Multilayer ceramic electronic components
By optimizing the internal conductor layers with specific hole distributions and ceramic pillar arrangements, the multilayer ceramic capacitor addresses electric field concentration issues, improving reliability and maintaining capacitance.
Patent Information
- Application Number
- JP2021100424
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-06-16
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-06-16
AI Technical Summary
Conventional multilayer ceramic capacitors do not adequately address the influence of holes in internal electrode layers on electric field concentration, which can lead to reliability issues.
The multilayer ceramic electronic component features internal conductor layers with holes of varying area equivalent diameters, where the abundance ratio of larger holes with ceramic pillars is increased to suppress electric field concentration, maintaining reliability while minimizing capacitance reduction.
This configuration effectively suppresses electric field concentration, enhancing the reliability of the multilayer ceramic capacitor without significantly reducing its capacitance.
Smart Images

Figure 0007585990000001 
Figure 0007585990000002 
Figure 0007585990000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a multilayer ceramic electronic component. [Background technology]
[0002] Conventionally, multilayer ceramic capacitors have been known. In general, multilayer ceramic capacitors include a laminate in which a plurality of dielectric layers and internal electrode layers are alternately stacked. For example, Patent Document 1 discloses a multilayer ceramic capacitor including a laminate in which a plurality of dielectric layers and internal electrode layers are alternately stacked, and a plurality of auxiliary electrodes. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-46086 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the multilayer ceramic capacitor of Patent Document 1, the electric field concentration is suppressed by providing multiple auxiliary electrodes, and the reliability of the product is improved. However, Patent Document 1 does not take into consideration the effect that holes in the internal electrode layers have on the electric field concentration of the multilayer ceramic capacitor.
[0005] An object of the present invention is to provide a multilayer ceramic electronic component capable of suppressing electric field concentration. [Means for solving the problem]
[0006] A multilayer ceramic electronic component according to the present invention comprises a laminate having a plurality of laminated ceramic layers and a plurality of internal conductor layers laminated on the ceramic layers, the laminate having first and second main surfaces opposing each other in a height direction, first side surfaces and second side surfaces opposing each other in a width direction perpendicular to the height direction, and first end surfaces and second end surfaces opposing each other in a length direction perpendicular to the height direction and the width direction, and external electrodes connected to the internal conductor layers, the internal conductor layers having a plurality of holes with different area-equivalent diameters, the plurality of holes having a first hole with a ceramic pillar disposed therein that connects a ceramic layer on one side of the internal conductor layer to a ceramic layer on the other side of the internal conductor layer, and a second hole in which the ceramic pillar is not disposed therein, wherein when an area-equivalent diameter D90 is defined as a cumulative value of 90% in a cumulative distribution of the area-equivalent diameters of the plurality of holes present in the internal conductor layer, the abundance ratio of the first holes in a first population composed of holes whose area-equivalent diameter is equal to or greater than the area-equivalent diameter D90 is 14% or more. Effect of the Invention
[0007] According to the present invention, it is possible to provide a multilayer ceramic electronic component capable of suppressing electric field concentration. [Brief description of the drawings]
[0008] [Figure 1] 1 is an external perspective view of a multilayer ceramic capacitor according to an embodiment; [Diagram 2] 2 is a cross-sectional view taken along line II-II of the multilayer ceramic capacitor shown in FIG. [Diagram 3] 3 is a cross-sectional view taken along line III-III of the multilayer ceramic capacitor shown in FIG. 2. [Figure 4A] 3 is a cross-sectional view taken along line IVA-IVA of the multilayer ceramic capacitor shown in FIG. 2. [Figure 4B] 4 is a cross-sectional view taken along line IVB-IVB of the multilayer ceramic capacitor shown in FIG. 2. [Diagram 5] 4B is an enlarged view of a portion V of the multilayer ceramic capacitor 1 shown in FIG. 4A. [Figure 6] FIG. 13 is a diagram showing area-equivalent diameter distribution data of a plurality of holes present in an internal electrode layer. [Figure 7A] FIG. 4 is a diagram showing a model of an internal electrode layer used in a first simulation. [Figure 7B] FIG. 13 is a diagram showing the electric field strength distribution in the vicinity of a hole in an internal electrode layer. [Figure 8] 13 is a graph plotting the maximum electric field intensity in each simulation model calculated by changing the value of the area equivalent diameter D99. [Figure 9] 13 is a graph plotting the average electric field intensity of holes of equivalent area diameter D90 or more, calculated in a simulation model in which the ratio of ceramic pillars present in holes of equivalent area diameter D90 or more is changed. [Figure 10] 11 is a graph showing normalized maximum electric field strength values of a first model and a second model. [Figure 11] 13 is a graph plotting maximum electric field strength in each simulation model in which the coverage of the internal electrode layer is changed. [Figure 12] 13 is a graph plotting maximum electric field strength in each simulation model in which the thickness of the internal electrode layer is changed. [Figure 13A] FIG. 13 is a diagram showing a model of a hole in an internal electrode layer used in a fifth simulation. [Figure 13B] FIG. 13 is a diagram showing the electric field strength distribution in the vicinity of a hole in an internal electrode layer. [Figure 14] 1 is a graph plotting scaled values of maximum electric field intensity generated near holes of different circularity. [Figure 15] 13 is a graph showing normalized maximum electric field strength values of the third and fourth models. [Figure 16] 4 is a scanning electron microscope image corresponding to an enlarged view of a portion XVI of the multilayer ceramic capacitor shown in FIG. 3, showing a burnt state at the time of dielectric breakdown of the laminate when an accelerated life test is performed. FIG. [Figure 17A] FIG. 1 is a diagram showing a multilayer ceramic capacitor having a double structure. [Figure 17B] FIG. 1 is a diagram showing a triple-structure multilayer ceramic capacitor. [Figure 17C] FIG. 1 is a diagram showing a multilayer ceramic capacitor having a four-row structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, a multilayer ceramic capacitor 1 as a multilayer ceramic electronic component according to an embodiment of the present disclosure will be described. Fig. 1 is an external perspective view of the multilayer ceramic capacitor 1 of this embodiment. Fig. 2 is a cross-sectional view taken along line II-II of the multilayer ceramic capacitor 1 in Fig. 1. Fig. 3 is a cross-sectional view taken along line III-III of the multilayer ceramic capacitor 1 in Fig. 2. Fig. 4A is a cross-sectional view taken along line IVA-IVA of the multilayer ceramic capacitor 1 in Fig. 2. Fig. 4B is a cross-sectional view taken along line IVB-IVB of the multilayer ceramic capacitor 1 in Fig. 2.
[0010] The multilayer ceramic capacitor 1 includes a laminate 10 and external electrodes 40 .
[0011] 1 to 4B show an XYZ orthogonal coordinate system. The length direction L of the multilayer ceramic capacitor 1 and the laminate 10 corresponds to the X direction. The width direction W of the multilayer ceramic capacitor 1 and the laminate 10 corresponds to the Y direction. The height direction T of the multilayer ceramic capacitor 1 and the laminate 10 corresponds to the Z direction. Here, the cross section shown in FIG. 2 is also referred to as an LT cross section. The cross section shown in FIG. 3 is also referred to as a WT cross section. The cross sections shown in FIGS. 4A and 4B are also referred to as an LW cross section.
[0012] As shown in Figures 1 to 4B, the laminate 10 includes a first main surface TS1 and a second main surface TS2 facing each other in a height direction T, a first side surface WS1 and a second side surface WS2 facing each other in a width direction W perpendicular to the height direction T, and a first end surface LS1 and a second end surface LS2 facing each other in a length direction L perpendicular to the height direction T and the width direction W.
[0013] As shown in FIG. 1, the laminate 10 has a substantially rectangular parallelepiped shape. The dimension of the laminate 10 in the length direction L is not necessarily longer than the dimension in the width direction W. The corners and ridges of the laminate 10 are preferably rounded. A corner is a portion where three faces of the laminate intersect, and a ridge is a portion where two faces of the laminate intersect. Incidentally, unevenness may be formed on a part or all of the surfaces constituting the laminate 10.
[0014] The dimensions of the laminate 10 are not particularly limited, but if the dimension of the laminate 10 in the length direction L is the L dimension, then the L dimension is preferably 0.2 mm or more and 6 mm or less. If the dimension of the laminate 10 in the height direction T is the T dimension, then the T dimension is preferably 0.05 mm or more and 5 mm or less. If the dimension of the laminate 10 in the width direction W is the W dimension, then the W dimension is preferably 0.1 mm or more and 5 mm or less.
[0015] As shown in Figures 2 and 3, the laminate 10 has an inner layer portion 11, and a first main surface side outer layer portion 12 and a second main surface side outer layer portion 13 arranged to sandwich the inner layer portion 11 in the height direction T.
[0016] The internal layer portion 11 includes a plurality of dielectric layers 20 as a plurality of ceramic layers, and a plurality of internal electrode layers 30 as a plurality of internal conductor layers. The internal layer portion 11 includes the internal electrode layer 30 located closest to the first main surface TS1 side to the internal electrode layer 30 located closest to the second main surface TS2 side in the height direction T. In the internal layer portion 11, the multiple internal electrode layers 30 are arranged opposite each other with the dielectric layer 20 interposed therebetween. The internal layer portion 11 is a portion that generates electrostatic capacitance and substantially functions as a capacitor.
[0017] The multiple dielectric layers 20 are made of a dielectric material. The dielectric material may be, for example, a dielectric ceramic containing a component such as BaTiO3, CaTiO3, SrTiO3, or CaZrO3. The dielectric material may also be a material in which a subcomponent such as a Mn compound, an Fe compound, a Cr compound, a Co compound, or a Ni compound is added to the main component. It is particularly preferable that the dielectric material is a material containing BaTiO3 as the main component.
[0018] The thickness of the dielectric layer 20 is preferably 0.2 μm or more and 10 μm or less. The number of laminated dielectric layers 20 is preferably 15 to 1200. The number of dielectric layers 20 is the total number of the dielectric layers in the inner layer portion 11 and the dielectric layers in the first main surface side outer layer portion 12 and the second main surface side outer layer portion 13.
[0019] The multiple internal electrode layers 30 (internal conductor layers 30) have multiple first internal electrode layers 31 (first internal conductor layers 31) and multiple second internal electrode layers 32 (second internal conductor layers 32). The multiple first internal electrode layers 31 are arranged on the multiple dielectric layers 20. The multiple second internal electrode layers 32 are arranged on the multiple dielectric layers 20. The multiple first internal electrode layers 31 and the multiple second internal electrode layers 32 are arranged alternately in the height direction T of the laminate 10 with the dielectric layer 20 interposed therebetween. The first internal electrode layers 31 and the second internal electrode layers 32 are arranged so as to sandwich the dielectric layer 20 therebetween.
[0020] The first internal electrode layer 31 has a first opposing portion 31A opposing the second internal electrode layer 32, and a first lead portion 31B led from the first opposing portion 31A to the first end face LS1. The first lead portion 31B is exposed at the first end face LS1.
[0021] The second internal electrode layer 32 has a second opposing portion 32A opposing the first internal electrode layer 31, and a second lead portion 32B led from the second opposing portion 32A to the second end face LS2. The second lead portion 32B is exposed at the second end face LS2.
[0022] In this embodiment, the first opposing portion 31A and the second opposing portion 32A face each other via the dielectric layer 20, forming a capacitance and exhibiting the characteristics of a capacitor.
[0023] The shapes of the first opposing portion 31A and the second opposing portion 32A are not particularly limited, but are preferably rectangular. However, the corners of the rectangular shape may be rounded or the corners of the rectangular shape may be formed at an angle. The shapes of the first drawn-out portion 31B and the second drawn-out portion 32B are not particularly limited, but are preferably rectangular. However, the corners of the rectangular shape may be rounded or the corners of the rectangular shape may be formed at an angle.
[0024] The dimension in the width direction W of the first opposing portion 31A and the dimension in the width direction W of the first drawn-out portion 31B may be the same dimension, or one of the dimensions may be smaller. The dimension in the width direction W of the second opposing portion 32A and the dimension in the width direction W of the second drawn-out portion 32B may be the same dimension, or one of the dimensions may be smaller.
[0025] As shown in Fig. 4A, the first internal electrode layer 31 has a first side WE1 on the first side surface WS1 side and a second side WE2 on the second side surface WS2 side. As shown in Fig. 4B, the second internal electrode layer 32 has a third side WE3 on the first side surface WS1 side and a fourth side WE4 on the second side surface WS2 side.
[0026] The first internal electrode layer 31 and the second internal electrode layer 32 are made of an appropriate conductive material such as a metal such as Ni, Cu, Ag, Pd, Au, or an alloy containing at least one of these metals. When an alloy is used, the first internal electrode layer 31 and the second internal electrode layer 32 may be made of, for example, an Ag-Pd alloy.
[0027] The thickness of each of the first internal electrode layers 31 and the second internal electrode layers 32 is preferably, for example, about 0.2 μm or more and 2.0 μm or less. The total number of the first internal electrode layers 31 and the second internal electrode layers 32 is preferably 15 to 1000.
[0028] The first main surface side outer layer portion 12 is located on the first main surface TS1 side of the laminate 10. The first main surface side outer layer portion 12 is an assembly of a plurality of dielectric layers 20 located between the first main surface TS1 and the internal electrode layer 30 closest to the first main surface TS1. The dielectric layer 20 used in the first main surface side outer layer portion 12 may be the same as the dielectric layer 20 used in the internal layer portion 11.
[0029] The second main surface side outer layer portion 13 is located on the second main surface TS2 side of the laminate 10. The second main surface side outer layer portion 13 is an assembly of a plurality of dielectric layers 20 located between the second main surface TS2 and the internal electrode layer 30 closest to the second main surface TS2. The dielectric layer 20 used in the second main surface side outer layer portion 13 may be the same as the dielectric layer 20 used in the internal layer portion 11.
