Dry offset printing plates

The printing plate for dry offset printing, featuring a fluorine-containing organic compound and partially saponified polyvinyl acetate, addresses durability and reproducibility issues by enhancing ink transfer and image stability in seamless can printing.

JP7585726B2Active Publication Date: 2024-11-19TORAY INDUSTRIES INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020190057
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-16
Publication Date
2024-11-19
Estimated Expiration
2040-11-16

AI Technical Summary

Technical Problem

Existing printing plates for dry offset printing face issues with long-run durability, ink transfer properties, and printing reproducibility, particularly in seamless can printing, where fine images are prone to crushing.

Method used

A printing plate for dry offset printing incorporating a fluorine-containing organic compound with ionic groups and/or ethylene glycol chains, combined with partially saponified polyvinyl acetate and polyamide having basic nitrogen, enhances ink transferability and printing reproducibility by reducing ink supply and pressure requirements.

Benefits of technology

The solution enables long-run printing with improved ink transfer properties and printing reproducibility, maintaining relief shape and preventing ink spillage while preserving fine image integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585726000001
    Figure 0007585726000001
  • Figure 0007585726000002
    Figure 0007585726000002
Patent Text Reader

Abstract

To provide a plate for dry off-set printing that allows long-run printing and is excellent in ink transfer and printing reproduction.SOLUTION: A plate for dry off-set printing has, on a support, a relief containing a fluorinated organic compound.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a printing plate for dry offset printing, a method for producing the same, a printing method using the same, and a printing plate precursor for dry offset printing. [Background technology]

[0002] 2. Description of the Related Art Dry offset printing, in which each color ink is transferred from a printing plate to a blanket and then from the blanket to the printing target, is commonly used as a printing method for packaging products such as labels for cans and plastic bottles.

[0003] As a printing plate suitable for can printing, particularly seamless can printing, a waterless plate for printing on the outer surface of a seamless can has been proposed, which has at least a substrate and a laser heat-sensitive layer, and on the heat-sensitive layer, a non-printing area made of a silicone rubber layer and a printing area from which the silicone rubber has been removed, and the thickness of the silicone rubber layer in the non-printing area is in the range of 2.2 to 5.5 μm (see, for example, Patent Document 1). Furthermore, as a printing plate precursor used in dry offset printing, there has been proposed a photosensitive resin printing plate precursor having at least a support and a photosensitive resin layer, the photosensitive resin layer containing (A) a partially saponified polyvinyl acetate compound, (B) a polyamide having a basic nitrogen, (C) a compound having an ethylenic double bond, and (D) a photopolymerization initiator, the photosensitive resin layer including at least a lower layer and a printing surface layer, the support, the lower layer, and the printing surface layer being arranged in this order, and the (A) partially saponified polyvinyl acetate compound containing (A1) having an average degree of polymerization of 1200 to 2600 in the printing surface layer and (A2) having an average degree of polymerization of 400 to 800 in the lower layer (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-58257 A [Patent Document 2] International Publication No. 2017-38970 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the waterless planographic plate described in Patent Document 1 has a problem with printing durability for long-run printing. On the other hand, the printing plate obtained from the printing plate precursor described in Patent Document 2 has sufficient printing durability for long-run printing, but has insufficient ink transferability. In order to obtain a printed matter with a high ink concentration, it is possible to increase the amount of ink supplied to the printing plate or to increase the pressure for transferring the ink to the blanket, but in this case, fine images such as letters and halftone dots are easily crushed, resulting in a problem with print reproducibility.

[0006] In view of the above problems, an object of the present invention is to provide a printing plate for dry offset printing which is capable of long-run printing and has excellent ink transfer properties and print reproducibility. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention mainly has the following configuration. Printing plate for dry offset printing having a relief containing a fluorine-containing organic compound on a support a printing plate for dry offset printing, the relief containing partially saponified polyvinyl acetate and / or a polyamide having basic nitrogen, and the fluorine-containing organic compound having an ionic group and / or an ethylene glycol chain; . A printing plate precursor for dry offset printing, comprising a support and a photosensitive resin layer containing a fluorine-containing organic compound, the photosensitive resin layer containing partially saponified polyvinyl acetate and / or a polyamide having basic nitrogen, and the fluorine-containing organic compound has an ionic group and / or an ethylene glycol chain. Effect of the Invention

[0008] The printing plate for dry offset printing of the present invention is capable of long-run printing and is excellent in ink transfer property and print reproducibility. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described.

[0010] The printing plate for dry offset printing of the present invention (hereinafter sometimes simply referred to as "printing plate") has a relief containing a fluorine-containing organic compound on at least a support. The relief corresponds to an image formed by transferring ink supplied by an inker to a blanket, and the support has the function of holding the relief. The relief is generally formed by photolithography of a photosensitive resin layer or laser etching of a resin layer. A floor layer made of a photocured product of a photosensitive resin layer or a resin layer may be formed on the support, and a relief may be formed on the floor layer.

