Surface treatment method, processing method, storage method for silicon blocks, manufacturing method for silicon wafers, and silicon ingots

By forming irregularities on the silicon ingot surface through physical impact treatment, Cu is gettered and removed, addressing the inefficiencies and defects in existing methods, resulting in high-quality silicon wafers with reduced Cu concentration and stable long-term storage.

JP7586012B2Active Publication Date: 2024-11-19SHIN ETSU HANDOTAI CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021118563
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-07-19
Publication Date
2024-11-19
Estimated Expiration
2041-07-19

AI Technical Summary

Technical Problem

Existing methods for reducing Cu concentration in silicon wafers are costly, complex, and impose restrictions on production management, leading to potential defects like OSF in silicon wafers due to long-term storage.

Method used

Applying physical impact treatment to form irregularities with an Rz of 50 μm or more on the silicon ingot surface before cylindrical grinding, gettering Cu in a strained layer and removing it through grinding, followed by storing and processing the ingot into wafers.

Benefits of technology

Reduces Cu concentration uniformly and stably, suppressing OSF changes over time in silicon wafers even after long-term storage, ensuring high-quality wafer production without increased costs or production restrictions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586012000001
    Figure 0007586012000001
Patent Text Reader

Abstract

To provide a treatment method for a silicon ingot by which Cu concentration in the ingot can be reduced with ease and at low cost and that can produce a silicon ingot with suppressed occurrence of secular change in OSF (Oxidation-Induced Stacking Fault) in manufactured silicon wafers even when the ingot is stored for a long time before being processed into wafers, and to provide a silicon ingot with reduced Cu inside that can suppress occurrence of secular change in OSF in manufactured silicon wafers even when the ingot is stored for a long time.SOLUTION: In a surface treatment method for a silicon ingot, a surface of a silicon ingot before cylindrical grinding is subjected to physical shock treatment to form unevenness whose Rz is equal to or more than 50 μm on the surface of the silicon ingot.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a surface treatment method, a processing method, a silicon block storage method, a silicon wafer manufacturing method, and a silicon ingot. [Background technology]

[0002] It is known that Cu, a metal impurity, induces various defects in silicon wafers. For example, Patent Documents 1 and 2 describe the change over time of OSF (Oxidation-Induced Stacking Fault). As a countermeasure, Patent Document 1 describes storing silicon single crystal ingots or blocks at low temperatures or cutting them early. Patent Document 2 describes specifying the Al and Cu concentrations of a quartz glass crucible used in manufacturing silicon single crystals, or doping Al when manufacturing silicon single crystals. In addition, Patent Document 3 describes that "unevenly distributed LPD" is detected when the boron concentration and oxygen donor concentration in a silicon wafer are almost the same, and therefore, as a countermeasure, cutting the wafer within 50 days or performing heat treatment at 300°C or higher when cutting the wafer after more than 50 days. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 5-58800 [Patent Document 2] Japanese Patent Application Publication No. 8-73293 [Patent Document 3] JP 2017-200878 A [Patent Document 4] Japanese Patent Application Publication No. 54-5378 [Non-patent literature]

[0004] [Non-Patent Document 1] "Investigation of Cu and Ni diffusion amount into Si substrate", Sales and Technology Department, DISCO Technical Review Nov. 2018 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the low-temperature storage method described in Patent Document 1 has the problem of high costs, and the method of limiting the number of days for cutting into wafers requires production management with restrictions on block inventory, making efficient manufacturing difficult. Also, the method of changing the silicon single crystal manufacturing conditions (presence or absence of Al doping) by changing the Al concentration or Cu concentration of the quartz glass crucible described in Patent Document 2, and the method of changing the wafer manufacturing process (presence or absence of 300°C heat treatment) depending on the number of days until wafer cutting as described in Patent Document 3 require complicated process management and carry the risk of errors.

[0006] In addition, Patent Document 4 only describes impurities introduced during crystal growth, so it is unclear what kind of impurities are intended, but as a countermeasure against impurities that promote the generation of stacking faults, a method is described in which lattice distortion is applied to a silicon single crystal ingot, followed by annealing and etching the surface layer to remove the lattice distortion and silicon fracture layer. As the method of introducing lattice distortion, it is described that "the ingot is ground to form its outer shape and introduce lattice distortion", so in short, lattice distortion is introduced by cylindrical grinding. However, this method does not sufficiently remove impurities, so new methods such as Patent Documents 1 to 3 have been proposed.

