Artificial graphite, its manufacturing method, secondary battery and power consumption device containing same
Artificial graphite with a controlled density ratio addresses the issue of volumetric expansion in secondary batteries, enhancing cycle performance and safety by improving deformation resistance and structural stability.
Patent Information
- Application Number
- JP2022569629
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-13
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-09-13
AI Technical Summary
Secondary batteries experience volumetric expansion during the cycling process, leading to increased internal stress and affecting their service life and safety, which is a concern for the growing market demand for improved performance and safety in new energy vehicles.
The use of artificial graphite with a specific density ratio (PD 5t/PD 0.5t ≦1.35) as a negative electrode material, manufactured through a process involving mixing raw and calcined coke particles with an adhesive and solvent, shaping, graphitization, and powdering, to enhance deformation resistance and stability.
The artificial graphite material exhibits reduced expansion force during cycling, improving cycle performance, energy density, and shelf life of secondary batteries by maintaining structural integrity and enhancing deformation resistance.
Smart Images

Figure 0007584541000001 
Figure 0007584541000002 
Figure 0007584541000003
Abstract
Description
[Technical field]
[0001] This application relates to the field of graphite materials, and in particular to artificial graphite, its manufacturing method, secondary batteries and power consuming devices containing same. [Background technology]
[0002] Secondary batteries have been widely used due to their outstanding characteristics such as high energy density, non-pollution, and long service life.
[0003] However, during the cycle process of the secondary battery, the volume expansion occurs, which causes an increase in the internal stress of the battery, affecting the service life and safety of the battery. For example, with the rapid popularization of new energy vehicles, the market requirements for the service life and safety of power-type secondary batteries are increasing. In order to improve the market competitiveness of new energy vehicles, it is necessary to provide a secondary battery that has both good electrical performance and safety. Summary of the Invention
[0004] The present application provides artificial graphite capable of reducing the volume expansion during cycling of a secondary battery, a method for producing the same, a secondary battery containing the same, and a power consuming device.
[0005] According to some embodiments, the present application provides an artificial graphite. The artificial graphite is a PD 5t / PD 0.5t ≦1.35, where PD 5t is the compacted density of the synthetic graphite measured at a pressure of 5 tons, and PD 0.5t is the compacted density of the synthetic graphite measured at a pressure of 0.5 tonnes.
[0006] This application is filed by P.D. 5t / PD 0.5t reflects the sensitivity of graphite density to pressure changes, where PD 5t is the compacted density of the synthetic graphite measured at a pressure of 5 tons, and PD 0.5tis the compaction density of the artificial graphite measured at a pressure of 0.5 tons. As a negative electrode material for secondary batteries, the artificial graphite undergoes changes in force as it repeatedly absorbs and releases lithium. 5t / PD 0.5t It was found that the PD of artificial graphite can reflect the expansion change of artificial graphite during the repeated lithium absorption and desorption process. 5t / PD 0.5t When the PD of the artificial graphite is less than 1.35, the expansion force during the cycle is small, and the battery has a low full charge expansion rate, so that the battery has good cycle performance. 5t / PD 0.5t When the ratio is ≦1.35, the material has high deformation resistance. During the cycle process of a lithium-ion battery, the negative electrode repeatedly absorbs and releases lithium, which causes it to expand and contract under repeated forces. If the negative electrode has high deformation resistance, it will expand less during the cycle process and its structure will be more stable, resulting in better cycle performance.
[0007] PD 5t / PD 0.5t can effectively reflect the ability of a material to resist deformation caused by external forces, and PD 5t / PD 0.5t When the ratio is less than or equal to 1.35, the material has high deformation resistance. During the cycle process of the battery, the negative electrode will repeatedly absorb and release lithium, which will cause it to expand and contract under repeated forces. If the negative electrode has high deformation resistance, it will expand less during the cycle process and its structure will be more stable, resulting in better cycle performance.
[0008] In an optional embodiment, the artificial graphite has a PD of 1.23 or less. 5t / PD 0.5t ≦1.3. For example, PD 5t / PD 0.5t The value of may be 1.20 to 1.25, 1.25 to 1.30, or 1.30 to 1.35. By using artificial graphite according to these methods in a secondary battery, the battery performance is further improved.
[0009] In some implementations, the synthetic graphite is 5t ≧1.8g / cm 3 For example, 1.8 g / cm 3 ≦PD 5t ≦1.95g / cm 3 In some implementation plans, PD 5t The value is 1.8 to 1.85 g / cm 3 For example, 1.85 to 1.90 g / cm 3 For example, 1.90 to 1.95 g / cm 3 By using this artificial graphite in a secondary battery, the energy density performance of the battery can be further improved.
[0010] In some implementations, the synthetic graphite is 0.5t ≧1.4g / cm 3 For example, 1.4 g / cm 3 ≦PD 0.5t ≦1.5g / cm 3 In some implementation plans, PD 0.5t The value is 1.4 to 1.45 g / cm 3 For example, 1.45 to 1.50 g / cm 3 By using this artificial graphite in a secondary battery, the energy density performance of the battery can be further improved.
[0011] In some embodiments, the median diameter Dv50 of the artificial graphite satisfies Dv50≧10 μm, for example, 19 μm≦Dv50≦22 μm. In some embodiments, the median diameter Dv50 of the artificial graphite is 10-13 μm, for example, 13-16 μm, for example, 16-19 μm, for example, 19-22 μm. The use of the artificial graphite according to this embodiment in a secondary battery is advantageous in that the particle size can be reasonably controlled to prevent the negative electrode material from expanding too much, thereby further improving the dynamic performance and cycle performance of the battery.
[0012] In some embodiments, the specific surface area SSA of the artificial graphite is SSA≦1.5 g / m 2 For example, 1.0 g / m2 ≦SSA≦1.4g / m 2 In some embodiments, the specific surface area (SSA) of the artificial graphite is 1.0-1.2 g / m 2 For example, 1.2 to 1.4 g / m 2 For example, 1.4 to 1.5 g / m 2 The use of the artificial graphite according to this method in a secondary battery is advantageous for further improving the rapid charging ability of the battery, since the negative electrode of the battery has a sufficient active area for lithium absorption.
[0013] In some embodiments, the tap density of the synthetic graphite is 0.9 g / cm 3 For example, the tap density of artificial graphite is 1.0 g / cm 3 ~1.4g / cm 3 In some embodiments, the tap density of the artificial graphite is 0.9 to 1.1 g / cm 3 For example, 1.1 to 1.3 g / cm 3 The use of the artificial graphite according to this scheme in secondary batteries is advantageous for improving the compaction density of the negative plate, thereby further improving the energy density of the battery.
[0014] In some embodiments, the graphitization degree of the artificial graphite is 90% or more, for example 92% or more, for example 94% or more, for example 96% or more, for example 98% or more, for example 90-100%. The use of the artificial graphite according to this embodiment in a secondary battery further improves the performance of the secondary battery, which is advantageous for improving the graphite gram capacity and eliminating lattice defects, and therefore for improving the cell energy density and storage performance.
[0015] In some embodiments, the gram capacity of the artificial graphite is 340 mAh / g or more, for example, 345-355 mAh / g. In some embodiments, the gram capacity of the artificial graphite is 340-345 mAh / g, for example, 345-350 mAh / g, for example, 350-355 mAh / g. By using the artificial graphite according to this embodiment in a secondary battery, the capacity performance of the secondary battery is further improved.
[0016] According to some aspects, the present application provides a method for producing artificial graphite, the method comprising: (1) mixing raw coke particles, calcined coke particles, an adhesive, and a solvent; (2) shaping the product of the previous step; (3) removing at least some or all of the solvent from the product of the previous step to obtain a green body; (4) subjecting the green compact to an artificial graphitization treatment to obtain a graphite matrix; and (5) converting the graphite base into powder to obtain artificial graphite. Here, the artificial graphite is PD 5t / PD 0.5t ≦1.35, where PD 5t is the compacted density of the synthetic graphite measured at a pressure of 5 tons, and PD 0.5t is the compacted density of the synthetic graphite measured at a pressure of 0.5 tonnes.
[0017] In some implementations, step (1) includes mechanically stirring and mixing the raw coke particles, the calcined coke particles, and the adhesive, while adding an appropriate amount of a solvent and stirring to obtain a stirred product, which is a mud or adhesive particles (e.g., millimeter- or centimeter-scale adhesive particles).
[0018] In some embodiments, step (2) includes placing the stirred product from the previous step into a molding device and extruding or pressing it to form a wet body having a preset shape.
[0019] In some embodiments, step (3) includes drying the wet body to remove the solvent and obtain a green body.
