Manufacturing method of filter for solid-state imaging device, manufacturing method of solid-state imaging device, and filter for solid-state imaging device
The method for manufacturing a solid-state image sensor filter addresses the issue of dye elution by using a dry etching process with precise thickness and height controls, along with an etching stopper and oxygen blocking layer, enhancing the sensor's functionality and spectral performance.
Patent Information
- Application Number
- JP2020142710
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-26
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-08-26
AI Technical Summary
The miniaturization of pixel sizes in solid-state image sensors poses a challenge for infrared light cut filters, as the stripping liquid used to remove the resist pattern during dry etching can elute infrared light-absorbing dye, degrading the functionality of the sensor.
A method for manufacturing a filter for a solid-state image sensor involves forming an infrared light pass filter and color filters on a semiconductor substrate, followed by a dry etching process to create an infrared light cut filter, with specific thickness and height differences, and incorporating an etching stopper layer and oxygen blocking layer to prevent dye elution.
This method suppresses functional deterioration of the solid-state imaging device by preventing the elution of infrared light-absorbing dye, ensuring uniform microlens heights and maintaining spectral performance across various pixel sizes.
Smart Images

Figure 0007585663000001 
Figure 0007585663000002 
Figure 0007585663000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a filter for a solid-state image sensor. , solid Manufacturing method of body imaging device , and a filter for a solid-state image sensor Regarding. [Background technology]
[0002] Solid-state imaging devices such as CMOS image sensors and CCD image sensors include photoelectric conversion elements that convert the intensity of light into an electrical signal. Solid-state imaging devices can detect light corresponding to a plurality of colors, for example. Some solid-state imaging devices include color filters for each color and photoelectric conversion elements for each color, and detect light for each color using the photoelectric conversion elements for each color (see, for example, Patent Document 1). Other solid-state imaging devices include organic photoelectric conversion elements and inorganic photoelectric conversion elements, and detect light of each color using each photoelectric conversion element without using a color filter (see, for example, Patent Document 2).
[0003] Some solid-state imaging devices are provided with an infrared light cut filter on a photoelectric conversion element. In this type of solid-state imaging device, the infrared light absorbing pigment in the infrared light cut filter absorbs infrared light, thereby cutting off infrared light that can be detected by each photoelectric conversion element to the photoelectric conversion element. This improves the detection accuracy of visible light in each photoelectric conversion element. For example, some infrared light cut filters contain a cyanine pigment that is an infrared light absorbing pigment (see, for example, Patent Document 3). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2003-060176 A [Patent Document 2] JP 2018-060910 A [Patent Document 3] JP 2007-219114 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, with the miniaturization of pixel size in solid-state imaging devices, miniaturization of infrared cut filters is required. Miniaturization of infrared cut filters is realized by dry etching using a resist pattern formed on the infrared cut filter. In patterning of an infrared cut filter using dry etching, a resist pattern is first formed on the infrared cut filter. Next, the infrared cut filter is etched using the resist pattern, and then the resist pattern is peeled off from the infrared cut filter. The stripping solution used to peel off the resist pattern from the infrared cut filter may dissolve a part of the infrared light absorbing dye contained in the infrared cut filter to the outside of the infrared cut filter by contacting the infrared cut filter. This may cause the function of the solid-state imaging device to deteriorate.
[0006] The present invention aims to provide a method for manufacturing a filter for a solid-state imaging device, which is capable of suppressing functional degradation caused by partial elution of the infrared light absorbing dye contained in the infrared light cut filter, and a method for manufacturing a solid-state imaging device. [Means for solving the problem]
[0007] One embodiment of a method for manufacturing a filter for a solid-state imaging device to solve the above problem includes the steps of forming at least one color filter of red (R), green (G), and blue (B) and an infrared light pass filter on a semiconductor substrate, forming an infrared light cut precursor layer on the semiconductor substrate on which the at least one color filter of red (R), green (G), and blue (B) and the infrared light pass filter have been formed, and forming the infrared light cut filter on the color filter by dry etching the infrared light cut precursor layer.
[0008] Furthermore, in the step of forming the infrared light-cutting precursor layer, the infrared light-cutting precursor layer may be formed on the semiconductor substrate on which at least one color filter of the red (R), green (G), and blue (B) color filters and an infrared light-passing filter are formed, so as to cover the surfaces of the color filters and the infrared light-passing filter, and in the step of forming the infrared light-cutting filter, the infrared light-cutting precursor layer may be dry-etched to form the infrared light-cutting filter so as to cover the surface of the color filter while exposing the surface of the infrared light-passing filter.
[0009] In addition, the infrared light pass filter may be thicker than the red (R), green (G), and blue (B) color filters, and the height difference between the infrared light pass filter and the uppermost color filter among the red (R), green (G), and blue (B) color filters may be within a range of 0.5 μm or more and 1.0 μm or less, and the dry etching amount of the infrared light cut precursor layer may be 1.0 μm or less.
[0010] Furthermore, among the red (R), green (G), and blue (B) color filters, the thickness of the topmost color filter may be in the range of 0.5 μm or more and 1.0 μm or less, and the thickness of the infrared light-cut precursor layer may be in the range of 0.5 μm or more and 1.1 μm or less.
[0011] The method may further include a step of forming an etching stopper layer made of polysiloxane on the surface of the infrared light pass filter and on the surfaces of each of the red (R), green (G), and blue (B) color filters before forming the infrared light cut precursor layer.
[0012] The method may further include the steps of forming an oxygen barrier layer that covers a surface of the infrared cut filter and a surface of the infrared pass filter, and forming a plurality of microlenses on the oxygen barrier layer.
[0013] The method may further include the steps of forming a plurality of microlenses on a surface including the surface of the infrared light cut filter and the surface of the infrared light pass filter, and forming an oxygen barrier layer covering the surfaces of the plurality of microlenses.
