Electrode plate for plasma processing apparatus and method for manufacturing same

The electrode plate's unique surface morphology, achieved through mixed abrasive grain polishing, effectively traps deposits, preventing particle generation and substrate defects by dispersing shear stress and utilizing anchoring effects.

JP7585900B2Active Publication Date: 2024-11-19MITSUBISHI MATERIALS CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021041363
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-15
Publication Date
2024-11-19
Estimated Expiration
2041-03-15

AI Technical Summary

Technical Problem

Existing electrode plates for plasma processing apparatuses struggle to efficiently capture deposits generated during plasma processing, leading to particle generation that can cause defects on substrates.

Method used

The electrode plate features a surface morphology with a specific distribution of spatial frequency components, combining low and high spatial frequencies to trap deposits effectively, achieved through a polishing process using mixed abrasive grains.

Benefits of technology

This design efficiently captures deposits, preventing particle generation and substrate defects by dispersing shear stress and utilizing anchoring effects of fine irregularities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585900000002
    Figure 0007585900000002
  • Figure 0007585900000003
    Figure 0007585900000003
  • Figure 0007585900000004
    Figure 0007585900000004
Patent Text Reader

Abstract

To prevent generation of particles by efficiently capturing deposits generated during plasma processing.SOLUTION: The sum of the amplitude spectrum for the spatial frequency obtained by fast Fourier transforming the measured cross-sectional curve of the surface has 38% to 50% of the total components with spatial frequencies of 1 cycle to 30 cycles, the components with spatial frequencies over 30 cycles to 120 cycles of 35% or more and 50% or less of the whole, and the remainder exceeding the spatial frequency of 120 cycles, and a base plate for an electrode plate is manufactured so as to be polished by using mixed abrasive grains containing fine abrasive grains with a grain size of 800 or more and 1500 or less and coarse grains with a grain size of 80 or more and 200 or less.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrode plate for a plasma processing apparatus, which discharges plasma while passing a plasma generating gas in the thickness direction, and a method for manufacturing the same. [Background technology]

[0002] Plasma processing equipment such as plasma etching equipment and plasma CVD equipment used in semiconductor device manufacturing processes has a configuration in which a pair of electrodes connected to a high-frequency power source are arranged vertically opposite each other in a vacuum chamber. In this configuration, a substrate to be processed is placed on the lower electrode, and while a plasma generating gas is circulated toward the substrate through a plurality of vent holes formed in the upper electrode, a high-frequency voltage is applied between the upper and lower electrodes to generate plasma, thereby performing processing such as etching on the substrate to be processed.

[0003] The upper electrode used in such plasma processing equipment is generally a silicon electrode plate with multiple ventilation holes of the same diameter. A cooling plate is fixed to the back side of this electrode plate opposite to the surface exposed to the plasma in order to release the heat that rises during plasma processing. When plasma processing is performed on this electrode plate for a long period of time, by-products from the plasma reaction adhere to the surface as solid matter (these adherent matters are called deposits, or simply "deposits"), and the accumulated deposits fall off and become particles, which can adhere to the substrate being processed and cause defects. Therefore, there is a demand for an electrode plate that suppresses the generation of particles.

[0004] Patent Documents 1 and 2 disclose electrode plates that suppress the generation of such particles. Patent Document 1 describes that, based on the recognition that particles are generated from the contact area between the silicon electrode plate and the support protrusion of the shield support electrode that supports the silicon electrode plate, in a disk-shaped silicon electrode plate having a mirror-like surface with a center line surface roughness Ra of 1 μm or less, at least the portion covered by the upper surface of the support part of the shield support electrode is roughened to a center line surface roughness Ra of more than 1 μm to 1.6 μm.

