Ferritic-austenitic duplex stainless steel welded structure, ferritic-austenitic duplex stainless steel welded joint, and welding method for ferritic-austenitic duplex stainless steel material

The welding method for ferritic-austenitic duplex stainless steel using high nitrogen concentration in the aftergas and backgas addresses corrosion resistance issues by reducing chromium nitride formation, enhancing weld metal and heat-affected zone performance.

JP7584317B2Active Publication Date: 2024-11-15NIPPON STEEL CORPORATION
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021011358
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-27
Publication Date
2024-11-15
Estimated Expiration
2041-01-27

AI Technical Summary

Technical Problem

Existing welding methods for ferritic-austenitic duplex stainless steel result in reduced corrosion resistance due to chromium nitride precipitation in the weld metal and heat-affected zone, limiting applications and increasing costs, especially in thin plates where reheat treatment and filler metal use are challenging.

Method used

A welding method using gas-shielded arc welding with high nitrogen concentration in the aftergas and/or backgas to control the nitrogen content, maintaining the austenite phase ratio and reducing chromium nitride formation, thereby enhancing corrosion resistance.

Benefits of technology

The method improves corrosion resistance of weld metal parts and heat-affected zones, reducing costs and increasing welding workability by minimizing chromium nitride precipitation and maintaining the austenite phase ratio.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584317000003
    Figure 0007584317000003
  • Figure 0007584317000004
    Figure 0007584317000004
  • Figure 0007584317000005
    Figure 0007584317000005
Patent Text Reader

Abstract

To provide ferrite-austenite duplex stainless steel welded structures having a welded metal part with excellent corrosion resistance.SOLUTION: Provided is a ferrite-austenite duplex stainless steel welded structure comprising a base material made of a ferrite-austenite duplex stainless steel material and a weld, wherein a reduction margin of an austenite phase ratio (γBM-γWM) in a surface layer of a weld metal in the weld, which is the difference between an austenite phase ratio γBM in a metallographic structure of the base metal and an austenite phase ratio γWM in the surface layer of the weld metal, is less than 20 area%, and a pitting potential reduction margin (PBM - PWM), which is the difference between a pitting potential PBM of the base metal and a pitting potential PWM of the weld, is less than 150 mV.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ferritic-austenitic duplex stainless steel welded structure, a ferritic-austenitic duplex stainless steel welded joint, and a method for welding ferritic-austenitic duplex stainless steel material. [Background technology]

[0002] Duplex stainless steel is a stainless steel that has both austenite and ferrite phases in the steel structure. Duplex stainless steel has a low Ni content and high strength compared to austenitic stainless steel, which generally has the same corrosion resistance, and is therefore attracting attention as a material that can be alloyed at low cost and thinned. Taking advantage of its high corrosion resistance, it has long been used as thick plate for petrochemical equipment materials, pump materials, chemical tank materials, etc., but in recent years, it has also been used as a thin plate for structural components, etc., taking advantage of its high strength.

[0003] There are many types of duplex stainless steel, such as the alloy-saving type SUS821L1, the SUS329J4L with a relatively medium amount of alloy, and the SUS327L1 with a relatively high amount of alloy. These currently widely used steel types contain about 0.1 to 0.3% N (nitrogen), which is an excellent alloy cost element, along with Cr, Ni, and Mo, as elements that improve corrosion resistance.

[0004] In addition, non-consumable electrode welding or consumable electrode welding is used as a welding method when constructing a welded structure of duplex stainless steel. Examples of non-consumable electrode welding include TIG welding, plasma welding, and laser welding. Examples of consumable electrode welding include MIG welding, gas-shielded arc welding using flux-cored wire, covered metal arc welding, and submerged arc welding. Among these, non-consumable electrode welding is inferior to consumable electrode welding in terms of welding efficiency, but since it uses pure Ar gas as a shielding gas, the amount of oxygen in the weld metal is extremely low and the weld metal has excellent toughness, making it suitable for constructing welded structures with strict quality requirements.

[0005] When applying welded structures using ferritic-austenitic duplex stainless steel as the base metal to necessary applications, the problem is the decrease in corrosion resistance due to the precipitation of σ-phase or chromium nitride in the weld metal and heat-affected zone. Therefore, when using duplex stainless steel as the base metal for welding, it is often necessary to sacrifice welding workability by limiting its use to applications where corrosion resistance is not a major issue, restricting the welding method, performing reheat treatment after welding, and changing the welding gas to a special one.

[0006] As mentioned earlier, ferritic-austenitic stainless steels with relatively low Cr, Ni, and Mo contents and high N content, such as SUS821L1, ASTM S32101, and NSSC 2351, are called alloy-saving duplex stainless steels. Depending on their corrosion resistance level, alloy-saving duplex stainless steels are sometimes used as replacements for general-purpose austenitic stainless steels such as SUS304 and SUS316L. In particular, the formation of chromium nitrides often causes problems with the corrosion resistance of these alloy-saving duplex stainless steels. The corrosion resistance degradation occurs due to the following mechanism:

[0007] In duplex stainless steel, the phase ratio between ferrite and austenite varies depending on the heating temperature. Therefore, when duplex stainless steel is welded, the heating for melting the base metal increases the ratio of ferrite and decreases the ratio of austenite in the parts that will become the weld metal and weld heat-affected zone. On the other hand, the austenite phase increases during cooling when the weld metal and weld heat-affected zone are formed. However, in general, the cooling rate during the formation of the weld metal and weld heat-affected zone is fast, so the ratio of austenite in the weld metal and weld heat-affected zone is less than that in the base metal.

[0008] In addition, N easily evaporates from the weld metal at high temperatures during welding. Since N acts as an austenite stabilizing element and has the effect of increasing the amount of austenite, a decrease in N in the weld metal increases the amount of ferrite.

[0009] Most of the N in duplex stainless steel is dissolved in the austenite phase. However, the proportion of austenite in the weld metal and weld heat-affected zone is smaller than that in the base material, so the N content in the ferrite phase is higher. The solubility limit of N in the ferrite phase is much smaller than that of the austenite phase, so even if there is a slight decrease due to evaporation of N during welding, the N that cannot be dissolved in the ferrite phase precipitates as chromium nitride in the ferrite phase or in the grain boundaries between ferrite phases in the weld metal and weld heat-affected zone during cooling during welding.

[0010] The formation of chromium nitrides consumes Cr in the steel, resulting in the formation of a so-called chromium-deficient zone, which reduces the corrosion resistance of the weld. Therefore, reducing the amount of chromium nitrides that precipitate in the weld metal and weld heat-affected zone is important for improving the corrosion resistance of the weld.

