Ethylene-based copolymer composition and its use

The ethylene copolymer composition, with specific ethylene/α-olefin/non-conjugated polyene ratios and silylated polyolefin, addresses adhesion issues in conventional copolymers, enhancing laminate production speed and strength for applications like hoses and belts.

JP7584231B2Active Publication Date: 2024-11-15MITSUI CHEMICALS INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020067777
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-03
Publication Date
2024-11-15
Estimated Expiration
2040-04-03

AI Technical Summary

Technical Problem

Conventional ethylene/α-olefin/nonconjugated polyene copolymers face challenges in achieving sufficient adhesion to synthetic fibers, particularly in environments where halogen-based adhesives are not optimal, impacting the productivity and mechanical properties of laminates.

Method used

An ethylene copolymer composition containing specific ratios of ethylene, α-olefin, and non-conjugated polyene, combined with a silylated polyolefin, which enhances adhesion to fiber materials while maintaining mechanical properties, allowing for improved laminate production speed and adhesive strength.

Benefits of technology

The ethylene copolymer composition improves adhesion with fiber materials, enabling faster laminate production and achieving excellent adhesive strength, suitable for applications such as hoses and belts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584231000001
    Figure 0007584231000001
  • Figure 0007584231000002
    Figure 0007584231000002
  • Figure 0007584231000003
    Figure 0007584231000003
Patent Text Reader

Abstract

To provide an ethylenic copolymer composition that improves tackiness to a layer containing fiber material for improved productivity, has excellent adhesion to the layer containing fiber material, and can maintain the mechanical properties of a resultant laminate.SOLUTION: An ethylenic copolymer composition contains: an ethylene-α-olefin-nonconjugated polyene copolymer (L) containing a constitutional unit derived from an ethylene [A], a constitutional unit derived from a C4-20 α-olefin [B], and a constitutional unit derived from a nonconjugated polyene [C], and satisfying predetermined requirements; and silylated polyolefin (H).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a crosslinkable ethylene copolymer composition, a laminate using said composition and a layer containing a fiber material, and uses thereof. [Background technology]

[0002] Ethylene-α-olefin-non-conjugated polyene copolymers such as EPDM (ethylene-propylene-diene rubber) generally have excellent weather resistance, heat resistance, and ozone resistance, and are used in industrial automotive parts, industrial rubber products, electrical insulation materials, civil engineering and construction materials, rubberized fabrics, etc.

[0003] Conventional ethylene-α-olefin-non-conjugated polyene copolymers have the disadvantage of inferior adhesion to synthetic fibers compared to polar rubbers such as nitrile rubber, chloroprene rubber, and chlorosulfonated polyethylene. As a method to solve this drawback, it has been disclosed that an adhesive solution of a chlorosulfonated copolymer is used to improve the adhesion between ethylene-α-olefin-non-conjugated polyene copolymer and synthetic fibers (Patent Document 1).

[0004] However, in today's world where environmental issues such as non-halogenation are a concern, it is difficult to say that such adhesive technology that utilizes the polarity of halogenation is optimal. Also, a conventional adhesive method is known in which synthetic fibers are treated with resorcinol-formaldehyde latex (RFL) and then embedded in rubber to crosslink and adhere. More specifically, a method is known in which isocyanates or isocyanuric acid derivatives are used in the RFL treatment. However, even if these methods are applied to rubbers that use ethylene-α-olefin-non-conjugated polyene copolymers, it is difficult to obtain sufficient adhesion. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 42-23632 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to obtain an ethylene-based copolymer composition which can improve productivity by improving adhesion to a layer containing a fiber material, has excellent adhesion to a layer containing a fiber material, and can maintain the mechanical properties of the resulting laminate. [Means for solving the problem]

[0007] The present invention relates to an ethylene copolymer composition containing the following (L) and (H) and uses thereof. (L) An ethylene-α-olefin-non-conjugated polyene copolymer comprising ethylene [A], an α-olefin [B] having 4 to 20 carbon atoms, and a non-conjugated polyene [C], which satisfies the following requirements (1) to (4): (H) Silylated polyolefin. (1) the molar ratio [[A] / [B]] of the structural unit derived from ethylene [A] to the structural unit derived from an α-olefin having 4 to 20 carbon atoms is 40 / 60 to 90 / 10; (2) the content of the structural unit derived from the non-conjugated polyene [C] is 0.1 to 6.0 mol % relative to 100 mol % of the total of the structural units [A], [B] and [C]; (3) Mooney viscosity ML at 125°C (1+4) 125°C is 5 to 100; (4) The B value represented by the following formula (i) is 1.20 or more. B value=([EX]+2[Y]) / [2×[E]×([X]+[Y])]···(i) [Here, [E], [X] and [Y] respectively represent the mole fractions of ethylene [A], α-olefin [B] having 4 to 20 carbon atoms, and non-conjugated polyene [C], and [EX] represents the dyad chain fraction of ethylene [A]-α-olefin [B] having 4 to 20 carbon atoms.] Effect of the Invention

[0008] The ethylene-based copolymer composition of the present invention has improved adhesion to a layer containing a fiber material when used to produce a laminate, making it possible to increase the production speed. Furthermore, the laminate obtained by crosslinking has excellent adhesive strength and can be used for a wide range of applications including hoses, belts, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be specifically described below. The ethylene-based copolymer composition of the present invention and the ethylene-based copolymer composition constituting the layer [I] of the laminate of the present invention contain an ethylene-α-olefin-non-conjugated polyene copolymer (L) and a silylated polyolefin (H) described below.

[0010] <Ethylene-α-olefin-non-conjugated polyene copolymer (L)> The ethylene-α-olefin-non-conjugated polyene copolymer (L), which is one of the components constituting the ethylene-based copolymer composition of the present invention and the ethylene-based copolymer composition that forms the layer [I] of the laminate of the present invention, is an ethylene-α-olefin-non-conjugated polyene copolymer (hereinafter also referred to as "ethylene-based copolymer (L)") that contains structural units derived from ethylene [A], structural units derived from an α-olefin [B] having 4 to 20 carbon atoms, and structural units derived from a non-conjugated polyene [C] and satisfies the following requirements (1) to (4):

[0011] (1) The molar ratio (A / B) of the structural unit derived from ethylene [A] to the structural unit derived from an α-olefin [B] having 4 to 20 carbon atoms is 40 / 60 to 90 / 10. (2) The content of structural units derived from the non-conjugated polyene [C] is 0.1 to 6.0 mol %, relative to 100 mol % of the total of structural units derived from ethylene [A], the α-olefin [B] having 4 to 20 carbon atoms, and the non-conjugated polyene [C]. (3) Mooney viscosity ML at 125°C (1+4) (125℃) is 5 to 100. (4) The B value represented by the following formula (i) is 1.20 or more. B value=([EX]+2[Y]) / [2×[E]×([X]+[Y])]···(i) [Here, [E], [X] and [Y] respectively represent the mole fractions of ethylene [A], α-olefin [B] having 4 to 20 carbon atoms, and non-conjugated polyene [C], and [EX] represents the dyad chain fraction of ethylene [A]-α-olefin [B] having 4 to 20 carbon atoms.]

[0012] Examples of the α-olefin [B] having 4 to 20 carbon atoms include 1-butene having 4 carbon atoms, which has a linear structure without side chains, through 1-nonene having 9 carbon atoms and 1-decene having 10 carbon atoms, 1-nonadecene having 19 carbon atoms, 1-eicosene having 20 carbon atoms, and 4-methyl-1-pentene, 9-methyl-1-decene, 11-methyl-1-dodecene, and 12-ethyl-1-tetradecene, which have side chains. These α-olefins [B] can be used alone or in combination of two or more kinds. Among these, α-olefins having 4 to 10 carbon atoms are preferred, 1-butene, 1-hexene and 1-octene are more preferred, and 1-butene is even more preferred.

[0013] Examples of the non-conjugated polyene [C] include linear non-conjugated dienes such as 1,4-hexadiene, 1,6-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, and 7-methyl-1,6-octadiene; cyclohexadiene, dicyclopentadiene, methyltetrahydroindene, 5-vinyl-2-norbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, and 5-isopropylidene-2-norbornene. cyclic non-conjugated dienes such as bornene and 6-chloromethyl-5-isopropenyl-2-norbornene; and trienes such as 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, 2-propenyl-2,5-norbornadiene, 1,3,7-octatriene, 1,4,9-decatriene, 4,8-dimethyl-1,4,8-decatriene, and 4-ethylidene-8-methyl-1,7-nonadiene.

