Molded product of carbon fiber reinforced composite material and its manufacturing method

By controlling surface roughness and energy, and using plasma treatment, carbon fiber composite materials achieve strong and durable adhesion with metals, addressing bonding challenges and reducing processing time and costs.

JP7586071B2Active Publication Date: 2024-11-19TORAY INDUSTRIES INC
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2021509490
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-28
Filing Date
2020-03-25
Publication Date
2024-11-19
Estimated Expiration
2040-03-25

AI Technical Summary

Technical Problem

Carbon fiber composite materials face challenges in bonding with adhesives and metals due to variations in adhesive types and metal materials, leading to reduced bonding strength over time and requiring time-consuming pre-treatments like blasting to remove mold release agents, which increases processing time and cost.

Method used

The solution involves controlling the surface roughness, surface energy, and chemical composition of carbon fiber composite materials to enhance bonding strength, using a specific range of surface roughness (0.01 μm to 2 μm), surface free energy (30 to 80 mJ/m²), and controlled plasma treatment to introduce functional groups, thereby improving adhesion without the need for pre-treatments like blasting.

Benefits of technology

The method ensures strong and durable adhesion with metals, maintaining bonding strength over time and reducing processing time and costs by eliminating the need for pre-treatments, suitable for structural applications in automobiles, aircraft, and buildings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586071000004
    Figure 0007586071000004
  • Figure 0007586071000001
    Figure 0007586071000001
  • Figure 0007586071000002
    Figure 0007586071000002
Patent Text Reader

Abstract

The present invention addresses the problem of providing a molded article of a carbon-fiber-reinforced composite material that makes it possible to achieve favorable adhesion, regardless of the adhesive or metal used in combination therewith, and that also makes it possible to maintain adhesive force, even after a long period of time has passed after adhesion. A molded article of a carbon-fiber-reinforced composite material that comprises at least carbon fibers and a resin composition. The molded article of a carbon-fiber-reinforced composite material is characterized in that the surface roughness Ra thereof is 0.01-2 μm and in that the tensile shear adhesive strength (F0) thereof when a metal has been adhered to the surface thereof via an adhesive layer that contains an epoxy compound and is 0.1-3 mm thick is 10-40 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a molded article of a carbon fiber reinforced composite material that exhibits high tensile shear bond strength when adhesively bonded to a metal material. [Background technology]

[0002] There are several methods for joining molded products to other molded products made of the same or different materials, including mechanical fastening with bolts or screws, joining using adhesives, and joining by temporarily softening the surface of the material and then bringing it into contact with the other material before it hardens. Examples of joining using adhesives are shown below.

[0003] In the case of bonding between a carbon fiber-reinforced thermosetting resin and a thermoplastic resin, the absolute value of the difference between the total surface free energy of the thermoplastic resin composition and the total surface free energy of the thermosetting resin composition is 10 mJ / m 2 It is known that by doing so, the two can be well adhered to each other (Patent Document 1).

[0004] When bonding crystalline thermoplastic resins together via an adhesive layer, it is known that good adhesion can be achieved by controlling the rate of change in surface free energy of the materials before and after dry processing (Patent Document 2).

[0005] When joining aluminum and thermoplastic resin via an adhesive layer made of thermosetting resin, it is known that good adhesion can be achieved by controlling the relationship between the surface free energy of the primer coating formed on the aluminum surface and the surface free energy of the thermosetting resin layer, and the surface roughness of the primer coating on the aluminum surface (Patent Document 3). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2004-269878 A [Patent Document 2] JP 2017-128683 A [Patent Document 3] JP 2008-132650 A Summary of the Invention [Problem to be solved by the invention]

[0007] When joining a molded carbon fiber composite material product to a metal via an adhesive, the design and combination of materials for the molded carbon fiber composite material product, adhesive, and metal have been selected based on the relative relationships between their properties. Therefore, even when a carbon fiber composite material with excellent properties has been developed, it has sometimes been difficult to use a molded carbon fiber composite material product due to the properties of other adhesives used in combination or the metal materials to be joined.

[0008] Furthermore, when carbon fiber composite materials are molded into molded products, in order to make it easier to remove the molded product from the mold, a release agent may be applied to the mold before the molding operation, or the material to be molded may be sandwiched between release films. In such cases, some of the components of the release agent or release film may adhere to the surface of the molded product removed from the mold. This adhesion may hinder bonding with an adhesive in subsequent steps or processing when the molded product is used, thereby reducing the bonding strength.

[0009] Furthermore, when bonding a molded product to another resin, a fiber-reinforced resin molded product, or a metal with an adhesive in a post-process, pre-processing was performed, such as removing the release agent or release film components by abrading the surface of the molded product with a blasting treatment or a peel ply, or forming unevenness on the surface, etc. Therefore, there were problems such as an increase in the takt time of the manufacturing process due to processing and an increase in processing costs.

[0010] The object of the present invention is to solve the above problems, that is, to provide a molded article of a carbon fiber reinforced composite material which can be bonded well regardless of the type of adhesive or metal to be used in combination, and which can maintain its bonding strength even after a long period of time has passed since bonding. Another object of the present invention is to provide a molded product which can be satisfactorily bonded with an adhesive without the need for time-consuming blasting treatment after molding. [Means for solving the problem]

[0011] The present inventors have found that the above problems can be solved by the following invention.

[0012] The following inventions relate to molded articles made of carbon fiber reinforced composite materials. (1) A molded article of a fiber-reinforced composite material comprising at least carbon fiber and a resin composition, characterized in that the molded article has a surface roughness Ra of 0.01 μm or more and 2 μm or less, and when bonded to a metal via an adhesive layer containing an epoxy compound and having a thickness of 0.1 mm or more and 3 mm or less on the surface, the tensile shear bond strength (F0) is 10 MPa or more and 40 MPa or less.

[0013] As a preferred embodiment of the molded article of the carbon fiber reinforced composite material, there is the following invention. (2) The surface free energy (γ TOTAL ) is 30mJ / m 2 More than 80mJ / m 2 The surface free energy (γ TOTAL ) which constitutes the surface free energy dispersion component (γ d ) and the polar component of the surface free energy (γ p ) and the ratio {γ p / γ d} is 0 or more and 1 or less. (3) A molded article of any of the carbon fiber composite materials described above, wherein the ratio of the number of fluorine (F) atoms to the number of carbon (C) atoms {F / C} on the surface of the molded article, as measured by X-ray photoelectron spectroscopy, is 0 or more and 0.5 or less. (4) A molded article made of any of the carbon fiber composite materials described above, wherein the ratio of the number of oxygen (O) atoms to the number of carbon (C) atoms {O / C} on the surface of the molded article, as measured by X-ray photoelectron spectroscopy, is 0.2 or more and 1.2 or less. (5) A molded article of any of the above carbon fiber composite materials, in which, in narrow scan C1s peak division measured on the surface of the molded article by X-ray photoelectron spectroscopy, the intensity ratio {X / M} of the peaks (X) assigned to CO and CN to the main peak (M) is 0.4 or more and 0.8 or less.

