Inkjet recording medium

The inkjet recording medium with a specific polyvinyl alcohol resin and inorganic particles addresses cracking, slow drying, and low water resistance issues, enabling a simpler manufacturing process and improved performance.

JP7584338B2Active Publication Date: 2024-11-15KYODO PRINTING CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021048771
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-23
Publication Date
2024-11-15
Estimated Expiration
2041-03-23

AI Technical Summary

Technical Problem

Existing inkjet recording media face issues with cracking, slow ink drying, and low water resistance, particularly when using polyvinyl alcohol resin as a hydrophilic binder, and require complex manufacturing processes.

Method used

An inkjet recording medium with a base material layer and an ink receiving layer containing a specific polyvinyl alcohol resin with a monomer unit and inorganic particles, optimized in terms of mass ratio and particle properties, along with a dispersant and curing agent, to enhance adhesion and reduce cracking while improving quick drying and water resistance.

Benefits of technology

The solution allows for a simpler manufacturing process that suppresses cracking, enhances ink drying speed, and improves water resistance, resulting in a more durable and efficient inkjet recording medium.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584338000008
    Figure 0007584338000008
  • Figure 0007584338000009
    Figure 0007584338000009
  • Figure 0007584338000001
    Figure 0007584338000001
Patent Text Reader

Abstract

To provide an inkjet recording medium which can be manufactured by a simple method while suppressing cracking and improving ink quick-drying property and water resistance.SOLUTION: An inkjet recording medium 1 has a base material layer 10, and an ink reception layer 20 laminated on the base material layer 10, where the ink reception layer 20 contains a polyvinyl alcohol resin having a monomer unit represented by the following formula (1), and inorganic particles.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an inkjet recording medium. [Background technology]

[0002] 2. Description of the Related Art As a recording medium for use in an inkjet printer, an inkjet recording medium has been proposed in which an ink receiving layer is provided on a substrate such as paper, cloth, or plastic film.

[0003] Such an inkjet recording medium is produced by a method such as that disclosed in Patent Document 1, for example.

[0004] Specifically, Patent Document 1 discloses a method for producing a recording medium, which includes applying a coating liquid for a primer layer containing a resin and a crosslinking agent, drying the coating liquid to form a primer layer, and after forming the primer layer, performing an aging treatment for 10 days or more in an environment of 25°C or higher and 45°C or lower, and then applying a coating liquid for an ink-receiving layer onto the primer layer and drying the coating liquid to form an ink-receiving layer.

[0005] Specific examples of the ink receiving layer include those containing inorganic particles and a hydrophilic binder, as disclosed in Patent Documents 2 and 3. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2003-164798 A [Patent Document 2] JP 2018-171747 A [Patent Document 3] JP 2004-338100 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present inventors have investigated the use of a polyvinyl alcohol resin as the hydrophilic binder in an ink receiving layer containing inorganic particles and a hydrophilic binder.

[0008] The greater the porosity of the ink receiving layer, the faster the ink dries. One possible way to increase the porosity of the ink receiving layer is to increase the amount of inorganic particles packed in the ink receiving layer. However, in a configuration in which a polyvinyl alcohol resin is used as a hydrophilic binder, if the content of inorganic particles is high, the ink receiving layer formed is prone to cracking.

[0009] Furthermore, when the inkjet recording medium is exposed for a long period of time to an environment where it is likely to come into contact with water, such as outdoors, it is also required to have high water resistance.

[0010] Therefore, there is a demand for an inkjet recording medium that is less susceptible to cracking, has quick ink drying properties, and has improved water resistance.

[0011] In addition, polyvinyl alcohol resins, which have been used as hydrophilic binders in the past, have low adhesion to substrates, such as plastic substrates, and therefore require pretreatment such as forming a primer layer and aging for a long period of time of 10 days or more, as well as complex steps and special manufacturing equipment for these steps, as in the manufacturing method disclosed in Patent Document 1.

[0012] Therefore, there is a demand for an inkjet recording medium that can be produced by a simpler method.

