Nozzle, developing device, and processing method for processed object
The nozzle with an annular injection port and cylindrical housing addresses dimensional variations in resist patterns by uniformly spraying developer and gas, enhancing processing accuracy and precision in developing devices.
Patent Information
- Application Number
- JP2020198652
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-11-30
AI Technical Summary
Existing developing devices inject developer in directions that cause variations in resist pattern dimensions, leading to inaccuracies in processing depending on the in-plane direction, especially when high accuracy is required.
A nozzle with an annular injection port and a cylindrical housing that sprays developer and compressed gas uniformly around a central axis, combined with a diffusion plate and inclined surfaces to ensure even distribution and minimize swelling, allowing for precise and uniform processing.
The nozzle ensures uniform development of resist films and etching processes, improving processing accuracy and precision by uniformly supplying developer in a controlled manner, reducing swelling and enhancing pattern uniformity.
Smart Images

Figure 0007585745000001 
Figure 0007585745000002 
Figure 0007585745000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a nozzle, a developing device, and a method for processing an object to be processed. [Background technology]
[0002] Patent Document 1 describes a developing device that supplies a developer to a resist film formed on the surface of a workpiece to develop the resist film. This developing device has a nozzle including a horizontally long slit-shaped injection port, and sprays the developer together with high-pressure air from the nozzle in a direction inclined to the short side direction of the injection port to form a resist pattern on the workpiece. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5153332 Summary of the Invention [Problem to be solved by the invention]
[0004] As described above, in the nozzle described in Patent Document 1, the developer is sprayed in a direction inclined to the short side direction of the nozzle, thereby promoting the development of the resist film in the short side direction. On the other hand, in the longitudinal direction of the nozzle, the developer is supplied from a direction approximately perpendicular to the resist film, thereby suppressing the progress of the development of the resist film. Therefore, when the development process is performed using the nozzle described in Patent Document 1, the pattern dimensions of the resist pattern may differ in the longitudinal direction and the short side direction of the nozzle. When the processed object is processed using such a resist pattern, the processing accuracy of the processed object may vary depending on the in-plane direction. Therefore, when high accuracy is required for processing the processed object, it may be difficult to process the processed object with the required accuracy.
[0005] Therefore, an object of the present disclosure is to improve the uniformity of processing of a workpiece. [Means for solving the problem]
[0006] In one aspect, a nozzle for spraying a treatment liquid is provided. The nozzle includes a cylindrical housing having a central axis. The housing has a liquid supply port for supplying the treatment liquid into the housing, a gas supply port for supplying compressed gas into the housing, and a spray port for spraying the treatment liquid together with the compressed gas. The spray port has an annular shape centered on the central axis.
[0007] The nozzle according to the above aspect has an injection port having an annular shape, and the processing liquid introduced from the liquid supply port and the compressed gas introduced from the gas supply port are injected from the injection port. Since the processing liquid is injected uniformly in the circumferential direction around the central axis from the injection port having an annular shape, the variation in processing accuracy in the circumferential direction is suppressed. Therefore, the uniformity of processing of the workpiece can be improved.
[0008] The nozzle of one embodiment is a rod member disposed between the liquid supply port and the jet port in the direction of extension of the central axis, and further includes the rod member having an inclined surface whose diameter increases toward the jet port side, and a fluid passage for guiding the processing liquid supplied from the liquid supply port and the compressed gas supplied from the gas supply port to the jet port may be formed between the inner peripheral surface of the housing and the inclined surface. The processing liquid and the compressed gas that flow into the fluid passage formed between the inner peripheral surface of the housing and the rod member are guided along the inclined surface of the rod member and are jetted from the jet port. As a result, the processing liquid is jetted in a direction inclined with respect to the central axis, so that the processing liquid can be evenly supplied to the side wall surface of the opening of the processing object. As a result, the processing accuracy of the processing object can be improved.
[0009] In one embodiment, the nozzle may be configured to spray the treatment liquid from the nozzle in a mist form. By spraying the treatment liquid in a mist form, the treatment liquid can be easily supplied to the inside of the opening of the treatment object, thereby further improving the processing accuracy of the treatment object.
[0010] In one embodiment, the apparatus may further include a liquid supply pipe that introduces the treatment liquid into the housing along the central axis, and a diffusion plate that diffuses the treatment liquid flowing through the liquid supply pipe, the diffusion plate having a plurality of openings arranged in a circumferential direction around the central axis. In this embodiment, the treatment liquid that has flowed through the liquid supply pipe collides with the diffusion plate and is diffused, and then is guided to the fluid passage together with the compressed air. By introducing the treatment liquid thus diffused into the fluid passage, the uniformity of the treatment liquid sprayed from the spray port can be improved.
[0011] In one embodiment, the processing liquid may be a developer for developing a resist film or an etching liquid for etching the workpiece. By spraying the developer or the etching liquid onto the workpiece from the nozzle, the workpiece can be processed with high uniformity.
[0012] In one aspect, a developing apparatus for developing a resist film formed on a target object is provided, the developing apparatus including a processing vessel, the nozzle disposed in the processing vessel, a transport mechanism for moving the target object in the processing vessel relative to the nozzle, a developing solution supplying device for supplying a developing solution as a processing liquid to the nozzle, and a compressed gas supplying device for supplying a compressed gas to the nozzle.
[0013] In the developing device according to the above aspect, the developing solution is sprayed onto the workpiece together with the compressed gas from the nozzle, so that the resist film can be developed with high uniformity.
[0014] In one embodiment, the developer supplying device may supply the developer heated to 40° C. or higher to the nozzle. By supplying the developer heated to 40° C. or higher to the nozzle, the resist film can be effectively developed.
[0015] In one embodiment, a recovery device may be further provided that recovers the gas containing the developer from inside the processing container and separates the gas and liquid. By separating the gas containing the developer into gas and liquid by the recovery device, the developer can be recovered from the gas.