[0014] (6) A molded article of any of the carbon fiber composite materials described above, wherein in narrow scan C1s peak division measured on the surface of the molded article by X-ray photoelectron spectroscopy, the intensity ratio {Y / M} of the peak (Y) assigned to C=O to the main peak (M) is 0.1 or more and 0.3 or less. (7) A molded article of any of the above carbon fiber composite materials, wherein in narrow scan C1s peak division measured on the surface of the molded article by X-ray photoelectron spectroscopy, the intensity ratio {Z / M} of the peak (Z) assigned to C(=O)-O to the main peak (M) is 0.1 or more and 0.3 or less. (8) A molded product of any of the carbon fiber composite materials described above, wherein the carbon fibers contained in the molded product have an average diameter of 1 to 20 μm and an average length of 10 mm or more, and the carbon fiber content in the carbon fiber composite material is 5 to 75 volume %. (9) Any of the above molded products of carbon fiber composite material, wherein the resin composition contained in the molded product of the carbon fiber composite material is a thermosetting resin composition containing an epoxy resin. (10) Tensile shear bond strength (F0) and the tensile shear bond strength measured after moist heat treatment (F 11 ) ratio {F 11 / F0} is 0.75 or more and 1 or less.

[0015] The following invention is a preferred method for producing a molded article of the above carbon fiber composite material. (11) A method for producing a molded article of any one of the above carbon fiber composite materials by molding a carbon fiber composite material, characterized in that a release agent containing elemental fluorine or a release film containing elemental fluorine is used in the molding. (12) A method for producing a molded article of a carbon fiber composite material, comprising the steps of: (a) subjecting the carbon fiber composite material to a plasma treatment after the press molding; and (b) treating the surface of the carbon fiber composite material. Effect of the Invention

[0016] The molded article of the carbon fiber composite material of the present invention can be well bonded regardless of the type of adhesive or metal used in combination, and can maintain its bonding strength even after a long period of time has passed since bonding.

[0017] In this way, good adhesion can be achieved regardless of the type of adhesive or metal used in combination. Therefore, by using a molded product of the carbon fiber composite material of the present invention, it is possible to join materials having completely different mechanical properties, for example, and when designing final products, it is possible to create structures with shapes and properties that were previously impossible.

[0018] Furthermore, even when release agents or release films are used when molding carbon fiber composite materials as in the past, pretreatment that requires a long processing time, such as blasting before bonding, is not required, which can contribute to cost reduction. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a graph showing narrow scan C1s peak splitting measured by X-ray photoelectron spectroscopy for a molded article of the carbon fiber composite material of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] First, we will explain carbon fiber composite materials. Carbon fiber composite materials that have been molded are also carbon fiber composite materials, and carbon fiber composite materials before being molded into a desired shape are also carbon fiber composite materials. However, in order to distinguish between before and after molding, the former is called a molded product of carbon fiber composite material, and the latter is simply called carbon fiber composite material.

[0021] It is important to use carbon fibers in the carbon fiber composite material of the present invention in order to realize excellent mechanical properties and ease in designing these properties.

[0022] Carbon fiber composite materials contain at least carbon fibers and a resin composition. When the carbon fibers are present in an amount of 1% by mass or more relative to the resin in the resin composition, the carbon fibers adhere well to the resin that forms a matrix around the carbon fibers, and the carbon fiber composite material exhibits excellent mechanical properties.

[0023] The carbon fiber used in the carbon fiber composite material of the present invention is preferably a polyacrylonitrile-based carbon fiber. The polyacrylonitrile-based carbon fiber is excellent in terms of realizing low cost while having a good balance of specific strength, specific rigidity, light weight, and electrical conductivity.

[0024] The carbon fibers in the carbon fiber composite material of the present invention and in the molded article made therefrom preferably have an average fiber diameter of 1 to 20 μm, more preferably 3 to 15 μm, and most preferably 4 to 10 μm.

[0025] By being within the above range, a molded article of the carbon fiber composite material of the present invention can exhibit excellent mechanical properties and processability.

[0026] The carbon fibers in the carbon fiber composite material of the present invention and in the molded products made therefrom may be continuous or discontinuous, but preferably have an average length of 10 mm or more and 2000 mm or less. By being in the above range, excellent specific strength and rigidity can be imparted.

[0027] The carbon fiber composite material of the present invention and molded articles made therefrom preferably contain 5 to 75% by volume of carbon fibers. This range allows the carbon fiber composite material of the present invention to have excellent moldability and the molded articles to have excellent mechanical properties. The content is more preferably 10 to 65% by volume.

[0028] It is important that the matrix portion of the carbon fiber composite material in the present invention and the molded article made therefrom is a resin composition. By including a resin in the resin composition, it is possible to easily form a composite with the carbon fiber, and it is also possible to maintain a good balance between the specific strength and specific rigidity of the molded article and the manufacturing cost. The resin composition is not particularly limited, and for example, a thermosetting resin, a thermoplastic resin, or the like can be used.

[0029] From the viewpoints of mechanical properties and processing properties during molding, the resin composition used in the carbon fiber composite material of the present invention preferably contains a thermosetting resin.

[0030] Examples of thermosetting resins that can be used include unsaturated polyester resins, vinyl ester resins, epoxy resins, phenolic resins (resol type), urea-melamine resins, polyimide resins, and copolymers, modified products, or blends of two or more of these resins.

[0031] Among these, epoxy resins are preferred for obtaining molded products of carbon fiber composite materials with excellent mechanical properties, because it is easy to mix the resin with carbon fibers. Another advantage of using epoxy resins is that they are easy to mold. Among these, epoxy resins that are mainly composed of bisphenol A type epoxy resins are preferred from the viewpoints of economic efficiency and balance of mechanical properties.

[0032] In order to improve impact resistance, an elastomer or rubber component may be added to the thermosetting resin composition. Examples of such carbon fiber composite materials include thermosetting prepregs and thermoplastic prepregs using woven fabrics or unidirectional continuous carbon fibers, carbon fiber reinforced SMCs and carbon fiber reinforced stampable substrates in which discontinuous carbon fibers are randomly dispersed, and long fiber pellets and short fiber pellets used in injection molding.