[0011] Examples of the support include a plastic sheet made of polyester, etc., a synthetic rubber sheet made of styrene-butadiene rubber, etc., and a metal plate made of steel, stainless steel, aluminum, etc. From the viewpoints of handling and flexibility, the thickness of the support is preferably in the range of 100 to 350 μm.

[0012] The support is preferably subjected to an easy-adhesion treatment, which can improve adhesion to the relief or floor layer. Examples of the easy-adhesion treatment method include mechanical treatment such as sandblasting, physical treatment such as corona discharge, and chemical treatment such as coating. Among these, from the viewpoint of adhesion, it is preferable to provide an easy-adhesion layer by coating.

[0013] The printing plate of the present invention contains a fluorine-containing organic compound in the relief. By containing a fluorine-containing organic compound in the relief, ink transferability can be improved. This makes it possible to reduce the amount of ink supplied and reduce the pressure for transferring the ink to the blanket, thereby improving print reproducibility. Furthermore, the ink repellency of the relief makes it possible to suppress the ink supplied to the printing plate from spilling out from the relief apex to the slope, thereby maintaining excellent print reproducibility.

[0014] Examples of organic compounds containing fluorine include compounds having a perfluoroalkyl group, a perfluoroalkenyl group, etc. Commercially available products of such compounds include the "Ftergent" (registered trademark) series (manufactured by Neos Corporation) and the "Surflon" (registered trademark) series (manufactured by AGC Seimi Chemical Co., Ltd.). Two or more of these may be contained.

[0015] The fluorine-containing organic compound preferably further has an ionic group and / or an ethylene glycol chain. The ionic group and the ethylene glycol chain have high affinity with the polymer described below as a preferred component constituting the relief, and therefore the compatibility between the fluorine-containing organic compound and the polymer is improved, and the bleed-out of the fluorine-containing organic compound from the relief can be suppressed. Examples of the ionic group include a sulfonic acid group, a quaternary ammonium group, a phosphoric acid group, and a carboxyl group. Examples of the fluorine-containing organic compound having such a functional group include "Ftergent" 100 (NEOS Corporation) as one having a sulfonic acid group, "Ftergent" 300 (NEOS Corporation) as one having a quaternary ammonium group, FPE-50 (AGC Seimi Chemical Co., Ltd.) as one having a phosphoric acid group, and "Ftergent" 251 (NEOS Corporation) as one having an ethylene glycol chain.

[0016] Betaine is also preferred as an organic compound containing fluorine. Betaine is a compound (intramolecular salt) that has a positive charge and a negative charge at non-adjacent positions in the same molecule, has no dissociable hydrogen bonded to the positively charged atom, and has no charge as a whole molecule. When an ionic substance comes into contact with the relief from the outside, it forms a salt, which can prevent the salt from adhering to the plate surface and the organic compound containing fluorine from bleeding out of the relief.

[0017] Examples of commercially available fluorine-containing organic compounds having such functional groups include "Ftergent" 400SW (Neos) and S-231 (AGC Seimi Chemical Co., Ltd.).

[0018] The content of the fluorine-containing organic compound in the relief is preferably 0.1% by weight or more, which can further improve the ink transferability. The content of the fluorine-containing organic compound is more preferably 0.3% by weight or more. On the other hand, the content of the fluorine-containing organic compound in the relief is preferably 10% by weight or less, which can suppress bleeding out from the relief. The content of the fluorine-containing organic compound is more preferably 5% by weight or less, and further preferably 2% by weight or less.

[0019] The relief of the printing plate of the present invention contains, in addition to the fluorine-containing organic compound, a photocured product of the photosensitive resin layer when the relief is formed by photolithography of the photosensitive resin layer, and a component of the resin layer when the relief is formed by laser etching of the resin layer. In either case, it is preferable to contain a polymer for forming the relief. In addition, when the relief is formed from the photosensitive resin layer, components other than the fluorine-containing organic compound and the polymer component contained in the photosensitive resin layer will be described later as components of the photosensitive resin layer of the dry offset printing plate precursor.

[0020] Examples of the polymer include styrene-butadiene copolymer, polybutadiene latex, styrene-butadiene copolymer latex, acrylonitrile-butadiene copolymer latex, methyl methacrylate-butadiene copolymer latex, polyurethane, cellulose derivatives, polyester, polyacrylic acid derivatives, polyvinyl acetate, partially saponified polyvinyl acetate, polyvinyl alcohol, polyvinylpyrrolidone, polyamide, etc. Two or more of these may be contained. The content of the polymer in the relief is preferably 30 to 95% by weight.