[0007] The present invention has been made to solve the above problems, and has an object to provide a method for treating a silicon ingot that can reduce the Cu concentration inside the ingot simply and at low cost, and that can produce a silicon ingot in which the occurrence of change over time in OSF in the silicon wafers to be produced is suppressed even when a block cut from the ingot is stored for a long period of time before being processed into wafers, and a silicon ingot in which the Cu concentration inside the ingot is reduced, and the occurrence of change over time in OSF in the silicon wafers to be produced is suppressed even when stored for a long period of time. [Means for solving the problem]

[0008] The present invention has been made to achieve the above-mentioned object, and provides a surface treatment method for a silicon ingot, which comprises subjecting the surface of a silicon ingot before cylindrical grinding to a physical impact treatment, thereby forming irregularities with Rz of 50 μm or more on the surface of the silicon ingot.

[0009] According to such a method for surface treatment of a silicon ingot, the Cu concentration inside the ingot can be reduced easily and at low cost, and it is possible to obtain a silicon ingot in which the occurrence of change over time in OSF in the silicon wafers produced therefrom is suppressed even if a block cut from the ingot is stored for a long period of time.

[0010] In this case, the physical impact treatment may be a blasting treatment as a surface treatment method for a silicon ingot.

[0011] This makes it possible to form irregularities on the ingot surface extremely easily, and to reduce the Cu concentration inside the ingot more uniformly and stably throughout the entire ingot.

[0012] In this case, the silicon ingot can be manufactured by the Czochralski method (CZ method) or the Floating Zone Melting method (FZ method), and the physical impact treatment can be performed while the silicon ingot is held by a seed crystal.

[0013] When the ingot is held by the seed crystal, the ingot can be easily rotated, so that unevenness can be formed evenly over the entire outer surface of the ingot more easily and stably to impart distortion.

[0014] The present invention also provides a method for processing a silicon ingot, comprising cylindrical grinding the silicon ingot that has been treated by the above-mentioned method for surface treatment of a silicon ingot.

[0015] This makes it possible to remove Cu gettered to the strained layer on the surface of the silicon ingot outside the ingot, thereby obtaining an ingot with a reduced Cu concentration.

[0016] The present invention also provides a method for storing silicon blocks, which comprises cutting the silicon ingot into blocks of a predetermined length and storing the blocks after cylindrical grinding using the silicon ingot processing method.

[0017] With this storage method, Cu gettered to the strained layer is removed, and therefore it is possible to prevent Cu from diffusing into the block during storage.

[0018] The present invention also provides a method for producing silicon wafers, comprising slicing the silicon block stored by the above-described method for storing a silicon block to produce silicon wafers.

[0019] This makes it possible to obtain a silicon wafer with a reduced Cu concentration.

[0020] The present invention also provides a silicon ingot, wherein the entire surface of the body portion has been subjected to a physical shock treatment, the surface having irregularities of Rz of 50 μm or more.

[0021] This reduces the Cu concentration inside the ingot, suppresses the occurrence of changes in OSF over time in the silicon wafers to be manufactured even during long-term storage, and results in a silicon ingot that does not deteriorate in quality for the silicon wafers to be manufactured.

[0022] In this case, the silicon ingot may have a blasted surface as the physical shock treatment surface.

[0023] This results in a more uniform and stable reduction in the Cu concentration inside the ingot throughout the entire ingot. Effect of the Invention

[0024] As described above, according to the surface treatment method of the silicon ingot of the present invention, the Cu concentration inside the ingot can be easily reduced. In addition, even if the block cut from the ingot is stored for a long period of time before being processed into wafers, the occurrence of change over time in the OSF in the silicon wafer to be manufactured is suppressed, and it is possible to obtain a silicon ingot that does not deteriorate in quality. According to the silicon ingot of the present invention, the Cu concentration inside the ingot is reduced, and even if the block cut from the silicon ingot is stored for a long period of time, the occurrence of change over time in the OSF in the silicon wafer to be manufactured is suppressed, and the quality of the silicon wafer to be manufactured does not deteriorate. [Brief description of the drawings]

[0025] [Figure 1] 1 shows an example of a silicon ingot according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The present invention will be described in detail below, but the present invention is not limited thereto.

[0027] As described above, there has been a need to provide a silicon ingot in which change over time in OSF is suppressed even when a block cut from the ingot is stored for a long period of time before being processed into wafers, and a method for treating a silicon ingot that can reduce the Cu concentration inside the ingot simply and at low cost to obtain a silicon ingot in which change over time in OSF is suppressed in silicon wafers produced from the silicon ingot even when the block cut from the ingot is stored for a long period of time before being processed into wafers, and a silicon ingot in which the Cu concentration inside the ingot is reduced and change over time in OSF is suppressed in silicon wafers produced from the silicon ingot even when the block cut from the silicon ingot is stored for a long period of time.