[0033] The molding method for the carbon fiber composite material of the present invention can be appropriately selected from resin transfer molding (RTM) molding, autoclave molding, press molding, filament winding molding, etc., but is not particularly limited.

[0034] Hereinafter, preferred embodiments for achieving high tensile shear bond strength and durability in a molded article obtained from the above-mentioned carbon fiber composite material of the present invention will be described.

[0035] It is important that the surface roughness Ra of the molded product of the carbon fiber composite material in the present invention is 0.01 μm or more and 2 μm or less. The smaller the Ra value of the molded product, the smoother the surface of the molded product. If the Ra value is less than 0.01 μm, the handleability of the molded product may be significantly reduced. On the other hand, if the Ra value of the molded product is more than 2 μm, the surface may be easily damaged, such as carbon fibers being exposed on the material surface, the material surface being deteriorated, and the strength being reduced.

[0036] To obtain a molded product of a carbon fiber composite material with an Ra of 0.01 to 2 μm, it is important that the carbon fibers are uniformly dispersed in the resin composition, that highly smooth materials are used for the mold and film that come into contact with the resin composition during molding, and that the adhesion and releasability to the mold are appropriately adjusted.

[0037] For example, when a carbon fiber composite material is produced by press-molding a prepreg in which carbon fibers are impregnated with a thermosetting resin into a molded product, a desired surface roughness Ra can be obtained by using a film with small surface roughness between the prepreg and the mold of the press machine or by lowering the processing temperature so that the irregularities on the film surface are less likely to be transferred.

[0038] Furthermore, by subjecting a molded product of a carbon fiber composite material to atmospheric pressure plasma treatment under the conditions described below, it is possible to impart good adhesive bonding to other components in a short period of time while maintaining the Ra value within the above range, even if a release agent or release film is used during molding.

[0039] An example of atmospheric pressure plasma treatment conditions: Plasma nozzle rotation speed: 1000-3000 rpm Plasma nozzle back pressure 40-60mbar Gas flow rate from plasma nozzle: Q35~55L / min Plasma power Pp: 400~490W Gas used: air, oxygen or nitrogen Processing speed (movement speed of plasma nozzle during processing): 1m / min to 10m / min Processing distance (distance between the tip of the plasma nozzle and the material being processed): 1mm~30mm.

[0040] In the present invention, when atmospheric pressure plasma treatment is performed, it is preferable that the plasma density Pd, defined by the electric power Pp (plasma power) determined by the voltage value and current value for generating plasma, and the flow rate Q of the gas flowing in per unit time, be 7.2 to 14, as defined by the following formula. Pd = Pp / Q.

[0041] The surface roughness RSm of the molded product of the carbon fiber composite material of the present invention is preferably 0.01 μm or more and 250 μm or less, because within this range, the minute irregularities on the material surface combine with the adhesive to exhibit an anchor effect while minimizing exposure of the carbon fibers on the material surface, thereby improving adhesive bonding.

[0042] It is also important that the molded product of the carbon fiber composite material of the present invention has a tensile shear bonding strength of 10 MPa or more and 40 MPa or less when a metal is bonded to the surface of the product via an adhesive containing an epoxy compound with a thickness of 0.1 mm or more and 3 mm or less.

[0043] If the thickness of the adhesive layer formed on the surface of the molded article of the carbon fiber composite material of the present invention is less than 0.1 mm, when the molded article of the carbon fiber composite material and the metal are distorted by heat, the difference in the degree of expansion between them cannot be alleviated, and peeling may occur. On the other hand, if the thickness of the adhesive layer is more than 3 mm, the shear stress decreases, and the bonded body may become unstable against an external force.

[0044] The thickness of the adhesive formed on the surface of the molded article of the carbon fiber composite material of the present invention is preferably 0.2 mm to 2.5 mm, and more preferably 0.3 mm to 2 mm, from the viewpoints of adhesive strength and productivity.

[0045] For example, in order to set the thickness of the adhesive layer within the above range, for example, an adhesive can be applied to either or both of the surfaces of the molded product of the carbon fiber composite material of the present invention and the metal, and when laminating them together, glass beads having a particle size corresponding to the desired thickness can be added, or a metal wire having a diameter corresponding to the desired thickness can be installed, and then the molded product and the metal at the joint can be clamped with a clip, or one of them can be fixed and pressure can be applied from the surface of the other material between which the adhesive is sandwiched to fix them.

[0046] It is important that the molded product of the carbon fiber composite material of the present invention has a tensile shear bond strength of 10 MPa or more and 40 MPa or less when a metal is bonded to the surface of the molded product via an adhesive containing an epoxy compound. It is important that the adhesive used in the present invention contains an epoxy compound. An epoxy compound is a compound having an epoxy group. By containing an epoxy compound, the epoxy group chemically reacts with the functional group present on the surface of the molded product, and the chemical interaction caused by the reaction can impart good adhesion and excellent tensile shear bond strength.

[0047] When the tensile shear bond strength of the molded product of the carbon fiber composite material of the present invention is less than 10 MPa when the surface of the molded product is bonded to a metal via an adhesive containing an epoxy compound, the adhesive bond strength is weak, making the product less practical for use in bonding structural members for automobiles, aircraft, buildings, etc.

[0048] On the other hand, if the tensile shear bond strength is greater than 40 MPa, when the molded article of the carbon fiber composite material of the present invention and the metal are distorted by heat, the adhesive layer cannot follow the deformation, and the bonded body may be destroyed.

[0049] The tensile shear bonding strength is preferably 15 MPa to 35 MPa, and more preferably 20 to 30 MPa, from the viewpoints of the substantial strength of the bonded body and durability against deformation due to heat.

[0050] In order to make the tensile shear bond strength of the test specimen in which the molded product of the carbon fiber composite material of the present invention and the metal are adhesively bonded to 10 to 40 MPa, it is important to use an adhesive having more epoxy groups in the adhesive, to apply the adhesive evenly to the entire bonding surface, and to thoroughly degas the adhesive before application so that no voids or bubbles are generated in the applied adhesive. This is because the more epoxy groups in the adhesive, the stronger the chemical interaction with the functional groups present on the surface of the molded product of the carbon fiber composite material of the present invention, and the fewer voids and bubbles in the adhesive, the higher the shear strength of the adhesive layer itself.

[0051] The surface free energy (γTOTAL ) is 30mJ / m 2 More than 80mJ / m 2 It is preferably 35 to 75 mJ / m or less. 2 The surface free energy is 30 to 80 mJ / m 2 This is preferable because it can impart good adhesive activity to the surface of the molded article of the present invention.

