Sclerosing compound product

The curable compound product with a specific formula addresses moldability and insulation issues by providing high solvent solubility and low-temperature moldability, ensuring stable film formation and excellent heat-resistant insulation.

JP7584651B2Active Publication Date: 2024-11-15DAICEL CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023528600
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-25
Publication Date
2024-11-15
Estimated Expiration
2040-12-25

AI Technical Summary

Technical Problem

Engineering plastics face challenges in moldability due to low solvent solubility and high processing temperatures, and curable compounds used for high-speed communications lack sufficient insulation properties and storage stability, leading to difficulties in film formation and thickening during storage.

Method used

A curable compound product with a specific formula (1) is developed, featuring high solvent solubility, low melt viscosity, and a ring closure rate of 97% or more, allowing for low-temperature melt molding and formation of cured products with excellent heat resistance and insulation properties.

Benefits of technology

The curable compound product achieves stable solutions for film formation, prevents thickening during storage, and forms cured products with superior heat resistance and insulation, suitable for applications requiring ultra-heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention provides a curable compound product that, when subjected to a heat treatment, forms a cured product having excellent heat resistance and high insulating properties. The curable compound product of the present disclosure contains a compound represented by the following formula (1), and the ratio of the group represented by the following formula (r-1) to the total of the group represented by the following formula (r-1) and the group represented by the following formula (r-2) is 97% or more. 1 , R 2 are the same or different and represent a group represented by the following formula (r-1) or a group represented by the following formula (r-2). 1 , D 2 are the same or different and represent a single bond or a linking group. L represents a divalent group having a repeating unit including a structure represented by the following formula (I) and a structure represented by the following formula (II). [Formula 1] TIFF2024502535000042.tif23152 [C2] TIFF2024502535000043.tif95156 [3] TIFF2024502535000044.tif42149
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a molded article including a curable compound product, or a cured or semi-cured product of the curable compound product. [Background technology]

[0002] Engineering plastics are plastics with improved heat resistance and mechanical properties, and are used as essential materials for making various parts smaller, lighter, more highly functional, and more reliable. However, engineering plastics need to be heated at high temperatures when melted and molded. In addition, engineering plastics have low solvent solubility, making them difficult to subject to solution cast molding. Therefore, the problem with engineering plastics is that they are not easily molded.

[0003] For example, the polyimide described in Patent Document 1 and the like has excellent heat resistance and strength properties, but is difficult to dissolve and melt, and therefore it is difficult to use it as a molding material for melt molding, solution cast molding, and the like, or as a matrix resin for composite materials.

[0004] Patent Document 2 describes a curable compound represented by the following formula, which describes that the compound can be melt molded at low temperatures and is solvent soluble, and therefore can form a cured product that has excellent moldability and ultra-heat resistance. [ka] [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2000-219741 A [Patent Document 2] International Publication No. 2019 / 244694 Summary of the Invention [Problem to be solved by the invention]

[0006] In addition, engineering plastics used as substrate materials for high-speed communication are also required to have insulating properties. However, as a result of the inventors' investigation of the curable compound described in Patent Document 2, it was found that the insulating properties were insufficient. It was also found that the storage stability in solution was insufficient and the viscosity increased over time. And, when the curable compound product was subjected to film molding by a solution casting method, the prepared solution was found to thicken during storage, making it difficult to mold it into a film.

[0007] Therefore, an object of the present disclosure is to provide a curable compound product that, when subjected to a heat treatment, forms a cured product having excellent heat resistance and high insulating properties. Another object of the present disclosure is to provide a curable compound product that has excellent storage stability in solution and that, when subjected to heat treatment, forms a cured product that has excellent heat resistance and high insulating properties. Another object of the present disclosure is to provide a curable compound product that has excellent moldability and storage stability in a solution, and that, when subjected to a heat treatment, forms a cured product that has excellent heat resistance and high insulating properties. Another object of the present disclosure is to provide a cured product having excellent heat resistance and high insulating properties, or a molded product including a semi-cured product thereof. Another object of the present disclosure is to provide a laminate having a configuration in which a cured product having excellent heat resistance and high insulating properties, or a semi-cured product thereof, is laminated onto a substrate. Another object of the present disclosure is to provide a cured product having excellent heat resistance and high insulating properties, or a composite material containing the semi-cured product thereof and fibers. Another object of the present disclosure is to provide an adhesive, sealant, or paint that has excellent storage stability in solution and that, when subjected to heat treatment, forms a cured product that has excellent heat resistance and high insulating properties.

[0008] In this specification, the term "product" refers to a product that is industrially manufactured and distributed in the market, and does not refer to a chemical substance itself. Therefore, the "curable compound product" of the present disclosure is an aggregate of a plurality of curable compounds, and in this sense, the "curable compound product" is a composition. [Means for solving the problem]

[0009] As a result of extensive investigations, the present inventors have found that a curable compound product containing a compound represented by the following formula (1) has the following properties. 1.Excellent solubility in solvents 2. When the ring closure rate of the imide bond is 97% or more, storage stability in solution is significantly improved. 3. Melting and forming at low temperatures is possible 4.Low melt viscosity 5.High heat generation starting temperature 6. When heated to a temperature equal to or higher than the heat generation initiation temperature, a cured product with excellent heat resistance and high insulating properties is obtained. The present disclosure has been completed based on these findings.

[0010] That is, the present disclosure relates to a compound represented by the following formula (1): [ka] [In the formula, R 1 , R 2 are the same or different and are a group represented by the following formula (r-1) or the following formula (r-2): [ka] (In the formula, Q represents C or CH. Two Qs in the formula are bonded via a single bond or a double bond. R 3 ~R 6 R may be the same or different and represent a hydrogen atom or a hydrocarbon group. 3 and R 4 may be bonded to each other to form a ring. n' represents an integer of 0 or more. 1 Or D 2 (Join to D 1 , D 2 are the same or different and each represents a single bond or a linking group. L represents a structure represented by the following formula (I) and a structure represented by the following formula (II) [ka] (In the formula, Ar 1 ~Ar 3 are the same or different and represent a group in which two hydrogen atoms have been removed from the structural formula of an aromatic ring, or a group in which two or more aromatic rings are bonded via a single bond or a linking group and two hydrogen atoms have been removed from the structural formula. The aromatic ring may have an alkyl group. X represents -CO-, -S-, or -SO2-, and Y is the same or different and represents -S-, -SO2-, -O-, -CO-, -COO-, or -CONH-. n represents an integer of 0 or more. It represents a divalent group having a repeating unit containing a structure represented by the following formula: 1 ~Ar 3 At least one of the Ar 1 ~Ar 3 At least one of the above is a group in which two hydrogen atoms have been removed from a structural formula in which two or more aromatic rings are bonded via a halogenated alkylene group. wherein the ratio of the groups represented by formula (r-1) to the total of the groups represented by formula (r-1) and the groups represented by formula (r-2) is 97% or more.

[0011] The present disclosure also relates to D in formula (1). 1 , D 2 are the same or different and are represented by the following formulas (d-1) to (d-4): [ka] The curable compound product is provided, wherein the group is selected from groups containing a structure represented by:

[0012] The present disclosure also relates to a method for measuring the viscosity (η0) of a 20% by weight NMP solution obtained by subjecting the curable compound product to a reduced pressure drying treatment and then dissolving it in NMP, and a method for measuring the viscosity (η) of the solution after allowing the solution to stand for 10 days in a desiccator maintained at 23°C. 10 ) satisfies the following formula (F): η 10 / η0<2 (F)

[0013] The present disclosure also provides the curable compound product, which has a weight average molecular weight of 1,000 to 10,000 in terms of standard polystyrene.

[0014] The present disclosure also provides the curable compound product, which has a glass transition temperature of 80 to 230°C.

[0015] The present disclosure also provides a molded article comprising a cured or semi-cured product of the curable compound product.

[0016] The present disclosure also provides a laminate having a configuration in which a cured or semi-cured product of the curable compound product is laminated on a substrate.

[0017] The present disclosure also provides a method for producing a laminate, comprising placing the curable compound product on a substrate and subjecting the substrate to a heat treatment to obtain a laminate having a structure in which a cured or semi-cured product of the curable compound product and the substrate are laminated together.

[0018] The present disclosure also provides a method for producing the laminate, which comprises applying a molten curable compound product onto a plastic support, solidifying the molten product, obtaining a thin film containing the curable compound product, peeling the obtained thin film from the support, laminating it on a substrate, and subjecting it to a heat treatment.

[0019] The present disclosure also provides a composite material comprising a cured or semi-cured product of the curable compound product and fibers.

[0020] The present disclosure also provides an adhesive comprising the curable compound product.

[0021] The present disclosure also provides a coating composition comprising the curable compound product.

[0022] The present disclosure also provides a sealant comprising the curable compound product. Effect of the Invention

[0023] The curable compound product of the present disclosure has excellent solvent solubility. When the curable compound product is dissolved in a solvent, a solution having a viscosity suitable for film formation by a solution casting method is obtained. The solution can be prevented from thickening for a long period of time and can be stored while maintaining the viscosity.

[0024] In addition, the curable compound product can be melt molded at low temperatures. The melt viscosity is low and the heat generation starting temperature is high. Therefore, when the curable compound product is subjected to melt molding, there is a high degree of freedom in setting the conditions during the molding process. In addition, the curable compound product can be prevented from hardening during injection into a mold or the like.

[0025] From the above, the curable compound product has excellent moldability, and the solution obtained by dissolving the curable compound product in a solvent has high storage stability. If the curable compound product is subjected to a heat treatment at a temperature equal to or higher than the heat generation initiation temperature, a cured product having excellent heat resistance and high insulating properties can be obtained.

[0026] Therefore, the curable compound products can be suitably used as adhesives, sealants, paints, etc. in fields where extreme heat resistance is required (e.g., electronic information devices, home appliances, automobiles, precision machinery, aircraft, space industry equipment, etc.). [Brief description of the drawings]

[0027] [Figure 1] FIG. 2 is a diagram showing the results of 1H-NMR measurement of the compound product (1-2) obtained in the example. [Diagram 2] FIG. 2 is a diagram showing the results of 1H-NMR measurement of the compound product (1-3) obtained in the example. [Diagram 3]FIG. 2 is a diagram showing the results of 1H-NMR measurement of the compound product (1-4) obtained in the example. [Figure 4] FIG. 2 is a diagram showing the results of 1H-NMR measurement of the compound product (1-6) obtained in the example. [Diagram 5] FIG. 2 is a diagram showing the results of 1H-NMR measurement of the compound product (1-9) obtained in the comparative example. [Figure 6] FIG. 2 is a diagram showing the results of DSC measurement of compound products (1-1), (1-2), (1-3), and (1-7) obtained in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] [Curable compound products] The curable compound product of the present disclosure includes a compound represented by formula (1): [ka] [In the formula, R 1 , R 2 are the same or different and represent a group represented by the following formula (r-1) or a group represented by the following formula (r-2). [ka] (In the formula, Q represents C or CH. Two Qs in the formula are bonded via a single bond or a double bond. R 3 ~R 6 R may be the same or different and represent a hydrogen atom or a hydrocarbon group. 3 and R 4 may be bonded to each other to form a ring. n' represents an integer of 0 or more. 1 Or D 2 (Join to

[0029] D 1 , D 2 are the same or different and each represents a single bond or a linking group. L represents a divalent group having a repeating unit including a structure represented by the following formula (I) and a structure represented by the following formula (II). However, all Ar 1 ~Ar 3At least one of the Ar 1 ~Ar 3 At least one of the above is a group in which two hydrogen atoms have been removed from a structural formula in which two or more aromatic rings are bonded via a halogenated alkylene group. [ka] (In the formula, Ar 1 ~Ar 3 are the same or different and represent a group in which two hydrogen atoms have been removed from the structural formula of an aromatic ring, or a group in which two or more aromatic rings are bonded via a single bond or a linking group and two hydrogen atoms have been removed from the structural formula. The aromatic ring may have an alkyl group. X represents -CO-, -S-, or -SO2-, and Y is the same or different and represents -S-, -SO2-, -O-, -CO-, -COO-, or -CONH-. n represents an integer of 0 or more.