[0005] Patent Document 2 describes that, based on the understanding that deposits attached to the inner surface of the ventilation hole through which the etching gas flows will fall off and become particles, the inner wall surface of the ventilation hole (through hole) is composed of a surface portion with large surface roughness (rough surface portion) and a surface portion with small surface roughness (smooth surface portion), and the rough surface portion is formed on the inner wall surface of the ventilation hole on the etching gas inlet side, and the smooth surface portion is formed on the inner wall surface of the ventilation hole on the etching gas outlet side. In this Patent Document 2, deposits are attached to the rough surface portion to prevent them from falling off. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2008-85027 A [Patent Document 2] JP 2006-196491 A Summary of the Invention [Problem to be solved by the invention]

[0007] The technology described in Patent Document 1 is an attempt to eliminate the source of particle generation, and although it is effective in itself, it cannot completely eliminate particle generation. On the other hand, the technology described in Patent Document 2 is an attempt to prevent particle generation by attaching the deposits that cause particles to the inner surface of the back side of the vent hole (the opposite side to the plasma surface) to prevent them from scattering, but the vent hole has a diameter of, for example, 0.5 mm and its inner surface area is also small, so there is a limit to the amount of deposits that can be attached and fixed.

[0008] The present invention has been made in consideration of the above circumstances, and has an object to provide an electrode plate for a plasma processing apparatus that can efficiently capture deposits generated during plasma processing and prevent the generation of particles. [Means for solving the problem]

[0009] In the electrode plate for plasma processing equipment of the present invention, the sum of the amplitude spectrum versus spatial frequency obtained by fast Fourier transform of the measured cross-sectional curve of the surface has spatial frequency components of 1 cycle or more and 30 cycles or less that account for 38% or more and 50% or less of the total, spatial frequency components exceeding 30 cycles and up to 120 cycles that account for 35% or more and 50% or less of the total, and the remainder has a spatial frequency exceeding 120 cycles.

[0010] By mixing low spatial frequency components of 1 cycle or more and 30 cycles or less with higher spatial frequency components of more than 30 cycles and 120 cycles or less with almost equal strength, it is possible to effectively capture deposits and suppress the generation of particles. In this case, in a surface morphology specified by components of a low spatial frequency band, the relatively rough unevenness distributes the shear stress applied to the attached deposits, making them less likely to fall off, while in a surface morphology specified by components of a higher spatial frequency band, the anchor effect of the fine unevenness makes it difficult for the deposits to fall off. These synergistic effects suppress the generation of particles.

[0011] The mixed form of the low spatial frequency band components and the higher spatial frequency band components may be the entire surface of the electrode plate (the surface facing the plasma region during use), but it is preferable to adjust it so that at least the surface of the outer periphery outside the region where the air holes are formed is such a surface. Since the plasma processing gas does not blow out from this outer periphery, it is possible to efficiently capture deposits generated during plasma processing.

[0012] The manufacturing method of an electrode plate for a plasma processing device of the present invention uses a mixture of abrasive grains containing fine abrasive grains with a grit size of 800 or more and 1500 or less and coarse abrasive grains with a grit size of 80 or more and 200 or less when polishing the surface of a raw sheet for an electrode plate.

[0013] By using a mixture of fine and coarse abrasive grains during polishing, it is possible to create a state in which the sum of the amplitude spectrum for spatial frequency obtained by fast Fourier transform of the measured cross-sectional curve is appropriately mixed with components in low spatial frequency bands and components in higher spatial frequency bands. In this manufacturing method, the mixing ratio of the fine abrasive grains to the coarse abrasive grains is preferably within a range of 1:1 to 1:3. Effect of the Invention

[0014] According to the present invention, deposits generated during plasma processing can be efficiently captured to prevent generation of particles. [Brief description of the drawings]

[0015] [Figure 1] 1 is a plan view showing one embodiment of an electrode plate for a plasma processing apparatus according to the present invention; [Diagram 2] 2 is a vertical sectional view of the electrode plate for the plasma processing apparatus of FIG. 1 supported by a shield support electrode. [Diagram 3] 4 is an example of a measured cross-sectional curve graph and an amplitude spectrum graph of a surface of an electrode plate for a plasma processing apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] As shown in FIG. 1, an electrode plate for a plasma processing apparatus (hereinafter simply referred to as an electrode plate) 10 is formed in a disk shape and has a number of ventilation holes 11 penetrating in the thickness direction in the central part except for the outer periphery 15 thereof. Although the dimensions of this electrode plate 10 are not necessarily limited, it is a disk with a thickness of 8 to 12 mm and a diameter of 200 to 600 mm. The inner diameter of each air hole 11 is 0.5 to 1.0 mm, and the center-to-center distance between the air holes 11 is 5 to 10 mm.