[0014] Furthermore, one aspect of a method for manufacturing a solid-state imaging element to solve the above problem includes the steps of preparing a semiconductor substrate, and forming a filter for a solid-state imaging element on the semiconductor substrate by the above-mentioned method for manufacturing a filter for a solid-state imaging element. Effect of the Invention
[0015] According to the present invention, it is possible to suppress deterioration in the performance of a solid-state imaging element caused by partial elution of an infrared absorbing dye contained in an infrared cut filter. [Brief description of the drawings]
[0016] [Figure 1] 1 is an exploded perspective view showing a structure of a solid-state imaging element according to an embodiment of the present invention. [Diagram 2] 5A to 5C are process diagrams illustrating a method for manufacturing a solid-state imaging device according to an embodiment of the present invention. [Diagram 3] 5A to 5C are process diagrams illustrating a method for manufacturing a solid-state imaging device according to an embodiment of the present invention. [Figure 4] 5A to 5C are process diagrams illustrating a method for manufacturing a solid-state imaging device according to an embodiment of the present invention. [Diagram 5] 5A to 5C are process diagrams illustrating a method for manufacturing a solid-state imaging device according to an embodiment of the present invention. [Figure 6] 5A to 5C are process diagrams illustrating a method for manufacturing a solid-state imaging device according to an embodiment of the present invention. [Figure 7] 5A to 5C are process diagrams illustrating a method for manufacturing a solid-state imaging device according to an embodiment of the present invention. [Figure 8] 10A to 10C are process diagrams illustrating a method for manufacturing a solid-state imaging device according to a modified example of an embodiment of the present invention. [Figure 9]10A to 10C are process diagrams illustrating a method for manufacturing a solid-state imaging device according to a modified example of an embodiment of the present invention. [Figure 10] 10A to 10C are process diagrams illustrating a method for manufacturing a solid-state imaging device according to a modified example of an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] 1 to 10, embodiments of a method for manufacturing a filter for a solid-state imaging device and a method for manufacturing a solid-state imaging device according to the present invention will be described. The structure of a solid-state imaging device and a method for manufacturing a solid-state imaging device will be described in order below. In this embodiment, infrared light is light having a wavelength in the range of 0.7 μm to 1 mm, and near-infrared light is infrared light having a wavelength in the range of 700 nm to 1100 nm.
[0018] [Solid-state imaging element] The structure of a solid-state imaging element according to this embodiment will be described with reference to Fig. 1. Fig. 1 is a schematic configuration diagram (exploded perspective view) showing each layer in a portion of the solid-state imaging element in a separated manner.
[0019] As shown in FIG. 1, the solid-state imaging device 10 includes a filter 10F for solid-state imaging devices and a plurality of photoelectric conversion elements 11. The plurality of photoelectric conversion elements 11 include a red photoelectric conversion element 11R, a green photoelectric conversion element 11G, a blue photoelectric conversion element 11B, and an infrared photoelectric conversion element 11P.
[0020] The solid-state imaging device 10 includes a plurality of red photoelectric conversion elements 11R, a plurality of green photoelectric conversion elements 11G, a plurality of blue photoelectric conversion elements 11B, and a plurality of infrared light photoelectric conversion elements 11P. The infrared light photoelectric conversion elements 11P measure the intensity of infrared light. For convenience of illustration, FIG. 1 shows a repeating unit of the photoelectric conversion elements 11 in the solid-state imaging device 10.
[0021] The solid-state imaging device filter 10F includes a plurality of visible light filters, an infrared light pass filter 12P, an etching stopper layer 13, an infrared light cut filter 14, an oxygen barrier layer 15, a plurality of visible light microlenses, and an infrared light microlens 16P.
[0022] The visible light color filter is composed of a red filter 12R, a green filter 12G, and a blue filter 12B. The red filter 12R is located on the light incident side of the red photoelectric conversion element 11R. The green filter 12G is located on the light incident side of the green photoelectric conversion element 11G. The blue filter 12B is located on the light incident side of the blue photoelectric conversion element 11B.
[0023] The infrared light pass filter 12P is located on the light incident side of the infrared light photoelectric conversion element 11P. The infrared light pass filter 12P blocks visible light that can be detected by the infrared light photoelectric conversion element 11P from the infrared light photoelectric conversion element 11P. This improves the detection accuracy of infrared light by the infrared light photoelectric conversion element 11P. The infrared light that can be detected by the infrared light photoelectric conversion element 11P is, for example, near-infrared light.
[0024] The etching stopper layer 13 is located on the light incident side of the color filters (color filters) 12R, 12G, 12B and the infrared light pass filter 12P. More specifically, when viewed from a viewpoint opposite to the plane on which the etching stopper layer 13 extends, the etching stopper layer 13 is located on the red filter 12R, the green filter 12G, the blue filter 12B and the infrared light pass filter 12P.
[0025] The infrared cut filter 14 is located on the light incident side with respect to the etching stopper layer 13. The infrared cut filter 14 has a through hole 14H. When viewed from a viewpoint opposite to the plane on which the infrared cut filter 14 extends, the infrared pass filter 12P is located within the region defined by the through hole 14H. On the other hand, when viewed from a viewpoint opposite to the plane on which the infrared cut filter 14 extends, the infrared cut filter 14 is located on the red filter 12R, the green filter 12G, the blue filter 12B, and the etching stopper layer 13.
[0026] The oxygen barrier layer 15 is located on the light incident side of the infrared cut filter 14. The oxygen barrier layer 15 is a layer common to the red filter 12R, the green filter 12G, the blue filter 12B, and the infrared pass filter 12P. The oxygen barrier layer 15 suppresses the transmission of an oxidation source toward the infrared cut filter 14. The oxidation source is, for example, oxygen and water.
[0027] The oxygen barrier layer 15 has an oxygen permeability of, for example, 5.0 cc / m 2 / day / atom or less. This oxygen permeability is a value measured by a method in accordance with JIS K7126:2006. The oxygen barrier layer 15 has an oxygen permeability of 5.0 cc / m 2 / day / atom or less, the oxygen barrier layer 15 prevents the oxidizing source from reaching the infrared cut filter 14. Therefore, the infrared cut filter 14 is less likely to be oxidized by the oxidizing source. This makes it possible to improve the light resistance of the infrared cut filter 14.
