Positive electrode active material for all-solid-state lithium-ion batteries, precursor for positive electrode active material for all-solid-state lithium-ion batteries, positive electrode for all-solid-state lithium-ion batteries, all-solid-state lithium-ion battery, method for producing precursor for positive electrode active material for all-solid-state lithium-ion batteries, and method for producing positive electrode active material for all-solid-state lithium-ion batteries

The use of a specifically formulated positive electrode active material with a Li and Nb oxide coating addresses the interfacial issues in all-solid-state lithium ion batteries, enhancing charge/discharge capacity and conductivity through controlled production methods.

JP7584337B2Active Publication Date: 2024-11-15JX NIPPON MINING & METALS CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021047833
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-22
Publication Date
2024-11-15
Estimated Expiration
2041-03-22

AI Technical Summary

Technical Problem

All-solid-state lithium ion batteries face issues with poor interfacial contact between the solid electrolyte and the positive electrode active material, leading to decreased battery performance and charge/discharge capacity due to uneven shapes and non-uniform coating with LiNbO3, which increases thickness and reduces capacity.

Method used

A positive electrode active material with a specific composition formula Li a Ni x Co y Mn 1-x-y O 2, coated with a layer of Li and Nb oxide, is produced using a controlled crystallization reaction and firing process to ensure uniformity and high circularity, enhancing the contact area with the solid electrolyte.

Benefits of technology

The solution results in improved charge and discharge capacity, reduced interfacial resistance, and increased conductivity of Li ions, leading to better battery performance and capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584337000003
    Figure 0007584337000003
  • Figure 0007584337000001
    Figure 0007584337000001
  • Figure 0007584337000002
    Figure 0007584337000002
Patent Text Reader

Abstract

To provide a cathode active material for an all-solid lithium ion battery, having good charge / discharge capacity; a precursor thereof, a production method of the precursor, and a production method of the cathode active material for an all-solid lithium ion battery, and to provide a cathode for an all-solid lithium ion battery, and an all-solid lithium ion battery, each arranged by use of the cathode active material for an all-solid lithium ion battery.SOLUTION: A cathode active material for an all-solid lithium ion battery has a composition represented by the following formula: LiaNixCoyMn1-x-yO2 (where 1.00≤a≤1.03, 0.8≤x≤0.9 and 0≤y≤0.16). The cathode active material has a 50%-cumulative volume particle size D50 of 3.0-7.0 μm, a tap density of 1.9-2.5 g / cc, and a roundness of 0.90-0.93.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material for an all-solid-state lithium ion battery, a precursor for a positive electrode active material for an all-solid-state lithium ion battery, a positive electrode for an all-solid-state lithium ion battery, an all-solid-state lithium ion battery, a method for producing a precursor for a positive electrode active material for an all-solid-state lithium ion battery, and a method for producing a positive electrode active material for an all-solid-state lithium ion battery. [Background technology]

[0002] In recent years, with the rapid spread of information-related devices and communication devices such as personal computers, video cameras, and mobile phones, the development of batteries to be used as power sources for these devices has become important. Among these batteries, lithium ion batteries have attracted attention from the viewpoint of their high energy density. In addition, there is a demand for improvements in the energy density and battery characteristics of lithium secondary batteries for large-scale applications such as vehicle-mounted power sources and load leveling.

[0003] However, in the case of lithium-ion batteries, the electrolyte is mostly organic compounds, and even if a flame-retardant compound is used, it cannot be said that there is no risk of fire. As an alternative to these liquid-based lithium-ion batteries, all-solid-state lithium-ion batteries, which use a solid electrolyte, have been attracting attention in recent years. Among them, all-solid-state lithium-ion batteries that use sulfides such as Li2S-P2S5 as the solid electrolyte or that add lithium halides to them are becoming mainstream.

[0004] For example, Patent Document 1 discloses a lithium metal composite oxide powder as a positive electrode active material used in an all-solid-state lithium ion battery, the lithium metal composite oxide powder being composed of secondary particles formed by aggregation of primary particles and single particles existing independently of the secondary particles, the lithium metal composite oxide powder being represented by the following composition formula (1) and satisfying the following requirements (A), (B), and (C): Li x (Ni (1-y-z-w) Co y Mn z M w )1-x O2(1) (However, M is one or more elements selected from the group consisting of Fe, Cu, Ti, Mg, Al, W, B, Mo, Nb, Zn, Sn, Zr, Ga, and V, and -0.1 ≦ x ≦ 0.2, 0 < y ≦ 0.4, 0 ≦ z ≦ 0.4, 0 ≦ w ≦ 0.1 are satisfied.) (A) The BET specific surface area of the lithium metal composite oxide powder is less than 2 m 2 / g. (B) The lithium metal composite oxide powder has two or more peaks in the circularity distribution based on the number of circularities obtained by the following formula (2). Circularity = 4πS / L 2 (2) (S is the projected area of the projected image of the particle, and L is the perimeter of the particle.) (C) The average particle diameter D of the lithium metal composite oxide powder 50 is 2 μm or more and 20 μm or less.

[0005] Patent Document 2 discloses a non-aqueous electrolyte secondary battery positive electrode active material including a lithium transition metal composite oxide having a spinel structure and containing nickel and manganese, wherein the lithium transition metal composite oxide has a surface region in which niobium is solid-solved, and the molar ratio of the amount of niobium to the total amount of nickel and manganese in the surface region decreases according to the distance in the depth direction from the surface in the region up to a depth of 0.3 nm from the surface.

[0006] Patent Document 3 discloses a positive electrode material for a non-aqueous electrolyte secondary battery, characterized by including a mixture of a lithium metal composite oxide powder represented by the general formula Li z Ni 1-x-y Co x M y O2 (where 0.01 ≦ x ≦ 0.35, 0 ≦ y ≦ 0.35, 0.97 ≦ z ≦ 1.20, M is an additive element, and at least one element selected from Mn, V, Mg, Mo, Nb, Ti, and Al) and a lithium lanthanum niobate powder, which consists of primary particles and secondary particles formed by aggregation of the primary particles.