[0052] The higher the surface free energy of the molded article of the present invention, the better the above-mentioned properties tend to be, and this is preferable. However, if the surface free energy is too high, the surface of the material may become brittle, or its activity may not last for a long period of time, and good adhesion may not be achieved when the adhesive is applied.

[0053] The surface free energy of a molded carbon fiber composite material can be controlled by the release agent or release film used during molding, or by surface treatment after molding. The lower the fluorine content in the release agent or release film, the higher the surface free energy. In addition, the surface free energy can be increased by subjecting the surface of the molded carbon fiber composite material to atmospheric pressure plasma treatment.

[0054] Surface free energy (γ TOTAL ) can be changed by changing the resin used to form the matrix resin of the carbon fiber composite material, such as epoxy resin, polyphenylene sulfide resin, polypropylene resin, vinyl ester resin, unsaturated polyester resin, cyanate ester resin, etc.

[0055] The surface free energy dispersion component (γ d ) and the polar component of the surface free energy (γ p ) ratio {γ p / γ d} is preferably 0 or more and 1 or less, more preferably 0.1 to 1, even more preferably 0.2 to 1, and most preferably 0.3 to 1. By having the ratio of the surface free energy dispersion component to the surface free energy polar component within the above range, it is possible to impart good reactivity with the adhesive to the surface of the molded article of the present invention. At the same time, it is possible to maintain good strength of the surface of the molded article of the present invention. As a result, when an impact is applied from the outside to the bonded body with the metal, it is possible to make it difficult for peeling failure to occur at the interface between the adhesive and the molded article, and for the molded article of the carbon fiber composite material itself to be broken near the surface.

[0056] Surface free energy polar component (γ p ) can be controlled by the release agent or release film used during molding, or by surface treatment after molding. For example, when performing atmospheric pressure plasma treatment on the surface of a molded carbon fiber composite material after molding, it can be controlled by adjusting the type and amount of functional groups introduced onto the surface of the molded product by adjusting the type of gas used, the distance between the plasma nozzle and the molded product during treatment, and the treatment speed.

[0057] The surface of a molded article of the carbon fiber composite material of the present invention preferably has a ratio of the number of fluorine (F) atoms to the number of carbon (C) atoms {F / C} on the surface of the molded article of the carbon fiber composite material, as measured by X-ray photoelectron spectroscopy, of 0 or more and 0.5 or less, more preferably 0 to 0.4, even more preferably 0 to 0.3, and most preferably 0 to 0.2.

[0058] The lower the fluorine concentration on the surface of the molded article of the present invention, the higher the adhesion can be imparted, because elemental fluorine inhibits chemical interaction between the epoxy groups of the adhesive and the surface of the molded article of the carbon fiber composite material of the present invention.

[0059] The fluorine concentration can be controlled by the release agent or release film used during molding, or by surface treatment of the molded product of the present invention after molding. The fluorine concentration can be reduced by molding using a release agent or release film with a low fluorine content, or by subjecting the surface of the carbon fiber composite material to atmospheric pressure plasma treatment after molding.

[0060] In the case where a release agent or film containing fluorine is used in molding, the ratio may actually be 0.1 or more and 3.0 or less.

[0061] The surface of the molded article of the carbon fiber composite material of the present invention preferably has a ratio of the number of oxygen (O) atoms to the number of carbon (C) atoms {O / C} of 0.2 or more and 1.2 or less, more preferably 0.2 to 1.0, and most preferably 0.2 to 0.8, as measured by X-ray photoelectron spectroscopy.

[0062] The higher the oxygen concentration on the surface of the molded article of the present invention, the higher the adhesiveness that can be imparted. This is because the functional groups containing oxygen are present in large numbers on the surface of the molded article of the carbon fiber composite material, and they tend to chemically interact with the epoxy groups of the adhesive.

[0063] If the {O / C} value is greater than 1.2, the surface of the molded product will react with water vapor in the air, making it practically difficult to store the product with a high {O / C} value.

[0064] The ratio of the number of oxygen (O) and carbon (C) atoms on the surface can be controlled by treating the surface after molding. For example, by subjecting the surface of the obtained molded article to atmospheric pressure plasma treatment, a larger amount of oxygen element can be introduced into the surface of the molded article of the carbon fiber composite material of the present invention. In order to control the amount of oxygen element to be introduced, the distance between the nozzle irradiating atmospheric pressure plasma and the molded article can be shortened, or the treatment speed can be slowed down. Furthermore, the oxygen concentration on the surface of the molded article can be increased by using oxygen gas or nitrogen gas instead of dry air as the gas introduced into the plasma generating nozzle during plasma irradiation, and further by adjusting the gas concentration, mixing ratio, and flow rate (L / min) of these gases.

[0065] When the surface of the molded article of the carbon fiber composite material of the present invention is measured by X-ray photoelectron spectroscopy and the narrow scan C1s data is peak-split, the area ratio {X / M} of the peak (X) assigned to CO and CN to the main peak (M) (assigned to CHx and CC bonds) having the largest peak area observed near 284.6 eV is preferably 0.4 or more and 0.8 or less, more preferably 0.6 to 0.8.

[0066] When the surface of the molded article of the present invention is measured by X-ray photoelectron spectroscopy and the narrow scan C1s data is peak-divided, the intensity ratio {Y / M} of the peak (Y) attributed to C=O to the main peak (M) having the largest peak area is preferably 0.1 or more and 0.3 or less, more preferably 0.15 to 0.3.

[0067] When the surface of the molded article of the present invention is measured by X-ray photoelectron spectroscopy and the narrow scan C1s data is peak-divided, the intensity ratio {Z / M} of the peak (Z) assigned to C(=O)-O to the main peak (M) having the largest peak area is preferably 0.1 or more and 0.3 or less, more preferably 0.15 to 0.3.

[0068] When the functional groups present on the surface of the molded article of the present invention are many, such as CO, CN, C=O, and C(=O)-O, the number of sites for chemical interaction with the epoxy groups in the adhesive increases, and good adhesive strength can be imparted between the carbon fiber composite material and the adhesive. Among these, it is most preferable that the peak intensity of C=O, which has high reactivity with epoxy groups, is high.

[0069] The type of functional group on the surface of the molded article of the present invention can be controlled by the type of resin composition contained in the carbon fiber composite material and by surface treatment after molding. For example, the concentration of the functional group can be adjusted by using a resin that contains many of the components CO, CN, C=O, and C(=O)-O in the chemical structure of the resin, or by increasing the oxygen concentration in the atmosphere in which the plasma is generated when the surface after molding is treated with atmospheric pressure plasma.

