to cool to obtain orthorhombic Li4SnS4 powder.
[0096] [Test Example 5: X-ray diffraction (part 2)] X-ray diffraction (XRD) was measured using CuKα radiation for the powders obtained in Examples 4 to 6 and Comparative Examples 9 to 12. The results are shown in Figure 5. In the XRD measurement, a polymeric air-protected folder was used to prevent the prepared samples from being exposed to the air.
[0097] In the X-ray diffraction diagram shown in FIG. 5, Examples 4 to 6 and Comparative Example 10 had a structure similar to β-Li3PS4 of Comparative Example 9. On the other hand, Comparative Example 11 had a structure more similar to the orthorhombic Li4SnS4 of Comparative Example 12. Moreover, Examples 4 to 6 and Comparative Examples 9 and 10 had peaks at five positions, 2θ=17.5°, 18.1°, 25.9°, 29.1°, and 29.8°, within an allowable range of ±0.4°. Furthermore, Examples 4 to 6 had peaks at two positions, 2θ=22.0° and 22.6°, within an allowable range of ±0.2°, and the ratio of the peak intensity at 22.6° to the peak intensity at 22.0° (peak intensity at 22.6° / peak intensity at 22.0°) was in the range of 1.0 to 1.3.
[0098] [Test Example 6: Measurement of ionic conductivity of solid electrolyte pellets (part 2)] 100 mg of the powders obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were uniformly filled into a molding machine with a diameter of 10 mm, and uniaxially molded at 360 MPa for 5 minutes to produce pellets with a thickness of 0.6 to 0.8 mm and a diameter of 10 mm. These were heat-treated at the above temperatures to obtain sintered pellets made of the powders of Examples 4 to 6 and Comparative Examples 9 to 11. The resistance of these pellets at 25°C (room temperature) and 60°C was measured by an AC impedance method, and the ionic conductivity σ at 25°C (room temperature) and 60°C was calculated from the resistance. The results are shown in Table 2.
[0099] [Table 2]
[0100] As a result, in Examples 4 to 6, where x is in the range of 0.10 to 0.30, the ionic conductivity increased significantly. FIG. 6 shows the ionic conductivity at room temperature in Examples 1 to 6 and Comparative Examples 1 to 3, and 9 to 11. In Examples 4 to 6, the conductivity improved by the heat treatment, but in Comparative Example 9, the conductivity did not change significantly even after the heat treatment, and in Comparative Examples 10 to 11, the conductivity decreased by the heat treatment. Therefore, it can be understood that in glass ceramics, the ionic conductivity improves specifically in the range of x = 0.10 to 0.30.
[0101] 7 shows the results of investigating the temperature dependence of ionic conductivity in Examples 1 to 6 and Comparative Examples 1 and 9. Table 3 shows the results of calculating the activation energy from the temperature dependence of ionic conductivity.
[0102] [Table 3]
[0103] As a result, it can be understood that the activation energy is reduced by obtaining glass ceramic powder through heat treatment.
[0104] [Test Example 7: Amount of hydrogen sulfide gas generated] Approximately 2000cm at 50% RH and 25°C (room temperature) 3A solution of 20 mg of electrolyte powder dissolved in 2 mL of distilled water was sealed in a container and the amount of hydrogen sulfide (H2S) generated was measured.
[0105] As the electrolyte powder, the powders obtained in Examples 1 to 6 and Comparative Examples 1, 2, 4, 6 and 8 were used.
[0106] The electrolyte powder was placed in screw tube No. 2 and double sealed with Lamipack to prevent reaction before the measurement started.
[0107] Next, a small electric fan, a temperature and humidity logger, a hydrogen sulfide detector, and the electrolyte powder sealed in a laminated zip-lock bag were placed in the glove box, and the box was left to stand until the humidity reached 50% RH.
[0108] Next, the electrolyte powder was removed from the laminated zipper bag, 2 mL of distilled water was brought into the glove box, and the distilled water was added to the screw tube containing the electrolyte powder to completely dissolve the electrolyte powder. Then, as shown in Figure 8, the electrolyte powder was placed in a sealed container (volume: approximately 2000 cm). 3 ) was closed.
[0109] Temperature, humidity, and hydrogen sulfide concentration were measured (automatically) every 10 seconds. When the hydrogen sulfide concentration reached the detection limit of the detector (approximately 230 ppm), the measurement was stopped (approximately 1 hour).