[0014] These non-conjugated polyenes [C] can be used alone or in combination of two or more kinds. Among these, linear non-conjugated dienes such as 1,4-hexadiene, and cyclic non-conjugated dienes such as 5-ethylidene-2-norbornene and 5-vinyl-2-norbornene are preferred, with 5-ethylidene-2-norbornene and 5-vinyl-2-norbornene being more preferred.

[0015] Examples of the ethylene copolymer (L) include the following. Ethylene-1-butene-1,4-hexadiene copolymer, Ethylene-1-pentene-1,4-hexadiene copolymer, Ethylene-1-hexene-1,4-hexadiene copolymer, Ethylene-1-heptene-1,4-hexadiene copolymer, Ethylene-1-octene-1,4-hexadiene copolymer, Ethylene-1-nonene-1,4-hexadiene copolymer, Ethylene-1-decene-1,4-hexadiene copolymer, Ethylene-1-butene-1-octene-1,4-hexadiene copolymer, Ethylene-1-butene-5-ethylidene-2-norbornene copolymer, Ethylene-1-pentene-5-ethylidene-2-norbornene copolymer, Ethylene-1-hexene-5-ethylidene-2-norbornene copolymer, Ethylene-1-heptene-5-ethylidene-2-norbornene copolymer, Ethylene-1-octene-5-ethylidene-2-norbornene copolymer, Ethylene-1-nonene-5-ethylidene-2-norbornene copolymer, Ethylene-1-decene-5-ethylidene-2-norbornene copolymer copolymers, ethylene-1-butene-1-octene-5-ethylidene-2-norbornene copolymers, ethylene-1-butene-5-ethylidene-2-norbornene-5-vinyl-2-norbornene copolymers, ethylene-1-pentene-5-ethylidene-2-norbornene-5-vinyl-2-norbornene copolymers, ethylene-1-hexene-5-ethylidene-2-norbornene-5-vinyl-2-norbornene copolymers, ethylene-1-heptene-5-ethylidene-2-norbornene-5 ethylene-1-octene-5-ethylidene-2-norbornene-5-vinyl-2-norbornene copolymer, ethylene-1-nonene-5-ethylidene-2-norbornene-5-vinyl-2-norbornene copolymer, ethylene-1-decene-5-ethylidene-2-norbornene-5-vinyl-2-norbornene copolymer, and ethylene-1-butene-1-octene-5-ethylidene-2-norbornene-5-vinyl-2-norbornene copolymer.

[0016] The ethylene copolymer (L) may be used alone or in combination of two or more, as required. The α-olefin [B] having 4 to 20 carbon atoms and the non-conjugated polyene [C] may each be used alone or in combination of two or more. The ethylene copolymer (L) according to the present invention satisfies the following requirements (1) to (4).

[0017] Requirement (1) The ethylene-based copolymer (L) according to the present invention has a molar ratio (A / B) of structural units derived from ethylene [A] to structural units derived from an α-olefin [B] having 4 to 20 carbon atoms of 40 / 60 to 90 / 10. The ethylene-based copolymer (L) having a molar ratio within the above range has an excellent balance between rubber elasticity at low temperatures and tensile strength at room temperature. The molar ratio (A / B) of the structural units derived from ethylene [A] to the structural units derived from an α-olefin [B] having 4 to 20 carbon atoms is preferably 45 / 55 to 80 / 20, more preferably 50 / 50 to 75 / 25, and further preferably 55 / 45 to 70 / 30.

[0018] Requirement (2) The ethylene-based copolymer (L) according to the present invention has a content of structural units derived from the non-conjugated polyene [C] of 0.1 to 6.0 mol % relative to 100 mol % of the total of the structural units derived from ethylene [A], the α-olefin [B] having 4 to 20 carbon atoms, and the non-conjugated polyene [C]. The ethylene-based copolymer (L) having the structural units derived from the non-conjugated polyene [C] within the above range has sufficient crosslinkability and flexibility. The lower limit of the content of the structural unit derived from the non-conjugated polyene [C] is preferably 0.5 mol %. The upper limit of the content of the structural unit derived from the non-conjugated polyene [C] is preferably 4.0 mol %, more preferably 3.5 mol %, and further preferably 3.0 mol %.

[0019] Requirement (3) The ethylene copolymer (L) according to the present invention has a Mooney viscosity ML (1+4) (125°C) is 5 to 100, preferably 20 to 95, and more preferably 30 to 90. Mooney Viscosity ML (1+4)When the temperature (125° C.) is within the above range, the ethylene copolymer (L) is excellent in processability, flowability, and post-treatment quality (ribbon handling property).

[0020] Requirement (4) The ethylene copolymer (L) according to the present invention has a B value represented by the following formula (i) of 1.20 or more, preferably 1.20 to 1.80, and more preferably 1.22 to 1.40. B value=([EX]+2[Y]) / [2×[E]×([X]+[Y])]···(i) [Here, [E], [X] and [Y] respectively represent the mole fractions of ethylene [A], α-olefin [B] having 4 to 20 carbon atoms, and non-conjugated polyene [C], and [EX] represents the dyad chain fraction of ethylene [A]-α-olefin [B] having 4 to 20 carbon atoms.] An ethylene copolymer having a B value within the above range has a small compression set at low temperatures and an excellent balance between rubber elasticity at low temperatures and tensile strength at room temperature.

[0021] <Production method of ethylene-α-olefin-non-conjugated polyene copolymer (L)> The ethylene-α-olefin-non-conjugated polyene copolymer (L) according to the present invention can be obtained by various known production methods, for example, a conventionally known production method using a metallocene catalyst. As the metallocene catalyst and the production method using the catalyst, for example, the examples described in WO 2015 / 122415, particularly paragraphs

[0249] to

[0320] of the publication, can be adopted.

[0022] <Silylated polyolefin (H)> The silylated polyolefin (H), which is one of the components constituting the ethylene copolymer composition of the present invention and the ethylene copolymer composition forming the layer [I] of the laminate of the present invention, is a reaction product between a silicon-containing compound containing a structural unit represented by the following formula (1) and a vinyl group-containing compound having a number average molecular weight (Mn) of 100 to 500,000 measured by gel permeation chromatography (GPC) (however, this does not include the case where the silicon-containing compound has two or more SiH groups per molecule and the vinyl group-containing compound has an average of 2.0 or more vinyl groups per molecule, i.e., a silylated polyolefin that is a reaction product between a silicon-containing compound having two or more SiH groups per molecule and a vinyl group-containing compound having an average of 2.0 or more vinyl groups per molecule, and a derivative thereof).

[0023] -Si(R 1 )HY 1 - (1) In the above formula (1), R 1 is a hydrogen atom, a halogen atom or a hydrocarbon group, and Y 1 is O, S or NR 30 (R 30 is a hydrogen atom or a hydrocarbon group).

[0024] <Silicon-containing compounds> The silicon-containing compound constituting the silylated polyolefin (H) according to the present invention is a hydrosilane compound having a structural unit represented by the following formula (1). -Si(R 1 )HY 1 - (1)

[0025] In the above formula (1), R 1 is a hydrogen atom, a halogen atom or a hydrocarbon group, and Y 1 is O, S or NR 30 (R 30 is a hydrogen atom or a hydrocarbon group).

[0026] Examples of halogen atoms include fluorine, chlorine, bromine, and iodine.

[0027] The hydrocarbon group is preferably a hydrocarbon group having 2 to 40 carbon atoms, more preferably a hydrocarbon group having 2 to 20 carbon atoms. Specific examples include an alkyl group, an alkenyl group, and an aryl group. 1 and R 30 In the formula, the hydrocarbon groups may be the same or different.

[0028] Examples of the alkyl group include linear or branched alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, a hexyl group, a 2-ethylhexyl group, an octyl group, a decyl group, and an octadecyl group; cycloalkyl groups such as a cyclopentyl group, a cyclohexyl group, and a norbornyl group; and arylalkyl groups such as a benzyl group, a phenylethyl group, and a phenylpropyl group.