[0070] The carbon fiber composite material molded article of the present invention has a surface to which a metal is bonded via an adhesive layer containing an epoxy compound, and the tensile shear bond strength (F0) of a joint is measured, and the tensile shear bond strength (F 11 ) ratio {F 11 / F0} is preferably 0.75 or more and 1 or less, more preferably 0.80 to 1, and most preferably 0.85 to 1.

[0071] Tensile shear bond strength ratio {F 11 By setting the value of {F0} within the above range, when a bonded body obtained by bonding the molded article of the present invention and a metal via an adhesive layer is used as an automobile part, an aircraft part, or a building part, the desired bonding strength can be maintained for a long period of time, which is preferable because it can impart high durability and reliability to the final product.

[0072] The ratio of the tensile shear bond strengths {F 11 / F0} can be controlled by adjusting the epoxy group content, moisture absorption, and heat resistance of the adhesive used.

[0073] An example of a method for producing a molded product using press molding, in which carbon fiber prepregs are used as the carbon fiber composite material before molding, is shown below.

[0074] For example, unidirectional prepreg P3842S-20 (manufactured by Toray Industries, Inc.) is laminated in a configuration (0 / 0) so that the carbon fibers are parallel to one another, and polypropylene films (Toray Industries, Inc. "Treyfan" (registered trademark) BO2500, thickness 50 μm, glossy type) are placed on both surfaces of this laminate. The laminate is then heated and compressed at 120°C and a pressure of 2 MPa for 40 minutes using a hot press to obtain a laminated plate with a thickness of approximately 3 mm.

[0075] The obtained laminate is treated using a plasma generating device (generator FG5001, rotation nozzle RD1004) manufactured by Japan Plasmatreat, with the distance between the plasma treatment nozzle and the laminate set to 5 mm and the speed at which the treatment nozzle moves over the laminate set to 5 m / min. The plasma is generated in air at normal temperature and humidity and irradiated onto the laminate, thereby obtaining a molded product of a carbon fiber composite material having the characteristics of the present invention.

[0076] The treatment conditions for the plasma treatment are preferably a plasma nozzle rotation speed of 1000 to 3000 rpm, a plasma nozzle back pressure of 40 to 60 mbar, and a gas flow rate from the plasma nozzle of 35 to 55 L / min. More preferably, the plasma nozzle rotation speed is 1500 to 2800 rpm, a plasma nozzle back pressure of 45 to 55 mbar, and a gas flow rate from the plasma nozzle of 40 to 50 L / min. By performing treatment under these conditions, it becomes possible to effectively and efficiently introduce functional groups into the surface of a molded article of a carbon fiber composite material.

[0077] The molded article of the carbon fiber composite material of the present invention can form a strong bond with metal via an adhesive layer. In particular, when used as a structural member of an automobile, aircraft, or building, which is difficult to dismantle or modify after completion of the final product, it is preferable because it has excellent bondability with metal materials and can maintain its bond strength for a long period of time, thereby providing higher reliability than molded articles of conventional carbon fiber composite materials. EXAMPLES

[0078] The present invention will be described with reference to examples. Hereinafter, a molded article made of a carbon fiber composite material will be simply referred to as a molded article.

[0079] I. Characteristics Measurement Method The characteristics were measured as follows.

[0080] 1. Tensile shear bond strength Adhesive is applied to the bonding surface of the molded product, and a metal material is bonded to the adhesive to form a test piece for measuring the tensile shear bond strength. A tensile test is performed using a universal testing machine, and the load at which the test piece breaks and the state of fracture of the bond are visually observed.

[0081] The tensile test was carried out in an atmosphere of 23° C. and 50% RH with the distance between the chucks of the test machine set to 115 mm.

[0082] 2. Destruction state of the joint The state of destruction of the joints was observed and classified as follows. The results are shown in the table as A, B, and C. A. Cohesive failure of adhesive: This refers to the state in which the adhesive remains attached to both the metal side and the molded product side of the test specimen that is destroyed after the tensile shear test. B. Peeling off at the interface between molded product and adhesive...This refers to the state in which, for a destroyed test piece after a tensile shear test, the entire adhesive layer remains on the metal side, and no adhesive adheres to the carbon fiber composite material side. C. Peeling off at the interface between metal and adhesive...This refers to the state in which, for a destroyed test specimen after a tensile shear test, the entire adhesive layer remains on the molded product side, and no adhesive adheres to the metal side.

[0083] 3. Surface Free Energy The test piece to be measured was placed on a horizontally placed glass plate. Using a fully automatic handheld contact angle meter MSA manufactured by KRUSS GmbH and software ADVANCE (Ver.1.8), 2μL of each liquid, ultrapure water ("CAS RN":7732-18-5) and diiodomethane ("CAS RN":75-11-6), was dropped onto the test piece. The droplet formed on the test piece 3 seconds after the drop was observed from the side, and the contact angle θ between the test piece and the droplet was measured.

[0084] In calculating the contact angle θ (°), similar measurements were performed at five random locations on the test piece, and the average value of the measurement results for three locations excluding the maximum and minimum values ​​was used as the contact angle θ (°) of the test piece.

[0085] Using the contact angle θ (°) obtained, the surface free energy (γ TOTAL ), the dispersion component of the surface free energy (γ d ), the polar component of the surface free energy (γ p ) was calculated.

[0086] The conditions for measuring the contact angle of ultrapure water were as follows. Contact angle measurement ambient temperature: 20℃ Surface tension data of ultrapure water used to calculate surface free energy: 72.8 mN / m (polarity 51.0 mN / m, dispersion 21.8 mN / m) (Reference: J. Colloid Interface Sci, 127, 1989, 189 - 204, author: Janczuk, B.).

[0087] The conditions for measuring the contact angle of diiodomethane were as follows. Contact angle measurement ambient temperature: 25℃ Surface tension data for diiodomethane used to calculate surface free energy: 50.8 mN / m (polarity 0 mN / m, dispersion 50.8 mN / m) (Reference: J. Colloid Interface Sci, 119, 1987, 352 - 361, author: Strom, G.).