[0020] In some embodiments, step (4) includes placing the green body in a graphitization furnace and graphitizing the green body at 2800° C. or higher to obtain a graphite green body.
[0021] In some embodiments, step (5) includes crushing and / or grinding the graphite matrix, sieving (e.g., 200 mesh or larger, e.g., 200-400 mesh), and demagnetizing the graphite matrix to obtain artificial graphite powder.
[0022] In some embodiments, after the graphite body is crushed into powder, it is further subjected to one or more of the following operations: sieving, demagnetizing, and a combination thereof.
[0023] In some embodiments of the method for producing artificial graphite, the total mass of raw coke particles, calcined coke particles and adhesive is 100%, and the content of raw coke particles is 35wt% or more, for example, 35-55wt%. According to this scheme, the amount of raw coke particles is sufficient to generate sufficient adhesive strength and maintain the structural integrity during the graphitization process of the green body. In addition, the artificial graphite obtained according to this scheme has low adhesive strength between particles and can be easily depolymerized into powder. If the content of raw coke particles is lower, the adhesive effect of graphite during the high-temperature graphitization stage is low, and the reinforcing effect is insufficient, in which case the PD 5t / PD 0.5t is big.
[0024] In some embodiments of the method for producing artificial graphite, the content of calcined coke particles is more than 35wt%, for example 35-62wt%, and the performance of the artificial graphite is improved.
[0025] In some embodiments of the method for producing artificial graphite, the content of adhesive is 3wt% or more, for example 3-10wt%. According to this method, the amount of adhesive is sufficient to produce sufficient adhesive strength and maintain the structural integrity during the graphitization process of the green body. In addition, in the artificial graphite obtained according to this method, the residual carbon content of the adhesive is low, and the performance of the artificial graphite is good.
[0026] In some embodiments, the apparent density of the green body is 1.3 g / cm 3 or more, for example 1.3 g / cm 3 ~1.5g / cm 3 , 1.35g / cm 3 ~1.45g / cm 3 According to this method, the green body has sufficient strength at the graphitization stage, and the phenomenon of collapse and powdering does not occur. In addition, the graphite matrix obtained by this method has low interparticle adhesion and is easy to depolymerize into powder, and the obtained graphite powder has good performance. By using this graphite powder in a secondary battery, the secondary battery shows good cycle and storage performance. The high apparent density indicates that the adhesion between the coke particles is denser, which leads to higher stress during the graphitization process, and thus the PD 5t / PD 0.5t will be lower and the cell performance will be better.
[0027] In some embodiments, the bulk density of the green body is 0.85 g / cm 3 For example, 0.45 to 0.85 g / cm 3 In some embodiments, the bulk density of the green body is 0.45 to 0.55 g / cm 3 For example, 0.55 to 0.65 g / cm 3 For example, 0.65 to 0.75 g / cm 3 For example, 0.75 to 0.85 g / cm 3 According to this method, the degree of graphitization of the artificial graphite is high and the defects are few, and the secondary battery obtained based on this artificial graphite has better cycle performance and storage life. The bulk density of the green body is in the range of 0.45-0.85 g / cm 3 When the bulk density is too high, the resistivity is low, and according to Joule's law, the heat generated by the graphitization furnace is reduced. Therefore, the graphitization temperature is lower, and the lower the temperature, the weaker the strengthening effect of the coke particles, which leads to the PD 5t / PD 0.5t becomes larger. (The strengthening effect is mainly influenced by the adhesive effect and temperature.)
[0028] In some embodiments, the green body has at least one dimension that is ≧1 cm, such as 1-10 cm, such as 1-3 cm, such as 3-5 cm, such as 5-7 cm, such as 7-9 cm.
[0029] In some embodiments, the green body has at least two mutually perpendicular dimensions of ≧1 cm, such as 1-10 cm, such as 1-3 cm, such as 3-5 cm, such as 5-7 cm, such as 7-9 cm.
[0030] In some embodiments, the green body has three mutually perpendicular dimensions that are all ≧1 cm, such as 1-10 cm, such as 1-3 cm, such as 3-5 cm, such as 5-7 cm, such as 7-9 cm.
[0031] In some embodiments, the shape of the green bodies is selected from one or more of: cylindrical, spherical, ellipsoidal, and block-shaped.
[0032] In some implementations, the volatile matter content of the raw coke particles is ≧6wt%, for example, the content is ≧8wt%, for example, the content is 8wt%-12wt%. According to this implementation, the raw coke particles can maintain the structural integrity of the green body by producing volatile matter with adhesive effect at 1000°C or higher. If the volatile matter content of the raw coke particles is lower, the adhesive effect of the graphite in the high-temperature graphitization stage is lower, and the strengthening effect is lower, in this case, the PD 5t / PD 0.5t is big.
[0033] In some implementations, the median diameter Dv50 of the green coke particles is smaller than the median diameter Dv50 of the calcined coke particles. This allows the green coke particles to better fill the gaps between the calcined coke particles, and better play an adhesive role, so as to better maintain the structural integrity of the block matrix during the graphitization process. When the Dv50 of the green coke is lower than the Dv50 of the calcined coke, the green coke can be more easily dispersed uniformly in the precursor, which has a more uniform adhesive effect, is favorable for maintaining a more uniform compressive stress, and has a more uniform reinforcing effect, so that the PD 5t / PD 0.5t will be lower.
[0034] In some embodiments, the median diameter Dv50 of the raw coke particles is less than 15 μm, for example, 8-14 μm, so that the raw coke particles can better perform adhesive function and better maintain the structural integrity of the block matrix during the graphitization process.
[0035] In some embodiments, the median diameter Dv50 of the calcined coke particles is less than 20 μm, for example, 15-17 μm, so that the raw coke particles can better perform the adhesive function and better maintain the structural integrity of the block matrix during the graphitization process.
[0036] In some implementations, the adhesive can be evaporated or decomposed above 1000°C. According to this implementation, the raw coke particles in the green body mainly bond at the high temperature stage above 1000°C, while the adhesive components mainly bond at the low temperature stage below 1000°C, so that the green body is effectively bonded throughout all the temperature stages of graphitization and the structural integrity of the block matrix is maintained. If the adhesive content is low, the adhesive effect between the coke particles is insufficient, the compressive stress is difficult to maintain, and the reinforcing effect is insufficient, which results in the PD 5t / PD 0.5t will be larger.
[0037] In some embodiments, the adhesive is a polymeric adhesive.
[0038] In some embodiments, the polymeric adhesive comprises a water soluble polymeric adhesive, a water insoluble polymeric adhesive, or a combination thereof.
[0039] In some embodiments, the water-soluble polymer adhesive is selected from polyvinyl alcohol, starch, cellulose, or combinations thereof.
[0040] In some embodiments, the water insoluble polymer adhesive is selected from a rubber based adhesive, a thermoset based adhesive, or a combination thereof.
[0041] According to some aspects, the present application provides a secondary battery comprising the artificial graphite described in any one of the above claims, or comprising artificial graphite produced by employing the method described in any one of the above claims.
[0042] According to some aspects, the present application further provides a power consuming device including the secondary battery described above. [Brief description of the drawings]
[0043] In order to more clearly explain the technical solutions of the embodiments of the present application, the following will briefly describe the drawings that need to be used in the embodiments of the present application. Of course, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on the drawings without paying creative efforts. [Figure 1] 4(a) and (b) are scanning electron microscope photographs of artificial graphite according to an example and a comparative example of the present application, respectively. [Diagram 2] FIG. 1 is a schematic diagram of a secondary battery according to an embodiment of the present application. [Diagram 3] FIG. 1 is a schematic diagram of a battery module according to an embodiment of the present application. [Figure 4] FIG. 1 is a schematic diagram of a battery pack according to an embodiment of the present application. [Diagram 5] FIG. 5 is an exploded view of the battery pack of FIG. [Figure 6] 1 is a schematic diagram of an apparatus according to an embodiment of the present application;
[0044] In the drawings, the drawings are not drawn to scale. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0045] The following describes the embodiments of the present application in more detail in conjunction with the drawings and examples. The detailed description of the following embodiments and the drawings are for illustrative purposes of the principles of the present application, but are not intended to limit the scope of the present application, i.e. the present application is not limited to the described embodiments.
[0046] Hereinafter, the present application will be described in detail with reference to the drawings, with particular reference to the embodiments specifically disclosing the negative electrode active material and the manufacturing method thereof, the secondary battery, and the power consumption device. However, unnecessary detailed description may be omitted. For example, detailed description of well-known matters and duplicate description of the same structure may be omitted. This is to avoid the following description from becoming unnecessarily long and to allow those skilled in the art to easily understand. It should be noted that the drawings and the following description are provided to allow those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.