[0021] When forming a relief by photolithography, particularly when removing non-image areas by water development, a polymer that is dispersible or soluble in water is preferred. As the polymer that is dispersible or soluble in water, a polymer having a hydrophilic group or a polymer whose polymer main chain itself is water-swellable or water-soluble is preferred. Examples of the hydrophilic group include a carboxyl group, an amino group, a hydroxyl group, a phosphoric acid group, a sulfonic acid group, and salts thereof. Examples of the polymer having a hydrophilic group include a carboxylated styrene butadiene latex, a polymer of an aliphatic conjugated diene having a carboxyl group, an emulsion polymer of an ethylenically unsaturated compound having a phosphoric acid group and / or a carboxyl group, and a polyurethane containing a sulfonic acid group. Examples of polymers whose polymer backbone chains themselves are water-swellable or water-soluble include polyvinyl alcohol, partially saponified polyvinyl acetate, vinyl alcohol-sodium acrylate copolymer, vinyl alcohol-sodium methacrylate copolymer, polyvinylpyrrolidone, polyether-containing polyamide, polyamide having a tertiary amino group, polyether, cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, carboxymethyl cellulose, starch, starch-sodium polyacrylate grafted product, saponified starch-polyacrylonitrile grafted product, cellulose polyacrylic acid grafted product, partially crosslinked sodium polyacrylate, polyethylene glycol, polyethylene glycol derivatives, etc. Among these, partially saponified polyvinyl acetate and polyamide having a tertiary amino group are preferred.

[0022] Partially saponified polyvinyl acetate has excellent moldability. In addition, since it is difficult to swell or shrink in response to 1-hexadecene, a solvent contained in inks generally used in dry offset printing, it is possible to maintain the relief shape even in long-run printing, and the suitability for long-run printing can be further improved. The saponification degree of the partially saponified polyvinyl acetate is preferably 60 to 99 mol%.

[0023] Polyamides having basic nitrogen can improve the toughness of the relief and suppress relief chipping during printing. The basic nitrogen may be present in either the main chain or the side chain, but is preferably present in the main chain. Polyamides having basic nitrogen can be obtained by subjecting a monomer having basic nitrogen to condensation polymerization or polyaddition reaction together with other diamines, dicarboxylic acids, ω-amino acids, lactams, etc., as necessary. As the monomer having basic nitrogen, a monomer having a piperazine group or an N,N-dialkylamino group is preferred, and a monomer having a piperazine group is more preferred.

[0024] Preferred examples of monomers are N,N'-bis(aminomethyl)-piperazine, N,N'-bis(β-aminoethyl)-piperazine, N,N'-bis(γ-aminobenzyl)-piperazine, N-(β-aminoethyl)piperazine, N-(β-aminopropyl)piperazine, N-(ω-aminohexyl)piperazine, N-(β-aminoethyl)-2,5-dimethylpiperazine, N,N-bis(β-aminoethyl)-benzylamine, N,N-bis(γ-aminopropyl)-amine, N,N'-dimethyl-N,N'-bis(γ-aminopropyl)- Diamines such as ethylenediamine, N,N'-dimethyl-N,N'-bis(γ-aminopropyl)-tetramethylenediamine; N,N'-bis(carboxymethyl)-piperazine, N,N'-bis(carboxymethyl)-methylpiperazine, N,N'-bis(carboxymethyl)-2,6-dimethylpiperazine, N,N'-bis(β-carboxyethyl)-piperazine, N,N-bis(carboxymethyl)-methylamine, N,N-bis(β-carboxyethyl)-ethylamine, N,N-bis(β-carboxyethyl)-methylamine dicarboxylic acids such as N,N-di(β-carboxyethyl)-isopropylamine, N,N'-dimethyl-N,N'-bis(carboxymethyl)-ethylenediamine, N,N'-dimethyl-N,N'-bis(β-carboxyethyl)-ethylenediamine, or their lower alkyl esters; acid halides, N-(aminomethyl)-N'-(carboxymethyl)-piperazine, N-(aminomethyl)-N'-(β-carboxyethyl)-piperazine, N-(β-aminoethyl)-N'-(β-carboxyethyl)-piperazine and ω-amino acids such as N-(aminomethyl)-N-(carboxymethyl)-methylamine, N-(β-aminoethyl)-N-(β-carboxyethyl)-methylamine, N-(aminomethyl)-N-(β-carboxyethyl)-isopropylamine, and N,N'-dimethyl-N-(aminomethyl)-N'-(carboxymethyl)-ethylenediamine.Moreover, by polymerizing diamines, dicarboxylic acids, ω-amino acids, lactams, and the like other than these monomers in combination, polyamides containing basic nitrogen can be obtained.

[0025] It is preferable to use 10 to 80 mol% of a monomer having basic nitrogen out of all components constituting the polyamide, i.e., the total of aminocarboxylic acid units (including lactams as raw materials), dicarboxylic acid units and diamine structural units. By using 10 mol% or more of a monomer having basic nitrogen, water solubility can be improved, and compatibility can be improved when partially saponified polyvinyl acetate is used in combination. On the other hand, by using 80 mol% or less of a monomer having basic nitrogen, water absorption during storage of the printing plate can be suppressed, and the thickness precision of the printing plate can be maintained at a high level.

[0026] The weight average molecular weight of the polymer is preferably 10,000 or more and 200,000 or less. Here, the weight average molecular weight can be determined by GPC measurement. More specifically, the weight average molecular weight can be measured using a gel permeation chromatograph-multiangle light scattering photometer manufactured by Wyatt Technology under the conditions of a column temperature of 40°C and a flow rate of 0.7 mL / min. Polyethylene oxide and polyethylene glycol are used as standard samples.