[0030] In the above formulas (r-1) and (r-2), Q represents C or CH. Two Qs in the formula are bonded via a single bond or a double bond.

[0031] R 3 ~R 6 are the same or different and represent a hydrogen atom, a saturated or unsaturated aliphatic hydrocarbon group (preferably an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, or an alkynyl group having 2 to 10 carbon atoms), an aromatic hydrocarbon group (preferably an aryl group having 6 to 10 carbon atoms, such as a phenyl group or a naphthyl group), or a group formed by bonding two or more groups selected from the above-mentioned saturated or unsaturated aliphatic hydrocarbon groups and aromatic hydrocarbon groups.

[0032] R 3 and R 4may be bonded to each other to form a ring together with the adjacent carbon atom (Q in formulae (r-1) and (r-2)). Examples of the ring include an alicyclic ring having 3 to 20 carbon atoms and an aromatic ring having 6 to 14 carbon atoms. Examples of the alicyclic ring having 3 to 20 carbon atoms include a cycloalkane ring having about 3 to 20 members (preferably 3 to 15 members, particularly preferably 5 to 8 members) such as a cyclopropane ring, a cyclobutane ring, a cyclopentane ring, and a cyclohexane ring; a cycloalkene ring having about 3 to 20 members (preferably 3 to 15 members, particularly preferably 5 to 8 members) such as a cyclopentene ring and a cyclohexene ring; a perhydronaphthalene ring, a norbornane ring, a norbornene ring, an adamantane ring, a tricyclo[5.2.1.0 2,6 ] Decane ring, tetracyclo[4.4.0.1 2,5 .1 7,10 The aromatic ring having 6 to 14 carbon atoms includes a bridged cyclic hydrocarbon group such as a dodecane ring, etc. The aromatic ring having 6 to 14 carbon atoms includes a benzene ring, a naphthalene ring, etc.

[0033] n' is an integer of 0 or more, for example, an integer of 0 to 3, and preferably 0 or 1.

[0034] As the group represented by the above formula (r-1), a group selected from the groups represented by the following formulas (r-1-1) to (r-1-6) is preferable. [ka] (The bond extending from the nitrogen atom in the formula is D in formula (1). 1 Or D 2 (combined with

[0035] The groups represented by the formulae (r-1-1) to (r-1-6) may have one or more kinds of substituents bonded thereto. Examples of the substituents include an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, and a halogen atom.

[0036] Examples of the alkyl group having 1 to 6 carbon atoms include linear or branched alkyl groups such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a s-butyl group, a t-butyl group, a pentyl group, and a hexyl group.

[0037] Examples of the alkoxy group having 1 to 6 carbon atoms include linear or branched alkoxy groups such as a methoxy group, an ethoxy group, a butoxy group, and a t-butyloxy group.

[0038] Examples of the group represented by the above formula (r-2) include groups corresponding to the groups represented by the above formulae (r-1-1) to (r-1-6), which are formed by ring-opening of the imide bond in the groups represented by the above formulae (r-1-1) to (r-1-6).

[0039] As the group represented by the above formula (r-1) and the group represented by the above formula (r-2), a group represented by the following formula (r-1') and a group represented by the following formula (r-2') are particularly preferred. [ka] (In the formula, Q, R 3 , R 4 The bond marked with a wavy line in the formula is D. 1 Or D 2 (Join to

[0040] The group represented by the above formula (r-1) is particularly preferably a group selected from the groups represented by the above formulas (r-1-1) to (r-1-5) (= a group containing an imide bond), and particularly preferably a group represented by the above formula (r-1-1) or (r-1-5).

[0041] As the group represented by the above formula (r-2), among others, a group corresponding to the groups represented by the above formulae (r-1-1) to (r-1-5), in which the imide bond in the group represented by the above formulae (r-1-1) to (r-1-5) is ring-opened (= a group containing an amic acid structure), is preferred, and a group in which the imide bond in the group represented by the above formula (r-1-1) or (r-1-5) is ring-opened is particularly preferred.

[0042] In formula (1), D 1 , D 2 are the same or different and each represents a single bond or a linking group. Examples of the linking group include a divalent hydrocarbon group, a divalent heterocyclic group, a carbonyl group, an ether bond, an ester bond, a carbonate bond, an amide bond, an imide bond, and a group in which a plurality of these are linked together.

[0043] The divalent hydrocarbon group includes a divalent aliphatic hydrocarbon group, a divalent alicyclic hydrocarbon group, and a divalent aromatic hydrocarbon group.

[0044] Examples of the divalent aliphatic hydrocarbon group include linear or branched alkylene groups having 1 to 18 carbon atoms and linear or branched alkenylene groups having 2 to 18 carbon atoms. Examples of linear or branched alkylene groups having 1 to 18 carbon atoms include methylene, methylmethylene, dimethylmethylene, ethylene, propylene, and trimethylene. Examples of linear or branched alkenylene groups having 2 to 18 carbon atoms include vinylene, 1-methylvinylene, propenylene, 1-butenylene, and 2-butenylene.

[0045] Examples of the divalent alicyclic hydrocarbon group include divalent alicyclic hydrocarbon groups having 3 to 18 carbon atoms, such as cycloalkylene groups (including cycloalkylidene groups) such as a 1,2-cyclopentylene group, a 1,3-cyclopentylene group, a cyclopentylidene group, a 1,2-cyclohexylene group, a 1,3-cyclohexylene group, a 1,4-cyclohexylene group, and a cyclohexylidene group.

[0046] Examples of the divalent aromatic hydrocarbon group include arylene groups having 6 to 14 carbon atoms, such as a 1,4-phenylene group, a 1,3-phenylene group, a 4,4'-biphenylene group, a 3,3'-biphenylene group, a 2,6-naphthalenediyl group, a 2,7-naphthalenediyl group, a 1,8-naphthalenediyl group, and an anthracenediyl group.

[0047] The heterocycle constituting the divalent heterocyclic group includes aromatic heterocycles and non-aromatic heterocycles. Examples of such heterocycles include 3- to 10-membered rings (preferably 4- to 6-membered rings) having carbon atoms and at least one heteroatom (e.g., oxygen atom, sulfur atom, nitrogen atom, etc.) as atoms constituting the ring, and condensed rings thereof. Specifically, heterocycles containing an oxygen atom as a heteroatom (e.g., 3-membered rings such as oxirane ring; 4-membered rings such as oxetane ring; 5-membered rings such as furan ring, tetrahydrofuran ring, oxazole ring, isoxazole ring, γ-butyrolactone ring; 6-membered rings such as 4-oxo-4H-pyran ring, tetrahydropyran ring, morpholine ring; condensed rings such as benzofuran ring, isobenzofuran ring, 4-oxo-4H-chromene ring, chroman ring, isochroman ring; 3-oxatricyclo[4.3.1.1 4,8 ]Undecane-2-one ring, 3-oxatricyclo[4.2.1.0 4,8 ]nonan-2-one ring and other bridged rings), heterocycles containing a sulfur atom as a heteroatom (e.g., 5-membered rings such as thiophene ring, thiazole ring, isothiazole ring, thiadiazole ring, etc.; 6-membered rings such as 4-oxo-4H-thiopyran ring, etc.; condensed rings such as benzothiophene ring, etc.), heterocycles containing a nitrogen atom as a heteroatom (e.g., 5-membered rings such as pyrrole ring, pyrrolidine ring, pyrazole ring, imidazole ring, triazole ring, etc.; 6-membered rings such as isocyanuric ring, pyridine ring, pyridazine ring, pyrimidine ring, pyrazine ring, piperidine ring, piperazine ring, etc.; condensed rings such as indole ring, indoline ring, quinoline ring, acridine ring, naphthyridine ring, quinazoline ring, purine ring, etc.), etc. Divalent heterocyclic groups are groups obtained by removing two hydrogen atoms from the structural formula of the above heterocycle.

[0048] D 1 , D2 Among them, a group containing a divalent aromatic hydrocarbon group is preferable because it gives a cured product having particularly excellent heat resistance. The divalent aromatic hydrocarbon group is preferably a divalent aromatic hydrocarbon group having 6 to 14 carbon atoms, more preferably a group selected from the groups represented by the following formulas (d-1) to (d-4), particularly preferably a group represented by the following formula (d-1) (1,2-phenylene group, 1,3-phenylene group, or 1,4-phenylene group), and most preferably a 1,4-phenylene group. [ka]

[0049] In addition, the above D 1 , D 2 is preferably a group in which at least one group selected from the group consisting of a carbonyl group, an ether bond, an ester bond, a carbonate bond, an amide bond, and an imide bond is linked to the divalent aromatic hydrocarbon group, and in particular, a group in which an ether bond is linked to the divalent aromatic hydrocarbon group is preferred.

[0050] Therefore, R in Equation (1) 1 -D 1 - group, and R 2 -D 2 The - groups are, for example, the same or different, and are selected from the groups represented by the following formulas (rd-1'-1) to (rd-2'-2), and are particularly preferably the groups represented by the following formula (rd-1'-2) or (rd-2'-2). [ka] (In the formula, Q, R 3 , R 4 is the same as above)

[0051] In formula (1), L represents a divalent group having a repeating unit containing the structure represented by formula (I) above and the structure represented by formula (II) above.

[0052] Ar in the formula (I) and formula (II) 1 ~Ar3 are the same or different and each represents a group in which two hydrogen atoms have been removed from a structural formula of an aromatic ring, or a group in which two or more aromatic rings are bonded via a single bond or a linking group and two or more hydrogen atoms have been removed. The aromatic ring may have an alkyl group as a substituent.

[0053] L in formula (1) satisfies at least one of the following conditions 1 and 2. Condition 1: All Ar in L 1 ~Ar 3 At least one of the above is a group in which two hydrogen atoms have been removed from the structural formula of an aromatic ring having an alkyl group. Condition 2: All Ar in L 1 ~Ar 3 At least one of the above is a group in which two hydrogen atoms have been removed from a structural formula in which two or more aromatic rings are bonded via a halogenated alkylene group.

[0054] In the formula (II), n represents an integer of 0 or more, for example, an integer of 0 to 5, preferably an integer of 1 to 5, and particularly preferably an integer of 1 to 3.

[0055] Examples of the aromatic ring (= aromatic hydrocarbon ring) include aromatic rings having 6 to 14 carbon atoms, such as benzene, naphthalene, anthracene, and phenanthrene. Among these, aromatic rings having 6 to 10 carbon atoms, such as benzene and naphthalene, are preferred.

