Manufacturing method and manufacturing equipment for membrane-catalyst assembly
By applying a liquid to the electrolyte membrane surface before bonding and using controlled thermocompression, the method addresses the challenge of achieving adequate adhesion and productivity in membrane-catalyst assembly manufacturing, resulting in a high-quality assembly with improved gas diffusivity and reduced costs.
Patent Information
- Application Number
- JP2021512598
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-23
- Filing Date
- 2020-12-21
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-12-21
AI Technical Summary
Existing methods for manufacturing a membrane-catalyst assembly in polymer electrolyte fuel cells face challenges in achieving adequate adhesion between the electrolyte membrane and catalyst layer while maintaining high productivity, as they often require harsh thermocompression bonding conditions that can damage the membrane or result in poor gas diffusivity and increased costs.
A method involving the application of a liquid, preferably water, to the surface of the electrolyte membrane before bonding, followed by thermocompression, which expels air and softens the membrane to improve adhesion, while using controlled conditions to prevent swelling and maintain shape, allowing for high productivity.
The method enhances adhesion between the electrolyte membrane and catalyst layer while reducing the risk of damage and maintaining productivity, resulting in a high-quality membrane-catalyst assembly with improved gas diffusivity and reduced production costs.
Smart Images

Figure 0007586072000004 
Figure 0007586072000005 
Figure 0007586072000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method and apparatus for producing a membrane-catalyst assembly, which is a member formed by bonding a polymer electrolyte membrane and a catalyst layer and is used in electrochemical devices such as solid polymer fuel cells. [Background technology]
[0002] Fuel cells are a type of power generation device that extracts electrical energy by electrochemically oxidizing fuels such as hydrogen and methanol, and have been attracting attention in recent years as a clean energy supply source. Among them, solid polymer fuel cells have a low standard operating temperature of around 100°C and a high energy density, and are therefore expected to be used in a wide range of applications as power generation devices for relatively small-scale distributed power generation facilities and mobile vehicles such as automobiles and ships. The polymer electrolyte membrane (hereinafter sometimes simply referred to as the "electrolyte membrane") is the key material of solid polymer fuel cells, and in recent years, further research has been conducted into their application to hydrogen infrastructure-related equipment such as solid polymer electrolyte membrane water electrolysis devices and electrochemical hydrogen pumps.
[0003] When applying a polymer electrolyte membrane to such electrochemical devices, a member in which an electrolyte membrane and a catalyst layer are bonded is used. A representative example of such a member is a catalyst-coated electrolyte membrane in which a catalyst layer is formed on the surface of an electrolyte membrane.
[0004] The following method is known as a method for manufacturing an electrolyte membrane with a catalyst layer. First, a sheet of polytetrafluoroethylene (PTFE) or the like with excellent releasability is used as a temporary substrate, and a catalyst solution is applied to the surface of this sheet. Then, the solvent in the applied catalyst solution is evaporated to form a dried catalyst layer. Furthermore, this dried catalyst layer and the electrolyte membrane are thermocompressed using a surface press or a roll press to transfer the catalyst layer to the polymer electrolyte membrane. Finally, the temporary substrate is peeled off from the catalyst layer transferred to the polymer electrolyte membrane. The reason for adopting this method of once drying the catalyst layer and then transferring it to the electrolyte membrane is that if the solvent in the catalyst solution adheres to the electrolyte membrane, the electrolyte membrane will swell and wrinkle, causing it to lose its shape.
[0005] However, when a dry catalyst layer is thermocompressed to an electrolyte membrane, the adhesion between the catalyst layer and the electrolyte membrane may be insufficient unless the catalyst layer is pressed at high temperature and high pressure for a long time. On the other hand, if harsh thermocompression conditions are applied to improve the adhesion between the catalyst layer and the electrolyte membrane, the catalyst layer may be compressed and deformed, which may reduce gas diffusion and prevent good power generation performance, or the electrolyte membrane may be damaged by thermal stress and its durability may be reduced. On the other hand, simply lowering the temperature and pressure of the press to reduce damage to the catalyst layer and electrolyte membrane requires an increased pressing time, which significantly reduces productivity.
[0006] Therefore, various techniques have been proposed to realize good adhesion between the electrolyte membrane and the catalyst layer while mitigating the thermocompression bonding conditions. [Prior art documents] [Patent documents]
[0007] For example, proposed methods include a method in which a catalyst solution is semi-dried and a small amount of solvent component remains in the catalyst layer before bonding it to an electrolyte membrane (Patent Document 1); a method in which a solution containing a binder resin having proton conductivity is applied to the surface of a dried catalyst layer and then the catalyst layer is bonded to the electrolyte membrane before the solution is completely dried (Patent Document 2); and a method in which a laminate including an electrolyte membrane and a catalyst layer is pressure-bonded while immersed in a liquid (Patent Document 3). [Patent Document 1] Patent No. 4240272 specification [Patent Document 2] JP 2013-69535 A [Patent Document 3] JP 2009-140652 A Summary of the Invention [Problem to be solved by the invention]
[0008] According to the method described in Patent Document 1, by leaving a solvent component in the catalyst layer to the extent that only the bonding surface of the electrolyte membrane with the catalyst layer can be softened, wrinkles are not generated in the electrolyte membrane, and the adhesion between the electrolyte membrane and the catalyst layer can be improved under relaxed thermocompression conditions. However, it is difficult to control the drying so that the amount of remaining solvent is uniform over the entire surface of the catalyst layer while partially removing the solvent in the catalyst solution by heating, and there is a problem that the quality is unstable because there are mixtures of catalyst layers with high interfacial resistance between the electrolyte membrane and the catalyst layer, wrinkles due to deformation of the electrolyte membrane, and cracks on the catalyst layer surface due to differences in the drying state within the catalyst layer. In addition, there is a problem that the margin for the amount of remaining solvent is narrow, which leads to increased costs due to reduced productivity. Furthermore, there is a restriction on the solvent composition of the catalyst solution, so it is difficult to flexibly respond to changes in the type of catalyst layer.
[0009] According to the method described in Patent Document 2, a solution of a binder resin having proton conductivity is applied to the joining surface of the catalyst layer with the electrolyte membrane, and the catalyst layer is joined before the solution dries completely, so that the solution acts as an adhesive, and the adhesion between the electrolyte membrane and the catalyst layer can be improved even at low temperature and low pressure. However, the use of a solution of a binder resin having proton conductivity to join the electrolyte membrane and the catalyst layer leads to an increase in manufacturing costs. Furthermore, there are problems in that the binder resin is the same component as the electrolyte membrane, and the thickness of the electrolyte membrane increases substantially, resulting in an increase in electrical resistance, and that the organic solvent in the solution remains at the interface between the electrolyte membrane and the catalyst layer, which may cause a decrease in power generation performance.
[0010] According to the method described in Patent Document 3, the bonding process involves pressing the bonded bodies including the electrolyte membrane and the bonded bodies including the catalyst layer while immersed in a liquid, and the electrolyte in the electrolyte membrane and the catalyst layer absorbs the liquid sufficiently, and is pressed in a softened state, penetrating into the unevenness of the bonding surfaces of the bonding counterparts, the catalyst layer and the gas diffusion layer, to obtain strong bonding, and the bonding between the layers constituting the membrane-electrode bond can be improved without increasing the temperature or pressure during pressing. However, since the entire members other than the interface involved in the bonding are immersed in the liquid, it is difficult to suppress swelling of the electrolyte membrane and maintain its shape. Furthermore, since the deformation behavior of each member due to drying after bonding is different, it is difficult to obtain a uniform and flat bonded body, and there is also a problem that it is difficult to improve productivity by continuous processing using a roll-shaped long member.
[0011] An object of the present invention is to provide a method for producing a member in which a polymer electrolyte membrane and a catalyst layer are bonded together (hereinafter referred to as a "membrane-catalyst assembly"), which can achieve both relaxation of thermocompression bonding conditions (pressing pressure, pressing temperature, pressing time) and improvement of adhesion between the catalyst layer and the electrolyte membrane with high productivity. [Means for solving the problem]
[0012] In order to solve the above problems, the method for producing a membrane-catalyst assembly of the present invention has the following features: This is a manufacturing method for a membrane-catalyst assembly in which a catalyst layer is bonded to an electrolyte membrane, the manufacturing method for the membrane-catalyst assembly comprising: a liquid application step of applying a liquid under atmospheric conditions only to the surface of the electrolyte membrane before bonding; and a thermocompression bonding step of bonding the electrolyte membrane to which the liquid has been applied and the catalyst layer by thermocompression bonding.
[0013] The apparatus for producing a membrane-catalyst assembly of the present invention has the following configuration: An apparatus for producing a membrane-catalyst assembly in which a catalyst layer is bonded to an electrolyte membrane, comprising: A liquid applying means for applying a liquid only to the surface of the electrolyte membrane before bonding in an atmospheric environment; a thermocompression bonding means for bonding the electrolyte membrane to which the liquid has been applied and the catalyst layer by thermocompression bonding; The present invention relates to a manufacturing apparatus for a membrane-catalyst assembly having the above structure.
[0014] In the method for producing a membrane-catalyst assembly of the present invention, it is preferable that the electrolyte membrane before bonding has a support on a surface different from the surface to which a liquid is applied.
[0015] In the method for producing a membrane-catalyst assembly of the present invention, the liquid applied in the liquid application step is preferably a liquid containing water.