[0013] An object of the present invention is to provide an inkjet recording medium which can be produced by a simple method while suppressing cracking, improving ink quick-drying properties, and water resistance. [Means for solving the problem]

[0014] The present inventors have found that the above object can be achieved by the following means:

[0015] Aspect 1 The ink-receiving layer includes a base layer and an ink-receiving layer laminated on the base layer. The ink receiving layer contains a polyvinyl alcohol resin having a monomer unit represented by the following formula (1) and inorganic particles: Inkjet recording media:

[0016] [ka]

[0017] Aspect 2 2. The inkjet recording medium according to aspect 1, wherein the content of the monomer unit represented by formula (1) in the polyvinyl alcohol resin is 6.0 mol % to 11.0 mol %.

[0018] Aspect 3 The inkjet recording medium according to aspect 1 or 2, wherein the polyvinyl alcohol resin further has a monomer unit represented by the following formula (2):

[0019] [ka]

[0020] Aspect 4 4. The inkjet recording medium according to any one of aspects 1 to 3, wherein the proportion of the mass of the polyvinyl alcohol resin to the total mass of the polyvinyl alcohol resin and the inorganic particles is 10% by mass to 30% by mass.

[0021] Aspect 5 5. The inkjet recording medium according to any one of aspects 1 to 4, wherein the inorganic particles are fumed silica particles.

[0022] Aspect 6 The average primary particle size of the inorganic particles is 7 nm to 20 nm, and The specific surface area of ​​the inorganic particles is 100 m 2 / g~400m 2 / g, The inkjet recording medium according to any one of aspects 1 to 5.

[0023] Aspect 7 7. The inkjet recording medium according to any one of aspects 1 to 6, wherein the ink receiving layer further comprises a dispersant and a curing agent.

[0024] Aspect 8 8. The inkjet recording medium according to embodiment 7, wherein the dispersant is a quaternary ammonium salt compound having a molecular weight of 5,000 to 50,000.

[0025] Aspect 9: 9. The inkjet recording medium according to embodiment 8, wherein the curing agent is a water-dispersible hexamethylene diisocyanate or a water-based chelating agent.

[0026] Aspect 10 10. The inkjet recording medium according to any one of aspects 1 to 9, wherein the ink receiving layer has a thickness of 10 μm to 30 μm. Effect of the Invention

[0027] According to the present invention, it is possible to provide an inkjet recording medium that can be produced by a simple method while simultaneously suppressing cracking and providing quick drying of ink. [Brief description of the drawings]

[0028] [Figure 1] FIG. 1 is a schematic diagram showing an inkjet recording medium according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an inkjet recording medium according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the preferred embodiments. It should be noted that the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the present invention.

[0030] The inkjet recording medium of the present invention has a base layer and an ink receiving layer laminated on the base layer. The ink receiving layer contains a polyvinyl alcohol resin having a monomer unit represented by the following formula (1) and inorganic particles:

[0031] [ka]

[0032] FIG. 1 is a schematic diagram showing an inkjet recording medium 1 according to a first embodiment of the present invention.

[0033] 1, an inkjet recording medium 1 according to a first embodiment of the present invention has a base layer 10 and an ink receiving layer 20 laminated on the base layer 10. Here, the ink receiving layer contains a polyvinyl alcohol resin having a monomer unit represented by the above formula (1), and inorganic particles.

[0034] Although not limited by the theory, the principle by which the inkjet recording medium of the present invention can be produced by a simple method while suppressing cracking, improving ink quick-drying properties, and water resistance is as follows.

[0035] As described above, the ink quick-drying property of the ink receiving layer can be improved by increasing the filling amount of inorganic particles in the ink receiving layer, however, the increase in the filling amount of inorganic particles in the ink receiving layer tends to increase the cracking of the ink receiving layer.

[0036] When a polyvinyl alcohol resin having a monomer unit represented by the above formula (1) is used as the binder resin for the ink receiving layer, even when the filling amount of inorganic particles is high, cracks are less likely to occur in the ink receiving layer, and the water resistance of the ink receiving layer can be improved.

[0037] In addition, the polyvinyl alcohol resin having the monomer unit represented by the above formula (1) has high adhesion to the substrate. Therefore, the inkjet recording medium of the present invention can significantly reduce the pretreatment required to ensure adhesion between the ink receiving layer and the substrate. In other words, it can be produced more easily.