Prior Art Documents

[0007] [Patent Document 1] JP 2020-083750 A [Patent Document 2] JP 2019-067506 A [Patent Document 3] JP 2018-077937 A Summary of the Invention [Problem to be solved by the invention]

[0008] All-solid-state batteries are safer because they do not use non-aqueous electrolytes that can cause fires, leaks, or explosions. However, they can sometimes cause poor contact between the solid electrolyte and the positive electrode active material in the positive electrode layer, resulting in reduced battery performance.

[0009] In addition, in solid-state batteries, the surface of the positive electrode active material is uniformly coated with LiNbO3 to reduce the interfacial resistance between the positive electrode active material and the solid electrolyte and ensure the movement of Li ions. However, since LiNbO3 does not contribute to charge / discharge capacity, if the positive electrode active material has an uneven shape, a large amount of LiNbO3 is required to coat it uniformly, which increases the thickness of LiNbO3, lowering the ratio of the positive electrode active material and resulting in a decrease in charge / discharge capacity. [Means for solving the problem]

[0010] The present invention has been made to solve the above-mentioned problems, and aims to provide a positive electrode active material for an all-solid-state lithium-ion battery having a good charge / discharge capacity, a precursor for the positive electrode active material for an all-solid-state lithium-ion battery, a method for producing the precursor for the positive electrode active material for an all-solid-state lithium-ion battery, and a method for producing the positive electrode active material for an all-solid-state lithium-ion battery. Another aim of the present invention is to provide a positive electrode for an all-solid-state lithium-ion battery and an all-solid-state lithium-ion battery using the positive electrode active material for an all-solid-state lithium-ion battery.

[0011] The present invention, which has been completed based on the above findings, is defined as follows (1) to (8). (1) Composition formula: Li a Ni x Co y Mn 1-x-y O2 (In the above formula, 1.00≦a≦1.03, 0.8≦x≦0.9, and 0≦y≦0.16.) a 50% cumulative volume particle size D50 of 3.0 to 7.0 μm, a tap density of 1.9 to 2.5 g / cc, and a circularity of 0.90 to 0.93. (2) The positive electrode active material for an all-solid-state lithium ion battery according to (1), further comprising a coating layer made of an oxide of Li and Nb on a surface of the positive electrode active material. (3) The positive electrode active material for an all-solid-state lithium-ion battery according to (1) or (2), wherein the ratio (B) / (A) of the 50% cumulative volume particle size D50×π(A) to the average particle circumference (B) of the positive electrode active material is 0.91 to 0.98. (4) Composition formula: Ni x Co y Mn 1-x-y (OH)2 (In the above formula, 0.8≦x≦0.9, 0≦y≦0.16.) A precursor for a positive electrode active material for an all-solid-state lithium ion battery, having a 50% cumulative volume particle size D50 of 2.0 to 7.0 μm, a tap density of 1.6 to 2.0 g / cc, and a circularity of 0.87 to 0.97. (5) The precursor for a positive electrode active material for an all-solid-state lithium ion battery according to (4), wherein the ratio (B) / (A) of the 50% cumulative volume particle size D50×π(A) to the average particle circumference (B) of the precursor is 0.86 to 1.06. (6) A positive electrode for an all-solid-state lithium-ion battery, comprising the positive electrode active material for an all-solid-state lithium-ion battery according to any one of (1) to (3). (7) An all-solid-state lithium ion battery comprising: a positive electrode layer formed of the all-solid-state lithium ion battery positive electrode according to (6); a negative electrode layer; and a solid electrolyte layer. (8) A method for producing a precursor of a positive electrode active material for an all-solid-state lithium ion battery according to (4) or (5), comprising the steps of: using an aqueous solution containing (a) a nickel salt, (b) a cobalt salt, (c) a manganese salt, and (d) a basic aqueous solution of ammonia water and an alkali metal as a reaction solution; and carrying out a crystallization reaction while controlling the pH of the reaction solution to 10.8 to 11.4, the ammonium ion concentration to 10 to 22 g / L, and the solution temperature to 55 to 65° C. (9) The precursor produced by the method for producing a precursor of a positive electrode active material for an all-solid-state lithium ion battery according to (8) and a lithium source are mixed together to obtain a cathode active material having a total atomic number of metals consisting of Ni, Co and Mn (Me n ) and the number of lithium atoms (Li n ) and the ratio (Li n / Me n ) is 1.01 to 1.03 to form a lithium mixture; calcining the lithium mixture in an oxygen atmosphere at 450 to 520° C. for 2 to 15 hours, and then calcining the lithium mixture at 680 to 850° C. for 2 to 15 hours; The method for producing a positive electrode active material for an all-solid-state lithium ion battery includes the steps of: Effect of the Invention

[0012] According to the present invention, it is possible to provide a positive electrode active material for an all-solid-state lithium-ion battery having a good charge / discharge capacity, a precursor for the positive electrode active material for an all-solid-state lithium-ion battery, a method for producing the precursor for the positive electrode active material for an all-solid-state lithium-ion battery, and a method for producing the positive electrode active material for an all-solid-state lithium-ion battery. Furthermore, the present invention can provide a positive electrode for an all-solid-state lithium-ion battery and an all-solid-state lithium-ion battery using the positive electrode active material for an all-solid-state lithium-ion battery. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic diagram of an all-solid-state lithium-ion battery according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Next, the embodiments of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiments, and that appropriate changes and improvements in the design may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.

[0015] (Positive electrode active material for all-solid-state lithium-ion batteries) The positive electrode active material for an all-solid-state lithium-ion battery according to an embodiment of the present invention has the composition formula: Li a Ni x Co y Mn 1-x-y O2 (wherein 1.00≦a≦1.03, 0.8≦x≦0.9, and 0≦y≦0.16). In the composition formula of the positive electrode active material, a, which indicates the lithium composition, is controlled to 1.00≦a≦1.03. Since a, which indicates the lithium composition, is 1.00 or more, it is possible to suppress the reduction of nickel due to lithium deficiency. In addition, since a, which indicates the lithium composition, is 1.03 or less, it is possible to suppress residual alkaline components such as lithium carbonate and lithium hydroxide present on the surface of the positive electrode active material particles, which may become resistance components when used in a battery.

[0016] In the positive electrode active material for an all-solid-state lithium-ion battery according to the embodiment of the present invention, x, which indicates the nickel composition in the composition formula, is controlled to 0.8≦x≦0.9, which is a so-called high nickel composition. Since x, which indicates the nickel composition, is 0.8 or more, a good battery capacity of the all-solid-state lithium-ion battery can be obtained.