[0047] The "ranges" disclosed in this application are defined in the form of lower and upper limits, and a given range is defined by selecting one lower limit and one upper limit that define the boundaries of the particular range. Such defined ranges may or may not include the end values, and may be arbitrarily combined, i.e., any lower limit and any upper limit may be combined to form a range. For example, if ranges of 60-120 and 80-110 are recited for a particular parameter, it is also conceivable that they are understood as ranges of 60-110 and 80-120. It is noted that if the recited minimum range values are 1 and 2, and the recited maximum range values are 3, 4, and 5, all of the ranges of 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5 are conceivable. In this application, unless otherwise stated, the numerical range "a-b" is an abbreviation representing all real number combinations between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed herein, with "0-5" being merely a shorthand for combinations of these numbers. Also, when a parameter is described as an integer ≧2, this is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0048] Unless otherwise stated, all the embodiments and optional embodiments in the present application may be combined with each other to form a new technical solution.
[0049] Unless otherwise stated, all technical features and optional technical features in the present application may be combined with each other to form a new technical solution.
[0050] Unless otherwise stated, all steps in the application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b) to mean that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method further includes step (c) as mentioned above to mean that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0051] Unless otherwise stated, the terms "comprise" and "comprises" referred to in this application may be open ended or closed ended. For example, the terms "comprise" and "comprises" may further include or include other components not listed, or may include or include only the listed components.
[0052] In this application, unless otherwise stated, the term "or" is inclusive. For example, the term "A or B" means "A, B, or both A and B." More specifically, "A or B" is satisfied by the condition where A is true (or exists) and B is false (or does not exist), the condition where A is false (or does not exist) but B is true (or exists), and the condition where both A and B are true (or exist).
[0053] In the description of this application, unless otherwise specified, "plurality" means two or more. The orientations or positional relationships indicated by the terms "up", "down", "left", "right", "inside", "outside", etc. are for the purpose of easily and simply describing this application, and do not indicate or imply that the devices or elements shown have a particular orientation and must be constructed and operated in a particular orientation, and should not be understood as limiting this application. The terms "first", "second", "third", etc. are merely for illustrative purposes and should not be understood as indicating or implying relative importance. "Perpendicular" is not strictly perpendicular, but is within a margin of error. "Parallel" is not strictly parallel, but is within a margin of error.
[0054] secondary battery
[0055] In some embodiments, the present application provides a secondary battery.
[0056] A secondary battery generally includes a positive electrode plate, a negative electrode plate, an electrolyte, and a separator. During the charging and discharging process of the battery, active ions shuttle between the positive electrode plate and the negative electrode plate to store and release. The electrolyte serves to conduct ions between the positive electrode plate and the negative electrode plate. The separator is provided between the positive electrode plate and the negative electrode plate, and mainly serves to prevent short-circuiting between the positive and negative electrodes, while also allowing ions to pass through.
[0057] [Negative plate]
[0058] The negative electrode plate generally includes a negative electrode current collector and a negative electrode film provided on at least one surface of the negative electrode current collector.
[0059] For example, the negative electrode current collector has two surfaces opposing each other in the thickness direction of the negative electrode current collector, and the negative electrode film is laminated on either one or both of the two opposing surfaces of the negative electrode current collector.
[0060] The negative electrode current collector may be made of a material having good electrical conductivity and mechanical strength to perform the functions of electrical conductivity and current collection. In some embodiments, the negative electrode current collector may be made of copper foil.
[0061] The negative electrode film contains a negative electrode active material.
[0062] In some embodiments, the present application provides an anode active material of artificial graphite. The artificial graphite is a PD 5t / PD 0.5t When the ratio is less than or equal to 1.35, the material has strong deformation resistance. During the cycling process of a lithium-ion battery, the negative electrode repeatedly absorbs and releases lithium, which causes expansion and contraction due to repeated forces. If the negative electrode has high deformation resistance, it will expand less during the cycling process and its structure will be more stable, resulting in better cycle performance.
[0063] This application is filed by P.D. 5t / PD 0.5t We found for the first time that PD can reflect the sensitivity of graphite density to pressure changes. 5t 5 tons (49000N The power of ) is the compacted density of the artificial graphite measured at a pressure of PD 0.5t 0.5 ton (4900N The power of ) is the compaction density of the artificial graphite measured at a pressure of 10 ... 5t / PD 0.5t We discovered that the expansion change of artificial graphite during the repeated lithium absorption and desorption process can be reflected by the PD of artificial graphite. 5t / PD 0.5t When ≦1.35, the swelling force during the cycling process is small, and the battery exhibits a low full charge swelling rate, and optionally, the battery further exhibits one or more advantages of high gram capacity, high first cycle cycling efficiency, good cycling performance, and long shelf life.
[0064] In some embodiments, the synthetic graphite has a PD of 1.23 or less. 5t / PD0.5t ≦1.3. For example, PD 5t / PD 0.5t may be 1.20 to 1.25, 1.25 to 1.30, or 1.30 to 1.35. When the artificial graphite satisfies this condition, the cycle performance of the battery is further improved.
[0065] In some implementations, the synthetic graphite is 5t ≧1.8g / cm 3 For example, 1.8 g / cm 3 ≦PD 5t ≦1.95g / cm 3 , 1.8g / cm 3 ≦PD 5t ≦1.85g / cm 3 , 1.85g / cm 3 ≦PD 5t ≦1.90g / cm 3 , 1.90g / cm 3 ≦PD 5t ≦1.95g / cm 3 By using the artificial graphite according to this method in a secondary battery, the energy density performance of the battery can be further improved.
[0066] In some implementations, the synthetic graphite is 0.5t ≧1.4g / cm 3 For example, 1.4 g / cm 3 ≦PD 0.5t ≦1.5g / cm 3 In some implementation plans, PD 0.5t The value is 1.4 to 1.45 g / cm 3 For example, 1.45 to 1.50 g / cm 3 By using the artificial graphite of this invention in a secondary battery, the energy density of the secondary battery can be further improved.
[0067] The compaction density of artificial graphite at a certain pressure is a known meaning in the art, and can be tested by adopting a method known in the art. For example, refer to GB / T 24533-2019, and use an electronic pressure tester (such as UTM7305) to test as follows: Place a pre-set mass M of the artificial graphite powder sample to be tested on a press mold (bottom area S), set different pressures (for example, 4900N and 49000N are adopted in this application), hold the pressure for 30s, remove the pressure, wait for 10s, read the thickness H of the powder after pressing at this pressure on the instrument, and calculate to obtain the compaction density at this pressure. The compaction density of the negative electrode active material at this pressure = M / (H*S).
[0068] In some embodiments, the median diameter Dv50 of the artificial graphite satisfies Dv50≧10 μm, for example, 19 μm≦Dv50≦22 μm. For example, 19 μm≦Dv50≦22 μm. In some embodiments, the median diameter Dv50 of the artificial graphite is 10-13 μm, for example, 13-16 μm, for example, 16-19 μm, for example, 19-22 μm. The use of the artificial graphite according to this embodiment in a secondary battery is advantageous in that the particle size can be reasonably controlled to prevent the negative electrode material from expanding too much, thereby further improving the dynamic performance and cycle performance of the battery.
[0069] Dv50 is the particle size when the cumulative volume distribution percentage of the artificial graphite reaches 50%, and can be tested by adopting a method known in the art. For example, it can be measured by adopting a laser diffraction particle size analysis method. Refer to the standard GB / T 19077-2016, and use a laser particle size analyzer (such as Malvern Master s ize r 3000).
[0070] In some embodiments, the specific surface area SSA of the artificial graphite is SSA≦1.5 g / m 2 For example, 1.0 g / m 2 ≦SSA≦1.4g / m 2In some embodiments, the specific surface area (SSA) of the artificial graphite is 1.0-1.2 g / m 2 For example, 1.2 to 1.4 g / m 2 For example, 1.4 to 1.5 g / m 2 The use of the artificial graphite according to this method in a secondary battery is advantageous in further improving the rapid charging ability of the battery, since the negative electrode has a sufficient active area for lithium absorption.
[0071] The specific surface area SSA of artificial graphite has a meaning known in the art, and can be tested by using a method known in the art. For example, it can be tested by using the nitrogen gas adsorption specific surface area analysis test method in accordance with the standard GB / T 19587-2017, and calculated by the BET (Brunauer Emmett Teller) method. Here, the nitrogen gas adsorption specific surface area analysis test is carried out by the Tr. iS tar II This can be done using a Model 3020 specific surface area pore size analyzer.