[0016] A method for processing a workpiece according to one embodiment includes the steps of forming a photosensitive resist film on the workpiece, exposing the resist film to light, and spraying a developer together with compressed gas from a nozzle having a circular injection port onto the exposed resist film to form a resist pattern.
[0017] In the processing method according to the above aspect, a resist pattern is formed by spraying a developer from a nozzle having an annular injection port. The developer is sprayed uniformly from the annular injection port in the circumferential direction of the injection port, so that the resist film can be developed with high uniformity. By using the resist pattern thus formed, the uniformity of processing of the workpiece can be improved.
[0018] In one embodiment, the developer may be sprayed in a mist form from the spray nozzle. By spraying the developer in a mist form, swelling of the resist film can be suppressed, and the developer can be easily supplied to the inside of the openings in the resist film. Therefore, a pattern can be formed in the resist film with high accuracy.
[0019] In one embodiment, the developer may be sprayed in a spray pattern that is annular when viewed from a direction along the central axis of the spray nozzle and has a diameter that increases with distance from the spray nozzle. By spraying the developer in such a spray pattern, a pattern can be formed on the resist film with high uniformity and high precision.
[0020] In one embodiment, the spray direction of the developer may be inclined at an angle of 10° or less with respect to the central axis. By spraying the developer in a direction inclined at an angle of 10° or less with respect to the central axis, the developer can be evenly supplied to the side wall surface of the opening of the resist film, so that a pattern can be formed in the resist film with high accuracy.
[0021] In one embodiment, the method may further include a step of spraying an abrasive onto the workpiece through the resist pattern to remove a portion of the workpiece. By processing the workpiece using the resist pattern formed by the above-mentioned method, the workpiece can be processed with high uniformity.
[0022] In one embodiment, the method further includes a step of spraying an etching solution onto the workpiece through the resist pattern from a nozzle to remove a portion of the workpiece. By spraying the etching solution using the nozzle, the workpiece can be processed with high uniformity.
[0023] In one embodiment, the method may further include a step of supplying a stripping liquid to the resist pattern to remove the resist pattern from the object to be processed. Effect of the Invention
[0024] According to one aspect and various embodiments of the present invention, it is possible to improve the uniformity of processing of a workpiece. [Brief description of the drawings]
[0025] [Figure 1] FIG. 2 is a diagram illustrating a development device according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a perspective view of a nozzle according to an embodiment. [Diagram 3] FIG. 2 is a cross-sectional view of a nozzle according to an embodiment. [Figure 4] FIG. [Diagram 5] FIG. [Figure 6] 6 is a cross-sectional view of the jet of developer taken along line VI-VI in FIG. 2. [Figure 7] FIG. 4 is a diagram showing a scanning direction of a nozzle relative to a processing object. [Figure 8] 1A and 1B are diagrams showing a state in which a part of the resist film is removed by a development process. [Figure 9] 1 is a flowchart showing a method for processing a target object according to an embodiment. [Figure 10] 1A to 1C are diagrams illustrating a process of forming a resist film. [Figure 11] 1A to 1C are diagrams illustrating a step of exposing a resist film. [Figure 12] 1A to 1C are diagrams illustrating a process of developing a resist film. [Figure 13] FIG. 1 is a diagram showing a process of blasting a processing object. [Figure 14] 1A to 1C are diagrams illustrating a step of removing the resist pattern. [Figure 15] 1(a) is an SEM photograph showing the resist pattern formed in Comparative Example 1, and FIG. 1(b) is an SEM photograph showing the resist pattern formed in Example 1. [Figure 16] 1A is an SEM photograph showing the resist pattern formed in Comparative Example 2, and FIG. 1B is an SEM photograph showing the resist pattern formed in Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. In the following description, the same or corresponding elements are given the same reference numerals, and overlapping descriptions will not be repeated. The dimensional ratios of the drawings do not necessarily match those in the description. In the following description, a photosensitive film to which a pattern is transferred by exposure is referred to as a resist film, and a film in which an opening having a shape corresponding to the pattern transferred to the resist film is formed by developing the resist film is referred to as a resist pattern.
[0027] Fig. 1 is a schematic diagram of a developing device 100 according to an embodiment. The developing device 100 shown in Fig. 1 is a developing device that develops a resist film on which a pattern has been exposed by photolithography, for example. In the following description, the movement direction of a nozzle 2 (described later) is defined as the X direction, the transport direction of a target object 10 (described later) is defined as the Y direction, and the direction perpendicular to the X direction and the Y direction is defined as the Z direction.
[0028] As shown in FIG. 1, the developing device 100 includes a processing container 1, a nozzle 2, a processing object transport mechanism 3, a nozzle transport mechanism 4, a developer supplying device 5, a compressed air supplying device (compressed gas supplying device) 6, and a recovery device .
[0029] The processing vessel 1 defines a developing chamber S1 therein. A processing target object 10, which is an object to be processed, is placed in the developing chamber S1. The processing target object 10 is, for example, a processed substrate such as a printed circuit board, a silicon substrate, a glass substrate, a metal substrate, or the like, and may be an intermediate product in which a predetermined process is performed on such a processed substrate. A resist film 12 to which a predetermined pattern is transferred is formed on the surface of the processing target object 10. The resist film 12 is, for example, a photosensitive dry film resist.
[0030] The nozzle 2 is disposed in the developing chamber S1 with an ejection port 20, which will be described later, facing the workpiece 10. The nozzle 2 ejects a developer 14 as a processing liquid onto the resist film 12 formed on the workpiece 10. The developing device 100 may include a plurality of nozzles 2.
[0031] The above-mentioned object transport mechanism 3 and nozzle transport mechanism 4 constitute a transport device that moves the object 10 to be processed relative to the nozzle 2 in the developing chamber S1. The object transport mechanism 3 supports the object 10 to be processed in the developing chamber S1. The object transport mechanism 3 is, for example, a belt conveyor device, and transports the object 10 to be processed placed thereon in the Y direction.