[0011] As a general method for welding duplex stainless steel, Patent Document 1 describes a technique for suppressing the precipitation of chromium nitride by controlling the welding method of the final welding pass.

[0012] Furthermore, Patent Document 2 describes a technique in which the heat-affected zone after welding is heat-treated at 700° C. to 1000° C. to reprecipitate the austenite phase and recover the corrosion resistance of the heat-affected zone.

[0013] Furthermore, Patent Document 3 describes a technology in which a mixed gas of argon and nitrogen is used as a shielding gas during welding, rather than pure argon, to increase the amount of austenite phase in the weld metal and dissolve nitrogen in the austenite phase, thereby suppressing a decrease in corrosion resistance in the heat-affected zone of welding. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] Japanese Patent Application Laid-Open No. 62-199272 [Patent Document 2] JP 2015-217434 A [Patent Document 3] Patent No. 6726499 Summary of the Invention [Problem to be solved by the invention]

[0015] However, in Patent Document 1, control of welding conditions is important, while heat treatment after welding is required in Patent Document 2. In thin plate applications, welding is often performed in large quantities, and restrictions on the welding method or heat treatment after welding may be difficult.

[0016] In Patent Document 3, it is necessary to add nitrogen to the welding gas, but since the shape of the welding arc changes compared to when normal pure argon gas is used, it may take time to optimize the welding conditions. In addition, since nitrogen is more reactive than argon, it may cause the welding electrode to wear out faster in TIG welding, etc.

[0017] Furthermore, in thin plate applications, since no filler metal is generally used during welding, it is difficult to improve corrosion resistance by using filler metal. Therefore, it is possible to improve the corrosion resistance of the weld metal and the weld heat-affected zone by adding alloy elements to the base metal, but this creates another problem of increased alloy costs.

[0018] In view of the above, from the viewpoint of reducing the costs of welding processes and manufacturing welded structures, a method for welding duplex stainless steels that has less restrictions on the welding method, does not require reheat treatment after welding, and reduces the consumption of welding electrodes is desired. Also, from the viewpoint of improving corrosion resistance, a welded structure and a welded joint that have excellent corrosion resistance of the welded part are desired.

[0019] The present invention aims to provide a method for welding ferritic-austenitic duplex stainless steel material, which has two phases, austenite and ferrite, and which reduces the decrease in corrosion resistance of the weld metal and weld heat-affected zone when welding duplex stainless steel, thereby improving welding workability and reducing welding costs, which can be bottlenecks when using such steel. Another object of the present invention is to provide a ferritic-austenitic duplex stainless steel welded structure and a ferritic-austenitic duplex stainless steel welded joint having excellent corrosion resistance in the weld metal zone. [Means for solving the problem]

[0020] The present inventors carried out various tests for steels having various compositions and plate thicknesses in order to evaluate factors that affect the corrosion resistance of the weld metal and the weld heat affected zone when the steels are welded.

[0021] Regarding the above test results, the inventors discovered that the surface vicinity of the weld metal part is more likely to have a structure with lower corrosion resistance than the interior. In welded structures, the weld metal part is not necessarily polished, and in many cases, the weld burn is simply removed with a chemical such as a burn remover. In such cases, the structure near the surface of the weld metal part determines the corrosion resistance.

[0022] Therefore, focusing on the corrosion resistance near the surface of the weld metal, the researchers investigated factors that improve the corrosion resistance near the surface of the weld metal. As a result, they discovered that by using an after-gas and back-gas containing a high concentration of nitrogen during welding, the nitrogen concentration in the surface of the weld metal can be increased, thereby improving corrosion resistance.

[0023] The present invention has been made based on the above findings, and provides the following welding method, welded structure, and welded joint for ferritic-austenitic duplex stainless steel material.

[0024] [1] A base material made of a ferritic-austenitic duplex stainless steel material; a welded portion; Austenite phase ratio γ in the metal structure of the base material BM and the austenite fraction γ of the surface layer of the weld metal part of the weld part WM The difference between the austenite phase ratio decrease in the surface layer of the weld metal part (γ BM -γ WM ) is less than 20% by area, The pitting potential P of the base material BMand the pitting potential P of the weld WM The difference between the pitting potential drop (P BM -P WM ) is less than 150 mV for ferritic-austenitic duplex stainless steel welded structures. [2] A base material made of a ferritic-austenitic duplex stainless steel material; a welded portion; Austenite phase ratio γ in the metal structure of the base material BM and the austenite fraction γ of the surface layer of the weld metal part of the weld part WM The difference between the austenite phase ratio decrease in the surface layer of the weld metal part (γ BM -γ WM ) is less than 20% by area, The pitting potential P of the base material BM and the pitting potential P of the weld WM The difference between the pitting potential drop (P BM -P WM ) is less than 150mV for ferritic-austenitic duplex stainless steel welded joints. [3] A method for welding a base material made of a ferritic-austenitic duplex stainless steel material by a gas-shielded arc welding method, comprising the steps of: No filler metal is used, After gas and / or back gas, N 2 gas This is a welding method for ferritic-austenitic dual phase stainless steels using a ferritic-austenitic dual phase welding method. [4] A method for welding ferritic-austenitic dual-phase stainless steel according to [3], in which a gas containing less than 60% by volume of N2 is used as a torch shielding gas. 。 Effect of the Invention

[0025] According to the welding method of the present invention, in a duplex stainless steel having two phases, that is, an austenite phase and a ferrite phase, there is little decrease in the corrosion resistance of the weld metal zone and the weld heat-affected zone when the steel is welded, thereby improving the welding workability and reducing the welding costs, which can be bottlenecks when using the steel. Furthermore, according to the welded structure and welded joint of the present invention, the corrosion resistance of the welded metal portion can be improved. [Brief description of the drawings]

[0026] [Figure 1] FIG. 1 is a set of photographs showing the metal structure of the surface layer of a weld metal part obtained by welding a base metal made of steel type B of the embodiment, where (a) is a photograph showing an example in which Ar gas was used as an after-gas (sample number 27), and (b) is a photograph showing an example in which N2 was used as an after-gas (sample number 5). [Diagram 2] FIG. 2 is a graph showing the distribution of nitrogen concentration in the depth direction of the surface layer of a weld metal part obtained by welding a base metal made of steel type B of the embodiment, where (a) is a graph for an example (sample number 32) in which Ar was used for the torch shielding gas and Ar was used for the after-gas, and (b) is a graph for an example (sample number 15) in which Ar+5% N gas was used for the torch shielding gas and Ar gas was used for the after-gas. [Diagram 3] FIG. 3 is a schematic diagram for explaining a welding method in the embodiment. [Figure 4] FIG. 4 is a graph showing the relationship between the reduction in the γ phase rate and the reduction in the pitting potential in the surface layer of the weld metal part in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Below, we will explain embodiments of the present invention, namely, a ferritic-austenitic duplex stainless steel welded structure (sometimes referred to as a welded structure in the following description), a ferritic-austenitic duplex stainless steel welded joint (sometimes referred to as a welded joint in the following description), and a method for welding ferritic-austenitic duplex stainless steel sheets (sometimes referred to as a welding method in the following description).