[0072] In some embodiments, the tap density of the synthetic graphite is 0.9 g / cm 3 For example, the tap density of artificial graphite is 1.0 g / cm 3 ~1.4g / cm 3 In some embodiments, the tap density of the artificial graphite is 0.9 to 1.1 g / cm 3 For example, 1.1 to 1.3 g / cm 3 The use of the artificial graphite according to this scheme in a secondary battery is advantageous for improving the compaction density of the negative plate, thereby further improving the energy density of the battery.
[0073] The tap density of artificial graphite has a meaning known in the art, and can be tested by adopting a method known in the art. For example, it can be measured by using a powder tap density tester, referring to the standard GB / T 5162-2006. For example, the FZS4-4B tap density tester of Beijing Iron and Steel Research Institute is used. The test parameters are as follows: 250±15 times / min, amplitude 3±0.2mm, vibration frequency 5000 times, measuring cylinder 25mL.
[0074] In some embodiments, the graphitization degree of the artificial graphite is 90% or more, for example 92% or more, for example 94% or more, for example 96% or more, for example 98% or more, for example 90-100%. The use of the artificial graphite according to this embodiment in a secondary battery further improves the performance of the secondary battery, and this embodiment is favorable for improving the graphite gram capacity and eliminating lattice defects, and therefore favorable for improving the cell energy density and storage performance.
[0075] The graphitization degree of artificial graphite is a known meaning in the art, and can be tested by adopting a method known in the art. For example, an X-ray diffraction apparatus (e.g., Bruker D8 Discover) can be used, and the test can refer to JIS K 0131-1996, JB / T 4220-2011, measure the size of d002, and calculate the graphitization degree according to the formula G=(0.344-d002) / (0.344-0.3354)×100%, where d002 is the interlayer distance in the graphite crystal structure expressed in nanometers (nm). In the X-ray diffraction analysis test, a copper target can be used as the anode target, and CuKα radiation can be used as the radiation source, with the radiation wavelength λ=1.5418Å, the scanning 2θ angle range being 20°-80°, and the scanning speed can be 4° / min.
[0076] In some embodiments, the gram capacity of the artificial graphite is 340 mAh / g or more, for example, 345-355 mAh / g. In some embodiments, the gram capacity of the artificial graphite is 340-345 mAh / g, for example, 345-350 mAh / g, for example, 350-355 mAh / g. By using the artificial graphite according to this embodiment in a secondary battery, the performance of the secondary battery is further improved.
[0077] The gram capacity of the artificial graphite is a known meaning in the art, and can be tested by adopting a method known in the art. For example, it can be tested according to the following method. The prepared artificial graphite, conductive agent Super P, adhesive (SBR), and thickener (CMC) are mixed in a suitable amount of deionized water with sufficient stirring according to a mass ratio of 96.2:0.8:1.8:1.2 to prepare a slurry. The prepared slurry is applied onto a copper foil current collector, and dried in an oven for use. A metallic lithium sheet is used as the counter electrode, a polyethylene (PE) film is used as the separator, ethylene carbonate (EC), methyl ethyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte. Here, the concentration of LiPF6 is 1 mol / L, and the above parts are assembled into a CR2430 type coin battery in a glove box protected by argon gas. The resulting coin battery is left to stand for 12 hours, then discharged at a constant current of 0.05 C to 0.005 V, left to stand for 10 minutes, discharged again at a constant current of 50 μA to 0.005 V, and charged at a constant current of 0.1 C to 2 V, and the charge capacity is recorded. The ratio of the charge capacity to the mass of the artificial graphite is the gram capacity of the artificial graphite.
[0078] In some embodiments, the present application provides a method for producing artificial graphite, the method comprising: (1) preparing a mixture of raw coke particles, calcined coke particles, an adhesive, and a solvent; (2) forming the mixture to obtain an intermediate; (3) removing at least some or all of the solvent from the intermediate to obtain a green compact; (4) subjecting the green body to a graphitization treatment to obtain a graphite matrix; and (5) powdering the graphite matrix to obtain artificial graphite.
[0079] Here, the artificial graphite is PD 5t / PD 0.5t ≦1.35, where PD 5t is the compacted density of the synthetic graphite measured at a pressure of 5 tons, and PD 0.5t is the compacted density of the synthetic graphite measured at a pressure of 0.5 tonnes.
[0080] In some implementations, step (1) includes mechanically stirring and mixing the raw coke particles, the calcined coke particles, and the adhesive, while adding an appropriate amount of a solvent and stirring to obtain a stirred product, which is a mud or adhesive particles (e.g., millimeter- or centimeter-scale adhesive particles).
[0081] The term "green coke" has its meaning as known in the art, e.g., green coke conforms to the provisions of NBSHT 0527-2019 Petroleum Coke (Green Coke).
[0082] In some implementations, the volatile matter content of the raw coke particles is ≧6wt%, for example, the content is ≧8wt%, for example, the content is 8wt%-12wt%. Based on this implementation, the raw coke particles can maintain the structural integrity of the green body by producing volatile matter with adhesive effect at 1000°C or higher. If the volatile matter content of the raw coke particles is lower, the adhesive effect of the graphite in the high-temperature graphitization stage is lower, and the strengthening effect is lower, in which case the PD 5t / PD 0.5t is big.
[0083] For testing the volatile content of raw coke, refer to "SHT0026-1990 - Method for measuring volatile content of petroleum coke."
[0084] In some implementations, the total mass of the raw coke particles, the calcined coke particles and the adhesive is 100%, and the content of the raw coke particles is 35wt% or more, for example, 35wt%-55wt%. According to this scheme, the amount of raw coke particles is sufficient to generate a suitable adhesive strength, and the structural integrity can be maintained during the graphitization process of the green body, and the artificial graphite obtained according to this scheme has low adhesive strength between particles and can be easily depolymerized into powder. If the content of raw coke particles is lower, the adhesive effect of graphite during the high-temperature graphitization stage will be low, and the reinforcing effect will be insufficient, in which case the PD 5t / PD 0.5t is big.
[0085] In some implementations, the median diameter Dv50 of the green coke particles is smaller than the median diameter Dv50 of the calcined coke particles. Based on this implementation, the green coke particles can be better filled into the gaps between the calcined coke particles, and can better play an adhesive role and maintain the structural integrity of the block matrix during the graphitization process. The Dv50 of the green coke is lower than the Dv50 of the calcined coke, in which case the green coke is more easily dispersed uniformly in the precursor, which has a more uniform adhesive effect, is favorable for maintaining a more uniform compressive stress, and has a more uniform reinforcing effect, thereby improving the PD 5t / PD 0.5t will be lower.
[0086] In some embodiments, the median diameter Dv50 of the raw coke particles is less than 15 μm, for example, 8-14 μm, so that the raw coke particles can better perform adhesive function and better maintain the structural integrity of the block matrix during the graphitization process.
[0087] The term "calcined coke" has its meaning as known in the art. The calcined coke conforms, for example, to YS T 625-2012 Calcined Petroleum Coke for Pre-baked Anodes.
[0088] In some embodiments, the median diameter Dv50 of the calcined coke particles is less than 20 μm, for example, 15-17 μm, so that the raw coke particles can better perform the adhesive function and better maintain the structural integrity of the block matrix during the graphitization process.
[0089] In some embodiments, the content of the calcined coke particles is more than 35 wt%, for example, 35 wt% to 62 wt%, which improves the performance of the artificial graphite.
[0090] In some implementations, the adhesive is vaporizable or decomposable above 1000° C. According to this implementation, the raw coke particles in the green body mainly bond at the high temperature stage above 1000° C., while the adhesive components mainly bond at the low temperature stage below 1000° C., so that the green body is effectively bonded throughout all temperature stages of graphitization and the structural integrity of the block matrix is maintained.
[0091] In some embodiments, the adhesive is a polymeric adhesive, which may include a water-soluble polymeric adhesive, a water-insoluble polymeric adhesive, or a combination thereof.
[0092] In some embodiments, the water-soluble polymer adhesive may include polyvinyl alcohol, starch, cellulose, or combinations thereof.
[0093] In some embodiments, the water insoluble polymer adhesive is selected from a rubber based adhesive, a thermoset based adhesive, or a combination thereof.
[0094] In some embodiments, the content of the adhesive is more than 2wt%, for example, 3wt%-10wt%, for example, the content of the adhesive is ≦6%, for example, the content of the adhesive is 2%-4%. According to this method, the amount of the adhesive is sufficient to generate sufficient adhesive strength, and the structural integrity during the graphitization process of the green body can be maintained. In addition, the artificial graphite obtained according to this method has a low residual carbon content of the adhesive, and the performance of the artificial graphite is good. The carbonization decomposition residue (residual carbon) of the adhesive belongs to hard carbon and is difficult to graphitize. When the residual carbon content of the artificial graphite is large, the specific surface area of the artificial graphite is improved, which reduces its capacity and the coulombic efficiency in the first cycle, and further reduces the energy density and cycle performance of the battery. If the content of the adhesive is low, the adhesive action between the coke particles is insufficient, making it difficult to maintain the compressive stress and the reinforcing effect insufficient, thereby making it difficult to improve the PD 5t / PD 0.5t will be larger.