[0016] In the method for producing a membrane-catalyst assembly of the present invention, the water content in the water-containing liquid is preferably 90 mass % or more and 100 mass % or less.
[0017] In the method for producing a membrane-catalyst assembly of the present invention, the liquid applied in the liquid application step is preferably pure water.
[0018] In the method for producing a membrane-catalyst assembly of the present invention, it is preferable that in the liquid applying step, the liquid is applied in the form of droplets only onto the surface of the electrolyte membrane.
[0019] In the method for producing a membrane-catalyst assembly of the present invention, it is preferable that in the liquid applying step, the liquid is applied by spraying.
[0020] In the method for producing a membrane-catalyst assembly of the present invention, in the liquid application step, the amount of the liquid in the thermocompression bonding step is set to 1 cm 2 on the surface of the electrolyte membrane. 2 It is preferable that the volume is 0.1 μL or more and 5 μL or less per unit area.
[0021] In the method for producing a membrane-catalyst assembly of the present invention, it is preferable to use a hydrocarbon-based electrolyte membrane as the electrolyte membrane.
[0022] The method for producing a membrane-catalyst assembly of the present invention preferably includes bonding a catalyst layer to the surface of the electrolyte membrane by any one of the methods described above.
[0023] In the method for producing a membrane-catalyst assembly of the present invention, the catalyst layer is supported by a substrate before being bonded to the electrolyte membrane, and the substrate is preferably air-permeable.
[0024] The method for producing a membrane-catalyst assembly of the present invention preferably comprises the steps of applying a catalyst solution to one surface of an electrolyte membrane and drying the solution to form a first catalyst layer, and joining a catalyst to the other surface of the electrolyte membrane by any of the methods described above to form a second catalyst layer.
[0025] It is preferable that the method for producing a membrane-catalyst assembly of the present invention further comprises a step of covering the first catalyst layer with a cover film, and that the step of forming the second catalyst layer is carried out in a state in which the first catalyst layer is covered with the cover film.
[0026] In the apparatus for producing a membrane-catalyst assembly of the present invention, the liquid applying means is preferably a means for applying the liquid in the form of droplets only onto the surface of the electrolyte membrane.
[0027] In the apparatus for producing a membrane-catalyst assembly of the present invention, the liquid applying means is preferably a spray. Effect of the Invention
[0028] According to the present invention, it is possible to manufacture a membrane-catalyst layer assembly while achieving both relaxation of thermocompression bonding conditions (pressing pressure, pressing temperature, pressing time) and improvement of adhesion between the catalyst layer and the electrolyte membrane with high productivity. [Brief description of the drawings]
[0029] [Figure 1] 1 is a side view showing a schematic configuration of a first embodiment of a membrane-catalyst assembly manufacturing apparatus of the present invention. [Diagram 2] 1 is a side view showing a schematic configuration of a second embodiment of a membrane-catalyst assembly manufacturing apparatus according to the present invention. [Diagram 3] FIG. 11 is a side view showing a schematic configuration for forming a first catalyst layer in a third embodiment of the membrane-catalyst assembly manufacturing apparatus of the present invention. [Figure 4]FIG. 11 is a side view showing a schematic configuration for forming a second catalyst layer in a third embodiment of the membrane-catalyst assembly manufacturing apparatus of the present invention. [Diagram 5] FIG. 13 is a side view showing a schematic configuration for forming a first catalyst layer in a fourth embodiment of the membrane-catalyst assembly manufacturing apparatus of the present invention. [Figure 6] FIG. 13 is a side view showing a schematic configuration for forming a second catalyst layer in a fourth embodiment of the membrane-catalyst assembly manufacturing apparatus of the present invention. [Figure 7] FIG. 2 is a side view showing a schematic configuration for explaining a different method for peeling off a temporary substrate in the first embodiment of the membrane-catalyst assembly manufacturing apparatus of the present invention. [Figure 8] 1 is a side view showing a schematic configuration for explaining a heat shield plate in a first embodiment of a membrane-catalyst assembly manufacturing apparatus of the present invention.
[0023] FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] Although the present invention is not limited to the above, the following is considered as the function of the present invention. In the thermocompression bonding process, the electrolyte membrane and the catalyst layer are pressed together while a liquid is applied to the bonding surface of the catalyst layer with the electrolyte membrane, so that the air present at the interface is expelled and only the liquid exists between the electrolyte membrane and the catalyst layer. In this state, the liquid is evaporated and the interface is evacuated, improving the adhesion between the catalyst layer and the electrolyte membrane. Furthermore, the liquid is forced into the electrolyte membrane by the pressure and penetrates into it, softening the electrolyte membrane, thereby further improving the adhesion between the two. The electrolyte membrane is held by the pressure during thermocompression bonding immediately after the liquid penetrates, so that swelling can be prevented. The liquid evaporated at the interface is discharged to the outside of the membrane-catalyst assembly by passing through the pores of the catalyst layer having a porous structure.
[0031] In this specification, the term "membrane-catalyst assembly" refers not only to a so-called electrolyte membrane with a catalyst layer formed on the surface of the electrolyte membrane, but also to a laminate having a bonding surface between the electrolyte membrane and the catalyst layer. For example, a membrane-electrode assembly in which a so-called gas diffusion electrode formed with a catalyst layer on one side of a substrate made of gas-permeable carbon paper or the like and an electrolyte membrane are bonded is also an embodiment of the "membrane-catalyst assembly". In addition, the "manufacture of the membrane-catalyst assembly" also includes an operation of bonding a catalyst layer (only the catalyst layer, or the gas diffusion electrode, etc.) to the other side of the electrolyte membrane in a state in which a catalyst layer has already been formed on one side of the electrolyte membrane. As a method for forming a catalyst layer on one side of the electrolyte membrane, for example, a method of directly applying the catalyst layer or a method of transferring the catalyst layer using a catalyst layer transfer sheet can be adopted.
[0032] [Electrolyte membrane] The electrolyte membrane to be used in the manufacturing method and manufacturing apparatus for the membrane-catalyst assembly of the present invention is not particularly limited as long as it has proton conductivity and operates as an electrolyte membrane for use in solid polymer fuel cells, solid polymer electrolyte membrane water electrolysis devices, electrochemical hydrogen pumps, etc., and known or commercially available electrolyte membranes can be used. As such an electrolyte membrane, a polymer electrolyte membrane is preferable, and for example, a fluorine-based electrolyte membrane made of perfluorosulfonic acid or a hydrocarbon-based electrolyte membrane made of a hydrocarbon polymer with proton conductivity imparted to a hydrocarbon skeleton can be used.
[0033] In particular, hydrocarbon-based electrolyte membranes have a higher glass transition temperature and are subject to greater shrinkage and deformation when heated than fluorine-based electrolyte membranes, so that it is often difficult to find transfer conditions that provide excellent productivity using conventional thermocompression bonding methods, and the manufacturing method and manufacturing apparatus of the present invention can be suitably applied to these membranes.
[0034] Furthermore, as the electrolyte membrane, a composite electrolyte membrane in which a polymer electrolyte and a porous substrate are composited can be used.
[0035] [Composite electrolyte membrane] The composite electrolyte membrane is a composite of a polymer electrolyte and a porous substrate, and can be obtained, for example, by filling (impregnating) a porous substrate with a polymer electrolyte. Examples of the porous substrate include a hydrocarbon-based porous substrate mainly composed of a hydrocarbon-based polymer compound, and a fluorine-based porous substrate mainly composed of a fluorine-based polymer compound.
[0036] Examples of the hydrocarbon polymer compound include polyethylene (PE), polypropylene (PP), polystyrene (PS), polyacrylate, polymethacrylate, polyvinyl chloride (PVC), polyvinylidene chloride (PVdC), polyester, polycarbonate (PC), polysulfone (PSU), polyethersulfone (PES), polyphenylene oxide (PPO), polyarylene ether polymer, polyphenylene sulfide (PPS), polyphenylene sulfide sulfone, polyparaphenylene (PPP), polyarylene polymer, polyarylene ketone, polyether ketone (PEK), polyarylene phosphine oxide, polyether phosphine oxide, polybenzoxazole (PBO), polybenzothiazole (PBT), polybenzimidazole (PBI), polyamide (PA), polyimide (PI), polyetherimide (PEI), and polyimide sulfone (PIS).
[0037] Examples of fluorine-based polymer compounds include polytetrafluoroethylene (PTFE), polyhexafluoropropylene, tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-tetrafluoroethylene copolymer (ETFE), polyvinylidene fluoride (PVdF), polychlorotrifluoroethylene (PCTFE), perfluoroalkoxy fluorine resin (PFA), and ethylene-chlorotrifluoroethylene copolymer (ECTFE).
[0038] From the viewpoints of water resistance, chemical resistance, and mechanical properties, PE, PP, PPS, PEK, PBI, PTFE, polyhexafluoropropylene, FEP, and PFA are preferred, and further from the viewpoint of chemical resistance and chemical durability, PTFE, polyhexafluoropropylene, FEP, and PFA are more preferred, with PTFE being particularly preferred since it has high mechanical strength due to molecular orientation.
[0039] The composite electrolyte membrane is particularly preferably a composite of a hydrocarbon electrolyte and a fluorine-based porous substrate. In this case, by adding a nonionic fluorine-based surfactant to the hydrocarbon electrolyte solution during the composite formation, the fluorine-based porous substrate can be easily filled (impregnated) with the hydrocarbon electrolyte with high efficiency without gaps.