[0029] Examples of the alkenyl group include a vinyl group, a propenyl group, and a cyclohexenyl group.

[0030] Examples of the aryl group include a phenyl group, a tolyl group, a dimethylphenyl group, a trimethylphenyl group, an ethylphenyl group, a propylphenyl group, a biphenyl group, a naphthyl group, a methylnaphthyl group, an anthryl group, and a phenanthryl group.

[0031] The above-mentioned hydrocarbon groups may contain one or more heteroatoms.Specific examples of such groups include those in which at least one hydrogen atom is substituted with a group containing a halogen atom, oxygen, nitrogen, silicon, phosphorus, or sulfur.

[0032] In one embodiment, the silicon-containing compound has a structure represented by formula (2):

[0033] R 22 -(Si(R 21 )HY 21 ) m -Z-(Y 22-Si(R 23 )H) n -R 24 (2)

[0034] In the above formula (2), R 21 and R 23 each independently represents a hydrogen atom, a halogen atom, or a hydrocarbon group, R 22 and R 24 are each independently a halogen atom or a hydrocarbon group, Y 21 and Y 22 each independently represents O, S, or NR 30 (R 30 is a hydrogen atom or a hydrocarbon group, m is 0 or 1, n is 0 or 1, R 21 , R 23 , Y 21 and Y 22 When more than one is present, each group may be the same or different, Z is a divalent group represented by the following formula (3): -Si(R 41 )(R 41 )-(Y 23 -Si(R 41 )(R 41 )) l - (3) In the above formula (3), R 41 is a hydrogen atom, a halogen atom, or a hydrocarbon group, and each R 41 may be the same or different, and Y 23 each independently represents O, S, or NR 30 (R 30 is a hydrogen atom or a hydrocarbon group), and l is an integer of 0 to 10,000.

[0035] However, when m=n=0 in the above formula (2), at least one R 41 is a hydrogen atom.

[0036] The definitions of the halogen atoms and the hydrocarbon groups in the above formulas (2) and (3) are the same as those in the above formula (1).

[0037] In addition, one typical embodiment is that the hydrocarbon group in the above formulas (1), (2) and (3) is composed only of carbon atoms and hydrogen atoms.

[0038] In one embodiment, the silicon-containing compound preferably has 3 or more silicon atoms, more preferably 5 or more silicon atoms, and even more preferably 10 or more silicon atoms. The silicon-containing compound also preferably has 10,000 or less silicon atoms, more preferably 1,000 or less silicon atoms, particularly preferably 300 or less silicon atoms, and even more preferably 50 or less silicon atoms.

[0039] In one embodiment, l in the above formula (3) is an integer of 0 to 10,000, and preferred upper and lower limits include numbers determined from the values ​​of m and n in the above formula (2) and the above preferred number of silicon atoms.

[0040] In one embodiment, a silicon-containing compound in which m=n=1 in the above formula (2), that is, a compound having SiH groups at both ends, is preferably used. In one embodiment, a silicon-containing compound in which m=1 and n=0 in the above formula (2), that is, a silicon-containing compound having a SiH group at one end, is preferably used.

[0041] Particularly preferred silicon-containing compounds are those represented by the above formulas (2) and (3), where m=n=1, and R 21 , R 23 and R 41 and R are each a hydrocarbon group. The hydrocarbon groups may be the same or different.

[0042] Particularly preferred silicon-containing compounds include those represented by the above formulas (2) and (3), in which m=1, n=0, and R 21 and R 41and R are each a hydrocarbon group. The hydrocarbon groups may be the same or different.

[0043] Specific examples of the silicon-containing compound used in this embodiment are shown below: The silicon-containing compound in this embodiment is a compound having one SiH group.

[0044] Examples of silicon-containing compounds having one SiH group include compounds represented by the following formula (2a), and compounds in which some or all of the methyl groups in formula (2a) have been substituted with hydrocarbon groups which may contain one or more heteroatoms, such as ethyl groups, propyl groups, phenyl groups, and trifluoropropyl groups.

[0045] HSi(CH3)2O-(-Si(CH3)2-O-) d -Si(CH3)3···(2a) (In the above formula (2a), d is an integer of 1 or more, and the upper limit is, for example, 1000, preferably 300, and more preferably 50.)

[0046] More specifically, such compounds include the following compounds, but are not limited to these.

[0047] C4H9-((CH3)2SiO)9-(CH3)2SiH C4H9-((CH3)2SiO) 65 -(CH3)2SiH Other examples of silicon-containing compounds having one SiH group include dimethylsiloxane-methylhydrogensiloxane copolymers represented by the following formula (2b), and compounds in which some or all of the methyl groups in the following formula (2b) have been substituted with hydrocarbon groups which may contain one or more heteroatoms, such as ethyl groups, propyl groups, phenyl groups, and trifluoropropyl groups.

[0048] Si(CH3)3O-(-Si(CH3)2-O-) e -(-SiH(CH3)-O-)-Si(CH3)3···(2b) (In the above formula (2b), e is an integer of 0 or more, and the upper limit is, for example, 1000, preferably 300, and more preferably 50.)

[0049] The order in which the -Si(CH3)2-O- units and -SiH(CH3)-O- units are arranged is not particularly limited, and may be block-like, disordered, or statistically random.

[0050] More specifically, such compounds include the following compounds, but are not limited to these.

[0051] Si(CH3)3O-SiH(CH3)-O-Si(CH3)3 Silicon-containing compounds of the present embodiment also include compounds having two or more SiH groups.

[0052] Examples of silicon-containing compounds having two or more SiH groups include methylhydrogenpolysiloxanes represented by the following formula (2c), and compounds in which some or all of the methyl groups in the following formula (2c) have been substituted with hydrocarbon groups which may contain one or more heteroatoms, such as ethyl groups, propyl groups, phenyl groups, and trifluoropropyl groups.

[0053] (CH3)3SiO-(-SiH(CH3)-O-) f -Si(CH3)3···(2c) (In the above formula (2c), f is an integer of 2 or more, and the upper limit is, for example, 1000, preferably 300, and more preferably 50.)

[0054] Other examples of silicon-containing compounds having two or more SiH groups include, for example, a dimethylsiloxane-methylhydrogensiloxane copolymer represented by the following formula (2d), and a compound represented by the following formula (2d) in which some or all of the methyl groups have been substituted with a hydrocarbon group which may contain one or more heteroatoms, such as an ethyl group, a propyl group, a phenyl group, or a trifluoropropyl group.

[0055] (CH3)3SiO-(-Si(CH3)2-O-) g -(-SiH(CH3)-O-) h -Si(CH3)3···(2d) (In the above formula (2d), g is an integer of 1 or more, h is an integer of 2 or more, and the upper limit of the total of g and h is, for example, 1000, preferably 300, and more preferably 50.)

[0056] In addition, in the above formula (2d), the order in which the -Si(CH3)2-O- units and the -SiH(CH3)-O- units are arranged is not particularly limited, and they may be arranged in a block manner, disordered, or statistically random manner.

[0057] More specifically, such compounds include the following compounds, but are not limited to these.

[0058] [ka]

[0059] Further examples of silicon-containing compounds having two or more SiH groups include methylhydrogenpolysiloxanes represented by the following formula (M-2e), and compounds in which some or all of the methyl groups in the following formula (2e) have been substituted with hydrocarbon groups which may contain one or more heteroatoms, such as ethyl groups, propyl groups, phenyl groups, and trifluoropropyl groups.

[0060] HSi(CH3)2O-(-Si(CH3)2-O-) i -Si(CH3)2H (2e) (In the above formula (2e), i is an integer of 1 or more, and the upper limit is, for example, 1000, preferably 300, and more preferably 50.)

[0061] More specifically, such compounds include the following compounds, but are not limited to these.

[0062] HSi(CH3)2O-(-Si(CH3)2-O-)5-Si(CH3)2H HSi(CH3)2O-(-Si(CH3)2-O-)8-Si(CH3)2H HSi(CH3)2O-(-Si(CH3)2-O-) 18 -Si(CH3)2H HSi(CH3)2O-(-Si(CH3)2-O-) 80 -Si(CH3)2H HSi(CH3)2O-(-Si(CH3)2-O-) 230 -Si(CH3)2H Further examples of silicon-containing compounds having two or more SiH groups include methylhydrogenpolysiloxanes represented by the following formula (2f), and compounds in which some or all of the methyl groups in the following formula (2f) have been substituted with hydrocarbon groups which may contain one or more heteroatoms, such as ethyl groups, propyl groups, phenyl groups, and trifluoropropyl groups.