[0030] In this manner, the laminate 10 has a plurality of laminated dielectric layers 20 and a plurality of internal electrode layers 30 laminated on the dielectric layers 20. In other words, the multilayer ceramic capacitor 1 has the laminate 10 in which the dielectric layers 20 and the internal electrode layers 30 are alternately laminated.
[0031] The laminate 10 has a counter electrode portion 11E. The counter electrode portion 11E is a portion where the first counter portion 31A of the first internal electrode layer 31 and the second counter portion 32A of the second internal electrode layer 32 face each other. The counter electrode portion 11E is configured as a part of the inner layer portion 11. FIGS. 4A and 4B show the range of the width direction W and length direction L of the counter electrode portion 11E. The counter electrode portion 11E is also called a capacitor effective portion.
[0032] The laminate 10 has a side surface outer layer portion. The side surface outer layer portion has a first side surface outer layer portion WG1 and a second side surface outer layer portion WG2. The first side surface outer layer portion WG1 is a portion including the dielectric layer 20 located between the counter electrode portion 11E and the first side surface WS1. The second side surface outer layer portion WG2 is a portion including the dielectric layer 20 located between the counter electrode portion 11E and the second side surface WS2. In FIG. 3, FIG. 4A, and FIG. 4B, the range of the width direction W of the first side surface outer layer portion WG1 and the second side surface outer layer portion WG2 are shown. The side surface outer layer portion is also called a W gap or a side gap.
[0033] The laminate 10 has an end surface side outer layer portion. The end surface side outer layer portion has a first end surface side outer layer portion LG1 and a second end surface side outer layer portion LG2. The first end surface side outer layer portion LG1 is a portion including the dielectric layer 20 located between the counter electrode portion 11E and the first end surface LS1. The second end surface side outer layer portion LG2 is a portion including the dielectric layer 20 located between the counter electrode portion 11E and the second end surface LS2. In FIG. 2, FIG. 4A, and FIG. 4B, the range of the length direction L of the first end surface side outer layer portion LG1 and the second end surface side outer layer portion LG2 are shown. The end surface side outer layer portion is also called an L gap or an end gap.
[0034] The external electrode 40 has a first external electrode 40A arranged on the first end face LS1 side, and a second external electrode 40B arranged on the second end face LS2 side.
[0035] The first external electrode 40A is disposed on the first end face LS1. The first external electrode 40A is connected to the first internal electrode layer 31. The first external electrode 40A may also be disposed on a part of the first main surface TS1 and a part of the second main surface TS2, as well as a part of the first side surface WS1 and a part of the second side surface WS2. In this embodiment, the first external electrode 40A is formed extending from the first end face LS1 to a part of the first main surface TS1 and a part of the second main surface TS2, as well as a part of the first side surface WS1 and a part of the second side surface WS2.
[0036] The second external electrode 40B is disposed on the second end face LS2. The second external electrode 40B is connected to the second internal electrode layer 32. The second external electrode 40B may also be disposed on a part of the first main surface TS1 and a part of the second main surface TS2, as well as a part of the first side surface WS1 and a part of the second side surface WS2. In this embodiment, the second external electrode 40B is formed extending from the second end face LS2 to a part of the first main surface TS1 and a part of the second main surface TS2, as well as a part of the first side surface WS1 and a part of the second side surface WS2.
[0037] As described above, in the laminate 10, the first opposing portion 31A of the first internal electrode layer 31 and the second opposing portion 32A of the second internal electrode layer 32 face each other via the dielectric layer 20, thereby forming a capacitance. Therefore, the characteristics of a capacitor are exhibited between the first external electrode 40A to which the first internal electrode layer 31 is connected and the second external electrode 40B to which the second internal electrode layer 32 is connected.
[0038] The first external electrode 40A has a first base electrode layer 50A and a first plating layer 60A disposed on the first base electrode layer 50A.
[0039] The second external electrode 40B has a second base electrode layer 50B and a second plating layer 60B disposed on the second base electrode layer 50B.
[0040] The first base electrode layer 50A is disposed on the first end face LS1. The first base electrode layer 50A is connected to the first internal electrode layer 31. In this embodiment, the first base electrode layer 50A is formed to extend from the first end face LS1 to a part of the first main surface TS1 and a part of the second main surface TS2, as well as a part of the first side surface WS1 and a part of the second side surface WS2.
[0041] The second base electrode layer 50B is disposed on the second end face LS2. The second base electrode layer 50B is connected to the second internal electrode layer 32. In this embodiment, the second base electrode layer 50B is formed to extend from the second end face LS2 to a part of the first main surface TS1 and a part of the second main surface TS2, as well as a part of the first side surface WS1 and a part of the second side surface WS2.
[0042] The first base electrode layer 50A and the second base electrode layer 50B of this embodiment are baked layers. The baked layer preferably contains a metal component and either a glass component or a ceramic component, or both. The metal component includes at least one selected from, for example, Cu, Ni, Ag, Pd, Ag-Pd alloy, Au, etc. The glass component includes at least one selected from, for example, B, Si, Ba, Mg, Al, Li, etc. The ceramic component may be the same type of ceramic material as the dielectric layer 20, or a different type of ceramic material. The ceramic component includes at least one selected from, for example, BaTiO3, CaTiO3, (Ba,Ca)TiO3, SrTiO3, CaZrO3, etc.
[0043] The baked layer is, for example, a conductive paste containing glass and metal applied to the laminate and baked. The baked layer may be a layered chip having an internal electrode and a dielectric layer and a conductive paste applied to the laminated chip, which are simultaneously baked, or a layered chip having an internal electrode and a dielectric layer is baked to obtain a laminate, and then a conductive paste is applied to the laminate and baked. In the case where a laminated chip having an internal electrode and a dielectric layer and a conductive paste applied to the laminated chip are simultaneously baked, it is preferable to form the baked layer by baking a layer to which a ceramic material is added instead of a glass component. In this case, it is particularly preferable to use the same type of ceramic material as the dielectric layer 20 as the ceramic material to be added. The baked layer may be a multi-layered layer.
[0044] The thickness in the longitudinal direction of the first base electrode layer 50A located on the first end face LS1 is preferably, for example, about 3 μm or more and 200 μm or less at the center in the height direction T and width direction W of the first base electrode layer 50A.
[0045] The thickness in the longitudinal direction of the second base electrode layer 50B located on the second end face LS2 is preferably, for example, about 3 μm or more and 200 μm or less at the center in the height direction T and width direction W of the second base electrode layer 50B.
[0046] When the first base electrode layer 50A is provided on a portion of at least one of the first main surface TS1 or the second main surface TS2, the height-wise thickness of the first base electrode layer 50A provided on this portion is preferably, for example, approximately 3 μm or more and 25 μm or less at the center in the length direction L and width direction W of the first base electrode layer 50A provided on this portion.
[0047] When the first base electrode layer 50A is provided on a portion of at least one of the first side surface WS1 or the second side surface WS2, the widthwise thickness of the first base electrode layer 50A provided on this portion is preferably, for example, approximately 3 μm or more and 25 μm or less at the center in the length direction L and height direction T of the first base electrode layer 50A provided on this portion.
[0048] When the second base electrode layer 50B is provided on a portion of at least one of the first main surface TS1 or the second main surface TS2, the height-wise thickness of the second base electrode layer 50B provided on this portion is preferably, for example, approximately 3 μm or more and 25 μm or less at the center in the length direction L and width direction W of the second base electrode layer 50B provided on this portion.
[0049] When the second base electrode layer 50B is provided on a portion of at least one of the first side surface WS1 or the second side surface WS2, the widthwise thickness of the second base electrode layer 50B provided on this portion is preferably, for example, approximately 3 μm or more and 25 μm or less at the center in the length direction L and height direction T of the second base electrode layer 50B provided on this portion.
[0050] The first base electrode layer 50A and the second base electrode layer 50B are not limited to baked layers. The first base electrode layer 50A and the second base electrode layer 50B include at least one selected from a baked layer, a conductive resin layer, a thin film layer, and the like. For example, the first base electrode layer 50A and the second base electrode layer 50B may be a thin film layer. The thin film layer is formed by a thin film formation method such as a sputtering method or a vapor deposition method. The thin film layer is a layer of 10 μm or less in which metal particles are deposited.
[0051] The first plating layer 60A is disposed so as to cover the first base electrode layer 50A.
[0052] The second plating layer 60B is disposed so as to cover the second base electrode layer 50B.
[0053] The first plating layer 60A and the second plating layer 60B may contain at least one selected from, for example, Cu, Ni, Sn, Ag, Pd, an Ag-Pd alloy, Au, etc. The first plating layer 60A and the second plating layer 60B may each be formed of a plurality of layers. The first plating layer 60A and the second plating layer 60B are preferably of a two-layer structure in which a Sn plating layer is formed on a Ni plating layer.
[0054] The first plating layer 60A is disposed so as to cover the first base electrode layer 50A. In this embodiment, the first plating layer 60A has a first Ni plating layer 61A and a first Sn plating layer 62A located on the first Ni plating layer 61A.
[0055] The second plating layer 60B is disposed so as to cover the second base electrode layer 50B. In the present embodiment, the second plating layer 60B has a second Ni plating layer 61B and a second Sn plating layer 62B located on the second Ni plating layer 61B.
[0056] The Ni plating layer prevents the first base electrode layer 50A and the second base electrode layer 50B from being eroded by solder when mounting the multilayer ceramic capacitor 1. The Sn plating layer improves the wettability of the solder when mounting the multilayer ceramic capacitor 1, thereby facilitating mounting of the multilayer ceramic capacitor 1. The thickness of each of the first Ni plating layer 61A, the first Sn plating layer 62A, the second Ni plating layer 61B, and the second Sn plating layer 62B is preferably 2 μm or more and 10 μm or less.
[0057] The first external electrode 40A and the second external electrode 40B of this embodiment may have a conductive resin layer containing, for example, conductive particles and a thermosetting resin. When a conductive resin layer is provided as the base electrode layer (first base electrode layer 50A, second base electrode layer 50B), the conductive resin layer may be disposed so as to cover the baked layer, or may be disposed directly on the laminate 10 without providing a baked layer. When the conductive resin layer is disposed so as to cover the baked layer, the conductive resin layer is disposed between the baked layer and the plating layer (first plating layer 60A, second plating layer 60B). The conductive resin layer may completely cover the baked layer, or may cover a part of the baked layer.
[0058] The conductive resin layer containing a thermosetting resin is more flexible than a conductive layer made of, for example, a plating film or a fired conductive paste. Therefore, even if the multilayer ceramic capacitor 1 is subjected to a physical shock or a shock caused by a thermal cycle, the conductive resin layer functions as a buffer layer. Therefore, the conductive resin layer suppresses the occurrence of cracks in the multilayer ceramic capacitor 1.
[0059] The metal constituting the conductive particles may be Ag, Cu, Ni, Sn, Bi, or an alloy containing them. The conductive particles preferably contain Ag. The conductive particles are, for example, Ag metal powder. Ag has the lowest resistivity among metals, so it is suitable as an electrode material. In addition, Ag is a precious metal, so it is resistant to oxidation and has high weather resistance. Therefore, Ag metal powder is suitable as a conductive particle.
[0060] The conductive particles may be metal powder with Ag coating on the surface. When using metal powder with Ag coating on the surface, the metal powder is preferably Cu, Ni, Sn, Bi or an alloy powder thereof. In order to make the base metal inexpensive while maintaining the characteristics of Ag, it is preferable to use Ag-coated metal powder.
[0061] Furthermore, the conductive particles may be Cu or Ni that has been subjected to an anti-oxidation treatment. The conductive particles may also be metal powders whose surfaces are coated with Sn, Ni, or Cu. When using metal powders whose surfaces are coated with Sn, Ni, or Cu, the metal powder is preferably Ag, Cu, Ni, Sn, Bi, or an alloy powder thereof.
[0062] The shape of the conductive particles is not particularly limited. The conductive particles may be spherical, flat, or the like, but it is preferable to use a mixture of spherical metal powder and flat metal powder.
[0063] The conductive particles contained in the conductive resin layer mainly play a role in ensuring the electrical conductivity of the conductive resin layer. Specifically, a plurality of conductive particles come into contact with each other to form an electrical path inside the conductive resin layer.
[0064] The resin constituting the conductive resin layer may contain at least one selected from various known thermosetting resins such as epoxy resin, phenol resin, urethane resin, silicone resin, and polyimide resin. Among them, epoxy resin, which has excellent heat resistance, moisture resistance, and adhesion, is one of the most suitable resins. In addition, it is preferable that the resin of the conductive resin layer contains a curing agent together with the thermosetting resin. When an epoxy resin is used as the base resin, the curing agent of the epoxy resin may be various known compounds such as phenol-based, amine-based, acid anhydride-based, imidazole-based, active ester-based, and amide-imide-based compounds.
[0065] The conductive resin layer may be formed of a plurality of layers. The conductive resin layer preferably has a thickness of 10 μm or more and 150 μm or less at its thickest portion.
[0066] Alternatively, a configuration may be adopted in which a first plating layer 60A and a second plating layer 60B, which will be described later, are disposed directly on the laminate 10 without providing the first base electrode layer 50A and the second base electrode layer 50B. That is, the multilayer ceramic capacitor 1 may be configured to include plating layers that are directly and electrically connected to the first internal electrode layer 31 and the second internal electrode layer 32. In such a case, the plating layers may be formed after a catalyst is disposed on the surface of the laminate 10 as a pretreatment.