[0040] The composite electrolyte membrane can be produced, for example, by impregnating a porous substrate with a polymer electrolyte solution, and then drying the substrate to remove the solvent contained in the polymer electrolyte solution. Examples of the impregnation method include the following methods.
[0041] (1) A method of controlling the membrane thickness by removing excess solution while pulling up a porous substrate immersed in a polymer electrolyte solution; (2) A method of casting a polymer electrolyte solution onto a porous substrate, (3) A method in which a porous substrate is attached onto a polymer electrolyte solution cast onto a supporting substrate, and the substrate is impregnated with the polymer electrolyte solution.
[0042] [Catalyst layer] The catalyst layer to be used in the manufacturing method and manufacturing apparatus for the membrane-catalyst assembly of the present invention is not particularly limited as long as it operates as a catalyst layer for use in a solid polymer fuel cell, a solid polymer electrolyte membrane water electrolysis device, an electrochemical hydrogen pump, etc. In general, a catalyst layer having a porous structure composed of conductive particles such as carbon particles, catalyst particles such as platinum particles or platinum alloy particles supported on the conductive particles, and an electrolyte component such as an ionomer having proton conductivity can be used.
[0043] As an example, suitable conductive particles include oil furnace black, gas furnace black, acetylene black, thermal black, graphite, carbon nanotubes, graphene, and other carbons, metal oxides such as tin oxide and titanium oxide, etc. Suitable catalyst particles include platinum, iridium, ruthenium, rhodium, palladium, and other noble metals, alloys of platinum with manganese, iron, cobalt, nickel, copper, zinc, and other metals, ternary alloys of platinum and ruthenium, iridium oxide, and the like. Suitable electrolyte components include perfluorocarbon sulfonic acid polymers such as "Nafion" (registered trademark, manufactured by Chemours), "Aquivion" (registered trademark, manufactured by Solvay), "Flemion" (registered trademark, manufactured by Asahi Glass Co., Ltd.), "Aciplex" (registered trademark, manufactured by Asahi Kasei Corporation), and "Fumion" F (registered trademark, manufactured by FuMA-Tech), as well as hydrocarbon polymers such as polysulfone sulfonic acid, polyaryl ether ketone sulfonic acid, polybenzimidazole alkyl sulfonic acid, polybenzimidazole alkyl phosphonic acid, polystyrene sulfonic acid, polyether ether ketone sulfonic acid, and polyphenyl sulfonic acid.
[0044] The catalyst solution is a dispersion of the catalyst layer material in a solvent that evaporates by drying, and is not particularly limited as long as it is sufficient to form a catalyst layer on the electrolyte membrane. In general, the solvent is preferably water, alcohol such as methanol, ethanol, 1-propanol, 2-propanol, tert-butanol, ethylene glycol, N,N-dimethylformamide, N-methyl-2-pyrrolidone, or the like.
[0045] [Liquid application step] The liquid application step is a step of applying a liquid to the surface of the electrolyte membrane before bonding, i.e., the bonding surface with the catalyst layer. Applying a liquid means forming a state in which the liquid is exposed and attached to the surface of the electrolyte membrane. At this time, the liquid application is performed in an air atmosphere in order to minimize the penetration of the liquid into the electrolyte membrane until the thermocompression bonding step. This is because if a large amount of liquid penetrates into the electrolyte membrane, it may swell and lose its shape.
[0046] In the liquid application process, the liquid is applied only to the surface of the electrolyte membrane in an atmospheric environment. By applying the liquid only to the surface of the electrolyte membrane, the number of process control parameters is reduced compared to applying the liquid to both the electrolyte membrane and the catalyst layer, which has the advantages of stabilizing the manufacturing conditions and making it easier to control and manage the amount of liquid applied to the bonding surface, as well as suppressing the variation in the amount of liquid on the bonding surface caused by droplets coming into contact with each other before the thermocompression bonding process.
[0047] Moreover, by applying the liquid under an atmospheric environment, it is possible to apply the liquid only to the surface of the electrolyte membrane, and it is possible to suppress the penetration of the liquid into the electrolyte membrane. By suppressing the penetration of the liquid into the electrolyte membrane, the shape of the electrolyte membrane is prevented from being distorted. Furthermore, since the liquid that has penetrated into the electrolyte membrane does not contribute to improving the adhesion at the interface, and rather increases the energy consumption for evaporating the liquid, suppressing the penetration of the liquid into the electrolyte membrane is also effective in terms of manufacturing costs.
[0048] In addition, in the liquid application step, by previously supporting the electrolyte membrane on a support on the surface of the electrolyte membrane other than the surface on which the liquid is applied, swelling of the electrolyte membrane in the liquid application step can be further reduced. As such a support, a support that is used during the production of the electrolyte membrane and on which the electrolyte membrane is previously supported, a support that is newly applied to the surface of the electrolyte membrane other than the surface on which the liquid is applied, or a support that is newly applied via a catalyst layer formed on one surface of the electrolyte membrane, can be used. However, the method of applying the support is not particularly limited as long as it does not interfere with the production of the membrane-catalyst assembly of the present invention. The material of the support may be a film made of a general-purpose plastic such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate, polyethylene naphthalate (PEN), polybutylene naphthalate, polycarbonate (PC), polyphenylene ether, polyethersulfone, polyarylate, polyetherimide, polyamideimide, polyetheretherketone, polyphenylene sulfide (PPS), aromatic polyimide, or aromatic hydrocarbon polymer; a porous film made of these materials; or a film made of a combination of multiple materials, such as having an adhesive layer on one side of these films; however, the material is not particularly limited as long as it has a suitable thickness, flexibility, strength, etc. that contributes to good processability in each process.
[0049] In the liquid application process, the liquid is not particularly limited as long as it is a material that evaporates by heating in the subsequent thermocompression bonding process and is not toxic to the electrolyte membrane and the catalyst layer. For example, water, alcohols such as methanol, ethanol, 1-propanol, 2-propanol, tert-butanol, and mixtures thereof can be used, but it is preferable to use a liquid containing at least water. If the liquid undergoes a sudden temperature change during thermocompression bonding, wrinkles may occur in the electrolyte membrane, but since water has a higher boiling point and specific heat than the above alcohols and the temperature rise during thermocompression bonding is gradual, such damage can be suppressed if the liquid contains water. In addition, since water has a lower permeability into the electrolyte membrane than alcohol, it is possible to prevent the electrolyte membrane from deforming due to the liquid permeating into the electrolyte membrane. Furthermore, by using a liquid containing water, the present invention can be implemented at low cost, and the environmental burden during production can be reduced. Note that even if liquid remains in the membrane-catalyst assembly bonded by the manufacturing method and manufacturing apparatus of the present invention, if it is water, it will not affect the performance of the device using it. The water content of the water-containing liquid is more preferably 50% by mass to 100% by mass, even more preferably 90% by mass to 100% by mass, and even more preferably 100% by mass. In other words, it is most preferable to use pure water as the liquid. Here, pure water refers to high-purity water that does not contain impurities, and refers to water of JIS K 0557 (1998) A4 level obtained by a commercially available pure water production device in which water is collected through a reverse osmosis membrane and an ion exchange resin, or water of equivalent quality.
[0050] The liquid may contain solid materials in a dissolved or dispersed state, so long as the liquid as a whole has fluidity and the effects of the present invention can be obtained.
[0051] In the liquid application step, the method of applying the liquid is not particularly limited, and examples of the method include a method of forming a uniform coating film on the electrolyte membrane surface using a gravure coater, die coater, comma coater, etc., and a method of applying the liquid to the electrolyte membrane surface in the form of droplets. The method of applying the liquid to the electrolyte membrane surface in the form of droplets is particularly preferred. Here, the droplet form refers to a state in which countless droplets are attached to the electrolyte membrane surface. The droplets are liquid masses that are held together by surface tension and have a size of 1 cm on the electrolyte membrane. 2 If the liquid is applied in droplet form, it is possible to apply a small amount of liquid, the minimum amount necessary to soften the electrolyte membrane, uniformly to the joining surface. 2 This means that the total amount of liquid applied around the electrolyte membrane is the same at each position. Even liquids such as water, which are easily repelled by the electrolyte membrane and difficult to form a uniform coating film, can be easily applied in droplet form. Furthermore, since the contact area with the electrolyte membrane is small in droplet form, it is possible to minimize the penetration of the liquid into the electrolyte membrane until it is thermocompressed. In addition, the pressure applied during the thermocompression process spreads the droplets at the interface and bonds with the surrounding droplets, making it possible to soften the electrolyte membrane on all surfaces of the interface.