[0056] Examples of the alkyl group that the aromatic ring may have include alkyl groups having 1 to 6 carbon atoms. As the alkyl group, secondary alkyl groups having 3 to 6 carbon atoms (= alkyl groups having a tertiary carbon atom) or tertiary alkyl groups having 4 to 6 carbon atoms (= alkyl groups having a quaternary carbon atom) are preferred, and tertiary alkyl groups having 4 to 6 carbon atoms (= alkyl groups having a quaternary carbon atom) are particularly preferred, in that a cured product having high insulating properties can be obtained. Examples of the tertiary alkyl groups having 4 to 6 carbon atoms include t-butyl, t-pentyl, and t-hexyl groups.

[0057] The aromatic ring has, for example, 1 to 4 alkyl groups, preferably 2 to 4 alkyl groups, and particularly preferably 2 to 3 alkyl groups.

[0058] Examples of the linking group include a divalent hydrocarbon group having 1 to 5 carbon atoms, and a divalent hydrocarbon group having 1 to 5 carbon atoms in which one or more hydrogen atoms have been substituted with a halogen atom.

[0059] The divalent hydrocarbon group having 1 to 5 carbon atoms includes, for example, linear or branched alkylene groups having 1 to 5 carbon atoms, such as methylene, methylmethylene, dimethylmethylene, dimethylene, and trimethylene groups; linear or branched alkenylene groups having 2 to 5 carbon atoms, such as vinylene, 1-methylvinylene, and propenylene groups; linear or branched alkynylene groups having 2 to 5 carbon atoms, such as ethynylene, propynylene, and 1-methylpropynylene groups. Of these, linear or branched alkylene groups having 1 to 5 carbon atoms are preferred, and branched alkylene groups having 1 to 5 carbon atoms are particularly preferred.

[0060] The above-mentioned hydrocarbon group in which one or more hydrogen atoms have been substituted with halogen atoms is preferably a halogenated alkylene group having 1 to 5 carbon atoms, such as a bis(trifluoromethyl)methylene group.

[0061] The Ar 1 ~Ar 3 are preferably the same or different and selected from the groups represented by the following formulae (a-1) to (a-5). The aromatic ring in the following formula may have an alkyl group as a substituent. The attachment position of the bond in the following formula is not particularly limited. [ka]

[0062] Ar in formula (I) 1 , Ar 2 Among them, the group represented by the above formula (a-1) or (a-2) is preferable, and the group represented by the above formula (a-1) is particularly preferable.

[0063] Of these, -CO- is preferable as X.

[0064] Therefore, the structure represented by formula (I) is preferably a structure represented by the following formula (I'). [ka]

[0065] The structure represented by formula (I) preferably includes a structure derived from benzophenone.

[0066] The proportion of the structural unit derived from benzophenone in the total amount of the compound represented by the above formula (1) is, for example, 5% by weight or more, preferably 10 to 62% by weight, and particularly preferably 15 to 60% by weight.

[0067] All Ar contained in L in formula (I) 3 At least one of the above is preferably a group represented by the above formula (a-1) or (a-3) in which the aromatic ring has an alkyl group (preferably a secondary or tertiary alkyl group), or a group represented by the above formula (a-5), and particularly preferably a group represented by the above formula (a-1) in which the aromatic ring has an alkyl group (preferably a secondary or tertiary alkyl group), or a group represented by the above formula (a-5).

[0068] The Ar 3 may be a group represented by the above formula (a-1) or (a-3) in which the aromatic ring has an alkyl group (preferably a secondary or tertiary alkyl group) in combination with a group represented by the above formula (a-4) or (a-5).

[0069] Of these, -S-, -SO2-, -O-, or -CO- is preferable, -O- or -S- is particularly preferable, and -O- is particularly preferable.

[0070] Therefore, the structure represented by formula (II) preferably contains at least one structure selected from the following formulae (II'-1) to (II'-11), and particularly preferably contains at least one structure selected from the following formulae (II'-6) to (II'-9), in that a cured product having excellent insulating properties can be obtained. In the following formulae, the bond marked with a wavy line bonds to the structure represented by formula (I). [ka]

[0071] The structure represented by formula (II) may include a combination of at least one selected from the structures represented by formulas (II'-1) to (II'-10) above and a structure represented by formula (II'-11) above or a structure represented by formula (II'-12) above.

[0072] When the structure represented by formula (II) contains a combination of two types of structures as described above, and one of the structures is at least one structure selected from the above formulas (II'-6) to (II'-9), the other structure may be either the structure represented by the above formula (II'-11) or the structure represented by the above formula (II'-12).

[0073] When the structure represented by formula (II) contains a combination of two types of structures as described above, and one of the structures is at least one structure selected from the above formulas (II'-4), (II'-5), and (II'-10), it is preferable that the other structure is the structure represented by the above formula (II'-11), in that a cured product with excellent insulating properties can be obtained.

[0074] The proportion of the structural unit represented by formula (II) in the total amount of the compound represented by formula (1) is, for example, 5% by weight or more, preferably 10 to 55% by weight, and particularly preferably 15 to 53% by weight.

[0075] As L in formula (1), a divalent group represented by the following formula (L-1) is preferable, since it gives a cured product having particularly excellent heat resistance. [ka]

[0076] In the above formula (L-1), m is the number of repeating units shown in parentheses in the molecular chain (=divalent group represented by the above formula (L-1)), i.e., the average degree of polymerization, and is, for example, 2 to 50, preferably 3 to 40, more preferably 4 to 30, particularly preferably 5 to 20, and most preferably 5 to 10. When m is below the above range, the strength and heat resistance of the obtained cured product tend to be insufficient. On the other hand, when m is above the above range, the glass transition temperature tends to be high. In addition, the solvent solubility also tends to decrease. Furthermore, the melt viscosity of the curable compound product (= the viscosity when the curable compound product is melted) and the solution viscosity of the curable compound product (= the viscosity of the solution obtained by dissolving the curable compound product in a solvent) tend to be too high, and the molding processability tends to decrease. The value of m can be determined by GPC measurement or NMR spectrum analysis. In addition, n'' in the above formula (L-1) represents an integer of 0 or more. Ar 1 ~Ar 3 X and Y are the same as above. In addition, a plurality of Ar 1 represents the same group. 2 , Ar 3 The same applies to.

[0077] As L in formula (1), a divalent group represented by the following formula (L-1-1) is particularly preferable. 3 is the same as above. In the following formula, [-O-Ar 3 The group represented by —O— preferably contains at least one structure selected from the above formulae (II'-1) to (II'-11). [ka]

[0078] In the above formula, m1 is the number of repeating units shown in parentheses in the molecular chain represented by the above formula (L-1-1), i.e., the average degree of polymerization, and is, for example, 2 to 50, preferably 3 to 40, more preferably 4 to 30, particularly preferably 5 to 20, most preferably 5 to 10, and particularly preferably 5 or more and less than 10. The value of m1 can be determined by GPC measurement or NMR spectrum analysis.

[0079] If m1 is below the above range, the resulting cured product tends to be brittle and have poor mechanical properties, whereas if m1 is above the above range, the solubility in solvents tends to decrease, the melt viscosity tends to increase, and so on, resulting in poor moldability.

[0080] The ratio of the compound represented by the formula (1) in the total amount of the curable compound product is, for example, 80% by weight or more, preferably 90% by weight or more, more preferably 95% by weight or more, particularly preferably 98% by weight or more, most preferably 99% by weight or more, and particularly preferably 99.5% by weight or more. The upper limit is 100% by weight.

[0081] In all the compounds represented by the following formula (1) contained in the curable compound product, the ratio of the group represented by the formula (r-1) to the total of the group represented by the formula (r-1) and the group represented by the formula (r-2) (the ratio represented by the following formula, hereinafter sometimes referred to as the "ring closure ratio") is 97% or more. Therefore, the storage stability in solution is excellent. Ring closure rate=[number of moles of groups represented by the formula (r-1) / (number of moles of groups represented by the formula (r-1)+number of moles of groups represented by the formula (r-2)]×100

[0082] The ring closure rate of the curable compound product is preferably 98% or more, particularly preferably 98.5% or more, and most preferably 99% or more.

[0083] The number of moles of each group is: 1 It can be determined by calculation from the peak areas corresponding to each group in the H-NMR spectrum.

[0084] The number of moles of the group represented by formula (r-1) per gram of the curable compound product (hereinafter, sometimes referred to as the "functional group concentration") is, for example, 0.5 × 10 -4 ~20×10 -4 The upper limit of the functional group concentration is preferably 15×10 -4 moles / g, most preferably 10×10 -4 The lower limit of the functional group concentration is preferably 1.0×10 -4 moles / g, most preferably 1.5×10 -4 mol / g. When the functional group concentration of the curable compound product is within the above range, a cured product having excellent solvent solubility, toughness, and heat resistance can be formed. On the other hand, when the functional group concentration is below the above range, the solvent solubility tends to decrease. Also, when the functional group concentration is above the above range, it tends to be difficult to obtain a cured product having excellent toughness.

[0085] The functional group concentration of the curable compound product 1 It can be obtained by calculating the area of ​​each peak from the H-NMR spectrum and inputting the calculated value into the following formula. Functional group concentration = [peak area of ​​group represented by formula (r-1) / number of protons of group represented by formula (r-1)] / Σ [(each peak area / number of protons of group to which each peak belongs) × chemical formula weight corresponding to each peak]

[0086] Furthermore, the number of moles of the group represented by the formula (r-2) (=group containing an amic acid structure) per gram of the curable compound product (hereinafter, sometimes referred to as the "unclosed ring concentration") is, for example, 0.15 × 10 -4 mol / g or less, preferably 0.10×10 -4 moles / g or less.

[0087] The unclosed ring concentration is the concentration of the curable compound product. 1 It can be obtained by calculating the area of ​​each peak from the H-NMR spectrum and inputting the calculated value into the following formula. Unclosed ring concentration = (peak area of ​​group represented by formula (r-2) / number of protons of group represented by formula (r-2)) / Σ [(each peak area / number of protons of group to which each peak belongs) × chemical formula weight corresponding to each peak]

[0088] The number average molecular weight (Mn) of the curable compound product is, for example, 1000 to 15000. The lower limit of the number average molecular weight (Mn) is preferably 1500, more preferably 2000, particularly preferably 2200, most preferably 2600, and particularly preferably 2700. The upper limit of the number average molecular weight (Mn) is preferably 12000, more preferably 10000, still more preferably 7000, still more preferably 5000, particularly preferably 4000, and particularly preferably 3600.

[0089] The weight average molecular weight (Mw; standard polystyrene equivalent) of the curable compound product is, for example, 1000 to 15000. The lower limit of the weight average molecular weight (Mw) is preferably 2000, more preferably 2500, particularly preferably 3000, and most preferably 4000. The upper limit of the weight average molecular weight (Mw) is preferably 10000, more preferably 9000, still more preferably 8000, particularly preferably 7500, most preferably 7000, and particularly preferably 6500.