[0027] The contact angle of the relief of the printing plate of the present invention with 1-hexadecene is preferably 40° or more and 70° or less. 1-Hexadecene is a solvent contained in inks generally used in dry offset printing, and in the present invention, the contact angle with 1-hexadecene is an index of ink repellency with respect to inks for dry offset printing. When the contact angle is 40° or more, the ink transferability can be further improved due to the excellent ink repellency of the relief. The contact angle is more preferably 43° or more. On the other hand, when the contact angle is 70° or less, the ink repellency of the relief is appropriately suppressed, and the ink can be efficiently supplied to the relief. The contact angle is more preferably 60° or less. The contact angle of the relief with 1-hexedecene can be measured using a contact angle meter DMe-201 (manufactured by Kyowa Interface Science Co., Ltd.). At room temperature, 1 μL of 1-hexadecene is dropped onto the relief surface, and the contact angle is measured 5 times 50 seconds after the drop is dropped, and the arithmetic average value is calculated. In addition, as a means for adjusting the contact angle to 1-hexadecene to the above range, for example, the content of the fluorine-containing organic compound may be adjusted to the above-mentioned preferable range.

[0028] The Shore D hardness of the relief of the printing plate of the present invention is preferably 40° or more and 80° or less. When the Shore D hardness is 40° or more, the crushing of fine images can be further suppressed, and the printing reproducibility can be further improved. The Shore D hardness is more preferably 50° or more. On the other hand, when the Shore D hardness is 80° or less, scratches on the inker or blanket can be suppressed. The Shore D hardness is more preferably 70° or less. The Shore D hardness of the relief can be measured using a Type D durometer GS-702N (manufactured by Tecrock) in accordance with JIS K 7215 (1986). The Shore D hardness of a laminate having a relief laminated to a thickness of 6 mm or more is measured six times, and the arithmetic average value is calculated. As a means for adjusting the Shore D hardness to the above range, for example, a printing plate precursor for dry offset printing having a photosensitive resin layer of a preferred composition described later can be used.

[0029] The film thickness change rate when the relief of the printing plate of the present invention is immersed in 1-hexedecene at 50° C. for 24 hours is preferably within ±2%. If the film thickness change rate is within ±2%, the relief shape can be maintained even in long-run printing, and the suitability for long-run printing can be further improved. The film thickness change rate is more preferably within ±0.5%. The film thickness change rate (%) of the relief can be calculated by {(film thickness after immersion-film thickness before immersion) / film thickness before immersion}×100. The film thickness before and after immersion is measured at the same position for each of six points, and the arithmetic average value of the film thickness change rates at the six points is calculated. As a means for setting the film thickness change rate within the above range, for example, a printing plate precursor for dry offset printing having a photosensitive resin layer of a preferred composition described later can be used.

[0030] Next, the printing plate precursor for dry offset printing of the present invention (hereinafter, sometimes simply referred to as "printing plate precursor") will be described. The printing plate precursor of the present invention has a photosensitive resin layer containing a fluorine-containing organic compound on a support. The support and the fluorine-containing organic compound are the same as the support and the fluorine-containing organic compound in the printing plate of the present invention. The content of the fluorine-containing organic compound in the photosensitive resin layer is preferably 0.1 to 10% by weight, more preferably 0.3 to 5% by weight.

[0031] The photosensitive resin layer preferably contains a polymer for forming a relief. The polymer is the same as that contained in the relief of the printing plate, and is preferably a partially saponified polyvinyl acetate or a polyamide having a tertiary amino group.

[0032] The partially saponified polyvinyl acetate preferably has an ethylenic double bond in the side chain. When a relief is formed by photolithography, the ethylenic double bond forms a covalent bond by exposure, so that the relief shape can be maintained at the time of printing. Examples of groups having an ethylenic double bond include a vinyl group, an acryloyl group, and a methacryloyl group.

[0033] Methods for introducing ethylenic double bonds into partially saponified polyvinyl acetate include, for example, (1) a method in which the hydroxyl groups of the partially saponified polyvinyl acetate are reacted with an acid anhydride, and a reactive group such as a carboxyl group is introduced into the polymer side chain starting from the hydroxyl group of the partially saponified polyvinyl acetate, and an unsaturated epoxy compound is reacted with the reactive group; and (2) a method in which a copolymer of vinyl acetate and an unsaturated carboxylic acid, an unsaturated carboxylate, and / or an unsaturated carboxylate ester is partially saponified, and the carboxyl groups of this polymer are reacted with an unsaturated epoxy compound.

[0034] The content of the polymer in the photosensitive resin layer is preferably 30 to 95% by weight.

[0035] The photosensitive resin layer preferably further contains a monomer having an ethylenically unsaturated group, a photopolymerization initiator, and the like.

[0036] Examples of monomers having an ethylenically unsaturated group include (meth)acrylates described in International Publication No. 2017 / 038970, glycerol di(meth)acrylate, (meth)acrylic acid adduct of propylene glycol diglycidyl ether, and tetrahydrofurfuryl (meth)acrylate. Two or more of these may be contained. Here, (meth)acrylate is a general term for acrylate and methacrylate, and (meth)acrylic acid is a general term for acrylic acid and methacrylic acid. The molecular weight of the monomer having an ethylenically unsaturated group is preferably 10,000 or less, more preferably 1,000 or less.