[0017] The positive electrode active material for an all-solid-state lithium-ion battery according to an embodiment of the present invention has a composition formula in which y represents a cobalt composition and y represents a manganese composition. 1-x-ySince the sum of the cobalt composition and manganese composition is 1-x and 0.8≦x≦0.9, the sum of the cobalt composition and manganese composition is controlled to 0.1 to 0.2, which improves cycle characteristics and reduces the expansion and contraction behavior of the crystal lattice due to the insertion and desorption of lithium during charging and discharging. If the sum of the cobalt composition and manganese composition is less than 0.1, it becomes difficult to obtain the above-mentioned effects of cycle characteristics and expansion and contraction behavior, and if the sum of the cobalt composition and manganese composition exceeds 0.2, the amounts of cobalt and manganese added are too large, which may result in a large decrease in initial discharge capacity or may be disadvantageous in terms of cost.

[0018] The positive electrode active material for all-solid-state lithium-ion batteries according to the embodiment of the present invention may have a form of secondary particles in which a plurality of primary particles are aggregated, and may partially include primary particles that are not aggregated as secondary particles. The shapes of the primary particles constituting the secondary particles and the primary particles existing alone are not particularly limited, and may be various shapes such as, for example, substantially spherical, substantially elliptical, substantially plate-like, and substantially needle-like. The form in which the plurality of primary particles are aggregated is also not particularly limited, and may be various forms such as, for example, a form in which the particles are aggregated in a random direction, or a form in which the particles are aggregated almost evenly radially from the center to form substantially spherical or substantially elliptical secondary particles.

[0019] In the case where the positive electrode active material for an all-solid-state lithium-ion battery according to the embodiment of the present invention contains lithium hydroxide, which is excess lithium generated in a manufacturing process, etc., the content of the lithium hydroxide is preferably 1.5 mass% or less, and more preferably 1.0 mass% or less. If the lithium hydroxide content in the positive electrode active material exceeds 1.5 mass%, the lithium hydroxide is oxidized and decomposed, and gas is likely to be generated when the positive electrode active material is charged in a high-temperature environment.

[0020] In the case where the positive electrode active material for an all-solid-state lithium-ion battery according to the embodiment of the present invention contains lithium carbonate, which is excess lithium generated in a manufacturing process, etc., the content of the lithium carbonate is preferably 1.5 mass% or less, and more preferably 1.0 mass% or less. If the lithium carbonate content in the positive electrode active material exceeds 1.5 mass%, the lithium carbonate is oxidized and decomposed, and gas is easily generated when the positive electrode active material is charged in a high-temperature environment.

[0021] The contents of lithium hydroxide and lithium carbonate contained in the positive electrode active material for all-solid-state lithium-ion batteries according to the embodiment of the present invention can be determined by neutralization titration. Lithium hydroxide and lithium carbonate as excess lithium present on the surface of lithium metal composite oxide particles are dissolved in water, and hydroxide ions and carbonate ions are ionized from the lithium ions, respectively. These ionized anions can be titrated with an inorganic acid, etc., which makes it possible to separately quantify lithium hydroxide and lithium carbonate.

[0022] The moisture content of the positive electrode active material for all-solid-state lithium ion batteries according to the embodiment of the present invention is preferably 0.10% by mass or less, more preferably 0.05% by mass or less. If the moisture content of the positive electrode active material exceeds 0.10% by mass, the metal elements constituting the positive electrode may be damaged, and various battery characteristics may be deteriorated. The moisture content of the positive electrode active material may be measured by dry weight method, Karl Fischer titration method, distillation method, or the like.

[0023] The positive electrode active material for all-solid-state lithium-ion batteries according to the embodiment of the present invention has a 50% cumulative volume particle size D50 of 3.0 to 7.0 μm. Here, the 50% cumulative volume particle size D50 is the volume particle size at 50% accumulation in a volume-based cumulative particle size distribution curve. When the 50% cumulative volume particle size D50 of the positive electrode active material for all-solid-state lithium-ion batteries is 3.0 μm or more, the specific surface area is suppressed and the amount of Li and Nb oxide coating can be suppressed. When the 50% cumulative volume particle size D50 of the positive electrode active material for all-solid-state lithium-ion batteries is 7.0 μm or less, the specific surface area can be suppressed from being excessively small. The 50% cumulative volume particle size D50 of the positive electrode active material for all-solid-state lithium-ion batteries is more preferably 3.0 to 6.0 μm, and even more preferably 4.0 to 5.0 μm. The 50% cumulative volume particle size D50 can be measured using a laser diffraction particle size distribution measuring device "MT3300EXII" manufactured by Microtrac.

[0024] The positive electrode active material for all-solid-state lithium-ion batteries according to the embodiment of the present invention has a tap density of 1.9 to 2.5 g / cc. When the tap density of the positive electrode active material is 1.9 g / cc or more, a battery with a high energy density per volume can be formed. The tap density of the positive electrode active material is preferably 2.1 to 2.5 g / cc, more preferably 2.3 to 2.5 g / cc. The tap density of the positive electrode active material is measured, for example, by putting 5 g of the positive electrode active material (powder) into a 10 cc graduated cylinder, placing it in a powder density measuring instrument "KYT-4000K" manufactured by Seishin Enterprise Co., Ltd., tapping with a stroke length of 55 mm 1500 times, and then reading the graduations on the graduated cylinder. Next, "sample amount (5 g) / graduated cylinder graduation reading (cc)" is calculated, and this is taken as the tap density (g / cc).

[0025] The circularity of the positive electrode active material for all-solid-state lithium ion batteries according to the embodiment of the present invention is 0.90 to 0.93. The circularity is an index showing how close the shape of a particle is to a sphere, and for example, the circularity of a truly spherical particle is 1.00, which is the upper limit. When the circularity of the positive electrode active material is 0.90 or more, the contact area between the solid electrolyte and the positive electrode active material becomes large, and the conductivity of Li ions between the positive electrode active material and the solid electrolyte becomes good. Therefore, it is possible to manufacture a high-capacity all-solid-state lithium ion battery. The circularity is preferably 0.91 to 0.93, and more preferably 0.92 to 0.93. The circularity of the positive electrode active material can be measured, for example, by a particle image analyzer "Morphologi G3" manufactured by Malvern. Specifically, the particle image analyzer performs filtering using a parameter "solidity=0.93" from an optical image of 20,000 or more particles obtained, and measures the circularity. In this particle image analyzer, first, a sample (positive electrode active material) is placed in a sample cartridge and then set in a dispersion unit. A nitrogen gas introduction line is connected to the dispersion unit, and the sample is dispersed on a glass plate by spraying nitrogen gas. Particle images of the dispersed sample on the glass plate are continuously photographed and analyzed. Then, the circularity is calculated from the projected area and perimeter of each photographed particle (18,000 or more) using the following formula. The average circularity refers to the average circularity of all the measured positive electrode active material particles.