[0028] The microlenses are composed of a red microlens 16R, a green microlens 16G, a blue microlens 16B, and an infrared microlens 16P. The red microlens 16R is located on the light incident side of the red filter 12R. The green microlens 16G is located on the light incident side of the green filter 12G. The blue microlens 16B is located on the light incident side of the blue filter 12B. The infrared microlens 16P is located on the light incident side of the infrared light pass filter 12P.
[0029] Each of the microlenses 16R, 16G, 16B, and 16P has an incident surface 16S which is an outer surface. Each of the microlenses 16R, 16G, 16B, and 16P has a refractive index difference between itself and the outside air so as to collect light entering the incident surface 16S toward each of the photoelectric conversion elements 11R, 11G, 11B, and 11P. Each of the microlenses 16R, 16G, 16B, and 16P may be made of a transparent resin.
[0030] The thickness (layer thickness) of each of the color filters 12R, 12G, and 12B is thinner than the thickness (layer thickness) of the infrared light pass filter 12P. That is, the height of each of the color filters 12R, 12G, and 12B is lower than the height of the infrared light pass filter 12P. The sum of the thickness of the etching stopper layer 13 and the thickness of the infrared light cut filter 14 corresponds to the difference between the thickness of each of the color filters 12R, 12G, and 12B and the thickness of the infrared light pass filter 12P. As described above, the thickness of the infrared light pass filter 12P is larger (thicker) than the thickness of each of the color filters 12R, 12G, and 12B. On the other hand, the step TP (see FIG. 2) between the infrared light pass filter 12P and each of the color filters 12R, 12G, and 12B is filled by the etching stopper layer 13 and the infrared light cut filter 14. Therefore, flatness is easily obtained in the layers below the microlenses 16R, 16G, and 16B for each color and the microlens 16P for infrared light. The step TP is preferably in the range of 0.5 μm to 1.0 μm. If the step TP exceeds 1.0 μm, flatness in the layers below the microlenses 16P for infrared light cannot be obtained, and the heights of the microlenses 16R, 16G, and 16B for each color within the wafer surface become non-uniform, which increases the possibility of causing a decrease in the function of the solid-state imaging element 10. If the step TP is less than 0.5 μm, the performance of the infrared cut filter 14 cannot be fully exhibited.
[0031] [Method of manufacturing solid-state imaging device] A method for manufacturing a solid-state imaging device including a filter for a solid-state imaging device will be described with reference to FIGS.
[0032] The method for manufacturing a filter for a solid-state imaging device according to this embodiment includes at least a step of forming a color filter and an infrared light pass filter, a step of forming an etching stopper layer, a step of forming an infrared light cut precursor layer, and a step of forming an infrared light cut filter. In the step of forming the color filter and the infrared light pass filter, the color filter and the infrared light pass filter are formed on a semiconductor substrate. In the step of forming the etching stopper layer, the etching stopper layer is formed on the semiconductor substrate on which the color filter and the infrared light pass filter are formed. In the step of forming the infrared light cut precursor layer, an infrared light cut precursor layer having an etching rate in dry etching different from that of the etching stopper layer is formed on the etching stopper layer. In the step of forming the infrared light cut filter, the infrared light cut precursor layer is dry etched to form the infrared light cut filter.
[0033] Hereinafter, the method for manufacturing a filter for a solid-state imaging device and the method for manufacturing a solid-state imaging device according to the present embodiment will be described in more detail with reference to the drawings. Figures 2 to 10 each show a schematic cross section of a solid-state imaging device cut along the direction in which the layers constituting the solid-state imaging device are stacked.
[0034] As shown in Fig. 2, in the method for manufacturing a filter for a solid-state imaging device according to this embodiment, first, a semiconductor substrate 21 is prepared. A plurality of photoelectric conversion elements 11 are two-dimensionally arranged on the semiconductor substrate 21 such that one photoelectric conversion element 11 corresponds to one pixel. Note that two blue photoelectric conversion elements 11B and three infrared photoelectric conversion elements 11P are illustrated in Figs. 2 to 10. The material forming the semiconductor substrate 21 may be, for example, Si, an oxide such as SiO2, a nitride such as SiN, or a mixture thereof.
[0035] 2, a blue filter 12B is formed at a position on the semiconductor substrate 21 corresponding to the blue photoelectric conversion element 11B of the semiconductor substrate 21, and an infrared light pass filter 12P is formed at a position on the semiconductor substrate 21 corresponding to the infrared light photoelectric conversion element 11P. At this time, the infrared light pass filter 12P is formed so as to be thicker than the blue filter 12B. The step thus formed between the surface of the infrared light pass filter 12P and the surface of the blue filter 12B is indicated as a "step TP" in FIG. 2.
[0036] In addition, in Figure 2, the red photoelectric conversion element 11R and the red filter 12R at a position corresponding to the red photoelectric conversion element 11R, as well as the green photoelectric conversion element 11G and the green filter 12G at a position corresponding to the green photoelectric conversion element 11G, are omitted.
[0037] The blue filter 12B is formed, for example, by forming a coating film containing a blue photosensitive resin and patterning the coating film using a photolithography method. The coating film containing a blue photosensitive resin is formed, for example, by applying a coating liquid containing a blue photosensitive resin and drying the coating film. The blue filter 12B is formed, for example, by exposing the coating film containing the blue photosensitive resin to an area corresponding to the blue filter 12B and developing it.
[0038] The infrared pass filter 12P is formed, for example, by forming a coating film containing a colored photosensitive resin and patterning the coating film using a photolithography method. The coating film containing a colored photosensitive resin is formed, for example, by applying a coating liquid containing an infrared photosensitive resin and drying the coating film.
[0039] It should be noted that the green filter 12G and the red filter 12R are formed on the semiconductor substrate 21 in the same manner as the blue filter 12B. In order to ensure the desired spectral distribution, it is preferable that the thickness of each of blue filter 12B, green filter 12G, and red filter 12R is within the range of 0.5 μm to 1.0 μm.