[0037] The content of the monomer component having an ethylenically unsaturated group in the photosensitive resin layer is preferably from 10 to 70% by weight.

[0038] As the photopolymerization initiator, one having a function of generating radicals by self-decomposition or hydrogen abstraction due to light absorption is preferably used. For example, benzoin alkyl ethers, benzophenones, anthraquinones, benzils, acetophenones, diacetyls, etc. may be mentioned. Two or more of these may be contained.

[0039] The content of the photopolymerization initiator in the photosensitive resin layer is preferably 0.1 to 10% by weight.

[0040] The photosensitive resin layer may contain, as necessary, a compatible auxiliary, a polymerization inhibitor, a dye, a pigment, a surfactant, an antifoaming agent, an ultraviolet absorbing agent, a fragrance, and the like.

[0041] By including a compatibility aid in the photosensitive resin layer, the compatibility of the components constituting the photosensitive resin layer can be increased, the bleeding out of low molecular weight components can be suppressed, and the flexibility of the photosensitive resin layer can be improved. Examples of the compatibility aid include polyhydric alcohols such as ethylene glycol, diethylene glycol, triethylene glycol, glycerin, trimethylolpropane, trimethylolethane, pentaerythritol, and derivatives thereof. The content of the compatibility aid in the photosensitive resin layer is preferably 30% by weight or less, and the Shore D hardness of the relief and the film thickness change rate with respect to 1-hexedecene can be easily adjusted to the above-mentioned preferred range. The content of the compatibility aid is more preferably 10% by weight or less.

[0042] By including a polymerization inhibitor in the photosensitive resin layer, the thermal stability can be improved. Examples of the polymerization inhibitor include phenols, hydroquinones, catechols, and hydroxylamine derivatives. Two or more of these may be included. The content of the polymerization inhibitor in the photosensitive resin layer is preferably 0.001 to 5% by weight.

[0043] The photosensitive resin printing plate precursor may have, in addition to the above-mentioned support and photosensitive resin layer, a cover film or a heat-sensitive mask layer on the photosensitive resin layer, if necessary.

[0044] By providing a cover film on the photosensitive resin layer, the surface of the photosensitive resin layer can be protected and adhesion of foreign matter, etc. The photosensitive resin layer and the cover film may be in direct contact with each other, or one or more layers such as an anti-adhesive layer may be provided between the photosensitive resin layer and the cover film.

[0045] Examples of the cover film include plastic sheets made of polyester, polyethylene, polypropylene, etc. The thickness of the cover film is preferably 10 to 150 μm from the viewpoint of handling and flexibility. The surface of the cover film may be roughened to improve adhesion to the original film. Examples of methods for roughening the surface include sandblasting, chemical etching, and coating with a coating agent containing matte particles.

[0046] In addition, when the printing plate precursor of the present invention is used in a so-called CTP plate making method in which laser irradiation is performed based on image data controlled by a digital device, an image mask is formed on the spot from the mask layer element, and exposed and developed, the printing plate precursor may further have a heat-sensitive mask layer. The heat-sensitive mask layer is preferably one that effectively blocks ultraviolet light, absorbs infrared laser light during drawing, and is instantly sublimated or ablated in part or in whole by the heat. This creates a difference in optical density between the laser irradiated part and the non-irradiated part, allowing it to function similarly to a conventional original film. When the printing plate precursor has a heat-sensitive mask layer, it may have an adhesion adjustment layer between the photosensitive resin layer and the heat-sensitive mask layer, and may have a peeling auxiliary layer between the heat-sensitive mask layer and the cover film.

[0047] Examples of the heat-sensitive mask layer, adhesion adjustment layer, and peeling auxiliary layer include those described in WO 2017 / 038970.

[0048] Next, the method for producing the printing plate precursor of the present invention will be described. A photosensitive resin layer can be formed by casting a photosensitive resin composition solution, in which the above-mentioned organic compound containing fluorine and, if necessary, a polymer, a monomer having an ethylenically unsaturated group, a photopolymerization initiator, etc. are dissolved in an organic solvent such as water or a lower alcohol, on a support, and drying the solution. Furthermore, a cover film or a heat-sensitive mask layer may be formed on the photosensitive resin layer. For example, a method for forming a heat-sensitive mask layer on a photosensitive resin layer includes a method in which a cover film is coated with a heat-sensitive mask layer, and a structure consisting of a cover film / heat-sensitive mask layer is adhered to the photosensitive layer.

[0049] Next, a method for producing the printing plate of the present invention from the printing plate precursor of the present invention will be described. The method preferably includes an exposure step of partially photocuring the photosensitive resin layer of the printing plate precursor, and a development step of removing the uncured parts of the photosensitive resin layer.