[0026] Circularity = 4πS / L 2 ···(formula) (In the above formula, S is the projected area of ​​the particle, L is the perimeter of the projected image of the particle, and π is the circular constant.)

[0027] The positive electrode active material for all-solid-state lithium-ion batteries according to the embodiment of the present invention may further have a coating layer of an oxide of Li and Nb on the surface of the positive electrode active material. By coating the surface of the positive electrode active material with a coating layer of such a configuration, the reaction occurring at the interface between the positive electrode active material and the solid electrolyte is suppressed. Therefore, deterioration of the positive electrode active material can be suppressed. Examples of the oxide of Li and Nb constituting the coating layer include LiNbO3. The positive electrode active material according to the embodiment of the present invention has a high circularity, and the thickness of LiNbO3 or the like coated on the surface of the positive electrode active material can be reduced, thereby increasing the proportion of Li composite oxide in the positive electrode active material, and a high-capacity positive electrode active material can be obtained.

[0028] In the positive electrode active material for an all-solid-state lithium ion battery according to the embodiment of the present invention, the ratio (B) / (A) of the 50% cumulative volumetric particle size D50×π(A) to the average particle perimeter (B) is preferably 0.91 to 0.98. The 50% cumulative volumetric particle size D50×π(A) indicates the circumference of a nearly perfect circle calculated from D50. Meanwhile, the average particle perimeter (B) indicates the average value obtained by actually measuring the perimeter of the positive electrode active material. Therefore, when the ratio (B) / (A) is 0.91 to 0.98, the contact area between the positive electrode active material and the solid electrolyte is increased, and the Li ion conductivity between the positive electrode active material and the solid electrolyte is improved. The ratio (B) / (A) is more preferably 0.93 to 0.98. The average particle perimeter (B) of the positive electrode active material can be measured by, for example, performing image analysis of the particles of the positive electrode active material using a particle image analyzer "Morphologi G3" manufactured by Malvern. The ratio (B) / (A) is obtained by calculating the ratio (B) / (A) of the 50% cumulative volumetric particle size D50 (A) of the positive electrode active material obtained by the above-mentioned measurement to the average particle perimeter (B) of the positive electrode active material.

[0029] (Precursor of positive electrode active material for all-solid-state lithium-ion batteries) The precursor of the positive electrode active material for an all-solid-state lithium-ion battery according to the embodiment of the present invention has the composition formula: Ni x Co y Mn 1-x-y(OH)2 (wherein 0.8≦x≦0.9, 0≦y≦0.16). The precursor of the positive electrode active material for an all-solid-state lithium ion battery according to the embodiment of the present invention has a 50% cumulative volume particle size D50 of 2.0 to 7.0 μm, a tap density of 1.6 to 2.0 g / cc, and a circularity of 0.87 to 0.97. By producing a positive electrode active material using a precursor according to such a configuration, it is possible to obtain the positive electrode active material according to the embodiment of the present invention, which has a small particle size and a high tap density as described above.

[0030] The precursor of the positive electrode active material for all-solid-state lithium ion batteries according to the embodiment of the present invention preferably has a ratio (B) / (A) of 0.86 to 1.06 between the 50% cumulative volumetric particle size D50×π(A) and the average particle perimeter (B). The 50% cumulative volumetric particle size D50×π(A) indicates the circumference of a nearly perfect circle calculated from D50. Meanwhile, the average particle perimeter (B) indicates the average value obtained by actually measuring the perimeter of the precursor. Therefore, when the ratio (B) / (A) is 0.86 to 1.06, the contact area between the positive electrode active material and the solid electrolyte after firing is large, and the Li ion conductivity between the positive electrode active material and the solid electrolyte is good. The ratio (B) / (A) is more preferably 0.90 to 1.05, and even more preferably 0.95 to 1.03. The average particle perimeter (B) of the precursor can be measured, for example, by image analysis of the precursor particles using a particle image analyzer "Morphologi G3" manufactured by Malvern. The ratio (B) / (A) is obtained by calculating the ratio (B) / (A) of the 50% cumulative volumetric particle size D50 (A) of the precursor obtained by the above-mentioned measurement to the average particle perimeter (B) of the precursor.

[0031] (Method for producing precursor of positive electrode active material for all-solid-state lithium-ion battery) Next, a method for producing a precursor of a positive electrode active material for an all-solid-state lithium-ion battery according to an embodiment of the present invention will be described in detail. In the method for producing a precursor of a positive electrode active material for an all-solid-state lithium-ion battery according to an embodiment of the present invention, first, an aqueous solution containing (a) a nickel salt, (b) a cobalt salt, (c) a manganese salt, and (d) a basic aqueous solution of ammonia water and an alkali metal is prepared. (a) The nickel salt includes nickel sulfate, nickel nitrate, nickel hydrochloride, etc. (b) The cobalt salt includes cobalt sulfate, cobalt nitrate, cobalt hydrochloride, etc. (c) The manganese salt includes manganese sulfate, manganese nitrate, manganese hydrochloride, etc. (d) The basic aqueous solution containing ammonia includes an aqueous ammonia solution, ammonium sulfate, ammonium carbonate, ammonium hydrochloride, etc. The basic aqueous solution of an alkali metal may be an aqueous solution of sodium hydroxide, potassium hydroxide, carbonate, etc. In addition, the aqueous solution of the carbonate includes, for example, an aqueous solution using a salt of a carbonate group such as an aqueous sodium carbonate solution, an aqueous potassium carbonate solution, an aqueous sodium hydrogen carbonate solution, and an aqueous potassium hydrogen carbonate solution.