[0052] In the liquid application process, the amount of liquid at the start of the thermocompression process is set to 1 cm per 1 cm of the electrolyte membrane surface. 2 It is preferable to apply liquid in an amount of 0.1 μL to 5 μL per cm of the electrolyte membrane. When the amount of liquid in the thermocompression bonding step is within the above-mentioned preferred range, the electrolyte membrane can be sufficiently softened, adhesion is sufficient, and there is no risk of the electrolyte membrane being left unsoftened in parts due to partial liquid droplets not bonding when pressed in the thermocompression bonding step, while no liquid drips during transportation, and since almost the entire amount of liquid evaporates due to heating during thermocompression bonding, there is no risk of the electrolyte membrane swelling due to liquid remaining at the interface the moment the pressure is removed. It is more preferable that the amount of liquid is within the above-mentioned preferred range. 2The amount of liquid is 0.1 μL to 0.8 μL per cm. A sample piece of a PET film or the like whose weight has been measured is attached to the surface of the electrolyte membrane so as to be laminated with the electrolyte membrane, and after the liquid is applied in the liquid application step, the liquid-attached sample piece is taken out immediately before the sample piece and the catalyst layer come into contact in the thermocompression bonding step, and its weight is measured. The difference in weight is used to determine the amount of liquid per cm. 2 The size of the sample can be measured by calculating the volume of liquid around the sample. The size of the sample can be a square with sides of 1 to 10 cm.
[0053] In addition, the smaller the average diameter of the applied droplets, the more preferable, specifically, the smaller the diameter of the droplets when attached to the electrolyte membrane surface is, since the distance between the droplets can be shortened as the average diameter is smaller, the droplets can be bonded with a smaller amount of liquid when pressed in the thermocompression bonding process.
[0054] In the liquid application step, the means for applying the liquid in the form of droplets is not particularly limited, and may include a method of spraying droplets by a spray or inkjet, a method of condensing droplets on the joining surface in a humid atmosphere, a method of spraying a mist of liquid by an ultrasonic vibrator, etc., but a method of spraying droplets by a spray is preferred in that the liquid can be applied efficiently while controlling the amount of liquid. In addition, the spray for spraying droplets is not particularly limited, and may include a two-fluid spray nozzle that atomizes and sprays the liquid by compressed air.
[0055] When using the above-mentioned means for applying liquid in the form of droplets, it is preferable to surround the liquid applying means such as a spray nozzle with a chamber in order to prevent the droplets from scattering around. In addition, although it is not necessary to reduce the pressure inside the chamber, it is preferable to reduce the pressure slightly to a negative pressure relative to atmospheric pressure, since this prevents the droplets from scattering around from the gap between the chamber and the electrolyte membrane.
[0056] [Thermocompression bonding process] The electrolyte membrane that has been through the liquid application step is then subjected to a thermocompression bonding step in which it is thermocompressed to a catalyst layer. The thermocompression bonding step is a step in which the electrolyte membrane and the catalyst layer are bonded to each other by heating and clamping while in a laminated state in which the surface of the electrolyte membrane to which the liquid has been applied is in contact with the catalyst layer.
[0057] The heating temperature in the thermocompression bonding process is not particularly limited, but is preferably from the boiling point of the liquid applied to the electrolyte membrane (hereinafter referred to as the "liquid boiling point") to 220°C. The heating temperature is the maximum temperature reached at the bonding surface of the electrolyte membrane and the catalyst layer during the thermocompression bonding process, and a thermocouple can be used for measurement. When the heating temperature is in the above-mentioned preferred range, it does not take much time for the liquid to evaporate, resulting in excellent productivity, while there is no risk of the electrolyte membrane being damaged by heat. The heating temperature in the thermocompression bonding process is more preferably from the liquid boiling point to 160°C. The liquid boiling point is the boiling point when the external pressure is 1 atmosphere, and when the evaporated liquid is a single composition, it means the boiling point of the liquid, and when it is a mixture, it means the value of the component of the mixture with the highest boiling point as a single component.
[0058] The pressure applied to the electrolyte membrane and catalyst layer in the thermocompression bonding process can be set as appropriate, but is preferably 1 MPa or more and 20 MPa or less. In the above preferred range, the electrolyte membrane and catalyst layer can be sufficiently adhered to each other, while excessive pressure is not applied to the catalyst layer and electrolyte membrane, so that the structure of the catalyst layer is not destroyed, mechanical damage to the electrolyte membrane is not large, and there is no risk of a decrease in durability or power generation performance. The pressure in the thermocompression bonding process is more preferably 1 MPa to 10 MPa.
[0059] The pressing form in the thermocompression step is not particularly limited, and may be a line contact form in which the electrolyte membrane and the catalyst layer are in contact in a single line, as in the case of a hot press roll, or a surface contact form in which the electrolyte membrane and the catalyst layer are in contact in a planar manner with a width in the transport direction, as in the case of a double belt press mechanism.
[0060] [Roll-to-roll manufacturing method] The method for producing the membrane-catalyst assembly of the present invention is preferably carried out by a roll-to-roll system, that is, a liquid application step and a thermocompression bonding step are carried out continuously by the roll-to-roll system.
[0061] The roll-to-roll manufacturing method is a manufacturing method in which, for example, a long-roll electrolyte membrane and a long-roll catalyst layer (catalyst layer transfer sheet or gas diffusion electrode) are continuously unwound and transported, and the membrane-catalyst assembly obtained by carrying out a liquid application step and a heat-press bonding step is wound into a roll.
[0062] The manufacturing apparatus for a membrane-catalyst assembly, which will be described later, is an example of a manufacturing apparatus capable of implementing a roll-to-roll manufacturing method.
[0063] The above is an explanation of the manufacturing method of the present invention, but as will be easily understood from the above explanation and the description of the embodiments below, this specification also discloses a manufacturing apparatus as described below for carrying out the manufacturing method. (1) A manufacturing apparatus for a membrane-catalyst assembly in which a catalyst layer is bonded to an electrolyte membrane, the manufacturing apparatus for a membrane-catalyst assembly comprising: a liquid applying means for applying a liquid only to the surface of the electrolyte membrane before bonding in an atmospheric environment; and a thermocompression bonding means for bonding the electrolyte membrane to which the liquid has been applied and the catalyst layer by thermocompression bonding; (2) The apparatus for producing a membrane-catalyst assembly according to (1), wherein the liquid supplying means is a means for supplying the liquid in droplets only onto the surface of the electrolyte membrane. (3) The apparatus for producing a membrane-catalyst assembly according to (2), wherein the liquid applying means is a spray.
[0064] Hereinafter, specific embodiments of the present invention will be described with reference to schematic diagrams of a manufacturing apparatus for implementing the manufacturing method of the present invention. Note that the following description is provided to facilitate understanding of the present invention and does not limit the present invention in any way, but as will be easily understood by those skilled in the art, references to preferred aspects and modifications of aspects in each embodiment can be interpreted as descriptions of the manufacturing method or manufacturing apparatus of the present invention as a higher-level concept. Note that in this specification, for convenience, the top of each drawing is described as "upper" and the bottom as "lower," but the up-down direction of each drawing is not necessarily limited to the vertical direction relative to the ground.
[0065] [First embodiment: Production of membrane-catalyst assembly (catalyst-layered electrolyte membrane) 1] FIG. 1 is a side view showing a schematic configuration of an apparatus for producing a catalyst-layered electrolyte membrane, which is one embodiment of the membrane-catalyst assembly production apparatus of the present invention.
[0066] In the membrane / catalyst assembly manufacturing apparatus 100 according to this embodiment, a catalyst-layered electrolyte membrane is manufactured as follows.
[0067] The electrolyte membrane 10 is unwound from the electrolyte membrane supply roll 11 and supplied to the thermocompression bonding section P through the guide roll 12. Above and below the unwound electrolyte membrane 10, catalyst layer transfer sheet supply rolls 21A and 21B are provided, respectively. The catalyst layer bonded to the upper surface of the electrolyte membrane 10 is formed using the catalyst layer transfer sheet 20A. The catalyst layer transfer sheet 20A is prepared in advance by, for example, applying a catalyst solution to a sheet that will be a substrate, and is unwound from the catalyst layer transfer sheet supply roll 21A in a state in which the substrate supports the catalyst layer, and is transported in the order of the backup roll 31A and the guide roll 22A while each of them supports the substrate side opposite to the catalyst layer formation surface. Note that the substrate is also called a temporary substrate because it is peeled off after bonding the catalyst layer and the electrolyte membrane. The catalyst layer transfer sheet 20B for forming the catalyst layer formed on the lower surface of the electrolyte membrane 10 is unwound from the catalyst layer transfer sheet supply roll 21B, and is transported in the order of the backup roll 31B and the guide roll 22B while each of them supports the substrate side. In this manner, the catalyst layer transfer sheets 20A and 20B are supplied to the thermocompression bonding section P so that the surfaces on which the catalyst layers are formed face the electrolyte membrane 10.
[0068] The material of the substrate of the catalyst layer transfer sheets 20A and 20B is not particularly limited, and examples of the material that can be used include hydrocarbon-based plastic films such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyethylene (PE), polypropylene (PP), polyimide, and polyphenylene sulfide, and fluorine-based films such as perfluoroalkoxyalkane (PFA), polytetrafluoroethylene (PTFE), and ethylene tetrafluoroethylene copolymer (ETFE).
[0069] It is more preferable that the substrate has air permeability. Having air permeability means that the substrate has a property of being permeable to gas, for example, the substrate has pores that are connected in the thickness direction. By using a substrate having air permeability, the vapor of the liquid generated during thermocompression bonding can be effectively discharged even when the substrate is in a state where it is bonded to the catalyst layer. As the substrate having air permeability, for example, a porous body formed from the above-mentioned material can be used.
[0070] In order to remove wrinkles and slack in the electrolyte membrane 10 and catalyst layer transfer sheets 20A and 20B supplied to the thermocompression bonding section P, it is preferable to use expander rolls for the guide rolls 12, 22A, and 22B.