[0040] The infrared light photosensitive resin includes a black pigment or black dye and a photosensitive resin. The black pigment is a single pigment having a black color, or a mixture having a black color due to two or more pigments. The black dye may be, for example, an azo dye, an anthraquinone dye, an azine dye, a quinoline dye, a perinone dye, a perylene dye, or a methine dye. The transparent resin that is the photosensitive resin may be, for example, an acrylic resin, a polyamide resin, a polyimide resin, a polyurethane resin, a polyester resin, a polyether resin, a polyolefin resin, a polycarbonate resin, a polystyrene resin, or a norbornene resin.
[0041] The material forming the infrared light pass filter 12P may contain inorganic oxide particles to adjust the refractive index. Examples of inorganic oxides include aluminum oxide, silicon oxide, zirconium oxide, and titanium oxide. The infrared light pass filter 12P may contain additives to provide other functions, such as a light stabilizer, an antioxidant, a heat stabilizer, and an antistatic agent.
[0042] The filters for each color including the blue filter 12B may be formed before the infrared pass filter 12P, or the infrared pass filter 12P may be formed before the filters for each color. Since the infrared pass filter 12P is formed to be thicker than the filters for each color, it is preferable to form the filters for each color before the infrared pass filter 12P from the viewpoint of manufacturing.
[0043] In this embodiment, the thicknesses (heights) of the green filter 12G, the red filter 12R, and the blue filter 12B may be different from each other or may be the same. Here, when the thicknesses (heights) of the green filter 12G, the red filter 12R, and the blue filter 12B are different from each other, the filter with the thickest thickness (highest) is defined as the "top color filter." When the thicknesses (heights) of the green filter 12G, the red filter 12R, and the blue filter 12B are the same from each other, each color filter is defined as the "top color filter." In the present embodiment, the blue filter 12B shown in FIG. 2 will be described below as the "uppermost color filter."
[0044] As shown in FIG. 3, an etching stopper layer 13 is formed on a semiconductor substrate 21 on which a blue filter 12B and an infrared light pass filter 12P are formed. When forming the etching stopper layer 13, first, a coating liquid is prepared using a resin containing silicon. The resin containing silicon may be, for example, polysiloxane. The polysiloxane is formed from a repeating structure of siloxane bonds. The polysiloxane may be silicone. The silicone is polysiloxane and contains organic groups such as an alkyl group and an aryl group.
[0045] Next, the above-mentioned coating liquid is applied onto the semiconductor substrate 21 on which the blue filter 12B and the infrared light pass filter 12P are formed, and the coating film is dried. Then, the dried coating film is cured by heating. As a result, the etching stopper layer 13 is formed on each of the color filters 12R, 12G, and 12B and on the infrared light pass filter 12P.
[0046] Next, as shown in FIG. 4, an infrared light cutting precursor layer 24 is formed on the etching stopper layer 13. When forming the infrared light cutting precursor layer 24, first, a coating liquid containing an infrared light absorbing dye, a transparent resin, and an organic solvent is applied onto the etching stopper layer 13, and the coating film is dried. Next, the dried coating film is cured by heating. As a result, the infrared light cutting precursor layer 24 is formed on the etching stopper layer 13.
[0047] The infrared light absorbing dye for forming the infrared light cutting precursor layer 24 may be at least one selected from, for example, anthraquinone dyes, cyanine dyes, phthalocyanine dyes, dithiol dyes, diimonium dyes, squarylium dyes, and croconium dyes. Of these dyes, the infrared light absorbing dye is preferably at least one of cyanine dyes and phthalocyanine dyes.
[0048] The transparent resin for forming the infrared light cut precursor layer 24 may be at least one selected from, for example, acrylic resin, polyamide resin, polyimide resin, polyurethane resin, polyester resin, polyether resin, polyolefin resin, polycarbonate resin, polystyrene resin, and norbornene resin. Of these resins, the transparent resin is preferably an acrylic resin. By using an acrylic resin, a flattened and uniform infrared light cut precursor layer 24 can be formed without being affected by the step TP between the infrared light pass filter 12P and the color filters 12R, 12G, and 12B.
[0049] Next, as shown in FIG. 5, the entire etching surface of the semiconductor substrate 21 having the infrared light cutting precursor layer 24 is dry etched to form the infrared light cut filter 14. The etching stopper layer 13 formed in the above-mentioned process functions as an etching stopper in this dry etching. In order to exhibit the infrared light cutting function of the infrared light cut filter 14, the film thickness of the infrared light cut filter 14 is preferably in the range of 0.5 μm to 1.0 μm, and more preferably in the range of 0.8 μm to 1.0 μm. If the film thickness of the infrared light cut filter 14 is less than 0.5 μm, the infrared light cut filter function cannot be fully exhibited. If the film thickness of the infrared light cut filter 14 exceeds 1.0 μm (for example, if the film thickness of the infrared light cut filter 14 is 1.01 μm), flatness cannot be obtained in the layer below the infrared light microlens 16P, and the heights of the microlenses 16R, 16G, and 16B for each color within the wafer surface become non-uniform, which increases the possibility of causing a deterioration in the function of the solid-state imaging element 10.
[0050] The dry etching of the infrared light cutting precursor layer 24 may be, for example, plasma etching. In this dry etching, a reactive gas and a rare gas may be used as an etching gas. The reactive gas may be, for example, oxygen gas. Also, the rare gas may be, for example, argon gas. In the dry etching of the infrared light cutting precursor layer 24, a bias may be applied to the infrared light cutting precursor layer 24.
[0051] Here, the dry etching amount ET of the infrared-cut precursor layer 24 (see FIG. 4) corresponds to the thickness of the infrared-cut precursor layer 24 (for example, within a range of 0.5 μm to 1.1 μm) minus the step TP between the infrared pass filter 12P and each of the color filters 12R, 12G, and 12B. The upper limit of the dry etching amount ET of the infrared-cut precursor layer 24 is 1.0 μm. If the dry etching amount ET of the infrared-cut precursor layer 24 is greater than this, an altered layer may be formed on the etched surface by etching, and the unevenness of the etched surface may become large. As a result, flatness within the wafer surface may not be ensured.