[0032] The nozzle transport mechanism 4 holds the nozzle 2 in the developing chamber S1. The nozzle transport mechanism 4 includes a rail 41 extending in the X direction, for example, a holding member 42 that holds the nozzle 2, and a drive unit 43 that drives the holding member 42. The nozzle transport mechanism 4 moves the holding member 42 along the rail 41 by the driving force of the drive unit 43, thereby transporting the nozzle 2 in the X direction.
[0033] The developing device 100 may include either a workpiece transport mechanism 3 or a nozzle transport mechanism 4 as a transport device, and may move only the workpiece 10 or the nozzle 2 in the X direction and Y direction, or may include both a workpiece transport mechanism 3 and a nozzle transport mechanism 4, and may move both the workpiece 10 and the nozzle 2.
[0034] The developer supplying device 5 stores the developer 14 for developing the resist film 12 under high pressure and high temperature conditions. The developer 14 contains, for example, an aqueous sodium carbonate solution. A pipe 51 is connected to the developer supplying device 5, and the developer supplying device 5 supplies the developer 14 to the nozzle 2 through the pipe 51. The developer supplying device 5 may pressure-feed the developer 14 heated to 40° C. or higher to the nozzle 2.
[0035] The compressed air supplying device 6 includes, for example, a compressor, and supplies compressed air (compressed gas) 15 to the nozzle 2 through the piping 52. The pressure of the compressed air 15 supplied from the compressed air supplying device 6 to the nozzle 2 may be slightly lower than the pressure of the developer 14 supplied from the developer supplying device 5 to the nozzle 2. The amount of developer 14 sprayed from the nozzle 2 is adjusted by adjusting the pressure difference between the pressure of the compressed air 15 supplied to the nozzle 2 and the pressure of the developer 14 supplied to the nozzle 2. The amount of developer 14 sprayed increases as the pressure difference between the pressure of the compressed air 15 supplied to the nozzle 2 and the pressure of the developer 14 supplied to the nozzle 2 increases. For example, this pressure difference may be set to 0.01 MPa or more and 0.05 MPa or less. The compressed air supplying device 6 may supply a gas other than air to the nozzle 2.
[0036] The recovery device 7 recovers the gas containing the developer 14 from the developing chamber S1 and separates the gas and liquid. As shown in FIG. 1, the recovery device 7 includes a gas-liquid separator 61. The gas-liquid separator 61 is, for example, a cyclone type gas-liquid separator, and is connected to the developing chamber S1 via a pipe 53 and to a blower 62 via a pipe 54. When the resist film 12 is developed, the developer 14 and compressed air 15 are sprayed from the nozzle 2, increasing the internal pressure of the developing chamber S1. Therefore, it is required to make the developing chamber S1 negative pressure. The blower 62 sucks the gas in the gas-liquid separator 61 through the pipe 54. When the pressure in the gas-liquid separator 61 becomes negative pressure by the blower 62, the gas containing the developer 14 in the developing chamber S1 is sucked into the gas-liquid separator 61 through the pipe 53. The gas-liquid separator 61 includes a filter, and collects the developer 14 contained in the gas sucked by the filter, and recovers the collected developer 14 in a recovery tank 63. The developer 14 collected in the collection tank 63 is reused for the developing process of the resist film 12.
[0037] The developer 14 sprayed from the nozzle 2 is collected in a tank provided below the developing chamber S1. The developer 14 collected in the tank is discharged to the outside of the developing device 100 by a pump. The collected developer 14 may be returned to the developer supply device 5 and reused in the developing process of the resist film 12.
[0038] A nozzle according to an embodiment will be described in detail with reference to Figures 2 and 3. Figure 2 is a perspective view of the nozzle 2, and Figure 3 is a cross-sectional view taken along the central axis line AX of the nozzle 2. As shown in Figures 2 and 3, the nozzle 2 has an ejection port 20 having an annular shape, and ejects the developer 14 and compressed air 15 as a gas-liquid two-phase flow from the ejection port 20. In the following description, the direction on the ejection port 20 side may be referred to as the tip side of the nozzle 2, and the direction opposite to the ejection port 20 may be referred to as the base side of the nozzle 2.
[0039] As shown in FIG. 2 and FIG. 3, the nozzle 2 includes a cylindrical housing 22. The housing 22 has a cylindrical shape whose axis coincides with the central axis AX, and has a mixing chamber S2 inside. The housing 22 includes a base end 221, an intermediate portion 222, and a tip portion 223. The base end 221, the intermediate portion 222, and the tip portion 223 are arranged in this order from the base end side of the nozzle 2. The base end 221, the intermediate portion 222, and the tip portion 223 may be integrally formed, or may be configured as separate bodies and connected to each other. The inner peripheral surface 221s of the base end 221 has a substantially constant diameter in a direction parallel to the central axis AX. The inner peripheral surface 222s of the intermediate portion 222 gradually decreases in diameter toward the tip side of the nozzle 2. The inner peripheral surface 223s of the tip portion 223 gradually increases in diameter toward the tip portion of the nozzle 2. An inner circumferential surface 221s of the base end portion 221 and an inner circumferential surface 222s of the intermediate portion 222 define a mixing chamber S2. An inner circumferential surface 223s of the tip portion 223 defines a fluid passage 40, which will be described later.
[0040] The housing 22 is formed with a liquid supply port 24 for supplying the developer 14 into the housing 22 and a gas supply port 26 for supplying compressed air 15 into the housing 22. The liquid supply port 24 is formed on the central axis AX of the housing 22, and a liquid supply pipe 25 is inserted into the liquid supply port 24. The liquid supply pipe 25 provides an introduction path 28 for introducing the developer 14 along the central axis AX to the mixing chamber S2. The base end of the liquid supply pipe 25 is connected to a pipe 51. The tip end of the liquid supply pipe 25 is disposed in the mixing chamber S2. The developer 14 supplied from the developer supply device 5 is introduced to the mixing chamber S2 through the pipe 51 and the liquid supply pipe 25.