[0095] In some embodiments, step (2) involves placing the mixture from the previous step into a molding machine and extruding or pressing it to form an intermediate body having a preset shape, which may be referred to as a wet body.
[0096] In some embodiments, step (3) includes drying the wet body to remove the solvent and obtain a green body.
[0097] In some embodiments, the apparent density of the green body is 1.3 g / cm 3 or more, for example 1.3 g / cm 3 ~1.5g / cm 3 ,1.35g / cm 3 ~1.45g / cm 3 Based on this method, the green body has sufficient strength at the graphitization stage, and the phenomenon of collapse and powdering does not occur. In addition, the graphite matrix obtained by this method has low interparticle adhesion and is easy to depolymerize into powder, and the obtained graphite powder has good performance. By using this graphite powder in a secondary battery, the secondary battery shows good cycle and storage performance.
[0098] In the above proposal, the apparent density affects the stability and internal stress of the green body. 3 or more, for example 1.3 g / cm 3 ~1.5g / cm 3 , 1.35g / cm 3 ~1.45g / cm 3 During the graphitization process, the graphite particles are strengthened under the action of stress, i.e., their deformation resistance ability is enhanced, so the PD of the obtained artificial graphite is 5t / PD 0.5t The value of PD is ≦1.35. The higher apparent density indicates tighter adhesion between coke particles, which leads to higher stress during the graphitization process, and thus the PD 5t / PD 0.5t will be lower and the cell performance will be better.
[0099] The test method for the apparent density of the green body is the drainage method. An example of the test method includes the following: Take one block-shaped adhesive precursor and weigh it, and its mass is m1. Add an appropriate amount of water to a beaker and weigh it, and its mass is m2. Tie the precursor with a thin copper wire (diameter <0.05 mm) whose volume is negligible, and place it in water, so that the precursor is submerged just below the water surface and does not come into contact with the bottom of the beaker, and the total mass of the beaker, water, and the precursor floating in the water is weighed to be m3. When the density of water is about 1 g / cm 3 where the density of the precursor is m / (m-m)g / cm 3 Ten samples are taken, measured, and the average value is calculated, which is the apparent density of the green body.
[0100] In some embodiments, the bulk density of the green body is 0.85 g / cm 3 For example, 0.45 to 0.85 g / cm 3 In some embodiments, the bulk density of the green body is 0.45 to 0.55 g / cm 3 For example, 0.55 to 0.65 g / cm3 For example, 0.65 to 0.75 g / cm 3 For example, 0.75 to 0.85 g / cm 3 According to this method, the degree of graphitization of the artificial graphite is high and the defects are few, and the secondary battery obtained based on this artificial graphite has better cycle performance and storage life. The bulk density of the green body is in the range of 0.45-0.85 g / cm 3 When the bulk density is too high, the resistivity is low, and according to Joule's law, the heat generated by the graphitization furnace is reduced. This leads to a lower graphitization temperature, but the lower the temperature, the weaker the strengthening effect of the coke particles, which leads to the poor PD 5t / PD 0.5t is larger. (The strengthening effect is mainly affected by the adhesive effect and temperature.)
[0101] For the test of the bulk density of the green body, refer to GB / T 14685-2011 Construction Pebbles and Crushed Stone, Chapter 7.13 Bulk Density and Porosity (Loose Bulk Density).
[0102] In some embodiments, the green body has at least one dimension that is ≧1 cm, such as 1-10 cm, such as 1-3 cm, such as 3-5 cm, such as 5-7 cm, such as 7-9 cm.
[0103] In some embodiments, the green body has at least two mutually perpendicular dimensions of ≧1 cm, such as 1-10 cm, such as 1-3 cm, such as 3-5 cm, such as 5-7 cm, such as 7-9 cm.
[0104] In some embodiments, all three mutually perpendicular dimensions of the green body are ≧1 cm, such as 1-10 cm, such as 1-3 cm, such as 3-5 cm, such as 5-7 cm, such as 7-9 cm.
[0105] In some implementations, the shape of the green body is selected from one or more of a cylindrical, spherical, ellipsoidal, and block-like shape, where a cylindrical, spherical, ellipsoidal, and block-like shape should be understood as an approximately cylindrical, approximately spherical, approximately ellipsoidal, and approximately block-like shape.
[0106] In some embodiments, step (4) includes placing the green body in a graphitization furnace and graphitizing the green body at 2800° C. or higher to obtain a graphite green body.
[0107] In some embodiments, step (5) includes crushing and / or grinding the graphite matrix, sieving (e.g., 200 mesh or larger, e.g., 200-400 mesh), and demagnetizing the graphite matrix to obtain artificial graphite powder.
[0108] In some embodiments, after the graphite body is crushed into powder, it is further subjected to one or more of the following operations: sieving, demagnetizing, and a combination thereof.
[0109] By using the artificial graphite produced above for the negative electrode film, the cycle performance of the battery can be effectively improved.
[0110] In some embodiments, the negative electrode film optionally further comprises other negative electrode active materials that can be applied to the negative electrode of the secondary battery. The other negative electrode active materials may be one or more of other graphite materials (e.g., other artificial graphite, natural graphite), mesocarbon microbeads (abbreviated as MCMB), hard carbon, soft carbon, silicon-based materials, and tin-based materials.
[0111] In some embodiments, the negative electrode membrane may further include an adhesive. Exemplarily, the adhesive may be selected from one or more of polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), styrene butadiene rubber (SBR), sodium alginate (SA), polymethyl methacrylate (PMAA), and carboxymethyl chitosan (CMCS).
[0112] In some embodiments, the negative electrode membrane optionally further comprises a thickener. Exemplarily, the thickener may be sodium carboxymethylcellulose (CMC-Na).
[0113] In some embodiments, the negative electrode film optionally further includes a conductive agent. Exemplarily, the conductive agent used in the negative electrode film may be selected from one or more of graphite, conductive carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0114] [Positive plate]
[0115] The positive electrode plate includes a positive electrode collector and a positive electrode film provided on at least one surface of the positive electrode collector. For example, the positive electrode collector has two surfaces facing each other in the thickness direction of the positive electrode collector, and the positive electrode film is provided by lamination on one or both of the two facing surfaces of the positive electrode collector.
[0116] The positive electrode current collector may be made of a material having good electrical conductivity and mechanical strength, and in some embodiments, may be made of aluminum foil.
[0117] The positive electrode film includes a positive electrode active material. In the present application, the specific type of the positive electrode active material is not specifically limited, and any active material that is known in the art and can be applied to the positive electrode of a secondary battery may be adopted, and those skilled in the art may select according to actual needs.
[0118] In some embodiments, the secondary battery may be a lithium-ion secondary battery. The positive electrode active material may be selected from lithium transition metal oxides and their modified materials, and the modified materials may be doped and / or coated lithium transition metal oxides. For example, the lithium transition metal oxide may be selected from one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and lithium-containing phosphates of an olivine structure.
[0119] Exemplarily, the positive electrode active material is LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523), LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811), LiNi 0.85 Co 0.15 Al 0.05 It may be selected from one or more of O2, LiFePO4 (LFP) and LiMnPO4.
[0120] In some embodiments, the positive electrode membrane optionally further includes an adhesive. There is no specific limitation on the type of adhesive, and those skilled in the art can select it according to actual needs. For example, the adhesive used in the positive electrode membrane may include one or more of polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE).
[0121] In some embodiments, the positive electrode film optionally further comprises a conductive agent. There is no specific limitation on the type of conductive agent, and those skilled in the art can select it according to actual needs. Exemplarily, the conductive agent used in the positive electrode film may include one or more of graphite, superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0122] [Electrolytes]
[0123] The electrolyte serves to conduct ions between the positive and negative plates. In the present application, the type of electrolyte is not specifically limited, and can be selected according to need. For example, the electrolyte may be selected from at least one of a solid electrolyte and a liquid electrolyte (i.e., an electrolyte solution).
[0124] In some embodiments, the electrolyte employs an electrolyte solution, the electrolyte solution including an electrolyte salt and a solvent.