[0071] Although the membrane-catalyst assembly manufacturing apparatus 100 according to this embodiment is configured to transfer catalyst layers onto both sides of the electrolyte membrane 10, it may also be configured to transfer catalyst layers onto only one side of the electrolyte membrane 10.
[0072] In this embodiment, a spray nozzle 30A is provided between the guide roll 12 and the thermocompression bonding unit P. The spray nozzle 30A has an outlet facing the electrolyte membrane surface and is provided at a predetermined distance from the electrolyte membrane surface. Note that one or more spray nozzles 30A are provided in the width direction of the electrolyte membrane 10 depending on the width of the electrolyte membrane 10.
[0073] The spray nozzle 30A is supplied with water from a water supply tank (not shown), and discharges the supplied water from a discharge port to apply droplets to the bonding surface of the electrolyte membrane with the catalyst layer.
[0074] Furthermore, the spray nozzle 30A and the space S in which the droplets fly from the discharge port of the spray nozzle 30A to the electrolyte membrane are surrounded by a nozzle chamber 32A, and a pressure reduction tank 34A that reduces the pressure in the space S is connected to the nozzle chamber 32A by piping via a valve 33A that switches between pressure reduction. The pressure reduction tank 34A creates a negative pressure in the space S relative to the environmental pressure of the manufacturing apparatus, so that a small amount of outside air is sucked in through a gap between the nozzle chamber 32A and the electrolyte membrane 10, preventing excess droplets from the spray nozzle 30A from scattering around. The water that accumulates in the nozzle chamber 32A is discharged from a drain (not shown) provided in the nozzle chamber 32A and returned to a water supply tank for reuse.
[0075] Note that the above is an explanation of the means for applying liquid to the electrolyte membrane surface facing the catalyst layer transfer sheet 20A, but the means for applying liquid to the electrolyte membrane surface facing the catalyst layer transfer sheet 20B (spray nozzle 30B, nozzle chamber 32B, valve 33B, pressure reduction tank 34B) are also configured in the same way, so their explanation will be omitted.
[0076] The nozzle chambers 32A and 32B do not need to be depressurized, but a small reduction in pressure is preferable because it can prevent droplets from scattering to the surroundings. In this case, if the degree of reduction in pressure is too large, the amount of outside air sucked into the nozzle chambers 32A and 32B increases, which may disturb the air flow in the nozzle chambers 32A and 32B and reduce the accuracy of applying droplets. Therefore, the degree of reduction in pressure in the nozzle chambers 32A and 32B is, for example, appropriate in the range of up to -50.0 kPa with respect to the environmental pressure (atmospheric pressure) of the manufacturing apparatus, preferably up to -10.0 kPa, and more preferably up to -5.0 kPa.
[0077] In this way, the electrolyte membrane 10 with the liquid applied to the bonding surfaces of the catalyst layer transfer sheets 20A, 20B with the catalyst layers is supplied to the thermocompression bonding section P and passes between the heat press rolls 40A, 40B. As shown in Fig. 8, it is preferable to provide heat shields 41A, 41B between the catalyst layer transfer sheet 20A and the heat press roll 40A, and between the catalyst layer transfer sheet 20B and the heat press roll 40B, respectively. By providing the heat shields 41A, 41B, it is possible to prevent the liquid applied to the electrolyte membrane 10 from evaporating before the heat press due to the radiant heat radiated from the heat press rolls 40A, 40B.
[0078] The hot press rolls 40A, 40B are connected to a driving means (not shown) and can be rotated while controlling the speed. The hot press rolls 40A, 40B rotate at a constant speed while applying heat and pressure to the electrolyte membrane 10 and the catalyst layer transfer sheets 20A, 20B, and thus the catalyst layers are thermocompression-bonded to both sides of the electrolyte membrane 10 while the transport speeds of the electrolyte membrane 10 and the catalyst layer transfer sheets 20A, 20B are synchronously transported to form the membrane-catalyst layer assembly 13a. Note that illustrations of heating devices, pressure devices, etc. for the hot roll presses 40A, 40B are omitted.
[0079] The material of the heat press rolls 40A and 40B is not particularly limited, but it is preferable that one roll is made of a metal such as stainless steel, and the other roll is made of an elastic material such as a resin or elastomer material, typically rubber, coated on the surface. By making one of the heat press rolls 40A and 40B a metal, it is possible to sufficiently heat the electrolyte membrane and the catalyst layer, and by making the surface layer of the other press roll an elastic material, the press roll flexibly deforms with respect to the catalyst layer transfer sheets 20A and 20B, and good line contact is maintained, making it possible to uniformize the line pressure in the width direction of the substrate.
[0080] As the material of the elastic body, for example, when rubber is used, fluororubber, silicone rubber, EPDM (ethylene propylene diene rubber), neoprene, CSM (chlorosulfonated polyethylene rubber), urethane rubber, NBR (nitrile rubber), ebonite, etc. can be used. In addition, the rubber hardness of the elastic body is preferably in the range of 70 to 97° in Shore A standard. When the rubber hardness of the elastic body is in the above-mentioned preferable range, the deformation amount of the elastic body is appropriate, the clamping contact width with the catalyst layer transfer sheets 20A and 20B is not too large, and the pressure required for bonding the electrolyte membrane 10 and the catalyst layer can be secured, while the clamping contact width is not too small, and the clamping time required for bonding can be secured.
[0081] As a heating means for the hot press rolls 40A and 40B, various heaters, steam, oil, and other heat transfer media can be used, but are not particularly limited. The heating temperatures of the upper and lower rolls may be the same or different.
[0082] The method of controlling the clamping pressure of the hot press rolls 40A and 40B is not particularly limited, and the clamping pressure may be controlled using a pressure means such as a hydraulic cylinder, or a constant gap may be provided between the hot press rolls 40A and 40B by position control using a servo motor or the like, and the clamping pressure may be controlled according to the size of the gap.
[0083] In this embodiment, the heat press rolls 40A and 40B, which are a line contact mechanism, are used in the thermocompression bonding section P, but the present invention is not limited to this. A mechanism in which the electrolyte membrane 10 and the catalyst layer transfer sheets 20A and 20B are pressed by multiple line contacts using multiple rolls may be used, or a double belt press mechanism in which pressing is performed by surface contact may be used. When multiple sets of rolls are used, the number of rolls to be installed is not particularly limited, but 2 to 10 sets are preferable.
[0084] In this manner, the electrolyte membrane 10 passes through the thermocompression bonding section P, and the catalyst layers are transferred onto both sides of the electrolyte membrane 10, forming a membrane-catalyst assembly (electrolyte membrane with catalyst layer) 13a.
[0085] Next, the temporary substrates 24A and 24B are peeled off from the membrane-catalyst assembly 13a serving as a catalyst-layered electrolyte membrane.
[0086] When the temporary substrates 24A and 24B are breathable substrates, the peeling method is not particularly limited. For example, the temporary substrates 24A and 24B can be passed between the guide rolls 23A and 23B, and the temporary substrates 24A and 24B can be peeled off at this time. In addition, since the temporary substrate supports the electrolyte membrane via the catalyst layer while the temporary substrate is bonded, the effect of preventing swelling of the electrolyte membrane can be obtained. Therefore, when it is difficult to evaporate almost the entire amount of liquid only by the thermocompression bonding process, an additional drying process can be provided to dry the liquid between passing through the thermocompression bonding part P and peeling off the temporary substrate. The additional drying process can also serve as a heating process. The drying temperature (hot air temperature or surface temperature of the heating roll) is, for example, appropriate from 120°C to 250°C, and preferably from 150°C to 230°C. When the temporary substrates 24A and 24B are breathable substrates, it is preferable to peel off the temporary substrates 24A and 24B from the membrane-catalyst assembly 13a by holding the temporary substrate 24A and the temporary substrate 24B in the heat press roll 40A and the heat press roll 40B, respectively, as shown in FIG. 7. By peeling off the temporary substrate immediately after thermocompression bonding to expose the catalyst layer, the vapor of the liquid generated during the thermocompression bonding step can be effectively discharged.
[0087] The temporary substrates peeled off from the membrane-catalyst layer assembly 13a pass through guide rolls 23A and 23B, respectively, and are taken up by temporary substrate take-up rolls 25A and 25B. The membrane-catalyst assembly 13a from which the temporary substrates 24A and 24B have been peeled off is sent out by a send-out roll 14 and taken up into a roll by a take-up roll 15.
[0088] The feed roll 14 can be connected to a driving means not shown, and when the press rolls 40A, 40B are not clamping the electrolyte membrane 10 and the catalyst layer transfer sheets 20A, 20B, the electrolyte membrane 10 can be transported by controlling the speed.
[0089] [Second embodiment: Production of membrane-catalyst assembly (membrane-electrode assembly) 2] FIG. 2 is a side view showing a schematic configuration of an apparatus for producing a membrane / electrode assembly, which is one embodiment of the membrane / catalyst assembly production apparatus of the present invention.
[0090] In the membrane / catalyst assembly manufacturing apparatus 101 according to the embodiment shown in Fig. 2, a membrane / electrode assembly is manufactured as follows: Note that a description of the same parts as in the first embodiment will be omitted.