[0063] HSi(CH3)2O-(-SiH(CH3)-O-) j -Si(CH3)2H (2f) (In the above formula (2f), j is an integer of 1 or more, and the upper limit is, for example, 1000, preferably 300, and more preferably 50.)

[0064] Further examples of silicon-containing compounds having two or more SiH groups include, for example, dimethylsiloxane-methylhydrogensiloxane copolymers represented by the following formula (2g), and compounds in which some or all of the methyl groups in the following formula (2g) have been substituted with hydrocarbon groups which may contain one or more heteroatoms, such as ethyl groups, propyl groups, phenyl groups, and trifluoropropyl groups.

[0065] HSi(CH3)2O-(-Si(CH3)2-O-) k -(-SiH(CH3)-O-) l -Si(CH3)2H (2g) (In the above formula (2g), k and l are each an integer of 1 or more, and the upper limit of the total of k and l is, for example, 1000, preferably 300, and more preferably 50.)

[0066] Furthermore, the order in which the -Si(CH3)2-O- units and -SiH(CH3)-O- units are arranged is not particularly limited, and may be block-like, disordered, or statistically random.

[0067] The number average molecular weight (Mn) of the vinyl group-containing compound measured by gel permeation chromatography (GPC) is usually 100 to 500,000, and more preferably 100 to 100,000. When the number average molecular weight is equal to or greater than the lower limit, the resulting silylated polyolefin can be further prevented from bleeding or blooming from the rubber layer. When the number average molecular weight is equal to or less than the upper limit, the dispersibility of the silylated polyolefin in the rubber layer is improved, and the rubber layer can be handled more easily. In this embodiment, the number average molecular weight (Mn), weight average molecular weight (Mw) and Mw / Mn are expressed as values ​​calculated in terms of polyethylene, as described later.

[0068] <Vinyl group-containing compound> The vinyl group-containing compound constituting the silylated polyolefin (H) according to the present invention is usually obtained by polymerizing or copolymerizing one or more olefins selected from olefins having 2 to 50 carbon atoms.

[0069] Specific examples of the olefin having 2 to 50 carbon atoms include ethylene, propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 3,4-dimethyl-1-pentene, 4-methyl-1-hexene, 3-ethyl-1-pentene, 3-ethyl-4-methyl-1-pentene, 3,4-dimethyl-1-hexene, 4-methyl-1-heptene, 3,4-dimethyl-1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, α-olefins such as 1-octadecene, 1-eicosene, and vinylcyclohexane; olefins containing internal double bonds such as cis-2-butene and trans-2-butene; isobutene, 2-methyl-1-pentene, 2,4-dimethyl-1-pentene, 2,4-dimethyl-1-hexene, 2,4,4-trimethyl-1-pentene, 2,4-dimethyl-1-heptene, 2-methyl-1-butene, 2-methyl-1-hexene, 2-methyl-1-heptene, 2-methyl-1-octene, 2,3-dimethyl-1-butene, 2,3-dimethyl-1-pentene, 2,3-dimethyl-1-hexene, 2,3-dimethyl-1-octene, 2,3,3-trimethyl-1-butene, 2,3,3-trimethyl-1-pentene, 2,3,3-trimethyl-1-hexene, 2,3,3-trimethyl-1-octene, 2,3,4-trimethyl-1-pentene, 2,3,4-trimethyl-1-hexene, 2,3,4-trimethyl-1-octene, 2,4,4-trimethyl-1-hexene, 2,4,4-trimethyl-1-octene, 2-methyl-3-cyclohexyl-1-propylene, vinylidene cyclohexyl vinylidene compounds such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, o-ethylstyrene, m-ethylstyrene, p-ethylstyrene; arylvinylidene compounds such as α-methylstyrene, α-ethylstyrene, 2-methyl-3-phenylpropylene;Functional group-substituted vinylidene compounds such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, 2-cyanopropylene, 2-aminopropylene, 2-hydroxymethylpropylene, 2-fluoropropylene, and 2-chloropropylene; cyclobutene, cyclopentene, 1-methyl-1-cyclopentene, 3 -Methyl-1-cyclopentene, 2-methyl-1-cyclopentene, cyclohexene, 1-methyl-1-cyclohexene, 3-methyl-1-cyclohexene, 2-methyl-1-cyclohexene, cycloheptene, cyclooctene, norbornene, 5-methyl-2-norbornene, tetracyclododecene, 5,6-dihydrodicyclopentadiene, 3a,4,5,6,7,7a-hexahydro-1H-indene, tricyclo[6.2.1.0; 2,7 ]Aliphatic cyclic olefins containing internal double bonds, such as undec-4-ene, cyclopentadiene, and dicyclopentadiene; cyclic olefins containing aromatic rings, such as cyclopent-2-enylbenzene, cyclopent-3-enylbenzene, cyclohex-2-enylbenzene, cyclohex-3-enylbenzene, indene, 1,2-dihydronaphthalene, 1,4-dihydronaphthalene, and 1,4-methino-1,4,4a,9a-tetrahydrofluorene; butadiene, isoprene, 4-methyl-1,3-pentadiene, 4-methyl-1,4-pentadiene, and 1,3-pentene. Examples of the polyenes include cyclic polyenes having two or more double bonds and chain polyenes having two or more double bonds, such as 1,4-pentadiene, 1,5-hexadiene, 1,4-hexadiene, 1,3-hexadiene, 1,3-octadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, 1,7-octadiene, ethylidenenorbornene, vinylnorbornene, dicyclopentadiene, 7-methyl-1,6-octadiene, 4-ethylidene-8-methyl-1,7-nonadiene, and 5,9-dimethyl-1,4,8-decatriene.

[0070] The olefin having 2 to 50 carbon atoms may have a functional group containing an atom such as oxygen, nitrogen, or sulfur. For example, unsaturated carboxylic acids such as acrylic acid, fumaric acid, itaconic acid, and bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic acid, and unsaturated carboxylic acid metal salts thereof such as sodium salts, potassium salts, lithium salts, zinc salts, magnesium salts, and calcium salts; unsaturated carboxylic acid anhydrides such as maleic anhydride, itaconic anhydride, and bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic anhydride; unsaturated carboxylic acid esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, and 2-ethylhexyl acrylate; vinyl acetate, vinyl propionate, vinyl caproate, vinyl caprate, vinyl laurate, vinyl stearate, and trimethylol acrylate. vinyl esters such as vinyl fluoroacetate; unsaturated glycidyl esters such as glycidyl acrylate, glycidyl methacrylate, and monoglycidyl itaconic acid ester; halogenated olefins such as vinyl chloride, vinyl fluoride, and allyl fluoride; unsaturated cyano compounds such as acrylonitrile and 2-cyano-bicyclo[2.2.1]hept-5-ene; unsaturated ether compounds such as methyl vinyl ether and ethyl vinyl ether; unsaturated amides such as acrylamide, methacrylamide, and N,N-dimethylacrylamide; functional group-containing styrene derivatives such as methoxystyrene, ethoxystyrene, vinylbenzoic acid, methyl vinylbenzoate, vinylbenzyl acetate, hydroxystyrene, o-chlorostyrene, p-chlorostyrene, and divinylbenzene; and N-vinylpyrrolidone.

[0071] In a preferred embodiment, the vinyl group-containing compound has a structure represented by the following formula (4) and is a compound having a number average molecular weight of 100 or more and 500,000 or less.

[0072] A-CH=CH2 (4) In the above formula (4), A is a polymer chain containing one or more structural units derived from an α-olefin having 2 to 50 carbon atoms.

[0073] In the above formula (4), the part A of the vinyl group-containing compound is preferably an ethylene polymer chain, a propylene polymer chain, or a copolymer chain of two or more olefins selected from the group consisting of α-olefins having 2 to 50 carbon atoms. The α-olefin is preferably an α-olefin having 2 to 20 carbon atoms.