[0067] Even in this case, the plating layer is preferably a multi-layer. The lower plating layer and the upper plating layer each preferably contain at least one metal selected from, for example, Cu, Ni, Sn, Pb, Au, Ag, Pd, Bi, or Zn, or an alloy containing these metals. The lower plating layer is more preferably formed using Ni, which has solder barrier properties. The upper plating layer is more preferably formed using Sn or Au, which has good solder wettability. For example, when the first internal electrode layer 31 and the second internal electrode layer 32 are formed using Ni, the lower plating layer is preferably formed using Cu, which has good bonding properties with Ni. The upper plating layer may be formed as necessary, and the external electrode 40 may be composed of only the lower plating layer. In addition, the plating layer may be the upper plating layer as the outermost layer, or another plating layer may be formed on the surface of the upper plating layer.
[0068] The thickness of each plating layer disposed without providing a base electrode layer is preferably 2 μm to 10 μm. The plating layer preferably does not contain glass. The metal ratio per unit volume of the plating layer is preferably 99 volume % or more.
[0069] In addition, when the plating layer is formed directly on the laminate 10, the thickness of the base electrode layer can be reduced. Therefore, the dimension of the multilayer ceramic capacitor 1 in the height direction T can be reduced by the amount of the reduction in the thickness of the base electrode layer, and the height of the multilayer ceramic capacitor 1 can be reduced. Alternatively, the thickness of the dielectric layer 20 sandwiched between the first internal electrode layer 31 and the second internal electrode layer 32 can be increased by the amount of the reduction in the thickness of the base electrode layer, and the thickness of the element can be improved. In this way, by forming the plating layer directly on the laminate 10, the design freedom of the multilayer ceramic capacitor can be improved.
[0070] If the lengthwise dimension of the multilayer ceramic capacitor 1 including the laminate 10 and the external electrodes 40 is defined as L dimension, then L dimension is preferably 0.2 mm or more and 6 mm or less. If the heightwise dimension of the multilayer ceramic capacitor 1 is defined as T dimension, then T dimension is preferably 0.05 mm or more and 5 mm or less. If the widthwise dimension of the multilayer ceramic capacitor 1 is defined as W dimension, then W dimension is preferably 0.1 mm or more and 5 mm or less.
[0071] Here, the inventors of the present application have found, through repeated investigations, experiments, and simulations, that in order to improve the reliability of a multilayer ceramic capacitor, it is desirable to make the holes in the internal electrode layers in an appropriate state. This point will be described below.
[0072] Conventionally, various methods have been used to improve the reliability of multilayer ceramic capacitors. For example, Patent Document 1 discloses a multilayer ceramic capacitor including a laminate in which dielectric layers and internal electrode layers are alternately stacked, and a plurality of auxiliary electrodes. In the multilayer ceramic capacitor of Patent Document 1, the provision of a plurality of auxiliary electrodes suppresses electric field concentration, improving the reliability of the product. However, since the multilayer ceramic capacitor of Patent Document 1 has a plurality of auxiliary electrodes, it is difficult to ensure the area of the capacitor effective portion that generates capacitance. Therefore, it is difficult to improve reliability while suppressing a decrease in capacitance.
[0073] The inventor of the present application has considered the above and diligently studied the configuration of the internal electrode layer that can improve reliability. As a result, the inventor of the present application has found that the configuration of this embodiment can suppress the decrease in capacitance while suppressing electric field concentration, thereby improving product reliability. Specifically, the inventor of the present application has discovered that when insulation breakdown occurs in a multilayer ceramic capacitor, burnout begins at a location where a hole exists in the internal electrode layer. The inventor of the present application has found that electric field concentration can be suppressed by increasing the presence ratio of holes with ceramic pillars arranged inside, particularly in holes with a large area equivalent diameter, among the multiple holes existing in the internal electrode layer. The internal electrode layer 30 of this embodiment will be described in detail below.
[0074] FIG. 5 is an enlarged view of the V portion of the multilayer ceramic capacitor 1 shown in FIG. 4A, and is a diagram illustrating an example of the state of the first internal electrode layer 31 as the internal electrode layer 30. More specifically, FIG. 5 is a diagram of the internal electrode layer 30 in the WT cross section of the multilayer ceramic capacitor 1 of this embodiment, as viewed in the height direction T connecting the first main surface TS1 and the second main surface TS2, that is, as viewed in a plan view. Note that, when viewed in the height direction T connecting the first main surface TS1 and the second main surface TS2, the covering state of the first internal electrode layer 31 with respect to the dielectric layer 20 and the covering state of the second internal electrode layer 32 with respect to the dielectric layer 20 are basically in the same state. Therefore, in the following description, the first internal electrode layer 31 and the second internal electrode layer 32 are collectively described as the internal electrode layer 30 as necessary.
[0075] Fig. 5 is a diagram showing the internal electrode layer 30 in the vicinity of a first side WE1 as a side of the internal electrode layer 30. As shown in Fig. 5, the internal electrode layer 30 has a plurality of holes H having different area equivalent diameters. The thickness of the internal electrode layer 30 shown in Fig. 5 is 0.6 µm, and the coverage, which is the coverage rate of the internal electrode layer with respect to the dielectric layer 20, is 82%.
[0076] FIG. 6 is a diagram showing area-equivalent diameter distribution data of a plurality of holes H present in the internal electrode layer 30. FIG. 6 shows cumulative % relative to the area-equivalent diameter. The horizontal axis of FIG. 6 is the area-equivalent diameter of the hole H, and the vertical axis of FIG. 6 is cumulative % showing the value obtained by dividing the number of holes H with an area-equivalent diameter or less (accumulated value of the number of holes) by the total number (number of holes forming the population). That is, the area-equivalent diameter distribution data shown in FIG. 6 is area-equivalent diameter distribution data based on the number. Note that the data in FIG. 6 is area-equivalent diameter distribution data in a measurement target region near the side of the internal electrode layer 30, and is data when holes present in a region wider than the region shown in FIG. 5 are used as the population.
[0077] In the multilayer ceramic capacitor 1 of this embodiment, when the area-equivalent diameter D99 is defined as the diameter at which the cumulative value of the cumulative distribution of the area-equivalent diameters of the multiple holes H present in the internal electrode layer 30 is 99%, the area-equivalent diameter D99 is preferably 8.0 μm or less, for example. In the example of the area-equivalent diameter distribution data shown in FIG. 6, the area-equivalent diameter D99 is 4.4 μm.
[0078] In addition, when the area-equivalent diameter D90 is defined as the area-equivalent diameter at which the cumulative value in the cumulative distribution of the area-equivalent diameters of the multiple holes H present in the internal electrode layer 30 is 90%, the area-equivalent diameter D90 is preferably, for example, 4.0 μm or less. For example, in the area-equivalent diameter distribution data of FIG. 6, the area-equivalent diameter D90 is 2.8 μm. This makes it possible to suppress electric field concentration and improve the reliability of the product.
[0079] The area equivalent diameter is the diameter of a perfect circle having an area equal to the area of the hole defined by the outline of the hole. For example, if the area of the hole defined by the outline of the hole is 50 μm 2 When , the area equivalent diameter is 8.0 μm.
[0080] As described above, the area-equivalent diameter D99 is the area-equivalent diameter at which the cumulative value in the cumulative distribution of the area-equivalent diameters of a plurality of holes is 99%. In other words, the value at which the ratio of holes with an area-equivalent diameter equal to or less than this is 99% is called the area-equivalent diameter D99. The area-equivalent diameter D90 is the area-equivalent diameter at which the cumulative value in the cumulative distribution of the area-equivalent diameters of a plurality of holes is 90%. In other words, the value at which the ratio of holes with an area-equivalent diameter equal to or less than this is called the area-equivalent diameter D90. The area-equivalent diameter D50 is also called the median diameter, and is the area-equivalent diameter at which the cumulative value in the cumulative distribution of the area-equivalent diameters of a plurality of holes is 50%. In other words, the value at which the ratio of holes with an area-equivalent diameter equal to or less than this is called the area-equivalent diameter D50. In other words, when the plurality of holes H are divided into two based on a certain area-equivalent diameter, the area-equivalent diameter at which the number of holes larger than the standard and the number of holes smaller than the standard are the same is called the area-equivalent diameter D50.
[0081] Here, in this embodiment, the multiple holes present in the internal electrode layer 30 include a first hole in which a ceramic pillar is disposed inside and a second hole in which a ceramic pillar is not disposed inside. In this embodiment, the abundance ratio of the first holes in the first population composed of holes having an area equivalent diameter D90 or more is 17% or more. Here, the material of the ceramic pillar is preferably the same dielectric material as that of the dielectric layer 20. It is particularly preferable that the dielectric material used for the dielectric layer 20 and the ceramic pillar is a material containing BaTiO3 as a main component. The ceramic pillar may be doped with the same type of subcomponent as that used for the dielectric layer 20. However, a different subcomponent may be doped. The ceramic pillar does not have to fill all of the holes. The inside of the second hole may be a gap, or a glass component such as silica may be present.
[0082] The abundance ratio R1 of the first holes in the first population is calculated by the following formula (1) using the number N1 of the first holes and the number N2 of the second holes in the first population. R1 = N1 / (N1 + N2) (1)
[0083] Next, the fact that the above-mentioned effects are obtained will be described using a simulation.
[0084] <First Simulation> FIG. 7A is a model of the internal electrode layer 30 used in the first simulation. In this model, the internal electrode layer 30 is provided on the dielectric layer 20. In this model, a plurality of holes H are randomly arranged as shown in FIG. 7A. The area equivalent diameters of the plurality of holes H vary. In this model, the plurality of holes H are formed as perfect circles. In this model, the back side of the dielectric layer 20 is also provided with an internal electrode layer 30 in which a plurality of holes H are randomly arranged, similar to the front side.
[0085] In the first simulation, a plurality of holes H were set in the internal electrode layer 30 so that the above-mentioned area equivalent diameter D99 was 8.0 μm. In addition, the thickness of the internal electrode layer 30 was set to 0.6 μm, the coverage of the internal electrode layer 30 with respect to the dielectric layer 20 was set to 88%, the thickness of the dielectric layer 20 was set to 2.0 μm, and the applied voltage was set to 37.5 V. In the simulation, a voltage was applied between the internal electrode layer 30 on the front side and the internal electrode layer 30 on the back side sandwiching the dielectric layer 20.
[0086] When a simulation was performed under these set conditions, it was confirmed that the electric field tends to concentrate around the outline of the hole H. FIG. 7B is a diagram showing the electric field strength distribution in the vicinity of the hole H. In FIG. 7B, the electric field strength is shown in grayscale, with areas with higher electric field strength being shown in lighter colors. FIG. 7B confirms that the electric field is concentrated around the outline of the hole H. It is also confirmed that the electric field tends to concentrate around the outline of a relatively large hole as shown on the left side of FIG. 7B, rather than around the outline of a relatively small hole as shown on the right side of FIG. 7B.
[0087] When the electric field strength generated in the model was calculated under these set conditions, as mentioned above, although the high electric field strength was concentrated around the relatively large holes, the maximum electric field strength in the model was 72MV / m or less, which is an allowable value for ensuring the reliability of the multilayer ceramic capacitor.
[0088] Next, the electric field intensity generated in each model was calculated using models in which the value of the area equivalent diameter D99 was changed. The thickness of the internal electrode layer 30, the coverage of the internal electrode layer 30 with respect to the dielectric layer 20, the thickness of the dielectric layer 20, and the applied voltage were set to constant values for the simulation. FIG. 8 is a graph showing the results. The horizontal axis of FIG. 8 is the value of the area equivalent diameter D99 in the model, and the vertical axis of FIG. 8 is the maximum electric field intensity in the model. FIG. 8 also shows an approximation curve obtained by fitting the plotted points.
[0089] First, it was confirmed that when a relatively large hole exists as in the conventional internal electrode layer 30, specifically, when the area-equivalent diameter D99 of the multiple holes H existing in the internal electrode layer 30 exceeds 8.0 μm, the value of the maximum electric field intensity in the model becomes high. For example, when the area-equivalent diameter D99 is 14.0 μm or more, the value of the maximum electric field intensity in the model exceeds 80 MV / m. More specifically, when the area-equivalent diameter D99 is 14.0 μm, 16.0 μm, 18.0 μm, and 20.0 μm, the maximum electric field intensity in the model is 80.7 MV / m, 86.9 MV / m, 87.5 MV / m, and 89.0 MV / m, respectively, all of which exceed 80 MV / m.
[0090] On the other hand, it was confirmed that if the area equivalent diameter D99 is 8.0 μm or less, the maximum electric field strength value generated in the model is below 72 MV / m, and electric field concentration is suppressed. For example, if the area equivalent diameter D99 is 4.0 μm or 2.0 μm, the maximum electric field strength value is about 60 MV / m or less, and electric field concentration is further suppressed. More specifically, when the area equivalent diameter D99 is 8.0 μm, 7.5 μm, 4.0 μm, and 2.0 μm, the maximum electric field strength is 70.7 MV / m, 71.3 MV / m, 56.0 MV / m, and 52.0 MV / m, respectively, all of which are 72 MV / m or less.
[0091] It can be seen from the data in FIG. 8 that the electric field concentration is suppressed when the area-equivalent diameter D99 is 2.0 μm or more and 8.0 μm or less. It can also be seen that the electric field concentration is further suppressed when the area-equivalent diameter D99 is 2.0 μm or more and 4.0 μm or less. In addition, based on the tendency of the data in FIG. 8, it is considered that the electric field concentration is suppressed even when the area-equivalent diameter D99 is 2.0 μm or less. For example, it is considered that the electric field concentration is suppressed even when the area-equivalent diameter D99 is 1.5 μm. For example, it is considered that the electric field concentration is suppressed even when the area-equivalent diameter D99 is 1.5 μm or more and 8.0 μm or less, and it is considered that the electric field concentration is further suppressed when the area-equivalent diameter D99 is 1.5 μm or more and 4.0 μm or less.