[0090] The proportion of the aromatic ring-derived structure in the total amount of the curable compound product is 50% by weight or more, preferably 60% by weight or more, and particularly preferably 65% ​​by weight or more. The upper limit of the proportion of the aromatic ring-derived structure is, for example, 95% by weight. Therefore, the curable compound product has high solvent solubility and low melt viscosity, and the cured product has high thermal stability. If the proportion of the aromatic ring-derived structure is below the above range, the thermal stability of the cured product tends to decrease. On the other hand, if the proportion of the aromatic ring-derived structure is above the above range, the solvent solubility tends to decrease, the melt viscosity tends to increase, and the moldability tends to decrease.

[0091] The nitrogen atom content of the curable compound product is, for example, 0.1 to 2.8% by weight, preferably 0.2 to 2.5% by weight, more preferably 0.25 to 2.0% by weight, and particularly preferably 0.3 to 1.8% by weight. The nitrogen atom content can be determined by CHN elemental analysis. A curable compound product having a nitrogen atom content in the above range can form a cured product having excellent solvent solubility, toughness, and heat resistance. On the other hand, if the nitrogen atom content is below the above range, it tends to be difficult to form a cured product having excellent toughness and heat resistance. Also, if the nitrogen atom content exceeds the above range, the solvent solubility tends to decrease.

[0092] Since the curable compound product has the above molecular weight, it is highly soluble in a solvent, and when dissolved in a solvent, a solution with a viscosity suitable for solution cast molding is obtained. In addition, the melt viscosity is low, and melt molding processing is easy. Furthermore, the obtained cured product (or molded product after curing) exhibits high toughness. If the number average molecular weight is below the above range, the toughness of the obtained cured product decreases, and it tends to become brittle and easily break when punching processing or the like is performed, and it tends to easily crack when drying. In addition, when subjected to melt press molding, there is a tendency for resin leakage from the mold to occur easily. On the other hand, if the number average molecular weight exceeds the above range, the solvent solubility decreases or the melt viscosity becomes too high, and molding processability tends to decrease. Incidentally, Mn and Mw are determined by gel permeation chromatography (GPC) measurement (solvent: chloroform, standard polystyrene conversion).

[0093] The solubility of the curable compound product in a solvent is 1 g or more, preferably 5 g or more, and particularly preferably 10 g or more per 100 g of solvent at 23° C. The solution obtained by dissolving the curable compound product in a solvent is cast into a film shape by a casting method, and cured to form a film-like cured product.

[0094] Examples of the solvent include chain ketones such as methyl ethyl ketone and methyl isobutyl ketone; cyclic ketones such as cyclohexanone and cycloheptanone; amides such as formamide, acetamide, N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide, and N,N-dimethylacetamide; halogenated hydrocarbons such as methylene chloride, chloroform, 1,2-dichloroethane, chlorobenzene, bromobenzene, dichlorobenzene, benzotrifluoride, and hexafluoro-2-propanol; sulfoxides such as dimethyl sulfoxide (DMSO), diethyl sulfoxide, and benzylphenyl sulfoxide; tetrahydrofuran (THF); aromatic hydrocarbons such as benzene, toluene (Tol), and xylene; and mixtures of two or more of these. The curable compound product exhibits excellent solubility in at least one solvent selected from ethers, chain ketones, cyclic ketones, amides, halogenated hydrocarbons, and sulfoxides.

[0095] In addition, the 20 wt% NMP solution obtained by subjecting the curable compound product to a drying treatment under reduced pressure and then dissolving it in NMP has a low viscosity and is suitable for solution cast molding. The viscosity (η0) of the 20 wt% NMP solution is, for example, 5 to 1000 mPa·s. The lower limit of the viscosity (η0) is preferably 10 mPa·s, particularly preferably 15 mPa·s. The upper limit of the viscosity (η0) is preferably 700 mPa·s, more preferably 500 mPa·s, even more preferably 300 mPa·s, even more preferably 200 mPa·s, even more preferably 150 mPa·s, even more preferably 100 mPa·s, particularly preferably 70 mPa·s, most preferably 50 mPa·s, and particularly preferably 40 mPa·s. If the viscosity (η0) is too low, it becomes difficult to mold a thick film, and if it is too high, it is likely to cause thickness unevenness and other molding defects.

[0096] The curable compound product has excellent storage stability in a solution. The curable compound product is subjected to a reduced pressure drying treatment, and then dissolved in NMP to obtain a 20 wt% NMP solution. The viscosity (η 10The viscosity (η 10 The lower limit of the viscosity (η 10 ) is preferably 1400 mPa·s, more preferably 1000 mPa·s, even more preferably 600 mPa·s, particularly preferably 400 mPa·s, most preferably 300 mPa·s, and especially preferably 200 mPa·s.

[0097] In addition, the viscosity (η0) and the viscosity (η 10 ) preferably satisfies the following formula (F). η 10 / η0<2 (F)

[0098] The viscosity (η0) and the viscosity (η 10 ) more preferably satisfies the following formula (F-1), and particularly preferably satisfies the following formula (F-2). η 10 / η0<1.75 (F-1) η 10 / η0<1.5 (F-2)

[0099] The viscosity (η0) and the viscosity (η 10 ) preferably satisfies the following formula (F-3). 1≦η 10 / η0<2 (F-3)

[0100] The viscosity of the NMP solution is measured at room temperature (e.g., 23°C) and normal pressure using an E-type viscometer. The reduced pressure drying treatment of the curable compound product is carried out until the residual moisture content in the curable compound product becomes 0.05% or less.

[0101] The 5% weight loss temperature (T d5 ) is 300°C or higher, preferably 400°C or higher, particularly preferably 450°C or higher, and most preferably 470°C or higher. d5) is, for example, 600°C, preferably 550°C, and particularly preferably 530°C.

[0102] The 10% weight loss temperature (T d10 ) is, for example, 410° C. or higher, preferably 460° C. or higher, particularly preferably 480° C. or higher, and most preferably 500° C. or higher. d10 ) is, for example, 600°C, preferably 550°C.

[0103] The 5% weight loss temperature and the 10% weight loss temperature can be determined by thermogravimetry (TGA) using a TG / DTA (thermogravimetry / differential thermal analyzer).

[0104] The glass transition temperature (Tg) of the curable compound product is, for example, 80 to 230° C. The upper limit of the glass transition temperature (Tg) is preferably 220° C., particularly preferably 200° C., and most preferably 185° C. The lower limit of the glass transition temperature (Tg) is preferably 90° C., particularly preferably 100° C. Tg can be determined by differential scanning calorimetry (DSC).

[0105] The curable compound product has a low glass transition temperature (Tg) as described above, and therefore has excellent moldability by melting. If the glass transition temperature (Tg) exceeds the above range, the moldability decreases because high temperature heating is required for melting. For example, when a composite material is produced by impregnating a molten curable compound product into fibers, the curing reaction of the curable compound product may progress, making it difficult to impregnate fine fibers.

[0106] The heat generation initiation temperature of the curable compound product is, for example, 220° C. or higher, preferably 230° C. or higher, more preferably 240° C. or higher, and particularly preferably 250° C. or higher. The upper limit of the heat generation initiation temperature is, for example, 300° C. The heat generation initiation temperature can be measured using a DSC at a temperature rise rate of 20° C. / min (in nitrogen).

[0107] When the curable compound product is heated at a temperature equal to or higher than the heat generation initiation temperature, it can be quickly cured to form a cured product having a highly crosslinked structure and having ultra-heat resistance. In addition, since the curing reaction does not proceed at a temperature lower than the heat generation initiation temperature, for example, when molding is performed, the curable compound product can be injected into a mold at a temperature lower than the heat generation initiation temperature while suppressing the thickening of the curable compound product, so that the injection work can be stabilized and molding can be performed with high precision.

[0108] The heating may be performed while maintaining a constant temperature, or may be performed by changing the temperature stepwise. The heating temperature can be appropriately adjusted according to the heating time. For example, when it is desired to shorten the heating time, it is preferable to set the heating temperature higher. Since the curable compound product has a high proportion of structures derived from aromatic rings, it can form a cured product (specifically, a cured product having ultra-heat resistance) without decomposition even when heated at a high temperature, and can form a cured product efficiently with excellent workability by heating at a high temperature for a short time. In addition, the heating means is not particularly limited, and known or commonly used means can be used.

[0109] In addition, when it is difficult to heat the curable compound product at a temperature equal to or higher than the heat generation initiation temperature, a polymerization initiator such as a radical polymerization initiator may be added to the curable compound product in an amount of about 0.05 to 10.0 parts by weight per 100 parts by weight of the curable compound product, which allows a cured product to be formed at a temperature lower than the heat generation temperature.

[0110] The curing of the curable compound product can be carried out under normal pressure, reduced pressure or increased pressure.

[0111] The curing reaction of the curable compound product is stopped midway through the heating temperature and heating time adjustment, and a semi-cured product (B stage) is obtained. The degree of curing of the semi-cured product is, for example, 85% or less (for example, 10 to 85%, particularly preferably 15 to 75%, and further preferably 20 to 70%).

[0112] The degree of curing of the semi-cured product can be calculated from the following formula by measuring the calorific value of the curable compound product and the calorific value of the semi-cured product by DSC. Degree of cure (%) = [1 - (heat generation amount of semi-cured product / heat generation amount of curable compound product)] x 100

[0113] The semi-cured product of the curable compound product can be temporarily fluidized by heating and can conform to uneven surfaces, and can be further heated to form a cured product with excellent heat resistance.

[0114] The glass transition temperature (Tg) of the cured product of the curable compound product is, for example, 160 to 250° C. The upper limit of the glass transition temperature is preferably 230° C., more preferably 220° C., and particularly preferably 210° C. The lower limit of the glass transition temperature is preferably 165° C., and particularly preferably 170° C. Tg can be measured by a DSC method.

[0115] The 5% weight loss temperature (T d5 ) is 300°C or higher, preferably 400°C or higher, particularly preferably 450°C or higher, and most preferably 500°C or higher. d5 ) is, for example, 600°C, preferably 550°C, and particularly preferably 530°C.

[0116] The 10% weight loss temperature (T d10 ) is, for example, 300° C. or higher, preferably 400° C. or higher, particularly preferably 480° C. or higher, and most preferably 500° C. or higher. d10 ) is, for example, 600°C, preferably 550°C.

[0117] The cured product of the curable compound has excellent insulating properties, and the relative dielectric constant and dielectric loss tangent are within the following ranges. The relative dielectric constant (εr) at a frequency of 10 GHz is, for example, 2.55 or less, preferably 2.50 or less, and particularly preferably 2.45 or less. The lower limit of the dielectric constant is, for example, 2.20. The dielectric tangent (tan δ) is, for example, 0.0045 or less (eg, 0.0001 to 0.0045) at a frequency of 10 GHz.

[0118] The "dielectric constant" and "dielectric loss tangent" are values ​​measured at a frequency of 10 GHz and a measurement temperature of 23° C. in accordance with the cavity resonance perturbation method ASTM D2520.

[0119] The elastic modulus of the cured product of the curable compound (measured according to a method in accordance with JIS K7161) is, for example, 1000 MPa or more (preferably 1150 MPa or more, and particularly preferably 1200 MPa or more).

[0120] The yield stress of the cured product of the curable compound (measured according to a method in accordance with JIS K7161) is, for example, 70 MPa or more (preferably 80 MPa or more).

[0121] The cured product of the curable compound has a breaking elongation (measured according to a method in accordance with JIS K7161) of, for example, 10% or more.