[0074] In a preferred embodiment, A of the vinyl group-containing compound represented by the above formula (4) is a polymer chain composed only of an α-olefin having 2 to 50 carbon atoms. More preferably, A of the vinyl group-containing compound is a polymer chain composed only of an α-olefin having 2 to 20 carbon atoms. Even more preferably, A of the vinyl group-containing compound is an ethylene homopolymer chain, a propylene homopolymer chain, or an ethylene / α-olefin copolymer chain having 3 to 20 carbon atoms.

[0075] The vinyl group-containing compound represented by the above formula (4) is preferably an ethylene-α-olefin copolymer containing 81 to 100 mol % of ethylene-derived structural units and 0 to 19 mol % of C3 to C20 α-olefin-derived structural units. More preferably, it is an ethylene-α-olefin copolymer containing 90 to 100 mol % of ethylene-derived structural units and 0 to 10 mol % of C3 to C20 α-olefin-derived structural units. However, the total of the ethylene-derived structural units and the C3 to C20 α-olefin-derived structural units is 100 mol %. It is particularly preferred that the ethylene-derived structural units are 100 mol %.

[0076] Moreover, the vinyl group-containing compound represented by the above formula (4) preferably has a molecular weight distribution (ratio of weight average molecular weight to number average molecular weight, Mw / Mn) measured by gel permeation chromatography (GPC) in the range of 1.1 to 3.0.

[0077] The vinyl group-containing compound represented by the above formula (4) desirably has a number average molecular weight (Mn) in the range of 100 or more and 500,000 or less, more preferably 100 or more and 100,000 or less, even more preferably 500 or more and 50,000 or less, and even more preferably 700 or more and 10,000 or less.

[0078] The vinyl group-containing compound represented by the above formula (4) preferably has a melting point of 70°C or higher and 130°C or lower.

[0079] More preferably, the vinyl group of the vinyl group-containing compound represented by the above formula (4) is present at the terminal of the main chain, and even more preferably, the vinyl group is present only at the terminal of the main chain.

[0080] In addition, when the vinyl group-containing compound represented by the above formula (4) contains a vinyl group only at the terminal of the main chain, 1 It is preferable that the terminal unsaturation rate calculated by H-NMR is 60 mol % or more and 100 mol % or less. 1 The percentage of terminal unsaturation calculated by H-NMR is 80 mol % or more and 99.5 mol % or less, more preferably 90 mol % or more and 99 mol % or less.

[0081] As the vinyl group-containing compound represented by the above formula (4), for example, the examples described in JP-A-2017-155159, particularly paragraphs

[0117] to

[0156] of the publication, can be used.

[0082] The silylated polyolefin used in the present embodiment may be one produced by any method. For example, the examples described in JP 2017-155159 A, particularly the examples described in paragraphs

[0159] to

[0189] of the publication, can be used.

[0083] The silylated polyolefin (H) is presumed to have a structure such as that represented by the formulas (5) to (9). Of course, the combination of the silicon-containing compound and the vinyl group-containing compound is not limited to these examples.

[0084] [ka]

[0085] [ka]

[0086] [ka]

[0087] [ka]

[0088] [ka]

[0089] The layer made of the ethylene copolymer composition containing the ethylene copolymer (L) and the silylated polyolefin (H) has good adhesion to the layer [II] containing a fiber material described below.

[0090] The silylated polyolefin (H) according to the present invention is manufactured and sold by Mitsui Fine Chemicals, Inc. under the trade names of Exfora (registered trademark), Exfora (registered trademark) PE, and the like.

[0091] <Ethylene-Based Copolymer Composition> The ethylene-based copolymer composition of the present invention and the ethylene-based copolymer composition forming the layer [I] of the laminate of the present invention are compositions containing the above-mentioned ethylene-α-olefin-non-conjugated polyene copolymer (L) and the above, and preferably contain 0.1 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, of the silylated polyolefin (H) per 100 parts by mass of the ethylene-α-olefin-non-conjugated polyene copolymer (L).

[0092] The ethylene-based copolymer composition of the present invention contains the silylated polyolefin (H) in addition to the ethylene-α-olefin-non-conjugated polyene copolymer (L), and therefore has good adhesion to other materials, for example layers containing fibrous materials such as industrial belts, and a crosslinked laminate has excellent adhesive strength with layers containing fibrous materials.

[0093] In addition to the ethylene copolymer (L) and the silylated polyolefin (H), the ethylene copolymer composition of the present invention may contain other components according to the desired purpose within the range that does not impair the effects of the present invention. The other components may contain at least one selected from, for example, a crosslinking agent, a crosslinking aid, a vulcanization accelerator, a vulcanization aid, a filler, a softener, an antiaging agent (stabilizer), a processing aid, an activator, a heat stabilizer, a weather stabilizer, an antistatic agent, a colorant, a lubricant, and a thickener. Each additive may be used alone or in combination of two or more.

[0094] <Crosslinking agents, crosslinking assistants, vulcanization accelerators and vulcanization assistants> Examples of the crosslinking agent include crosslinking agents generally used when crosslinking rubber, such as organic peroxides, phenolic resins, sulfur-based compounds, hydrosilicone-based compounds, amino resins, quinones or their derivatives, amine-based compounds, azo-based compounds, epoxy-based compounds, isocyanate-based compounds, etc. Among these, organic peroxides and sulfur-based compounds (hereinafter also referred to as "vulcanizing agents") are preferred.

[0095] Examples of organic peroxides include dicumyl peroxide (DCP), di-tert-butyl peroxide, 2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(tert-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butyl peroxybenzoate, ert-butylperoxyisopropyl carbonate, diacetyl peroxide, lauroyl peroxide, and tert-butylcumyl peroxide.

[0096] When an organic peroxide is used as a crosslinking agent, the amount of the organic peroxide in the copolymer composition is generally 0.1 to 20 parts by mass, preferably 0.2 to 15 parts by mass, and more preferably 0.5 to 10 parts by mass, based on 100 parts by mass of the ethylene copolymer (L). When the amount of the organic peroxide is within the above range, the ethylene copolymer composition exhibits excellent crosslinking properties without blooming on the surface of the obtained molded article, which is preferable.

[0097] When an organic peroxide is used as a crosslinking agent, it is preferable to use a crosslinking assistant in combination. Examples of the crosslinking assistant include sulfur; quinone dioxime crosslinking assistant such as p-quinone dioxime; acrylic crosslinking assistant such as ethylene glycol dimethacrylate and trimethylolpropane trimethacrylate; allyl crosslinking assistant such as diallyl phthalate and triallyl isocyanurate; maleimide crosslinking assistant; divinylbenzene; and metal oxides such as zinc oxide (e.g., ZnO#1·zinc oxide type 2 (JIS standard (K-1410)), manufactured by Hakusui Tech Co., Ltd.), magnesium oxide, and activated zinc oxide (e.g., META-Z102, manufactured by Inoue Seki Kogyo Co., Ltd.).

[0098] When a crosslinking aid is used, the amount of the crosslinking aid in the ethylene copolymer composition is usually 0.5 to 10 mol, preferably 0.5 to 7 mol, more preferably 1 to 6 mol, per mol of the organic peroxide.

[0099] Examples of sulfur-based compounds (vulcanizing agents) include sulfur, sulfur chloride, sulfur dichloride, morpholine disulfide, alkylphenol disulfide, tetramethylthiuram disulfide, and selenium dithiocarbamate.

[0100] When a sulfur-based compound is used as a crosslinking agent, the blending amount in the copolymer composition is usually 0.1 to 10 parts by mass, preferably 0.2 to 7.0 parts by mass, and more preferably 0.3 to 5.0 parts by mass, based on 100 parts by mass of the ethylene-based copolymer (L). When the blending amount of the sulfur-based compound is within the above range, there is no bloom on the surface of the obtained molded article, and the ethylene-based copolymer composition shows excellent crosslinking properties.