[0092] In this simulation, the area-equivalent diameter D90 of the model with the area-equivalent diameter D99 of 8.0 μm is 4.0 μm, the area-equivalent diameter D90 of the model with the area-equivalent diameter D99 of 7.5 μm is 3.8 μm, the area-equivalent diameter D90 of the model with the area-equivalent diameter D99 of 4.0 μm is 2.6 μm, and the area-equivalent diameter D90 of the model with the area-equivalent diameter D99 of 2.0 μm is 1.9 μm. The area-equivalent diameter D90 is preferably 4.0 μm or less. The area-equivalent diameter D90 is more preferably 2.6 μm or less. The area-equivalent diameter D90 is preferably 1.9 μm or more and 4.0 μm or less. The area-equivalent diameter D90 is more preferably 1.9 μm or more and 2.6 μm or less.
[0093] Here, in order to confirm the presence or absence of the dependence of the maximum electric field strength on the average hole diameter, a supplementary simulation was performed using a model in which the area-equivalent diameter D99 of a plurality of holes H present in the internal electrode layer 30 was fixed and the average diameter was changed. Specifically, a model in which the area-equivalent diameter D99 of the holes H was 7.5 μm and the average diameter of the holes H was 3.0 μm, and a model in which the area-equivalent diameter D99 of the holes H was 7.5 μm and the average diameter of the holes H was 2.0 μm were created. At this time, in both models, the coverage of the internal electrode layer 30 with respect to the dielectric layer 20 was adjusted to be 88%. In addition, in both models, the thickness of the internal electrode layer 30 was set to 0.6 μm, the thickness of the dielectric layer 20 was set to 2.0 μm, and the applied voltage was set to 37.5 V. As a result, in both models, the value of the maximum electric field strength in the model was 70 MV / m, and no difference was observed. This confirmed that the dependence of the average hole diameter on the maximum electric field strength was low.
[0094] From the above, it was confirmed that, for example, the smaller the value of the area-equivalent diameter D99 or the area-equivalent diameter D90, the more the electric field concentration tends to be suppressed. In contrast, the dependence of the average hole diameter on the maximum electric field strength is low. Therefore, it is expected that the change in the state of holes with a larger area-equivalent diameter contributes more to the suppression of the maximum electric field strength.
[0095] <Second Simulation> Next, a second simulation of this embodiment will be described. In the second simulation, it was confirmed whether it is possible to suppress electric field concentration by adjusting the abundance ratio of ceramic pillars present in holes in the internal electrode layer 30. Specifically, in a case where a plurality of holes present in the internal electrode layer 30 have a first hole in which a ceramic pillar that connects the dielectric layer 20 on one side of the internal electrode layer 30 and the dielectric layer 20 on the other side is arranged, and a second hole in which a ceramic pillar is not arranged, it was confirmed whether it is possible to suppress electric field concentration by adjusting the abundance ratio of the first hole.
[0096] Here, from the results of the simulations, it is expected that the change in the state of holes with a relatively large equivalent area diameter contributes to the suppression of electric field concentration. Therefore, using a model in which the state of the existence ratio of ceramic pillars is changed, it was confirmed whether the electric field concentration can be suppressed. Specifically, when the equivalent area diameter D90 is defined as the equivalent area diameter at which the cumulative value in the cumulative distribution of the equivalent area diameters of a plurality of holes present in the internal electrode layer 30 is 90%, the electric field intensity generated in each model was calculated using a model in which the existence ratio R1 of the first holes in the first population composed of holes with an equivalent area diameter of equal to or larger than the equivalent area diameter D90 is changed.
[0097] In the second simulation, the area equivalent diameter D99 was set to 7.5 μm, the thickness of the internal electrode layer 30 was set to 0.6 μm, the coverage of the internal electrode layer to the dielectric layer 20 was set to 88%, the thickness of the dielectric layer was set to 2.0 μm, and the applied voltage was set to 37.5 V, and the average value of the maximum electric field intensity occurring near each hole constituting the first population in the model was calculated. FIG. 9 is a graph showing the results. The horizontal axis of FIG. 9 is the abundance ratio R1 of the first hole in the first population composed of holes whose area equivalent diameter is equal to or larger than the area equivalent diameter D90, and the vertical axis of FIG. 9 is the average value of the maximum electric field intensity occurring near each hole constituting the first population. In the model, the material of the dielectric layer 20 and the ceramic pillars was the same dielectric material, and the holes whose area equivalent diameter is smaller than the area equivalent diameter D90 were composed of second holes in which no ceramic pillars were arranged.
[0098] The abundance ratio R1 of the first holes in the first population composed of holes whose area-equivalent diameter is equal to or larger than the area-equivalent diameter D90 is defined by the number N1 of the first holes and the number N2 of the second holes in the holes constituting the first population, as given by the following formula (1).
[0099] R1 = N1 / (N1 + N2) (1)
[0100] That is, the abundance ratio R1 of the first holes is calculated by dividing the number N1 of the first holes in the holes that make up the first population by the total number of holes that make up the first population.
[0101] As shown in FIG. 9, it was confirmed that if the abundance ratio R1 of the first holes in the holes constituting the first population is 14% or more, the average value of the maximum electric field strength occurring near each hole constituting the first population falls below 70MV / m. For example, if the abundance ratio R1 of the first holes is 29% or more, the average value of the maximum electric field strength is further reduced, and electric field concentration is further suppressed. Furthermore, if the abundance ratio R1 of the first holes is 43% or more, the average value of the maximum electric field strength is further reduced, and electric field concentration is further suppressed. Furthermore, if the abundance ratio R1 of the first holes is 71% or more, the average value of the maximum electric field strength is about 60MV / m, and electric field concentration is further suppressed. More specifically, when the abundance ratio R1 of the first holes was 14%, 29%, 43%, 57%, 71%, 86%, and 100%, the average values of the above-mentioned maximum electric field strength were 68.8MV / m, 66.3MV / m, 62.9MV / m, 61.7MV / m, 59.4MV / m, 56.9MV / m, and 54.2MV / m, respectively, all of which were below 70MV / m.
[0102] From the data in FIG. 9, it can be confirmed that electric field concentration is suppressed if the abundance ratio R1 of the first holes in the first population is 14% or more and 86% or less. It can also be confirmed that electric field concentration is suppressed if the abundance ratio R1 of the first holes in the first population is 29% or more and 86% or less. It can also be confirmed that electric field concentration is further suppressed if the abundance ratio R1 of the first holes in the first population is 43% or more, 57% or more, or 71% or more. The abundance ratio R1 of the first holes in the first population may be 86% or more. However, it may be 86% or less in consideration of productivity.
[0103] From the above, it was confirmed that the higher the abundance ratio R1 of the first holes in the holes constituting the first population, the more the electric field concentration tends to be suppressed. Specifically, by setting the abundance ratio R1 of the first holes in the holes constituting the first population to 14% or more, the electric field concentration can be suppressed. This can improve the reliability of the multilayer ceramic capacitor.
[0104] Here, from the results of the simulations so far, it is expected that the change in the state of holes with a relatively large equivalent area diameter contributes to the suppression of the maximum electric field intensity. Therefore, an additional simulation was performed using a model in which the state of the abundance ratio of the ceramic pillars was changed. Specifically, when the equivalent area diameter D90 is the equivalent area diameter at which the cumulative value in the cumulative distribution of the equivalent area diameters of a plurality of holes present in the internal electrode layer is 90%, a model was created in which the abundance ratio of the first holes in the first population composed of holes whose equivalent area diameter is equal to or larger than the equivalent area diameter D90 is 80%, and the abundance ratio of the first holes in the second population composed of holes whose equivalent area diameter is smaller than the equivalent area diameter D90 is 100%. In addition, a model was created in which the abundance ratio of the first holes in the first population composed of holes whose equivalent area diameter is equal to or larger than the equivalent area diameter D90 is 100%, and the abundance ratio of the first holes in the second population composed of holes whose equivalent area diameter is smaller than the equivalent area diameter D90 is 80%.
[0105] In the first and second models, the area equivalent diameter D99 was set to 7.5 μm, the thickness of the internal electrode layer was set to 0.6 μm, the coverage of the internal electrode layer relative to the dielectric layer was set to 88%, the thickness of the dielectric layer was set to 2.0 μm, and the applied voltage was set to 37.5 V, and the maximum electric field strength generated in the models was confirmed. Figure 10 is a graph showing the results. The vertical axis of Figure 10 shows the numerical value obtained by normalizing the maximum electric field strength, that is, the index when the maximum electric field strength in the first model is set to 1.
[0106] As shown in Fig. 10, it was confirmed that the maximum electric field strength value in the second model was lower than that in the first model. Specifically, it was confirmed that the maximum electric field strength value in the second model was about 25% lower than that in the first model. In other words, it was confirmed that the abundance ratio of ceramic pillars in holes with a relatively large equivalent area diameter contributes to suppressing the maximum electric field strength.
[0107] From the above, it can be seen that the maximum electric field strength can be reduced by making the abundance ratio of the first holes in the first population composed of holes whose equivalent area diameter is equal to or larger than the equivalent area diameter D90 higher than the abundance ratio of the first holes in the second population composed of holes whose equivalent area diameter is smaller than the equivalent area diameter D90, thereby improving the reliability of the multilayer ceramic capacitor.
[0108] <Third Simulation> Next, a third simulation will be described as an additional simulation. In the third simulation, a model in which the coverage, which is the coverage rate of the internal electrode layer 30 to the dielectric layer 20, is changed is used, and the electric field intensity generated in each model is calculated.
[0109] In the third simulation, the area equivalent diameter D99 was set to 7.5 μm, the thickness of the internal electrode layer 30 was set to 0.6 μm, the thickness of the dielectric layer 20 was set to 2.0 μm, and the applied voltage was set to 37.5 V, and the maximum electric field strength generated in the model was confirmed. Figure 11 is a graph showing the results. The horizontal axis of Figure 11 is the coverage of the internal electrode layer 30 in the model, and the vertical axis of Figure 11 is the maximum electric field strength in the model.
[0110] As shown in Fig. 11, it was confirmed that the maximum electric field strength value does not depend on the coverage value. Specifically, it was confirmed that the maximum electric field strength value is 72MV / m or less when the coverage is 70% or more and 99% or less. For example, it was confirmed that the maximum electric field strength value is 72MV / m or less when the coverage is 70%, 77%, 82%, 86%, 88%, 93%, 97%, and 99%.
[0111] In order to ensure capacitance, a high coverage is preferable. The third simulation confirms that even when the coverage is relatively high, for example, when the coverage is 70% or more and 99% or less, the configuration of this embodiment can be adopted to suppress the decrease in capacitance and improve the reliability of the product. It was also confirmed that even when the coverage is 86% or more and 93% or less, which is a range where the coverage is high and the productivity is good, the configuration of this embodiment can be adopted to suppress the decrease in capacitance and improve the reliability of the product.
[0112] It should be noted that the data of the third simulation shown in FIG. 11 is based on a model in which no ceramic pillars are present in the holes of the internal electrode layer 30. However, a similar trend is obtained even in a model in which ceramic pillars are present in the holes of the internal electrode layer 30, and the maximum electric field strength hardly changes even when the coverage is changed.
[0113] <Fourth Simulation> Next, a fourth simulation as an additional simulation will be described. In the third simulation, models in which the thickness of the internal electrode layer 30 was changed were used to calculate the electric field intensity generated in each model.
[0114] In the fourth simulation, the area equivalent diameter D99 was set to 7.5 μm, the coverage of the internal electrode layer 30 to the dielectric layer 20 was set to 88%, the thickness of the dielectric layer 20 was set to 2.0 μm, and the applied voltage was set to 37.5 V, and the maximum electric field intensity generated in the model was confirmed. Figure 12 is a graph showing the results. The horizontal axis of Figure 12 is the thickness of the internal electrode layer 30 in the model. The vertical axis of Figure 10 is the maximum electric field intensity in the model.
[0115] As shown in Fig. 12, the maximum electric field strength was not found to depend on the thickness of the internal electrode layer 30. Specifically, it was confirmed that the maximum electric field strength was 72 MV / m or less when the thickness of the internal electrode layer 30 was 0.2 µm or more and 2.0 µm or less. For example, it was confirmed that the maximum electric field strength was 72 MV / m or less when the thickness of the internal electrode layer 30 was 0.2 µm, 0.3 µm, 0.6 µm, 0.8 µm, 1.0 µm, 1.5 µm, and 2.0 µm.
[0116] By reducing the thickness of the internal electrode layer 30, the number of layers can be increased even for a laminate of the same size, so that the capacitance can be ensured. The fourth simulation confirms that even if the thickness of the internal electrode layer 30 is thin, for example, when the thickness of the internal electrode layer 30 is 0.2 μm or more and 2.0 μm or less, it is possible to improve the reliability of the product while suppressing the decrease in capacitance by adopting the configuration of this embodiment. It can be confirmed from the data in FIG. 12 that the thickness of the internal electrode layer 30 may be 0.2 μm or more and 1.0 μm or less, 0.2 μm or more and 0.8 μm or less, 0.2 μm or more and 0.6 μm or less, or 0.2 μm or more and 0.3 μm or less.
[0117] The thickness dimension of the internal electrode layer 30 may be smaller than the value of the above-mentioned area-equivalent diameter D99. For example, the area-equivalent diameter D99 may be 2.0 μm or more and 8.0 μm or less, while the thickness dimension of the internal electrode layer 30 may be less than 2.0 μm. For example, the area-equivalent diameter D99 may be 1.5 μm or more and 8.0 μm or less, while the thickness dimension of the internal electrode layer 30 may be 0.8 μm or less. In this case, the area-equivalent diameter D99 is a value larger than the thickness dimension of the internal electrode layer 30. By making the area-equivalent diameter D99 a predetermined value or less and making the thickness dimension of the internal electrode layer 30 smaller than the value of the area-equivalent diameter D99, it is possible to adopt a configuration that makes it easy to ensure capacitance while suppressing electric field concentration.