[0038] Therefore, the ink jet recording medium of the present invention can be produced by a simple method while suppressing cracking, improving the quick drying property of the ink, and improving water resistance.

[0039] The inkjet recording medium of the present invention can be applied to any object on which inkjet printing is performed. The inkjet recording medium of the present invention may be, for example, printing paper, packaging, signs, stickers, etc. In particular, since the inkjet recording medium of the present invention has high water resistance, it may be used for signs, such as stickers, applied to walls and bulletin boards of buildings, and vehicles such as automobiles and motorcycles.

[0040] <Ink Receiving Layer> The ink receiving layer is a layer in the ink recording medium that absorbs and retains ink. The ink receiving layer is laminated on the base layer.

[0041] The ink receiving layer contains a polyvinyl alcohol resin having a monomer unit represented by the above formula (1) and inorganic particles.

[0042] The proportion of the mass of the polyvinyl alcohol resin to the total mass of the polyvinyl alcohol resin and the inorganic particles in the ink receiving layer is preferably 10% by mass to 30% by mass.

[0043] When the mass ratio of the polyvinyl alcohol resin is 10% by mass or more, the content of the polyvinyl alcohol resin is significantly larger than the content of the inorganic particles, so that cracking of the ink receiving layer is further suppressed.On the other hand, when the mass ratio of the polyvinyl alcohol resin is 30% by mass or less, the content of the inorganic particles can be significantly increased, so that the porosity of the ink receiving layer can be improved, and thus the ink quick-drying property can be further improved.

[0044] The mass proportion of the above polyvinyl alcohol resin may be 10% by mass or more, 15% by mass or more, 20% by mass or more, or 25% by mass or more, and may be 30% by mass or less, 25% by mass or less, 20% by mass or less, or 15% by mass or less.

[0045] The thickness of the ink receiving layer is preferably 10 μm to 30 μm.

[0046] When the thickness of the ink receiving layer is 10 μm or more, the amount of voids in the ink receiving layer can be increased, so that the ink can be absorbed more easily. Therefore, the ink can be dried quickly. On the other hand, when the thickness of the ink receiving layer is 30 μm or less, the ink recording medium as a whole can be made thinner. Furthermore, for example, when the substrate layer is a transparent substrate layer, the transparency of the ink recording medium can be increased when the thickness of the ink receiving layer is 30 μm or less.

[0047] The thickness of the ink receiving layer may be 10 μm or more, 15 μm or more, 20 μm or more, or 25 μm or more, and may be 30 μm or less, 25 μm or less, 20 μm or less, or 15 μm or less. Note that the "thickness" of the ink receiving layer means the average thickness.

[0048] The ink receiving layer preferably further contains a dispersing agent and a hardening agent.

[0049] <Polyvinyl alcohol resin> The polyvinyl alcohol resin contained in the ink receiving layer of the present invention has a monomer unit represented by the above formula (1). Hereinafter, the polyvinyl alcohol resin having a monomer unit represented by the above formula (1) may be referred to as a "partially benzacetalized polyvinyl alcohol".

[0050] The content of the monomer unit represented by formula (1) in the partially benzacetalized polyvinyl alcohol may be 6.0 mol % to 11.0 mol %.

[0051] The content of the above monomer units in the partially benzacetalized polyvinyl alcohol may be 6.0 mol% or more, 7.0 mol% or more, 8.0 mol% or more, or 9.0 mol% or more, and may be 11.0 mol% or less, 10.0 mol% or less, 9.0 mol% or less, or 8.0 mol% or less.

[0052] The degree of polymerization of the partially benzacetalized polyvinyl alcohol may be from 1000 to 5000. The degree of polymerization may be 1000 or more, 1500 or more, 2000 or more, or 2500 or more, and may be 5000 or less, 4500 or less, 4000 or less, or 3500 or less.

[0053] Partially benzacetalized polyvinyl alcohol can be produced, for example, by reacting polyvinyl alcohol with benzaldehyde.