[0050] In the exposure step, if a cover film is present, it is preferable to peel off the photosensitive resin layer, adhere a negative or positive original film to the photosensitive resin layer, irradiate ultraviolet light with a wavelength of 300 to 400 nm, and photocure the exposed part of the photosensitive resin layer. If a heat-sensitive mask layer is present, it is preferable to form a negative or positive image on the heat-sensitive mask layer and irradiate ultraviolet light through it. Examples of the exposure light source include a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a xenon lamp, a carbon arc lamp, a chemical lamp, and a UV-LED lamp.

[0051] In the developing step, it is preferable to remove the photosensitive resin layer in the unexposed areas with water and / or an organic solvent. Examples of the developing device include a spray type developing device and a brush type washing machine.

[0052] Furthermore, if necessary, a post-exposure step of irradiating with ultraviolet light after development may be carried out, which makes it possible to make the relief stronger by reaction of unreacted monomer components through the post-exposure step.

[0053] It is preferable to use the printing plate of the present invention to perform offset printing on a container having a curved surface. As the ink for offset printing, it is preferable to use an ink containing an alkyd resin. Inks containing alkyd resins have excellent weather resistance and can be suitably used for containers exposed to the external environment. EXAMPLES

[0054] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto. Evaluation methods in the examples and comparative examples are described below. It should be noted that Example 9 described below should be read as a comparative example, and the evaluation result of the bleed-out of Example 9 should be read as "0.120 C."

[0055] (1) Contact angle 1 μL of 1-hexedecene was deposited at room temperature on the solid surface of the printing plate obtained in each Example and Comparative Example, and the contact angle 50 seconds after deposition was measured five times using a contact angle meter "DMe-201" (manufactured by Kyowa Interface Science Co., Ltd.), and the arithmetic average value was recorded as the contact angle.

[0056] (2) Shore D hardness The relief was peeled off from the support of the printing plate obtained in each of the Examples and Comparative Examples, and laminated to a thickness of 6 mm or more. The Shore D hardness of the laminate was measured six times using a Type D durometer GS-702N (manufactured by Techclock) in accordance with JIS K 7215, and the arithmetic average value was taken as the Shore D hardness of the relief.

[0057] (3) Bleeding out A piece of "GATSBY" (registered trademark) oil blotting paper film type (manufactured by Mandom) was cut into a piece of 2 cm x 2 cm, and its weight was measured. The weight of the "GATSBY" oil blotting paper film type (manufactured by Mandom) was measured and attached to the surface of the printing plate obtained in each of the Examples and Comparative Examples, and after absorbing the bleed-out components, the weight was similarly measured. The amount of bleed-out was calculated from the change in weight before and after absorption of the bleed-out components (weight after absorption - weight before absorption). Bleed-out was evaluated according to the following criteria. A: Less than 0.02g B: 0.02g or more but less than 0.1g C: 0.1g or more.

[0058] (4) Ink transferability For the printing plates obtained in each of the Examples and Comparative Examples, printing was performed on aluminum cans using a printing proofing machine (InterCan), AIR-TACK FS (Kinyosha) as the blanket, and EXP6448 Indigo (Matsukagaku Co., Ltd.) as the ink. At this time, the pressing amount of the printing plate onto the blanket was adjusted to 100 μm. The ink concentration of the aluminum can of a 2 cm x 2 cm solid image was measured at four points using SpectroEye (X-rite), and the arithmetic average value was taken as the ink concentration. The higher the ink concentration, the better the ink transferability.

[0059] (5)Printing reproducibility For the printing plates obtained in each of the Examples and Comparative Examples, printing was performed on aluminum cans under the conditions described in (4) Ink transferability. The line width of the printed matter corresponding to the relief with a line width of 50 μm was measured at five points at a magnification of 200 times using a digital microscope VHX-2000 (manufactured by Keyence), and the print reproducibility was evaluated from the arithmetic average value. If the line width of the printed matter was 65 μm or less, it was marked as ○, and if it was greater than 65 μm, it was marked as ×.

[0060] (6) Suitable for long-run printing The solid portion of the printing plate obtained in each Example and Comparative Example was cut into 20 mm x 20 mm samples, and the film thicknesses T1 to T6 were measured at six randomly selected points using a Digimatic Thickness Gauge (manufactured by Mitutoyo). The sample was then immersed in 1-hexedecene at 50°C for 24 hours, and the film thicknesses T1' to T6' at the same points were measured. The film thickness change rate at each measurement point was calculated using the following formula, and the suitability for long-run printing was evaluated from the arithmetic average value. Film thickness change rate (%) = (T1'-T1) / T1 x 100 If the rate of change in film thickness is within ±2%, the film is excellent in suitability for long-run printing, and if it is within ±0.5%, this is even more preferable.

[0061] Next, the methods for producing the materials used in the examples and comparative examples will be described.