[0028] The welded structure of the present embodiment includes a base material made of a ferritic-austenitic duplex stainless steel material and a welded portion, and the austenite phase ratio γ BM and the austenite fraction γ of the surface layer of the weld metal of the weld WMThe difference between the austenite fraction in the surface layer of the weld metal and the BM -γ WM ) is less than 20% by area, and the pitting potential P BM and the pitting potential P of the weld WM The difference between the pitting potential drop (P BM -P WM ) is less than 150mV.

[0029] In addition, the welded joint of this embodiment includes a base material made of a ferritic-austenitic duplex stainless steel material and a welded portion, and the austenite phase ratio γ BM and the austenite fraction γ of the surface layer of the weld metal of the weld WM The difference between the austenite fraction in the surface layer of the weld metal and the BM -γ WM ) is less than 20% by area, and the pitting potential P BM and the pitting potential P of the weld WM The difference between the pitting potential drop (P BM -P WM ) is less than 150 mV. Each requirement is explained in detail below.

[0030] (Welded structures and welded joints) In this embodiment, a welded structure and welded joint formed by butt welding will be described as an example, but the present invention is not limited to butt welding and can also be applied to welded structures and welded joints welded by lap welding, fillet welding, etc. In addition, examples of welded structures and welded joints formed by butt welding include welded structures and welded joints in which steel plates are butt welded to each other, and welded structures and welded joints in which ends of steel pipes are butt welded to each other.

[0031] (base material) The base material according to this embodiment is a ferritic-austenitic duplex stainless steel material. The ferritic-austenitic duplex stainless steel material contains a two-phase structure of a ferrite phase and an austenite phase in the metal structure. The shape of the base material is not particularly limited, and may be a plate material, a tube material, a bar material, a wire material, or the like.

[0032] The chemical composition of ferritic-austenitic duplex stainless steel is described below.

[0033] (Regarding welds and weld metal parts) The welded portion according to the present embodiment is composed of a weld metal portion and a weld heat affected zone. In this embodiment, from the viewpoint of improving the corrosion resistance of the welded portion, attention is paid to the reduction in the austenite phase ratio in the weld metal portion and the reduction in the pitting potential in the welded portion.

[0034] (Reduction in the austenite phase ratio of the surface of the weld metal: less than 20% by area) Austenite fraction γ in the metal structure of the base material BM and the austenite fraction γ WM The difference between the austenite fraction in the surface layer of the weld metal and the BM -γ WM ) should be less than 20% by area. The reduction is preferably less than 10%. By keeping the reduction to less than 20% by area, the corrosion resistance of the weld metal part can be increased to the same level as the corrosion resistance of the base material.

[0035] Austenite phase ratio γ in the surface layer of the weld metal BM The reason for focusing on is based on the findings of the present inventors. That is, the present inventors discovered that the vicinity of the surface layer of the welded metal part after welding is more likely to have a structure with lower corrosion resistance than the inside. In this case, the structure near the surface layer of the welded metal part determines the corrosion resistance. Also, in welded structures and welded joints, the surface layer of the welded metal part is not polished, and the weld burn is only removed as necessary with a chemical such as a burn remover, and the surface layer after welding is often left as it is. Therefore, in order to improve the corrosion resistance, it is necessary to reduce the decrease in the austenite phase ratio near the surface layer of the welded metal part.

[0036] In addition, the lower limit of the reduction does not need to be set in particular, but it is preferable to set it to 0%, that is, the austenite phase ratio γ BM and the austenite fraction γ of the surface layer of the weld metal WM It is preferable that the difference between the above is 0%.

[0037] The surface layer of the weld metal is defined as the region from the surface of the weld metal to a depth of 30 μm. The austenite phase content in this region is the austenite phase fraction γ WM Let us assume that.

[0038] In addition, the austenite phase ratio γ BM is the content of the austenite phase in the region from the surface of the base material to a depth of 200 μm.

[0039] Austenite fraction γ in the metal structure of the base material BM The measurement method is as follows. When the base material is a steel plate, the metal structure of a 200 μm wide x 200 μm deep area from the surface layer of a cross section perpendicular to the rolling direction (TD cross section) at the center position in the rolling width direction is observed with an optical microscope. The microstructure image of the observed surface is classified into ferrite phase and austenite phase by image analysis, and the austenite phase ratio γ of the base material is measured. BM Request.

[0040] In addition, the austenite phase ratio γ WM The measurement method is as follows: The metal structure of a 200 μm wide x 30 μm deep area from the surface of a cross section perpendicular to the welding direction at the center of the width of the weld metal part is observed with an optical microscope. The microstructure image of the observed surface is classified into ferrite phase and austenite phase by image analysis, and the austenite phase ratio γ WM Request.

[0041] The decrease in the austenite phase ratio in the surface layer of the weld metal (γ BM -γ WM ) is the austenite fraction of the base material γ BMFrom the austenite fraction γ of the weld metal surface WM The value is the subtracted value.

[0042] (Welded part pitting potential drop: less than 150mV) When chromium nitride precipitates in a welded portion, the corrosion resistance of the welded portion deteriorates more than that of the base material portion. On the other hand, the pitting potential of steel changes depending on the degree of precipitation of chromium nitride, and as the precipitation of chromium nitride progresses, the pitting potential decreases. Therefore, the present inventors focused on the reduction in the pitting potential of the welded portion. The allowable reduction in the pitting potential of the welded portion in this embodiment is less than 150 mV. It is more preferable to make it less than 100 mV. Since the reduction in the pitting potential is preferably as small as possible, no lower limit is set. By making the reduction in the pitting potential of the welded portion less than 150 mV, the corrosion resistance of the welded portion can be improved.

[0043] The decrease in the pitting potential of the weld is the pitting potential P BM and the pitting potential P of the weld WM Difference from (P BM -P WM ).