[0054] In addition, polyvinyl alcohol resins may be saponified during production and may have acetyl groups in their side chains. Therefore, partially benzacetalized polyvinyl alcohol may further have a monomer unit represented by the following formula (2):

[0055] [ka]

[0056] <Inorganic particles> In the present invention, the ink receiving layer contains inorganic particles.

[0057] The inorganic particles can be any inorganic particles that can form voids in the ink-receiving layer and allow the voids to receive, for example, absorb and / or hold ink.

[0058] Examples of the inorganic particles that can be used include silica, talc, kaolin, clay, alumina white, calcium carbonate, magnesium carbonate, aluminum sulfate, barium sulfate, and mixtures thereof. The silica may be fumed silica particles.

[0059] The inorganic fine particles used in the present invention preferably have an average primary particle size of 7 nm to 20 nm.

[0060] When the inorganic fine particles have an average primary particle size of 7 nm or more, the size of the voids formed in the ink receiving layer can be more appropriately maintained, and the ink quick-drying property can be further improved. On the other hand, when the inorganic fine particles have an average primary particle size of 20 nm or less, the transparency of the ink receiving layer can be further improved.

[0061] The average primary particle diameter refers to the arithmetic mean value of the measurements taken using a transmission electron microscope (TEM), such as a Titan Cubed G2 60-300 (manufactured by Thermo Fisher Scientific), to measure the maximum diagonal of 100 or more randomly selected particles, or, if the particles are rounded, to measure the major axis (the tangent in the major direction).

[0062] The specific surface area of ​​the inorganic fine particles used in the present invention is 100 m 2 / g~400m 2 The specific surface area can be measured by the BET flow method using an HM model-1208 (manufactured by Mountech Co., Ltd.) in accordance with JIS Z8830.

[0063] The specific surface area of ​​inorganic particles is 100m 2When the specific surface area of ​​the inorganic fine particles is 400 m / g or more, the size of the voids formed in the ink receiving layer can be kept more appropriate, and the ink quick-drying property can be further improved. 2 When the viscosity is 100 / g or less, cracking of the ink receiving layer can be further suppressed.

[0064] The specific surface area of ​​inorganic particles is 100m 2 / g or more, 150m 2 / g or more, 200m 2 / g or more, or 250m 2 / g or more, 2 / g or less, 350m 2 / g or less, 300m 2 / g or less, or 250m 2 / g or less.

[0065] <Dispersant> In the present invention, the ink receiving layer may contain a dispersant.

[0066] When the ink receiving layer contains a dispersant, the viscosity of the coating liquid for forming the ink receiving layer can be increased during production, making it easier to form the ink receiving layer.

[0067] From the viewpoint of dispersibility and sedimentation stability, the dispersant is preferably a cationic polymer. Among them, a quaternary ammonium salt compound having a molecular weight of 5000 to 50000 is particularly preferable. Other cationic compounds may also be used in combination.

[0068] When a quaternary ammonium salt compound is used as a dispersant, the dispersion stability can be improved if the molecular weight is 5000 or more. On the other hand, if the molecular weight is 50000 or less, the viscosity of the coating liquid can be kept at an appropriate level, making coating easy.

[0069] When a quaternary ammonium salt compound is used as a dispersant, the molecular weight may be 5,000 or more, 5,000 or more, 15,000 or more, or 20,000 or more, and may be 50,000 or less, 45,000 or less, 30,000 or less, or 25,000 or less.

[0070] The content of the dispersant is preferably 1 to 10% by mass relative to the content of the inorganic filler in the ink receiving layer.

[0071] The content of the dispersant may be 1% by mass or more, 2% by mass or more, 3% by mass or more, or 4% by mass or more, and may be 10% by mass or less, 9% by mass or less, 8% by mass or less, or 7% by mass or less, relative to the content of the inorganic filler in the ink receiving layer.

[0072] <Hardening agent> In the present invention, the ink receiving layer may contain a curing agent.

[0073] When the ink receiving layer contains a curing agent, the water resistance of the ink receiving layer can be improved.

[0074] The curing agent may be a boron compound, a glyoxylate, an aqueous chelating agent such as an organic titanium or organic zirconium type, or a water-dispersible hexamethylene diisocyanate.