[0101] When a sulfur-based compound is used as the crosslinking agent, it is preferable to use a vulcanization accelerator in combination. Examples of the vulcanization accelerator include N-cyclohexyl-2-benzothiazole sulfenamide, N-oxydiethylene-2-benzothiazole sulfenamide, N,N'-diisopropyl-2-benzothiazole sulfenamide, 2-mercaptobenzothiazole (e.g., Suncerer M, manufactured by Sanshin Chemical Industry Co., Ltd.), 2-(4-morpholinodithio)benzothiazole (e.g., Noccelaer MDB-P, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 2-(2,4-dinitrophenyl)mercaptobenzothiazole, 2-(2,6-dinitrophenyl)mercaptobenzothiazole, Thiazole-based vulcanization accelerators such as diethyl-4-morpholinothio)benzothiazole and dibenzothiazyl disulfide (e.g., Suncerer DM, manufactured by Sanshin Chemical Industry Co., Ltd.); guanidine-based vulcanization accelerators such as diphenylguanidine, triphenylguanidine, and diorthotolylguanidine; aldehyde amine-based vulcanization accelerators such as acetaldehyde-aniline condensation product and butyraldehyde-aniline condensation product; imidazoline-based vulcanization accelerators such as 2-mercaptoimidazoline; tetramethylthiuram monosulfide (e.g., For example, thiuram-based vulcanization accelerators such as Sancerer TS, manufactured by Sanshin Chemical Industry Co., Ltd.), tetramethylthiuram disulfide (for example, Sancerer TT, manufactured by Sanshin Chemical Industry Co., Ltd.), tetraethylthiuram disulfide (for example, Sancerer TET, manufactured by Sanshin Chemical Industry Co., Ltd.), tetrabutylthiuram disulfide (for example, Sancerer TBT, manufactured by Sanshin Chemical Industry Co., Ltd.), and dipentamethylenethiuram tetrasulfide (for example, Sancerer TRA, manufactured by Sanshin Chemical Industry Co., Ltd.); zinc dimethyldithiocarbamate, diethyldithiocarbamate, dithioacid salt-based vulcanization accelerators such as zinc dibutyldithiocarbamate (e.g., Sanseller PZ, Sanseller BZ, and Sanseller EZ, all manufactured by Sanshin Chemical Industry Co., Ltd.) and tellurium diethyldithiocarbamate; thiourea-based vulcanization accelerators such as ethylenethiourea (e.g., Sanseller BUR, manufactured by Sanshin Chemical Industry Co., Ltd.), Sanseller 22-C, manufactured by Sanshin Chemical Industry Co., Ltd.), N,N'-diethylthiourea, and N,N'-dibutylthiourea; and xanthate-based vulcanization accelerators such as zinc dibutylxantogenate.

[0102] When a vulcanization accelerator is used, the blending amount of the vulcanization accelerator in the copolymer composition is generally 0.1 to 20 parts by mass, preferably 0.2 to 15 parts by mass, and more preferably 0.5 to 10 parts by mass, based on 100 parts by mass of the ethylene-based copolymer (L). When the blending amount of the vulcanization accelerator is within the above range, the copolymer composition exhibits excellent crosslinking properties without blooming on the surface of the obtained molded article. When a sulfur-based compound is used as a crosslinking agent, a vulcanization assistant can be used in combination.

[0103] Examples of the vulcanization aid include zinc oxide (eg, ZnO#1 / zinc oxide type 2, manufactured by Hakusui Tech Co., Ltd.), magnesium oxide, and activated zinc oxide (eg, META-Z102, zinc oxide manufactured by Inoue Sekikogyo Co., Ltd.).

[0104] When a vulcanization aid is used, the blending amount of the vulcanization aid in the ethylene-based copolymer composition is usually 1 to 20 parts by mass based on 100 parts by mass of the ethylene-based copolymer (L).

[0105] <Filler> The filler is a known rubber reinforcing agent that is compounded in the rubber composition, and is usually an inorganic substance called carbon black or an inorganic reinforcing agent. Specific examples of the filler include carbon black such as Asahi #55G, Asahi #60UG, Asahi #70 (all manufactured by Asahi Carbon Co., Ltd.), Seast V, SO, 116, 3, 6, 9, SP, TA, etc. (all manufactured by Tokai Carbon Co., Ltd.), these carbon blacks surface-treated with a silane coupling agent or the like, silica, activated calcium carbonate, finely divided talc, finely divided silicic acid, light calcium carbonate, heavy calcium carbonate, talc, clay, etc., and preferably carbon black, light calcium carbonate, heavy calcium carbonate, talc, clay, etc.

[0106] These fillers may be used alone or in combination of two or more. When the copolymer composition of the present invention contains a filler, the filler may be blended in an amount of preferably 10 to 300 parts by mass, more preferably 30 to 250 parts by mass, per 100 parts by mass of the ethylene copolymer (L).

[0107] <Softener> Examples of softeners include petroleum-based softeners such as process oil, lubricating oil, paraffin oil, liquid paraffin, petroleum asphalt, and Vaseline; coal tar-based softeners such as coal tar; fatty oil-based softeners such as castor oil, linseed oil, rapeseed oil, soybean oil, and coconut oil; waxes such as beeswax and carnauba wax; naphthenic acid, pine oil, rosin or derivatives thereof; synthetic polymeric substances such as terpene resins, petroleum resins, and coumarone-indene resins; ester-based softeners such as dioctyl phthalate and dioctyl adipate; and others, such as microcrystalline wax, liquid polybutadiene, modified liquid polybutadiene, hydrocarbon-based synthetic lubricating oils, tall oil, and sub(factice). Of these, petroleum-based softeners are preferred, and process oil is particularly preferred.

[0108] When the ethylene copolymer composition contains a softener, the blending amount of the softener is preferably 2 to 100 parts by mass, more preferably 10 to 100 parts by mass, based on 100 parts by mass of the ethylene copolymer (L).

[0109] <Anti-aging agent (stabilizer)> By blending an antioxidant (stabilizer) with the ethylene copolymer composition of the present invention, the life of the seal packing formed therefrom can be extended. Examples of such antioxidants include conventionally known antioxidants, such as amine-based antioxidants, phenol-based antioxidants, and sulfur-based antioxidants.

[0110] Examples of the anti-aging agents include aromatic secondary amine-based anti-aging agents such as phenylbutylamine and N,N-di-2-naphthyl-p-phenylenediamine; phenol-based anti-aging agents such as dibutylhydroxytoluene and tetrakis[methylene(3,5-di-t-butyl-4-hydroxy)hydrocinnamate]methane; thioether-based anti-aging agents such as bis[2-methyl-4-(3-n-alkylthiopropionyloxy)-5-t-butylphenyl]sulfide; dithiocarbamate-based anti-aging agents such as nickel dibutyldithiocarbamate; and sulfur-based anti-aging agents such as 2-mercaptobenzoylimidazole, 2-mercaptobenzimidazole, zinc salt of 2-mercaptobenzimidazole, dilaurylthiodipropionate, and distearylthiodipropionate.

[0111] When the ethylene copolymer composition contains an antioxidant, the amount of the antioxidant is preferably 0.3 to 10 parts by mass, more preferably 0.5 to 7.0 parts by mass, based on 100 parts by mass of the ethylene copolymer (L). When the amount of the antioxidant is within the above range, there is no bloom on the surface of the obtained molded article, and furthermore, the occurrence of vulcanization inhibition can be suppressed.

[0112] <Processing aids> As the processing aid, a wide variety of processing aids that are generally compounded with rubber can be used.Specific examples include ricinoleic acid, stearic acid, palmitic acid, lauric acid, barium stearate, zinc stearate, calcium stearate, zinc laurate, and esters.Of these, stearic acid is preferred.

[0113] When the copolymer composition contains a processing aid, it can be appropriately blended in an amount of preferably 1 to 3 parts by mass per 100 parts by mass of the ethylene copolymer (L). When the blending amount of the processing aid is within the above range, it is preferable because the processability such as kneading processability, extrusion processability, and injection moldability is excellent. The processing aid may be used alone or in combination with two or more kinds.

[0114] <Activator> Examples of the activator include amines such as di-n-butylamine, dicyclohexylamine, and monoethanolamine; activators such as diethylene glycol, polyethylene glycol, lecithin, triaryl methylate, and zinc compounds of aliphatic or aromatic carboxylic acids; zinc peroxide preparations; octadecyltrimethylammonium bromide, synthetic hydrotalcite, and special quaternary ammonium compounds.

[0115] When the copolymer composition contains an activator, the amount of the activator is preferably 0.2 to 10 parts by mass, more preferably 0.3 to 5 parts by mass, based on 100 parts by mass of the ethylene copolymer (L).