[0122] Since the curable compound product has the above-mentioned properties, it can be used as a molding material for composite materials used under severe environmental temperature conditions in electronic information devices, home appliances, automobiles, precision machinery, etc., as well as functional materials such as insulating materials and heat-resistant adhesives. In addition, it can be preferably used in sealants, paints, adhesives, inks, sealants, resists, forming materials [for example, forming materials for substrates, electrical insulating materials (insulating films, etc.), laminates, composite materials (fiber-reinforced plastics, prepregs, etc.), optical elements (lenses, etc.), photolithography, electronic paper, touch panels, solar cell substrates, optical waveguides, light guide plates, holographic memories, etc.], etc.

[0123] Since the curable compound product has the above-mentioned properties, it can be preferably used as a sealant for covering semiconductor elements in high heat-resistant and high voltage-resistant semiconductor devices (such as power semiconductors), which have been difficult to achieve with conventional resin materials.

[0124] In addition, since the curable compound product has the above-mentioned properties, it can be preferably used as an adhesive (for example, a heat-resistant adhesive used for stacking semiconductors in high heat-resistant and high voltage-resistant semiconductor devices (such as power semiconductors)).

[0125] In addition, since the curable compound product has the above-mentioned properties, it can be preferably used as a paint (solvent-based paint or powder paint) [for example, a paint (solvent-based paint or powder paint) for high heat-resistant and high voltage-resistant semiconductor devices (power semiconductors, etc.)].

[0126] [Manufacturing method of hardening compound products] The curable compound product may be, for example, a compound represented by the following formula (2): [ka] [In the formula, D 1 , D 2 are the same or different and each represents a single bond or a linking group. L represents a structure represented by the following formula (I) and a structure represented by the following formula (II) [ka] (In the formula, Ar 1 ~Ar 3 are the same or different and represent a group in which two hydrogen atoms have been removed from the structural formula of an aromatic ring, or a group in which two or more aromatic rings are bonded via a single bond or a linking group and two hydrogen atoms have been removed from the structural formula. The aromatic ring may have an alkyl group. X represents -CO-, -S-, or -SO2-, and Y is the same or different and represents -S-, -SO2-, -O-, -CO-, -COO-, or -CONH-. n represents an integer of 0 or more. It represents a divalent group having a repeating unit containing a structure represented by the following formula: 1 ~Ar3 At least one of the Ar 1 ~Ar 3 At least one of the above is a group in which two hydrogen atoms have been removed from a structural formula in which two or more aromatic rings are bonded via a halogenated alkylene group. and a compound represented by the following formula (3): [ka] (In the formula, Q represents C or CH. Two Qs in the formula are bonded via a single bond or a double bond. R 3 ~R 6 R may be the same or different and represent a hydrogen atom or a hydrocarbon group. 3 and R 4 may be bonded to each other to form a ring. n' represents an integer of 0 or more. The compound represented by the following formula (1) can be produced by reacting

[0127] When the compound represented by formula (2) is reacted with the compound represented by formula (3), the above-mentioned curable compound product is obtained through a two-stage reaction as shown in the following formula. 1 The substituent side is described, but D 2 The reaction proceeds similarly on the substituent side. 1 , D 1 , Q, R 3 ~R 6 , n' is the same as above. [ka]

[0128] The reaction can be carried out in the presence of a solvent. Examples of the solvent include N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone. These can be used alone or in combination of two or more.

[0129] <First stage> The first reaction step is a reaction in which the compound represented by formula (3) reacts with the NH2 group, which is the terminal group of the compound represented by formula (2), to convert the terminal group into a group represented by formula (r-2). 1 , R 2 is a group represented by formula (r-2).

[0130] The amount of the compound represented by formula (3) used is, for example, about 2.0 to 4.0 moles per mole of the compound represented by formula (2).

[0131] The above reaction can be carried out at room temperature (1 to 40° C.). The reaction time is, for example, about 1 to 30 hours. In addition, this reaction can be carried out by any method such as a batch method, a semi-batch method, or a continuous method.

[0132] In addition, it is preferable to select and use raw materials such as the compound represented by formula (2) and the compound represented by formula (3) that have a low alkali metal content, since this allows the production of a curable compound product having an alkali metal content of, for example, 500 ppm by weight or less (preferably 100 ppm by weight or less, particularly preferably 50 ppm by weight or less, and most preferably 35 ppm by weight or less). A curable compound product having an alkali metal content reduced to the above range can form a cured product having excellent heat resistance.

[0133] <Step 2: Ring-closing reaction> The second step reaction is a reaction in which the group represented by formula (r-2) of the terminal group is converted to a group represented by formula (r-1) by a ring-closing reaction. 1 , R 2 A compound in which at least one of the above is a group represented by formula (r-1) is obtained.

[0134] The above reaction can be promoted by heating at a temperature of 200° C. or higher or by adding a catalyst.

[0135] Among them, adding a catalyst is preferable because it can suppress the progress of the curing reaction while proceeding with the ring-closing reaction, and can provide a curable compound product with a high ring-closing rate and excellent storage stability in solution. As the catalyst, for example, a base catalyst, an acid catalyst, etc. can be used. As the catalyst, it is preferable to proceed with the reaction using an acid catalyst because it can suppress side reactions and produce a curable compound product in which the inclusion of side reaction products is suppressed.

[0136] Examples of the base catalyst include amine compounds, sodium acetate, etc. These may be used alone or in combination of two or more.

[0137] Examples of the acid catalyst include inorganic acids such as hydrochloric acid, hydrogen bromide, hydrogen iodide, sulfuric acid, sulfuric anhydride, nitric acid, phosphoric acid, phosphorous acid, phosphotungstic acid, and phosphomolybdic acid; sulfonic acids such as methanesulfonic acid, ethanesulfonic acid, trifluoromethanesulfonic acid, benzenesulfonic acid, and p-toluenesulfonic acid; carboxylic acids such as acetic acid and oxalic acid; halogenated carboxylic acids such as chloroacetic acid, dichloroacetic acid, trichloroacetic acid, fluoroacetic acid, difluoroacetic acid, and trifluoroacetic acid; solid acids such as silica, alumina, and activated clay; and cationic ion exchange resins. These can be used alone or in combination of two or more. As the acid catalyst, it is preferable to use at least one selected from p-toluenesulfonic acid, methanesulfonic acid, sulfuric acid, and phosphoric acid.

[0138] The amount of the base catalyst used is, for example, 0.02 to 1.0 mol, preferably 0.02 to 0.5 mol, and particularly preferably 0.05 to 0.4 mol, relative to 1 mol of the compound represented by the formula (3).

[0139] The amount of the acid catalyst used is, for example, 0.02 to 1.0 mol, preferably 0.05 to 0.5 mol, and particularly preferably 0.1 to 0.4 mol, relative to 1 mol of the compound represented by the formula (3).

[0140] The catalyst concentration in the reaction system is, for example, 0.003 to 0.10 mmol / g, preferably 0.005 to 0.07 mmol / g, and particularly preferably 0.007 to 0.04 mmol / g. If the amount of the catalyst used is below the above range, the ring closure rate of the curable compound product tends to decrease, and the storage stability in the solution tends to decrease with the decrease in the ring closure rate.

[0141] In the above reaction, it is preferable to quickly remove the water by-produced by the reaction from the reaction system in order to further promote the progress of the ring-closing reaction. Examples of methods for removing the by-produced water include a method using a dehydrating agent such as a carboxylic acid anhydride, and a method using a solvent that forms an azeotrope with water. In this case, the removal efficiency may vary depending on the shape and space volume of the reaction vessel, the piping layout, and the heat retention state.

[0142] However, when dehydration is performed using carboxylic acid acetic anhydride, a side reaction proceeds at the same time as the ring-closing reaction, and a large amount of side reaction products are generated. For example, when the reaction of a compound represented by formula (2) with maleic anhydride is performed while dehydration is performed using acetic anhydride, side reaction products represented by the following formulas (Ia) and (Ib) are generated together with the target compound represented by the following formula (I). If the side reaction products are mixed into the curable compound product, the exothermic start temperature tends to decrease. Therefore, when dehydration is performed using carboxylic acid anhydride, it is preferable to suppress the progression of side reactions by adjusting the amount of raw materials used and the method and speed of supplying the raw materials, and to thoroughly purify the product. In the following formula, D 1 , D 2 , L is the same as above. [ka]

[0143] When an acid catalyst is used, it is preferable to remove the water generated by the ring-closing reaction by azeotropy, for example, benzene, toluene, xylene, ethylbenzene, etc. as the azeotropic agent.

[0144] The ratio of the amount of the azeotropic agent to the amount of the solvent (the former / the latter; weight ratio) is preferably in the range of, for example, 25 / 75 to 45 / 55, in order to promote the progress of the reaction and to obtain the effect of improving the ring closure rate of the curable compound product.

[0145] The reaction is preferably terminated after confirming that the reaction has progressed sufficiently by, for example, sampling and checking the rate of ring closure.

[0146] After the reaction is completed, the reaction product obtained can be separated and purified by conventional methods such as precipitation, washing and filtration.

[0147] (Preparation of compound represented by formula (2)) Among the compounds represented by the above formula (2) used as raw materials for the curable compound product, for example, the compound represented by the following formula (2-1) can be produced via the following steps [1-1] and [1-2]. Step [1-1]: A compound represented by the following formula (4) is reacted with a compound represented by the following formula (5) in the presence of a base to obtain a compound represented by the following formula (6). Step [1-2]: reacting a compound represented by the following formula (6) with an amino alcohol (a compound represented by the following formula (7))

[0148] [ka]

[0149] In the above formula, Ar 1 ~Ar 3 , X, Y, and n are the same as above. D represents a linking group, D 1 , D 2 Examples of the linking group are the same as those in the formula (1). m is an average degree of polymerization of the repeating units, and is, for example, from 3 to 50, preferably from 4 to 30, and particularly preferably from 5 to 20. Z represents a halogen atom.

[0150] (Process [1-1]) Examples of the compound represented by the above formula (4) include benzophenone halides and derivatives thereof.

[0151] Examples of the compound represented by the above formula (5) include hydroquinone, resorcinol, catechol, 2,6-naphthalenediol, 2,7-naphthalenediol, 1,5-naphthalenediol, 4,4'-dihydroxybiphenyl, 2,5-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxybenzophenone, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl sulfone, bisphenol A (BisA), bisphenol F, bisphenol S, 4,4'-bis(trifluoromethyl)methylenebisphenol (BisAF), and derivatives thereof. These may be used alone or in combination of two or more.

[0152] Examples of the derivative include compounds in which a substituent is bonded to the aromatic hydrocarbon group of the compound represented by formula (4) or the compound represented by formula (5). Examples of the substituent include an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, and a halogen atom. Of these, the alkyl group is preferably a secondary alkyl group having 3 to 6 carbon atoms or a tertiary alkyl group having 4 to 6 carbon atoms.