[0075] From the viewpoint of ensuring the transparency of the ink receiving layer, the curing agent is preferably a water-based chelating agent or a water-dispersible hexamethylene diisocyanate.

[0076] 《Base material layer》 The substrate layer is a layer that serves as a substrate on which the ink receiving layer is laminated.

[0077] The substrate layer may be a layer made of any material on which the ink-receiving layer can be laminated. The substrate layer may be paper, cloth, plastic, etc. When the substrate layer is plastic, polycarbonate, nylon, polyethylene, polypropylene, polystyrene, polyethylene terephthalate, etc. may be used.

[0078] The substrate layer may be a transparent substrate layer.

[0079] In the present invention, since the amount of inorganic particles loaded in the ink receiving layer can be increased while suppressing cracking, the ink quick-drying property of the ink receiving layer can be improved while reducing the thickness of the ink receiving layer. Furthermore, reducing the thickness of the ink receiving layer improves the transparency of the ink receiving layer.

[0080] Therefore, in the present invention, when the substrate layer is a transparent substrate layer, the transparency of the inkjet recording medium itself can also be improved.

[0081] Here, "transparent" means that a layer, such as a base layer, is transparent to such an extent that one side of the layer can be seen sufficiently from the other side.

[0082] Here, being transparent means, for example, that the total light transmittance is 80% or more, 85% or more, 90% or more, 95% or more, or 100%. The haze value may be 30% or less, 25% or less, 20% or less, or 15% or less.

[0083] Here, the total light transmittance can be measured in accordance with JIS K 7361. The haze value can be measured in accordance with JIS K7136.

[0084] 《Adhesive layer》 In the ink jet recording medium of the present invention, an adhesive layer can be laminated on the side of the base layer opposite to the side on which the ink receiving layer is laminated.

[0085] The adhesive layer is a layer for attaching the ink jet recording medium of the present invention to another object.

[0086] The adhesive layer may be, for example, an acrylic adhesive resin.

[0087] The adhesive layer may contain, for example, an ultraviolet absorbing agent in order to prevent deterioration of adhesiveness over time.

[0088] When a transparent substrate layer is used as the substrate layer, it is preferable that the adhesive layer is also a transparent layer.

[0089] FIG. 2 is a schematic diagram showing an inkjet recording medium 2 according to a second embodiment of the present invention.

[0090] As shown in FIG. 2, an inkjet recording medium 2 according to a second embodiment of the present invention is similar to that shown in FIG. 1, except that an adhesive layer 30 is laminated on the side of the base layer 10 opposite to the side on which the ink receiving layer 20 is laminated. EXAMPLES

[0091] Examples 1 to 3 and Comparative Examples 1 to 4 Example 1 The inkjet recording medium of Example 1 was prepared as follows.

[0092] (Preparation of vapor-phase silica dispersion) To 50 parts by weight of ion-exchanged water, 1.7 parts by weight of a cationic polymer aqueous solution (solid content: 52.3 wt%) was added as a dispersant, followed by the addition of 35 parts by weight of 2-propanol to prepare a dispersion medium.

[0093] The dispersion medium was stirred at 3000 rpm with a homogenizer (product name: Biomixer BM-2, manufactured by Nippon Seiki Seisakusho Co., Ltd.) while 15 parts by weight of fumed silica was added little by little to obtain a dispersion liquid with a solid content of 15.6 wt %.

[0094] (Preparation of Coating Fluid) 31 parts by weight of a water / 2-propanol solution (solid content 8.4 wt%) of partially benzacetalized polyvinyl alcohol (polyvinyl alcohol resin having a monomer unit represented by the above formula (1), degree of polymerization: 3500, degree of benzacetalization: 8 mol%) was mixed with 70 parts by weight of a silica dispersion to give a resin / silica solid content ratio of 20 / 80. Next, 0.1 parts by weight of a hexamethylene diisocyanate-based curing agent (solid content 100 wt%) was added and stirred to obtain a coating liquid.

[0095] (Formation of ink receiving layer) A transparent biaxially oriented polyethylene terephthalate film having a thickness of 75 μm was used as the substrate.