[0032] The composition of the aqueous solution can be appropriately adjusted depending on the composition of the precursor to be produced, but is preferably (a) an aqueous solution containing 45 to 110 g / L of nickel ions, (b) an aqueous solution containing 4 to 20 g / L of cobalt ions, (c) an aqueous solution containing 1 to 4 g / L of manganese ions, or (d) 10 to 28 mass% ammonia water and a basic aqueous solution with an alkali metal concentration of 10 to 30 mass%.

[0033] Next, the aqueous solution containing the above-mentioned (a) nickel salt, (b) cobalt salt, (c) manganese salt, and (d) ammonia water and a basic aqueous solution of an alkali metal is used as a reaction solution, and a crystallization reaction is performed while controlling the pH of the reaction solution to 10.8 to 11.4, the ammonium ion concentration to 10 to 22 g / L, and the liquid temperature to 55 to 65° C. In this case, the chemical solutions may be sent to the reaction tank from three tanks, namely, a tank containing a mixed aqueous solution of nickel salt, cobalt salt, and manganese salt, a tank containing ammonia water, and a tank containing a basic aqueous solution with an alkali metal. Fine particles precipitated by the coprecipitation reaction of a precursor hydroxide having a small average particle size aggregate to generate coarse particles, but by performing the crystallization reaction while controlling the pH of the reaction solution during the coprecipitation reaction to 10.8 to 11.4, the ammonium ion concentration to 10 to 22 g / L, and the liquid temperature to 55 to 65° C., the above-mentioned fine particles having a small particle size, a high tap density, and a high circularity according to the embodiment of the present invention having the composition formula: Ni x Co y Mn 1-x-y A precursor of a positive electrode active material represented by (OH)2 (wherein 0.8≦x≦0.9, 0≦y≦0.16) can be produced.

[0034] (Method of manufacturing positive electrode active material for all-solid-state lithium-ion batteries) Next, a method for producing a positive electrode active material for an all-solid-state lithium-ion battery according to an embodiment of the present invention will be described in detail. In the method for producing a positive electrode active material for an all-solid-state lithium-ion battery according to an embodiment of the present invention, first, a lithium source is added to a precursor of a positive electrode active material for an all-solid-state lithium-ion battery, and the total number of atoms of metals consisting of Ni, Co, and Mn (Me n ) and the number of lithium atoms (Li n ) and the ratio (Li n / Me n ) is 1.01 to 1.03 to form a lithium mixture. Examples of the lithium source include lithium carbonate and lithium hydroxide. As a mixing method, it is preferable to adjust the mixing ratio of each raw material and dry mix it with a Henschel mixer, an automatic mortar, a V-type mixer, or the like.

[0035] Next, the lithium mixture is calcined in an oxygen atmosphere at 450 to 520° C. for 2 to 15 hours, and then further calcined at 680 to 850° C. for 2 to 15 hours. Thereafter, if necessary, the calcined body can be crushed using, for example, a pulverizer to obtain a powder of the positive electrode active material.

[0036] In addition, when a coating layer is provided on the surface of the positive electrode active material, the coating treatment shown in the following method can be performed. First, the surface of the powder of the positive electrode active material is coated with a coating liquid. In this case, for example, when the coating layer is made of lithium niobate, the coating liquid may be a solution containing LiOC2H5 and Nb(OC2H5)5. In addition, the coating method may use a known coating device such as a tumbling fluidized bed coating device. In this way, the surface of the positive electrode active material can be coated with lithium niobate or the like.

[0037] (Positive electrodes for all-solid-state lithium-ion batteries and all-solid-state lithium-ion batteries) A positive electrode is formed by the positive electrode active material for an all-solid-state lithium ion battery according to the embodiment of the present invention, and the positive electrode is used as a positive electrode layer, and an all-solid-state lithium ion battery including the positive electrode layer, a solid electrolyte layer, and a negative electrode layer can be produced. The solid electrolyte layer and the negative electrode layer constituting the all-solid-state lithium ion battery according to the embodiment of the present invention are not particularly limited and can be formed of known materials and can have a known configuration as shown in FIG.

[0038] The positive electrode layer of the lithium ion battery can be a layer of a positive electrode mixture obtained by mixing the positive electrode active material for all-solid-state lithium ion batteries according to the embodiment of the present invention with a solid electrolyte. The content of the positive electrode active material in the positive electrode layer is, for example, preferably 50% by mass or more and 99% by mass or less, and more preferably 60% by mass or more and 90% by mass or less.

[0039] The positive electrode mixture may further include a conductive assistant. As the conductive assistant, a carbon material, a metal material, or a mixture thereof may be used. The conductive assistant may include at least one element selected from the group consisting of, for example, carbon, nickel, copper, aluminum, indium, silver, cobalt, magnesium, lithium, chromium, gold, ruthenium, platinum, beryllium, iridium, molybdenum, niobium, osmium, rhodium, tungsten, and zinc. The conductive assistant is preferably a highly conductive carbon element, a metal element, a mixture, or a compound containing carbon, nickel, copper, silver, cobalt, magnesium, lithium, ruthenium, gold, platinum, niobium, osmium, or rhodium. As the carbon material, for example, carbon black such as Ketjen Black, acetylene black, denka black, thermal black, and channel black, graphite, carbon fiber, activated carbon, and the like may be used.

[0040] The average thickness of the positive electrode layer of the lithium ion battery is not particularly limited and can be appropriately designed depending on the purpose. The average thickness of the positive electrode layer of the lithium ion battery may be, for example, 1 μm to 100 μm, or 1 μm to 10 μm.

[0041] The method for forming the positive electrode layer of the lithium ion battery is not particularly limited and can be appropriately selected depending on the purpose. For example, the method for forming the positive electrode layer of the lithium ion battery includes a method of compression molding positive electrode active material particles.

[0042] The negative electrode layer of the lithium ion battery may be a layer of a known negative electrode active material for all-solid-state lithium ion batteries. The negative electrode layer may be a layer of a negative electrode mixture obtained by mixing a known negative electrode active material for lithium ion batteries with a solid electrolyte. The content of the negative electrode active material in the negative electrode layer is, for example, preferably 10% by mass or more and 99% by mass or less, and more preferably 20% by mass or more and 90% by mass or less.