[0041] In one embodiment, a diffusion plate 30 for diffusing the developer 14 flowing through the liquid supply pipe 25 may be provided at the tip end of the liquid supply pipe 25. The diffusion plate 30 has a substantially circular plate shape and is disposed on the central axis AX.
[0042] Fig. 4 is a plan view of the diffusion plate 30. As shown in Fig. 4, the diffusion plate 30 is formed with a plurality of openings 32 through which the developer 14 can pass. These openings 32 are arranged at equal intervals along an imaginary circle C centered on the central axis line AX. The diffusion plate 30 diffuses the developer 14 flowing in the introduction path 28 in the direction of the central axis line AX, and sprays it from the plurality of openings 32.
[0043] The gas supply port 26 is formed in the base end portion 221 of the housing 22. A gas supply pipe 27 is connected to the gas supply port 26. The gas supply pipe 27 is connected to the compressed air supply device 6 via a pipe 52. The compressed air 15 supplied from the compressed air supply device 6 is guided to the mixing chamber S2 via the pipe 52 and the gas supply pipe 27, and is mixed with the developer 14 in the mixing chamber S2.
[0044] The nozzle 2 further includes a rod member 36 and a protruding portion 38. The rod member 36 and the protruding portion 38 are disposed between the liquid supply port 24 and the jet port 20 in a direction parallel to the central axis AX. The protruding portion 38 has a substantially cylindrical shape and is connected to the lower surface of the diffusion plate 30. The upper surface of the rod member 36 has substantially the same diameter as the protruding portion 38 and is fixed to the protruding portion 38. The lower surface of the rod member 36 has a larger diameter than the upper surface of the rod member 36. That is, the rod member 36 has a truncated cone shape whose diameter increases toward the tip side of the nozzle 2, and has an inclined surface 36s whose diameter increases toward the jet port 20.
[0045] As shown in Fig. 3, the inclined surface 36s is inclined at an angle θ with respect to the central axis AX. The angle θ is set arbitrarily depending on the pattern dimensions formed in the resist pattern, etc. The spray angle of the developer 14 sprayed from the spray nozzle 20 is determined depending on this angle θ. For example, the angle θ is set to be greater than 0° and equal to or less than 10°.
[0046] The inclined surface 36s of the rod member 36 is disposed so as to face the inner peripheral surface 223s of the tip portion 223 via a gap. In other words, the inner peripheral surface 223s of the tip portion 223 is disposed so as to surround the inclined surface 36s of the rod member 36. A fluid passage 40 is formed between the inner peripheral surface 223s and the inclined surface 36s, which guides the developing solution 14 supplied from the liquid supply port 24 and the compressed air 15 supplied from the gas supply port 26 from the mixing chamber S2 to the injection port 20.
[0047] The fluid passage 40 extends along the inclined surface 36s of the rod member 36, and has a substantially constant width (the distance between the inner circumferential surface 223s and the inclined surface 36s) in the extending direction of the fluid passage 40. The fluid passage 40 has a circular shape when viewed from a cross section perpendicular to the central axis AX, and the diameter thereof increases toward the ejection port 20. The fluid passage 40 guides the developer 14 and compressed air 15 mixed in the mixing chamber S2 to the ejection port 20.
[0048] An outlet of the fluid passage 40 constitutes an ejection port 20 that ejects the developer 14 and the compressed air 15. Fig. 5 is a bottom view of the nozzle 2. As shown in Fig. 5, the ejection port 20 of the nozzle 2 is formed between the bottom surface of the rod member 36 and the bottom surface of the inner circumferential surface 223s of the tip portion 223, and has a circular ring shape centered on the central axis line AX. When the developer 14 is ejected from the ejection port 20, it is atomized by the shear force of the compressed air 15 and ejected in the form of a mist.
[0049] The flow of the developer 14 and compressed air 15 in the nozzle 2 will be described with reference to Fig. 3. The developer 14 supplied from the developer supply device 5 is guided to the liquid supply pipe 25 through the piping 51, and flows through the introduction path 28 along the extension direction of the central axis line AX. The developer 14 that reaches the end of the introduction path 28 collides with the diffusion plate 30 and is diffused in the introduction path 28. The developer 14 diffused in the introduction path 28 passes through any of the multiple openings 32 at random and is sprayed into the mixing chamber S2. As a result, a uniform amount of developer 14 is discharged from the multiple openings 32.
[0050] On the other hand, the compressed air 15 supplied from the compressed air supply device 6 is introduced into the mixing chamber S2 through the piping 52 and the gas supply port 26. The compressed air 15 introduced into the mixing chamber S2 is guided to the fluid passage 40 together with the developer 14 along the inner peripheral surface 222s of the intermediate portion 222 while being mixed with the developer 14 that has passed through the multiple openings 32. Then, the developer 14 and the compressed air 15 are introduced into the inlet of the fluid passage 40 and flow through the fluid passage 40 toward the nozzle 20. At this time, the flow directions of the developer 14 and the compressed air 15 are aligned along the inclined surface 36s of the rod member 36. The developer 14 that has flowed through the fluid passage 40 is sprayed from the annular nozzle 20 together with the compressed air 15. At this time, the developer 14 is sheared by the compressed air 15 and sprayed from the nozzle 20 in the form of mist.
[0051] The spray direction of the developer 14 from the jet nozzle 20 coincides with the inclination direction of the inclined surface 36s of the rod member 36. That is, the spray angle of the developer 14 from the jet nozzle 20 based on the central axis AX coincides with the angle θ of the inclined surface 36s. That is, the developer 14 is sprayed from the jet nozzle 20 at an angle θ of 10° or less with respect to the central axis AX. The developer 14 is sprayed from the jet nozzle 20 at an angle greater than 0° with respect to the central axis AX.