[0052] The etching rate of the etching stopper layer 13 is different from the etching rate of the infrared light cutting precursor layer 24. The etching rate is the thickness of each layer etched per unit time. The etching rate of the etching stopper layer 13 is preferably lower than the etching rate of the infrared light cutting precursor layer 24. This makes it easier to adjust the etching time since the etchant is less likely to collide with the layer below the etching stopper layer 13 compared to when the etching rate of the etching stopper layer 13 is higher than the etching rate of the infrared light cutting precursor layer 24.
[0053] Next, as shown in FIG. 6, an oxygen barrier layer 15 is formed to cover the surface of the infrared cut filter 14 and the surface of the infrared pass filter 12P when viewed from a viewpoint opposite to the plane on which the semiconductor substrate 21 extends. The oxygen barrier layer 15 is formed by film formation using a gas phase film formation method such as a sputtering method, a CVD method, or an ion plating method, or a liquid phase film formation method such as a coating method. The oxygen barrier layer 15 formed of silicon oxide may be formed through film formation by a sputtering method using a target made of silicon oxide, for example. The oxygen barrier layer 15 formed of silicon oxide may also be formed through film formation by a CVD method using silane and oxygen, for example. The oxygen barrier layer 15 composed of silicon oxide may also be formed by, for example, applying a coating liquid containing polysilazane, modifying it, and drying the coating.
[0054] Next, as shown in FIG. 7, a plurality of microlenses 16 are formed on the oxygen barrier layer 15. This makes it possible to obtain the solid-state imaging element 10 according to this embodiment. The plurality of microlenses 16 are formed at positions overlapping with the color filters 12R, 12G, and 12B and the infrared light pass filter 12P when viewed from a viewpoint opposite to the plane on which the oxygen barrier layer 15 extends. Each microlens 16 is formed, for example, by using an etch-back method. In the etch-back method, first, a transparent resin layer for forming each microlens 16 is formed on the oxygen barrier layer 15. Next, a resist pattern having a shape (lens shape) in which a plurality of hemispheres are arranged is formed on the transparent resin layer. Then, the transparent resin layer having the resist pattern is dry-etched to transfer the shape (lens shape) of the resist pattern to the transparent resin layer, thereby forming the plurality of microlenses 16.
[0055] This makes it possible to form a plurality of solid-state imaging elements 10, which have been described above with reference to FIG. As described above, according to the method for manufacturing the filter 10F for a solid-state imaging device and the method for manufacturing the solid-state imaging device 10 of the embodiment, the following effects can be obtained.
[0056] (1) A manufacturing method for the solid-state imaging device filter 10F of this embodiment includes the steps of forming at least one color filter (e.g., blue filter 12B) of the red filter 12R, the green filter 12G, and the blue filter 12B, and an infrared light pass filter 12P on a semiconductor substrate 21; forming an infrared light cut precursor layer 24 on the semiconductor substrate 21 on which the at least one color filter (e.g., blue filter 12B) of the red filter 12R, the green filter 12G, and the blue filter 12B, and the infrared light pass filter 12P have been formed; and forming the infrared light cut filter 14 by dry etching the infrared light cut precursor layer 24.
[0057] (2) Furthermore, in the step of forming the infrared light-cutting precursor layer 24 in the manufacturing method for the solid-state imaging element filter 10F of this embodiment, the infrared light-cutting precursor layer 24 is formed on a semiconductor substrate 21 on which at least one color filter (e.g., blue filter 12B) of the red filter 12R, green filter 12G, and blue filter 12B and the infrared light-pass filter 12P are formed, so as to cover each surface of the color filter (e.g., blue filter 12B) and the infrared light-pass filter 12P. In the step of forming the infrared light-cutting filter 14, the infrared light-cutting precursor layer 24 may be dry-etched to form the infrared light-cutting filter 14 so as to cover the surface of the color filter (e.g., blue filter 12B) while exposing the surface of the infrared light-passing filter 12P.
[0058] With this configuration, the infrared cut filter 14 can be formed without forming a resist pattern by etching (dry etching) the entire surface of the infrared cut precursor layer 24. In other words, the manufacturing method for the solid-state imaging device filter 10F according to this embodiment is a manufacturing method that does not form a resist pattern, and therefore does not use a resist pattern stripping solution that is a factor in deteriorating the spectral characteristics of the infrared cut filter 14. As a result, the deterioration of the function of the solid-state imaging device 10 caused by partial elution of the infrared absorbing dye contained in the infrared cut filter 14 is suppressed.
[0059] Furthermore, with such a configuration, the formation of the infrared cut filter 14 does not depend on the pixel size, and therefore the formation of the infrared cut filter 14 is easy. In other words, with the above-described configuration, infrared cut filters 14 of various pixel sizes can be easily formed. In addition, in the conventional method for manufacturing a filter for a solid-state imaging device, it was necessary to prepare a resist pattern (mask pattern) for each pixel using, for example, a photolithography method. In that case, since there is a production limit for the size of the resist pattern (mask pattern), it was difficult to form infrared cut filters for various pixel sizes.
[0060] (3) Furthermore, the manufacturing method for the solid-state imaging element filter 10F of this embodiment may further include a step of forming an oxygen barrier layer 15 covering the surface of the infrared light cut filter 14 and the surface of the infrared light pass filter 12P, and a step of forming a plurality of microlenses 16 on the oxygen barrier layer 15. With this configuration, the oxygen blocking layer 15 prevents an oxidation source from reaching the infrared pass filter 12P, so that the infrared pass filter 12P is less likely to be oxidized.