[0062] <Preparation of a support having an easy-adhesion layer> A mixture of 260 parts by mass of "Vylon" (registered trademark) 31SS (toluene solution of unsaturated polyester resin, manufactured by Toyobo Co., Ltd.) and 2 parts by mass of PS-8A (benzoin ethyl ether, manufactured by Wako Pure Chemical Industries, Ltd.) was heated at 70°C for 2 hours, cooled to 30°C, and 7 parts by mass of ethylene glycol diglycidyl ether dimethacrylate was added and mixed for 2 hours. Furthermore, 25 parts by mass of "Coronate" (registered trademark) 3015E (ethyl acetate solution of polyisocyanate resin, manufactured by Tosoh Co., Ltd.) and 14 parts by mass of EC-1368 (industrial adhesive, manufactured by Sumitomo 3M Co., Ltd.) were added and mixed to obtain coating solution 1 for easy adhesion layer.

[0063] Next, 50 parts by mass of "GOHSENOL" (registered trademark) KH-17 (polyvinyl alcohol with a saponification degree of 78.5 to 81.5 mol%, manufactured by Mitsubishi Chemical Corporation) was mixed in a mixed solvent of 200 parts by mass of "SOLMIX" (registered trademark) H-11 (alcohol mixture, manufactured by Nippon Alcohol Co., Ltd.) and 200 parts by mass of water at 70°C for 2 hours, and then 1.5 parts by mass of "BLEMMER" (registered trademark) G (glycidyl methacrylate, manufactured by Nippon Oil & Fats Corporation) was added and mixed for 1 hour. To this was further added 3 parts by weight of a copolymer having a weight ratio of (dimethylaminoethyl methacrylate) / (2-hydroxyethyl methacrylate) of 2 / 1 (manufactured by Kyoeisha Chemical Co., Ltd.), 5 parts by weight of "Irgacure" (registered trademark) 651 (benzyl methyl ketal, manufactured by Ciba-Geigy Corporation), 21 parts by weight of Epoxy Ester 70PA (acrylic acid adduct of propylene glycol diglycidyl ether, manufactured by Kyoeisha Chemical Co., Ltd.), and 20 parts by weight of ethylene glycol diglycidyl ether dimethacrylate, and mixed for 90 minutes. After cooling to 50°C, 0.1 parts by weight of "Megafac" (registered trademark) F-556 (manufactured by DIC Corporation) was added and mixed for 30 minutes to obtain coating liquid 2 for the easy-adhesion layer.

[0064] On a chrome-plated steel plate having a thickness of 250 μm, the above-mentioned coating liquid 1 for easy adhesion layer was applied using a bar coater so that the film thickness after drying would be 40 μm, and the solvent was removed by heating for 3 minutes in an oven at 180° C. On top of that, the above-mentioned coating liquid 2 for easy adhesion layer was applied using a bar coater so that the film thickness after drying would be 30 μm, and the coating was heated for 3 minutes in an oven at 160° C. to obtain a support having an easy adhesion layer.

[0065] <Cover film production> A 100 μm-thick "Lumilar" (registered trademark) S10 (polyester film, manufactured by Toray Industries, Inc.) roughened to a surface roughness Ra of 0.1 to 0.6 μm was coated with "GOHSENOL" (registered trademark) AL-06 (partially saponified polyvinyl alcohol with a saponification degree of 91 to 94 mol%, manufactured by Mitsubishi Chemical Corporation) to a dry thickness of 1 μm, and dried at 100° C. for 25 seconds to obtain a cover film.

[0066] <Synthesis of polymer for photosensitive resin layer> Synthesis example 1: Partially saponified polyvinyl alcohol "GOHSENOL" KL-05 (average polymerization degree 500, saponification degree 80 mol%, Mw = 38,000) manufactured by Mitsubishi Chemical Corporation was swollen in acetone, and 4.2 parts by mass of succinic anhydride were added to 100 parts by mass of "GOHSENOL" KL-05, and the mixture was stirred at 60°C for 6 hours to add a carboxyl group to the molecular chain. The polymer was washed with acetone to remove unreacted succinic anhydride, and then dried. 100 parts by mass of this polymer was dissolved at 80°C in 200 parts by mass of a mixed solvent of ethanol / water = 30 / 70 (weight ratio). 6 parts by mass of glycidyl methacrylate were added thereto to introduce an ethylenic double bond into the partially saponified polyvinyl alcohol, thereby obtaining polymer A. The ethylenic double bond equivalent of the obtained polymer A was 5,611 g / eq, and the weight average molecular weight was 40,000. The weight average molecular weight was measured using a gel permeation chromatograph-multiangle light scattering photometer manufactured by Wyatt Technology under the conditions of a column temperature of 40° C. and a flow rate of 0.7 mL / min, using polyethylene oxide and polyethylene glycol as standard samples. The ethylenic double bond equivalent was measured using polymer A as an internal standard and sodium 3-(trimethylsilyl)propionate-2,2,3,3d 4 Dissolve 30 mg in 1 ml of heavy water / heavy methanol mixed solvent containing 1 H-NMR measurement was performed to measure the number of moles of ethylenic double bonds. The ethylenic double bond equivalent was calculated by dividing the polymer A in the sample used for the analysis by the number of moles of the detected ethylenic double bonds.