[0044] Pitting potential P of base material BM is obtained by polishing the surface of the base material to a depth of 0.2 mm and then measuring the pitting potential of the polished surface. In addition, the pitting potential P of the weld WM can be obtained by removing any welding scale adhering to the surface of the weld, masking areas other than the weld, and then measuring the pitting potential of the weld.

[0045] More specifically, the surface of the base material was wet-polished with abrasive grain size #600 at a position 0.2 mm below the surface, and then, using a method specified in JIS G 0577, a current density of 100 μA / cm was applied using a 1 mol / NaCl solution at 30°C and a saturated silver chloride electrode (SSE). 2 The corresponding pitting potential (V´ c100 ) was measured, and the average of the six measured data was taken as the pitting potential PBM Let us assume that.

[0046] In addition, after removing the weld scale from the weld using a burn remover, the weld was carefully dry-polished with P600 abrasive paper immediately before the measurement, and the measurement was performed in accordance with the method specified in JIS G 0577 using a 1 mol / L NaCl solution at 30°C and a saturated silver chloride electrode (SSE) at a current density of 100 μA / cm. 2 The corresponding pitting potential (V´ c100 ) was measured, and the average of the six measured data was taken as the pitting potential P WM An example of a burn remover is Lasnonwell JL-500 (manufactured by Bansho Co., Ltd.), but other chemicals or methods may be used as long as they can sufficiently remove the weld scale.

[0047] In addition, to evaluate the internal corrosion resistance of the welded metal of the welded joint, the center of the weld in the plate thickness direction was exposed as the evaluation surface, and a current density of 100 μA / cm was applied using a 1 mol / L NaCl solution at 30°C and a saturated silver chloride electrode (SSE) according to the method specified in JIS G 0577. 2 The corresponding pitting potential (V´ c100 ) was measured, and the average of the six measured data was determined as the pitting potential P mid Let us assume that.

[0048] In this embodiment, the pitting potential P BM and the pitting potential P inside the weld mid Difference from (P BM -P mid ) may be set to 200 mV or less. This can further improve the corrosion resistance of the welded portion. It is preferably set to 150 mV or less.

[0049] Pitting potential P inside the weld mid The center of the weld in the thickness direction is exposed as the evaluation surface, and a current density of 100 μA / cm is applied using a 1 mol / L NaCl solution at 30°C and a saturated silver chloride electrode (SSE) in accordance with the method specified in JIS G 0577. 2 The corresponding pitting potential (V´ c100) was measured, and the average of the six measured data was determined as the pitting potential P mid This can be done as follows.

[0050] In the welded structure and welded joint of this embodiment, it is sufficient that the austenite fraction reduction in the surface layer of the weld metal part is less than 20 area % and the pitting potential reduction of the weld part is less than 150 mV on either or both of the front side of the weld part (the side of the welding torch during welding) and the back side of the weld part (the side opposite to the welding torch during welding). In other words, it is not necessary for the austenite fraction reduction and the pitting potential reduction on both the front and back sides of the weld part to satisfy the ranges of the present invention. This is because the welded structure and welded joint of this embodiment may be satisfactory if the corrosion resistance of either the front or back side of the weld part is improved, depending on the installation environment.

[0051] Next, the welding method of this embodiment will be described. The welding method of this embodiment is a method for welding a base material made of ferritic-austenitic duplex stainless steel by gas-shielded arc welding, in which a gas containing 60 to 100 volume % N2 is used as either an aftergas or a backgas, or both. In the welding method of the present embodiment, it is preferable to use a gas containing less than 60% by volume of N2 as the torch shield gas. In the welding method of this embodiment, it is preferable to use a gas containing 60% by volume or more of N2 and the balance Ar as either one or both of the after-gas and the back-gas.

[0052] In the welding method of the present embodiment, the welding method or welding conditions and the use or non-use of a filler metal can be appropriately set and are not limited in any way. In addition, the shape of the base metal and the shape of the welded joint are not limited in any way.

[0053] As a welding method, gas-shielded arc welding is preferably used. Among gas-shielded arc welding methods, non-consumable electrode welding is preferred. A filler metal may or may not be used. Whether or not a filler metal is used may be appropriately selected depending on the shape of the base material, the thickness of the base material, the shape of the welding groove, and the type of weld joint. For example, when butt welding a duplex stainless steel plate having a relatively thin plate thickness, a non-consumable electrode welding method that does not use a filler metal is preferred.

[0054] (After gas and back gas) In the welding method of this embodiment, a gas containing 60 to 100 volume % of N2 (hereinafter referred to as nitrogen-containing gas) is used as either or both of the after-gas and back gas. The after-gas is used to control the atmosphere of the welded part in a high temperature state immediately after welding, facing the welding torch side during welding.

[0055] Back gas is used to control the atmosphere at the weld, which is in a high temperature state immediately after welding, facing the opposite side of the steel material from the welding torch during welding.

[0056] When a nitrogen-containing gas is used as an after-gas, the corrosion resistance of the welded portion that faced the welding torch side during construction is improved. When a nitrogen-containing gas is used as a back gas, the corrosion resistance of the welded portion that faced the opposite side to the welding torch side during construction is improved. Furthermore, when a nitrogen-containing gas is used as both an after-gas and a back gas, the corrosion resistance of both the welded portion that faced the welding torch side and the opposite side during construction is improved.

[0057] The range in which the atmosphere is controlled by the aftergas and / or backgas may be such that the temperature of the weld falls to, for example, 600°C or less, preferably 500°C or less. Because the cooling rate of the weld is relatively fast, control for a maximum of about 20 seconds from immediately after welding is sufficient. By controlling the atmosphere with the aftergas or backgas to this range, the welded joint and welded structure of this embodiment can be manufactured.

[0058] The nitrogen-containing gas is a gas containing 60 to 100 volume % of N2, and preferably industrial pure nitrogen gas containing 99 volume % or more of N2. When using a gas containing 60 volume % or more but less than 100 volume % of N2, the remainder is preferably a non-oxidizing gas, more preferably an inert gas, and even more preferably Ar gas, from the viewpoint of suppressing oxidation of the welded part. The nitrogen concentration in the nitrogen-containing gas is not particularly specified as long as the austenite phase ratio of the surface layer of the welded metal part is reduced by less than 20 area %, but it is necessary to contain at least 60% or more of N2. If necessary, a mixed gas containing N2 may be used from the viewpoint of other than corrosion resistance.