[0116] <Laminate> In the laminate of the present invention, a layer [I] made of the ethylene copolymer composition of the present invention is in contact with a layer [II] containing a fibrous material.

[0117] <Layer [I] made of ethylene-based copolymer composition> In the layer [I] made of an ethylene-based copolymer composition constituting the laminate of the present invention, the ethylene-based copolymer composition may be crosslinked or uncrosslinked.

[0118] When the ethylene copolymer composition constituting the layer [I] of the laminate is crosslinked, it exhibits excellent peel strength to the layer [II] containing a fibrous material described below. When the ethylene copolymer composition constituting the layer [I] of the laminate is uncrosslinked, it exhibits excellent adhesion to the layer [II] containing a fibrous material described below.

[0119] <Layer containing fiber material [II]> The layer [II] containing a fiber material that constitutes the laminate of the present invention contains a fiber material in at least a part of the layer.

[0120] Examples of fiber materials forming the layer [II] of the present invention include various known fiber materials, for example, natural fibers such as canvas, cotton, and wood cellulose fibers; organic fiber materials such as fibers made of synthetic resins such as polyamide, polyester, polyvinyl alcohol, rayon, polyparaphenylene benzobisoxazole, polyethylene, polypropylene, polyarylate, polyimide, polyphenylene sulfide, polyether ether ketone, polylactic acid, polycaprolactone, polybutylene succinate, and fluorine-based polymers; and inorganic fiber materials such as glass fibers, PAN-based carbon fibers, pitch-based carbon fibers, alumina fibers, silicon carbide fibers, aluminum borate fibers, and potassium titanate whiskers.

[0121] These fiber materials may be long fibers (filaments) or short fibers (staples), and may be cord yarns, spun yarns, woven fabrics, knitted fabrics, nonwoven fabrics, and the like.

[0122] Examples of the polyamide include aliphatic polyamides such as nylon 6, nylon 6,6, and nylon 6,10; semi-aromatic polyamides such as polymetaxylylene adipamide (MXD6), polyhexamethylene terephthalamide (6T), and copolymer polyamides containing these units; and fully aromatic polyamides such as polybenzamide, poly-p-phenylene terephthalamide, and poly-m-phenylene isophthalamide.

[0123] In addition, these fiber materials may be surface-treated by a known method such as RFL treatment in order to improve adhesion between the fiber materials themselves or with the layer [I] made of the above-mentioned ethylene-based copolymer composition, and it is preferable that the fiber material of layer [II] contains RFL-treated fibers.

[0124] RFL treatment is a process in which textile materials are treated with a treatment liquid (RFL liquid) containing resorcinol, formalin, and latex, and the RFL liquid is a mixture of the initial condensation product of resorcinol and formalin and rubber latex. Examples of rubber latex that can be used include styrene-butadiene-vinylpyridine terpolymer (VP), styrene-butadiene copolymer (SBR), chloroprene (CR), acrylonitrile-butadiene copolymer (NBR), hydrogenated NBR (H-NBR), chlorosulfonated ethylene (CSM), and natural rubber. These can be used alone or in a blend of two or more types.

[0125] <Method of manufacturing laminate> To produce the laminate of the present invention, various known methods for producing laminates can be adopted. For example, a method of laminating a layer [I] of an uncrosslinked ethylene-based copolymer composition produced (molded) in advance by a known method with a layer [II] containing a fiber material, and then crosslinking the layer [I] of the ethylene-based copolymer composition, a method of laminating a layer [I] of a crosslinked ethylene-based copolymer composition with a layer [II] containing a fiber material, or a method of extrusion coating a layer [I] of an ethylene-based copolymer composition on a layer [II] containing a fiber material, and then crosslinking the layer [I] of the ethylene-based copolymer composition.

[0126] The layer [I] made of the ethylene copolymer composition can be produced by various known methods. The ethylene copolymer composition can be obtained by kneading the ethylene-α-olefin-non-conjugated polyene copolymer (L) with the silylated polyolefin (H), and further with a crosslinking agent, and, if necessary, additives such as a filler, a softener, an antioxidant, and a processing aid, using any of various known kneading and mixing devices, for example, a Banbury mixer, a kneader, an internal mixer (internal mixer) such as an Intermix, and a roll.

[0127] The uncrosslinked ethylene-based copolymer composition obtained by kneading may be molded into an intended shape by various molding methods such as an extrusion molding machine, a calendar roll, a press, an injection molding machine, or a transfer molding machine, and then crosslinked to form a layer [I] consisting of the ethylene-based copolymer composition, which may then be laminated (bonded) with a layer [II] containing a fiber material; alternatively, the uncrosslinked ethylene-based copolymer composition may be molded into an intended shape by the above-mentioned method, and then laminated (bonded) with a layer [II] containing a fiber material, thereby crosslinking the composition.

[0128] The layer [I] made of the ethylene copolymer composition may be crosslinked by heating using a crosslinking agent or by irradiating with light, gamma rays or electron beams. In addition, when crosslinking, a mold may be used, or crosslinking may be performed without using a mold. When a mold is not used, the molding and crosslinking steps are usually performed continuously. As a heating method in the crosslinking tank, a heating tank using hot air, a glass bead fluidized bed, UHF (ultra-high frequency electromagnetic waves), steam, etc. may be used.

[0129] <Applications of laminate> A laminate in which a layer [I] made of the ethylene-based copolymer composition of the present invention is in contact with a layer [II] containing a fiber material is suitably used for automobile hoses, water hoses, gas hoses, power transmission belts, conveyor belts, escalator handrails, and other industrial belts.

[0130] Examples of the automobile hose include brake hoses, radiator hoses, heater hoses, and air cleaner hoses. Examples of the transmission belt include a V-belt, a flat belt, a toothed belt, etc. Examples of the conveyor belt include a light conveyor belt, a cylindrical belt, a rough top belt, a flanged conveyor belt, a U-shaped guide conveyor belt, a V-guide conveyor belt, etc. EXAMPLES

[0131] Next, examples of the present invention will be shown and described in more detail, but the present invention is not limited thereto.

[0132] [Composition and Physical Properties of Ethylene Copolymer] The composition of the ethylene copolymer and the evaluation methods for various physical properties are as follows. [Ratio of Each Structural Unit in Ethylene Copolymer]< The ratio of the structural unit derived from ethylene, the ratio of the structural unit derived from α-olefin, and the ratio of the structural unit derived from non-conjugated polyene contained in the ethylene copolymer are 1 determined by 1H-NMR. Details of the measurement conditions are described in International Publication No. 2015 / 122415.

[0133] [Mooney Viscosity]< The Mooney viscosity (ML (1+4) at 100 °C and 125 °C) was measured in accordance with JIS K6300 (1994) using a Mooney viscometer (SMV202 type manufactured by Shimadzu Corporation).

[0134] [B Value]< Using o-dichlorobenzene-d4 / benzene-d6 (4 / 1 [v / v]) as the measurement solvent and a measurement temperature of 120 °C, 13 the 13C-NMR spectrum (100 MHz, ECX400P manufactured by JEOL Ltd.) was measured and calculated based on the following formula (i). B value = ([EX] + 2[Y]) / 〔2 × [E] × ([X] + [Y])〕 ··· (i) [Here, [E], [X], and [Y] represent the mole fractions of the structural units derived from ethylene [A], α-olefin [B] having 4 to 20 carbon atoms, and non-conjugated polyene [C], respectively, and [EX] represents the ethylene [A]-α-olefin [B] having 4 to 20 carbon atoms dyad chain fraction.]