[0091] In the second embodiment, gas diffusion electrodes 80A and 80B are supplied from gas diffusion electrode supply rolls 81A and 81B instead of the catalyst layer transfer sheet used in the first embodiment. Gas diffusion electrode supply rolls 81A and 81B are installed above and below the unwound electrolyte membrane 10, respectively. The gas diffusion electrode 80A bonded to the upper surface of the electrolyte membrane 10 is unwound from the gas diffusion electrode supply roll 81A and transported in the order of the backup roll 31A and the guide roll 22A while being supported by the gas diffusion electrode substrate side opposite to the catalyst layer forming surface. The gas diffusion electrode 80B bonded to the lower surface of the electrolyte membrane 10 is unwound from the gas diffusion electrode supply roll 81B and transported in the order of the backup roll 31B and the guide roll 22B while being supported by the gas diffusion electrode substrate side opposite to the catalyst layer forming surface. In this way, the gas diffusion electrodes 80A and 80B are supplied to the thermocompression bonding section P so that the surfaces on which the catalyst layers are formed face the electrolyte membrane 10.
[0092] The electrolyte membrane 10, to which a liquid has been applied to the gas diffusion electrodes 80A, 80B and the bonding surfaces with the gas diffusion electrodes 80A, 80B, is supplied to a thermocompression bonding section P and passes between hot press rolls 40A, 40B, where it is bonded to form a membrane-catalyst assembly (membrane-electrode assembly) 13b. The membrane-catalyst assembly 13b as a membrane-electrode assembly is sent out by a send-out roll 14 and taken up into a roll by a take-up roll 15.
[0093] In addition, the manufacturing apparatus 101 for the membrane-catalyst assembly according to this embodiment is configured so that the gas diffusion electrodes 80A, 80B are transferred to both sides of the electrolyte membrane 10, but it may be configured so that the gas diffusion electrodes are transferred to only one side of the electrolyte membrane 10.
[0094] Here, the gas diffusion electrode is an electrode substrate on which the above-mentioned catalyst layer is laminated. As the electrode substrate, those that operate as gas diffusion electrodes for solid polymer fuel cells, solid polymer electrolyte membrane water electrolysis devices, electrochemical hydrogen pumps, etc. are used. For example, the material can be carbonaceous or conductive inorganic material, and more specifically, carbon materials such as sintered bodies from polyacrylonitrile, sintered bodies from pitch, graphite and expanded graphite, stainless steel, molybdenum, titanium, etc. are exemplified. The form of these is not particularly limited, and for example, they are used in a fibrous or particulate form, but fibrous conductive materials (conductive fibers) such as carbon fibers are preferred from the viewpoint of fuel permeability. As the electrode substrate using conductive fibers, either a woven fabric or a nonwoven fabric structure can be used. As such woven fabrics, plain weave, twill weave, satin weave, patterned weave, tapestry weave, etc. can be used without any particular limitation. As nonwoven fabrics, those made by papermaking method, needle punch method, spunbond method, water jet punch method, melt blow method, etc. can be used without any particular limitation. Knitted fabrics may also be used. In these fabrics, particularly when carbon fibers are used, woven fabrics obtained by carbonizing or graphitizing plain weave fabrics using flame-resistant spun yarns, nonwoven fabrics obtained by processing flame-resistant yarns into nonwoven fabrics using a needle punch method or a water jet punch method, etc., and matte nonwoven fabrics obtained by a papermaking method using flame-resistant yarns, carbonized yarns, or graphitized yarns are preferably used. In particular, nonwoven fabrics or cloths are preferably used because they are thin and strong fabrics. Examples of carbon fibers used in such electrode substrates include polyacrylonitrile (PAN)-based carbon fibers, phenol-based carbon fibers, pitch-based carbon fibers, and rayon-based carbon fibers. Examples of such electrode substrates include, for example, Toray Industries, Inc.'s carbon paper TGP series and SO series, and E-TEK's carbon cloth.
[0095] In addition, such electrode substrates can be subjected to water-repellent treatment to prevent the deterioration of gas diffusion and permeability due to water retention, partial water-repellent treatment to form a water drainage path, hydrophilic treatment, addition of carbon powder to reduce resistance, platinum plating to impart potential corrosion resistance, etc. In addition, a conductive intermediate layer containing at least an inorganic conductive material and a hydrophobic polymer can be provided between the electrode substrate and the catalyst layer. In particular, when the electrode substrate is a carbon fiber woven fabric or nonwoven fabric with a large porosity, the provision of a conductive intermediate layer can suppress the deterioration of performance caused by the catalyst solution permeating into the gas diffusion layer. [Third embodiment: Production of membrane-catalyst assembly (electrolyte membrane with catalyst layer) 3] In the third embodiment, first, a first catalyst layer is formed on one side of an electrolyte membrane by a catalyst layer forming apparatus 102 shown in Fig. 3. The first catalyst layer is formed as follows.
[0096] In this embodiment, the electrolyte membrane 10' is supported on a support and supplied to the catalyst layer forming apparatus 102. The material of the support for the electrolyte membrane is not particularly limited, but for example, a PET film can be used.
[0097] The electrolyte membrane 10' with the support is unwound from an electrolyte membrane supply roll 11 and supplied to a catalyst solution coating means 72 through a guide roll 12. The catalyst solution coating means 72 is provided facing the electrolyte membrane 10' supported on a backup roll 73. The catalyst solution coating means 72 receives catalyst solution from a catalyst solution tank 70 using a catalyst solution delivery pump 71, and forms a coating film by coating the supplied catalyst solution on the electrolyte membrane. The method of coating the catalyst solution in the catalyst solution coating means 72 is not particularly limited. Methods such as a gravure coater, a die coater, a comma coater, a roll coater, a spray coater, and a screen printing method can be used.
[0098] In this embodiment, the catalyst layer is formed by applying a catalyst solution to the electrolyte membrane 10', but the catalyst layer may be transferred and formed on the electrolyte membrane 10' using a catalyst layer transfer sheet.
[0099] Next, the coating film of the catalyst solution formed on the electrolyte membrane is dried by drying means 74, and the solvent in the catalyst solution is evaporated to form a dried first catalyst layer. The method of drying the catalyst solution in drying means 74 is not particularly limited. A method of blowing a heat medium such as hot air, a thermal oven method using a heater, or the like can be used.
[0100] The membrane / first catalyst layer assembly 16 in which the first catalyst layer is formed on the electrolyte membrane in this manner is delivered by a delivery roll 14 and taken up in a roll by a take-up roll 17 with the support attached.
[0101] Next, a second catalyst layer is formed on the surface of the electrolyte membrane opposite to the surface on which the first catalyst layer has been formed, by using a membrane-catalyst assembly manufacturing apparatus 103 according to the embodiment shown in Fig. 4. The second catalyst layer is formed as follows.
[0102] The membrane / first catalyst layer assembly 16 is unwound from the supply roll 18, passes through the guide roll 12, and is further passed through guide rolls 26A and 26B, whereby the support 51 is peeled off from the interface with the electrolyte membrane. The peeled support 51 is taken up by the support take-up roll 50.
[0103] A cover film 61 unwound from a cover film supply roll 60 is laminated onto the first catalyst layer surface of the membrane / first catalyst layer assembly 16 from which the support 51 has been peeled off via guide rolls 27A and 27B, and then the assembly is supplied to a thermocompression bonding section P. Note that the lamination of the cover film 61 may be performed before the support 51 is peeled off.
[0104] The cover film 61 is used to protect the first catalyst layer during the process of forming the second catalyst layer, and the material is not particularly limited as long as the function of the catalyst layer is not impaired by attachment and detachment. In general, natural fiber sheets such as paper, hydrocarbon-based plastic films such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyethylene (PE), polypropylene (PP), polyimide, and polyphenylene sulfide, fluorine-based films such as perfluoroalkoxyalkane (PFA), polytetrafluoroethylene (PTFE), and ethylene tetrafluoroethylene copolymer (ETFE), or materials with improved adhesion to the adherend by adding an acrylic adhesive, a urethane acrylate adhesive, a rubber adhesive, a silicone adhesive, or the like to these materials can be used. Materials with improved adhesion can support the electrolyte membrane while it is in contact with the liquid, and therefore can further prevent swelling of the electrolyte membrane.
[0105] The membrane-first catalyst layer assembly 16 supplied to the thermocompression bonding section P is subjected to a liquid application process and a thermocompression bonding process similar to those in the first embodiment, whereby the second catalyst layer is thermocompressed with the first catalyst layer covered with a cover film to form a membrane-catalyst assembly (electrolyte membrane with catalyst layer) 13c.
[0106] The membrane-catalyst assembly 13c as the catalyst-layered electrolyte membrane that has passed through the thermocompression bonding section P passes between the guide rolls 23A and 23B, at which time the temporary substrate 24A is peeled off from the membrane-catalyst layered assembly 13c and taken up by the temporary substrate take-up roll 25A. The membrane-catalyst assembly 13c from which the temporary substrate 24A has been peeled off is sent out by the delivery roll 14 and taken up in a roll by the take-up roll 15. The cover film 61 may be taken up while still bonded to the membrane-catalyst assembly 13c, or may be peeled off from the membrane-catalyst assembly 13c by the heat press roll 40B immediately after pressing. By taking up the membrane-catalyst assembly 13c while the cover film 61 is bonded to the membrane-catalyst assembly 13c, it is possible to suppress wrinkling and stretching of the catalyst-layered electrolyte membrane and protect the catalyst layer from physical damage caused by external factors. In addition, by peeling off the cover film 61 immediately after thermocompression bonding to expose the catalyst layer, it is possible to effectively discharge the liquid vapor generated in the thermocompression bonding process. In this case, the catalyst layer can be protected with a new cover film before being wound up.