[0088] 4.X-ray photoelectron spectroscopy measurement Using a photoelectron spectrometer (model Quantera SHM) manufactured by PHI, small pieces of the molded article of the present invention were arranged on a sample support table. 8 The pressure was kept at 1.2 MPa and the concentration was kept at 1.2 MPa. Qualitative analysis (wide scan analysis) was performed under the following conditions to detect elements with high sensitivity by scanning the entire energy range (high energy resolution analysis) and high resolution analysis (narrow scan analysis) was performed to scan a narrow energy range under high energy resolution conditions for carbon element (C1s). After that, data processing and analysis were performed. For each analysis, linear baselines were drawn in the ranges of 0-1100 eV and 278-298 eV to calculate the area intensity of each peak.

[0089] For the narrow scan analysis of C1s, as shown in Figure 1, the peak at around 284.61 eV was divided into CHx, CC, and C=C bonds, the peak at around 286.34 eV into CO or CN bonds, the peak at around 287.66 eV into C=O bonds, the peak at around 289.01 eV into O=CO bonds, and the peak at around 290.80 eV into π-π* satellite and OC(=O)-O bonds, and the areas of each peak were then calculated.

[0090] The atomic percentage of the elements obtained from the wide scan analysis was taken as the atomic percentage of the corresponding elements on the surface of the molded article. The peak intensities of the CO and CN bonds obtained from the narrow scan analysis were taken as X, CH x The peak intensity of CC and C=C bonds was designated as M, the peak intensity of C=O bonds was designated as Y, and the peak intensity of O=CO bonds was designated as Z.

[0091] The measurement conditions were as follows. Excited X-ray: monochromatic Al Kα 1,2 Rays (1486.6 eV) X-ray diameter: 200μm Photoelectron detection angle: 45° (detector angle relative to sample surface) X-ray power: 15kV, 45W.

[0092] The data was processed as follows. Smoothing: 9-point smoothing Horizontal axis correction: The main peak (M) (CHx, CC bonds) of the C1s scan was set to 284.6 eV.

[0093] 5. Surface roughness Ra The center line average roughness Ra of the molded article is measured using a stylus surface roughness meter under the following conditions: The molded article is scanned 20 times in the direction perpendicular to the carbon fibers, and the average value of the obtained results is defined as the average roughness Ra in the present invention. Measurement equipment: Kosaka Laboratory's high-precision thin film step measuring instrument ET-10 Stylus tip radius: 0.5μm Stylus load: 5mg Measurement length: 1mm Cutoff value: 0.08mm Measurement environment: temperature 23℃, humidity 65%RH.

[0094] 6. 10-point average roughness Rz and average length of roughness curve element RSm Kosaka Laboratory's 3D micro shape measuring instrument (model ET-350K) and 3D surface roughness analysis The surface roughness Rz (10-point average roughness) and the average length of the roughness curve element RSm were measured using a system (model TDA-22). The conditions were as follows, and the average value of 20 measurements was used. Stylus diameter: 2μm Stylus load: 0.04mN Vertical magnification: 50,000 times Cutoff: 0.5mm Feed pitch: 5μm Measurement length: 0.5mm Measurement area: 0.2mm 2 Measurement speed: 0.1mm / sec.

[0095] 7. Pretreatment time required to prepare the material surface before applying adhesive.

[0096] The processing time required for surface treatment of the molded product, which is carried out after the product has been molded and removed from the metal mold, etc. and before the adhesive is applied, was evaluated based on the following criteria in terms of the takt time of the production process. The time required to uniformly treat the surface of a test specimen measuring 25 mm in width and 100 mm in length was classified as follows: Processing time 1 minute or less: A Processing time exceeds 1 minute: B.

[0097] 8.Durability test The overlapping test pieces bonded with adhesive were left for 30 days in a highly accelerated life tester (Espec Corp. Lightspec thermohygrostat LHU-114) under a humid heat environment of 85°C and 95% RH, then naturally cooled and left for 24 hours under standard conditions (23±2°C, 50±5% RH). Tensile tests were performed 20 times on these bonded test pieces under the same conditions as above, and the average load at break (F 11 The average value of the obtained load (F 11 ) and F0, the strength retention rate F11 / F0 was calculated using the following formula. Strength retention rate (%)=(F 11 / F0) x ​​100.

[0098] 9. Overall rating The evaluation was based on the following criteria. Note that "joint strength is within the specified range" means that "the tensile shear joint strength (F0) is 10 MPa or more and 40 MPa or less." If the bonding strength is not within the specified range: Defective If pretreatment time exceeds 1 minute: Defective If the bonding strength is within the specified range, and the processing time is within 1 minute, 11 / If F0 is greater than 0.8: Excellent If the bonding strength is within the specified range, and the processing time is within 1 minute, 11 / F0 is greater than 0.75 and less than or equal to 0.8: Good If the bonding strength is within the specified range, and the processing time is within 1 minute, 11 / If F0 is greater than 0.6 and less than 0.75: Normal. II. Molded products in examples and comparative examples and materials used therein <Molded product 1> Sixteen sheets of unidirectional carbon fiber prepregs (P3832S-20, manufactured by Toray Industries, Inc.) were laminated with the fiber direction all aligned, and polypropylene films ("Treyfan" (registered trademark) BO2500, manufactured by Toray Industries, Inc., thickness 50 μm, glossy type) were placed on both surfaces of this laminate, and then molded product 1 with an average thickness of 3 mm was obtained by press molding. The table shows the surface free energy, surface free energy dispersion component, surface free energy polar component, and measurement results and analysis results by X-ray photoelectron spectroscopy for each example described below using this molded product 1. Then, each molded product was cut into a 45 mm x 10 mm rectangular piece.

[0099] <Molded product 2> Molded article 2 was obtained by molding in the same manner as in the production of molded article 1, except that a fluororesin film (AGC Corporation's "Aflex" (registered trademark) 25MW 1080NT) was used instead of the polypropylene film. The surface free energy, surface free energy dispersion component, surface free energy polar component, and measurement results and analysis results by X-ray photoelectron spectroscopy for each of the examples described below using this molded article 2 are shown in the table.

[0100] After that, each molded product was cut into a rectangular piece of 45 mm x 10 mm.

[0101] <Adhesive 1> 3M's two-component curing epoxy adhesive "Automix TM The adhesive was applied to the test piece using Panel Bond 8115 (registered trademark) with a dedicated hand gun (3M Automix Hand Gun 8117) and a dedicated mixing nozzle (3M Automix Mixing Nozzle 8193). In order to control the adhesive area, masking paper was used to prevent the adhesive from adhering to more than the desired area. The thickness of the adhesive layer was adjusted with glass beads of φ0.5±0.1 mm. <Adhesive 2> LORD's two-component curing urethane adhesive "LORD" (registered trademark) 7545-A / D (A is the main material, D is the curing agent) was applied to the test pieces using a hand gun and a dedicated mixing nozzle. In order to control the adhesive area, masking paper was used to ensure that the adhesive did not adhere to more than the desired area. The thickness of the adhesive layer was adjusted using glass beads with a diameter of 0.5 ± 0.1 mm.