[0028] The inventors have intensively studied measures to solve the above problems, and have come up with the idea of ​​a method for easily processing silicon wafers in a lump by processing them in the form of an ingot rather than a wafer, by applying distortion to the surface of the ingot before cylindrical grinding, so that Cu is gettered in the distortion layer, and then removing Cu from the silicon ingot by cylindrical grinding. With such a method, there is no significant increase in cost, such as low-temperature storage, and no need for a limit on the number of days until slicing, so there are no constraints on production management, and there is no need to change the manufacturing conditions according to the quality of the quartz crucible used or the number of days until the wafer is cut out. It has been found that a silicon wafer in which crystal defects caused by Cu are suppressed can be simply and easily manufactured without any constraints on production management in this respect.

[0029] That is, the surface treatment method of a silicon ingot, which performs physical shock treatment on the surface of the silicon ingot before cylindrical grinding to form irregularities of Rz of 50 μm or more on the surface of the silicon ingot, makes it possible to reduce the Cu concentration inside the ingot easily and at low cost. In addition, it was found that even if a block cut from the ingot is stored for a long period of time before being processed into wafers, the occurrence of change over time in OSF in the silicon wafer to be manufactured can be suppressed, and it is possible to obtain a silicon ingot with no deterioration in the quality of the silicon wafer to be manufactured, and the present invention has been completed.

[0030] The present inventors have also discovered that a silicon ingot in which the entire surface of the straight body portion has been subjected to a physical shock treatment having unevenness with Rz of 50 μm or more reduces the Cu concentration inside the ingot, and even if a block cut from the silicon ingot is stored for a long period of time, the occurrence of change over time in OSF in the silicon wafers produced therefrom is suppressed, and the quality of the silicon wafers produced does not deteriorate, thereby completing the present invention.

[0031] The present invention will be described in detail below.

[0032] (Silicon ingot) First, a silicon ingot to be subjected to the silicon ingot surface treatment method according to the present invention will be described. The silicon ingot to be surface-treated will eventually be processed into a silicon wafer through processing steps such as slicing, and the manufacturing method is not particularly limited. The silicon ingot surface treatment method according to the present invention can be applied regardless of the manufacturing method of the ingot (crystal), such as the CZ method, the MCZ method, or the FZ method.

[0033] (Silicon ingot surface treatment method) Next, the method for surface treatment of silicon ingot according to the present invention will be described. The surface of a prepared silicon ingot is subjected to physical shock treatment before cylindrical grinding, and unevenness with Rz (maximum height) of 50 μm or more is formed on the surface of the silicon ingot to form a physical shock treatment surface. By forming such unevenness, a distorted layer is formed near the ingot surface before cylindrical grinding, and Cu in the ingot can be gettered into this distorted layer.

[0034] FIG. 1 shows an example of a silicon ingot according to the present invention. In the silicon ingot 10 according to the present invention, the entire surface of the straight body portion 1 is a physically impact treated surface having unevenness with Rz (maximum height) of 50 μm or more. Here, the physically impact treated surface refers to a surface in a state where it has been treated by physical impact. In a silicon ingot in which the entire surface of the straight body portion 1 is a physically impact treated surface 2 having unevenness with Rz of 50 μm or more, Cu is gettered in a strain layer near the physically impact treated surface, so that the Cu concentration inside the silicon ingot except for the vicinity of the physically impact treated surface is extremely low. A block cut from such a silicon ingot has excellent long-term storage properties, and even if it is sliced ​​into silicon wafers after long-term storage, various defects caused by Cu, particularly OSF, are not formed.

[0035] On the other hand, even if the entire surface of the body portion 1 is a surface that has been subjected to physical shock treatment, if the surface has irregularities with Rz of less than 50 μm, the long-term storage property is particularly poor. This is because the effect of reducing the Cu concentration inside the silicon ingot is insufficient, and as the storage period becomes longer, problems arise over time, such as the occurrence of OSF in silicon wafers produced from the ingot.

[0036] The physical shock treatment surface may be any surface, but is preferably a blasted surface formed by blasting. The blasted surface can be easily formed over a wide area, and has a strained layer capable of stably gettering Cu.

[0037] The unevenness (roughness) of the surface subjected to physical shock treatment is not particularly limited as long as Rz is 50 μm or more, but it is preferably 75 μm or more, more preferably 100 μm or more. The upper limit is not particularly limited, but it can be, for example, Rz is 300 μm or less, more preferably 200 μm or less.