[0052] FIG. 6 is a cross-sectional view of the jet flow of the developer 14 taken along line VI-VI in FIG. 2. Since the jet nozzle 20 has a circular ring shape, as shown in FIG. 6, the flow of the developer 14 jetted from the jet nozzle 20 has a circular ring pattern when viewed from a cross section perpendicular to the central axis AX. In addition, since the developer 14 is jetted from the jet nozzle 20 at an angle θ to the central axis AX, the jet width W of the developer 14 increases with distance from the jet nozzle 20. That is, the developer 14 is jetted from the circular jet nozzle 20 in a hollow cone type jet pattern. By jetting the developer 14 in such a jet pattern, it becomes possible to develop the resist film 12 with high uniformity and high precision.
[0053] Referring again to FIG. 1, as shown in FIG. 1, the developing device 100 further includes a control device 8. The control device 8 is a computer including a processor, a storage unit, an input device, a display device, etc., and controls each part of the developing device 100. In the control device 8, an operator can use the input device to input commands to manage the developing device 100, and the display device can visualize and display the operating status of the developing device 100. The storage unit of the developing device 100 stores a control program for controlling various processes executed by the developing device 100 with a processor, and a program for causing each component of the developing device 100 to execute a process according to processing conditions.
[0054] The control device 8 is connected to be able to communicate with the workpiece transport mechanism 3, the nozzle transport mechanism 4, the developer supply device 5, the compressed air supply device 6, and the recovery device 7. For example, the control device 8 sends control signals to the developer supply device 5 and the compressed air supply device 6 to control the flow rates of the developer 14 and the compressed air 15 supplied to the nozzle 2. The control device 8 also sends control signals to the recovery device 7 to control the operations of the gas-liquid separator 61 and the blower 62. Furthermore, the control device 8 sends control signals to the workpiece transport mechanism 3 and the nozzle transport mechanism 4 to control the transport speed of the workpiece 10 in the Y direction and the movement speed of the nozzle 2 in the X direction.
[0055] FIG. 7 is a diagram showing a schematic diagram of the relative movement direction of the nozzle 2 with respect to the workpiece 10. With the developer 14 and compressed air 15 supplied to the nozzle 2, the control device 8 controls the workpiece transport mechanism 3 to move the workpiece 10 from the start position S to one side in the Y direction at a constant speed, and then controls the nozzle transport mechanism 4 to move the nozzle 2 to one side in the X direction at a constant speed. Next, the control device 8 controls the workpiece transport mechanism 3 to move the workpiece 10 to the other side in the Y direction at a constant speed, and then controls the nozzle transport mechanism 4 to move the nozzle 2 to one side in the X direction at a constant speed. The control device 8 repeatedly controls the workpiece transport mechanism 3 and the nozzle transport mechanism 4 as described above, and scans the nozzle 2 two-dimensionally with respect to the workpiece 10, thereby uniformly spraying the developer 14 onto the entire surface of the resist film 12 formed on the workpiece 10.
[0056] As described above, the developer 14 is sprayed onto the resist film 12 formed on the workpiece 10, whereby the resist film 12 is developed. FIG. 8(a) is a cross-sectional view showing the resist film 12 including the exposed region 12a and the unexposed region 12b. As shown in FIG. 8(b), when the developer 14 is sprayed onto the resist film 12 from the spray port 20 of the nozzle 2, the unexposed region 12b of the resist film 12 is dissolved and selectively removed. As shown in FIG. 8(c), when the exposed region 12a of the resist film 12 is completely removed, a resist pattern 16 is obtained in which openings 45 corresponding to the exposed pattern are formed.
[0057] As described above, the developing device 100 sprays the developer 14 in a hollow cone-shaped spray pattern from the annular spray nozzle 20. The developer 14 sprayed from the nozzle 2 is sprayed uniformly in the circumferential direction of the spray nozzle 20, so that it is possible to form the resist pattern 16 with high uniformity. In addition, by spraying the developer 14 from the annular spray nozzle 20, the developer 14 can be supplied to a wider range than when the developer is sprayed from, for example, a circular spray nozzle, so that it is possible to speed up the development process of the resist film 12.
[0058] In addition, the developer 14 is sprayed from the nozzle 2 in a direction inclined at an angle θ with respect to the central axis AX, so that the developer 14 can be evenly supplied to the sidewall surface of the exposure region 12a of the resist film 12. As a result, the verticality of the opening 45 of the resist pattern 16 can be improved, and the pattern can be formed with high accuracy. For example, the energy beam L irradiated to the resist film 12 during exposure attenuates as it moves toward the lower part of the resist film 12, so that the sidewall surface of the opening of the resist film 12 during development tends to have an inverse tapered shape in which the width narrows as it moves downward. Therefore, when the developer 14 is sprayed in a direction parallel to the central axis AX, the developer 14 does not directly hit the sidewall surface of the resist film 12, and development residue may occur at the lower part of the resist film 12. In contrast, the developer 14 is sprayed from the nozzle 2 in a direction inclined at an angle θ with respect to the central axis AX, so that the developer 14 can be brought into direct contact with the sidewall surface of the lower part of the resist film 12, so that the resist pattern 16 having a fine and highly uniform pattern can be formed even when the resist film 12 has a large thickness.
[0059] Furthermore, in the conventional developing apparatus, the resist film 12 may swell due to the developer 14 seeping in during development of the resist film 12. If the resist film 12 swells, this causes the width of the opening 45 formed in the resist pattern 16 to be reduced. In contrast, in the developing apparatus 100 described above, the mist of developer 14 is sprayed at high speed from the nozzle 20 of the nozzle 2, so that the developer 14 is prevented from seeping into the resist film 12, and the swelling of the resist film 12 is prevented. Furthermore, the mist of developer 14 penetrates deep into the unexposed region 12b of the resist film 12, so that the verticality of the opening 45 can be improved. Therefore, the accuracy of the pattern formed in the resist pattern 16 can be improved.