[0102] <Metal 1> Iron (grade SPCC-SD) (thickness 1.5 mm) was cut into 45 mm x 10 mm strips using a laser, and the surfaces of the strips were degreased with acetone before use.

[0103] <Molded product 3> Molded article 3 was obtained in the same manner as in the production of molded article 1, except that a poly-4-methylpentene-1 film ("Opulent" (registered trademark) X88B manufactured by Mitsui Chemicals Tohcello Co., Ltd.) was used instead of the polypropylene film. Table 1 shows the measurement results and analysis results of the surface free energy, the surface free energy dispersion component, the surface free energy polar component, and the X-ray photoelectron spectroscopy for each of the examples described below using this molded article 3.

[0104] After that, each molded product was cut into a rectangular piece of 45 mm x 10 mm.

[0105] <Molded product 4> Molded article 4 was obtained by molding in the same manner as in the production of molded article 1, except that a poly-4-methylpentene-1 film ("Opulent" (registered trademark) X44B manufactured by Mitsui Chemicals Tohcello Co., Ltd.) was used instead of the polypropylene film. The surface free energy, the surface free energy dispersion component, the surface free energy polar component, and the measurement results and analysis results by X-ray photoelectron spectroscopy for each of the examples described below using this molded article 4 are shown in the table.

[0106] After that, each molded product was cut into a rectangular piece of 45 mm x 10 mm.

[0107] <Molded product 5> Molded article 5 was obtained by molding in the same manner as in the production of molded article 1, except that a cycloolefin polymer film ("ZEONORFILM" (registered trademark) ZF16-050, manufactured by Zeon Corporation) was used instead of the polypropylene film. Table 1 shows the measurement results and analysis results of the surface free energy, the surface free energy dispersion component, the surface free energy polar component, and the X-ray photoelectron spectroscopy for each of the examples described below using this molded article 5.

[0108] After that, each molded product was cut into a rectangular piece of 45 mm x 10 mm. III. Examples and Comparative Examples Example 1 Atmospheric pressure plasma treatment was performed on the surface of the rectangular piece of molded product 1. The atmospheric pressure plasma treatment was performed by irradiating the carbon fiber composite material 1 with plasma generated in air at normal temperature and humidity using a plasma generator (generator FG5001, rotation nozzle RD1004) from Japan Plasmatreat, with the distance between the plasma treatment nozzle and the molded product set to 5 mm, the speed at which the treatment nozzle moved over the molded product 1 set to 5 m / min, the rotation speed of the plasma nozzle set to 1600 RPM, the air flow rate introduced into the treatment nozzle set to 45 L / min, and the wattage after boosting set to 433 W.

[0109] The surface free energy, the dispersive component of the surface free energy, the polar component of the surface free energy, and the measurement and analysis results by X-ray photoelectron spectroscopy of the molded article 1 after this plasma treatment are shown in the table.

[0110] Within 30 minutes of the treatment, adhesive 1 was applied to the plasma-treated surface of molded product 1 and bonded to metal 1 to prepare an overlapping test specimen type B (adhesive thickness: 0.5 mm) as described in ISO 19095-2 (2015).

[0111] When preparing the overlapping test pieces, the applied adhesive was left to stand in a hot air oven in a dry air atmosphere at 60°C for 5 hours to completely harden the adhesive, and a molded product and metal overlapping test piece was prepared. The test piece was stored in an atmosphere of 25°C and 50% RH.

[0112] Within one week of preparing the overlapping test pieces, a tensile test was carried out at room temperature of 25°C and a test speed of 5mm / min using a test piece holder of the tensile shear bond strength evaluation device described in ISO 19095-3 (2015). The tensile tester used was an INSTRON Universal Testing Machine 5969, and evaluation was performed with an n number of 3, and the average value was taken as the tensile shear bond strength (F0).

[0113] In addition, after preparing overlapping test pieces, samples were prepared according to the method described in the durability test above, and then a tensile test was performed at room temperature of 25°C and a test speed of 5 mm / min using a test piece holder described in ISO 19095-3 (2015). The tensile tester used was an INSTRON universal testing machine 5969, and evaluation was performed with an n number of 3, and the average value was calculated as the tensile shear bond strength (F 11 ) was decided.

[0114] The evaluation results of the obtained overlapping test pieces are shown in the table.

[0115] Example 2 Example 2 was carried out under the same conditions as Example 1, except that molded article 2 was used instead of molded article 1 in Example 1.

[0116] Example 3 Adhesive 1 was applied to one of the surfaces of molded article 1 and bonded to metal 1 to prepare an overlapping test specimen (adhesive thickness: 0.5 mm) as described in ISO 19095-2 (2015).

[0117] Within one week of preparing the overlapping test specimens, a tensile test was carried out at a test speed of 5 mm / min at room temperature of 25°C using a test specimen holder as specified in ISO 19095-3 (2015). The tensile tester used was an INSTRON Universal Testing Machine 5969, and evaluation was performed with an n number of 3, with the average value being the tensile shear bond strength (F0).

[0118] In addition, after preparing the overlapping test pieces, they were subjected to a wet heat treatment, and then a tensile test was performed at room temperature of 25°C and a test speed of 5 mm / min using a test piece holder as specified in ISO 19095-3 (2015). The tensile tester used was an INSTRON universal testing machine 5969, and evaluation was performed with an n number of 3, and the average value was calculated as the tensile shear bond strength (F 11 ) was decided.

[0119] The evaluation results of the obtained overlapping test pieces are shown in Table 1.

[0120] Example 4 Example 4 was carried out under the same conditions as Example 1, except that molded article 3 was used instead of molded article 1 in Example 1.

[0121] Example 5 Example 5 was carried out under the same conditions as Example 1, except that molded article 4 was used instead of molded article 1 in Example 1.

[0122] Example 6 Example 6 was carried out under the same conditions as Example 1, except that molded article 5 was used instead of molded article 1 in Example 1. Example 7 Example 7 was carried out under the same conditions as Example 1, except that the gas introduced into the treatment nozzle in Example 1 was not air, but a mixed gas of 70% by volume oxygen and 30% by volume air at a flow rate of 45 L / min, plasma generated at room temperature and normal humidity was used, and the molded product was cut into strips of 45 mm x 10 mm and then degreased with acetone before being used.