[0107] [Fourth embodiment: Production of membrane-catalyst assembly (electrolyte membrane with catalyst layer) 4] In the fourth embodiment, first, a first catalyst layer is formed on one side of an electrolyte membrane by a membrane / catalyst assembly manufacturing apparatus 104 according to an embodiment shown in Fig. 5. The first catalyst layer is formed as follows.
[0108] In this embodiment, the electrolyte membrane 10' is supplied to the catalyst layer forming apparatus 104 in a state where it is supported on a support. The electrolyte membrane 10' with the support is unwound from an electrolyte membrane supply roll 11 and supplied to a thermocompression bonding section P. The electrolyte membrane 10' supplied to the thermocompression bonding section P has a first catalyst layer thermocompression-bonded thereto by the liquid application step and thermocompression bonding step similar to those of the first embodiment, to form a membrane / first catalyst layer assembly 16'.
[0109] The membrane-first catalyst layer assembly 16 ′, with the support and the temporary base material of the catalyst layer transfer sheet 20 A attached, is delivered by the delivery roll 14 and taken up in a roll by the take-up roll 17 .
[0110] Next, a second catalyst layer is formed on the surface of the electrolyte membrane opposite to the surface on which the first catalyst layer has been formed, by a catalyst layer forming apparatus 105 according to the embodiment shown in Fig. 6. The second catalyst layer is formed as follows.
[0111] The membrane / first catalyst layer assembly 16′ is unwound from the supply roll 18, and the support 51 is peeled off from the interface with the electrolyte membrane via guide rolls 26A and 26B. The peeled support 51 is taken up by the support take-up roll 50.
[0112] The membrane-first catalyst layer assembly 16' from which the support 51 has been peeled off is subjected to a catalyst solution coating means 72 and a drying means 74 similar to those in the third embodiment to form a second catalyst layer, thereby forming a membrane-catalyst assembly (catalyst-layered electrolyte membrane) 13d.
[0113] The membrane-catalyst assembly 13d serving as a catalyst-layered electrolyte membrane is delivered by a delivery roll 14 and taken up in a roll by a take-up roll 15 with the temporary substrate still attached. EXAMPLES
[0114] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0115] In Examples 1 to 6, the catalyst layer transfer sheet was prepared by coating a catalyst coating liquid consisting of a Pt-supported carbon catalyst TEC10E50E manufactured by Tanaka Kikinzoku Kogyo Co., Ltd. and a "Nafion" (registered trademark) solution on a continuous belt-shaped PTFE sheet substrate, and drying the catalyst layer transfer sheet to prepare a rolled catalyst layer transfer sheet (substrate width 100 mm, thickness 8 μm) (platinum loading amount: 0.3 mg / cm 2 ).
[0116] The electrolyte membranes in Examples 2 to 6 were produced with reference to the production method described in JP 2018-60789 A.
[0117] [Example 1] Using an apparatus having a schematic configuration as shown in FIG. 1, and following the method described in the first embodiment, a catalyst layer was transferred from the catalyst layer transfer sheet onto one side of a commercially available "Nafion" (registered trademark) membrane, product name NR211 (film thickness 25 μm), which was used as an electrolyte membrane.
[0118] In the liquid application process, 100% pure water was sprayed onto the electrolyte membrane at a depth of 1 cm using a fan-shaped spray nozzle CBIMV 80005S manufactured by Ikeuchi Co., Ltd. 2 The solution was applied dropwise in an amount of 0.5 μL per drop.
[0119] In the thermocompression bonding process, a pair of heat press rolls with a diameter of 250 mm were used, one of which was a stainless steel roll and the other a fluororubber roll with a hardness of 90° (Shore A). The pressure of the heat press roll was 3.0 MPa. The pressure was measured using a press scale made by Fujifilm Corporation. The roll surface temperature was 160°C, and the heating temperature was measured using a thermocouple attached to the bonding interface, resulting in a value of 115°C. The transport speed of the electrolyte membrane and catalyst layer transfer sheet was 4.0 m / min.
[0120] Visual inspection of the resulting membrane-catalyst assembly revealed that there was no transfer failure of the catalyst layer, or swelling or wrinkling of the electrolyte membrane, and that the assembly was of high quality.
[0121] [Example 2] Using an apparatus having a schematic configuration as shown in FIG. 1 , and in accordance with the method described in the first embodiment, a catalyst layer was transferred from the same catalyst layer transfer sheet as used in the above-mentioned Example 1 onto one surface of a polyether ketone-based polymer electrolyte membrane made of a polymer represented by the following formula (G1).
[0122] [ka]
[0123] In the liquid application process, 100% pure water was sprayed onto the electrolyte membrane at a depth of 1 cm using a fan-shaped spray nozzle CBIMV 80005S manufactured by Ikeuchi Co., Ltd. 2 0.3 μL was added per unit area.
[0124] In the thermocompression bonding process, a pair of heat press rolls with a diameter of 250 mm were used, one of which was a stainless steel roll and the other a fluororubber roll with a hardness of 90° (Shore A). The pressure of the heat press roll was 4.5 MPa. The pressure was measured using a press scale made by Fujifilm Corporation. The temperature of the roll surface was 160°C, and the heating temperature was measured using a thermocouple attached to the bonding interface, resulting in a value of 115°C. The transport speed of the electrolyte membrane and catalyst layer transfer sheet was 4.0 m / min.
[0125] Visual inspection of the resulting membrane-catalyst assembly revealed that there was no transfer failure of the catalyst layer, or swelling or wrinkling of the electrolyte membrane, and that the assembly was of high quality.
[0126] [Example 3] Using an apparatus having a schematic configuration as shown in FIG. 1, a catalyst layer was transferred from the catalyst layer transfer sheet onto one side of a polyarylene-based polymer electrolyte membrane made of a polymer represented by the following formula (G2), in accordance with the method described in the first embodiment.
[0127] [ka]
[0128] (In formula (G2), k, m, and n are integers, k is 25, m is 380, and n is 8.) The liquid application step and the thermocompression bonding step were carried out in the same manner as in Example 2.
[0129] Visual inspection of the resulting membrane-catalyst assembly revealed that there was no transfer failure of the catalyst layer, or swelling or wrinkling of the electrolyte membrane, and that the assembly was of high quality.
[0130] [Example 4] Using an apparatus having a schematic configuration shown in FIG. 1, and in accordance with the method described in the first embodiment, a catalyst layer was transferred from the catalyst layer transfer sheet onto one side of a polyethersulfone-based polymer electrolyte membrane composed of a segment represented by the following formula (G3) and a segment represented by the following formula (G4).
[0131] [ka]
[0132] (In formulas (G3) and (G4), p, q, and r are integers, p is 170, q is 380, and r is 4.) The liquid application step and the thermocompression bonding step were carried out in the same manner as in Example 2.
[0133] Visual inspection of the resulting membrane-catalyst assembly revealed that there was no transfer failure of the catalyst layer, or swelling or wrinkling of the electrolyte membrane, and that the assembly was of high quality.
[0134] [Example 5] According to the method described in the third embodiment, an electrolyte membrane with a catalyst layer was produced.
[0135] Using an apparatus with a schematic configuration shown in Fig. 3, a catalyst solution was applied to one side of a polyetherketone-based polymer electrolyte membrane made of a polymer represented by the formula (G1) and dried to form a first catalyst layer. The catalyst solution used was a catalyst coating solution made of Pt-supported carbon catalyst TEC10E50E manufactured by Tanaka Kikinzoku Kogyo Co., Ltd. and a "Nafion" (registered trademark) solution. The solution was dried at 120°C for 5 minutes to obtain a catalyst layer with a thickness of 5 µm.
[0136] Next, using an apparatus having a schematic configuration as shown in Fig. 4, a second catalyst layer was transferred from the catalyst layer transfer sheet to the other surface of the polyetherketone-based polymer electrolyte membrane on which the first catalyst layer was formed, to form a second catalyst layer. For the cover film to be laminated on the surface of the first catalyst layer, a PET film "Lumirror" (registered trademark) manufactured by Toray Industries, Inc. with a film thickness of 75 µm was used. The liquid application process and the thermocompression bonding process were carried out in the same manner as in Example 2.
[0137] When the cover film was peeled off from the obtained electrolyte membrane with a catalyst layer, no deposits or the like were found on the cover film. In addition, as a result of visually evaluating the obtained electrolyte membrane with a catalyst layer, there was no transfer failure of the catalyst layer, and no swelling or wrinkling of the electrolyte membrane, and it was of high quality.
[0138] [Example 6] According to the method described in the fourth embodiment, an electrolyte membrane with a catalyst layer was produced.
[0139] The first catalyst layer was transferred from the catalyst layer transfer sheet onto one side of a polyetherketone-based polymer electrolyte membrane made of a polymer represented by the formula (G1) using an apparatus having a schematic configuration shown in Fig. 5. The liquid application step and the thermocompression bonding step were performed in the same manner as in Example 2.
[0140] Next, using an apparatus having a schematic configuration as shown in FIG. 6, the same catalyst solution as in Example 5 was applied to the other surface of the electrolyte membrane on which the first catalyst layer was formed, and dried to form a second catalyst layer.