[0043] The negative electrode layer may contain a conductive assistant, as in the positive electrode layer. The conductive assistant may be the same material as that described in the positive electrode layer. As the negative electrode active material, for example, a carbon material, specifically, artificial graphite, graphite carbon fiber, resin-calcined carbon, pyrolytic vapor-grown carbon, coke, mesocarbon microbeads (MCMB), furfuryl alcohol resin-calcined carbon, polyacene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, non-graphitizable carbon, or a mixture thereof may be used. As the negative electrode material, for example, a metal itself, such as metallic lithium, metallic indium, metallic aluminum, or metallic silicon, or an alloy in combination with other elements or compounds may be used.

[0044] The average thickness of the negative electrode layer of the lithium ion battery is not particularly limited and can be appropriately selected depending on the purpose. The average thickness of the negative electrode layer of the lithium ion battery may be, for example, 1 μm to 100 μm, or 1 μm to 10 μm.

[0045] The method for forming the negative electrode layer of the lithium ion battery is not particularly limited and can be appropriately selected depending on the purpose. Examples of the method for forming the negative electrode layer of the lithium ion battery include a method of compressing and molding negative electrode active material particles and a method of depositing a negative electrode active material.

[0046] The solid electrolyte may be a known solid electrolyte for all-solid-state lithium ion batteries, such as an oxide-based solid electrolyte or a sulfide-based solid electrolyte.

[0047] Examples of oxide-based solid electrolytes include LiTi2(PO4)3, Li2O-B2O3-P2O5, Li2O-SiO2, Li2O-B2O3, and Li2O-B2O3-ZnO.

[0048] Examples of sulfide-based solid electrolytes include LiI-Li2S-P2S5, LiI-Li2S-B2S3, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiPO4-Li2S-SiS, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li3PS4, and Li2S-P2S5.

[0049] Examples of solid electrolytes using a lithium-containing compound containing lithium and at least one element selected from niobium, tantalum, silicon, phosphorus, and boron include LiNbO3, Li 1.3 Al 0.3 Ti 0.7 (PO4)3, Li 1+x+y A x Ti 2-x S y P 3-y O 12 (A=Al or Ga, 0≦x≦0.4, 0 <y≦0.6)、[(B 1 / 2 Li 1 / 2 ) 1-z C z ]TiO3(B=La, Pr, Nd, Sm, C=Sr or Ba, 0≦x≦0.5), Li5La3Ta2O 12 , Li7La3Zr2O 12 , Li6BaLa2Ta2O 12 , LiPO (4-3 / 2w) N w (w<1), and Li 3.6 S 0.6 P 0.4 O4, etc., and LiI, LiI-Al2O3, LiN3, Li3N-LiI-LiOH, etc.

[0050] The average thickness of the solid electrolyte layer of the lithium ion battery is not particularly limited and can be appropriately designed according to the purpose. The average thickness of the solid electrolyte layer of the lithium ion battery may be, for example, 50 μm to 500 μm, or 50 μm to 100 μm.

[0051] The method for forming the solid electrolyte layer of the lithium ion battery is not particularly limited and can be appropriately selected depending on the purpose. For example, the method for forming the solid electrolyte layer of the lithium ion battery includes sputtering using a target material of the solid electrolyte, or compression molding of the solid electrolyte.

[0052] Other members constituting the lithium ion battery are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include a positive electrode collector, a negative electrode collector, and a battery case.

[0053] The size and structure of the positive electrode current collector are not particularly limited and can be appropriately selected depending on the purpose. Examples of the material for the positive electrode current collector include die steel, stainless steel, aluminum, aluminum alloys, titanium alloys, copper, gold, and nickel. The positive electrode current collector may have, for example, a foil shape, a plate shape, a mesh shape, etc. The average thickness of the positive electrode current collector may be, for example, 10 μm to 500 μm, or 50 μm to 100 μm.

[0054] The size and structure of the negative electrode current collector are not particularly limited and can be appropriately selected depending on the purpose. Examples of the material for the negative electrode current collector include die steel, gold, indium, nickel, copper, and stainless steel. The negative electrode current collector may be in the form of, for example, a foil, a plate, or a mesh. The average thickness of the negative electrode current collector may be, for example, 10 μm to 500 μm, or 50 μm to 100 μm.

[0055] The battery case is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include known laminate films that can be used in conventional all-solid-state batteries, etc. Examples of the laminate film include a resin laminate film and a film in which a metal is vapor-deposited on a resin laminate film. The shape of the battery is not particularly limited and can be appropriately selected depending on the purpose. Examples of the shape of the battery include cylindrical, square, button, coin, and flat types. EXAMPLES

[0056] The following examples are provided to provide a better understanding of the present invention and its advantages, but the present invention is not limited to these examples.

[0057] Example 1 First, nickel sulfate, cobalt sulfate, and manganese sulfate were weighed in predetermined amounts so that the ratio of Ni:Co:Mn was 90:7:3, and a 1.5 mol / L mixed metal salt solution was prepared. Next, the mixed metal salt solution, ammonia water, and 20% by mass aqueous sodium hydroxide solution were fed into a reaction vessel equipped with an agitator so that the pH in the reaction vessel was 10.8 and the ammonium ion concentration was 18.3 g / L. This caused a nickel-cobalt-manganese composite hydroxide compound to precipitate. At this time, the temperature in the reaction vessel was kept at 60°C by a water jacket. In addition, nitrogen gas was introduced into the reaction tank to prevent oxidation of the coprecipitate produced by the reaction. The gas introduced into the reaction tank is not limited to nitrogen gas, and any gas that does not promote oxidation, such as helium, neon, argon, or carbon dioxide, can be used. Next, the obtained precipitate was filtered by suction, washed with water, and dried for 12 hours at 120° C. using a tray dryer, thereby producing a precursor of the positive electrode active material. Next, lithium hydroxide and the precursor of the positive electrode active material were mixed so that the ratio (Li / Me) of the number of lithium (Li) atoms to the sum of the number of metal atoms of Ni, Co, and Mn in the precursor of the positive electrode active material was 1.01, and the mixture was mixed in an automatic mortar for 30 minutes to obtain a mixed powder. Next, the mixed powder was filled into an alumina sagger and fired in an oxygen atmosphere in a muffle furnace at 500°C for 4 hours, and then heated to 720°C and held at that temperature for 8 hours to obtain a positive electrode active material.