[0059] Other than using a nitrogen-containing gas containing 60 to 100% by volume of N2 as an after-gas and / or back gas, there are no particular limitations on the welding method according to this embodiment.

[0060] The mechanism by which the use of a nitrogen-containing gas containing 60 volume % or more of N2 as the aftergas and / or backgas can suppress the deterioration of the corrosion resistance of the surface of the weld is thought to be as follows.

[0061] FIG. 1 shows the metal structure of the surface layer of the weld metal part of the TIG welded joint in which the after gas was pure Ar or pure N2 when TIG welding was performed on the base material of the steel type B of the embodiment. Note that both FIG. 1(a) and FIG. 1(b) show the surface layer structure of the weld metal part on the side where the torch shielding gas and the after shielding gas were sprayed. FIG. 1(a) is an example where Ar gas was used as the after gas (sample number 27), and FIG. 1(b) is an example where N2 was used as the after gas (sample number 5). The weld joint using Ar gas as the after gas had an austenite phase ratio of 28.4 area %, while the weld joint using N2 as the after gas had an austenite phase ratio of 38.7 area %, and the weld joint using N2 as the after gas had a higher austenite phase ratio in the surface layer of the weld metal part. This is thought to be because the use of N2 gas as the after gas suppressed the desorption of nitrogen after the weld metal part solidified.

[0062] As mentioned above, the solubility limit of N in the ferrite phase is much smaller than that in the austenite phase, so N that cannot be dissolved in the ferrite phase precipitates as chromium nitrides in the ferrite phase or in the grain boundaries between ferrite phases in the weld metal and the weld heat-affected zone during cooling during welding. At this time, Cr is consumed, forming a so-called chromium-deficient layer, which reduces corrosion resistance. Conversely, if the surface layer of the weld metal has a high proportion of austenite phase, nitrogen is dissolved in the austenite phase, suppressing the precipitation of chromium nitrides and suppressing the reduction in corrosion resistance.

[0063] FIG. 2 shows a graph showing the distribution of nitrogen concentration in the depth direction from the surface layer of the weld metal obtained by welding the base metal made of steel type B of the embodiment. FIG. 2(a) is a graph when Ar was used as the torch shielding gas and Ar was used as the after gas (sample number 32). FIG. 2(b) is a graph when Ar+5% N2 gas was used as the torch shielding gas and Ar gas was used as the after gas (sample number 15). Both FIG. 2(a) and FIG. 2(b) show the nitrogen concentration distribution in the surface layer of the weld metal on the side where the torch shielding gas was sprayed. The nitrogen concentration in the figure was determined by EPMA measurement. The dotted line in the figure shows the nitrogen concentration of the base metal (0.17%).

[0064] As shown in Fig. 2(b), the welded joint with Ar+5%N2 gas as the torch shielding gas has a higher average nitrogen concentration at a depth of about 100 μm or more from the surface compared to the welded joint with pure Ar as the torch shielding gas as shown in Fig. 2(a). On the other hand, in the region of 0 to less than 100 μm deep, the nitrogen concentration of both welded joints decreases rapidly.

[0065] The process by which nitrogen is reduced in the weld metal must be considered in two stages: (A) the liquid phase diffusion process during melting, which is mainly in contact with the torch shielding gas, and (B) the solid phase diffusion process after solidification, which is mainly in contact with the after-gas. When Ar+5%N2 gas is used as the torch shielding gas, the nitrogen reduction in process (A) above can be suppressed, so the nitrogen concentration is about the same as that of the base metal at a depth of 100μm or more from the surface, but because the after-gas is pure Ar, the nitrogen reduction in process (B) cannot be suppressed, and it is thought that the nitrogen concentration in the surface layer decreased.

[0066] The inventors have confirmed that the nitrogen concentration in the surface layer of the weld metal is in good agreement with a simulation of nitrogen diffusion in the solid phase using the cooling temperature history after welding.

[0067] As described above, in order for the welded joint according to this embodiment to achieve the desired surface structure and corrosion resistance, it is sufficient to use a nitrogen-containing gas containing 60 volume % or more of N2 for the aftergas and / or backgas. The components of the torch shielding gas are not particularly specified, but the nitrogen content in the torch shielding gas is preferably less than 60%, more preferably 5% or less, and it is even more preferable to use pure Ar.

[0068] The reason why the nitrogen content in the torch shielding gas is preferably less than 60% is that nitrogen is an element that stabilizes the austenite phase and improves corrosion resistance, and at the same time, promotes the precipitation of chromium nitrides to form a chromium-depleted layer, thereby deteriorating corrosion resistance. That is, if the nitrogen concentration in the torch shielding gas is increased, nitrogen is introduced from the torch shielding gas side to the weld metal in the above-mentioned (A) process (liquid phase diffusion process during melting in contact with the torch shielding gas), so the nitrogen concentration in the weld metal increases. If a large amount of nitrogen is introduced into the weld metal at this time, the nitrogen concentration in the weld metal becomes a concentration higher than that at which solid solution can be obtained, and conversely, the precipitation of chromium nitrides is promoted, which may deteriorate the corrosion resistance of the surface and inside of the weld metal. In addition, in welding using a non-consumable electrode such as TIG welding, the nitrogen gas in the torch shielding gas reacts with the electrode and consumes it, so the frequency of electrode replacement increases, leading to a decrease in workability and an increase in electrode costs. Therefore, the torch shielding gas is as described above.

[0069] Next, ferritic-austenitic duplex stainless steel applicable to this embodiment has, for example, the following chemical composition in mass %: C: 0.10% or less, Si: 2.00% or less, Mn: 0.50 to 6.00%, P: 0.050% or less, S: 0.050% or less, Ni: 0.10 to 8.00%, Cr: 17.0 to 30.0%, N: 0.05 to 0.30%, Mo: 0 to 3.50%, Cu: 0 to 2.0%. , Nb: 0-0.10%, Sn: 0-1.00%, W: 0-1.00%, V: 0-1.00%, Ti: 0-0.05%, B: 0-0.0050%, Ca: 0-0.0050%, Mg: 0-0.0050%, Al: 0-0.05%, REM: 0-0.50%, the balance being Fe and impurities, and the PREN_Mn value calculated by the following formula (i) is less than 40.0. This chemical composition is merely an example, and the present invention is not limited thereto. The reason for giving this chemical composition is as follows. In the following description, "%" for the content means "mass %".