[0017] The vent hole 11 is formed in a circular area in the center of the electrode plate 10 except for the outer periphery 15. The vent hole forming area A1 has a diameter of about 150 to 500 mm. As shown in FIG. 2, the outer periphery 15 of the electrode plate 10 is fixed to a plasma processing device (not shown) by a ring-shaped shield support electrode 20. The shield support electrode 20 has a shape in which a cylindrical portion 21 and a support portion 22 extending radially inward from the lower end of the cylindrical portion 21 in an inward flange shape are integrally formed. The outer periphery of the electrode plate 10 is placed on the upper surface of the support portion 22 of the shield support electrode 21, and the electrode plate 10 is supported inside the inner periphery of the support portion 22 with the vent hole 11 in an open state.

[0018] In this case, if the circular region in the electrode plate 10 in which the air holes 11 are formed is defined as the air hole formation region A1, the outer peripheral edge of the air hole formation region A1 is positioned radially inwardly away from the inner peripheral edge of the support portion 22 of the shield support electrode 20, as shown in FIG. 2.

[0019] The sum of the amplitude spectrum versus spatial frequency obtained by performing a Fast Fourier Transform (FFT) on the measured cross-sectional curve of the surface of this electrode plate has spatial frequency components of 1 cycle or more and 30 cycles or less that account for 38% to 50% of the total, spatial frequency components of more than 30 cycles and 120 cycles or less that account for 35% to 50% of the total, and the remainder has a spatial frequency exceeding 120 cycles.

[0020] Here, the measured cross-sectional curve is a curve relating to the surface roughness obtained by, for example, taking an image of the surface of the electrode plate 10 using a laser microscope with a 20x objective lens and measuring a length of 640 μm in the surface image. The measured cross-sectional curve is subjected to a fast Fourier transform. The fast Fourier transform is a calculation method that resolves an arbitrary waveform into components of each spatial frequency and determines their magnitude (amplitude) and position (phase). It is a Fourier transform using a processing algorithm that can process data at high speed by limiting the number of data to the power of 2 (2, 4, 8, 16, 32, ...). The amplitude spectrum obtained as a result of this fast Fourier transform is the absolute value of a complex number. Then, by calculating the sum of the amplitude spectrum in a specific frequency range, the dominant shape of the measured surface can be grasped. Of the sum of the amplitude spectra, the proportion of specific spatial frequency components is 38% to 50% of the total for components with spatial frequencies between 1 cycle and 30 cycles, 35% to 50% of the total for components with spatial frequencies between 30 cycles and 120 cycles, and the remainder is a spatial frequency exceeding 120 cycles.

[0021] Figure 3 shows the amplitude spectrum graph on the right obtained by fast Fourier transform for the measured profile curve graph on the left. The measured profile curve graph shows the distance (μm) on the horizontal axis and the height of the unevenness (μm) on the vertical axis. The amplitude spectrum graph shows the spatial frequency (cycle) on the horizontal axis and the amplitude spectrum (μm) on the vertical axis.

[0022] By mixing the low spatial frequency band components of 1 cycle or more and 30 cycles or less and the higher spatial frequency band components of more than 30 cycles and 120 cycles or less in approximately equal proportions, it is possible to effectively capture the deposits and suppress the generation of particles. In this case, in the surface morphology specified by the components of the low spatial frequency band, the relatively rough unevenness distributes the shear stress applied to the attached deposits, making them less likely to fall off, while in the surface morphology specified by the components of the higher spatial frequency band, the anchor effect of the fine unevenness makes the deposits less likely to fall off. These synergistic effects suppress the generation of particles.