[0058] Next, the surface of the positive electrode active material was coated with 1.0 mol% LiNbO3 using a rolling fluidized bed coating device with a solution containing LiOC2H5 and Nb(OC2H5)5.The powder coated with LiNbO3 was then heat-treated at 300°C for 1 hour to obtain a positive electrode active material coated with lithium niobate on the surface.

[0059] Example 2 A 1.5 mol / L mixed metal salt solution was prepared by weighing out a predetermined amount of nickel sulfate, cobalt sulfate, and manganese sulfate so that Ni:Co:Mn=82:13.5:4.5. A precursor of a positive electrode active material was prepared in the same manner as in Example 1, except that the ammonium ion concentration was 17.9 g / L and the pH was 11.2 under the crystallization reaction conditions. Then, a positive electrode active material was prepared in the same manner as in Example 1, except that the firing temperature was 740° C. under the firing conditions.

[0060] Example 3 A 1.5 mol / L mixed metal salt solution was prepared by weighing out a predetermined amount of nickel sulfate, cobalt sulfate, and manganese sulfate so that Ni:Co:Mn=82:12:6. A precursor of a positive electrode active material was prepared in the same manner as in Example 1, except that the ammonium ion concentration was 14.6 g / L and the pH was 11.2 under the crystallization reaction conditions. Then, a positive electrode active material was prepared in the same manner as in Example 1, except that the firing temperature was 740° C. under the firing conditions.

[0061] Example 4 A 1.5 mol / L mixed metal salt solution was prepared by weighing out a predetermined amount of nickel sulfate, cobalt sulfate, and manganese sulfate so that Ni:Co:Mn=82:15:3. A precursor of a positive electrode active material was prepared in the same manner as in Example 1, except that the ammonium ion concentration was 14.4 g / L and the pH was 11.3 under the crystallization reaction conditions. Then, a positive electrode active material was prepared in the same manner as in Example 1.

[0062] Example 5 A precursor of a positive electrode active material was prepared in the same manner as in Example 4, except that the crystallization reaction conditions were a reaction temperature of 55° C., an ammonium ion concentration of 10.8 g / L, and a pH of 11.4. Then, a positive electrode active material was prepared in the same manner as in Example 1, except that the precursor was mixed with lithium hydroxide so that the Li / Me ratio was 1.03.

[0063] Example 6 A precursor of a positive electrode active material was prepared in the same manner as in Example 4, except that the crystallization reaction conditions were a reaction temperature of 65° C., an ammonium ion concentration of 21.3 g / L, and a pH of 11.3. Then, a positive electrode active material was prepared in the same manner as in Example 1, except that the firing temperature was 740° C.

[0064] Comparative Example 1 A precursor of a positive electrode active material was prepared in the same manner as in Example 1, except that the crystallization reaction conditions were an ammonium ion concentration of 7.9 g / L and a pH of 11.0. Then, a positive electrode active material was prepared in the same manner as in Example 1.

[0065] Comparative Example 2 A precursor of a positive electrode active material was prepared in the same manner as in Example 4, except that the crystallization reaction conditions were an ammonium ion concentration of 20.4 g / L and a pH of 11.5. Then, a positive electrode active material was prepared in the same manner as in Example 4, except that the firing temperature was 740° C.

[0066] (Composition of Positive Electrode Active Material) A specified amount of each obtained positive electrode active material sample (powder) was weighed out and decomposed by an alkali fusion method, and then a composition analysis was performed using an inductively coupled plasma optical emission spectrometer (ICP-OES) "PS7800" manufactured by Hitachi High-Tech Corporation.

[0067] (50% cumulative volumetric particle size D50) 100 mg of each positive electrode active material sample (powder) was dispersed by irradiating 40 W ultrasonic waves for 60 seconds at 50% flow rate using a Microtrac laser diffraction particle size distribution analyzer "MT3300EXII", and then the particle size distribution was measured to obtain a volume-based cumulative particle size distribution curve. In the obtained cumulative particle size distribution curve, the volume particle size at 50% accumulation was taken as the 50% cumulative volume particle size D50 of the positive electrode active material powder. In addition, the 50% cumulative volume particle size D50 of each positive electrode active material precursor sample (powder) was measured by the same method.

[0068] (Tap density) 5 g of each obtained positive electrode active material sample (powder) was placed in a 10 cc graduated cylinder and placed in a powder density measuring device "KYT-4000K" manufactured by Seishin Enterprise Co., Ltd. After tapping 1500 times with a stroke length of 55 mm, the graduations on the graduated cylinder were read. Next, "sample amount (5 g) / graduation reading on the graduated cylinder (cc)" was calculated, and this was taken as the tap density (g / cc). In addition, the tap density of each positive electrode active material precursor sample (powder) was measured by the same method.

[0069] (Circularity) The obtained samples (powders) of each positive electrode active material were measured using a particle image analyzer "Morphologi G3" manufactured by Malvern. Specifically, the particle image analyzer was used to measure the circularity of optical images of more than 20,000 particles, which were filtered using a parameter of "solidity = 0.93". In the particle image analyzer, first, a sample (positive electrode active material) was placed in a sample cartridge and then set in a dispersion unit. Next, a nitrogen gas introduction line was connected to the dispersion unit, and the sample was dispersed on a glass plate by spraying nitrogen gas. After continuously photographing particle images of the dispersed sample on the glass plate and analyzing the images, the circularity was calculated from the projected area and perimeter of each photographed particle (18,000 or more) using the following formula. The average circularity refers to the average circularity of all the measured particles of the positive electrode active material.

[0070] Circularity = 4πS / L 2 ···(formula) (In the above formula, S is the projected area of ​​the particle, L is the perimeter of the projected image of the particle, and π is the circular constant.)

[0071] The circularity of each positive electrode active material precursor sample (powder) was also measured by the same method.

[0072] (Ratio of 50% cumulative volumetric particle size of precursor D50×π to average particle circumference) The average particle perimeter of the precursor was measured by image analysis of the precursor particles using a particle image analyzer "Morphologi G3" manufactured by Malvern. Next, the ratio (B) / (A) of the 50% cumulative volumetric particle size D50 (A) of the precursor obtained by the above measurement to the average particle perimeter (B) of the precursor was calculated. In addition, the ratio of the 50% cumulative volume particle size D50×π to the average particle circumference was measured for each positive electrode active material sample (powder) by the same method.