[0118] The thickness dimension of the internal electrode layer 30 may be half or less than the value of the above-mentioned area-equivalent diameter D99. For example, the area-equivalent diameter D99 may be 2.0 μm or more and 8.0 μm or less, while the thickness dimension of the internal electrode layer 30 may be 0.8 μm or less. For example, the area-equivalent diameter D99 may be 1.5 μm or more and 8.0 μm or less, while the thickness dimension of the internal electrode layer 30 may be 0.6 μm or less. By setting the area-equivalent diameter D99 to a predetermined value or less and setting the thickness dimension of the internal electrode layer 30 to half or less than the value of the area-equivalent diameter D99, it is possible to suppress electric field concentration while adopting a configuration that makes it easy to ensure capacitance.
[0119] The thickness dimension of the internal electrode layer 30 may be smaller than the value of the above-mentioned area-equivalent diameter D90. In this case, the area-equivalent diameter D90 is larger than the thickness dimension of the internal electrode layer 30. For example, the area-equivalent diameter D90 may be 4.0 μm or less, 3.8 μm or less, or 2.6 μm or less, and the thickness dimension of the internal electrode layer 30 may be smaller than the value of the area-equivalent diameter D90. By making the area-equivalent diameter D90 a predetermined value or less and making the thickness dimension of the internal electrode layer 30 smaller than the value of the area-equivalent diameter D90, it is possible to adopt a configuration that makes it easy to ensure capacitance while suppressing electric field concentration.
[0120] The thickness dimension of the internal electrode layer 30 may be half or less than the value of the above-mentioned area-equivalent diameter D90. For example, the area-equivalent diameter D90 may be 4.0 μm or less, 3.8 μm or less, or 2.6 μm or less, and the thickness dimension of the internal electrode layer 30 may be half or less than the area-equivalent diameter D90. By setting the area-equivalent diameter D90 to a predetermined value or less and setting the thickness dimension of the internal electrode layer 30 to half or less than the area-equivalent diameter D90, it is possible to adopt a configuration that makes it easy to ensure capacitance while suppressing electric field concentration.
[0121] It should be noted that the data of the fourth simulation shown in FIG. 12 is based on a model in which no ceramic pillars are present in the holes of the internal electrode layer 30. However, a similar trend is obtained even in a model in which ceramic pillars are present in the holes of the internal electrode layer 30, and the maximum electric field strength hardly changes even if the thickness of the internal electrode layer 30 is changed.
[0122] <5th Simulation> Next, a fifth simulation as an additional simulation will be described. In the fifth simulation, it was confirmed whether it is possible to further suppress the electric field concentration by adjusting the shape of the holes present in the internal electrode layer 30.
[0123] The left diagram of FIG. 13A is a model of holes in the internal electrode layer 30 used in the fifth simulation. In this model, the shapes of the holes are different. The hole model shown in this figure is modeled based on the outline of a hole formed in the actually manufactured internal electrode layer 30, as shown in the right diagram of FIG. 13A. In the fifth simulation, the thickness of the internal electrode layer was set to 0.6 μm, the thickness of the dielectric layer was set to 2.0 μm, and the applied voltage was set to 37.5 V, and the maximum electric field intensity generated near each of the six holes H1 to H6 in the model was confirmed. The area equivalent diameters of all six holes H1 to H6 were set to the same value, 3.0 μm.
[0124] First, the circularity of the holes was calculated as a shape index of the holes. The circularity of hole H1 was 0.456, the circularity of hole H2 was 0.204, the circularity of hole H3 was 0.995, the circularity of hole H4 was 0.272, the circularity of hole H5 was 0.321, and the circularity of hole H6 was 0.704.
[0125] Next, a simulation was performed to confirm the maximum electric field strength occurring near each of the holes H1 to H6. FIG. 13B is a diagram showing, as an example, the electric field strength distribution near the hole H3 with a high circularity and the electric field strength distribution near the hole H5 with a lower circularity than the hole H3. In FIG. 13B, the electric field strength is shown in grayscale, and the higher the electric field strength, the lighter the color. As shown in FIG. 13B, it is confirmed that the maximum electric field strength occurring around the outline of the hole H5 with a low circularity tends to be lower than the maximum electric field strength occurring around the outline of the hole H3 with a high circularity.
[0126] Fig. 14 is a graph in which the maximum electric field strength values generated near each of the holes H1 to H6 with different circularity are plotted after being normalized. The horizontal axis of Fig. 14 represents the circularity of the hole. The vertical axis of Fig. 14 represents the normalized maximum electric field strength, that is, the index when the maximum electric field strength generated near the hole H3, which is close to a perfect circle, is set to 1. Fig. 14 shows a straight line obtained by fitting the plotted points.
[0127] As shown in Fig. 14, it was confirmed that the value of the maximum electric field strength depends on the circularity of the hole. Specifically, it was confirmed that the lower the circularity of the hole, the lower the value of the maximum electric field strength. For example, if the circularity of the hole is 0.7 or less, the maximum electric field strength is reduced by about 15% compared to when the hole is almost a perfect circle. Also, if the circularity is 0.46 or less, the maximum electric field strength is reduced by about 30% compared to when the hole is almost a perfect circle.
[0128] In this way, by reducing the circularity of the holes present in the internal electrode layer 30, there was a tendency for the electric field concentration to be further suppressed.
[0129] Here, from the results of the simulations, it is expected that the circularity of holes with a relatively large equivalent area diameter contributes to suppressing the maximum electric field strength. Therefore, using a model in which the distribution of the circularity is changed, it was confirmed whether it is possible to reduce the maximum electric field strength. Specifically, when the equivalent area diameter D90 is the equivalent area diameter at which the cumulative value in the cumulative distribution of the equivalent area diameters of the holes H present in the internal electrode layer 30 is 90%, a third model was created in which the average value of the circularity of holes whose equivalent area diameter is equal to or greater than the equivalent area diameter D90 is 0.99, and the average value of the circularity of holes whose equivalent area diameter is smaller than the equivalent area diameter D90 is 0.59. In addition, a fourth model was created in which the average value of the circularity of holes whose equivalent area diameter is equal to or greater than the equivalent area diameter D90 is 0.59, and the average value of the circularity of holes whose equivalent area diameter is smaller than the equivalent area diameter D90 is 0.99.
[0130] In the third and fourth models, the area equivalent diameter D99 was set to 7.5 μm, the thickness of the internal electrode layer was set to 0.6 μm, the coverage of the internal electrode layer relative to the dielectric layer was set to 88%, the thickness of the dielectric layer was set to 2.0 μm, and the applied voltage was set to 37.5 V, and the maximum electric field strength generated in the models was confirmed. Figure 15 is a graph showing the results. The vertical axis of Figure 15 shows the numerical value obtained by normalizing the maximum electric field strength, that is, the index when the maximum electric field strength in the third model is set to 1.
[0131] As shown in Fig. 15, it was confirmed that the maximum electric field strength value in the fourth model was lower than that in the third model. Specifically, it was confirmed that the maximum electric field strength value in the fourth model was about 25% lower than that in the third model. In other words, it was confirmed that the circularity of holes with a relatively large equivalent area diameter particularly contributed to suppressing the maximum electric field strength.
[0132] From the above, it can be seen that the maximum electric field strength can be further reduced by lowering the circularity of holes having an area-equivalent diameter D90 or more and setting the average value to 0.7 or less. That is, the maximum electric field strength can be further reduced by setting the average circularity of a plurality of holes in a first population formed by holes having an area-equivalent diameter D90 or more to 0.7 or less. This can further improve the reliability of the multilayer ceramic capacitor. More preferably, the average circularity of holes having an area-equivalent diameter D90 or more is set to 0.46 or less. This can further reduce the maximum electric field strength. Therefore, the reliability of the multilayer ceramic capacitor can be further improved. The average circularity of holes having an area-equivalent diameter D90 or more may be 0.2 or more and 0.7 or less, or 0.2 or more and 0.46 or less.
[0133] It should be noted that the data of the fifth simulation shown in Figures 13B to 15 is based on a model in which no ceramic pillars are present in the holes of the internal electrode layer 30. However, a similar trend is obtained even in a model in which ceramic pillars are present in the holes of the internal electrode layer 30, and electric field concentration is further suppressed by reducing the circularity of the holes in the internal electrode layer 30.
[0134] The measurement methods of the various parameters will be described below. The various parameters can be confirmed by the following methods.
[0135] First, a description will be given of measurement target regions when measuring parameters such as the area equivalent diameter D99, the area equivalent diameter D90, the abundance ratio of the first holes having ceramic pillars disposed therein, and the average circularity.
[0136] The inventors of the present application have found, through repeated studies, experiments, and simulations, that in order to improve the reliability of multilayer ceramic electronic components such as multilayer ceramic capacitors, it is desirable to make holes in particular in a predetermined region of the internal electrode layer in an appropriate state. Specifically, by repeatedly carrying out analyses after accelerated life tests of multilayer ceramic capacitors, the inventors of the present application have found that the burn position at the time of dielectric breakdown of the laminate of a multilayer ceramic capacitor is often in the vicinity of the outer layer portion on the side surface and in an area slightly away from the edge (end) of the internal electrode layer, and that it is desirable to make holes in this area in an appropriate state.
[0137] Fig. 16 is a scanning electron microscope (SEM) image corresponding to an enlarged view of part XVI of the WT cross section of the multilayer ceramic capacitor shown in Fig. 3, and shows a burnt state at the time of dielectric breakdown of the laminate 10 when an accelerated life test is performed. As described above, in the multilayer ceramic capacitor 1, burnt portion D of the laminate 10 is likely to occur in a region near the side outer layer portion WG and slightly away from the edge of the internal electrode layer 30.
[0138] Therefore, it is preferable to set the multiple holes H of the internal electrode layer 30 in this region in an appropriate state, and it is preferable that the above-mentioned measurement target region is set in the vicinity of the side outer layer portion WG and a little away from the edge of the internal electrode layer 30.
[0139] Specifically, when the region in the first internal electrode layer 31 is defined as a first region A1 from a position 10 μm away from the first side WE1 to a position 50 μm away from the first side WE1, the region in the first internal electrode layer 31 is defined as a second region A2 from a position 10 μm away from the second side WE2 to a position 50 μm away from the second side WE2, the region in the second internal electrode layer 32 is defined as a third region A3 from a position 10 μm away from the third side to a position 50 μm away from the third side, and the region in the second internal electrode layer 32 is defined as a fourth region A4 from a position 10 μm away from the fourth side to a position 50 μm away from the fourth side, it is preferable that these first region A1, second region A2, third region A3 and fourth region A4 are the measurement target regions. When the linearity of the first side WE1 to the fourth side WE4 is low, each side is defined as a straight line by straight line fitting using linear regression or the like, and then the first area A1 to the fourth area A4 are defined.
[0140] Fig. 4A shows a schematic diagram of a first region A1 and a second region A2 as measurement target regions, and Fig. 4B shows a schematic diagram of a third region A3 and a fourth region A4 as measurement target regions.
[0141] Then, the first region A1, the second region A2, the third region A3, and the fourth region A4 are set as measurement target regions, and parameters such as the area equivalent diameter D99, the area equivalent diameter D90, the abundance ratio of the first holes, and the average value of the circularity are measured. Here, in order to simultaneously measure the abundance ratio of the first holes in which the ceramic pillars are disposed, the measurement is performed by three-dimensional structure observation using the FIB-SEM method.
[0142] Specifically, first, the multilayer ceramic capacitor is cross-sectionally polished up to 20 μm before the position of 1 / 2 of the L dimension to expose a specific WT cross section.
[0143] Then, three-dimensional structure observation is performed by FIB-SEM on the internal electrode layers 30 in the above-mentioned measurement target regions (first region A1 to fourth region A4). Here, the three-dimensional structure observation is performed at the center in the stacking direction T of the laminate 10. Also, the observation is performed in a portion corresponding to the above-mentioned measurement target region in the width direction W of the laminate 10, that is, in the vicinity of the side of the internal electrode layer 30. Also, the observation is performed at the center in the length direction L of the laminate 10. Figs. 4A and 4B show observation ranges b1 and b2 for performing three-dimensional structure observation with respect to the width direction W and length direction L.
[0144] As the size of the observation range for three-dimensional structure observation, the length in the height direction T is set to a distance that includes the six internal electrode layers 30. The length in the width direction W is set to 40 μm. The length in the length direction L is set to 40 μm.
[0145] In three-dimensional structure observation, processing by FIB (focused ion beam) and acquisition of SEM images are repeated alternately. The processing step of FIB processing is set to 0.4 μm. The processing direction of FIB processing is the length direction L. The number of processing steps of FIB processing is set to 100. Three-dimensional reconstruction data is formed by three-dimensionally reconstructing multiple continuous cross-sectional SEM images in the length direction L obtained in this manner by image processing. It is possible to generate arbitrary cross sections and display them in volume rendering based on the three-dimensional reconstruction data formed in this manner.
[0146] The observation range b1 includes three layers of a portion of the first region A1 of the first internal electrode layer 31. Also, the observation range b1 includes three layers of a portion of the third region A3 of the second internal electrode layer 32. The observation range b2 includes three layers of a portion of the second region A2 of the first internal electrode layer 31. Also, the observation range b2 includes three layers of a portion of the fourth region A4 of the second internal electrode layer 32.
[0147] Therefore, from the observation range b1, three analysis ranges for the first region A1 of the first internal electrode layer 31 are set. From the observation range b1, three analysis ranges for the third region A3 of the second internal electrode layer are set. From the observation range b2, three analysis ranges for the second region A2 of the first internal electrode layer 31 are set. From the observation range b2, three analysis ranges for the fourth region A4 of the second internal electrode layer are set.