[0023] It is more preferable that the ratio of the spatial frequency components is 40% to 44% for the spatial frequency components of 1 cycle to 30 cycles, and 35% to 41% for the spatial frequency components of more than 30 cycles and 120 cycles. The ratio of the spatial frequency components may be 38% to 50% for the spatial frequency components of 1 cycle to 30 cycles, 35% to 50% for the spatial frequency components of more than 30 cycles and 120 cycles, and 13% to 18% for the spatial frequency components of more than 120 cycles and 511 cycles. When the ratio of the spatial frequency components of 1 cycle to 30 cycles is 44% to 50% for the spatial frequency components of more than 30 cycles and 120 cycles, the ratio of the spatial frequency components of more than 30 cycles and 120 cycles is 35% to 41% for the spatial frequency components of more than 120 cycles, and the remainder is the spatial frequency components of more than 120 cycles. In addition, the proportion of these spatial frequency components is such that while components with spatial frequencies of 1 cycle or more and 30 cycles or less account for 38% or more and 45% or less of the total, components with spatial frequencies greater than 30 cycles and less than 120 cycles account for 35% or more and 47% or less of the total, and the remainder are components with spatial frequencies greater than 120 cycles. In addition, for components in spatial frequency bands exceeding 120 cycles, the unevenness is too fine and almost smooth, resulting in poor anchoring effect, so it is better for their presence ratio in the overall spectrum to be smaller than that of other spatial frequency band components (in this case, components with spatial frequencies between 1 cycle and 30 cycles, and components with spatial frequencies between 30 cycles and 120 cycles).

[0024] This mixture of low spatial frequency band components and higher spatial frequency band components is formed over the entire surface of the electrode plate 10 (surface exposed to plasma), but is particularly effective in the outer peripheral portion 15 outside the air hole formation region A1. The outside of the air hole formation region A1 is less affected by plasma and is less affected by the flow of plasma gas, so deposits are particularly likely to adhere to it. For this reason, by making the outer surface of the air hole formation region A1 a state in which the amplitude spectrum of the above-mentioned low spatial frequency band components and the amplitude spectrum of the higher spatial frequency band components are mixed, the deposits adhered to the outer peripheral portion 15 can be captured, and the effect of suppressing particle generation can be improved.

[0025] The electrode plate 10 configured in this manner is manufactured by slicing a silicon ingot of single crystal silicon to form a disk-shaped electrode plate blank (hereinafter simply referred to as blank), subjecting the blank to heat treatment as necessary, and then carrying out an air hole forming process to form air holes in the blank, an etching process to etch the blank with the air holes formed in it, and a polishing process to polish the upper and lower surfaces of the blank after the etching process.

[0026] Of these steps, in the vent hole forming step, the vent holes 11 are formed while a drill is lowered parallel to the thickness direction from one surface of the blank. In the etching process, surface damage (such as microcracks) that occurred during the slicing process and the vent hole formation process are removed by etching. The etching solution used is hydrofluoric acid (HF), nitric acid (HNO3), and acetic acid (CH3COOH), which is a mixture of these.

[0027] In the polishing process, a raw plate is placed on a rotating polishing pad and polished while a slurry containing an abrasive such as diamond abrasive grains is supplied. In this polishing process, it is preferable to use a lapping pad as a lapping machine and to use relatively coarse abrasive grains as the abrasive grains. In this case, it is preferable to use a mixture of fine abrasive grains with a grain size of 800 to 1500 and coarse abrasive grains with a grain size of 80 to 200.

[0028] By using this mixed abrasive grain, the relatively large brittle fracture caused by the coarse abrasive grains and the minute cutting caused by the fine abrasive grains among the abrasive grains rolling between the lapping machine and the blank work together, and it is possible to reliably obtain a surface state in which the amplitude spectrum of the above-mentioned low spatial frequency band components and the amplitude spectrum of the higher spatial frequency band components coexist. In this case, if the mixing ratio of the fine abrasive grains to the coarse abrasive grains is within the range of 1:1 to 1:3, it is easy to obtain a surface form with the desired spatial frequency components.