[0061] (4) Furthermore, in the manufacturing method for filter 10F for a solid-state imaging device according to this embodiment, infrared light pass filter 12P has a thickness thicker than each of the red filter 12R, green filter 12G, and blue filter 12B color filters, and the height difference between infrared light pass filter 12P and the topmost color filter (e.g., blue filter 12B) among red filter 12R, green filter 12G, and blue filter 12B is within a range of 0.5 μm or more and 1.0 μm or less, and the amount of dry etching of infrared light cut precursor layer 24 in the process of forming infrared light cut filter 14 may be 1.0 μm or less.
[0062] With such a configuration, it is possible to reliably impart the desired infrared light cutting performance to the infrared light cut filter 14, while obtaining flatness in the layer below the infrared light microlens 16P, making the heights of the microlenses 16R, 16G, and 16B for each color uniform across the wafer surface, thereby suppressing deterioration in the functionality of the solid-state imaging element 10. Furthermore, with this configuration, it is possible to suppress the formation of an altered layer on the etched surface due to etching, which would cause the etched surface to become uneven.
[0063] (5) Furthermore, in the manufacturing method for the solid-state imaging device filter 10F according to this embodiment, the thickness of the topmost color filter (e.g., blue filter 12B) among the red filter 12R, the green filter 12G, and the blue filter 12B may be within a range of 0.5 μm or more and 1.0 μm or less, and the thickness of the infrared light cut precursor layer 24 may be within a range of 0.5 μm or more and 1.1 μm or less. With this configuration, it is possible to reliably impart the desired spectral performance to the color filters 12R, 12G, and 12B, and also to reliably impart the desired infrared light cutting performance to the infrared light cutting filter 14.
[0064] (6) Furthermore, the manufacturing method for the solid-state imaging element filter 10F of this embodiment may further include a step of forming an etching stopper layer 13 made of polysiloxane on the surface of the infrared light pass filter 12P and on the surfaces of each of the color filters, the red filter 12R, the green filter 12G, and the blue filter 12B, before forming the infrared light cut precursor layer 24.
[0065] With this configuration, even if a part of the infrared light cutting precursor layer 24 is removed by over-etching the infrared light cutting precursor layer 24, the etching stopper layer 13 is located below the infrared light cutting precursor layer 24, so collision of the etchant with the layer below the etching stopper layer 13 is suppressed. This suppresses deterioration in the function of the solid-state imaging element 10 caused by a change in the surface properties of the layer below the infrared light cutting precursor layer 24, which is the etching target.
[0066] (7) Furthermore, the manufacturing method for the solid-state imaging element filter 10F of this embodiment may further include a step of forming an oxygen barrier layer 15 covering the surface of the infrared light cut filter 14 and the surface of the infrared light pass filter 12P, and a step of forming a plurality of microlenses 16 on the oxygen barrier layer 15.
[0067] With this configuration, the oxygen blocking layer 15 prevents oxidation sources from reaching the infrared cut filter 14 and the infrared pass filter 12P, making the infrared cut filter 14 and the infrared pass filter 12P less susceptible to oxidation.
[0068] (8) Furthermore, the manufacturing method for the solid-state imaging element filter 10F of this embodiment may include the steps of forming the red filter 12R, the green filter 12G, and the blue filter 12B color filters, and a plurality of infrared light pass filters 12P on a semiconductor substrate 21; forming an infrared light cut precursor layer 24 on the semiconductor substrate 21 on which the red filter 12R, the green filter 12G, and the blue filter 12B color filters, and the plurality of infrared light pass filters 12P have been formed; and forming the infrared light cut filter 14 by dry etching the infrared light cut precursor layer 24.
[0069] (9) Furthermore, in the process of forming the infrared light-cutting precursor layer 24 in the manufacturing method for the solid-state imaging element filter 10F of this embodiment, the infrared light-cutting precursor layer 24 is formed on the semiconductor substrate 21 on which the color filters 12R, 12G, and 12B, and the multiple infrared light-pass filters 12P are formed, so as to cover all of the surfaces of the color filters 12R, 12G, and 12B, and the infrared light-pass filters 12P. In the process of forming the infrared light-cutting filter 14, the infrared light-cutting precursor layer 24 may be dry-etched to expose the surfaces of the multiple infrared light-pass filters 12P, while the infrared light-cutting filter 14 is formed so as to cover all of the surfaces of the color filters 12R, 12G, and 12B.
[0070] In this configuration, the infrared light cut precursor layer 24 is filled between the infrared light pass filters 12P, and then dry etching is performed, so there is no need to form a resist pattern. Therefore, a resist pattern remover, which is a factor in deteriorating the spectral characteristics of the infrared light cut filter 14, is not used. As a result, the deterioration of the function of the solid-state imaging element 10 caused by partial elution of the infrared light absorbing dye contained in the infrared light cut filter 14 is reliably suppressed.
[0071] [Modifications of the embodiment] The above-described embodiment can be modified as follows. [Oxygen barrier layer] In the above embodiment, the oxygen barrier layer 15 is formed between the infrared cut filter 14 and the infrared pass filter 12P and each microlens 16, but the present invention is not limited to this. The position where the oxygen barrier layer 15 is formed is not limited to between the infrared cut filter 14 and the infrared pass filter 12P and each microlens 16, but may be on the outer surface (incident surface 16S) of each microlens 16.
[0072] 8, when forming the solid-state imaging element 10 according to this modification, first, a plurality of microlenses 26 are formed on a surface including the surface of the infrared cut filter 14 and the surface of the infrared pass filter 12P. Next, each microlens 26 is formed so as to cover at least one of the color filters 12R, 12G, and 12B and the infrared pass filter 12P.
[0073] 9, an oxygen barrier layer 25 is formed so as to cover the surfaces of the multiple microlenses 26. The oxygen barrier layer 25 may also function as an anti-reflection layer.
[0074] As described above, the manufacturing method for the solid-state imaging element filter 10F of this embodiment may further include a step of forming a plurality of microlenses 26 on a surface including the surface of the infrared light cut filter 14 and the surface of the infrared light pass filter 12P, and a step of forming an oxygen barrier layer 25 covering the surfaces of the plurality of microlenses 26. With this configuration, the oxygen barrier layer 25 prevents sources of oxidation from reaching the microlenses 26, so that the microlenses 26 are less likely to be oxidized.