[0125] In some embodiments, the electrolyte salt is LiPF6 (lithium hexafluorophosphate), LiBF4 (lithium tetrafluoroborate), LiClO4 (lithium perchlorate), LiAsF6 (lithium hexafluoroarsenate), LiFSI (lithium bis(fluorosulfonyl)imide), LiTFSI (lithium bis(trifluoromethanesulfonyl imide)), LiTFS (lithium trifluoromethanesulfonate), LiDFOB (difluoro(oxalate)), LiFSO (lithium tetrafluoroborate ... ) LiBOB (lithium borate), LiBOB (lithium bis(oxalato)borate), LiPO2F2 (lithium difluorophosphate), LiDFOP (lithium difluorobis(oxalato)phosphate) and LiTFOP (lithium tetrafluoro(oxalato)phosphate).
[0126] In some examples, the solvent may be selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), methyl ethyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfone (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS), and diethyl sulfone (ESE).
[0127] In some embodiments, the electrolyte solution optionally further includes an additive, for example, the additive may include an anode film-forming additive, may include a cathode film-forming additive, or may include an additive that can improve some performance of the battery, such as an additive that improves the overcharge performance of the battery, an additive that improves the high temperature performance of the battery, or an additive that improves the low temperature performance of the battery.
[0128] [Separator]
[0129] A separator is further included in secondary batteries using an electrolyte and in some secondary batteries using a solid electrolyte. The separator is disposed between the positive and negative plates and serves to isolate them. In the present application, there is no particular limitation on the type of separator, and any well-known separator with a porous structure having good chemical and mechanical stability may be selected. In some embodiments, the material of the separator may be selected from one or more of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single-layered thin film or a multi-layered composite thin film. When the separator is a multi-layered composite thin film, the materials of each layer may be the same or different.
[0130] [Exterior]
[0131] In some embodiments, the secondary battery may include an exterior for packaging the positive plate, the negative plate, and the electrolyte. As an example, the positive plate, the negative plate, and the separator may be stacked or rolled to form a stacked cell or a rolled cell, and the cell is packaged in the exterior, and the electrolyte may be an electrolyte solution, which permeates the cell. The number of cells in the secondary battery may be one or more, and can be adjusted according to demand.
[0132] In some embodiments, the exterior of the secondary battery may be a soft bag, for example, a bag-type soft bag. The material of the soft bag may be plastic, for example, may include one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc. The exterior of the secondary battery may be a hard case, for example, an aluminum case, etc.
[0133] [Secondary battery manufacturing method]
[0134] A method for manufacturing a secondary battery includes a step of manufacturing a negative plate by employing the artificial graphite of the present application.
[0135] In some embodiments, the step of manufacturing a negative electrode plate by employing the artificial graphite according to the first aspect of the present application may include dispersing a negative electrode active material including the artificial graphite according to the first aspect of the present application, an adhesive, and an optional thickener and conductive agent in a solvent such as deionized water to form a uniform negative electrode slurry, applying the negative electrode slurry onto a negative electrode current collector, and obtaining a negative electrode plate through processes such as drying and cold pressing.
[0136] The method for manufacturing a secondary battery may further include a step of manufacturing a positive electrode plate. In some embodiments, the positive electrode active material, the conductive agent, and the adhesive are dispersed in a solvent (e.g., N-methylpyrrolidone, abbreviated as NMP) to form a uniform positive electrode slurry, and the positive electrode slurry is applied onto a positive electrode current collector, and the positive electrode plate can be obtained through processes such as drying and cold pressing.
[0137] The method for manufacturing a secondary battery further includes assembling a negative plate, a positive plate, and an electrolyte to form a secondary battery. In some embodiments, the positive plate, a separator, and a negative plate are sequentially wound or stacked, and a separator is positioned between the positive plate and the negative plate to perform an isolating function to obtain a cell, which is then packaged, injected with an electrolyte, and sealed to obtain the secondary battery of the present application.
[0138] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, rectangular or any other shape. In Fig. 2, a secondary battery 5 having a rectangular structure is shown as an example.
[0139] In some embodiments, the secondary batteries can be assembled into a battery module, and the number of secondary batteries included in the battery module can be multiple, and the specific number can be adjusted based on the application and capacity of the battery module.
[0140] Fig. 3 shows an example of a battery module 4. Referring to Fig. 3, in the battery module 4, the multiple secondary batteries 5 may be arranged in order along the vertical direction of the battery module 4. Of course, they may be arranged in any other manner. Furthermore, the multiple secondary batteries 5 may be fixed with a fastener.
[0141] Optionally, the battery module 4 may further include a housing having an accommodation space in which the multiple secondary batteries 5 are accommodated.
[0142] In some embodiments, the above battery modules can be further assembled into a battery pack, and the number of battery modules included in the battery pack can be adjusted based on the application and capacity of the battery pack.
[0143] 4 and 5 show an example of a battery pack 1. Referring to Fig. 4 and Fig. 5, the battery pack 1 may include a battery case and a plurality of battery modules 4 provided in the battery case. The battery case includes an upper case 2 and a lower case 3, and the upper case 2 is provided to cover the lower case 3 and forms an enclosed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery case in any manner.
[0144] power consumption equipment
[0145] In some embodiments, the present application provides a power consuming device. The power consuming device includes at least one of a secondary battery, a battery module, or a battery pack provided by the present application. The secondary battery, the battery module, or the battery pack may be used as a power source for the power consuming device, or may be used as an energy storage unit for the power consuming device. The power consuming device may include, but is not limited to, a mobile device (e.g., a mobile phone, a laptop, etc.), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), a train, a ship, a satellite, an energy storage system, etc.
[0146] The power consumption device can be selected as a secondary battery, a battery module, or a battery pack according to its usage demand.
[0147] 6 shows an example of a power consuming device, such as a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. The power consuming device may employ a battery pack or a battery module to meet the demand for high power and high energy density for secondary batteries.
[0148] Another example of the device may be a mobile phone, a tablet computer, a notebook computer, etc. These devices are generally required to be lightweight and may employ a secondary battery as a power source.
[0149] Although the present application has been described in connection with the preferred embodiments, various improvements may be made thereto, and parts therein may be replaced with equivalents without departing from the scope of the present application. In particular, as long as there is no structural contradiction, each technical feature mentioned in each embodiment may be combined in any manner. The present application is not limited to the specific embodiments disclosed in the present specification, but includes all technical solutions within the scope of the claims.
[0150] Working Example
[0151] The following describes the examples of the present application. The examples described below are illustrative and are used only to interpret the present application, and should not be understood as limiting the present application. In the examples, specific techniques or conditions are not specified, but are carried out according to the techniques or conditions described in the technical literature or product instructions. For reagents or equipment used, those without the manufacturer are all common products that can be purchased commercially.
[0152] 1. Manufacturing of artificial graphite
[0153] Examples 1 to 7
[0154] In Examples 1 to 7, artificial graphite was produced using a graphitization furnace, and the production method included the following steps.
[0155] (1) Manufacturing of green bodies
[0156] table 1 The precursor composition is mixed according to the precursor blending method shown in Table 1, water is added and stirred until it becomes muddy, and the muddy material is extruded, granulated and molded, and then dried until the water content is less than 3% to obtain a green compact. Each green compact is cylindrical in shape and has dimensions of Φ15mm×4mm. The apparent density and bulk density of the green compact are shown in Table 1. 1 As shown in the figure.
[0157] (2) Artificial graphitization treatment
[0158] The green body produced in the previous step is subjected to a graphitization process, the peak temperature of which reaches 2800° C. The graphitization is carried out using equipment known in the art, such as a graphitization furnace, further for example an Acheson graphitization furnace.
[0159] (3)Powderization
[0160] Use a crusher to crush the graphite base into powder, then sieve the powder through a 325 mesh sieve and collect the powdered product that passes through the sieve. Use a demagnetizer to demagnetize the powdered product that passes through the sieve, so that the content of Fe+Co+Ni+Cr+Zn elements in the powdered product is <0.1ppm. Artificial graphite (powder) is obtained.
[0161] Comparative Examples 1 to 9
[0162] Comparative Example 1 3 The main difference between Example 1 and Example 2 is that the apparent density and / or bulk density of the green body are different, and the details are shown in Table 1. 1 As shown in the figure.
[0163] Comparative Example 4 ~ 11 The main difference between Example 1 and Example 2 is the method of compounding the precursors. 1 As shown in the figure.
[0164] two Analysis and Detection Items
[0165] Tests are conducted on the artificial graphite and the intermediate products of each step manufactured in the examples and comparative examples. The main test methods include the following.
[0166] The test method for the integrity (V2 / V1) of the green body substrate includes the following. Randomly take 20 green bodies, adopt the drainage method to test the total volume V1 of the 20 green bodies, and after graphitization treatment, randomly take 20 graphite substrates and adopt the drainage method to test the total volume V2 of the 20 graphite substrates. The value of V2 / V1 represents the degree of integrity of the substrate. When V2 / V1 ≥ 70%, the structure is well retained; when 30% < V2 / V1 < 70%, the degree of substrate integrity is normal; when V2 / V1 ≤ 30%, the degree of substrate integrity is severely deteriorated.