[0060] Next, a processing method of a target object according to an embodiment will be described. Fig. 9 is a flow chart showing a processing method of a target object according to an embodiment. This method is performed using a substrate processing system including a developing device 100. Below, a method of removing a part of the target object 10 by processing the target object 10 using a resist pattern 16 having an opening will be described.
[0061] In this method, first, a resist film 12 is formed on the workpiece 10 (Step ST1: Formation of resist film). The resist film 12 formed on the workpiece 10 is a photoresist, and for example, a liquid resist or a dry film resist is used. When the resist film 12 is formed using a liquid resist, the liquid resist is uniformly applied onto the workpiece 10 using a coater (for example, a spin coater, a roll coater, a die coater, a bar coater, etc.) or by screen printing. Thereafter, the applied liquid resist is dried to form the resist film 12 on the workpiece 10.
[0062] On the other hand, when the resist film 12 is formed using a dry film resist, a laminating device is used. FIG. 10 shows an exemplary laminating device 70 used to form the resist film 12. The laminating device 70 includes a supply roller 71 that holds a photosensitive dry film resist, a pressure roller 72 that winds up the dry film resist and presses it onto the workpiece 10, and a table 73 that supports the workpiece 10. The pressure roller 72 presses the dry film resist wound from the supply roller 71 while peeling off the protective film, thereby pasting the dry film resist onto the workpiece 10. The pressure roller 72 may include, for example, a heating element, and may heat the dry film resist while pressing it onto the upper surface of the workpiece 10. As a result, the resist film 12 is formed on the upper surface of the workpiece 10. Note that a heating element may also be provided inside the table 73, and the dry film resist may be heated using one or both of the pressure roller 72 and the table 73 to paste the dry film resist onto the workpiece 10.
[0063] The lamination conditions of the dry film resist are appropriately set according to the processing conditions of the workpiece 10. For example, when an alumina substrate with a diameter of 300 mm and a thickness of 10 mm is used as the workpiece 10 and a resist pattern 16 having a dot shape with a diameter of 500 μm is formed on the workpiece 10, the dry film resist is formed on the workpiece 10 under the lamination conditions shown below as an example.
[0064] (Lamination conditions) Table temperature setting: 70℃ Table conveying speed: 500mm / min
[0065] The resist material contained in the dry film resist or the resist liquid may be a positive resist material or a negative resist material. The positive resist material is a resist material in which the exposed region 12a of the resist film 12 dissolves and the unexposed region 12b remains. The negative resist material is a resist material in which the unexposed region 12b of the resist film 12 dissolves and the exposed region 12a remains.
[0066] Next, the resist film 12 formed on the object 10 is exposed by an exposure device (step ST2: exposure process). This step is performed by irradiating the resist film 12 with energy rays L (e.g., visible light or ultraviolet light) from a light source of the exposure device through a pattern mask 18 having a predetermined pattern, for example, as shown in FIG. 11. As the pattern mask 18, for example, a negative mask having a configuration in which a black film is formed on a transparent plate material (e.g., glass, film, etc.) and having an area that transmits the energy rays L and an area that does not transmit the energy rays L is used. As a light source for irradiating the energy rays L, for example, an LED lamp, a mercury lamp, a metal halide lamp, an excimer lamp, a xenon lamp, etc. are used. In one example, ultraviolet light is irradiated onto the resist film 12 from an ultra-high pressure mercury lamp. By this exposure process, the pattern of the pattern mask 18 is transferred to the resist film 12.
[0067] Next, the pattern transferred to the resist film 12 is developed (step ST3: development process). In this step, the resist film 12 is developed by spraying the developer 14 onto the resist film 12. As a conventional developing apparatus, a shower type developing apparatus that sprays the developer pressurized by a pump using a developer spray nozzle is generally known. In such a shower type developing apparatus, it is difficult to supply the developer 14 to the inside of a fine pattern, and it is difficult to develop the fine pattern with high accuracy. In contrast, in a processing method of an object to be processed according to an embodiment, the resist film 12 is developed using a developing apparatus 100 shown in FIG. 1. For example, the developing apparatus 100 sprays the developer 14 together with compressed air 15 onto the resist film 12 from a nozzle 2 having a circular injection port 20 while scanning the nozzle 2 in the X direction and the Y direction relative to the object to be processed 10. For example, in step ST3, as shown in FIG. 1, the nozzle 2 is moved at high speed in the left-right direction (X direction) using the nozzle transport mechanism 4, while the object to be processed 10 is moved in the front-back direction (Y direction) using the object transport mechanism 3. At this time, the developer 14 in the form of a mist is sprayed from the spray nozzle 20 in a hollow cone-shaped spray pattern onto the resist film 12. By spraying the developer 14 onto the resist film 12, exposed or unexposed regions of the resist film 12 are selectively removed. Thereafter, the developed resist film 12 is washed with water and subjected to an air blow process, so that a resist pattern 16 having a fine and uniform pattern is formed on the workpiece 10, as shown in FIG.
[0068] The developing conditions of the resist film 12 by the exposure device are appropriately set according to the shape and dimensions of the pattern to be formed in the resist pattern 16. For example, when forming the resist pattern 16 having dot shapes with a diameter of 500 μm, the resist film 12 is developed under the developing conditions shown below.
[0069] (Developing conditions) Developer: Alkaline aqueous solution Developer temperature: 40℃ Nozzle travel: 500mm Nozzle moving speed: 10m / min - Processing object movement speed: 100mm / min
[0070] In one embodiment, the object 10 may be transferred to a heating furnace and subjected to a heating process (pre-bake) before the development process in order to harden the resist film 12. After the development process, the object 10 may be cleaned and re-heated (post-bake).
[0071] Next, the workpiece 10 is processed (step ST4: processing). For example, this processing is etching. For example, the etching processing is blasting. For example, this blasting processing is performed by a blasting processing device 80. As shown in FIG. 13, the blasting processing device 80 blows abrasives 84 together with compressed air against the workpiece 10 through the resist pattern 16 while scanning a blast nozzle 82 in the left-right and front-back directions, thereby cutting and removing the portions of the surface of the workpiece 10 exposed from the openings of the resist pattern 16. As a result, the pattern of the resist pattern 16 is transferred to the workpiece 10.