[0038] The surface to be treated by physical shock may be any surface. It may be a surface in an as-grown state immediately after the ingot is grown, or a surface after other surface treatment or surface processing has been performed. In addition, if the silicon ingot and the seed crystal are still connected, it is preferable because the physical shock treatment can be performed at a high temperature before the ingot is cooled, but the silicon ingot 10 according to the present invention may have the cone portion 3 and the tail portion 4 removed. In the case of the silicon ingot 10 having the cone portion 3 and the tail portion 4, not only the straight body portion 1 but also the surfaces of the cone portion 3 and the tail portion 4 may be treated by physical shock.

[0039] For example, it is known that Cu applied to one side of a silicon substrate (725 μm thick) is diffused to the opposite side by heat treatment at 350°C for 1 h (Non-Patent Document 1). Cu, which is so easily diffused, is gettered sufficiently into the strained layer even at room temperature if the ingot has a surface that has been subjected to the above-mentioned physical shock treatment.

[0040] In this case, examples of the physical impact treatment include blasting and barrel treatment, with blasting being particularly preferred as it is simpler. The blasting can more easily and stably form irregularities over a wide range of the ingot surface. Examples of the blasting include shot blasting and grit blasting.

[0041] In addition, when a silicon ingot is produced by the CZ method, the MCZ method, or the FZ method, it is preferable to perform the physical shock treatment while the silicon ingot is held by a seed crystal. If the seed crystal and the ingot are connected and the ingot is held by the seed crystal, the ingot can be easily rotated, so that it is easier to apply a distortion evenly to the entire surface of the ingot.

[0042] (Silicon ingot processing method) The method for processing a silicon ingot according to the present invention is a method for performing cylindrical grinding on a silicon ingot that has been treated by the above-mentioned method for treating the surface of a silicon ingot. By cylindrical grinding, Cu gettered into the strained layer is removed from the ingot. The silicon ingot that has been subjected to cylindrical grinding has an extremely low Cu concentration. At this time, the time from the physical shock treatment to the cylindrical grinding can be appropriately determined in consideration of the diffusion of Cu from the inside of the ingot to the strained layer and the past record of OSF generation.

[0043] (How to store blocks cut from ingots) The blocks cut from the ingots can be stored in any state after the physical shock treatment. They can be stored either before or after cylindrical grinding, but it is particularly preferable to store them after cylindrical grinding. After cylindrical grinding, the Cu gettered in the strained layer is removed, so it is possible to prevent Cu from diffusing into the blocks during storage.

[0044] (Silicon wafer manufacturing method) The method for producing a silicon wafer according to the present invention is a method for producing a silicon wafer by slicing a block stored by the above-mentioned method for storing a block obtained by cutting a silicon ingot. After subjecting the surface of the silicon ingot to physical shock treatment to form irregularities of a predetermined size to give distortion and removing Cu from the ingot by cylindrical grinding, a normal silicon wafer production process including a slicing step is performed to produce a silicon wafer. For example, after the silicon ingot is separated from the seed crystal and cooled, the above-mentioned cylindrical grinding, removal of the cone and tail parts, block cutting, slicing of the straight body part, lapping of the sliced ​​wafer, chamfering, etching, polishing, etc. are performed. The concentration of Cu contained in the silicon wafer produced in this way is extremely low compared to the conventional method, so that the formation of various defects caused by Cu is suppressed.

[0045] In this way, if the block is cut from a silicon ingot that has been subjected to the surface treatment according to the present invention, problems such as the occurrence of OSF can be suppressed even if the block is stored for a long period of time before slicing. Moreover, the only newly added process is a process of applying distortion to the surface of the ingot by physical impact treatment such as sandblasting, and it is possible to manufacture silicon wafers with a reduced Cu concentration by a simple method with only a slight increase in cost. EXAMPLES

[0046] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto.

[0047] (Example) Using the MCZ method, 130 silicon single crystal ingots with a diameter of 300 mm and a length of 150 cm were pulled. The Al concentration in the depth direction from the inner surface of the quartz crucible used in this experiment was less than 40 ppmw on average within a range of 30 μm from the inner surface, and the silicon single crystal ingots were not doped with Al during production.

[0048] When the silicon single crystal ingot was removed from the pulling machine, the ingot was held by the seed crystal and rotated at 6 rpm while sandblasting using a sandblasting device to form irregularities on the entire outer peripheral surface of the ingot. The abrasive used for sandblasting was glass beads with a grit size of 120. The air pressure for sandblasting was 0.5 to 0.7 MPa, the spray distance was 30 to 50 cm, the spray angle was 90±30°, and the treatment time for the entire ingot was 10 minutes.