[0153] The amount of the compound represented by formula (4) used is preferably adjusted according to the average degree of polymerization of the molecular chain in the desired compound represented by formula (6) within the range of 1 mole or more per mole of the compound represented by formula (5). For example, in the case of an average degree of polymerization of 5, it is preferable to use about 1.2 moles (e.g., 1.19 to 1.21 moles) of the compound represented by formula (4) per mole of the compound represented by formula (5), in the case of an average degree of polymerization of 10, it is preferable to use about 1.1 moles (e.g., 1.09 to 1.11 moles) of the compound represented by formula (4), and in the case of an average degree of polymerization of 20, it is preferable to use about 1.05 moles (e.g., 1.04 to 1.06 moles) of the compound represented by formula (4).

[0154] The reaction in step [1-1] is carried out in the presence of a base (for example, at least one selected from inorganic bases such as sodium hydroxide, potassium hydroxide, calcium hydroxide, sodium carbonate, potassium carbonate, and sodium hydrogen carbonate; and organic bases such as pyridine and triethylamine). The amount of the base used can be appropriately adjusted depending on the type of base. For example, the amount of a diacid base such as calcium hydroxide used is about 1.0 to 2.0 moles per mole of the compound represented by formula (5).

[0155] The reaction in step [1-1] can be carried out in the presence of a solvent, such as an organic solvent such as N-methyl-2-pyrrolidone, N,N-dimethylformamide, or dimethylsulfoxide, or a mixed solvent of two or more of these.

[0156] The amount of the solvent used is, for example, about 5 to 20 times by weight relative to the total weight of the compound represented by formula (4) and the compound represented by formula (5). If the amount of the solvent used exceeds the above range, the reaction rate tends to decrease.

[0157] The reaction atmosphere in the step [1-1] is not particularly limited as long as it does not inhibit the reaction, and may be, for example, a nitrogen atmosphere, an argon atmosphere, or the like.

[0158] The reaction temperature in the step [1-1] is, for example, about 100 to 200° C. The reaction time is, for example, about 3 to 24 hours. This reaction can be carried out by any method such as a batch method, a semi-batch method, or a continuous method.

[0159] After the reaction is completed, the reaction product obtained can be separated and purified by conventional methods such as precipitation, washing and filtration.

[0160] (Process [1-2]) Examples of the compound represented by the above formula (7) include 4-aminophenol, 2-amino-6-hydroxynaphthalene, and positional isomers and derivatives thereof. These can be used alone or in combination of two or more.

[0161] The amount of the compound represented by the above formula (7) used can be appropriately adjusted depending on the average degree of polymerization of the molecular chain in the desired compound represented by formula (2-1). For example, in the case of an average degree of polymerization of 5, the amount is about 0.4 to 0.6 mol per mol of the compound represented by formula (5), in the case of an average degree of polymerization of 10, the amount is about 0.2 to 0.4 mol per mol of the compound represented by formula (5), and in the case of an average degree of polymerization of 20, the amount is about 0.1 to 0.15 mol per mol of the compound represented by formula (5).

[0162] The reaction in step [1-2] is preferably carried out in the presence of a base. Examples of the base include inorganic bases such as sodium hydroxide, potassium hydroxide, calcium hydroxide, sodium carbonate, potassium carbonate, and sodium hydrogen carbonate; and organic bases such as pyridine and triethylamine. These may be used alone or in combination of two or more.

[0163] The amount of the base used can be appropriately adjusted depending on the type of base. For example, the amount of the monoacid base such as sodium hydroxide used is about 1.0 to 3.0 moles per mole of the compound represented by the above formula (7).

[0164] The reaction in step [1-2] can be carried out in the presence of a solvent, such as the same solvent as that used in step [1].

[0165] The reaction atmosphere in the step [1-2] is not particularly limited as long as it does not inhibit the reaction, and may be, for example, a nitrogen atmosphere, an argon atmosphere, or the like.

[0166] The reaction temperature in the step [1-2] is, for example, about 100 to 200° C. The reaction time is, for example, about 1 to 15 hours. This reaction can be carried out by any method such as a batch method, a semi-batch method, or a continuous method.

[0167] After the reaction is completed, the reaction product obtained can be separated and purified by conventional methods such as precipitation, washing and filtration.

[0168] In addition, the compound represented by the above formula (2-1) can also be produced by charging the compound represented by the above formula (4), the compound represented by the above formula (5), and the compound represented by the above formula (7) all at once and reacting them.

[0169] The curable compound product can also be produced by first obtaining a compound (8) in which the amino group (-NH2) of the compound represented by the above formula (7) is converted to the above formula (r-1) by a dehydrative imidization reaction between the compound represented by the above formula (7) and the compound represented by the above formula (3), and then charging the compound (8) with the compound represented by the above formula (4) and the compound represented by the above formula (5) all at once and reacting them. However, in this method, even if the compound (8) does not contain the above formula (r-2), the group represented by the above formula (r-1) is ring-opened by the water generated during the reaction to generate the group represented by the above formula (r-2). Therefore, even when producing by this method, it is preferable to carry out the reaction while removing the water generated in the reaction system, for example, by azeotropic dehydration, and it is preferable to stop the reaction after confirming that the reaction has progressed sufficiently by a method such as sampling and checking the ring closure rate.

[0170] [Curable composition] The curable composition of the present disclosure contains one or more of the above curable compound products. The content of the above curable compound products in the total amount of the curable composition (or the total amount of non-volatile content in the curable composition) (when two or more types are contained, the total amount) is, for example, 30% by weight or more, preferably 50% by weight or more, particularly preferably 70% by weight or more, and most preferably 90% by weight or more. The upper limit is 100% by weight. That is, the curable composition may consist of only the above curable compound products.

[0171] The curable composition may contain other components as necessary in addition to the curable compound product. Examples of other components include curable compounds other than the curable compound product, catalysts, fillers, organic resins (such as silicone resins, epoxy resins, and fluororesins), solvents, stabilizers (such as antioxidants, ultraviolet absorbers, light stabilizers, and heat stabilizers), flame retardants (such as phosphorus-based flame retardants, halogen-based flame retardants, and inorganic flame retardants), flame retardant assistants, reinforcing materials, nucleating agents, coupling agents, lubricants, waxes, plasticizers, release agents, impact resistance modifiers, hue modifiers, flow modifiers, colorants (such as dyes and pigments), dispersants, defoamers, defoamers, antibacterial agents, preservatives, viscosity modifiers, and thickeners. These may be used alone or in combination of two or more.

[0172] The curable composition may contain other curable compounds in addition to the curable compound product, but the ratio of the curable compound product to the total amount (100% by weight) of the curable compounds contained in the curable composition is, for example, 70% by weight or more, preferably 80% by weight or more, and particularly preferably 90% by weight or more. The upper limit is 100% by weight.

[0173] Since the curable compound product has excellent solvent solubility, the curable composition may be a solvent solution in which the curable compound product is dissolved in a solvent. The solvent is preferably a solvent in which the curable compound product has good solubility (for example, at least one solvent selected from ethers, chain ketones, cyclic ketones, amides, halogenated hydrocarbons, and sulfoxides), and particularly preferably at least one solvent selected from chain ketones, cyclic ketones, amides, and halogenated hydrocarbons.

[0174] Furthermore, even if the curable composition does not contain a crosslinking agent or a curing accelerator (even if the total content of the crosslinking agent and the curing accelerator in the total amount of the curable composition is, for example, 3% by weight or less, preferably less than 1% by weight), it can quickly form a cured product by heating at a temperature equal to or higher than the heat generation initiation temperature. If the total content of the crosslinking agent and the curing accelerator in the curable composition is within the above range, the content of unreacted curing accelerator and its decomposition products can be suppressed to an extremely low level, and therefore the resulting cured product can suppress the generation of outgassing derived from the crosslinking agent and the curing accelerator.

[0175] The curable composition can be rapidly cured by heating at a temperature equal to or higher than the heat generation initiation temperature to form a cured product having ultra-heat resistance and insulating properties. The heat treatment conditions can be appropriately set within the same range as the curing conditions for the above-mentioned curable compound product.

[0176] The curable composition can be suitably used as a molding material for composites (fiber reinforced plastics, prepregs, etc.) used under severe environmental temperature conditions in, for example, electronic information devices, home appliances, automobiles, precision machinery, aircraft, space industry equipment, the energy field (oil field drilling pipes / tubes, fuel containers), etc., as well as functional materials such as shielding materials, conductive materials (for example, heat conductive materials, etc.), insulating materials, adhesives (for example, heat resistant adhesives, etc.). In addition, it can be preferably used as a sealant, paint, ink, sealant, resist, modeling material, forming material [automotive parts such as thrust washers, oil filters, seals, bearings, gears, cylinder head covers, bearing retainers, intake manifolds, pedals, etc.; semiconductor and liquid crystal manufacturing equipment parts such as substrates, electrical insulating materials (insulating films, etc.), laminates, electronic paper, touch panels, solar cell substrates, optical waveguides, light guide plates, holographic memories, silicon wafer carriers, IC chip trays, electrolytic capacitor trays, insulating films, etc.; optical parts such as lenses; compressor parts such as pumps, valves, seals, etc.; aircraft cabin interior parts; medical equipment parts such as sterilization instruments, columns, piping, etc. and food and beverage manufacturing equipment parts; forming materials for electrical and electronic equipment parts such as housings used in personal computers and mobile phones, etc., and keyboard supports that are members that support the keyboard inside a personal computer], etc.

[0177] Since the curable composition has the above-mentioned properties, it can be preferably used as a sealant for covering semiconductor elements in high heat-resistant and high voltage-resistant semiconductor devices (such as power semiconductors), which have been difficult to achieve with conventional resin materials.

[0178] In addition, since the curable composition has the above-mentioned properties, it can be preferably used as an adhesive (for example, a heat-resistant adhesive used for stacking semiconductors in high heat-resistant and high voltage-resistant semiconductor devices (such as power semiconductors)).

[0179] In addition, since the curable composition has the above-mentioned properties, it can be preferably used as a paint (solvent-based paint or powder paint) [for example, a paint (solvent-based paint or powder paint) for high heat-resistant and high voltage-resistant semiconductor devices (power semiconductors, etc.)].

[0180] [Molded product] The molded product of the present disclosure includes a cured or semi-cured product of the curable compound product. The shape of the molded product is not particularly limited and can be appropriately selected depending on the application, and the molded product may be planar or three-dimensional. It may also be pellet-shaped or granular. The molded product can be produced by subjecting the curable compound product (or the curable composition) to a molding method such as injection molding, transfer molding, compression molding, or extrusion molding.

[0181] The molded product has excellent heat resistance. Therefore, it can be suitably used as a material to replace metals such as iron and aluminum in the fields of housing and construction, sports equipment, automobiles, and aerospace industries. When the molded product is a planar molded product (or a film-like molded product), it can be suitably used as an interlayer insulating film for electrical devices.

[0182] [Laminate] The laminate of the present disclosure has a configuration in which the cured or semi-cured product of the curable compound product is laminated on a substrate. The laminate includes a configuration of the cured or semi-cured product of the curable compound product / substrate, and a configuration of the substrate / cured or semi-cured product of the curable compound product / substrate.

[0183] Examples of materials for the substrate include semiconductor materials (eg, ceramics, SiC, gallium nitride, etc.), paper, coated paper, plastic films, wood, cloth, nonwoven fabrics, and metals (eg, stainless steel, aluminum alloys, copper).

[0184] The laminate has a structure in which a substrate is laminated via an adhesive layer containing the cured or semi-cured product of the curable compound product and having excellent heat resistance and adhesion to the substrate. The laminate can be suitably used as, for example, an electronic circuit board.