[0123] Example 8 Example 8 was carried out under the same conditions as Example 1, except that the gas introduced into the treatment nozzle in Example 1 was not air, but a mixed gas of 70 volume % nitrogen and 30 volume % air at a flow rate of 45 L / min, plasma generated at room temperature and normal humidity was used, and the molded product was cut into strips of 45 mm x 10 mm and then degreased with acetone before being used.

[0124] Example 9 Example 9 was produced under the same conditions as Example 2, except that when molding the molded product 2, instead of placing "Aflex" (registered trademark) 25MW 1080NT on both surfaces of the laminate, "Frelease" (registered trademark) 65 manufactured by NEOS Corporation was diluted 5 times with distilled water and sprayed onto the surface of the mold of the press device, and the molded product was cut into strips of 45 mm x 10 mm and then degreased with acetone before being used.

[0125] Example 10 Example 10 was produced under the same conditions as Example 2, except that when molding the molded product 2, "Aflex" (registered trademark) 25MW 1080NT) was not placed on both surfaces of the laminate, but "Daifree" (registered trademark) GW-251 manufactured by Daikin Industries, Ltd. was diluted 5 times with distilled water and sprayed onto the surface of the mold of the press machine, and the molded product was cut into a 45 mm x 10 mm rectangular piece, which was then degreased with acetone before being used.

[0126] Example 11 Example 11 was carried out under the same conditions as Example 2, except that Adhesive 2, a two-component urethane adhesive LORD7545 manufactured by LORD, was used instead of Adhesive 1, and the molded product was cut into strips of 45 mm x 10 mm and then degreased with acetone before use.

[0127] Comparative Example 1 Comparative Example 1 was carried out under the same conditions as in Example 1, except that molded article 2 was used instead of molded article 1 in Example 1.

[0128] Comparative Example 2 Sixteen sheets of unidirectional carbon fiber prepregs (P3832S-20, manufactured by Toray Industries, Inc.) were laminated together with the fiber direction aligned, and polyvinyl alcohol films ("Poval" (registered trademark) film #4000, manufactured by Kuraray Co., Ltd.) were placed on both surfaces of this laminate. An attempt was made to obtain a molded product with an average thickness of 3 mm by press molding, but the polyvinyl alcohol film could not be peeled off from the molded product after press molding, making it impossible to prepare test pieces.

[0129] [Table 1]

[0130] [Table 2]

[0131] [Table 3] [Industrial Applicability]

[0132] The molded product of the carbon fiber composite material of the present invention has excellent adhesiveness and long-term adhesiveness stability compared to conventional carbon fiber composite materials, and is therefore particularly useful in the fields of automobiles, aircraft, and construction, which have parts that need to be joined to metals by adhesive. In particular, it is suitable for joining structures in which outer and inner members made of metal are joined in panel structures such as hoods and doors of automobile bodies. Furthermore, for example, by changing the resin composition combined with the carbon fiber, it is possible to freely adjust properties other than adhesiveness, which allows for a wide range of applications.

Claims

1. A molded article of a fiber-reinforced composite material comprising at least carbon fiber and a thermosetting resin composition, the molded article having a surface roughness Ra of 0.01 μm or more and 2 μm or less, and a tensile shear bond strength (F) when the molded article is bonded to a metal via an adhesive layer containing an epoxy compound having a thickness of 0.1 mm or more and 3 mm or less on the surface. 0 ) is 10 MPa or more and 40 MPa or less, and the surface free energy (γ TOTAL ) is 30 mJ / m 2 80mJ / m or more 2 The surface free energy (γ TOTAL ) which constitutes the surface free energy dispersion component (γ d ) and the polar component of the surface free energy (γ p ) and the ratio {γ p / γ d } is 0 or more and 1 or less.

2. 2. The molded product of claim 1, wherein the ratio of the number of fluorine (F) atoms to the number of carbon (C) atoms on the surface of the carbon fiber composite material, {F / C}, as measured by X-ray photoelectron spectroscopy, is 0 or more and 0.5 or less.

3. 3. The molded article of carbon fiber composite material according to claim 1, wherein the ratio of the number of oxygen (O) atoms to the number of carbon (C) atoms on the surface of the molded article, {O / C}, as measured by X-ray photoelectron spectroscopy, is 0.2 or more and 1.2 or less.

4. 4. The molded article of any one of claims 1 to 3, wherein in narrow scan C1s peak division measured on the surface of the molded article by X-ray photoelectron spectroscopy, the intensity ratio {X / M} of the peaks (X) assigned to C-O and C-N to the main peak (M) is 0.4 or more and 0.8 or less.

5. 5. A molded article of a carbon fiber composite material according to claim 1, wherein in narrow scan C1s peak division measured on the surface of the molded article by X-ray photoelectron spectroscopy, the intensity ratio {Y / M} of the peak (Y) assigned to C=O to the main peak (M) is 0.1 or more and 0.3 or less.

6. 6. A molded article of a carbon fiber composite material according to any one of claims 1 to 5, wherein in narrow scan C1s peak division measured on the surface of the molded article by X-ray photoelectron spectroscopy, the intensity ratio {Z / M} of the peak (Z) assigned to C(=O)-O to the main peak (M) is 0.1 or more and 0.3 or less.

7. 7. The molded product of any one of claims 1 to 6, wherein the carbon fibers contained in the molded product have an average diameter of 1 to 20 μm and an average length of 10 mm or more, and the carbon fiber content in the carbon fiber composite material is 5 to 75 volume %.

8. The molded product of the carbon fiber composite material according to any one of claims 1 to 7, wherein the resin composition contained in the molded product of the carbon fiber composite material is a thermosetting resin composition containing an epoxy resin.

9. Tensile shear bond strength (F 0 ) and the tensile shear bond strength (F 11 ) ratio {F 11 / F 0 9. The carbon fiber composite material according to claim 1, wherein the value of} is 0.75 or more and 1 or less.

10. 10. A method for producing a molded product of a carbon fiber composite material according to any one of claims 1 to 9, comprising molding a carbon fiber composite material, the method being characterized in that a release agent containing elemental fluorine or a release film containing elemental fluorine is used in press molding.

11. 11. A method for producing a molded article of a carbon fiber composite material according to claim 10, further comprising the step of plasma-treating the surface of the carbon fiber composite material after the press molding.

Citation Information

Patent Citations

  • Self-adhesive tape

    JP1996319462A

  • Production of fiber formed product

    JP1997316763A

  • Printed wiring board and manufacturing method therefor

    JP2002176266A

  • Method for adhesion of thermosetting resin-molded products

    JP2003221458A

  • Release film

    JP2003334903A