[0167] To further evaluate the performance of using the manufactured artificial graphite as the negative electrode active material of a secondary battery, a secondary battery is assembled using the above-mentioned manufactured artificial graphite and the battery performance test is conducted. The method of assembling the secondary battery includes the following.
[0168] (1) Manufacture of the positive electrode plate
[0169] LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), a conductive agent (acetylene black), and an adhesive (PVDF) are mixed according to a mass ratio of 96:2:2, and the solvent NMP is added and uniformly mixed to obtain a positive electrode slurry. The positive electrode slurry is uniformly coated on a positive electrode current collector (aluminum foil), dried, cold-pressed, and slit to obtain a positive electrode plate.
[0170] (2) Manufacture of the negative electrode plate
[0171] The artificial graphite powder of each example and comparative example, the conductive agent acetylene black, the thickener CMC, and the adhesive SBR are mixed in a mass ratio of 96.4:1:1.2:1.4, and deionized water is added as a solvent and mixed uniformly to obtain a negative electrode slurry. The negative electrode slurry is uniformly applied onto a negative electrode current collector (copper foil), and the negative electrode plate is obtained through drying, cold pressing, and slitting.
[0172] (3) Electrolyte
[0173] The solute of the electrolyte is 1 mol / L LiPF6 lithium salt, and the solvent is a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a volume ratio of 1:1:1.
[0174] (4) Separator
[0175] The separator is a polyethylene film.
[0176] (5) Manufacture of secondary batteries
[0177] The positive electrode plate, the separator, and the negative electrode plate are stacked in order, the separator is placed between the positive and negative electrodes, and the stack is then wound to obtain a bare cell. The bare cell is then placed in an outer case, an electrolyte is injected, and the cell is vacuum packaged, left to stand, formed, and otherwise processed to obtain a secondary battery.
[0178] The performance parameter test items of the secondary battery include:
[0179] (1) The cycle performance test includes the following: A cycle test is performed on the secondary battery at 25°C, at 1C, by fully charging and discharging it until the capacity of the secondary battery decays to 80% of the initial capacity, and the number of cycles is recorded.
[0180] (2) Expansion performance test includes the following: Before the negative plate is wound on the cell, the thickness of the negative plate is measured and set as h1. After the negative plate is wound on the cell to produce a secondary battery, the secondary battery is fully charged at 1C, and then the battery is disassembled, the negative plate is separated, and the thickness of the negative plate is measured and set as h2. In this case, the full charge expansion rate of the negative plate of the secondary battery is (h2-h1) / h1.
[0181] (3) The storage life test includes the following. First, a charge / discharge capacity test is performed on the secondary battery at 25°C as follows. After leaving it to stand for 2 hours at 25°C, the secondary battery is fully discharged at 0.33C, fully charged at 0.33C, and fully discharged at 0.33C again. The capacity of the second fully discharged battery is the capacity C0 of the secondary battery. The secondary battery is then left to stand and stored at 60°C, and taken out at regular intervals to perform a capacity test at 25°C. The capacity C after N days of storage is determined as the capacity of the secondary battery. N Record the capacity retention rate and calculate it as R = C N When R first becomes 0.8 or less, the number of days N of storage up to that point is recorded and this is the storage life of the secondary battery.
[0182] The precursor blending methods, green body parameters, and graphite base parameters of the examples and comparative examples are as follows: Table 1 As shown in the figure.
[0183] The parameters of the artificial graphite (powder) in the examples and comparative examples are: Table 2 As shown in the figure.
[0184] The performance of the secondary batteries assembled using artificial graphite as the negative electrode material in the examples and comparative examples is as follows: Table 2 As shown in the figure.
[0185] Analyzing the experimental data in Tables 1-2, the following experimental conclusions can be obtained:
[0186] (1)PD 5t / PD 0.5t About values
[0187] PD of artificial graphite in Examples 1 to 7 5t / PD 0.5t is ≦1.35, specifically between 1.28 and 1.31. 5t / PD 0.5t reflects the sensitivity of graphite density to pressure changes, where PD 5t is the compacted density of the synthetic graphite measured at a pressure of 5 tons, and PD 0.5t is the compaction density of the artificial graphite measured at a pressure of 0.5 tons. Graphite materials, as negative electrodes of secondary batteries, undergo similar changes in force during the process of repeated lithium absorption and release, so PD 5t / PD 0.5t can reflect the change in the expansion of graphite during the repeated lithium absorption and desorption process. PD 5t / PD 0.5t When the ratio is ≦1.35, the lithium ion negative electrode material has a small expansion force during the cycle process, which is favorable for improving the cycle performance. According to the experimental results of the battery test, when the graphite materials of Examples 1 to 7 are used as the negative electrode active materials of the secondary battery, the secondary battery exhibits one or more advantages of high gram capacity, high first cycle efficiency, good cycle performance, low full charge expansion rate, and long storage life.
[0188] (2) Apparent density of the green body
[0189] One important difference between Comparative Examples 1-2 and Examples 1-7 is the apparent density of the green bodies. The apparent density affects the stability and internal stress of the green bodies, and the apparent density of Examples 1-7 is 1.3 g / cm 3 or more, for example 1.3 g / cm 3 ~1.5g / cm 3 , 1.35g / cm 3 ~1.45g / cm 3 During the graphitization process, the graphite particles are strengthened under the action of stress, i.e., their deformation resistance ability is enhanced, so the PD of the obtained artificial graphite is 5t / PD 0.5tThe value of is ≦1.35. The experimental results show that the green bodies of Examples 1 to 7 are stable without structural collapse during the graphitization stage, and the integrity of the obtained graphite matrix is 98% or more. At the same time, the adhesive strength between the graphite particles after graphitization is low, depolymerization can be achieved with minor crushing, and there is no or very little damage to the graphite surface. According to the experimental results of the battery test, when the graphite materials of Examples 1 to 7 are used as the negative electrode active material of a secondary battery, the secondary battery exhibits one or more advantages of high gram capacity, high first cycle efficiency, good cycle performance, low full charge expansion rate, and long storage life.
[0190] The apparent density of the green body of Comparative Example 1 was 1.3 g / cm 3 The stress on the graphite particles is insufficient, the strengthening effect is insufficient, and the deformation resistance is insufficient (or weak), so the PD of the obtained artificial graphite is 5t / PD 0.5t The value of σ exceeds 1.35. The strength at the graphitization stage is insufficient, and the structure of the green body collapses and is easily pulverized, so the integrity of the graphite matrix is low. In addition, pulverization of the green body causes accumulation of powder, which makes it difficult to release volatile gases and poses the risk of explosion.
[0191] The apparent density of the green body of Comparative Example 2 was 1.45 g / cm 3 The graphitized particles are tightly bonded together, making them difficult to depolymerize into powder, or must be crushed with a strong force to be crushed into powder. Crushing with a strong force can cause many irreparable processing defects on the surface of the graphite, which makes the specific surface area of the graphite too high (3.05 g / m 2 Therefore, the PD of the obtained artificial graphite 5t / PD 0.5t The value of >1.35, which further reduces the cycle performance and storage performance of the secondary battery.
[0192] (3) Method of compounding precursors
[0193] The main difference between Comparative Examples 3 to 10 and Examples 1 to 7 is the method of blending the precursors, in which the raw coke component is advantageous for volatilizing volatile matters at a high temperature of 1000°C or higher and acts as an adhesive, while the adhesive component mainly acts to bond the coke particles at temperatures below 1000°C.
[0194] The green bodies obtained by the precursor blending methods of Examples 1 to 7 have high substrate integrity after graphitization and are easy to depolymerize, and the PD of the obtained artificial graphite powder 5t / PD 0.5t is ≦1.35 and is between 1.23 and 1.3.
[0195] In Comparative Example 3, if the bulk density of the green body is too high (1.00 g / cm 3 ), the resistivity is lower, and according to Joule's law, the heat generation rate of the graphitization furnace is reduced. Therefore, the graphitization temperature is lower. At lower temperatures, the strengthening effect of coke particles is weak, which leads to the PD 5t / PD 0.5t becomes larger (PD 5t / PD 0.5t = 1.39).
[0196] In Comparative Example 7, the mass fraction of raw coke is less than 35%, and the volatile content is low at the high temperature stage above 1000°C, the adhesive strength is insufficient, the block body is easily collapsed, and the integrity of the matrix is poor. If the content of raw coke particles is lower, the adhesive effect of graphite at the high temperature graphitization stage is low, and the reinforcing effect is insufficient. In this case, PD 5t / PD 0.5t is big.