[0029] The electrode plate 10 thus manufactured is finally washed before being used. When the electrode plate 10 is mounted in a plasma processing apparatus, the peripheral portion of the outer periphery 15 is covered by the support portion 22 of the shield support electrode 20, and the inner surface of the outer periphery 15 is exposed to the plasma processing space. This exposed surface (plasma surface 10a) is exposed to the plasma environment, and mainly the vent hole formation region A1 is worn away as shown by the two-dot chain line in FIG. 1. At this time, by-products of the plasma reaction of the processing gas ejected from the vent hole 11 adhere to the surface of the electrode plate 10 as solid matter (deposits). If the deposits accumulate and fall off, they may become particles and adhere to the substrate to be processed, such as a silicon wafer.

[0030] The electrode plate 10 of this embodiment is formed in a surface state in which the sum of the amplitude spectra with respect to spatial frequencies obtained by fast Fourier transform of the measured cross-sectional curve of the surface is a mixture of the amplitude spectrum of components in a low spatial frequency band and the amplitude spectrum of components in a higher spatial frequency band, so that deposits can be efficiently captured on the surface to prevent the generation of particles. That is, in a surface morphology specified by components in a low spatial frequency band, the relatively coarse unevenness disperses the shear stress applied to the deposited material, making it difficult for the material to fall off, while in a surface morphology specified by components in a higher spatial frequency band, the fine unevenness has an anchoring effect, making the deposited material difficult to fall off. These synergistic effects suppress the generation of particles.

[0031] The present invention is not limited to the configuration of the above embodiment, and various changes can be made to the details of the configuration without departing from the spirit of the present invention. For example, in the embodiment, the entire surface of the plasma face of the electrode plate 10 is adjusted so that the sum of the amplitude spectrum with respect to the spatial frequency obtained by fast Fourier transforming the measured cross-sectional curve is within a predetermined range, but the surface of the vent hole formation region A1 of the entire surface of the plasma face of the electrode plate 10 may be adjusted to be a smooth surface, and only the surface of the outer periphery 15 outside the vent hole formation region A1 may be adjusted to have the above-mentioned specific surface form. When the surface state is to be different between the vent hole formation region A1 and the outer periphery 15 outside it, the entire surface of the blank may be polished with fine abrasive grains, and then the outer periphery 15 may be polished with mixed abrasive grains. In addition, in the embodiment, the polishing process for the raw plate is performed by lapping, but a blasting process using a mixture of two different sizes of projection material may also be used. EXAMPLES

[0032] A blank plate made of a single crystal silicon disk having a diameter of 390 mm and a thickness of 11 mm was prepared, and a hole having a diameter of 0.5 mm was drilled on one side of this blank plate with a diamond drill to prepare a blank electrode plate. After etching, the entire surface of the blank was polished by lapping. By changing the size of the polishing abrasive grains during the polishing process, electrode plates with various surface morphologies were produced.

[0033] The surface of the electrode plate was photographed using a laser microscope with a 20x objective lens, and a cross-sectional curve of 640 μm in a specified area of ​​the image was measured. The measured cross-sectional curve was divided into two sections. 10 = 1024 samples were decomposed and fast Fourier transformed to obtain the amplitude spectrum for each spatial frequency.Then, the sum of the amplitude spectrum for each spatial frequency band of 1 cycle or more and 30 cycles or less, the spatial frequency band of more than 30 cycles and 120 cycles or less, and the spatial frequency band of more than 120 cycles (spatial frequency band of more than 120 cycles and 511 cycles or less in the embodiment) was obtained, and the ratio of the total (sum of the amplitude spectrum for each spatial frequency band / sum of the total amplitude spectrum) was obtained.The measurement length of the cross-sectional curve and the number of samples (powers of 2) can be changed as appropriate.