[0070] PREN_Mn value=Cr+3.3Mo+16N-Mn (i)

[0071] C: 0.10% or less C is an element that dissolves in the austenite phase to increase strength. However, if the C content exceeds 0.050%, the strength of the steel increases and workability deteriorates. In addition, it promotes the precipitation of Cr carbides, which leads to the occurrence of intergranular corrosion. Therefore, the C content is set to 0.10% or less. The C content may be 0.050% or less, or may be 0.040% or less. In addition, it is preferable to keep the C content low from the viewpoint of corrosion resistance, but reducing the C content to 0.002% or less with existing steelmaking equipment would result in a large increase in costs. Therefore, the C content is preferably 0.002% or more.

[0072] Si:2.00% or less Si may be used as a deoxidizing element or may be added to improve oxidation resistance. However, if the Si content exceeds 2.00%, the steel plate becomes hard and its toughness and workability deteriorate. Therefore, the Si content is set to 2.00% or less. The Si content is preferably set to 1.50% or less, and more preferably set to 1.00% or less. In addition, reducing the Si content to a very small amount increases the cost of refining the steel. Therefore, the Si content is preferably set to 0.03% or more.

[0073] Mn: 0.50-6.00% Mn has the effect of increasing the austenite phase and increasing the solid solubility of nitrogen to suppress bubble defects during manufacturing. However, if a large amount of Mn is contained, the corrosion resistance and hot workability are reduced. Therefore, the Mn content is set to 0.50 to 6.00%. The Mn content is preferably 1.00% or more, and more preferably 2.50% or more. Also, the Mn content is preferably 4.00% or less.

[0074] P:0.050% or less P is an element that is inevitably mixed into steel, and is also contained in raw materials such as Cr, so it is difficult to reduce, but a large amount of P reduces formability. The lower the P content, the better, and it is set to 0.050% or less. The P content is preferably 0.040% or less. A lower P content is desirable, but reducing the P content would result in a significant increase in costs, so the P content may be 0.0005% or more.

[0075] S: 0.050% or less S is an element that is inevitably mixed into steel, and it can combine with Mn to form inclusions that can become the starting point for rusting. Therefore, the S content is set to 0.050% or less. The lower the S content, the better the corrosion resistance, so it is preferable that it is 0.0030% or less. Although it is desirable to have a low S content, reducing the S content would result in a significant increase in costs, so the S content may be 0.0001% or more.

[0076] Ni: 0.10~8.00% Ni is an austenite stabilizing element and is an important element for increasing the austenite phase ratio of the surface layer. Ni also has the effect of improving corrosion resistance. However, a large amount of Ni included increases the raw material cost and may cause problems such as stress corrosion cracking. Therefore, the Ni content is set to 0.10 to 8.00%. The Ni content is preferably 1.00% or more. The Ni content is preferably 6.00% or less, more preferably 4.00% or less, and even more preferably 3.00% or less.

[0077] Cr: 17.0~30.0% Cr is an element necessary for ensuring corrosion resistance. However, a large amount of Cr causes hot work cracking and increases the amount of chromium nitride precipitated in the weld metal zone and the weld heat affected zone. Therefore, the Cr content is set to 17.0 to 30.0%. The Cr content is preferably 20.0% or more, and more preferably 21.0% or more. The Cr content is preferably 25.0% or less, more preferably 23.0% or less, and even more preferably 22.0% or less.

[0078] N: 0.05~0.30% N is an element that dissolves in the austenite phase to increase strength and corrosion resistance, thereby contributing to alloy saving. However, N is an element that greatly affects the precipitation of chromium nitrides during welding cooling. If it is contained in an amount exceeding 0.30%, the amount of chromium nitrides precipitated in the weld metal part and the weld heat affected zone increases, and the difference in corrosion resistance between the base material and the welded part increases. Therefore, the N content is set to 0.05 to 0.30%. From the viewpoint of strength and corrosion resistance, the N content may be 0.08% or more, preferably 0.10% or more, and more preferably 0.15% or more. Also, from the viewpoint of suppressing the precipitation of chromium nitrides, the N content is preferably 0.25% or less, and more preferably 0.20% or less.

[0079] Mo: 0-3.50% Mo is an element that improves corrosion resistance, so it may be included as necessary. However, if a large amount of Mo is included, it will increase the raw material cost, and the corrosion resistance will decrease due to the precipitation of σ phase in the welded part. Therefore, the Mo content is set to 3.50% or less. In order to obtain the above effect, the Mo content is preferably 0.10% or more. In addition, the Mo content is preferably 2.50% or less, more preferably 1.00% or less, and even more preferably 0.60% or less.

[0080] Cu: 0-2.0% Cu is an element that is very effective in improving sulfuric acid resistance, and may be added as necessary. To obtain the above effects, the Cu content is preferably 0.1% or more. It is more preferable that the Cu content be 0.3% or more. On the other hand, since Cu is an element that increases the activity of N and makes it easier to precipitate chromium nitride in the weld metal, it is set to 2.0% or less. The Cu content is preferably 1.5% or less, and more preferably 1.0% or less.

[0081] Nb: 0 to 0.10% Nb may be added as necessary because it has the effect of suppressing the precipitation of chromium nitrides by forming a compound with N. However, if a large amount of Nb is added, the workability of the steel sheet is reduced. Therefore, the Nb content is set to 0.10% or less. To obtain the above effect, the Nb content is preferably 0.01% or more, and more preferably 0.04% or more.

[0082] Sn: 0 to 1.00% Sn is an element that improves corrosion resistance, so it may be contained as necessary. However, if a large amount of Sn is contained, it deteriorates hot workability. Therefore, the Sn content is set to 1.00% or less. In order to obtain the above effect, the Sn content is preferably 0.010% or more.

[0083] W:0~1.00% W is an element that improves corrosion resistance, so it may be contained as necessary. However, if a large amount of W is contained, the load during rolling increases, making it easier for manufacturing defects to occur. Therefore, the W content is set to 1.00% or less. In order to obtain the above effects, the W content is preferably 0.01% or more. In addition, the W content is preferably 0.50% or less.

[0084] V: 0~1.00% V is an element that improves corrosion resistance, and may be contained as necessary. However, if a large amount of V is contained, the load during rolling increases, making it easier for manufacturing defects to occur. Therefore, the V content is set to 1.00% or less. In order to obtain the above effects, the V content is preferably 0.01% or more. Also, the V content is preferably 0.50% or less.

[0085] Ti: 0 to 0.05% Like Nb, Ti has the effect of preventing coarsening of the heat-affected zone and further forming fine equiaxed crystals in the solidified structure, so it may be contained as necessary. However, if Ti is contained in a large amount, it reduces the uniform elongation and local elongation. Therefore, the Ti content is set to 0.05% or less. In order to obtain the above effect, the Ti content is preferably 0.005% or more.