[0072] The blast processing conditions for the workpiece 10 are appropriately set according to the pattern to be formed on the workpiece 10. For example, when a hole having a depth of 50 μm is formed in the workpiece 10 using the above-mentioned resist pattern 16, the workpiece 10 is processed under the blast processing conditions shown below.
[0073] (Blast processing conditions) Blast nozzle movement speed: 10m / min Blast nozzle internal pressure: 0.25MPa
[0074] Next, the resist pattern 16 is peeled off from the workpiece 10 by a peeling device 90 (step ST5). For example, as shown in Fig. 14, the peeling device 90 removes the resist pattern 16 from the surface of the workpiece 10 by spraying a stripping liquid 94 onto the surface of the workpiece 10 from a spray nozzle 92. Through the above-mentioned series of steps, the workpiece 10 having a fine pattern formed thereon is produced.
[0075] The above describes the nozzle 2, the developing device 100, and the processing method of the workpiece according to various embodiments. However, the present invention is not limited to the above-described embodiments, and various modifications can be made without departing from the spirit and scope of the invention.
[0076] For example, in the above embodiment, the developer 14 is sprayed from the nozzle 2 together with the compressed air 15, but in one embodiment, an etching solution may be sprayed from the nozzle 2. In this case, the etching device equipped with the nozzle 2 supplies the etching solution as a processing solution to the liquid supply pipe 25 of the nozzle 2, and supplies compressed air to the gas supply pipe 27. As a result, the etching solution and the compressed air are mixed in the mixing chamber S2, and the mist of the etching solution is sprayed from the nozzle 20 having a circular ring shape in a hollow cone-shaped spray pattern. By spraying the mist of the etching solution to the workpiece 10 through the resist pattern 16 in a hollow cone-shaped spray pattern, the etching solution is evenly supplied to the side wall surface of the opening of the workpiece 10, so that the workpiece 10 can be processed with high accuracy.
[0077] In step ST4 of the processing method of the workpiece 10 shown in FIG. 9, the workpiece 10 is blasted through the resist pattern 16 to remove a part of the workpiece 10. In one embodiment, however, the workpiece 10 may be partially removed by wet etching (chemical etching). Wet etching is a method of partially removing the workpiece 10 by chemically corroding the surface of the workpiece 10 using an etching solution (chemical). In one embodiment, the workpiece 10 may be immersed in the etching solution, or the etching solution may be sprayed onto the workpiece 10 through the resist pattern 16 to remove a part of the workpiece 10. When spraying the etching solution onto the workpiece 10, the etching solution may be sprayed onto the workpiece 10 from the nozzle 2 described above in a hollow cone-shaped spray pattern. By spraying the etching solution onto the workpiece 10 from the nozzle 2 having a circular ring shape, the workpiece 10 can be processed with high uniformity and precision.
[0078] In another embodiment, the workpiece 10 may be plated using the resist pattern 16 developed in step ST4. For example, by forming a plating layer via the resist pattern 16 formed on the workpiece 10, a metal mask corresponding to the shape of the pattern formed in the resist pattern 16 can be formed on the workpiece 10.
[0079] As an example, when a dry film resist is attached onto a 300 mm x 300 mm stainless steel substrate to form a resist pattern 16 having a dot shape and this resist pattern 16 is used to form a metal mask on the workpiece 10, the formation of the resist film 12, the exposure process, and the development process are performed, for example, according to the following lamination conditions, exposure conditions, and development conditions.
[0080] (Lamination conditions) Table temperature setting: 70℃ Table conveying speed: 500mm / min
[0081] (Exposure conditions) Energy rays: UV rays
[0082] (Developing conditions) Developer: Alkaline aqueous solution Developer temperature: 60℃ Nozzle travel: 400mm Nozzle moving speed: 10m / min - Processing object movement speed: 30mm / min
[0083] In this embodiment, a nickel plating layer is formed by electroplating on the workpiece 10 having the resist pattern 16 formed under the above-mentioned conditions. Then, the resist pattern 16 is stripped using a stripping solution 94 to form a metal mask.
[0084] The effects of the nozzle 2 and the developing device 100 described above will be described below based on examples and comparative examples, but the present invention is not limited to the following examples.
[0085] In Example 1 and Comparative Example 1, a photosensitive dry film resist was formed on the workpiece 10, and the dry film resist was exposed and developed using photolithography technology to form a wet etching resist pattern 16 covering a part of the workpiece 10. The design dimensions of the resist pattern 16 to be formed on the workpiece 10 were a thickness of 15 μm and a line width of 12 μm. In Example 1, the resist pattern 16 was formed by spraying the mist-like developer 14 from the nozzle 2 shown in FIG. 2 in a hollow cone-shaped spray pattern onto the dry film resist. Meanwhile, in Comparative Example 1, the resist pattern 16 was formed by supplying the liquid developer 14 from a shower nozzle onto the dry film resist. The resist patterns 16 formed in Example 1 and Comparative Example 1 were observed with an electron microscope (SEM).
[0086] FIG. 15(a) is an SEM photograph of the resist pattern 16 formed by Comparative Example 1. FIG. 15(b) is an SEM photograph of the resist pattern 16 formed by Example 1. As shown in FIG. 15(a), it was confirmed that the line width of the resist pattern 16 formed by Comparative Example 1 was narrower than the line width of 12 μm exposed to the dry film resist. In Comparative Example 1, it is considered that the liquid developer 14 permeates the dry film resist and swells it, thereby reducing the opening of the resist pattern 16. In contrast, as shown in FIG. 15(b), the line width of the resist pattern 16 formed by Example 1 was 12 μm, and it was confirmed that the resist pattern 16 could be formed with high accuracy.