[0197] In Comparative Example 8, the mass fraction of the raw coke is more than 55%, the volatile content is too high at the high temperature stage above 1000°C, the adhesion between particles is too strong, and it is difficult to depolymerize after graphitization.
[0198] In Comparative Example 9, the mass fraction of the adhesive is less than 3%, and when heated at a low temperature stage below 1000°C, the adhesive strength is low, the structure is not stable and is easily collapsed, and the integrity of the substrate is poor. If the content of the adhesive is low, the adhesive action between the coke particles is insufficient, the compressive stress is difficult to maintain, and the reinforcing effect is insufficient, so the PD 5t / PD 0.5t will be larger.
[0199] In Comparative Example 10, the mass fraction of the adhesive exceeds 10%, the residual carbon in the adhesive is large, and the performance of the graphite material is deteriorated.
[0200] In Comparative Example 11, the volatile content of the raw coke is less than 8%, and the structural integrity of the green body is not well maintained. If the volatile content of the raw coke particles is lower, the graphite will have a lower adhesive effect in the high-temperature graphitization stage, and the strengthening effect will be lower. In this case, the PD 5t / PD 0.5t is big.
[0201] 1(a) and 1(b) are scanning electron microscope photographs of the artificial graphite of an embodiment and a comparative example of the present application, respectively. As shown in FIG. 1(a), compared to the sample of the embodiment of the present invention, the raw material particles have a good adhesion effect during the graphitization process, so the particle size is larger, the particles have an irregular geometric shape, and there are fewer surface defects. As shown in FIG. 1(b), compared to the sample of the comparative example, the raw material particles have a poor adhesion effect during the graphitization process, so the particle size is smaller, and the particle shape is irregular.
[0202] The above experimental phenomena and rules compiled based on the experimental phenomena have all been discovered for the first time in this application, and a person skilled in the art could not have predicted them before filing the application. The technical effects of the artificial graphite produced in Examples 1 to 7 have all been discovered for the first time in this application, and a person skilled in the art could not have predicted them before filing the application.
Claims
1. Artificial graphite, The artificial graphite is PD 5t / PD 0.5t ≦1.35, where PD 5t is the compacted density of the artificial graphite measured by pressing it under a force of 5 tons and a circular area of 13 mm in diameter, PD 0.5t is the compaction density of the artificial graphite measured by pressing under a force of 0.5 tons and a circular area of 13 mm in diameter.
2. The artificial graphite has a PD of 1.23 or less. 5t / PD 0.5t 2. The artificial graphite according to claim 1, wherein the ratio of the stoichiometric ratio to the total stoichiometric ratio is ≦1.
3.
3. The artificial graphite is PD 5t ≧1.8 g / cm 3 The artificial graphite according to claim 1 or 2, which satisfies the above.
4. The artificial graphite has a density of 1.8 g / cm 3 ≦PD 5t ≦1.95 g / cm 3 The artificial graphite according to claim 1 or 2,
5. The artificial graphite is PD 0.5t ≧1.4 g / cm 3 The artificial graphite according to any one of claims 1 to 4, which satisfies the above.
6. The artificial graphite has a density of 1.4 g / cm 3 ≦PD 0.5t ≦1.5 g / cm 3 The artificial graphite according to any one of claims 1 to 4.
7. The artificial graphite according to any one of claims 1 to 6, wherein the median diameter Dv50 of the artificial graphite satisfies Dv50 ≧ 10 μm.
8. The artificial graphite according to any one of claims 1 to 6, wherein the median diameter Dv50 of the artificial graphite is 14 µm ≦ Dv50 ≦ 17 µm.
9. The specific surface area (SSA) of the artificial graphite is SSA≦1.5 g / m 2 The artificial graphite according to any one of claims 1 to 8, which satisfies the above.
10. The specific surface area (SSA) of the artificial graphite is 1.0 g / m 2 ≦SSA≦1.4g / m 2 The artificial graphite according to any one of claims 1 to 8.
11. The tap density of the artificial graphite is 0.9 g / cm 3 The artificial graphite according to any one of claims 1 to 10.
12. The tap density of the artificial graphite is 1.0 g / cm 3 ~1.4g / cm 3 The artificial graphite according to any one of claims 1 to 10.
13. The artificial graphite according to any one of claims 1 to 12, wherein the degree of graphitization of the artificial graphite is 90% or more.
14. The artificial graphite according to any one of claims 1 to 12, wherein the degree of graphitization of the artificial graphite is 94% or more.
15. The artificial graphite according to any one of claims 1 to 14, wherein the gram capacity of the artificial graphite is 340 mAh / g or more.
16. The artificial graphite according to any one of claims 1 to 14, wherein the gram capacity of the artificial graphite is between 345 mAh / g and 355 mAh / g.
17. A method for producing artificial graphite, comprising the steps of: (1) preparing a mixture of raw coke particles, calcined coke particles, an adhesive, and a solvent; (2) forming the mixture to obtain an intermediate; (3) removing at least a portion of the solvent from the intermediate to obtain a green body; (4) subjecting the green body to a graphitization treatment to obtain a graphite matrix; and (5) converting the graphite base into powder to obtain artificial graphite. Here, the mixture includes raw coke particles, calcined coke particles, and an adhesive, and the total mass of these is 100%, The content of the raw coke particles is 35 to 55 wt %, and the volatile matter content of the raw coke particles is 8 wt % to 12 wt %, The content of the adhesive is 3 wt % to 10 wt %, The apparent density of the green bodies is between 1.3 g / cm 3 and 1.5 g / cm 3 , and the bulk density of the green bodies is between 0.45 g / cm 3 and 0.85 g / cm 3 ; The artificial graphite is PD 5t / PD 0.5t ≦1.35, where PD 5t is the compacted density of the artificial graphite measured by pressing it under a force of 5 tons and a circular area of 13 mm in diameter, PD 0.5t is the compaction density of the artificial graphite measured by pressing the artificial graphite under a force of 0.5 tons and a circular area of 13 mm in diameter.
18. The green body is (1) the green body has a dimension in at least one direction of ≧1 cm; (2) the green body has at least two mutually perpendicular dimensions of ≧1 cm; (3) the green body has three mutually perpendicular dimensions that are all ≧1 cm; 18. The method of claim 17, further comprising one or more of the following characteristics: (4) the shape of the green body is selected from one or more of the following: cylindrical, spherical, ellipsoidal, and block-shaped.
19. The green body is (1) the green body has a dimension in at least one direction of 1 cm to 10 cm; (2) the green body has at least two mutually perpendicular dimensions of 1 cm to 10 cm; (3) the green body has three mutually perpendicular dimensions of 1 cm to 10 cm; (4) The method according to claim 17 or 18, wherein the shape of the green body is selected from one or more of the following: cylindrical, spherical, ellipsoidal, and block-like.
20. The method comprises: the median diameter Dv50 of the raw coke particles is smaller than the median diameter Dv50 of the calcined coke particles; - the raw coke particles have a median diameter Dv50 of 15 μm or less; The method according to any one of claims 17 to 19, wherein the method satisfies one or more of the following characteristics: - the median diameter Dv50 of the calcined coke particles is less than or equal to 20 μm.
21. The method comprises: the median diameter Dv50 of the raw coke particles is smaller than the median diameter Dv50 of the calcined coke particles; - the raw coke particles have a median diameter Dv50 of 8 μm to 14 μm; The method according to any one of claims 17 to 19, wherein the method satisfies one or more of the following characteristics: - the median diameter Dv50 of the calcined coke particles is between 15 μm and 17 μm.
22. The method according to any one of claims 17 to 21, wherein the adhesive is vaporizable or decomposable at 1000°C or higher.
23. the adhesive is a polymeric adhesive; the polymer adhesive comprises a water soluble polymer adhesive, a water insoluble polymer adhesive, or a combination thereof; the water-soluble polymer adhesive is selected from polyvinyl alcohol, starch, cellulose, or a combination thereof; The method of any one of claims 17 to 22, wherein the water insoluble polymer adhesive is selected from a rubber adhesive, a thermosetting resin adhesive, or a combination thereof.
24. A secondary battery comprising the artificial graphite according to any one of claims 1 to 16.
25. 25. A power consuming device comprising the secondary battery of claim 24.
Citation Information
Patent Citations
Electrode material and secondary battery
CN109704323A
Highly elastic graphite formed body and production thereof
JP1990283607A
Negative electrode active material for secondary batteries, electrode for secondary batteries containing the same, and secondary battery
JP2010522969A
Artificial graphite, secondary battery, manufacturing method and device
JP2022545912A
Composite graphite material, secondary battery, device, and preparation method
WO2021108987A1