[0073] (Battery characteristics) Hereinafter, the preparation of the all-solid-state battery cell was carried out in a glove box under an argon atmosphere. First, each was coated with LiOC2H5 and Nb(OC2H5)5, and then baked at 400°C for 1 hour in an oxygen atmosphere to produce a positive electrode active material whose surface was coated with an amorphous layer of lithium niobate. Next, 75 mg of the surface-coated positive electrode active material and 425 mg of a sulfide solid electrolyte material Li3PS were mixed to obtain a positive electrode mixture. In addition, 480 mg of the sulfide solid electrolyte material Li3PS was pressed at a pressure of 5 MPa using a pellet molding machine to form a solid electrolyte layer. 10 mg of the positive electrode composite was placed on the solid electrolyte layer and pressed at a pressure of 30 MPa to form a composite layer. Next, the obtained composite layer of the solid electrolyte layer and the positive electrode active material layer was turned over, and a SUS plate with Li foil (5 mm diameter × 0.1 mm thickness) attached thereto was placed on the solid electrolyte layer side, and pressed at a pressure of 20 MPa to form a Li negative electrode layer. In this way, a laminate in which the positive electrode active material layer, the solid electrolyte layer, and the Li negative electrode layer were laminated in this order was produced. Next, the laminate was placed in a battery test cell made of SUS304 and subjected to a confining pressure to form an all-solid-state secondary battery, and the initial battery characteristics (charge capacity, discharge capacity, charge and discharge characteristics) were measured at 25°C. The charge and discharge conditions were: charge condition: CC / CV 4.2V, 0.1C, discharge condition: CC 0.05C, up to 3.0V. The above manufacturing conditions and test results are shown in Tables 1 and 2.

[0074] [Table 1]

[0075] [Table 2]

[0076] (Evaluation Results) The positive electrode active materials according to Examples 1 to 6 all have the composition formula: Li a Ni x Co y Mn 1-x-y O2 (wherein 1.00≦a≦1.03, 0.8≦x≦0.9, 0≦y≦0.16), the 50% cumulative volume particle size D50 was 3.0 to 7.0 μm, the tap density was 1.9 to 2.5 g / cc, and the circularity was 0.90 to 0.93, so that the discharge capacity was good. In Comparative Example 1, the tap density was outside the range of 1.9 to 2.5 g / cc and the circularity was outside the range of 0.90 to 0.93, so that the discharge capacity was poor. In Comparative Example 2, the 50% cumulative volume particle size D50 was outside the range of 3.0 to 7.0 μm, the tap density was outside the range of 1.9 to 2.5 g / cc, and the circularity was outside the range of 0.90 to 0.93, so that the discharge capacity was poor.

Claims

1. Composition formula: Li a Ni x Co y Mn 1-x-y O 2 (In the above formula, 1.00≦a≦1.03, 0.8≦x≦0.9, and 0≦y≦0.16.) The 50% cumulative volume particle size D50 is 3.0 to 7.0 μm, the tap density is 1.9 to 2.5 g / cc, and the circularity is 0.90 to 0.93, A positive electrode active material for an all-solid-state lithium-ion battery, in which the ratio (B) / (A) of a 50% cumulative volume particle size D50×π (A) to an average particle perimeter (B) is 0.91 to 0.

98.

2. 2. The positive electrode active material for an all-solid-state lithium ion battery according to claim 1, further comprising a coating layer made of an oxide of Li and Nb on a surface of the positive electrode active material.

3. Composition formula: Ni x Co y Mn 1-x-y (OH) 2 (In the above formula, 0.8≦x≦0.9, 0≦y≦0.16.) The 50% cumulative volume particle size D50 is 2.0 to 7.0 μm, the tap density is 1.6 to 2.0 g / cc, and the circularity is 0.87 to 0.97, A precursor of a positive electrode active material for an all-solid-state lithium ion battery, in which the ratio (B) / (A) of a 50% cumulative volume particle size D50×π (A) to an average particle circumference (B) is 0.86 to 1.

06.

4. A positive electrode for an all-solid-state lithium ion battery, comprising the positive electrode active material for an all-solid-state lithium ion battery according to claim 1 or 2.

5. An all-solid-state lithium ion battery comprising: a positive electrode layer formed of the positive electrode for an all-solid-state lithium ion battery according to claim 4; a negative electrode layer; and a solid electrolyte layer.

6. 4. A method for producing a precursor of a positive electrode active material for an all-solid-state lithium ion battery according to claim 3, comprising the steps of: using an aqueous solution containing (a) a nickel salt, (b) a cobalt salt, (c) a manganese salt, and (d) a basic aqueous solution of ammonia water and an alkali metal as a reaction solution; and carrying out a crystallization reaction while controlling the pH of the reaction solution to 10.8 to 11.4, the ammonium ion concentration to 10 to 22 g / L, and the solution temperature to 55 to 65° C.

7. The precursor produced by the method for producing a precursor for a positive electrode active material for an all-solid-state lithium ion battery according to claim 6 and a lithium source are mixed together to obtain a cathode active material for an all-solid-state lithium ion battery. n ) and the number of lithium atoms (Li n ) and the ratio (Li n / Me n ) is 1.01 to 1.03 to form a lithium mixture; calcining the lithium mixture in an oxygen atmosphere at 450 to 520° C. for 2 to 15 hours, and then calcining the mixture at 680 to 850° C. for 2 to 15 hours; The method for producing a positive electrode active material for an all-solid-state lithium ion battery includes the steps of:

Citation Information

Patent Citations

  • Positive electrode material for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery arranged by use thereof, and method for manufacturing positive electrode material for nonaqueous electrolyte secondary battery

    JP2018077937A

  • Positive electrode active material for nonaqueous electrolyte secondary battery and method for manufacturing the same

    JP2019067506A

  • Lithium metal composite oxide powder, positive electrode active material for lithium secondary batteries, positive electrode and lithium secondary battery

    JP2020083750A

  • Oxide-based positive electrode active material for all-solid-state lithium ion batteries, method for producing precursor of oxide-based positive electrode active material for all-solid-state lithium ion batteries, method for producing oxide-based positive electrode active material for all-solid-state lithium ion batteries, and all-solid-state lithium ion battery

    WO2020202602A1