[0185] The laminate can be produced, for example, by placing the above-mentioned curable compound product on a substrate and subjecting it to a heat treatment.

[0186] The laminate can also be produced by applying a melt of the curable compound product onto a plastic support, solidifying it to obtain a thin film containing the curable compound product, peeling the obtained thin film from the support, laminating it on a substrate, and subjecting it to a heat treatment.

[0187] [Composite material] The composite material of the present disclosure includes a cured or semi-cured product of the curable compound product and fibers. The shape of the composite material is not particularly limited and may be fibrous or sheet-like.

[0188] Examples of the fibers include carbon fibers, aramid fibers, and glass fibers. These may be used alone or in combination of two or more. The fibers may be in the form of threads or may be processed into a sheet (woven or nonwoven fabric).

[0189] The composite material can be produced, for example, by impregnating fibers with a solution of the curable compound product in a solvent or a molten product of the curable compound product, and then subjecting the fibers to a heat treatment. The composite material obtained by semi-curing the impregnated curable compound product through the heat treatment can be suitably used as an intermediate product such as a prepreg.

[0190] The composite material has a structure in which the curable compound product is inserted into the voids of the fibers and cured, and is lightweight, high strength, and excellent in heat resistance. Therefore, it can be suitably used as a material to replace metals such as iron and aluminum in the fields of housing and construction, sports equipment, automobiles, and aviation and space industries. In addition, it can be suitably used as a material for firefighting clothing (fireproof clothing, activity clothing, rescue clothing, heat-resistant clothing), curtain, carpet material; separators such as separators for secondary batteries and separators for fuel cells; filters such as industrial filters, vehicle filters, and medical filters; space materials, etc.

[0191] The above-described components of the present disclosure and their combinations, etc. are merely examples, and additions, omissions, substitutions, and modifications of the components can be made as appropriate without departing from the gist of the present disclosure. Further, the present disclosure is not limited by the embodiments, but is limited only by the description in the claims.

Example

[0192] Hereinafter, the present disclosure will be described more specifically by way of examples, but the present disclosure is not limited to these examples.

[0193] In addition, the measurements were carried out under the following conditions. <NMR measurement> Measuring device: JEOL ECA500 or BRUKER AVANCE600MHz Measuring solvent: deuterated DMSO, deuterated chloroform, or a mixed solution of deuterated chloroform / pentafluorophenol (PFP) = 2 / 1 (wt / wt) Chemical shift: referenced to TMS <GPC measurement> Device: pump "LC-20AD" (manufactured by Shimadzu Corporation) Detector: RID-10A (manufactured by Shimadzu Corporation) or MODEL302TDA (manufactured by Viscotek), and UV2501 (manufactured by Viscotek) Solvent: THF or chloroform Column: Shodex KF-803 + Shodex KF802 + Shodex KF801×2 Flow rate: 1.0 mL / min Temperature: 40°C Sample concentration: 0.1% (wt / vol) Converted to standard polystyrene <DSC measurement> Device: TA Instruments Q2000 Heating rate: 20°C / min Atmosphere: nitrogen atmosphere <TGA measurement> Device: Seiko Instruments TG / DTA6200 Heating rate: 20℃ / min Atmosphere: Nitrogen atmosphere

[0194] Example 1 (Production of Compound (1-1)) (Process 1-1) In a reactor equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark apparatus, 70.00 g of 4,4'-difluorobenzophenone (DFBP), 30.52 g of bisphenol A (BisA), 32.39 g of 4,4'-dihydroxy-3,3',5,5'-tetramethylbiphenyl (TMP), 55.42 g of anhydrous potassium carbonate (K2CO3), 528.5 g of N-methylpyrrolidone (NMP), and 324.0 g of toluene (Tol) were placed, and the mixture was heated with stirring under a nitrogen atmosphere to reflux the toluene at 130-140°C for 4 hours. The mixture was then further heated to 170-180°C to distill off the toluene. Stirring was continued for 10 hours at 170-180°C, and the mixture was then returned to room temperature.

[0195] (Step 1-2) Then, 12.253 g of 4-aminophenol (4-AP), 15.518 g of anhydrous potassium carbonate (K2CO3), 50.8 g of N-methylpyrrolidone (NMP), and 397.8 g of toluene (Tol) were added to the reactor containing the reaction product, and the mixture was heated again under stirring in a nitrogen atmosphere to reflux the toluene at 130-140°C for 3 hours. Then, the mixture was heated to 170-180°C to distill off the toluene, and stirring was continued for 4 hours while maintaining the temperature. Then, the mixture was cooled to room temperature, and the reaction liquid was added to 3000 mL of methanol and filtered to obtain a powdery solid. This powdery solid was repeatedly washed with methanol and water, and then dried under reduced pressure at 80°C overnight to obtain a powdery solid, diamine-1 [Diamine-1, a compound represented by the following formula (Ar 3 : residues obtained by removing two hydroxyl groups from BisA, and residues obtained by removing two hydroxyl groups from TMP).

[0196] [ka]

[0197] (Process 2) In a reactor equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark apparatus, 100.00 g of the diamine-1 obtained in step 1, 11.94 g of maleic anhydride (MAH), 289.7 g of N-methylpyrrolidone (NMP), and 150.3 g of toluene (Tol) were placed and stirred at room temperature for 5 hours under a nitrogen atmosphere. Then, 1.934 g of p-toluenesulfonic acid (pTSA) was added as a catalyst, and the temperature was raised to 140°C, followed by stirring for 8 hours, and the toluene was refluxed to remove moisture. After the reaction solution was returned to room temperature, the reaction solution was added to 3000 mL of methanol to obtain a powdered solid. This powdered solid was repeatedly washed with methanol and water, and then dried under reduced pressure at 80°C overnight to obtain the compound product (1-1) (represented by the following formula (1-1), where Ar 3 is a repeating unit obtained by removing two hydroxyl groups from BisA, and Ar 3 The compound thus obtained had a repeating unit which is a residue obtained by removing two hydroxyl groups from TMP (101.5 g). The properties of the resulting compound product are shown in Table 2 below.

[0198] [ka]

[0199] Example 2 (Production of Compound (1-2)) Compound product (1-2) (represented by the above formula (1-1), where Ar 3 is a repeating unit obtained by removing two hydroxyl groups from BisA, and Ar 3 The compound thus obtained had a repeating unit which is a residue obtained by removing two hydroxyl groups from DAQ. The properties of the resulting compound product are shown in Table 2 below.

[0200] Example 3 (Production of Compound (1-3)) Compound product (1-3) (represented by the above formula (1-1), where Ar 3is a repeating unit obtained by removing two hydroxyl groups from BisA, and Ar 3 The compound thus obtained had a repeating unit which is a residue in which two hydroxyl groups have been removed from DBQ. The properties of the resulting compound product are shown in Table 2 below.

[0201] Example 4 (Production of Compound (1-4)) Compound (1-4) product (represented by the above formula (1-1), where Ar 3 The compound thus obtained had a repeating unit which is a residue in which two hydroxyl groups have been removed from BisAF. The properties of the resulting compound product are shown in Table 2 below.

[0202] Example 5 (Production of Compound (1-5)) Compound (1-5) product (represented by the above formula (1-1), where Ar 3 is a repeating unit obtained by removing two hydroxyl groups from BisAF, and Ar 3 The compound thus obtained had a repeating unit which is a residue obtained by removing two hydroxyl groups from TMP. The properties of the resulting compound product are shown in Table 2 below.

[0203] Example 6 (Production of Compound (1-6)) Compound (1-6) product (represented by the above formula (1-1), where Ar 3 is a repeating unit obtained by removing two hydroxyl groups from BisAF, and Ar 3 The compound thus obtained had a repeating unit which is a residue obtained by removing two hydroxyl groups from DAQ. The properties of the resulting compound product are shown in Table 2 below.

[0204] Comparative Example 1 (Production of Compound (1-7) Product) Compound (1-7) product (represented by the above formula (1-1), where Ar 3The compound thus obtained had a repeating unit in which two hydroxyl groups had been removed from BisA. The properties of the resulting compound product are shown in Table 2 below.

[0205] Comparative Example 2 (Production of Compound (1-8) Product) Compound (1-8) product (represented by the above formula (1-1), where Ar 3 The compound thus obtained had a repeating unit in which two hydroxyl groups had been removed from BisA. The properties of the resulting compound product are shown in Table 2 below.

[0206] Comparative Example 3 (Production of Compound (1-9) Product) Compound (1-9) product (represented by the above formula (1-1), where Ar 3 The compound thus obtained had a repeating unit in which two hydroxyl groups had been removed from BisA. The properties of the resulting compound product are shown in Table 2 below.

[0207] [Table 1]

[0208] The abbreviations in Table 1 are explained below. TMP: 4,4'-dihydroxy-3,3',5,5'-tetramethylbiphenyl DAQ: 2,5-di-t-pentylhydroquinone DBQ: 2,5-di-t-butylhydroquinone BisAF: 4,4'-bis(trifluoromethyl)methylene bisphenol

[0209] Regarding the compound products obtained in the examples and comparative examples, 1 The functional group concentration, unclosed ring concentration, and ring closure rate were calculated from the integrated intensity ratio of the H-NMR spectrum signals. The number average molecular weight and weight average molecular weight were determined by GPC measurement. Furthermore, the Tg and heat generation amount were determined by DSC measurement, and the 5% thermal weight loss temperature (T d5) was sought.

[0210] Compound products (1-2), (1-3), (1-4), (1-6), and (1-9) 1 The results of H-NMR measurement are shown in Figures 1 to 5.

[0211] FIG. 6 shows the results of DSC measurement of the compound products (1-1), (1-2), (1-3), and (1-7) obtained in the examples.

[0212] The storage stability of the resulting compound products in solution was evaluated by the following method. The compound products were dried under reduced pressure at 80° C. overnight and then cooled to room temperature in dry nitrogen before use as samples. A predetermined amount of the sample was weighed into a vial whose interior had been replaced with dry nitrogen, and NMP (reduced moisture content) was added to give a 20 wt % solution, to obtain a 20 wt % NMP solution. The obtained 20 wt% NMP solution was stored in a desiccator (temperature: 23°C) for 10 days, and the viscosity before storage (η0) and after storage (η 10 The storage stability was evaluated from the ratio of the viscosity to the viscosity at 23° C. using an E-type viscometer.

[0213] The solvent solubility of the resulting compound product was evaluated by the following method. The compound product (0.1 g) was mixed with N-methyl-2-pyrrolidone (NMP) or chloroform (10 g) and stirred at room temperature (23°C) for 24 hours to evaluate the solubility in the solvent. As a result, both were completely dissolved. The solvent solubility was good.

[0214] The results are summarized in Table 2 below. [Table 2]

[0215] [Melt press molding] Each compound product obtained in the Examples and Comparative Examples was filled into a molding die, set in a press (30-ton manual hydraulic vacuum press, IMC-462-3 model, manufactured by Imoto Machinery Co., Ltd.), and while drawing a vacuum, the temperature was raised from 50°C to 280°C at 20°C / min and held for 1 hour, and then the temperature was further raised to 320°C at 20°C / min and held for 30 minutes. The press was then cooled, and when the temperature reached 100°C or less, the molding die was removed, and a flat plate-shaped molded body (thickness: 1 mm) consisting of the cured product of the compound product was obtained.