[0067] Synthesis example 2: 20 parts by mass of ε-caprolactam, 80 parts by mass of nylon salt of N-(2-aminoethyl)piperazine and adipic acid, and 100 parts by mass of water were placed in a stainless steel autoclave, and the air inside was replaced with nitrogen gas, and then the autoclave was heated at 180°C for 1 hour, and then the water was removed to obtain a water-soluble polyamide resin, a polyamide having a tertiary amino group, polymer B. The weight-average molecular weight of the obtained polymer B was 72,000. The weight-average molecular weight was measured in the same manner as in Synthesis Example 1.

[0068] As other components, the compounds shown in Tables 1 and 2 were used.

[0069] [Example 1] <Preparation of Photosensitive Resin Layer> Polymers A and B and a mixed solvent of ethanol / water = 30 / 70 (weight ratio) were added in the amounts shown in Table 1 to a three-necked flask equipped with a stirring spatula and a cooling tube, and dissolved by heating at 90 ° C for 2 hours. After cooling the resulting mixture to 70 ° C, the other components shown in Table 1 were added and stirred for 30 minutes to obtain a solution for a photosensitive resin layer. The solution for a photosensitive resin layer obtained as described above was cast onto the easy-adhesion layer side of the support having the easy-adhesion layer, and dried at 60 ° C for 2.5 hours to form a photosensitive resin layer of a printing plate precursor. At this time, the plate thickness after drying (chrome-plated steel plate + photosensitive resin layer) was adjusted to be 0.84 mm.

[0070] A mixed solvent of water / ethanol = 50 / 50 (weight ratio) was applied onto the photosensitive resin layer thus obtained, and the cover film for the analog plate was pressed onto the surface to obtain a photosensitive resin printing plate precursor.

[0071] Exposure and development were carried out using a batch-type exposure and development machine "Tomiflex" (manufactured by Tomihaku Sangyo Co., Ltd.) as follows. First, the cover film of the obtained photosensitive resin plate precursor was peeled off, and a negative film on which a predetermined image was formed was vacuum-attached to the exposed photosensitive resin layer using a vinyl chloride film, and then the integrated light amount was 8,000 mJ / cm 2 The film was exposed to light so that the accumulated light intensity was about 8,000 mJ / cm 2 in the atmosphere. Then, the film was developed for 60 seconds with tap water adjusted to a temperature of 25°C. After that, the film was dried in an oven at 60°C for 10 minutes and then exposed to light so that the accumulated light intensity was about 8,000 mJ / cm 2 in the atmosphere. 2 The resulting printing plate was evaluated by the above-mentioned method, and the results are shown in Table 1.

[0072] [Examples 2 to 10] A printing plate was obtained in the same manner as in Example 1, except that the composition of the photosensitive resin layer was changed as shown in Table 1. The evaluation results are shown in Table 1.

[0073] [Comparative Example 1] A printing plate was obtained in the same manner as in Example 1, except that the composition of the photosensitive resin layer was changed as shown in Table 1. The evaluation results are shown in Table 1.

[0074] In addition, in the evaluation of (4) ink transfer and (5) print reproducibility, when the amount of pressing of the printing plate against the blanket was changed to 200 μm, the ink transfer and print reproducibility were evaluated, and the ink concentration was 2.0 and the line width was 80 μm.

[0075] The photosensitive resin layer compositions and evaluation results of each of the examples and comparative examples are shown in Tables 1 and 2.

[0076] [Table 1]

[0077] [Table 2]

Claims

1. A printing plate for dry offset printing having a relief on a support, the relief containing a fluorine-containing organic compound, the relief containing partially saponified polyvinyl acetate and / or a polyamide having basic nitrogen, and the fluorine-containing organic compound having an ionic group and / or an ethylene glycol chain.

2. 2. The printing plate for dry offset printing according to claim 1, wherein the relief contains 0.1 to 10% by weight of a fluorine-containing organic compound.

3. 3. The printing plate for dry offset printing according to claim 1, wherein the contact angle of the relief with 1-hexadecene is from 40° to 70°.

4. 4. The printing plate for dry offset printing according to claim 1, wherein the relief has a Shore D hardness of 40° or more and 80° or less.

5. A method for producing a printed matter, comprising printing on a container having a curved surface using a printing plate for dry offset printing described in any one of claims 1 to 4.

6. A method for producing a printed matter as described in claim 5 using an ink containing an alkyd resin.

7. A printing plate precursor for dry offset printing having on a support a photosensitive resin layer containing a fluorine-containing organic compound, wherein the photosensitive resin layer contains partially saponified polyvinyl acetate and / or a polyamide having basic nitrogen, and the fluorine-containing organic compound has an ionic group and / or an ethylene glycol chain.

8. A method for manufacturing a printing plate for dry offset printing described in any one of claims 1 to 4, comprising an exposure step for partially photo-curing the photosensitive resin layer of the printing plate precursor for dry offset printing described in claim 7, and a development step for removing the uncured portions of the photosensitive resin layer with a developer.

Citation Information

Patent Citations

  • Waterless planographic printing original plate

    JP1996227149A

  • Waterless plate ink composition

    JP1996325499A

  • Negative image recording material

    JP1999231509A

  • Plate making method for planographic printing plate without dampening water

    JP2002131894A

  • Pattern forming body and pattern forming method

    JP2002274077A