[0141] When the temporary substrate was peeled off from the obtained electrolyte membrane with a catalyst layer, no deposits or the like were found on the temporary substrate. In addition, as a result of visually evaluating the obtained electrolyte membrane with a catalyst layer, there was no transfer failure of the catalyst layer, and no swelling or wrinkling of the electrolyte membrane, and the membrane was of high quality.
[0142] [Example 7] A membrane-catalyst assembly was produced in the same manner as in Example 1, except that the following composite electrolyte membrane was used as the electrolyte membrane. The resulting membrane-catalyst assembly was visually evaluated and found to be of high quality with no transfer failure of the catalyst layer or swelling or wrinkling of the electrolyte membrane.
[0143] <Composite electrolyte membrane> A composite electrolyte membrane made by impregnating a 6 μm thick PTFE porous substrate (Tetratex, a registered trademark of Donaldson Company) with the following fluorine-based electrolyte solution.
[0144] <Fluorine-based electrolyte solution> Eighty parts by mass of ethylene glycol was added to 100 parts by mass of a 20% "Nafion (registered trademark)" n-propanol solution, and the n-propanol was removed under reduced pressure to replace the solvent, thereby obtaining an ethylene glycol solution of Nafion.
[0145] [Example 8] A membrane-catalyst assembly was produced in the same manner as in Example 5, except that the following composite electrolyte membrane was used as the electrolyte membrane. The resulting membrane-catalyst assembly was visually evaluated and found to be of high quality with no transfer failure of the catalyst layer or swelling or wrinkling of the electrolyte membrane.
[0146] <Composite electrolyte membrane> A composite electrolyte membrane made by impregnating a 6 μm thick PTFE porous substrate (Tetratex, a registered trademark of Donaldson Company) with the following hydrocarbon electrolyte solution.
[0147] <Hydrocarbon-based electrolyte solution> The solution was prepared by dissolving 0.26 parts by mass of a nonionic fluorine-based surfactant (polyoxyethylene ether-based surfactant "Ftergent" (registered trademark) FTX-218 manufactured by Neos Corporation) in 100 parts by mass of an N-methylpyrrolidone (NMP) solution (electrolyte concentration: 13% by mass) in which the polyether ketone-based polymer electrolyte represented by the formula (G1) was dissolved.
[0148] [Example 9] A membrane-catalyst assembly was produced in the same manner as in Example 1, except that the nozzle chambers 32A and 32B were not depressurized in the production apparatus of Figure 1. The obtained membrane-catalyst assembly was visually evaluated and found to be of high quality, with no transfer failure of the catalyst layer or swelling or wrinkling of the electrolyte membrane.
[0149] [Comparative Example 1] A catalyst layer was transferred onto one side of an electrolyte membrane from the same catalyst layer transfer sheet as used in Example 1 in the same manner as in Example 2, except that the liquid application step was not performed. The obtained membrane-catalyst assembly was visually evaluated, and poor transfer of the catalyst layer was found. [Industrial Applicability]
[0150] The membrane-catalyst assembly of the present invention can be applied, for example, as a catalyst-layered electrolyte membrane or a membrane-electrode assembly, to solid polymer fuel cells, solid polymer electrolyte membrane water electrolysis devices, electrochemical hydrogen pumps, etc. When the membrane-catalyst assembly of the present invention is an electrolyte membrane with a catalyst layer, it is preferable to further laminate an electrode substrate and apply it to the above-mentioned uses as a membrane-electrode assembly. [Explanation of symbols]
[0151] 100, 101, 103, 104: Membrane / catalyst assembly manufacturing equipment 102, 105: Catalyst layer forming device 10, 10': Electrolyte membrane 11, 18: Electrolyte membrane supply roll 13a, 13b, 13c, 13d: Membrane / catalyst assembly 14: Delivery roll 15, 17: Winding roll 16, 16': membrane-first catalyst layer assembly 12, 22A, 22B, 23A, 23B, 26A, 26B, 27A, 27B: Guide rolls 20A, 20B: Catalyst layer transfer sheet 21A, 21B: catalyst layer transfer sheet supply roll 24A, 24B: Temporary substrate 25A, 25B: Temporary substrate winding roll 30A, 30B: Spray nozzle 31A, 31B, 73: Backup roll 32A, 32B: Nozzle chamber 33A, 33B: Valve 34A, 34B: Pressure reducing tank 40A, 40B: Heat press roll 41A, 41B: Heat shield 50: Support winding roll 51:Support 60: Cover film supply roll 70: Catalyst solution tank 71: Catalyst solution delivery pump 72: Application means 74:Drying means 80A, 80B: Gas diffusion electrodes 81A, 81B: Gas diffusion electrode supply roll P:Thermocompression bonding part S: Space
Claims
1. A method for producing a membrane-catalyst assembly in which a catalyst layer is joined to an electrolyte membrane, comprising the steps of: a liquid applying step of applying a liquid under an atmospheric environment only to a surface of the electrolyte membrane before bonding; a thermocompression bonding step of bonding the electrolyte membrane to which the liquid has been applied and the catalyst layer by thermocompression bonding; wherein the electrolyte membrane before bonding has a support on a surface different from a surface to which a liquid is applied.
2. 2. The method for producing a membrane-catalyst assembly according to claim 1, wherein the liquid applied in the liquid application step is a liquid containing water.
3. 3. The method for producing a membrane-catalyst assembly according to claim 2, wherein the water content in the water-containing liquid is 50 mass % or more and 100 mass % or less.
4. 4. The method for producing a membrane-catalyst assembly according to claim 3, wherein the liquid applied in the liquid application step is pure water.
5. 5. The method for producing a membrane-catalyst assembly according to claim 1, wherein in the liquid applying step, the liquid is applied in the form of droplets only onto the surface of the electrolyte membrane.
6. The method for producing a membrane-catalyst assembly according to claim 5 , wherein in the liquid applying step, the liquid is applied by spraying.
7. In the liquid application step, the amount of the liquid in the thermocompression bonding step is set to 1 cm over the surface of the electrolyte membrane. 2 The method for producing a membrane-catalyst assembly according to any one of claims 1 to 6, wherein the amount of the mixture is 0.1 µL or more and 5 µL or less per unit time.
8. 8. The method for producing a membrane-catalyst assembly according to claim 1, wherein the electrolyte membrane is a hydrocarbon-based electrolyte membrane.
9. A method for producing a membrane-catalyst assembly, comprising bonding a catalyst layer to a surface of the electrolyte membrane by the method according to any one of claims 1 to 8.
10. 10. The method for producing a membrane-catalyst assembly according to claim 1, wherein the catalyst layer is supported by a substrate before being bonded to the electrolyte membrane, and the substrate has air permeability.
11. A method for producing a membrane-catalyst assembly comprising an electrolyte membrane and catalyst layers bonded to both sides of the electrolyte membrane, comprising the steps of: applying a catalyst solution to one surface of the electrolyte membrane and drying the solution to form a first catalyst layer; forming a second catalyst layer on the other surface of the electrolyte membrane; The step of forming the second catalyst layer includes a liquid applying step of applying a liquid only to a surface of the electrolyte membrane before bonding in an atmospheric environment; a thermocompression bonding step of bonding the electrolyte membrane to which the liquid has been applied and the second catalyst layer by thermocompression bonding; A method for producing a membrane-catalyst assembly having the above structure.
12. 12. The method for producing a membrane-catalyst assembly according to claim 11, further comprising the step of covering the first catalyst layer with a cover film, and the step of forming the second catalyst layer is performed in a state in which the first catalyst layer is covered with the cover film.
13. A method for producing a membrane-catalyst assembly comprising an electrolyte membrane and catalyst layers bonded to both sides of the electrolyte membrane, comprising the steps of: forming a first catalyst layer on one surface of the electrolyte membrane; and applying and drying a catalyst solution on the other surface of the electrolyte membrane to form a second catalyst layer, The step of forming the first catalyst layer includes a liquid applying step of applying a liquid only to a surface of the electrolyte membrane before bonding under an atmospheric condition, and a thermocompression bonding step of bonding the electrolyte membrane to which the liquid has been applied and the first catalyst layer by thermocompression bonding. A method for producing a membrane-catalyst assembly having the above structure.
14. An apparatus for manufacturing a membrane-catalyst assembly in which a catalyst layer is joined to an electrolyte membrane, comprising: The electrolyte membrane has a support on one surface thereof, a liquid applying means for applying a liquid to only a surface of the electrolyte membrane before bonding, the surface being different from the surface on which the support is disposed, under an atmospheric environment; a thermocompression bonding means for bonding the electrolyte membrane to which the liquid has been applied and the catalyst layer by thermocompression bonding; A manufacturing apparatus for a membrane-catalyst assembly having the above structure.
15. 15. The apparatus for producing a membrane-catalyst assembly according to claim 14, wherein the liquid applying means applies the liquid in the form of droplets only onto the surface of the electrolyte membrane.
16. 16. The apparatus for producing a membrane-catalyst assembly according to claim 15, wherein the liquid applying means is a spray.
Citation Information
Patent Citations
Manufacturing method for electrolytic membrane -electrode substrate complex
JP2004253267A
Manufacturing method of junction of electrolyte membrane and electrode
JP2005158518A
Manufacturing method of membrane electrode junction
JP2005222894A
Membrane-electrode assembly manufacturing method
JP2009140652A
Manufacturing method of membrane electrode assembly for polymer electrolyte fuel cell
JP2013069535A