[0135] [Raw Materials] In the examples, an ethylene-1-butene-5-ethylidene-2-norbornene (ENB) copolymer having the following physical properties was used in accordance with the description of [Synthesis Example C1] in WO 2015 / 122415. Hereinafter, this is referred to as "ethylene copolymer (L-1)". Structural units derived from ethylene: 67.7 mol% Structural units derived from 1-butene: 30.0 mol% Structural units derived from ENB: 2.3 mol% Mooney Viscosity ML (1+4) 100℃:30 Mooney Viscosity ML (1+4) 125℃:22 B value: 1.3

[0136] In addition, in the comparative examples, an ethylene-propylene-ENB copolymer (Mitsui EPT 4045M, manufactured by Mitsui Chemicals, Inc.) (hereinafter also referred to as "copolymer-2") having the following physical properties was used as the ethylene-α-olefin-non-conjugated polyene copolymer. Ethylene content: 45% by mass Diene (ENB) content: 7.6% by weight Mooney Viscosity ML (1+4) 100℃:45

[0137] <Physical Properties of Ethylene-Based Copolymer Composition (Cross-Linked Product)> <Durometer A hardness> According to JIS K 6253, the sheet hardness (type A durometer, HA) was measured using six 2 mm crosslinked sheets with smooth surfaces, stacking the flat parts to a thickness of approximately 12 mm. However, specimens with foreign matter, air bubbles, or scratches were not used. The dimensions of the measurement surface of the specimen were set so that the tip of the indenter could be measured at a position 12 mm or more away from the end of the specimen.

[0138] <Tensile stress at break, tensile elongation at break> The tensile stress at break and the tensile elongation at break of the sheet were measured by the following method. The sheet was punched out to prepare No. 3 dumbbell test pieces described in JIS K 6251 (1993). Using these test pieces, tensile tests were performed according to the method specified in JIS K6251, section 3, at a measurement temperature of 25°C and a tensile speed of 500 mm / min, and the modulus at 100% elongation (M100), tensile stress at break (TB), and tensile elongation at break (EB) were measured.

[0139] <<Physical Properties of Uncrosslinked Ethylene-Based Copolymer Composition>> <Adhesiveness> The adhesion between the layer [I] made of the uncrosslinked ethylene copolymer composition and the layer [II] containing a fiber material was measured by a probe tack test. The test was carried out using a Rhesca tack tester (TAC-II). A stainless steel cylindrical probe with a diameter of 5 mm was brought into contact with the test specimen, and the tack (gf) that occurred when peeling was evaluated. The contact speed of the probe to the test specimen was 120 mm / min, the pressure applied was 50 gf, the pressure time was 20 seconds, the peel speed was 120 mm / min, and the temperature was 23°C or 50°C.

[0140] <<Physical Properties of Crosslinked Ethylene-Based Copolymer Composition>> (peel strength) The peel strength (adhesion strength) between the layer [I] made of the crosslinked ethylene copolymer composition and the layer [II] containing a fiber material was measured by the following method. A 3 mm thick uncrosslinked sheet was placed on a woven fabric of RFL-treated nylon fiber [manufactured by Ayaha Kogyo Co., Ltd.] and pressed at 170°C for 15 minutes using a 200-ton press molding machine to crosslink the uncrosslinked sheet and obtain a laminate. A test piece with a width of 25 mm was punched out from the laminate and subjected to a T-peel test at a tensile speed of 200 mm / min.

[0141] [Example 1] The ethylene copolymer (L-1) was masticated for 30 seconds, and 100 parts by mass of the masticated ethylene copolymer (L-1) was mixed with 5 parts by mass of zinc oxide (ZnO#1) as a crosslinking aid, 1 part by mass of stearic acid as a processing aid, 2 parts by mass of tetrakis[methylene(3,5-di-t-butyl-4-hydroxy)hydrocinnamate]methane (Irganox (registered trademark) 1010, manufactured by BASF Japan Ltd.) as an antiaging agent, 4 parts by mass of 2-mercaptobenzimidazole (Sandant MB, manufactured by Sanshin Chemical Industry Co., Ltd.), 50 parts by mass of carbon black (Asahi #70, manufactured by Asahi Carbon Co., Ltd.), and 10 parts by mass of a softener (Diana Process Oil PW-380, manufactured by Idemitsu Kosan Co., Ltd.) in a 1.7-liter Banbury mixer (manufactured by Kobe Steel, Ltd.) for 2 minutes.

[0142] Thereafter, the ram was raised and cleaned, and further kneading was carried out for 1 minute, and the mixture was discharged at about 150° C. to obtain a compound. This kneading was carried out at a filling rate of 70%. Next, 172 parts by mass of the obtained ethylene copolymer (L-1) composition was wound around an 8-inch roll (surface temperature of front roll 50°C, surface temperature of rear roll 50°C, rotation speed of front roll 16 rpm, rotation speed of rear roll 18 rpm), and 6.8 parts by mass of dicumyl peroxide (manufactured by Kayaku Akzo Co., Ltd., trade name Mitsui DCP-40C) as a crosslinking agent and 5 parts by mass of silylated polyolefin (H-1) (trade name Exfora (registered trademark) PE, manufactured by Mitsui Chemicals Fine Co., Ltd.) were added and kneaded for 10 minutes, and then separated into sheets to prepare uncrosslinked sheets with thicknesses of 2 mm and 3 mm.

[0143] The adhesive strength (gf) of the resulting uncrosslinked sheet having a thickness of 2 mm was measured by the method described above. The results are shown in Table 1. Next, the obtained uncrosslinked sheet having a thickness of 2 mm was pressed at 170° C. for 15 minutes using a 100-ton press molding machine to produce a crosslinked sheet. The physical properties of the obtained crosslinked sheet were measured by the methods described above. The results are shown in Table 1.

[0144] Comparative Example 1 Except for using copolymer-2 instead of copolymer (L-1) used in Example 1, and changing the types and amounts of the compounding agents (additives) to those shown in Table 1, an uncrosslinked copolymer composition, a crosslinked copolymer composition, and a laminate were obtained in the same manner as in Example 1, and their physical properties were evaluated by the methods described above. The results are shown in Table 1.

[0145] [Table 1]

Claims

1. An ethylene copolymer composition comprising 100 parts by mass of the following (L) and 0.5 to 10 parts by mass of the following (H): (L) An ethylene / α-olefin / non-conjugated polyene copolymer containing ethylene [A], an α-olefin [B] having 4 to 20 carbon atoms, and a non-conjugated polyene [C], which satisfies the following requirements (1) to (4): (H) Silylated polyolefins. (1) The molar ratio (A / B) of the structural unit derived from ethylene [A] to the structural unit derived from an α-olefin [B] having 4 to 20 carbon atoms is 40 / 60 to 90 / 10. (2) The content of the structural units derived from the non-conjugated polyene [C] is 0.1 to 6.0 mol %, relative to 100 mol % of the total of the structural units derived from ethylene [A], the α-olefin [B] having 4 to 20 carbon atoms, and the non-conjugated polyene [C]. (3) Mooney viscosity ML at 125°C (1+4) (125°C) is 5 to 100. (4) The B value represented by the following formula (i) is 1.20 or more. B value = ([EX] + 2[Y]) / [2 x [E] x ([X] + [Y])]... (i) [Here, [E], [X] and [Y] respectively represent the molar fractions of ethylene [A], the α-olefin [B] having 4 to 20 carbon atoms, and the non-conjugated polyene [C], and [EX] represents the dyad chain fraction of ethylene [A]-α-olefin [B] having 4 to 20 carbon atoms.]

2. The ethylene-based copolymer composition according to claim 1, wherein the α-olefin [B] having 4 to 20 carbon atoms constituting the ethylene / α-olefin / non-conjugated polyene copolymer (L) is 1-butene.

3. The ethylene-based copolymer composition according to claim 1 or 2, further comprising an organic peroxide as a crosslinking agent.

4. A laminate comprising a layer [I] made of the ethylene copolymer composition according to any one of claims 1 to 3 and a layer [II] containing a fiber material in contact with each other.

5. The laminate according to claim 4, wherein the ethylene copolymer composition of the layer [I] is crosslinked.

6. The laminate according to claim 4 or 5, wherein the fiber material of the layer [II] comprises RFL-treated fiber.

7. The laminate according to any one of claims 4 to 6, wherein the textile material of the layer [II] is canvas.

8. An industrial belt comprising the laminate according to any one of claims 4 to 7.

Citation Information

Patent Citations

  • JP1967-023632B

  • ADHEREND OF ETHYLENE / alpha-OLEFIN RUBBER COMPOSITION WITH FIBER AND DRIVING BELT USING THE SAME

    JP2003027376A

  • Belt for power transmission

    JP2003254390A

  • Ethylene-based copolymer, crosslinked ethylene-based copolymer and molded product thereof

    JP2012214576A

  • Composition for hulling roll and hulling roll

    JP2018130645A