[0086] B: 0~0.0050% B has the effect of improving hot workability, so it may be contained as necessary. However, if a large amount of B is contained, the corrosion resistance is significantly deteriorated. Therefore, the B content is set to 0.0050% or less. In order to obtain the above effect, the B content is preferably 0.0003% or more. Also, the B content is preferably 0.0030% or less.

[0087] Ca: 0 to 0.0050% Ca may be added as necessary for desulfurization and deoxidization. However, if a large amount of Ca is added, hot work cracks are likely to occur and corrosion resistance is reduced. Therefore, the Ca content is set to 0.0050% or less. To obtain the above effects, the Ca content is preferably 0.0001% or more.

[0088] Magnesium: 0 to 0.0050% Mg may be added as necessary since it not only has the effect of deoxidizing but also of refining the solidified structure. However, the inclusion of a large amount of Mg increases the cost of the steelmaking process. Therefore, the Mg content is set to 0.0050% or less. To obtain the above effect, the Mg content is preferably 0.0001% or more.

[0089] Al: 0 to 0.05% Al may be added as necessary for desulfurization and deoxidization. However, if a large amount of Al is added, it will increase manufacturing defects and raw material costs. Therefore, the Al content is set to 0.05% or less. To obtain the above effects, the Al content is preferably 0.0030% or more.

[0090] REM: 0~0.50% REM (rare earth elements) have the effect of improving hot workability, so they may be contained as necessary. However, if a large amount of REM is contained, it impairs manufacturability and increases costs. Therefore, the REM content is set to 0.50% or less. To obtain the above effect, the REM content is preferably 0.005% or more. The REM content is preferably 0.020% or more, and 0.20% or less.

[0091] REM is a general term for 17 elements, including Sc, Y, and 15 elements from La to Lu (lanthanoids), and the REM content refers to the total content of these elements. Lanthanoids are added industrially in the form of misch metals.

[0092] In the chemical composition of the steel of the present invention, the balance is Fe and impurities. Here, the term "impurities" refers to components that are mixed in due to various factors in raw materials such as ores and scraps and in the manufacturing process during industrial production of steel, and are permissible within a range that does not adversely affect the present invention.

[0093] PREN_Mn value: less than 40.0 The PREN_Mn value is a general index showing the pitting corrosion resistance of a stainless steel sheet, and is calculated from the chemical composition of the stainless steel using the following formula (i).

[0094] PREN_Mn value=Cr+3.3Mo+16N-Mn (i)

[0095] In the above formula (i), the element symbols represent the content (mass%) of each element contained in the steel, and 0 is substituted when the element is not contained.

[0096] An increase in the PREN_Mn value may cause problems such as increased alloy cost due to an increase in the Cr and Mo content and reduced corrosion resistance due to the precipitation of σ phase. Furthermore, the generation of nitrogen bubbles due to an increase in the N content and a decrease in the Mn content becomes a problem. Therefore, the PREN_Mn value is set to less than 40.0. The PREN_Mn value is preferably less than 30.0. There is no need to specify a lower limit, but in order to obtain corrosion resistance equivalent to SUS304, it is preferably 18.0 or more, and more preferably 20.0 or more.

[0097] The welded structure according to this embodiment can be obtained by performing welding under the above conditions. The welded structure thus obtained has a pitting potential drop of less than 150 mV relative to the base metal, and therefore can be used as a welded structure with good corrosion resistance. EXAMPLES

[0098] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0099] Ferrite-austenitic duplex stainless steel with the chemical composition shown in Table 1 was melted and made into billets, which were then hot-rolled to a thickness of 5 mm and annealed. This hot-rolled and annealed sheet was then cold-rolled to produce cold-rolled steel sheets with thicknesses of 1 mm and 3 mm, which were then subjected to final annealing.

[0100] [Table 1]

[0101] After that, one pass of TIG fillet welding was performed on the produced cold-rolled annealed steel sheet to produce a welded joint. An after-shield box with a length of 140 mm, width of 40 mm, and height of 40 mm was installed behind the welding torch, as shown in Figure 3, and the mixture ratio of N2 and Ar in the torch shield gas, back gas, and after gas was changed in various ways. The gas flow rates were torch shield gas: 10 L / min, back gas: 15 L / min, and after gas: 30 L / min. The appropriate welding conditions changed depending on the composition of the torch shield gas. For this reason, the arc length was kept constant at 1 mm, and the welding current and welding speed were adjusted so that the back bead width was about 2 to 3 times the plate thickness. Welding was performed without using a filler metal, with the rolling direction as the welding direction, for a length of 300 mm or more.

[0102] For the steel sheets before welding, the surface 0.2 mm below the surface was wet-polished with abrasive grain size #600, and then, using the method specified in JIS G 0577, a current density of 100 μA / cm was applied using a 1 mol / NaCl solution at 30°C and a saturated silver chloride electrode (SSE). 2 The corresponding pitting potential (V´ c100 ) was measured, and the average of the six measured data was taken as the pitting potential P BM It was decided.

[0103] Furthermore, to evaluate the corrosion resistance of the surface of the welded metal part of the welded joint, the weld scale was removed using a burnt remover instead of the usual wet polishing, and then the weld was carefully dry-polished with P600 abrasive paper immediately before the measurement. The method specified in JIS G 0577 was used to measure the corrosion resistance of the surface of the welded metal part using a 1 mol / L NaCl solution at 30°C and a saturated silver chloride electrode (SSE) at a current density of 100 μA / cm. 2 The corresponding pitting potential (V´ c100 ) was measured, and the average of the six measured data was taken as the pitting potential P WM In order to limit the measurement surface of the pitting potential to the welded surface, the areas other than the welded area were masked. Note that Lasnonwell JL-500 (Bansho Co., Ltd.) was used as the burn removal material, but other chemicals or methods may be used as long as they can sufficiently remove the weld scale.

[0104] In addition, to evaluate the internal corrosion resistance of the welded metal of the welded joint, the center of the weld in the plate thickness direction was exposed as the evaluation surface, and a current density of 100 μA / cm was applied using a 1 mol / L NaCl solution at 30°C and a saturated silver chloride electrode (SSE) according to the method specified in JIS G 0577. 2 The corresponding pitting potential (V´ c100 ) was measured, and the average of the six measured data was determined as the pitting potential P mid It was decided.