[0075] In the above-mentioned embodiment, the case where the oxygen barrier layer 15 is formed has been described, but the present invention is not limited to this. The solid-state imaging device filter 10F does not need to include the oxygen barrier layer 15. Even in this case, it is possible to obtain an effect similar to that obtained in a form in which the oxygen barrier layer 15 is formed, by forming the infrared light cut precursor layer 24 on the etching stopper layer 13 covering the surface of the semiconductor substrate 21.
[0076] The layer structure of the oxygen barrier layer 25 may be a single layer structure made of a single compound, a laminated structure of layers made of a single compound, or a laminated structure of layers made of different compounds.
[0077] In addition, the surface of the infrared cut filter 14 and the surface of the infrared pass filter 12P may have a step in the thickness direction of the semiconductor substrate 21. Specifically, the surface of the infrared cut filter 14 and the surface of the infrared pass filter 12P may have a step of 5 μm or less, more preferably a step of 3 μm or less, and even more preferably a step of 1 μm or less, in the thickness direction of the semiconductor substrate 21. In this case, for example, the oxygen barrier layer 15 formed of SiO2 can function as a planarizing layer that fills the step formed by the surface of the infrared cut filter 14 and the surface of the infrared pass filter 12P. Note that the oxygen barrier layer 15 can function as a planarizing layer by having a thickness that can fill the step between the surface of the infrared cut filter 14 and the surface of the infrared pass filter 12P.
[0078] [Etching stopper layer] The portion of the etching stopper layer 13 formed on the surface of the semiconductor substrate 21 does not need to be completely removed. Even in this case, since the etching stopper layer 13 is made of a transparent resin, light incident on the solid-state imaging element 10 can be incident on the photoelectric conversion element 11 through the etching stopper layer 13.
[0079] In the above-mentioned embodiment, the case where the etching stopper layer 13 is formed has been described, but the present invention is not limited to this. As shown in Fig. 10, the solid-state imaging device filter 10F does not need to include the etching stopper layer 13. In this case, it is difficult to obtain the effect obtained by forming the etching stopper layer 13, but even in this case, it is possible to form the infrared light cut filter 14 by adjusting the etching time until the surface of the infrared light pass filter 12P appears.
[0080] [Example] A manufacturing example of a solid-state imaging device corresponding to the embodiment will be described below. Note that in the manufacturing example described below, a manufacturing example of a solid-state imaging device in which the thickness of the infrared pass filter is thicker than the thickness of each color filter and no etching stopper layer is provided will be described.
[0081] A green resist layer was formed by spin-coating a green resist containing a green pigment, a photosensitive curable resin, and a thermosetting resin at a rotation speed of 1000 rpm on a semiconductor substrate on which a plurality of photoelectric conversion elements were arranged two-dimensionally. CIPG58 in the color index was used as the green pigment. In the green resist, the concentration of the green pigment was set to 70 mass %. Next, the green resist layer was selectively exposed using a green mask, and then the exposed green resist layer was developed to form a green filter pattern. Then, the green filter pattern was cured by heating it at 230°C for 6 minutes using a hot plate. This formed a green filter having a thickness of 600 nm.
[0082] Next, a blue resist layer was formed by spin-coating a blue resist containing a pigment, a photosensitive curing resin, and a thermosetting resin at a rotation speed of 1000 rpm on the green filter and the portion of the semiconductor substrate not covered by the green filter. CIPB156 and CIPV23 in the color index were used as the pigments. The concentration of the blue pigment in the blue resist was set to 50 mass%. Next, the blue resist layer was selectively exposed by photolithography using a blue mask, and then the exposed blue resist layer was developed to form a blue filter pattern. Then, the blue filter pattern was cured by heating at 230°C for 6 minutes using a hot plate. This formed a blue filter having a thickness of 600 nm. At this time, the blue filter was formed at a position different from the position where the green filter was formed on the surface of the semiconductor substrate.
[0083] Next, a red resist layer containing a pigment, a photosensitive curable resin, and a thermosetting resin was spin-coated at a rotation speed of 1000 rpm on the green filter, the blue filter, and the portion of the semiconductor substrate not covered by these filters to form a red resist layer. CIPR254 and CIPY139 in the color index were used as the pigments. In the red resist, the pigment concentration was set to 60 mass%. Next, the red resist layer was selectively exposed using a red mask, and then the exposed red resist layer was developed to form a red filter pattern. Then, the red filter pattern was cured by heating it at 230°C for 6 minutes using a hot plate. This formed a red filter having a thickness of 600 nm. At this time, the red filter was formed at a position on the surface of the semiconductor substrate different from the positions where the blue filter and the green filter were formed.
[0084] Next, a photosensitive infrared light path resist containing blue, purple, and yellow pigments was applied onto each color filter and onto the semiconductor substrate in the areas not covered by the color filters. This formed an infrared light path resist layer. The blue pigment was CIPB15:6 in the color index, the purple pigment was CIPV23 in the color index, and the yellow pigment was CIPY139 in the color index. The pigment concentration in the infrared light path resist was set to 78% by mass.
[0085] Next, the infrared light pass resist layer was selectively exposed using an infrared light pass mask, and the exposed infrared light pass resist layer was developed to form an infrared light pass filter pattern. The infrared light pass filter pattern was then cured by heating at 230°C for 6 minutes using a hot plate. This resulted in the formation of an infrared light pass filter having a thickness of 1300 nm. At this time, the infrared light pass filter was formed at a position on the surface of the semiconductor substrate different from the position where the above-mentioned color filters were formed. In addition, in the infrared light pass filter, the maximum value of the transmittance for light having a wavelength of 400 nm or more and 650 nm or less was 4.8%, and the maximum value of the transmittance for light having a wavelength of 650 nm or more and 730 nm or less was 8.6%. In addition, in the infrared light pass filter, the minimum value of the transmittance for light having a wavelength of 800 nm or more and 1000 nm or less was 92.1%. The step between the infrared light pass filter and each color filter was 700 nm.