[0087] Next, Example 2 and Comparative Example 2 will be described. In Example 2 and Comparative Example 2, a photosensitive dry film resist was formed on the object 10, and the dry film resist was exposed and developed using photolithography technology to form a sandblasting resist pattern 16 covering a part of the object 10. The design dimensions of the resist pattern 16 to be formed on the object 10 were a thickness of 35 μm and a line width of 30 μm. In Example 2, the resist pattern 16 was formed by spraying the mist-like developer 14 from the nozzle 2 shown in FIG. 2 in a hollow cone-shaped spray pattern onto the dry film resist. On the other hand, in Comparative Example 2, the resist pattern 16 was formed by supplying the liquid developer 14 from a shower nozzle onto the dry film resist. The resist patterns 16 formed in Example 2 and Comparative Example 2 were observed with an electron microscope (SEM).
[0088] FIG. 16(a) is an SEM photograph of the resist pattern 16 formed by Comparative Example 2. FIG. 16(b) is an SEM photograph of the resist pattern 16 formed by Example 2. As shown in FIG. 16(a), it was confirmed that the width of the opening near the bottom was reduced in the resist pattern 16 formed by Comparative Example 2. This reduction in the opening width is believed to be due to a part of the developer supplied from the shower nozzle remaining at the bottom of the opening, and the developer 14 not being sufficiently supplied to the sidewall surface of the opening. In contrast, as shown in FIG. 16(b), it was confirmed that the sidewall surface of the opening has high verticality in the resist pattern 16 formed by Example 2, and the resist pattern 16 was developed with high accuracy. [Explanation of symbols]
[0089] 1... processing vessel, 2... nozzle, 3... workpiece transport mechanism, 4... nozzle transport mechanism, 5... developer supply device, 6... compressed air supply device (compressed gas supply device), 7... recovery device, 10... workpiece, 12... resist film, 14... developer, 15... compressed air (compressed gas), 16... resist pattern, 20... injection port, 22... housing, 24... liquid supply port, 25... liquid supply pipe, 26... gas supply port, 30... diffusion plate, 32... opening, 36... rod member, 36s... inclined surface, 40... fluid passage, 84... abrasive, 94... stripping solution, 100... developing device, 221s, 222s, 223s... inner circumferential surface, AX... central axis, θ... angle.
Claims
1. A nozzle for spraying a treatment liquid, A cylindrical housing having a central axis, The housing includes: a liquid supply port for supplying the processing liquid into the housing; a gas supply port for supplying compressed gas into the housing; an injection port for injecting the treatment liquid together with the compressed gas; having The injection port has a circular ring shape centered on the central axis line, The nozzle further includes a rod member disposed between the liquid supply port and the ejection port in the direction of extension of the central axis, the rod member having an inclined surface whose diameter increases toward the ejection port, A nozzle, wherein a fluid passage is formed between the inner surface of the housing and the inclined surface, for guiding a mixture of the processing liquid supplied from the liquid supply port and the compressed gas supplied from the gas supply port to the injection port.
2. A nozzle for spraying a treatment liquid, comprising: A cylindrical housing having a central axis, The housing includes: a liquid supply port for supplying the processing liquid into the housing; a gas supply port for supplying compressed gas into the housing; an injection port for injecting the treatment liquid together with the compressed gas; having The injection port has a circular ring shape centered on the central axis line, a liquid supply pipe for guiding the treatment liquid into the housing along the central axis; a diffusion plate that diffuses the treatment liquid flowing through the liquid supply pipe, the diffusion plate having a plurality of openings arranged in a circumferential direction around the central axis; The nozzle further comprises:
3. The nozzle according to claim 1 or 2, configured to spray the treatment liquid in a mist form from the spray outlet.
4. 4. The nozzle according to claim 1, wherein the processing liquid is a developing liquid for developing a resist film, or an etching liquid for etching an object to be processed.
5. A developing apparatus for developing a resist film formed on a target object, comprising: A processing vessel; The nozzle according to any one of claims 1 to 4, which is disposed in the processing vessel; a transport mechanism for moving the object to be processed relative to the nozzle within the processing vessel; a developer supplying device that supplies a developer as the processing liquid to the nozzle; a compressed gas supply device that supplies the compressed gas to the nozzle; A developing device comprising:
6. The developing device according to claim 5 , wherein the developer supplying device supplies the developer heated to 40° C. or higher to the nozzle.
7. 7. The developing apparatus according to claim 5, further comprising a recovery device that recovers gas containing the developing solution from within the processing container and separates the gas and liquid.
8. forming a photosensitive resist film on a target object; exposing the resist film to light; mixing the developer and compressed air inside a nozzle having an annular jet port; a step of spraying a mixture of compressed gas and a developer from the nozzle onto the exposed resist film to form a resist pattern; Including, The method for processing a processing object includes spraying the developer in a spray pattern that forms an annular shape when viewed from a direction along a central axis of the spray nozzle and whose diameter increases with increasing distance from the spray nozzle.
9. The processing method according to claim 8 , wherein the developer is sprayed in a mist form from the spray nozzle.
10. The processing method according to claim 8 , wherein a spray direction of the developer is inclined at an angle of 10° or less with respect to the central axis.
11. The processing method according to any one of claims 8 to 10, further comprising the step of spraying an abrasive onto the object through the resist pattern to remove a portion of the object.
12. 12. The processing method according to claim 8, further comprising the step of spraying an etching liquid from the nozzle onto the object through the resist pattern to remove a portion of the object.
13. 13. The processing method according to claim 8, further comprising the step of supplying a stripping liquid to the resist pattern to remove the resist pattern from the object to be processed.
Citation Information
Patent Citations
Shutsuryokujikunishindooataerusadokiko
JP1976053332A
Spray gun for circular spraying
JP1986129055A
Device and method for development
JP2004274028A
Two-fluid nozzle and spraying method
JP2005288390A
Two fluid nozzle, substrate treatment apparatus and substrate treatment method using the same
JP2008114183A