[0096] The coating liquid was applied onto the substrate using a desktop coating machine (product name: Control Coater 7000, manufactured by Imoto Manufacturing Co., Ltd.), and then the substrate was dried in an oven at 80°C for 3 minutes and then aged at 60°C for 1 day to form an ink-receiving layer.

[0097] The composition of the inkjet recording medium of Example 1 is shown in Table 1 below.

[0098] Example 2 An inkjet recording medium of Example 2 was prepared in the same manner as in Example 1, except that the solids ratio of resin / silica was 30 / 70.

[0099] The composition of the inkjet recording medium of Example 2 is shown in Table 1 below.

[0100] Example 3 An inkjet recording medium of Example 2 was prepared in the same manner as in Example 2, except that a partially benzacetalized polyvinyl alcohol having a benzacetalization degree of 9 mol % and a polymerization degree of 2000 was used.

[0101] The composition of the inkjet recording medium of Example 3 is shown in Table 1 below.

[0102] Comparative Example 1 An inkjet recording medium of Comparative Example 1 was prepared in the same manner as in Example 1, except that the coating liquid was prepared as follows.

[0103] 59 parts by weight of the above silica dispersion was mixed with 42 parts by weight of a water / 2-propanol solution (solid content 9.0 wt%) of partially saponified polyvinyl alcohol (polymerization degree: 3000, saponification degree: 88 mol%) to give a resin / silica solid content ratio of 30 / 70. Next, 0.1 parts by weight of a hexamethylene diisocyanate-based curing agent (solid content 100 wt%) was added and stirred to obtain a coating liquid.

[0104] The configuration of the inkjet recording medium of Comparative Example 1 is shown in Table 1 below.

[0105] Comparative Example 2 An inkjet recording medium of Comparative Example 2 was prepared in the same manner as in Comparative Example 1, except that the solids ratio of resin / silica was set to 40 / 60.

[0106] The configuration of the inkjet recording medium of Comparative Example 2 is shown in Table 1 below.

[0107] Comparative Example 3 An inkjet recording medium of Comparative Example 3 was prepared in the same manner as in Example 1, except that the coating liquid was prepared as follows.

[0108] 59 parts by weight of the above silica dispersion was mixed with 42 parts by weight of a water / 2-propanol solution (solid content 9.0 wt%) of acetoacetyl-modified polyvinyl alcohol (polymerization degree: 1200, saponification degree: 91 mol%) to give a resin / silica solid content ratio of 30 / 70. Next, 0.1 parts by weight of a hexamethylene diisocyanate-based curing agent (solid content 100 wt%) was added and stirred to obtain a coating liquid.

[0109] The configuration of the inkjet recording medium of Comparative Example 3 is shown in Table 1 below.

[0110] Comparative Example 4 An inkjet recording medium of Comparative Example 4 was prepared in the same manner as in Comparative Example 3, except that the solids ratio of resin / silica was 40 / 60.

[0111] The configuration of the inkjet recording medium of Comparative Example 4 is shown in Table 1 below.

[0112] <evaluation> The performance of the ink jet recording medium of each example was evaluated as follows.

[0113] (Cracks) The ink receiving layer of each example of the ink jet recording medium was visually inspected for the presence or absence of cracks. The evaluation results are shown in Table 1 below.

[0114] In Table 1 below, a sample in which no cracks were observed in the ink-receiving layer is rated "good," a sample in which slight cracks were observed is rated "fair," and a sample in which cracks were observed over the entire surface of the ink-receiving layer or in which the ink-receiving layer could not be formed is rated "poor."

[0115] (transparency) The inkjet recording medium of each example was measured in accordance with JIS K 7361 using a haze meter (product name: haze transmittance / reflectance measuring meter HR-100, manufactured by Murakami Color Research Laboratory Co., Ltd.).

[0116] In Table 1 below, a total light transmittance of 85% or more is rated as "good," a total light transmittance of 80% or more but less than 85% is rated as "fair," and a total light transmittance of less than 80% is rated as "poor."

[0117] (Quick-drying ink) Using an inkjet printer (Canon PIXUS iP4830), we measured the time it took for 100-point characters to dry after they were printed in water-based pigment ink. Specifically, we set the time when the print was ejected from the printer as 0 seconds, and after 5 seconds had passed, we pressed the printed surface with gauze to check whether the ink was transferred to the gauze.