[0049] The silicon single crystal ingot was then separated from the seed crystal, cooled, and then cylindrically ground and cut into blocks. Before cylindrical grinding, the roughness of the ingot surface was measured at 10 points using a surface roughness measuring instrument (Mitutoyo, Surftest SJ-210), and the Rz was 55 to 65 μm.

[0050] The storage period of the blocks was set at one-month intervals, from 0 months (3 days left standing) to 12 months, and 10 silicon single crystal ingots were sliced, lapped, chamfered, etched, polished, etc., for each month to produce silicon wafers. Every 50th silicon wafer was taken out and heat-treated at 1150°C / 100min. to check for OSF occurrence. Not a single silicon wafer had OSF occurrence, regardless of storage period.

[0051] Comparative Example 1 Surface treatment and processing of silicon single crystal ingots, manufacture and evaluation of silicon wafers were performed in the same manner as in the example, except that the size of the glass beads of the abrasive used in sandblasting was 150. The roughness of the silicon single crystal ingot surface before cylindrical grinding was 35 to 45 μm in Rz. No OSF occurred when the block storage period was 0 months (3 days) to 3 months, but OSF occurred in 80% or more of the silicon wafers after 4 months.

[0052] Comparative Example 2 Using the MCZ method, 130 silicon single crystal ingots with a diameter of 300 mm and a length of 150 cm were pulled. The Al concentration in the depth direction from the inner surface of the quartz crucible used in this experiment was less than 40 ppmw on average within a range of 30 μm from the inner surface, and no Al was doped during the production of the silicon single crystals.

[0053] The silicon single crystal ingot was separated from the seed crystal, cooled, and then cylindrically ground and cut into blocks. Before cylindrical grinding, the roughness of the ingot surface was measured at 10 points using a surface roughness measuring instrument (Mitutoyo Surftest SJ-210), and the Rz was 5 to 15 μm.

[0054] The storage period of the blocks was set at one-month intervals, from 0 months (3 days left standing) to 12 months, and 10 silicon single crystal ingots were sliced, lapped, chamfered, etched, polished, etc., for each month to produce silicon wafers. Every 50th silicon wafer was sampled and heat-treated at 1150°C / 100min to check for OSF occurrence. No OSF occurred after 0 and 1 month storage, but OSF occurred in more than 80% of the silicon wafers after 2 months.

[0055] As described above, according to the examples of the present invention, the Cu concentration in a silicon ingot can be reduced simply and at low cost, and the long-term storage stability of a block cut from the ingot can be improved.

[0056] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]

[0057] 1...straight body portion, 2...physical impact treatment surface, 3...cone portion, 4...tail portion, 10...Silicon ingot.

Claims

1. A surface treatment method for a silicon ingot, comprising: subjecting a surface of the silicon ingot before cylindrical grinding to a physical impact treatment, thereby forming irregularities on the surface of the silicon ingot having an Rz of 50 μm or more and 300 μm or less.

2. 2. The method for treating a surface of a silicon ingot according to claim 1, wherein the physical impact treatment is a blast treatment.

3. 3. The method for treating a surface of a silicon ingot according to claim 1, wherein the silicon ingot is produced by a CZ method or an FZ method, and the physical impact treatment is performed in a state where the silicon ingot is held by a seed crystal.

4. A method for processing a silicon ingot, comprising: subjecting the silicon ingot treated by the method for surface treatment of a silicon ingot according to any one of claims 1 to 3 to cylindrical grinding.

5. 5. A method for storing silicon blocks, comprising the steps of: cutting the silicon ingot into blocks of a predetermined length after cylindrical grinding using the method for processing a silicon ingot according to claim 4; and storing the blocks.

6. 6. A method for producing silicon wafers, comprising slicing the silicon block stored by the method for storing silicon blocks according to claim 5 to produce silicon wafers.

7. A silicon ingot, A silicon ingot, wherein the entire surface of a straight body portion is a physically impact treated surface having an unevenness of Rz of 50 μm or more and 300 μm or less.

8. 8. The silicon ingot according to claim 7, wherein the physical impact treated surface is a blasted surface.

Citation Information

Patent Citations

  • Method of processing silicon monocrystal

    JP1979005378A

  • Treatment of silicon single crystal

    JP1993058800A

  • Method for processing ingot of semiconductor

    JP1994166600A

  • Production of silicon single crystal and quartz glass crucible used therefor

    JP1996073293A

  • Method of manufacturing semiconductor wafer and semiconductor wafer

    JP2013074066A