[0034] The electrode plate thus prepared is set on the upper surface of the support portion 22 of the shield support electrode 20, and a silicon wafer having a diameter of 200 mm is placed on the electrode as a substrate to be processed. Chamber pressure: 10 -1 Torr Etching gas composition: 90sccmCHF3+4sccmO2+150sccmHe High frequency power: 2kW Frequency: 20kHz Plasma etching was carried out for 500 hours under the conditions above. Note that sccm is an abbreviation for standard cc / min, and refers to the flow rate (cc) per minute standardized at 1 atm (atmospheric pressure 1013 Pa) and a constant temperature such as 0°C or 25°C.

[0035] The number of particles on the silicon wafer was measured immediately after the start of etching, and after 10 hours, 20 hours, 50 hours, 100 hours, and 200 hours, and the results are shown in Table 1. The particle number was measured by scanning the wafer surface with a laser beam and measuring the intensity of scattered light from the attached particles to identify the position and size of the particles. The results are shown in Table 1. In Table 1, Examples 4 and 5 are examples in which only the outer peripheral portion of the electrode plate outside the region where the air vent holes are formed was polished by lapping. The surface of the region where the air vent holes are formed was polished to a normal mirror finish.

[0036] [Table 1]

[0037] As can be seen from the results in Table 1, in Examples 1 to 5, in which the spatial frequency components of 1 cycle or more and 30 cycles or less account for 38% to 50% of the total, the spatial frequency components of more than 30 cycles and 120 cycles or less account for 35% to 50% of the total, and the remainder are spatial frequencies exceeding 120 cycles, particle generation is suppressed even during long-term plasma processing. It can be seen that Examples 4 and 5, in which only the outer periphery is polished by lapping, are also effective in preventing particle generation. In contrast, Comparative Examples 1 to 3 had a high ratio of spatial frequencies between 1 cycle and 30 cycles, Comparative Examples 4 to 7 had a low ratio of spatial frequencies between 1 cycle and 30 cycles (Comparative Examples 6 and 7 also had a high ratio of spatial frequencies greater than 30 cycles and less than 120 cycles), and Comparative Examples 8 and 9 had a low ratio of spatial frequencies greater than 30 cycles and less than 120 cycles. As a result, a large number of particles were generated in each case, especially in plasma processing lasting more than 200 hours. [Explanation of symbols]

[0038] 10 Electrode plate for plasma processing device 11 Ventilation holes 15 Outer periphery 20 Shield support electrode 22 Support part A1 Vent forming area

Claims

1. An electrode plate for a plasma processing apparatus, characterized in that the sum of the amplitude spectrum with respect to spatial frequency obtained by fast Fourier transform of the measured cross-sectional curve of the surface is such that components with spatial frequencies of 1 cycle or more and 30 cycles or less account for 38% or more and 50% or less of the total, components with spatial frequencies exceeding 30 cycles and 120 cycles or less account for 35% or more and 50% or less of the total, and the remainder has a spatial frequency exceeding 120 cycles.

2. 2. The electrode plate for a plasma processing apparatus according to claim 1, wherein a large number of vent holes are formed in a penetrating state, and said surface is at least the surface in the outer periphery outside the region where the vent holes are formed.

3. A method for manufacturing an electrode plate for a plasma processing device, characterized in that a mixture of abrasive grains containing fine abrasive grains having a grit size of 800 or more and 1500 or less and coarse abrasive grains having a grit size of 80 or more and 200 or less is used when polishing the surface of a raw plate for the electrode plate.

4. The method for manufacturing an electrode plate for a plasma processing apparatus according to claim 3, characterized in that a large number of ventilation holes are formed in the electrode plate raw material, and the mixed abrasive grains are used when polishing the surface at least in the outer periphery outside the ventilation hole formation area.

Citation Information

Patent Citations

  • Apparatus and method for mask trimming

    JP2005085878A

  • Plasma CVD system and electrode for CVD system

    JP2006173343A

  • Plasma etching electrode plate

    JP2006196491A

  • Silicone electrode plate with a few partices produced for plasma etching apparatus

    JP2008085027A

  • Method and apparatus for refurbishing the surface of a gas distribution plate