[0118] In Table 1 below, samples with absolutely no ink transfer to the gauze and no smearing or crumbling of the printed characters are rated "good," samples with some ink transfer but no smearing or crumbling of the characters are rated "fair," and samples with significant ink transfer and smearing or crumbling of the characters are rated "poor."

[0119] (Adhesion to substrate) A Cellophane (registered trademark) tape was applied to the ink receiving layer and then peeled off, and it was confirmed whether the ink receiving layer was also peeled off at that time.

[0120] In Table 1 below, samples in which the ink-receiving layer did not peel off are rated "good," samples in which the ink-receiving layer partially peeled off but did not pose any problems in use are rated "fair," and samples in which most of the ink-receiving layer peeled off are rated "poor."

[0121] (water resistance) The ink receiving layer was wiped 200 times with water-soaked gauze to check whether the ink receiving layer disappeared or not.

[0122] In Table 1 below, the following rating is given: "Good" indicates that none of the ink receiving layer was lost; "Average" indicates that a small amount of the ink receiving layer was lost but there was no problem in use; and "Poor" indicates that most of the ink receiving layer was lost.

[0123] <result> The configuration and evaluation results of each example are shown in Table 1 below.

[0124] [Table 1]

[0125] As shown in Table 1, the inkjet recording media of Examples 1 to 3, which used partially benzacetalized polyvinyl alcohol as the binder resin in the ink receiving layer, showed good results in terms of cracking, transparency, ink quick-drying property, substrate adhesion, and water resistance. In other words, all of the evaluations were "good."

[0126] In contrast, the inkjet recording media of Comparative Examples 1 to 4, which used partially saponified polyvinyl alcohol or acetoacetyl-modified polyvinyl alcohol as the binder resin in the ink receiving layer, were rated "good" or "fair" in some evaluations, but "poor" in others. [Explanation of symbols]

[0127] 1 and 2 Inkjet recording medium 10 Base material layer 20 Ink receiving layer 30 Adhesive layer

Claims

1. The ink-receiving layer includes a base layer and an ink-receiving layer laminated on the base layer. The ink receiving layer contains a polyvinyl alcohol resin having a monomer unit represented by the following formula (1) and inorganic particles, The ratio of the mass of the polyvinyl alcohol resin to the total mass of the polyvinyl alcohol resin and the inorganic particles is 10% by mass to 30% by mass. Inkjet recording media: [Formula 1]

2. 2. The inkjet recording medium according to claim 1, wherein the content of the monomer unit represented by formula (1) in the polyvinyl alcohol resin is 6.0 mol % to 11.0 mol %.

3. 3. The inkjet recording medium according to claim 1, wherein the polyvinyl alcohol resin further comprises a monomer unit represented by the following formula (2): [chemical 2]

4. The inkjet recording medium according to any one of claims 1 to 3, wherein the inorganic particles are fumed silica particles.

5. The average primary particle size of the inorganic particles is 7 nm to 20 nm; and The specific surface area of ​​the inorganic particles is 100 m 2 / g to 400m 2 / g, The inkjet recording medium according to any one of claims 1 to 4.

6. The ink-jet recording medium according to any one of claims 1 to 5, wherein the ink-receiving layer further comprises a dispersant and a hardener.

7. 7. The inkjet recording medium according to claim 6, wherein the dispersant is a quaternary ammonium salt compound having a molecular weight of 5,000 to 50,000.

8. The inkjet recording medium according to claim 7, wherein the curing agent is a water-dispersible hexamethylene diisocyanate or a water-based chelating agent.

9. The inkjet recording medium according to any one of claims 1 to 8, wherein the ink receiving layer has a thickness of 10 µm to 30 µm.

Citation Information

Patent Citations

  • Ink jet recording sheet

    JP2002225418A

  • Ink jet recording medium

    JP2002283699A

  • Method for manufacturing recording medium

    JP2003164798A

  • Ink jet recording sheet

    JP2003191627A

  • Manufacturing method for recording material

    JP2003191630A