[0110] The results are shown in Figure 9. As a result, in the range of x = 0.00 to 0.20, the hydrogen sulfide concentration reached the detection limit of the detector in the order of Comparative Example 1 and Examples 4, 1, 2, and 5. From this, it can be understood that in the composition containing Sn, the time until hydrogen sulfide is generated is longer compared to x = 0.00, which does not contain Sn. Furthermore, under the condition of x = 0.30 or more, the hydrogen sulfide concentration did not change significantly from the start of measurement even after 1 hour.
[0111] From the above results, in the glass, Example 1, which has a composition of x=0.10, has the highest ion conductivity, and took a longer time to generate hydrogen sulfide than Comparative Example 1, which has a composition of x=0.00, which has the second highest conductivity among the glasses. From this, it can be understood that Example 1 is a glass electrolyte that can achieve both high ion conductivity and high water resistance. In addition, since glass is generally softer than glass ceramics, it is thought that it is easier to bond particles together. Therefore, the glass electrolyte such as that of Example 1 is more suitable for use in the positive electrode layer and the negative electrode layer in combination with electrode active material particles, etc.
[0112] In addition, in the glass ceramic, the hydrogen sulfide concentration in Example 6, which has a composition of x=0.30, did not change before and after the measurement. From this, it can be understood that the composition of x=0.30 in particular not only has an ion conductivity equivalent to that of x=0.20, which had the highest ion conductivity, but also suppresses the generation of hydrogen sulfide. Therefore, it is essential that the glass ceramic electrolyte in Example 6 has high conductivity, and it is more suitable for use in the solid electrolyte layer, which is a portion in which a relatively large amount of electrolyte is used.
Claims
1. General formula (1): xLi n1 SnS m1 ・(1-x)Li n2 PSm2 (1) [In the formula, n1, n2, m1, m2, and x satisfy the following conditions: 3.0≦n1≦5.0; 2.0≦n2≦4.0; 3.0≦m1≦5.0; 3.0≦m2≦5.0; 0.00<x<0.40.] The composition is represented by the formula: having crystals and / or glasses, The crystal has peaks at at least five positions, 17.5 °, 18.1 °, 25.9 °, 29.1 °, and 29.8 °, within the range of diffraction angles 2θ = 10 ° to 80 ° in an X-ray diffraction diagram by CuKα rays. Tin-containing lithium phosphorus sulfide.
2. A tin-containing lithium phosphosulfide as described in claim 1 having the crystals.
3. The tin-containing lithium phosphorus sulfide according to claim 2, which has peaks at at least two positions, 22.0 ° and 22.6 °, within a tolerance of ±0.2 ° within the range of diffraction angles 2θ = 10 ° to 80 ° in an X-ray diffraction diagram by CuKα rays, and has a ratio of the peak intensity at 22.6 ° to the peak intensity at 22.0 ° (peak intensity at 22.6 ° / peak intensity at 22.0 °) of 0.9 to 1.
4.
4. β-Li 3 P.S. 4 The tin-containing lithium phosphorus sulfide according to claim 2 or 3, having a type crystal structure.
5. The tin-containing lithium phosphorus sulfide according to claim 1, which has no peak within the range of diffraction angle 2θ = 10 ° to 80 ° in an X-ray diffraction diagram by CuKα rays.
6. A method for producing the tin-containing lithium phosphorus sulfide according to any one of claims 1 to 5, comprising using a raw material containing lithium sulfide, tin sulfide and phosphorus sulfide as a raw material and subjecting the raw material to a mechanical milling treatment. A manufacturing method comprising:
7. The method according to claim 6, wherein the amount of lithium sulfide used is 4.5 to 16.0 moles per mole of tin sulfide.
8. The method according to claim 6 or 7, wherein the amount of the phosphorus sulfide used is 0.8 to 5.0 moles per mole of the tin sulfide.
9. The method according to any one of claims 6 to 8, further comprising subjecting the material to a heat treatment after the mechanical milling treatment.
10. A solid electrolyte for lithium ion secondary batteries comprising the tin-containing lithium phosphorus sulfide according to any one of claims 1 to 5.
11. A lithium ion secondary battery using the tin-containing lithium phosphorus sulfide according to any one of claims 1 to 5, or the solid electrolyte for lithium ion secondary batteries according to claim 10.
Citation Information
Patent Citations
Sulfide solid electrolyte material, battery, and method for producing sulfide solid electrolyte material
WO2013118722A1