[0148] The measurement range in which various parameters are measured is set by a set of 12 analysis ranges (4 regions x 3 locations).
[0149] When the chip size of the multilayer ceramic electronic component is large, the three-dimensional structure observation targeting the observation area b1 and the three-dimensional structure observation targeting the observation area b2 may be performed separately. When the chip size of the multilayer ceramic electronic component is small, the observation targeting the observation area b1 and the observation area b2 may be performed in a single three-dimensional structure observation. When the chip size of the multilayer ceramic electronic component is particularly small, the first area A1 to the fourth area A4 may be set in overlapping positions. That is, the observation area b1 and the observation area b2 may overlap. In this case, the observation targeting the observation area b1 and the observation area b2 is performed in a single three-dimensional structure observation.
[0150] <Measuring method for area equivalent diameter D99, D90> A method for measuring the area-equivalent diameters D99 and D90 of holes present in the internal electrode layer 30 will be described.
[0151] Based on the three-dimensional reconstruction data obtained by the FIB-SEM method, the outline of each hole formed in the internal electrode layer 30 is identified. Then, for each hole formed in the internal electrode layer 30, the area-equivalent diameter of the hole is calculated based on the area of the hole defined by the outline of the hole. The area-equivalent diameter is the diameter of a perfect circle having an area equal to the area of the hole defined by the outline of the hole.
[0152] For the 12 analysis ranges a constituting the measurement range, the area equivalent diameter of each of the holes is calculated. 2 Anything less than this value may be noise rather than a hole. Therefore, to eliminate the effect of noise, we will exclude it from the analysis below.
[0153] All holes identified in the measurement range, i.e., the 12 analysis ranges (the above-mentioned holes have an area of 1.0 μm 2 The set of all the holes (excluding those with values less than 0.01) is set as the population of holes.
[0154] Based on the data of the area-equivalent diameter of the population of holes in the measurement range, the area-equivalent diameter D99 and the area-equivalent diameter D90 are calculated. The area-equivalent diameter D99 is calculated as the area-equivalent diameter at which the cumulative value in the number-based cumulative distribution of the area-equivalent diameters of the multiple holes present in the measurement range is 99%. The area-equivalent diameter D90 is calculated as the area-equivalent diameter at which the cumulative value in the number-based cumulative distribution of the area-equivalent diameters of the multiple holes present in the measurement range is 90%.
[0155] In addition, as an arbitrary cross section based on the three-dimensional reconstruction data, a WL cross section in which the internal electrode layer 30 is viewed in a plane in the height direction T may be created, and the contours of each hole formed in the internal electrode layer 30 may be identified based on the WL cross section in which the internal electrode layer 30 is viewed in a plane, and the parameters may be calculated thereafter. Alternatively, the contours of each hole formed in the internal electrode layer 30 may be automatically identified from the three-dimensional reconstruction data by a pre-programmed process, and the parameters may be calculated thereafter.
[0156] <Method for measuring ceramic pillar abundance ratio> A method for measuring the abundance ratio of the first holes in which ceramic pillars are arranged will be described. In detail, when the multiple holes present in the internal electrode layer 30 have a first hole in which a ceramic pillar is arranged connecting the dielectric layer 20 on one side of the internal electrode layer 30 and the dielectric layer 20 on the other side, and a second hole in which no ceramic pillar is arranged, the abundance ratio of the first holes is measured by the following method. More specifically, when the area-equivalent diameter D90 is set as the area-equivalent diameter at which the cumulative value in the cumulative distribution of the area-equivalent diameters of the multiple holes present in the internal electrode layer 30 is 90%, the abundance ratio R1 of the first holes in which ceramic pillars are arranged in holes having an area-equivalent diameter larger than the area-equivalent diameter D90 is measured by the following method.
[0157] Based on the three-dimensional reconstruction data obtained by the FIB-SEM method, the contours of each hole formed in the internal electrode layer 30 are identified. Then, for each hole formed in the internal electrode layer 30, an area equivalent diameter of the hole is calculated based on the area of the hole defined by the hole contour. In addition, based on the three-dimensional reconstruction data, for each hole, a first hole having a ceramic pillar disposed therein and a second hole having no ceramic pillar disposed therein are identified.
[0158] The area equivalent diameter of each of the holes is calculated for the 12 analysis ranges that make up the measurement range. 2 Anything less than this value may be noise rather than a hole. Therefore, to eliminate the effect of noise, we will exclude it from the analysis below.
[0159] All holes identified in the measurement range, i.e., the 12 analysis ranges (the above-mentioned holes have an area of 1.0 μm 2 The set of all the holes (excluding those with values less than 0.01) is set as the population of holes.
[0160] The population of holes present in the measurement target area is divided into a first population consisting of holes whose area-equivalent diameter is equal to or larger than the area-equivalent diameter D90, and a second population consisting of holes whose area-equivalent diameter is smaller than the area-equivalent diameter D90. Then, the number of first holes and the number of second holes are counted in each of the first population and the second population.
[0161] The abundance ratio R1 of the first holes in the first population composed of holes whose area-equivalent diameter is equal to or larger than the area-equivalent diameter D90 is defined by the number N1 of the first holes and the number N2 of the second holes in the holes constituting the first population, as given by the following formula (1).
[0162] R1 = N1 / (N1 + N2) (1)
[0163] That is, the abundance ratio R1 of the first holes in the first population is calculated by dividing the number N1 of the first holes in the holes that make up the first population by the total number of holes that make up the first population.
[0164] The abundance ratio R2 of the first holes in the second population composed of holes whose area-equivalent diameter is smaller than the area-equivalent diameter D90 is defined by the number N3 of the first holes and the number N4 of the second holes in the holes that compose the second population, as given by the following equation (2).
[0165] R2 = N3 / (N3 + N4) (2)
[0166] That is, the abundance ratio R2 of the first holes in the second population is calculated by dividing the number N3 of the first holes in the holes that make up the second population by the total number of holes that make up the second population.
[0167] <Method of measuring the circularity of a hole> A method for measuring the circularity of holes present in the internal electrode layer 30 will be described.
[0168] Based on the three-dimensional reconstruction data obtained by the FIB-SEM method, the outline of each hole formed in the internal electrode layer 30 is identified. Then, for each hole formed in the internal electrode layer 30, the area-equivalent diameter of the hole is calculated based on the area of the hole defined by the outline of the hole. The area-equivalent diameter is the diameter of a perfect circle having an area equal to the area of the hole defined by the outline of the hole.
[0169] The area equivalent diameter of each of the holes is calculated for the 12 analysis ranges that make up the measurement range. 2 Anything less than this value may be noise rather than a hole. Therefore, to eliminate the effect of noise, we will exclude it from the analysis below.
[0170] All holes identified in the measurement range, i.e., the 12 analysis ranges (the above-mentioned holes have an area of 1.0 μm 2 The set of all the holes (excluding those with values less than 0.01) is set as the population of holes.
[0171] For each hole in the hole population, the circularity of the hole is calculated based on the area and circumference of the hole defined by the outline of the hole, using the following formula (3). Circularity = 4π × (area) / (circumference) 2 (3)
[0172] Furthermore, the population of holes present in the measurement target area is divided into a first population consisting of holes whose equivalent area diameter is equal to or larger than D90, and a second population consisting of holes whose equivalent area diameter is smaller than D90. Then, the average value of the circularity of the holes in the first population consisting of holes whose equivalent area diameter is equal to or larger than D90 is calculated. This is set as the average value of the circularity of the holes in the first population in this embodiment.
[0173] <How coverage is measured> A method for measuring the coverage as the coverage rate of the internal electrode layer 30 to the dielectric layer 20 will be described.
[0174] Based on the three-dimensional reconstruction data obtained by the FIB-SEM method, the area of the internal electrode layer 30 covering the dielectric layer 20 in the analysis range is identified. Then, based on the area of the analysis range and the area of the area of the internal electrode layer 30, the coverage rate of the internal electrode layer 30 with respect to the dielectric layer 20 is calculated by the following formula (4). Coverage rate (%) = (area of internal electrode layer / area of analysis range) × 100 (4)
[0175] The coverage of the internal electrode layers 30 to the dielectric layers 20 is calculated for the 12 analysis ranges constituting the measurement range. Then, the average value is set as the coverage of the internal electrode layers 30 to the dielectric layers 20 in this embodiment.
[0176] In addition, as an arbitrary cross section based on the three-dimensional reconstruction data, a WL cross section in which the internal electrode layer 30 is viewed in a plane in the height direction T may be generated, and the coverage of the internal electrode layer 30 with respect to the dielectric layer 20 may be calculated based on the WL cross section in which the internal electrode layer 30 is viewed in a plane. Alternatively, the coverage of the internal electrode layer 30 with respect to the dielectric layer 20 may be automatically calculated from the three-dimensional reconstruction data by a process programmed in advance.
[0177] <Method for measuring the thickness of the internal electrode layer> A method for measuring the thicknesses of the internal electrode layers 30 will be described.
[0178] First, the multilayer ceramic capacitor is cross-sectionally polished to a position 20 μm short of the half position of the L dimension to expose a specific WT cross section. Then, the WT cross section of the laminate 10 exposed by polishing is observed by SEM.
[0179] Next, the thicknesses of the internal electrode layers 30 are measured on a total of five lines, including a center line along the stacking direction passing through the center of the cross section of the laminate 10, and two lines drawn equally spaced on each side of the center line. Here, the thicknesses of the internal electrode layers 30 at these five locations are measured in each of three parts in the stacking direction of the laminate 10. The average value of the thicknesses of the internal electrode layers 30 at a total of 15 locations (three parts x five locations) is set as the thickness of the internal electrode layers 30 in this embodiment.
[0180] Next, a method for manufacturing the multilayer ceramic capacitor 1 of this embodiment will be described.
[0181] A dielectric sheet for the dielectric layer 20 and a conductive paste for the internal electrode layer 30 are prepared. The dielectric sheet and the conductive paste for the internal electrodes contain a binder and a solvent. The binder and the solvent may be known.
[0182] A conductive paste for the internal electrode layer 30 is printed in a predetermined pattern on the dielectric sheet by, for example, screen printing, gravure printing, etc. In this way, a dielectric sheet on which the pattern of the first internal electrode layer 31 is formed and a dielectric sheet on which the pattern of the second internal electrode layer 32 is formed are prepared.
[0183] A predetermined number of dielectric sheets on which the pattern of the internal electrode layer is not printed are laminated to form a portion that will become the first main surface side outer layer portion 12 on the first main surface TS1 side. A dielectric sheet on which the pattern of the first internal electrode layer 31 is printed and a dielectric sheet on which the pattern of the second internal electrode layer 32 is printed are laminated in order thereon to form a portion that will become the internal layer portion 11. A predetermined number of dielectric sheets on which the pattern of the internal electrode layer is not printed are laminated on the portion that will become the internal layer portion 11 to form a portion that will become the second main surface side outer layer portion 13 on the second main surface TS2 side. In this way, a laminated sheet is produced.
[0184] The laminated sheets are pressed in the height direction by means of a hydrostatic press or the like to produce a laminated block.
[0185] The laminated block is cut to a predetermined size to obtain laminated chips. At this time, corners and edges of the laminated chips may be rounded by barrel polishing or the like.
[0186] The laminated chip is fired to produce the laminate 10. The firing temperature depends on the materials of the dielectric layers 20 and the internal electrode layers 30, but is preferably 900° C. or higher and 1400° C. or lower.
[0187] Here, the above-mentioned manufacturing conditions are adjusted in order to set the area-equivalent diameter D99 of the holes present in the internal electrode layer 30 to a predetermined value or less, for example, 8.0 μm or less, 7.5 μm or less, or 4.0 μm or less, and to keep it within a predetermined range.
[0188] Specifically, the pressure, temperature, and pressurization time during lamination of the dielectric sheets on which the patterns of the internal electrode layers 30 are printed are adjusted so that the area-equivalent diameter D99 of the holes present in the internal electrode layers 30 is adjusted to a predetermined value or less. For example, when the internal electrode layers 30 are relatively thin, the pressure during pressing of the laminated sheets is set to be higher.
[0189] In addition, the material of the conductive paste for the internal electrode layer 30 may be prepared so that the area equivalent diameter D99 of the holes present in the internal electrode layer 30 is equal to or less than a predetermined value. For example, when the main component of the internal electrode layer 30 is Ni, the Ni particles as the raw material of the conductive paste may have a larger average particle diameter, so that the bonding start temperature between the Ni particles and the sintering shrinkage start temperature of the ceramic are brought closer to each other. As a result, the internal electrode layer 30 is prevented from becoming a ball, and the area equivalent diameter D99 is adjusted to be equal to or less than a predetermined value. In addition, when the same ceramic powder as the ceramic powder contained in the dielectric layer 20 is added as a co-material to the conductive paste for the internal electrode layer 30, the co-material having a larger average particle diameter is used, so that the bonding start temperature between the Ni particles and the sintering shrinkage start temperature of the ceramic are brought closer to each other. As a result, the internal electrode layer 30 is prevented from becoming a ball, and the area equivalent diameter D99 is adjusted to be equal to or less than a predetermined value. In addition, the affinity between the Ni particles, the co-material, and the solvent of the conductive paste for the internal electrode layer 30 may be controlled to enhance the co-material dispersibility. This suppresses the internal electrode layer 30 from becoming a ball, and adjusts the hole area equivalent diameter D99 to a predetermined value or less.