[0086] Next, a coating solution containing an infrared absorbing dye and a thermosetting resin was spin-coated on each color filter and on the infrared pass filter at a rotation speed of 1000 rpm to form a coating film. The coating film was then cured by heating at 200°C for 20 minutes using a hot plate. As a result, an infrared cut precursor layer having a thickness of 1000 nm was formed on each color filter and on the infrared pass filter. The infrared cut precursor layer had a transmittance of 8% for light having a wavelength of around 940 nm.
[0087] Next, the infrared light cutting precursor layer was dry etched. In this case, an ICP type dry etching device was used as the dry etching device. A mixed gas containing argon gas and oxygen gas was used as the etching gas, and a bias was applied to the etching object to perform anisotropic etching on the infrared light cutting precursor layer. The dry etching amount of the infrared light cutting precursor layer was 300 nm. As a result, an infrared light cutting filter having a thickness of 700 nm was formed.
[0088] Next, an oxygen blocking layer made of SiO2 and having a thickness of 100 nm was formed on the surface of the infrared light cut filter and the surface of the infrared light pass filter by using a plasma CVD method.
[0089] Next, a plurality of microlenses having a height of 500 nm were formed on the oxygen barrier layer by using an etch-back method, thereby obtaining a solid-state imaging device according to this example. In this way, the method for manufacturing a solid-state imaging device according to the present embodiment does not require the formation of a resist pattern to form an infrared cut filter. Therefore, a stripping solution for stripping the resist pattern is not required. As a result, the elution of the infrared light absorbing dye contained in the infrared cut filter during the formation of the infrared cut filter is suppressed, and the deterioration of the function of the solid-state imaging device can be suppressed. Specifically, the light receiving sensitivity of the solid-state imaging device according to the present embodiment is improved by about 1.2 to 1.5 times in each pixel (each color) compared with a solid-state imaging device manufactured by a method for manufacturing a solid-state imaging device according to the conventional technology in which a resist pattern is formed to form an infrared cut filter. [Explanation of symbols]
[0090] 10...Solid-state image sensor 10F…Solid-state image sensor filter 11...Photoelectric conversion element 12B…Blue filter 12G…Green filter 12R…Red filter 12P…Infrared pass filter 13...Etching stopper layer 14…Infrared cut filter 15,25...Oxygen barrier layer 16,26...Micro lenses 21...Semiconductor substrate 24…Infrared light blocking precursor layer
Claims
1. forming at least one color filter of red (R), green (G), and blue (B) color filters and an infrared light pass filter on a semiconductor substrate; forming an infrared light cut precursor layer on the semiconductor substrate on which at least one color filter of the red (R), green (G), and blue (B) color filters and an infrared light pass filter are formed; forming an infrared light cut filter on the color filter by dry etching the infrared light cut precursor layer; and forming an etching stopper layer made of polysiloxane on a surface of the infrared pass filter having a thickness greater than that of each of the red (R), green (G), and blue (B) color filters, and on a surface of each of the red (R), green (G), and blue (B) color filters, before forming the infrared light cut precursor layer. A method for manufacturing a filter for a solid-state imaging device.
2. In the step of forming the infrared light cutting precursor layer, the infrared light cutting precursor layer is formed on the semiconductor substrate on which at least one color filter of the red (R), green (G), and blue (B) color filters and an infrared light pass filter are formed, so as to cover each surface of the color filter and the infrared light pass filter; In the step of forming the infrared cut filter, the infrared cut precursor layer is dry etched to expose a surface of the infrared pass filter, and the infrared cut filter is formed so as to cover a surface of the color filter. A method for producing the filter for a solid-state imaging device according to claim 1.
3. Among the red (R), green (G), and blue (B) color filters, the height difference between the uppermost color filter and the uppermost color filter is within a range of 0.5 μm or more and 1.0 μm or less; The amount of dry etching of the infrared light-cutting precursor layer is 1.0 μm or less. A method for producing the filter for a solid-state imaging device according to claim 1 or 2.
4. Among the red (R), green (G), and blue (B) color filters, the thickness of the uppermost color filter is within a range of 0.5 μm or more and 1.0 μm or less; The thickness of the infrared light-cutting precursor layer is in the range of 0.5 μm to 1.1 μm. A method for producing the filter for a solid-state imaging device according to any one of claims 1 to 3.
5. forming an oxygen barrier layer covering a surface of the infrared cut filter and a surface of the infrared pass filter; forming a plurality of microlenses on the oxygen barrier layer; or, forming a plurality of microlenses on a surface including a surface of the infrared light cut filter and a surface of the infrared light pass filter; forming an oxygen barrier layer covering the surfaces of the microlenses; A method for producing the filter for a solid-state imaging device according to any one of claims 1 to 4.
6. The method further includes a step of forming a plurality of microlenses on a surface including a surface of the infrared light cut filter and a surface of the infrared light pass filter, The thickness of the microlenses formed on the infrared light cut filter is greater than the thickness of the microlenses formed on the infrared light pass filter. A method for producing the filter for a solid-state imaging device according to any one of claims 1 to 4.
7. Providing a semiconductor substrate; forming a filter for a solid-state imaging device on the semiconductor substrate by the method for producing a filter for a solid-state imaging device according to any one of claims 1 to 6. A method for manufacturing a solid-state imaging device.
8. a color filter of at least one color selected from red (R), green (G), and blue (B) color filters and an infrared light pass filter are provided on a semiconductor substrate; an etching stopper layer made of polysiloxane is provided on a surface of the infrared pass filter having a thickness larger than that of the color filter and on a surface of the color filter; The etching stopper layer is only one layer, At least an oxygen barrier layer is provided on the surface of the etching stopper layer opposite to the infrared light pass filter. Filter for solid-state imaging devices.
Citation Information
Patent Citations
Solid state imaging element
JP2003060176A
Optical filter
JP2007219114A
Method of manufacturing color filter
JP2008122891A
Method of manufacturing color filter
JP2008256745A
Solid-state image pick-up device and solid-state imaging system
JP2018060910A