[0105] The corrosion resistance test pieces for the welded joints were prepared from welded parts that were 50 mm or more away from the start or end point of the weld, had melted to the back side, and had no defects such as burn-through. The corrosion resistance test pieces were prepared from welded parts with a measurement area of ​​1 cm2, with the welded part in the center. 2 The specimens were prepared so that the weld length was 10 mm. Therefore, the measurement area of ​​the corrosion-resistant test piece included the weld metal part, the weld heat-affected zone, and the base metal part. After measuring the pitting potential, the position of pitting corrosion in the corrosion-resistant test piece was confirmed, and if pitting corrosion occurred in a part other than the weld metal part or the weld heat-affected zone, such as a gap with the resin, or if welding scale remained due to insufficient burn removal, it was excluded from the measurement data. In addition, the part of the corrosion-resistant test piece from which the measurement data was taken was defined as the weld in this invention. The weld is composed of the weld metal part and the weld heat-affected zone.

[0106] And the pitting potential P of the base material BM From this, the pitting potential P of the weld WM minus (P BM -P WM ) [(mV vs SSE)] was calculated as the decrease in pitting potential.

[0107] Additionally, to investigate the microstructural morphology of the steel plate before welding, the metal structure of a 200 μm wide region from the surface to a depth of 200 μm in a cross section perpendicular to the rolling length direction at the center of the rolling width direction (TD cross section) was examined using an optical microscope. Similarly, to investigate the microstructural morphology of the welded metal part, the metal structure of a 200 μm wide region from the surface to a depth of 30 μm in a cross section perpendicular to the welding direction at the center of the width of the welded metal part was examined using an optical microscope. The obtained microstructural images were classified into ferrite and austenite phases by image analysis, and the austenite phase fraction γ in the base metal and the surface layer of the welded metal part was calculated. BM , γ WM The austenite fraction of the base metal γ BM From this, the austenite phase ratio γ WM The value obtained by subtracting (γ BM -γ WM ) (area %) was calculated as the austenite fraction decrease.

[0108] In order to evaluate the influence of back gas, the corrosion resistance and austenite fraction of the surface layer of the weld metal part on the back side of the weld joint were also evaluated in the same manner as above.

[0109] The above production conditions and measurement results are shown in Table 2. The symbols in Table 2 have the following meanings:

[0110] Plate thickness: Base material plate thickness Evaluation surface: The front surface was evaluated for the effect of after-gas, and the back surface was evaluated for the effect of back gas. γ phase rate reduction: γ phase rate of base material γ BM (%) - γ phase ratio in the surface layer of the weld metal WM (%) Drop in pitting potential of surface: pitting potential P of base material BM (mV) - pitting potential P of the weld surface WM (mV) Internal pitting potential drop: Base material pitting potential P BM (mV) - pitting potential P inside the weld mid (mV)

[0111] The above results are also shown in Table 2.

[0112] [Table 2]

[0113] Sample numbers 1 to 30 are examples of the present invention, and by using N2 gas (100% N2) as the after gas and / or back gas, the decrease in the gamma phase rate of the surface layer of the evaluation surface was small, and the decrease in pitting potential was good at less than 150 mV. However, since sample numbers 25 to 30 used 100% N2 gas or Ar + 60% N2 gas as the torch shielding gas, the corrosion resistance inside the weld metal was slightly inferior to when 100% Ar gas or Ar + 5% N2 gas was used as the torch shielding gas.

[0114] Sample numbers 31 to 38 are comparative examples. Since 100% Ar gas was used as the after-gas and back-gas, the decrease in the γ phase rate in the surface layer of the evaluation surface was large and the decrease in pitting potential was poor, at 150 mV or more.

[0115] As explained above, in the examples of the present invention, the decrease in the gamma phase rate in the surface layer was small, and a good pitting potential was obtained at the weld. On the other hand, in the comparative examples, the decrease in the gamma phase rate in the surface layer was large, and the corrosion resistance was poor. In addition, in the present invention, the restrictions on the welding method were relaxed except for the restrictions on after-gas and back-gas, reheat treatment after welding was not required, and further, the wear of the welding electrodes was small.

[0116] Fig. 4 is a diagram showing the relationship between the reduction in the gamma phase rate of the surface layer and the reduction in the pitting potential of the welded portion. As shown in Fig. 4, it is understood that there is a relationship between the reduction in the gamma phase rate of the surface layer and the reduction in the pitting potential of the welded portion. [Industrial Applicability]

[0117] According to the present invention, it is possible to obtain a ferritic-austenitic duplex stainless steel welded structure and welded joint having excellent corrosion resistance of the welded portion in an alloy-saving duplex stainless steel material.

Claims

1. A base material made of a ferritic-austenitic duplex stainless steel material; a welded portion; Austenite phase ratio γ in the metal structure of the base material BM and the austenite fraction γ of the surface layer of the weld metal part of the weld part WM The difference between the austenite phase ratio decrease in the surface layer of the weld metal part and the BM -γ WM ) is less than 20 area %, The pitting potential P of the base material BM and the pitting potential P of the weld WM The difference between the pitting potential drop (P BM -P WM ) is less than 150 mV.

2. A base material made of a ferritic-austenitic duplex stainless steel material; a welded portion; Austenite phase ratio γ in the metal structure of the base material BM and the austenite fraction γ of the surface layer of the weld metal part of the weld part WM The difference between the austenite phase ratio decrease in the surface layer of the weld metal part and the BM -γ WM ) is less than 20 area %, The pitting potential P of the base material BM and the pitting potential P of the weld WM The difference between the pitting potential drop (P BM -P WM ) is less than 150 mV.

3. A method for welding a base material made of a ferritic-austenitic duplex stainless steel material by a gas-shielded arc welding method, comprising the steps of: No filler metal is used, A method for welding ferritic-austenitic dual phase stainless steel, in which N 2 gas is used as either or both of an after gas and a back gas.

4. The torch shield gas contains less than 60% by volume of N. 2 4. The method for welding ferritic-austenitic dual phase stainless steel material according to claim 3, wherein a gas containing

Citation Information

Patent Citations

  • Welding method for two phase stainless steel excellent in corrosion resistance

    JP1987199272A

  • Manufacture of duplex stainless steel welded tube excellent in toughness and corrosion resistance of weld zone

    JP1996155662A

  • Welding method of ferritic stainless steel

    JP2011173124A

  • Method for improving corrosion resistance of duplex stainless steel welded part

    JP2015217434A

  • Welded joint and its welding material, welding method

    JP2018529522A