[0216] The Tg of the obtained molded product was determined by DSC measurement.

[0217] The dielectric constant and dielectric loss tangent of the obtained molded article were measured by the following methods. <Measurement method> The molded body was cut to prepare a test piece with a width of 1.5 mm, and the relative dielectric constant and dielectric loss tangent were measured by the cavity resonator perturbation method (based on ASTM D2520) at a frequency of 10 GHz.

[0218] The results are summarized in Table 3 below. [Table 3]

[0219] In summary, the configuration of the present disclosure and its variations are set forth below. [1] The following formula (1) [ka] [In the formula, R 1 , R 2 are the same or different and are a group represented by the following formula (r-1) or the following formula (r-2): [ka] (In the formula, Q represents C or CH. Two Qs in the formula are bonded via a single bond or a double bond. R 3 ~R 6 R may be the same or different and represent a hydrogen atom or a hydrocarbon group. 3and R 4 may be bonded to each other to form a ring. n' represents an integer of 0 or more. 1 Or D 2 (Join to D 1 , D 2 are the same or different and each represents a single bond or a linking group. L represents a structure represented by the following formula (I) and a structure represented by the following formula (II) [ka] (In the formula, Ar 1 ~Ar 3 are the same or different and represent a group in which two hydrogen atoms have been removed from the structural formula of an aromatic ring, or a group in which two or more aromatic rings are bonded via a single bond or a linking group and two hydrogen atoms have been removed from the structural formula. The aromatic ring may have an alkyl group. X represents -CO-, -S-, or -SO2-, and Y is the same or different and represents -S-, -SO2-, -O-, -CO-, -COO-, or -CONH-. n represents an integer of 0 or more. It represents a divalent group having a repeating unit containing a structure represented by the following formula: 1 ~Ar 3 At least one of the Ar 1 ~Ar 3 At least one of the above is a group in which two hydrogen atoms have been removed from a structural formula in which two or more aromatic rings are bonded via a halogenated alkylene group. wherein the ratio of the groups represented by formula (r-1) to the total of the groups represented by formula (r-1) and the groups represented by formula (r-2) is 97% or more. [2] The curable compound product according to [1], wherein the group represented by formula (r-1) is a group selected from formulae (r-1-1) to (r-1-6), and the group represented by formula (r-2) is a group formed by ring-opening of an imide bond moiety of the group selected from formulae (r-1-1) to (r-1-6). [3] The curable compound product according to [1] or [2], wherein the group represented by the formula (r-1) is a group represented by the following formula (r-1'): [ka] (In the formula, Q, R 3 , R 4 The bond marked with a wavy line in the formula is D. 1 Or D 2 (Join to [4] The curable compound product according to any one of [1] to [3], wherein the group represented by the formula (r-2) is a group represented by the formula (r-2'). [ka] (In the formula, Q, R 3 , R 4 The bond marked with a wavy line in the formula is D. 1 Or D 2 (Join to [5] R in Equation (1) 1 -D 1 -group and R 2 -D 2 The curable compound product according to any one of [1] to [4], wherein the - groups are the same or different and are selected from the group consisting of formulas (rd-1'-1), (rd-1'-2), (rd-2'-1), and (rd-2'-2). [6] R in Equation (1) 1 -D 1 -group and R 2 -D 2 The curable compound product according to any one of [1] to [4], wherein the - groups are the same or different and are groups represented by the following formula (rd-1'-2) or the following formula (rd-2'-2): [ka] (In the formula, Q, R 3 , R 4 is the same as above) [7] The curable compound product according to any one of [1] to [6], wherein the structure represented by formula (II) comprises a combination of at least one structure selected from formulas (II'-1) to (II'-10) and a structure represented by formula (II'-11) or a structure represented by formula (II'-12). [8] The curable compound product according to any one of [1] to [7], wherein the structure represented by formula (II) comprises a combination of at least one structure selected from the following formulas (II'-6) to (II'-9) and a structure represented by the following formula (II'-11) or (II'-12): [ka] [9] The curable compound product according to any one of [1] to [8], wherein the structure represented by formula (II) comprises a combination of at least one structure selected from the following formulae (II'-4), (II'-5), and (II'-10) and a structure represented by the following formula (II'-11): [ka]

[10] D in Eq. (1) 1 , D 2 are the same or different and are selected from groups containing structures represented by formulas (d-1) to (d-4).

[11] After subjecting the curable compound product to a reduced pressure drying treatment, the viscosity of a 20% by weight NMP solution obtained by dissolving the product in NMP (η0) and the viscosity of the solution after standing for 10 days in a desiccator kept at 23°C (η 10 ) satisfies the following formula (F): η 10 / η0<2 (F)

[12] The viscosity (η0) and the viscosity (η 10 ) satisfies the following formula (F-1):

[0023]

[0024] The curable compound product according to any one of [1] to

[10] . η 10 / η0<1.75 (F-1)

[13] The viscosity (η0) and the viscosity (η 10) satisfies the following formula (F-2): η 10 / η0<1.5 (F-2)

[14] The viscosity (η0) and the viscosity (η 10 ) satisfies the following formula (F-4): 1≦η 10 / η0(F-4)

[15] The curable compound product according to any one of [1] to

[14] , which has a weight average molecular weight in terms of standard polystyrene of 1,000 to 10,000.

[16] The curable compound product according to any one of [1] to

[15] , which has a glass transition temperature of 80 to 230°C.

[17] A molded article comprising a cured or semi-cured product of the curable compound product according to any one of [1] to

[16] .

[18] A laminate having a configuration in which a cured or semi-cured product of the curable compound product according to any one of [1] to

[16] is laminated on a substrate.

[19] A method for producing a laminate, comprising placing the curable compound product according to any one of [1] to

[16] on a substrate and subjecting the substrate to a heat treatment to obtain a laminate having a structure in which a cured or semi-cured product of the curable compound product and the substrate are laminated together.

[20] A method for producing a laminate described in

[19] , comprising applying a molten curable compound product onto a plastic support, solidifying the molten product, obtaining a thin film containing the curable compound product, peeling the obtained thin film from the support, laminating the thin film on a substrate, and subjecting the substrate to a heat treatment.

[21] A composite material comprising a cured or semi-cured product of the curable compound product according to any one of [1] to

[16] and fibers.

[22] A method for producing a composite material, comprising: impregnating a fiber with a solvent solution of the curable compound product according to any one of [1] to

[16] or a molten product of the curable compound product; and subjecting the fiber to a heat treatment to produce a composite material containing a cured or semi-cured product of the curable compound product and a fiber.

[23] An adhesive comprising the curable compound product according to any one of [1] to

[16] .

[24] Use of the curable compound product according to any one of [1] to

[16] as an adhesive.

[25] A method for producing an adhesive, comprising producing an adhesive using the curable compound product according to any one of [1] to

[16] .

[26] A coating material comprising the curable compound product according to any one of [1] to

[16] .

[27] Use of the curable compound product according to any one of [1] to

[16] in a coating material.

[28] A method for producing a coating material, comprising producing a coating material using the curable compound product according to any one of [1] to

[16] .

[29] A sealant comprising the curable compound product according to any one of [1] to

[16] .

[30] Use of the curable compound product according to any one of [1] to

[16] as a sealant.

[31] A method for producing a sealant, comprising producing the sealant using the curable compound product according to any one of [1] to

[16] . [Industrial Applicability]

[0220] The curable compound product of the present disclosure has excellent moldability, and a solution obtained by dissolving the curable compound product in a solvent has high storage stability. When the curable compound product is subjected to a heat treatment at a temperature equal to or higher than the heat generation initiation temperature, a cured product having excellent heat resistance and high insulating properties is obtained. Therefore, the curable compound product can be suitably used as an adhesive, a sealant, a coating material, etc. in fields where extreme heat resistance is required.

Claims

1. The following formula (1) [Formula 1] [In the formula, R 1 , R 2 are the same or different and are a group represented by the following formula (r-1) or the following formula (r-2): [Case 2] (In the formula, Q represents C or CH. The two Qs in the formula are bonded via a single bond or a double bond. R 3 ~R 6 are the same or different and each represents a hydrogen atom or a hydrocarbon group. 3 and R 4 may be bonded to each other to form a ring. n' represents an integer of 0 or more. 1 Or D 2 (Binds to D represents a group represented by the formula: 1 , D 2 are the same or different and each represents a single bond or a linking group. L represents a group represented by the following formula (L-1-1): [C3] (In the formula, m1 represents the average degree of polymerization of the repeating unit shown in parentheses, and is 2 to 50. 3 are the same or different and are represented by the following formulas (a-1) to (a-5): [C4] The aromatic ring in the formulae (a-1) to (a-5) may have an alkyl group as a substituent. It represents a divalent group represented by the following formula: 3 at least one of the formulae (a-1) to (a-4) is a group having an alkyl group as a substituent on an aromatic ring in the formula, or a group represented by the formula (a-5). wherein the ratio of the group represented by formula (r-1) to the total of the group represented by formula (r-1) and the group represented by formula (r-2) is 97% or more.

2. D in formula (1) 1 , D 2 are the same or different and are represented by the following formulas (d-1) to (d-4): [C5] The curable compound product according to claim 1, wherein the group is selected from the group containing a structure represented by:

3. The curable compound product is subjected to a reduced pressure drying treatment, and then dissolved in NMP to obtain a 20 wt % NMP solution having a viscosity (η 0 ) and the viscosity (η 10 3. The curable compound product according to claim 1 or 2, wherein: η 10 / 0 <2 (F)

4. The curable compound product according to any one of claims 1 to 3, having a weight average molecular weight of 1,000 to 10,000 in terms of standard polystyrene.

5. The curable compound product according to any one of claims 1 to 4, having a glass transition temperature of 80 to 230°C.

6. A molded article comprising a cured or semi-cured product of the curable compound product according to any one of claims 1 to 5.

7. A laminate having a configuration in which a cured or semi-cured product of the curable compound product according to any one of claims 1 to 5 is laminated on a substrate.

8. A method for producing a laminate, comprising placing the curable compound product according to any one of claims 1 to 5 on a substrate and subjecting the substrate to a heat treatment to obtain a laminate having a structure in which a cured or semi-cured product of the curable compound product and the substrate are laminated together.

9. 9. The method for producing a laminate according to claim 8, comprising applying a melt of the curable compound product onto a plastic support, solidifying the melt, obtaining a thin film containing the curable compound product, peeling the obtained thin film from the support, laminating the thin film on a substrate, and subjecting the substrate to a heat treatment.

10. A composite material comprising a cured or semi-cured product of the curable compound product according to any one of claims 1 to 5 and fibers.

11. An adhesive comprising the curable compound product according to any one of claims 1 to 5.

12. A coating material comprising the curable compound product according to any one of claims 1 to 5.

13. A sealant comprising the curable compound product according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Terminally modified imide oligomer and its cured item

    JP2000219741A

  • biomaterial

    JP2019217048A

  • Fiber having super heat resistance, and cloth

    JP2019218659A

  • Aromatic polymer blends and adducts obtained therefrom - Patent Application 20070122997

    JP2020509140A

  • Curable compound

    WO2019244694A1