[0190] Also, when firing the laminated chip, the laminated chips may be arranged closely together to improve the uniformity of the temperature inside the chip during firing. This suppresses the balling of the internal electrode layer 30, and the area equivalent diameter D99 is adjusted to be equal to or less than a predetermined value. Also, the laminated chip may be fired while embedded in ceramic powder to improve the uniformity of the temperature inside and outside the chip during firing. This suppresses the balling of the internal electrode layer 30, and the area equivalent diameter D99 is adjusted to be equal to or less than a predetermined value. Note that, during firing, the temperature of the portion close to the first side surface and the second side surface of the laminated chip, for example, the side of the internal electrode layer 30 on the first side surface WS1 side and the side of the internal electrode layer 30 on the second side surface WS2 side, tends to rise. Therefore, the internal electrode layer 30 tends to ball in this portion. However, the above-mentioned method suppresses the balling of the first region A1 to the fourth region A4 of the internal electrode layer 30, and the area equivalent diameter D99 of the hole present in the internal electrode layer 30 can be set to be equal to or less than a predetermined value.
[0191] In addition, the internal electrode layer 30 may be formed by two-step printing so that the area-equivalent diameter D99 of holes present at least in the portions close to the first and second side faces of the laminated chip, for example, the first region A1 to the fourth region A4, is a predetermined value or less. In this case, a conductive paste containing Ni particles with a large average particle diameter and a common material with a large average particle diameter is printed at least in the first region A1 to the fourth region A4. Then, a conductive paste containing Ni particles with a relatively small average particle diameter and a common material with a relatively small average particle diameter is printed in other regions including the central region of the internal electrode layer 30. As a result, the area-equivalent diameter D99 of holes present at least in the first region A1 to the fourth region A4 can be made to be a predetermined value or less.
[0192] The above-mentioned methods for adjusting the area-equivalent diameter D99 of the hole present in the internal electrode layer 30 to a predetermined value or less can be appropriately combined. This allows the area-equivalent diameter D99 of the hole present in the internal electrode layer 30 to be adjusted to a predetermined value or less, for example, 8.0 μm or less, 7.5 μm or less, or 4.0 μm or less, or within a predetermined range. Similarly, the above-mentioned methods allow the area-equivalent diameter D90 of the hole present in the internal electrode layer 30 to be adjusted to a predetermined value or less, for example, 4.0 μm or less, 3.8 μm or less, 2.6 μm or less, or within a predetermined range.
[0193] Here, in order to facilitate the arrangement of ceramic columns in the multiple holes present in the internal electrode layer 30, the material of the conductive paste for the internal electrode layer 30 may be prepared. For example, a conductive paste with an increased amount of added common material is used. This increases the amount of common material discharged into the holes. Also, a conductive paste in which the common material is atomized and the amount of added common material is increased may be used. This increases the amount of common material discharged into the holes. In this way, by increasing the amount of common material blown into the holes, the probability of ceramic columns occurring is increased. Also, by increasing the pressure when pressing the laminated sheet, particularly in the region where the coating film of the conductive paste near the end of the internal electrode layer 30 is thin, a portion where the upper and lower ceramic sheets sandwiching the conductive paste come close to each other is generated, and a portion where the continuity of the conductive paste is partially impaired is generated. During firing, the internal electrode layer 30 is interrupted at that portion, and the material of the ceramic sheet enters, making it easier to generate ceramic columns, especially for large holes of D90 or more. That is, the presence ratio of the first hole in which the ceramic column is arranged can be increased in the large holes of D90 or more.
[0194] In addition, by forming the internal electrode layer 30 by two-step printing, the presence ratio of the first holes in which the ceramic pillars are arranged may be increased at least in the portions close to the first side surface and the second side surface of the laminated chip, for example, in the holes present in the first region A1 to the fourth region A4. In this case, a conductive paste with an increased amount of common material is printed at least in the first region A1 to the fourth region A4. Then, a conductive paste using a common material with a relatively small amount of common material is printed in other regions including the central region of the internal electrode layer 30. This makes it possible to increase the first presence ratio of the first holes in which the ceramic pillars are arranged at least in the holes present in the first region A1 to the fourth region A4.
[0195] In addition, the material of the conductive paste for the internal electrode layer 30 may be prepared so that the circularity of the holes present in the internal electrode layer 30 is a predetermined value or less, for example, the average value of the circularity of the holes having an area equivalent diameter D90 or more is 0.7 or less, or 0.46 or less. For example, when the main component of the internal electrode layer 30 is Ni, particles having a variation in particle diameter may be used as Ni particles as the raw material of the conductive paste. As a result, holes having an irregular shape such as a plurality of small holes connected to each other are formed, and the circularity of the larger holes can be reduced. In addition, when the same ceramic powder as the ceramic powder contained in the dielectric layer 20 is added as a common material, a common material having a variation in particle diameter may be used as the common material. As a result, holes having an irregular shape such as a plurality of small holes connected to each other are formed, and the circularity of the larger holes can be reduced. By using these methods, the average value of the circularity of the holes having an area equivalent diameter D90 or more can be set to a predetermined value or less.
[0196] The internal electrode layer 30 may be formed by two-step printing, so that the circularity of holes present at least in the portions close to the first and second side faces of the laminated chip, for example, in the first region A1 to the fourth region A4, is a predetermined value or less. In this case, a conductive paste using Ni particles having a variation in particle diameter and a common material having a variation in particle diameter is printed at least in the first region A1 to the fourth region A4. Then, a conductive paste containing Ni particles with suppressed variation in particle diameter and a common material with suppressed variation in particle diameter is printed in other regions including the central region of the internal electrode layer 30. As a result, for holes present at least in the first region A1 to the fourth region A4, the average value of the circularity of holes having an area equivalent diameter D90 or more can be set to a predetermined value or less. The internal electrode layer 30 may be formed using such a method so that the average value of the circularity of holes present in the first region A1 to the fourth region A4 is lower than the average value of the circularity of holes present in the central region of the internal electrode layer 30.
[0197] A conductive paste that will become the base electrode layers (first base electrode layer 50A, second base electrode layer 50B) is applied to both end surfaces of the laminate 10. In this embodiment, the base electrode layers are baked layers. A conductive paste containing a glass component and a metal is applied to the laminate 10 by a method such as dipping. Then, a baking process is performed to form the base electrode layers. The temperature of the baking process at this time is preferably 700°C or higher and 900°C or lower.
[0198] In addition, when the laminated chip before firing and the conductive paste applied to the laminated chip are fired at the same time, it is preferable to form the fired layer by firing a material to which a ceramic material is added instead of a glass component. In this case, it is particularly preferable to use the same type of ceramic material as that of the dielectric layer 20 as the ceramic material to be added. In this case, the conductive paste is applied to the laminated chip before firing, and the laminated chip and the conductive paste applied to the laminated chip are fired at the same time to form the laminate 10 with the fired layer.
[0199] Thereafter, a plating layer is formed on the surface of the base electrode layer. In this embodiment, a first plating layer 60A is formed on the surface of the first base electrode layer 50A. Also, a second plating layer 60B is formed on the surface of the second base electrode layer 50B. In this embodiment, a Ni plating layer and an Sn plating layer are formed as the plating layers. Either electrolytic plating or electroless plating may be used for plating. However, electroless plating has the disadvantage of complicating the process because it requires pretreatment with a catalyst or the like to improve the plating deposition rate. Therefore, it is usually preferable to use electrolytic plating. The Ni plating layer and the Sn plating layer are formed in sequence, for example, by barrel plating.
[0200] When the base electrode layer is formed as a thin film layer, a thin film layer is formed as the base electrode layer in the area where the external electrode is to be formed by performing masking or the like. The thin film layer is formed by a thin film formation method such as sputtering or vapor deposition. The thin film layer is a layer of 1.0 μm or less in which metal particles are deposited.
[0201] When a conductive resin layer is provided as the base electrode layer, the conductive resin layer may be disposed so as to cover the baked layer, or may be disposed directly on the laminate 10 without providing a baked layer. When a conductive resin layer is provided, a conductive resin paste containing a thermosetting resin and a metal component is applied onto the baked layer or onto the laminate 10, and then heat-treated at a temperature of 250 to 550°C or higher. As a result, the thermosetting resin is thermally cured to form a conductive resin layer. The atmosphere during this heat treatment is preferably an N2 atmosphere. In addition, in order to prevent the resin from scattering and to prevent the oxidation of various metal components, the oxygen concentration is preferably 100 ppm or less.
[0202] The plating layer may be disposed directly on the exposed portion of the internal electrode layer 30 of the laminate 10 without providing a base electrode layer. In this case, the first end face LS1 and the second end face LS2 of the laminate 10 are plated to form a plating layer on the exposed portion of the internal electrode layer 30. Either electrolytic plating or electroless plating may be used for the plating process. However, electroless plating has a disadvantage in that the process becomes complicated because pretreatment with a catalyst or the like is required to improve the plating deposition rate. Therefore, it is usually preferable to use electrolytic plating. As a plating method, it is preferable to use barrel plating. In addition, if necessary, an upper layer plating layer formed on the surface of the lower layer plating layer may be formed by the same method as the lower layer plating layer.
[0203] Through these manufacturing steps, the multilayer ceramic capacitor 1 is manufactured.
[0204] The configuration of the multilayer ceramic capacitor 1 is not limited to the configurations shown in Figures 1 to 4B. For example, the multilayer ceramic capacitor 1 may be a multilayer ceramic capacitor having a double structure, a triple structure, or a quadruple structure as shown in Figures 17A, 17B, and 17C.
[0205] The multilayer ceramic capacitor 1 shown in FIG. 17A is a multilayer ceramic capacitor 1 having a double structure, and includes, as the internal electrode layer 30, a floating internal electrode layer 35 that is not drawn to either the first end face LS1 or the second end face LS2, in addition to the first internal electrode layer 33 and the second internal electrode layer 34. The multilayer ceramic capacitor 1 shown in FIG. 17B is a multilayer ceramic capacitor 1 having a triple structure, including a first floating internal electrode layer 35A and a second floating internal electrode layer 35B as the floating internal electrode layer 35. The multilayer ceramic capacitor 1 shown in FIG. 17C is a multilayer ceramic capacitor 1 having a quadruple structure, including a first floating internal electrode layer 35A, a second floating internal electrode layer 35B, and a third floating internal electrode layer 35C as the floating internal electrode layer 35. In this way, by providing the floating internal electrode layer 35 as the internal electrode layer 30, the multilayer ceramic capacitor 1 has a structure in which the opposing electrode portion is divided into multiple parts. As a result, a plurality of capacitor components are formed between the opposing internal electrode layers 30, and these capacitor components are connected in series. This reduces the voltage applied to each capacitor component, thereby enabling the multilayer ceramic capacitor 1 to withstand high voltage. It goes without saying that the multilayer ceramic capacitor 1 of this embodiment may have a multi-row structure of four or more rows.
[0206] The multilayer ceramic capacitor 1 may be a two-terminal type having two external electrodes, or a multi-terminal type having many external electrodes.
[0207] In the above-described embodiment, a multilayer ceramic capacitor in which the dielectric layer 20 made of a dielectric ceramic is used as the ceramic layer is exemplified as the multilayer ceramic electronic component. However, the multilayer ceramic electronic component of the present disclosure is not limited thereto. For example, the ceramic electronic component of the present disclosure can be applied to various multilayer ceramic electronic components such as a piezoelectric component using a piezoelectric ceramic as the ceramic layer, and a thermistor using a semiconductor ceramic as the ceramic layer. Examples of the piezoelectric ceramic include PZT (lead zirconate titanate) ceramics, and examples of the semiconductor ceramic include spinel ceramics.
[0208] The multilayer ceramic electronic component of the present embodiment provides the following advantages.
[0209] (1) The multilayer ceramic electronic component 1 of the present embodiment includes a laminate 10 having a plurality of laminated ceramic layers 20 and a plurality of internal conductor layers 30 laminated on the ceramic layers 20, the laminate having a first main surface TS1 and a second main surface TS2 opposing each other in a height direction, a first side surface WS1 and a second side surface WS2 opposing each other in a width direction perpendicular to the height direction, and a first end surface LS1 and a second end surface LS2 opposing each other in a length direction perpendicular to the height direction and the width direction, and an external electrode 40 connected to the internal conductor layers 30, the internal conductor layers 30 having: There are a plurality of holes having different equivalent area diameters, the plurality of holes having a first hole with a ceramic pillar disposed therein connecting the ceramic layer 20 on one side of the internal conductor layer 30 to the ceramic layer 20 on the other side, and a second hole with no ceramic pillar disposed therein, and when the equivalent area diameter D90 is defined as the diameter at which the cumulative value of the cumulative distribution of the equivalent area diameters of the plurality of holes present in the internal conductor layer 30 is 90%, the abundance ratio of the first holes in a first population composed of holes having an equivalent area diameter equal to or larger than the equivalent area diameter D90 is 14% or more. This makes it possible to provide a multilayer ceramic electronic component capable of suppressing electric field concentration.
[0210] (2) In the monolithic ceramic electronic component 1 of this preferred embodiment, the abundance ratio of the first holes in the first population composed of holes whose equivalent area diameter is equal to or larger than the equivalent area diameter D90 is 29% or more, which makes it possible to further suppress electric field concentration.
[0211] (3) In the monolithic ceramic electronic component 1 of this preferred embodiment, the abundance ratio of the first holes in the first population formed by holes whose equivalent area diameter is equal to or larger than D90 is equal to or larger than 14% and equal to or smaller than 86%, which makes it possible to further suppress electric field concentration.
[0212] (4) In the monolithic ceramic electronic component 1 of this preferred embodiment, the abundance ratio of the first holes in the first population formed by holes whose equivalent area diameter is equal to or larger than D90 is equal to or larger than 29% and equal to or smaller than 86%, which makes it possible to further suppress electric field concentration.
[0213] (5) In the multilayer ceramic electronic component 1 of the present embodiment, the abundance ratio of the first holes in the first population of holes whose equivalent-area diameter is equal to or larger than the equivalent-area diameter D90 is higher than the abundance ratio of the first holes in the second population of holes whose equivalent-area diameter is smaller than the equivalent-area diameter D90. This makes it possible to effectively suppress electric field concentration.
[0214] (6) In the multilayer ceramic electronic component 1 of this embodiment, the coverage of the internal conductor layers 30 with respect to the ceramic layers 20 is 70% or more and 99% or less. This makes it possible to improve the reliability of the product while suppressing a decrease in capacitance.
[0215] (7) In the multilayer ceramic electronic component 1 of this embodiment, the coverage of the internal conductor layers 30 with respect to the ceramic layers 20 is 86% or more and 93% or less. This makes it possible to improve the reliability of the product while suppressing a decrease in capacitance.
[0216] (8) In the multilayer ceramic electronic component 1 of this preferred embodiment, the internal conductor layers 30 have a thickness of 0.2 μm or more and 2.0 μm or less. This makes it possible to employ a configuration that makes it easy to ensure capacitance while suppressing electric field concentration.
[0217] (9) In the multilayer ceramic electronic component 1 of this preferred embodiment, the internal conductor layers 30 have a thickness of 0.2 μm or more and 0.3 μm or less. This makes it possible to employ a configuration that makes it easy to ensure capacitance while suppressing electric field concentration.
[0218] (10) In the multilayer ceramic electronic component 1 of this preferred embodiment, the area-equivalent diameter D90 of the multiple holes present in the internal conductor layers 30 is 4.0 μm or less, which makes it possible to further suppress electric field concentration.
[0219] (11) In the multilayer ceramic electronic component 1 of this preferred embodiment, the area-equivalent diameter D90 of the multiple holes present in the internal conductor layers 30 is 1.9 μm or more and 4.0 μm or less, thereby making it possible to further suppress electric field concentration.
[0220] (12) In the multilayer ceramic electronic component 1 of this preferred embodiment, the thickness dimension of the internal conductor layers 30 is smaller than the area-equivalent diameter D90. This makes it possible to employ a configuration that makes it easy to ensure capacitance while suppressing electric field concentration.
[0221] (13) In the multilayer ceramic electronic component 1 of this embodiment, the thickness dimension of the internal conductor layers 30 is equal to or less than half the value of the area-equivalent diameter D90. This makes it possible to employ a configuration that makes it easy to ensure capacitance while suppressing electric field concentration.
[0222] (14) In the monolithic ceramic electronic component 1 of the present embodiment, the average circularity of the holes in the first population having an equivalent area diameter equal to or larger than D90 is 0.7 or less, thereby further suppressing electric field concentration.
[0223] (15) In the monolithic ceramic electronic component 1 of the present embodiment, the average circularity of the holes in the first population having an equivalent area diameter equal to or larger than D90 is 0.46 or less, thereby further suppressing electric field concentration.
[0224] (16) In the multilayer ceramic electronic component 1 of the present embodiment, the average circularity of the holes in the first population having an equivalent area diameter D90 or more is 0.2 or more and 0.7 or less, thereby further suppressing electric field concentration.
[0225] (17) In the multilayer ceramic electronic component 1 of the present embodiment, the average circularity of the holes in the first population having an equivalent area diameter D90 or more is 0.2 or more and 0.46 or less, thereby further suppressing electric field concentration.
[0226] (18) In the multilayer ceramic electronic component 1 of the present embodiment, when the area-equivalent diameter D99 is defined as the diameter at which the cumulative value of the cumulative distribution of the area-equivalent diameters of the multiple holes present in the internal conductor layer 30 is 99%, the area-equivalent diameter D99 of the multiple holes present in the internal conductor layer 30 is 8.0 μm or less. This makes it possible to further suppress electric field concentration.
[0227] (19) In the multilayer ceramic electronic component 1 of this preferred embodiment, the area-equivalent diameter D99 of the multiple holes present in the internal conductor layers 30 is 3.2 μm or less. This makes it possible to further suppress electric field concentration.
[0228] (20) In the multilayer ceramic electronic component 1 of this preferred embodiment, the area-equivalent diameter D99 of the multiple holes present in the internal conductor layers 30 is not less than 2.0 μm and not more than 8.0 μm, thereby making it possible to further suppress electric field concentration.
[0229] (21) In the multilayer ceramic electronic component 1 of this preferred embodiment, the area-equivalent diameter D99 of the multiple holes present in the internal conductor layers 30 is not less than 2.0 μm and not more than 4.0 μm. This makes it possible to further suppress electric field concentration.
[0230] (22) The external electrode 40 of the multilayer ceramic electronic component 1 of this embodiment includes a first external electrode 40A arranged on the first end face LS1 side and a second external electrode 40B arranged on the second end face LS2 side. The multiple internal conductor layers 30 include a multiple number of first internal conductor layers 31 electrically connected to the first external electrode 40A and a multiple number of second internal conductor layers 32 electrically connected to the second external electrode 40B. The first internal conductor layer 31 has a first side WE1 on the first side face WS1 side and a second side WE2 on the second side face WS2 side. The second internal conductor layer 32 has a third side WE3 on the first side face WS1 side and a fourth side WE4 on the second side face WS2 side. The region from the first side WE1 to a position 50 μm away is defined as the first region A1, the region from a position 10 μm away from the second side WE2 to a position 50 μm away from the second side WE2 is defined as the second region A2, the region in the second internal conductor layer 32 from a position 10 μm away from the third side WE3 to a position 50 μm away from the third side WE3 is defined as the third region A3, and the region from a position 10 μm away from the fourth side WE4 to a position 50 μm away from the fourth side WE4 is defined as the fourth region A4, and the collection of holes present in the first region A1, the second region A2, the third region A3, and the fourth region A4 is defined as a hole population, the area-equivalent diameter D90 is the area-equivalent diameter at which the cumulative value in the cumulative distribution of the area-equivalent diameters of the holes in the hole population is 90%. This makes it possible to suppress electric field concentration and provide a highly reliable multilayer ceramic electronic component.
[0231] (23) The multilayer ceramic electronic component 1 of the present embodiment includes a laminate 10 having a plurality of laminated ceramic layers 20 and a plurality of internal conductor layers 30 laminated on the ceramic layers 20, the laminate having a first main surface TS1 and a second main surface TS2 opposing each other in a height direction, a first side surface WS1 and a second side surface WS2 opposing each other in a width direction perpendicular to the height direction, and a first end surface LS1 and a second end surface LS2 opposing each other in a length direction perpendicular to the height direction and the width direction, and an external electrode 40 connected to the internal conductor layers 30, the internal conductor layers 30 having a shape and an area equivalent diameter The internal conductor layer 30 has a plurality of holes having different sizes, the plurality of holes including a first hole having a ceramic pillar disposed therein that connects the ceramic layer 20 on one side of the internal conductor layer 30 to the ceramic layer 20 on the other side thereof, and a second hole having no ceramic pillar disposed therein. The external electrode 40 has a first external electrode 40A disposed on the first end face LS1 side and a second external electrode 40B disposed on the second end face LS2 side. The plurality of internal conductor layers 30 include a plurality of first internal conductor layers 31 electrically connected to the first external electrode 40A and a plurality of second external electrodes 40B electrically connected to the second external electrode 40B. The first internal conductor layer 31 has a first side WE1 on the first side surface WS1 side and a second side WE2 on the second side surface WS2 side, and the second internal conductor layer 32 has a third side WE3 on the first side surface WS1 side and a fourth side WE4 on the second side surface WS2 side. A region of the first internal conductor layer 31 from a position 10 μm away from the first side WE1 to a position 50 μm away from the first side WE1 is defined as a first region A1, and a region from a position 10 μm away from the second side WE2 to a position 50 μm away from the second side WE2 is defined as a second region A2. 2, a region in the second internal conductor layer 32 from a position 10 μm away from the third side WE3 to a position 50 μm away from the third side WE3 is defined as a third region A3, a region from a position 10 μm away from the fourth side WE4 to a position 50 μm away from the fourth side WE4 is defined as a fourth region A4, a collection of holes present in the first region A1, the second region A2, the third region A3, and the fourth region A4 is defined as a hole population, and an area-equivalent diameter D90 is defined as a diameter at which the cumulative value in the cumulative distribution of the area-equivalent diameters of holes in the hole population is 90%. In the hole population,The ratio of the first holes in the first population constituted by holes having an equivalent area diameter D90 or more is 17% or more. This makes it possible to suppress electric field concentration and provide a highly reliable multilayer ceramic electronic component.
[0232] The present invention is not limited to the configurations of the above-mentioned embodiments, and can be appropriately modified and applied within the scope of the present invention. Note that the present invention also includes a combination of two or more of the individual desirable configurations described in the above-mentioned embodiments. [Explanation of symbols]
[0233] 1. Multilayer ceramic capacitors (multilayer ceramic electronic components) 10 Laminate LS1 First end face LS2 Second end face WS1 First Aspect WS2 The Second Side TS1 First main surface TS2 Second main surface 20 Dielectric layer (ceramic layer) 30 Internal electrode layer (internal conductor layer) 31 First internal electrode layer (first internal conductor layer) 32 Second internal electrode layer (second internal conductor layer) H hole WE1 First Edge WE2 Second Side WE3 The Third Side WE4 The Fourth Side A1 First Area A2 Second Area A3 The third area A4 The fourth area 40 External electrode 40A First outer electrode 40B Second external electrode L Length direction W Width direction T Height direction
Claims
1. a laminate having a plurality of laminated ceramic layers and a plurality of internal conductor layers laminated on the ceramic layers, the laminate having a first main surface and a second main surface opposing each other in a height direction, a first side surface and a second side surface opposing each other in a width direction perpendicular to the height direction, and a first end surface and a second end surface opposing each other in a length direction perpendicular to the height direction and the width direction; an external electrode connected to the internal conductor layer; The internal conductor layer has a plurality of holes having different equivalent area diameters, the plurality of holes include a first hole having a ceramic pillar disposed therein, the ceramic pillar connecting a ceramic layer on one side of the internal conductor layer to a ceramic layer on the other side of the internal conductor layer, and a second hole having no ceramic pillar disposed therein; When the area-equivalent diameter D90 is defined as the area-equivalent diameter at which the cumulative value in the cumulative distribution of the area-equivalent diameters of the plurality of holes present in the internal conductor layer is 90%, an abundance ratio of the first holes in a first population constituted by holes having an equivalent area diameter D90 or more is 14% or more; When the area-equivalent diameter D99 is defined as the area-equivalent diameter at which the cumulative value in the cumulative distribution of the area-equivalent diameters of the plurality of holes present in the internal conductor layer is 99%, The area equivalent diameter D99 is 8.0 μm or less, The thickness of the internal conductor layer is 0.2 μm or more and 0.8 μm or less, A multilayer ceramic electronic component, wherein the coverage of the internal conductor layers is 70% or more and 99% or less.
2. 2. The monolithic ceramic electronic component according to claim 1, wherein an abundance ratio of said first holes in a first population of holes having an equivalent area diameter of said equivalent area diameter D90 or more is 29% or more.
3. 2. The multilayer ceramic electronic component according to claim 1, wherein an abundance ratio of said first holes in a first population of holes having an equivalent area diameter of said equivalent area diameter D90 or more is 14% or more and 86% or less.
4. 2. The multilayer ceramic electronic component according to claim 1, wherein an abundance ratio of the first holes in a first population constituted by holes having an equivalent area diameter of D90 or more is 29% or more and 86% or less.
5. The multilayer ceramic electronic component according to any one of claims 1 to 4, wherein an abundance ratio of the first holes in a first population composed of holes whose equivalent-area diameter is equal to or greater than the equivalent-area diameter D90 is higher than an abundance ratio of the first holes in a second population composed of holes whose equivalent-area diameter is smaller than the equivalent-area diameter D90.
6. 6. The multilayer ceramic electronic component according to claim 1, wherein a coverage of said internal conductor layers with respect to said ceramic layers is 86% or more and 93% or less.
7. 7. The multilayer ceramic electronic component according to claim 1, wherein the internal conductor layers have a thickness of 0.2 μm or more and 0.3 μm or less.
8. 8. The multilayer ceramic electronic component according to claim 1, wherein the area equivalent diameter D90 is 4.0 μm or less.
9. 8. The multilayer ceramic electronic component according to claim 1, wherein the area equivalent diameter D90 is 1.9 μm or more and 4.0 μm or less.
10. 10. The multilayer ceramic electronic component according to claim 1, wherein a thickness dimension of said internal conductor layers is smaller than said area equivalent diameter D90.
11. 10. The multilayer ceramic electronic component according to claim 1, wherein a thickness dimension of said internal conductor layers is equal to or less than half the value of said area equivalent diameter D90.
12. 12. The multilayer ceramic electronic component according to claim 1, wherein an average value of the circularity of the holes in a first population constituted by holes whose equivalent area diameter is equal to or larger than the equivalent area diameter D90 is 0.7 or less.
13. 12. The multilayer ceramic electronic component according to claim 1, wherein an average value of the circularity of the plurality of holes in a first population constituted by holes whose equivalent area diameter is equal to or larger than the equivalent area diameter D90 is 0.46 or less.
14. The laminated ceramic electronic component according to any one of claims 1 to 11, wherein an average circularity of the plurality of holes in a first population constituted by holes whose equivalent area diameter is equal to or greater than the equivalent area diameter D90 is 0.2 or more and 0.7 or less.
15. The laminated ceramic electronic component according to any one of claims 1 to 11, wherein an average circularity of the plurality of holes in a first population constituted by holes whose equivalent area diameter is equal to or greater than the equivalent area diameter D90 is 0.2 or more and 0.46 or less.
Citation Information
Patent Citations
Metal film retainer, ceramic green sheet feeder, and ceramic laminate for electronic parts
JP1994349674A
Stacked electronic component and manufacturing method of stack electronic component
JP2002164248A
Multilayer chip varistor
JP2006269985A
Multilayer ceramic capacitor
JP2018046086A
Capacitor
JP2019114753A